Composite absorbents and polymeric absorbents

The composite absorbent with a hydrophilic continuous skeleton and large-pore structure addresses the inefficiency of small-pore polymer foam materials by optimizing pore distribution and density for improved liquid absorption capacity and rate.

JP7591925B2Active Publication Date: 2024-11-29ORGANO CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2020219829
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-29
Publication Date
2024-11-29
Estimated Expiration
2040-12-29

AI Technical Summary

Technical Problem

Porous materials with small pore radii in polymer foam materials face challenges in liquid absorption efficiency, as liquid components tend to be drawn into larger pores, leading to reduced absorption capacity.

Method used

A composite absorbent with a hydrophilic continuous skeleton and pores predominantly larger than 1 μm, ensuring at least 90% of the pore volume is utilized for liquid absorption, combined with a controlled pore distribution and density to enhance absorption performance.

Benefits of technology

The composite absorbent effectively suppresses the decrease in liquid absorption, ensuring a sufficient amount is absorbed, with enhanced absorption rates and stability during liquid uptake.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007591925000002
    Figure 0007591925000002
  • Figure 0007591925000003
    Figure 0007591925000003
  • Figure 0007591925000004
    Figure 0007591925000004
Patent Text Reader

Abstract

To provide a composite absorber for a sanitary article that can suppress a decline in liquid absorption relative to the pore volume and has excellent absorption performance.SOLUTION: A composite absorber (4) for a sanitary article according to the present invention is for absorbing liquid, the composite absorber (4) comprising a polymer absorbent having hydrophilic continuous skeletons and continuous pores. The proportion of pore volume from pores having a pore radius of 1 μm or more in the polymeric absorber is at least 90% of the pore volume of all the pores.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a composite absorbent and a polymeric absorbent. [Background technology]

[0002] As an absorbent used for absorbing liquids such as aqueous solutions, those containing porous materials such as sponge materials are known. For example, Patent Document 1 discloses an absorbent article containing a polymer foam material consisting of a hydrophilic flexible structure of interconnected open cells. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent No. 3231320 Summary of the Invention [Problem to be solved by the invention]

[0004] According to the study by the inventors of the present application, porous materials such as the polymer foam material of Patent Document 1 have many pores with a relatively small pore radius. However, in a porous structure, liquid components tend to be easily drawn into pores with a relatively large pore radius. Therefore, in a porous material having many pores with small pore diameters as described above, the liquid components do not enter the pores with small pore diameters during liquid absorption, and the amount of liquid absorbed may be reduced compared to the pore volume.

[0005] The present invention has been made in consideration of such problems, and aims to provide a composite absorbent and a polymer absorbent that can suppress a decrease in the amount of liquid absorbed relative to the pore volume and have excellent absorption performance. [Means for solving the problem]

[0006] One aspect (Aspect 1) of the present invention is a composite absorbent for sanitary products for absorbing liquids, comprising a polymer absorbent having a hydrophilic continuous skeleton and continuous pores, wherein in the polymer absorbent, the proportion of the pore volume of pores having a pore radius of 1 μm or more is 90% or more of the pore volume of all pores.

[0007] In the composite absorbent of this embodiment, the ratio of the pore volume of pores with a pore radius of 1 μm or more to the pore volume of all pores in the polymer absorbent is 90% or more. Therefore, during liquid absorption, liquid is unlikely to enter pores with a relatively small pore radius of less than 1 μm, and even if it cannot enter, liquid can enter pores with a pore radius of 1 μm or more, ensuring a sufficient amount of liquid absorption. Therefore, it is possible to suppress a decrease in the amount of liquid absorption compared to the pore volume, and to obtain excellent absorption performance.

[0008] In another aspect (Aspect 2) of the present invention, in the composite absorbent of Aspect 1 above, the proportion of the pore volume of pores having a pore radius of 0.005 μm or less in the polymer absorbent is less than 10% of the pore volume of all pores.

[0009] In the composite absorbent of this embodiment, the proportion of the pore volume of pores with a very small pore radius, such as 0.005 μm or less, that are difficult to absorb liquid, is very small, and the proportion of the pore volume of pores with a large pore radius, such as 1 μm or more, that are capable of absorbing liquid, is large. This allows the pores of the polymer absorbent to be effectively used for absorbing liquid, and ensures a sufficient amount of liquid absorption.

[0010] In still another aspect (Aspect 3) of the present invention, in the composite absorbent of Aspect 1 or 2 above, the polymer absorbent has a pore radius at the maximum pore volume of 500 μm or less.

[0011] By setting the pore radius at the maximum pore volume to 500 μm or less, the composite absorbent of this embodiment can prevent the continuous skeletal structure of the polymer absorbent from being destroyed (crushed) during liquid absorption, making it easier to obtain an excellent absorption speed and ensuring a stable and sufficient amount of liquid absorption (if the pore radius at the maximum pore volume is 500 μm or more, there is a risk that the continuous skeletal structure cannot be maintained during liquid absorption and may be crushed).

[0012] In yet another aspect (Aspect 4) of the present invention, in the composite absorbent described in any one of Aspects 1 to 3 above, the polymer absorbent is characterized in that the coefficient of variation of the pore distribution for pores having a pore radius of 1 μm or more is 1.4 or less.

[0013] The composite absorbent of this embodiment has a coefficient of variation of pore distribution of 1.4 or less, so that the variation of pore radius relative to the average value of pore radius is small, and the peak of the pore distribution is sharp near the average value of pore radius. Therefore, the polymer absorbent can absorb liquid almost uniformly from all directions and all surfaces. As a result, the pores of the polymer absorbent can be effectively used for liquid absorption, and a sufficient amount of liquid absorption can be secured.

[0014] In yet another aspect (Aspect 5) of the present invention, in the composite absorbent described in any one of Aspects 1 to 3 above, the polymer absorbent is characterized in that the coefficient of variation of the pore distribution in pores having a pore radius of 1 μm or more is greater than 1.4.

[0015] The composite absorbent of this embodiment has a coefficient of variation of pore distribution exceeding 1.4, so that the variation of pore radius with respect to the average value of pore radius is large, and the peak of the pore distribution is broad near the average value of pore radius. That is, the polymer absorbent has pores with small pore radius and pores with large pore radius. Therefore, in pores with small pore radius, capillary force is likely to work, and therefore the liquid absorption speed is likely to be fast, and in pores with large pore radius, the liquid absorption volume is likely to be large. Therefore, due to the synergistic effect of the two, the polymer absorbent can instantly absorb a large amount of liquid inside the pores.

[0016] In yet another aspect (Aspect 6) of the present invention, in the composite absorbent described in Aspect 5 above, the polymer absorbent is characterized in that the portion of the polymer absorbent with a larger pore radius is broader than the portion with a smaller pore radius, relative to the pore radius corresponding to the maximum value of the pore volume in the curve showing the pore distribution.

[0017] In the composite absorbent of this embodiment, the polymer absorbent has the above-mentioned configuration, i.e., a configuration in which there are more pores with a large pore diameter than pores with a small pore radius. By having more pores with a large pore radius, the liquid absorption volume tends to be larger, and a larger amount of liquid can be absorbed inside the pores.

[0018] In yet another aspect (Aspect 7) of the present invention, in the composite absorbent described in Aspect 5 above, the polymer absorbent is characterized in that the portion on the side where the pore radius is smaller is broader than the portion on the side where the pore radius is larger, relative to the pore radius corresponding to the maximum value of the pore volume in the curve showing the pore distribution.

[0019] In the composite absorbent of this embodiment, the polymer absorbent has the above-mentioned configuration, i.e., a configuration in which there are more pores with small pore diameters than pores with large pore radiuses. The presence of more pores with small pore radiuses makes it easier for capillary force to work, which makes it easier for the liquid absorption speed to be faster, and allows liquid to be instantly absorbed inside the pores.

[0020] In yet another aspect (Aspect 8) of the present invention, in the composite absorbent described in any one of Aspects 1 to 3 above, the polymer absorbent is characterized in that there are at least two maximum values ​​of pore volume in the curve showing the pore distribution.

[0021] In the composite absorbent of this embodiment, the polymer absorbent has the above-mentioned configuration, that is, pores having a predetermined small pore radius and a pore radius nearby it, and pores having a predetermined large pore radius and a pore radius nearby it are present. Therefore, in the pores with a relatively small pore radius, capillary force is likely to act, and therefore the liquid absorption speed is likely to be fast, and in the pores with a relatively large pore radius, the liquid absorption volume is likely to be large. Therefore, due to the synergistic effect of the two, the polymer absorbent can instantly absorb a large amount of liquid inside the pores.

[0022] In yet another aspect (Aspect 9) of the present invention, in the composite absorbent described in Aspect 8 above, the polymer absorbent is characterized in that the two maximum values ​​of pore volume in the curve showing the pore distribution are such that the maximum value of the relatively small pore radius is larger than the maximum value of the relatively large pore radius.

[0023] In the composite absorbent of this embodiment, the polymer absorbent has the above-mentioned configuration, that is, there are more pores with small pore diameters than pores with large pore radius. The presence of many pores with small pore radiuses makes it easier for capillary force to work, which makes it easier for the liquid absorption speed to increase, and allows liquid to be instantly absorbed inside the pores.

[0024] In yet another aspect (Aspect 10) of the present invention, in the composite absorbent described in Aspect 8 above, the polymer absorbent is characterized in that the two maximum values ​​of pore volume in the curve showing the pore distribution are such that the maximum value of the relatively small pore radius is smaller than the maximum value of the relatively large pore radius.

[0025] In the composite absorbent of this embodiment, the polymer absorbent has the above-mentioned configuration, i.e., there are more pores with a larger pore diameter than those with a smaller pore radius. The presence of more pores with a larger pore radius makes it easier for the liquid absorption volume to become larger, and a larger amount of liquid can be absorbed inside the pores.

[0026] In still another aspect (Aspect 11) of the present invention, in the composite absorbent according to any one of Aspects 1 to 10 above, the polymer absorbent has a total pore volume of 0.9 mL / g or more.

[0027] In the composite absorbent of this embodiment, the total pore volume of the polymer absorbent is 0.9 mL / g or more, so that the polymer absorbent can have a sufficient pore volume, and therefore a sufficient amount of liquid can be absorbed. In addition, the spaces (pores) for absorbing the liquid to be absorbed in the porous body can be made less likely to collapse during absorption, and the amount and speed of absorption can be made less likely to decrease.

[0028] In still another aspect (aspect 12) of the present invention, in the composite absorbent according to any one of aspects 1 to 11 above, the polymer absorbent has a bulk density of 0.07 to 0.6 g / cm 3 It is characterized in that:

[0029] In the composite absorbent of this embodiment, the polymer absorbent has a bulk density of 0.07 to 0.6 g / cm 3 Therefore, the liquid absorption speed (DW) performance can be made 6mL / 30sec or more. In other words, since the liquid absorption speed is fast, the polymer absorbent can instantly absorb liquid inside the pores.

[0030] In still another aspect (aspect 13) of the present invention, in the composite absorbent according to any one of aspects 1 to 12 above, the polymer absorbent is a monolithic absorbent.

[0031] The composite absorbent of this embodiment can quickly absorb liquid because the polymer absorbent is a monolithic absorbent.

[0032] In yet another aspect (Aspect 14) of the present invention, in the composite absorbent described in any one of Aspects 1 to 13 above, the polymer absorbent is a hydrolysate of a crosslinked polymer of a (meth)acrylic acid ester and a compound containing two or more vinyl groups in one molecule, and is characterized in that it contains at least one -COONa group.

[0033] In the composite absorbent of this embodiment, since the polymer absorbent has the above-mentioned specific configuration, when absorbing liquid, the hydrophilic continuous skeleton is easily extended and the continuous pores are easily expanded, so that a larger amount of liquid can be taken up into the continuous pores more quickly, and the absorbent can exhibit even better absorption performance.

[0034] Furthermore, still another embodiment (embodiment 15) of the present invention is a polymeric absorbent characterized in that it has a hydrophilic continuous skeleton and continuous pores, and the proportion of the pore volume due to pores having a pore radius of 1 μm or more is 90% or more of the pore volume of all pores.

[0035] In the polymer absorbent of this embodiment, the ratio of the pore volume of pores with a pore radius of 1 μm or more to the pore volume of all pores is 90% or more, so that even if liquid does not enter pores with a relatively small pore radius, such as a pore radius of less than 1 μm, during liquid absorption, a sufficient amount of liquid absorption can be ensured. This makes it possible to suppress a decrease in the amount of liquid absorption compared to the pore volume, and to obtain excellent absorption performance. Effect of the Invention

[0036] According to the present invention, it is possible to provide a composite absorbent body having excellent absorption performance, which can suppress a decrease in the amount of absorbed liquid relative to the pore volume, and a sanitary product having the same. [Brief description of the drawings]

[0037] [Figure 1] FIG. 1 is an exploded perspective view of a composite absorbent body 1 according to one embodiment of the present invention. [Diagram 2] FIG. 2 is an exploded perspective view of a composite absorbent body 1' according to another embodiment of the present invention. [Diagram 3] FIG. 3 is a diagram illustrating a manufacturing process of absorbent A, which is an example of a polymer absorbent. [Figure 4] FIG. 4 is an SEM photograph of absorbent A at a magnification of 50 times. [Diagram 5] FIG. 5 is a SEM photograph of absorbent A at a magnification of 100 times. [Figure 6] FIG. 6 is an SEM photograph of absorbent A at a magnification of 500 times. [Figure 7] FIG. 7 is a SEM photograph of absorbent A at a magnification of 1000 times. [Figure 8] FIG. 8 is an SEM photograph of absorbent A at a magnification of 1500 times. [Figure 9] FIG. 9 is a graph showing the relationship between the pore radius of the pores of absorbent A and the cumulative pore volume. [Figure 10] FIG. 10 is a graph showing the relationship between the pore radius of the pores of absorbent A and the differential pore volume. [Figure 11] FIG. 11 is a graph showing the relationship between the bulk density and the absorption performance (DW) in absorbent A. [Figure 12] FIG. 12 is a schematic diagram showing a measurement device used in the pressureless DW method. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0038] A preferred embodiment of the present invention will be described in detail below using a composite absorbent body 1 as one embodiment. In this specification, unless otherwise specified, "planar view" simply means "viewing an object (e.g., a composite absorbent body) placed on a horizontal surface in an unfolded state in the thickness direction of the object from above in the vertical direction."

[0039] [Composite absorber] FIG. 1 is an exploded perspective view of a composite absorbent body 1 according to one embodiment of the present invention. The composite absorbent 1 shown in Figure 1 has a roughly rectangular outer shape in a plan view, and is equipped with a first retention sheet 2 that forms one surface of the composite absorbent 1 in the thickness direction, a second retention sheet 3 that forms the other surface of the composite absorbent 1, and a liquid-absorbent member that is located between these sheets and contains a polymer absorbent 4.

[0040] The liquid-absorbent member in the composite absorbent body 1 is configured to absorb and retain liquid that has permeated through the first retention sheet 2 by using a polymer absorbent 4 that is located between the first retention sheet 2 and the second retention sheet 3 and has a hydrophilic continuous skeleton and continuous pores. Furthermore, the above-mentioned polymer absorbent 4 exhibits a unique liquid absorption behavior in that, when absorbing a liquid, the liquid is incorporated into the continuous skeleton and then into the continuous pores.

[0041] When the above-mentioned polymer absorbent 4 absorbs a liquid such as an aqueous solution, the hydrophilic continuous skeleton instantly takes up the liquid due to osmotic pressure and expands, thereby expanding the volume of the continuous pores, and the expanded continuous pores can further take up the liquid, so that the polymer absorbent 4 can instantly absorb a large amount of liquid and can transfer the absorbed liquid to the SAP, which has a high water retention capacity, and steadily retain it within the SAP. Therefore, the composite absorbent body 1 containing such an absorbent polymer 4 can exhibit high absorption performance as an absorbent body.

[0042] In the present invention, the liquid-absorbent member is not limited to the form of the composite absorbent 1 of the above embodiment, and the liquid-absorbent member may or may not contain other liquid-absorbent materials as long as it contains at least the polymer absorbent exhibiting the above-mentioned specific liquid-absorbing behavior. For example, as in the composite absorbent 1' of another embodiment of the present invention shown in Fig. 2, the liquid-absorbent member located between the first retention sheet 2 and the second retention sheet 3 may be composed of a mixture of a polymer absorbent 4 and a superabsorbent polymer 5 (SAP).

[0043] Furthermore, in the present invention, the configuration of the composite absorbent is not limited to the form of the composite absorbent 1 of the above-mentioned embodiment, and the composite absorbent may have, for example, a hydrophilic fiber sheet 6 located between the first retention sheet 2 and the liquid-absorbent member (i.e., the polymer absorbent 4 and the highly absorbent polymer 5), as in a composite absorbent 1' of another embodiment of the present invention shown in Figure 2.

[0044] In the present invention, the outer shape, various dimensions, basis weight, etc. of the composite absorbent body are not particularly limited as long as they do not impair the effects of the present invention, and any outer shape (e.g., circular, elliptical, polygonal, hourglass, design shape, etc.), various dimensions, basis weight, etc. can be adopted according to various applications and usage modes, etc.

[0045] Various constituent members of the composite absorbent body of the present invention will be described in further detail below, taking as an example the composite absorbent body 1 of the embodiment shown in FIG.

[0046] (Retaining sheet) 1, a first retention sheet 2 forming one surface of the composite absorbent body 1 has a substantially rectangular outer shape in a plan view similar to the outer shape of the composite absorbent body 1. The first retention sheet 2 is formed of a liquid-permeable sheet-like member that allows liquid supplied to the composite absorbent body 1 to pass therethrough and be absorbed and retained in the liquid-absorbent member on the inside.

[0047] The first retaining sheet 2 has an overall size that is slightly larger than the absorbent member located on the inside (i.e., compared to the area in which absorbent materials such as polymer absorbent 4 are located), and is joined at its peripheral portion to the second retaining sheet 3 located on the other side of the composite absorbent 1 in the thickness direction by any adhesive or heat sealing means, etc.

[0048] On the other hand, the second retention sheet 3 forming the other surface of the composite absorbent body 1 has a substantially rectangular outer shape in a plan view similar to the outer shape of the composite absorbent body 1. The second retention sheet 3 is made of a liquid-impermeable sheet-like member that prevents liquid that has not been absorbed and retained in the inner liquid-absorbent member and liquid that has seeped out from the liquid-absorbent member from leaking out to the outside of the composite absorbent body 1.

[0049] In the present invention, the sheet-like members usable as the first and second retaining sheets are not limited to those in the above-mentioned embodiments, and the composite absorbent of the present invention may be any one of the first and second retaining sheets formed from a liquid-permeable sheet-like member. That is, the composite absorbent of the present invention may be any one of the first and second retaining sheets formed from a liquid-impermeable sheet-like member.

[0050] When a liquid-permeable sheet-like member is used as the holding sheet, the liquid-permeable sheet-like member is not particularly limited as long as it does not impair the effects of the present invention, and any liquid-permeable sheet-like member can be used according to various applications, usage modes, etc. Examples of such liquid-permeable sheet-like members include hydrophilic nonwoven fabrics such as air-through nonwoven fabrics, spunbond nonwoven fabrics, and point-bond nonwoven fabrics, woven fabrics, knitted fabrics, and porous resin films.

[0051] Furthermore, when hydrophilic nonwoven fabrics, woven fabrics, knitted fabrics, etc. (hereinafter collectively referred to as "fiber sheets") are used as the liquid-permeable sheet-like member, these fiber sheets may have a single-layer structure or a multi-layer structure of two or more layers. The type of fiber constituting such a fiber sheet is not particularly limited, and examples thereof include hydrophilic fibers such as cellulosic fibers and thermoplastic resin fibers that have been subjected to a hydrophilization treatment. These fibers may be used alone or in combination of two or more types of fibers. Examples of cellulose-based fibers that can be used as constituent fibers of the fiber sheet include natural cellulose fibers (e.g., plant fibers such as cotton), regenerated cellulose fibers, refined cellulose fibers, and semi-synthetic cellulose fibers. Examples of thermoplastic resin fibers that can be used as constituent fibers of the fiber sheet include fibers made of known thermoplastic resins such as olefin resins such as polyethylene (PE) and polypropylene (PP), polyester resins such as polyethylene terephthalate (PET), and polyamide resins such as 6-nylon. These resins may be used alone or in combination of two or more types.

[0052] In addition, when a liquid-impermeable sheet-like member is used as the holding sheet, the liquid-impermeable sheet-like member is not particularly limited as long as it does not impair the effects of the present invention, and any liquid-impermeable sheet-like member can be adopted according to various applications and usage modes, etc. Examples of such liquid-impermeable sheet-like members include hydrophobic nonwoven fabrics formed from any hydrophobic thermoplastic resin fibers (for example, polyolefin fibers such as PE and PP, polyester fibers such as PET, various composite fibers such as core-sheath type, etc.); porous or nonporous resin films formed from hydrophobic thermoplastic resins such as PE and PP; laminates in which a nonwoven fabric is bonded to the resin film; laminated nonwoven fabrics such as SMS nonwoven fabrics, etc.

[0053] In the present invention, the external shape, various dimensions, basis weight, etc. of the retaining sheet are not particularly limited as long as they do not impair the effects of the present invention, and any external shape (e.g., circular, oval, polygonal, hourglass, design shape, etc.), various dimensions, basis weight, etc. can be adopted according to various applications and usage modes, etc.

[0054] (Liquid-absorbent member) In the composite absorbent 1 shown in Figure 1, the liquid-absorbent member is configured to absorb and retain liquid that has permeated through the first retaining sheet 2 by means of the polymer absorbent 4, which is located between the first retaining sheet 2 and the second retaining sheet 3 as described above and has a hydrophilic continuous skeleton and continuous pores.

[0055] In the composite absorbent 1, the polymer absorbent 4 of the liquid-absorbent member is bonded to each of the above-mentioned first retaining sheet 2 and second retaining sheet 3 by any adhesive such as a hot melt adhesive, but in the composite absorbent of the present invention, the polymer absorbent does not have to be bonded to the retaining sheet.

[0056] In the present invention, the liquid-absorbent member contains a polymer absorbent having a hydrophilic continuous skeleton and continuous pores and exhibiting the above-mentioned specific liquid-absorbing behavior. The polymer absorbent will be described later.

[0057] In the present invention, the liquid-absorbent member located between the first holding sheet and the second holding sheet may or may not contain other liquid-absorbent materials as long as it contains at least the above-mentioned polymer absorbent. That is, the liquid-absorbent member may contain only the above-mentioned polymer absorbent as the liquid-absorbent material, or may further contain a liquid-absorbent material known in the art in addition to the above-mentioned polymer absorbent. Examples of such liquid-absorbent materials include hydrophilic fibers and superabsorbent polymers, and more specifically, cellulose fibers such as pulp fibers (e.g., ground pulp), cotton, rayon, and acetate; granules made of superabsorbent polymers (SAP) such as sodium acrylate copolymer; and mixtures of any combination of these. For example, in a composite absorbent 1' according to another embodiment of the present invention shown in FIG. 2, the liquid-absorbent member located between the first retention sheet 2 and the second retention sheet 3 contains a superabsorbent polymer 5 in addition to a particulate polymer absorbent 4 having a hydrophilic continuous skeleton and continuous pores and the above-mentioned specific particle size.

[0058] In the present invention, the outer shape (planar shape of the area where the absorbent material is arranged), various dimensions, basis weight, etc. of the absorbent member are not particularly limited as long as they do not impair the effects of the present invention, and any outer shape, various dimensions, basis weight, etc. can be adopted depending on the desired absorbency, flexibility, strength, etc.

[0059] (hydrophilic fiber sheet) In the present invention, the composite absorbent may have a hydrophilic fiber sheet 6 between the first retention sheet 2 and the liquid-absorbent member (i.e., the polymer absorbent 4 and the highly absorbent polymer 5), for example, as in another embodiment of the composite absorbent 1' shown in Figure 2.

[0060] In the present invention, the hydrophilic fiber sheet that can be used in the composite absorbent is not particularly limited as long as it does not impair the effects of the present invention, and any hydrophilic fiber sheet can be used depending on various applications and usage modes. Examples of such hydrophilic fiber sheets include nonwoven fabrics, woven fabrics, knitted fabrics, etc. that have hydrophilicity. The hydrophilic fiber sheet may have a single-layer structure or a multi-layer structure of two or more layers.

[0061] The type of fibers constituting the hydrophilic fiber sheet is not particularly limited, and examples thereof include hydrophilic fibers such as cellulosic fibers and thermoplastic resin fibers that have been subjected to a hydrophilic treatment. These fibers may be used alone or in combination of two or more types of fibers. Furthermore, examples of cellulose-based fibers that can be used as constituent fibers of the hydrophilic fiber sheet include natural cellulose fibers (e.g., plant fibers such as cotton), regenerated cellulose fibers, refined cellulose fibers, and semi-synthetic cellulose fibers. Examples of thermoplastic resin fibers that can be used as constituent fibers of the hydrophilic fiber sheet include fibers made of known thermoplastic resins such as olefin resins such as PE and PP, polyester resins such as PET, and polyamide resins such as 6-nylon. These resins may be used alone or in combination of two or more types.

[0062] In the present invention, the outer shape, various dimensions, basis weight, etc. of the hydrophilic fibrous sheet are not particularly limited as long as they do not impair the effects of the present invention, and any outer shape, various dimensions, basis weight, etc. can be adopted according to various applications, usage modes, etc.

[0063] The polymer absorbent used in the composite absorbent of the present invention will be described in more detail below.

[0064] [Polymer absorbent] In the present invention, the polymer absorbent is not particularly limited as long as it has a hydrophilic continuous skeleton and continuous pores, and exhibits a unique liquid absorption behavior in which the liquid is absorbed in the continuous skeleton and then in the continuous pores when absorbing a liquid. Examples of such polymer absorbents include a polymer compound that is a hydrolyzate of a crosslinked polymer of two or more monomers including at least a (meth)acrylic acid ester and has at least one hydrophilic group in the functional group. More specifically, examples of such polymer absorbents include a polymer compound that is a hydrolyzate of a crosslinked polymer of a compound containing a (meth)acrylic acid ester and two or more vinyl groups in one molecule and has at least a -COONa group. Such a polymer absorbent is an organic porous body having at least one -COONa group in one molecule, and may further have a -COOH group. The -COONa group is distributed approximately uniformly in the skeleton of the porous body.

[0065] If the polymer absorbent is a hydrolyzate of a crosslinked polymer of such a (meth)acrylic acid ester and a compound containing two or more vinyl groups in one molecule, and contains at least one or more -COONa groups, as described below, when absorbing a liquid such as an aqueous solution, the hydrophilic continuous skeleton is easily extended (i.e., it is easily expanded), and the continuous pores are easily expanded, so that more liquid can be taken in the continuous pores more quickly. Therefore, a composite absorbent containing such a polymer absorbent can exhibit even better absorption performance as an absorbent.

[0066] In this specification, the (meth)acrylic acid ester refers to an acrylic acid ester or a methacrylic acid ester.

[0067] In such a polymer absorbent formed by the hydrolysis product of a cross-linked polymer of a (meth)acrylic acid ester and divinylbenzene, a hydrophilic continuous skeleton is formed by an organic polymer having at least -COONa groups, and the skeleton has interconnected pores (interconnected pores) that serve as liquid absorption fields. In addition, since the hydrolysis treatment converts the -COOR groups (that is, carboxylate groups) of the crosslinked polymer into -COONa groups or -COOH groups (see FIG. 2), the polymer absorbent may have -COOR groups.

[0068] The presence of -COOH and -COONa groups in the organic polymer forming the hydrophilic continuous backbone can be confirmed by analysis using infrared spectroscopy and a quantitative method for weakly acidic ion exchange groups.

[0069] Here, Fig. 3 is a diagram for explaining the manufacturing process of absorbent A, which is an example of a polymer absorbent. In this Fig. 3, the upper diagram shows the constituent raw materials for polymerization, the middle diagram shows monolith A, which is a crosslinked polymer of (meth)acrylic acid ester and divinylbenzene, and the lower diagram shows absorbent A obtained by subjecting monolith A in the middle diagram to hydrolysis and drying treatment.

[0070] Hereinafter, an explanation will be given using absorbent A, which is an example of a polymer absorbent and is formed from a hydrolysate of a crosslinked polymer of a (meth)acrylic acid ester and divinylbenzene.

[0071] The polymer absorbent is not limited to the absorbent A, but may be a hydrolysate of a cross-linked polymer of a (meth)acrylic acid ester and a compound having two or more vinyl groups in one molecule, or a hydrolysate of a cross-linked polymer of two or more monomers including at least a (meth)acrylic acid ester. However, if the polymer absorbent is a monolithic absorbent, it has the advantage that it can absorb liquid quickly and that the liquid temporarily held in the polymer absorbent can be transferred to the SAP more reliably.

[0072] In the following description, "Monolith A" refers to an organic porous material consisting of a crosslinked polymer of (meth)acrylic acid ester and divinylbenzene before hydrolysis treatment, and may be referred to as a "monolithic organic porous material." In addition, "absorbent A" is a hydrolyzate of a crosslinked polymer (monolith A) of (meth)acrylic acid ester and divinylbenzene after hydrolysis and drying. In the following description, absorbent A refers to the absorbent in a dry state.

[0073] First, the structure of absorbent A will be described. As described above, absorbent A has a hydrophilic continuous skeleton and continuous pores. As shown in Fig. 3, absorbent A, which is an organic polymer having a hydrophilic continuous skeleton, is obtained by cross-linking polymerizing (meth)acrylic acid ester, which is a polymerization monomer, and divinylbenzene, which is a cross-linking monomer, and further hydrolyzing the obtained cross-linked polymer (monolith A).

[0074] The organic polymer that forms a hydrophilic continuous skeleton has, as structural units, a polymerized residue of an ethylene group (hereinafter referred to as "structural unit X") and a cross-linked polymerized residue of divinylbenzene (hereinafter referred to as "structural unit Y"). Furthermore, the polymerized residue of the ethylene group (structural unit X) in the organic polymer forming the hydrophilic continuous skeleton has a -COONa group generated by hydrolysis of the carboxylate group, or both a -COOH group and a -COONa group. When the polymerized monomer is a (meth)acrylic acid ester, the polymerized residue of the ethylene group (structural unit X) has a -COONa group, a -COOH group, and an ester group.

[0075] In the absorbent A, the ratio of the crosslinked polymer residue of divinylbenzene (structural unit Y) in the organic polymer forming the hydrophilic continuous skeleton is, for example, 0.1 to 30 mol %, preferably 0.1 to 20 mol %, based on the total structural units. For example, in the absorbent A in which butyl methacrylate is used as the polymerization monomer and divinylbenzene is used as the crosslinked monomer, the ratio of the crosslinked polymer residue of divinylbenzene (structural unit Y) in the organic polymer forming the hydrophilic continuous skeleton is, for example, about 3 mol %, preferably 0.1 to 10 mol %, more preferably 0.3 to 8 mol %, based on the total structural units. Furthermore, when the ratio of cross-linked polymerized residues of divinylbenzene in the organic polymer forming the hydrophilic continuous skeleton is 0.1 mol % or more, the strength of absorbent A is less likely to decrease, and when the ratio of cross-linked polymerized residues of divinylbenzene is 30 mol % or less, the absorption amount of the liquid to be absorbed is less likely to decrease.

[0076] In addition, in the absorbent A, the organic polymer forming the hydrophilic continuous skeleton may be composed only of the structural unit X and the structural unit Y, or may have, in addition to the structural unit X and the structural unit Y, a structural unit other than the structural unit X and the structural unit Y, that is, a polymerized residue of a monomer other than a (meth)acrylic acid ester and divinylbenzene.

[0077] Examples of structural units other than the structural unit X and the structural unit Y include polymerized residues of monomers such as styrene, α-methylstyrene, vinyltoluene, vinylbenzyl chloride, glycidyl (meth)acrylate, isobutene, butadiene, isoprene, chloroprene, vinyl chloride, vinyl bromide, vinylidene chloride, tetrafluoroethylene, (meth)acrylonitrile, vinyl acetate, ethylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, and trimethylolpropane tri(meth)acrylate.

[0078] The proportion of structural units other than the structural unit X and the structural unit Y in the organic polymer that forms the hydrophilic continuous skeleton is, for example, 0 to 50 mol %, and preferably 0 to 30 mol %, relative to all structural units.

[0079] The thickness of the hydrophilic continuous skeleton of the absorbent A is preferably 0.1 to 100 μm. When the thickness of the hydrophilic continuous skeleton of the absorbent A is 0.1 μm or more, the spaces (pores) for absorbing liquid in the porous body are less likely to collapse during absorption, and the amount of absorbed liquid is less likely to decrease. On the other hand, when the thickness of the hydrophilic continuous skeleton is 100 μm or less, an excellent absorption speed is easily obtained.

[0080] In addition, since the pore structure of the hydrophilic continuous skeleton of absorbent A is an open-cell structure, the thickness of the continuous skeleton is measured by evaluating the cross section of the skeleton that appears on the test piece for electron microscope measurement. The continuous skeleton is often polygonal in shape because it is formed by the gaps between water (water droplets) removed by the dehydration and drying process after hydrolysis. Therefore, the thickness of the continuous skeleton is the average value of the diameter (μm) of the circle circumscribing the polygonal cross section. In rare cases, there may be small holes in the polygon, in which case the circumscribing circle of the polygonal cross section surrounding the small holes is measured.

[0081] Furthermore, the absorbent A preferably has an average diameter of interconnected pores of 1 to 1000 μm. When the average diameter of interconnected pores in the absorbent A is 1 μm or more, the spaces (pores) for absorbing liquid in the porous body are less likely to collapse during absorption, and the absorption rate is less likely to decrease. On the other hand, when the average diameter of interconnected pores is 1000 μm or less, an excellent absorption rate is easily obtained.

[0082] The average diameter (μm) of the interconnected pores of absorbent A can be measured by mercury intrusion porosimetry, and the maximum value of the pore distribution curve obtained by the mercury intrusion porosimetry is used. Regardless of the ionic form of absorbent A, samples for measuring the average diameter of interconnected pores are those dried for 18 hours or more in a reduced pressure dryer set at a temperature of 50°C. The final pressure reached is 0 Torr.

[0083] Here, FIG. 4 is an SEM photograph of absorbent A at a magnification of 50 times, FIG. 5 is an SEM photograph of absorbent A at a magnification of 100 times, FIG. 6 is an SEM photograph of absorbent A at a magnification of 500 times, FIG. 7 is an SEM photograph of absorbent A at a magnification of 1000 times, and further, FIG. 8 is an SEM photograph of absorbent A at a magnification of 1500 times. The absorbents A shown in these Figs. 4 to 8 are examples of absorbents that use butyl methacrylate as a polymerization monomer and divinylbenzene as a cross-linking monomer, and each has a cubic structure with a side length of 2 mm.

[0084] 4 to 8 has a large number of cellular macropores and further has portions where these cellular macropores overlap. Absorbent A has an open cell structure in which the overlapping portions of the macropores form common openings (mesopores), i.e., it has an open cell structure (open macropore structure).

[0085] The overlapping portions of the macropores form common openings (mesopores) having an average diameter in a dry state of 1 to 1000 μm, preferably 10 to 200 μm, and particularly preferably 20 to 100 μm, and most of them have an open pore structure. When the average diameter of the mesopores in a dry state is 1 μm or more, the absorption rate of the liquid to be absorbed is improved. On the other hand, when the average diameter of the mesopores in a dry state is 1000 μm or less, the absorbent A is less likely to become embrittled. The number of overlapping macropores in each macropore is about 1 to 12, and in most cases, about 3 to 10.

[0086] In addition, since absorbent A has such an open cell structure, macropores and mesopores can be uniformly formed, and there are advantages in that the pore volume and specific surface area can be significantly increased compared to particle agglomeration type porous bodies such as those described in JP-A-8-252579 and the like.

[0087] The continuous pores of the absorbent A are a plurality of pores (voids) that are connected to each other. The total pore volume of the pores (voids) of the absorbent A is preferably 0.5 to 50 mL / g, more preferably 0.9 to 40 mL / g, and even more preferably 2 to 30 mL / g. When the total pore volume of the absorbent A is 0.5 mL / g or more, a sufficient pore volume can be secured in the absorbent A, and therefore a sufficient amount of liquid absorption can be secured. In addition, the space (pores) for absorbing liquid in the porous body can be made difficult to collapse during absorption, and the amount and speed of liquid absorption can be made difficult to decrease. On the other hand, when the total pore volume of the absorbent A is 50 mL / g or less, the strength of the absorbent A can be made difficult to decrease.

[0088] The total pore volume can be measured by mercury intrusion porosimetry. The sample for measuring the total pore volume is dried for 18 hours or more in a vacuum dryer set at a temperature of 50°C, regardless of the ion form of absorbent A. The final pressure is 0 Torr. The mercury intrusion porosimetry can obtain the cumulative (integrated) pore volume distribution (relationship between pore radius and cumulative pore volume) and the log differential pore volume distribution (relationship between pore radius and log differential pore volume), and can calculate the total pore volume (mL / g), average pore radius (μm), maximum pore radius (μm), pore volume (mL / g) and ratio (%) of pores with a given pore radius or more (or less), and the coefficient of variation of the pore volume. The maximum pore diameter (μm) refers to the pore radius of the pore that shows the maximum pore volume. In addition, the pore volume (mL / g) for each pore radius is the log differential pore volume (mL / g) in the log differential pore volume distribution.

[0089] Here, in the pores (voids) of the absorbent A, the ratio of the pore volume of pores with a pore radius of 1 μm or more to the pore volume of all pores (total pore volume) is 90% or more, preferably 93% or more, and more preferably 95% or more. When the ratio of the pore volume of pores with a pore radius of 1 μm or more is 90% or more, during liquid absorption, it is difficult for liquid components to enter pores with a relatively small pore radius, such as a pore radius of less than 1 μm, and even if they cannot enter, a sufficient amount of liquid absorption can be ensured. Therefore, it is possible to suppress a decrease in the amount of liquid absorption compared to the pore volume, and excellent absorption performance can be obtained.

[0090] In the pores of the absorbent A, the proportion of the pore volume of pores with a pore radius of 0.005 μm or less is preferably less than 10% of the pore volume of all pores (total pore volume), and the proportion of the pore volume of pores with a pore radius of 0.05 μm or less is more preferably less than 10% of the pore volume of all pores (total pore volume). In the absorbent A, the proportion of the pore volume of pores with a pore radius of 0.005 μm or less, which are very small and difficult to absorb liquid, is very small, and the proportion of the pore volume of pores with a pore radius of 1 μm or more, which are large and capable of absorbing liquid, is large (90% or more). This allows the pores of the absorbent A to be effectively used for absorbing liquid, and a sufficient amount of liquid can be absorbed.

[0091] In addition, the pores of the absorbent A preferably have a pore radius of (0.5 μm or more) 500 μm or less at the pores showing the maximum pore volume, more preferably 300 μm or less, and more preferably 150 μm or less. By making the pore radius at the maximum pore volume 500 μm or less, it is possible to suppress the continuous skeleton structure of the absorbent A from being broken (crushed) during liquid absorption, making it easy to obtain an excellent absorption speed, and ensuring a stable and sufficient amount of liquid absorption. If the pore radius at the maximum pore volume is 500 μm or more, there is a risk that the continuous skeleton structure cannot be maintained during liquid absorption and may be collapsed.

[0092] Furthermore, the pores of absorbent A may have a coefficient of variation of pore distribution (pore volume) of 1.4 or less for pores with a pore radius of 1 μm or more. When the coefficient of variation of the pore distribution is 1.4 or less, the variation of the pore radius relative to the average value of the pore radius is small, and the peak of the pore distribution is sharp near the average value of the pore radius. Therefore, absorbent A can absorb liquid almost uniformly from all directions and all surfaces. This allows the pores of the polymer absorbent to be effectively used for liquid absorption, ensuring a sufficient amount of liquid absorption.

[0093] On the other hand, the pores of the absorbent A may have a coefficient of variation of pore distribution (pore volume) of more than 1.4 in the pores having a pore radius of 1 μm or more. In this case, since the coefficient of variation of the pore distribution is more than 1.4, the variation of the pore radius with respect to the average value of the pore radius is large, and the peak of the pore distribution is broad near the average value of the pore radius. That is, the absorbent A has pores with small pore radius and pores with large pore radius. Therefore, the capillary force is likely to work in the pores with a small pore radius, and therefore the liquid absorption speed is likely to be fast, and the liquid absorption volume is likely to be large in the pores with a large pore radius. Therefore, due to the synergistic effect of the two, the absorbent A can instantly absorb a large amount of liquid inside the pores.

[0094] Here, in the case of the pores of the absorbent A, when the peak of the pore distribution is broad, the portion on the side of the pore radius larger than the portion on the side of the pore radius smaller than the pore radius corresponding to the maximum value of the pore volume in the curve showing the pore distribution may be broader. In this case, the absorbent A has a configuration in which there are more pores with a larger pore diameter than pores with a smaller pore radius. Therefore, by having more pores with a larger pore radius, the liquid absorption volume tends to be larger, and a larger amount of liquid can be absorbed inside the pores.

[0095] On the other hand, even if the pores of absorbent A have a broad peak in the pore distribution, the portion with a smaller pore radius may be broader than the portion with a larger pore radius with respect to the pore radius corresponding to the maximum value of the pore volume in the curve showing the pore distribution. In this case, absorbent A has a configuration in which there are more pores with a smaller pore radius than pores with a larger pore radius. The presence of more pores with a smaller pore radius makes it easier for capillary force to work, which makes it easier for the liquid absorption speed to become faster, and liquid can be instantly absorbed inside the pores.

[0096] Furthermore, the pores of absorbent A may have at least two maximum values ​​of pore volume in the curve showing the pore distribution. In this case, absorbent A has pores having a predetermined small pore radius and a pore radius nearby it, and pores having a predetermined large pore radius and a pore radius nearby it. Therefore, in pores with a relatively small pore radius, capillary force is likely to work, and therefore the liquid absorption speed is likely to be fast, and in pores with a relatively large pore radius, the liquid absorption volume is likely to be large. Therefore, due to the synergistic effect of the two, the polymer absorbent can instantly absorb a large amount of liquid inside the pores.

[0097] Here, in the case where there are two maxima of the pore volume in the pores of absorbent A, the two maxima of the pore volume in the curve showing the pore distribution may be such that the maximum value of the relatively small pore radius is larger than the maximum value of the relatively large pore radius. In this case, absorbent A has more pores with small pore diameters than pores with large pore radius. The presence of more pores with small pore radiuses makes it easier for capillary force to work, which makes it easier for the liquid absorption speed to become faster, and liquid can be instantly absorbed inside the pores.

[0098] On the other hand, even if there are two maxima in the pore volume of the pores of absorbent A, the two maxima in the pore volume in the curve showing the pore distribution may be such that the maximum value of the relatively small pore radius is smaller than the maximum value of the relatively large pore radius. In this case, absorbent A has more pores with large pore diameters than pores with small pore radius. The presence of more pores with large pore radiuses makes the liquid absorption volume larger, and a larger amount of liquid component can be absorbed inside the pores.

[0099] In addition, the pores of absorbent A have a bulk density of 0.07 to 0.6 g / cm 3 and preferably 0.1 to 0.4 g / cm 3 More preferably, the density is 0.15 to 0.35 g / cm 3 In this case, as described later, the liquid absorption speed (DW) performance can be set to 6 mL / 30 sec. or more, more preferably 10 mL / 30 sec. or more, and even more preferably 12 mL / 30 sec. or more. In other words, since the liquid absorption speed is increased, the polymer absorbent can instantly absorb liquid inside the pores.

[0100] <Method of measuring liquid absorption rate (DW)> The liquid absorption rate of the absorbent is measured by the non-pressurized DW (Demand Wettability) method. FIG. 12 is a schematic diagram showing a measuring device used in the non-pressurized DW method. A DW device (Demand Wettability device, manufactured by Taiyo Create Co., Ltd.) 11 is used as such a measuring device. As shown in the figure, the DW device 11 includes a burette 12 (50 ml graduated capacity, 86 cm long, 1.05 cm inner diameter), a rubber stopper 13, an air inlet capillary (3 mm inner diameter at tip) 14, a cock 15, a cock 16, a measuring table 17, a liquid outlet (3 mm inner diameter) 18, a cylinder 19, and a test liquid 20. A conduit (7 mm inner diameter) is attached from the burette 12 to the measuring table 17. A 0.9% sodium chloride aqueous solution is used as the test liquid. The measurement is performed in an atmosphere of 25°C x 50% humidity RH (constant temperature and humidity room).

[0101] The measurement procedure is as follows. (1) With both cocks 15, 16 of the DW apparatus 11 closed, pour the test liquid 20 above the 0 point (the top of the burette 12 scale (0 ml line)) and place the rubber stopper 13 on the top of the burette 12 to seal it. (2) After placing filter paper on the liquid outlet 18 of the measuring table 17, open both cocks 15 and 16 and adjust the liquid level to the zero point while using the filter paper to suck up the liquid coming out of the liquid outlet 18. After adjustment, close the cocks 15 and 16. (3) Place 100% wood pulp tissue (basis weight 15±1 gsm, thickness 0.1±0.02 mm when measured with a nonwoven fabric thickness meter at a pressure of 3 g / cm2) on the measurement table 17 with the liquid outlet 18 at the center. (4) A cylinder 19 with a diameter of 30 mm is placed in the center of the tissue, and a test object (polymeric absorbent) is placed in it, centered on the liquid outlet 18. The test object is placed in the cylinder 19, and its periphery is constrained by the cylinder 19. (5) Open the taps 15 and 16, and the measurement start time is the time when the test object begins to absorb the test liquid 20 and the first bubble introduced from the air inlet capillary 14 reaches the surface of the test liquid 20 in the burette 12 (the time when the surface of the test liquid 20 in the burette 12 drops). (6) Continuously read the amount of test liquid 20 in the burette 12 (the amount of test liquid 20 absorbed by the test object) M (ml). (7) The amount of absorption of the test object after a predetermined time has elapsed since the start of absorption (in this embodiment, after 30 seconds has elapsed) is calculated using the DW method: Absorption amount (ml / g) = M (ml) / (weight (g) of the test object (polymer absorbent)).

[0102] The following describes the state when the absorbent A comes into contact with liquid, but the same applies to the state when liquid comes into contact with the liquid-absorbent member or composite absorbent 4 containing the absorbent A. In addition, since the mass of absorbed liquid is approximately proportional to the amount of liquid, in the following description, the mass of liquid may be simply referred to as the "amount of liquid."

[0103] First, the continuous pores of the absorbent A shown in Figs. 4 to 8 are pores in which a plurality of pores (voids) are interconnected, and it is possible to visually confirm with the naked eye that a large number of voids are provided from the outside. When liquid comes into contact with the absorbent A having such a large number of voids, the hydrophilic continuous skeleton first instantly takes in a portion of the liquid due to osmotic pressure and expands (i.e., expands). This expansion of the continuous skeleton occurs in almost all directions. The absorbent A thus becomes enlarged by absorbing a certain amount of liquid, and is then able to absorb a further predetermined amount of liquid into the expanded continuous pores due to capillary action. Thus, when absorbing liquid, the absorbent A exhibits a unique liquid absorption behavior in which the liquid is taken in by the hydrophilic continuous skeleton and then taken in and absorbed by the continuous pores.

[0104] In addition, the liquid absorbed into the hydrophilic continuous skeleton of absorbent A is not easily released from the continuous skeleton (i.e., it is not easily synergized), whereas the liquid absorbed into the continuous pores is easily released. Therefore, within the composite absorbent, the liquid absorbed into the continuous pores synergizes and is transferred to the superabsorbent polymer (SAP) with high liquid retention capacity, and is steadily retained within the SAP. Here, the amount of liquid absorbed into the continuous skeleton of absorbent A and the amount of liquid absorbed into the continuous pores are determined as follows: out of the total amount of liquid absorbed by absorbent A, the amount of liquid released from absorbent A during centrifugation (amount of liquid released) is the amount of liquid absorbed into the continuous pores, and the remaining amount of liquid (i.e., the amount of liquid that did not release liquid from absorbent A during centrifugation) is the amount of liquid absorbed into the continuous skeleton.

[0105] Furthermore, of the liquid absorbed by absorbent A, more remains in the pores than in the hydrophilic continuous skeleton. Most of the liquid absorbed by absorbent A is achieved by retaining the liquid in the pores through capillary action, so the greater the porosity (the volume of the pores relative to the volume of absorbent A), which is the ratio of the volume of the voids in the pores (total pore volume), the more liquid can be absorbed. It is preferable that this porosity is 85% or more.

[0106] For example, when the porosity of the absorbent A shown in the above-mentioned Figs. 4 to 8 is calculated, it is as follows. First, the specific surface area of ​​absorbent A obtained by mercury porosimetry is 400 m 2 / g, and the pore volume is 15.5 mL / g. This pore volume of 15.5 mL / g means that the volume of the pores in 1 g of absorbent A is 15.5 mL. If the specific gravity of absorbent A is assumed to be 1 g / mL, the volume occupied by pores in 1 g of absorbent A, i.e., the pore volume, is 15.5 mL, and the volume of 1 g of absorbent A is 1 mL. In this case, the total volume (volume) of 1 g of absorbent A is 15.5 + 1 (mL), and the ratio of the pore volume to that is the porosity, so the porosity of absorbent A is 15.5 / (15.5 + 1) × 100 ≒ 94%.

[0107] In the present invention, the absorbent A having such a hydrophilic continuous skeleton and continuous pores, that is, a polymeric absorbent, is applied to the composite absorbent in the form of, for example, particles or a sheet. Furthermore, as described above, this polymer absorbent exhibits a unique liquid absorption behavior in which, when absorbing liquid, the liquid is first incorporated into the hydrophilic continuous skeleton and then into the continuous pores, so that it can instantly absorb a large amount of liquid and can transfer the absorbed liquid (mainly the liquid absorbed into the continuous pores) to the SAP with high water retention capacity and steadily retain it within the SAP. Therefore, a composite absorbent using such a polymer absorbent can exhibit high absorption performance as an absorbent.

[0108] However, the liquid absorption amount of the polymer absorbent can be measured according to the <Method for measuring the liquid absorption amount of the polymer absorbent> below.

[0109] <Method for measuring the amount of liquid absorbed by polymer absorbents> (1) 1 g of the measurement sample (polymer absorbent) is cut into a 10 cm square mesh bag (NBC Meshtec Co., Ltd., N-NO255HD 115 (standard width: 115 cm, 255 mesh / 2.54 cm, opening: 57 μm, wire diameter: 43 μm, thickness: 75 μm)) and enclosed. The mass (g) of the mesh bag is measured in advance. This measurement method is performed under conditions of a temperature of 25°C and a humidity of 60%. Furthermore, when the measurement sample (polymer absorbent) is to be recovered from a sanitary product and used, it can be obtained according to the <Recovery method of the measurement sample (polymer absorbent)> described below. (2) The mesh bag containing the sample is immersed in a 0.9% sodium chloride solution for one hour. (3) Hang the mesh bag for 5 minutes and measure the mass (g) after draining. (4) The amount of liquid absorbed by the sample (g) is calculated by subtracting the total mass of the sample (= 1 g) and the mesh bag from the mass of the mesh bag after draining measured in (3) above, and this amount of liquid absorbed is further divided by the mass of the sample (= 1 g) to obtain the amount of liquid absorbed per unit mass of the sample (polymer absorbent) (g / g).

[0110] In addition, when the measurement sample (polymer absorbent) is recovered from the composite absorbent product, it can be obtained according to the following <Method for recovering the measurement sample (polymer absorbent)>.

[0111] <How to collect the measurement sample (polymer absorbent)> (1) Peel off the retaining sheet or the like from the composite absorbent product to expose the liquid-absorbent member. (2) The object to be measured (polymer absorbent) is dropped from the exposed liquid-absorbent member, and anything other than the (particulate) object to be measured (e.g., pulp, synthetic resin fibers, etc.) is removed using tweezers or the like. (3) A microscope or a simple magnifying glass is used as a magnifying observation means, and the measurement object is collected using tweezers or the like while observing at a magnification at which the difference from SAP can be recognized or at which the pores of the porous body can be visually recognized. The magnification of the simple magnifying glass is not particularly limited as long as the pores of the porous body can be visually recognized, and may be, for example, 25 to 50 times. (4) The objects to be measured thus collected are used as samples for measurement in various measurement methods.

[0112] Hereinafter, the method for producing such a polymer absorbent will be described in detail using the above-mentioned absorbent A as an example.

[0113] [Method of manufacturing polymer absorbent] The above-mentioned absorbent A can be obtained through a cross-linking polymerization step and a hydrolysis step, as shown in Fig. 3. Each of these steps will be described below.

[0114] (Crosslinking polymerization process) First, an oil-soluble monomer for crosslinking polymerization, a crosslinkable monomer, a surfactant, water, and optionally a polymerization initiator are mixed to obtain a water-in-oil emulsion, which is an emulsion in which the oil phase is the continuous phase and water droplets are dispersed within it.

[0115] In the above-mentioned absorbent A, as shown in the upper diagram of Figure 3, butyl methacrylate, which is a (meth)acrylic acid ester, is used as the oil-soluble monomer, divinylbenzene is used as the cross-linking monomer, sorbitan monooleate is used as the surfactant, and isobutyronitrile is used as the polymerization initiator to cause cross-linking polymerization to obtain monolith A.

[0116] Specifically, for absorbent A, as shown in the upper diagram of Figure 3, first, 9.2 g of t-butyl methacrylate as an oil-soluble monomer, 0.28 g of divinylbenzene as a cross-linking monomer, 1.0 g of sorbitan monooleate (hereinafter abbreviated as "SMO") as a surfactant, and 0.4 g of 2,2'-azobis(isobutyronitrile) as a polymerization initiator are mixed and dissolved uniformly. Next, the mixture of t-butyl methacrylate / divinylbenzene / SMO / 2,2'-azobis(isobutyronitrile) is added to 180 g of pure water and stirred under reduced pressure using a planetary stirring device, a vacuum stirring and degassing mixer (manufactured by EME), to obtain a water-in-oil emulsion.

[0117] Furthermore, this emulsion is quickly transferred to a reaction vessel, sealed, and polymerized at 60°C for 24 hours under stationary conditions. After the polymerization is completed, the contents are removed, extracted with methanol, and then dried under reduced pressure to obtain Monolith A, which has a continuous macropore structure. The internal structure of Monolith A was observed by SEM, and it was found that Monolith A had a continuous cell structure and the thickness of the continuous skeleton was 5.4 μm. The average diameter of the continuous pores measured by mercury intrusion porosimetry was 36.2 μm, and the total pore volume was 15.5 mL / g.

[0118] The content of divinylbenzene in the total monomers is preferably 0.3 to 10 mol%, more preferably 0.3 to 5 mol%. The ratio of divinylbenzene to the total of butyl methacrylate and divinylbenzene is preferably 0.1 to 10 mol%, more preferably 0.3 to 8 mol%. In the above-mentioned absorbent A, the ratio of butyl methacrylate to the total of butyl methacrylate and divinylbenzene is 97.0 mol%, and the ratio of divinylbenzene is 3.0 mol%.

[0119] The amount of surfactant added can be set depending on the type of oil-soluble monomer and the desired size of emulsion particles (macropores), and is preferably in the range of about 2 to 70% of the total amount of the oil-soluble monomer and surfactant.

[0120] In order to control the shape and size of the bubbles in Monolith A, alcohols such as methanol and stearyl alcohol; carboxylic acids such as stearic acid; hydrocarbons such as octane, dodecane, and toluene; cyclic ethers such as tetrahydrofuran and dioxane, etc. may be allowed to coexist in the polymerization system.

[0121] In addition, the mixing method for forming the water-in-oil emulsion is not particularly limited, and any mixing method can be used, such as a method of mixing all the components at once, or a method of separately and uniformly dissolving oil-soluble components such as the oil-soluble monomer, surfactant, and oil-soluble polymerization initiator, and water-soluble components such as water and the water-soluble polymerization initiator, and then mixing the respective components.

[0122] Furthermore, the mixing device for forming the emulsion is not particularly limited, and any device such as a normal mixer, homogenizer, or high-pressure homogenizer can be used depending on the desired emulsion particle size. Furthermore, a so-called planetary mixing device can also be used in which the material to be treated is placed in a mixing container and rotated while revolving around the revolution axis while tilting the mixing container, thereby stirring and mixing the material to be treated.

[0123] In addition, there are no particular limitations on the mixing conditions, and the stirring rotation speed, stirring time, etc. can be set as desired according to the desired emulsion particle size. Note that, with the above planetary stirring device, water droplets in the W / O emulsion can be uniformly generated, and the average diameter can be set as desired within a wide range.

[0124] The polymerization conditions for the water-in-oil emulsion can be various, depending on the type of monomer and initiator, etc. For example, when azobisisobutyronitrile, benzoyl peroxide, potassium persulfate, etc. are used as the polymerization initiator, the polymerization can be carried out by heating in a sealed container under an inert atmosphere at a temperature of 30 to 100°C for 1 to 48 hours, and when hydrogen peroxide-ferrous chloride, sodium persulfate-acidic sodium sulfite, etc. are used as the polymerization initiator, the polymerization can be carried out in a sealed container under an inert atmosphere at a temperature of 0 to 30°C for 1 to 48 hours.

[0125] After the polymerization is completed, the contents are taken out and subjected to Soxhlet extraction with a solvent such as isopropanol to remove unreacted monomers and residual surfactants, thereby obtaining monolith A shown in the center diagram of Figure 3.

[0126] (Hydrolysis process) Next, the step of hydrolyzing the monolith A (crosslinked polymer) to obtain the absorbent A (hydrolysis step) will be described.

[0127] First, monolith A is immersed in dichloroethane containing zinc bromide and stirred at 40° C. for 24 hours, then contacted with methanol, 4% hydrochloric acid, 4% aqueous sodium hydroxide solution, and water in that order to carry out hydrolysis, and then dried to obtain a block-shaped absorbent A. Furthermore, this block-shaped absorbent A is crushed to a predetermined size to obtain a particulate absorbent A. Note that the form of this absorbent A is not limited to particulate, and for example, it may be formed into a sheet during or after drying.

[0128] In addition, the method of hydrolysis of monolith A is not particularly limited, and various methods can be adopted. For example, aromatic solvents such as toluene and xylene, halogen-based solvents such as chloroform and dichloroethane, ether-based solvents such as tetrahydrofuran and isopropyl ether, amide-based solvents such as dimethylformamide and dimethylacetamide, alcohol-based solvents such as methanol and ethanol, carboxylic acid-based solvents such as acetic acid and propionic acid, or water as a solvent are contacted with a strong base such as sodium hydroxide, or a hydrohalic acid such as hydrochloric acid, a Bronsted acid such as sulfuric acid, nitric acid, trifluoroacetic acid, methanesulfonic acid, and p-toluenesulfonic acid, or a Lewis acid such as zinc bromide, aluminum chloride, aluminum bromide, titanium (IV) chloride, cerium chloride / sodium iodide, and magnesium iodide.

[0129] Furthermore, among the polymerization raw materials of the organic polymer that forms the hydrophilic continuous skeleton of the absorbent A, the (meth)acrylic acid ester is not particularly limited, but is preferably a C1 to C10 (i.e., carbon number 1 to 10) alkyl ester of (meth)acrylic acid, and more preferably a C4 (i.e., carbon number 4) alkyl ester of (meth)acrylic acid. Examples of C4 alkyl esters of (meth)acrylic acid include t-butyl (meth)acrylic acid ester, n-butyl (meth)acrylic acid ester, and iso-butyl (meth)acrylic acid ester.

[0130] The monomers used in the crosslinking polymerization may be only (meth)acrylic acid esters and divinylbenzene, or may contain, in addition to (meth)acrylic acid esters and divinylbenzene, other monomers other than (meth)acrylic acid esters and divinylbenzene. In the latter case, the other monomers are not particularly limited, but examples thereof include styrene, α-methylstyrene, vinyltoluene, vinylbenzyl chloride, glycidyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isobutene, butadiene, isoprene, chloroprene, vinyl chloride, vinyl bromide, vinylidene chloride, tetrafluoroethylene, (meth)acrylonitrile, vinyl acetate, ethylene glycol di(meth)acrylate, and trimethylolpropane tri(meth)acrylate. The proportion of monomers other than (meth)acrylic acid ester and divinylbenzene in all monomers used in the crosslinking polymerization is preferably from 0 to 80 mol %, more preferably from 0 to 50 mol %.

[0131] The surfactant is not limited to the above-mentioned sorbitan monooleate, and may be any surfactant capable of forming a water-in-oil type (W / O) emulsion when the monomer for crosslinking polymerization is mixed with water. Examples of such surfactants include nonionic surfactants such as sorbitan monolaurate, sorbitan monopalmitate, sorbitan monostearate, sorbitan trioleate, polyoxyethylene nonylphenyl ether, polyoxyethylene stearyl ether, and polyoxyethylene sorbitan monooleate, anionic surfactants such as potassium oleate, sodium dodecylbenzenesulfonate, and dioctyl sodium sulfosuccinate, cationic surfactants such as distearyl dimethyl ammonium chloride, and amphoteric surfactants such as lauryl dimethyl betaine. These surfactants may be used alone or in combination of two or more.

[0132] In addition, the polymerization initiator is preferably a compound that generates radicals by heat and light irradiation. Furthermore, the polymerization initiator may be water-soluble or oil-soluble, and examples thereof include azobis(4-methoxy-2,4-dimethylvaleronitrile), azobisisobutyronitrile, azobisdimethylvaleronitrile, azobiscyclohexanenitrile, azobiscyclohexanecarbonitrile, azobis(2-methylpropionamidine)dihydrochloride, benzoyl peroxide, potassium persulfate, ammonium persulfate, hydrogen peroxide-ferrous chloride, sodium persulfate-acidic sodium sulfite, and tetramethylthiuram disulfide. However, in some cases, there are systems in which polymerization proceeds only by heating or light irradiation without the addition of a polymerization initiator, and in such systems, the addition of a polymerization initiator is not necessary. EXAMPLES

[0133] The present invention will be described below with reference to examples, but the present invention is not limited to these examples.

[0134] (A) Sample (a) Pore distribution The polymer absorbents of the present invention manufactured by the above manufacturing method were used as samples of Examples 1 to 5, and Infinity particles were used as samples of Comparative Examples 1 and 2. However, for the samples of Examples 1 to 5, the surfactant / monomer ratio (wt%) and the stirring time (min) were changed when forming the water-in-oil type emulsion in the manufacturing method. Infinity particles are absorbents manufactured by P&G, and although they have a structure (foam structure) similar to that of polymer absorbents, they do not have the function of absorbing liquid and expanding, unlike polymer absorbents. (b) Relationship between bulk density and liquid absorption rate Regarding the samples of the above examples, samples with various bulk densities were prepared by changing the conditions of ethanol immersion and drying. Specifically, the dried polymer absorbent was thoroughly immersed in a 40% ethanol aqueous solution, and then the supernatant liquid was removed and ethanol was added repeatedly to adjust the ethanol aqueous solution to a predetermined concentration. After thorough immersion, the wet polymer absorbent was filtered and dried overnight at 50°C under reduced pressure to obtain polymer absorbents with different bulk densities.

[0135] (B) Evaluation (a) Pore distribution Using mercury intrusion porosimetry, the cumulative (integrated) pore volume distribution (relationship between pore radius and cumulative pore volume) and log differential pore volume distribution (relationship between pore radius and log differential pore volume) were determined for each sample, and the total pore volume (mL / g), average pore radius (μm), maximum pore radius (μm), pore volume (proportion) of pores with a specified pore radius or more (or less), and pore volume variation coefficient were calculated. (b) Relationship between bulk density and liquid absorption rate The relationship between the bulk density and the liquid absorption rate (DW) of each sample was examined by measuring the liquid absorption rate (DW).

[0136] (C) Evaluation Results (a) Pore distribution The measurement results are shown in Figures 9 and 10, and a summary of them is shown in Table 1. Note that Figure 9 shows the obtained cumulative (integrated) pore volume distribution, i.e., the relationship between the pore radius (horizontal axis) and the cumulative pore volume (vertical axis), and Figure 10 shows the obtained log differential pore volume distribution, i.e., the relationship between the pore radius (horizontal axis) and the log differential pore volume (vertical axis). Note that in Figures 9 and 10, Example 1 is shown as a dashed line (thick line), Example 2 is shown as a dashed line (thin line), Example 3 is shown as a dashed line (thin line), Example 4 is shown as a dotted line, Example 5 is shown as a solid line (thin line), Comparative Example 1 is shown as a solid line (thick line), and Comparative Example 2 is shown as a dashed line (thick line).

[0137] [Table 1] *Pore radius 1μm or more

[0138] For the samples of Examples 1 to 5, the following was confirmed. The ratio of the pore volume of pores with a pore radius of 1 μm or more was 90% or more of the pore volume of all pores. The ratio of the pore volume of pores with a pore radius of 0.005 μm or less was less than 10% of the pore volume of all pores. The pore radius at the maximum pore volume was 500 μm or less. The coefficient of variation of the pore distribution in pores with a pore radius of 1 μm or more was sometimes 1.4 or less (Example 3). The coefficient of variation of the pore distribution in pores with a pore radius of 1 μm or more was sometimes more than 1.4 (Examples 4 and 5). In the curve showing the pore distribution, the part on the side with a larger pore radius was broader than the part on the side with a smaller pore radius with respect to the pore radius corresponding to the maximum value of the pore volume in the curve showing the pore distribution (Example 5). In the curve showing the pore distribution, the part on the side with a smaller pore radius was broader than the part on the side with a larger pore radius with respect to the pore radius corresponding to the maximum value of the pore volume in the curve showing the pore distribution (Example 4). There were at least two maximum values ​​of the pore volume in the curve showing the pore distribution (Examples 1 and 2). In the curve showing the pore distribution, the maximum value of the relatively small pore radius was larger than the maximum value of the relatively large pore radius in some cases (Example 2). In the curve showing the pore distribution, the maximum value of the relatively small pore radius was smaller than the maximum value of the relatively large pore radius in some cases (Example 1). The total pore volume was 0.9 mL / g or more. On the other hand, in Comparative Examples 1 and 2, the proportion of the pore volume of pores with a pore radius of 1 μm or more was less than 90% of the pore volume of all pores.

[0139] (b) Relationship between bulk density and liquid absorption rate The measurement results are shown in Figure 11. Figure 11 is a graph showing the relationship between the obtained bulk density (horizontal axis) and the liquid absorption rate (vertical axis). As shown in the figure, the bulk density was 0.07 to 0.6 g / cm 3 It was confirmed that the liquid absorption rate (DW) performance can be increased to 6mL / 30sec or more by setting the bulk density to 0.1-0.4g / cm 3 It was confirmed that the water absorption rate (DW) performance can be increased to 10 mL / 30 sec. or more by setting the bulk density to 0.15 to 0.35 g / cm. 3It was confirmed that by doing so, it is possible to achieve a liquid absorption rate (DW) of 12 mL / 30 sec. or more.

[0140] The composite absorbent of the present invention is not particularly limited, but can be applied to various fields of composite absorbents such as dew condensation prevention sheets, simple soil, and other civil engineering and construction materials, base materials for medicines, and materials for absorbing leaked liquids. Therefore, the liquid to be absorbed by the composite absorbent is not particularly limited, and examples thereof include water and aqueous solutions (e.g., seawater, etc.), acids (e.g., hydrochloric acid, etc.), bases (e.g., sodium hydroxide, etc.), organic solvents (e.g., alcohols such as methanol and ethanol, ketones such as acetone, ethers such as tetrahydrofuran (THF) and 1,4-dioxane, N,N-dimethylformamide (DMF), dimethyl sulfoxide (DMSO), etc.). These liquids may be mixtures of two or more liquids.

[0141] Furthermore, the present invention is not limited to the above-described embodiments, and appropriate combinations, substitutions, modifications, etc. are possible within the scope of the object and intent of the present invention. Note that in this specification, ordinal numbers such as "first" and "second" are used to distinguish the items to which the ordinal numbers are attached, and do not indicate the order, priority, importance, etc. of each item. [Explanation of symbols]

[0142] 1 Composite absorber 2. First retaining sheet 3 Second Retaining Sheet 4. Polymer absorbents 5. Superabsorbent polymer (SAP) 6 Hydrophilic fiber sheet

Claims

1. 1. A composite absorbent for absorbing liquid, comprising: The present invention relates to a polymeric absorbent material having a hydrophilic continuous skeleton and continuous pores, In the polymer absorbent, the ratio of the pore volume of pores having a pore radius of 1 μm or more to the pore volume of all pores is 90% or more, In the polymer absorbent, the pore radius at the maximum pore volume is 500 μm or less; In the polymer absorbent, the coefficient of variation of the pore distribution is more than 1.4 in pores having a pore radius of 1 μm or more. Composite absorber.

2. In the polymer absorbent, the ratio of the pore volume of pores having a pore radius of 0.005 μm or less is less than 10% of the pore volume of all pores. The composite absorbent body of claim 1.

3. 3. The composite absorbent according to claim 1 or 2, characterized in that in the polymer absorbent, the portion of the pore radius larger than the portion of the pore radius smaller than the pore radius corresponding to the maximum value of the pore volume in the curve showing the pore distribution is broader.

4. 3. The composite absorbent according to claim 1 or 2, characterized in that in the polymer absorbent, the portion on the side where the pore radius is smaller is broader than the portion on the side where the pore radius is larger, relative to the pore radius corresponding to the maximum value of the pore volume in a curve showing the pore distribution.

5. A composite absorbent for absorbing liquid, comprising: The present invention relates to a polymeric absorbent material having a hydrophilic continuous skeleton and continuous pores, In the polymer absorbent, the ratio of the pore volume of pores having a pore radius of 1 μm or more to the pore volume of all pores is 90% or more, In the polymer absorbent, the pore radius at the maximum pore volume is 500 μm or less; A composite absorbent body, characterized in that in the polymer absorbent, there are at least two maximum values ​​of pore volume in a curve showing the pore distribution.

6. The composite absorbent according to claim 5, characterized in that in the polymer absorbent, the two maximum values ​​of pore volume in the curve showing the pore distribution are such that the maximum value of the relatively small pore radius is larger than the maximum value of the relatively large pore radius.

7. The composite absorbent according to claim 5, characterized in that in the polymer absorbent, the two maximum values ​​of pore volume in the curve showing the pore distribution are such that the maximum value of the relatively small pore radius is smaller than the maximum value of the relatively large pore radius.

8. The composite absorbent according to any one of claims 1 to 7, wherein the polymer absorbent has a total pore volume of 0.9 mL / g or more.

9. The polymer absorbent has a bulk density of 0.07 to 0.6 g / cm 3 The composite absorbent body according to any one of claims 1 to 8, characterized in that

10. The composite absorbent according to any one of claims 1 to 9, wherein the polymer absorbent is a monolithic absorbent.

11. A composite absorbent for absorbing liquid, comprising: The present invention relates to a polymeric absorbent material having a hydrophilic continuous skeleton and continuous pores, In the polymer absorbent, the ratio of the pore volume of pores having a pore radius of 1 μm or more to the pore volume of all pores is 90% or more, In the polymer absorbent, the pore radius at the maximum pore volume is 500 μm or less; The polymer absorbent is a hydrolysis product of a crosslinked polymer of a (meth)acrylic acid ester and a compound containing two or more vinyl groups in one molecule, and contains at least one -COONa group.

12. It has a hydrophilic continuous skeleton and continuous pores, The proportion of the pore volume of pores having a pore radius of 1 μm or more is 90% or more of the pore volume of all pores, The pore radius at the maximum pore volume is 500 μm or less, The coefficient of variation of the pore distribution is greater than 1.4 for pores having a pore radius of 1 μm or more; Polymer absorbent.

13. A hydrophilic continuous skeleton and continuous pores, The proportion of the pore volume of pores having a pore radius of 1 μm or more is 90% or more of the pore volume of all pores, The pore radius at the maximum pore volume is 500 μm or less, The pore volume maximum in the pore distribution curve is characterized by having at least two maximum values. Polymer absorbent.

14. A hydrophilic continuous skeleton and continuous pores, The proportion of the pore volume of pores having a pore radius of 1 μm or more is 90% or more of the pore volume of all pores, The pore radius at the maximum pore volume is 500 μm or less, The present invention is characterized in that the crosslinked polymer is a hydrolyzate of a crosslinked polymer of a (meth)acrylic acid ester and a compound containing two or more vinyl groups in one molecule, and contains at least one -COONa group. Polymer absorbent.

Citation Information

Patent Citations

  • Polymer beads and their manufacturing method

    JP1998505118A

  • Moisture / Water absorbing exothermic diaper

    JP2003102784A

  • Monolithic organic porous material, method for producing the same, and monolithic organic porous ion exchanger

    JP2009221428A

  • Polyolefin porous sinter molding body

    JP2017137432A

  • Absorbent foam materials for aqueous body fluids and absorbent articles containing such materials

    JP3231320B2