Composition
A composition of nanosized luminescent materials and (meth)acrylic polymers with specific structures addresses the issues of low resolution and solvent resistance in optical devices by achieving high polymerization and crosslinking density, enhancing patterning and durability.
Patent Information
- Application Number
- JP2021505863
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-08-03
- Filing Date
- 2019-07-31
- Publication Date
- 2024-11-28
- Estimated Expiration
- 2039-07-31
AI Technical Summary
Existing photosensitive compositions containing nanosized luminescent materials suffer from insufficient polymerization during photocuring, leading to low resolution and poor solvent resistance in optical devices, particularly in micro-LED applications.
A composition comprising nanosized luminescent materials and (meth)acrylic polymers with specific chemical structures, allowing for high polymerization even at low UV exposure doses, resulting in high crosslinking density and improved solvent resistance.
The composition enables high-resolution patterning and enhanced solvent resistance of optical films, maintaining quantum yield and durability of quantum materials in optical media.
Smart Images

Figure 0007591493000001 
Figure 0007591493000002 
Figure 0007591493000003
Abstract
Description
[Technical field]
[0001] FIELD OF THEINVENTION The present invention relates to a composition comprising at least one nano-sized luminescent material and a (meth)acrylic polymer.The present invention further relates to the use of the (meth)acrylic polymer in a composition, the use of the composition in a process for producing an optical medium, and the use of the optical medium in an optical device.The present invention further relates to an optical device comprising the optical medium, and a method for preparing the optical medium and the optical device. [Background technology]
[0002] 2. Background of the Invention Photosensitive compositions containing nano-sized luminescent materials, quantum materials or quantum dots are used for various optical applications, such as quantum material-doped photoresist films, especially for preparing optical devices. Such quantum material-doped photoresist films have great potential to widen the color gamut and improve the energy efficiency of display and lighting devices. However, especially for micro LED applications, quantum material-doped photoresist films that have high solvent resistance and can be patterned at high resolution using conventional photolithography techniques are required.
[0003] However, due to insufficient polymerization during the photocuring process, such films cannot be easily patterned with high resolution, and the cured films exhibit poor solvent resistance. In particular, the quantum material embedded in the film largely absorbs the UV light exposed during the curing process, resulting in insufficient in-depth photopolymerization, which is mainly responsible for the low resolution of the photopattern, and the insufficient crosslink density at the film surface leads to poor durability to solvents of the overcoated material applied to the cured film. Thus, a need exists for compositions that can improve the resolution of photopatterns and the solvent resistance of cured films. Summary of the Invention
[0004] SUMMARY OF THE PRESENT APPLICATION The present invention has been made in view of the problems described above.Therefore, the object of the present invention is to provide a composition that can achieve sufficient polymerization even at lower UV exposure doses to improve photopatterning ability, and can form a highly crosslinked polymer surface, which can improve solvent resistance on the cured film.Preferably, the composition is a photosensitive composition.
[0005] The inventors have surprisingly found that one or more of the above mentioned problems can be solved by the features as defined in the claims. Specifically, in order to solve one or more of the problems described above, the present invention provides a composition comprising at least one nano-sized luminescent material and a (meth)acrylic polymer, wherein the (meth)acrylic polymer has the following chemical formula (1):
[0006] [ka] During the ceremony, R 1 denotes, identically or differently, each occurrence of hydrogen, a straight-chain alkyl group having 1 to 20 C atoms, a branched or cyclic alkyl group having 3 to 20 C atoms, an alkenyl or alkynyl group having 2 to 20 C atoms, an aryl or heteroaryl group having 5 to 24 C atoms, in which one or more non-adjacent methylene structural units (-CH2-) in the alkyl, alkenyl, alkynyl, aryl or heteroaryl group may in each case be replaced by a sulfonyl group, a carbonyl group, an ether group, a sulfide group, a sulfoxide group, an ester group, an amide group or an imine group,
[0007] and wherein the alkyl, alkenyl, alkynyl, aryl or heteroaryl group may have one or more H atoms replaced by F, Cl, Br, I, CN or OH, a carboxyl group (-COOH), a linear alkyl or alkoxy group having 2 to 20 C atoms, a branched alkyl or alkoxy group having 3 to 20 C atoms or an alkenyl or alkynyl group having 2 to 20 C atoms,
[0008] R 2 , R 2 ' denotes, identically or differently, for each occurrence, a hydrogen atom, a hydroxyl group (-OH), a carboxyl group (-COOH), a linear alkyl group having 1 to 20 C atoms, a branched or cyclic alkyl group having 3 to 20 C atoms, an alkenyl or alkynyl group having 2 to 20 C atoms, an aryl or heteroaryl group having 5 to 24 C atoms, in which one or more non-adjacent methylene structural units (-CH2-) in the alkyl, alkenyl, alkynyl, aryl or heteroaryl group may in each case be replaced by a sulfonyl group, a carbonyl group, an ether group, a sulfide group, a sulfoxide group, an ester group, an amide group or an imine group,
[0009] and wherein said alkyl, alkenyl, alkynyl, aryl or heteroaryl group may have one or more H atoms replaced by F, Cl, Br, I, CN or OH, a carboxyl group (-COOH), a linear alkyl or alkoxy group having 2 to 20 C atoms, a branched alkyl or alkoxy group having 3 to 20 C atoms or an alkenyl or alkynyl group having 2 to 20 C atoms, with the proviso that the radicals R 2 and R 2 ' may also represent a carboxyl group,
[0010] R 3denotes, identically or differently, for each occurrence, hydrogen, a straight-chain alkyl group having 1 to 20 C atoms, a branched or cyclic alkyl group having 3 to 20 C atoms, an alkenyl or alkynyl group having 2 to 20 C atoms, an aryl or heteroaryl group having 5 to 24 C atoms, in which one or more non-adjacent methylene structural units (-CH2-) in the alkyl, alkenyl, alkynyl, aryl or heteroaryl group may in each case be replaced by a sulfonyl group, a carbonyl group, an ether group, a sulfide group, a sulfoxide group, an ester group, an amide group or an imine group,
[0011] and wherein the alkyl, alkenyl, alkynyl, aryl or heteroaryl group may have one or more H atoms replaced by F, Cl, Br, I, CN or OH, a carboxyl group (-COOH), a linear alkyl or alkoxy group having 2 to 20 C atoms, a branched alkyl or alkoxy group having 3 to 20 C atoms or an alkenyl or alkynyl group having 2 to 20 C atoms,
[0012] R 4 denotes, identically or differently, at each occurrence, a straight-chain alkylene group having 1 to 20 C atoms, a branched alkylene group having 2 to 20 C atoms, an alkenylene or alkynylene group having 2 to 20 C atoms, or an arylene or heteroarylene group having 6 to 24 C atoms, in which one or more methylene structural units (-CH2-) in the alkylene, alkenylene, alkynylene, arylene or heteroarylene group may in each case be replaced by a sulfonyl group, a carbonyl group, an ether group, a sulfide group, a sulfoxide group, an ester group, an amide group, an imine group, a group CHR', or a group CR'R'',
[0013] R', R'' are identical or different and each occurrence represents a hydroxyl group, a linear alkyl group having 1 to 20 C atoms, a branched or cyclic alkyl group having 3 to 20 C atoms, an alkenyl or alkynyl group having 2 to 20 C atoms, an aryl or heteroaryl group having 5 to 24 C atoms, in which one or more non-adjacent methylene structural units (-CH2-) in the alkyl, alkenyl, alkynyl, aryl or heteroaryl group may in each case be replaced by a sulfonyl group, a carbonyl group, an ether group, a sulfide group, a sulfoxide group, an ester group, an amide group or an imine group;
[0014] and wherein the alkyl, alkenyl, alkynyl, aryl or heteroaryl group may have one or more H atoms replaced by F, Cl, Br, I, CN or OH, a linear alkyl or alkoxy group having 2 to 20 C atoms, a branched alkyl or alkoxy group having 3 to 20 C atoms or an alkenyl or alkynyl group having 2 to 20 C atoms, wherein the composition comprises at least one structural unit represented by the formula:
[0015] The inventors have surprisingly found that compositions according to the invention have a radiation energy density of, for example, about 80 mJ / cm2, which is acceptable for mass production processes. 2 It has been found that even at a low UV exposure dose of 10 μm, the photoresist composite film can be sufficiently polymerized for the preparation of the photoresist composite film, and such a film can be easily patterned with high resolution, for example in the range of 10 μm, allowing optical media such as optical films or patterned films to be manufactured at low cost. Due to the low UV dose, the quantum material in the photoresist composite film is not significantly damaged during UV exposure, and the quantum material can maintain a high quantum yield in the optical media.
[0016] Furthermore, the inventors have surprisingly found that the photosensitive composition according to the present invention exhibits high crosslink density at the film surface, and a highly crosslinked polymer surface can be formed, which leads to high solvent resistance and high chemical durability of the photoresist composite film, especially when a topcoat material is applied to the film, and especially prevents peeling of the photocured areas during the alkaline development process. Further, in order to solve one or more of the problems described above, the present invention provides the use of a (meth)acrylic polymer comprising at least one structural unit represented by chemical formula (1) in a composition comprising at least one nano-sized light-emitting material, preferably the composition is a photosensitive composition.
[0017] The present invention further relates to a method comprising the steps of: a) providing a composition to a substrate; and b) polymerizing the composition by exposing it to radiation; In one embodiment, a method for preparing an optical film is provided, the method comprising the steps of: In a preferred embodiment, the composition is a photosensitive composition.
[0018] The present invention also relates to optical media formed from the compositions, preferably from the photosensitive compositions of the present invention. The present invention further relates to the use of the optical medium in an optical device. The present invention further relates to an optical device comprising the optical medium, and to a method for preparing an optical device comprising the step of providing the optical medium to the optical device.
[0019] Further advantages of the present invention will become apparent from the following detailed description. Detailed Description of the Invention DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The best mode for carrying out the present invention is described below in detail. As used herein, an asterisk ("*" or " *") is generally used to indicate a link to an adjacent unit or group, including, for example, an adjacent repeat or constitutional unit in the case of a polymer or another group, for example, a side chain in the case of a monomeric compound. As used herein, the terms "photosensitive" or "photoreactive" mean that the respective composition chemically reacts in response to suitable light irradiation. The light is often selected from visible or UV light. The photosensitive response includes hardening or softening of the composition, preferably hardening.
[0020] For the purposes of this application, the term "copolymer" is used to indicate a polymer derived from more than one type of monomer (see also International Union of Pure and Applied Chemistry, Compendium of Chemical Terminology, Gold Book, Version 2.3.3, 2012-02-24, page 335). For the purposes of this application, the term "monomer" is used to denote a substance composed of monomer molecules, and the term "monomer molecule" is used to denote a molecule that can undergo polymerization, thereby contributing one or more building blocks to the essential structure of a macromolecule or polymer (see also International Union of Pure and Applied Chemistry, Compendium of Chemical Terminology, Gold Book, Version 2.3.3, 2012-02-24, page 662).
[0021] According to the present invention, a composition, preferably a photosensitive composition, comprising at least one nanosized luminescent material and a (meth)acrylic polymer is provided to solve the object of the present invention as described above. As used herein, the term "(meth)acrylic polymer" refers to a general term for a polymer obtained by polymerization of monomers selected from the group consisting of acrylic acid, methacrylic acid, acrylates, methacrylates, and any combination thereof. (Meth)acrylic polymers have the following chemical formula (1): [ka] During the ceremony,
[0022] R 1 denotes, identically or differently, each occurrence of hydrogen, a straight-chain alkyl group having 1 to 20 C atoms, a branched or cyclic alkyl group having 3 to 20 C atoms, an alkenyl or alkynyl group having 2 to 20 C atoms, an aryl or heteroaryl group having 5 to 24 C atoms, in which one or more non-adjacent methylene structural units (-CH2-) in the alkyl, alkenyl, alkynyl, aryl or heteroaryl group may in each case be replaced by a sulfonyl group, a carbonyl group, an ether group, a sulfide group, a sulfoxide group, an ester group, an amide group or an imine group,
[0023] and wherein the alkyl, alkenyl, alkynyl, aryl or heteroaryl group may have one or more H atoms replaced by F, Cl, Br, I, CN or OH, a carboxyl group (-COOH), a linear alkyl or alkoxy group having 2 to 20 C atoms, a branched alkyl or alkoxy group having 3 to 20 C atoms or an alkenyl or alkynyl group having 2 to 20 C atoms,
[0024] R 2 , R 2' denotes, identically or differently, for each occurrence, a hydrogen atom, a hydroxyl group (-OH), a carboxyl group (-COOH), a linear alkyl group having 1 to 20 C atoms, a branched or cyclic alkyl group having 3 to 20 C atoms, an alkenyl or alkynyl group having 2 to 20 C atoms, an aryl or heteroaryl group having 5 to 24 C atoms, in which one or more non-adjacent methylene structural units (-CH2-) in the alkyl, alkenyl, alkynyl, aryl or heteroaryl group may in each case be replaced by a sulfonyl group, a carbonyl group, an ether group, a sulfide group, a sulfoxide group, an ester group, an amide group or an imine group,
[0025] and wherein said alkyl, alkenyl, alkynyl, aryl or heteroaryl group may have one or more H atoms replaced by F, Cl, Br, I, CN or OH, a carboxyl group (-COOH), a linear alkyl or alkoxy group having 2 to 20 C atoms, a branched alkyl or alkoxy group having 3 to 20 C atoms or an alkenyl or alkynyl group having 2 to 20 C atoms, with the proviso that the radicals R 2 and R 2 ' may also represent a carboxyl group,
[0026] R 3 denotes, identically or differently, for each occurrence, hydrogen, a straight-chain alkyl group having 1 to 20 C atoms, a branched or cyclic alkyl group having 3 to 20 C atoms, an alkenyl or alkynyl group having 2 to 20 C atoms, an aryl or heteroaryl group having 5 to 24 C atoms, in which one or more non-adjacent methylene structural units (-CH2-) in the alkyl, alkenyl, alkynyl, aryl or heteroaryl group may in each case be replaced by a sulfonyl group, a carbonyl group, an ether group, a sulfide group, a sulfoxide group, an ester group, an amide group or an imine group,
[0027] and wherein the alkyl, alkenyl, alkynyl, aryl or heteroaryl group may have one or more H atoms replaced by F, Cl, Br, I, CN or OH, a carboxyl group (-COOH), a linear alkyl or alkoxy group having 2 to 20 C atoms, a branched alkyl or alkoxy group having 3 to 20 C atoms or an alkenyl or alkynyl group having 2 to 20 C atoms,
[0028] R 4 denotes, identically or differently, at each occurrence, a straight-chain alkylene group having 1 to 20 C atoms, a branched alkylene group having 2 to 20 C atoms, an alkenylene or alkynylene group having 2 to 20 C atoms, or an arylene or heteroarylene group having 6 to 24 C atoms, in which one or more methylene structural units (-CH2-) in the alkylene, alkenylene, alkynylene, arylene or heteroarylene group may in each case be replaced by a sulfonyl group, a carbonyl group, an ether group, a sulfide group, a sulfoxide group, an ester group, an amide group, an imine group, a group CHR', or a group CR'R'',
[0029] R', R'' are identical or different and each occurrence represents a hydroxyl group, a linear alkyl group having 1 to 20 C atoms, a branched or cyclic alkyl group having 3 to 20 C atoms, an alkenyl or alkynyl group having 2 to 20 C atoms, an aryl or heteroaryl group having 5 to 24 C atoms, in which one or more non-adjacent methylene structural units (-CH2-) in the alkyl, alkenyl, alkynyl, aryl or heteroaryl group may in each case be replaced by a sulfonyl group, a carbonyl group, an ether group, a sulfide group, a sulfoxide group, an ester group, an amide group or an imine group;
[0030] and wherein the alkyl, alkenyl, alkynyl, aryl or heteroaryl group may have one or more H atoms replaced by F, Cl, Br, I, CN or OH, a linear alkyl or alkoxy group having 2 to 20 C atoms, a branched alkyl or alkoxy group having 3 to 20 C atoms or an alkenyl or alkynyl group having 2 to 20 C atoms, The copolymer contains at least one (meth)acrylic structural unit containing an acryloyl group, as represented by the following formula:
[0031] As used herein, the term "cyclic alkyl group" is understood to include monocyclic alkyl groups, polycyclic alkyl groups such as bicyclic alkyl groups, and combinations of cyclic and straight-chain or branched alkyl groups. As used herein, the term "aryl group" is understood to also include "arylalkyl group," a term which is a substituent derived from an aromatic hydrocarbon, such as phenyl, and which is understood to mean an aryl group to which an alkyl group is attached.
[0032] As used herein, the term "heteroaryl group" is understood to mean an aryl group in which at least one carbon atom has been replaced by one of the heteroatoms O, N or S. As used herein, the term "arylene group" is a substituent derived from an aromatic hydrocarbon (arene) with hydrogen atoms removed from two ring carbon atoms, such as phenylene. The term "arylene group" is also understood to include "arylalkylene group", which is a term that is understood to mean the above arylalkyl group with hydrogen atoms removed from two carbon atoms, regardless of whether the carbon atoms are in a chain or ring. Thus, the term "heteroarylene group" is a substituent derived from the above heteroaryl group with hydrogen atoms removed from two ring atoms, and is also understood to include a heteroarylene group to which an alkyl group is bonded.
[0033] Preferably, in formula (1), the radical R 1denotes hydrogen, a linear alkyl group having 1 to 10 C atoms or a branched alkyl group having 3 to 10 C atoms. More preferably, the radical R 1 represents hydrogen or a methyl group. More preferably, in formula (1), the radical R 2 ' denotes a hydrogen or methyl group, and the radical R 2 denotes hydrogen, a carboxyl group, a linear alkyl group having 1 to 8 C atoms, where one or more H atoms may be replaced by F, Cl, OH or a carboxyl group (-COOH). Even more preferably, the radical R 2 ' denotes hydrogen, and the radical R 2 represents a methyl group or a carboxyl group.
[0034] More preferably, in formula (1), the radical R 3 denotes hydrogen, a linear alkyl group having 1 to 10 C atoms or a branched alkyl group having 3 to 10 C atoms. More preferably, the radical R 3 represents hydrogen or a methyl group. More preferably, in formula (1), the radical R 4 denotes a linear alkylene group having 1 to 10 C atoms, a branched alkylene group having 2 to 10 C atoms, an alkenylene group having 2 to 10 C atoms, or an arylene group having 6 to 10 C atoms, in which in the alkylene, alkenylene, or arylene group, one or more non-adjacent methylene structural units (-CH2-) may be replaced by a sulfonyl group, a carbonyl group, an ether group, a sulfide group, a sulfoxide group, an ester group, an amide group, an imine group, a group CHR' or a group CR'R'', where R', R'' have the same meaning as defined above. Even more preferably, the radical R 4 represents a linear alkylene group having 1 to 6 C atoms, an alkenylene group having 2 to 6 C atoms, or an arylene group having 6 C atoms.
[0035] Preferably, R', R'' are identical or different and each occurrence represents a hydroxyl group, a linear alkyl group having 1 to 10 C atoms, a branched alkyl group having 3 to 10 C atoms, an alkenyl or alkynyl group having 2 to 10 C atoms, an aryl group having 6 to 10 C atoms, in which one or more non-adjacent methylene structural units (-CH2-) in the alkyl, alkenyl, alkynyl or aryl group may in each case be replaced by a sulfonyl group, a carbonyl group, an ether group, a sulfide group, a sulfoxide group, an ester group, an amide group or an imine group; and wherein said alkyl, alkenyl, alkynyl, or aryl group may have one or more H atoms replaced by F, Cl, Br, I, CN, or OH.
[0036] Most preferably, the radical R 1 denotes hydrogen or a methyl group, and the radical R 2 ' denotes hydrogen and the radical R 2 denotes hydrogen, a carboxyl group or a methyl group, and the radical R 3 denotes hydrogen or a methyl group, and the radical R 4 denotes a methylene group or a straight-chain alkylene group having 2 to 6 C atoms. Without wishing to be bound by theory, it is believed that due to the (meth)acrylic polymer comprising at least one (meth)acrylic structural unit containing an acryloyl group as represented by chemical formula (1), the number of (photo)reactive sites increases, so that sufficient polymerization of the photosensitive composition can be achieved.Therefore, the composition ratio of (meth)acrylic polymer can be reduced while maintaining sufficient polymerization.Therefore, a higher loading of quantum dot material in the photosensitive composition can be realized to achieve high OD.
[0037] According to the present invention, the (meth)acrylic polymer is represented by the following chemical formulas (2), (3) and (4): [ka] In the formula, the radical R1 , R 2 and R 2 ' is, at each occurrence, identically or differently, as defined above for formula (1);
[0038] R 5 denotes, identically or differently, for each occurrence, a straight-chain alkylene group having 1 to 20 C atoms, a branched alkylene group having 2 to 20 C atoms, an alkenylene or alkynylene group having 2 to 20 C atoms, or an arylene or heteroarylene group having 6 to 24 C atoms, in which one or more methylene structural units (-CH2-) in the alkylene, alkenylene, alkynylene, arylene or heteroarylene group may in each case be replaced by a sulfonyl group, a carbonyl group, an ether group, a sulfide group, a sulfoxide group, an ester group, an amide group, an imine group, a group CHR', or a group CR'R'', in which the radicals R' and R'' are as defined above, and
[0039] R 6 denotes, identically or differently, each occurrence of a linear alkyl group having 1 to 20 C atoms, a branched alkyl group having 3 to 20 C atoms or a cyclic alkyl group having 3 to 20 C atoms, It is even more preferable if the polymer further comprises one or more structural units selected from:
[0040] More preferably, in formula (3), the radical R 5 denotes a linear alkylene group having 1 to 10 C atoms, a branched alkylene group having 2 to 10 C atoms or an alkenylene group having 2 to 10 C atoms, in which in the alkylene or alkenylene group one or more non-adjacent methylene structural units (-CH2-) may be replaced by a sulfonyl group, a carbonyl group, an ether group, a sulfide group, a sulfoxide group, an ester group, an amide group, an imine group, a group CHR' or a group CR'R'', in which the radicals R' and R'' are as defined above. Even more preferably, the radical R 5denotes a linear alkylene group having 1 to 6 C atoms, in which one or more non-adjacent methylene structural units (-CH2-) may be replaced by a group CHR' or a group CR'R'', where R' and R'' are identical or different and denote, at each occurrence, a hydroxyl group, a linear alkyl group having 1 to 6 C atoms or a branched alkyl group having 3 to 6 C atoms,
[0041] wherein the alkyl group has one or more H atoms that may be replaced by F, Cl, or OH. Even more preferably, in formula (4), the radical R 6 denotes a linear alkyl group having 1 to 10 C atoms, a branched alkyl group having 3 to 10 C atoms, or a cyclic alkyl group having 6 C atoms. Even more preferably, the radical R 6 represents a linear alkyl group having 2 to 8 C atoms.
[0042] This means that, according to the present invention, the (meth)acrylic polymer comprising at least one (meth)acrylic structural unit containing an acryloyl group (corresponding to the above chemical formula (1)) is preferably a copolymer further comprising one or more (meth)acrylic structural units containing a carboxyl group (corresponding to the above chemical formula (2)), and / or one or more (meth)acrylic structural units containing a hydroxyl group (corresponding to the above chemical formula (3)), and / or one or more (meth)acrylic structural units containing an alkyl ester group (corresponding to the above chemical formula (4)).
[0043] According to the present invention, it is particularly preferred if the (meth)acrylic polymer comprising at least one (meth)acrylic structural unit comprising an acryloyl group further comprises one or more (meth)acrylic structural units comprising a carboxyl group, one or more (meth)acrylic structural units comprising a hydroxyl group, and one or more (meth)acrylic structural units comprising an alkyl ester group, each group being as defined herein. The (meth)acrylic polymer is preferably a copolymer obtained by polymerization of different monomers. The meth)acrylic structural unit containing a carboxyl group serves to dissolve the polymer in an alkaline developer, and is preferably derived from an unsaturated carboxylic acid. Examples of the unsaturated carboxylic acid for forming the meth)acrylic structural unit containing a carboxyl group include (meth)acrylic acid, maleic acid, fumaric acid, crotonic acid, itaconic acid, citraconic acid, mesaconic acid, and cinnamic acid. It is also possible to use a mixture of these unsaturated carboxylic acids. Among the above, (meth)acrylic acid is particularly preferred.
[0044] The number of (meth)acrylic structural units including carboxyl groups is not particularly limited. The content of this structural unit in the polymer is preferably between 3 and 50 wt.%, more preferably between 5 and 30 wt.%. Within this range, the solubility of the polymer in areas where it is intended to dissolve in an alkaline developer is increased. In order to balance better reactivity and storage stability of the photosensitive composition, the acid value of the (meth)acrylic polymer is preferably in the range of 10 to 200 mg KOH / g. More preferably, it is from 15 mg KOH / g to 150 mg KOH / g.
[0045] The (meth)acrylic structural units containing hydroxyl groups play a role in forming crosslinked structures that give the polymer properties such as mechanical strength. These structural units are preferably derived from hydroxyl-containing unsaturated monomers such as 2-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 5-hydroxypentyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, or 8-hydroxyoctyl (meth)acrylate; 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 2-hydroxypropyl-3-phenoxypropyl (meth)acrylate, or 3-chloro-2-hydroxypropyl (meth)acrylate, and tertiary hydroxyl-containing monomers such as 2,2-dimethyl-2-hydroxyethyl (meth)acrylate, diethylene glycol (meth)acrylate, or glycerol (meth)acrylate. The content of the (meth)acrylic structural unit including a hydroxyl group in the polymer is preferably 3 wt.% or more so that the polymer can have properties such as mechanical strength, but is preferably 40 wt.% or less so as not to impair storage stability. The (meth)acrylic structural unit including a hydroxyl group is particularly preferably contained in an amount of 5 to 35 wt.%.
[0046] (Meth)acrylic structural units containing alkyl ester groups also provide properties such as mechanical strength to the polymer. These structural units are preferably methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, n-pentyl (meth)acrylate, isopentyl (meth)acrylate, neopentyl (meth)acrylate. It is derived from an unsaturated carboxylic acid ester monomer such as n-hexyl (meth)acrylate, isohexyl (meth)acrylate, n-heptyl (meth)acrylate, isoheptyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, n-nonyl (meth)acrylate, isononyl (meth)acrylate, n-decyl (meth)acrylate, isodecyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, or cyclohexyl (meth)acrylate.
[0047] The content of the (meth)acrylic structural unit including an alkyl ester group in the polymer is preferably 3 wt.% or more so that the polymer can have properties such as mechanical strength, but is preferably 40 wt.% or less so as not to impair storage stability. The (meth)acrylic structural unit including an alkyl ester group is particularly preferably contained in an amount of 5 to 35 wt.%.
[0048] The other polymerized units play a role in forming the main backbone of the polymer so that the polymer can have properties such as mechanical strength. These polymerized units are derived from copolymerizable monomers, but are not particularly limited. Examples of copolymerizable monomers include aromatic vinyl compounds such as styrene, a-methylstyrene, tert-butylstyrene, o-vinyltoluene, m-vinyltoluene, p-vinyltoluene, p-chlorotoluene, o-methoxystyrene, m-methoxystyrene, p-methoxystyrene, o-vinylbenzyl methyl ether, m-vinylbenzyl methyl ether, p-vinylbenzyl methyl ether, o-vinylbenzyl glycidyl ether, m-vinylbenzyl glycidyl ether, and p-vinylbenzyl glycidyl ether;
[0049] and tridecyl lauryl (meth)acrylate, cetyl lauryl (meth)acrylate, n-stearyl lauryl (meth)acrylate, i-stearyl lauryl (meth)acrylate, phenyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, isobornyl (meth)acrylate, 2-methyl-2-adamantyl (meth)acrylate, 2-ethyl-2-adamantyl (meth)acrylate, 2-isopropyl-2-adamantyl (meth)acrylate, 2-methoxyethyl (meth)acrylate, 2 -Phenoxyethyl (meth)acrylate, diethylene glycol monomethyl ether (meth)acrylate, triethylene glycol monomethyl ether (meth)acrylate, propylene glycol monomethyl ether (meth)acrylate, dipropylene glycol monomethyl ether (meth)acrylate, isobornyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, 2-aminoethyl (meth)acrylate, 2-dimethylaminoethyl (meth)acrylate, 2-aminopropyl (meth)acrylate, 2-dimethylaminopropyl (meth)acrylate, 3-aminoethyl (meth)acrylate, 3-dimethylaminoethyl (meth)acrylate, glycidyl (meth)acrylate, 2,2,2-trifluoroethyl (meth)acrylate, 2,2,3,3-tetrafluoropropyl (meth)acrylate, 2,2,3,3,3-pentafluoropropyl (meth)acrylate, 2,2,3,4,4,4-hexafluorobutyl (meth)acrylate, 2-(perfluorobutyl)ethyl (meth)acrylate , 3-perfluorobutyl-2-hydroxypropyl (meth)acrylate, 2-(perfluorohexyl)ethyl (meth)acrylate, 3-perfluorohexyl-2-hydroxyl-propyl (meth)acrylate, lH,lH,3H-tetrafluoropropyl (meth)acrylate, lH,lH,5H-octafluoropentyl (meth)acrylate, lH,lH,7H-dodecafluoroheptyl (meth)acrylate, and perfluorooctylethyl (meth)acrylate.
[0050] The content of other polymerized units in the polymer is preferably 40 wt.% or more so that the polymer can have properties such as mechanical strength, but is preferably 90 wt.% or less so that the polymer can reliably contain essential constituent substances. According to the present invention, the weight average molecular weight (Mw) of the (meth)acrylic polymer is not particularly limited. Preferably, the weight average molecular weight of the (meth)acrylic polymer is in the range of 2000 to 10,000, more preferably 3000 to 30000, and even more preferably 4000 to 20000. Here, "weight average molecular weight" means the weight average molecular weight in terms of polystyrene determined by gel permeation chromatography (GPC).
[0051] More preferably, according to the present invention, the equivalent weight of the (meth)acrylic structural unit containing an acryloyl group in the (meth)acrylic polymer ranges from 400 to 560, more preferably from 440 to 520, and even more preferably is 480. As used herein, the term "equivalent weight" should be understood to mean the molecular weight / number n of structural units containing an acryloyl group (unit: g / eq) and indicates the molecular weight per one structural unit containing an acryloyl group. By varying the equivalent weight of the (meth)acrylic structural unit including an acryloyl group in the (meth)acrylic polymer, the (photo)reactivity of the (meth)acrylic polymer can be adjusted as desired. -Nano-sized light-emitting materials
[0052] In accordance with the present invention, as the inorganic portion of the semiconducting nano-sized luminescent material, a wide variety of publicly known semiconducting nano-sized luminescent materials may be used as desired. The shape type of the nano-sized luminescent material of the present invention is not particularly limited. Any type of nano-sized luminescent material, such as spherical, elongated, star-shaped, polyhedral semiconducting luminescent nanoparticles, can be used. In a preferred embodiment of the present invention, the nano-sized luminescent material may be selected from the group consisting of nano-sized inorganic phosphor materials, quantum sized materials such as quantum dots and / or quantum rods, and any combination thereof. More preferably, the nano-sized luminescent material is a quantum sized material, and even more preferably a quantum dot material, a quantum rod material, or any combination thereof.
[0053] According to the present invention, the term "nano-sized" means a size ranging from 0.1 to 999 nm, preferably from 0.1 to 150 nm. Thus, according to the present invention, nano-sized luminescent material is understood to mean a luminescent material whose overall diameter size ranges from 0.1 to 999 nm, preferably from 0.1 to 150 nm. And, when the material has an elongated shape, the length of the overall structure of the fluorescent material ranges from 0.1 to 999 nm, preferably from 0.1 to 150 nm.
[0054] As used herein, the term "quantum size" refers to the size of the semiconducting luminescent material itself without ligands or other surface modifications, which can exhibit quantum confinement effects, as described, for example, in ISBN:978-3-662-44822-9. In general, quantum size materials, such as quantum dot materials and / or quantum rod materials, are said to be capable of tunable, sharp, and vibrant color light emission due to the "quantum confinement" effect. Preferably, the size of the overall structure of the quantum sized material is from 1 nm to 100 nm, more preferably from 1 nm to 30 nm, and even more preferably from 5 nm to 15 nm.
[0055] As quantum dots, publicly available quantum dots, such as CdSeS / ZnS alloyed quantum dots product numbers 753793, 753777, 753785, 753807, 753750, 753742, 753769, 753866, InP / ZnS quantum dots product numbers 776769, 776750, 776793, 776777, 776785, PbS core type quantum dots product numbers 747017, 747025, 747076, 747084, or CdSe / ZnS alloyed quantum dots product numbers 754226, 748021, 694592, 694657, 694649, 694630, 694622 from Sigma-Aldrich, may be used as desired. In another preferred embodiment of the present invention, the nanosized luminescent material is a semiconducting luminescent nanoparticle having a core-shell structure, in which a core is surrounded by one or more shell layers.
[0056] According to the present invention, the one or more shell layers of the semiconducting luminescent nanoparticles are preferably a single shell layer, a double shell layer, or a multishell layer having two or more shell layers, and most preferably it is a double shell layer. As used herein, the term "shell layer" refers to a structure that completely or partially covers the core. Preferably, the one or more shell layers completely cover the core. The terms "core" and "shell" are well known in the art and are typically used in the field of quantum materials, such as US 8221651 B2. According to the present invention, the core of semiconducting luminescent nanoparticles can be modified. For example, CdS, CdSe, CdTe, ZnS, ZnSe, ZnSeS, ZnTe, ZnO, GaAs, GaP, GaSb, HgS, HgSe, HgSe, HgTe, InAs, InP, InPS, InPZnS, InPZn, InPGa, InSb, AlAs, AlP, AlSb, Cu2S, Cu2Se, CuInS2, CuInSe2, Cu2(ZnSn)S4, Cu2(InGa)S4, TiO2 alloy, and any combination thereof can be used.
[0057] In a preferred embodiment of the invention, the core of the semiconducting luminescent nanoparticle comprises one or more elements from group 13 of the periodic table and one or more elements from group 15 of the periodic table, such as GaAs, GaP, GaSb, InAs, InP, InPS, InPZnS, InPZn, InPGa, InSb, AlAs, AlP, AlSb, CuInS2, CuInSe2, Cu2(InGa)S4, and any combination thereof. Even more preferably, the core comprises In and P atoms, for example InP, InPS, InPZnS, InPZn or InPGa.
[0058] According to a further preferred embodiment of the invention, at least one of the shell layers comprises a first element from group 12, 13 or 14 of the periodic table and a second element from group 15 or 16 of the periodic table. Preferably, all shell layers comprise a first element from group 12, 13 or 14 of the periodic table and a second element from group 15 or 16 of the periodic table. More preferably, at least one of the shell layers comprises a first element from group 12 of the periodic table and a second element from group 16 of the periodic table. For example, CdS, CdZnS, ZnS, ZnSe, ZnSSe, ZnSSeTe, CdS / ZnS, ZnSe / ZnS or ZnS / ZnSe shell layers may be used. Even more preferably, all shell layers comprise a first element from group 12 of the periodic table and a second element from group 16 of the periodic table.
[0059] Particularly preferably, at least one shell layer has the formula (5): ZnS x Se y Te z, Formula (5) wherein 0≦x≦1, 0≦y≦1, 0≦z≦1, and x+y+z=1, and even more preferably 0≦x≦1, 0≦y≦1, z=0, and x+y=1. Most preferably, ZnS, ZnSe, ZnSeS, ZnSeSTe, CdS / ZnS, ZnSe / ZnS, ZnS / ZnSe shell layers are used.
[0060] It is further preferred that all shell layers are represented by formula (5).For example, as core-shell semiconducting luminescent nanoparticles for green and / or red emission applications, CdSe / CdS, CdSeS / CdZnS, CdSeS / CdS / ZnS, ZnSe / CdS, CdSe / ZnS, InP / ZnS, InP / ZnSe, InP / ZnSe / ZnS, InP / ZnS / ZnSe, InPZn / ZnS, InPZn / ZnSe / ZnS, InPZn / ZnS / ZnSe, ZnSe / CdS, ZnSe / ZnS semiconducting luminescent nanoparticles or any combination thereof may be used. More preferably, InP / ZnS, InP / ZnSe, InP / ZnSe / ZnS, InP / ZnS / ZnSe, InPZn / ZnS, InPZn / ZnSe / ZnS, InPZn / ZnS / ZnSe may be used.
[0061] In a preferred embodiment of the present invention, the shell layer of the semiconducting luminescent nanoparticles is a double shell layer. The semiconducting luminescent nanoparticles are publicly available, e.g., from Sigma-Aldrich, and / or are described, e.g., in ACS Nano, 2016, 10 (6), pp 5769-5781, Chem. Mater. 2015, 27, 4893-4898, and International Patent Application No. WO 2010 / 095140 A2. Preferably, the nano-sized luminescent materials, such as quantum rods and / or quantum dots, include surface ligands. The surface of the quantum rod and / or quantum dot materials may be overcoated with one or more types of surface ligands.
[0062] Without wishing to be bound by theory, it is believed that such surface ligands lead to the nano-sized fluorescent material being more easily dispersible in a solvent. The wetting and dispersing agent can be attached to the surface of the ligands of the nano-sized fluorescent material, or can be attached directly to the surface of the nano-sized fluorescent material, partially or completely, using a ligand exchange process described below - Wetting and Dispersing Agents. According to the present invention, preferably the photosensitive composition is a green-type photosensitive composition containing a plurality of light-emitting nano-sized light-emitting materials capable of emitting green visible light, a red-type photosensitive composition comprising a plurality of nano-sized light-emitting materials capable of emitting red visible light, or a white-type photosensitive composition containing a plurality of different kinds of nano-sized light-emitting materials, such as a mixture of a light-emitting nano-sized light-emitting material capable of emitting green visible light and a nano-sized light-emitting material capable of emitting red visible light.
[0063] -Photopolymerization initiator According to an embodiment of the present invention, the photosensitive composition preferably further comprises a polymerization initiator, and thus functions as a negative-type photosensitive composition. The polymerization initiator used in the present invention is preferably a photoinitiator. In general, photoinitiators or photoinitiators, the terms used interchangeably herein, are a type of polymerization initiator that generates an acid, a base, or a radical when exposed to radiation. The polymerization initiator that can be used in the present invention is, for example, a photoacid generator that releases an acid that decomposes when exposed to radiation and acts as an active material for photocuring the composition, a photoradical generator that releases a radical, or a photobase generator that releases a base.Examples of radiation include visible light, UV rays, infrared rays, X-rays, electron beams, a-rays, and y-rays.It is particularly preferable to use a photoradical generator.
[0064] The optimum amount of polymerization initiator depends on the type of active substance released from the decomposed initiator, the amount of substance released, the sensitivity required, and the dissolution contrast between exposed and unexposed areas. In a preferred embodiment of the present invention, the amount of polymerization initiator ranges from 0.001 to 10 parts by weight, more preferably from 0.01 to 5 parts by weight, based on 100 parts by weight of (meth)acrylic polymer. More than 0.001 parts by weight is preferred to achieve better dissolution contrast between exposed and unexposed areas and to obtain the effect of initiator. On the other hand, less than 10 parts by weight of polymerization initiator is preferred to prevent cracking of the produced color conversion film or coloring of the produced film caused by decomposition of initiator, and to achieve good durability of coating against photoresist remover.
[0065] Examples of the photoacid generator include a diazomethane compound, a diphenyliodonium salt, a triphenylsulfonium salt, a sulfonium salt, an ammonium salt, a phosphonium salt and a sulfonamide compound. The structure of the photoacid generator can be represented by formula (A). R + X - (A) In the formula, R + is a hydrogen or an organic ion modified by carbon or other heteroatoms, where the organic ion is selected from the group consisting of alkyl, aryl, alkenyl, acyl, and alkoxy groups. For example, R + is a diphenyliodonium ion or a triphenylsulfonium ion.
[0066] In addition, X - is preferably of the formula SbYe - , AsYe - , R a p PY 6-p - , R a q BY 4-q - , R a q Gay 4-q - , R a SO3 - , (R a SO2)3C -, R a COO - , and SCN - , During the ceremony, Y is a halogen atom; R a is an alkyl group of 1 to 20 carbon atoms or an aryl group of 6 to 20 carbon atoms, each of which is substituted with a substituent selected from the group consisting of fluorine, nitro, and cyano; R b is hydrogen or an alkyl group of 1 to 8 carbon atoms; p is a number from 0 to 6, and q is a counter ion represented by any of the numbers from 0 to 4.5.
[0067] A specific example of a counterion is BF4 - , (C6F5)4B - , ((CF3)2C6H3)4B - , PF6 - , (CF3CF2)3PF3 - , SbF6 - , (C6F5)4Ga - , ((CF3)2C6H3)4Ga - , SCN - , (CF3SO2)3C - , (CF3SO2)2N - , formate ion, acetate ion, trifluoromethanesulfonate ion, nonafluorobutanesulfonate ion, methanesulfonate ion, butanesulfonate ion, benzenesulfonate ion, p-toluenesulfonate ion, and sulfonate ion.
[0068] Among the photoacid generators usable in the present invention, those that generate sulfonic acid or boric acid are particularly preferred, examples of which include tricumyl iodonium tetrakis(pentafluorophenyl)-borate (PHOTOINITIATOR 2074 [trademark], manufactured by Rhodorsil), diphenyl iodonium tetra(perfluorophenyl)borate, and compounds having sulfonium and pentafluoroborate ions as the cation and anion moieties, respectively. In addition, examples of photoacid generators also include triphenylsulfonium trifluoromethanesulfonate, triphenylsulfonium camphorsulfonate, triphenylsulfonium tetra(perfluorophenyl)borate, 4-acetoxyphenyldimethylsulfonium hexafluoroarsenate, 1-(4-n-butoxynaphthalen-1-yl)tetrahydrothiophenium trifluoro-methanesulfonate, 1-(4,7-dibutoxy-1-naphthalenyl)tetrahydrothiophenium trifluoro-methanesulfonate, diphenyliodonium trifluoromethanesulfonate, and diphenyliodonium hexafluoroarsenate. [ka] During the ceremony,
[0069] each A is independently a substituent selected from the group consisting of an alkyl group of 1 to 20 carbon atoms, an alkoxy group of 1 to 20 carbon atoms, an aryl group of 6 to 20 carbon atoms, an alkylcarbonyl group of 1 to 20 carbon atoms, an arylcarbonyl group of 6 to 20 carbon atoms, a hydroxyl group, and an amino group; Each p is independently an integer from 0 to 5, and B - is a fluorinated alkylsulfonate group, a fluorinated arylsulfonate group, a fluorinated alkylborate group, an alkylsulfonate group or an arylsulfonate group; It is also possible to employ a photoacid generator represented by the formula:
[0070] It is also possible to use photoacid generators in which the cations and anions of the above formula are exchanged with each other or are combined with various other cations and anions of the above formula.For example, any one of the sulfonium ions of the above formula can be combined with tetra(perfluorophenyl)borate ion, and any one of the iodonium ions of the above formula can be combined with tetra(perfluorophenyl)borate ion.They can also be employed as photoacid generators.
[0071] Examples of the photoradical generator include azo compounds, peroxides, acylphosphine oxides, alkylphenones, oxime esters, and titanocenes. According to the present invention, as the photoradical generator, acylphosphine oxides, alkylphenones, oxime esters, or any combination thereof are more preferred. Examples of preferred initiators are 2,2-dimethxye-1,2-diphenylethane-1-one, 1-hydroxy-cyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, 1-[4-(2-hydroxyethoxy)phenyl]-2-hydroxy-2-methyl-1-propan-1-one, 2-hydroxy-1-{4-[4-(2-hydroxy-2-methylpropionyl)benzyl]phenyl}-2-methylpropan-1-one, 2-methyl-1-(4-methylthiophenyl)-2-morpholinopropan-1-one, 2-benzyl -2-dimethylamino-1-(4-morpholinophenyl)-1-butanone, 2-(dimethylamino)-2-[(4-methylphenone)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, 1,2-octanedione 1-[4-(phenylthio)-2-(o-benzoyloxime)], ethanone 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-1-(o-acetyloxime) or any combination thereof may be preferably used. Particularly preferably, as photoradical generators, oxime esters such as 1,2-octanedione 1-[4-(phenylthio)-2-(o-benzoyloxime)], ethanone 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-1-(o-acetyloxime) (available as Irgacure® Oxe01 and Irgacure® Oxe02, respectively, from BASF) or Irgacure® Oxe03 (from BASF), or any combination thereof, are used.
[0072] Examples of photobase generators include polysubstituted amide compounds, lactams, imide compounds, and compounds having these structures.Examples of the above-mentioned thermal base generators include imidazole derivatives such as N-(2-nitrobenzyloxycarbonyl)imidazole, N-(3-nitrobenzyloxycarbonyl)imidazole, N-(4-nitrobenzyloxycarbonyl)imidazole, N-(5-methyl-2-nitrobenzyloxycarbonyl)imidazole, and N-(4-chloro-2-nitro-benzyloxycarbonyl)imidazole, 1,8-diazabicyclo(5,4,0)undecene-7, tertiary amines, quaternary ammonium salts, and mixtures thereof.These base generators and acid generators and / or radical generators can be used alone or in mixtures.
[0073] In accordance with an embodiment of the present invention, polymerization initiators that generate acids, bases, or radicals when exposed to radiation can be used. Thus, in a preferred embodiment of the present invention, the polymerization initiator may be selected from the group consisting of a photoradical generator, a photobase generator, a photoacid generator, and any combination thereof.
[0074] More preferably, the polymerization initiator is a photoradical generator, and most preferably an oxime ester. Preferred examples of oxime ester photoradical generators are listed above. -Dispersing and Wetting Agent It is further preferred, according to the invention, if the composition further comprises a wetting and dispersing agent, preferably comprising an anchor group selected from phosphine groups, phosphine oxide groups, phosphate groups, phosphonate groups, thiol groups, tertiary amine groups, carboxyl groups, heterocyclic groups, silane groups, sulfonic acid, hydroxyl groups and phosphonic acid. Examples of such preferred wetting and dispersing agents are disclosed, for example, in WO 2007 / 054898 A1.
[0075] In a preferred embodiment of the invention, the anchor groups of the wetting and dispersing agents may be selected from the group consisting of tertiary amines, phosphine oxide groups, phosphonic acids, and phosphate groups. More preferably, to avoid dark reactions, the anchor group is represented by the following chemical formula (6): -NR 11 R 21 Formula (6) In the formula, R 11 is a hydrogen atom, an alkyl group having 1 to 30 carbon atoms, or an aryl group having 1 to 30 carbon atoms, and R 22 is a hydrogen atom, an alkyl group having 1 to 30 carbon atoms, or an aryl group having 1 to 30 carbon atoms, and R 11 and R 21 may be the same or different from each other, and may be a tertiary amine represented by
[0076] Even more preferably, R 11 is an alkyl group having 1 to 30 carbon atoms, R 21 is an alkyl group having 1 to 30 carbon atoms, R 11 and R 21 may be the same or different from each other. Even more preferably, R 11 is a methyl group, an ethyl group, an n-propyl group, or an n-butyl group, and R 21 is a methyl group, an ethyl group, an n-propyl group, or an n-butyl group.
[0077] In a further preferred embodiment of the present invention, the wetting and dispersing agent is a copolymer selected from the group consisting of graft copolymers, block copolymers, alternating copolymers, and random copolymers. More preferably, the copolymer comprises a polymer unit A which includes an anchor group as defined above, and a polymer unit B which does not include any anchor group. Even more preferably, the copolymer has the following formula (7) or (8): A n -B mFormula (7) B o -A n -B m Formula (8) wherein in formulas (7) and (8), the symbol "A" represents a polymer unit A that includes an anchor group, the symbol "B" represents a polymer unit B that does not include any anchor group, and each of the symbols "n," "m," and "o" is an integer. Preferably, the polymer unit B of the wetting and dispersing agent comprises a polymer chain selected from the group consisting of polyethylene glycol, polyester, polylactic acid, polyvinyl alcohol, polyvinylpyrrolidone, cellulose, and any derivatives thereof. More preferably, the polymer chain of polymer unit B is a polyethylene glycol.
[0078] According to the present invention, the weight-average molecular weight of the wetting and dispersing agent is not particularly limited. From the viewpoint of better dispersibility and film strength, preferably it is in the range of 2,000-100,000, more preferably it is in the range of 5,000-30,000. According to the present invention, the molecular weight M w is determined using GPC (=gel permeation chromatography) against a polystyrene internal standard.
[0079] -solvent According to a further aspect of the present invention, the composition may further comprise a solvent.According to the present invention, a wide variety of publicly known solvents can be preferably used.As long as it can uniformly dissolve or disperse the above-mentioned (meth)acrylic polymer, polymerization initiator, and any additives incorporated, the solvent is not particularly limited.
[0080] In a preferred embodiment of the invention, the solvent is an ethylene glycol monoalkyl ether such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, and ethylene glycol monobutyl ether; a diethylene glycol dialkyl ether such as diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dipropyl ether, and diethylene glycol dibutyl ether; an ethylene glycol alkyl ether acetate such as methyl cellosolve acetate and ethyl cellosolve acetate; a propylene glycol monomethyl ether acetate (PGMEA), a propylene glycol monoethyl ... The solvent may be selected from the group consisting of propylene glycol alkyl ether acetates such as propylene glycol monoethyl ether acetate and propylene glycol monopropyl ether acetate; aromatic hydrocarbons such as benzene, toluene and xylene; ketones such as methyl ethyl ketone, acetone, methyl amyl ketone, methyl isobutyl ketone and cyclohexanone; alcohols such as ethanol, propanol, butanol, hexanol, cyclohexanol, ethylene glycol and glycerin; esters such as ethyl 3-ethoxypropionate, methyl 3-methoxypropionate and ethyl lactate; and cyclic esters such as gamma-butyrolactone. These solvents may be used alone or in combination of two or more, and the amount depends on the coating method and the thickness of the coating.
[0081] More preferably, a propylene glycol alkyl ether acetate such as propylene glycol monomethyl ether acetate (hereinafter "PGMEA"), propylene glycol monoethyl ether acetate, or propylene glycol monopropyl ether acetate is used. Even more preferably, PGMEA is used. The amount of solvent in the composition can be freely controlled according to the method of coating the composition.For example, when the composition is spray coated, it may contain solvent in an amount of 90wt.% or more.Furthermore, when the slit coating method, which is often adopted when coating a large substrate, is carried out, the content of solvent is usually 60wt.% or more, preferably 70wt.% or more.
[0082] - A chemical compound containing two or more (meth)acryloyl groups According to a preferred embodiment of the present invention, the composition, preferably the photosensitive composition, further comprises a chemical compound that includes two or more (meth)acryloyl groups. According to the present invention, the term "(meth)acryloyl group" is meant as a generic term for acryloyl and methacryloyl groups.
[0083] Chemical compounds containing two or more (meth)acryloyl groups can react with the (meth)acrylic polymer to create a crosslinked structure. Preferably, the chemical compound contains more than three or even four (meth)acryloyl groups to create a higher dimensional crosslinked structure with the (meth)acrylic polymer.
[0084] As an example of a chemical compound that includes two or more (meth)acryloyl groups, an ester formed by reacting a polyol with two or more (meth)acrylic acids is preferably used in the present invention. According to the present invention, the polyol has a basic structure selected from the group consisting of saturated or unsaturated aliphatic hydrocarbons, aromatic hydrocarbons, heterocyclic hydrocarbons, primary, secondary or tertiary amines, and ethers, and has two or more hydroxyl groups as substituents. The polyol of the present invention may further include one or more additional substituents such as a carboxyl group, a carbonyl group, an amino group, an ether bond, a thiol group, and a thioether bond, as long as the effect of the present invention is not impaired. Preferred examples of polyol compounds include alkyl polyols, aryl polyols, polyalkanolamines, cyanuric acid, and dipentaerythritol. When the polyol compound has three or more hydroxyl groups, it is not necessary for all hydroxyl groups to react with (meth)acrylic acid, and therefore the compound may be partially esterified. In other words, the ester may have unreacted hydroxyl groups. Examples of the ester include tris(2-acryloxyethyl)isocyanate, dipentaerythritol hexa(meth)acrylate, tripentaerythritol octa(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipropylene glycol diacrylate, tripropylene glycol diacrylate, trimethylolpropane triacrylate, polytetramethylene glycol dimethacrylate, trimethylolpropane trimethacrylate, ditrimethylolpropane tetraacrylate, tricyclodecane dimethanol diacrylate, 1,9-nonanediol diacrylate, 1,6-hexanediol diacrylate, and 1,10-decanediol diacrylate. Among the above, tris(2-acryloxyethyl)isocyanate and dipentaerythritol hexaacrylate are preferred in terms of reactivity and the number of crosslinkable groups. These compounds may be used in combination of two or more thereof to control the shape of the pattern formed. For example, a compound having three (meth)acryloyloxy groups can be employed in combination with one having two (meth)acryloyloxy groups.
[0085] From the point of view of reactivity, the above compounds are preferably molecular, preferably with a molecular weight of 2000 or less, more preferably 1500 or less. As publicly available functional acrylates, preferably difunctional acrylates, polyfunctional acrylates, such as A-DOD, A-DCP, and / or A-9300 (from Shin-Nakamura Chemical Co., Ltd.), may be used alone or in mixtures. In a further preferred embodiment of the present invention, the amount of chemical compound containing two or more (meth)acryloyl groups ranges from 0.001 to 90 parts by weight, based on 100 parts by weight of (meth)acrylic polymer, more preferably from 3 to 60 parts by weight, in order to achieve better solubility with other polymers used in the composition of the present invention. Even more preferably, it ranges from 5 to 50 parts by weight, based on 100 parts by weight of (meth)acrylic polymer.
[0086] - Scattering particles and / or refractive index adjusting materials In accordance with an embodiment of the present invention, the composition may further comprise an additive selected from scattering particles, refractive index adjusting materials, and any combination thereof. According to the present invention, as light-scattering particles, any type of publicly known light-scattering particles that contain said light-scattering particles and have a refractive index different from that of the matrix material of the layer that can provide the Mie scattering effect may be preferably used as desired. For example, small particles of inorganic oxides such as SiO2, SnO2, CuO, CoO, Al2O3, TiO2, Fe2O3, Y2O3, ZnO, MgO, etc.; organic particles such as polymerized polystyrene, polymerized PMMA, etc.; inorganic hollow oxides such as hollow silica, or any combination thereof may be preferably used. The aforementioned light scattering particles may be used as a refractive index adjusting material.
[0087] Preferably, the average particle size of the light scattering particles and / or the refractive index adjusting material is in the range of 350 nm to 5 μm, more preferably 500 nm to 2 μm. Without wishing to be bound by theory, it is believed that an average particle size of more than 350 nm may lead to strong forward scattering, which is subsequently caused by Mie scattering, even if the difference in refractive index between the light scattering particles and the layer matrix is as small as 0.1. On the other hand, in order to obtain better layer formation properties by using light scattering particles, the maximum average particle size is preferably 5 μm.
[0088] -Coloring agent Furthermore, coloring agent can be incorporated into the composition of the present invention according to need.Various known organic and inorganic coloring agents can be adopted, but inorganic coloring agents are preferred from the viewpoint of heat durability.Examples thereof include carbon black, titanium black pigment, iron oxide pigment, and complex metal oxide pigment. The amount of the colorant is preferably 0.1 to 50 parts by weight based on 100 parts by weight in the total of (meth)acrylic polymer. If it is less than 0.1 parts by weight, sufficient light-shielding effect cannot be obtained. On the other hand, if it is more than 50 parts by weight, the light-shielding effect becomes too large and the photosensitive material cannot be exposed sufficiently to obtain a pattern.
[0089] -Other additives The composition of the present invention may contain other additives, if necessary. Examples of additives include developer dissolution promoters, descumming agents, adhesion promoters, polymerization inhibitors, antifoaming agents, surfactants and sensitizers.
[0090] The developer dissolution promoter or scum remover functions to control the solubility of the coating formed in the developer and thereby prevent scum from remaining on the substrate after development. Crown ethers can be employed as this additive. The crown ethers having the simplest structure have the general formula (-CH2-CH2-O-) nAmong them, in the present invention, crown ethers of the formula where n is 4 to 7 are preferably used. Meanwhile, crown ethers are often individually referred to as "x-crown-y-ethers", where x and y respectively represent the total number of atoms forming the ring and the number of oxygen atoms contained therein. In the present invention, the additive may preferably be selected from the group consisting of crown ethers with X=12, 15, 18 and 21 and y=x / 3, their benzocondensation products, and their cyclohexylcondensation products. Preferred examples of crown ether include 2-crown-7-ether, 18-crown-6-ether, 15-crown-5-ether, 12-crown-4-ether, dibenzo-21-crown-7-ether, dibenzo-18-crown-6-ether, dibenzo-15-crown-5-ether, dibenzo-12-crown-4-ether, dicyclohexyl-21-crown-7-ether, dicyclohexyl-18-crown-6-ether, dicyclohexyl-5-crown-5-ether, and dicyclohexyl-12-crown-4-ether. Among them, it is particularly preferred to select an additive selected from the group consisting of 18-crown-6-ether and 15-crown-5-ether. The amount is preferably 0.05 to 15 parts by weight, more preferably 0.1 to 10 parts by weight, based on 100 parts by weight of (meth)acrylic polymer.
[0091] The adhesion promoter has a function of preventing the pattern from peeling off due to stress applied after curing when a cured film is formed from the photosensitive composition of the present invention. It is preferable to adopt imidazole and silane coupling agent as the adhesion promoter. Examples of imidazole include 2-hydroxybenzimidazole, 2-hydroxyethylbenzimidazole, benzimidazole, 2-hydroxyimidazole, imidazole, 2-mercaptoimidazole, and 2-aminoimidazole. Among them, 2-hydroxybenzimidazole, benzimidazole, 2-hydroxyimidazole, and imidazole are particularly preferred.
[0092] As the silane coupling agent, known compounds such as epoxy-silane coupling agents, amino-silane coupling agents and mercapto-silane coupling agents can be preferably adopted. Examples include 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-ureidopropyltrimethoxysilane, 3-chloropropyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, and 3-isocyanatopropyltrimethoxysilane. They can be used alone or in combination of two or more. The amount is preferably from 0.05 to 15 parts by weight based on 100 parts by weight of (meth)acrylic polymer. Further compounds which can be used as silane coupling agents, in particular silane or siloxane compounds having acidic groups, are disclosed in WO 2017 / 054898 A1.
[0093] As polymerization inhibitors, nitrone derivatives, nitroxide radical derivatives, and hydroquinone derivatives such as hydroquinone, methylhydroquinone, and butylhydroquinone can be incorporated. They can be used alone or in combination of two or more. The amount is preferably from 0.1 to 10 parts by weight based on 100 parts by weight of (meth)acrylic polymer.
[0094] Examples of defoamers are alcohols (C1-C 18), higher fatty acids such as oleic acid and stearic acid, higher fatty acid esters such as glycerol monolaurate, polyethers such as polyethylene glycol (PEG) (Mn: 200-10000) and polypropylene glycol (Mn: 200-10000), silicone compounds such as dimethyl silicone oil, alkyl-modified silicone oil, and fluorosilicone oil, and organosiloxane surfactants described in detail below. They may be used alone or in combination of two or more. The amount is preferably from 0.1 to 3 parts by weight based on 100 parts by weight of the (meth)acrylic polymer.
[0095] If necessary, the photosensitive composition of the present invention may further contain a surfactant incorporated for the purpose of improving coatability, developability, etc. Surfactants that can be used in the present invention include, for example, nonionic, anionic and amphoteric surfactants. Examples of nonionic surfactants include polyoxyethylene alkyl ethers such as polyoxyethylene lauryl ether, polyoxyethylene oleyl ether, and polyoxyethylene cetyl ether; polyoxyethylene fatty acid diethers; polyoxyethylene fatty acid monoethers; polyoxyethylene-polyoxypropylene block polymers; acetylene alcohol; acetylene glycol derivatives such as acetylene glycol, polyethoxylates of acetylene alcohol, and polyethoxylates of acetylene glycol; silicon-containing surfactants such as Fluorad (trademark, manufactured by Sumitomo 3M Limited), MEGAFAC (trademark, manufactured by DIC Corporation), and Surufuron (trademark, manufactured by Asahi Glass Co., Ltd.); and organosiloxane surfactants such as KP341 (trademark, manufactured by Shin-Etsu Chemical Co., Ltd.). Examples of the acetylene glycol include 3-methyl-1-butyn-3-ol, 3-methyl-1-pentyn-3-ol, 3,6-dimethyl-4-octyne-3,6-diol, 2,4,7,9-tetramethyl-5-decyne-4,7-diol, 3,5-dimethyl-1-hexyne-3-ol, 2,5-dimethyl-3-hexyne-2,5-diol, and 2,5-dimethyl-2,5-hexanediol.
[0096] Examples of anionic surfactants include ammonium salts and organic amine salts of alkyl diphenyl ether disulfonic acids, ammonium salts and organic amine salts of alkyl diphenyl ether sulfonic acids, ammonium salts and organic amine salts of alkyl benzene sulfonic acids, ammonium salts and organic amine salts of polyoxyethylene alkyl ether sulfates, and ammonium salts and organic amine salts of alkyl sulfates.Furthermore, examples of amphoteric surfactants include 2-alkyl-N-carboxymethyl-N-hydroxyethyl imidazolium betaine, and lauric acid amidopropyl hydroxysulfone betaine.
[0097] These surfactants may be used alone or in combination of two or more thereof. The amount of the surfactant is usually from 50 to 300,000 ppm, preferably from 100 to 200,000 ppm, based on the photosensitive composition of the present invention. Optionally, a sensitizer can be further incorporated into the photosensitive composition of the present invention. Examples of sensitizers preferably used in the composition of the present invention include coumarin, ketocoumarin, their derivatives, thiopyrylium salts, and acetophenone.Specific examples include p-bis(o-methylstyryl)benzene, 7-dimethylamino-4-methylquinolone-2,7-amino-4-methylcoumarin, 4,6-dimethyl-7-ethylaminocoumarin, 2-(p-dimethylaminostyryl)pyridyl methyl iodide, 7-diethylaminocoumarin, 7-diethylamino-4-methylcoumarin, 2,3,5,6-1H,4H-tetrahydro-8-methylquinolizino-<9,9a,1-gh>coumarin, 7-diethylamino-4-trifluoromethylcoumarin, 7-dimethylamino-4-trifluoromethylcoumarin, 7-amino-4-trifluoromethylcoumarin, 2,3,5,6-1H,4H-tetrahydroquinolizino-<9,9a,1-gh>coumarin, 7-ethylamino-4-trifluoromethyl ... sensitizing dyes such as styrylamino-6-methyl-4-trifluoromethylcoumarin, 7-ethylamino-4-trifluoromethylcoumarin, 2,3,5,6-1H,4H-tetrahydro-9-carboethoxyquinolizino-<9,9a,1-gh>coumarin, 3-(2'-N-methyl-benzimidazolyl)-7-N,N-diethylaminocoumarin, N-methyl-4-trifluoromethylpiperidino-<3,2-g>coumarin, 2-(p-dimethylaminostyryl)benzo-thiazolylethyl iodide, 3-(2'-benzimidazolyl)-7-N,N-diethylaminocoumarin, 3-(2'-benzothiazolyl)-7-N,N-diethylaminocoumarin, and pyrylium or thiopyrylium salts represented by the following formula:
[0098] The sensitizing dye can be used for patterning using an inexpensive light source such as a high-pressure mercury lamp (360 to 430 nm). The amount of the sensitizing dye is preferably 0.05 to 15 parts by weight, more preferably 0.1 to 10 parts by weight, based on 100 parts by weight of the (meth)acrylic polymer.
[0099] [ka] As the sensitizer, it is possible to employ, for example, a compound having an anthracene skeleton as disclosed in WO2012 / 059931 A1 or JP3820633 B. When the sensitizer having an anthracene skeleton is added, the amount is preferably 0.01 to 5 parts by weight based on 100 parts by weight of the (meth)acrylic polymer. Furthermore, if necessary, stabilizers may also be added to the composition of the present invention. The stabilizers may be freely selected from those generally known. However, in the present invention, aromatic amines are preferred because they have a high stabilizing effect. Among these aromatic amines, pyridine derivatives are preferred, and pyridine derivatives having bulky substituents at 2-position and 6-position are particularly preferred. Specific examples are as follows: [ka]
[0100] Furthermore, according to the need, a crosslinking agent may be incorporated into the composition of the present invention. Examples of crosslinking agents include melamine or isocyanate compounds with methylol or alkoxymethyl groups. Specific examples of melamine compounds include NIKAKAC NW-390, NW-100LM, MX-750LM, MX-270, and MX-280 with imino, methylol, or methoxymethyl groups. Specific examples of isocyanate compounds include X-12-9659, or KBM-9659, and X-12-9659, or KBM-585 (trademark, manufactured by Shin-Etsu Chemical Co., Ltd.). Polymers including these structures, which may be partially substituted with silicone groups, are also preferred.
[0101] The amount of crosslinking agent is 0 to 50 parts by weight, preferably 2 to 50 parts by weight, more preferably 5 to 20 parts by weight, based on 100 parts by weight of (meth)acrylic polymer. When it is 5 parts by weight or more, the resolution can be sufficiently improved. On the other hand, when it is 50 parts by weight or less, there is little concern that the gap in the pattern is filled and the resolution is reduced. As the crosslinking agent, the above-mentioned compound can be used alone or in a mixture of two or more.
[0102] The photosensitive composition according to the present invention comprises at least one nano-sized luminescent material, and a (meth)acrylic polymer comprising at least one (meth)acrylic structural unit containing an acryloyl group as defined herein, and preferably an oxime ester type photoinitiator, a dispersing agent, or a wetting agent, and a chemical compound containing two or more (meth)acryloyl groups, and can advantageously achieve highly crosslinked film production even at low UV exposure doses acceptable for mass production processes, and high resolution patterning using conventional photolithography techniques. Without being bound by any theory, it is believed that the photosensitive composition defined in the present invention can induce effective radical transport and achieve more in-depth polymerization.
[0103] Therefore, sufficient polymerization can be achieved even with low UV exposure dose. Due to the low UV dose, the quantum material of the quantum material-doped film can advantageously maintain high quantum yield in optical media. Furthermore, the photosensitive composition according to the present invention preferably allows the formation of a highly crosslinked polymer surface, which increases the solvent resistance and chemical durability of the cured film, especially when a topcoat material is applied to the film.
[0104] -use One or more of the problems of the present invention are also solved by the use of a (meth)acrylic polymer as defined herein, comprising at least one (meth)acrylic structural unit comprising an acryloyl group as represented by chemical formula (1), in a composition comprising at least one nano-sized light-emitting material, preferably said composition is a photosensitive composition. The nanosized luminescent materials included in such photosensitive compositions can be as defined herein.
[0105] The photosensitive composition may further comprise one or more of a photoinitiator, a wetting or dispersing agent, a solvent, a chemical compound that includes two or more (meth)acryloyl groups, scattering particles, and a refractive index adjusting material, each of which is as defined herein. The (meth)acrylic polymer may further comprise one or more (meth)acrylic structural units selected from formulas (2), (3), and (4), as defined herein. The present invention also relates to the use of a photosensitive composition comprising at least one nanosized luminescent material and a (meth)acrylic polymer as defined herein in a process for producing an optical medium. The optical medium according to the present invention is preferably an optical film, such as a color filter, a color conversion film, a remote phosphor tape, or another film or filter. In accordance with the present invention, the term "film" encompasses structures such as "layer" and "sheet."
[0106] -Manufacturing method The present invention further relates to a method comprising the steps of: a) and b) a) providing a photosensitive composition to a substrate; and b) polymerizing the photosensitive composition by exposing the photosensitive composition to radiation; The present invention relates to a method for preparing an optical medium, comprising, in order:
[0107] According to the present invention, to provide the photosensitive composition on the substrate according to step a), any type of publicly known coating method can be preferably used, such as dip coating, gravure coating, roll coating, bar coating, brush coating, spray coating, doctor coating, flow coating, spin coating, and slit coating. In step a), the substrate to be coated with the composition is also not particularly limited and can be appropriately selected from, for example, a silicon substrate, a glass substrate, and a polymer or resin film. The substrate can be solid or flexible, and transparent or non-transparent.
[0108] In a preferred embodiment of the present invention, optionally after step a), a pre-baking step may be applied to the photosensitive composition provided on the substrate for the purpose of drying and reducing the solvent remaining therein. The pre-baking step may generally be performed at a temperature of 50-150° C., preferably 90-120° C., for 10-300 seconds, preferably 30-120 seconds on a hot plate, or 1-30 minutes in a clean oven. Furthermore, according to need, the step of providing the photosensitive composition on the substrate may be repeated once or more times to form a coating or film of the desired thickness.
[0109] After the coating is formed, the surface is exposed to radiation. As a source of radiation for exposure, any light source used in conventional pattern formation processes can be adopted. Examples of light sources include high pressure mercury lamps, low pressure mercury lamps, metal halide lamps, xenon lamps, semiconductor lasers, and LEDs. The light for exposure is usually g-line, h-line, i-line UV rays or the like. Except for ultra-fine production such as semiconductors, it is common to use light with a wavelength of 360 to 430 nm (high pressure mercury lamp) for patterning of several micrometers to tens of micrometers.
[0110] Especially when manufacturing liquid crystal displays, 430 nm light is often used. The energy of the exposure radiation depends on the source of radiation and the thickness of the coating, but is generally between 10 and 2000 mJ / cm to obtain a satisfactory resolution and avoid halation. 2 , preferably 20 to 1000 mJ / cm 2 It is. According to this method, there is no particular limitation on the environmental conditions in the exposure, and the exposure can be carried out under an ambient atmosphere (normal atmosphere) or a nitrogen atmosphere. When forming a film on the entire surface of a substrate, the entire surface of the substrate is exposed to radiation. In the present invention, the term "pattern film" includes the film thus formed on the entire surface of the substrate.
[0111] After the exposure step b), optionally, post-exposure baking can be performed as necessary to promote the interpolymer reaction caused by the initiator in the exposed areas of the coating. The temperature of the post-exposure baking is preferably 40-150°C, more preferably 60-120°C. The post-exposure baking step can be performed using a hot plate, an oven, a furnace or the like. The atmosphere during baking is not particularly limited. In order to control the curing speed of the composition, the atmosphere can be selected from, for example, an atmosphere of an inert gas such as nitrogen gas, a vacuum atmosphere, a reduced pressure atmosphere, an oxygen gas atmosphere, etc. The baking time is preferably 20-500 seconds, more preferably 40-300 seconds, in order to prevent the diffusion of the acid as well as to maintain a higher uniformity of the heat balance on the wafer surface.
[0112] After the exposure step b), a step c) of developing the polymeric composition, preferably the photosensitive composition, may be optionally performed. If a film is formed on the entire surface of the substrate, the development step c) may be omitted. As the developer used in the development step, any developer used in the development of conventional photosensitive compositions can be adopted. In the present invention, TMAH aqueous solutions are used to determine the dissolution rate of the photosensitive composition, but they in no way limit the developer for forming a cured film. Preferred examples of the developer include alkaline developers, which are aqueous solutions of alkaline compounds such as tetraalkylammonium hydroxide, choline, alkali metal hydroxide, alkali metal (meta)silicate (hydrate), alkali metal (meta)phosphate (hydrate), ammonia, alkylamine, alkanolamine, and heterocyclic amine. Aqueous solutions of tetraalkylammonium hydroxide are particularly preferred. These alkaline developers may contain water-soluble organic solvents, such as methanol and ethanol, or surfactants, if necessary. The development method may be freely selected from known methods such as dip, puddle, shower, slit, cap coat, and spray development processes. As a result of the development, a pattern may be obtained. After being developed with the developer, the pattern is preferably washed with water. An acetone washing process after the development step can be optionally added.
[0113] After the development step, the resulting pattern film may be optionally heated and thereby cured. The heating device used in the heating step may be the same as that used in the post-exposure baking step. The heating temperature in this heating step is not particularly limited as long as the film can be cured. Specifically, the composition is preferably cured at a temperature of 360°C or less. In order to keep the cured film at a high film ratio, the heating temperature is more preferably 300°C or less, and even more preferably 250°C or less. On the other hand, in order to promote the curing reaction and obtain a sufficiently cured film, the temperature is preferably 70°C or more, more preferably 100°C or more, and particularly preferably 110°C or more. The heating time is also not particularly limited, but is generally 10 minutes to 24 hours, preferably 30 minutes to 3 hours. Here, the "heating time" means the time from when the temperature of the pattern film rises to when the target heating temperature is reached. It usually takes several minutes to several hours to heat the pattern film from the initial temperature to the target heating temperature.
[0114] The resulting optical media can be optical films such as color filters, color conversion films, remote fluorescent tapes, or other films or filters, and can achieve improved chemical and solvent resistance, fine patterning, high quantum yield, and high OD. The present invention therefore also relates to an optical medium obtained or obtainable by the method of the invention.
[0115] Furthermore, the present invention relates to optical media formed from a composition as defined herein, preferably a photosensitive composition. The optical medium according to the present invention can be advantageously used in various applications.For example, it can be advantageously used as the material of optical elements such as optical waveguides, and as the material of various films such as planarizing films on thin film transistor (TFT) substrates used as backplanes of displays such as LCD devices or organic EL devices, interlayer insulating films in semiconductor devices, and other insulating films, or the material of solid-state image sensors, anti-reflection panels or films, optical filters, transparent protective films of high brightness LED devices, touch panels, and solar cells. Thus, the present invention also relates to the use of the optical medium in an optical device.
[0116] The present invention also relates to an optical device that includes the optical medium. The optical device of the present invention is preferably a liquid crystal display, an electroluminescent display, a microelectromechanical system (MEMS) display, an electrowetting display, and an electrophoretic display.More preferably, the optical device is a liquid crystal display, such as a twisted nematic liquid crystal display, a vertical alignment mode liquid crystal display, an IPS mode liquid crystal display, a guest-host mode liquid crystal display, or a normally black TN mode liquid crystal display.Examples of optical devices are described, for example, in WO2010 / 095140 A2 and WO2012 / 059931 A1. The present invention further relates to a method comprising the steps of: A) A) providing an optical medium to an optical device; The present invention relates to a method for preparing an optical device, comprising:
[0117] Technical effects The present invention provides one or more of the following advantages. improved polymerization at lower UV irradiation intensities, finer patterning, improved resolution of the photopattern of the composition, improved solvent damage stability of the pattern when an overcoat material is applied to the pattern, improved photoluminescence of light emitted from the luminescent material after patterning, improved quantum yield of the luminescent material after patterning and / or after an overcoat material is fabricated over the pattern, improved solvent stability, improved crosslink density of the composition after UV irradiation. The present invention will now be described in more detail with reference to the following examples, which are merely illustrative and are not intended to limit the scope of the invention.
[0118] Working Example Example 1 - Preparation of Photosensitive Composition 1 A solution of 4.32 g of UV-reactive polymer (RNUV-071, obtained from Natoco Co., Ltd.) dispersed at 40 wt.% in t-butanol and propylene glycol monomethyl ether acetate (PGMEA) is mixed with 1.976 g of hexafunctional acrylic monomer (A-DPH, obtained from Shin-Nakamura Chem.) and 0.297 g of oxime ester type photoinitiator (IrgacureOXE03, obtained from BASF). Then, 4.408 g of PGMEA is added to the mixture, and the mixture is stirred by a magnetic stirrer at room temperature for 30 minutes to obtain a UV-reactive photopolymer mixture. A solution of 0.5 g of InP-based red quantum material in CHCl3 is added dropwise to a solution of 0.53 g of dispersant (BYK-LPN22822) in CHCl3. The mixture is first stirred with a magnetic stirrer at 60°C for 18 hours and then stirred under nitrogen atmosphere at 80°C for 2 hours. Then 1.428 g of PGMEA is added to the mixture and CHCl3 is evaporated using a rotary evaporator. The solution containing 667 mg of the red quantum dot material thus obtained is then mixed with a solution containing 500 mg of the UV-reactive photosensitive polymer mixture.
[0119] Comparative Example 1 - Preparation of Photosensitive Composition 2 A solution of 19.25 g of acrylic polymer (AZHT-003, obtained from Natoco Co., Ltd.) dispersed in n-butanol and PGMEA at 40 wt.% and 19.25 g of acrylic polymer dispersed in n-butanol and PGMEA at 40 wt.% (AZHT-002, obtained from Natoco Co., Ltd.) is mixed with 7.75 g of difunctional acrylic monomer (A-DCP, obtained from Shin-Nakamura Chem.), 7.75 g of difunctional acrylic monomer (A-DOD-N, obtained from Shin-Nakamura Chem.), 24.7 g of hexafunctional monomer (A-DPH, obtained from Shin-Nakamura Chem.), and 3.7 g of oxime ester type photoinitiator (IrgacureOXE03 obtained from BASF). The polymer mixture is stirred by a magnetic stirrer at room temperature for 30 minutes. A solution of 0.5 g of InP-based red quantum material in CHCl3 is added dropwise to a solution of 0.53 g of dispersant (BYK-LPN22822) in CHCl3. The mixture is first stirred with a magnetic stirrer at 60 °C for 18 h and then stirred at 80 °C for 2 h under nitrogen atmosphere. Then 1.428 g of PGMEA is added to the mixture and CHCl3 is evaporated using a rotary evaporator. The solution thus obtained containing 500 mg of red quantum dot material is mixed with 500 mg of the solution of the polymer mixture.
[0120] Example 2 - Fabrication of patterned films A glass substrate is cleaned by ultrasonication in water with detergent. A UV-reactive solution of Photosensitive Composition 1 is then coated onto the cleaned glass substrate using a bar coating technique. The resulting film-coated substrate is heated at 100° C. for 90 seconds in air conditions to evaporate the solvent. After baking, the photosensitive composite film coated on the substrate was exposed to a 3.9 mW / cm 2 i, g, and h line emission (80 mJ / cm 2 The test subjects were exposed to a 30-μm-diameter 10-mm ... The photosensitive composite film coated on the substrate is then exposed to tetramethylammonium hydroxide (TMAH) for 30 seconds, rinsed with running water at room temperature for 10 seconds, and then heated on a hot plate at 100° C. for 90 seconds to evaporate the water. A patterned film is produced using the photosensitive composition 2 of Comparative Example 1 in the same manner and under the same conditions.
[0121] Example 3 - Solvent resistance test PGMEA is coated onto each cured resist film obtained in Example 2 by spin-coating technique at 150 rpm for 10 seconds, and the PGMEA-coated film is left for 3 minutes, after which the film is heated on a hot plate at 90° C. for 90 seconds. Measurement results of solvent resistance test by using an optical microscope equipped with a camera. Result A is an image of the appearance of the resist film doped with the quantum dot material obtained in Example 2 using UV-reactive photosensitive composition 1 after solvent resistance test. Result B is an image of the appearance of the resist film doped with the quantum dot material obtained in Example 2 using the photosensitive composition 2 after the solvent resistance test (reference).
[0122] The photoresist composite film obtained using a photosensitive composition including a UV-reactive photosensitive (meth)acrylic polymer as defined herein maintains a solid and smooth surface (Result A), whereas the photoresist composite film obtained using a photosensitive composition without a UV-reactive polymer exhibits wrinkles (Result B).
Claims
1. At least one nano-sized luminescent material, a (meth)acrylic polymer, and A composition comprising a wetting and dispersing agent, the (meth)acrylic polymer having the following chemical formula (1): 【Chemistry 1】 During the ceremony, R 1 represents, identically or differently, each occurrence of hydrogen, a straight-chain alkyl group having 1 to 20 C atoms, a branched or cyclic alkyl group having 3 to 20 C atoms, an alkenyl or alkynyl group having 2 to 20 C atoms, an aryl or heteroaryl group having 5 to 24 C atoms, in which one or more non-adjacent methylene structural units (-CH 2 -) may in each case be replaced by a sulfonyl, carbonyl, ether, sulfide, sulfoxide, ester, amide or imine group, and in which the alkyl, alkenyl, alkynyl, aryl or heteroaryl group has one or more H atoms which may be replaced by F, Cl, Br, I, CN or OH, a carboxyl group (-COOH), a straight-chain alkyl or alkoxy group having 2 to 20 C atoms, a branched alkyl or alkoxy group having 3 to 20 C atoms or an alkenyl or alkynyl group having 2 to 20 C atoms, R 2 , R 2 ' represents, identically or differently, each occurrence of hydrogen, a hydroxyl group (-OH), a carboxyl group (-COOH), a linear alkyl group having 1 to 20 C atoms, a branched or cyclic alkyl group having 3 to 20 C atoms, an alkenyl or alkynyl group having 2 to 20 C atoms, an aryl or heteroaryl group having 5 to 24 C atoms, wherein one or more non-adjacent methylene structural units (-CH 2 -) can in each case be replaced by a sulfonyl, carbonyl, ether, sulfide, sulfoxide, ester, amide, or imine group, and wherein said alkyl, alkenyl, alkynyl, aryl or heteroaryl group may have one or more H atoms replaced by F, Cl, Br, I, CN or OH, a carboxyl group (—COOH), a linear alkyl or alkoxy group having 2 to 20 C atoms, a branched alkyl or alkoxy group having 3 to 20 C atoms or an alkenyl or alkynyl group having 2 to 20 C atoms, with the proviso that the radicals R 2 and R 2 ' may also represent a carboxyl group, R 3 represents, identically or differently, each occurrence of hydrogen, a straight-chain alkyl group having 1 to 20 C atoms, a branched or cyclic alkyl group having 3 to 20 C atoms, an alkenyl or alkynyl group having 2 to 20 C atoms, an aryl or heteroaryl group having 5 to 24 C atoms, in which one or more non-adjacent methylene structural units (-CH 2 -) can in each case be replaced by a sulfonyl, carbonyl, ether, sulfide, sulfoxide, ester, amide, or imine group, and wherein said alkyl, alkenyl, alkynyl, aryl or heteroaryl group may have one or more H atoms replaced by F, Cl, Br, I, CN or OH, a carboxyl group (-COOH), a linear alkyl or alkoxy group having 2 to 20 C atoms, a branched alkyl or alkoxy group having 3 to 20 C atoms or an alkenyl or alkynyl group having 2 to 20 C atoms, R 4 are identically or differently, and each occurrence denotes a straight-chain alkylene group having 1 to 20 C atoms, a branched alkylene group having 2 to 20 C atoms, an alkenylene or alkynylene group having 2 to 20 C atoms, or an arylene or heteroarylene group having 6 to 24 C atoms, in which one or more methylene structural units (-CH 2 -) may in each case be replaced by a sulfonyl group, a carbonyl group, an ether group, a sulfide group, a sulfoxide group, an ester group, an amide group, an imine group, a CHR' group, or a CR'R'' group, R', R'' are identical or different and each occurrence represents a hydroxyl group, a linear alkyl group having 1 to 20 C atoms, a branched or cyclic alkyl group having 3 to 20 C atoms, an alkenyl or alkynyl group having 2 to 20 C atoms, an aryl or heteroaryl group having 5 to 24 C atoms, wherein one or more non-adjacent methylene structural units (-CH) in the alkyl, alkenyl, alkynyl, aryl or heteroaryl group are 2 -) may in each case be replaced by a sulfonyl, carbonyl, ether, sulfide, sulfoxide, ester, amide or imine group, and in which the alkyl, alkenyl, alkynyl, aryl or heteroaryl group is optionally one or more H atoms are optionally replaced by F, Cl, Br, I, CN or OH, a straight-chain alkyl or alkoxy group having 2 to 20 C atoms, a branched alkyl or alkoxy group having 3 to 20 C atoms or an alkenyl or alkynyl group having 2 to 20 C atoms, At least one (meth)acrylic structural unit represented by The composition, wherein the wetting and dispersing agent is a copolymer comprising anchor groups selected from phosphine groups, phosphine oxide groups, phosphate groups, phosphonate groups, thiol groups, tertiary amine groups, carboxyl groups, heterocyclic groups, silane groups, sulfonic acids, hydroxyl groups, and phosphonic acids.
2. R 1 denotes hydrogen, a straight-chain alkyl group having 1 to 10 C atoms or a branched alkyl group having 3 to 10 C atoms, and / or R 2 ' represents hydrogen or a methyl group, and R 2 denotes hydrogen, a carboxyl group, a straight-chain alkyl group having 1 to 8 C atoms, where one or more H atoms may be replaced by F, Cl, OH or a carboxyl group (-COOH), and / or R 3 denotes hydrogen, a straight-chain alkyl group having 1 to 10 C atoms or a branched alkyl group having 3 to 10 C atoms, and / or R 4 represents a linear alkylene group having 1 to 10 C atoms, a branched alkylene group having 2 to 10 C atoms, an alkenylene group having 2 to 10 C atoms, or an arylene group having 6 to 10 C atoms, wherein one or more non-adjacent methylene structural units (-CH 2 2. The composition of claim 1, wherein -) may be replaced by a sulfonyl group, a carbonyl group, an ether group, a sulfide group, a sulfoxide group, an ester group, an amide group, an imine group, a CHR' group, or a CR'R'' group.
3. The (meth)acrylic polymer is represented by the following chemical formulas (2), (3) and (4): 【Chemistry 2-1】 【Chemistry 2-2】 In the formula, the radical R 1 , R 2 and R 2’ are, for each occurrence, identically or differently, as defined in claim 1 or claim 2, R 5 denotes, identically or differently, each occurrence of a linear alkylene group having 1 to 20 C atoms, a branched alkylene group having 2 to 20 C atoms, an alkenylene or alkynylene group having 2 to 20 C atoms, or an arylene or heteroarylene group having 6 to 24 C atoms, in which one or more methylene structural units (-CH 2 -) may in each case be replaced by a sulfonyl, carbonyl, ether, sulfide, sulfoxide, ester, amide, imine, CHR' or CR'R'', where the radicals R' and R'' are as defined above, and R 6 denotes, identically or differently, each occurrence a straight-chain alkyl group having 1 to 20 C atoms, a branched alkyl group having 3 to 20 C atoms or a cyclic alkyl group having 3 to 20 C atoms, The composition according to claim 1 or 2, further comprising one or more (meth)acrylic structural units selected from:
4. R 5 represents a linear alkylene group having 1 to 10 C atoms, a branched alkylene group having 2 to 10 C atoms, or an alkenylene group having 2 to 10 C atoms, wherein one or more non-adjacent methylene structural units (-CH 2 -) may be replaced by a sulfonyl group, a carbonyl group, an ether group, a sulfide group, a sulfoxide group, an ester group, an amide group, an imine group, a group CHR', or a group CR'R'', where the radicals R' and R'' are as defined above, and / or R 6 The composition according to claim 3, wherein denotes a linear alkyl group having 1 to 10 C atoms, a branched alkyl group having 3 to 10 C atoms, or a cyclic alkyl group having 6 C atoms.
5. The composition according to any one of claims 1 to 4, wherein the weight average molecular weight of the (meth)acrylic polymer is in the range of from 2,000 to 100,000.
6. The composition according to any one of claims 1 to 5, wherein the equivalent weight of the (meth)acrylic structural unit including the acryloyl group in the (meth)acrylic polymer is in the range of 400 to 560.
7. The composition according to any one of claims 1 to 6, further comprising a photoinitiator.
8. The composition of any one of claims 1 to 7, wherein the composition further comprises a solvent.
9. The composition of any one of claims 1 to 8, wherein the composition further comprises an additive selected from scattering particles, refractive index adjusting materials, and any combination thereof.
10. The composition of any one of claims 1 to 9, wherein the composition further comprises a chemical compound that includes two or more (meth)acryloyl groups.
11. Use of a (meth)acrylic polymer comprising at least one (meth)acrylic structural unit represented by the chemical formula (1) as defined in any one of claims 1 to 6 in the composition according to any one of claims 1 to 10.
12. Use of a composition according to any one of claims 1 to 10 in a process for producing an optical medium.
13. The method comprises the steps of: a) providing a composition according to any one of claims 1 to 10 to a substrate; and b) polymerizing the composition by exposing it to radiation; A method for preparing an optical medium comprising, in order:
14. The method further comprises the steps of: c) developing the polymerized composition; 14. The method for preparing the optical medium of claim 13, further comprising:
15. An optical medium formed from a composition according to any one of claims 1 to 10 or obtained by a method according to claims 13 or 14.
16. Use of the optical medium of claim 15 in an optical device.
17. 16. An optical device comprising the optical medium of claim 15.
18. The method comprises the steps of: A) A) providing an optical medium according to claim 15 in an optical device; A method for preparing an optical device comprising:
Citation Information
Patent Citations
Self-luminescent photosensitive resin composition, color filter prepared by using same, and image display device
WO2018093028A1