Manufacturing method of brake disc rotor

The described method for manufacturing brake disc rotors using a viscous body of activated ceramics addresses high costs and thermal property challenges by eliminating high-temperature treatment, resulting in a cost-effective and thermally optimized rotor production process.

JP7591880B2Active Publication Date: 2024-11-29ADVICS CO LTD +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020113631
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-06-30
Publication Date
2024-11-29
Estimated Expiration
2040-06-30

AI Technical Summary

Technical Problem

Conventional brake disc rotors made of silicon-impregnated ceramic composites with short fibers like silicon carbide and carbon fibers face high manufacturing costs due to the need for a firing step and impregnation step, and the thermal properties are difficult to adjust.

Method used

A method involving the use of a viscous body containing activated ceramics, coated on a linear member, wound into a disk shape, and processed through alkali treatment, press forming, curing, and polishing to form a brake disc rotor without high-temperature heat treatment, using materials like graphite and alumina for improved thermal conductivity.

Benefits of technology

This method reduces manufacturing costs and ensures the production of a brake disc rotor with desired strength and thermal properties, while allowing for easier adjustment of thermal conductivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007591880000001
    Figure 0007591880000001
  • Figure 0007591880000002
    Figure 0007591880000002
  • Figure 0007591880000003
    Figure 0007591880000003
Patent Text Reader

Abstract

To enable easy manufacturing of a brake disc rotor having a desired strength and suppression of the manufacturing cost.SOLUTION: A brake disc rotor of an embodiment includes a linear member wound a few revolutions in a circumferential direction, and a non-burned ceramic covering the linear member and formed in a disc shape.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention Is, The present invention relates to a method for manufacturing a rake disc rotor. [Background technology]

[0002] 2. Description of the Related Art A known conventional brake disc rotor is made of a silicon-impregnated ceramic composite material using short fibers such as silicon carbide and carbon fibers as reinforcing fibers (see, for example, Patent Document 1).

[0003] The above-mentioned conventional method for manufacturing a brake disc rotor requires a firing step for obtaining a ceramic composite material from a ceramic precursor, and an impregnation step for impregnating the obtained ceramic composite material with metal silicon. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2019-156682 A Summary of the Invention [Problem to be solved by the invention]

[0005] In the above-mentioned conventional brake disc rotor, short fibers such as silicon carbide and carbon fibers are used as reinforcing fibers, which increases the manufacturing cost. In addition, the thermal properties required for brake disc rotors, such as thermal conductivity, are greatly affected by the dispersion state of the reinforcing fibers, but adjustments were not easy due to restrictions on the blending amount, etc.

[0006] Furthermore, in the manufacturing method of the brake disc rotor, in addition to the precursor molding step, it is necessary to provide a firing step and an impregnation step, each of which requires a heating step, which results in high manufacturing costs.

[0007] Therefore, the present invention is easy to manufacture and can reduce manufacturing costs. Nabu The object of the present invention is to provide a method for manufacturing a rake disc rotor. [Means for solving the problem]

[0012] A manufacturing method for a brake disc rotor according to an embodiment includes the steps of impregnating a linear member with a viscous body containing activated ceramics, which is a raw material for unsintered ceramics, and coating the surface of the linear member with the viscous body; winding the linear member coated with the viscous body into a disk shape to form a preform; alkali treating the preform; press-molding the preform; curing the press-molded preform to promote bonding of the activated ceramics in the preform; drying the preform after curing; and polishing the preform after drying. According to the above-mentioned configuration, a brake disc rotor having a desired strength can be reliably manufactured at low cost without high-temperature heat treatment. Furthermore, there is no particular restriction on the timing of the alkali treatment step as long as it is performed before press molding, and it may be performed at the stage of producing a viscous body containing activated ceramics.

[0013] In the above-mentioned configuration, a step of kneading one or more friction modifiers selected from graphite, silicon carbide, alumina, zirconium oxide, zirconium silicate, potassium titanate, barium sulfate, magnesium oxide, calcium silicate, barium sulfate, antimony sulfide, molybdenum sulfide, tin sulfide, iron sulfide, coke, zinc oxide, calcium carbonate, magnesium carbonate, iron powder, zinc powder, and tin powder, and activated ceramics to form a viscous body may be provided. According to the above-mentioned configuration, the viscous body can be easily obtained, and therefore the brake disc rotor can be easily manufactured. [Brief description of the drawings]

[0014] [Figure 1] FIG. 1 is an external front view of a brake disc rotor according to an embodiment. [Diagram 2]FIG. 2 is an explanatory diagram of the manufacturing process of the brake disc rotor. [Diagram 3] FIG. 3 is an explanatory diagram of the linear member after impregnation. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] Exemplary embodiments of the present invention will now be described in detail with reference to the drawings. The configurations of the embodiments shown below, and the actions and results (effects) brought about by the configurations are merely examples. The present invention can be realized by configurations other than those disclosed in the following embodiments. Furthermore, according to the present invention, it is possible to obtain at least one of the various effects (including derivative effects) obtained by the configurations.

[0016] FIG. 1 is an external front view of a brake disc rotor according to an embodiment. The brake disc rotor 10 includes a disc portion 11 having a linear member and a non-sintered ceramic friction member, and a hat member 12 provided around the rotation axis of the brake disc rotor 10.

[0017] In the following description, the direction of the rotation axis of the brake disc rotor 10 is referred to as the rotor axial direction, the radial direction of the brake disc rotor 10 is referred to as the rotor radial direction, and the circumferential direction of the brake disc rotor 10 is referred to as the rotor circumferential direction. The rotor circumferential direction intersects with the rotor radial direction.

[0018] The disk portion 11 includes a linear member, a non-sintered ceramic, and a friction modifier. In the disk portion 11, the linear member is used to ensure the strength of the brake disk rotor 10. The linear member is wound in the rotor circumferential direction as described below. The linear members are contained in the disk portion 11 at 5 to 10 vol %. The linear members are made of at least one of a material having high heat resistance and a material having high thermal conductivity, such as inorganic fibers or metal fibers as long fibers.

[0019] Examples of inorganic fibers include basalt fibers, alumina fibers, and silica fibers. Basalt fiber is obtained by melt extrusion (centrifugal) spinning of basalt (basalt rock), a type of igneous rock.

[0020] For example, the components of basalt fiber are as follows: SiO 2 (40-60%), Al 2 O 3 (10~20%), CaO (5~15%), MgO (5~15%), Fe+Fe 2 O 3 (5-15%), K 2 O(0-3%), Na 2 O(0-5%).

[0021] Examples of metal fibers include iron fibers and stainless steel fibers.

[0022] As an example of non-sintered ceramics, Fe 2+ , Fe 3+ , silica ion Si 4+ , aluminum ion Al 3+ The metal cations used are, for example, those firmly bonded to the surface of activated ceramic powder (surface-activated silica powder) made from silica powder as the raw material. The non-sintered ceramics is contained in the disk portion 11 in an amount of 40 to 60 vol %.

[0023] Examples of friction modifiers include graphite, silicon carbide, alumina, zirconium oxide, zirconium silicate, potassium titanate, barium sulfate, magnesium oxide, calcium silicate, barium sulfate, antimony sulfide, molybdenum sulfide, tin sulfide, iron sulfide, coke, zinc oxide, calcium carbonate, magnesium carbonate, iron powder, zinc powder, and tin powder. The friction modifier is contained in the disk portion 11 in an amount of 25 to 50 vol %.

[0024] FIG. 2 is an explanatory diagram of the manufacturing process of the brake disc rotor. Impregnation step (step S11) First, one or more types of linear members 22A to 22C are prepared and wound around bobbins 21A to 21C, respectively.

[0025] The activated ceramic powder, which is the raw material for the non-sintered ceramic as a binder, and the friction modifier are mixed uniformly to prepare an activated ceramic viscous body.

[0026] The content ratios of the linear members, activated ceramic powder, and friction modifier in the brake disc rotor are summarized as follows: Linear material: 5 to 10 vol% Activated ceramic powder: 40~60vol% (Binder): 5vol% or less Friction modifier: 25~50vol%

[0027] First, the activated ceramic powder constituting the activated ceramic viscous body will be described. The activated ceramic powder is a surface-active ceramic powder, and has an amorphous active layer whose surface has been mechanochemically amorphized.

[0028] The amorphous active layer is in a state where it is easily corroded by the alkaline aqueous solution in the alkaline treatment described below.

[0029] Activated ceramic powders are, for example, silica (SiO 2 The ceramic powder is obtained by activating the surface of the ceramic powder such as CrN 2 O 4 by mechanochemical treatment, for example, by grinding in a planetary ball mill for 15 minutes.

[0030] In order to achieve the above-mentioned mechanochemical action, it is effective to apply various forces such as impact, friction, compression, shear, etc. in combination. Specifically, in addition to the above-mentioned planetary ball mill, mixing devices such as a ball mill, a vibration mill, and a media stirring type mill, grinding machines such as a ball media mill, a roller mill, and a mortar may be used.

[0031] However, it is not necessary to apply all of the various forces such as impact, friction, compression, shear, etc. in a combined manner. For example, it is also possible to carry out mechanochemical processing using a jet grinder or the like which can apply forces such as impact and grinding to the material to be ground.

[0032] In carrying out the mechanochemical treatment, it is preferable to carry out the grinding until there is no change in particle size distribution with time. As a result, dissolution by an aqueous alkaline solution in the subsequent alkaline treatment proceeds more easily, and the resulting solidified ceramic body becomes dense and has high mechanical strength.

[0033] FIG. 3 is an explanatory diagram of the linear member after impregnation. On the other hand, a binder 41 is applied to the surface of each of the linear members 22A to 22C. In FIG. 3, the linear member 22A is illustrated as an example, but the same applies to the linear members 22B and 22C.

[0034] In this case, there is no need to use a specific binder 41 as long as the activated ceramic viscous body 42, and ultimately the activated ceramic powder and friction modifier, can be adhered and coated to a thickness of a predetermined thickness or more on the fibrous material constituting the linear member.

[0035] Then, the linear members 22A to 22C having the surfaces coated with the binder 41 are immersed in the activated ceramic viscous body to coat the surfaces of the linear members 22A to 22C with the activated ceramic viscous body 42 via the binder 41.

[0036] In FIG. 3, an activated ceramic viscous body 42 containing activated ceramic powder and a friction modifier is attached to the periphery of the linear member 22A with a binder interposed therebetween to a predetermined thickness or more. In this case, the predetermined thickness is, for example, approximately equal to or greater than the radius of the linear members 22A to 22C.

[0037] Drying process (step S12) Then, the activated ceramic viscous body 42 is dried as necessary so that the moisture content becomes suitable for the next step of winding. Therefore, if the moisture content is suitable for the next step of winding in the initial state, this drying step can be omitted.

[0038] Winding process (step S13) One or more fibers coated with activated ceramic viscous body 42 having a predetermined moisture content are wound up into a roughly disk-like shape having a hole in the center for forming a hole for attaching a hat component by a predetermined winding device WD, and then wound into a preliminary formed body 51.

[0039] Alkaline treatment / pressing process (step S14) The disk-shaped preform 51 is set in a hot press machine HPM, and an alkaline aqueous solution is added. Then, press molding is performed to allow the alkaline aqueous solution to permeate the entire preform 51. Generally, the molding temperature may be room temperature, but heating may be performed appropriately to promote molding.

[0040] This alkali treatment / pressing process causes the amorphous active layer to dissolve and undergo dehydration and condensation, which causes it to begin to solidify.

[0041] In this case, the iron ions Fe contained in the amorphous active layer 2+ , Fe3+ , silica ion Si 4+ , aluminum ion Al 3+ The metal cations such as these are in a state where they are likely to form ionic bonds with, for example, hydroxyl groups (OH groups) and silanol groups (Si-OH groups) contained in the amorphous active layer, which are likely to become negatively charged.

[0042] In this case, the press die is provided with protrusions for forming, during pressing, mounting holes (excluding bolt holes for fixing) into which the hat component is inserted. Therefore, by maintaining the pressed state for a predetermined time, it is possible to obtain a press-molded body that will become the disk portion 11 having an attachment hole formed therein for inserting the hat member.

[0043] Curing and drying process (Step S15) First, the press-molded body that will become the disk portion 11 is sealed and cured by being held at a predetermined temperature (for example, 80° C.) for a predetermined time (for example, 5 hours) or more.

[0044] Possible methods for curing press-molded bodies include a method in which each press-molded body is sealed and moistened, and a method in which multiple press-molded bodies are left in a furnace maintained at a specified humidity level (wet state) (batch processing). By carrying out the curing, it is possible to promote the bonding and solidification of the non-sintered ceramics, and in turn, it is possible to impart the desired strength to the disc portion 11 as the brake disc rotor main body.

[0045] Next, the sealed state is released and the container is dried at 100°C or less for a predetermined period of time. In this case, drying at a temperature below 100° C. is performed in order to prevent rapid evaporation of water, making it less likely for cracks to occur and maintaining the strength of the brake disc rotor.

[0046] Polishing process (step S16) After drying, the disk portion 11 where the non-fired ceramics has been bonded and solidified is deburred, and the disk portion 11 is polished by a polishing device so that it has a predetermined flatness and thickness.

[0047] Assembly process (step S17) Next, bolt holes for attaching the hat member are drilled using a drill, the hat member main body 12A is placed on one side of the brake disc rotor main body, the fastening ring member 12D is placed on the other side, and they are fitted together and fastened together with bolts 12B and nuts 12C to form the brake disc rotor 10.

[0048] As described above, according to the present embodiment, it is possible to provide a brake disc rotor that has a desired strength, can be easily manufactured, and can also reduce manufacturing costs, and a method for manufacturing a brake disc rotor.

[0049] In the above explanation, the alkaline aqueous solution is added in the alkaline treatment / pressing step, but it is also possible to carry out the alkaline treatment by mixing the alkaline powder in the impregnation step and adding water in the pressing step. Alternatively, it may be added in advance in the step of preparing the activated ceramic viscous body by uniformly mixing the activated ceramic powder and the friction modifier in step 11 described above.

[0050] In the above description, the bolt holes for attaching the hat member are formed by a drill. However, it is also possible to provide the press die with protrusions for forming the bolt holes. [Explanation of symbols]

[0051] 10...brake disc rotor, 11...disc portion, 12...hat member, 12A...hat member main body, 12B...bolt, 12C...nut, 12D...fastening ring member, 21A to 21C...bobbin, 22A to 22C...linear member, 41...binder, 42...activated ceramic viscous body, 51...preform, HPM...hot press machine, WD...winding device.

Claims

1. a step of impregnating the linear member with a viscous body containing activated ceramics, which is a raw material for the non-sintered ceramics, and coating the surface of the linear member with the viscous body; a step of winding the linear member coated with the viscous material into a disk shape to obtain a preform; subjecting the preform to an alkali treatment; A step of press-molding the preform; a curing step for promoting bonding of the activated ceramic in the press-formed preform; drying the preform after the curing; polishing the preform after drying; A method for manufacturing a brake disc rotor comprising:

2. The method includes a step of kneading one or more friction modifiers selected from graphite, silicon carbide, alumina, zirconium oxide, zirconium silicate, potassium titanate, barium sulfate, magnesium oxide, calcium silicate, barium sulfate, antimony sulfide, molybdenum sulfide, tin sulfide, iron sulfide, coke, zinc oxide, calcium carbonate, magnesium carbonate, iron powder, zinc powder, and tin powder with the activated ceramics to obtain the viscous body. The method for manufacturing the brake disc rotor according to claim 1 .

Citation Information

Patent Citations

  • Abrasive composition

    JP1981011981A

  • Melt-infiltrated fiber-reinforced composite ceramic

    JP2000512260A

  • Clutch facing

    JP2001065596A

  • Braking member and brake rotor

    JP2008069932A

  • Production method of silicon-impregnated ceramic composite, production method of friction plate, and production method of brake disc

    JP2019156682A