Silica-based particle dispersion and method for producing same
By using highly irregular silica gel particles with controlled crushing and growth, the method addresses inefficiencies in producing silica particles for chemical-mechanical polishing, achieving high polishing rates and surface accuracy with reduced defects.
Patent Information
- Application Number
- JP2020168315
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-10-09
- Filing Date
- 2020-10-05
- Publication Date
- 2024-11-28
- Estimated Expiration
- 2040-10-05
AI Technical Summary
Existing methods for producing irregularly shaped silica particles with controlled particle size, distribution, and strength for chemical-mechanical polishing are inefficient, leading to low polishing rates and increased scratches or residue due to coarse or small particles.
A method involving the use of highly irregular silica gel particles with controlled crushing and growth using a silicic acid solution maintains particle irregularity and strength, resulting in a silica-based particle group with specific size, distribution, and strength suitable for abrasive applications.
The method achieves high polishing rates with reduced scratches and residue, providing high surface accuracy and efficiency in chemical-mechanical polishing processes.
Smart Images

Figure 0007591376000003 
Figure 0007591376000004 
Figure 0007591376000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a silica-based particle dispersion etc. In particular, the present invention relates to a silica-based particle dispersion etc. that contains a silica-based particle group having a particle size, particle size distribution, irregularity, etc. that are preferable as an abrasive, and is particularly suitable as a polishing abrasive dispersion for planarizing NiP-plated polished substrates and silica-based substrates by chemical mechanical polishing (CMP) in the manufacture of magnetic disks. [Background technology]
[0002] In the manufacturing process of magnetic disks and semiconductors, chemical mechanical polishing (CMP) is used to planarize substrates such as silicon wafers, glass HDs, and aluminum HDs. In this chemical mechanical polishing, a polishing slurry is used, in which abrasive particles such as silica or ceria are dispersed in water and chemical components are added to control the polishing performance. In particular, it is known that abrasive particles have a large effect on polishing performance, and the performance required of abrasive particles is that they can achieve a high polishing rate and do not cause defects such as scratches on the polished surface.
[0003] A common method for achieving a high polishing rate is to use abrasives with a large particle size. However, if the particle size of the abrasives becomes too large, the number of abrasives per mass decreases, which in turn reduces the polishing rate and tends to increase scratches. Therefore, in order to achieve a high polishing rate without increasing scratches, it is known to be effective to use non-spherical abrasives, that is, to use irregularly shaped abrasives.
[0004] Conventional methods for preparing silica particle groups containing irregular silica particles having a particle size suitable for use as an abrasive include a method in which water glass is used as a raw material to aggregate silica particles during nucleation, and a method in which a silicic acid liquid is added to irregular seed particles prepared by this method or the like to increase the particle size (Patent Document 1).
[0005] In addition to Patent Document 1, a method for preparing silica-based particles having irregular shapes and relatively large particle diameters is known, which includes a process (Patent Document 2) for producing irregular silica particles, which comprises step a) of wet-crushing porous silica gel under alkaline conditions to produce a crushed gel containing irregular silica particles, step b) of adding silicic acid liquid under alkaline conditions to a solution containing the crushed gel and heating the solution to build up and fill the pores of the irregular silica particles through a reaction with silicic acid while growing the particles while maintaining their irregular shapes, and step c) of recovering the grown irregular silica particles. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Patent No. 5127452 [Patent Document 2] JP 2017-177576 A Summary of the Invention [Problem to be solved by the invention]
[0007] In irregular particles, the irregularity (ratio of weight average particle diameter to particle diameter equivalent to projected area) also has a large effect on the polishing performance. Specifically, particles with a large irregularity tend to have a high polishing speed. On the other hand, particles with a small irregularity tend to have a low polishing speed because they are close to a perfect sphere or ellipse. However, since irregular particles are non-spherical in shape, they usually tend to cause scratches more easily than spherical or nearly spherical particles (non-irregular particles), and this tendency is particularly noticeable when the irregularity is high.
[0008] In addition, it is generally known that the particle size and particle size distribution of polishing abrasives greatly affect polishing performance, and abrasives with large particle sizes have a high polishing speed, but tend to deteriorate the surface precision (surface roughness, waviness, scratches, etc.) of the polished substrate. On the other hand, abrasives with small particle sizes can finish the substrate surface smoothly and are less likely to cause scratches, but the polishing speed is slow. This is not limited to spherical particles, but also applies to irregularly shaped particles. Although the particle size distribution of irregular particles is diverse, particles with a relatively large particle size usually have a high polishing rate, so irregular particles with as large an average particle size as possible are used when a high polishing rate is required. However, irregular particles with a relatively large average particle size tend to have a large tail in the particle size distribution, so they often contain a small amount of coarse particles compared to the average particle size. These coarse particles tend to cause scratches on the polished substrate, or to deteriorate the surface roughness and waviness of the substrate. Therefore, irregular particles with a relatively large average particle size and very few coarse particles or excessively large particles (collectively called "coarse particles") are desired as abrasives used in polishing that requires a high polishing rate.
[0009] Furthermore, particles with a relatively small particle size, regardless of whether they are spherical or irregularly shaped, tend to have a low polishing rate because the amount of polishing per abrasive grain is small. Also, particles with a relatively small particle size tend to leave abrasive grains on the substrate after polishing (this is called "abrasive grain residue"). These abrasive grain residues tend to be difficult to remove even in the cleaning process after polishing. This tendency is also seen in irregularly shaped particles with a relatively large average particle size, and it can be said that irregularly shaped particles with a relatively large average particle size and a particle size distribution with the tail of the particle size distribution spreading toward the small particle size side are prone to leaving abrasive grain residues. Therefore, in order to achieve suitable chemical mechanical polishing that achieves both a high polishing rate and high surface precision, it is desirable to have abrasive grains that contain relatively large irregularly shaped particles, have a large number of abrasive grains per mass, contain as few coarse particles as possible that would reduce polishing performance, and further contain as few relatively small particles as possible that would cause residual abrasive grains.
[0010] However, in the method of aggregating silica particles during nucleation using water glass as a raw material, it was difficult to obtain irregular silica particles with a specific surface area equivalent particle diameter of 100 nm or more. Furthermore, in this method, in the silica particle aggregation process during nucleation, some core particles may undergo a runaway reaction, resulting in coarse aggregates, and these coarse aggregates may cause scratches. In addition, in the method of using irregular silica particles with a specific surface area equivalent particle diameter of 100 nm or less as seed particles and adding silicic acid liquid to these seed particles to grow the particle diameter to a large size, when the particles are grown using silicic acid liquid so that the specific surface area equivalent particle diameter is 100 nm or more, the seed particles grow into a spherical or nearly spherical shape, so it was difficult to grow the irregular seed particles as they are to obtain relatively large irregular silica particles.
[0011] Furthermore, the present inventors have investigated a method of obtaining irregular silica particles by crushing wet silica as another method for preparing silica particle groups containing irregular silica particles, and although irregular silica particles were obtained, wet silica with a gel structure has a high particle strength for controlling particle size and particle size distribution by crushing or disintegration, so that, for example, when performing such control by disintegration treatment, it is necessary to proceed with the treatment under strong disintegration conditions for a relatively long period of time, and as a result, the irregularity of the particles tends to decrease. Furthermore, when the porous silica gel obtained in this way with a low irregularity is used as an abrasive for polishing, only polishing abrasives with a significantly low polishing rate are obtained because of the porosity. In addition, there is a method of using the obtained porous silica gel with a low irregularity as a seed to grow particles with silicic acid or the like, and reinforcing the surface and internal pores with silica to improve particle strength, but the present inventors have investigated it and found that the irregularity is further reduced by particle growth, so that a sufficient polishing rate cannot be obtained.
[0012] Therefore, an object of the present invention is to provide a silica-based particle group (a silica-based particle group that is an abrasive containing relatively large irregularly shaped particles, exhibits a specific particle size distribution, and contains irregularly shaped particles having the required particle strength and irregularity) that can achieve a high polishing rate and high surface precision when applied to polishing applications, for example, on silica-based substrates or NiP-plated substrates to be polished, as well as a silica-based particle dispersion liquid containing this silica-based particle group, and a method for producing this silica-based particle group. [Means for solving the problem]
[0013] In order to solve the above problems, the present inventors have investigated a method of using highly irregular silica-based gel particles obtained by crushing silica-based gel having a relatively small specific surface area and a relatively large primary particle size under specific conditions as seed particles, instead of irregular seed particles having a relatively large specific surface area and a relatively small primary particle size obtained from conventional water glass, and further growing the seed particles by adding silicic acid liquid. The highly irregular silica-based gel particles are obtained by wet crushing silica-based gel under alkaline conditions, and are almost free of coarse particles and have a relatively uniform particle size. Furthermore, since the raw material silica-based gel has a relatively small specific surface area and a relatively large primary particle size, the strength of the silica-based gel particles is weak and they are easily crushed, so the high irregularity derived from the structure of the raw material silica-based gel is maintained.
[0014] By using such highly irregular silica gel particles as seed particles and growing the seed particles in the presence of silicic acid liquid, silicic acid is preferentially deposited from the pores between the primary particles of the seed particles (recesses between the primary particles). Since the primary particle diameter of the seed particles is relatively large, the pores between the primary particles can be completely filled with silicic acid. For this reason, it is presumed that the particles can be grown while maintaining high particle strength and high irregularity. In addition, since the raw silica gel particles are made of silica-based gel with a relatively small specific surface area and a relatively large primary particle size, they are easily crushed, and the coarse particles are preferentially crushed during crushing, so that the product contains almost no coarse particles. By using this silica-based particle group as an abrasive, it has been found that the polishing speed is relatively high, the occurrence of scratches on the polished surface is greatly suppressed, and a polished surface with small surface roughness and waviness can be obtained.
[0015] Based on the above findings, the present inventors have completed the present invention, which is a silica-based particle group consisting of irregular silica-based particles and non-irregular silica-based particles having particle size, particle size distribution, degree of irregularity and particle strength suitable as an abrasive, a silica-based particle dispersion containing the same, and a method for efficiently producing the silica-based particle group. The present invention relates to the following (1) to (13).
[0016] (1) A silica-based particle dispersion liquid containing a silica-based particle group consisting of irregularly shaped silica-based particles and non-irregularly shaped silica-based particles, The silica-based particle group is a silica-based particle dispersion that satisfies the following [1] to [3]. [1] The weight average particle diameter (D1) is 60 to 400 nm, and the specific surface area converted particle diameter (D2) is 20 to 300 nm. [2] The irregularity D (D=D1 / D3), which is the ratio of the weight average particle diameter (D1) to the projected area equivalent particle diameter (D3), is in the range of 1.1 to 5.0. [3] When the volumetric particle size distribution is subjected to waveform separation, it becomes a multi-modal distribution in which three or more separation peaks are detected. (2) The silica-based particle dispersion liquid according to (1) above, wherein the silica-based particles have a skewness in the range of −20 to 20 in their volume-based particle size distribution. (3) The silica-based particle dispersion liquid according to any one of (1) and (2) above, characterized in that, among the separation peaks obtained as a result of waveform separation of the volume-based particle size distribution of the silica-based particle group, the volume ratio of the largest particle component is 75% or less. (4) The silica-based particle dispersion according to any one of (1) to (3) above, wherein in a number-based particle size distribution obtained by SEM image analysis of the silica-based particle group, the aspect ratio of a small particle component is in the range of 1.05 to 5.0. (5) The silica-based particle dispersion according to any one of (1) to (4) above, wherein the silica-based particles have a particle size variation coefficient of 30% or more in a volume-based particle size distribution. (6) The silica-based particle dispersion liquid according to any one of (1) to (5) above, characterized in that the silica-based particle group has a smoothness S (S=S2 / S1) in the range of 1.1 to 5.0, the smoothness S being expressed as the ratio of the area (S2) of a circle equivalent to the average peripheral length as determined by image analysis to the average area (S1) as determined by image analysis. (7) The silica-based particle dispersion liquid according to any one of (1) to (6), wherein in a volume-based particle size distribution of the silica-based particle group, a ratio Q (Q=Q2 / Q1) of a volume (Q2) of particles having a particle size of 0.7 μm or more to a total volume (Q1) is 5.0% or less. (8) A polishing abrasive dispersion containing the silica-based particle dispersion according to any one of (1) to (7) above. (9) A silica-based particle group consisting of irregularly shaped silica-based particles and non-irregularly shaped silica-based particles, A group of silica-based particles that satisfy the following [1] to [3]. [1] The weight average particle diameter (D1) is 60 to 400 nm, and the specific surface area converted particle diameter (D2) is 20 to 300 nm. [2] The irregularity D (D=D1 / D3), which is the ratio of the weight average particle diameter (D1) to the projected area equivalent particle diameter (D3), is in the range of 1.1 to 5.0. [3] When the volumetric particle size distribution is subjected to waveform separation, it becomes a multi-modal distribution in which three or more separation peaks are detected.
[0017] (10) A method for producing a silica-based particle group comprising irregularly shaped silica-based particles and non-irregularly shaped silica-based particles, comprising the following steps a to c: (Step a) Silica-based gel (Specific surface area 50~200m 2 / g)The mixture is wet-disintegrated under alkaline conditions to produce particles made of highly irregular silica-based gel. (Weight average particle diameter 60~142nm) forming a solution containing (Step b) adding a silicic acid liquid under alkaline conditions to a solution containing particles made of the highly irregular silica-based gel and heating the solution; filling the pores between the primary particles of the particles made of the highly irregular silica-based gel by a reaction with the silicic acid contained in the silicic acid liquid, while growing the particles while maintaining a high degree of irregularity, to form irregular silica-based particles. (Specific surface area 136m 2 / g or less [However, 30m 2 / g or less], weight average particle size 60 to 400 nm) The process of making it. (Step c) A step of concentrating and recovering the silica-based particle group including the grown irregularly shaped silica-based particles. 。 (11 In the step (a), the silica-based gel is wet-disintegrated under an alkaline condition of pH 8.0 to 11.5 to obtain a solution containing particles made of the highly irregular silica-based gel; In the step b, the SiO2 concentration of the solution containing the particles made of the highly irregular silica-based gel is adjusted to 1 to 10 mass%, the solution is heated to 60°C to 170°C, and the silicic acid liquid is added continuously or intermittently under an alkaline condition of pH 9 to 12.5, so that the pores between the primary particles of the particles made of the highly irregular silica-based gel are filled by a reaction with the silicic acid, thereby reducing the specific surface area of the particles and allowing the particles to grow while maintaining their irregular shapes; In the step c), a solution containing the grown irregular shaped silica-based particles is concentrated to recover a silica-based particle group containing the irregular shaped silica-based particles. 9 )or( 10 A method for producing a silica-based particle group comprising irregularly shaped silica-based particles and non-irregularly shaped silica-based particles as described in (1) above. ( 12 In the step b), the amount of the silicic acid solution added is in a range in which the SiO2 molar concentration of the silicic acid solution is 0.5 to 20 times the SiO2 molar concentration of the solution containing the particles made of the highly irregular silica-based gel. 9 )~( 11 2. A method for producing a silica-based particle group comprising irregularly shaped silica-based particles and non-irregularly shaped silica-based particles according to any one of 1 to 10. Effect of the Invention
[0018] The silica-based particle group consisting of the irregular silica-based particles and non-irregular silica-based particles of the present invention has particle size, particle size distribution, irregularity and particle strength suitable for use as an abrasive, and therefore when a silica-based particle dispersion containing this is used, for example, as a polishing abrasive dispersion, or when this polishing abrasive dispersion is used as a polishing slurry as is, even objects to be polished, such as NiP-plated polished coatings and silica-based substrates, can be polished at high speed without the abrasive particles penetrating the substrate, and at the same time high surface precision (few scratches, small surface roughness (Ra) and waviness (Wa) of the substrate to be polished, etc.) can be achieved. In addition, the silica-based particle group consisting of irregularly shaped silica-based particles and non-irregularly shaped silica-based particles of the present invention has an uneven surface, with minute protrusions, and also has a scavenger effect of adsorbing polishing debris, ion components, oligomer components, organic matter, etc., generated during polishing. Therefore, it is possible to prevent redeposition of these components onto the polishing substrate, and to achieve a polished surface with little residue.
[0019] Furthermore, in the method for producing a silica-based particle group consisting of irregular silica-based particles and non-irregular silica-based particles of the present invention, by using the particles that have been subjected to the external shape adjustment of the silica-based gel as seed particles, the seed particles can be grown large while maintaining a high degree of irregularity in the process of adding silicic acid liquid, and the strength of the particles can also be increased. As a result, a silica-based particle group consisting of irregular silica-based particles and non-irregular silica-based particles having particle size, particle size distribution, degree of irregularity and particle strength suitable for use as an abrasive can be efficiently obtained. [Brief description of the drawings]
[0020] [Figure 1] Illustrative diagram of kurtosis in particle size distribution [Diagram 2] Illustrative diagram of skewness in particle size distribution DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] The silica-based particle group consisting of irregularly shaped silica-based particles and non-irregularly shaped silica-based particles of the present invention and the silica-based particle dispersion liquid containing the same will be specifically described. Note that in the present invention, the term "particle group" means an assembly of a large number of particles.
[0022] <Weight average particle diameter (D1)> The weight average particle diameter (D1) of the silica-based particle group of the present invention is 60 to 400 nm, preferably 80 to 350 nm, and most preferably 100 to 300 nm. When a silica-based particle group having a weight average particle diameter in the range of 60 to 400 nm is used as an abrasive, a high polishing speed can be obtained and scratches are unlikely to occur. When a silica-based particle group having a weight average particle diameter of less than 60 nm is used as an abrasive, it is difficult to obtain a required polishing speed, and furthermore, small particles tend to remain on the substrate after polishing. When a silica-based particle group having a weight average particle diameter of more than 400 nm is used as an abrasive, scratches tend to occur easily, and even if the weight average particle diameter is increased further, the number of abrasive particles per mass decreases, so that the polishing speed may not be improved.
[0023] Here, in the present invention, the weight-average particle diameter (D1) is the average particle diameter obtained from the weight-based particle diameter distribution obtained by diluting the silica-based particle dispersion to be measured with a 0.05% by mass sodium dodecyl sulfate aqueous solution to a solid content concentration of 2% by mass, injecting 0.1 ml of the diluted solution into a conventionally known disk centrifugal particle diameter distribution measuring device (e.g., manufactured by CPS Instruments, Inc.) with a syringe, and measuring the diluted solution in a density gradient solution of 8% to 24% sucrose at 18,000 rpm. In other words, in the present invention, this weight-average particle diameter means the "average particle diameter of the weight-converted particle diameter distribution".
[0024] <Specific surface area equivalent particle diameter (D2)> The silica-based particle group of the present invention has a specific surface area converted particle diameter (D2) of 20 to 300 nm, preferably 25 to 250 nm, more preferably 30 to 200 nm, and most preferably 35 to 150 nm. When a silica-based particle group having a specific surface area converted particle diameter (D2) in the range of 20 to 300 nm is used as an abrasive, a high polishing rate can be obtained and scratches are unlikely to occur. When a silica-based particle group having a specific surface area converted particle diameter (D2) of less than 20 nm is used as an abrasive, it is difficult to obtain a required polishing rate, and furthermore, small particles tend to remain on the substrate after polishing. When a silica-based particle group having a specific surface area converted particle diameter (D2) of more than 300 nm is used as an abrasive, scratches tend to occur and the surface roughness of the substrate after polishing tends to deteriorate. Furthermore, even if the specific surface area converted particle diameter is made larger than this, the number of abrasive particles per mass decreases, and the polishing rate tends to decrease conversely.
[0025] In the present invention, the particle diameter converted into specific surface area (D2) means the average particle diameter converted into specific surface area, and is the specific surface area (SA: m 2 / g) and the particle density (ρ) [ρ = 2.2 for silica], using the formula D2 = 6000 / (SA × ρ). The BET method is as follows. First, 50 ml of silica sol (silica-based particle dispersion liquid) to be measured is adjusted to pH 3.5 with nitric acid, 40 ml of 1-propanol is added to it, and the sample is dried at 110 ° C for 16 hours. The sample is then crushed in a mortar and baked in a muffle furnace at 500 ° C for 1 hour to prepare a measurement sample. Then, using a known specific surface area measuring device (e.g., Yuasa Ionics, model number Multisorb 12, etc.), the specific surface area is calculated from the amount of nitrogen adsorption by the nitrogen adsorption method (BET method) using the BET one-point method. In the specific surface area measuring device, 0.5 g of the baked sample is placed in a measurement cell and degassed for 20 minutes at 300 ° C in a mixed gas flow of 30 vol % nitrogen / 70 vol % helium, and then the sample is kept at liquid nitrogen temperature in the mixed gas flow to allow equilibrium adsorption of nitrogen to the sample. Next, the sample temperature is gradually raised to room temperature while the mixed gas is being flowed, during which the amount of nitrogen desorbed is detected, and the specific surface area (SA) of the silica fine particles in the sample is calculated using a calibration curve prepared in advance.
[0026] In addition, when the specific surface area of the silica-based particles is high, sintering occurs during firing in the BET method, and the specific surface area (SA) of the particles increases to 100 m. 2 / g or more, the specific surface area (SA) is calculated by the titration method. The titration method here is the following method. First, a sample equivalent to 1.5 g of SiO2 is collected in a beaker, then transferred to a thermostatic reaction tank (25°C), and pure water is added to make the liquid volume 90 ml (the following operations are performed in a thermostatic reaction tank maintained at 25°C). Next, 0.1 mol / L hydrochloric acid aqueous solution is added to this to make the pH 3.6. Furthermore, 30 g of sodium chloride is added, and the solution is diluted to 150 ml with pure water and stirred for 10 minutes. Then, a pH electrode is set, and 0.1 mol / L sodium hydroxide solution is dropped while stirring to adjust the pH to 4.0. Furthermore, the sample adjusted to pH 4.0 is titrated with 0.1 mol / L sodium hydroxide solution, and the titration amount and pH value in the range of pH 8.7 to 9.3 are recorded at least four points, and a calibration curve is made by setting the titration amount of 0.1 mol / L sodium hydroxide solution as X and the pH value at that time as Y. Then, the consumption amount V (ml) of 0.1 mol / L sodium hydroxide solution required to change the pH from 4.0 to 9.0 per 1.5 g of SiO2 is calculated from the equation V = (A × f × 100 × 1.5) / (W × C), and this is used to calculate the specific surface area according to the equation SA = 29.0V-28. In the above formula, A is the titer (ml) of 0.1 mol / L sodium hydroxide solution required per 1.5 g of SiO2 to change the pH from 4.0 to 9.0, f is the titer of 0.1 mol / L sodium hydroxide solution, C is the SiO2 concentration of the sample (%), and W is the amount of sample taken (g).
[0027] <Deformity degree> The irregularity is expressed by dividing the weight average particle diameter (D1) by the particle diameter equivalent to projected area (D3). The particle diameter equivalent to projected area (D3) is measured and calculated by the following method. First, a scanning electron microscope (SEM) is used to measure an arbitrary portion of the surface of a silica-based particle at a magnification of 3000 times and a resolution of 1.1 x 10 per visual field. -3 mm 2 Then, for all silica fine particles contained in each image taken in each field of view, the projected area of each particle is measured by image analysis using an image analysis system, the particle diameter (circle diameter) of the circular particle corresponding to each measured area is calculated, and the number average (arithmetic mean diameter) of these is taken as the particle diameter equivalent to the projected area (D3). The silica-based particle group of the present invention has a degree of irregularity D (D=D1 / D3) in the range of 1.1 to 5.0, preferably in the range of 1.1 to 4.0, and more preferably in the range of 1.1 to 3.5. A silica-based particle group with a high degree of irregularity indicates that the average aspect ratio of the particle group (the average value of the "long axis / short axis ratio of the smallest circumscribing rectangle") is high. When this average aspect ratio is high, the particles mainly come into contact with the substrate at the long axis during polishing, the contact area with the substrate increases, and the polishing rate increases, which is preferable. However, when this degree of irregularity exceeds 5.0, even if the degree of irregularity is further increased, the polishing rate does not improve, and scratches and undulations tend to occur more easily. In addition, when this degree of irregularity is less than 1.1, it indicates that the shape of the particles is close to a perfect sphere, and when polishing is performed using a silica-based particle dispersion containing such a silica-based particle group, the polishing rate tends to decrease. Here, the aspect ratio means the ratio of the long side to the short side (long side / short side) of the smallest area of the rectangle or square inscribed by the particle. Also, the average aspect ratio means the simple average value of the aspect ratios of a certain number of particles or more.
[0028] The proportion of irregular silica-based particles contained in the silica-based particle dispersion liquid containing a silica-based particle group consisting of irregular silica-based particles and non-irregular silica-based particles according to the present invention is not particularly limited as long as it satisfies the requirements of [1], [2], and [3] above. However, it is recommended that the proportion of irregular silica-based particles having an aspect ratio of 1.1 or more to the total (said silica-based particle group) is preferably 30% or more, and more preferably 40% or more. The method for measuring the proportion of the number of irregular shaped silica particles having an aspect ratio of 1.1 or more is as shown in the examples described later.
[0029] <Kurtosis> The kurtosis in the volumetric particle size distribution of the silica-based particle group of the present invention is preferably −20 to 20, more preferably −10 to 10, and most preferably −5 to 3. When a silica-based particle group having a kurtosis in this range is used as an abrasive, a higher polishing rate can be obtained, and a substrate having a smoother surface (small surface roughness (Ra), small substrate waviness (Wa), and fewer scratches) can be obtained after polishing.
[0030] Here, kurtosis is calculated only from the particle size distribution, regardless of the shape or size of the particles, and when kurtosis is close to zero (normal distribution), it indicates that the particle size distribution is close to the normal distribution. Also, a particle size distribution with a kurtosis value greater than zero indicates that the center of the peak is sharper than the normal distribution, and the distribution has wider tails (Figure 1(a)), while a particle size distribution with a kurtosis value less than zero indicates that the peak is flat and the tails are not wider (Figure 1(b)).
[0031] In the present invention, the kurtosis in the volumetric particle size distribution of the silica-based particle group may be a negative value. When the kurtosis is negative, it indicates that the peak is flat, there are few small and large particle components on the left and right of the distribution, and the particle size distribution is flat and the particle size is relatively uniform. When such a silica-based particle group with few small and large particle components is used as an abrasive, there is little abrasive residue and the polishing speed is high, which is preferable.
[0032] <skewness> The skewness in the volumetric particle size distribution of the silica-based particle group of the present invention is preferably −20 to 20, more preferably −15 to 15, and most preferably −10 to 10. When a silica-based particle group having a skewness in this range is used as an abrasive, a higher polishing rate can be obtained, and a substrate having a smoother surface (small surface roughness (Ra), small substrate waviness (Wa), and few scratches) can be obtained after polishing.
[0033] Here, skewness, like kurtosis, is calculated only from the particle size distribution, regardless of particle shape or size, and skewness close to zero indicates that the particle size distribution is close to a normal distribution. Also, a particle size distribution with a skewness value greater than zero has a peak on the left side of the distribution (the side with smaller particle sizes) and a long tail to the right (Figure 2(a)), whereas a particle size distribution with a skewness value less than zero has a peak on the right side of the distribution (the side with larger particle sizes) and a long tail to the left (Figure 2(b)).
[0034] Usually, the skewness of the volumetric particle size distribution of silica-based particles obtained by the crushing and grinding method is often positive, while particles obtained by the build-up method tend to have a normal distribution, so the skewness is often close to zero. When the skewness is positive, the particle size distribution has a peak at a slightly smaller particle size position and a wide tail on the larger particle size side. When silica-based particles having a particle size distribution with a peak on the small particle size side are used as abrasives, a smooth surface tends to be obtained after polishing because there are many components with small particle sizes. On the other hand, silica-based particles with a significantly large skewness have a particle size distribution with a wide tail on the large particle size side, and when used as abrasives, scratches tend to occur easily, depending on the average particle size.
[0035] In the present invention, the skewness in the volumetric particle size distribution of the silica-based particle group may be a negative value. A silica-based particle group with a negative skewness has a particle size distribution with a peak at a larger particle size position and a broad tail on the small particle side, but since the large particle side of the particle size distribution is sharp (i.e., there are few significantly large particles), scratches are unlikely to occur even when used as an abrasive. However, a silica-based particle group with a skewness smaller than -20 has a particle size distribution with a too broad tail on the small particle side, and since the small particle component increases, there is a tendency for abrasive residue to occur when used as an abrasive.
[0036] <Measuring volumetric particle size distribution and calculating kurtosis and skewness> In the present invention, the volumetric particle size distribution of the silica-based particle group is measured by centrifugal sedimentation. For example, the silica-based particle dispersion is diluted with a 0.05% by mass sodium dodecyl sulfate aqueous solution to adjust the solid content concentration to 2% by mass, and the volumetric particle size distribution can be measured using a known disk centrifugal particle size distribution measuring device (e.g., manufactured by CPS Instruments, etc.). The kurtosis and skewness are calculated from the average value and standard deviation of the volume-based particle size distribution thus obtained by a conventional formula. For example, the kurtosis and skewness can be calculated using JMP Ver. 13.2 manufactured by SAS Institute Japan. In addition, in the volume-based particle size distribution, the frequency of a certain particle size may rarely be a negative value, and in such a case, the frequency is calculated as zero.
[0037] <Multimodal distribution> When the volumetric particle size distribution of the silica-based particle group of the present invention is subjected to waveform separation by the following method, it becomes a multi-modal distribution in which three or more separation peaks are detected. In the case of a particle group with a unimodal distribution, the polishing speed and waviness occur according to the particle size, and when the particle size is large, the polishing speed is high but the waviness is large, and when the particle size is small, the waviness is improved but the polishing speed is low. In contrast, in the case of a particle group with a multimodal distribution, polishing proceeds while leaving polishing marks according to the particle size of each component, and the sum of these becomes the waviness and polishing speed. Therefore, if the distribution is such that the small particle component shows a sufficient polishing speed at the same time as the large particle component (for example, a trapezoidal distribution that contains many small and large particles and becomes multi-modal when waveform separation is performed), the polishing speed and waviness can be compatible.
[0038] Waveform separation is performed by analyzing the volumetric particle size distribution obtained by the above-mentioned disk centrifugal particle size distribution measuring device using the peak analyzer of the graph creation and data analysis software Origin (manufactured by OriginLab Corporation). First, the baseline is set to 0, the peak type is set to Gaussian, the maximum point of the particle size distribution is selected as the peak position, and peak fitting is performed without weighting. It is confirmed that the calculated peak does not deviate from the following conditions 1 and 2. If it does deviate, the peak position is shifted to an arbitrary position within the distribution range until the following conditions 1 and 2 are satisfied, and the peak fitting is repeated. After that, if the corrected R-squared value is 0.99 or less, a peak is added to an arbitrary position within the distribution range, and the peak fitting is repeated until the corrected R-squared value is 0.99 or more. The number of separated peaks at this time is taken as the number of peaks. Condition 1: Each calculated peak does not take a value greater than the original distribution. Condition 2: None of the calculated peaks take negative values. Such a silica-based particle group having a multimodal volume-based particle size distribution has a wide range from large particles to small particles (broad distribution), and has more suitable polishing performance. Specifically, it is desirable that the volume ratio of the maximum peak after waveform separation is 75% or less of the total volume. If the volume ratio of the maximum peak is 75% or less, the distribution becomes broad, and when waveform separation is performed, the separated peaks tend to become a multi-modal distribution with three or more separated peaks. When the volume ratio of this maximum peak exceeds 75%, the distribution is substantially close to a unimodal distribution, and even if such a volume-based particle size distribution is subjected to waveform separation, the number of separated peaks tends to be less than 3.
[0039] Furthermore, the silica-based particle group of the present invention has a volume ratio of the largest particle component of the separation peak detected when the volume-based particle size distribution is subjected to waveform separation, preferably 75% or less, more preferably 73% or less. When such a silica-based particle group is used as an abrasive, the surface roughness and waviness of the substrate during polishing are improved due to the small amount of large particle components. Here, in the present invention, the "largest particle component" means the particle component contained in the separation peak on the side of the largest particle diameter when the volume-based particle size distribution of the silica-based particle group is subjected to waveform separation.
[0040] <Aspect ratio> In the silica-based particle group of the present invention, the aspect ratio of the small particle component in the number-based particle size distribution obtained as a result of SEM image analysis is preferably in the range of 1.05 to 5.0, more preferably in the range of 1.05 to 3.0, even more preferably in the range of 1.05 to 2.0, and most preferably in the range of 1.05 to 1.5. The aspect ratio of the small particle component in the number-based particle size distribution obtained by SEM image analysis is measured and calculated by the following method. First, the total number of particles of the silica-based particle group is counted using a known scanning electron microscope (SEM) and a known image analysis system. In addition, the area of each particle is calculated, and the diameter of a circle having an area equal to the area is calculated, and this is taken as the particle size. The obtained particle diameters are then arranged in order of size, and the particles up to 1 / 3 of the total number of particles, counting from the smallest side, are designated as the small particle side component.The aspect ratio (the long axis / short axis ratio of the smallest circumscribing rectangle) is calculated for each particle in the small particle side component, and the simple average of these is designated as the "aspect ratio of the small particle side component." The aspect ratio of the small particle side component of the silica-based particle group of the present invention is usually smaller than the average aspect ratio of the silica-based particle group. When the aspect ratio of the small particle side component is less than 1.05, such particles are substantially equivalent to spherical particles, so the polishing rate is low, and the polishing rate of the silica-based particle group also tends to decrease. However, when a silica-based particle group with an aspect ratio of the small particle side component exceeding 1.05 is used as an abrasive, the small particle side component also shows a high polishing rate, so the polishing rate of the silica-based particle group can be made higher, defects are less likely to occur, and high surface accuracy tends to be obtained. In addition, when the aspect ratio of the small particle side component is larger than this range, the average aspect ratio of the entire distribution is also higher, so the polishing rate is high, but defects are more likely to occur, and the surface roughness and waviness also tend to deteriorate.
[0041] Here, as a method for producing particles with a high aspect ratio in which single particles are bonded, there are, for example, a method of increasing the aspect ratio by associating particles of several tens of nm using ionic strength adjustment or polymers, or a method of associating particles by adjusting ionic strength etc. at the same time as nucleation during particle preparation, and then growing the generated irregular seed particles to obtain particles with a high aspect ratio. However, in these methods, particles with a high aspect ratio are generated, and at the same time, particles that do not associate tend to remain, so that particles with a small particle size tend to be close to a sphere and have a small aspect ratio, and spherical particles have a low polishing rate, so the polishing rate of the particle group as a whole tends to be low. In contrast, the silica-based particle group containing the irregular silica-based particles of the present invention can obtain a high polishing rate because the small particle side component also contains irregular particles due to the densification effect of the crushing process.
[0042] <Coefficient of variation (CV value)> The coefficient of variation of the particle size of the volumetric particle size distribution of the silica-based particle group according to the present invention is preferably 30% or more, more preferably 50% or more. By setting the coefficient of variation within a predetermined range, the volumetric particle size distribution becomes broad, that is, the silica-based particle group has a wide particle size distribution, and exhibits more suitable polishing performance. In the present invention, the "coefficient of variation (CV value)" is the value obtained by dividing the standard deviation by the average value, expressed as a percentage, and indicates relative variation. The CV value in the present invention is determined from the volume-based particle size distribution using a disk centrifugal particle size distribution measuring device (manufactured by CPS Instruments).
[0043] <Smoothness S> In the silica-based particle group of the present invention, the smoothness S (S=S2 / S1), which is expressed by the ratio of the area (S2) of a circle equivalent to the average perimeter by image analysis to the average area (S1) by image analysis, is preferably in the range of 1.1 to 5.0, more preferably in the range of 1.3 to 4.0. When the S value is higher than 1.0, it indicates that the surface of the irregular silica-based particles contained in the silica-based particle group is not smooth but has a shape with fine irregularities. This is because the irregular seed particles are an aggregate of primary particles, and the surface of these seed particles also has fine protrusions, and the irregular silica-based particles obtained by particle growth of these seed particles have a shape in which the fine protrusions are maintained. Furthermore, when a silica-based particle group containing irregular silica-based particles having appropriate fine protrusions on the surface of the irregular silica-based particles is used as an abrasive, a high polishing rate can be obtained because the polishing pressure is concentrated on the protrusions. Note that, when the protrusions on the particle surface are excessive, the surface roughness and waviness of the substrate surface after polishing do not deteriorate, but the abrasive grains tend to be easily worn and the polishing rate tends to decrease.
[0044] Here, the measurement and calculation of the average area (S1) by image analysis and the area of a circle equivalent to the average perimeter (S2) by image analysis for the silica-based particle group will be described. These were measured and calculated by the following method. First, a known scanning electron microscope (SEM) was used to measure an arbitrary portion of the particle surface at a magnification of 3000 times, with a resolution of 1.1 × 10 per field of view. -3 mm 2 15 fields of view are photographed with an area of 100 mm. For all silica fine particles contained in each image photographed in each field of view, the area and perimeter of each particle are measured using a known image analysis system, and the average area (S1) (simple average value) and average perimeter (simple average value) are calculated from the measured area and perimeter data, and the area (S2) of a circle equivalent to the average perimeter (a circle with the same circumference as the average perimeter) is calculated from this average perimeter.
[0045] <q2 q1> In the silica-based particle group of the present invention, in its volume-based particle size distribution, the ratio Q (Q=Q2 / Q1, expressed as a percentage) of the volume (Q2) of particles with a diameter of 0.7 μm or more to the total volume (Q1) is preferably 5.0% or less, more preferably 4.5% or less. Since such silica-based particle group has a small ratio of coarse particles, defects such as scratches are less likely to occur during polishing, and the surface roughness of the polished substrate can be reduced.
[0046] The total volume (Q1) in the volume-based particle size distribution of the silica-based particle group of the present invention, the volume proportion of each component of the separated peak obtained by waveform separation thereof, the volume proportion of the largest particle component, and the volume of particles of 0.7 μm or more (Q2) can also be measured by the method using the disc centrifugal particle size distribution measurement device described above.
[0047] <Polishing abrasive dispersion liquid> The silica-based particle dispersion liquid (silica-based particle dispersion liquid containing the silica-based particle group of the present invention) in which the silica-based particle group of the present invention is dispersed in a dispersion solvent can be preferably used as an abrasive dispersion liquid for polishing (hereinafter also referred to as "polishing abrasive dispersion liquid of the present invention"). In particular, it can be preferably used for polishing magnetic disks. Furthermore, it can be preferably used as an abrasive dispersion liquid for polishing for planarizing a semiconductor substrate on which an SiO2 insulating film is formed. In addition, it can be preferably used as a polishing slurry by adding a chemical component to control the polishing performance.
[0048] The abrasive polishing dispersion of the present invention has excellent effects such as a high polishing rate when polishing magnetic disks, semiconductor substrates, etc., causing fewer scratches on the polishing surface during polishing, and leaving fewer abrasive particles on the substrate, thereby dramatically improving the efficiency of the polishing work.
[0049] The abrasive dispersion liquid for polishing of the present invention contains water and / or organic solvent as a dispersion solvent. As the dispersion solvent, it is preferable to use water such as pure water, ultrapure water, and ion-exchanged water. Furthermore, by adding one or more additives selected from the group consisting of polishing accelerators, surfactants, heterocyclic compounds, pH adjusters, pH buffers, and precipitation inhibitors to the abrasive dispersion liquid for polishing of the present invention as additives for controlling polishing performance, the abrasive dispersion liquid for polishing of the present invention can be more suitably used as a polishing slurry.
[0050] <Polishing accelerator> The polishing abrasive dispersion of the present invention can be used as polishing slurry by adding a conventionally known polishing accelerator as necessary, depending on the type of polishing material.Examples of such accelerators include hydrogen peroxide, peracetic acid, urea peroxide, and mixtures thereof.When using the polishing agent composition containing such a polishing accelerator as hydrogen peroxide, when the polishing material is metal, the polishing speed can be effectively improved.
[0051] Other examples of the polishing accelerator include inorganic acids such as sulfuric acid, nitric acid, phosphoric acid, oxalic acid, and hydrofluoric acid, organic acids such as acetic acid, and the sodium salts, potassium salts, ammonium salts, and amine salts of these acids, and mixtures thereof. In the case of a polishing composition containing these polishing accelerators, when polishing a polished material consisting of multiple components, the polishing rate of a specific component of the polished material can be accelerated, and a flat polished surface can be finally obtained.
[0052] When the abrasive grain dispersion liquid for polishing of the present invention contains a polishing accelerator, the content thereof is preferably 0.1 to 10 mass %, and more preferably 0.5 to 5 mass %.
[0053] <Surfactant and / or hydrophilic compound> In order to improve the dispersibility and stability of the polishing abrasive dispersion of the present invention, a cationic, anionic, nonionic, or amphoteric surfactant or hydrophilic compound can be added. Both the surfactant and the hydrophilic compound have the effect of reducing the contact angle with the polished surface and promoting uniform polishing. As the surfactant and / or hydrophilic compound, for example, those selected from the following group can be used.
[0054] Examples of anionic surfactants include carboxylates, sulfonates, sulfates, and phosphates. Examples of carboxylates include soaps, N-acylamino acid salts, polyoxyethylene or polyoxypropylene alkyl ether carboxylates, and acylated peptides. Examples of sulfonates include alkyl sulfonates, alkylbenzene and alkylnaphthalene sulfonates, naphthalene sulfonates, sulfosuccinates, α-olefin sulfonates, and N-acylsulfonates. Examples of sulfates include sulfated oils, alkyl sulfates, alkyl ether sulfates, polyoxyethylene or polyoxypropylene alkyl allyl ether sulfates, and alkylamide sulfates. Examples of phosphates include alkyl phosphates and polyoxyethylene or polyoxypropylene alkyl allyl ether phosphates.
[0055] Examples of cationic surfactants include aliphatic amine salts, aliphatic quaternary ammonium salts, benzalkonium chloride salts, benzethonium chloride, pyridinium salts, and imidazolinium salts; examples of amphoteric surfactants include carboxybetaine type, sulfobetaine type, aminocarboxylate salts, imidazolinium betaine, lecithin, and alkylamine oxide.
[0056] Examples of nonionic surfactants include ether type, ether ester type, ester type, and nitrogen-containing type, and examples of ether type include polyoxyethylene alkyl and alkylphenyl ether, alkylaryl formaldehyde condensed polyoxyethylene ether, polyoxyethylene polyoxypropylene block polymer, and polyoxyethylene polyoxypropylene alkyl ether, examples of ether ester type include polyoxyethylene ether of glycerin ester, polyoxyethylene ether of sorbitan ester, and polyoxyethylene ether of sorbitol ester, examples of ester type include polyethylene glycol fatty acid ester, glycerin ester, polyglycerin ester, sorbitan ester, propylene glycol ester, and sucrose ester, and examples of nitrogen-containing type include fatty acid alkanolamide, polyoxyethylene fatty acid amide, and polyoxyethylene alkylamide. Other examples include fluorine-based surfactants.
[0057] The surfactant is preferably an anionic surfactant or a nonionic surfactant, and the salt includes ammonium salts, potassium salts, sodium salts, etc., with ammonium salts and potassium salts being particularly preferred.
[0058] Further, other surfactants, hydrophilic compounds, etc. include esters such as glycerin esters, sorbitan esters, and alanine ethyl esters; ethers such as polyethylene glycol, polypropylene glycol, polytetramethylene glycol, polyethylene glycol alkyl ethers, polyethylene glycol alkenyl ethers, alkyl polyethylene glycols, alkyl polyethylene glycol alkyl ethers, alkyl polyethylene glycol alkenyl ethers, alkenyl polyethylene glycols, alkenyl polyethylene glycol alkyl ethers, alkenyl polyethylene glycol alkenyl ethers, polypropylene glycol alkyl ethers, polypropylene glycol alkenyl ethers, alkyl polypropylene glycols, alkyl polypropylene glycol alkyl ethers, alkyl polypropylene glycol alkenyl ethers, and alkenyl polypropylene glycols; polysaccharides such as alginic acid, pectinic acid, carboxymethylcellulose, curdlan, and pullulan; ammonium glycine salts and sodium glycine. amino acid salts such as polyaspartic acid, polyglutamic acid, polylysine, polymalic acid, polymethacrylic acid, ammonium polymethacrylic acid, sodium polymethacrylic acid, polyamic acid, polymaleic acid, polyitaconic acid, polyfumaric acid, poly(p-styrene carboxylic acid), polyacrylic acid, polyacrylamide, aminopolyacrylamide, ammonium polyacrylic acid, sodium polyacrylic acid, polyamic acid, ammonium polyamic acid, sodium polyamic acid, and polyglyoxylic acid; vinyl polymers such as polyvinyl alcohol, polyvinylpyrrolidone, and polyacrolein; sulfonic acids and salts thereof such as ammonium methyl taurate, sodium methyl taurate, sodium methyl sulfate, ethyl ammonium sulfate, butyl ammonium sulfate, sodium vinyl sulfonate, sodium 1-allyl sulfonate, sodium 2-allyl sulfonate, sodium methoxymethyl sulfonate, ammonium ethoxymethyl sulfonate, and sodium 3-ethoxypropyl sulfonate;Amides such as propionamide, acrylamide, methylurea, nicotinamide, succinamide, and sulfanilamide may be mentioned. Among these surfactants, it is preferable to use polyacrylic acid sodium salt or polyacrylic acid sodium salt. Among the polyacrylic acid sodium salts, polyacrylic acid sodium salts having a weight average molecular weight in the range of 20,000 to 140,000 and a ratio (ratio of the number) of carbon atoms directly bonded to carbonyl carbon atoms in the total carbon atoms contained in the polyacrylic acid sodium salt is particularly preferable. If the ratio (ratio of the number) of carbon atoms directly bonded to the carbonyl carbon atom is in the range of 50 to 60%, the silica-based particle dispersion containing the polyacrylic acid sodium salt can exhibit excellent redispersibility even if the silica-based particles are precipitated. The polyacrylic acid sodium salt may be a copolymer of acrylic acid sodium salt and ethylene unit.
[0059] When the substrate to be polished is a glass substrate or the like, any surfactant can be suitably used. However, when the substrate is a silicon substrate for a semiconductor integrated circuit or the like, and the influence of contamination by alkali metals, alkaline earth metals, halides, or the like must be avoided, it is preferable to use an acid or an ammonium salt-based surfactant.
[0060] When the polishing abrasive dispersion of the present invention contains a surfactant and / or a hydrophilic compound, the total content thereof is preferably 0.001 to 10 g, more preferably 0.01 to 5 g, and particularly preferably 0.1 to 3 g, per liter of the polishing abrasive dispersion.
[0061] In order to obtain a sufficient effect, the content of the surfactant and / or hydrophilic compound is preferably 0.001 g or more per liter of the polishing abrasive dispersion, and preferably 10 g or less in order to prevent a decrease in the polishing rate.
[0062] The surfactant or hydrophilic compound may be only one kind, or two or more kinds may be used, and different kinds may be used in combination.
[0063] <Heterocyclic compound> Regarding the abrasive grain dispersion liquid for polishing of the present invention, when the substrate to be polished contains a metal, a heterocyclic compound may be contained for the purpose of forming a passive layer or a dissolution inhibition layer on the metal to suppress the erosion of the substrate to be polished. Here, the "heterocyclic compound" is a compound having a heterocycle containing one or more heteroatoms. The heteroatom means an atom other than a carbon atom or a hydrogen atom. The heterocycle means a cyclic compound having at least one heteroatom. The heteroatom means only an atom that forms a constituent part of the ring system of the heterocycle, and does not mean an atom that is located outside the ring system, separated from the ring system by at least one non-conjugated single bond, or is a part of a further substituent of the ring system. Preferred examples of the heteroatom include, but are not limited to, a nitrogen atom, a sulfur atom, an oxygen atom, a selenium atom, a tellurium atom, a phosphorus atom, a silicon atom, and a boron atom. As examples of the heterocyclic compound, imidazole, benzotriazole, benzothiazole, tetrazole, etc. can be used. More specifically, 1,2,3,4-tetrazole, 5-amino-1,2,3,4-tetrazole, 5-methyl-1,2,3,4-tetrazole, 1,2,3-triazole, 4-amino-1,2,3-triazole, 4,5-diamino-1,2,3-triazole, 1,2,4-triazole, 3-amino-1,2,4-triazole, 3,5-diamino-1,2,4-triazole, etc. can be mentioned, but are not limited thereto.
[0064] Regarding the content when a heterocyclic compound is blended in the abrasive grain dispersion liquid for polishing of the present invention, it is preferably 0.001 to 1.0% by mass, more preferably 0.001 to 0.7% by mass, and even more preferably 0.002 to 0.4% by mass.
[0065] <pH adjuster> Acids, bases, and their salt compounds can be added as needed, for example, to enhance the effects of the above additives, to adjust the pH of the polishing composition.
[0066] When adjusting the pH of the abrasive grain dispersion liquid of the present invention to 7 or higher, an alkaline substance is used as the pH adjuster. Desirably, amines such as sodium hydroxide, aqueous ammonia, ammonium carbonate, ethylamine, methylamine, triethylamine, and tetramethylamine are used.
[0067] When adjusting the pH of the abrasive grain dispersion liquid of the present invention to less than 7, an acidic substance is used as the pH adjuster. For example, mineral acids such as hydrochloric acid and nitric acid, and hydroxy acids such as acetic acid, lactic acid, citric acid, malic acid, tartaric acid, and glyceric acid are used.
[0068] <pH buffer> In order to keep the pH value of the abrasive grain dispersion liquid of the present invention constant, a pH buffer may be used. As the pH buffer, for example, phosphates and borates such as ammonium dihydrogen phosphate, diammonium hydrogen phosphate, ammonium tetraborate tetrahydrate, or organic acid salts can be used.
[0069] <Sedimentation inhibitor> The polishing abrasive dispersion of the present invention may contain a sedimentation inhibitor for the purpose of suppressing sedimentation and, if sedimentation does occur, making the abrasive dispersion easy to disperse. The settling inhibitor is not particularly limited, and examples thereof include polycarboxylic acid surfactants, anionic polymer surfactants, cationic surfactants, sodium polyacrylate, carboxylic acid copolymer sodium salts, carboxylic acid copolymer ammonium salts, ammonium polyacrylate, polyacrylic acid, sulfonic acid copolymer sodium salts, fatty acid salts, α-sulfofatty acid ester salts, alkylbenzenesulfonates, alkyl sulfates, alkyl ether sulfate esters, alkyl sulfate triethanolamine, fatty acid diethanolamides, polyoxyethylene alkyl ethers, polyoxyethylene alkylphenyl ethers, alkyl trimethylammonium salts, dialkyldimethylammonium chlorides, alkylpyridinium chlorides, alkylcarboxybetaines, styrene-maleic anhydride copolymers, formalin-bound naphthalene sulfonates, carboxymethylcellulose, olefin-maleic anhydride copolymers, sodium alginate, polyvinyl alcohol, polyalkylene polyamines, polyacrylamides, polyoxypropylene-polyoxyethylene blocks, polymer starches, polyethyleneimines, aminoalkyl acrylate copolymers, polyvinyl imidazoline, and satokine. In addition, the content of the settling inhibitor in the polishing abrasive dispersion of the present invention is preferably 0.001-10g, more preferably 0.01-5g, and particularly preferably 0.1-3g in total in 1L of the polishing abrasive dispersion. In order to obtain sufficient effect, the content is preferably 0.001g or more in 1L of the polishing abrasive dispersion, and is preferably 10g or less in order to prevent the polishing speed from decreasing.
[0070] Examples of the dispersion solvent for the abrasive grain dispersion of the present invention include alcohols such as methanol, ethanol, isopropanol, n-butanol, and methyl isocarbinol; ketones such as acetone, 2-butanone, ethyl amyl ketone, diacetone alcohol, isophorone, and cyclohexanone; amides such as N,N-dimethylformamide and N,N-dimethylacetamide; ethers such as diethyl ether, isopropyl ether, tetrahydrofuran, 1,4-dioxane, and 3,4-dihydro-2H-pyran; glycol ethers such as 2-methoxyethanol, 2-ethoxyethanol, 2-butoxyethanol, and ethylene glycol dimethyl ether; Organic solvents that can be used include glycol ether acetates such as 2-methoxyethyl acetate, 2-ethoxyethyl acetate, and 2-butoxyethyl acetate; esters such as methyl acetate, ethyl acetate, isobutyl acetate, amyl acetate, ethyl lactate, and ethylene carbonate; aromatic hydrocarbons such as benzene, toluene, and xylene; aliphatic hydrocarbons such as hexane, heptane, isooctane, and cyclohexane; halogenated hydrocarbons such as methylene chloride, 1,2-dichloroethane, dichloropropane, and chlorobenzene; sulfoxides such as dimethyl sulfoxide; and pyrrolidones such as N-methyl-2-pyrrolidone and N-octyl-2-pyrrolidone. These may be mixed with water.
[0071] The solid content of the polishing abrasive dispersion of the present invention is preferably in the range of 0.3 to 50 mass %. If the solid content is too low, the polishing rate may decrease. Conversely, if the solid content is too high, the polishing rate is rarely improved, which may be uneconomical.
[0072] <Method of manufacturing a silica-based particle group consisting of irregularly shaped silica-based particles and non-irregularly shaped silica-based particles> Next, a method for producing the silica-based particle group consisting of irregularly shaped silica-based particles and non-irregularly shaped silica-based particles of the present invention will be specifically described. This is a silica-based gel. (Specific surface area 50~200m 2 / g) The mixture is wet-disintegrated under alkaline conditions to produce particles made of highly irregular silica gel. (Weight average particle diameter 60~142nm) a step of adding a silicic acid liquid under alkaline conditions to the solution containing the particles made of the highly irregular silica-based gel and heating the solution, and growing the particles while maintaining a high degree of irregularity while filling spaces between the primary particles of the particles made of the highly irregular silica-based gel by a reaction with the silicic acid contained in the silicic acid liquid to form irregular silica-based particles. (Specific surface area 136m 2 / g or less [However, 30m 2 / g or less], weight average particle size 60 to 400 nm) and a step c of concentrating and recovering the silica-based particle group including the grown irregular shaped silica-based particles.
[0073] [Step a] This process uses silica-based gel as the starting material. As long as the silica-based gel is a silica-based gel, it can be not only silica gel but also composite gels such as silica-alumina gel, silica-titania gel, and silica-zirconia gel. The gel can be in the form of a hydrogel, xerogel, or organogel. This process involves wet-disintegrating such silica-based gel under alkaline conditions to produce a solution containing particles made of highly irregular silica-based gel. By crushing the silica-based gel and using it as seed particles, the seed particles become silica gel with a high degree of irregularity, and the seed particles are rarely spherical, resulting in highly irregular particles. This tendency is more pronounced when a silica-based gel raw material with a small specific surface area and large primary particle size is used for crushing, while the irregularity tends to be low when a silica-based gel raw material with a large specific surface area and small primary particle size is used for crushing. Furthermore, the irregularity tends to be low when the seed size is reduced. Then, in the subsequent step b, the added silicic acid liquid is deposited while penetrating into the silica surface and inside of the particles (seed particles) made of highly irregular silica-based gel, and reacts preferentially with the pores between the primary particles to fill the pores, while silica is deposited on the outer surface of the particles, promoting particle growth (in the following explanation, this is called build-up). Due to this build-up, the convex parts on the outer surface of the particles contribute more to increasing the outer diameter, while the concave parts contribute less to the outer shape, so that the strength of the grown particles is increased and the deformation of the irregular shape of the particles is suppressed, and irregular silica-based particles with a large particle diameter and high degree of irregularity can be produced.
[0074] In addition, the present invention uses a silica-based gel with a small specific surface area and a large primary diameter as a manufacturing raw material, so its strength is weak. Therefore, even if the silica-based gel is crushed so that the weight-average particle diameter is several hundred nm, fine particles of about several tens of nm are also generated at the same time during crushing. Therefore, when the silica-based gel is used as a manufacturing raw material, the particles obtained by crushing it range from small particles to large particles. Therefore, the silica-based particle group of the present invention has a large weight-average particle diameter and also contains fine particles, so the skewness and kurtosis are high.
[0075] The silica-based gel used as the raw material is preferably a gel that is easily disintegrated, such as a wet hydrogel obtained by washing a gel produced by the water glass method, or a dried silica gel, xerogel, white carbon, precipitated silica, gel silica, or gel produced by the alkoxide method, which are obtained by drying the hydrogel. The gel produced by the alkoxide method has a small number of hydroxyl groups that undergo dehydration condensation, so the dried powder is soft and can be used as a dry powder with good productivity. The particle size distribution of the particles made of the irregular silica-based gel obtained by disintegrating the silica-based gel is preferably controlled within a certain range, and large gel lumps that are difficult to disintegrate are not preferable because they take a long time to disintegrate and tend to have a wide particle size distribution.
[0076] The silica-based gel used in the present invention has a specific surface area of 50 to 200 m 2 / g range It is. Specific surface area is 50m 2 If the specific surface area is less than 1 / g, the pores between the primary particles of the silica-based gel are small, so when silicic acid liquid is added to a solution containing particles made of irregularly shaped silica-based gel obtained by crushing, the amount of silicic acid that penetrates into the pores between the primary particles of the particles made of irregularly shaped silica-based gel is small, and it becomes difficult to fill these pores by reaction with silicic acid, and the added silicic acid liquid is consumed to make the particles grow round, which tends to make it difficult to maintain the irregular shape. 200 m 2 If it is greater than 1 / g, the particle strength is too high and crushing becomes difficult, and long-term crushing is required to reduce coarse particles or to adjust the particle size to a specified size, which tends to result in a low irregularity. Moreover, the size (particle diameter) of the silica-based gel is preferably in the range of 1 μm to 10 mm.
[0077] The silica-based gel is then wet-disintegrated under alkaline conditions to form particles of highly irregular silica-based gel. 200 m 2 By simultaneously deforming and crushing a relatively soft silica-based gel of about 1 / g under a strong shear such as with a bead mill, particles made of irregular silica-based gel can be prepared into particles with a high degree of irregularity. For example, a sand mill grinder or a bead mill containing glass media can be used for crushing. It is preferable to perform crushing for as short a time as possible.
[0078] Normally, when powder is pulverized using a bead mill, the particle size of the powder decreases in proportion to the pulverization time. However, silica gel, which has a small specific surface area and a large primary diameter, can reduce its weight-average particle size to 60 in a short period of time. ~142 The particles made of highly irregular silica-based gel are crushed into particles of about nm, and while maintaining the specific surface area before crushing, the particles have a coarse structure containing a large number of necks between primary particles. Therefore, even if these particles are used as a polishing material as they are, they are prone to crumbling due to insufficient strength, and only a very low polishing rate can be obtained. Therefore, in the present invention, in the subsequent step b, highly irregular silica-based gel is crushed into particles of about 1 nm. S The strength of the particles is increased by adding a silicic acid liquid to a solution containing particles made of silica-based gel, and building up and filling the pores between the primary particles inside the particles made of the irregular silica-based gel with the silicic acid liquid. Here, the silicic acid liquid used for the build-up may be derived from alkoxide, sodium silicate, or amine silicate. In addition, as long as it can fill the gaps between the primary particles, it is not limited to silicic acid, and may be a silicate such as an alkali salt or an alkaline earth salt of silicic acid.
[0079] In step a, the silica-based gel is wet-disintegrated under alkaline conditions, that is, alkaline conditions, and the alkalinity is preferably in the range of pH 8.0 to 11.5. As the pH decreases from the alkaline region, the negative potential gradually decreases, and the particles become unstable in the neutral to acidic regions, so that the particles generated by disintegration cannot exist stably and tend to aggregate immediately. Furthermore, if the pH exceeds 11.5, dissolution of silica is promoted, so that the particles also tend to aggregate. The pH during the wet disintegration is preferably recommended to be in the range of 8.5 to 11.0. The method for adjusting the pH is not particularly limited, but may be, for example, by adding sodium hydroxide.
[0080] The weight average particle diameter of the particles made of the highly irregular silica-based gel obtained by the wet disintegration is 60 to 142 nm range do. If the weight average particle diameter of the particles made of highly irregular silica-based gel is smaller than 60 nm, it may be difficult to make the particles have a particle diameter suitable for abrasives even if the particles are grown by adding silicic acid liquid thereafter. 142 If the particle size is larger than nm, it may exceed the particle size suitable for the abrasive, which is not preferable. Such coarse particles exceeding the particle size suitable for the abrasive may cause scratches. Although coarse particles and large particles tend to be preferentially crushed by crushing, centrifugation may be performed for the purpose of removing coarse particles remaining in the highly irregular silica-based gel. The weight average particle size of the particles made of the highly irregular silica-based gel is preferably 80 to 100 μm. 142 nm range is recommended.
[0081] Here, the weight average particle diameter of the particles made of highly irregular silica-based gel means a value obtained by measuring in the same manner as the weight average particle diameter (D1) of the silica-based particles described above.
[0082] This crushing can be carried out in multiple stages using media of different materials and sizes. For example, if silica gel is crushed using large zirconia media, the first stage crushing can be carried out at high speed in a short time due to strong shearing force. If the second stage crushing is then carried out using glass media smaller than the first stage, crushing proceeds with moderate shearing force, and the desired particle size can be adjusted. At this time, since the weak parts between the primary particles are destroyed, there is a tendency for the shape to become irregular at the same time as the particles are refined. In addition, since the wet crushing is carried out under alkaline conditions, part of the particles made of highly irregular silica gel dissolves and can preferentially fill the neck parts between the primary particles, so excessive refinement does not proceed during crushing.
[0083] [Step b] This process is a build-up process in which a silicic acid liquid is added to a solution containing particles made of highly irregular silica-based gel under alkaline conditions and heated, and the pores between the primary particles of the particles made of highly irregular silica-based gel are filled by reaction with silicic acid, and the particles grow while maintaining their irregular shape. The SiO2 concentration of the solution containing the particles made of highly irregular silica-based gel is preferably in the range of 1 to 10 mass%. If the SiO2 concentration of the solution containing particles made of highly irregular silica-based gel is less than 1 mass%, the efficiency of producing irregular silica-based particles tends to decrease. In addition, if the SiO2 concentration is more than 10 mass%, fine silica nuclei are generated, the irregular shape cannot be maintained, and the particle growth of the irregular silica-based particles tends to be uneven. Incidentally, this step b may be performed by a method of adding a silicic acid liquid while subjecting particles made of highly irregular silica gel to hydrothermal treatment. In this method, the particles are supersaturated with the added silicic acid liquid, and some of the particles are dissolved, while silica is precipitated and the particles grow. However, since the deposition rate of the necks between the primary particles is faster than the dissolution rate, the pores between the primary particles are preferentially filled.
[0084] The heating temperature is preferably in the range of 60° C. to 170° C. Because if it is lower than 60° C., the growth of the particles made of the highly irregular silica-based gel tends to be slow, and if it is higher than 170° C., the obtained irregular silica-based particles tend to be spherical. The heating temperature is more preferably in the range of 60° C. to 100° C.
[0085] Furthermore, the pH range of 9 to 12.5 is preferable when adding silicic acid liquid to a solution containing particles made of highly irregular silica-based gel. If the pH is less than 9, the solubility of silica is low, so the degree of supersaturation is significantly high, and the added silicic acid liquid is not consumed for particle growth and is easily generated as fine particles. In addition, the negative potential is also low, so the particles are easily aggregated. Furthermore, the dissociation of hydroxyl groups is insufficient, so the reactivity with primary particles is reduced, and the reinforcement of the neck portion is insufficient. Also, if the pH is higher than 12.5, the dissolution of silica may be promoted.
[0086] The pH of the solution containing the particles made of highly irregular silica-based gel is adjusted as necessary to be within the above-mentioned range. The adjustment means is not particularly limited, but the adjustment is usually performed by adding an alkaline substance. Examples of such alkaline substances include sodium hydroxide and water glass. The pH of the solution containing the particles made of highly irregular silica-based gel is preferably in the range of 9.5 to 12.0 when adding a silicic acid liquid.
[0087] The amount of silicic acid liquid added is preferably in the range where the SiO2 molar concentration of the silicic acid liquid is 0.5 to 20 times the SiO2 molar concentration of the solution containing particles made of the highly irregular silica-based gel. If the amount of silicic acid liquid added is less than the above range, the strength between primary particles cannot be sufficiently increased, so the strength of the particles tends to decrease. In addition, when silicic acid liquid or the like is added to grow particles, the irregularity and aspect ratio usually decrease, but if the amount of silicic acid liquid added is more than the above range, the irregularity of the particles decreases significantly and the desired irregularity tends to be difficult to maintain. Furthermore, since small particle components grow preferentially compared to large particle components during particle growth, if the amount of silicic acid liquid added is more than the above range, it tends to be difficult to obtain small particle side components with the desired aspect ratio. It is also preferable to add the silicic acid solution continuously or intermittently.
[0088] The silicic acid liquid penetrates into the inside of the particles through the pores between the primary particles of the particles made of highly irregular silica-based gel, and is deposited on the neck part of the particle, thereby reducing the specific surface area and increasing the strength of the particle. In this step (b), the specific surface area of the particles made of highly irregular silica-based gel is 136 m 2 / g or less (However, 30m 2 / g or less) , more preferably a specific surface area of 9m 2 / g~136m 2 / g (However, 30m 2 / g or less) It is desirable to set the specific surface area of the particles made of irregular silica gel to within 136 m 2 If it is greater than 1 / g, the size of the obtained irregularly shaped silica particles will be too small, and the removal rate will tend to be slow. The specific surface area of the particles made of the irregular silica gel is measured by the BET method as described in the "Measurement of Specific Surface Area" section of the Examples below.
[0089] The silicic acid liquid dripped from the outside falls uniformly from the liquid phase onto the surface of the irregular silica-based gel, and bonds to the outer surface of the particles made of the irregular silica-based gel, growing the particle shape, so that irregular silica-based particles with a large particle size can be obtained while maintaining the irregular shape. The particle size of the irregular silica-based particles after particle growth is in the range of 60 to 400 nm, which is the weight average particle size. do. The weight average particle size of the irregular shaped silica-based particles herein means a value obtained by measurement in the same manner as the weight average particle size (D1) of the silica-based particles described above.
[0090] [Process c] This step is a step of concentrating and recovering the silica-based particle group including the grown irregular silica-based particles. Specifically, for example, the solution containing the grown irregular silica-based particles is cooled to room temperature to about 40°C, concentrated using an ultrafiltration membrane, etc., and further concentrated using an evaporator, etc., to recover the remaining silica-based particle group. In addition, centrifugation may be performed to remove coarse particles. Concentration using an ultrafiltration membrane is preferable from the viewpoint of preventing the formation of coarse aggregates due to drying. EXAMPLES
[0091] Examples of the present invention will be described below together with comparative examples. In the examples and comparative examples, the measurement of the specific surface area of the silica-based particle group, the calculation of the specific surface area converted particle diameter (D2), the measurement of the weight average particle diameter (D1), the measurement and calculation of the projected area equivalent particle diameter (D3), the calculation of the skewness and kurtosis in the volumetric particle diameter distribution, the waveform separation of the volumetric particle diameter distribution, the measurement of the volume in the volumetric particle diameter distribution, the calculation of the aspect ratio of the small particle component, the calculation of the coefficient of variation, the measurement and calculation of the average area (S1) and the area of the circle equivalent to the average perimeter (S2), the measurement and calculation of the average pore diameter of the pores inside the core of the irregular silica-based particles, the measurement and calculation of the average thickness of the coating silica layer of the irregular silica-based particles, and the polishing test were performed as follows.
[0092] [Measurement of specific surface area] Example 1 2 For the comparative examples 3 to 5, the specific surface area was measured and calculated by the BET method. Specifically, the pH of 50 ml of the silica sol to be measured was adjusted to 3.5 with nitric acid, 40 ml of 1-propanol was added thereto, and the sample was dried at 110°C for 16 hours. The sample was then pulverized in a mortar and fired at 500°C for 1 hour in a muffle furnace to obtain a measurement sample. Then, the specific surface area was calculated from the amount of nitrogen adsorption by the nitrogen adsorption method (BET method) using a specific surface area measuring device (manufactured by Yuasa Ionics, model number Multisorb 12) using the BET one-point method. In the specific surface area measuring device, 0.5 g of the calcined sample was placed in a measurement cell, and degassed for 20 minutes at 300°C in a 30v% nitrogen / 70v% helium mixed gas flow, and then the sample was kept at liquid nitrogen temperature in the mixed gas flow to allow equilibrium adsorption of nitrogen onto the sample. Next, the sample temperature was gradually raised to room temperature while the mixed gas was being passed, and the amount of nitrogen desorbed during this period was detected, and the specific surface area of the silica fine particles in the sample was calculated using a calibration curve created in advance. For Comparative Examples 1, 2 and 6 in which the silica gel was crushed (no build-up was performed), the specific surface area was measured and calculated by the titration method. Specifically, a sample equivalent to 1.5 g of SiO2 was collected in a beaker, then transferred to a thermostatic reaction tank (25°C), and pure water was added to make the liquid volume 90 ml (the following operations are performed in a thermostatic reaction tank maintained at 25°C), and then a 0.1 mol / L hydrochloric acid aqueous solution was added to adjust the pH to 3.6. Furthermore, 30 g of sodium chloride was added, diluted to 150 ml with pure water, and stirred for 10 minutes. Then, a pH electrode was set, and a 0.1 mol / L sodium hydroxide solution was added dropwise while stirring to adjust the pH to 4.0. Furthermore, the sample adjusted to pH 4.0 was titrated with 0.1 mol / L sodium hydroxide solution, and the titration amount and pH value in the range of pH 8.7 to 9.3 were recorded at four or more points, and a calibration curve was created with the titration amount of 0.1 mol / L sodium hydroxide solution as X and the pH value at that time as Y. Then, the consumption of 0.1 mol / L sodium hydroxide solution required to change the pH from 4.0 to 9.0 per 1.5 g of SiO2 was calculated from a specified formula, and the specific surface area was calculated using this according to a specified formula.
[0093] [Calculation of specific surface area converted particle diameter (D2)] Using the specific surface area (SA) measured by the above method and the particle density (ρ=2.2), the specific surface area converted particle diameter (D2) was calculated from the formula D2=6000 / (SA×ρ).
[0094] [Measurement of weight average particle size (D1)] The silica-based particle dispersion was diluted with 0.05% by mass sodium dodecyl sulfate aqueous solution to a solid concentration of 2% by mass, and 0.1 ml of the solution was injected with a syringe into a disk centrifugal particle size distribution measuring device (model number: DC24000UHR, manufactured by CPS Instruments) and the weight average particle size (D1) was measured at 18,000 rpm in a density gradient solution of 8 to 24% by mass sucrose. The silica-based gel disintegrated product (particles made of highly irregular silica-based gel) was also measured in the same manner.
[0095] [Measurement and calculation of projected area equivalent particle diameter (D3)] The projected area equivalent particle diameter (D3) of the silica-based particle group was measured and calculated by image analysis. Specifically, a scanning electron microscope (SEM) was used to measure an arbitrary point on the surface of a silica-based particle at a magnification of 3000 times, with a resolution of 1.1 × 10 per field of view. -3 mm 2 The area of 15 fields of view was photographed. Then, for all silica fine particles contained in each image photographed in each field of view, the projected area of each particle was measured by image analysis using an image analysis system, the particle diameter (circle diameter) of the circular particle corresponding to each measured area was calculated, and the number average of these was taken as the particle diameter equivalent to the projected area (D3).
[0096] [Calculation of kurtosis and skewness in volume-based particle size distribution] The volumetric particle size distribution was also measured by the method using the disk centrifugal particle size distribution measuring device described above.Then, the volumetric particle size distribution data obtained was used to calculate the kurtosis and skewness using JMP Ver.13.2 manufactured by SAS Institute Japan.In addition, when the frequency of a certain particle size in the volumetric particle size distribution was a negative value, the frequency was calculated as zero.
[0097] [Waveform separation of volumetric particle size distribution] The volume-based particle size distribution measurement data described above was analyzed using the peak analyzer of the graph creation and data analysis software Origin (manufactured by OriginLab Corporation). First, the baseline was set to 0, the peak type was set to Gaussian, and the maximum point of the particle size distribution was selected as the peak position, and peak fitting was performed without weighting. It was confirmed that the calculated peak did not deviate from the following conditions 1 and 2. If it did deviate, the peak position was shifted to an arbitrary position within the distribution range until the following conditions 1 and 2 were satisfied, and the peak fitting was repeated. Then, if the corrected R-squared value was 0.99 or less, a peak was added to an arbitrary position within the distribution range, and the peak fitting was repeated until the corrected R-squared value was 0.99 or more. The number of separated peaks at this time was taken as the number of peaks. Condition 1: Each calculated peak does not take a value greater than the original distribution. Condition 2: None of the calculated peaks take negative values.
[0098] [Volume measurement in volume-based particle size distribution] The total volume (Q1) in the volumetric particle size distribution of the silica-based particle group, the volume fraction of each component of the separated peak obtained by waveform separation of this, the volume fraction of the largest particle component, and the volume of particles of 0.7 μm or more (Q2) were measured using the above-mentioned disk centrifugal particle size distribution measuring device.
[0099] [Calculation of aspect ratio of small particle components] The aspect ratio of the small particle component was determined by counting the total number of particles in the silica-based particle group using a scanning electron microscope (SEM) and an image analysis system, calculating the area of each particle, and determining the diameter of a circle with an area equal to that area, which was taken as the particle diameter.The particle diameters obtained were then arranged in order of size, and the particles up to 1 / 3 of the total number of particles counted from the smallest side were taken as the small particle component, and the average of their aspect ratios (ratio of the long axis / short axis of the smallest circumscribing rectangle) was taken as the "aspect ratio of the small particle component."
[0100] [Calculation of coefficient of variation] The coefficient of variation of the volume ratio of each component of the separated peak obtained as a result of waveform separation of the volumetric particle size distribution of the silica-based particle group, and the coefficient of variation of the particle size of the volumetric particle size distribution were calculated by calculating the respective standard deviations and average values from the above-mentioned volumetric particle size distribution measurement data, dividing this standard deviation by the above-mentioned average value, and expressing the result as a percentage.
[0101] [Measurement and calculation of the average area (S1) and the area of a circle equivalent to the average circumference (S2)] The average area (S1) and the area of the circle equivalent to the average circumference (S2) of the silica-based particle group were measured by image analysis. Specifically, a scanning electron microscope (SEM) was used to measure an arbitrary point on the surface of a silica-based particle at a magnification of 3000 times, with a resolution of 1.1 × 10 per field of view. -3 mm 2 The area of 15 fields of view was photographed. The area and perimeter of all silica microparticles contained in each image photographed in each field of view were measured by image analysis using an image analysis system, and the average area (S1) and average perimeter (simple average value) were calculated from the measured area and perimeter data. Furthermore, the area (S2) of a circle equivalent to the average perimeter (a circle with the same circumference as the average perimeter) was calculated from the average perimeter.
[0102] [Measurement and calculation of the average pore size inside the core of irregular silica particles and the average thickness of the coating silica layer] The average pore size of the pores inside the core of the irregular silica-based particles and the average thickness of the coating silica layer were measured and calculated as follows. First, the irregular silica-based particles were observed at 200,000 times magnification using a transmission electron microscope (TEM), and the maximum diameter of the particle was taken as the major axis. A point was determined on the major axis that divided the major axis into two equal parts, and two points were determined where a straight line perpendicular to the major axis intersected with the outer edge of the particle, and the distance between these two points was taken as the minor axis. Then, the thicknesses of the coating silica layer on both sides of the major axis and the minor axis were determined, and these were simply averaged to obtain the average thickness of the coating silica layer of one particle. Similarly, the thicknesses of the silica layer were determined for 20 random particles, and the simple average of these was taken to obtain the average thickness of the coating silica layer of the irregular silica-based particles. In addition, the pore sizes on the major and minor axes were determined, and the average was taken as the average pore size for one particle. Similarly, the pore sizes of 20 randomly selected particles were determined, and the simple average of these was taken as the average pore size for the irregularly shaped silica particles.
[0103] [Method for measuring the size of silica gel] The size of the silica-based gel was measured using HORIBA's LA-950 under the following measurement conditions. The LA-950V2 version was 7.02, the algorithm option was standard calculation, the refractive index of the solid was 1.450, the refractive index of the solvent (pure water) was 1.333, the number of repetitions was 15, the circulation speed of the sample input bath was 5, and the stirring speed was 2. Measurements were performed using a measurement sequence with these settings set in advance. The measurement sample was then input as is into the sample input port of the device using a dropper. The sample was input so that the transmittance (R) value was 90%. After the transmittance (R) value stabilized, ultrasonic waves were irradiated for 5 minutes and the particle size was measured.
[0104] [Method for measuring the proportion of irregularly shaped silica-based particles contained in a silica-based particle dispersion liquid containing a silica-based particle group consisting of irregularly shaped silica-based particles and non-irregularly shaped silica-based particles] The silica-based particle dispersion was photographed at a magnification of 250,000 times (or 500,000 times) using an electron microscope (Hitachi, model number "S-5500"), and the aspect ratio (ratio of major axis / minor axis of the smallest circumscribed rectangle) of each of 100 random particles was determined in the photographic projection image. Particles with an aspect ratio of 1.1 or more were irregular silica-based particles. The proportion of the irregular silica-based particles was determined from the number of particles with an aspect ratio of 1.1 or more and the number of particles measured (100 particles). The results are shown in Table 1.
[0105] [Polishing test] Substrate to be polished The substrate to be polished was a nickel-plated aluminum substrate for hard disks (nickel-plated substrate manufactured by Toyo Kohan Co., Ltd.) This substrate was a doughnut-shaped substrate (outer diameter 95 mmφ, inner diameter 25 mmφ, thickness 1.27 mm). Abrasion test 344 g of a 9% by mass silica-based particle dispersion was prepared, to which 5.65 g of a 31% by mass hydrogen peroxide solution was added, and then the pH was adjusted to 1.5 with 10% by mass nitric acid to prepare a polishing slurry. The above substrate to be polished was set in a polishing apparatus (NF300 manufactured by Nanofactor), and a polishing pad (Bellatrix NO178 manufactured by FILWEL) was used to polish the substrate by 1 μm while supplying polishing slurry at a rate of 40 g / min at a substrate load of 0.05 MPa, a platen rotation speed of 50 rpm, and a head rotation speed of 50 rpm. polishing speed The polishing rate was calculated from the difference in weight of the polished substrate before and after polishing and the polishing time. Stable polishing speed Polishing was repeated five times under the above conditions, and the coefficient of variation (CV value) of the polishing rate was calculated. Substrate smoothness The polished substrate obtained from the polishing test was observed using an ultrafine defect visualization macro device (manufactured by VISION PSYTEC, product name: Micro-Max VMX-3100) with the white light of MME-250W adjusted to 10% and LA-180Me adjusted to 0%. In this observation, if there are defects such as scratches on the substrate surface, the white light is diffusely reflected and the defective parts are observed as white. On the other hand, the white light is specularly reflected in parts without defects and the whole surface is observed as black. Observations were made in this way and the area of defects (area of the substrate observed as white) caused by scratches (linear marks) on the substrate surface was evaluated according to the following criteria. Defect area evaluation Less than 3% "Very little" 3% or more, less than 20% "Low" 20% or more, but less than 40% "Many" Over 40% "Very common" undulation The measurement was made at an arbitrary point dividing the outer and inner edges of a polished doughnut-shaped aluminum substrate into two equal parts, and then the measurement was made at a point dividing the two equal parts on the opposite side to the measurement point, and the average of these values was taken as the waviness measurement value. The measurement conditions were as follows: Equipment:ZygoNewView7200 Lens: 2.5x Zoom ratio: 1.0 Filter: 50~500μm Measurement area: 3.75mm x 2.81mm
[0106] [Example 1] <Highly irregular silica gel particle dispersion (1)> Silica powder (dried silica gel) ("TOKUSIL928" manufactured by Oriental Silicas Corporation [SiO2 concentration 88.9 mass%, average particle size 14 μm, specific surface area 130 m]) was placed in a 2 L glass beaker. 2 28 g of the mixture (1.0 g / g) and 472 g of pure water were added, and a 4.8% by mass aqueous solution of sodium hydroxide was added to adjust the pH to 10.0. 1135 g of glass media with a diameter of 0.25 mm was added thereto, and the mixture was crushed in a sand mill until the weight average particle diameter became 135 nm, to obtain a dispersion liquid (1) of highly irregular silica-based gel microparticles with an SiO2 concentration of 4.0% by mass.
[0107] Preparation of silica-based particle group consisting of irregularly shaped silica-based particles and non-irregularly shaped silica-based particles Ion-exchanged water was added to the obtained highly irregular silica-based gel microparticle dispersion (1) to obtain 2716 g of a solution with a SiO2 concentration of 2.76 mass%. Next, a 4.8 mass% aqueous sodium hydroxide solution and ion-exchanged water were added to adjust the solution to a pH of 10.7 and a SiO2 concentration of 2.5 mass%. The temperature was then raised to 98°C and maintained at 98°C for 30 minutes. Next, while maintaining the temperature at 98°C, 5573.1 g of 4.6 mass% acidic silicic acid solution was added over 20 hours, and stirring was continued for another hour while maintaining the temperature at 98°C. After cooling this mixture to room temperature, it was concentrated to a SiO2 concentration of 12% by mass using an ultrafiltration membrane (SIP-1013 manufactured by Asahi Kasei Corporation). It was further concentrated to 30% by mass using a rotary evaporator to obtain a silica-based particle group consisting of irregular silica-based particles and non-irregular silica-based particles. The weight average particle diameter of the obtained silica-based particle group was 111 nm.
[0108] [Example 2] <Highly irregular silica gel particle dispersion (2)> To 1194.7 g of 0.77% by mass potassium chloride aqueous solution, 600 g of sodium silicate (SiO2 concentration 24% by mass) and 70.3 g of acidic silicic acid solution with SiO2 concentration of 4.5% by mass were added while stirring. The mixture was then heated to 98°C, and after the temperature increase, it was held at 98°C for 40 minutes. While maintaining the temperature at 98°C, 4792.4 g of acidic silicic acid solution was added, and after the addition was completed, it was held at 98°C for 1 hour. The mixture was allowed to cool to room temperature to obtain silica gel. The silica gel was dried overnight at 110°C to obtain silica powder (dried silica gel) with an average particle size of 60 μm and a specific surface area of 200 m 2 / g, and the SiO2 content (concentration) was 90.5 mass%. 28 g of this silica powder and 472 g of pure water were added to a 2 L glass beaker, and a 4.8 mass% aqueous solution of sodium hydroxide was added to adjust the pH to 10.0. 2390 g of 1.0 mmφ zirconia media was added to this, and the mixture was crushed in a sand mill until the weight average particle diameter became 142 nm, to obtain a highly irregular silica gel microparticle dispersion (2) with an SiO2 concentration of 4.0 mass%.
[0109] Preparation of silica-based particle group consisting of irregularly shaped silica-based particles and non-irregularly shaped silica-based particles Ion-exchanged water was added to the obtained highly irregular silica gel microparticle dispersion (2) to obtain 2400g of a solution with a SiO2 concentration of 2.76% by mass. Next, a 4.8% by mass aqueous solution of sodium hydroxide and ion-exchanged water were added to adjust the solution to a pH of 10.7 and a SiO2 concentration of 2.5% by mass. The temperature was then raised to 98°C and maintained at 98°C for 30 minutes. Next, while maintaining the temperature at 98°C, 8208g of a 4.6% by mass acidic silicic acid solution was added over 20 hours, and stirring was continued for another hour while maintaining the temperature at 98°C. After cooling this mixture to room temperature, it was concentrated to a SiO2 concentration of 12% by mass using an ultrafiltration membrane (SIP-1013 manufactured by Asahi Kasei Corporation). It was further concentrated to 30% by mass using a rotary evaporator to obtain a silica-based particle group consisting of irregular silica-based particles and non-irregular silica-based particles. The weight average particle diameter of the obtained silica-based particle group was 230 nm.
[0115] [Comparative Example 1] "Cataloid SI-80P" (manufactured by JGC Catalysts and Chemicals, silica concentration 40% by mass), which is a dispersion liquid in which silica fine particles are dispersed, was used as Comparative Example 1.
[0116] [Comparative Example 2] "SS-160" (manufactured by JGC Catalysts and Chemicals, silica concentration 20% by mass), which is a dispersion liquid in which silica fine particles are dispersed, was used as Comparative Example 2.
[0117] [Comparative Example 3] "SS-300" (manufactured by JGC Catalysts and Chemicals, silica concentration 20% by mass), which is a dispersion liquid in which silica fine particles are dispersed, was used as Comparative Example 3.
[0118] All analytical and measurement results in the examples and comparative examples are shown in Tables 1 and 2. Specifically, Table 1 shows the weight-average particle size (D1), specific surface area converted particle size (D2), kurtosis, skewness, irregularity (D=D1 / D3), the number of separated peaks by waveform separation of the volume-based particle size distribution, the volume fraction of the largest particle component among the separated peaks obtained as a result of waveform separation of the volume-based particle size distribution, the aspect ratio of the small particle diameter component in the number-based particle size distribution obtained by SEM image analysis, the coefficient of variation of particle size in the volume-based particle size distribution, the ratio (S=S2 / S1) of the area of the circle equivalent to the average perimeter by image analysis to the average area (S1) by image analysis, the ratio (Q=Q2 / Q1) of the volume of particles of 0.7 μm or more to the total volume (Q1) in the volume-based particle size distribution, and the fraction of particles with an aspect ratio value of 1.1 or more. Table 2 shows the specific surface area of the silica gel used in step a, the weight average particle size of the particles after crushing, and the pH during wet crushing, and Table 2 shows the specific surface area after the particles made of silica gel are reacted with silicic acid in step b, the weight average particle size of the particles made of silica gel after growth, the SiO2 concentration of the solution containing particles made of silica gel, the temperature after the solution containing particles made of silica gel is heated, the pH of the solution containing particles made of silica gel, and the SiO2 molar concentration of the silicic acid solution to be added relative to the SiO2 molar concentration of the solution containing particles made of irregular silica gel. Furthermore, the measurement results of the polishing rate and waviness are shown in Table 2.
[0119] [Table 1]
[0120] [Table 2] [Industrial Applicability]
[0121] Since the silica-based particle group of the present invention has a suitable particle size, particle size distribution, irregularity and particle strength, a silica-based particle dispersion containing the same can be preferably used for surface polishing of NiP-plated substrates to be polished, silica-based substrates and the like.
Claims
1. A silica-based particle dispersion liquid containing a silica-based particle group consisting of irregularly shaped silica-based particles and non-irregularly shaped silica-based particles, The silica-based particle group is a silica-based particle dispersion liquid that satisfies the following [1] to [3]. [1] Weight average particle diameter (D 1 ) is 60 to 400 nm, and the specific surface area converted particle diameter (D 2 ) is 20 to 300 nm (but the specific surface area is 30 m 2 / g or less). [2] Weight average particle diameter (D 1 ) and projected area equivalent particle diameter (D 3 The irregularity D (D = D 1 / D 3 ) is in the range of 1.1 to 5.
0. [3] When the volumetric particle size distribution is subjected to waveform separation, it becomes a multi-modal distribution in which three or more separation peaks are detected.
2. 2. The silica-based particle dispersion according to claim 1, wherein the silica-based particles have a skewness in the range of −20 to 20 in their volume-based particle size distribution.
3. 3. The silica-based particle dispersion liquid according to claim 1, wherein the volume ratio of the largest particle component among the separation peaks obtained as a result of waveform separation of the volume-based particle size distribution of the silica-based particle group is 75% or less.
4. 4. The silica-based particle dispersion liquid according to claim 1, wherein in a number-based particle size distribution obtained by SEM image analysis of the silica-based particle group, an aspect ratio of a small particle component is in the range of 1.05 to 5.
0.
5. 5. The silica-based particle dispersion according to claim 1, wherein the silica-based particles have a particle size variation coefficient of 30% or more in a volume-based particle size distribution.
6. The average area (S 1) using image analysis to find the average circumference and the equivalent circle area (S 2 Smoothness S, expressed as the ratio of 2 / S 1 6. The silica-based particle dispersion liquid according to claim 1, wherein the ratio of the surface area to the surface area of the silica-based particle dispersion liquid is in the range of 1.1 to 5.
0.
7. In the volume-based particle size distribution of the silica-based particle group, the total volume (Q 1 ) to the volume of particles 0.7 μm or larger (Q 2 ) ratio Q (Q = Q 2 / Q 1 7. The silica-based particle dispersion liquid according to claim 1, wherein the content of the silica-based particle dispersion liquid is 5.0% or less.
8. 8. A polishing abrasive dispersion comprising the silica-based particle dispersion according to claim 1.
9. A silica-based particle group consisting of irregularly shaped silica-based particles and non-irregularly shaped silica-based particles, A group of silica-based particles that satisfy the following [1] to [3]: [1] Weight average particle diameter (D 1 ) is 60 to 400 nm, and the specific surface area converted particle diameter (D 2 ) is 20 to 300 nm (but the specific surface area is 30 m 2 / g or less). [2] Weight average particle diameter (D 1 ) and projected area equivalent particle diameter (D 3 The irregularity D (D = D 1 / D 3 ) is in the range of 1.1 to 5.
0. [3] When the volumetric particle size distribution is subjected to waveform separation, it becomes a multi-modal distribution in which three or more separation peaks are detected.
10. A method for producing a silica-based particle group comprising irregularly shaped silica-based particles and non-irregularly shaped silica-based particles, comprising the steps of: (Step a) A step of wet-disintegrating a silica-based gel having a specific surface area of 50 to 200 m 2 / g under alkaline conditions to obtain a solution containing particles made of highly irregular silica-based gel having a weight-average particle size of 60 to 142 nm. (Step b) A process in which a silicic acid liquid is added under alkaline conditions to a solution containing particles made of the highly irregular silica-based gel and heated, filling the pores between the primary particles of the particles made of the highly irregular silica-based gel by reaction with the silicic acid contained in the silicic acid liquid, thereby growing the particles while maintaining a high degree of irregularity, thereby forming irregular silica-based particles having a specific surface area of 136 m2 / g or less [excluding particles having a specific surface area of 30 m2 / g or less] and a weight average particle diameter of 60 to 400 nm. (Step c) A step of concentrating and recovering the silica-based particle group including the grown irregular shaped silica-based particles.
11. In the step (a), the silica-based gel is wet-disintegrated under an alkaline condition of pH 8.0 to 11.5 to obtain a solution containing particles made of the highly irregular silica-based gel; In the step b, the SiO of the solution containing the particles made of the highly irregular silica-based gel is 2 The silicic acid liquid is added continuously or intermittently to a concentration of 1 to 10% by mass, heated to 60°C to 170°C, and under an alkaline condition of pH 9 to 12.5, so that pores between primary particles of the particles made of the highly irregular silica-based gel are filled by a reaction with the silicic acid, thereby reducing the specific surface area of the particles and allowing the particles to grow while maintaining their irregular shapes; The method for producing a silica-based particle group consisting of irregular silica-based particles and non-irregular silica-based particles, as described in claim 10, characterized in that in step c, a solution containing the grown irregular silica-based particles is concentrated to recover a silica-based particle group containing the irregular silica-based particles.
12. In the step b, the amount of the silicic acid solution added is such that the SiO 2 The SiO of the silicic acid solution relative to the molar concentration 2 The method for producing a silica-based particle group comprising irregularly shaped silica-based particles and non-irregularly shaped silica-based particles according to claim 10 or 11, characterized in that the molar concentration is in the range of 0.5 to 20 times the molar concentration.
Citation Information
Patent Citations
Jikiseigyosochi
JP1976027452A
Deformed silica sol
JP2013032276A
System and method
JP2017177576A
Dispersion liquid, and production method of the same and polishing agent for cmp using the same
JP2017197693A
Ceria-based composite fine particle dispersion, manufacturing method therefor and polishing abrasive dispersion containing the ceria-based composite fine particle dispersion
JP2018123046A