Polymers with stable cationic pendant groups for use as anion exchange membranes - Patents.com

Polymers with quaternary ammonium or phosphonium groups and nitrogen-containing heterocyclic groups, integrated into anion exchange membranes through specific polymerization and ion exchange methods, address the stability and conductivity issues of current HEMs, enhancing HEMFC performance and durability.

JP7591515B2Active Publication Date: 2024-11-28UNIVERSITY OF DELAWARE
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2021556830
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-03-28
Filing Date
2020-03-27
Publication Date
2024-11-28
Estimated Expiration
2040-03-27

AI Technical Summary

Technical Problem

Current hydroxide exchange membranes (HEMs) and ionomers (HEIs) face challenges such as poor chemical stability, low hydroxide conductivity, high water absorption, and mechanical brittleness, especially under dry conditions, which hinder their performance in hydroxide exchange membrane fuel cells (HEMFCs).

Method used

Development of polymers with structural units featuring quaternary ammonium or phosphonium groups and nitrogen-containing heterocyclic groups, combined with aromatic and crown ether monomers, to form anion exchange membranes that enhance chemical stability, conductivity, and mechanical properties, using methods like polymerization and ion exchange processes.

Benefits of technology

The resulting membranes exhibit improved chemical stability, hydroxide conductivity, reduced water absorption, and mechanical strength, enabling higher performance and durability in HEMFCs, particularly at elevated temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007591515000074
    Figure 0007591515000074
  • Figure 0007591515000075
    Figure 0007591515000075
  • Figure 0007591515000076
    Figure 0007591515000076
Patent Text Reader

Abstract

Provided are poly(aryl alkylene) polymers or poly(aryl-crown ether-alkylene) polymers containing pendant cationic groups with alkali-stable cations, such as imidazolium, incorporated into a rigid aromatic polymer backbone free of ether linkages. Hydroxide exchange membranes or hydroxide exchange ionomers formed from these polymers exhibit superior chemical stability, hydroxide conductivity, reduced water absorption, good solubility in select solvents, and improved mechanical properties under ambient dry conditions compared to conventional hydroxide exchange membranes or ionomers. Hydroxide exchange membrane fuel cells and hydroxide exchange membrane electrolyzers containing poly(aryl alkylene) polymers or poly(aryl-crown ether-alkylene) polymers with pendant cationic groups exhibit improved performance and durability at relatively high temperatures.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] Government Licensing Rights This invention was made in part with Government support under Grant DE-AR0000814 awarded by the Advanced Research Projects Agency of Energy of the U.S. Department of Energy. The Government has certain rights in this invention.

[0002] Anion exchange polymers are provided that can form anion exchange membranes (AEM) and ionomers (AEI) for use in anion exchange membrane fuel cells (AEMFC). More specifically, hydroxide exchange polymers are provided that can form hydroxide exchange membranes (HEM) and ionomers (HEI) for use in a variety of applications, such as hydroxide exchange membrane fuel cells (HEMFC) and hydroxide exchange membrane electrolyzers (HEMEL). [Background technology]

[0003] Proton exchange membrane fuel cells (PEMFCs) are considered a clean and efficient power source. Steele et al.,Nature 2001,414,345. However, the high cost and insufficient durability of the catalysts are major barriers to large-scale commercialization of PEMFCs. Borup et al.,Chem Rev 2007,107,3904. By switching the polymer electrolyte from an "acidic" to a "basic" state, HEMFCs can function with non-precious metal catalysts, which are expected to be more durable. Other cheaper fuel cell components, such as metallic bipolar plates, are also possible. Varcoe, et al.,Fuel Cells 2005,5,187; Gu et al.,Angew Chem Int Edit 2009,48,6499; Gu et al.,Chem Commun 2013,49,131. However, currently available HEM and HEI have poor alkaline / chemical stability, low hydroxide conductivity, high water absorption, and poor mechanical integrity under dry conditions, especially after wet-dry cycling.

[0004] The biggest challenge for current HEM / HEIs is achieving high chemical stability at the desired operating temperatures (e.g., in the presence of nucleophilic hydroxide ions) of 80°C or higher, ideally 95°C or higher. Varcoe et al.,Energ Environ Sci 2014,7,3135. The most commonly encountered cationic functional groups (e.g., benzyltrimethylammonium and alkyl chain ammonium) can undergo many decomposition processes in the presence of hydroxide ion nucleophiles, by direct nucleophilic substitution and Hoffman elimination. In addition, the polymer backbones of most base polymers for HEM / HEI applications (e.g., polysulfone and poly(phenylene oxide)) inevitably contain ether bonds along the backbone, which may lead to instability of HEM / HEIs under high pH conditions. Lee et al.,Acs Macro Lett 2015,4,453, Lee et al.,Acs Macro Lett 2015,4,814. Strongly nucleophilic hydroxide ions attack these weak bonds and degrade the polymer backbone. Therefore, alternative cationic groups, organic tethers, and polymer backbones are needed to enhance the chemical stability of HEM / HEI.

[0005] Another concern with current HEM / HEIs is their hydroxide conductivity. Because the mobility of OH- is lower than that of H+, HEMs have inherently lower ionic conductivity compared to Nafion under similar conditions. Hibbs et al.,Chem Mater 2008,20,2566. For HEM / HEIs to achieve higher hydroxide conductivity, a higher ion exchange capacity (IEC) is required. However, a high IEC usually leads to a membrane with high water absorption (i.e., high swelling ratio) and reduced dimensional stability and mechanical strength, especially after repeated wet-dry cycles. This highly swollen state when wet is the main reason that HEMs become less flexible and brittle when dry. Eliminating the trade-off between high hydroxide conductivity and low water absorption is a major hindrance in the design of high-performance HEM / HEIs. Pan et al.,Energ Environ Sci 2013,6,2912. Chemical cross-linking, physical reinforcement, side chain polymerization, and block copolymer structures have been attempted to reduce water absorption while maintaining acceptable hydroxide conductivity, but these techniques pose difficult challenges such as reduced mechanical flexibility, poor alkaline stability, and / or increased cost. Gu et al., Chem Commun 2011, 47, 2856; Park et al., Electrochem Solid St 2012, 15, B27; Wang et al., Chemsuschem 2015, 8, 4229; Ran et al., Sci Rep-Uk 2014, 4; Tanaka et al., J Am Chem Soc 2011, 133, 10646. Furthermore, almost all side chain or block copolymer HEMs are based on flexible aliphatic polymer chains due to limited available synthesis methods. As a result, the membranes still cannot provide shape stability (low swelling ratio) at high IEC and elevated temperatures. Wang et al.,Chemsuschem 2015,8,4229, Ran et al.,Sci Rep-Uk 2014,4, Marino et al.,Chemsuschem 2015,8,513, Li et al,M.Macromolecules 2015,48,6523.

[0006] An additional obstacle to the use of HEMs is achieving mechanical flexibility and strength at ambient dry conditions. Most HEMs have poor mechanical strength and become very brittle, especially when fully swollen and then fully dried. It is difficult to obtain and handle large thin films at the sizes required for commercial use of HEMs. Without good mechanical properties, ionomers cannot form and maintain the proper three-phase structure in fuel cell electrodes at high temperatures, such as above 80°C. Li et al., J Am Chem Soc 2013,135,10124.

[0007] Another highly desirable feature of HEIs is that the polymers are soluble in mixtures of low boiling alcohols and water, but insoluble in pure alcohol or water, so that HEIs can be easily incorporated into electrocatalyst layers and cannot be dissolved away by water or alcohol.

[0008] In recent years, PEMFCs have been deployed as zero-emission power sources in commercial vehicles, demonstrating long driving ranges and short refueling times, two features that have won them customer acceptance. However, PEMFCs use platinum electrocatalysts and are not yet cost-competitive with gasoline engines. The main approaches to reducing the cost of PEMFCs include the development of membrane electrode assemblies (MEAs) with low platinum loadings and high power densities, and platinum group metal-free (PGM-free) cathode catalysts. A fundamentally different route to low-cost fuel cells is to switch from PEMFCs to hydroxide exchange membrane fuel cells (HEMFCs), which, due to their basic operating environment, can function with PGM-free anode and cathode catalysts and are potentially economically viable. However, to replace PEMFCs, HEMFCs need to offer performance comparable to that of PEMFCs, and similarly require highly active anode and cathode catalysts as well as chemically very stable, ionic conductive, and mechanically robust hydroxide exchange membranes (HEMs) / hydroxide exchange ionomers (HEIs) with the ability to establish efficient three-phase boundaries, significantly improve catalyst particle utilization, and reduce internal resistance.

[0009] Typically, HEM / HEIs are composed of organic cations tethered to a polymer backbone, with OH- being the balancing anion. A chemically stable HEM / HEI requires a stable organic cation and a stable polymer backbone. These hydroxide-conducting organic cations have been obtained by introducing quaternary ammonium, imidazolium, guanidinium, phosphonium, sulfonium, ruthenium and cobaltocenium using chloromethylation of aromatic rings or bromination of benzylmethyl groups of the polymer. Various polymer backbone structures - poly(olefins), poly(styrene), poly(phenylene oxide), poly(phenylene), poly(arylene ether) - have been recently investigated. So far, most HEM / HEIs based on traditional cationic groups (e.g., benzyltrimethylammonium) and aromatic polymer backbones (e.g., polysulfones) have poor alkaline / chemical stability, low hydroxide conductivity, high water absorption and poor mechanical properties when dry.

[0010] Polymer backbones with ether bonds are generally weak in alkaline media, and therefore HEM / HEIs with ether-free polymer backbones are highly desirable. Acid-catalyzed hydroxylation reactions have been demonstrated to efficiently produce ether-free polymer backbones, and HEM / HEIs with such backbones have been shown to have good alkaline stability and mechanical properties. Zolotukhin et al. Chem. Comm. 2004, 1030. Diaz et al. Macromol. Rapid Commun. 2007, 28, 183. Lee et al. ACS Macro Lett. 2015, 4, 814. Bae et al. US Patent, App. 15 / 527, 967.

[0011] To further enhance the alkaline stability of HEM / HEI under both high temperature and low relative humidity, cations other than the traditional ammonium cation are highly sought. Imidazolium cations, when appropriately substituted, have shown improved alkaline stability. Gu et al. Macromolecules, 2014, 47, 208. Wang et al. ChemSusChem 2013, 6, 2079. Hugar et al. J.Am.Chem.Soc. 2015, 137, 8730. Summary of the Invention

[0012] A polymer is provided comprising structural units of formula (1A), (3A), or (3′A), and optionally (4A), wherein the structural units of formula (1A), (3A), (3′A), and (4A) have the following structure: [ka] During the ceremony, R 11 are each independently a quaternary ammonium or phosphonium group or a nitrogen-containing heterocyclic group or a salt thereof, the quaternary ammonium or phosphonium group having the formula (5A): [ka] the nitrogen-containing heterocyclic group is an optionally substituted pyrrole, pyrroline, pyrazole, pyrazoline, imidazole, imidazoline, triazole, pyridine, triazine, pyrazine, pyridazine, pyrimidine, azepine, quinoline, piperidine, pyrrolidine, pyrazolidine, imidazolidine, azepane, isoxazole, isoxazoline, oxazole, oxazoline, oxadiazole, oxatriazole, dioxazole, oxazine, oxadiazine, isoxazolidine, morpholine, thiazole, isothiazole, oxathiazole, oxathiazine, or caprolactam, each substituent being independently alkyl, alkenyl, alkynyl, aryl, or aralkyl; R 20 , R30 , R 40 , R 50 , R 60 , R 70 , R 80 , R 90 , R 130 , R 140 , R 150 , R 160 , and R 170 are each independently hydrogen, a halide, an alkyl, an alkenyl, an alkynyl, or an aryl, the alkyl, alkenyl, alkynyl, or aryl being optionally substituted with a halide; R 30 and R 60 are optionally joined to form a five-membered ring optionally substituted with halide or alkyl; Each R 100 is independently an alkyl, alkenyl, alkynyl, or a substituent having the formula (4B), [ka] The alkyl, alkenyl, or alkynyl is optionally substituted with fluoride; R 180 and R 240 are each independently alkylene; R 190 , R 200 , R 210 , R 220 , and R 230 are each independently alkyl, alkenyl, or alkynyl; q is 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, or 20; m is 0, 1, 2, 3, 4, 5, or 6; n is 0, 1, 2, or 3; each m' and each n' is independently 0, 1, or 2; X - is an anion, When structural units of formula (3A) are present in the polymer but structural units of formula (3'A) are not present in the polymer, Z is P, and when structural units of formula (3'A) are present in the polymer, Z is N or P.

[0013] A polymer comprising the reaction product of the polymerization mixture is also provided, (i) a cationically functionalized trifluoroketone monomer having the formula: [ka] (ii) an aromatic monomer having the formula: [ka] or A crown ether monomer having the formula: [ka] and (iii) optionally, a trifluoromethyl ketone monomer having the formula: [ka] During the ceremony, Each R1 is independently a quaternary ammonium or phosphonium group, or a nitrogen-containing heterocyclic group or a salt thereof, the quaternary ammonium or phosphonium group having the formula (5A): [ka] the nitrogen-containing heterocyclic group is an optionally substituted pyrrole, pyrroline, pyrazole, pyrazoline, imidazole, imidazoline, triazole, pyridine, triazine, pyrazine, pyridazine, pyrimidine, azepine, quinoline, piperidine, pyrrolidine, pyrazolidine, imidazolidine, azepane, isoxazole, isoxazoline, oxazole, oxazoline, oxadiazole, oxatriazole, dioxazole, oxazine, oxadiazine, isoxazolidine, morpholine, thiazole, isothiazole, oxathiazole, oxathiazine, or caprolactam, each substituent being independently alkyl, alkenyl, alkynyl, aryl, or aralkyl; R2, R3, R4, R5, R6, R7, R8, R9, R 10 , R 13 , R 14 , R 15 , R 16 , and R 17 are each independently hydrogen, halide, alkyl, alkenyl, alkynyl, or aryl, where alkyl, alkenyl, alkynyl, or aryl is optionally substituted with halide, and R3 and R6 are optionally joined to form a five-membered ring optionally substituted with halide or alkyl; Each R 12 is independently an alkyl, alkenyl, alkynyl, or a substituent of formula (4C); [ka] The alkyl, alkenyl, or alkynyl is optionally substituted with fluoride; R 180 and R 240 are each independently alkylene; R 190 , R 200 , R 210 , R 220 , and R 230 are each independently alkyl, alkenyl, or alkynyl; m is 0, 1, 2, 3, 4, 5, or 6; n is 0, 1, 2, or 3; each m' and each n' is independently 0, 1, or 2; q is 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, or 20; X - is an anion, When an aromatic monomer of formula (3) is present in the polymerization mixture but a crown ether monomer of formula (3') is not present in the polymerization mixture, Z is P; when a crown ether monomer of formula (3') is present in the polymerization mixture, Z is N or P.

[0014] Another polymer is provided comprising a second reaction product of the second polymerization mixture; a quaternary ammonium or phosphonium compound or a nitrogen-containing heterocycle or a salt thereof, and An intermediate polymer is included, The intermediate polymer is (i) a halogenated trifluoromethyl ketone monomer having the formula: [ka] (ii) an aromatic monomer having the formula (3) shown above, or a crown ether monomer having the formula (3') shown above, and (iii) optionally, a first reaction product of a first polymerization mixture comprising a trifluoromethyl ketone monomer having formula (4) shown above; wherein the quaternary phosphonium compound has the formula (5): [ka] Nitrogen-containing heterocycle, m', n', n, q, R2, R3, R4, R5, R6, R7, R8, R9, R 10 , R 12 , R 13 , R 14 , R 15 , R 16 , and R 17is as above, R 18 and R 24 are each independently alkylene; R 19 , R 20 , R 21 , R 22 , and R 23 are each independently alkyl, alkenyl, or alkynyl; R 111 is a halide, m is 0, 1, 2, 3, 4, 5, or 6; X - is an anion, When an aromatic monomer of formula (3) is present in the first polymerization mixture but a crown ether monomer of formula (3') is not present in the first polymerization mixture, Z is P; when a crown ether monomer of formula (3') is present in the first polymerization mixture, Z is N or P.

[0015] Also provided is an anion exchange polymer comprising the reaction product of a base and any one of the polymers described above.

[0016] Also provided is a method of making an anion exchange polymer membrane comprising an anion exchange polymer, the method comprising: reacting a cationically functionalized trifluoroketone monomer, an optional trifluoromethyl ketone monomer, and an aromatic monomer or a crown ether monomer in the presence of an organic solvent and a polymerization catalyst to form a cationically functionalized polymer; dissolving a cationically functionalized polymer in a solvent to form a polymer solution; casting the polymer solution to form a polymer film; and exchanging the anions of the polymer membrane with hydroxide ions, bicarbonate ions, or carbonate ions, or a combination thereof, to form an anion exchange polymer membrane.

[0017] Another method is provided for making an anion exchange polymer membrane comprising an anion exchange polymer, the method comprising: reacting a halogenated trifluoroketone monomer, an optional trifluoromethyl ketone monomer, and an aromatic monomer in the presence of an organic solvent and a polymerization catalyst to form a halogen-functionalized polymer; reacting the halogen-functionalized polymer with a quaternary phosphonium compound or a nitrogen-containing heterocycle or a salt thereof in the presence of an organic solvent to form a cationically functionalized polymer; dissolving a cationically functionalized polymer in a solvent to form a polymer solution; casting the polymer solution to form a polymer film; and exchanging the anions of the polymer membrane with hydroxide ions, bicarbonate ions, or carbonate ions, or a combination thereof, to form an anion exchange polymer membrane.

[0018] Another method is provided for making an anion exchange polymer membrane comprising an anion exchange polymer, the method comprising: reacting a halogenated trifluoroketone monomer, an optional trifluoromethyl ketone monomer, and a crown ether monomer in the presence of an organic solvent and a polymerization catalyst to form a halogen-functionalized polymer; reacting the halogen-functionalized polymer with a quaternary ammonium or quaternary phosphonium compound or a nitrogen-containing heterocycle or salt thereof in the presence of an organic solvent to form a cationically functionalized polymer; dissolving a cationically functionalized polymer in a solvent to form a polymer solution; casting the polymer solution to form a polymer film; and exchanging the anions of the polymer membrane with hydroxide ions, bicarbonate ions, or carbonate ions, or a combination thereof, to form an anion exchange polymer membrane.

[0019] Also provided is an anion exchange membrane, optionally configured and sized to be suitable for use in a fuel cell, an electrolyzer, an electrodialysis device, a solar hydrogen generator, a flow battery, a desalination device, a sensor, a demineralizer, a water purifier, a wastewater treatment system, an ion exchange device, or a CO2 separator, the anion exchange membrane comprising an anion exchange polymer.

[0020] Also provided is an anion exchange membrane fuel cell, an electrolyzer, an electrodialysis device, a solar hydrogen generator, a flow battery, a desalination device, a sensor, a demineralization device, a water purifier, a wastewater treatment system, an ion exchange device, or a CO2 separator, wherein the fuel cell, the electrolyzer, the electrolysis device, the solar hydrogen generator, the flow battery, the desalination device, a sensor, a demineralization device, a water purifier, a wastewater treatment system, an ion exchange device, or a CO2 separator comprises an anion exchange polymer.

[0021] Also provided is a reinforced electrolyte membrane, optionally configured and sized to be suitable for use in a fuel cell, an electrolyzer, an electrodialysis device, a solar hydrogen generator, a flow battery, a desalination device, a sensor, a demineralizer, a water purifier, a wastewater treatment system, an ion exchange device, or a CO2 separator. The membrane includes a porous substrate impregnated with an anion exchange polymer.

[0022] Other objects and features will be in part apparent and in part pointed out hereinafter. [Brief description of the drawings]

[0023] [Figure 1A] 1 illustrates an exemplary hydroxide exchange membrane fuel cell. [Figure 1B] 1 illustrates an exemplary hydroxide exchange membrane electrolyzer. [Diagram 2] 1H NMR spectrum of BP-CF3-Br-1 in CDCl3. [Diagram 3] 1H NMR spectrum of BP-CF3-IM-1 in DMSO-d6. [Figure 4A]1H NMR spectra of BP-CF3-IM-1 before and after alkaline stability test in 1M KOH (10% TFA in DMSO-d6) at 130° C. for 1200 hours. [Figure 4B] The 1H NMR spectra of TP-CF3-IM-1 before and after an alkaline stability test in 10M KOH at 80°C for 300 hours (in DMSO-d6). [Figure 4C] Figure 1 shows 1H NMR spectra of TP-CF3-IM-1 before and after alkaline stability testing at 95 °C for 300 h at RH of 50.9% and 23.3%, respectively (10% TFA in DMSO-d6). [Diagram 5] 1H NMR spectrum of TP-CF3-Br-1 in CDCl3. [Figure 6] 1H NMR spectrum of TP-CF3-IM-1 in DMSO-d6. [Figure 7] FIG. 13 is a graph showing tensile stress as a function of elongation for the bicarbonate form of the TP-CF3-IM-1 polymer. [Figure 8] Illustrates the polarization (voltage as a function of current density) and power density (power density as a function of current density) curves of a HEMFC at 95°C. Materials: TP-CF3-IM-1 membrane, ionomer loading 20%, catalyst: 0.4mgPt cm-2 PtRu / C on anode, 0.4mgPt cm-2 PtRu / C on cathode. Test conditions: 95°C, anode humidifier temperature: 90°C, cathode humidifier temperature: 97°C, H2 flow rate: 1.0L / min, O2 flow rate: 2.0L / min. [Figure 9] Illustrates the polarization (voltage as a function of current density) curves of HEMEL at 80°C. Materials: TP-CF3-IM-1 membrane, ionomer loading 30%, catalyst: 4.0mgPt cm-2 Pt / C on the anode, 2.9mg cm-2 IrO2 on the cathode. Test conditions: water and electrolyzer at 80°C, water flow rate: 3.0mL / min. [Figure 10] Figure 1 shows the 1H NMR spectrum of PCE-C5-Br-1 in CDCl3. [Figure 11]1H NMR spectrum of PCE-C5-IM-Br-1 in DMSO-d6. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0024] It has been discovered that HEM / HEIs formed from polymers with various pendant cationic groups and with intrinsic hydroxide conducting channels simultaneously provide improved chemical stability, conductivity, water uptake, good solubility in selected solvents, mechanical properties, and other attributes related to HEM / HEI performance. Attaching pendant side chains to the rigid aromatic polymer backbone of polymers that do not contain ether linkages allows fine tuning of the membrane mechanical properties, and incorporating alkali-stable cations such as imidazolium, phosphonium, and ammonium improves the stability of the polymer. HEM / HEIs formed from these polymers exhibit superior chemical stability, anion conductivity, reduced water uptake, good solubility in selected solvents, and improved mechanical properties at ambient dry conditions compared to conventional HEM / HEIs. The HEMFCs of the present invention exhibit improved performance and durability at relatively high temperatures.

[0025] In a first aspect of the present invention there is provided a polymer comprising structural units of formula (1A), (3A) and / or (3'A), and optionally (4A).

[0026] The structural unit of formula (1A) has the following structure: [ka] In the formula, q is 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, or 20; R 11 are each independently a quaternary ammonium or phosphonium group, or a nitrogen-containing heterocyclic group or a salt thereof.

[0027] The quaternary ammonium or phosphonium group has the formula (5A): [ka] In the formula, R 180 and R 240 are each independently alkylene; R 190 , R 200 , R 210 , R 220 , and R 230 are each independently alkyl, alkenyl, or alkynyl; m is 0, 1, 2, 3, 4, 5, or 6; X - is an anion, Z is P when structural units of formula (3A) are present in the polymer but structural units of formula (3'A) are not present in the polymer, and Z is N or P when structural units of formula (3'A) are present in the polymer. - is a halide, BF4 - , PF6 - , CO3 2- , or HCO3 - Includes.

[0028] For example, the quaternary ammonium or quaternary phosphonium group of formula (5A) can be R 180 and R 240 Each of C1 to C 22 alkylene, R 190、 R 200、 R 210、 R 220、 and R 230 may each independently be C1-C6 alkyl; m may be 0, 1, 2, 3, 4, 5, or 6; and Z is N or P.

[0029] As another example, the quaternary ammonium or quaternary phosphonium group of formula (5A) can be R 180 and R 240 each independently being a C1-C6 alkylene; 190、 R 200、 R 210、 R 220、 and R 230may each independently be C1-C6 alkyl; m may be 0, 1, 2, or 3; and Z is N or P.

[0030] As yet another example, the quaternary ammonium or quaternary phosphonium group of formula (5A) can be R 180 and R 240 Each independently may have C8 to C 22 alkylene, R 190、 R 200、 R 210、 R 220、 and R 230 are each independently C1 to C6 alkyl; m is 0, 1, 2, or 3; and Z is N or P.

[0031] In other examples, the quaternary ammonium or quaternary phosphonium group of formula (5A) can be R 180 and R 240 Each of these is a C2-C6 alkylene, and R 190 , R 200 , R 210 , R 220 , and R 230 are each independently methyl, m is 1, and Z is N or P.

[0032] In yet another example, the quaternary ammonium or quaternary phosphonium group of formula (5A) is R 180 and R 240 each of which is n-hexylene and R 190 , R 200 , R 210 , R 220 , and R 230 are each methyl, m is 1, and Z is N or P.

[0033] The nitrogen-containing heterocyclic group can be an optionally substituted pyrrole, pyrroline, pyrazole, pyrazoline, imidazole, imidazoline, triazole, pyridine, triazine, pyrazine, pyridazine, pyrimidine, azepine, quinoline, piperidine, pyrrolidine, pyrazolidine, imidazolidine, azepane, isoxazole, isoxazoline, oxazole, oxazoline, oxadiazole, oxatriazole, dioxazole, oxazine, oxadiazine, isoxazolidine, morpholine, thiazole, isothiazole, oxathiazole, oxathiazine, or caprolactam, where each substituent is independently alkyl, alkenyl, alkynyl, aryl, or aralkyl.

[0034] Preferably, the nitrogen-containing heterocyclic group is unsaturated, such as pyrrole, pyrroline, pyrazole, pyrazoline, imidazole, imidazoline, triazole, pyridine, triazine, pyrazine, pyridazine, pyrimidine, azepine, or quinoline, and each substitutable position of the heterocycle is independently substituted with an alkyl group (e.g., methyl, ethyl, propyl, n-butyl) or an aryl group (e.g., phenyl with an alkyl substituent).

[0035] The nitrogen-containing heterocyclic group can include an imidazolium having the formula (6A): [ka] In the formula, R 25 , R 26 , R 27 , and R 28 are each independently hydrogen, a halide, an alkyl, an alkenyl, an alkynyl, or an aryl, wherein the alkyl, alkenyl, alkynyl, or aryl is optionally substituted with a halide. 28 is 2,4,6-alkylphenyl, R 25 , R 26 , and R 27is independently C1-C6 alkyl. An example of an imidazole as a nitrogen-containing heterocycle is 1-butyl-2-mesityl-4,5-dimethyl-1H-imidazole-imidazole having the following formula: [ka]

[0036] The structural unit of formula (3A) has the following structure: [ka] In the formula, n is 0, 1, 2, or 3; R 20 , R 30 , R 40 , R 50 , R 60 , R 70 , R 80 , and R 90 are each independently hydrogen, a halide, an alkyl, an alkenyl, an alkynyl, or an aryl, the alkyl, alkenyl, alkynyl, or aryl being optionally substituted with a halide; R 30 and R 60 are optionally joined to form a five-membered ring optionally substituted with halide or alkyl.

[0037] For example, in the structural unit of formula (3A), R 20 , R 30 , R 40 , R 50 , R 60 , R 70 , R 80 , and R 90 At least one of may be a halide or an aryl, which may be optionally substituted with a halide.

[0038] As another example, in the structural unit of formula (3A), R 30 and R 60 may be joined to form a five-membered ring optionally substituted with halide or alkyl.

[0039] The structural units of formula (3A) may be derived from aromatic monomers including biphenyl, para-terphenyl, meta-terphenyl, para-quaterphenyl, 9,9-dimethyl-9H-fluorene, or benzene.

[0040] The structural unit of formula (3'A) has the following structure: [ka] In the formula, R 20 , R 40 , R 50 , R 70 , R 80 , and R 90 are each independently hydrogen, a halide, an alkyl, an alkenyl, an alkynyl, or an aryl, where the alkyl, alkenyl, alkynyl, or aryl is optionally substituted with a halide. 90 The group may be present or absent. When the benzo ring shown by the dashed line in formula (3'A) is absent, the benzo ring of the structural unit is divalent, so that R 90 When the benzo ring shown by the dashed line in formula (3'A) is present, R 90 Since the benzo ring bearing the group is monovalent, R 90 The group exists.

[0041] For example, the structural unit may be a dibenzo-18-crown-6 polyether such as that shown by the formula (3'A-1) (wherein m' and n' are 0), a dibenzo-21-crown-7 polyether such as that shown by the formula (3'A-1) (wherein m' is 0 and n' is 1), a dibenzo-24-crown-8 polyether such as that shown by the formula (3'A-1) (wherein m' and n' are 1), or a dibenzo-30-crown-10 polyether such as that shown by the formula (3'A-1) (wherein m' and n' are 2 and R 20 , R 40 , R 50 , R 70 , R 80 , and R 90 is as defined in formula (3'A) [ka] or benzo-18-crown-6 ethers such as those of formula (3'A-2) (wherein m' and n' are 2 and R 70 and R 80 is as defined in formula (3'A)). [ka]

[0042] For example, in any one of the structural units of formulae (3'A) to (3'A-2), R 20 , R 40 , R 50 , R 70 , R 80 , and R 90 When present, may be hydrogen or a halide.

[0043] The structural unit of formula (3'A-1) can be derived from a reactive dibenzo-crown ether, R 20 , R 40 , R 50 , R 70 , R 80 , and R 90 are each hydrogen. Dibenzo-18-crown-6 polyethers can be made from catechol and bis(chloroethyl) ether as described by Charles J. Pedersen, Org. Synth., 1972, 52, 66, and are commercially available. Dibenzo-21-crown-7 polyethers, dibenzo-24-crown-8 polyethers, and dibenzo-30-crown-10 polyethers are also commercially available.

[0044] The structural unit of formula (3'A-2) can be derived from benzo-18-crown-6 polyether, R 70 and R 80 are hydrogen. Benzo-18-crown-6 polyethers are commercially available.

[0045] The optional structural unit of formula (4A) has the structure [ka] In the formula, each R 100 is independently an alkyl, alkenyl, alkynyl, or a substituent having the formula (4B), [ka] The alkyl, alkenyl, or alkynyl is optionally substituted with fluoride, R 130 , R 140 , R 150 , R 160 , and R 170 are each independently hydrogen, a halide, an alkyl, an alkenyl, an alkynyl, or an aryl, wherein the alkyl, alkenyl, alkynyl, or aryl is optionally substituted with a halide.

[0046] For example, in the structural unit of formula (4A), R 100 can be an alkyl, alkenyl, or alkynyl, where the alkyl, alkenyl, or alkynyl can be optionally substituted with fluoride.

[0047] As another example, in the structural unit of formula (4A), R 100 may be a substituent of formula (4B), R 130 , R 140 , R 150 , R 160 , and R 170 At least one of may be a halide or an aryl, which may be optionally substituted with fluoride.

[0048] As another example, R 20 , R 40 , R 50 , R 70 , R 80 , R 90 , R 130 , R 140 , R 150, R 160 , and R 170 may each independently be hydrogen or alkyl optionally substituted with fluoride; R 100 can be fluoride or alkyl optionally substituted with a substituent of formula (4B).

[0049] In another example, R 20 , R 40 , R 50 , R 70 , R 80 , R 90 , R 130 , R 140 , R 150 , R 160 , and R 170 may each independently be hydrogen, methyl, ethyl, propyl, butyl, pentyl, or hexyl, or methyl, ethyl, propyl, butyl, pentyl, or hexyl optionally substituted with fluoride; R 100 can be methyl, ethyl, propyl, butyl, pentyl, or hexyl, optionally substituted with fluoride or a substituent of formula (4B).

[0050] The sum of the molar fractions of structural units of formula (1A) and formula (4A) in the polymer may be approximately equal to the sum of the molar fractions of structural units of formula (3A) and (3'A) in the polymer, and the ratio of the molar fraction of structural units of formula (1A) in the polymer to the sum of the molar fractions of structural units of formula (3A) and (3'A) in the polymer may be about 0.01 to 1.

[0051] The molar ratio of the sum of the molar fractions of structural units of formula (1A) or (4A) to the sum of the molar fractions of structural units of formula (3A) and (3'A) in the polymer can be from about 0.95:1 to about 1.4:1, and the ratio of the molar fraction of structural units of formula (1A) to the sum of the molar fractions of structural units of formula (3A) and (3'A) can be from about 0.01 to 1.

[0052] The molar ratio of the sum of the molar fractions of structural units of formula (1A) and formula (4A) to the sum of the molar fractions of structural units of formula (3A) and formula (3'A) in the polymer can be from about 1:1 to about 1.2:1.

[0053] In a second aspect of the present invention, there is provided a polymer comprising the reaction product of a polymerization mixture comprising a cationically functionalized trifluoroketone monomer, an aromatic monomer and / or a crown ether monomer, and, optionally, a trifluoromethyl ketone monomer.

[0054] The cationic functionalized trifluoroketone monomer has the formula: [ka] wherein q is 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, or 20, and each R is independently a quaternary ammonium or phosphonium group or a nitrogen-containing heterocyclic group or a salt thereof, wherein the quaternary ammonium or phosphonium group and the nitrogen-containing heterocyclic group are as defined above for the first aspect of the invention.

[0055] The aromatic monomer has the formula: [ka] In the formula, n is 0, 1, 2, or 3; R2, R3, R4, R5, R6, R7, R8, R9, and R 10 are each independently hydrogen, halide, alkyl, alkenyl, alkynyl, or aryl, where alkyl, alkenyl, alkynyl, or aryl are optionally substituted with halide, and R and R are optionally joined to form a five-membered ring optionally substituted with halide or alkyl.

[0056] For example, in the aromatic monomer of formula (3), R2, R3, R4, R5, R6, R7, R8, R9, and R 10 At least one of is a halide or an aryl, the aryl being optionally substituted with a halide.

[0057] As another example, in the aromatic monomer of formula (3), R3 and R6 are joined to form a five-membered ring optionally substituted with halide or alkyl.

[0058] The aromatic monomer of formula (3) can include biphenyl, para-terphenyl, meta-terphenyl, para-quaterphenyl, 9,9-dimethyl-9H-fluorene, or benzene.

[0059] The crown ether monomer has the formula: [ka] Wherein, if present, R2, R4, R5, R7, R8, R9, and R 10 is each independently hydrogen, a halide, an alkyl, an alkenyl, an alkynyl, or an aryl, where the alkyl, alkenyl, alkynyl, or aryl is optionally substituted with a halide, and each m' and each n' is independently 0, 1, or 2. The benzo ring shown with a dashed line in formula (3') can be present or absent.

[0060] For example, the crown ether monomer may be a dibenzo-18-crown-6 polyether as shown in formula (3'-1) (wherein m' and n' are 0), a dibenzo-21-crown-7 polyether as shown in formula (3'-1) (wherein m' is 0 and n' is 1), a dibenzo-24-crown-8 polyether as shown in formula (3'-1) (wherein m' and n' are 1), or a dibenzo-30-crown-10 polyether as shown in formula (3'-1) (wherein m' and n' are 2 and R2, R4, R5, R7, R8, R9, and R 10 is as defined in formula (3'), [ka] or benzo-18-crown-6 ether such as formula (3'-2) (wherein m' and n' are 2 and R7, R8, R9, and R 10is as defined in formula (3'). [ka]

[0061] The optional trifluoromethyl ketone monomer has the formula: [ka] In the formula, each R 12 is independently an alkyl, alkenyl, alkynyl, or a substituent of formula (4C); [ka] The alkyl, alkenyl, or alkynyl is optionally substituted with fluoride, R 13 , R 14 , R 15 , R 16 , and R 17 are each independently hydrogen, halide, alkyl, alkenyl, alkynyl, or aryl.

[0062] For example, in the trifluoromethyl ketone monomer of formula (4), R 12 is an alkyl, alkenyl, or alkynyl, wherein the alkyl, alkenyl, or alkynyl is optionally substituted with fluoride.

[0063] As another example, in the trifluoromethyl ketone monomer of formula (4), R 12 is a substituent of formula (4C), R 13 , R 14 , R 15 , R 16 , and R 17 At least one of is a halide or aryl, the aryl being optionally substituted with fluoride.

[0064] As another example, R2, R3, R4, R5, R6, R7, R8, R9, R 10 , R13 , R 14 , R 15 , R 16 , and R 17 are each independently hydrogen or alkyl optionally substituted with fluoride; R 12 is an alkyl optionally substituted with fluoride or a substituent of formula (4C).

[0065] In another example, R2, R3, R4, R5, R6, R7, R8, R9, R 10 , R 13 , R 14 , R 15 , R 16 , and R 17 are each independently hydrogen, methyl, ethyl, propyl, butyl, pentyl, or hexyl, or methyl, ethyl, propyl, butyl, pentyl, or hexyl optionally substituted with fluoride; R 12 is methyl, ethyl, propyl, butyl, pentyl, or hexyl optionally substituted with fluoride or a substituent of formula (4C).

[0066] A third aspect of the invention is a polymer comprising a second reaction product of a second polymerization mixture comprising a quaternary ammonium or phosphonium compound or a nitrogen-containing heterocycle or a salt thereof, and an intermediate polymer.

[0067] The intermediate polymer comprises a first reaction product of a first polymerization mixture comprising halogenated trifluoromethyl ketone monomers, aromatic monomers and / or crown ether monomers, and, optionally, trifluoromethyl ketone monomers.

[0068] The halogenated trifluoromethyl ketone monomer has the formula: [ka] In the formula, q is 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, or 20; R 111 is a halide. Preferably, the halide is a fluoride, chloride, bromide, or iodide.

[0069] The aromatic monomer has formula (3) and is as described for the polymer in the second aspect of the invention.

[0070] The crown ether has the formula (3') and is as described for the polymer in the second aspect of the invention.

[0071] The trifluoromethyl ketone monomer has formula (4) and is as described for the polymer in the second aspect of the invention.

[0072] The quaternary ammonium or phosphonium compound has the formula (5): [ka] In the formula, m is 0, 1, 2, 3, 4, 5, or 6; R 18 and R 24 are each independently alkylene; R 19 , R 20 , R 21 , R 22 , and R 23 are each independently an alkyl, alkenyl, or alkynyl; X - is an anion, Z is P when the aromatic monomer of formula (3) is present in the first polymerization mixture but the crown ether monomer of formula (3') is not present in the first polymerization mixture, and Z is N or P when the crown ether monomer of formula (3') is present in the first polymerization mixture. - is a halide, BF4 - , PF6 - , CO3 2- , or HCO3 - Includes.

[0073] For example, the quaternary ammonium or phosphonium compound of formula (5) is R 18 and R 24 Each of C1 to C 22 alkylene, R 19 , R 20 , R 21 , R 22 , and R 23 may each independently be C1-C6 alkyl; m may be 0, 1, 2, 3, 4, 5, or 6; and Z is N or P.

[0074] As another example, the quaternary ammonium or phosphonium compound of formula (5) can be R 18 and R 24 each independently being a C1-C6 alkylene; 19 , R 20 , R 21 , R 22 , and R 23 may each independently be C1-C6 alkyl; m may be 0, 1, 2, or 3; and Z is N or P.

[0075] As yet another example, the quaternary ammonium or phosphonium compound of formula (5) can be R 18 and R 24 Each independently may have C8 to C 22 alkylene, R 19 , R 20 , R 21 , R 22 , and R 23 may each independently be C1-C6 alkyl; m may be 0, 1, 2, or 3; and Z is N or P.

[0076] In another example, the quaternary ammonium or phosphonium compound of formula (5) is R 18 and R 24 Each of these is a C2-C6 alkylene, and R 19 , R 20 , R 21 , R22 , and R 23 may each independently be methyl, m may be 1, and Z is N or P.

[0077] In yet another example, the quaternary ammonium or phosphonium compound of formula (5) is R 18 and R 24 each of which is n-hexylene and R 19 , R 20 , R 21 , R 22 , and R 23 Each can be methyl, m can be 1, and Z is N or P.

[0078] The nitrogen-containing heterocycle can be an optionally substituted pyrrole, pyrroline, pyrazole, pyrazoline, imidazole, imidazoline, triazole, pyridine, triazine, pyrazine, pyridazine, pyrimidine, azepine, quinoline, piperidine, pyrrolidine, pyrazolidine, imidazolidine, azepane, isoxazole, isoxazoline, oxazole, oxazoline, oxadiazole, oxatriazole, dioxazole, oxazine, oxadiazine, isoxazolidine, morpholine, thiazole, isothiazole, oxathiazole, oxathiazine, or caprolactam, where each substituent is independently alkyl, alkenyl, alkynyl, aryl, or aralkyl.

[0079] Preferably, the nitrogen-containing heterocycle is unsaturated, such as pyrrole, pyrroline, pyrazole, pyrazoline, imidazole, imidazoline, triazole, pyridine, triazine, pyrazine, pyridazine, pyrimidine, azepine, or quinoline, and each substitutable position of the heterocycle is independently substituted with an alkyl group (e.g., methyl, ethyl, propyl, n-butyl) or an aryl group (e.g., phenyl with an alkyl substituent).

[0080] For example, the nitrogen-containing heterocycle can include an imidazole having the formula (6): [ka] In the formula, R 25 , R 26 , R 27 , R 28 , and R 29 are each independently hydrogen, a halide, an alkyl, an alkenyl, an alkynyl, or an aryl, wherein the alkyl, alkenyl, alkynyl, or aryl is optionally substituted with a halide. 29 is hydrogen and R 28 is 2,4,6-alkylphenyl, R 25 , R 26 , and R 27 is independently C1-C6 alkyl. An example of an imidazole as a nitrogen-containing heterocycle is 1-butyl-2-mesityl-4,5-dimethyl-1H-imidazole-imidazole having the following formula: [ka]

[0081] The nitrogen-containing heterocycle can be an optionally substituted pyrrole, pyrroline, pyrazole, pyrazoline, imidazole, imidazoline, triazole, pyridine, triazine, pyrazine, pyridazine, pyrimidine, azepine, quinoline, piperidine, pyrrolidine, pyrazolidine, imidazolidine, azepane, isoxazole, isoxazoline, oxazole, oxazoline, oxadiazole, oxatriazole, dioxazole, oxazine, oxadiazine, isoxazolidine, morpholine, thiazole, isothiazole, oxathiazole, oxathiazine, or caprolactam, where each substituent is independently alkyl, alkenyl, alkynyl, aryl, or aralkyl.

[0082] A fourth aspect of the invention is an anion exchange polymer comprising the reaction product of a base and any one of the polymers as described above in the first, second or third aspects of the invention.

[0083] Preferably, the base comprises a hydroxide-containing base, such as sodium or potassium hydroxide, a bicarbonate-containing base, such as sodium or potassium bicarbonate, or a carbonate-containing base, such as sodium or potassium carbonate.

[0084] Representative anion exchange polymers include the following, where x is from 0.01 to 1: [ka] [ka] [ka] [ka] [ka]

[0085] The imidazolium-tethered poly(aryl alkylene) polymer or the imidazolium-tethered poly(aryl-crown ether-alkylene) polymer can be a hydroxide exchange polymer that contains a poly(aryl alkylene) or poly(aryl crown ether-alkylene) backbone that is free of ether linkages and has a water absorption of 47% or less based on the dry weight of the polymer when immersed in pure water at 80° C. or has a hydroxide conductivity of at least 31 mS / cm in pure water at 20° C. The polymer is also stable to degradation when immersed in 1 M potassium hydroxide for 1,200 hours at 130° C. 1 It is stable to decomposition when immersed in 10 M potassium hydroxide at 80 °C for 300 h (as evidenced by no change in the H NMR spectrum). 1It was stable to decomposition (as evidenced by no change in the H NMR spectrum) when kept at 95 °C for 300 h and at 23.3% and 50.9% relative humidity. 1 It may be insoluble in pure water and isopropanol at 100° C. (as evidenced by no change in the H NMR spectrum), but soluble in a 50 / 50 by weight mixture of water and ethanol at 100° C. The polymer may also have a tensile strength of at least 30 MPa and / or an elongation at break of at least 250%.

[0086] The uptake of imidazolium-tethered poly(aryl-crown ether-alkylene) polymers can be 47% or less if the polymer is crosslinked with a crosslinker or chemically bonded to the membrane. For example, when measured, the water uptake of polycrown ether-CF3-TMA (also known as PCE-C5-QA-1) in Example 10 was 364%, and the water uptake of poly(aryl-crown ether-alkylene)-CF3-IM in Example 7 was about 200%, which can be reduced by crosslinking or chemically bonding the polymer to the membrane.

[0087] Crosslinking agents for use in crosslinking any of the polymers described herein include, for example, dibromoalkanes (dibromohexane, dibromobutane), diiodoalkanes (diiodohexane, diiodobutane), and ammonium cation-containing dibromoalkanes and diiodoalkanes.

[0088] The imidazolium-tethered poly(aryl alkylene) polymer or the imidazolium-tethered poly(aryl-crown ether-alkylene) polymer comprises an imidazolium-tethered poly(aryl alkylene) or poly(aryl-crown ether-alkylene) backbone that does not contain an ether linkage, and the polymer is used as a hydroxide exchange membrane in a hydroxide exchange membrane fuel cell, loaded at 20% as a hydroxide exchange ionomer in the cathode and anode catalyst layers of the fuel cell, and the fuel cell is loaded with 0.4 mg of ethylenediaminetetraacetate on the anode. Pt cm-2 PtRu / C, 0.4 mg on the cathode Pt cm -2 At least 130 mW / cm with PtRu / C and test conditions of 1.0 L / min hydrogen flow rate, 2.0 L / min oxygen flow rate, 95°C cell temperature, and anode and cathode humidifier temperatures of 90°C and 97°C, respectively 2 The power density of the hydroxide exchange polymer may be 0.1 to 0.5 wt %.

[0089] Preferably, the aryl linkages of the imidazolium-tethered poly(aryl alkylene) backbone that does not contain an ether linkage comprise p-phenyl and the alkylene linkages comprise hydroxide, bicarbonate, or carbonate anions, or combinations thereof. The imidazolium-tethered poly(aryl-crown ether-alkylene) polymer backbone that does not contain an ether linkage also preferably comprises dibenzo-18-crown-6, dibenzo-21-crown-7 polyether, dibenzo-24-crown-8 polyether, or dibenzo-30-crown-10 polyether.

[0090] The aryl linkages of the imidazolium-tethered poly(aryl alkylene) polymer backbone can be derived, for example, from biphenyl, para-terphenyl, meta-terphenyl, para-quaterphenyl, 9,9-dimethyl-9H-fluorene, or benzene monomers. The imidazolium-tethered poly(aryl-crown ether-alkylene) polymer backbone that does not contain an ether linkage can be derived, for example, from dibenzo-18-crown-6, dibenzo-21-crown-7 polyether, dibenzo-24-crown-8 polyether, or dibenzo-30-crown-10 polyether.

[0091] The alkylene linkages of the imidazolium-tethered poly(arylalkylene) backbone are derived from 7-bromo-1,1,1-trifluoroheptan-2-one monomers.

[0092] The imidazolium-tethered poly(aryl alkylene) polymer backbone or the imidazolium-tethered poly(aryl-crown ether-alkylene) polymer backbone may further comprise 2,2,2-trifluoroethylbenzene linkages derived from 2,2,2-trifluoroacetophenone monomers, or trifluoromethylmethylene linkages derived from trifluoromethyl ketone monomers, such as 1,1,1-trifluoropropane linkages derived from 1,1,1-trifluoroacetone.

[0093] The fifth aspect of the present invention is a method for making an anion exchange polymer membrane comprising the anion exchange polymer of the fourth aspect of the present invention. The method includes reacting a cationically functionalized trifluoroketone monomer, an optional trifluoromethylketone monomer, and an aromatic monomer and / or a crown ether monomer in the presence of an organic solvent and a polymerization catalyst to form a cationically functionalized polymer, dissolving the cationically functionalized polymer in a solvent to form a polymer solution, casting the polymer solution to form a polymer membrane, and exchanging anions of the polymer membrane with hydroxide ions, bicarbonate ions, or carbonate ions, or a combination thereof, to form an anion exchange polymer membrane.

[0094] For example, a cationically functionalized trifluoroketone monomer, such as imidazolium-functionalized 7-bromo-1,1,1-trifluoroheptan-2-one, any trifluoromethylketone monomer, such as 2,2,2-trifluoroacetophenone or 1,1,1-trifluoroacetone, and an aromatic monomer, such as benzene, biphenyl, p-terphenyl, m-terphenyl, or p-quaterphenyl, or a crown ether monomer, such as dibenzo-18-crown-6, dibenzo-21-crown-7 polyether, dibenzo-24-crown-8 polyether, or dibenzo-30-crown-10 polyether, may be placed in a stirred vessel and dissolved or dispersed in an organic solvent. A polymerization catalyst in a solvent may then be added dropwise at -78 to 60°C over a period of up to 60 minutes. The reaction is then continued at this temperature for about 1 to about 120 hours. The resulting solution is slowly poured into an aqueous solution of ethanol. The resulting solid is filtered, washed with water, and immersed in 1M K2CO3 at room temperature for about 1 to 48 hours. Finally, the product is filtered, washed with water, and thoroughly dried under vacuum to form the cationically functionalized polymer. The cationically functionalized polymer is then anion exchanged, e.g., hydroxide exchanged in 1 M KOH at about 20-100° C. for about 12-48 hours, followed by washing and immersion in DI water in an oxygen-free atmosphere for about 12-48 hours to remove residual KOH.

[0095] A representative reaction scheme of the fifth aspect of the invention is shown below, in which R5, R6, R7, R8, and R 100 are each independently hydrogen, alkyl, alkenyl, phenyl, or alkynyl, the alkyl, alkenyl, phenyl, or alkynyl being optionally substituted with halide; R 11 is a phosphonium or nitrogen-containing heterocycle, n is the number of repeat units in the polymer, q is 0 to 20, and x is 0.01 to 1. [ka] [ka] [ka]

[0096] The sixth aspect of the present invention is a method for making an anion exchange polymer membrane comprising the anion exchange polymer in the fourth aspect of the present invention. The method includes reacting halogenated trifluoroketone monomers, optional trifluoromethylketone monomers, and aromatic monomers and / or crown ether monomers in the presence of an organic solvent and a polymerization catalyst to form a halogen-functionalized polymer, reacting the halogen-functionalized polymer with a quaternary phosphonium compound or a nitrogen-containing heterocycle or its salt in the presence of an organic solvent to form a cation-functionalized polymer, dissolving the cation-functionalized polymer in a solvent to form a polymer solution, casting the polymer solution to form a polymer membrane, and exchanging the anions of the polymer membrane with hydroxide ions, bicarbonate ions, or carbonate ions or a combination thereof to form an anion exchange polymer membrane.

[0097] For example, a halogenated trifluoroketone monomer, such as 7-bromo-1,1,1-trifluoroheptan-2-one, any trifluoromethylketone monomer, such as 2,2,2-trifluoroacetophenone or 1,1,1-trifluoroacetone, and an aromatic monomer, such as benzene, biphenyl, p-terphenyl, m-terphenyl, or p-quaterphenyl, or a crown ether monomer, such as dibenzo-18-crown-6, dibenzo-21-crown-7 polyether, dibenzo-24-crown-8 polyether, or dibenzo-30-crown-10 polyether, may be placed in a stirred vessel and dissolved or dispersed in an organic solvent. A polymerization catalyst in a solvent may then be added dropwise at -78 to 60°C over a period of up to 60 minutes. The reaction is then continued at this temperature for about 1 to about 120 hours. The resulting solution is slowly poured into an aqueous solution of ethanol. The resulting solid is filtered, washed with water, and immersed in 1M K2CO3 at room temperature for about 1 to 48 hours. Finally, the product is filtered, washed with water and thoroughly dried under vacuum to form the halogen-functionalized polymer.

[0098] The halogen-functionalized polymer is then placed in a stirred vessel along with a quaternary phosphonium compound or nitrogen-containing heterocycle or salt thereof, such as a functionalized imidazole, and dissolved or dispersed in an organic solvent. The reaction is continued for about 1 to about 120 hours at a temperature of about 50-100° C. The resulting solution is then cast to form a polymer membrane. The polymer membrane is then anion-exchanged, e.g., hydroxide-exchanged in 1 M KOH at about 20-100° C. for about 12-48 hours, followed by washing and immersion in DI water for about 12-48 hours in an oxygen-free atmosphere to remove residual KOH.

[0099] A representative reaction scheme of the sixth aspect of the invention is shown below, in which R5, R6, R7, R8, and R 100 are each independently hydrogen, alkyl, alkenyl, phenyl, or alkynyl, the alkyl, alkenyl, phenyl, or alkynyl being optionally substituted with halide; R 11is a quaternary ammonium or phosphonium group or a nitrogen-containing heterocyclic group as defined in the first aspect of the invention, n is the number of repeat units in the polymer, q is 0 to 20 and x is 0.01 to 1. [ka] [ka] [ka]

[0100] A seventh aspect of the present invention is an anion exchange membrane, optionally configured and sized to be suitable for use in a fuel cell, an electrolyzer, an electrodialysis device, a solar hydrogen generator, a flow battery, a desalination device, a sensor, a demineralization device, a water purifier, a wastewater treatment system, an ion exchange device, or a CO2 separator, and comprising the anion exchange polymer of the fourth aspect of the present invention.

[0101] The anion exchange polymer can be made into a reinforced hydroxide exchange membrane as described below. Such a reinforced hydroxide exchange membrane can be prepared by a method including wetting a porous substrate with a liquid to form a wet substrate, dissolving a poly(aryl alkylene) polymer in a solvent to form a homogeneous solution, applying the solution onto the wet substrate to form a reinforced membrane, drying the reinforced membrane, and exchanging the anions of the reinforced membrane with hydroxide ions to form a reinforced hydroxide exchange polymer membrane. The solution can be applied to the wet substrate by any known membrane forming technique, such as casting, spraying, or doctor knife.

[0102] The resulting reinforced membrane can be impregnated multiple times with poly(aryl alkylene) polymer, if desired, by rewetting the reinforced membrane and repeating the dissolving, casting, and drying steps.

[0103] The polymerization catalyst used in forming the polymer can include trifluoromethanesulfonic acid, pentafluoroethanesulfonic acid, heptafluoro-1-propanesulfonic acid, trifluoroacetic acid, perfluoropropionic acid, heptafluorobutyric acid, or combinations thereof.

[0104] Each of the organic solvents used in any of the above methods can be independently selected from polar aprotic solvents (e.g., dimethylsulfoxide, 1-methyl-2-pyrrolidinone, 1-methyl-2-pyrrolidone, 1-methyl-2-pyrrolidone, or dimethylformamide) or other suitable solvents including, but not limited to, methylene chloride, trifluoroacetic acid, trifluoromethanesulfonic acid, chloroform, 1,1,2,2-tetrachloroethane, dimethylacetamide, or combinations thereof.

[0105] The solvent in the dissolution step can include methanol, ethanol, n-propanol, isopropanol, n-butanol, sec-butanol, tert-butanol, pentanol, hexanol, dimethylsulfoxide, 1-methyl-2-pyrrolidone, dimethylformamide, chloroform, ethyl lactate, tetrahydrofuran, 2-methyltetrahydrofuran, water, phenol, acetone, or combinations thereof.

[0106] The liquid used to wet the porous substrate can be a low boiling point solvent such as a lower alcohol (e.g., methanol, ethanol, propanol, isopropanol) and / or water. Preferably, the liquid is absolute ethanol.

[0107] Additional aspects of the invention are described below.

[0108] Anion exchange membranes, such as hydroxide exchange membranes, are also provided, the membranes being configured and sized to be suitable for use in fuel cells, electrolyzers, electrodialysis devices, solar hydrogen generators, flow batteries, desalination devices, sensors, demineralization devices, water purifiers, wastewater treatment systems, ion exchange devices, or CO2 separators, and comprising any of the poly(aryl alkylene) polymers described herein.

[0109] Reinforced electrolyte membranes, such as reinforced hydroxide exchange membranes, are also provided to enhance the mechanical robustness of the anion exchange membrane for stability through multiple wet-dry cycles (relative humidity cycling) in fuel cells. The membranes are configured and sized to be suitable for use in fuel cells, electrolyzers, electrodialysis devices, solar hydrogen generators, flow batteries, desalination devices, sensors, demineralizers, water purifiers, wastewater treatment systems, ion exchange devices, or CO2 separators, and include a porous substrate impregnated with any of the poly(aryl alkylene) polymers described herein. Methods for preparing reinforced membranes are well known to those skilled in the art, such as those disclosed in U.S. Patents RE37,656 and RE37,701, and are incorporated herein by reference for their description of the synthesis and materials of reinforced membranes.

[0110] The porous substrate can include a membrane made of polytetrafluoroethylene, polypropylene, polyethylene, poly(etherketone), polyaryletherketone, imidazolium-tethered poly(arylalkylene), imidazole-tethered poly(arylalkylene), polysulfone, perfluoroalkoxyalkane, or fluorinated ethylenepropylene polymer, or other porous polymer known in the art, such as dimensionally stable membranes from Giner for use in preparing reinforced membranes for fuel cells. Such porous substrates are commercially available, for example, from WL Gore & Associates.

[0111] The porous substrate may have a porous microstructure of polymer fibrils. Such substrates made of polytetrafluoroethylene are commercially available. The porous substrate may include a microstructure of nodes interconnected by fibrils.

[0112] The interior volume of the porous substrate can be substantially occluded by impregnation with a poly(aryl alkylene) polymer described herein.

[0113] The porous substrate may have a thickness of from about 1 micron to about 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95 or 100 microns. Preferably, the porous substrate has a thickness of from about 5 microns to about 30 microns, or from about 7 microns to about 20 microns.

[0114] Also provided is an anion exchange membrane fuel cell, an electrolyzer, an electrodialysis device, a solar hydrogen generator, a flow battery, a desalination device, a sensor, a demineralization device, a water purifier, a wastewater treatment system, an ion exchange device, or a CO2 separator, wherein the fuel cell, the electrolyzer, the electrolysis device, the solar hydrogen generator, the flow battery, the desalination device, a sensor, a demineralization device, a water purifier, a wastewater treatment system, an ion exchange device, or a CO2 separator comprises an anion exchange polymer.

[0115] The polymers of the present invention having high water absorption are useful as ionomers in electrolyzers or fuel cells when the polymer is attached to the catalyst layer so that it is not washed away during operation of the electrolyzer or fuel cell. Attachment can be achieved by chemically bonding the polymer to the membrane or catalyst layer in the electrolyzer or fuel cell, or by crosslinking the polymer with a crosslinker such as those mentioned above. For example, functional groups on the polymers of the present invention, such as bromoalkyl groups, can be reacted with functional groups on the membrane, such as amine groups, to bond the polymer ionomer to the membrane.

[0116] When the polymer of the present invention is used as a membrane, the water absorption rate of the polymer is preferably in the range of about 20 to about 50% in order to maintain the mechanical strength of the membrane.

[0117] Poly(aryl alkylene) polymers or poly(aryl-crown ether-alkylenes) may be used in HEMFCs, such as a typical fuel cell 10, as shown in FIG. 1A. FIG. 1A illustrates a typical fuel cell 10 with an anode portion 12 (illustrated on the left) and a cathode portion 14 (illustrated on the right) separated by an electrolyte membrane 16. The electrolyte membrane 16 may be any membrane including any of the poly(aryl alkylene) polymers or poly(aryl-crown ether-alkylenes) as described herein, and may be a reinforced membrane. Support members are not shown. The anode portion performs an anode half-reaction that oxidizes a fuel to release electrons to an external circuit and produce an oxidation product. The cathode portion performs a cathode half-reaction that reduces an oxidant consuming electrons from the external circuit. Gas diffusion layers (GDLs) 18 and 20 function to distribute the fuel 22 and oxidant 24 uniformly across the respective catalyst layers 26 and 28. Charge neutrality is maintained by the flow of ions from the anode to the cathode for positive ions and from the cathode to the anode for negative ions. The electrolyte membrane is typically selected to be as thin as possible while maintaining the structural integrity of the membrane, so the illustrated dimensions are not representative.

[0118] In the illustrated hydroxide exchange membrane fuel cell (HEMFC), the anode half-reaction consumes fuel and OH- ions to produce waste water (and carbon dioxide in the case of carbon-containing fuels). The cathode half-reaction consumes oxygen and produces OH- ions that flow from the cathode to the anode through the electrolyte membrane. The fuel is limited only by the oxidation capacity of the anode catalyst and typically includes hydrogen gas, methanol, ethanol, ethylene glycol, and glycerol. Preferably, the fuel is H2 or methanol. The catalyst is typically one or more transition metals such as platinum (Pt), silver (Ag), or Ni. In the case of a PEMFC, the anode half-reaction consumes fuel and produces H+ ions and electrons. The cathode half-reaction consumes oxygen, H+ ions, and electrons to produce waste water, and H+ ions (protons) flow from the anode to the cathode through the electrolyte membrane.

[0119] Thus, it can be seen how electrolyte membranes made from poly(aryl alkylene) polymers or poly(aryl-crown ether-alkylene) polymers can significantly improve fuel cell performance. First, to achieve higher fuel cell efficiency, low internal resistance is required, so electrolyte membranes with higher ionic conductivity (low ionic resistance) are preferred. Second, higher power requires higher fuel cell current, so electrolyte membranes with higher ionic current capacity are preferred. A practical electrolyte membrane must also resist chemical degradation, be mechanically stable in the fuel cell environment, and be easy to fabricate.

[0120] Poly(aryl alkylene) polymers or poly(aryl-crown ether-alkylene) polymers may be used in HEMELs, such as electrolyzer 30, as shown in FIG. 1B. FIG. 1B illustrates a typical electrolyzer 30 with an anode portion 32 (illustrated on the left) and a cathode portion 34 (illustrated on the right) separated by an electrolyte membrane 36. The electrolyte membrane 36 may be any membrane including any of the poly(aryl alkylene) polymers or poly(aryl-crown ether-alkylene)s as described herein, and may be a reinforced membrane. Support members are not shown. The anode portion performs an anode half-reaction that oxidizes ions to release electrons to an external circuit and produces oxidation products. The cathode portion performs a cathode half-reaction that reduces an oxidant consuming electrons from the external circuit. Gas diffusion layers (GDLs) 38 and 40 function to uniformly release the oxidant 42 and fuel 44 across the respective catalyst layers 46 and 48. Charge neutrality is maintained by the flow of ions from the anode to the cathode for positive ions and from the cathode to the anode for negative ions. The electrolyte membrane is typically selected to be as thin as possible while maintaining the structural integrity of the membrane, so the illustrated dimensions are not representative.

[0121] In the illustrated hydroxide exchange membrane fuel cell (HEMFC), the anode half-reaction consumes OH- ions and produces oxygen. The cathode half-reaction consumes water and produces hydrogen and OH- ions that flow from the cathode to the anode through the electrolyte membrane. The fuel is limited only by the oxidation capacity of the cathode catalyst and typically includes hydrogen gas, methanol, ethanol, ethylene glycol, and glycerol. Preferably, the fuel is H2 or methanol. The catalyst is typically one or more transition metals such as platinum (Pt), silver (Ag), or Ni.

[0122] Thus, it can be seen how electrolyte membranes made from poly(aryl alkylene) or poly(aryl-crown ether-alkylene) polymers can significantly improve electrolyzer performance. First, higher efficiency in electrolyzers requires lower internal resistance, so electrolyte membranes with higher ionic conductivity (lower ionic resistance) are preferred. Second, higher fuel production requires higher electrolyzer currents, so electrolyte membranes with higher ionic current capacity are preferred. A practical electrolyte membrane must also resist chemical degradation, be mechanically stable in the electrolyzer environment, and be easy to fabricate.

[0123] The primary application of poly(aryl alkylene) polymers or poly(aryl-crown ether-alkylene) polymers is for energy conversion, such as for use in anion exchange membranes, hydroxide exchange membranes, anion exchange membrane fuel cells, and hydroxide exchange membrane fuel cells, however, anion / hydroxide exchange ionomers and membranes can be used for many other purposes such as for use in fuel cells (e.g., hydrogen / alcohol / ammonia fuel cells), electrolyzers (e.g., water / carbon dioxide / ammonia electrolyzers), electrodialysis units, ion exchange units, solar hydrogen generators, desalination units (e.g., sea / brackish water desalination), hardness removal units (e.g., water hardness removal), water purifiers (e.g., ultrapure water production), wastewater treatment systems, concentration of electrolyte solutions in the food, pharmaceutical, chemical, and biotechnology fields, electrolysis (e.g., chlor-alkali generation and H2 / O2 generation), energy storage (e.g., supercapacitors, metal air batteries, and redox flow batteries), sensors (e.g., pH / RH sensors), and other applications where anion conducting ionomers are advantageous.

[0124] Also provided is a reinforced electrolyte membrane, optionally configured and sized to be suitable for use in a fuel cell, an electrolyzer, an electrodialysis device, a solar hydrogen generator, a flow battery, a desalination device, a sensor, a demineralizer, a water purifier, a wastewater treatment system, an ion exchange device, or a CO2 separator. The membrane includes a porous substrate impregnated with an anion exchange polymer.

[0125] Although the invention has been described in detail, it will be appreciated that modifications and variations are possible without departing from the scope of the invention as defined in the appended claims. EXAMPLES

[0126] To further illustrate the present invention, the following non-limiting examples are provided.

[0127] Example 1 Imidazolium-tethered poly(arylalkylene) polymers were prepared from 7-bromo-1,1,1-trifluoroheptan-2-one, 1,1,1-trifluoroacetone, and biphenyl (designated BP-CF3-IM-x, where x is the molar ratio of 7-bromo-1,1,1-trifluoroheptan-2-one to biphenyl, ranging from 1 to 100). BP-CF3-IM-x was prepared in three major steps: (1) synthesis of bromide-functionalized polymer, (2) synthesis of imidazolium-functionalized polymer, and (3) film casting and hydroxide exchange. The reaction scheme is shown below, where n is the number of repeat units in the polymer. [ka]

[0128] (1) Synthesis of bromide-functionalized polymer (BP-CF3-Br-1). In a 100 mL three-neck flask equipped with an overhead mechanical stirrer, 7-bromo-1,1,1-trifluoroheptan-2-one (3.000 g, 12.1 mmol) and biphenyl (1.560 g, 10.1 mmol) were dissolved in methylene chloride (6.7 mL). Trifluoromethanesulfonic acid (TFSA) (6.7 mL) was then added dropwise over 30 min at 0° C. The reaction was then continued at this temperature for 24 h. The resulting viscous brown solution was slowly poured into ethanol. The precipitated solid was filtered, washed with water, and immersed in 1 M K2CO3 at room temperature for 12 h. Finally, the product was filtered, washed with water, and dried completely under vacuum at 60° C. The polymer yield was nearly 100%.1 H NMR (CDCl3, δ, ppm): 7.58 (H2, 4H), 7.36 (H1, 4H), 3.33 (H3, 2H), 2.45 (H4, 2H), 1.80 (H5, 2H), 1.45 (H7, 2H), and 1.27 (H6, 2H) (see Figure 2).

[0129] (2) Synthesis of imidazolium functionalized polymer (BP-CF3-IM-1). In a 50 mL one-neck flask equipped with a magnetic bar, bromide functionalized polymer (2.0 g, 5.2 mmol) and imidazole (1.7 g, 6.3 mmol) were added to NMP (37 mL). The solution was stirred at 75 °C for 12 h. The resulting yellow solution was used to cast a membrane. The resulting membrane was washed three times with hydrochloride solution (pH 1) and DI water and thoroughly dried at 60 °C under vacuum. The yield of polymer BP-CF3-IM-1 was nearly 100%. 1H NMR (DMSO-d6, δ, ppm): 7.70 (H2, 4H), 7.29 (H1, 4H), 7.02 (H3, 2H), 3.67 (H4, 4H), 2.27-2.19 (H5, H6, H12, 11H), 1.89 (H7, 6H), 1.38-1.07 (H8, H9, H10, 10H), 0.68 (H11, 3H) (see Figure 3).

[0130] (3) BP-CF3-IM-1 membrane casting and hydroxide exchange. Membranes were prepared by dissolving BP-CF3-IM-1 polymer (1.0 g) in NMP (10 mL) and casting on a clear glass plate at 80° C. for 8 h. The membrane (in bromide form) was peeled off from the glass plate in contact with deionized (DI) water. The hydroxide form membrane was obtained by ion exchange in 1 M KOH at 60° C. for 24 h, followed by washing and immersion in DI water under argon for 48 h to remove residual KOH.

[0131] Other BP-CF3-IM-x membranes are prepared by using different molar ratios of 7-bromo-1,1,1-trifluoroheptan-2-one and biphenyl.

[0132] (4) Alkaline stability. The alkaline stability of the imidazolium-containing polymers was evaluated under various conditions to investigate their high chemical stability. The BP-CF3-IM-1 membrane was immersed in 1 M KOH aqueous solution at 130 °C for 1200 h, and the 1H NMR spectrum showed no change before and after the alkaline test (Figure 4A). The TP-CF3-IM-1 membrane was immersed in 10 M KOH solution at 80 °C for 300 h, and no degradation was observed based on the 1H NMR spectrum shown in Figure 4B. Furthermore, the TP-CF3-IM-1 membrane was kept at 95 °C for 300 h under low relative humidity (RH) of 23.3% and 50.9%, respectively, as shown in Figure 4C, and also showed no sign of degradation. These results strongly suggested that the highly alkaline stable imidazolium cation tethered to the rigid poly(aryl alkylene) polymer backbone structure could indeed result in a remarkable chemically stable HEM.

[0133] (5) Water absorption and hydroxide conductivity. An ideal material for HEM / HEI should have good ionic conductivity with low water absorption. All membranes are expected to show very high conductivity in pure water. For example, at 20°C, the hydroxide conductivity of BP-CF3-IM-x polymer is expected to be much higher than PSFQN (reference HEM) with an IEC value of 36 mS / cm. PSFQN is derived from benzyltrimethylammonium polysulfone and has the following formula: [ka]

[0134] Increasing the temperature also increases the hydroxide conductivity of the membrane samples.

[0135] (6) Solubility and mechanical properties. The BP-CF3-IM-x polymers are expected to exhibit excellent solubility in dimethylformamide, N-methylpyrrolidone, dimethylsulfoxide, and isopropanol / water (1 / 1 weight ratio), but are expected to be insoluble in pure water and isopropanol.

[0136] (7) Hydroxide exchange membrane fuel cell (HEMFC) performance. BP-CF3-IM-x polymer membranes are expected to have excellent chemical stability, hydroxide conductivity, low water uptake, good solubility and mechanical properties, but the most practical evaluation of these materials will be their performance in HEMFC cells as HEIs in catalyst layers and as HEMs. Membrane electrode assemblies (MEAs) were fabricated using a robotic sprayer (Sono-Tek ExactaCoat) by spraying 5 cm of BP-CF3-IM-x polymer membranes on both sides. 2 The electrode ink is prepared by adding 250 mg of catalyst (Tanaka Kikinzoku Kogyo (TKK), 50% Pt on high surface area C) and the desired amount of ionomer (BP-CF3-IM-x polymer, prepared by dissolving BP-CF3-IM-x polymer in a mixture of water and isopropanol) to 10 g water and 10 g isopropanol, followed by sonication for 1 hour. The catalyst loading is 0.4 mg Pt / cm. 2 A rubber gasket, GDL (SGL25CC), and graphite flow field (ElectroChem) are added to both sides of the MEA to complete the sandwich. Performance is characterized in a fuel cell test system equipped with a backpressure module (Scribner 850e). Typically, the cells are powered at 100 mA / cm 2 for 30 minutes and then 200mA / cm 2 Activate for 30 minutes at 400° C. After activation, record the performance by measuring the current.

[0137] Example 2 Imidazolium-tethered poly(aryl alkylene) polymers were prepared from 7-bromo-1,1,1-trifluoroheptan-2-one, 1,1,1-trifluoroacetone, and p-terphenyl (designated TP-CF3-IM-x, where x is the molar ratio of 7-bromo-1,1,1-trifluoroheptan-2-one to p-terphenyl, ranging from 1 to 100). TP-CF3-IM-x was prepared in three major steps: (1) synthesis of bromide-functionalized polymer, (2) synthesis of imidazolium-functionalized polymer, and (3) membrane casting and hydroxide exchange. The reaction scheme is shown below, where n is the number of repeat units in the polymer. [ka]

[0138] (1) Synthesis of bromide-functionalized polymer (TP-CF3-Br-1). In a 100 mL three-neck flask equipped with an overhead mechanical stirrer, 7-bromo-1,1,1-trifluoroheptan-2-one (3.600 g, 14.6 mmol) and p-terphenyl (2.797 g, 12.1 mmol) were dissolved in methylene chloride (30 mL). Trifluoromethanesulfonic acid (TFSA) (30 mL) was then added dropwise over 30 min at 0° C. The reaction was then continued at this temperature for 24 h. The resulting viscous brown solution was slowly poured into ethanol. The precipitated solid was filtered, washed with water, and immersed in 1 M K2CO3 at room temperature for 12 h. Finally, the product was filtered, washed with water, and dried completely under vacuum at 60° C. The yield of the polymer was nearly 100%. 1 H NMR(CDCl3, δ, ppm):7.70(H 13 , 4H), 7.62(H1, 4H), 7.40(H2, 4H), 3.34(H4, 2H), 2.47(H 12 , 2H), 1.82(H8, 2H), 1.47(H 10 , 2H), 1.30 (H9, 2H) (Fig. 5).

[0139] (2) Synthesis of imidazolium functionalized polymer (TP-CF3-IM-1). In a 50 mL one-neck flask equipped with a magnetic bar, bromide functionalized polymer (2.0 g, 4.4 mmol) and functionalized imidazole (1.5 g, 5.5 mmol) were added to NMP (25 mL). The solution was stirred at 75 °C for 12 h. The resulting yellow solution was used to cast a membrane. The resulting membrane was washed three times with hydrochloride solution (PH=1) and DI water, and thoroughly dried at 60 °C under vacuum. The yield of polymer TP-CF3-IM-x was nearly 100%. 1H NMR (DMSO-d6, δ, ppm): 7.80 (H13, 4H), 7.72 (H1, 4H), 7.30 (H2, 4H), 7.05 (H3, 4H), 3.69~3.67 (H4, 4 H), 2.29~2.23 (H5, H6, H12, 11H), 1.91 (H7, 6H), 1.38~1.01 (H8, H9, H10, 10H), 0.68 (H11, 3H) (Figure 6).

[0140] (3) TP-CF3-IM-x membrane casting and hydroxide exchange. Membranes were prepared by dissolving TP-CF3-IM-x polymer (1.0 g) in NMP (10 mL) and casting on a clear glass plate at 80° C. for 8 h. The membrane (in bromide form) was peeled off from the glass plate in contact with deionized (DI) water. The hydroxide form membrane was obtained by ion exchange in 1 M KOH at 60° C. for 24 h, followed by washing and immersion in DI water under argon for 48 h to remove residual KOH.

[0141] (4) Water absorption and hydroxide conductivity. When x=1, TP-CF3-IM-1 has a conductivity of 31.4 mS / cm at 20°C. It has low water absorption and dimensional swelling in the bicarbonate form in pure water at 20°C to 80°C (shown in Table 1). [Table 1]

[0142] (5) Hydroxide exchange membrane fuel cell (HEMFC) performance. Although TP-CF3-IM-x polymer membranes are expected to have excellent chemical stability, hydroxide conductivity, low water uptake, good solubility and mechanical properties, the most practical evaluation of these materials will be their performance in HEMFC cells as HEIs in catalyst layers and as HEMs. Membrane electrode assemblies (MEAs) were fabricated using a robotic sprayer (Sono-Tek ExactaCoat) by spraying 5 cm on each side of the TP-CF3-IM-x polymer membrane. 2 The electrode ink is prepared by adding 250 mg of catalyst (Tanaka Kikinzoku Kogyo (TKK), 50% Pt on high surface area C) and the desired amount of ionomer (TP-CF3-IM-x polymer, prepared by dissolving BP-CF3-IM-x polymer in a mixture of water and isopropanol) to 10 g of water and 10 g of isopropanol, followed by sonication for 1 hour. The catalyst loading is 0.4 mg on the anode. Pt cm -2 PtRu / C, 0.4 mg on the cathode Pt cm -2 PtRu / C. Add rubber gaskets, GDLs (SGL25CC), and graphite flow fields (ElectroChem) on both sides of the MEA to complete the sandwich. Performance is characterized in a fuel cell test system equipped with a backpressure module (Scribner 850e) (Materials: TP100-CF3-IM-1 membrane, ionomer loading 20%, catalyst: 0.4 mg on the anode). Pt cm -2 PtRu / C, 0.4 mg on the cathode Pt cm -2 PtRu / C. Test conditions: 95°C, anode humidifier temperature: 90°C, cathode humidifier temperature: 97°C, H2 flow rate: 1.0L / min, O2 flow rate: 2.0L / min). The battery is usually driven at 100mA / cm 2 for 30 minutes and then 200mA / cm 2 Activate for 30 minutes at 40°C. After activation, record the performance by measuring the current. The results are shown in Figure 8.

[0143] (6) Hydroxide Exchange Membrane Electrolyzer (HEMEL) Performance. Although the TP-CF3-IM-x polymer membranes are expected to have excellent chemical stability, hydroxide conductivity, low water uptake, good solubility and mechanical properties, the most practical evaluation of these materials will be their performance in HEMEL cells as HEIs in the catalyst layers and as HEMs. Membrane electrode assemblies (MEAs) were fabricated by spraying 5 cm of TP-CF3-IM-x polymer membranes on both sides using a robotic sprayer (Sono-Tek ExactaCoat). 2 The electrodes were fabricated by depositing 1000 μm of Pt / cm2 on a 1000 μm-sized 10-well plate. The electrode ink was prepared by adding 250 mg of catalyst (Tanaka Kikinzoku Kogyo (TKK), 50% Pt on high surface area C) and the desired amount of ionomer (TP-CF3-IM-x polymer, prepared by dissolving TP-CF3-IM-x polymer in a mixture of water and ethanol) to 10 g of water and 10 g of ethanol, followed by sonication for 1 h. The catalyst loading was 4 mg Pt / cm2. 2 The Pt-coated Ti plate and TGP-H-060 Toray carbon paper (5% wetproof) were the gas diffusion layers on the anode and cathode sides, respectively. The temperature of the cell and deionized water were maintained at a constant temperature. The performance was characterized with an Arbin test system (Material: TP100-CF3-IM-1 membrane, ionomer loading 30%, catalyst: 4.0 mg on the anode). Pt cm -2 Pt / C, 2.9 mg cm on the cathode -2 IrO2. Test conditions: 80°C water and electrolytic cell, water flow rate: 3.0mL / min. Normally, the battery is charged at 100mA / cm 2 for 30 minutes and then 200mA / cm 2 The electrode was activated at 400 K for 30 minutes. After activation, the performance was recorded by measuring the current. The results are shown in Figure 9.

[0144] Example 3 Another imidazolium-tethered poly(aryl alkylene) polymer is prepared from 7-bromo-1,1,1-trifluoroheptan-2-one, 1,1,1-trifluoroacetone, and m-terphenyl (referred to as mTP-CF3-IM-x, where x is the molar ratio of 7-bromo-1,1,1-trifluoroheptan-2-one to biphenyl, ranging from 1 to 100). mTP-CF3-IM-x is prepared in three major steps similar to TP-CF3-IM-x: (1) synthesis of bromide-functionalized polymer, (2) synthesis of imidazolium-functionalized polymer, and (3) membrane casting and hydroxide exchange. The reaction scheme is shown below, where n is the number of repeat units in the polymer. [ka]

[0145] Example 4 Another method to prepare the BP-CF3-IM-x polymer of Example 1 is from the reaction of imidazolium-functionalized 7-bromo-1,1,1-trifluoroheptan-2-one, 1,1,1-trifluoroacetone, and biphenyl (referred to as BP-CF3-IM-x, where x is the molar ratio of imidazolium-functionalized 7-bromo-1,1,1-trifluoroheptan-2-one to biphenyl, which ranges from 1 to 100). BP-CF3-IM-x is prepared in two major steps: (1) synthesis of the imidazolium-functionalized polymer, and (2) membrane casting and hydroxide exchange. The reaction scheme is shown below, where n is the number of repeat units in the polymer. [ka]

[0146] Example 5 Another method to prepare the TP-CF3-IM-x polymer of Example 2 is from the reaction of imidazolium-functionalized 7-bromo-1,1,1-trifluoroheptan-2-one, 1,1,1-trifluoroacetone, and p-terphenyl (referred to as TP-CF3-IM-x, where x is the molar ratio of imidazolium-functionalized 7-bromo-1,1,1-trifluoroheptan-2-one to p-terphenyl, which ranges from 1 to 100). TP-CF3-IM-x is prepared in two major steps: (1) synthesis of the imidazolium-functionalized polymer, and (2) membrane casting and hydroxide exchange. The reaction scheme is shown below, where n is the number of repeat units in the polymer. [ka]

[0147] Example 6 Another method to prepare m-TP-CF3-IM-x in Example 3 is from the reaction of imidazolium-functionalized 7-bromo-1,1,1-trifluoroheptan-2-one, 1,1,1-trifluoroacetone, and m-terphenyl (referred to as mTP-CF3-IM-x, where x is the molar ratio of imidazolium-functionalized 7-bromo-1,1,1-trifluoroheptan-2-one to m-terphenyl, which ranges from 1 to 100). mTP-CF3-IM-x is prepared in two major steps: (1) synthesis of imidazolium-functionalized polymer, and (2) membrane casting and hydroxide exchange. The reaction scheme is shown below, where n is the number of repeat units in the polymer. [ka]

[0148] Example 7 Imidazolium-tethered poly(crown ether) polymers were prepared from 7-bromo-1,1,1-trifluoroheptan-2-one, 1,1,1-trifluoroacetone, and dibenzo-18-crown-6 (designated PCE-C5-IM-x, where x is the molar ratio of 7-bromo-1,1,1-trifluoroheptan-2-one to dibenzo-18-crown-6, ranging from 1 to 100). PCE-C5-IM-x was prepared in three major steps: (1) synthesis of bromide-functionalized polymer, (2) synthesis of imidazolium-functionalized polymer, and (3) membrane casting and hydroxide exchange. The reaction scheme is shown below, where n is the number of repeat units in the polymer. [ka]

[0149] Synthesis of bromide-functionalized polymer (PCE-C5-Br-1). In a 250 mL three-neck flask equipped with an overhead mechanical stirrer, dibenzo-18-crown-6 (7.2082 g, 20.00 mmol) and 7-bromo-1,1,1-trifluoroheptan-2-one (5.9294 g, 24.00 mmol) were suspended in chloroform (35 mL). Then, TFSA (30 mL) was slowly added dropwise at -15 °C. Then, the reaction was continued at 0 °C for 8 h. The resulting viscous solution was slowly poured into ethanol. The white fibrous solid was filtered, washed with water, and soaked in 1 M K2CO3 at 50 °C for 12 h. Finally, the white fibrous product was filtered, washed with water, and dried completely under vacuum at 60 °C. The yield of the polymer was 95%. 1 H NMR (CDCl3, δ, ppm): 6.82-6.68 (6H), 4.15-3.96 (16H), 3.33 (2H), 2.27 (2H), 1.76 (2H), 1.38 (2H), 1.15 (2H) (see Figure 10).

[0150] Synthesis of imidazolium functionalized polymer (PCE-C5-IM-Br-1). In a 50 mL one-neck flask equipped with a magnetic bar, the bromide functionalized polymer (1.0 g, 1.7 mmol) and imidazole (0.5 g, 1.9 mmol) were added to DMSO (20 mL). The solution was stirred at 60° C. for 24 h. The resulting yellow solution was used to cast a membrane. The resulting membrane was washed three times with hydrochloride solution (pH 1) and DI water and thoroughly dried at 60° C. under vacuum. The yield of polymer PCE-C5-IM-Br-1 was 90%. 1H NMR (DMSO-d6, δ, ppm): 7.14 (2H), 6.91-6.61 (6H), 4.06-3.66 (20H), 2.34 (2H), 2.34-2.30 (9H), 1.94 (6H), 1.40-1.38 (6H), 1.16-1.14 (4H), 0.72 (3H) (see Figure 11)

[0151] PCE-C5-IM OH-1 membrane casting and hydroxide exchange. Membranes were prepared by dissolving PCE-C5-IM-Br-1 polymer (1.0 g) in NMP (10 mL) and casting on a clear glass plate at 80 °C for 8 h. The membrane (in bromide form) was peeled off from the glass plate in contact with deionized (DI) water. The hydroxide form membrane was obtained by ion exchange in 1 M KOH at 60 °C for 24 h, followed by washing and immersion in DI water under argon for 48 h to remove residual KOH.

[0152] Example 8 Another imidazolium-tethered poly(crown ether) polymer is prepared from 7-bromo-1,1,1-trifluoroheptan-2-one, 1,1,1-trifluoroacetone, and dibenzo-18-crown-6 (designated PCE-C5-IM-x, where x is the molar ratio of 7-bromo-1,1,1-trifluoroheptan-2-one to dibenzo-18-crown-6, ranging from 1 to 100). PCE-C5-IM-x is prepared in three major steps similar to PCE-C5-IM-1: (1) synthesis of bromide-functionalized polymer, (2) synthesis of imidazolium-functionalized polymer, and (3) membrane casting and hydroxide exchange. The reaction scheme is shown below, where n is the number of repeat units in the polymer. [ka]

[0153] Example 9 Another method to prepare PCE-C5-IM-x in Example 8 is from the reaction of imidazolium-functionalized 7-bromo-1,1,1-trifluoroheptan-2-one, 1,1,1-trifluoroacetone, and dibenzo-18-crown-6 (referred to as PCE-C5-IM-x, where x is the molar ratio of imidazolium-functionalized 7-bromo-1,1,1-trifluoroheptan-2-one to PCE-C5-IM-x, which is 1 to 100). PCE-C5-IM-x is prepared in two major steps: (1) synthesis of imidazolium-functionalized polymer, and (2) membrane casting and hydroxide exchange. The reaction scheme is shown below, where n is the number of repeat units in the polymer. [ka]

[0154] Example 10 A quaternary ammonium-tethered poly(crown ether) polymer was prepared from 7-bromo-1,1,1-trifluoroheptan-2-one and dibenzo-18-crown-6 (designated PCE-C5-QA-x, where x is the molar ratio of 7-bromo-1,1,1-trifluoroheptan-2-one to dibenzo-18-crown-6, ranging from 1 to 100). PCE-C5-QA-x was prepared in three major steps: (1) synthesis of bromide-functionalized polymer, (2) synthesis of quaternary ammonium-functionalized polymer, and (3) membrane casting and hydroxide exchange. The reaction scheme is shown below, where n is the number of repeat units in the polymer. [ka]

[0155] Example 11 A quaternary ammonium-tethered poly(crown ether) polymer was prepared from 7-bromo-1,1,1-trifluoroheptan-2-one, 1,1,1-trifluoroacetone, and dibenzo-18-crown-6 (designated PCE-C5-IM-x, where x is the molar ratio of 7-bromo-1,1,1-trifluoroheptan-2-one to dibenzo-18-crown-6, ranging from 1 to 100). PCE-C5-QA-x is prepared in three major steps: (1) synthesis of bromide-functionalized polymer, (2) synthesis of quaternary ammonium-functionalized polymer, and (3) membrane casting and hydroxide exchange. The reaction scheme is shown below, where n is the number of repeat units in the polymer. [ka]

[0156] definition As used herein, the term "suitable substituent" is intended to mean a chemically acceptable functional group, preferably a moiety that does not nullify the activity of the compound of the present invention.Such suitable substituents include, but are not limited to, halo group, perfluoroalkyl group, perfluoroalkoxy group, alkyl group, alkenyl group, alkynyl group, hydroxy group, oxo group, mercapto group, alkylthio group, alkoxy group, aryl or heteroaryl group, aryloxy or heteroaryloxy group, aralkyl or heteroaralkyl group, aralkoxy or heteroaralkoxy group, HO-(C=O)- group, heterocyclic group, cycloalkyl group, amino group, alkyl- and dialkylamino group, carbamoyl group, alkylcarbonyl group, alkoxycarbonyl group, alkylaminocarbonyl group, dialkylaminocarbonyl group, arylcarbonyl group, aryloxycarbonyl group, alkylsulfonyl group, and arylsulfonyl group.Those skilled in the art will understand that many substituents can be substituted by additional substituents.

[0157] As used herein, the term "alkyl" refers to a straight chain, branched or cyclic hydrocarbon radical, preferably having 1 to 32 carbon atoms (i.e., 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 39, 30, 31, or 32 carbons), more preferably having 1 to 18 carbon atoms. Alkyl groups include, but are not limited to, methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, and tert-butyl. Alkyl groups can be unsubstituted or substituted with one or more suitable substituents.

[0158] As used herein, the term "alkenyl" refers to a straight-chain, branched or cyclic hydrocarbon radical, preferably having 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 39, 30, 31, or 32 carbons, more preferably having 1 to 18 carbon atoms, and having one or more carbon-carbon double bonds. Alkenyl groups include, but are not limited to, ethenyl, 1-propenyl, 2-propenyl (allyl), iso-propenyl, 2-methyl-1-propenyl, 1-butenyl, and 2-butenyl. Alkenyl groups can be unsubstituted or substituted with one or more suitable substituents, as defined above.

[0159] As used herein, the term "alkynyl" refers to a straight-chain, branched or cyclic hydrocarbon radical, preferably having 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 39, 30, 31, or 32 carbons, more preferably having 1 to 18 carbon atoms, and having one or more carbon-carbon triple bonds. Alkynyl groups include, but are not limited to, ethynyl, propynyl, and butynyl. Alkynyl groups can be unsubstituted or substituted with one or more suitable substituents, as defined above.

[0160] The term "aryl" or "ar" as used herein alone or as part of another group (e.g., aralkyl) means a monocyclic, bicyclic, or tricyclic aromatic radical, such as phenyl, naphthyl, tetrahydronaphthyl, indanyl, and the like, optionally substituted with one or more suitable substituents, preferably 1 to 5 suitable substituents, as defined above. The term "aryl" also includes heteroaryl.

[0161] "Arylalkyl" or "aralkyl" refers to an aryl group attached to a parent molecule via an alkylene group. The number of carbon atoms in the aryl and alkylene groups is selected so that there are a total of about 6 to about 18 carbon atoms in the arylalkyl group. A preferred arylalkyl group is benzyl.

[0162] As used herein, the term "cycloalkyl" refers to a monocyclic, bicyclic or tricyclic carbocyclic radical (e.g., cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl, cyclooctyl, cyclononyl, cyclopentenyl, cyclohexenyl, bicyclo[2.2.1]heptanyl, bicyclo[3.2.1]octanyl, bicyclo[5.2.0]nonanyl, etc.), optionally containing one or two double bonds. Cycloalkyl groups can be unsubstituted or substituted with one or more suitable substituents, preferably 1 to 5 suitable substituents, as defined above.

[0163] When used as a suffix as part of another group, the term "-ene" represents a divalent radical in which a hydrogen atom is removed from each of the two terminal carbons of the group, or, if the group is cyclic, from each of two different carbon atoms within the ring. For example, alkylene represents a divalent alkyl group such as ethylene (-CH2CH2-) or isopropylene (-CH2(CH3)CH2-). For clarity, the addition of the suffix -ene is not intended to change the definition of the main word other than to represent a divalent radical. Thus, continuing with the above example, alkylene represents an optionally substituted straight chain saturated divalent hydrocarbon radical.

[0164] As used herein, the term "ether" refers to a divalent (ie, difunctional) group that contains at least one ether linkage (ie, --O--).

[0165] As used herein, the term "heteroaryl" refers to a monocyclic, bicyclic, or tricyclic aromatic heterocyclic group containing in the ring one or more heteroatoms (e.g., 1-3 heteroatoms) selected from O, S, and N. Heteroaryl groups include, but are not limited to, pyridyl, pyrazinyl, pyrimidinyl, pyridazinyl, thienyl, furyl, imidazolyl, pyrrolyl, oxazolyl (e.g., 1,3-oxazolyl, 1,2-oxazolyl), thiazolyl (e.g., 1,2-thiazolyl, 1,3-thiazolyl), pyrazolyl, tetrazolyl, triazolyl (e.g., 1,2,3-triazolyl, 1,2,4-triazolyl), oxadiazolyl (e.g., 1,2,3-oxadiazolyl), thiadiazolyl (e.g., 1,3,4-thiadiazolyl), quinolyl, isoquinolyl, benzothienyl, benzofuryl, and indolyl. A heteroaryl group can be unsubstituted or substituted with one or more suitable substituents, preferably 1 to 5 suitable substituents, as defined above.

[0166] As used herein, the term "hydrocarbon" refers to compounds or radicals consisting solely of the elements carbon and hydrogen.

[0167] The term "substituted" means that in the group in question, at least one hydrogen atom bonded to a carbon atom is replaced with one or more substituents, such as hydroxy (-OH), alkylthio, phosphino, amido (-CON(RA)(RB), where RA and RB are independently hydrogen, alkyl, or aryl), amino (-N(RA)(RB), where RA and RB are independently hydrogen, alkyl, or aryl), halo (fluoro, chloro, bromo, or iodo), silyl, nitro (-NO), ether (-ORA, where RA is alkyl or aryl), ester (-OC(O)RA, where RA is alkyl or aryl), keto (-C(O)RA, where RA is alkyl or aryl), heterocyclo, and the like. When the term "substituted" introduces or follows a list of possible substituents, it is intended that the term apply to all members of the group. That is, the phrase "optionally substituted alkyl or aryl" should be interpreted as "optionally substituted alkyl or optionally substituted aryl." Similarly, the phrase "alkyl or aryl optionally substituted with fluoride" should be interpreted as "alkyl optionally substituted with fluoride or aryl optionally substituted with fluoride."

[0168] The term "tethered" means that the group in question is attached to the designated polymer backbone. For example, an imidazolium-tethered poly(aryl alkylene) polymer is a polymer having imidazolium groups attached to a poly(aryl alkylene) polymer backbone.

[0169] In presenting elements of the invention or preferred embodiments thereof, the articles "a," "an," "the," and "said" are intended to mean that there are one or more of the elements. The terms "comprising," "including," and "having" are intended to be inclusive and mean that there may be additional elements other than the listed elements.

[0170] In view of the above, it will be seen that the several objects of the invention are achieved and other advantageous results attained.

[0171] Because various changes can be made in the products and methods described above without departing from the scope of the invention, it is intended that all matter contained in the above description and shown in the accompanying drawings be interpreted as illustrative and not in a limiting sense.

Claims

1. A polymer comprising structural units of formulae (1A), (3′A), optionally (3A), and optionally (4A), wherein said structural units of formulae (1A), (3A), (3′A), and (4A) have the following structure: 【Chemistry 1】 During the ceremony, R 11 are each independently a quaternary ammonium or phosphonium group, or a nitrogen-containing heterocyclic group or a salt thereof, said quaternary ammonium or phosphonium group having the formula (5A): 【Chemistry 2】 the nitrogen-containing heterocyclic group is an optionally substituted pyrrole, pyrroline, pyrazole, pyrazoline, imidazole, imidazoline, triazole, pyridine, triazine, pyrazine, pyridazine, pyrimidine, azepine, quinoline, piperidine, pyrrolidine, pyrazolidine, imidazolidine, azepane, isoxazole, isoxazoline, oxazole, oxazoline, oxadiazole, oxatriazole, dioxazole, oxazine, oxadiazine, isoxazolidine, morpholine, thiazole, isothiazole, oxathiazole, oxathiazine, or caprolactam, each substituent being independently alkyl, alkenyl, alkynyl, aryl, or aralkyl; R 20 , R 30 , R 40 , R 50 , R 60 , R 70 , R 80 , R 90 , R 130 , R 140 , R 150 , R 160 , and R 170 are each independently hydrogen, a halide, an alkyl, an alkenyl, an alkynyl, or an aryl, wherein the alkyl, alkenyl, alkynyl, or aryl is optionally substituted with a halide; R 30 and R 60 are optionally joined to form a five-membered ring optionally substituted with halide or alkyl; Each R 100 is independently an alkyl, alkenyl, alkynyl, or a substituent having the formula (4B): 【Chemistry 3】 the alkyl, alkenyl, or alkynyl is optionally substituted with fluoride; R 180 and R 240 are each independently alkylene; R 190 , R 200 , R 210 , R 220 , and R 230 are each independently alkyl, alkenyl, or alkynyl; q is 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, or 20; m is 0, 1, 2, 3, 4, 5, or 6; n is 0, 1, 2, or 3; each m′ and each n′ is independently 0, 1, or 2; the benzo ring of formula (3'A) shown by the dashed bond is either present or absent; X - is an anion, Z is N or P, an anion exchange polymer.

2. A polymer comprising the reaction product of a polymerization mixture, (i) a cationically functionalized trifluoromethyl ketone monomer having the formula: 【Chemistry 4】 (ii) a crown ether monomer having the formula: 【Chemistry 5】 (iii) optionally, an aromatic monomer having the formula: 【Chemistry 6】 and (iv) optionally, a trifluoromethyl ketone monomer having the formula: 【Chemistry 7】 During the ceremony, R 1 are each independently a quaternary ammonium or phosphonium group, or a nitrogen-containing heterocyclic group or a salt thereof, said quaternary ammonium or phosphonium group having the formula (5A): 【Chemistry 8】 the nitrogen-containing heterocyclic group is an optionally substituted pyrrole, pyrroline, pyrazole, pyrazoline, imidazole, imidazoline, triazole, pyridine, triazine, pyrazine, pyridazine, pyrimidine, azepine, quinoline, piperidine, pyrrolidine, pyrazolidine, imidazolidine, azepane, isoxazole, isoxazoline, oxazole, oxazoline, oxadiazole, oxatriazole, dioxazole, oxazine, oxadiazine, isoxazolidine, morpholine, thiazole, isothiazole, oxathiazole, oxathiazine, or caprolactam, each substituent being independently alkyl, alkenyl, alkynyl, aryl, or aralkyl; R 2 , R 3 , R 4 , R 5 , R 6 , R 7 , R 8 , R 9 , R 10 , R 13 , R 14 , R 15 , R 16 , and R 17 are each independently hydrogen, a halide, an alkyl, an alkenyl, an alkynyl, or an aryl, wherein the alkyl, alkenyl, alkynyl, or aryl is optionally substituted with a halide; R 3 and R 6 are optionally joined to form a five-membered ring optionally substituted with halide or alkyl; Each R 12 is independently an alkyl, alkenyl, alkynyl, or a substituent of formula (4C); 【Chemistry 9】 the alkyl, alkenyl, or alkynyl is optionally substituted with fluoride; R 180 and R 240 are each independently alkylene; R 190 , R 200 , R 210 , R 220 , and R 230 are each independently alkyl, alkenyl, or alkynyl; m is 0, 1, 2, 3, 4, 5, or 6; n is 0, 1, 2, or 3; each m′ and each n′ is independently 0, 1, or 2; q is 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, or 20; the benzo ring of formula (3') shown by the dashed bond is either present or absent; A polymer wherein X is an anion and Z is N or P.

3. a polymer comprising a second reaction product of a second polymerization mixture, a quaternary ammonium or phosphonium compound or a nitrogen-containing heterocycle or a salt thereof, and An intermediate polymer is included, The intermediate polymer is (i) a halogenated trifluoromethyl ketone monomer having the formula: 【Chemistry 10】 (ii) a crown ether monomer having the formula: 【Chemistry 11】 (iii) optionally, an aromatic monomer having the formula: 【Chemistry 12】 and (iv) optionally, a first reaction product of a first polymerization mixture comprising a trifluoromethyl ketone monomer having the formula: 【Chemistry 13】 The quaternary ammonium or phosphonium compound has the formula (5): 【Chemistry 14】 the nitrogen-containing heterocycle is an optionally substituted pyrrole, pyrroline, pyrazole, pyrazoline, imidazole, imidazoline, triazole, pyridine, triazine, pyrazine, pyridazine, pyrimidine, azepine, quinoline, piperidine, pyrrolidine, pyrazolidine, imidazolidine, azepane, isoxazole, isoxazoline, oxazole, oxazoline, oxadiazole, oxatriazole, dioxazole, oxazine, oxadiazine, isoxazolidine, morpholine, thiazole, isothiazole, oxathiazole, oxathiazine, or caprolactam, each substituent being independently alkyl, alkenyl, alkynyl, aryl, or aralkyl; R 2 , R 3 , R 4 , R 5 , R 6 , R 7 , R 8 , R 9 , R 10 , R 13 , R 14 , R 15 , R 16 , and R 17 are each independently hydrogen, a halide, an alkyl, an alkenyl, an alkynyl, or an aryl, wherein the alkyl, alkenyl, alkynyl, or aryl is optionally substituted with a halide; R 3 and R 6 are optionally joined to form a five-membered ring optionally substituted with halide or alkyl; Each R 12 is independently an alkyl, alkenyl, alkynyl, or a substituent of formula (4C); 【Chemistry 15】 the alkyl, alkenyl, or alkynyl is optionally substituted with fluoride; R 18 and R 24 are each independently alkylene; R 19 , R 20 , R 21 , R 22 , and R 23 are each independently alkyl, alkenyl, or alkynyl; R 111 is a halide, m is 0, 1, 2, 3, 4, 5, or 6; n is 0, 1, 2, or 3; each m′ and each n′ is independently 0, 1, or 2; q is 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, or 20; the benzo ring of formula (3') shown by the dashed bond is either present or absent; X − is an anion; A polymer wherein X is an anion having no negative charge and Z is N or P.

4. 13. An anion exchange polymer comprising the reaction product of a base and the polymer of claim 1.

5. An anion exchange polymer comprising the reaction product of a base and the polymer of claim 2.

6. An anion exchange polymer comprising the reaction product of a base and the polymer of claim 3.

7. The polymer of any one of claims 4 to 6, wherein the base comprises a hydroxide-containing base, a bicarbonate-containing base, or a carbonate-containing base.

8. 8. The polymer of claim 7, wherein the hydroxide-containing base comprises sodium or potassium hydroxide, the bicarbonate-containing base comprises sodium or potassium bicarbonate, or the carbonate-containing base comprises sodium or potassium carbonate.

9. R 1 Or R 11 is an optionally substituted nitrogen-containing heterocyclic group or a salt thereof.

10. The polymer of claim 9, wherein the optionally substituted nitrogen-containing heterocyclic group comprises a fully substituted pyrrole, pyrroline, pyrazole, pyrazoline, imidazole, imidazoline, triazole, pyridine, triazine, pyrazine, pyridazine, pyrimidine, azepine, or quinoline, each substituent being independently alkyl or aryl.

11. The optionally substituted nitrogen-containing heterocyclic group comprises an imidazolium having the formula (6A): 【Chemistry 16】 During the ceremony, R25, R 26 , R 27 10. The polymer of claim 9, wherein R28 is independently hydrogen, an optionally substituted alkyl, alkenyl, alkynyl, or aryl.

12. R 28 is 2,4,6-alkylphenyl, and R 25 , R 26 , and R 27 are each independently 1 ~C 6 The polymer of claim 11 which is alkyl.

13. The optionally substituted nitrogen-containing heterocyclic group having the formula: 【Chemistry 17】 The polymer of claim 9.

14. The quaternary ammonium or phosphonium group of formula (5A) is R 180 and R 240 each independently having 1 ~C 22 alkylene, R 190 , R 200 , R 210 , R 220 , and R 230 are each independently 1 ~C 6 alkyl, m is 0, 1, 2, 3, 4, 5, or 6, Z is N or P, or the quaternary ammonium or phosphonium compound of formula (5) is 18 and R 24 each independently having 1 ~C 22 alkylene, R 19 , R 20 , R 21 , R 22 , and R 23 are each independently 1 ~C 6 alkyl, m is 0, 1, 2, 3, 4, 5, or 6, and Z is N or P; or The quaternary ammonium or phosphonium group of formula (5A) is R 180 and R 240 each independently having 1 ~C 6 alkylene, R 190 , R 200 , R 210 , R 220 , and R 230 are each independently 1 ~C 6 alkyl, m is 0, 1, 2, or 3, Z is N or P, or the quaternary ammonium or phosphonium compound of formula (5) is 18 and R 24 each independently having 1 ~C 6 alkylene, R 19 , R 20 , R 21 , R 22 , and R 23 are each independently 1 ~C 6 alkyl, m is 0, 1, 2, or 3, and Z is N or P; or The quaternary ammonium or phosphonium group of formula (5A) is R 180 and R 240 each independently having 8 ~C 22 alkylene, R 190 , R 200 , R 210 , R 220 , and R 230 are each independently 1 ~C 6 alkyl, m is 0, 1, 2, or 3, Z is N or P, or the quaternary ammonium or phosphonium compound of formula (5) is 18 and R 24 each independently having 8 ~C 22 alkylene, R 19 , R 20 , R 21 , R 22 , and R 23 are each independently 1 ~C 6 alkyl, m is 0, 1, 2, or 3, and Z is N or P; or The quaternary ammonium or phosphonium group of formula (5A) is R 180 and R 240 each having C 2 ~C 6 alkylene, R 190 , R 200 , R 210 , R 220 , and R 230 are each independently methyl, m is 1, Z is N or P, or the quaternary ammonium or phosphonium compound of formula (5) is 18 and R 24 each having C 2 ~C 6 alkylene, R 19 , R 20 , R 21 , R 22 , and R 23 are each independently methyl, m is 1 and Z is N or P; or The quaternary ammonium or phosphonium group of formula (5A) is R 180 and R 240 each is n-hexylene; R 190 , R 200 , R 210 , R 220 , and R 230 are each independently methyl, m is 1, Z is N or P, or the quaternary ammonium or phosphonium compound of formula (5) is 18 and R 24 each is n-hexylene; R 19 , R 20 , R 21 , R 22 , and R 23 is independently methyl; m is 1; and Z is N or P.

15. R 1 Or R 11 is the quaternary phosphonium group or the second polymerization mixture comprises the quaternary phosphonium compound.

16. R 1 Or R 11 is the quaternary ammonium group or the second polymerization mixture comprises the quaternary ammonium compound.

17. 7. The polymer of claims 2, 3, 5, or 6, wherein the aromatic monomer of formula (3) comprises biphenyl, para-terphenyl, meta-terphenyl, para-quaterphenyl, 9,9-dimethyl-9H-fluorene, or benzene.

18. In the structural unit of the formula (3A), R 20 , R 30 , R 40 , R 50 , R 60 , R 70 , R 80 , and R 90 At least one of R is a halide or an aryl, and the aryl is optionally substituted with a halide, or in the aromatic monomer of formula (3), R 2 , R 3 , R 4 , R 5 , R 6 , R 7 , R 8 , R 9 , and R 10 at least one of is a halide or an aryl, said aryl being optionally substituted with a halide; or In the structural unit of the formula (3A), R 30 and R 60 are linked to form a five-membered ring optionally substituted with halide or alkyl, or in the aromatic monomer of formula (3), R 3 and R 6 are joined to form a five-membered ring optionally substituted with halide or alkyl, or In the structural unit of the formula (3′A), R 20 , R 40 , R 50 , R 70 , R 80 , and R 90 are each hydrogen, or in the crown ether monomer of formula (3′), R 2 , R 4 , R 5 , R 7 , R 8 , R 9 , and R 10 The polymer of any one of claims 1 to 17, wherein is hydrogen.

19. 19. The polymer of any one of claims 1 to 18, wherein the polymer comprises structural units of formula (4A) or the reaction product of the polymerization mixture further comprises a trifluoromethyl ketone monomer of formula (4).

20. 20. The polymer of claim 19, wherein the trifluoromethyl ketone monomer comprises 2,2,2-trifluoroacetophenone or 1,1,1-trifluoroacetone.

21. In the structural unit of the formula (4A), R 100 is an alkyl, alkenyl, or alkynyl, the alkyl, alkenyl, or alkynyl being optionally substituted with fluoride, or in the trifluoromethyl ketone monomer of formula (4), R 12 is alkyl, alkenyl, or alkynyl, said alkyl, alkenyl, or alkynyl being optionally substituted with fluoride; or In the structural unit of the formula (4A), R 100 is a substituent of the formula (4B), and R 130 , R 140 , R 150 , R 160 , and R 170 At least one of R is a halide or an aryl, the aryl being optionally substituted with a fluoride, or in the trifluoromethyl ketone monomer of formula (4), R 12 is a substituent of the formula (4C), and R 13 , R 14 , R 15 , R 16 , and R 17 The polymer of any one of claims 1 to 20, wherein at least one of is a halide or an aryl, said aryl being optionally substituted with fluoride.

22. R 20 , R 30 , R 40 , R 50 , R 60 , R 70 , R 80 , R 90 , R 130 , R 140 , R 150 , R 160 , and R 170 are each independently hydrogen or alkyl optionally substituted with fluoride; R 100 is an alkyl optionally substituted with a fluoride or a substituent of formula (4B) above, or R 2 , R 3 , R 4 , R 5 , R 6 , R 7 , R 8 , R 9 , R 10 , R 13 , R 14 , R 15 , R 16 , and R 17 are each independently hydrogen or alkyl optionally substituted with fluoride; R 12 is an alkyl optionally substituted with a fluoride or a substituent of formula (4C) above; or R 20 , R 30 , R 40 , R 50 , R 60 , R 70 , R 80 , R 90 , R 130 , R 140 , R 150 , R 160 , and R 170 are each independently hydrogen, methyl, ethyl, propyl, butyl, pentyl, or hexyl, or methyl, ethyl, propyl, butyl, pentyl, or hexyl optionally substituted with fluoride; R 100 is methyl, ethyl, propyl, butyl, pentyl, or hexyl optionally substituted with fluoride or a substituent of formula (4B), or R 2 , R 3 , R 4 , R 5 , R 6 , R 7 , R 8 , R 9 , R 10 , R 13 , R 14 , R 15 , R 16 , and R 17 are each independently hydrogen, methyl, ethyl, propyl, butyl, pentyl, or hexyl, or methyl, ethyl, propyl, butyl, pentyl, or hexyl optionally substituted with fluoride; R 12 22. The polymer of any one of claims 1 to 21, wherein is methyl, ethyl, propyl, butyl, pentyl, or hexyl optionally substituted with fluoride or a substituent of formula (4C).

23. X - However, hydroxides, halides, BF 4 - , P.F. 6 - , CO 3 2- , or HCO 3 - The polymer of any one of claims 1 to 22, comprising:

24. The sum of the molar fractions of the structural units of formula (1A) and formula (4A) in the polymer is approximately equal to the sum of the molar fractions of the structural units of formula (3A) and (3'A) in the polymer, and the ratio of the molar fraction of the structural units of formula (1A) in the polymer to the sum of the molar fractions of the structural units of formula (3A) and (3'A) in the polymer is about 0.01 to 1; or the molar ratio of the sum of the molar fractions of the structural units of formula (1A) and formula (4A) to the sum of the molar fractions of the structural units of formula (3A) and (3'A) in the polymer is from about 0.95:1 to about 1.4:1, and the ratio of the molar fraction of the structural units of formula (1A) to the sum of the molar fractions of the structural units of formula (3A) and (3'A) is from about 0.01 to 1; or The polymer according to claim 1 or 4, wherein the molar ratio of the sum of the molar fractions of structural units of formula (1A) and formula (4A) to the sum of the molar fractions of structural units of formula (3A) and (3'A) in the polymer is from about 1:1 to about 1.2:

1.

25. Said X - But, OH - and The polymer has a water absorption rate of 47% or less based on the dry weight of the polymer when immersed in pure water at 80° C., or has a hydroxide conductivity of at least 31 mS / cm in pure water at 20° C., and the polymer is stable to decomposition when immersed in 1M potassium hydroxide at 130° C. for 1,200 hours; or the polymer is stable to degradation when immersed in 10M potassium hydroxide at 80° C. for 300 hours; or the polymer is stable to degradation when kept at 95° C. for 300 hours at relative humidity of 23.3% and 50.9%, or The polymer has a tensile strength of at least 30 MPa and / or an elongation at break of at least 250%. The polymer according to any one of claims 1 to 24, which is at least one of:

26. The nitrogen-containing heterocyclic group contains imidazole, and the X - But, OH - and The polymer is used as a hydroxide exchange membrane in a hydroxide exchange membrane fuel cell, loaded at 20% as a hydroxide exchange ionomer in the cathode and anode catalyst layers of the fuel cell, and the fuel cell is loaded with 0.4 mg of ethylenediaminetetraacetate on the anode. Pt cm -2 PtRu / C, and the test conditions were 1.0 L / min H 2 Flow rate: 2.0 L / min O 2 flow rate, a cell temperature of 95° C., and anode and cathode humidifier temperatures of 90° C. and 97° C., respectively. 2 or The polymer was used as a hydroxide exchange membrane in a hydroxide exchange membrane water electrolyser, loaded at 30% as a hydroxide exchange ionomer in the cathode and anode catalyst layers of the electrolyser, and the electrolyser was loaded at 4.0 mg cm for Pt / C catalyst on the cathode. -2 and IrO on the anode 2 2.9 mg cm for catalyst -2 and having a current of at least 20 mA / cm when the voltage is 1.8 volts, when the test conditions are a water flow rate of 3.0 mL / min, a cell temperature of 80° C., and a water temperature of 80° C. 2 10. The polymer of claim 9 having a current density of

27. A method for making an anion exchange polymer membrane comprising the polymer of claim 5, comprising the steps of: reacting the cationically functionalized trifluoromethyl ketone monomer, the optional trifluoromethyl ketone monomer, the optional aromatic monomer, and the crown ether monomer in the presence of an organic solvent and a polymerization catalyst to form a cationically functionalized intermediate polymer; dissolving the cationically functionalized intermediate polymer in a solvent to form a polymer solution; casting the polymer solution to form a polymer film; exchanging the anions of said polymer membrane with hydroxide ions, bicarbonate ions, or carbonate ions, or a combination thereof, to form said anion exchange polymer membrane.

28. A method for making an anion exchange polymer membrane comprising the polymer of claim 6, comprising the steps of: reacting the halogenated trifluoromethyl ketone monomer, the optional trifluoromethyl ketone monomer, the optional aromatic monomer and the crown ether monomer in the presence of an organic solvent and a polymerization catalyst to form a halogen-functionalized polymer; reacting the halogen-functionalized polymer with the quaternary phosphonium compound or the nitrogen-containing heterocycle or salt thereof in the presence of an organic solvent to form a cationically functionalized polymer; dissolving the cationically functionalized polymer in a solvent to form a polymer solution; casting the polymer solution to form a polymer film; exchanging the anions of said polymer membrane with hydroxide ions, bicarbonate ions, or carbonate ions, or a combination thereof, to form said anion exchange polymer membrane.

29. the polymerization catalyst comprises trifluoromethanesulfonic acid, pentafluoroethanesulfonic acid, heptafluoro-1-propanesulfonic acid, trifluoroacetic acid, perfluoropropionic acid, heptafluorobutyric acid, or a combination thereof; and / or 29. The method of claim 27 or 28, wherein each of the organic solvents independently comprises dimethylsulfoxide, 1-methyl-2-pyrrolidinone, 1-methyl-2-pyrrolidone, dimethylformamide, methylene chloride, trifluoroacetic acid, trifluoromethanesulfonic acid, chloroform, 1,1,2,2-tetrachloroethane, dimethylacetamide, or a combination thereof, and the solvent in the dissolving step comprises methanol, ethanol, n-propanol, isopropanol, n-butanol, sec-butanol, tert-butanol, pentanol, hexanol, dimethylsulfoxide, 1-methyl-2-pyrrolidone, dimethylformamide, chloroform, ethyl lactate, tetrahydrofuran, 2-methyltetrahydrofuran, water, phenol, acetone, or a combination thereof.

30. Fuel cells, electrolyzers, electrodialysis equipment, solar hydrogen generators, flow batteries, desalination equipment, sensors, water demineralization, ultrapure water generation, wastewater treatment, ion exchange equipment, or CO 2 An anion exchange membrane, optionally configured and sized to be suitable for use in a separator, comprising a polymer according to any one of claims 4 to 6.

31. An anion exchange membrane fuel cell, an electrolyzer, an electrodialysis device, a solar hydrogen generator, a flow battery, a desalination device, a sensor, a demineralizer, a water purifier, a wastewater treatment system, an ion exchange device, or a CO 2 separator.

32. Fuel cells, electrolyzers, electrodialysis equipment, solar hydrogen generators, flow batteries, desalination equipment, sensors, demineralization equipment, water purifiers, wastewater treatment systems, ion exchange equipment, or CO 2 7. A reinforced electrolyte membrane, optionally configured and sized to be suitable for use in a separator, said membrane comprising a porous substrate impregnated with the polymer of any one of claims 4 to 6.

33. the porous substrate comprises a membrane of polytetrafluoroethylene, polypropylene, polyethylene, polyetherketone, polyaryletherketone, imidazole-tethered poly(arylalkylene), imidazolium-tethered poly(arylalkylene), polysulfone, perfluoroalkoxyalkane, or fluorinated ethylene propylene polymer, which membrane is optionally a dimensionally stable membrane; and / or below: the porous substrate has a porous microstructure of polymer fibrils; or the interior volume of the porous substrate is substantially occluded by impregnation with the polymer; or the porous substrate comprises a microstructure of nodes interconnected by fibrils; or the porous substrate has a thickness of from about 1 micron to about 100 microns; or the membrane is prepared by multiple impregnation of the substrate with the polymer; or The membrane, wetting the porous substrate with a liquid to form a wet substrate; dissolving the polymer in a solvent to form a homogeneous solution; applying the solution onto the wet substrate to form the reinforced membrane; drying the membrane; and is adjusted by 33. The membrane of claim 32, wherein the at least one of

Citation Information

Patent Citations

  • Novel polymer and its production method

    JP2018502180A

  • Anion exchange polymers and anion exchange membranes incorporating same

    US20170252707A1

  • Phosphate anion-quaternary ammonium ion pair coordinated polymer membranes

    WO2020112721A1