Fuel Cells
The fuel cell design with a thinner gas diffusion layer using conductive fibers and particles addresses the issue of reduced reactant gas supply, improving gas diffusion and power generation performance, especially in high current density regions.
Patent Information
- Application Number
- JP2020113059
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-06-30
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2040-06-30
AI Technical Summary
In existing fuel cells, the thick gas diffusion layer relative to the rib width of the separator results in decreased reactant gas supply, increased diffusion overvoltage, and reduced power generation performance, especially in high current density regions.
A fuel cell design with a gas diffusion layer composed of conductive particles, fibers, and polymer resin, where the average fiber length is less than half the rib width and the average fiber diameter is less than one-hundredth of the layer thickness, enhancing gas diffusion properties and reducing layer thickness to improve power generation performance.
The improved gas diffusion layer design ensures sufficient gas permeability and enhances power generation performance, particularly in high current density regions, by minimizing anisotropy in gas diffusivity and reducing contact resistance.
Smart Images

Figure 0007591757000003 
Figure 0007591757000004 
Figure 0007591757000005
Abstract
Description
[Technical field]
[0001] The present disclosure relates to fuel cells, and in particular to solid polymer electrolyte fuel cells. [Background technology]
[0002] A solid polymer fuel cell, one example of a fuel cell, exposes one side of a proton-conducting polymer electrolyte membrane to a fuel gas such as hydrogen and the other side to oxygen, synthesizing water through a chemical reaction via the electrolyte membrane, and extracting the reaction energy generated electrically.
[0003] A single cell of a polymer electrolyte fuel cell has a membrane electrode assembly (hereinafter referred to as MEA) and a pair of conductive separators arranged on both sides of the MEA. The MEA has a proton-conductive polymer electrolyte membrane and a pair of electrode layers that sandwich the electrolyte membrane. The pair of electrode layers are formed on both sides of the polymer electrolyte membrane and have a catalyst layer mainly composed of carbon powder carrying a platinum group catalyst, and a gas diffusion layer formed on the catalyst layer and having a current collecting function, gas permeability, and water repellency.
[0004] The separator has ribs and grooves on the surface in contact with the gas diffusion layer for forming gas flow paths through which reactant gases used for power generation flow.
[0005] The gas diffusion layer in the MEA supplies the reactant gas from the gas flow path in the separator to the catalyst layer. The gas diffusion layer also functions as a conductive path for electrons between the catalyst layer and the separator. For this reason, conductive porous materials are used for the gas diffusion layer in the MEA.
[0006] For example, Patent Document 1 discloses a fuel cell that uses a separator with ribs and grooves to form a gas flow path through which a reactant gas flows, and that aims to increase the amount of reactant gas supplied to the area of the gas diffusion layer facing the contact between the rib and the gas diffusion layer and to reduce the contact resistance between the rib and the gas diffusion layer. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2010-218817 A Summary of the Invention [Problem to be solved by the invention]
[0008] However, in the fuel cell described in Patent Document 1, the thickness h of the gas diffusion layer is large (h≧0.7Rw) relative to the rib width Rw of the separator (2x in Patent Document 1), so the amount of reactant gas reaching the catalyst decreases, and the diffusion overvoltage increases, particularly in the high current density region, resulting in reduced power generation performance.
[0009] The present disclosure aims to provide a fuel cell with improved power generation performance by improving gas diffusivity, particularly in the high current density region, by reducing the thickness of the gas diffusion layer relative to the rib width of the separator. [Means for solving the problem]
[0010] In order to achieve the above object, the present inventors conducted extensive research and found that, in a gas diffusion layer made of conductive particles, conductive fibers, and a polymer resin, the gas diffusion properties in the thickness direction and the surface direction of the gas diffusion layer can be made uniform by using a gas diffusion layer in which the average fiber length of the conductive fibers is shorter than 1 / 2 the rib width of the separator and the average fiber diameter of the conductive fibers is 1 / 100 or less of the thickness of the gas diffusion layer. Based on this finding, the inventors found that even if the thickness of the gas diffusion layer is formed thin relative to the rib width, gas diffusion under the rib is not easily hindered, and power generation performance is significantly improved, especially in the high current density region.
[0011] A fuel cell according to an embodiment of the present disclosure is a fuel cell in which a membrane electrode assembly (MEA) formed by laminating a catalyst layer and a gas diffusion layer on both sides of a polymer electrolyte membrane is sandwiched between separators, the separator having ribs and grooves on a surface in contact with the gas diffusion layer for forming a gas flow path through which a reactant gas to be used for power generation flows, the gas diffusion layer has a thickness h and a width Rw of the rib in contact with the gas diffusion layer, and the gas diffusion layer contains conductive particles, conductive fibers, and a polymer resin, and the conductive fibers have an average fiber length Fl and an average fiber diameter Fd of Fl and / or Rw. <Rw / 2、Fd<h / 100である。 Effect of the Invention
[0012] According to the present disclosure, it is possible to provide a fuel cell in which the gas diffusion layer has sufficient gas permeability, and in particular, the power generation performance in the membrane electrode assembly (MEA) is improved in the high current density range. [Brief description of the drawings]
[0013] [Figure 1] FIG. 1 is a schematic diagram showing a cell stack of a polymer electrolyte fuel cell according to a first embodiment of the present disclosure. [Diagram 2] FIG. 1 is a schematic cross-sectional view showing a part of a battery cell of a polymer electrolyte fuel cell according to a first embodiment of the present disclosure; [Figure 3A] FIG. 1 is a schematic cross-sectional view showing a gas diffusion layer according to a first embodiment of the present disclosure. [Figure 3B] FIG. 2 is an enlarged cross-sectional view showing a schematic enlargement of a part of the gas diffusion layer according to the first embodiment of the present disclosure. [Figure 4] FIG. 1 is a schematic cross-sectional view showing a part of a battery cell of a polymer electrolyte fuel cell according to a first embodiment of the present disclosure. [Figure 5A] FIG. 11 is a schematic cross-sectional view showing a part of a battery cell of a polymer electrolyte fuel cell according to a second embodiment of the present disclosure. [Figure 5B] A cross-sectional SEM photograph of an enlarged portion of a battery cell according to the second embodiment of the present disclosure. [Figure 6]An enlarged cross-sectional SEM image of a part of a battery cell using a conventional gas diffusion layer [Figure 7] Graph showing the results of evaluation tests of Examples 1 to 3 and Comparative Examples 1 to 2 with respect to cell voltage and gas diffusion layer thickness (h) / rib width (RW). [Figure 8] Graph showing the results of evaluation tests of Examples 4 to 7 and Comparative Examples 3 to 5 with respect to cell voltage and gas diffusion layer thickness (h) / rib width (RW). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] A polymer electrolyte fuel cell will be described below as a specific embodiment of the fuel cell of the present disclosure with reference to the accompanying drawings. Note that the fuel cell of the present disclosure is not limited to the fuel cell configuration described in the following embodiment, but includes a fuel cell configuration based on a technology equivalent to the technical concept having the technical features described in the following embodiment.
[0015] In addition, the numerical values, shapes, configurations, manufacturing processes, and the order of manufacturing processes shown in the following embodiments are merely examples, and the invention is not limited to the contents of this disclosure. Among the components in the following embodiments, components that are not described in an independent claim showing the highest concept are described as optional components. Note that in each embodiment, the same elements are given the same reference numerals, and descriptions may be omitted. In addition, the drawings mainly show each component in a schematic manner to facilitate understanding.
[0016] First, various aspects of the fuel cell of the present disclosure will be illustrated. The fuel cell according to the first aspect of the present disclosure comprises: A fuel cell in which a membrane-electrode assembly, which is formed by laminating a catalyst layer and a gas diffusion layer on either side of a polymer electrolyte membrane, is sandwiched between separators, the separator has ribs and grooves on a surface in contact with the gas diffusion layer to define a gas flow path through which a reactant gas for power generation flows, The thickness of the gas diffusion layer is h, When the width of the portion of the rib in contact with the gas diffusion layer is defined as Rw, 0.29Rw ≦ h ≦ 0.55Rw and, the gas diffusion layer contains conductive particles, conductive fibers, and a polymer resin, the average fiber length Fl and average fiber diameter Fd of the conductive fibers are Fl < Rw / 2, and Fd < h / 100 A fuel cell.
[0017] The fuel cell according to the second aspect of the present disclosure is a fuel cell in which a membrane - electrode assembly (MEA) formed by laminating a catalyst layer and a gas diffusion layer on both sides of a polymer electrolyte membrane is sandwiched by separators, the separator has ribs and grooves for forming gas flow paths through which reaction gases for power generation flow on the surface on the side in contact with the gas diffusion layer, the thickness of the gas diffusion layer is defined as h, when the width of the portion of the rib in contact with the gas diffusion layer is defined as Rw, 0.29Rw ≦ h ≦ 0.48Rw and, the gas diffusion layer contains conductive particles, conductive fibers, and a polymer resin, the average fiber length Fl and average fiber diameter Fd of the conductive fibers are Fl < Rw / 2, and Fd < h / 100, A fuel cell.
[0018] The fuel cell according to the third aspect of the present disclosure is, in the first aspect or the second aspect described above, the average fiber length Fl and average fiber diameter Fd of the conductive fibers are 0.5μm ≦ Fl ≦ 50μm, and 0.05μm ≦ Fd ≦ 0.3μm It is more preferable that this is the case.
[0019] A fourth aspect of the fuel cell according to the present disclosure is the third aspect, further preferably configured such that the amount of the conductive fibers in the gas diffusion layer is greater than the amount of the conductive particles.
[0020] In a fuel cell of a fifth aspect according to the present disclosure, it is more preferable that in the gas diffusion layer of the fourth aspect, a step is provided at the boundary between the rib and the groove, and the surface in contact with the flat top portion of the rib and the surface facing the groove are formed as discontinuous uneven surfaces.
[0021] In a sixth aspect of the fuel cell according to the present disclosure, in the fifth aspect, it is more preferable that the height of the step in the gas diffusion layer at the boundary between the rib and the groove is 5 to 30 μm.
[0022] A fuel cell according to a seventh aspect of the present disclosure is the sixth aspect, wherein the gas diffusion layer has a surface roughness Sa of less than 3 μm on the side that comes into contact with the separator.
[0023] A fuel cell according to an eighth aspect of the present disclosure is any one of the first to seventh aspects, wherein the rib width Rw and the groove width Gw of the separator are: 0.7Gw≦Rw≦1.3Gw It is more preferable that:
[0024] A fuel cell according to a ninth aspect of the present disclosure is any one of the first to eighth aspects, wherein the gas diffusion layer and the separator are more preferably configured on the cathode side.
[0025] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings.
[0026] (Embodiment 1) The basic configuration of a polymer electrolyte fuel cell (hereinafter simply referred to as a fuel cell) 100 according to a first embodiment of the present disclosure will be described with reference to Fig. 1. Fig. 1 is a schematic diagram showing the basic configuration (also referred to as a fuel cell stack) of the fuel cell 100 according to the first embodiment. Note that the first embodiment is not limited to polymer electrolyte fuel cells and can be applied to various fuel cells.
[0027] <Fuel cell stack structure> As shown in FIG. 1, the fuel cell stack of a fuel cell 100 is formed by stacking one or more battery cells 10, which are basic units, with current collector plates 11, insulating plates 12, and end plates 13 arranged on both sides of the stacked battery cells 10, which are then compressed from both sides with a predetermined load and fastened together.
[0028] The current collecting plate 11 is made of a gas-impermeable conductive material. For example, copper, brass, etc. are used for the current collecting plate 11. A current extracting terminal portion (not shown) is provided on the current collecting plate 11, and a current is extracted from the current extracting terminal portion during power generation.
[0029] The insulating plate 12 is made of an insulating material such as resin, etc. For example, fluorine-based resin, PPS resin, etc. are used for the insulating plate 12.
[0030] The end plates 13 on both ends fasten and hold one or more stacked battery cells 10, current collector plates 11, and insulating plates 12 at a predetermined load using a pressure means (not shown). The end plates 13 are made of a highly rigid metal material such as steel.
[0031] 2 is a schematic cross-sectional view showing a cross section of a battery cell 10. In the battery cell 10, a membrane electrode assembly (hereinafter also referred to as MEA) 20 is sandwiched between an anode side separator 4a and a cathode side separator 4b. Hereinafter, the anode side separator 4a and the cathode side separator 4b will be collectively referred to as separator 4. The same description will be used for other components when multiple components are described together.
[0032] In the separator 4, a gas flow path through which the reactant gas flows is formed on the surface in contact with the gas diffusion layer 3. Grooves 5 and ribs 6 for forming this gas flow path are formed in the separator 4. The space of the grooves 5 between the ribs 6 formed in the anode side separator 4a becomes the gas flow path through which the reactant gas for the fuel gas flows. The grooves 5 between the ribs 6 formed in the cathode side separator 4b become the gas flow path through which the reactant gas for the oxidant gas flows. The separator 4 can be made of a carbon-based or metal-based material.
[0033] <mea> The MEA 20 has a polymer electrolyte membrane 1, a catalyst layer 2, and a gas diffusion layer 3. An anode catalyst layer 2a and a cathode catalyst layer 2b (the anode-side and cathode-side catalyst layers 2a, 2b are collectively referred to as catalyst layer 2) are formed on both sides of the polymer electrolyte membrane 1, which selectively transports protons, and an anode-side gas diffusion layer 3a and a cathode-side gas diffusion layer 3b (the both-side gas diffusion layers 3a, 3b are collectively referred to as gas diffusion layer 3) are disposed on the outside thereof, respectively. The gas diffusion layer 3 is in contact with the protruding end of a rib 6 of a separator 4.
[0034] As the polymer electrolyte membrane 1, for example, a perfluorocarbon sulfonic acid polymer is used, but there is no particular limitation as long as it has proton conductivity.
[0035] As the catalyst layer 2, a layer containing a carbon material carrying catalyst particles such as platinum and a polymer electrolyte can be used.
[0036] <Gas diffusion layer> Next, the configuration of the gas diffusion layer 3 (gas diffusion layer without a substrate) in the fuel cell 100 according to the first embodiment of the present disclosure will be described in detail with reference to Figures 3A and 3B. Figure 3A is a schematic cross-sectional view showing an enlarged cross section of the gas diffusion layer 3. Figure 3B is a schematic cross-sectional view showing a further enlarged view of a portion of the gas diffusion layer 3 shown in Figure 3A. As shown in Figure 3A, the gas diffusion layer 3 in the first embodiment is composed of conductive particles 31, conductive fibers 32, and polymer resin 33, and is a free-standing membrane having a self-supporting structure.
[0037] The conductive particles 31 are particles with excellent electrical conductivity, and contribute to improving the conductivity of the gas diffusion layer 3. As a material for the conductive particles 31, for example, carbon particles are used.
[0038] The conductive fibers 32 contribute to improving the electrical conductivity and mechanical strength of the gas diffusion layer 3. The material of the conductive fibers 32 is not particularly limited, but for example, carbon fibers such as carbon nanotubes can be used.
[0039] The inventor of the present invention conducted various experiments on the gas diffusion layer 3 in the fuel cell 100 and found that favorable results can be obtained when the following relationship holds for the average fiber length Fl and the average fiber diameter Fd of the conductive fibers 32.
[0040] The average fiber length Fl and the average fiber diameter Fd of the conductive fibers 32 are preferably such that Fl < Rw / 2 and Fd < h / 100, where Rw is the rib width of the separator 4. When the average fiber length Fl and the average fiber diameter Fd satisfy Fl < Rw / 2 and Fd < h / 100, the gas diffusibility in the thickness direction (the left - right direction in FIG. 2) and the surface direction (the up - down direction in FIG. 2) of the gas diffusion layer 3 is likely to be uniform. On the other hand, when the average fiber length Fl and the average fiber diameter Fd of the conductive fibers 32 in the gas diffusion layer 3 satisfy Fl ≥ R / 2 or Fd ≥ h / 100, anisotropy occurs in the gas diffusibility in the thickness direction and the surface direction of the gas diffusion layer 3. In particular, when Fd ≥ h / 100, as the thickness of the gas diffusion layer 3 is reduced, the area of the conductive fibers 32 in the cross - sectional area in the surface direction increases, and the gas diffusibility in the surface direction decreases. As a result, the gas diffusion in the gas diffusion film 3 under the rib decreases, and the cell voltage decreases.
[0041] The average fiber length Fl of the conductive fibers 32 is preferably 0.5 μm or more and 50 μm or less. When the average fiber length Fl of the conductive fibers 33 is 0.5 μm or more, it effectively contributes to improving the conductivity of the gas diffusion layer 3 and can further enhance the mechanical strength of the gas diffusion layer 3. Also, when the average fiber length Fl of the conductive fibers 32 is 50 μm or less, the anisotropy in the gas diffusibility in the thickness direction and the surface direction of the gas diffusion layer 3 can be minimized.
[0042] The average fiber diameter Fd of the conductive fibers 32 is preferably 50 nm or more and 300 nm or less. When the average fiber diameter Fd of the conductive fibers 32 is 50 nm or more, the electrical conductivity of the gas diffusion layer 3 is effectively improved, and the mechanical strength of the gas diffusion layer 3 can be further increased, so that the gas diffusion layer 3 can have sufficient strength as a self-supporting membrane. When the average fiber diameter Fd of the conductive fibers 32 is 300 nm or less, the diameter does not become too large, so that when the thickness of the gas diffusion layer 3 is reduced, the area ratio of the conductive fibers 32 to the cross-sectional area in the surface direction can be reduced, and sufficient gas diffusivity in the surface direction can be ensured.
[0043] Examples of materials for the polymer resin 33 include PTFE (polytetrafluoroethylene), FEP (tetrafluoroethylene-hexafluoropropylene copolymer), PVDF (polyvinylidene fluoride), ETFE (tetrafluoroethylene-ethylene copolymer), PCTFE (polychlorotrifluoroethylene), and PFA (polyfluoroethylene-perfluoroalkylvinylether copolymer). In particular, from the viewpoints of heat resistance, water repellency, and chemical resistance, it is preferable that the polymer resin 33 contains PTFE. Examples of the raw material form of PTFE include dispersion and powder, but it is preferable to use a dispersion from the viewpoint of excellent dispersibility.
[0044] The polymer resin 33 functions as a binder that bonds the conductive particles 31 together. The polymer resin 33 also has water repellency, which prevents water from remaining in the pores inside the gas diffusion layer 3 and impeding gas permeation.
[0045] The amount (wt%) of the conductive fibers 32 in the gas diffusion layer 3 is preferably greater than the amount (wt%) of the conductive particles 31. The reason for this will be described below. The gas diffusion layer 3 has the role of diffusing gas and retaining water generated by the reaction while discharging excess water to the outside through the pores of the gas diffusion layer 3. The excess water passes through the pores inside the gas diffusion layer 3 as water vapor, but if the pore diameter is on the order of several tens of nm, water vapor cannot permeate sufficiently. Therefore, the excess water inside the membrane electrode assembly (MEA) 20 is not discharged, gas diffusion to the catalyst layer 2 is hindered, and the cell performance is reduced. On the other hand, if the pores are on the order of microns, water vapor permeates too much, causing the inside of the MEA 20 to become dry, reducing the proton conductivity and reducing the cell performance. Therefore, the pore diameter inside the gas diffusion layer 3 is suitable for pores on the order of 0.1 μm. Pores on the order of 0.1 μm are likely to be formed by gaps between the conductive fibers 32, and pores on the order of several tens of nm are likely to be formed by gaps between the primary particles of the conductive particles. For this reason, by making the amount (wt%) of the conductive fibers 32 greater than the amount (wt%) of the conductive particles 31, the pores in the gas diffusion layer 3 are on the order of 0.1 μm, improving the battery performance. Furthermore, in the gas diffusion layer 3, the conductive particles 31 are present in the gaps between the conductive fibers 32, and the conductive fibers 32 and the conductive particles 31 can be satisfactorily bound by the fibrous polymer resin 33, so that the gas diffusion layer 3 can have sufficient strength.
[0046] <Battery cell> Next, the configuration of the battery cell 10 in the fuel cell 100 according to the first embodiment of the present disclosure will be described in detail with reference to FIG. 4. FIG. 4 is a schematic cross-sectional view showing the configuration of the polymer electrolyte membrane 1, catalyst layer 2, gas diffusion layer 3, and separator 4 on the cathode side of the battery cell 10. In FIG. 4, the contact portion between the separator 4 (4b) and the gas diffusion layer 3 (3b) is enlarged. In the gas diffusion layer 3 shown in FIG. 4, only the conductive fiber 32 is shown, and the conductive particle 31 and polymer resin 33 shown in FIG. 3 are omitted. Although FIG. 4 shows the configuration of the cathode side of the battery cell 10, the configuration of the anode side may be the same.
[0047] As described above, the separator 4 is provided with grooves 5 and ribs 6 for forming gas flow paths through which the reaction gas flows on the surface on the side in contact with the gas diffusion layer 3. Let the width of the rib 6 be Rw, the width of the groove 5 be Gw, and the thickness of the gas diffusion layer be h. The condition (1) 0.29Rw ≤ h ≤ 0.55Rw is satisfied, and more preferably, the condition (1') 0.29Rw ≤ h ≤ 0.48Rw is satisfied. Further, the average fiber length Fl of the conductive fibers 32 of the gas diffusion layer 3 satisfies the condition (2) Fl < Rw / 2, and the average fiber diameter Fd of the conductive fibers satisfies the condition (3) Fd < h / 100. Here, the width Rw of the rib 6 and the width Gw of the groove 5 are the width of the rib 6 and the width of the groove 5 in the cross section orthogonal to the main flow direction of the reaction gas. Also, the thickness h of the gas diffusion layer 3 was measured using a digital indicator manufactured by Mitutoyo Corporation, and the thickness of the gas diffusion layer alone was measured.
[0048] In addition, in the configuration of Embodiment 1, the relationship between the rib width Rw and the groove width Gw of the separator 4 is preferably 0.7Gw ≤ Rw ≤ 1.3Gw. When the relationship between the rib width Rw and the groove width Gw of the separator 4 is 0.7Gw > Rw, the contact area between the rib 6 and the gas diffusion layer 3 decreases, so the electronic resistance increases and the cell voltage decreases. On the other hand, when Rw > 1.3Gw, the reaction gas in the region of the catalyst layer 2 facing the rib 6 decreases, and the cell voltage decreases. Further, since the cross-sectional area orthogonal to the main flow direction of the reaction gas in the groove 5 decreases, the pressure loss of the reaction gas increases, and particularly on the cathode side, the load on the auxiliary devices increases.
[0049] By satisfying all of the above conditions (1) to (3), it becomes possible to reduce the thickness h of the gas diffusion layer 3 with respect to the rib width Rw of the separator 4. In particular, in the high current density region, the diffusibility of the gas is also dramatically improved, and the improvement of the battery performance can be realized. The reasons are considered as follows.
[0050] The amount of reaction gas that reaches the catalyst layer 2 is reduced in the region of the catalyst layer 2 facing the rib 6 than in the region of the catalyst layer 2 facing the groove 5 because the path for the gas to diffuse is longer. Furthermore, the conventional gas diffusion layer 30 (gas diffusion layer with substrate: see FIG. 6) is a carbon fiber substrate on which a microporous layer (MPL) is formed, and the carbon fiber substrate constituting the substrate has an average fiber length Fl of about 10 mm and an average fiber diameter Fd of about 10 μm, so that the gas diffusion in the plane direction is poorer than the gas diffusion in the thickness direction. For this reason, in the conventional battery cell, the thickness h of the gas diffusion layer is made thicker to a certain extent relative to the rib width Rw, so that the gas can easily reach the region of the catalyst layer 2 facing the rib 6.
[0051] In contrast, in the configuration of the battery cell 10 in the first embodiment of the present disclosure, the average fiber length Fl of the conductive fibers 32 constituting the gas diffusion layer 3 is short, and the average fiber diameter Fd is also extremely small compared to the thickness h of the gas diffusion layer 3, so that anisotropy in gas diffusion in the thickness direction and the surface direction is reduced. As a result, even if the thickness h of the gas diffusion layer 3 is reduced, it is possible to ensure the amount of gas permeating into the region of the catalyst layer 2 facing the rib 6. In addition, because the thickness h of the gas diffusion layer 3 is reduced, the amount of gas permeating into the region of the catalyst layer 2 facing the groove 5 is also improved.
[0052] If the above condition (1) is not satisfied and 0.29Rw>h, the amount of gas permeating into the region of the catalyst layer 2 facing the rib 6 decreases, and the cell voltage decreases. Conversely, if h≧0.55Rw, the thickness h of the gas diffusion layer 3 becomes thicker, and the amount of gas permeating into both the groove 5 and the region of the catalyst layer 2 facing the rib 6 decreases, and the cell voltage decreases.
[0053] Furthermore, if the above conditions (2) and (3) are not satisfied and Fl≧Rw / 2 and Fd≧h / 100, then as described above, anisotropy occurs in the gas diffusivity in the thickness direction and in the plane direction of the gas diffusion layer 3, the amount of gas permeating into the region of the catalyst layer 2 facing the rib 6 decreases, and the cell voltage decreases.
[0054] (Embodiment 2) Using FIGS. 5A and 5B, the configuration of the battery cell in the fuel cell according to Embodiment 2 of the present disclosure will be described in detail.
[0055] Hereinafter, in the description of the fuel cell of Embodiment 2, the differences from the aforementioned Embodiment 1 will be mainly described. In the description of Embodiment 2, elements having the same functions and configurations as those in the aforementioned Embodiment 1 are denoted by the same reference numerals, and the description thereof will be omitted. Also, the description of the content having the same operation as that in the aforementioned Embodiment 1 will be omitted.
[0056] FIG. 5A is a schematic cross-sectional view schematically showing the configuration of the cathode-side polymer electrolyte membrane 1, catalyst layer 2, gas diffusion layer 3, and separator 4 in the battery cell 10. In FIG. 5A, the contact portion between the separator 4 and the gas diffusion layer 3 is enlarged and schematically shown. In the gas diffusion layer 3 shown in FIG. 5A, only the conductive fibers 32 are shown, and the conductive particles 31 and the polymer resin 33 are omitted. In FIG. 5A, the configuration on the cathode side in the battery cell 10 is shown, but the configuration on the anode side may be the same.
[0057] As shown in FIG. 5A, with the width of the rib 6 of the separator 4 being Rw, the width of the groove 5 being Gw, and the thickness of the gas diffusion layer being h, the condition (1) 0.29Rw ≦ h ≦ 0.55Rw is satisfied, and more preferably, the condition (1') 0.29Rw ≦ h ≦ 0.48Rw is satisfied. Further, the average fiber length Fl of the conductive fibers 32 in the gas diffusion layer 3 satisfies the condition (2) Fl < Rw / 2, and the average fiber diameter Fd of the conductive fibers satisfies the condition (3) Fd < h / 100.
[0058] FIG. 5B is a cross-sectional SEM photograph showing an enlarged contact state between the rib 6 of the separator 4 and the gas diffusion layer 3 in the battery cell of Embodiment 2. As can be understood from the photograph in FIG. 5B, the protruding end portion of the rib 6 is in a contact state of being embedded in the gas diffusion layer 3, and the protruding end portion of the rib 6 is surely in contact with the gas diffusion layer 3 together with its side surface. That is, the gas diffusion layer 3 protrudes into the groove 5, and a discontinuous surface having a step S is formed at the boundary surface between the rib 6 and the groove 5 with respect to the gas diffusion layer 3.
[0059] As described above, the gas diffusion layer 3 in the second embodiment has a step S at the boundary between the groove 5 and the rib 6 in the separator 4, and the surface in contact with the flat top portion of the rib 6 of the separator 4 and the surface facing the groove 5 of the separator 4 are formed of discontinuous uneven surfaces. Therefore, the gas diffusion layer 3 protrudes inside the groove 5 from the boundary surface between the gas diffusion layer 3 and the rib 6. The protrusion amount p, which is the height of the step S of the gas diffusion layer 3 at the boundary between the groove 5 and the rib 6 of the separator 4, is 5 to 30 μm.
[0060] FIG. 6 is a cross-sectional SEM photograph showing the contact state between the rib 6 of the separator 4 and the gas diffusion layer 30 in a battery cell using a conventional gas diffusion layer 30. The conventional gas diffusion layer 30 used here has a carbon fiber base material constituting the substrate with an average fiber length Fl of about 10 mm and an average fiber diameter Fd of about 10 μm, and the carbon fiber base material has a long fiber length and uses thick carbon fibers. As is clear from the photograph in FIG. 6, in the conventional gas diffusion layer 30, there is no step at the boundary between the rib 6 and the groove 5, and only the protruding end face of the rib 6 is in planar contact with the conventional gas diffusion layer 30. This is thought to be because the carbon fiber base material constituting the substrate has a long carbon fiber with an average fiber length Fl of about 10 mm and a thick carbon fiber with an average fiber diameter Fd of about 10 μm is used in the conventional gas diffusion layer 30.
[0061] In the battery cell 10 in the second embodiment, a step S is formed at the boundary between the rib 6 and the groove 5 so that the gas diffusion layer 3 enters the inside of the groove 5, and the protruding amount p, which is the height of the step S, is 5 to 30 μm. In this manner, in the configuration of the second embodiment, the gas diffusion layer 3 has a step S at the boundary between the rib 6 and the groove 5, and the protruding end of the rib 6 is in contact with the gas diffusion layer 3 as if it were embedded therein, and the side of the protruding end of the rib 6 is also in contact with the gas diffusion layer 3. As a result, in the configuration of the battery cell in the second embodiment, the adhesion between the gas diffusion layer 3 and the rib 6 is improved, and the contact resistance can be reduced. If the protruding amount p (the height of the step S) of the gas diffusion layer 3 into the groove 5 is smaller than 5 μm, the effect of reducing the contact resistance is reduced. On the other hand, if the protruding amount p of the gas diffusion layer 3 into the groove 5 is larger than 30 μm, the cross-sectional area of the gas flow path formed by the groove 5 is reduced because the depth of the groove 5 is generally about 100 to 300 μm, and the pressure loss of the reactant gas increases.
[0062] Moreover, the surface roughness Sa of the surface of the gas diffusion layer 3 in contact with the rib 6 is preferably 3 μm or less. When the surface roughness Sa is 3 μm or less, the contact between the gas diffusion layer 3 and the rib 6 is improved, and the contact resistance can be further reduced.
[0063] In the above embodiment, the configuration of the cathode side of the battery cell has been described, but the anode side can be configured in a similar manner. In the gas diffusion layer included in the fuel cell, oxygen used as an oxidant gas is less likely to diffuse than hydrogen used as a fuel gas, so it is preferable to apply at least the cathode side configuration in the fuel cell of the present disclosure.
[0064] The fuel cell of the present disclosure is not limited to the contents described in the above embodiment, but can be embodied in various other forms. Examples and Comparative Examples
[0065] Hereinafter, specific configurations and manufacturing methods of examples and comparative examples of the fuel cell of the present disclosure that were used when the inventors conducted experiments will be described.
[0066] A: Gas diffusion layer without substrate (material) [Conductive particles] Granular Denka Black (registered trademark) (manufactured by Denka Co., Ltd.) [Conductive fiber] ·VGCF (registered trademark) (VGCF-H, manufactured by Showa Denko K.K.) [Polymer resin] Polyflon PTFE D series (manufactured by Daikin Industries, Ltd.), average particle size 0.25 μm
[0067] (Method for manufacturing a gas diffusion layer without a substrate) A gas diffusion layer without a substrate was manufactured with a ratio of 20 wt% conductive particles, 50 wt% conductive fibers, and 30 wt% polymer resin. First, the conductive particles, conductive fibers, surfactant, and dispersion solvent were mixed and kneaded using a planetary mixer. Next, polymer resin was added to the kneaded mixture and further kneaded using a planetary mixer. Next, the kneaded mixture was rolled five times using a rolling mill under rolling conditions of 0.1 ton / cm. After that, the rolled sheet was placed in an IR furnace and baked at 300°C for 0.5 hours. The baked sheet was re-rolled three times using a roll press under rolling conditions of 1 ton / cm to obtain a gas diffusion layer with the thickness listed in Table 1 below.
[0068] B: Gas diffusion layer with substrate (material) [Base material] TORAYCA (registered trademark) carbon paper (TGP-H-030 manufactured by Toray Industries, Inc.) [Conductive particles] Granular Denka Black (registered trademark) (manufactured by Denka Co., Ltd.) [Polymer resin] Polyflon PTFE D series (manufactured by Daikin Industries, Ltd.), average particle size 0.25 μm
[0069] (Method for manufacturing a gas diffusion layer with a substrate) For the MPL layer, 80 wt% conductive particles, 20 wt% polymer resin, surfactant, and dispersion solvent were mixed and ink was prepared using a planetary mixer. The ink was applied to the substrate using a spray coater to obtain a gas diffusion layer with a thickness of 165 μm.
[0070] C: Separator (material) [Carbon plate material] Carbon plate (manufactured by Tokai Carbon Co., Ltd.) G347B (Separator manufacturing) A separator having gas flow paths with the rib width and groove width shown in the table was obtained by cutting a carbon plate material.
[0071] D: Fuel cell Fuel cells of Examples 1 to 3 shown in Table 1 and Comparative Examples 1 and 2 shown in Table 2, which will be described later, were produced by the following method.
[0072] (1) Preparation of dispersion for cathode catalyst layer The dispersion for the cathode catalyst layer was prepared as follows. A particulate conductive member (carbon black) carrying catalyst particles (Pt-Co alloy) was added to an appropriate amount of water and stirred to disperse. An appropriate amount of ethanol was added to the obtained dispersion while stirring, and then 35 parts by mass of a fibrous conductive member (first fibrous conductive member) (vapor-grown carbon fiber, average diameter 150 nm, average fiber length 10 μm) and 100 parts by mass of a proton conductive resin (perfluorocarbon sulfonic acid polymer) were added to 100 parts by mass of the particulate conductive member carrying catalyst particles, and stirred to prepare a catalyst dispersion for the cathode catalyst layer.
[0073] (2) Preparation of dispersion for anode catalyst layer The dispersion liquid for the anode catalyst layer was prepared as follows. A particulate conductive member (carbon black) carrying catalyst particles (Pt) was added to an appropriate amount of water and stirred to disperse. An appropriate amount of ethanol was added to the obtained dispersion liquid while stirring, and then 35 parts by mass of a fibrous conductive member (first fibrous conductive member) (vapor-grown carbon fiber, average diameter 150 nm, average fiber length 10 μm) and 120 parts by mass of a proton conductive resin (perfluorocarbon sulfonic acid polymer) were added to 100 parts by mass of the particulate conductive member carrying catalyst particles, and stirred to prepare a catalyst dispersion liquid for the anode catalyst layer.
[0074] (Preparation of CCM) In the preparation of the CCM (Catalyst Coated Membrane), two PET sheets were prepared, and the obtained catalyst dispersion for the cathode catalyst layer was applied in a uniform thickness to the smooth surface of one PET sheet using a screen printing method, and the obtained catalyst dispersion for the anode catalyst layer was applied in a uniform thickness to the smooth surface of the other PET sheet. After that, they were dried to form two catalyst layers on both sides of the polymer electrolyte membrane. The thickness of the cathode catalyst layer was 6 μm, and the thickness of the anode catalyst layer was 4.5 μm.
[0075] (Preparation of a single cell) In the fabrication of the unit cells, the above-mentioned gas diffusion layer having the substrate was used as the anode-side gas diffusion layer in all cases.
[0076] The gas diffusion layers of Examples 1 to 7 and Comparative Examples 1 to 5 were joined to a cathode catalyst layer as a cathode side gas diffusion layer, and the anode side gas diffusion layer was joined to an anode catalyst layer, thereby obtaining an MEA.
[0077] Next, a fuel cell was manufactured using a separator with a rib width of 0.5 mm and a groove width of 0.5 mm as the anode side separator, and a separator with a rib width of 0.5 mm and a groove width of 0.5 mm as the cathode side separator. First, the manufactured MEA was sandwiched between the anode side separator having a fluid flow path for fuel gas supply and a cooling water flow path, and the cathode side separator having a gas flow path for oxidant gas supply, and a fluororubber gasket was placed around the cathode and anode to manufacture a single cell. The effective electrode (anode or cathode) area was 36 cm2. 2 This unit cell was used as a test piece.
[0078] (Evaluation Tests of Examples 1 to 3 and Comparative Examples 1 to 2) The following evaluation tests were carried out for Examples 1 to 3 and Comparative Examples 1 and 2. Table 1 shows the results of the evaluation tests for Examples 1 to 3 and Comparative Examples 1 and 2. In the evaluation tests, the cell voltage, diffusion overvoltage, and resistance overvoltage were measured as follows. In Table 1, the gas diffusion layer is abbreviated as GDL.
[0079] [Cell voltage] The cell voltage was measured under the following conditions. The cell temperature of the single cell was controlled at 75°C, hydrogen gas was supplied as fuel gas to the gas flow passage on the anode side, and air was supplied to the gas flow passage on the cathode side. The stoichiometry of hydrogen gas was 1.5, and that of air was 1.8. Both the fuel gas and air were humidified to a dew point of 75°C before being supplied to the single cell. Current density: 0 A / cm 2 to 2.0A / cm 2 Up to 0.5A / cm 2 Hold for 3 minutes and apply 2.0A / cm 2 The cell voltage at this time was measured, and the value normalized to the cell voltage of Comparative Example 1 was recorded.
[0080] [Diffusion overvoltage] The diffusion overvoltage was 2.0 A / cm under the same conditions as the cell voltage measurement above. 2 The diffusion overvoltage at this time was measured, and the value normalized to the diffusion overvoltage of Comparative Example 1 was recorded.
[0081] [Overvoltage Resistance] The overvoltage resistance was measured under the same conditions as the measurement of the cell voltage above at 2.0 A / cm 2 and the value normalized with respect to the overvoltage resistance of Comparative Example 1 was recorded.
[0082]
Table 1
[0083] As shown in Table 1, for the fuel cells of Examples 1 to 3, the thickness h of the gas diffusion layer and the rib width Rw of the separator satisfy 0.29Rw ≤ h ≤ 0.55Rw, and the average fiber length Fl of the conductive fibers in the gas diffusion layer satisfies Fl < Rw / 2. Therefore, when using a separator with the same rib width Rw, it was confirmed that in the configurations of Examples 1 to 3, compared with Comparative Examples 1 to 2 shown in Table 1, the cell voltage was higher and the diffusion overvoltage was lower. Fig. 7 plots the results of the evaluation tests of Examples 1 to 3 and Comparative Examples 1 to 2 with respect to the cell voltage and the ratio of the thickness h of the gas diffusion layer to the rib width RW.
[0084] As described above, the fuel cell of the present disclosure has sufficient gas permeability in the gas diffusion layer, and in particular, the power generation performance in the high current density region in the membrane electrode assembly (MEA) has been improved.
[0085] (Evaluation Tests of Examples 4 to 7 and Comparative Examples 3 to 5) In the evaluation tests of Examples 4 to 7, single cells were fabricated and cell evaluations were performed in the same manner as in Examples 1 to 3 described above. The difference from Examples 1 to 3 is only that a separator with a rib width of 0.3 mm and a groove width of 0.3 mm was used as the cathode-side separator. Table 2 shows the results of the evaluation tests of Examples 4 to 7 and Comparative Examples 3 to 5.
[0086]
Table 2
[0087] As shown in Table 2, in the fuel cells of Examples 4 to 7, the thickness h of the gas diffusion layer and the rib width Rw of the separator satisfy 0.29Rw ≤ h ≤ 0.55Rw, and the average fiber length Fl of the conductive fibers in the gas diffusion layer satisfies Fl < Rw / 2. Therefore, when using a separator with the same rib width Rw, it was confirmed that in the configurations of Examples 4 to 7, compared with Comparative Examples 3 to 5 shown in Table 2, the cell voltage was higher and the diffusion overvoltage was lower. FIG. 8 plots the results of the evaluation tests of Examples 4 to 7 and Comparative Examples 3 to 5 with respect to the cell voltage and the thickness h / rib width RW of the gas diffusion layer.
[0088] As described above, the fuel cell of the present disclosure has sufficient gas permeability in the gas diffusion layer, and in particular, the power generation performance in the high current density region in the membrane electrode assembly (MEA) is improved.
[0089] The invention has been described in terms of preferred embodiments with a certain degree of detail. However, the presently disclosed content of this preferred embodiment is subject to change in the details of the configuration, and changes in the combination and order of each element can be realized without departing from the scope and spirit of the claimed invention.
Industrial Applicability
[0090] The fuel cell of the present disclosure can be applied to applications such as household cogeneration systems, automotive fuel cells, mobile fuel cells, and backup fuel cells.
Explanation of Reference Numerals
[0091] 1 Polymer electrolyte membrane 2 Catalyst layer 2a Anode catalyst layer 2b Cathode catalyst layer 3 Gas diffusion layer 3a Anode-side gas diffusion layer 3b Cathode-side gas diffusion layer 4 Separator 4a Anode-side separator 4b Cathode-side separator 5 Groove 6. Ribs 10 Battery Cells 11 Current collector plate 12 Insulating plate 13 End plate 20 Membrane-electrode assembly 31 Conductive particles 32 Conductive Fiber 33 Polymer resin 100 fuel cell< / mea>
Claims
1. A fuel cell in which a membrane electrode assembly (MEA) is sandwiched between separators, the MEA being formed by laminating a catalyst layer and a gas diffusion layer on either side of a polymer electrolyte membrane, the separator has ribs and grooves on a surface in contact with the gas diffusion layer to define a gas flow path through which a reactant gas for power generation flows, The thickness of the gas diffusion layer is h, When the width of the portion of the rib in contact with the gas diffusion layer is Rw, 0.29Rw≦h≦0.48Rw and the gas diffusion layer includes conductive particles, conductive fibers, and a polymer resin; The average fiber length Fl and the average fiber diameter Fd of the conductive fibers Fl<Rw / 2, and Fd<h / 100 and A fuel cell, wherein the amount of the conductive fibers in the gas diffusion layer is greater than the amount of the conductive particles.
2. The average fiber length Fl and the average fiber diameter Fd of the conductive fibers are 0.5 μm≦Fl≦50 μm, and 0.05μm≦Fd≦0.3μm 2. The fuel cell according to claim 1 ,
3. 3. The fuel cell according to claim 1, wherein the gas diffusion layer has a step at the boundary between the rib and the groove, and the surface in contact with the flat top portion of the rib and the surface facing the groove are formed as discontinuous uneven surfaces.
4. 4. The fuel cell according to claim 3, wherein the height of a step in the gas diffusion layer at the boundary between the rib and the groove is 5 to 30 μm.
5. 5. The fuel cell according to claim 4, wherein the gas diffusion layer has a surface roughness Sa of less than 3 [mu]m on the side in contact with the separator.
6. The rib width Rw and the groove width Gw of the separator are 0.7Gw≦Rw≦1.3Gw 6. The fuel cell according to claim 1 , wherein
7. 7. The fuel cell according to claim 1, wherein the gas diffusion layer and the separator are on the cathode side.
Citation Information
Patent Citations
Solid high polymer fuel cell and power generating system using it
JP2003317793A
Fuel cell
JP2004087491A
Solid polymer fuel cell
JP2004319137A