Polymer Compositions Containing Phosphonate Flame Retardants - Patent application

Aminomethylbisphosphonate flame retardants with specific functional groups address the limitations of existing flame retardants by providing high thermal stability and reduced smoke gas production, ensuring effective flame retardancy and material compatibility in polymeric materials.

JP7591556B2Active Publication Date: 2024-11-28CHEM FAB BUDENHEIM AG
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2022506956
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-02-13
Filing Date
2020-08-12
Publication Date
2024-11-28
Estimated Expiration
2040-08-12

AI Technical Summary

Technical Problem

Existing flame retardants, particularly halogenated phosphates, pose environmental and health risks, are difficult to incorporate into polymeric materials, and their use at low concentrations is limited by low thermal stability and high smoke gas production during decomposition.

Method used

Development of aminomethylbisphosphonate-based flame retardants with specific functional groups that allow for incorporation at low concentrations, providing high thermal stability and reduced smoke gas production by forming stable phosphonate groups at the alpha position to nitrogen, enhancing flame retardancy and compatibility with polymeric materials.

Benefits of technology

The aminomethylbisphosphonate flame retardants exhibit improved thermal stability, reduced smoke gas generation, and effective flame retardancy even at low concentrations, maintaining material properties and processability of polymeric materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007591556000056
    Figure 0007591556000056
  • Figure 0007591556000057
    Figure 0007591556000057
  • Figure 0007591556000058
    Figure 0007591556000058
Patent Text Reader

Abstract

The present invention relates to compounds comprising a polymeric material and an aminomethylbisphosphonate-based phosphorus-based flame retardant, methods for making the compounds, uses of the flame retardant, and selected structures of the flame retardant.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to compounds comprising polymeric materials and aminomethylbisphosphonate-based phosphorus-based flame retardants, methods for making the compounds, uses of the flame retardants, and selected structures of the flame retardants. [Background technology]

[0002] Several substances are known to provide flame retardancy to polymeric materials, either alone or in combination with other substances that provide similar or additional flame retardancy. The best known flame retardants are halogenated organic compounds, metal hydroxides, organic or inorganic phosphates, phosphonates, phosphinates, and derivatives of 1,3,5-triazine compounds and mixtures thereof. Flame retardants are classified into low molecular and high molecular types. Polymeric flame retardants, such as the halogenated polyol Exolit OP550 from Clariant, advantageously have only a slight softening effect and low migration capacity in polymeric materials, but in contrast to low molecular flame retardant additives, they are often not readily miscible with the polymeric materials to be protected during technological processing, especially with their lower melting capacity. Furthermore, the addition of polymeric flame retardants can have a negative effect on the curing of the polymeric materials.

[0003] Therefore, the majority of flame retardants employed are low molecular weight compounds. Among them, phosphorus-based compounds are known to be particularly good in this field. In flame, they form a voluminous protective layer in the polymer material, which is called intumescent. In the process, an insulating layer is formed that blocks the supply of oxygen and prevents the polymer material from continuing to burn. In the solid phase, the flame retardant effect can also be based on an increase in the carbonization rate of the polymer material or on the formation of inorganic glasses. Flame retardant activity is also promoted by a gas-phase mechanism that involves a radical combination with PO radicals generated by the combustion of phosphorus compounds, which significantly slows down the combustion process of the polymer material. The halogenated phosphates tris(2-chloroethyl)phosphate (TCEP) and tris(2-chloroisopropyl)phosphate (TCPP) are the most important phosphorus-based compounds. However, their use is often restricted due to their potential toxicity and the ecological problems associated with their use, since such phosphates are bioaccumulative and are very difficult to remove from wastewater in municipal water treatment plants. They also contain halogens, which generate and release toxic compounds such as HX gas in the flame. Such corrosive fire gases pose a particular risk in electronic equipment applications.

[0004] The phosphorus-based flame retardant options are halogenated phosphates and halogen-free phosphates. Compared to the phosphates, these have a particularly pronounced flame retardant gas-phase activity. German published patent DE 2128060 describes the use of aminomethanephosphonic esters with phosphorus concentrations of up to 23.2% by weight as flame retardants in polyurethanes. The aminomethanephosphonic esters are prepared from hexamethylenetetramine and dialkyl or diaryl phosphonates. These phosphonates are used by dissolving them in the polyol component of the polyurethane-forming mixture together with other necessary additives, followed by the addition of a polyisocyanate. The esters bearing NH groups are incorporated into the polymeric material by addition to the isocyanate groups.

[0005] European Patent Application No. EP0001996 relates to the preparation of N,N-bis-(2-hydroxyalkyl)aminomethane-phosphonic acid dimethyl esters, which are primarily used as flame retardant additives in polymeric materials, especially polyurethanes. They are synthesized by adding H-acid compounds as catalysts to a mixture of dimethyl phosphite and oxazolidine. These products have terminal secondary hydroxyl groups and can be incorporated into the polymeric material when the polymeric components of the polyurethane-forming mixture are added. However, the added H-acidic substances may remain in the polymeric material and impair its properties. Alternatively, they need to be converted to the corresponding alkali salts and separated from the phosphonic acid esters before adding the polyol components.

[0006] Canadian Patent No. CA2027078 relates to aminomethanephosphonic acid aryl esters, which can be used as flame retardants in foams, thermoplastics, and thermosets. The corresponding compounds are produced by reacting amines with trialkyl or triaryl phosphites and paraformaldehyde. The compounds can be added to polymeric materials processed in extrusion processes or used as additives of co-condensation components in condensation reactions of polymers.

[0007] Liu et al., Ind. Eng. Chem. Res. (2017), 56, 8789-8696, discuss flame-retardant DOPO derivatives made from DOPO (9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide), paraformaldehyde and piperazine. These are halogen-free and can be used in polycarbonates to provide flame retardancy. However, these compounds, like those in the above literature, only have low thermal stability, which is due to the weak PC bond of the P-CH2N group. Although the PC bond is basically chemically and thermally stable, the α-amino group stabilizes the carbon radicals generated by homolysis, and as a result, the PC bond of these flame retardants is already broken at relatively low temperatures. Tertiary amines formed by homolysis have a small molar mass, so they dissipate as volatile components and lose their mass accordingly. If the flame retardant is incorporated into a polymeric material, the release of the amines will cause smoke gas to rise. Due to the low decomposition temperature of the flame retardants, they are partially decomposed during the molding process of the polymeric material they are incorporated in. Another drawback of these flame retardants is that due to the low phosphorus concentration, they must be added to the polymeric material in high concentrations, which significantly impairs the processability, flexibility and other product properties of the polymeric material. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] German published patent no. DE2128060 [Patent Document 2] European Patent Application No. EP0001996 [Patent Document 3] Canadian Patent No. CA2027078 [Non-patent literature]

[0009] [Non-Patent Document 1] Liu et al., Ind.Eng.Chem.Res.(2017),56,8789-8696 Summary of the Invention [Problem to be solved by the invention]

[0010] Against this background, the object of the present invention is to provide a composition using a polymeric material, which has a flame retardant with flame retardant properties equal to or better than those known in the prior art, which can be used in low concentrations in the composition while providing good flame retardancy, which decomposes only at higher temperatures than the known flame retardants, preferably at temperatures much higher than the processing and / or manufacturing temperatures, and at temperatures slightly lower than or equal to the decomposition temperature of the polymeric material, and which, when decomposed in the polymeric material, gives lower smoke gas concentrations and / or reduced toxicity of the smoke gases. [Means for solving the problem]

[0011] The present invention achieves this object by defining a composition comprising a polymeric material, in particular a thermosetting polymeric material, containing and / or bonded to it a flame retardant in an amount ranging from 1 to 40% by weight relative to the total composition, said flame retardant being a compound of formula (I) or its corresponding ammonium salt, its corresponding phosphonate or a mixture thereof, [ka] (Ni)R 1 and R 2 are the same or different substituents and are selected from the group consisting of linear, branched or cyclic alkyl, alkenyl and alkynyl, unsubstituted and alkyl-substituted phenyl, mono- and polynuclear aromatics with up to four nuclei, mono- or polynuclear heteroaromatics with up to four nuclei, silyl, allyl, alkyl or aryl alcohols, or (N-ii)R 1 and R 2form a saturated, monounsaturated or polyunsaturated heterocycle having 4 to 8 ring atoms selected from carbon, oxygen, sulfur, phosphorus, silicon and nitrogen, including the N atom, and these nitrogen atoms are preferably substituted on the heterocycle with H, an alkyl, an aryl, or a methylbisphosphonate group having the following structure (II) when the heterocycle has a nitrogen atom as a ring atom: [ka] On said heterocycle, if it has carbon, phosphorus or silicon as ring atoms, these atoms are preferably H, alkyl, aryl, -NH2, -NHR, -NR2, -OH, -OR, =O, -I, -Cl, -Br, F, -N3, -SH, -SR, -OCN, epoxy, lactam, lactone, aziridine, glycolide, oxazoline, ether, alkenylene and alkynylene, -SiR x H y where R=alkyl, alkenyl, alkynyl or aryl, and x+y=3; -X- is an oxygen atom -O-, or -X- is a single bond; (Pi)R 3 , R 4 , R 5 and R 6 are the same or different substituents, and have the following structures (III) and (IV) with H, linear, branched or cyclic alkyl, alkenyl and alkynyl, unsubstituted and alkyl-substituted phenyl, polynuclear aromatics having up to four nuclei, mononuclear or polynuclear heteroaromatics having up to four nuclei, silyl, allyl, alkyl or aryl alcohol, n=0 to 100; [ka] cations selected from the group consisting of Na + , K + , Mg 2+ , Ca 2+ , B 3+ , Al 3+ , Zn 2+ , N.H.4+ or melamine or a condensate thereof, preferably the ammonium ion of an amine compound selected from the group consisting of melam, melem, melon, urea, guanidine, morpholine and piperazine; and / or (P-ii) When -X- is an oxygen atom, -O-, -OR 3 -OR 4 Both and / or -OR 5 AND -OR 6 and / or -OR 3 AND -OR 5 Both and / or -OR 4 AND -OR 6 together form a cyclic phosphonate ester or cyclic phosphonic anhydride having a ring size of 4 to 10 atoms, including the P atom of the phosphonate group, and / or (P-iii) When -X- is a single bond, -R 3 AND -OR 4 and / or -R 3 AND -OR 5 together form a cyclic phosphonic acid ester or cyclic phosphonic acid anhydride having a ring size of 4 to 10 atoms, including the P atom of the phosphinate group, and / or -OR 5 AND -OR 6 And / or -OR 4 AND -OR 6 together form a cyclic phosphonate ester or cyclic phosphonic anhydride having a ring size of 4 to 10 atoms, including the P atom of the phosphonate group; A) Substituent R 1 ~R 6 or B) 1) Substituent R 3 ~R 6 forming a cyclic phosphine or phosphonate ester according to (P-ii) or (P-iii), or 2) Substituent R 3 ~R 6 forming a cyclic phosphine or phosphonic anhydride according to (P-ii) or (P-iii), or 3) Substituent R 1 and R 2 When forming a heterocycle according to (N-ii), One of the cycles that forms in a) heteroatoms selected from the group consisting of P, O, N, S, I, Cl, Br, F, and / or b) an alkene or alkyne group and a first uncharged or negatively charged functional group having the formula: The functional group is not -OH, and when one of the cycles according to 1) to 3) has the functional group, the ring atom of the cycle is substituted with the functional group or with a substituent having the functional group. [Brief description of the drawings]

[0012] [Figure 1] Differential calorimetry of DAMP-H4 [Diagram 2] Thermogravimetric measurement of DAMP-H4 [Diagram 3] Differential calorimetry of MOMP-H4 [Figure 4] Thermogravimetric measurements of MOMP-H4 [Diagram 5] Differential calorimetry of ATMP [Figure 6] Thermogravimetric measurements of ATMPs [Figure 7] Differential calorimetry of MOMP-Et4 [Figure 8] Thermogravimetric measurements of MOMP-Et4 [Figure 9] Differential calorimetry of MOMP-DOPO2 [Figure 10] Thermogravimetric measurements of MOM-DOPO2 [Figure 11] Differential calorimetry of MOMP-H2Zn [Figure 12] Thermogravimetry of MOMP-H2Zn [Figure 13] Differential calorimetry of PIMP [Figure 14] Thermogravimetric measurements of PIMP DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] In the present invention, functional groups are defined as groups of atoms in a bond that materially determine the material properties and reaction behavior of a compound, for example because they affect the polarity of the molecule and / or because they can react with other compounds, but functional groups as defined in the present invention do not include groups of atoms in which any of the heteroatoms or alkene or alkyne groups referred to in a) are part of a ring of an aromatic system, such as aromatics or heteroaromatics.

[0014] For the purposes of the present invention, the fact that the uncharged or negatively charged functional group is not -OH does not imply that the substituent R 1 ~R 6 or a substituent R 3 ~R 6 forms a cyclic phosphine or phosphonate ester according to (P-ii) or (P-iii), or the substituent R 3 ~R 6 when forming a cyclic phosphine or phosphonic anhydride according to (P-ii) or (P-iii), or when the substituent R 1 and R 2 This does not mean that one of the cycles formed when (N-ii) forms a heterocycle cannot bear an OH group, but for the purposes of the present invention, they must additionally bear a first uncharged or negatively charged functional group as defined in claim 1.

[0015] Substituent R 1 ~R 6 or a substituent R 3 ~R 6 forms a cyclic phosphine or phosphonate ester according to (P-ii) or (P-iii), or the substituent R 3 ~R 6 when forming a cyclic phosphine or phosphonic anhydride according to (P-ii) or (P-iii), or when the substituent R 1 and R 2 One of the cycles formed when forming a heterocycle according to (N-ii) preferably does not have an OH group, which is advantageous, for example, when the OH group reacts with other additives in the polymer material.

[0016] Substituent R 1 ~R 6 When R forms a cycle according to 1) to 3), functional groups can only be placed on the substituents of ring atoms and therefore cannot be part of the ring itself. Thus, functional groups are placed on the substituents of ring atoms of the cycle, not within the cycle. 1 ~R 2 can form, for example, a morpholine ring and thus a cycle according to 3), but the ether group contained in the ring does not represent a functional group as defined in the present invention. However, the ring atoms of the morpholine can additionally be substituted either with a functional group according to the present invention or with a substituent carrying a functional group according to the present invention.

[0017] In a preferred embodiment, -X- is an oxygen atom -O-, and -OR 3 AND -OR 4 together form a cyclic phosphonate ester or cyclic phosphonic anhydride having a ring size of 4 to 10 atoms, including the P atom of the phosphonate group, -OR 5 AND -OR 6 Both of these form cyclic phosphonate esters or cyclic phosphonic anhydrides having a ring size of 4 to 10 atoms, including the P atom of the phosphonate group.

[0018] In a preferred embodiment, -X- is an oxygen atom -O-, and -OR 3 AND -OR 5 together form a cyclic phosphonate ester or cyclic phosphonic anhydride having a ring size of 4 to 10 atoms, including the P atom of the phosphonate group, -OR 4 AND -OR 6 Both of these form cyclic phosphonate esters or cyclic phosphonic anhydrides having a ring size of 4 to 10 atoms, including the P atom of the phosphonate group.

[0019] In a further preferred embodiment, -X- is a single bond and -R 3 AND -OR 4 together form a cyclic phosphinic ester or cyclic phosphinic anhydride having a ring size of 4 to 10 atoms, including the P atom of the phosphinate group, -OR 5 AND -OR6 Both of these form cyclic phosphonate esters or cyclic phosphonic anhydrides having a ring size of 4 to 10 atoms, including the P atom of the phosphonate group.

[0020] In a further preferred embodiment, -X- is a single bond and -R 3 AND -OR 5 together form a cyclic phosphinic ester or cyclic phosphinic anhydride having a ring size of 4 to 10 atoms, including the P atom of the phosphinate group, -OR 4 AND -OR 6 Both of these form cyclic phosphonate esters or cyclic phosphonic anhydrides having a ring size of 4 to 10 atoms, including the P atom of the phosphonate group.

[0021] Particularly preferably, R 1 and R 2 together with the N atom form a morpholine or piperidine ring.

[0022] In a preferred embodiment of the present invention, the substituent R 3 ~R 6 Or the cycle formed thereby has a first functional group.

[0023] In a preferred embodiment of the present invention, R 1 and R 2 together with the N atom form a heterocycle according to (N-ii), the atoms on the heterocycle, if it has carbon, phosphorus or silicon as a ring atom, are preferably H, alkyl, aryl, -NH, -NHR, -NR, -OH, -OR, =O, -I, -Cl, -Br, F, -N, -SH, -SR, -OCN, epoxy, lactam, lactone, aziridine, glycolide, oxazoline, ether, alkenylene and alkynylene, -SiR x H y where R=alkyl, alkenyl, alkynyl or aryl and x+y=3.

[0024] In a preferred embodiment of the invention, the first and / or second further functional group comprises a heteroatom from the group consisting of P, O, N, S, Si, or an alkene or alkyne group. Halogen-based substituents cause smoke to rise when the flame retardant decomposes in a flame, so by avoiding halogen-based substituents, the amount of smoke gas can be minimized.

[0025] Particularly preferably, the composition has a total halogen content of less than 1000 ppm by weight, preferably less than 850 ppm by weight. The halogen content can be measured by conventional methods known to those skilled in the art, such as combustion ion chromatography (CIC). The particularly low halogen content is advantageous compared to prior art flame retardants, since known flame retardants have undesirably high amounts of halogen in the form of inorganic and organically bound halogen. The term "halogen-free" as defined by the present invention allows for minor contamination with halogen in the aforementioned maximum values. However, halogens must generally be limited in amount to avoid the adverse effects of halogens.

[0026] In a preferred embodiment of the present invention, the substituent R 3 , R 4 , R 5 and R 6 is an organic residue, each of which has 2 or more, preferably 3 or more, carbon atoms.

[0027] The flame retardant according to the invention can be prepared using the method described in DE 3133308. According to this, alkylaminomethanediphosphonic acid or its acrylic derivatives can be obtained in very good yields when the reaction product of acetic anhydride or acetyl chloride and phosphorous acid is converted in stoichiometric ratios with alkylformamide. In order to obtain the highest possible yield, the reaction temperature of the first conversion step, for example the conversion of acetic anhydride or acetyl chloride with phosphorous acid, is kept between 40 and 60°C. Instead of the reactants acetic anhydride or acetyl chloride and phosphorous acid, the first reaction step can also be carried out with a mixture of phosphorus trichloride and acetic acid. As suitable alkylformamides, mono- and dialkylformamides such as methyl and dimethylformamide, ethyl and diethylformamide, morpholine, piperidine, pyrrolidine, oxazolidine, formyl compounds of alkanolamines are described.

[0028] The flame retardant according to the invention has a higher thermal stability than the phosphonates known in the prior art, on which carbon is substituted by nitrogen in the α-position and has only one phosphonate group. This means that the decomposition temperature is higher than that of comparable known phosphonates. In the context of the present invention, the decomposition temperature is defined as the temperature at which the mass loss of a dried sample of the flame retardant reaches 2% by weight. For example, aminotrimethylenephosphonic acid (ATMP, CAS: 6419-19-8) reaches a mass loss of 2% by weight already at 176.4°C (see Figure 5). In the phosphonates according to the present invention, the corresponding mass loss is only reached at much higher temperatures (see Figures 2 and 4).

[0029] The loss of mass of the sample as a function of temperature can be determined by thermogravimetric analysis. "Dry" in this case means that the moisture content of the flame retardant is less than 0.5% by weight. The moisture content of the flame retardant can be measured by methods known to those skilled in the art, such as colorimetric Karl Fischer titration or NIR spectroscopy. The flame retardant according to the invention is not decomposed at the processing temperatures typically used in extrusion, but only at the high temperatures generated in a flame, after which it exerts its flame retardant effect, and is therefore particularly suitable for incorporation into polymeric materials processed by extrusion.

[0030] The flame retardant according to the present invention is also characterized by a low smoke gas generation rate, which is also expressed by a high residual mass after decomposition.

[0031] The inventors assume that the improved thermal stability of the flame retardants according to the invention is based on their special structure. In the thermal decomposition of aminomethanephosphonates, the bond is first broken at the weak PC bond of the P-CH2N group. Although the PC bond is basically chemically and thermally stable, the α-amino group stabilizes the carbon radicals generated by homolysis, and as a result, the PC bond of these flame retardants is already broken at relatively low temperatures. Due to the relatively low molar weight of the α-amino group in the compounds known in the prior art, the corresponding amine is released as a gaseous product after homolysis. The release of the amine is the thermodynamic driving force of the reaction and therefore occurs preferentially. In the flame retardants according to the invention, a phosphonate group is further bonded to the amine group at the α-position carbon radical. As a result, the amine has a higher molar weight and can only be released mainly at a much lower rate. In order to release the amine at low temperatures, the mass must be reduced, which can only be achieved by isotropically breaking the PC bond of the second phosphonate group. However, this reaction does not occur or does not occur essentially at all, since it would generate a particularly unstable carbanion. Thus, when the polymeric material is decomposed, the release of amines is significantly reduced, which results in less smoke gas generation. Furthermore, since the amine does not immediately dissipate when the bond is broken, the reverse reaction is also possible, for example, the combination of two radicals back to the original bond. As a result of the aforementioned effects, the cleavage of the PC bond is less favorable than in the prior art compounds, and the aminomethanephosphonates according to the present invention therefore have a much higher thermal stability.

[0032] Also, at least one heteroatom and / or at least one alkene or alkyne group with the first functional group and any further functional groups results in increased flame retardancy. The inventors assume that the heteroatom and / or alkene or alkyne group can form radicals with high energy free electron pairs and / or π-bonded electron pairs. These radicals, in combination with additional radicals generated in the combustion process, slow down the decomposition reaction. The particularly good flame retardant behavior is obtained due to the very homogeneous distribution of the flame retardant according to the invention in the polymeric material.

[0033] In a preferred embodiment of the present invention, the substituent R 1 ~R 6 Or the cycle formed by these further has at least one functional group which is a heteroatom selected from the group consisting of P, O, N, S, Si, I, Cl, Br, F and / or an alkene or alkyne group, which can enhance the effect of retarding the decomposition process caused by the above-mentioned radicals, and thus the flame retardant effect.

[0034] In a preferred embodiment of the present invention, the substituent R 1 ~R 6 Or the cycles formed thereby further have at least two, preferably at least three, even more preferably at least four, most preferably at least five functional groups.

[0035] In a preferred embodiment of the present invention, the substituent R 1 ~R 6 or the cycles formed thereby each have at least one functional group. In a particularly preferred embodiment of the present invention, the substituent R 3 ~R 6 or the cycles formed thereby each have at least one functional group. Particularly preferably, the number of functional groups is the same for all the substituents or the cycles formed thereby. Most preferably, R 3 ~R 6are the same substituent. Such compounds of the general formula (I) are particularly easily obtainable, for example, by esterifying the corresponding phosphonic acids.

[0036] In a preferred embodiment of the invention, the polarity of the flame retardant is matched to the polarity of the polymeric material using first and / or further functional groups. If the polarity of the flame retardant and the polymeric material is similar, the flame retardant is more easily incorporated into the polymeric material, resulting in better distribution. The flame retardant is then less likely to migrate out of the polymeric material.

[0037] In a preferred embodiment of the invention, the first and / or further functional groups of the flame retardant are selected from the group consisting of NH, -NHR, -NR, -OH, -OR, =O, -SH, -SR, -COOH, -COOR, -OCN, -SCN, -SiR x H y , -I, -Cl, -Br, -F, -N3 and epoxy, lactam, lactone, aziridine, glycolide, oxazoline, where R=alkyl, alkenyl, alkynyl or aryl and x+y=3.

[0038] The selection of these functional groups has the advantage that the polarity of the substituents is increased compared to unfunctionalized alkyl and / or aryl substituents, so that the corresponding flame retardants can be more easily incorporated into polar polymeric materials (polyacrylates, polyurethanes, polyamides, etc.) and are more difficult to migrate out of the polymeric materials.

[0039] In a further preferred embodiment of the present invention, the first and / or further functional groups of the flame retardant are -SiR x H y , alkenylene, and alkynylene, where R=alkyl, alkenyl, alkynyl, or aryl, and x+y=3.

[0040] The selection of these functional groups has the advantage that the polarity of the substituents is reduced compared to non-functional alkyl and / or aryl substituents, so that the corresponding flame retardants can be more easily incorporated into non-polar polymeric materials such as polyalkalenes (polyethylene, polypropylene, etc.) and are less susceptible to migration out of the polymeric materials.

[0041] Furthermore, by using the above-mentioned functional group-containing compounds as comonomers in the production of polymeric materials, the flame retardant can be covalently bonded to the polymeric materials, which has the advantage that the flame retardant cannot migrate out of the polymeric materials or migrates very difficultly. Also, the distribution of the flame retardant in the polymeric materials becomes more uniform, which results in improved flame retardancy.

[0042] In a preferred embodiment, the first and / or further functional groups may be NH2- groups. The flame retardant can then be added to the condensation reaction of the polymer and incorporated into the polymer chain by reaction with the electrophilic group of one of the monomers. As an example of this, the formation of polyamide 6,6 is shown below.

[0043] [ka]

[0044] In a particularly preferred embodiment of the invention, the flame retardant according to the invention is selected from the group consisting of NH2, -NHR, -NR2, -OH, -OR, =O, -SH, -SR, -COOH, -COOR, -OCN, -SiR x H y , -I, -Cl, -Br, -F, and further functional groups selected from the group consisting of epoxy, lactam, lactone, aziridine, glycolide, oxazoline, ether, alkenylene, alkynylene, where R=alkyl, alkenyl, alkynyl or aryl and x+y=3.

[0045] This increases the probability that the flame retardant will be incorporated into the polymer chain, maximizing the benefits of incorporation. In a particularly preferred embodiment of the invention, the flame retardant according to the invention has at least two functional groups that match those of the monomers of the polymeric material. As a result, the flame retardant can be incorporated into the polymer chain without causing chain termination reactions.

[0046] In a particularly preferred embodiment of the present invention, the flame retardant according to the present invention has at least two different functional groups. As a result, the flame retardant can be incorporated into different polymerization reactions. For example, one functional group can be an NH2 group and another functional group can be an alkene group. The flame retardant can then be incorporated into the polymer chain with the alkene group using radical polymerization or using a polycondensation reaction with the NH2 group.

[0047] The flame retardants according to the invention have the advantage that they are liquid and / or easily soluble in polar solvents and therefore only have a small effect on the viscosity of the solvent. They are therefore easily processed and incorporated into polymerization reactions. In particular, viscosity problems that arise during polyaddition and condensation reactions can be reduced by using the flame retardants according to the invention. This slows down the onset of the Trommsdorff-Norrish effect and, as a result, allows the polymer material to have a higher average molar mass.

[0048] In a preferred embodiment, R 1 and R 2 form a cycle, with the same or different substituents, at least one of the substituents being melamine, the nitrogen atom of the amino group being substituted with H, alkyl, aryl, or a methyl bisphosphonate group of the following structure (II):

[0049] [ka]

[0050] Particularly preferred is that at each of the nitrogen atoms of the amino group, one of the substituents is H and the other is a methyl bisphosphonate group of structure (II). In another preferred embodiment, both substituents on each nitrogen atom are methyl bisphosphonate groups of structure (II).

[0051] Due to the polarity differences between the flame retardant and the polymeric material, polar flame retardants such as this class of phosphates migrate easily from non-polar polymeric materials such as polyethylene.

[0052] Particularly preferably, the first and / or further functional groups of the flame retardant are alkene or alkyne groups, which has the advantage that the flame retardant can be bound to non-polar polymeric materials, such as polyolefins, during polymerization reactions, especially radical or ionic polymerization reactions, thereby preventing migration out of the polymeric material.

[0053] In particular, it may be advantageous to use the flame retardants according to the invention as acids, especially when the protected polymeric material is not a non-polar polyolefin but a polar polymer such as polyamide, polyurethane, polyester, etc. The flame retardant is preferably an acid, especially when used as a co-condensation / addition component. In a preferred embodiment of the invention, at least one, preferably at least two, particularly preferably at least three and most preferably four of the groups are thus R 3 , R 4 , R 5 and R 6H. The flame retardant according to the invention can be added, for example, preferably in the form of an acid, to the polyurethane foaming process as a co-additive component. Without being bound by this theory, the inventors assume that the flame retardant is incorporated into the polymer by reaction of the isocyanate with the phosphonic acid group to form a particularly stable POC(=O)-N group, which has a positive effect on the degradation behavior of the polyurethane. This also applies to other polymers produced by polyaddition, such as polyethylene oxide, polypropylene oxide, polyethylene glycol and polyurea. Here too, the phosphonic acid group reacts with one of the components and is thus incorporated into the polymer. Therefore, when producing these polymers, it is particularly preferred to use the flame retardant in the form of an acid as a co-additive component.

[0054] Likewise, in a preferred embodiment, the flame retardant according to the present invention is used in the form of an acid as a co-condensation component in a polymerization reaction.The inventors assume that in this case, the phosphonic acid group reacts with the hydroxyl or amine group of the component of the condensation reaction, and incorporates them into the polymer.Therefore, the flame retardant according to the present invention is preferably used in the form of an acid as a co-condensation component for producing polyesters, polycarbonates, and polyamides.

[0055] In a preferred embodiment of the present invention, the substituent R 3 and / or R 4 and / or R 5 and / or R 6 are organic residues with two or more carbon atoms. Phosphonates with short-chain carbon residues, especially methyl, are known from the prior art. However, they can be highly toxic, since under decomposition conditions they have an alkylating effect. For example, human DNA can be permanently damaged. However, the alkylating effect decreases significantly with increasing chain length.

[0056] The decomposition temperature of the polymer is preferably higher than the processing temperature of the plastic matrix in the thermal processing method in which the polymer is incorporated into the plastic matrix, so that the decomposition process of the polymer does not occur when the processing temperature of the plastic matrix is ​​reached. The decomposition temperature of the polymer is preferably at least 10°C higher than the processing temperature of the plastic matrix, particularly preferably at least 20°C higher than the processing temperature of the plastic matrix, and most preferably at least 50°C higher than the processing temperature of the plastic matrix.

[0057] If the decomposition temperature of the polymer is significantly higher than the temperature of the plastic matrix in which it is incorporated, the plastic matrix will decompose before the polymer can partially decompose in a flame and exert its flame retardant effect. Conversely, if the decomposition temperature of the polymer is significantly lower than the temperature of the plastic matrix, the decomposed polymer may already have undergone further reactions, resulting in a significant reduction in the flame retardant effect. Therefore, the difference between the decomposition temperature of the polymer and that of the plastic matrix is ​​preferably not more than 100°C, particularly preferably not more than 50°C, most preferably not more than 20°C.

[0058] In a preferred embodiment of the invention, the decomposition temperature, e.g. a mass loss of 2% by weight of the dried flame retardant, is reached starting from a temperature of 200°C, particularly preferably starting from a temperature of 220°C, most preferably starting from a temperature of 245°C.

[0059] The decomposition temperature of the polymer is determined by the thermogravimetric analysis method described in the "Methods" section. The decomposition temperature is the temperature at which the mass loss of the dry sample reaches 2% at a heating rate of 10 K / min.

[0060] Due to the carbon atom being substituted twice with a phosphonate group in the alpha position to the nitrogen, the flame retardant according to the invention has a higher phosphorus content than the phosphonates known from the prior art. It was confirmed that the flame retardant effect of this phosphorus-based flame retardant increases with increasing phosphorus content. As a result, the effect of the flame retardant according to the invention, for example the flame retardant effect per unit mass of the flame retardant employed, is particularly high. Therefore, a good flame retardant effect is obtained even at low concentrations of the flame retardant in the polymer material. At the same time, the properties of the material, in particular the processability and the elongation at break, are hardly affected. In a preferred embodiment, the phosphorus content of the flame retardant is at least 10% by weight, preferably at least 12% by weight, particularly preferably at least 14% by weight, most preferably at least 15% by weight. In order to ensure a high phosphorus content of the flame retardant according to the invention, the substituent R 1 ~R 6 advantageously has as low a mass as possible.

[0061] In particular, when one or more components of a preferably catalyzed polymerization reaction are added as additives, it is advantageous to use the flame retardants according to the invention as salts or esters, particularly preferably as salts. This makes it possible to avoid potential interactions between the free acid groups of the flame retardant and components such as the catalyst of the reaction. The flame retardants according to the invention, as salts or esters, are also advantageously used in pH-sensitive polymeric materials, for example polymeric materials that change structure or decompose when exposed to acid. In such applications, the salt form can also be dissolved in water and mixed homogeneously with the polyol in some way. The salt form dissolved in water can be easily and homogeneously incorporated into water-based paints and coating systems. When the flame retardants are used as esters, the associated hydrophobization can further promote better bonding to the matrix, resulting in improved mechanical properties and reduced migration from the polymer.

[0062] Thus, in a preferred embodiment of the present invention, the group R 3 , R 4 , R 5 and R 6At least one, preferably at least two, particularly preferably at least three, and most preferably at least four of the cations are Na + , K + , Mg 2+ , Ca 2+ , B 3+ , Al 3+ , Zn 2+ , N.H. 4+ or melamine or a condensate thereof, preferably an ammonium ion of an amine compound selected from the group consisting of melam, melem, melon, urea, guanidine, morpholine, and piperazine. + and Ca 2+ As the cation, Na having a small molar mass is preferred. + is most preferred, so that the weight percentage of phosphorus in the flame retardant can be made as high as possible.

[0063] In a preferred embodiment, the polymeric material comprises a flame retardant in an amount of at least 1.5 wt%, or at least 5 wt%, or at least 10 wt%, or at least 15 wt%, and / or in an amount of 35 wt% or less, or 30 wt% or less, or 25 wt% or less, based on the total polymeric composition.

[0064] In a preferred embodiment of the invention, the overall composition comprises polymeric material in an amount of at least 50% by weight, preferably at least 70% by weight, particularly preferably at least 80% by weight, most preferably at least 90% by weight.

[0065] These quantitative ratios firstly ensure good flame retardancy of the polymer composition and secondly have only a slight effect on the processing and material properties of the polymer material.

[0066] The flame retardants according to the invention may be advantageously used in combination with other flame retardants, for example flame retardants that provide flame retardancy by a different mechanism, whereby the interaction between the flame retardants according to the invention and the other flame retardants can result in a synergistic effect, for example an effect that exceeds the mere sum of the flame retardant effects of the individual components.

[0067] The polymeric material of the composition according to the invention may be an elastomeric, thermosetting or thermoplastic polymeric material. The polymeric material is preferably a thermosetting or thermoplastic polymeric material, particularly preferably a thermosetting polymeric material.

[0068] In a preferred embodiment, the polymeric material is preferably selected from nitrogen bases, melamine derivatives, phosphates, pyrophosphates, polyphosphates, organic and inorganic phosphinates, organic and inorganic phosphonates, and derivatives of the aforementioned compounds, preferably melamine, melam, melem, melon, ammeline, ammelide, 2-ureidomelamine, acetoguanamine, benzoguanamine, diaminephenyltriazines, salts and adducts of melamine, melamine cyanurate, melamine borate, melamine orthophosphate, melamine pyrophosphate, dimelamine pyrophosphate, aluminum diethylphosphinate, melamine polyphosphate, oligomeric and polymeric 1,3,5 triazine compounds and 1,3,5 triazine compounds. The flame retardant composition further comprises at least one additional flame retardant component selected from melamine, melamine resins, melamine derivatives, ammonium polyphosphate with silanes, siloxanes, polysiloxanes, silicones or polystyrenes, coated and / or uncoated crosslinked ammonium polyphosphate particles, and 1,3,5 triazine compounds, polyphosphate salts of 1,3,5 triazine compounds, guanine, piperazine phosphate, piperazine polyphosphate, ethylenediamine phosphate, pentaerythritol, dipentaerythritol, boron phosphate, 1,3,5 trihydroxyethyl isocyanurate, 1,3,5 triglycidyl isocyanurate, triallyl isocyanurate, and derivatives of the aforementioned compounds. In a preferred embodiment, the polymeric material comprises wax, silicon, siloxane, fat, or mineral oil to improve the dispersion of the additional flame retardant component.

[0069] In addition to the flame retardant according to the invention, the polymeric material preferably comprises as a further flame-retardant component a phosphate, in particular ammonium polyphosphate, particularly preferably ammonium polyphosphate of crystalline form I, II or V or mixtures thereof, the latter being particularly preferably coated.

[0070] In particular, ammonium polyphosphate in crystalline form II is preferred, which is essentially insoluble in water compared to other crystalline forms. This is a powdery substance that already has good flame retardant effect without coating and has low solubility in water. The advantage of using coated aluminum polyphosphate in crystalline form II is that it has high thermal stability and high compatibility with polymers. This results in better dispersion of the flame retardant in the polymer, improved processability of the polymer, and more efficient fire protection.

[0071] Generally, phosphates have higher solid-phase activity than phosphonates, and phosphonates have higher gas-phase activity, so that their combination provides a particularly significant flame retardant effect.

[0072] In a preferred embodiment, the ratio of the flame retardant according to the invention to at least one further flame-retardant component in the polymeric material is 1:18 to 1:1, preferably 1:9 to 1:4, particularly preferably 1:6 to 1:4. These ratios also apply when ammonium polyphosphate is used as the further flame-retardant component.

[0073] In addition to the flame retardant according to the invention, the polymeric material contains other fillers selected from calcium carbonate, talcum, clay or silicates such as glimmer, kaolin or wollastonite, diatomaceous earth, calcium and barium sulfates, aluminum hydroxide, glass fibres and glass balls, as well as wood flour, cellulose powder and lamp black and graphite. These fillers can provide the polymeric material with additional desired properties, in particular reducing its cost, colouring it or improving its mechanical properties, for example by reinforcing it with glass fibres.

[0074] If the flame retardant is incorporated into the protected polymeric material using a molding process, dispersing agents are advantageously used when incorporating the flame retardant. Thus, in a further embodiment of the present invention, the polymeric material according to the present invention comprises a dispersing agent in an amount of 0.01-10% by weight, preferably 0.1-5.0% by weight, based on the weight of the flame retardant according to the present invention, preferably selected from among fatty acids, including fatty acid monoamides, fatty acid bisamides such as oleamide and erucamide, and fatty acid alkanolamides, among fatty acid esters, including glycerol esters and wax esters, among C16-C18 fatty acids, among fatty acid alcohols, including cetyl and stearyl fatty acid alcohols, among natural and synthetic waxes, polyethylene waxes and oxidized polyethylene waxes, and among metal stearates, preferably Ca, Zn, Mg, Ba, Al, Cd and Pb stearates. The addition of said dispersing agents improves the dosing ability of the flame retardant, the extrusion ability of the polymeric material, and the homogeneity of the dispersed flame retardant in the polymeric material.

[0075] In a further embodiment of the present invention, the flame retardant according to the present invention has a free water content (moisture content) of less than 0.6% by weight, preferably less than 0.4% by weight. A low moisture content also improves the ability to dose the flame retardant, the extrusion ability of the polymeric material, and the homogeneity of the dispersed flame retardant in the composition, and prevents hydrolytic degradation.

[0076] The flame retardant can be incorporated into the polymeric material in various ways. The flame retardant can first be incorporated into the polymeric material in a molding process. If the polymeric material is processed, for example, by extrusion, the flame retardant can be added during the extrusion process, for example using a masterbatch. A masterbatch as defined in the present invention is a granular or powdery polymeric material that contains a higher concentration of flame retardant and other additives than in the final application. To produce the polymeric material according to the present invention, the masterbatch or various masterbatches are combined with further polymeric materials that do not contain the flame retardant contained in the masterbatch in an amount or ratio that corresponds to the desired concentration of the flame retardant in the final product. Compared to the addition of various substances in paste, powder or liquid form, masterbatches have the advantage that they are easy to process and administer, with high process reliability. The flame retardant is homogeneously distributed in the polymeric material by extrusion.

[0077] Polymeric materials that can be compounded with flame retardants include polyesters such as polyvinyl butyral (PVB), polypropylene (PP), polyethylene (PE), polyamide (PA), polybutylene terephthalate (PBT), polyethylene terephthalate (PET), polyurethane (PU), thermoplastic polyurethane (TPU), polyurea, polyphenylene oxide, polyacetal, polyacrylate, polymethacrylate, polyoxymethylene, polyvinyl acetal, polystyrene, acryl-butadiene-styrene (ABS), acrylonitrile-styrene (ACN), and styrene-butadiene-styrene (SBFS). Preferably, the flame retardant is selected from the group consisting of esters of polyols (ASA), polycarbonates, polyethersulfones, polysulfonates, polytetrafluoroethylene, polyureas, formaldehyde resins, melamine resins, polyetherketones, polyvinyl chlorides, polylactides, polysiloxanes, phenolic resins, epoxy resins, poly(imides), bismaleimide-triazines, thermoplastic polyurethanes, ethylene-vinyl acetate copolymers (EVA), polylactides (PLA), polyhydrobutyric acid (PHB), copolymers and / or mixtures of the aforementioned polymers. The flame retardant according to the invention is particularly preferably used in foams of the aforementioned polymer materials, particularly preferably in polyurethane foams. The flame retardant is preferably added in this case as an additive or co-condensation / addition component of the polyol component. If the flame retardant is added as an additive, it is preferably a salt or an ester. If the flame retardant is added as a co-condensation / addition component, it is preferably an acid.

[0078] It was confirmed that these phosphonates not only have a flame retardant effect, but also catalyze the foaming of polyurethane.

[0079] The present invention also relates to a flame retardant which is a compound of formula I, its corresponding ammonium salt, its corresponding phosphonate, or a mixture thereof, wherein the substituents R3 to R6 or the cycle formed by them preferably have a first functional group and / or not more than three of the substituents R3 to R6 are H.

[0080] The present invention also provides a method for producing a flame retardant comprising the steps of: a) at least one phosphonic or phosphinic acid selected from the group consisting of compounds of formulae (V) and (VI) in a reaction vessel, [ka] -X- is an oxygen atom -O-, or -X- is a single bond; (Pi)R 3 , R 4 , R 5 and R 6 are the same or different substituents, and have the following structures (III) and (IV) with H, linear, branched or cyclic alkyl, alkenyl and alkynyl, unsubstituted and alkyl-substituted phenyl, polynuclear aromatics having up to four nuclei, mononuclear or polynuclear heteroaromatics having up to four nuclei, silyl, allyl, alkyl or aryl alcohol, n=0 to 100;

[0081] [ka] cations selected from the group consisting of Na + , K + , Mg 2+ , Ca 2+ , B 3+ , Al 3+ , Zn 2+ , N.H. 4+ or melamine or a condensate thereof, preferably an amine-bound ammonium ion selected from the group consisting of melam, melem, melon, urea, guanidine, morpholine, and piperazine; and / or (P-ii) When -X- is an oxygen atom, -O-, -OR 3 -OR 4 Both and / or -OR 5 AND -OR 6 and / or -OR 3 AND -OR 5 Both and / or -OR 4 AND -OR 6together form a cyclic phosphonate ester or cyclic phosphonic anhydride having a ring size of 4 to 10 atoms, including the P atom of the phosphonate group, and / or (P-iii) When -X- is a single bond, -R 3 AND -OR 4 and / or -R 3 AND -OR 5 together form a cyclic phosphonic acid ester or cyclic phosphonic acid anhydride having a ring size of 4 to 10 atoms, including the P atom of the phosphinate group, and / or -OR 5 AND -OR 6 And / or -OR 4 AND -OR 6 together with the P atom of the phosphonate group form a cyclic phosphonate ester or cyclic phosphonic anhydride having a ring size of 4 to 10 atoms, b)R 7 = alkyl, aryl or alkenyl, preferably triethoxymethane HC(OR 7 )3, and c) an amino compound of formula (VII) [ka] providing a mixture of (Ni)R 1 and R 2 are the same or different substituents and are selected from the group consisting of linear, branched or cyclic alkyl, alkenyl and alkynyl, unsubstituted and alkyl-substituted phenyl, mono- and polynuclear aromatics with up to four nuclei, mono- or polynuclear heteroaromatics with up to four nuclei, silyl, allyl, alkyl or aryl alcohols, or (N-ii)R 1 and R 2 form a saturated, monounsaturated or polyunsaturated heterocycle having 4 to 8 ring atoms selected from carbon, oxygen, sulfur, phosphorus, silicon and nitrogen, including the N atom, and these nitrogen atoms are preferably substituted on the heterocycle with H, an alkyl, an aryl, or a methylbisphosphonate group having the following structure (II) when the heterocycle has a nitrogen atom as a ring atom: [ka] On said heterocycle, if it has carbon, phosphorus or silicon as ring atoms, these atoms are preferably H, alkyl, aryl, -NH, -NHR, -NR, -OH, -OR, =O, -I, -Cl, -Br, F, -N, -SH, -SR, -OCN, epoxy, lactam, lactone, aziridine, glycolide, oxazoline, alkenylene and alkynylene, -SiR x H y where R=alkyl, alkenyl, alkynyl or aryl, and x+y=3; Preferably A) Substituent R 1 ~R 6 or B) 1) Substituent R 3 ~R 6 forming a cyclic phosphine or phosphonate ester according to (P-ii) or (P-iii), or 2) Substituent R 3 ~R 6 forming a cyclic phosphine or phosphonic anhydride according to (P-ii) or (P-iii), or 3) Substituent R 1 and R 2 When forming a heterocycle according to (N-ii), One of the cycles that forms in a) heteroatoms selected from the group consisting of P, O, N, S, I, Cl, Br, F, and / or b) an alkene or alkyne group and a first uncharged or negatively charged functional group having the formula: The functional group is not -OH, and when one of the cycles according to 1) to 3) has the functional group, the ring atom of the cycle is substituted with the functional group or with a substituent having the functional group. The process and Heating the mixture to a temperature in the range of 40 to 150°C.

[0082] Heating of the mixture can be followed by a purification step, which preferably comprises distillation or chromatographic purification of the mixture.

[0083] During the conversion, the phosphonic or phosphinic acid or the amino compound of formula (VII) utilizes the free electron pair of the PH or NH group to form the ortho ester H C (OR 7 ) forms a nucleophilic bond with the central carbon atom of 3. This results in the formation of 3 equivalents of alcohol HOR 7 While releasing, a compound of formula (I) is produced.

[0084] [ka]

[0085] In order to achieve a higher conversion rate, in a preferred embodiment of the present invention, during the conversion, HOR is preferably added by distillation, particularly preferably by distillation under reduced pressure. 7 Separate.

[0086] The present invention also provides methods for preparing compounds of general formulas (V) and (VI). [ka]

[0087] These are phosphinic or phosphonic acids of the formula HC(OR 3 / 4 / 5 / 6 In a preferred embodiment of this method, the compound can be obtained by esterification with a compound of formula HC(OR 3 / 4 / 5 / 6 For the purposes of the process according to the invention, phosphinic or phosphonic acids are represented by the formula HC(OR 3 / 4 / 5 / 6The mixture is mixed with the compound of formula (I) 3 and heated to a temperature in the range of 40-140°C, preferably 80-120°C, more preferably 90-120°C, and most preferably 100-120°C. Particularly preferably, the mixture is heated to boiling. The reaction mixture is stirred at these temperatures for 10 minutes to 10 hours, preferably 1 hour to 5 hours, more preferably 1 hour to 3 hours, and most preferably 1 hour to 2 hours. After this reaction period, the reaction liquid for fractionation contains the main component HOR 3 / 4 / 5 / 6 and a further fraction comprising a compound of formula (V) or (VI). The above-described method is particularly preferably used for the production of diethyl phosphite.

[0088] The present invention also provides the use of a compound of formula (I), its corresponding ammonium salt, its corresponding phosphonate, or a mixture thereof, for the treatment of surfaces, preferably in the form of a coating, [ka] (Ni)R 1 and R 2 are the same or different substituents and are selected from the group consisting of linear, branched or cyclic alkyl, alkenyl and alkynyl, unsubstituted and alkyl-substituted phenyl, mono- and polynuclear aromatics with up to four nuclei, mono- or polynuclear heteroaromatics with up to four nuclei, silyl, allyl, alkyl or aryl alcohols, or (N-ii)R 1 and R 2 form a saturated, monounsaturated or polyunsaturated heterocycle having 4 to 8 ring atoms selected from carbon, oxygen, sulfur, phosphorus, silicon and nitrogen, including the N atom, and these nitrogen atoms are preferably substituted on the heterocycle with H, an alkyl, an aryl, or a methylbisphosphonate group having the following structure (II) when the heterocycle has a nitrogen atom as a ring atom: [ka] On said heterocycle, if it has carbon, phosphorus or silicon as ring atoms, these atoms are preferably H, alkyl, aryl, -NH, -NHR, -NR, -OH, -OR, =O, -I, -Cl, -Br, F, -N, -SH, -SR, -OCN, epoxy, lactam, lactone, aziridine, glycolide, oxazoline, alkenylene and alkynylene, -SiR x H y where R=alkyl, alkenyl, alkynyl or aryl, and x+y=3; -X- is an oxygen atom -O-, or -X- is a single bond; (Pi)R 3 , R 4 , R 5 and R 6 are the same or different substituents, and have the following structures (III) and (IV) with H, linear, branched or cyclic alkyl, alkenyl and alkynyl, unsubstituted and alkyl-substituted phenyl, polynuclear aromatics having up to four nuclei, mononuclear or polynuclear heteroaromatics having up to four nuclei, silyl, allyl, alkyl or aryl alcohol, n=0 to 100; [ka] cations selected from the group consisting of Na + , K + , Mg 2+ , Ca 2+ , B 3+ , Al 3+ , Zn 2+ , N.H. 4+ or melamine or a condensate thereof, preferably an amine-bound ammonium ion selected from the group consisting of melam, melem, melon, urea, guanidine, morpholine, and piperazine; and / or (P-ii) When -X- is an oxygen atom, -O-, -OR 3 -OR 4 Both and / or -OR 5 AND -OR 6 and / or -OR 3 AND -OR5 Both and / or -OR 4 AND -OR 6 together form a cyclic phosphonate ester or cyclic phosphonic anhydride having a ring size of 4 to 10 atoms, including the P atom of the phosphonate group, and / or (P-iii) When -X- is a single bond, -R 3 AND -OR 4 and / or -R 3 AND -OR 5 together form a cyclic phosphonic acid ester or cyclic phosphonic acid anhydride having a ring size of 4 to 10 atoms, including the P atom of the phosphinate group, and / or -OR 5 AND -OR 6 And / or -OR 4 AND -OR 6 together form a cyclic phosphonate ester or cyclic phosphonic anhydride having a ring size of 4 to 10 atoms, including the P atom of the phosphonate group; Preferably, A) Substituent R 1 ~R 6 or B) 1) Substituent R 3 ~R 6 forming a cyclic phosphine or phosphonate ester according to (P-ii) or (P-iii), or 2) Substituent R 3 ~R 6 forming a cyclic phosphine or phosphonic anhydride according to (P-ii) or (P-iii), or 3) Substituent R 1 and R 2 When forming a heterocycle according to (N-ii), One of the cycles that forms in a) heteroatoms selected from the group consisting of P, O, N, S, I, Cl, Br, F, and / or b) an alkene or alkyne group and a first uncharged or negatively charged functional group having the formula: The functional group is not -OH, and when one of the cycles according to 1) to 3) has the functional group, the ring atom of the cycle is substituted with the functional group or with a substituent having the functional group.

[0089] In a preferred embodiment, the coating acts as a flame retardant for the object, and preferably acts as a flame retardant for polymeric materials.

[0090] This embodiment is particularly preferably used as a surface treatment for metal or polymeric materials, in particular thermosetting polymers. For example, the use in composite materials is particularly preferred. In this case, the aforementioned phosphonates can be applied in liquid form, for example as a solution or as a liquid pure substance, onto the polymer matrix and / or reinforcing material (for example glass fibers). The advantage in this case is that the flame retardant according to the invention is liquid or causes only a slight change in viscosity in suspension. As a result, the flame retardant can be uniformly dispersed in the composite material. On the other hand, the flame retardants known in the prior art are generally solid or require large amounts of solvent to obtain a low-viscosity solution. Therefore, it is very difficult to incorporate them into composite materials. Woven composite materials also provide a filtration effect for the flame retardant. As a result, protection is only provided on one side. The aforementioned disadvantages can be overcome with the flame retardant according to the invention.

[0091] In a particularly preferred embodiment of the present invention, the compound of formula (I) is used to form a coating, for example a gel coat.This has the advantage that the compound according to the present invention has good solubility in a number of polar solvents.As a result, it is possible to achieve a uniform distribution in the solvent and thus on the final treated surface.Due to the good solubility, the viscosity of the solution is not affected or is only slightly affected.

[0092] The compound of formula (I) is used in the coating in an amount of preferably 1 to 40% by weight, more preferably 2 to 30% by weight, even more preferably 3 to 20% by weight, and most preferably 4 to 10% by weight, based on the total coating composition.

[0093] Solutions of compounds of formula (I) may be used, for example, to coat textiles, paper, ceramics, or composite materials or interphases thereof, such as prepregs.

[0094] Due to their low absorption and uniform mixing with the other components of the coating system, especially the binder, the compounds of formula (I) are suitable for so-called "clear coatings" or transparent coatings, which are particularly useful when it is not desired to hide the underlying structure, such as for example clear coatings on wood. EXAMPLES

[0095] The present invention will be described in detail below based on specific embodiments of the flame retardant according to the present invention, a production example of the composition according to the present invention, examples of the flame retardant, and based on the enclosed drawings.

[0096] Specific embodiments of the flame retardant according to the present invention Embodiments having a first functional group on an amino group [Table 1]

[0097] Embodiments with First and Second Functional Groups on the Amino Group [Table 2]

[0098] Embodiments having a first functional group on one of the phosphonic acid groups [Table 3]

[0099] Embodiments having a first functional group on one of the phosphonic acid groups [Table 4]

[0100] Embodiments having a first functional group on one of the phosphonic acid groups

Table 5

[0101] Embodiments having a first functional group on one of the phosphonic acid groups

Table 6

[0102] Embodiments with First and Second Functional Groups on the Phosphonic Acid Group

Table 7

[0103] Embodiments having a first functional group on one of the phosphonic acid groups

Table 8

[0104] Embodiments Having a First Cyclic Functional Group

Table 9

[0105] Embodiments Having a First Cyclic Functional Group

Table 10

[0106] Embodiments Having a First Cyclic Functional Group

Table 11

[0107] Morpholine, MOMP

Table 12

[0108] Piperazine, PIMP embodiment

Table 13

[0109] Preparation examples of the composition according to the present invention Input material: [Table 14]

[0110] Further flame retardants: Budit240: A phosphorus-based partially crosslinked polyacrylate prepared according to Example 1 of WO2014 / 124933 Budit315: Melamine cyanurate from Chemische Fabrik Budenheim KG Budit342: Melamine polyphosphate from Chemische Fabrik Budenheim KG Budit 667: an intumescent flame retardant system from Chemische Fabrik Budenheim KG based on ammonium polyphosphate. TCPP: Tris(2-chloroisopropyl)phosphate TCPP (CAS: 13674-84-5) from Sigma Aldrich OP550: Phosphorus-based polyol Exolit OP550 (CAS: 184538-58-7) from Clariant AG

[0111] Measurement method: Dynamic Differential Calorimetry (DSC) The measurements were performed using a simultaneous thermogravimetric analysis-dynamic differential scanning calorimetry (STA / TG-DSC) instrument Model STA409PC / 3 / H Luxx, Netzsch Geratebau GmbH, in a nitrogen atmosphere at a heating rate of 10 K / min in the range of 25-500 °C. The initial sample weight was about 15 mg. The analysis was performed using the software NETZSCH Proteus.

[0112] Thermogravimetric analysis (TAG)The simultaneous thermogravimetric analysis-differential dynamic scanning calorimetry (STA / TG-DSC) was carried out in a nitrogen atmosphere at a heating rate of 10 K / min in the range of 25-800 °C. The initial sample weight was about 12-15 mg. The software NETZSCH Proteus was used to analyze the TGA graphs.

[0113] Preparation examples of the composition according to the present invention Example 1: Synthesis of morpholine-methylaminodiphosphonic acid (MOMP-H4) 0.1 mol of 4-formylmorpholine was weighed into a 500 ml round flask, mixed with 0.2 mol of phosphonic acid and 30 ml of acetic anhydride. The reaction was stirred at 65 °C for 90 min. The acetic acid formed and excess water were then removed under reduced pressure of about 30 mbar on a rotary evaporator. The remaining solvent was then removed in a drying cabinet at 85 °C for 4 h.

[0114] Example 2 : Synthesis of piperazine-di(methylaminodiphosphonic acid) (PIMP-H4) In a 250 ml round flask, 0.28 mol of phosphonic acid was dissolved in 31 ml of fully deionized water with stirring. A solution of 0.07 mol of diformylpiperazine was added dropwise to 30 ml of fully deionized water over 15 minutes. A temperature rise of several degrees was observed during the addition. After the addition was complete, the reaction mixture was stirred under reflux for 3 hours. After the solution had cooled, the excess water was removed on a rotary evaporator. A saturated piperazine solution was added dropwise to the liquid distillation residue. Upon heating, a white amorphous precipitate formed.

[0115] Example 3: Synthesis of Dimethyl-Methylaminodiphosphonic Acid (DAMP-H4) 0.9 mol of dimethylformamide was weighed into a 500 ml round flask, 1.8 mol of phosphonic acid and 225 ml of acetic anhydride were added and mixed. The acetic acid formed and excess water were then removed under reduced pressure of about 300 mbar on a rotary evaporator. The remaining solvent was then removed in a drying cabinet at 85 °C for 4 hours.

[0116] Example 4: Synthesis of aqueous solutions of the trisodium salt of morpholine-methylaminodiphosphonic acid (MOMP-H-Na3) 0.289 mmol of morpholine-methylaminodiphosphonic acid (MOMP-H4) was dissolved in 50 ml of fully deionized water, then 0.867 mmol of NaOH was added, for which a pH value of about 9 was obtained.

[0117] Example 5: Synthesis of morpholine-methylaminodiphosphonic acid tetraethyl ester (MOMP-H4) MOMP-Et4 was obtained by weighing 0.1 mol of morpholine into a reactor while stirring. Then, 0.1 mol of triethoxymethane is added dropwise. Then, 0.2 mol of diethyl phosphite is added. The mixture is heated to 120°C and stirred at this temperature for 4 hours. After the reaction is over, the product is washed by vacuum distillation at 50 mbar and 150°C.

[0118] In a preferred embodiment, all the substituents R are selected from the group consisting of aryl, ... 3 , R 4 , R 5 and R 6 is a cation or an organic residue, particularly preferably ethyl. The use of such compounds is particularly advantageous since they accelerate the synthesis and also improve the flame retardancy of the finished polymer. Compounds with a P-OH group, such as MOMP-H4, do not show a corresponding catalytic effect, probably because they are dipolar ions (PO - / NH + ) because it exists in the form

[0119] As shown on the basis of the following tests, the so-called onset time to foaming is significantly reduced when using the corresponding substituted compounds compared to compounds having a P-OH group such as MOMP-H4.

[0120] General methodology: Polyol (22.5 g) is mixed with catalyst (ethylene glycol, 1.05 g), pentane (4.5 g) and the respective flame retardant at 1000 R / min. Isocyanate (MDI, 60.0 g) is added with the disperser switched off and the mixture is stirred at 1500 R / min for 10 seconds before being quickly refilled.

[0121] [Table 15]

[0122] Example 6: Synthesis of morpholine-methylaminodiDOPO (MOM-DOPO2) [ka] [Table 16]

[0123] The reaction is a condensation reaction between the formyl function on 4-formylmorpholine (4-FM) and the PH group of the DOPO molecule, splitting off H2O to produce the product MOM-DOPO2. 40 g of DOPO is dissolved in 100 ml of acetic anhydride (Ac2O) with stirring, placed in a 250 ml beaker and heated to 120 °C. Once at that temperature, 10 g of 4-FM is added. After 5 hours, the solution is neutralized with 80 ml of water, followed by setting an external tempering. After cooling, a white solid precipitates, which is filtered and washed with water. Acetic acid is also produced as a by-product.

[0124] Example 7: Synthesis of morpholine-methylaminodiphosphonic acid Zn salt (MOMP-H2) The Zn salt (1:1) was obtained by dispersing 50.0 g (0.191 mol) of MOMP in 500 g of H2O, followed by cleavage with 14.6 g of ZnO (0.191 mol). The reaction mixture is heated to 95°C and stirred at this temperature for 4 hours. The batch is then cooled below 50°C, followed by separation of the solid from the mother liquor. The filter cake is dried at 120°C in circulating air. [Table 17]

[0125] Example 8: Synthesis of piperazine-di(methylaminodiphosphonic acid) (PIMP-H4) [Table 18]

[0126] 0.1 mol of 1,4-diformylpiperazine and 0.1 mol of acetic anhydride are charged to the reactor and mixed. The mixture is heated to 120 ° C. 0.4 mol of phosphorus is dissolved separately in 0.3 mol of acetic anhydride. This solution is added dropwise to the reactor. Finally, another 0.5 mol of acetic anhydride is added and the batch is then heated to 135 ° C. After a reaction time of 30 minutes, 2.1 mol of water are added dropwise. After a further reaction time of 40 minutes, the batch is cooled to room temperature. Then 70 ml of sodium hydroxide solution are added. The product is separated from the mother liquor and dissolved in water. The solution is reprecipitated with sulfuric acid, followed by filtering, washing and drying the product.

[0127] Example 9: Synthesis of diethyl phosphite Phosphonic acid (29.7 g, 0.36 mol) and triethoxymethane (107.3 g, 0.72 mol) are mixed in a 500 ml three-necked flask equipped with a distillation apparatus and then heated to 90 °C with stirring. After 45 min, the temperature is increased to 135 °C to start boiling (gas phase temperature 73 °C) and the first fraction of ethanol and ethyl formate is obtained. After the boiling has ceased, a vacuum (30 mbar) is applied to obtain the second fraction. The associated product is diethyl phosphite. 35.0 g of a colorless, low-odor liquid is obtained.

[0128] Example 10: Synthesis of 4-hydroxy-1-(methylaminodiphosphonic acid)piperidine ("OH-PIDMP-H4") [ka]

[0129] "OH-PIDMP-Et4" was obtained by stirring 4-hydroxypiperidine (0.1 mol) in a 250 ml flask. Triethoxymethane (0.1 mol) was added dropwise. Then 0.2 mol of diethyl phosphite was added. The mixture was heated to 120°C and stirred at this temperature for 4 hours, after which the product "OH-PIDMP-Et4" was washed by vacuum distillation at 50 mbar and 150°C.

[0130] [ka]

[0131] Next, when this product is mixed with 5 times the amount of 1N hydrochloric acid, slight heating is observed. The resulting ethanol is distilled to obtain "OH-PIDMP-H4" in 89% yield. The melting point is 250°C.

[0132] Example 11: Synthesis of 4-Methylen-1(methylaminodiphosphonic acid tetraethyl ester)-piperidine ("4-Methylen-PIDMP-Et4") [ka]

[0133] "4-Methylen-PIDMP-Et4" was obtained by stirring 4-Methylidenepiperidine-hydrochloride (0.05 mol) and triethylamine (0.1 mol) in a 250 ml flask. Triethoxymethane (0.12 mol) was added dropwise. Diethyl phosphite (0.31 mol) was then added. The mixture was heated to 140 °C and stirred at this temperature for 6 hours. After cooling to room temperature, diethyl ether (125 ml) was added, the mixture was neutralized with aqueous sodium hydroxide solution (0.5N, 50 ml), the phases were separated and the organic phase was washed with water (250 ml). The organic phase was worked up by distillation and the product has a boiling point of 180 °C at 2 mmbar. The yield is 58%.

[0134] Example 12: Synthesis of 4-hydroxy-4-vinyl-1-(methylaminodiphosphonic acid tetraethyl ester)-piperidine ("OH-Vinyl-PIDMP-Et4") [ka]

[0135] "OH-Vinyl-PIDMP-Et4" was obtained by stirring 4-piperidone-ethylene ketal (0.1 mol) in a 250 ml flask. Triethoxymethane (0.1 mol) was added dropwise. Then, 0.2 mol of diethyl phosphite was added. The mixture was heated to 120 °C and stirred for 4 h, after which the product "Ketal-PIDMP-Et4" was washed by vacuum distillation at 50 mbar and 150 °C. [ka]

[0136] "Ketal-PIDMP-Et4" is cleaved with a 5-fold molar excess of 80% acetic acid and stirred for 2 hours at 80° C. The resulting ethylene glycol is distilled and the intermediate product "Keton-PIDMP-Et4" is washed by vacuum distillation at 50 mbar and 150° C. [ka]

[0137] "OH-Vinyl-PIDMP-Et4" is obtained by filling the solvent THF (absolute) in an anhydrous apparatus and forming the Grignard reagent therein (c=1.5 mol). Then magnesium chips are added to the THF while continuously dropping vinyl bromide (1.2 mmol). "Keton-PIDMP-Et4" (1 mmol) is continuously dropped. After the reaction is over (as evidenced by the reduction of boiling, total reaction time: about 2 hours), the reaction mixture is hydrolyzed with cooled 1N hydrochloric acid (aq). The mixture is worked up by separating the aqueous phase and removing the solvent by distillation from the organic phase. The melting point of the obtained "OH-Vinyl-PIDMP-Et4" is 239 °C. The reaction yield is 85%.

[0138] Examples of flame retardants: composition The UL94 test was carried out using test specimens according to the IEC / DIN EN60695-11-10 standard to confirm the flame retardancy and to classify the flame retardant composition according to the present invention in various polymers.

[0139] UL94-V Test For each test, five specimens were clamped vertically and then held at the open end of a Bunsen burner flame. A cotton pad was placed under the specimen to assess burning time and falling of burning particles. This test and exposure to a 2 cm high Bunsen burner flame was performed precisely according to the Underwriter Laboratories standard UL94.

[0140] As a result, classifications of fire protection ratings V-0 to V-2 are quoted. V-0 in this case means that the total burning time of the five tested specimens was less than 50 seconds and the cotton pad did not burn due to the luminescence or burning droplets of the specimens. Classification V-1 means that the total burning time of the five tested specimens was more than 50 seconds but less than 250 seconds and similarly the cotton pad did not burn. V-2 in this case means that the total burning time of the five tested specimens was less than 250 seconds, but in at least one of the five tests the cotton pad burned due to the luminescence or burning droplets. The abbreviation NC means "not classifiable" and indicates that a total burning time of more than 250 seconds was measured. In many cases of not classifiable, the specimens burned completely.

[0141] UL94-HB Test For each test, at least three specimens were clamped horizontally and then held at the open end of a Bunsen burner flame to assess burn rate and total burn distance. These tests and exposure to a 2 cm high Bunsen burner flame were performed precisely according to Underwriter Laboratories standard UL94.

[0142] As a result, a classification into fire class HB is cited. A classification into HB means that the burning rate between a first marker at a distance of 25 mm from the flame front and a second marker at a distance of 100 mm from the flame front is less than or equal to 40 mm / min. Also, the flame front did not extend beyond the 100 mm marker. A classification of "NC" means "not classifiable" and indicates either a burning rate at a distance of 75 mm greater than 40 mm / min or a total burning distance greater than 100 mm.

[0143] L * a * b * value L * a * b *The values ​​were measured using an UltraScanVIS-2 spectrophotometer equipped with an UltraScanVIS sensor from HunterLab. For this purpose, the sample was filled into a glass cuvette, followed by impacting the cuvette or densifying the sample to form a homogenous surface on the side of the cuvette towards the measurement port. The associated EasyMatchQC4.64b software used the "USVIS1145" sensor and the "RSIN Mode" setting to measure the L * a * b * Calculate the value. The method complies with the currently valid version of EN ISO 11664-4.

[0144] Example 13: Flame retardancy of MOMP-H4 in polypropylene polymer In the following examples, the following polymeric materials were used to prepare the flame retardant compositions: Polypropylene (PP) HD120MO from Borealis AG

[0145] Granules with an approximate particle size of 3x1x1 mm were produced using a twin-screw extruder, model Process 11, Thermo Fisher Scientific Inc., under extrusion conditions typical for polypropylene. The extrusion process was run at a screw speed of 450-500 rpm and a temperature in the extrusion zone of 190-220 °C, with a throughput of approximately 5-7 kg / h. High-quality UL94-compliant test specimens were then obtained by hot pressing. The thicknesses of the test specimens were 1.6 mm and 3.2 mm, respectively. The phosphonate produced according to Example 1 was then compounded into the polymeric material during the extrusion process.

[0146] [Table 19]

[0147] Example 14: Flame retardancy of MOMP-H4 in polyurethane (PU) The flame retardant composition was prepared by combining the following ingredients together in a foaming reaction: Polyol: 22.5g Catalyst (ethylene glycol): 1.05g Pentane: 4.5g Isocyanate (MDI): 60g

[0148] The flame retardant according to the present invention was added to the polyol component prior to reaction. The weight ratios of the flame retardant quoted in the tables below refer to the sum of the weights of the polyol, catalyst, flame retardant, and isocyanate. [Table 20]

[0149] Example 15: Flame retardancy of MOMP-H4 in thermoplastic polyurethane (PU) In the following examples, the following polymeric materials were used to prepare the flame retardant compositions: Thermoplastic polyurethane (TPU) Elastollan 1185A from BASF SE

[0150] A twin-screw extruder, model Process 11, Thermo Fisher Scientific Inc., was used to produce granules with an approximate particle size of 3x1x1 mm under typical extrusion conditions for TPU. The extrusion process was run at a screw speed of 300 rpm and a temperature of 205°C in the extrusion zone with a throughput of approximately 5 kg / h. High-quality UL94-compliant test specimens were then obtained by hot pressing. The thickness of the test specimens was 0.8 mm. The phosphonate produced according to Example 1 was then incorporated into the polymeric material during the extrusion process. [Table 21]

[0151] Example 16: Flame retardancy of MOMP-H2Zn in thermoplastic polyamide (PA) The following materials were used in the following examples to prepare flame retardant compositions. Polyamide 6: Ultramid B3S (BASF) PA glass fiber (GF): CS7928 (Lanxess)

[0152] Granules with an approximate particle size of 3x1x1 mm were produced using a twin-screw extruder, model Process 11, Thermo Fisher Scientific Inc., under extrusion conditions typical for PA6. The extrusion process was run at a screw speed of 300 rpm and a temperature of 280°C in the extrusion zone, with a throughput of approximately 5 kg / h. High-quality UL94-compliant test specimens were then obtained by hot pressing. The thickness of the test specimens was 0.8 mm. The phosphonate produced according to Example 7 (MOMP-H2Zn) was then incorporated into the polymeric material during the extrusion process. [Table 22]

[0153] Example 17: Enhancement of flame retardancy and transparency of MOMP-Et4 in thermoplastic polyurethane coatings The polyurethane resin topcoat Goylake A-1219-9 from Irurena Group was cut with MOMP-Et4 and mixed under vigorous stirring. The ratio of MOMP-Et4 to the total mass (250 g) consisting of the mass of MOMP-Et4 and the mass of polyurethane resin was 5 wt% (Recipe A) or 10 wt% (Recipe B). To this total mass, 10 wt% of the curing catalyst C-212 from Irurena Group was added, and then mixed under vigorous stirring.

[0154] The transparent mixture was then applied to a commercial chipboard using a 500 μm scraper, and the panels were subsequently dried at 80°C. In a subsequent Epiradiator fire test according to NF P 92-501, both Recipe A and Recipe B achieved an M3 classification.

[0155] Transparency measurement To confirm the transparency of recipes A and B, they were coated on white and black substrates using a 500 μm scraper. For each substrate, two coated samples (Test Nos. 1 and 2) and two uncoated control samples (Test Nos. 3 and 4) were measured using the L * a * b * The values ​​were measured.

[0156] As shown in the table below, the coatings of recipes A and B are * a * b * The flame retardants according to the invention are therefore particularly suitable for use in transparent coatings, as they cause negligible changes in the colour space values, e.g. the coatings are highly transparent and have no or only a minor effect on the appearance of the substrate.

[0157] Recipe A Black Board [Table 23]

[0158] white board [Table 24]

[0159] Recipe B Black Board [Table 25]

[0160] white board [Table 26]

[0161] Description of diagram Figures 1 to 14 represent the thermogravimetric measurements and the results are shown in the table below. [Table 27]

Claims

1. A halogen-free composition comprising a polymeric material and containing and / or bonded thereto a flame retardant in an amount of 1-40% by weight relative to the total composition, said flame retardant being a compound of formula (I), its corresponding ammonium salt, its corresponding phosphonate, or a mixture thereof, [Formula 1] (N-i)R 1 and R 2 are the same or different substituents and are selected from the group consisting of linear, branched or cyclic alkyl, alkenyl and alkynyl, unsubstituted and alkyl-substituted phenyl, mono- and polynuclear aromatics with up to four nuclei, mono- or polynuclear heteroaromatics with up to four nuclei, silyl, allyl, alkyl or aryl alcohols, or (N-ii)R 1 and R 2 together form a saturated or mono- or polyunsaturated heterocyclic ring having 4 to 8 ring atoms selected from carbon, oxygen, sulfur, phosphorus, silicon and nitrogen, including the N atom; -X- is an oxygen atom -O-, or -X- is a single bond; R 3 , R 4 , R 5 and R 6 are specified by (P-i), (P-i) and (P-ii), or (P-i) and (P-iii); (P-i)R 3 , R 4 , R 5 and R 6 are the same or different substituents, and have the following structures (III) and (IV) with n=0 to 100: H, linear, branched or cyclic alkyl, alkenyl and alkynyl, unsubstituted and alkyl-substituted phenyl, polynuclear aromatics with up to 4 nuclei, mononuclear or polynuclear heteroaromatics with up to 4 nuclei, silyl, allyl, alkyl or aryl alcohols, [chemical 2] cations selected from the group consisting of Na + , K + , Mg 2+ , Ca 2+ , B 3+, Al 3+ , Zn 2+ , N.H. 4+ or melamine or a condensate thereof. (P-ii) When R 3 to R 6 form a ring and —X— is an oxygen atom —O—, —OR 3 and -OR 4 and / or -OR 5 and -OR 6 and / or -OR 3 and -OR 5 and / or -OR 4 and -OR 6 together form a cyclic phosphonate or cyclic phosphonic anhydride having a ring size of 4 to 10 atoms, including the P atom of the phosphonate group. (P-iii) When R 3 to R 6 form a ring and —X— is a single bond, —R 3 and -OR 4 And / or -R 3 and -OR 5 together form a cyclic phosphinic ester or cyclic phosphinic anhydride having a ring size of 4 to 10 atoms, including the P atom of the phosphinate group, and / or -OR 5 and -OR 6 And / or -OR 4 and -OR 6 together form a cyclic phosphonate or cyclic phosphonic anhydride having a ring size of 4 to 10 atoms, including the P atom of the phosphonate group. A) Substituent R 1 ~R 6 or B) 1) Substituent R 3 ~R 6 forms a cyclic phosphine or phosphonate ester according to (P-ii) or (P-iii), or 2) Substituent R 3 ~R 6 forming a cyclic phosphine or phosphonic anhydride according to (P-ii) or (P-iii), or 3) Substituent R 1 and R 2 When a heterocyclic ring is formed according to (N-ii), One of the cycles that forms in a) heteroatoms selected from the group consisting of P, O, N, S, and / or b) an alkene or alkyne group and a first uncharged or negatively charged functional group having the formula: The functional group is not -OH, and if one of the cycles according to 1) to 3) has the functional group, the ring atom of the cycle is substituted with the functional group or with a substituent having the functional group. A composition comprising:

2. The substituent R 1 ~R 6 or at least one of the substituents R 1 ~R 6 2. The composition of claim 1, characterized in that any of the cycles formed by further comprises at least one functional group having a heteroatom selected from the group consisting of N, S, O, Si and / or an alkene or alkyne group.

3. The first and / or further functional groups are -NH 2 , -NHR, -NR 2 , -OH, -OR, =O, -SH, -SR, -COOH, -COOR, -OCN, -SiR x H y , -N 3 3. The composition of claim 1 or 2, wherein R=alkyl, alkenyl, alkynyl or aryl, and x+y=3.

4. The composition according to any one of claims 1 to 3, characterized in that the flame retardant is covalently bonded to the polymeric material.

5. R 1 and R 2The composition according to any one of claims 1 to 4, wherein are the same substituents.

6. A composition according to any one of claims 1 to 5, characterised in that the first and / or further functional groups are alkenyl or epoxy groups.

7. The composition according to any one of claims 1 to 6, characterized in that the flame retardant is a dry flame retardant which reaches a mass loss of 10% by weight starting at a temperature of 180°C.

8. The composition according to any one of claims 1 to 7, characterized in that the phosphorus content of the flame retardant is at least 10.0% by weight.

9. The group R 3 , R 4 , R 5 and R 6 At least one of is a cation or H, and the cation is Na + , K + , Mg 2+ , Ca 2+ , B 3+ , Al 3+ , Zn 2+ , N.H. 4+ 9. The composition according to claim 1, wherein the ammonium ion of an amine compound selected from the group consisting of melamine and a condensate thereof.

10. 10. The composition according to claim 1, wherein the polymeric material comprises the flame retardant in an amount of at least 3% by weight and / or in an amount not greater than 35% by weight relative to the total composition.

11. The composition according to any one of claims 1 to 10, characterized in that the polymeric material comprises at least one further flame retardant component.

12. 12. A method for producing a composition according to any one of claims 1 to 11, characterized in that the flame retardant is a co-condensation or co-addition component of a polymeric material which is incorporated into the polymeric material being produced by polycondensation or polyaddition, the polymeric material being a polyester or polyurethane.

13. The substituent R 3 ~R 6 The flame retardant according to any one of claims 1 to 12, characterized in that the cycle formed by these has a first functional group.

14. A method for producing a flame retardant comprising the following steps: Providing a mixture of the following components: a) component, b) component, and c) component; a) at least one phosphonic or phosphinic acid selected from the group consisting of compounds of formulae (V) and (VI) in a reaction vessel; [C3] -X- is an oxygen atom -O-, or -X- is a single bond; R 3 , R 4 , R 5 and R 6 are specified by (P-i), (P-i) and (P-ii), or (P-i) and (P-iii); (P-i)R 3 , R 4 , R 5 and R 6 are the same or different substituents, and have the following structures (III) and (IV) with n=0 to 100: H, linear, branched or cyclic alkyl, alkenyl and alkynyl, unsubstituted and alkyl-substituted phenyl, polynuclear aromatics with up to 4 nuclei, mononuclear or polynuclear heteroaromatics with up to 4 nuclei, silyl, allyl, alkyl or aryl alcohols, [C4] cations selected from the group consisting of Na + , K + , Mg 2+ , Ca 2+ , B 3+ , Al 3+ , Zn 2+, N.H. 4+ or melamine or a condensate thereof. (P-ii) When R 3 to R 6 form a ring and —X— is an oxygen atom —O—, —OR 3 and -OR 4 and / or -OR 5 and -OR 6 and / or -OR 3 and -OR 5 and / or -OR 4 and -OR 6 together form a cyclic phosphonate or cyclic phosphonic anhydride having a ring size of 4 to 10 atoms, including the P atom of the phosphonate group. (P-iii) When R 3 to R 6 form a ring and —X— is a single bond, —R 3 and -OR 4 and / or -R 3 and -OR 5 together form a cyclic phosphonic ester or cyclic phosphonic anhydride having a ring size of 4 to 10 atoms, including the P atom of the phosphinate group, and / or -OR 5 and -OR 6 And / or -OR 4 and -OR 6 together form a cyclic phosphonate or cyclic phosphonic anhydride having a ring size of 4 to 10 atoms, including the P atom of the phosphonate group. b) R 7 HC(OR) = alkyl, aryl or alkenyl 7 ) 3, c) an amino compound of formula (VII); [C5] (N-i)R 1 and R 2 are the same or different substituents and are selected from the group consisting of linear, branched or cyclic alkyl, alkenyl and alkynyl, unsubstituted and alkyl-substituted phenyl, mono- and polynuclear aromatics with up to four nuclei, mono- or polynuclear heteroaromatics with up to four nuclei, silyl, allyl, alkyl or aryl alcohols, or (N-ii)R 1 and R 2 together form a saturated or mono- or polyunsaturated heterocycle having from 4 to 8 ring atoms selected from carbon, oxygen, sulfur, phosphorus, silicon, and nitrogen, including the N atom. Heating the mixture to a temperature in the range of 40 to 150°C.

15. Use of a compound of formula (I), its corresponding ammonium salt, its corresponding phosphonate, or a mixture. [C6] (N-i)R 1 and R 2 are the same or different substituents and are selected from the group consisting of linear, branched or cyclic alkyl, alkenyl and alkynyl, unsubstituted and alkyl-substituted phenyl, mono- and polynuclear aromatics with up to four nuclei, mono- or polynuclear heteroaromatics with up to four nuclei, silyl, allyl, alkyl or aryl alcohols, or (N-ii)R 1 and R 2 together form a saturated or mono- or polyunsaturated heterocyclic ring having 4 to 8 ring atoms selected from carbon, oxygen, sulfur, phosphorus, silicon and nitrogen, including the N atom; -X- is an oxygen atom -O-, or -X- is a single bond; R 3 , R 4 , R 5 and R 6 are specified by (P-i), (P-i) and (P-ii), or (P-i) and (P-iii); (P-i)R 3 , R 4 , R 5 and R 6 are the same or different substituents, and have the following structures (III) and (IV) with n=0 to 100: H, linear, branched or cyclic alkyl, alkenyl and alkynyl, unsubstituted and alkyl-substituted phenyl, polynuclear aromatics with up to 4 nuclei, mononuclear or polynuclear heteroaromatics with up to 4 nuclei, silyl, allyl, alkyl or aryl alcohols, [C7] cations selected from the group consisting of Na + , K + , Mg 2+ , Ca 2+ , B 3+ , Al 3+ , Zn 2+ , N.H. 4+ or melamine or a condensate thereof. (P-ii) When R 3 to R 6 form a ring and —X— is an oxygen atom —O—, —OR 3 and -OR 4 and / or -OR 5 and -OR 6 and / or -OR 3 and -OR 5 and / or -OR 4 and -OR 6 together form a cyclic phosphonate or cyclic phosphonic anhydride having a ring size of 4 to 10 atoms, including the P atom of the phosphonate group. (P-iii) When R 3 to R 6 form a ring and —X— is a single bond, —R 3 and -OR 4 And / or -R 3 and -OR 5 together form a cyclic phosphinic ester or cyclic phosphinic anhydride having a ring size of 4 to 10 atoms, including the P atom of the phosphinate group, and / or -OR 5 and -OR 6 And / or -OR 4 and -OR 6 together form a cyclic phosphonate or cyclic phosphonic anhydride having a ring size of 4 to 10 atoms, including the P atom of the phosphonate group.

Citation Information

Patent Citations

  • Aminomethane phosphonic acid aryl esters and a process for their preparation

    CA2027078A1

  • Reactive phosphate ester flame retardant, preparation method thereof, and application thereof in polyurethane foam

    CN109651584A

  • Aminomethanephosphonates - used as flame retardants for polyurethanes

    DE2128060A1

  • Process for the preparation of N,N-bis-(2-hydroxyalkyl)-aminomethane-phosphonic acid dimethyl esters, and their use as flame retardants for polymers

    EP0001996A1

  • Alkenylaminoalkylenephosphonic ester, and prodction of copolymer of alkenylaminoalkylenephosphonate with ethylenically unsaturated compound

    JP1994049082A