Composite absorbents and polymer absorbents
The composite absorbent with ion exchange groups in a polymer absorbent addresses the slow absorption rate and ion interference issues of SAPs, ensuring stable liquid absorption and retention by modifying the liquid before delivery to SAP.
Patent Information
- Application Number
- JP2020219823
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-29
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2040-12-29
AI Technical Summary
Conventional superabsorbent polymers (SAPs) have a slow liquid absorption rate and are adversely affected by divalent ions in liquids, leading to unstable absorption performance due to variations in salt concentration.
A composite absorbent comprising a polymer absorbent with hydrophilic continuous pores and ion exchange groups (-COOH and -COONa) that modifies the liquid to reduce the impact of divalent ions, ensuring stable absorption performance by quickly absorbing and temporarily retaining liquid before delivering it to SAP.
The composite absorbent stabilizes absorption performance by reducing the adverse effects of divalent ions, allowing for consistent liquid retention and absorption rates, even in the presence of ions.
Smart Images

Figure 0007591924000001 
Figure 0007591924000002 
Figure 0007591924000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a composite absorbent and a polymer absorbent. [Background technology]
[0002] 2. Description of the Related Art As an absorbent used for absorbing liquids such as aqueous solutions, there is known one that uses a superabsorbent polymer (so-called "SAP") having a high liquid absorption capacity. For example, as disclosed in Patent Documents 1 to 5, the present invention is applied to various fields, including disposable paper diapers, civil engineering and construction materials such as anti-condensation sheets and simple soil, base materials for pharmaceuticals, and materials for absorbing leaked liquids. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] International Publication No. 2013 / 018571 [Patent Document 2] JP 2017-36638 A [Patent Document 3] JP 2017-205225 A [Patent Document 4] Japanese Patent Application Publication No. 63-75016 [Patent Document 5] Japanese Patent Application Publication No. 8-38893 Summary of the Invention [Problem to be solved by the invention]
[0004] Although such superabsorbent polymers (SAPs) can retain large amounts of liquid (i.e., have high liquid retention capacity), they have a slow liquid absorption speed, and therefore in conventional absorbents, they are used in combination with pulp to enable temporary and quick liquid retention. In such conventional absorbents, when liquid is discharged, the liquid is quickly absorbed by the pulp in the absorbent and temporarily retained within the pulp, and then transferred to the SAP, which has high liquid retention capacity, and is retained within the SAP. On the other hand, the liquid to be absorbed by the absorbent generally contains a certain amount of ions, especially divalent ions (e.g., Ca 2+ , Mg 2+ Even a small amount of these substances can have a significant adverse effect on the absorption performance of SAP (particularly the amount of liquid absorbed, the amount of liquid retained, and the absorption speed). However, conventional absorbents do not have the function to modify the salt concentration in the liquid, so the liquid temporarily held within the pulp is passed on to the SAP in its original state. This causes variations in the absorption performance of the SAP due to the influence of the salt concentration in the liquid (especially the concentration of divalent ions), and as a result, there is a risk that the absorption performance of the absorbent will not be stable.
[0005] The present invention has been made in consideration of such problems, and has an object to provide an absorbent body that can stably exhibit absorption performance. [Means for solving the problem]
[0006] One aspect of the present invention (Aspect 1) is a composite absorbent for absorbing liquid, comprising: The composite absorbent body includes a polymer absorbent having a hydrophilic continuous skeleton and continuous pores, and a superabsorbent polymer; The polymer absorbent is characterized in that it contains at least -COOH groups and -COONa groups as ion exchange groups, and that the total ion exchange capacity of the -COOH groups and -COONa groups per mass in a dry state is 4.0 mg equivalent / g or more.
[0007] In the composite absorbent of this embodiment, the polymer absorbent has a hydrophilic continuous skeleton and continuous pores, so that it can quickly absorb and temporarily retain liquid. Furthermore, since it contains a certain amount or more of -COOH groups and -COONa groups, which are ion exchange groups, when the polymer absorbent absorbs and temporarily retains liquid, the ions in the liquid (especially Ca 2+ , Mg 2+By exchanging divalent ions (such as -COOH groups and -COONa groups) with -COOH groups and -COONa groups, the liquid can be modified to one that is less likely to adversely affect the absorption performance (particularly the liquid absorption capacity, liquid retention capacity, and absorption speed) of the superabsorbent polymer (SAP). As a result, in the composite absorbent of this embodiment, the liquid is modified with the polymer absorbent before being handed over to the SAP, so that variation in the absorption performance of the SAP is less likely to occur and the absorbent can stably exhibit its absorption performance as an absorbent.
[0008] In another aspect (aspect 2) of the present invention, in the composite absorbent of aspect 1, the polymer absorbent has an ion exchange rate of polyvalent ions of 50% or more.
[0009] The composite absorbent of this embodiment has an ion exchange rate of 50% or more for the polyvalent ions (ions with a valence of two or more) of the polymer absorbent, and can modify the liquid more reliably, thereby making it possible to reduce variation in the absorption performance of the SAP and to more stably exhibit the absorption performance as an absorbent.
[0010] In still another aspect (aspect 3) of the present invention, in the composite absorbent of aspect 1 or 2 above, the polymer absorbent has a liquid absorption capacity per unit mass of 30 g / g or more.
[0011] In the composite absorbent of this embodiment, the polymer absorbent has a certain or greater liquid absorption capacity and can absorb more liquid and steadily modify it, making it possible to reduce variation in the absorption performance of the SAP and to more stably exhibit the absorption performance of the absorbent.
[0012] In yet another aspect (Aspect 4) of the present invention, in the composite absorbent of any of Aspects 1 to 3 above, the polymer absorbent is characterized in that the porosity per unit volume of the polymer absorbent is 85% or more.
[0013] In the composite absorbent of this embodiment, the polymer absorbent has a certain level of porosity or more, and can absorb more liquid and steadily improve its properties, making it less likely that the absorption performance of the SAP will vary, and the absorbent can exhibit its absorption performance as an absorbent more stably and effectively.
[0014] In still another aspect (aspect 5) of the present invention, in the composite absorbent of any one of the above aspects 1 to 4, the polymer absorbent is characterized in that the average diameter of the interconnected pores is 1 μm to 1000 μm.
[0015] In the composite absorbent of this embodiment, since the average diameter of the interconnected pores of the polymer absorbent is within the above-mentioned specific range, the spaces (pores) for absorbing liquid in the polymer absorbent are less likely to collapse, and the composite absorbent can have a higher absorption rate and stably exhibit excellent absorption performance. In particular, when the porosity per unit volume of the polymer absorbent is 85% or more and the average diameter of the continuous pores is 1 μm to 1000 μm, there is an advantage that more pores can absorb and modify the liquid, thereby achieving better ion exchange efficiency.
[0016] In still another aspect (aspect 6) of the present invention, in the composite absorbent of any one of aspects 1 to 5 above, the polymer absorbent is a monolithic absorbent.
[0017] In the composite absorbent of this embodiment, the polymer absorbent is a monolithic absorbent, which is capable of absorbing liquid quickly and more reliably transferring the temporarily held liquid to the SAP, thereby enabling the composite absorbent to stably exhibit even more excellent absorption performance.
[0018] In yet another aspect (Aspect 7) of the present invention, in the composite absorbent of any of Aspects 1 to 6 above, the polymer absorbent is a hydrolysate of a cross-linked polymer of a (meth)acrylic acid ester and a compound containing two or more vinyl groups in one molecule.
[0019] In the composite absorbent of this embodiment, since the polymer absorbent has the above-mentioned specific configuration, when absorbing liquid, the hydrophilic continuous skeleton is easily extended and the continuous pores are easily expanded, so that a larger amount of liquid can be taken up into the continuous pores more quickly, thereby enabling the absorbent to exhibit even higher absorption performance and steadily modify a larger amount of liquid, thereby making it even less likely that variation in the absorption performance of the SAP will occur.
[0020] In yet another aspect (Aspect 8) of the present invention, in the composite absorbent of any of Aspects 1 to 7 above, the superabsorbent polymer is an acrylic acid-based superabsorbent polymer having cations present on the surface.
[0021] Acrylic acid-based superabsorbent polymers (SAP) that have cations on their surface are particularly susceptible to adverse effects of ions in liquid on their absorption performance (particularly, the amount of liquid absorbed, the amount of liquid retained, and the absorption speed). However, even when the composite absorbent of this embodiment contains such SAP, when the polymer absorbent absorbs and temporarily retains the liquid, the ions in the liquid are ion-exchanged with -COOH groups and -COONa groups, thereby modifying the liquid, thereby making it less likely for the absorption performance of the SAP to vary, and the absorbent can stably exhibit its absorption performance as an absorbent.
[0022] Further, yet another aspect (aspect 9) of the present invention is a polymer absorbent used together with a superabsorbent polymer, It has a hydrophilic continuous skeleton and continuous pores, The polymeric absorbent contains at least -COOH groups and -COONa groups as ion exchange groups, and is characterized in that the total ion exchange capacity of the -COOH groups and -COONa groups per mass in a dry state is 4.0 mg equivalent / g or more.
[0023] The polymer absorbent of this embodiment has a hydrophilic continuous skeleton and continuous pores, and thus can quickly absorb and temporarily retain liquid. Furthermore, since it contains a certain amount or more of -COOH groups and -COONa groups, which are ion exchange groups, when the polymer absorbent absorbs and temporarily retains liquid, it can absorb and retain ions (especially Ca 2+ , Mg 2+ By exchanging divalent ions (such as -COOH groups and -COONa groups) with -COOH groups and -COONa groups, the liquid can be modified to one that is less likely to adversely affect the absorption performance (particularly the liquid absorption capacity, liquid retention capacity, and absorption speed) of the superabsorbent polymer (SAP). As a result, the polymer absorbent of this embodiment is delivered to the SAP after the liquid has been modified by the polymer absorbent, so that the absorption performance of the SAP is less likely to vary, and the absorption performance of the absorbent as an absorbent can be stably exhibited. Effect of the Invention
[0024] The present invention can provide an absorbent body that can stably exhibit absorption performance. [Brief description of the drawings]
[0025] [Figure 1] FIG. 1 is an exploded perspective view of a composite absorbent body 1 according to one embodiment of the present invention. [Diagram 2] FIG. 2 is an exploded perspective view of a composite absorbent body 1' according to another embodiment of the present invention. [Diagram 3] FIG. 3 is a diagram illustrating a manufacturing process of absorbent A, which is an example of a polymer absorbent. [Figure 4] FIG. 4 is an SEM photograph of absorbent A at a magnification of 50 times. [Diagram 5] FIG. 5 is a SEM photograph of absorbent A at a magnification of 100 times. [Figure 6] FIG. 6 is an SEM photograph of absorbent A at a magnification of 500 times. [Figure 7] FIG. 7 is a SEM photograph of absorbent A at a magnification of 1000 times. [Figure 8] FIG. 8 is an SEM photograph of absorbent A at a magnification of 1500 times. [Figure 9] FIG. 9 is a graph showing the relationship between the monovalent and divalent ion concentrations in a liquid and the absorption performance (liquid absorption amount, liquid retention amount, and absorption speed) of SAP. [Figure 10] FIG. 10 is a graph showing the effect of absorbent A, which is an example of a polymer absorbent, on the divalent ion concentration in a liquid. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0026] A preferred embodiment of the present invention will be described in detail below using a composite absorbent body 1 as one embodiment. In this specification, unless otherwise specified, "planar view" simply means "viewing an object (e.g., a composite absorbent body) placed on a horizontal surface in an unfolded state in the thickness direction of the object from above in the vertical direction."
[0027] [Composite absorber] FIG. 1 is an exploded perspective view of a composite absorbent body 1 according to one embodiment of the present invention. The composite absorbent 1 shown in FIG. 1 has a generally rectangular outer shape in a plan view, and basically comprises a first retention sheet 2 forming one surface of the composite absorbent 1 in the thickness direction, a second retention sheet 3 forming the other surface of the composite absorbent 1, and a liquid-absorbent member located between these sheets and consisting of a mixture of a polymer absorbent 4 and a superabsorbent polymer 5 (SAP).
[0028] The liquid-absorbent member in the composite absorbent body 1 is configured to absorb and retain liquid that has permeated through the first retaining sheet 2, using a polymer absorbent 4 and a highly absorbent polymer 5 that are located between the first retaining sheet 2 and the second retaining sheet 3 and have a hydrophilic continuous skeleton and continuous pores.
[0029] Furthermore, the above-mentioned polymeric absorbent contains at least -COOH groups and -COONa groups as ion exchange groups, and has a unique ion exchange ability in which the total ion exchange capacity of -COOH groups and -COONa groups per mass in a dry state is 4.0 mg equivalent / g or more.
[0030] The composite absorbent 4 can quickly absorb and temporarily hold liquid because the polymer absorbent has a hydrophilic continuous skeleton and continuous pores. Furthermore, because the polymer absorbent contains a certain amount or more of -COOH groups and -COONa groups, which are ion exchange groups, when the polymer absorbent absorbs and temporarily holds liquid, the ions in the liquid (especially Ca 2+ , Mg 2+ By exchanging the -COOH group and -COONa group with the -COOH group, the liquid can be modified to one that does not adversely affect the absorption performance of the SAP (particularly the amount of liquid absorbed, the amount of liquid held, and the absorption speed). As a result, the composite absorbent 4 can transfer the liquid to the SAP after modifying it with the polymer absorbent, so that the absorption performance of the SAP is less likely to vary and the absorbent can stably exhibit its absorption performance as an absorbent.
[0031] In the present invention, the absorbent member is not limited to the form of the composite absorbent 1 in the above-mentioned embodiment, and the absorbent member may or may not contain other absorbent materials as long as it contains at least a polymer absorbent exhibiting the above-mentioned specific absorbent behavior and SAP.
[0032] Furthermore, in the present invention, the configuration of the composite absorbent is not limited to the form of the composite absorbent 1 of the above-mentioned embodiment, and the composite absorbent may have, for example, a hydrophilic fiber sheet 6 located between the first retention sheet 2 and the liquid-absorbent member (i.e., the polymer absorbent 4 and the highly absorbent polymer 5), as in a composite absorbent 1' of another embodiment of the present invention shown in Figure 2.
[0033] In the present invention, the outer shape, various dimensions, basis weight, etc. of the composite absorbent body are not particularly limited as long as they do not impair the effects of the present invention, and any outer shape (e.g., circular, elliptical, polygonal, hourglass, design shape, etc.), various dimensions, basis weight, etc. can be adopted according to various applications and usage modes, etc.
[0034] Various constituent members of the composite absorbent body of the present invention will be described in further detail below, taking as an example the composite absorbent body 1 of the embodiment shown in FIG.
[0035] (Retaining sheet) 1, a first retention sheet 2 forming one surface of the composite absorbent body 1 has a substantially rectangular outer shape in a plan view similar to the outer shape of the composite absorbent body 1. The first retention sheet 2 is formed of a liquid-permeable sheet-like member that allows liquid supplied to the composite absorbent body 1 to pass therethrough and be absorbed and retained in the liquid-absorbent member on the inside.
[0036] The first retaining sheet 2 has an overall size that is slightly larger than the absorbent member located on the inside (i.e., compared to the area in which absorbent materials such as polymer absorbent 4 are located), and is joined at its peripheral portion to the second retaining sheet 3 located on the other side of the composite absorbent 1 in the thickness direction by any adhesive or heat sealing means, etc.
[0037] On the other hand, the second retention sheet 3 forming the other surface of the composite absorbent body 1 has a substantially rectangular outer shape in a plan view similar to the outer shape of the composite absorbent body 1. The second retention sheet 3 is made of a liquid-impermeable sheet-like member that prevents liquid that has not been absorbed and retained in the inner liquid-absorbent member and liquid that has seeped out from the liquid-absorbent member from leaking out to the outside of the composite absorbent body 1.
[0038] In the present invention, the sheet-like members usable as the first and second retaining sheets are not limited to those in the above-mentioned embodiments, and the composite absorbent of the present invention may be any one of the first and second retaining sheets formed from a liquid-permeable sheet-like member. That is, the composite absorbent of the present invention may be any one of the first and second retaining sheets formed from a liquid-impermeable sheet-like member.
[0039] When a liquid-permeable sheet-like member is used as the holding sheet, the liquid-permeable sheet-like member is not particularly limited as long as it does not impair the effects of the present invention, and any liquid-permeable sheet-like member can be used according to various applications, usage modes, etc. Examples of such liquid-permeable sheet-like members include hydrophilic nonwoven fabrics such as air-through nonwoven fabrics, spunbond nonwoven fabrics, and point-bond nonwoven fabrics, woven fabrics, knitted fabrics, and porous resin films.
[0040] Furthermore, when hydrophilic nonwoven fabrics, woven fabrics, knitted fabrics, etc. (hereinafter collectively referred to as "fiber sheets") are used as the liquid-permeable sheet-like member, these fiber sheets may have a single-layer structure or a multi-layer structure of two or more layers. The type of fiber constituting such a fiber sheet is not particularly limited, and examples thereof include hydrophilic fibers such as cellulosic fibers and thermoplastic resin fibers that have been subjected to a hydrophilization treatment. These fibers may be used alone or in combination of two or more types of fibers.
[0041] Examples of cellulose-based fibers that can be used as constituent fibers of the fiber sheet include natural cellulose fibers (e.g., plant fibers such as cotton), regenerated cellulose fibers, refined cellulose fibers, and semi-synthetic cellulose fibers. Examples of thermoplastic resin fibers that can be used as constituent fibers of the fiber sheet include fibers made of known thermoplastic resins such as olefin resins such as polyethylene (PE) and polypropylene (PP), polyester resins such as polyethylene terephthalate (PET), and polyamide resins such as 6-nylon. These resins may be used alone or in combination of two or more types.
[0042] In addition, when a liquid-impermeable sheet-like member is used as the holding sheet, the liquid-impermeable sheet-like member is not particularly limited as long as it does not impair the effects of the present invention, and any liquid-impermeable sheet-like member can be adopted according to various applications and usage modes, etc. Examples of such liquid-impermeable sheet-like members include hydrophobic nonwoven fabrics formed from any hydrophobic thermoplastic resin fibers (for example, polyolefin fibers such as PE and PP, polyester fibers such as PET, various composite fibers such as core-sheath type, etc.); porous or nonporous resin films formed from hydrophobic thermoplastic resins such as PE and PP; laminates in which a nonwoven fabric is bonded to the resin film; laminated nonwoven fabrics such as SMS nonwoven fabrics, etc.
[0043] In the present invention, the external shape, various dimensions, basis weight, etc. of the retaining sheet are not particularly limited as long as they do not impair the effects of the present invention, and any external shape (e.g., circular, oval, polygonal, hourglass, design shape, etc.), various dimensions, basis weight, etc. can be adopted according to various applications and usage modes, etc.
[0044] (Liquid-absorbent member) In the composite absorbent 1 shown in Figure 1, the liquid-absorbent member is configured to absorb and retain liquid that has permeated through the first retaining sheet 2 by using a polymer absorbent 4 having a hydrophilic continuous skeleton and continuous pores and a superabsorbent polymer 5, which are located between the first retaining sheet 2 and the second retaining sheet 3 as described above.
[0045] In the composite absorbent 1, the polymer absorbent 4 and the highly absorbent polymer 5 of the liquid-absorbent member are bonded to each of the above-mentioned first retaining sheet 2 and second retaining sheet 3 by any adhesive such as a hot melt adhesive, but in the composite absorbent of the present invention, the polymer absorbent does not have to be bonded to the retaining sheet.
[0046] In the present invention, the liquid-absorbent member contains, as essential components, a polymer absorbent having the above-mentioned specific ion exchange ability with a hydrophilic continuous skeleton and continuous pores, and a superabsorbent polymer. The polymer absorbent will be described later, and the superabsorbent polymer is a powder or granular material made of a highly absorbent polymer such as a sodium acrylate copolymer known in the art, and is called SAP (Super Absorbent Polymer).
[0047] The specific type of superabsorbent polymer (SAP) is not particularly limited, but for example, an acrylic acid-based SAP with cations present on the surface can be suitably used. Such acrylic acid-based SAP with cations present on the surface is particularly susceptible to adverse effects of ions in the liquid on its absorption performance (particularly, the amount of liquid absorbed, the amount of liquid retained, and the absorption speed). However, even when the composite absorbent 4 contains such an SAP, when the polymer absorbent absorbs and temporarily retains the liquid, the ions in the liquid are ion-exchanged with -COOH groups and -COONa groups, and the liquid is modified. This makes it difficult for the absorption performance of the SAP to vary, and the absorbent can stably exhibit its absorption performance as an absorbent.
[0048] In the present invention, the liquid-absorbent member located between the first and second holding sheets may contain only the above-mentioned polymer absorbent and SAP as the liquid-absorbent material, or may further contain other liquid-absorbent materials known in the art. Examples of such liquid-absorbent materials include hydrophilic fibers, and more specifically, pulp fibers (e.g., ground pulp, etc.), cotton, rayon, acetate, and other cellulosic fibers.
[0049] In the present invention, the outer shape (planar shape of the area where the absorbent material is arranged), various dimensions, basis weight, etc. of the absorbent member are not particularly limited as long as they do not impair the effects of the present invention, and any outer shape, various dimensions, basis weight, etc. can be adopted depending on the desired absorbency, flexibility, strength, etc.
[0050] (hydrophilic fiber sheet) In the present invention, the composite absorbent may have a hydrophilic fiber sheet 6 between the first retention sheet 2 and the liquid-absorbent member (i.e., the polymer absorbent 4 and the highly absorbent polymer 5), for example, as in another embodiment of the composite absorbent 1' shown in Figure 2.
[0051] In the present invention, the hydrophilic fiber sheet that can be used in the composite absorbent is not particularly limited as long as it does not impair the effects of the present invention, and any hydrophilic fiber sheet can be used depending on various applications and usage modes. Examples of such hydrophilic fiber sheets include nonwoven fabrics, woven fabrics, knitted fabrics, etc. that have hydrophilicity. The hydrophilic fiber sheet may have a single-layer structure or a multi-layer structure of two or more layers.
[0052] The type of the constituent fiber of such a hydrophilic fiber sheet is not particularly limited, and examples thereof include hydrophilic fibers such as cellulosic fibers and thermoplastic resin fibers that have been subjected to a hydrophilic treatment. These fibers may be used alone or in combination of two or more types of fibers. Furthermore, examples of cellulose-based fibers that can be used as constituent fibers of the hydrophilic fiber sheet include natural cellulose fibers (e.g., plant fibers such as cotton), regenerated cellulose fibers, refined cellulose fibers, and semi-synthetic cellulose fibers. Examples of thermoplastic resin fibers that can be used as constituent fibers of the hydrophilic fiber sheet include fibers made of known thermoplastic resins such as olefin resins such as PE and PP, polyester resins such as PET, and polyamide resins such as 6-nylon. These resins may be used alone or in combination of two or more types.
[0053] In the present invention, the outer shape, various dimensions, basis weight, etc. of the hydrophilic fibrous sheet are not particularly limited as long as they do not impair the effects of the present invention, and any outer shape, various dimensions, basis weight, etc. can be adopted according to various applications, usage modes, etc.
[0054] The polymer absorbent used in the composite absorbent of the present invention will be described in more detail below. [Polymer absorbent] In the present invention, the polymer absorbent is not particularly limited as long as it has a hydrophilic continuous skeleton and continuous pores, contains at least -COOH groups and -COONa groups as ion exchange groups, and has a unique ion exchange capacity of 4.0 mg equivalent / g or more per mass in a dry state. Such a polymer absorbent is, for example, a hydrolyzate of a crosslinked polymer of two or more monomers containing at least (meth)acrylic acid ester, and has at least one hydrophilic group in the functional group. More specifically, a polymer compound is a hydrolyzate of a crosslinked polymer of a compound containing two or more vinyl groups in one molecule, and has at least -COOH groups and -COONa groups. Such a polymer absorbent is an organic porous body having at least one or more -COONa groups in one molecule, and further has -COOH groups. In the skeleton of the porous body, -COONa groups are distributed almost uniformly.
[0055] If the polymer absorbent is a hydrolysate of a crosslinked polymer of such a (meth)acrylic acid ester and a compound containing two or more vinyl groups in one molecule, as described below, the continuous hydrophilic skeleton is more likely to extend (i.e., expand) when absorbing a liquid such as an aqueous solution, and the continuous pores are more likely to expand, so that a larger amount of liquid can be more quickly incorporated into the continuous pores. This allows a composite absorbent containing such a polymer absorbent to exhibit even higher absorption performance as an absorbent, steadily modify a larger amount of liquid, and further reduce variation in the absorption performance of the SAP.
[0056] In this specification, the (meth)acrylic acid ester refers to an acrylic acid ester or a methacrylic acid ester.
[0057] In the polymer absorbent formed by the hydrolysis product of such a cross-linked polymer of (meth)acrylic acid ester and divinylbenzene, a hydrophilic continuous skeleton is formed by an organic polymer having at least -COONa groups and -COOH groups, and the skeleton has interconnected pores (interconnected pores) that serve as liquid absorption fields. In addition, since the hydrolysis treatment converts the -COOR groups (that is, carboxylate groups) of the crosslinked polymer into -COONa groups or -COOH groups (see FIG. 3), the polymer absorbent may have -COOR groups.
[0058] The presence of -COOH groups and -COONa groups in the organic polymer that forms a hydrophilic continuous skeleton and the total ion exchange capacity of -COOH groups and -COONa groups per mass in a dry state can be confirmed by analysis using infrared spectroscopy and a method for quantifying weakly acidic ion exchange groups.
[0059] Here, Fig. 3 is a diagram for explaining the manufacturing process of absorbent A, which is an example of a polymer absorbent. In this Fig. 3, the upper diagram shows the constituent raw materials for polymerization, the middle diagram shows monolith A, which is a crosslinked polymer of (meth)acrylic acid ester and divinylbenzene, and the lower diagram shows absorbent A obtained by subjecting monolith A in the middle diagram to hydrolysis and drying treatment.
[0060] Hereinafter, an explanation will be given using absorbent A, which is an example of a polymer absorbent and is formed from a hydrolysate of a crosslinked polymer of a (meth)acrylic acid ester and divinylbenzene.
[0061] The polymer absorbent is not limited to the absorbent A, but may be a hydrolysate of a cross-linked polymer of a (meth)acrylic acid ester and a compound having two or more vinyl groups in one molecule, or a hydrolysate of a cross-linked polymer of two or more monomers including at least a (meth)acrylic acid ester. However, when the polymer absorbent is a monolithic absorbent, it is possible to quickly absorb liquid and more reliably transfer the liquid temporarily held in the polymer absorbent to the SAP, so that a composite absorbent containing such a polymer absorbent can stably exhibit even more excellent absorption performance.
[0062] In the following description, "Monolith A" refers to an organic porous material consisting of a crosslinked polymer of (meth)acrylic acid ester and divinylbenzene before hydrolysis treatment, and may be referred to as a "monolithic organic porous material." In addition, "absorbent A" is a hydrolyzate of a crosslinked polymer (monolith A) of (meth)acrylic acid ester and divinylbenzene after hydrolysis and drying. In the following description, absorbent A refers to the absorbent in a dry state.
[0063] First, the structure of absorbent A will be described. As described above, absorbent A has a hydrophilic continuous skeleton and continuous pores. As shown in Fig. 3, absorbent A, which is an organic polymer having a hydrophilic continuous skeleton, is obtained by cross-linking polymerizing (meth)acrylic acid ester, which is a polymerization monomer, and divinylbenzene, which is a cross-linking monomer, and further hydrolyzing the obtained cross-linked polymer (monolith A).
[0064] The organic polymer that forms a hydrophilic continuous skeleton has, as structural units, a polymerized residue of an ethylene group (hereinafter referred to as "structural unit X") and a cross-linked polymerized residue of divinylbenzene (hereinafter referred to as "structural unit Y"). Furthermore, the polymerized residue of the ethylene group (structural unit X) in the organic polymer forming the hydrophilic continuous skeleton has both a -COOH group and a -COONa group generated by hydrolysis of the carboxylate group. When the polymerized monomer is a (meth)acrylic acid ester, the polymerized residue of the ethylene group (structural unit X) has a -COONa group, a -COOH group, and an ester group.
[0065] In the absorbent A, the ratio of the crosslinked polymer residue of divinylbenzene (structural unit Y) in the organic polymer forming the hydrophilic continuous skeleton is, for example, 0.1 to 30 mol %, preferably 0.1 to 20 mol %, based on the total structural units. For example, in the absorbent A in which butyl methacrylate is used as the polymerization monomer and divinylbenzene is used as the crosslinked monomer, the ratio of the crosslinked polymer residue of divinylbenzene (structural unit Y) in the organic polymer forming the hydrophilic continuous skeleton is, for example, about 3 mol %, preferably 0.1 to 10 mol %, more preferably 0.3 to 8 mol %, based on the total structural units. Furthermore, when the ratio of cross-linked polymerized residues of divinylbenzene in the organic polymer forming the hydrophilic continuous skeleton is 0.1 mol % or more, the strength of absorbent A is less likely to decrease, and when the ratio of cross-linked polymerized residues of divinylbenzene is 30 mol % or less, the absorption amount of the liquid to be absorbed is less likely to decrease.
[0066] In addition, in the absorbent A, the organic polymer forming the hydrophilic continuous skeleton may be composed only of the structural unit X and the structural unit Y, or may have, in addition to the structural unit X and the structural unit Y, a structural unit other than the structural unit X and the structural unit Y, that is, a polymerized residue of a monomer other than a (meth)acrylic acid ester and divinylbenzene.
[0067] Examples of structural units other than the structural unit X and the structural unit Y include polymerized residues of monomers such as styrene, α-methylstyrene, vinyltoluene, vinylbenzyl chloride, glycidyl (meth)acrylate, isobutene, butadiene, isoprene, chloroprene, vinyl chloride, vinyl bromide, vinylidene chloride, tetrafluoroethylene, (meth)acrylonitrile, vinyl acetate, ethylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, and trimethylolpropane tri(meth)acrylate.
[0068] The proportion of structural units other than the structural unit X and the structural unit Y in the organic polymer that forms the hydrophilic continuous skeleton is, for example, 0 to 50 mol %, and preferably 0 to 30 mol %, relative to all structural units.
[0069] The thickness of the hydrophilic continuous skeleton of the absorbent A is preferably 0.1 to 100 μm. When the thickness of the hydrophilic continuous skeleton of the absorbent A is 0.1 μm or more, the spaces (pores) for absorbing liquid in the porous body are less likely to collapse during absorption, and the amount of absorbed liquid is less likely to decrease. On the other hand, when the thickness of the hydrophilic continuous skeleton is 100 μm or less, an excellent absorption speed is easily obtained.
[0070] In addition, since the pore structure of the hydrophilic continuous skeleton of absorbent A is an open-cell structure, the thickness of the continuous skeleton is measured by evaluating the cross section of the skeleton that appears on the test piece for electron microscope measurement. The continuous skeleton is often polygonal in shape because it is formed by the gaps between water (water droplets) removed by the dehydration and drying process after hydrolysis. Therefore, the thickness of the continuous skeleton is the average value of the diameter (μm) of the circle circumscribing the polygonal cross section. In rare cases, there may be small holes in the polygon, in which case the circumscribing circle of the polygonal cross section surrounding the small holes is measured.
[0071] Furthermore, the absorbent A preferably has an average diameter of interconnected pores of 1 μm to 1000 μm. When the average diameter of interconnected pores in the absorbent A is 1 μm or more, the spaces (pores) for absorbing liquid in the porous body are less likely to collapse during absorption, and the absorption rate is less likely to decrease. On the other hand, when the average diameter of interconnected pores is 1000 μm or less, an excellent absorption rate is easily obtained. Therefore, a composite absorbent including such an absorbent A can stably exhibit excellent absorption performance. In particular, when the porosity per unit volume of the polymer absorbent described below is 85% or more and the average diameter of the continuous pores is 1 μm to 1000 μm, there is an advantage that more pores can absorb and modify the liquid, thereby achieving better ion exchange efficiency.
[0072] The average diameter (μm) of the interconnected pores of absorbent A can be measured by mercury intrusion porosimetry, and the maximum value of the pore distribution curve obtained by the mercury intrusion porosimetry is used. Regardless of the ionic form of absorbent A, samples for measuring the average diameter of interconnected pores are those dried for 18 hours or more in a reduced pressure dryer set at a temperature of 50°C. The final pressure reached is 0 Torr.
[0073] Here, FIG. 4 is an SEM photograph of absorbent A at a magnification of 50 times, FIG. 5 is an SEM photograph of absorbent A at a magnification of 100 times, FIG. 6 is an SEM photograph of absorbent A at a magnification of 500 times, FIG. 7 is an SEM photograph of absorbent A at a magnification of 1000 times, and further, FIG. 8 is an SEM photograph of absorbent A at a magnification of 1500 times. The absorbents A shown in these Figs. 4 to 8 are examples of absorbents that use butyl methacrylate as a polymerization monomer and divinylbenzene as a cross-linking monomer, and each has a cubic structure with a side length of 2 mm.
[0074] 4 to 8 has a large number of cellular macropores and further has portions where these cellular macropores overlap. Absorbent A has an open cell structure in which the overlapping portions of the macropores form common openings (mesopores), i.e., it has an open cell structure (open macropore structure).
[0075] The overlapping portions of the macropores form common openings (mesopores) having an average diameter in a dry state of 1 to 1000 μm, preferably 10 to 200 μm, and particularly preferably 20 to 100 μm, and most of them have an open pore structure. When the average diameter of the mesopores in a dry state is 1 μm or more, the absorption rate of the liquid to be absorbed is improved. On the other hand, when the average diameter of the mesopores in a dry state is 1000 μm or less, the absorbent A is less likely to become embrittled. The number of overlapping macropores in each macropore is about 1 to 12, and in most cases, about 3 to 10.
[0076] In addition, since absorbent A has such an open cell structure, macropores and mesopores can be uniformly formed, and there is an advantage in that the pore volume and specific surface area can be significantly increased compared to the particle agglomeration type porous bodies as described in JP-A-8-252579 and the like.
[0077] The total pore volume of the pores (voids) of the absorbent A is preferably 0.5 to 50 mL / g, more preferably 2 to 30 mL / g. When the total pore volume of the absorbent A is 0.5 mL / g or more, the spaces (voids) for absorbing liquid in the porous body are less likely to collapse during absorption, and the amount of absorbed liquid and the absorption rate are less likely to decrease. On the other hand, when the total pore volume of the absorbent A is 50 mL / g or less, the strength of the absorbent A is less likely to decrease.
[0078] The total pore volume can be measured by mercury intrusion porosimetry. The sample for measuring the total pore volume is dried for 18 hours or more in a vacuum dryer set at a temperature of 50°C, regardless of the ion form of absorbent A. The final pressure is 0 Torr.
[0079] Hereinafter, the state when the absorbent A comes into contact with a liquid will be described, but the same applies to the case when a liquid comes into contact with a liquid-absorbent member or a composite absorbent body containing the absorbent A.
[0080] First, the continuous pores of the absorbent A shown in Figs. 4 to 8 are pores in which a plurality of pores (voids) are interconnected, and it is possible to visually confirm with the naked eye that a large number of voids are provided from the outside. When liquid comes into contact with the absorbent A having such a large number of voids, the hydrophilic continuous skeleton first instantly absorbs a portion of the liquid by osmotic pressure and expands (i.e., expands). This expansion of the continuous skeleton occurs in almost all directions. The size of each pore of the absorbent A increases as the external shape of the absorbent A increases due to the expansion of the continuous skeleton when absorbing liquid. When the size of the pores increases in this way, the volume of the pores increases, and the amount of liquid that can be retained in the pores also increases. The absorbent A, which has thus absorbed a certain amount of liquid and expanded, can further absorb a predetermined amount of liquid into the expanded pores by capillary action.
[0081] Furthermore, while the liquid absorbed into the hydrophilic continuous skeleton of absorbent A is not easily released from the continuous skeleton (i.e., it is not easily synergized), the liquid absorbed into the continuous pores is easily synergized. Therefore, within the composite absorbent, the liquid absorbed into the continuous pores synerges and is transferred to the SAP, which has a high liquid-retaining capacity, and is steadily retained within the SAP.
[0082] Furthermore, of the liquid absorbed by absorbent A, more remains in the pores than in the hydrophilic continuous framework. Most of the liquid absorption by absorbent A is achieved by retaining the liquid in the pores through capillary action, so the greater the porosity, which is the ratio of the volume of the pores (total pore volume) (i.e., the volume of the pores per unit volume of absorbent A), the more liquid it can absorb.
[0083] The porosity per unit volume of such a polymer absorbent is preferably 85% or more, more preferably 90% or more. When the porosity per unit volume of the polymer absorbent is 85% or more, it can absorb more liquid and steadily improve the properties, so that the variation in the absorption performance of the SAP can be more unlikely to occur. As a result, a composite absorbent containing such a polymer absorbent can exhibit the absorption performance as an absorbent more stably and well.
[0084] For example, when the porosity of the absorbent A shown in the above-mentioned Figs. 4 to 8 is calculated, it is as follows. First, the specific surface area of absorbent A obtained by mercury porosimetry is 400 m 2 / g, and the pore volume is 15.5 mL / g. This pore volume of 15.5 mL / g means that the volume of the pores in 1 g of absorbent A is 15.5 mL. Here, assuming that the specific gravity of absorbent A is 1 g / mL, the volume occupied by pores in 1 g of absorbent A, i.e., the pore volume, is 15.5 mL, and the volume of 1 g of absorbent A is 1 mL. In this case, the total volume (volume) of 1 g of absorbent A is 15.5 + 1 (mL), and the ratio of the pore volume to that is the porosity, so the porosity of absorbent A is 15.5 / (15.5 + 1) × 100 ≒ 94%.
[0085] In the present invention, the absorbent A having such a hydrophilic continuous skeleton and continuous pores, that is, the polymer absorbent, is applied to the composite absorbent in the form of, for example, particles or a sheet. Furthermore, as described above, this polymer absorbent contains at least -COOH groups and -COONa groups as ion exchange groups, and has a unique ion exchange ability in which the total ion exchange capacity of -COOH groups and -COONa groups per mass in a dry state is 4.0 mg equivalent / g or more. Therefore, when the polymer absorbent absorbs and temporarily retains a liquid, the ions in the liquid (especially Ca 2+ , Mg 2+By exchanging the ions (divalent ions such as dimethyl ether, divalent ions such as dimethyl ether, etc.) with -COOH groups and -COONa groups, the liquid can be modified to one that is less likely to adversely affect the absorption performance (particularly the amount of liquid absorbed, the amount of liquid retained, and the absorption speed) of the superabsorbent polymer (SAP). Therefore, a composite absorbent using such a polymer absorbent can transfer the liquid to the SAP after modifying it with the polymer absorbent, so that the absorption performance of the SAP is less likely to vary, and the absorbent can stably exhibit its absorption performance as an absorbent.
[0086] Here, FIG. 9 is a graph showing the relationship between the monovalent and divalent ion concentrations in a liquid and the absorption performance (liquid absorption amount, liquid retention amount, and absorption speed) of SAP, and FIG. 10 is a graph showing the effect of absorbent A, which is an example of a polymer absorbent, on the divalent ion concentration in a liquid.
[0087] As shown in Figure 9, the liquid absorption amount, liquid retention amount, and absorption speed of SAP all decrease as the concentration of monovalent and divalent ions in the liquid increases. In particular, the concentration of divalent ions has a large effect on the absorption performance of SAP, and even a small amount of ion significantly decreases the liquid absorption amount, liquid retention amount, and absorption speed of SAP.
[0088] As described above, the ion concentration in a liquid has a significant adverse effect on the absorption performance of SAP. However, since the ion concentration varies from liquid to liquid, the absorption performance of SAP also varies accordingly.
[0089] However, absorbent A, which is an example of the present invention, contains at least -COOH groups and -COONa groups as ion exchange groups, and has a unique ion exchange ability in which the total ion exchange capacity of -COOH groups and -COONa groups per mass in a dry state is 4.0 mg equivalent / g or more.Therefore, as shown in Figure 10, ions in the liquid (especially divalent ions) can be ion-exchanged with -COOH groups and -COONa groups, thereby significantly reducing the ion concentration in the liquid. In other words, the liquid can be modified to one that is less likely to have a negative effect on the absorption performance of SAP.
[0090] The graph shown in FIG. 10 shows the rate of change in ion concentration (i.e., the ion exchange rate of absorbent A) before and after contact of actual urine from three humans (actual urine A, B, and C) with different divalent ion concentrations with absorbent A, measured as follows. First, the divalent ion concentration (mEq / L) of each of the three actual urine samples A, B, and C is measured using an ion meter (HORIBA Compact Calcium Ion Meter LAQUAtwin-Ca-11, manufactured by HORIBA Advanced Techno Co., Ltd.). The measured ion concentration is defined as the ion concentration "before contact with absorbent A."
[0091] Next, 0.2 g of polymer absorbent (absorbent A) is placed in a glass filter (climbing glass filter, model number: 0777-01-101, outer diameter x foot length (mm): φ7 x 80, filter diameter: φ20 mm, capacity: 30 mL, material: borosilicate glass, pore size: 100 to 120 μm), 30 mL of the above-mentioned actual urine is poured, and the divalent ion concentration (mEq / L) of the obtained filtrate is measured using the above-mentioned ion meter. The measured ion concentration is defined as the ion concentration "after contact with absorbent A".
[0092] The change in ion concentration (mEq / L) before and after contact with absorbent A is calculated by subtracting the ion concentration after contact with absorbent A from the ion concentration before contact with absorbent A. Furthermore, the change in ion concentration (mEq / L) before and after contact with absorbent A is divided by the ion concentration before contact with absorbent A and multiplied by 100 to calculate the rate of change (%) in divalent ion concentration in each of the tested urine samples A, B, and C. All of the above measurements are carried out at a temperature of 25°C and a humidity of 60%.
[0093] As described above, absorbent A of the present invention has the above-mentioned unique ion exchange ability not found in conventional liquid-absorbent materials, and is capable of quickly absorbing liquid and temporarily retaining it, as well as exchanging ions (especially divalent ions) in the liquid to modify the liquid into one that is less likely to adversely affect the absorption performance of SAP. As a result, a composite absorbent containing such absorbent A (polymer absorbent) can be handed over to the SAP after modifying the liquid, which reduces variation in the absorption performance of the SAP and enables the absorbent to stably exhibit its absorption performance as an absorbent.
[0094] In the present invention, the total ion exchange capacity of -COOH groups and -COONa groups per mass of the polymer absorbent in a dry state is preferably 6.0 mg equivalent / g or more, and more preferably 8.0 mg equivalent / g or more.
[0095] In the present invention, the polymer absorbent preferably has an ion exchange rate of 50% or more for polyvalent ions (i.e., ions with a valence of 2 or more). When the ion exchange rate of the polyvalent ions of the polymer absorbent is 50% or more, the liquid can be modified more reliably, so that the variation in the absorption performance of the SAP can be prevented more reliably. Therefore, a composite absorbent containing such a polymer absorbent can more stably exhibit the absorption performance as an absorbent. The ion exchange rate of the polyvalent ions in the polymer absorbent is more preferably 60% or more, and even more preferably 70% or more. Here, the ion exchange rate of the polyvalent ions of the polymer absorbent can be measured by any measurement method such as ICP emission spectrometry, IC analysis, atomic absorption spectrometry, etc., but for example, the ion exchange rate of the divalent ions can be measured as follows.
[0096] <Method for measuring the ion exchange rate of divalent ions in polymeric absorbents> (1) Prepare artificial urine by dissolving 200 g of urea, 80 g of sodium chloride, 8 g of magnesium sulfate, 3 g of calcium chloride, and approximately 1 g of dye: Blue No. 1 in 10 L of ion-exchanged water. (2) The divalent ion concentration (mEq / L) of the prepared artificial urine is measured using an ion meter (HORIBA Compact Calcium Ion Meter LAQUAtwin-Ca-11, manufactured by HORIBA Advanced Techno Co., Ltd.). The measured ion concentration is defined as the "ion concentration before contact with the polymer absorbent." (3) 0.2 g of the polymer absorbent, which is a sample for measurement, is placed in a glass filter (climbing glass filter, model number: 0777-01-101, outer diameter x foot length (mm): φ7 x 80, filter diameter: φ20 mm, capacity: 30 mL, material: borosilicate glass, pore size: 100 to 120 μm), 30 mL of the above artificial urine is poured, and the divalent ion concentration (mEq / L) of the obtained filtrate is measured using the above ion meter. The measured ion concentration is defined as the "ion concentration after contact with the polymer absorbent." (4) The amount of change in ion concentration (mEq / L) before and after contact with the polymer absorbent is calculated by subtracting the ion concentration after contact with the polymer absorbent from the ion concentration before contact with the polymer absorbent, and the rate of change in divalent ion concentration (%) is calculated by dividing the amount of change in ion concentration (mEq / L) before and after contact with the polymer absorbent by the ion concentration before contact with the polymer absorbent and multiplying the result by 100. In this specification, this "rate of change in divalent ion concentration (%)" is referred to as the "divalent ion exchange rate of the polymer absorbent." All of the above measurements are carried out at a temperature of 25°C and a humidity of 60%.
[0097] In addition, when a measurement sample (polymer absorbent) is recovered from the product for use, it can be obtained according to the following <Method for recovering a measurement sample (polymer absorbent)>.
[0098] <How to collect the measurement sample (polymer absorbent)> (1) Peel off the top sheet etc. from the product to expose the absorbent core. (2) The object to be measured (polymer absorbent) is dropped from the exposed absorbent, and anything other than the (particulate) object to be measured (e.g., pulp, synthetic resin fibers, etc.) is removed using tweezers or the like. (3) A microscope or a simple magnifying glass is used as a magnifying observation means, and the measurement object is collected using tweezers or the like while observing at a magnification at which the difference from SAP can be recognized or at which the pores of the porous body can be visually recognized. The magnification of the simple magnifying glass is not particularly limited as long as the pores of the porous body can be visually recognized, and may be, for example, 25 to 50 times. (4) The objects to be measured thus collected are used as samples for measurement in various measurement methods.
[0099] Furthermore, in the present invention, the polymer absorbent preferably has a liquid absorption capacity per unit mass of 30 g / g or more. If the polymer absorbent has a certain amount of liquid absorption or more, it can absorb more liquid and steadily modify the liquid, making it less likely that the absorption performance of the SAP will vary. Therefore, a composite absorbent containing such a polymer absorbent can more stably exhibit the absorption performance of an absorbent. The liquid absorption amount per unit mass of the polymer absorbent is more preferably 40 g / g or more, and further preferably 50 g / g or more. Here, the liquid absorption amount per unit mass of the polymer absorbent can be measured as follows.
[0100] <Method for measuring the amount of liquid absorbed per unit mass of polymer absorbents> (1) 1 g of the measurement sample (polymer absorbent) is cut into a 10 cm square mesh bag (NBC Meshtec Co., Ltd., N-NO255HD 115 (standard width: 115 cm, 255 mesh / 2.54 cm, opening: 57 μm, wire diameter: 43 μm, thickness: 75 μm)) and enclosed. The mass (g) of the mesh bag is measured in advance. In addition, when the measurement sample (polymer absorbent) is to be recovered from the product and used, it can be obtained according to the above-mentioned <Recovery method of measurement sample (polymer absorbent)>. (2) The mesh bag containing the sample is immersed in a 0.9% sodium chloride solution for one hour. (3) Hang the mesh bag for 5 minutes and drain, then measure its mass (g). (4) The amount of liquid absorbed by the sample (g) is calculated by subtracting the total mass of the sample (= 1 g) and the mesh bag from the mass of the mesh bag after draining measured in (3) above, and this amount of liquid absorbed is further divided by the mass of the sample (= 1 g) to obtain the amount of liquid absorbed per unit mass of the sample (polymer absorbent) (g / g). All of the above measurement methods are carried out at a temperature of 25°C and a humidity of 60%.
[0101] Hereinafter, the method for producing such a polymer absorbent will be described in detail using the above-mentioned absorbent A as an example.
[0102] [Method of manufacturing polymer absorbent] The above-mentioned absorbent A can be obtained through a cross-linking polymerization step and a hydrolysis step, as shown in Fig. 3. Each of these steps will be described below.
[0103] (Crosslinking polymerization process) First, an oil-soluble monomer for crosslinking polymerization, a crosslinkable monomer, a surfactant, water, and optionally a polymerization initiator are mixed to obtain a water-in-oil emulsion, which is an emulsion in which the oil phase is the continuous phase and water droplets are dispersed within it.
[0104] In the above-mentioned absorbent A, as shown in the upper diagram of Figure 3, butyl methacrylate, which is a (meth)acrylic acid ester, is used as the oil-soluble monomer, divinylbenzene is used as the cross-linking monomer, sorbitan monooleate is used as the surfactant, and isobutyronitrile is used as the polymerization initiator to cause cross-linking polymerization to obtain monolith A.
[0105] Specifically, for absorbent A, as shown in the upper diagram of Figure 3, first, 9.2 g of t-butyl methacrylate as an oil-soluble monomer, 0.28 g of divinylbenzene as a cross-linking monomer, 1.0 g of sorbitan monooleate (hereinafter abbreviated as "SMO") as a surfactant, and 0.4 g of 2,2'-azobis(isobutyronitrile) as a polymerization initiator are mixed and dissolved uniformly. Next, the mixture of t-butyl methacrylate / divinylbenzene / SMO / 2,2'-azobis(isobutyronitrile) is added to 180 g of pure water and stirred under reduced pressure using a planetary stirring device, a vacuum stirring and degassing mixer (manufactured by EME), to obtain a water-in-oil emulsion.
[0106] Furthermore, this emulsion is quickly transferred to a reaction vessel, sealed, and polymerized at 60°C for 24 hours under stationary conditions. After the polymerization is completed, the contents are removed, extracted with methanol, and then dried under reduced pressure to obtain Monolith A, which has a continuous macropore structure. The internal structure of Monolith A was observed by SEM, and it was found that Monolith A had a continuous cell structure and the thickness of the continuous skeleton was 5.4 μm. The average diameter of the continuous pores measured by mercury intrusion porosimetry was 36.2 μm, and the total pore volume was 15.5 mL / g.
[0107] The content of divinylbenzene in the total monomers is preferably 0.3 to 10 mol%, more preferably 0.3 to 5 mol%. The ratio of divinylbenzene to the total of butyl methacrylate and divinylbenzene is preferably 0.1 to 10 mol%, more preferably 0.3 to 8 mol%. In the above-mentioned absorbent A, the ratio of butyl methacrylate to the total of butyl methacrylate and divinylbenzene is 97.0 mol%, and the ratio of divinylbenzene is 3.0 mol%.
[0108] The amount of surfactant added can be set depending on the type of oil-soluble monomer and the desired size of emulsion particles (macropores), and is preferably in the range of about 2 to 70% of the total amount of the oil-soluble monomer and surfactant.
[0109] In order to control the shape and size of the bubbles in Monolith A, alcohols such as methanol and stearyl alcohol; carboxylic acids such as stearic acid; hydrocarbons such as octane, dodecane, and toluene; cyclic ethers such as tetrahydrofuran and dioxane, etc. may be allowed to coexist in the polymerization system.
[0110] In addition, the mixing method for forming the water-in-oil emulsion is not particularly limited, and any mixing method can be used, such as a method of mixing all the components at once, or a method of separately and uniformly dissolving oil-soluble components such as the oil-soluble monomer, surfactant, and oil-soluble polymerization initiator, and water-soluble components such as water and the water-soluble polymerization initiator, and then mixing the respective components.
[0111] Furthermore, the mixing device for forming the emulsion is not particularly limited, and any device such as a normal mixer, homogenizer, or high-pressure homogenizer can be used depending on the desired emulsion particle size. Furthermore, a so-called planetary mixing device can also be used in which the material to be treated is placed in a mixing container and rotated while revolving around the revolution axis while tilting the mixing container, thereby stirring and mixing the material to be treated.
[0112] In addition, there are no particular limitations on the mixing conditions, and the stirring rotation speed, stirring time, etc. can be set as desired according to the desired emulsion particle size. Note that, with the above planetary stirring device, water droplets in the W / O emulsion can be uniformly generated, and the average diameter can be set as desired within a wide range.
[0113] The polymerization conditions for the water-in-oil emulsion can be various, depending on the type of monomer and initiator, etc. For example, when azobisisobutyronitrile, benzoyl peroxide, potassium persulfate, etc. are used as the polymerization initiator, the polymerization can be carried out by heating in a sealed container under an inert atmosphere at a temperature of 30 to 100°C for 1 to 48 hours, and when hydrogen peroxide-ferrous chloride, sodium persulfate-acidic sodium sulfite, etc. are used as the polymerization initiator, the polymerization can be carried out in a sealed container under an inert atmosphere at a temperature of 0 to 30°C for 1 to 48 hours.
[0114] After the polymerization is completed, the contents are taken out and subjected to Soxhlet extraction with a solvent such as isopropanol to remove unreacted monomers and residual surfactants, thereby obtaining monolith A shown in the center diagram of Figure 3.
[0115] (Hydrolysis process) Next, the step of hydrolyzing the monolith A (crosslinked polymer) to obtain the absorbent A (hydrolysis step) will be described.
[0116] First, monolith A is immersed in dichloroethane containing zinc bromide and stirred at 40° C. for 24 hours, then contacted with methanol, 4% hydrochloric acid, 4% aqueous sodium hydroxide solution, and water in that order to carry out hydrolysis, and then dried to obtain a block-shaped absorbent A. Furthermore, this block-shaped absorbent A is crushed to a predetermined size to obtain a particulate absorbent A. The form of this absorbent A is not limited to particulate, and for example, it may be formed into a sheet during or after drying.
[0117] In addition, the method of hydrolysis of monolith A is not particularly limited, and various methods can be adopted. For example, aromatic solvents such as toluene and xylene, halogen-based solvents such as chloroform and dichloroethane, ether-based solvents such as tetrahydrofuran and isopropyl ether, amide-based solvents such as dimethylformamide and dimethylacetamide, alcohol-based solvents such as methanol and ethanol, carboxylic acid-based solvents such as acetic acid and propionic acid, or water as a solvent are contacted with a strong base such as sodium hydroxide, or a hydrohalic acid such as hydrochloric acid, a Bronsted acid such as sulfuric acid, nitric acid, trifluoroacetic acid, methanesulfonic acid, and p-toluenesulfonic acid, or a Lewis acid such as zinc bromide, aluminum chloride, aluminum bromide, titanium (IV) chloride, cerium chloride / sodium iodide, and magnesium iodide.
[0118] Furthermore, among the polymerization raw materials of the organic polymer that forms the hydrophilic continuous skeleton of the absorbent A, the (meth)acrylic acid ester is not particularly limited, but is preferably a C1 to C10 (i.e., carbon number 1 to 10) alkyl ester of (meth)acrylic acid, and more preferably a C4 (i.e., carbon number 4) alkyl ester of (meth)acrylic acid. Examples of C4 alkyl esters of (meth)acrylic acid include t-butyl (meth)acrylic acid ester, n-butyl (meth)acrylic acid ester, and iso-butyl (meth)acrylic acid ester.
[0119] Furthermore, the monomers used in the crosslinking polymerization may be only (meth)acrylic acid esters and divinylbenzene, or may contain, in addition to (meth)acrylic acid esters and divinylbenzene, other monomers other than (meth)acrylic acid esters and divinylbenzene. In the latter case, the other monomers are not particularly limited, but examples thereof include styrene, α-methylstyrene, vinyltoluene, vinylbenzyl chloride, glycidyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isobutene, butadiene, isoprene, chloroprene, vinyl chloride, vinyl bromide, vinylidene chloride, tetrafluoroethylene, (meth)acrylonitrile, vinyl acetate, ethylene glycol di(meth)acrylate, and trimethylolpropane tri(meth)acrylate. The proportion of monomers other than (meth)acrylic acid ester and divinylbenzene in all monomers used in the crosslinking polymerization is preferably from 0 to 80 mol %, more preferably from 0 to 50 mol %.
[0120] The surfactant is not limited to the above-mentioned sorbitan monooleate, and may be any surfactant capable of forming a water-in-oil type (W / O) emulsion when the monomer for crosslinking polymerization is mixed with water. Examples of such surfactants include nonionic surfactants such as sorbitan monolaurate, sorbitan monopalmitate, sorbitan monostearate, sorbitan trioleate, polyoxyethylene nonylphenyl ether, polyoxyethylene stearyl ether, and polyoxyethylene sorbitan monooleate, anionic surfactants such as potassium oleate, sodium dodecylbenzenesulfonate, and dioctyl sodium sulfosuccinate, cationic surfactants such as distearyl dimethyl ammonium chloride, and amphoteric surfactants such as lauryl dimethyl betaine. These surfactants may be used alone or in combination of two or more.
[0121] In addition, the polymerization initiator is preferably a compound that generates radicals by heat and light irradiation. Furthermore, the polymerization initiator may be water-soluble or oil-soluble, and examples thereof include azobis(4-methoxy-2,4-dimethylvaleronitrile), azobisisobutyronitrile, azobisdimethylvaleronitrile, azobiscyclohexanenitrile, azobiscyclohexanecarbonitrile, azobis(2-methylpropionamidine)dihydrochloride, benzoyl peroxide, potassium persulfate, ammonium persulfate, hydrogen peroxide-ferrous chloride, sodium persulfate-acidic sodium sulfite, and tetramethylthiuram disulfide. However, in some cases, there are systems in which polymerization proceeds only by heating or light irradiation without the addition of a polymerization initiator, and in such systems, the addition of a polymerization initiator is not necessary.
[0122] The composite absorbent of the present invention is not particularly limited, but can be applied to various fields of composite absorbents such as dew condensation prevention sheets, simple soil, and other civil engineering and construction materials, base materials for medicines, and materials for absorbing leaked liquids. Therefore, the liquid to be absorbed by the composite absorbent is not particularly limited, and examples thereof include water and aqueous solutions (e.g., seawater, etc.), acids (e.g., hydrochloric acid, etc.), bases (e.g., sodium hydroxide, etc.), organic solvents (e.g., alcohols such as methanol and ethanol, ketones such as acetone, ethers such as tetrahydrofuran (THF) and 1,4-dioxane, N,N-dimethylformamide (DMF), dimethyl sulfoxide (DMSO), etc.). These liquids may be mixtures of two or more liquids.
[0123] Furthermore, the present invention is not limited to the above-described embodiments, and appropriate combinations, substitutions, modifications, etc. are possible within the scope of the object and intent of the present invention. Note that in this specification, ordinal numbers such as "first" and "second" are used to distinguish the items to which the ordinal numbers are attached, and do not indicate the order, priority, importance, etc. of each item. [Explanation of symbols]
[0124] 1 Composite absorber 2. First retaining sheet 3 Second Retaining Sheet 4. Polymer absorbents 5. Superabsorbent polymer (SAP) 6 Hydrophilic fiber sheet
Claims
1. 1. A composite absorbent for absorbing liquid, comprising: The composite absorbent body includes a polymer absorbent having a hydrophilic continuous skeleton and continuous pores, and a superabsorbent polymer; The polymer absorbent is contains at least a -COOH group and a -COONa group as ion exchange groups, and has a total ion exchange capacity of the -COOH group and the -COONa group per mass in a dry state of 6.0 mg equivalent / g or more; The composite absorbent body as described above is characterized in that the amount of liquid absorbed per unit mass is 30 g / g or more.
2. 2. The composite absorbent according to claim 1, wherein the polymer absorbent has an ion exchange rate of polyvalent ions of 50% or more.
3. 3. The composite absorbent according to claim 1, wherein the polymer absorbent has a void ratio per unit volume of 85% or more.
4. The composite absorbent according to any one of claims 1 to 3, wherein the polymer absorbent has an average diameter of the interconnected pores of 1 µm to 1000 µm.
5. The composite absorbent according to any one of claims 1 to 4, wherein the polymer absorbent is a monolithic absorbent.
6. The composite absorbent according to any one of claims 1 to 5, characterized in that the polymer absorbent is a hydrolysate of a cross-linked polymer of a (meth)acrylic acid ester and a compound containing two or more vinyl groups in one molecule.
7. 7. The composite absorbent body according to claim 1, wherein the superabsorbent polymer is an acrylic acid-based superabsorbent polymer having cations present on the surface thereof.
8. A polymeric absorbent used together with a superabsorbent polymer, It has a hydrophilic continuous skeleton and continuous pores, contains at least a -COOH group and a -COONa group as ion exchange groups, and has a total ion exchange capacity of the -COOH group and the -COONa group per mass in a dry state of 6.0 mg equivalent / g or more; A polymeric absorbent characterized by having a liquid absorption per unit mass of 30 g / g or more.
Citation Information
Patent Citations
Alcohol absorbing porous polymer
JP1988075016A
Bag body for liquid absorption
JP1996038893A
Polymer beads and their manufacturing method
JP1998505118A
Absorbent material structures, methods of manufacture and uses thereof, and disposable absorbent articles containing such material structures
JP2002505702A
Moisture / Water absorbing exothermic diaper
JP2003102784A