Polishing composition, method for producing polishing composition, polishing method, and method for producing semiconductor substrate

A polishing composition with colloidal silica and a quaternary ammonium compound at specific pH and zeta potential enhances SiOC polishing rates, addressing inefficiencies in existing technologies and improving semiconductor substrate processing.

JP7591634B2Active Publication Date: 2024-11-28FUJIMI INCORPORATED
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2023182296
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-10-24
Publication Date
2024-11-28
Estimated Expiration
2039-09-13

AI Technical Summary

Technical Problem

Existing polishing compositions for SiOC surfaces have insufficient polishing rates, limiting the efficiency of semiconductor substrate processing.

Method used

A polishing composition containing colloidal silica with a zeta potential of -60 mV to -35 mV at pH less than 4.0 and a quaternary ammonium compound with specific hydrophobic groups is used to enhance the polishing rate of SiOC surfaces.

Benefits of technology

The composition achieves a significantly higher polishing rate for SiOC surfaces, reducing surface defects and improving processing efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007591634000001
    Figure 0007591634000001
  • Figure 0007591634000002
    Figure 0007591634000002
  • Figure 0007591634000003
    Figure 0007591634000003
Patent Text Reader

Abstract

To provide a polishing composition that can polish SiOC at a high polishing speed.SOLUTION: A polishing composition comprises colloidal silica and a quaternary ammonium cation represented by Formula (1), wherein the pH is less than 4.0, and the zeta potential of the colloidal silica is -60 mV or higher and -35 mV or lower.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polishing composition, a method for producing the polishing composition, a polishing method, and a method for producing a semiconductor substrate. [Background technology]

[0002] In recent years, with the trend toward multi-layer wiring on the surface of semiconductor substrates, a so-called chemical mechanical polishing (CMP) technique is used to physically polish and flatten the semiconductor substrate when manufacturing devices. CMP is a method for flattening the surface of an object to be polished (workpiece to be polished) such as a semiconductor substrate by using a polishing composition (slurry) containing abrasive grains such as silica, alumina, ceria, etc., an anticorrosive agent, a surfactant, etc., and the object to be polished (workpiece to be polished) is silicon, polysilicon, silicon oxide (SiO2), carbon-containing silicon oxide (SiOC), silicon nitride (SiN), wiring, plugs, etc. made of metal, etc.

[0003] For example, Patent Document 1 discloses a polishing composition for polishing insulating films with low relative dielectric constants such as SiOC, which contains colloidal silica particles, a benzotriazole compound, and a secondary or tertiary amino alcohol and has a pH in the range of 7 to 10. This technology is said to be capable of suppressing the occurrence of scratches on insulating films such as SiOC. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2008-091569 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, it has been found that the technique described in Patent Document 1 has a problem in that the improvement in polishing rate is still insufficient.

[0006] Therefore, an object of the present invention is to provide a polishing composition capable of polishing SiOC at a high polishing rate. [Means for solving the problem]

[0007] The present inventors have conducted extensive research to solve the above problems. As a result, they have discovered that a crystalline crystalline cellulose containing colloidal silica and a crystalline cellulose having the following formula (1):

[0008] [ka]

[0009] Here, R 1 ~R 4 R 1 ~R 4 Among A, the remaining 3 or 2 groups other than the first group are each independently a second group which is an alkyl group having 1 or 2 carbon atoms or an alkenyl group having 2 carbon atoms, - is a monovalent anion, It has been found that the above problem can be solved by a polishing composition comprising a quaternary ammonium compound represented by the following formula: Effect of the Invention

[0010] According to the present invention, there is provided a polishing composition capable of polishing SiOC at a high polishing rate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, the embodiments of the present invention will be described, but the present invention is not limited to only the following embodiments. Unless otherwise specified, the operation and measurement of physical properties are performed under the conditions of room temperature (20 to 25°C) and relative humidity 40 to 50% RH. In addition, in this specification, "X to Y" indicating a range means "X or more and Y or less."

[0012] <Polishing composition> The present invention relates to a polishing composition used for polishing an object to be polished, the polishing composition comprising colloidal silica and a fluorine-containing alumina compound represented by the following formula (1):

[0013] [ka]

[0014] Where: R 1 ~R 4 wherein the first or second group is independently an alkyl group having from 3 to 20 carbon atoms, an alkenyl group having from 3 to 20 carbon atoms, or an aryl group having from 6 to 20 carbon atoms; R 1 ~R 4 the remaining 3 or 2 groups other than the first group are each independently a second group which is an alkyl group having 1 or 2 carbon atoms or an alkenyl group having 2 carbon atoms, A - is a monovalent anion, and a quaternary ammonium compound represented by the formula (1), wherein the pH is less than 4.0, and the zeta potential of the colloidal silica is -60 mV or more and -35 mV or less. The polishing composition can polish SiOC at a high polishing rate.

[0015] The reason why the polishing composition of the present invention exhibits the above-mentioned effects is not necessarily clear, but is thought to be as follows.

[0016] The polishing composition of the present invention contains colloidal silica having a predetermined zeta potential at a pH of less than 4.0 and a quaternary ammonium compound having a specific structure. Specifically, the colloidal silica used in the polishing composition has a zeta potential of -60 mV to -35 mV at a pH of less than 4.0, and the quaternary ammonium compound has one or two hydrophobic groups (first groups).

[0017] Here, "zeta (ζ) potential" refers to the potential difference that occurs at the interface between a solid and a liquid when they are in contact with each other and undergo relative motion. In the polishing composition of the present invention, the pH is less than 4.0, and the zeta potential of the SiOC surface is significantly positive due to the presence of a quaternary ammonium compound with a specific structure at a pH of less than 4.0. That is, in the presence of a quaternary ammonium compound with a specific structure at a pH of less than 4.0, the SiOC surface is positively charged, and the absolute value of the zeta potential becomes large.

[0018] Therefore, when polishing SiOC using the polishing composition of the present invention, in the presence of a quaternary ammonium compound with a specific structure, colloidal silica is negatively charged and SiOC is positively charged. This makes SiOC and colloidal silica strongly attracted to each other, so that the polishing rate of SiOC increases. However, it goes without saying that this mechanism is merely speculation and does not limit the technical scope of the present invention.

[0019] [Polished object] The object to be polished by the polishing composition of the present invention preferably contains SiOC (carbon-containing silicon oxide). That is, the polishing composition of the present invention is preferably used for polishing an object to be polished that contains SiOC. The object to be polished may contain a material other than SiOC, and the material other than SiOC contained in the object to be polished is not particularly limited, and examples thereof include silicon oxide, silicon nitride, silicon carbonitride (SiCN), polycrystalline silicon (polysilicon), non-crystalline silicon (amorphous silicon), metal, SiGe, etc.

[0020] The object to be polished containing SiOC may be any object containing a SiOC (film) formed by a known method, and suitable examples of the object to be polished include an object to be polished containing a SiOC (film) formed by a SOG (spin on glass) method and an SiOC (film) formed by a flowable chemical vapor deposition (FCVD) method.

[0021] [Colloidal Silica] The polishing composition of the present invention contains colloidal silica as an abrasive. The colloidal silica used in the polishing composition of the present invention has a zeta potential of -60 mV or more and -35 mV or less at a pH of less than 4.0. The zeta potential of the colloidal silica is preferably -55 mV or more and -38 mV or less, more preferably -50 mV or more and -40 mV or less. When the colloidal silica has a zeta potential in this range, the polishing rate for SiOC can be further improved.

[0022] Here, the zeta potential of the colloidal silica in the polishing composition is calculated by subjecting the polishing composition to an ELS-Z2 manufactured by Otsuka Electronics Co., Ltd., measuring the composition at a measurement temperature of 25°C using a flow cell by a laser Doppler method (electrophoretic light scattering measurement method), and analyzing the obtained data by the Smoluchowski formula.

[0023] The colloidal silica can be produced by a sodium silicate method or a sol-gel method, and colloidal silica produced by either method can be suitably used as the colloidal silica of the present invention. However, from the viewpoint of reducing metal impurities, colloidal silica produced by the sol-gel method is preferred. Colloidal silica produced by the sol-gel method is preferred because it contains less metal impurities that are diffusible in semiconductors and less corrosive ions such as chloride ions. Colloidal silica can be produced by the sol-gel method using a conventionally known method, and specifically, colloidal silica can be obtained by hydrolysis and condensation reaction using a hydrolyzable silicon compound (e.g., alkoxysilane or its derivative) as a raw material.

[0024] The type of colloidal silica used is not particularly limited, but for example, surface-modified colloidal silica can be used. Surface modification of colloidal silica can be performed, for example, by chemically bonding a functional group of an organic acid to the surface of colloidal silica, that is, by immobilizing the organic acid. Alternatively, the surface modification of colloidal silica can be performed by mixing colloidal silica with a metal such as aluminum, titanium, or zirconium, or an oxide thereof, and doping the surface of silica particles.

[0025] In a preferred embodiment of the present invention, the colloidal silica contained in the polishing composition is colloidal silica with organic acid fixed on the surface. The colloidal silica with organic acid fixed on the surface tends to have a larger absolute value of zeta potential in the polishing composition than normal colloidal silica with no organic acid fixed on the surface. Therefore, the zeta potential of colloidal silica in the polishing composition is easily adjusted to a range of -60mV or more and -35mV or less.

[0026] The zeta potential of colloidal silica can be controlled to a desired range, for example, by using colloidal silica with the above-mentioned organic acid fixed on the surface, as well as by adjusting the type and amount of the quaternary ammonium compound described below.The zeta potential of colloidal silica can also be controlled to a desired range, for example, by using the below-mentioned acid as a pH adjuster.

[0027] Preferred examples of colloidal silica having an organic acid fixed to its surface include colloidal silica having an organic acid such as a carboxylic acid group, a sulfonic acid group, a phosphonic acid group, an aluminic acid group, etc. Among these, from the viewpoint of ease of production, colloidal silica having a sulfonic acid or a carboxylic acid fixed to its surface is preferred, and colloidal silica having a sulfonic acid fixed to its surface is more preferred.

[0028] Immobilization of an organic acid on the surface of colloidal silica cannot be achieved by simply having colloidal silica and an organic acid coexist. For example, if you want to immobilize sulfonic acid, which is a type of organic acid, on colloidal silica, you can use the method described in "Sulfonic acid-functionalized silica through of thiol groups", This can be done by the method described in Chem. Commun. 246-247 (2003). Specifically, a silane coupling agent having a thiol group, such as 3-mercaptopropyltrimethoxysilane, is coupled to colloidal silica, and then the thiol group is oxidized with hydrogen peroxide to obtain colloidal silica having sulfonic acid fixed on the surface (sulfonic acid-modified colloidal silica).

[0029] Alternatively, when a carboxylic acid, which is a type of organic acid, is immobilized on colloidal silica, it can be carried out by, for example, the method described in “Novel Silane Coupling Agents Containing a Photolabile 2-Nitrobenzyl Ester for Introduction of a Carboxy Group on the Surface of Silica Gel”, Chemistry Letters, 3, 228-229 (2000). Specifically, a silane coupling agent containing a photoreactive 2-nitrobenzyl ester is coupled to colloidal silica, followed by light irradiation, to obtain colloidal silica with a carboxylic acid immobilized on the surface (carboxylic acid-modified colloidal silica).

[0030] In the polishing composition of the present invention, the lower limit of the average primary particle size of colloidal silica is preferably 1 nm or more, more preferably 5 nm or more, and even more preferably 7 nm or more.In addition, in the polishing composition of the present invention, the upper limit of the average primary particle size of colloidal silica is preferably 100 nm or less, more preferably 75 nm or less, and even more preferably 50 nm or less.Within such a range, defects such as scratches that may occur on the surface of the object to be polished after polishing with the polishing composition can be suppressed.The average primary particle size of colloidal silica is calculated based on the specific surface area of ​​colloidal silica measured by BET method, for example.

[0031] In the polishing composition of the present invention, the lower limit of the average secondary particle size of colloidal silica is preferably 2 nm or more, more preferably 10 nm or more, and even more preferably 15 nm or more.In addition, in the polishing composition of the present invention, the upper limit of the average primary particle size of colloidal silica is preferably 200 nm or less, more preferably 150 nm or less, and even more preferably 100 nm or less.Within such a range, defects such as scratches that may occur on the surface of the object to be polished after polishing with the polishing composition can be suppressed.The average primary particle size of colloidal silica can be measured, for example, by dynamic light scattering method represented by laser diffraction scattering method.

[0032] The average degree of association of colloidal silica is preferably 5.0 or less, more preferably 3.0 or less, and even more preferably 2.5 or less. As the average degree of association of colloidal silica is smaller, it is easier to obtain a polished surface with fewer surface defects by polishing an object to be polished using the polishing composition. In addition, the average degree of association of colloidal silica is preferably 1.0 or more, more preferably 1.2 or more. As the average degree of association of colloidal silica is larger, there is an advantage that the removal rate of the object to be polished by the polishing composition is improved. The average degree of association of colloidal silica is obtained by dividing the average secondary particle size of colloidal silica by the average primary particle size.

[0033] In the present invention, the shape of colloidal silica is not particularly limited, and may be either spherical or non-spherical, but is preferably non-spherical.Specific examples of non-spherical shapes include polygonal prisms such as triangular prisms and square prisms, cylinders, bales in which the center of a cylinder is bulging out more than the ends, donuts in which the center of a disk is penetrated, plates, so-called cocoon shapes with a constriction in the center, so-called association-type spheres in which multiple particles are integrated, so-called confetti shapes with multiple protrusions on the surface, and rugby ball shapes, and various other shapes are not particularly limited.

[0034] The lower limit of the content of colloidal silica is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, and even more preferably 1% by mass or more, based on the polishing composition.The upper limit of the content of colloidal silica is preferably 20% by mass or less, more preferably 10% by mass or less, and even more preferably 5% by mass or less, based on the polishing composition.Within such a range, the polishing rate can be further improved.In addition, when the polishing composition contains two or more kinds of colloidal silica, the content of colloidal silica means the total amount of these.

[0035] As long as the polishing composition according to the embodiment of the present invention contains colloidal silica having a zeta potential in the specific range, it may contain other abrasive grains. Examples of the other abrasive grains include metal oxide grains such as alumina grains, zirconia grains, and titania grains.

[0036] [Quaternary ammonium compounds] The polishing composition of the present invention contains a quaternary ammonium compound represented by the following formula (1) (hereinafter also simply referred to as a "quaternary ammonium compound").

[0037] [ka]

[0038] In formula (1), R 1 ~R 4R 1 ~R 4 Among these, the remaining 3 or 2 groups other than the first group are each independently a second group which is an alkyl group having 1 or 2 carbon atoms or an alkenyl group having 2 carbon atoms.

[0039] Here, the first group acts as a hydrophobic group in the quaternary ammonium compound.It is presumed that in the polishing composition of the present invention, the quaternary ammonium compound having the first group with high hydrophobicity exists, so that the quaternary ammonium salt behaves as a cationic surfactant in the polishing composition, and as a result, the zeta potential of the SiOC surface can be significantly changed to positive.

[0040] When there are two first groups, the first groups may be the same or different from each other. Similarly, the three or two second groups may be the same or different from each other.

[0041] The alkyl group having 3 to 20 carbon atoms may be linear or branched. Specific examples of the alkyl group having 3 to 20 carbon atoms are not particularly limited, and include n-propyl group, isopropyl group, n-butyl group, isobutyl group, sec-butyl group, tert-butyl group, n-pentyl group, isopentyl group, neopentyl group, 2-ethylhexyl group, n-hexyl group, n-heptyl group, n-octyl group, n-nonyl group, n-decyl group, n-undecyl group, n-dodecyl group, n-tridecyl group, n-tetradecyl group (myristyl group), n-pentadecyl group, n-hexadecyl group (palmityl group), n-heptadecyl group, n-octadecyl group (stearyl group), n-nonadecyl group, and n-icosyl group.

[0042] The alkenyl group having 3 to 20 carbon atoms may be linear or branched. Specific examples of the alkenyl group having 3 to 20 carbon atoms are not particularly limited, but include 1-propenyl group, isopropenyl group, 2-methyl-1-propenyl group, 1-butenyl group, 2-butenyl group, 3-butenyl group, 2-ethyl-1-butenyl group, 1-pentenyl group, 2-pentenyl group, 3-pentenyl group, 4-pentenyl group, 4-methyl-3-pentenyl group, 1-hexenyl group, 2 ... Examples of the aryl group include cis-9-octadecenyl group, cis-1-octenyl group, 3-hexenyl group, 4-hexenyl group, 5-hexenyl group, 1-octenyl group, 2-octenyl group, 1-dodecenyl group, 2-dodecenyl group, 3-dodecenyl group, 2-tetradecenyl group, 1-hexadecenyl group, 2-hexadecenyl group, 1-octadecenyl group, 2-octadecenyl group, and oleyl group (cis-9-octadecenyl group).

[0043] Examples of the aryl group having 6 to 20 carbon atoms include a phenyl group, a 2-methylphenyl group, a 3-ethylphenyl group, and a naphthyl group.

[0044] Specific examples of the alkyl group having 1 or 2 carbon atoms include a methyl group and an ethyl group.

[0045] A specific example of the alkenyl group having 2 carbon atoms is a vinyl group.

[0046] In the quaternary ammonium compound represented by formula (1), the first group (i.e., R 1 ~R 4 Among these, the first or second group) is preferably an alkyl group having 4 to 18 carbon atoms, an alkenyl group having 4 to 18 carbon atoms, or an aryl group having 6 to 18 carbon atoms, more preferably an alkyl group having 6 to 16 carbon atoms, an alkenyl group having 6 to 16 carbon atoms, or an aryl group having 6 to 16 carbon atoms, still more preferably an alkyl group having 8 to 13 carbon atoms, an alkenyl group having 8 to 13 carbon atoms, or an aryl group having 6 to 13 carbon atoms, and most preferably an alkyl group having 8 to 13 carbon atoms. 1 ~R4 Among these, the remaining 3 or 2 groups other than the first group) are preferably a methyl group or an ethyl group, and more preferably a methyl group.

[0047] In the quaternary ammonium compound, the first group is R 1 ~R 4 and the second group is R 1 ~R 4 Of the four groups, three or two are preferred, but preferably the number of the first group is one and the number of the second groups is three. This allows for a greater improvement in the polishing rate.

[0048] In formula (1), A - is a monovalent anion. Monovalent anion A - is any monovalent anion, and is not particularly limited, but is preferably a halide ion such as a fluoride ion, a chloride ion, a bromide ion, or an iodide ion; a hydroxide ion; or an organic acid ion such as a benzoate ion. Among them, a halide ion is preferable, and a chloride ion is more preferable. The monovalent anion may be used alone or in combination of two or more kinds.

[0049] The quaternary ammonium compound represented by formula (1) is -When is a chloride ion, butyl trimethyl ammonium chloride, octyl trimethyl ammonium chloride, dioctyl dimethyl ammonium chloride, decyl trimethyl chloride, dodecyl trimethyl ammonium chloride, didodecyl dimethyl ammonium chloride, tetradecyl trimethyl ammonium chloride, hexadecyl trimethyl ammonium chloride, stearyl trimethyl ammonium chloride, distearyl dimethyl ammonium chloride, phenyl trimethyl ammonium chloride, etc. are preferably used. Among these, butyl trimethyl ammonium chloride, dodecyl trimethyl ammonium chloride, stearyl trimethyl ammonium chloride, and phenyl trimethyl ammonium chloride are preferred, and dodecyl trimethyl ammonium chloride and stearyl trimethyl ammonium chloride are more preferred.

[0050] These quaternary ammonium compounds may be used alone or in combination of two or more.

[0051] The lower limit of the content of the quaternary ammonium compound is preferably 0.001% by mass or more, more preferably 0.005% by mass or more, and even more preferably 0.01% by mass or more, based on the polishing composition. The upper limit of the content of the quaternary ammonium compound is preferably 5% by mass or less, more preferably 1% by mass or less, and even more preferably 0.5% by mass or less, based on the polishing composition. In this range, the polishing rate can be further improved. In addition, when the polishing composition contains two or more kinds of quaternary ammonium compounds, the content of the quaternary ammonium compound means the total amount of these.

[0052] [pH and pH adjusters] The pH of the polishing composition of the present invention is less than 4.0. If the pH is 4.0 or more, the polishing speed of the object to be polished cannot be improved. The pH of the polishing composition of the present invention may be less than 4.0, and is more preferably 3.9 or less. If the pH is less than 4.0, there is an advantageous effect of improving the polishing speed of the object to be polished, particularly SiOC. The lower limit of the pH is preferably 1.0 or more, more preferably 1.5 or more.

[0053] A pH adjuster may be used to adjust the pH of the polishing composition to a desired value.

[0054] The pH adjuster to be used may be an inorganic acid, an organic acid, an alkali, etc. These may be used alone or in combination of two or more kinds.

[0055] Specific examples of inorganic acids that can be used as pH adjusters include hydrochloric acid, sulfuric acid, nitric acid, hydrofluoric acid, boric acid, carbonic acid, hypophosphorous acid, phosphorous acid, and phosphoric acid. Among these, hydrochloric acid, sulfuric acid, nitric acid, and phosphoric acid are preferred.

[0056] Specific examples of organic acids that can be used as pH adjusters include formic acid, acetic acid, propionic acid, butyric acid, valeric acid, 2-methylbutyric acid, n-hexanoic acid, 3,3-dimethylbutyric acid, 2-ethylbutyric acid, 4-methylpentanoic acid, n-heptanoic acid, 2-methylhexanoic acid, n-octanoic acid, 2-ethylhexanoic acid, benzoic acid, glycolic acid, salicylic acid, glyceric acid, oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, maleic acid, phthalic acid, malic acid, tartaric acid, citric acid, lactic acid, diglycolic acid, 2-furan carboxylic acid, 2,5-furandicarboxylic acid, 3-furan carboxylic acid, 2-tetrahydrofuran carboxylic acid, methoxyacetic acid, methoxyphenylacetic acid, and phenoxyacetic acid. Organic sulfuric acids such as methanesulfonic acid, ethanesulfonic acid, and isethionic acid may also be used. Among these, dicarboxylic acids such as malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, maleic acid, phthalic acid, malic acid and tartaric acid, and tricarboxylic acids such as citric acid are preferred.

[0057] Instead of or in combination with an inorganic or organic acid, a salt such as an alkali metal salt of an inorganic or organic acid may be used as a pH adjuster. In the case of a combination of a weak acid and a strong base, a strong acid and a weak base, or a weak acid and a weak base, a pH buffering effect can be expected.

[0058] Specific examples of alkalis that can be used as pH adjusters include ammonia, sodium hydroxide, potassium hydroxide, tetramethylammonium hydroxide, etc. The content of the pH adjuster can be selected by appropriately adjusting it within the range in which the effects of the present invention can be achieved.

[0059] The pH of the polishing composition can be measured, for example, by a pH meter.

[0060] [Other ingredients] The polishing composition of the present invention may further contain other components such as a dispersion medium, inorganic salts, surfactants other than the quaternary ammonium compound represented by formula (1), a water-soluble polymer, a preservative, an antifungal agent, an oxidizing agent, etc. The other components, that is, the dispersion medium, inorganic salts, surfactants, water-soluble polymers, preservatives and antifungal agents, and an oxidizing agent, will be described below.

[0061] [Dispersion medium] The polishing composition may contain a dispersion medium (solvent) for dispersing each component constituting the polishing composition. The dispersion medium has the function of dispersing or dissolving each component. The dispersion medium may be an organic solvent or water, but it is preferable to contain water, and more preferable to be water.

[0062] From the viewpoint of suppressing contamination of the polishing object and inhibiting the action of other components, the dispersion medium is preferably water that contains as few impurities as possible. For example, the total content of transition metal ions is preferably 100 ppb or less. Here, the purity of water can be increased by, for example, removing impurity ions using ion exchange resin, removing foreign matter using a filter, distillation, etc. Specifically, for example, deionized water (ion-exchanged water), pure water, ultrapure water, distilled water, etc. are preferably used as the water. Usually, the dispersion medium contained in the polishing composition is preferably 90% by volume or more of water, more preferably 95% by volume or more of water, even more preferably 99% by volume or more of water, and particularly preferably 100% by volume of water.

[0063] The dispersion medium may be a mixed solvent of water and an organic solvent for dispersing or dissolving each component. In this case, examples of the organic solvent used include acetone, acetonitrile, ethanol, methanol, isopropanol, glycerin, ethylene glycol, propylene glycol, etc., which are organic solvents miscible with water. These organic solvents may be used without being mixed with water, and then each component may be dispersed or dissolved, and then mixed with water. These organic solvents may be used alone or in combination of two or more kinds.

[0064] [Inorganic salts] The polishing composition of the present invention may contain an inorganic salt. Specific examples of the inorganic salt added in the present invention include ammonium sulfate, magnesium chloride, potassium acetate, and aluminum nitrate.

[0065] [Surfactants] The polishing composition of the present invention may contain a surfactant other than the quaternary ammonium compound represented by formula (1). The surfactant added in the present invention may be any of an anionic surfactant, a cationic surfactant, an amphoteric surfactant, and a nonionic surfactant.

[0066] Examples of anionic surfactants include polyoxyethylene alkyl ether acetates, polyoxyethylene alkyl sulfates, alkyl sulfates, polyoxyethylene alkyl ether sulfates, alkyl ether sulfates, alkyl benzene sulfonates, alkyl phosphates, polyoxyethylene alkyl phosphates, polyoxyethylene sulfosuccinic acids, alkyl sulfosuccinic acids, alkyl naphthalene sulfonates, alkyl diphenyl ether disulfonic acids, and salts thereof.

[0067] Examples of cationic surfactants include those other than the quaternary ammonium compounds represented by formula (1), such as tetramethylammonium salts.

[0068] Examples of amphoteric surfactants include alkyl betaines and alkyl amine oxides.

[0069] Examples of nonionic surfactants include polyoxyethylene alkyl ethers, polyoxyalkylene alkyl ethers, sorbitan fatty acid esters, glycerin fatty acid esters, polyoxyethylene fatty acid esters, polyoxyethylene alkyl amines, and alkyl alkanolamides.

[0070] The surfactants can be used alone or in combination of two or more.

[0071] [Water-soluble polymer] The polishing composition of the present invention may contain water-soluble polymer.Specific examples of the water-soluble polymer added in the present invention include polystyrene sulfonate, polyisoprene sulfonate, polyacrylic acid salt, polymaleic acid, polyitaconic acid, polyvinyl acetate, polyvinyl alcohol, polyglycerin, polyvinylpyrrolidone, copolymer of isoprene sulfonic acid and acrylic acid, polyvinylpyrrolidone polyacrylic acid copolymer, polyvinylpyrrolidone vinyl acetate copolymer, salt of naphthalene sulfonic acid formalin condensate, diallylamine hydrochloride sulfur dioxide copolymer, carboxymethylcellulose, salt of carboxymethylcellulose, hydroxyethylcellulose, hydroxypropylcellulose, pullulan, chitosan, and chitosan salts.

[0072] [Preservatives and anti-fungal agents] Examples of the preservatives and antifungal agents used in the present invention include isothiazoline preservatives such as 2-methyl-4-isothiazolin-3-one and 5-chloro-2-methyl-4-isothiazolin-3-one, paraoxybenzoic acid esters, phenoxyethanol, etc. These preservatives and antifungal agents may be used alone or in combination of two or more kinds.

[0073] [Oxidizing agent] The polishing composition of the present invention preferably contains an oxidizing agent. The oxidizing agent has the effect of oxidizing the surface of the object to be polished, and can further increase the polishing rate of the object to be polished by the polishing composition.

[0074] Examples of oxidizing agents include hydrogen peroxide, sodium peroxide, barium peroxide, ozone water, silver (II) salts, iron (III) salts, permanganic acid, chromic acid, dichromate, peroxodisulfuric acid, peroxolinic acid, peroxosulfuric acid, peroxoboric acid, performic acid, peracetic acid, perbenzoic acid, perphthalic acid, hypochlorous acid, hypobromous acid, hypoiodous acid, chloric acid, chlorous acid, perchloric acid, bromic acid, iodic acid, periodic acid, persulfuric acid, dichloroisocyanuric acid, and salts thereof. These oxidizing agents can be used alone or in combination of two or more. Among these, hydrogen peroxide, ammonium persulfate, periodic acid, hypochlorous acid, and sodium dichloroisocyanurate are preferred, and hydrogen peroxide is more preferred.

[0075] The lower limit of the content of the oxidizing agent in the polishing composition is preferably 0.001% by mass or more, and more preferably 0.01% by mass or more. By setting the lower limit in this way, the polishing rate can be further improved. In addition, the upper limit of the content of the oxidizing agent in the polishing composition is preferably 30% by mass or less, and more preferably 10% by mass or less. By setting the upper limit in this way, the material cost of the polishing composition can be reduced, and the burden of treating the polishing composition after use for polishing, that is, the waste liquid treatment, can be reduced. In addition, the risk of excessive oxidation of the surface of the object to be polished by the oxidizing agent can be reduced.

[0076] [Use form of polishing composition] The polishing composition of the present invention is typically supplied to an object to be polished in the form of a polishing liquid containing the polishing composition, and is used to polish the object to be polished. The polishing composition of the present invention may be used as a polishing liquid by diluting (typically diluting with water), or may be used as a polishing liquid as it is. That is, the concept of the polishing composition in the technology according to the present invention includes both a polishing composition (working slurry) that is supplied to an object to be polished and used to polish the object to be polished, and a concentrated liquid (original liquid of working slurry) that is diluted and used for polishing. The concentration ratio of the concentrated liquid can be, for example, about 2 to 100 times on a volume basis, and is usually about 5 to 50 times.

[0077] <Method of manufacturing the polishing composition> The method for producing the polishing composition of the present invention is not particularly limited, and can be obtained, for example, by stirring and mixing colloidal silica, a quaternary ammonium compound, and other additives such as a pH adjuster, etc., in a dispersion medium. The details of each component are as described above. Therefore, the present invention provides a method for producing a polishing composition, which includes a step of mixing colloidal silica and a quaternary ammonium compound represented by the above formula (1), has a pH of less than 4.0, and has a zeta potential of -60 mV or more and -35 mV or less.

[0078] The temperature at which the components are mixed is not particularly limited, but is preferably 10° C. to 40° C. Heating may be performed to increase the dissolution rate. The mixing time is also not particularly limited as long as the components can be mixed uniformly.

[0079] <Polishing method and semiconductor substrate manufacturing method> The present invention provides a polishing method comprising a step of polishing an object to be polished with the polishing composition of the present invention or the polishing composition produced by the production method of the present invention. The present invention also provides a method for producing a semiconductor substrate, comprising the polishing method.

[0080] As a polishing device, a general polishing device can be used which is equipped with a holder for holding a substrate or the like having an object to be polished, a motor whose rotation speed can be changed, and a polishing platen onto which a polishing pad (polishing cloth) can be attached.

[0081] The polishing pad may be made of any material, including general nonwoven fabric, polyurethane, porous fluororesin, etc. It is preferable that the polishing pad has grooves formed thereon to allow the polishing liquid to accumulate.

[0082] Regarding the polishing conditions, for example, the rotation speed of the polishing platen was 10 rpm (0.17 s -1 ) or more 500rpm (8.3s -1 ) is preferred. The pressure (polishing pressure) applied to the substrate having the object to be polished is preferably 0.5 psi (3.4 kPa) or more and 10 psi (68.9 kPa) or less. The method of supplying the polishing composition to the polishing pad is not particularly limited, and for example, a method of continuously supplying the composition using a pump or the like is adopted. There is no limit to the amount of supply, but it is preferred that the surface of the polishing pad is always covered with the polishing composition of the present invention.

[0083] After polishing, the substrate is washed with running water, and water droplets adhering to the substrate are removed by a spin dryer or the like, followed by drying to obtain a substrate having a metal-containing layer.

[0084] The polishing composition of the present invention may be of a one-component type or a multi-component type such as a two-component type. EXAMPLES

[0085] The present invention will be described in more detail with reference to the following examples and comparative examples. However, the technical scope of the present invention is not limited to the following examples. Unless otherwise specified, "%" and "parts" mean "mass %" and "parts by mass", respectively. Furthermore, in the following examples, unless otherwise specified, the operations were carried out under the conditions of room temperature (20-25°C) / relative humidity 40-50%RH. The zeta potential of the sulfonic acid-modified colloidal silica or unmodified colloidal silica contained in the polishing composition was measured by the following method.

[0086] <Zeta potential measurement> Each polishing composition prepared below was subjected to measurement by the laser Doppler method (electrophoretic light scattering measurement method) using an ELS-Z2 manufactured by Otsuka Electronics Co., Ltd. and a flow cell at a measurement temperature of 25° C. The obtained data was analyzed by the Smoluchowski equation to calculate the zeta potential of the sulfonic acid-modified colloidal silica or unmodified colloidal silica in the polishing composition.

[0087] [Preparation of polishing composition] (Preparation of surface-modified colloidal silica) As colloidal silica, sulfonic acid-modified colloidal silica with an average primary particle size of 12 nm, an average secondary particle size of 24 nm, and an average degree of association of 2 was prepared. The sample was prepared according to the method described in (2003), 246-247.

[0088] In addition, a sulfonic acid-modified colloidal silica having an average primary particle size of 35 nm, an average secondary particle size of 70 nm, and an average degree of association of 2 was prepared in a similar manner.

[0089] Example 1 The sulfonic acid modified colloidal silica obtained above (average primary particle size: 12 nm, average secondary particle size: 24 nm, average degree of association: 2) was added as an abrasive grain to 4 mass%, and dodecyltrimethylammonium chloride as a quaternary ammonium compound was added to ion-exchanged water as a dispersion medium to a final concentration of 0.05 mass%, to obtain a mixed liquid at room temperature (25°C).

[0090] Thereafter, maleic acid was added as a pH adjuster to the mixture so that the pH was 2.3, and the mixture was stirred and mixed at room temperature (25°C) for 30 minutes to prepare a polishing composition. The pH of the polishing composition (liquid temperature: 25°C) was confirmed with a pH meter (manufactured by Horiba, Ltd., model number: LAQUA). The zeta potential of the sulfonic acid-modified colloidal silica in the obtained polishing composition was measured by the above method and was found to be -45mV.

[0091] (Examples 2, 4, 6 and Comparative Examples 1 and 3) Polishing compositions according to Examples 2, 4, and 6 and Comparative Examples 1 and 3 were prepared in the same manner as in Example 1, except that the type of abrasive grains and the type of quaternary ammonium compound were changed as shown in Table 1. In Table 1 below, "-" indicates that the agent was not contained. The pH of the obtained polishing compositions and the zeta potential of the sulfonic acid-modified colloidal silica or unmodified colloidal silica are shown in Table 1 below.

[0092] (Example 3, Comparative Example 2) Polishing compositions according to Example 3 and Comparative Example 2 were prepared in the same manner as in Example 1, except that the type and content of the pH adjuster were changed to obtain the pH shown in Table 1. In Example 3, maleic acid was added as a pH adjuster so that the polishing composition had a pH of 3.8, and in Comparative Example 2, maleic acid was added as a pH adjuster so that the polishing composition had a pH of 6.0. The pH of the obtained polishing compositions and the zeta potential of the sulfonic acid-modified colloidal silica in the polishing compositions are shown in Table 1 below.

[0093] Example 5 A polishing composition was prepared in the same manner as in Example 1, except that hydrogen peroxide was added as an oxidizing agent to a final concentration of 1 mass % in addition to the sulfonic acid-modified colloidal silica and the quaternary ammonium compound. The pH of the resulting polishing composition and the zeta potential of the sulfonic acid-modified colloidal silica in the polishing composition are shown in Table 1 below.

[0094] [Evaluation of average secondary particle size] The average secondary particle size of the colloidal silica in the polishing composition was measured by a light scattering method using laser light, and a dynamic light scattering particle size distribution analyzer UPA-UT151 manufactured by Nikkiso Co., Ltd. was used as the measuring instrument.

[0095] [Evaluation of polishing speed] As the objects to be polished, a silicon wafer (300 mm, blanket wafer) with a 450 Å thick SiOC film formed on the surface by FCVD (Flowable CVD) method and a silicon wafer with a 5000 Å thick SiOC film formed on the surface by SOG (Spin on glass) method were prepared. Each silicon wafer was cut into 30 mm x 30 mm chip coupons as test pieces, and the substrates were polished under the following polishing conditions using each of the polishing compositions obtained above.

[0096] (polishing conditions) The polishing machine used was EJ-380IN-CH (manufactured by Engis Japan Co., Ltd.), and the polishing pad used was a hard polyurethane pad IC1010 (manufactured by Rohm and Haas Co., Ltd.) Polishing was performed for 60 seconds under the conditions of a polishing pressure of 3.8 psi (21.0 kPa), a platen rotation speed of 60 rpm, a carrier rotation speed of 60 rpm, and a supply rate of the polishing composition of 100 ml / min.

[0097] (polishing speed) The removal rate (RR) was calculated according to the following formula.

[0098]

number

[0099] The film thickness was measured using an optical interference film thickness measuring device (manufactured by Dainippon Screen Mfg. Co., Ltd., model number: Lambda Ace VM-2030), and the polishing rate was evaluated by dividing the difference in film thickness before and after polishing by the polishing time.

[0100] The evaluation results of the removal rate are shown in Table 1 below.

[0101] [Table 1]

[0102] As shown in Table 1, when the polishing compositions of Examples 1 to 7 were used, the polishing rate exceeded 20 nm / min, and it was found that, compared with the polishing compositions of Comparative Examples 1 to 3, SiOC could be polished at a higher polishing rate.

[0103] A comparison between Example 1 and Comparative Example 2 shows that unless the pH is less than 4.0, the polishing rate clearly decreases in the presence of a quaternary ammonium compound having a hydrophobic first group, even if the zeta potential of colloidal silica is within a predetermined range. Also, a comparison between Example 1 and Comparative Example 3 shows that when the quaternary ammonium compound contained in the polishing composition does not have a hydrophobic first group, the polishing rate significantly decreases.

[0104] This shows that at a pH of less than 4.0, in the presence of a quaternary ammonium compound having a hydrophobic first group, the polishing rate for SiOC is improved when the zeta potential of colloidal silica is within a predetermined range.

[0105] Moreover, it was found that when the polishing composition of Example 5 containing hydrogen peroxide as an oxidizing agent was used, the removal rate of SiOC was further improved.

Claims

1. Colloidal silica and a compound represented by the following formula (1): 【Chemistry 1】 Where: R 1 ~R 4 wherein one or two of the groups are each independently a first group which is an alkyl group having from 8 to 13 carbon atoms, an alkenyl group having from 8 to 13 carbon atoms, or an aryl group having from 6 to 13 carbon atoms; R 1 ~R 4 the remaining three or two groups other than the first group are each independently a second group which is an alkyl group having 1 or 2 carbon atoms or an alkenyl group having 2 carbon atoms, A - is a monovalent anion, and a quaternary ammonium compound represented by the formula: The pH is less than 4.0, The polishing composition, wherein the colloidal silica has a zeta potential of -55 mV or more and -38 mV or less.

2. 2. The polishing composition according to claim 1, wherein in the formula (1), the first group is an alkyl group having 8 to 13 carbon atoms or an aryl group having 6 to 13 carbon atoms.

3. A polishing composition as described in claim 1 or 2, wherein the content of the quaternary ammonium compound is 0.005 mass % or more and 0.5 mass % or less relative to the polishing composition.

4. 4. The polishing composition according to claim 1, wherein the colloidal silica has an organic acid fixed to the surface thereof.

5. The polishing composition according to any one of claims 1 to 4, further comprising an oxidizing agent.

6. 6. The polishing composition according to claim 1, wherein the quaternary ammonium compound is at least one selected from the group consisting of dodecyltrimethylammonium chloride and phenyltrimethylammonium chloride.

7. A polishing composition described in any one of claims 1 to 6, further containing an organic acid.

8. The polishing composition according to any one of claims 1 to 7, which is used for polishing an object containing SiOC.

9. Colloidal silica and a compound represented by the following formula (1): 【Chemistry 2】 Where: R 1 ~R 4 wherein one or two of the groups are each independently a first group which is an alkyl group having from 8 to 13 carbon atoms, an alkenyl group having from 8 to 13 carbon atoms, or an aryl group having from 6 to 13 carbon atoms; R 1 ~R 4 the remaining three or two groups other than the first group are each independently a second group which is an alkyl group having 1 or 2 carbon atoms or an alkenyl group having 2 carbon atoms, A - is a monovalent anion, and a quaternary ammonium compound represented by the formula: The pH is less than 4.0, The method for producing a polishing composition, wherein the colloidal silica has a zeta potential of -55 mV or more and -38 mV or less.

10. 10. A polishing method comprising a step of polishing an object to be polished with the polishing composition according to any one of claims 1 to 8 or the polishing composition produced by the production method according to claim 9.

11. A method for manufacturing a semiconductor substrate, comprising the polishing method according to claim 10.

Citation Information

Patent Citations

  • Polishing composition and polishing method

    JP2008091569A

  • Polishing solution for CMP and polishing method

    JP2009278061A

  • CMP polishing liquid and polishing method using this polishing liquid

    JP2013120885A

  • Polishing composition

    JP2013138053A

  • Polishing composition, polishing method, and manufacturing method of substrate

    JP2019116627A