Method and apparatus for reducing HTO concentration in HTO-containing aqueous solution

The use of a boehmite-treated porous sintered aluminum powder body effectively addresses the inefficiencies of current HTO removal methods by selectively adsorbing and occluding tritium at low temperatures, providing a practical and cost-effective solution for large-scale HTO separation and storage.

JP7591777B2Active Publication Date: 2024-11-29KINKI UNIVERSITY +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2019521240
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2017-05-29
Filing Date
2018-05-29
Publication Date
2024-11-29
Estimated Expiration
2038-05-29

AI Technical Summary

Technical Problem

Current methods for removing tritium from contaminated water, such as those used at the Fukushima Daiichi Nuclear Power Plant, are insufficient in terms of performance and cost, and existing technologies are not practical for large-scale HTO separation and storage.

Method used

A method and apparatus using a porous sintered aluminum powder body, treated with boehmite, to selectively adsorb and occlude tritium at low temperatures through isotope exchange, utilizing its porous structure and high surface hydroxyl group density to achieve efficient HTO separation and storage.

Benefits of technology

The method allows for high-efficiency, low-cost HTO separation and storage, enabling recovery and reuse of tritium, suitable for large-scale applications like nuclear fusion experiments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007591777000006
    Figure 0007591777000006
  • Figure 0007591777000007
    Figure 0007591777000007
  • Figure 0007591777000008
    Figure 0007591777000008
Patent Text Reader

Abstract

The present invention relates to a method for reducing the HTO concentration in a tritium-containing aqueous solution. The method comprises bringing water vapor or the like of the tritium-containing aqueous solution into contact with a porous body having pores with a pore size of 500 Å or less to selectively occlude HTO in the tritium-containing aqueous solution into the porous body, thereby obtaining a tritium-containing aqueous solution with a reduced HTO concentration. The present invention also relates to an apparatus used for reducing the HTO concentration in a tritium-containing aqueous solution. The apparatus comprises a reservoir for a raw tritium-containing aqueous solution, a means for generating water vapor or the like of the tritium-containing aqueous solution, an occlusion means storing a porous body with pores with a pore size of 500 Å or less, and a means for recovering the tritium-containing aqueous solution with a reduced HTO concentration. The apparatus further comprises a transfer means for transferring the water vapor or the like to the occlusion means, and a means for transferring the tritium-containing aqueous solution with a reduced HTO concentration from the occlusion means to the recovery means.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method and an apparatus for reducing the concentration of tritiated water (HTO) in an aqueous solution containing HTO. In particular, the present invention relates to a method for reducing the concentration of HTO in an aqueous solution containing HTO by using a porous sintered aluminum powder body, which is useful for removing HTO from HTO-containing contaminated water. [Background technology]

[0002] Toshiba's Advanced Liquid Processing System (ALPS) continues to operate to treat the large amount of contaminated water that continues to be generated as a result of the Fukushima Daiichi Nuclear Power Plant accident, but decontamination is limited to radionuclides other than tritium. This is because the chemical properties of tritium in contaminated water (mostly existing as tritiated water (HTO)) are the same as water. Therefore, the treatment of contaminated water containing HTO has not progressed, and it continues to be stored every day, with the total amount of contaminated water stored in tanks exceeding 800,000 tons. For more information, please refer to the portal site "Decommissioning and Contaminated Water Countermeasures Portal Site" on the Ministry of Economy, Trade and Industry's website and the "Tritiated Water Task Force Report."

[0003] The main HTO removal methods used around the world today are 1) vacuum water rectification (WD method), 2) water / hydrogen isotope exchange reaction combined with electrolysis (CECE method), 3) dual-temperature water / hydrogen isotope exchange reaction (BHW method), and 4) water / hydrogen sulfide isotope exchange reaction (GS method) (Non-Patent Document 1). However, none of these methods are sufficient in terms of performance or cost for use as a countermeasure against contaminated water from the Fukushima nuclear power plant. Currently, the Russian state-run nuclear power company Rosatom has announced that a method that combines 2) and 3) has a high decontamination effect (Non-Patent Document 2).

[0004] Contaminated water containing HTO currently stored in tanks at the Fukushima Daiichi Nuclear Power Plant continues to be stored every day. Under these circumstances, development of HTO separation and removal technology is underway. According to a report by Mitsubishi Research Institute (Non-Patent Document 1) in October 2014, three companies were selected as subsidized operators for the "Tritium Separation Technology Verification Test Project": Kurion, Inc. (USA), GE Hitachi Nuclear Energy Canada Inc. (Canada), and RosRAO (Russia). However, the practicality of these projects is deemed insufficient in terms of energy consumption, facility size, the need for additional equipment to ensure safety, and running costs.

[0005] Non-patent literature 1: TEPCO website material "The status of tritium at the Fukushima Daiichi Nuclear Power Plant [Document 4-1] April 26, 2013" (http: / / www.tepco.co.jp / nu / fukushima-np / roadmap / images / c130426_06-j.pdf) Non-patent literature 2: Global Energy Policy Research website material "Removal of tritium from water now possible - Rosatom" (http: / / www.gepr.org / ja / contents / 20160719-01 / ) Non-patent document 3: Mitsubishi Research Institute document reported in October 2014 (regarding the "Tritium Separation Technology Verification Test Project") Non-patent document 4: J. Plasma Fusion Res., Vol. 85, No. 10 (2009) 726-735 Summary of the Invention [Problem to be solved by the invention]

[0006] The present invention provides a novel method and apparatus for separating tritiated water molecules (HTO) from HTO-containing water, which is highly likely to be practical. [Means for solving the problem]

[0007] It is known that when heavy water (DO) is adsorbed on Fe2O3 at room temperature instead of tritiated water (HTO), and then exposed to HO at room temperature to perform isotope exchange, the ease with which the exchange occurs varies depending on the state of DO (Non-Patent Document 4: J. Plasma Fusion Res., Vol. 85, No. 10 (2009) 726-735). Based on this knowledge, the inventors speculated that in the case of HTO, by adsorbing it in an environment where HTO is likely to interact, the isotope exchange reaction with light water (HO) becomes less likely to occur, making it possible to selectively adsorb HTO.

[0008] Based on this assumption, the inventors have investigated a method for separating tritiated water (HTO) from tritium-containing water by utilizing the difference in physical and chemical properties between light water (HO) and tritiated water (HTO).

[0009] The inventors of the present invention considered that if a structure with a developed microstructure of metal oxide or metal hydroxide, for example, a porous structure with gaps between layers through which water molecules can penetrate, could be prepared, it would be possible to provide a microscale (2 nm or less) or mesoscale (2 to 50 nm) space with a high density of surface hydroxyl groups, and that the site could function as a space for concentrating and absorbing HTO. The material they focused on was a sintered aluminum powder porous body used in the electrical absorption of cesium (Patent Application No. 2016-027321). By treating this material with boehmite, needle- or petal-shaped boehmite crystals (aluminum metal hydrated oxide) grow within the pores, and the amount of hydroxyl groups per unit volume increases along with the specific surface area (see Figure 1). Furthermore, boehmite has a layered structure in which unit layers of AlO6 octahedrons sharing ridgelines are stacked as shown in Figure 3 (Kenichi Sakamoto, Light Metals, Vol. 22, No. 4, P. 295 (1972)), and HTO is expected to be held in the micro- or meso-space between the layers by capillary condensation. Note that Al in this AlO6 octahedron is surrounded by five oxygen atoms and one hydroxyl group, and the structure of one layer formed by the AlO6 octahedron in Figure 3 is shown in Figure 4. The inventors experimentally discovered that the surface of the grown crystal of a sintered aluminum powder porous body treated with boehmite has a relatively strong interaction with HTO at a relatively low temperature.

[0010] Furthermore, the enrichment and occlusion action of HTO was examined using a number of porous bodies with known pore sizes other than the boehmite-treated aluminum powder sintered porous body. Since HTO and DO are isotopes and both have the same mass number of 20, DO was used in this examination on the premise that the effect of mass (on physical adsorption and physical desorption) can be determined to be the same for HTO and DO. As a result, it was found that HTO can be separated by using a porous body having pores with a pore size in the range of 500 Å or less, and that, in particular, by using a porous body having pores with a pore size in the range of more than 4 Å and not more than 25 Å, it is possible to highly efficiently separate HTO occluded in the porous body at a relatively low temperature, even if the porous body is other than the boehmite-treated aluminum powder sintered porous body, and the present invention was completed based on this finding.

[0011] The present invention is as follows. [1] A method for reducing an HTO concentration in a tritium-containing aqueous solution, comprising: The method includes continuously or intermittently contacting the water vapor and / or mist of the tritium-containing aqueous solution with a porous body having pores with a pore size in the range of 500 Å or less to selectively occlude HTO in the tritium-containing aqueous solution into the porous body, and obtaining a liquid that has not been occluded as a tritium-containing aqueous solution having a reduced HTO concentration (hereinafter referred to as low tritium-containing water), The method, wherein the porous body is a boehmite-treated product. [2] The method according to [1], wherein the porous body has at least pores having a pore size in the range of more than 4 Å and not more than 25 Å. [3] The method according to [1] or [2], wherein the porous body is an inorganic porous body. [4] The method according to [3], wherein the inorganic porous material is a porous material containing at least one selected from the group consisting of zeolite, γ-alumina, silica gel, boehmite, and aluminum. [5] The method according to [3], wherein the inorganic porous material is a porous aluminum body having a boehmite coating. [6] The method according to any one of [1] to [5], wherein the inorganic porous material is in the form of a powder. [7] The method according to any one of [1] to [5], wherein the inorganic porous material is a powder sintered porous material. [8] The porous body has a specific surface area of ​​5 to 250 m 2 The method according to any one of [1] to [7], wherein the range is 0.01 to 0.15. [9] The method according to any of [1] to [8], wherein the porous body with which the water vapor or mist of the HTO-containing aqueous solution is brought into contact is maintained at a temperature equal to or lower than an endothermic peak temperature of HTO adsorbed in the pores of the porous body in differential scanning calorimetry.

[10] The method according to [9], wherein the porous body has an endothermic peak temperature in a range of 60°C to 100°C in differential scanning calorimetry of HTO adsorbed in the pores of the porous body.

[11] The method according to any one of [1] to

[10] , wherein the water vapor and / or mist of the HTO-containing aqueous solution is supplied at a pressure in the range from atmospheric pressure to the saturated vapor pressure of the HTO-containing aqueous solution, and brought into contact with a porous body to selectively adsorb HTO to the porous body, and the HTO-containing aqueous solution having a reduced HTO concentration (low-HTO content water) is obtained by making the downstream side of the porous body more negative in pressure than the supply side of the HTO-containing aqueous solution, thereby giving priority to the evaporation of light water from the surface of the porous body.

[12] The method according to any one of [1] to

[11] , wherein the water vapor and / or mist of the HTO-containing aqueous solution is contacted with the porous body under reduced pressure.

[13] The method according to any one of [1] to

[12] , wherein the porous body comprises a plurality of porous bodies, and the water vapor and / or mist of the HTO-containing aqueous solution is contacted with the plurality of porous bodies in sequence.

[14] The method according to

[13] , in which an HTO-containing aqueous solution having a reduced HTO concentration obtained by contact with a porous body has a higher HTO concentration reduction rate as the number of porous bodies increases.

[15] The method according to any one of [1] to

[14] , comprising recovering and storing the porous body that has occluded a predetermined amount of HTO.

[16] The method according to any one of [1] to

[15] , further comprising releasing the occluded HTO from the recovered porous body and recovering the released HTO.

[17] An apparatus for reducing an HTO concentration in a tritium-containing aqueous solution, comprising: A reservoir for the raw HTO-containing aqueous solution, means for generating water vapor and / or mist of the HTO-containing aqueous solution in said reservoir; An occlusion means storing a porous body having pores with a pore diameter in the range of 500 Å or less; and A method for recovering HTO-containing aqueous solutions with reduced HTO concentrations and a transfer means for transferring the water vapor and / or mist to the storage means; and the apparatus further comprising a means for transferring the HTO-containing aqueous solution having a reduced HTO concentration from the storage means to the recovery means.

[18] The device described in

[17] , wherein the porous body has at least pores having a pore diameter in the range of more than 4 Å and not more than 50 Å.

[19] The apparatus according to

[17] or

[18] , wherein the porous body comprises a plurality of porous bodies, and the plurality of porous bodies are stored in multiple stages in the occlusion means.

[20] The device according to any one of

[17] to

[19] , wherein the porous body is an inorganic porous body. [twenty one] The apparatus according to

[20] , wherein the inorganic porous body is a porous body containing at least one selected from the group consisting of zeolite, γ-alumina, silica gel, boehmite, and aluminum. [twenty two] The apparatus described in

[20] , wherein the porous body is a porous aluminum body having a boehmite coating. [twenty three] The porous body has a specific surface area of ​​5 to 250 m 2 The device according to any one of

[17] to

[22] , wherein the range is 1 / g. [twenty four] The device according to any one of

[17] to

[23] , wherein the porous body is freely detachable from the occlusion means. [twenty five] The apparatus according to any one of

[17] to

[24] , which is used for carrying out any one of the methods [1] to 16. Effect of the Invention

[0012] According to the present invention, it is possible to separate HTO by absorption at a relatively low temperature. The material used for HTO absorption may be a porous body having pores with a pore diameter of 500 Å or less, for example, a porous body of sintered aluminum powder or other commercially available inorganic material porous bodies, and is relatively inexpensive. Furthermore, the absorbed HTO can be easily released from the absorption material by increasing the temperature, and can be separately recovered. Therefore, it is expected to be used as a means of supplying HTO to fuel for nuclear fusion reaction experiments, and if it is viable in the tritium economy, it can provide a removal method with excellent cost performance. [Brief description of the drawings]

[0013] [Figure 1] An electron microscope photograph of boehmite crystals grown on the surface of a porous aluminum material. [Diagram 2] FIG. 1 is a schematic diagram of an embodiment of a tritium absorption and removal device. [Diagram 3] The crystal structure of boehmite is shown. The double lines connecting the octahedra indicate hydrogen bonds. [Figure 4] The structure of one layer of boehmite formed by the AlO6 octahedron shown in Figure 3 is shown. [Diagram 5] FIG. 1 is a schematic diagram of an embodiment of a tritium absorption and removal device. [Figure 6] The relationship between the amount of pseudo-contaminated water (treatment amount) and the decontamination rate obtained in Example 3. [Figure 7] The relationship between the amount of pseudo-contaminated water (treatment amount) and the decontamination rate obtained in Example 4. [Figure 8] The relationship between the amount of pseudo-contaminated water (treatment amount) and the decontamination rate obtained in Example 5. [Figure 9] The relationship between the amount of pseudo-contaminated water (treatment amount) and the decontamination rate obtained in Example 6. [Figure 10] The relationship between the amount of pseudo-contaminated water (treatment amount) and the decontamination rate obtained in Example 7. [Figure 11] The figure shows the results of DSC measurements at elevated temperatures after H2O or D2O was saturated at 60°C on a zeolite with a pore size of 7 Å (mordenite, HSZ-640). [Figure 12]The DSC measurement results obtained by heating after saturating silica gel Wakosil C-200 (type B, pore diameter 60 Å) for column chromatography with H2O or D2O at 60 °C are shown.

Mode for Carrying Out the Invention

[0014] The present invention is a method for reducing the concentration of HTO in an HTO-containing aqueous solution. This method involves bringing the water vapor and / or mist of the HTO-containing aqueous solution into contact with a porous body having pores with a pore diameter in the range of 500 Å or less, selectively occluding the HTO of the HTO-containing aqueous solution in the porous body, and obtaining an HTO-containing aqueous solution with a reduced HTO concentration.

[0015] <HTO-containing aqueous solution> The HTO-containing aqueous solution can be a substance containing HTO, for example, in the range of 100 Bq / L to 5 MBq / L, although the HTO content concentration varies depending on the production process. Examples of the HTO-containing aqueous solution include contaminated water generated by the accident at the Fukushima Daiichi Nuclear Power Plant and water containing HTO generated by neutron capture during the operation of a light water reactor.

[0016] <Porous body> The porous body used in the present invention is a porous body having pores with a pore diameter in the range of 500 Å (50.0 nm) or less. The lower limit of the pore diameter of the porous body is preferably 4 Å (0.4 nm). Therefore, the porous body preferably has pores with a pore diameter in the range of 4 Å or more and 500 Å or less. In particular, there are cases where it is preferably a porous body having pores with a pore diameter larger than 4 Å (0.4 nm) and in the range of 50 Å (5.0 nm) or less. From the results of Test Examples 1 to 4 described later, the present inventors have found that a porous body with a pore diameter in this range can separate HTO by occlusion at a relatively low temperature. The porous body can also have pores with a pore diameter outside the above range. The pore diameter in the present invention is measured by a multi-sample high-performance specific surface area / pore size distribution measuring device 3Flex (manufactured by Shimadzu).

[0017] The porous body having a pore size in the above range can be, for example, an inorganic porous body. Furthermore, the inorganic porous body can be, for example, a porous body containing at least one selected from the group consisting of zeolite, γ-alumina, silica gel, boehmite, and aluminum. Furthermore, the porous body can be an aluminum porous body having a boehmite coating.

[0018] The porous body has a specific surface area of, for example, 5 to 250 m 2 / g, preferably 10 to 200m 2 / g range.

[0019] Zeolite materials having various pore distributions are known, and many of them are commercially available. In the present invention, the zeolite used as the porous body is preferably mordenite, which is a natural product, in consideration of the pore size, specific surface area, etc. However, it is not intended to be limited to mordenite.

[0020] The pore size of γ-alumina has been reported to be in the range of about 85 Å to 150 Å depending on the preparation conditions. From the DSC measurement results of samples adsorbing HO and DO (or HTO), it is preferable to use a pore size that causes a difference in the endothermic peak temperatures of HO and DO (or HTO).

[0021] The silica gel is preferably one having a pore size such that a difference appears in the endothermic peak temperatures of H2O and D2O (or HTO) in the DSC measurement results of a sample having H2O and D2O (or HTO) adsorbed thereon.

[0022] The aluminum powder sintered porous body before the boehmite treatment is, for example, a sintered body of aluminum powder having an average particle size of 1 to 20 μm and a calculated specific surface area of ​​0.1 to 1 m. 2 / g. The product before the boehmite treatment does not contain any components other than aluminum, except for unavoidable impurities. The purity of aluminum is preferably 99.9% by mass or more, more preferably 99.99% by mass or more. The product before the boehmite treatment has an average particle diameter D 50It is manufactured by sintering aluminum powder with a diameter of 1 to 20 μm in an inert atmosphere at a temperature range of 500 to 650°C, and has a porosity of about 45 to 60% and maintains high electrical conductivity. Furthermore, after sintering, the surface is naturally oxidized and the entire surface, including the inside of the voids, is covered with a thin oxide film. This oxide film not only exhibits high chemical stability and environmental resistance, but also functions as an adsorption (occlusion) site for cations.

[0023] The boehmite pre-treatment product thus obtained has a calculated specific surface area in the range of 0.1 to 1 m 2 / g, and the actual measured values ​​(method will be described later) are almost the same, 0.1 to 1 m 2 The specific surface area varies depending on the particle size of the aluminum powder used in sintering and the sintering conditions, but the calculated and measured specific surface areas are in the range of 0.1 to 1 m 2 / g, preferably 0.15 to 0.5 m 2 / g range. After sintering, the pre-boehmite-treated product is subjected to boehmite treatment to obtain a boehmite-treated product. The boehmite treatment is known as a technique for forming a finely uneven or petal-shaped boehmite thin film on a glass substrate or a polymer substrate by treating an alumina gel with hot water, for example. In the present invention, specifically, the boehmite treatment is performed by immersing the pre-boehmite-treated product in water at a temperature of 90°C or higher, preferably 95°C or higher, for 1 to 60 minutes.

[0024] The boehmite treatment forms an aluminum-based oxide film on the surface. The aluminum-based oxide film is a film of at least one aluminum-based oxide selected from the group consisting of γ-alumina and alumina hydrate. The boehmite treatment also increases the specific surface area (actual measured value). The specific surface area of ​​the boehmite-treated product is 5 to 50 m2 (actual measured value). 2 / g range, preferably 8 to 16m 2 / g, more preferably 9 to 16m 2 / g, more preferably 10 to 16 m 2 / g range, 10m 2The boehmite-treated product is a sintered body of aluminum powder having an average particle size of 1 to 20 μm, has an aluminum-based oxide coating on the surface, and has a specific surface area of ​​5 to 20 m2 as an actual measured value. 2 The specific surface area can be measured by a flow-type automatic specific surface area measuring device, FlowSorb III2305 (Shimadzu), using nitrogen molecules.

[0025] As a method for treating boehmite, in addition to the above-mentioned method using warm water (pure water), a method using an aqueous solution exhibiting basicity to which a basic compound such as an amine or ammonia is added can also be used.

[0026] The aluminum oxide film formed on the surface by boehmite treatment is an alumina hydrate represented by AlOOH or Al2O3·H2O. It is formed by treating aluminum with boiling water and is known to have excellent corrosion resistance. However, the hydroxide ion OH, which is the anion of aluminum, is also known to be a hydrate. - The general formula Al(OH) n (e.g., n=3) may additionally include an amphoteric hydroxide.

[0027] The porous body preferably has a predetermined shape, and the predetermined shape may be, for example, a powder shape, a disk shape, a plate shape, or a honeycomb structure.

[0028] <Occlusion in porous bodies> The HTO-containing aqueous solution is brought into contact with the porous body as water vapor and / or mist. More specifically, when the HTO-containing aqueous solution is converted into water vapor, the HTO-containing aqueous solution is heated, and when the HTO-containing aqueous solution is converted into mist, the HTO-containing aqueous solution is supplied to a mist generating device such as a nebulizer. The water vapor and / or mist comes into contact with the porous body, and the HTO contained in the HTO-containing aqueous solution is selectively occluded into the porous body by direct occlusion into the porous body or by an isotope exchange reaction with light water (H2O) that has already been occluded. The reason why the HTO contained in the HTO-containing aqueous solution is selectively occluded into the porous body is presumably basically due to the difference in equilibrium water vapor pressure between light water and HTO.

[0029] The reason why HTO contained in the HTO-containing aqueous solution is selectively absorbed into the porous material is presumably based on a principle similar to that of water distillation. Water distillation is a method of concentrating components with low equilibrium vapor pressure into the liquid phase by repeating evaporation and condensation distillation operations using the difference in equilibrium vapor pressure between multiple components in a solution. The equipment used in water distillation uses a distillation tower, a boiler is placed at the bottom of the tower to generate steam, and a condenser is placed at the top of the tower to convert the steam back into water to create a reflux. HTO, which has a low equilibrium vapor pressure, is condensed on the tower wall before reaching the condenser and returns to the bottom of the tower as a reflux. Light water reaches the condenser at the top of the tower, so separation of HTO and tritium enrichment in the reflux water progresses. The disadvantages of water distillation are that the tower becomes taller, resulting in a large-scale equipment, and the higher the distillation temperature, the smaller the separation factor between light water and HTO, so evaporation and condensation are repeated many times, and operation at reduced pressure is required. It has been widely used in oil plants and other places. The mechanism of separation by water distillation can be expressed as the following equilibrium equation (1) (J. Plasma Fusion Res., Vol. 85, No. 10 (2009) 726-735).

[0030] [ka]

[0031] That is, a mixed solution of H2O and HTO is heated, and after both are once turned into vapor, separation is carried out by returning only HTO, which is more likely to return to water, to the liquid state.

[0032] In the present invention, it is basically presumed to be based on a principle similar to the principle of the distillation method. However, the difference from the conventional distillation method is that the state change from water to water vapor in the conventional distillation method occurs at the gas-liquid interface, whereas when a porous body is used, it occurs in the adsorbed state on the inner surface of the microspace or mesospace between the layers of the porous body. In other words, the present invention can be said to be a separation technique that utilizes the state change at the gas-micro / meso-filled liquid phase interface by filling the microspace or mesospace, and is characterized in that the separation coefficient between H2O and HTO can be increased. That is, the separation coefficient α in the distillation method is represented by the ratio P(H2O) / P(HTO) of the saturated vapor pressure P(H2O) of water and the saturated vapor pressure P(HTO) of HTO at that temperature. However, the separation coefficient α(ad) in the state where the micro-pores of the porous body are filled is represented by P(H2O-ad) / P(HTO-ad). Since the degree of stabilization energy brought about by micro-filling is water < HTO, the difference between P(H2O-ad) and P(HTO-ad) becomes significant. Therefore, it is considered that the separation coefficient α(ad) in the adsorbed state is larger than the separation coefficient α in the distillation method. Considering this separation mechanism, it is preferable to carry out the separation at a low temperature at which micro-pore filling (capillary condensation) of HTO into the microspace or mesospace is likely to occur. However, appropriate heating is required to increase the separation speed. It is preferable from the viewpoint of efficiency that the porous body in contact with the water vapor or mist of the tritium-containing aqueous solution is maintained at a temperature of 60°C or lower, preferably in the range of 30 to 60°C.

[0033] The water vapor and / or mist of the tritium-containing aqueous solution is supplied at a pressure in the range from atmospheric pressure to the saturated vapor pressure of the tritium-containing aqueous solution and brought into contact with the porous body, and tritium-containing water (HTO) is selectively adsorbed onto the porous body. The tritium-containing aqueous solution (low-tritium-containing water) with a reduced HTO concentration can be obtained by making the downstream side of the porous body have a negative pressure relative to the supply side of the tritium-containing aqueous solution and giving priority to the transpiration of light water (H2O) from the surface of the porous body.

[0034] The contact of the water vapor and / or mist of the HTO-containing aqueous solution with the porous body can be carried out under reduced pressure, and is preferably carried out under reduced pressure. By carrying out the contact under reduced pressure, the temperature can be set relatively low (for example, 60° C. or less). The pressure of the reduced pressure is, for example, 10 3 ~10 5 Pa range, preferably 10 3 ~10 4 The range is Pa.

[0035] The porous bodies may be composed of a plurality of porous bodies, and the water vapor and / or mist of the HTO-containing aqueous solution may be contacted with the plurality of porous bodies in sequence. By contacting the plurality of porous bodies in sequence, the HTO concentration in the aqueous solution can be sequentially reduced. The HTO-containing aqueous solution having a reduced HTO concentration obtained by contacting the porous bodies has a higher HTO concentration reduction rate as the number of porous bodies increases.

[0036] The present invention includes recovering and storing the porous body having a predetermined amount of HTO occluded therein. Alternatively, the occluded HTO can be released from the recovered porous body and the released HTO can be recovered. Alternatively, the porous body having a predetermined amount of HTO occluded therein can be placed under conditions that facilitate the release of HTO, causing the HTO to be released and the released HTO can be recovered. For example, after the end of occlusion, the porous body having occluded HTO can be heated to release the occluded HTO, and the released HTO can be recovered again in a cold trap.

[0037] The porous body from which HTO has been released can be reused repeatedly.

[0038] <Device> The present invention includes an apparatus for use in reducing the concentration of HTO in an aqueous solution containing HTO, the apparatus comprising: a reservoir 10 for the raw HTO-containing aqueous solution; Means 12 for generating water vapor and / or mist of the HTO-containing aqueous solution in the reservoir 10; an occlusion means 20 containing a porous body; and Means for recovering HTO-containing aqueous solution with reduced HTO concentration 30 Furthermore, the device of the present invention comprises: a transfer means 40 for transferring said water vapor and / or mist to the storage means; and The apparatus further includes a means for transferring the HTO-containing aqueous solution having a reduced HTO concentration from the storage means to the recovery means. The porous body has pores with a pore diameter in the range of 500 .ANG.. The porous body is the same as that described above.

[0039] One embodiment of the device of the present invention will be described with reference to FIG. The reservoir 10 for storing the raw HTO-containing aqueous solution (TW) has a thermocouple 1 (11) for measuring temperature and a dry air inlet 12a, which is a means 12 for generating water vapor of the TW. When a mist of the TW is to be generated, a nebulizer can be provided separately (not shown). The reservoir 10 is set in a mantle heater 13 and adjusted to a predetermined temperature. The storage means 20 can be a reactor (sealed container) that contains the porous body 22, has a heater for adjusting the temperature on the side surface, and has openings 20in and 20out on the lower and upper sides. The storage means 20 has a thermocouple 22 for measuring the temperature near the porous body 22. The reservoir 10 and the occlusion means 20 are in communication with each other via a transfer means 40 , and the water vapor (or mist) generated in the reservoir 10 is transferred to the occlusion means 20 by the transfer means 40 . The storage means 20 is in communication with a means 30 for recovering TW with a reduced HTO concentration through a transfer means 50. The TW with a reduced HTO concentration produced by the storage means 20 is recovered. The recovery means 30 in Fig. 2 is cold traps 30a and 30b, but is not intended to be limited to cold traps.

[0040] When using a boehmite-treated porous body as an HTO occlusion material in TW, immersing the porous body in TW for a long period of time can cause concerns about the mechanical strength of the porous body. Therefore, in the present invention, the basic design of a removal device for stably removing HTO for a long period of time is preferably a method in which the porous body is used as a filter and negative pressure is used to allow TW vapor to pass through. The device shown in Figure 2 has a configuration that conforms to this method. The negative pressure is also 10 2 Since separation proceeds in a low vacuum region of 10 Pa or more, the components of the device can be connected using Teflon tubes and Teflon joints, which are less susceptible to HTO contamination, rather than stainless steel piping and stainless steel high vacuum joints. Another major advantage is that the device configuration is extremely simple.

[0041] The apparatus of the present invention used in the examples is composed of a reactor in which multiple sheets of boehmite-treated porous bodies processed into a disk shape with a thickness of 10 mm and a diameter of 74 mm can be stacked in multiple stages, a reservoir and mantle heater that vaporize HTO water used as simulated contaminated water into steam, a cold trap (made of PYREX (registered trademark) glass) that collects the water vapor that passes through the reactor, a diaphragm pump (KNF, N813.3 ANE, exhaust speed 13 L / min) that generates negative pressure for suction, and a dry air inlet. These are basically connected with Teflon tubes (12 φ). In addition, ribbon heaters are wrapped around the reactor and other main paths to enable temperature control. High-purity dry air in a high-pressure cylinder was used.

[0042] The porous body may be composed of a plurality of porous bodies 22, and the plurality of porous bodies 22 may be stored in multiple stages (series) in the occlusion means 20. However, the plurality of porous bodies 22 may also be stored in the occlusion means 20 partially or entirely in parallel, instead of in multiple stages (series).

[0043] The porous body has a specific surface area of ​​5 to 250 m 2 / g range.

[0044] The porous body 22 is detachable from the storage means 20. The detachable porous body 22 can be removed from the storage means 20 and transported to another location, and then the occluded HTO can be taken out and recovered.

[0045] Another embodiment of the device of the present invention is shown in FIG. The structure of the device is basically the same as that used for the porous material shown in Figure 2. The difference between the two is that the means for storing the HTO absorbent has been changed from a porous material to a powdered absorbent, and the accuracy of temperature control has been improved by placing everything except the cold trap and diaphragm pump in the thermostatic layer. The details are as follows.

[0046] This device is composed of a reactor (column) 23, a simulated contaminated water reservoir 14, and a cooling trap 31. All components except the cooling trap 31 are housed in a thermostatic chamber, allowing constant temperature operation. The column 23 and the cooling trap 31 are connected by a transfer means 60. The column 23 is a cylindrical column made of Pyrex (outer diameter: 50 mm, height: 230 mm), and glass filters 24a and 24b are attached to the top and bottom of the column to prevent the powder of the porous body 25 from escaping. The lower glass filter 24b is fixed to the column, while the upper filter 24a is sealed with packing and is fixed by tightening the lid. All piping is made of Teflon. The simulated contaminated water reservoir 14 has a capacity of 100 mL, and is designed so that when air is sucked from the top of the column by a diaphragm pump (not shown), dry air at atmospheric pressure flows into the reservoir 14 from the inlet 15.

[0047] When the dry air is sucked from the top of the column by a diaphragm pump (not shown), it is bubbled into the simulated contaminated water in the reservoir 14, and the simulated contaminated water becomes water vapor at the saturated vapor pressure at the temperature set in the thermostatic bath, and is supplied into the column 23 from the lower side of the column 23. The column 23 is filled with a porous body, and the air containing the saturated vapor of the simulated contaminated water that flows in pushes up the adsorbent from below and floats up to the surface of the porous body layer, during which the HTO in the simulated contaminated water collides with the adsorbent countless times, and H2O, which has a weaker interaction with the porous body than HTO, which has a stronger interaction with the porous body, is selectively evaporated from the surface of the porous body layer. As a result, the simulated contaminated water with a lower HTO concentration is collected in the trap downstream of the column. EXAMPLES

[0048] The present invention will be described in more detail below with reference to examples. However, the examples are merely illustrative of the present invention and are not intended to limit the present invention.

[0049] <Tritium Experiment 1> 50 mL of HTO prepared to a concentration of 0.5 MBq / L as simulated contaminated water was placed in a 100 mL round-bottom flask (reservoir) connected to the bottom of the apparatus shown in Figure 2, and a 10 mm thick, 74 mm diameter porous body (80 g) that had been dried under reduced pressure at 60°C for 6 hours was placed in the reactor. In the apparatus shown in Figure 2, the main two places to be heated were the reactor equipped with the porous body and the reservoir for the contaminated water. In addition, ribbon heaters were wrapped around the piping connecting these to the cold trap to prevent condensation, and the piping was heated to 40°C.

[0050] After that, the temperature of the reactor was set arbitrarily (60°C in Example 1, 100°C in Example 2), and it was confirmed that the temperature was stable. Then, powdered dry ice was packed into the Dewar flask of the trap, and dry air at atmospheric pressure was sucked into the pseudo-contaminated water in the round-bottom flask (reservoir) filled with the pseudo-contaminated water, and the mixture of the water vapor of the pseudo-contaminated water and the air was sent while bubbling, and the decontamination experiment was started. The amount of the pseudo-contaminated water vapor supplied to the porous body is greatly affected by the temperature of the reservoir as well as the air supply rate from the air supply of the reservoir. Here, the temperature was kept constant at 40°C, and this state was maintained for one hour. However, this temperature setting of 40°C is the temperature control temperature of the mantle heater, and is not the temperature at which the pseudo-contaminated water in the reservoir was directly measured.

[0051] After the experiment was completed, ion-exchanged water was added to the water collected in the trap to make the total volume 5 ml. The collected water with a total volume of 5 ml and 5 ml of tritium source water used in the experiment were measured using a liquid scintillation counter to determine their respective count rates. The count rate of the collected water was taken as the sample count rate, and the count rate of the tritium source water was taken as the stock count rate, and their specific radioactivity cpm / g was calculated. The equipment used was a Packard TRi-CARB 2050CA, and measurements were performed using the LSC cocktail method using a liquid scintillation cocktail. The decontamination rate (%) of the water collected in the trap was calculated by comparing the specific radioactivity (2546.5 cpm / g) of the water collected in the trap and the tritium source water used in the experiment. The following formula was used to calculate the decontamination rate.

[0052]

number

[0053] <Example 1> A porous body of sintered aluminum powder was subjected to boehmite treatment (immersed in pure water at a temperature of 90°C or higher for 10 minutes) (boehmite-treated product, specific surface area = 11.27 m 2A tritium experiment was carried out using a 1.82g sample of water, with a sample count rate of 510cpm and a specific activity of 280.2cpm / g, resulting in a decontamination rate of 89.1%.

[0054] <Example 2> The aluminum powder sintered porous body used in Example 1 (boehmite-treated product, specific surface area = 11.27 m 2 The temperature of the reactor was set to 100°C and a tritium experiment was carried out using the same water as it was. The amount of water recovered was 3.00g, the sample count rate was 4017cpm, the specific activity was 1339.0cpm / g, and the decontamination rate was 47.3%.

[0055] <Reference example 1> A tritium experiment was conducted without the porous medium. The amount of water recovered was 2.54 g, the sample count rate was 6426 cpm, the specific activity was 2530 cpm / g, and the decontamination rate was 0.65%.

[0056] [Table 1]

[0057] From the above results, it is believed that the decontamination of pseudo-tritium-contaminated water using porous aluminum works by taking in HTO between the boehmite layers on the surface of the porous aluminum and filling the micropores. Since filling of the micropores is a physical adsorption, the adsorbed tritium can be desorbed by a moderate temperature increase, and it can also be recovered again.

[0058] <Tritium Experiment 2> The experimental procedure was basically the same as that of Tritium Experiment 1, in which a porous sintered aluminum body was used. 50 mL of HTO prepared to a concentration of 0.2 MBq / L as simulated contaminated water was placed in a 100 mL round-bottom flask (reservoir) connected to the bottom of the apparatus shown in Figure 5, and 40 g of HTO adsorbent dried under reduced pressure at 25°C for 6 hours was weighed out and placed in the thermostatic chamber. A ribbon heater was wrapped around the piping outside the thermostatic chamber connected to the cooling trap to prevent condensation, and the piping was heated to 40°C.

[0059] After that, the temperature of the thermostatic bath was set to 40°C, and after confirming that the temperature had stabilized, crushed dry ice was packed into the trap's Dewar flask and the diaphragm pump was operated, which caused dry air at atmospheric pressure to be sucked into the simulated contaminated water in the round-bottom flask (reservoir) filled with the contaminated water, and while bubbling, the vapor of the contaminated water was supplied directly to the column along with the air, and the decontamination experiment began.

[0060] After the experiment, ion-exchanged water was added to the water collected in the trap to make the total volume 5 mL. The collected water with a total volume of 5 mL and 5 mL of tritium source water used in the experiment were measured using a liquid scintillation counter to determine their respective count rates. The count rate of the collected water was taken as the sample count rate, and the count rate of the tritium source water was taken as the stock count rate, and the specific radioactivity cpm / g was calculated for each. The instrument used was a Packard Tri-CARB 2050CA, and measurements were made using the LSC cocktail method using a liquid scintillation cocktail. The decontamination rate (%) of the water collected in the trap was calculated by comparing the specific radioactivity of the water collected in the trap and the tritium source water used in the experiment. The same calculation formula for the decontamination rate as described above was used.

[0061] <Example 3> The HTO absorbent was treated with boehmite (immersed in pure water at a temperature of 90°C or higher for 300 minutes and then hydrothermally treated) to give an aluminum powder (boehmite + hydrothermally treated product, specific surface area 77.11 m). 2 Tritium experiments were carried out using 40 g of tritium ions (15 g / g) and setting the temperature of the thermostatic chamber to 40°C. Figure 6 shows the relationship between the amount of pseudo-contaminated water that passed through the column (treatment amount) and the decontamination rate. There is a tendency for the decontamination rate to decrease as the integrated value of the treatment amount increases, but it can be seen that a decontamination rate of about 30% is maintained even when the treatment amount exceeds 15 g.

[0062] <Example 4> Zeolite (specific surface area 30.41 m) was used as the HTO storage material. 2 / g) was used, and the temperature of the thermostatic chamber was set to 40°C to carry out the tritium experiment. The relationship between the amount of pseudo-contaminated water (treatment amount) that permeated the column and the decontamination rate is shown in Figure 7.

[0063] <Example 5> The HTO adsorption material is γ-alumina (specific surface area 84.67 m 2 A tritium experiment was carried out using 40 g of 10 ...

[0064] <Example 6> The HTO adsorbent was silica gel (spherical silica gel for column chromatography, Wakosil-200, manufactured by Wako Pure Chemical Industries, Ltd., specific surface area 123.28 m). 2 A tritium experiment was carried out using 40 g of 10 ...

[0065] <Example 7> The HTO adsorption material was a commercially available boehmite (C-06, Taimei Chemicals, specific surface area 16.86 m 2 Tritium experiments were carried out using 40 g of 10 ...

[0066] As mentioned above, experiments were conducted using five types of tritium adsorbent, and from each plot in the figure, the straight line intersecting the X-axis and Y-axis was calculated using the least squares method, and the area of ​​the triangle enclosed by the straight line and the X-axis and Y-axis was calculated to calculate the amount of tritium adsorbed (adsorption capacity) per gram of tritium adsorbent. The results are shown in Table 2 below.

[0067] [Table 2]

[0068] [Table 3]

[0069] The results in Table 2 are listed in descending order of tritium absorption capacity: zeolite (83 Bq / g) > gamma-alumina (58.8 Bq / g) > hydrothermally treated boehmite (55.0 Bq / g) > silica gel (47.6 Bq / g) > commercial boehmite (42.0 Bq / g). These results suggest that the most important factor in tritium absorption capacity is the porous structure, and that a larger specific surface area is preferable. From these results, it is believed that a porous structure (having a specific range of pore size) is most important for tritium absorption and decontamination capacity, and that a larger specific surface area is preferable. Although silica gel is porous and has a large specific surface area, its tritium absorption capacity is relatively low. This is believed to be due to the relatively large pore size of the silica gel used, 60 Å.

[0070] On the other hand, the order of decontamination rate1 shown in Table 3 is zeolite (82.0%) > hydrothermally treated boehmite (77.6%) > γ-alumina (69.1%) > commercial boehmite (65.8%) > silica gel (63.6%). The decontamination rate is considered to depend on the difference in desorption property between H2O and HTO occluded in the pores in addition to the tritium absorption capacity. Under desorption conditions, when H2O occluded in the pores is more easily desorbed than HTO, the desorption of H2O proceeds preferentially, the proportion of HTO occluded in the pores becomes higher than H2O, and the proportion of HTO contained in the desorbed H2O becomes lower than the mixture of occluded H2O and HTO. As a result, HTO can be separated from H2O.

[0071] Whether HO occluded in the pores is more easily desorbed than HTO under desorption conditions can be evaluated by differential scanning calorimetry (DSC) of a porous material occluding HO or HTO. Note that HTO and DO are isotopes and both have the same mass number of 20, so the effect of mass (on physical adsorption and physical desorption) can be considered to be the same for HTO and DO.

[0072] Test Examples 1-2 DSC measurements are performed by placing a porous sample dried at 100°C in a desiccator with saturated vapor pressure at room temperature, and heating a 5 mg sample that has reached adsorption equilibrium at a heating rate of 10°C / min.

[0073] Figure 11 shows the results of DSC measurements at elevated temperatures after H2O or D2O was saturated and adsorbed at 60°C on a zeolite with a pore size of 7 Å (mordenite, HSZ-640). Figure 12 shows the results of DSC measurements at elevated temperatures after H2O or D2O was saturated and adsorbed at 60°C on column chromatography silica gel Wakosil C-200 (B type, pore size 60 Å). When A type silica gel (pore size 25 Å) was used, the results were almost the same as those in Figure 12 for B type silica gel (pore size 60 Å).

[0074] In the results of Figure 11, the endotherm due to the desorption (evaporation) of H2O and D2O starts at around 30°C, and the end temperatures are both around 120°C. However, the profiles of the endothermic peaks between them are clearly different. Comparing the temperatures of the endothermic peaks, H2O is 60°C and D2O is 73°C, a difference of more than 10°C. Therefore, it is presumed that decontamination at the temperature where the difference between the two lines is maximum (60°C) can maximize the H2O / D2O separation efficiency. In order to create a difference in the evaporation temperatures of H2O / D2O, the pore size of the porous adsorbent is important, and the pore size of 7Å for natural zeolite (mordenite) is considered to be important in terms of selective desorption of H2O from the pores at 60°C (if the diameter is too small, the evaporation temperature will be over 100°C and separation will not be possible, and if it is too large, selectivity will be lost). In addition, the endothermic profile of D2O from 30℃ to 80℃ (black line) clearly shows that evaporation is less likely to occur than that of H2O (gray line). This supports the idea that the interaction between D2O and the pores in the zeolite is greater than the interaction between H2O and the pores. In other words, this is presumably the key to the mechanism of H2O / D2O separation.

[0075] In the results of Figure 12, when comparing the endothermic peak temperatures, H2O is 87.5℃ and D2O is 90℃, which is slightly higher, but D2O is slightly more difficult to desorb. This suggests that silica gel also has a reasonable H2O / D2O separation effect. In the case of silica gel, the pore size is standardized to 25 Å for type A and 60 Å for type B (JIS Z 0701 Type 1 and JIS Z 0701 Type 2), both of which are more than four times larger than the pore size of natural zeolite. When the pore size is this large, condensation hardly occurs in the pores, and therefore no phase transition from gas to liquid occurs, reducing the difference in evaporation temperature, and it is thought that H2O / D2O separation is lower than that of natural zeolite. [Industrial Applicability]

[0076] The present invention is useful in the field of a method for decontaminating an aqueous solution containing tritium.

[0077] In particular, the average HTO concentration in tritium-contaminated water from the Fukushima nuclear accident is said to be about 1 MBq / L. TEPCO also releases groundwater pumped up through groundwater bypasses and sub-drains into the sea, with the standard value set at 1500 Bq / L in accordance with an agreement with the fishery association. To decontaminate contaminated water with a concentration of 1 MBq / L to a level of 1500 Bq / L requires a decontamination rate of 99.85% or more, but if the porous body is used in its current state, this can be achieved by stacking two or three sheets of porous body, which is useful in the field of tritium decontamination methods. [Explanation of symbols]

[0078] 10, 14 Reservoir, 11, 22 Thermocouples for temperature measurement, 12 Means for generating water vapor and / or mist; 12a, 15 Dry air inlet 13 Mantle heater 20, 23 storage means, 30, 31 Means for recovering HTO-containing aqueous solutions (cold traps); 40, 50, 60 means of transfer,

Claims

1. 1. A method for reducing a tritium (HTO) concentration in an aqueous solution containing HTO, comprising: The method includes continuously or intermittently contacting the water vapor and / or mist of an HTO-containing aqueous solution with an inorganic porous body, which is a powder-sintered porous body of aluminum having a boehmite coating and has pores with a pore size in the range of 10 Å to 500 Å, to selectively occlude the HTO from the HTO-containing aqueous solution into the inorganic porous body, and obtaining an HTO-containing aqueous solution having a reduced HTO concentration (hereinafter referred to as low-HTO-containing water) from the liquid that has not been occluded, the method comprising maintaining the inorganic porous body at a temperature of 40° C. or higher and 60° C. or lower and contacting the inorganic porous body with the water vapor and / or mist.

2. The inorganic porous body has a specific surface area of ​​5 to 250 m 2 The method of claim 1 , wherein the molecular weight is in the range of 1 / g.

3. The method according to any one of claims 1 to 2, wherein the temperature of the inorganic porous body with which the water vapor or mist of the HTO-containing aqueous solution is brought into contact is maintained at a temperature equal to or lower than an endothermic peak temperature based on desorption of the HTO occluded in the pores of the porous body during heating in differential scanning calorimetry.

4. The method according to any one of claims 1 to 3, wherein the water vapor and / or mist of the HTO-containing aqueous solution is supplied at a pressure in the range from atmospheric pressure to the saturated vapor pressure of the HTO-containing aqueous solution, and brought into contact with an inorganic porous body, thereby selectively adsorbing the HTO to the inorganic porous body, and the HTO-containing aqueous solution having a reduced HTO concentration (low HTO-containing water) is obtained by making the downstream side of the inorganic porous body under a more negative pressure than the supply side of the HTO-containing aqueous solution, thereby giving priority to the evaporation of light water from the surface of the inorganic porous body.

5. The method according to any one of claims 1 to 4, wherein the contact of the water vapor and / or mist of the HTO-containing aqueous solution with the inorganic porous body is carried out under reduced pressure.

6. The method according to any one of claims 1 to 5, wherein the inorganic porous body is composed of a plurality of inorganic porous bodies, and the water vapor and / or mist of the HTO-containing aqueous solution is contacted with the plurality of inorganic porous bodies in sequence.

7. The method according to claim 6, wherein the HTO-containing aqueous solution having a reduced HTO concentration obtained by contacting the inorganic porous body has a higher HTO concentration reduction rate as the number of porous bodies increases.

8. The method according to any one of claims 1 to 7, comprising recovering and storing the inorganic porous body having occluded a predetermined amount of HTO.

9. The method of claim 8 , further comprising releasing the occluded HTO from the recovered inorganic porous body and recovering the released HTO.

10. An apparatus for reducing an HTO concentration in a tritium-containing aqueous solution, comprising: a reservoir for the aqueous solution containing the raw HTO; means for generating water vapor and / or mist of the HTO-containing aqueous solution in said reservoir; An occlusion means storing an inorganic porous body, which is an aluminum powder sintered porous body having a boehmite coating and pores with a pore diameter in the range of 10 Å to 500 Å; Means for recovering HTO-containing aqueous solution with reduced HTO concentration and a transfer means for transferring the water vapor and / or mist to the storage means; and A means for transferring a gas containing HTO-containing water vapor with a reduced HTO concentration from the storage means to the recovery means. Including, The above-mentioned device, wherein the occlusion means is provided with a heater for maintaining the inorganic porous body at 40° C. or higher and 60° C. or lower to bring the inorganic porous body into contact with the water vapor and / or mist.

11. 11. The apparatus according to claim 10, wherein the porous inorganic body comprises a plurality of porous inorganic bodies, and the plurality of porous inorganic bodies are stored in multiple stages in the occlusion means.

12. The inorganic porous body has a specific surface area of ​​5 to 250 m 2 The device according to any one of claims 10 to 11, wherein the molecular weight is in the range of 1 / g.

13. An apparatus according to any one of claims 10 to 12, used for carrying out the method according to any one of claims 1 to 9.

14. The inorganic porous body is contacted with the water vapor and / or mist for 10 3 ~10 5 The method according to any one of claims 1 to 9, wherein the temperature is set to 0.1 Pa.

Citation Information

Patent Citations

  • Separation of tritium water, heavy water using zeolite

    JP1998128072A

  • Advanced tritium system and advanced permeation system for separation of tritium from radioactive wastes

    JP2017072599A

  • Decontamination of tritiated water

    JP2017504785A