Negative electrode and non-aqueous electrolyte secondary battery

The negative electrode design with distinct resin binders and a silicon-inhibiting resin in the second layer addresses silicon expansion, enhancing battery performance by reducing swelling and maintaining capacity.

JP7592043B2Active Publication Date: 2024-11-29PRIME PLANET ENERGY & SOLUTIONS INC
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2022066749
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-04-14
Publication Date
2024-11-29
Estimated Expiration
2042-04-14

AI Technical Summary

Technical Problem

Silicon-containing materials in negative electrodes of non-aqueous electrolyte secondary batteries undergo significant volumetric expansion during charging and discharging, leading to increased electrode thickness and the need for bulky mechanical components to manage the reaction force, which is undesirable for space-constrained applications.

Method used

A negative electrode design with a first active material layer containing graphite and a second active material layer containing a silicon-containing material, using different resin binders, where the second binder includes a silicon swelling-inhibiting resin, such as polyacrylamide, to suppress volumetric expansion.

Benefits of technology

The design effectively suppresses volumetric expansion, maintaining electrode thickness and improving battery performance by reducing swelling and maintaining capacity retention.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007592043000002
    Figure 0007592043000002
  • Figure 0007592043000003
    Figure 0007592043000003
  • Figure 0007592043000004
    Figure 0007592043000004
Patent Text Reader

Abstract

To provide a negative electrode containing a silicon-containing substance and suppressed in cubical expansion, and a nonaqueous electrolyte secondary battery including the same.SOLUTION: Provided is a negative electrode for a nonaqueous electrolyte secondary battery, the negative electrode including a current collector, a first active material layer and a second active material layer in the order. The first active material layer includes a first binder and a graphite material, and the second active material layer includes a second binder and a silicon-containing substance. The first binder and the second binder contain resin components different from each other. A BET specific surface area of the graphite material is 1.6 m2 / g or less. The resin component in the second binder includes a silicon swelling suppressing resin.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a negative electrode and a non-aqueous electrolyte secondary battery. [Background technology]

[0002] Patent Document 1 (JP 2015-179575 A) proposes using a silicon-containing material as an active material in a negative electrode for the purpose of increasing the capacity of a non-aqueous electrolyte secondary battery. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2015-179575 A Summary of the Invention [Problem to be solved by the invention]

[0004] Silicon-containing materials are prone to volume expansion, and the thickness of the electrode plates tends to increase with repeated charging and discharging. In order to suppress the reaction force (the force that pushes the battery can apart) that occurs due to the increase in the thickness of the electrode plates from the outside, mechanical parts of a size corresponding to the reaction force are required. However, from the perspective of the space in which the battery is installed, it is desirable for the mechanical parts to be space-saving, and there is a demand for reducing the reaction force.

[0005] An object of the present disclosure is to provide a negative electrode containing a silicon-containing material, in which volume expansion is suppressed, and a nonaqueous electrolyte secondary battery including the same. [Means for solving the problem]

[0006] The present disclosure provides the following negative electrode and nonaqueous electrolyte secondary battery. [1] A negative electrode for a non-aqueous electrolyte secondary battery, comprising a current collector, a first active material layer, and a second active material layer in this order, the first active material layer containing a first binder and a graphite material, the second active material layer containing a second binder and a silicon-containing material, the first binder and the second binder containing different resin components, and the graphite material having a BET specific surface area of ​​1.6 m 2 / g or less, and the resin component in the second binder contains a silicon swelling inhibiting resin. [2] The negative electrode according to [1], wherein the silicon expansion inhibiting resin is polyacrylamide. [3] The negative electrode according to [1] or [2], wherein the active material in the second active material layer is only the silicon-containing material. [4] The negative electrode according to any one of [1] to [3], wherein the active material in the first active material layer is the graphite material alone, or is the graphite material and a silicon-containing material. [5] The negative electrode according to any one of [1] to [4], wherein a mass ratio of the total silicon-containing material to the total active materials contained in the first active material layer and the second active material layer is 40% or less. [6] The negative electrode according to any one of [1] to [5], wherein the first binder does not contain a silicon expansion inhibiting resin. [7] The negative electrode according to any one of [1] to [6], wherein the second binder contains only a silicon expansion inhibiting resin. [8] A non-aqueous electrolyte secondary battery comprising the negative electrode according to any one of [1] to [7], a positive electrode, and a non-aqueous electrolyte. Effect of the Invention

[0007] According to the present disclosure, it is possible to provide a negative electrode containing a silicon-containing material in which volume expansion is suppressed, and a nonaqueous electrolyte secondary battery including the same. [Brief description of the drawings]

[0008] [Figure 1] FIG. 1 is a schematic diagram showing an example of the configuration of the negative electrode in this embodiment. [Diagram 2]FIG. 2 is a schematic flow chart showing a method for producing a negative electrode. [Diagram 3] FIG. 3 is a schematic diagram showing an example of the configuration of the battery in this embodiment. [Figure 4] FIG. 4 is a schematic diagram showing an example of the configuration of the electrode body in this embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, an embodiment of the present invention will be described with reference to the drawings, but the present disclosure is not limited to the following embodiment. In all of the drawings, the scale of each component is appropriately adjusted to make it easier to understand, and the scale of each component shown in the drawings does not necessarily match the scale of the actual component.

[0010] The negative electrode of the present disclosure will be described with reference to the drawings. The negative electrode 100 shown in FIG. 1 is a negative electrode for a non-aqueous electrolyte secondary battery. The negative electrode 100 includes a current collector 10 and a negative electrode active material layer 20. The negative electrode active material layer 20 includes a first active material layer 30 and a second active material layer 40 laminated in this order from the current collector 10 side. In the negative electrode of the present disclosure, the negative electrode active material layer may be provided on only one side of the current collector, or on both sides. Although not shown, the negative electrode 100 may have another layer interposed between the current collector 10 and the first active material layer 30 and / or between the first active material layer 30 and the second active material layer 40. For example, a coating layer may be provided on the current collector 10, and an intermediate layer in which components are mixed may be provided between the first active material layer 30 and the second active material layer 40.

[0011] The current collector 10 is a conductive sheet. The current collector 10 may include, for example, an aluminum (Al) foil, a copper (Cu) foil, or the like. The current collector 10 may have a thickness of, for example, 5 μm to 50 μm. For example, a coating layer may be formed on the surface of the current collector 10. The coating layer may include, for example, a conductive carbon material, or the like. The coating layer may have a thickness smaller than that of the negative electrode active material layer 20, for example.

[0012] The first active material layer 30 includes a first binder (not shown) and a graphite material 31. The first binder can bind the active materials together. The first binder can bind the active materials to the current collector. The first binder and a second binder described below contain different resin components. By the first binder and a second binder described below containing different resin components, the volume expansion of the negative electrode tends to be easily suppressed.

[0013] The first binder may contain at least one selected from the group consisting of polyvinylidene fluoride (PVdF), poly(vinylidene fluoride-co-hexafluoropropylene) (PVdF-HFP), polytetrafluoroethylene (PTFE), polyacrylic acid (PAA), carboxymethyl cellulose (CMC), polyethylene oxide (PEO), and styrene butadiene rubber (SBR). The first binder preferably does not contain a silicon swelling inhibiting resin described below. The amount of the first binder may be, for example, 0.1 to 10 parts by mass per 100 parts by mass of the active material in the first active material layer 30.

[0014] The first active material layer 30 contains a graphite material 31 as an active material. The graphite material 31 may contain at least one selected from the group consisting of graphite, soft carbon (easily graphitizable carbon), and hard carbon (non-graphitizable carbon). The BET specific surface area of ​​the graphite material 31 is 1.6 m 2 / g or less, preferably 1.3m 2 / g or less, more preferably 1.1m 2 / g or less. In the first active material layer 30, the BET specific surface area is 1.6 m 2 / g or less, there is a tendency to easily suppress volume expansion of the first active material layer 30. The BET specific surface area is measured by a BET multipoint method.

[0015] The first active material layer 30 may further include a silicon-containing material as an active material. The silicon-containing material may be, for example, substantially composed of Si metal (simple substance of Si). The silicon-containing material may include, for example, a Si-based alloy. The silicon-containing material may include at least one selected from the group consisting of a SiCu alloy, a SiNi alloy, a SiAl alloy, and a SiZn alloy. The silicon-containing material may include, for example, a Si compound. The silicon-containing material may include, for example, a silicon oxide. The silicon-containing material may include, for example, SiOx (0.5≦x≦1.5). The silicon-containing material may include, for example, a composite material of Si and other materials. The silicon-containing material may include, for example, a Si / C composite material. The Si / C composite material may be formed by supporting Si metal, Si oxide, etc. on a carbon material (graphite, amorphous carbon, etc.). The silicon-containing substance may include, for example, at least one selected from the group consisting of a Si metal, a Si-based alloy, a Si oxide, and a Si / C composite material.

[0016] The first active material layer 30 preferably contains only the graphite material 31, or contains the graphite material 31 and a silicon-containing material, as an active material. The first active material layer 30 may contain, for example, 50 parts by mass to 100 parts by mass of the graphite material 31, preferably 60 parts by mass to 100 parts by mass of the graphite material 31, and more preferably 80 parts by mass to 100 parts by mass of the graphite material 31, relative to 100 parts by mass of the active material in the first active material layer 30. When the first active material layer 30 contains the graphite material 31 and a silicon-containing material, the mass ratio of the graphite material and the silicon-containing material may be, for example, 99:1 to 1:99, preferably 99:1 to 70:30, and more preferably 99:1 to 90:10. The first active material layer 30 may contain, as other active materials, Sn, SnO, an Sn-based alloy, and Li4Ti5O 12 may further comprise at least one selected from the group consisting of:

[0017] The second active material layer 40 contains a second binder (not shown) and a silicon-containing material 41. The second binder can bind the active materials together. The second binder can bind the active materials and the second active material layer 40. The resin component in the second binder contains a silicon expansion inhibiting resin. When the second active material layer 40 contains a silicon expansion inhibiting resin, expansion of the negative electrode tends to be easily inhibited.

[0018] Examples of silicon expansion inhibitory resins include polyacrylamide (PAAm). From the viewpoint of expansion inhibition, the silicon expansion inhibitory resin may preferably have a higher number of hydrogen bonds than the resin component of the first binder. From the viewpoint of expansion inhibition, it is more preferable that the first binder contains CMC and SBR, and the second binder contains PAAm. The resin component in the second binder may further contain a resin other than the silicon expansion inhibitory resin. As the resin other than the silicon expansion inhibitory resin, the above-mentioned examples of the first binder are applicable. The second binder preferably contains only the silicon expansion inhibitory resin as the resin component. The amount of the second binder may be, for example, 0.1 to 15 parts by mass with respect to 100 parts by mass of the active material.

[0019] The second active material layer 40 contains a silicon-containing material 41 as an active material. The explanation of the silicon-containing material is the same as that of the first active material layer 30. The second active material layer 40 may contain the graphite material and other active materials in the first active material layer 30 as active materials other than the silicon-containing material 41. The second active material layer 40 preferably contains only the silicon-containing material 41 as an active material.

[0020] The second active material layer 40 may contain, for example, 1 part by mass to 100 parts by mass of silicon-containing material 41 relative to 100 parts by mass of the active material in the second active material layer 40, preferably contains 50 parts by mass to 100 parts by mass of silicon-containing material 41, and more preferably contains 80 parts by mass to 100 parts by mass of silicon-containing material 41. The mass ratio of the total silicon-containing material to the total active materials contained in the first active material layer and the second active material layer is 40% or less, and preferably 30% or less.

[0021] The first active material layer 30 and the second active material layer 40 may contain the active material in the form of active material particles. The active material particles contain an active material. The active material particles may further contain components other than the active material. The active material particles may have any size. The average particle diameter of the active material particles may be, for example, 1 μm to 50 μm, 1 μm to 35 μm, or 1 μm to 25 μm. In this specification, the average particle diameter of the active material particles refers to a particle diameter at which the cumulative particle volume from the small particle diameter side in the volume-based particle size distribution is 50% of the total particle volume. In this specification, the average particle diameter of the active material particles may also be expressed as D50. The average particle diameter may be measured by a laser diffraction / scattering method.

[0022] The method for producing the negative electrode 100 may include preparing a slurry (A1), applying (B1), drying (C1) and compressing (D1). FIG. 2 is a schematic flow chart showing the method for producing the negative electrode 100. In the present disclosure, the first active material layer 30 may be formed first, and then the second active material layer 40 may be formed on the first active material layer 30. The preparation of the slurry (A1) may include mixing an active material, a binder and an organic solvent. The organic solvent may include at least one selected from the group consisting of, for example, N-methyl-2-pyrrolidone (NMP), tetrahydrofuran (THF), dimethylformamide (DMF), methyl ethyl ketone (MEK) and dimethyl sulfoxide (DMSO). The amount of the organic solvent used is arbitrary. That is, the slurry may have any solid content concentration (mass fraction of solid content). The slurry may have a solid content concentration of, for example, 40% to 80%. Any stirring device, mixing device or dispersing device may be used for mixing.

[0023] Coating (B1) may include forming a coating film by coating the slurry on the surface of the substrate. In this embodiment, the slurry may be coated on the surface of the substrate by any coating device. For example, a slot die coater, a roll coater, etc. may be used. The coating device may be capable of multi-layer coating.

[0024] Drying (C1) may include heating the coating film to dry it. In this embodiment, any drying device may be used as long as the coating film can be heated. For example, the coating film may be heated by a hot air dryer or the like. Heating the coating film may cause the organic solvent to evaporate. This allows the organic solvent to be substantially removed.

[0025] In the present embodiment, the compression (D1) may include compressing the dried coating film to form an active material layer. Any compression device may be used. For example, a rolling machine or the like may be used. The dried coating film is compressed to form an active material layer, and the negative electrode 100 is completed. The negative electrode 100 may be cut to a predetermined planar size according to the specifications of the battery. The negative electrode 100 may be cut to have, for example, a strip-like planar shape. The negative electrode 100 may be cut to have, for example, a rectangular planar shape.

[0026] <Nonaqueous electrolyte secondary battery> FIG. 3 is a schematic diagram showing an example of a battery in this embodiment. The battery is a non-aqueous electrolyte secondary battery. The battery 200 shown in FIG. 3 includes an exterior body 90. The exterior body 90 houses an electrode body 50 and an electrolyte (not shown). The electrode body 50 is connected to a positive electrode terminal 91 by a positive electrode current collector 81. The electrode body 50 is connected to a negative electrode terminal 92 by a negative electrode current collector 82. FIG. 4 is a schematic diagram showing an example of an electrode body in this embodiment. The electrode body 50 is a wound type. The electrode body 50 includes a positive electrode 20, a separator 70, and a negative electrode 100. That is, the battery 200 includes the negative electrode 100. The positive electrode 60 includes a positive electrode active material layer 62 and a positive electrode current collector 61. The negative electrode 100 includes a negative electrode active material layer 20 and a current collector (negative electrode current collector) 10. EXAMPLES

[0027] The present disclosure will be described in more detail below with reference to examples. In the examples, "%" and "parts" are by mass % and parts by mass unless otherwise specified.

[0028] <Example 1> 100 parts by mass of graphite (C) as a negative electrode active material, 2.5 parts by mass of styrene butadiene rubber (SBR) as a binder, and 2.5 parts by mass of carboxymethyl cellulose (CMC) as a thickener were mixed in ion-exchanged water to prepare a first negative electrode composite slurry. Silicon oxide (SiO X 100 parts by mass of the sintered body 20 was mixed with 5 parts by mass of polyacrylamide (PAAm) as a binder in ion-exchanged water to prepare a second negative electrode composite slurry.

[0029] The first negative electrode composite slurry was applied to both sides of a copper foil negative electrode current collector, dried, and pressed and rolled with a rolling roller. Next, the second negative electrode composite slurry was applied to the dried coating of the first negative electrode composite slurry, dried, and rolled in the same manner as above. As a result, a negative electrode sheet of Example 1 was obtained in which a negative electrode active material layer including a first active material layer formed by the first negative electrode composite slurry and a second active material layer formed by the second negative electrode composite slurry was supported on a negative electrode current collector.

[0030] LiNi as a positive electrode active material 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (NCM), acetylene black (AB) as a conductive material, and polyvinylidene fluoride (PVdF) as a binder were mixed in N-methylpyrrolidone (NMP) in a mass ratio of NCM:AB:PVdF=97:2:1 to prepare a positive electrode composite slurry. This positive electrode composite slurry was applied onto an aluminum foil. It was then dried and roll-pressed to a predetermined thickness to produce a positive electrode sheet.

[0031] A porous polyolefin sheet having a three-layer structure of PP / PE / PE was prepared as a separator. The positive electrode sheet and the negative electrode sheet were stacked with the separator interposed therebetween and wound to obtain a wound body. The wound body was pressed to produce a flat wound electrode body.

[0032] An electrode terminal was attached to the electrode body, which was then inserted into a case made of an aluminum laminate film and welded, after which a non-aqueous electrolyte was poured in. The non-aqueous electrolyte used was a mixed solvent containing ethylene carbonate (EC) and dimethyl carbonate (DEC) in a volume ratio of 3:7, in which LiPF6 was dissolved at a concentration of 1.0 mol / L. The laminate case was then sealed to obtain a lithium-ion secondary battery for evaluation.

[0033] <Examples 2 to 4 and Comparative Examples 1 to 3> A negative electrode sheet was produced in the same manner as in Example 1 except that the materials and Si ratios shown in Table 1 were used, and a lithium ion secondary battery for evaluation was produced using the negative electrode sheet.

[0034] <Activation of evaluation lithium-ion secondary batteries> The lithium-ion secondary batteries for evaluation were placed in an environment of 25° C. Activation (initial charging) was performed using a constant current-constant voltage method, with each lithium-ion secondary battery for evaluation being charged at a constant current of 1 / 3 C up to 4.2 V, and then charged at a constant voltage until the current reached 1 / 50 C, until the battery was fully charged. After that, each lithium-ion secondary battery for evaluation was discharged at a constant current of 1 / 3 C up to 3.0 V.

[0035] <Swelling rate> After discharging the cell to 3.0V, several points (approximately 3 points) on the flat part of the cell were measured using a Mitutoyo micrometer (spindle diameter Φ6.3), and the average value was taken as the cell thickness. The change in cell thickness was measured at regular cycles, and the increase rate (%) from the initial value was taken as the swelling rate. The increase rate (%) from the initial value was evaluated as the swelling rate. The thickness was measured after initial activation (after discharge), and this thickness was taken as the initial thickness. A cycle test was then performed, and the final thickness was measured after 100 cycles to determine the increase rate. If the swelling rate was less than 105%, it was evaluated as "◎", if it was 105% or more but less than 110%, it was evaluated as "○", if it was 110% or more but less than 120%, it was evaluated as "△", if it was 120% or more but less than 130%, it was evaluated as "×", and if it was 130% or more, it was evaluated as "XX".

[0036] <Capacity retention rate measurement> Each activated lithium-ion secondary battery for evaluation was placed in an environment of 25°C. 100 cycles of charge and discharge were performed, with one cycle consisting of constant current charging at a current value of 0.5C up to 4.2V and constant current discharging at a current value of 0.5C up to 3.0V. The discharge capacities at the first and 100th cycles were measured, and the ratio of the discharge capacity at the 100th cycle to the discharge capacity at the first cycle was calculated as the capacity retention rate (%). If the capacity retention rate at this time was 95% or more, it was evaluated as "◎", if it was 85% or more but less than 95%, it was evaluated as "○", and if it was less than 85%, it was evaluated as "△". The results are shown in Table 1.

[0037] <Battery resistance measurement> Each activated lithium ion secondary battery for evaluation was adjusted to a state of SOC 50%. It was left to stand for 1 hour in an environment of 25°C. Then, constant current discharge was performed at a current value of 3C for 10 seconds. The voltage drop amount ΔV at this time was obtained, and the battery resistance was calculated by dividing ΔV by the current value (3C). When the resistance of the lithium ion secondary battery for evaluation in Example 1 was taken as 100%, if it was less than 90%, it was evaluated as "◎", if it was 90% or more and less than 120%, it was evaluated as "○", and if it was 120% or more, it was evaluated as "×". The results are shown in Table 1.

[0038] [Table 1] In the table, the Si content indicates the mass ratio of the silicon-containing material in the entire negative electrode active material layer.

[0039] In Examples 1 to 4, negative electrodes were produced that satisfied all of the swelling ratio, capacity retention rate, and battery resistance. In Comparative Example 1, the battery resistance tended to decrease. In Comparative Example 2, the decrease in the swelling ratio due to the cycle test was significant. In Comparative Example 3, the effect of suppressing swelling in the entire electrode tended to be small. [Explanation of symbols]

[0040] DESCRIPTION OF SYMBOLS 1, 2 positive electrode active material, 10 current collector, 20 negative electrode active material layer, 30 first active material layer, 31 graphite material, 40 second active material layer, 41 silicon-containing material, 50 electrode body, 60 positive electrode, 61 positive electrode current collector, 62 positive electrode active material layer, 70 separator, 81 positive electrode current collector, 82 negative electrode current collector, 90 exterior body, 91 positive electrode terminal, 92 negative electrode terminal, 100 negative electrode, 200 battery.

Claims

1. A negative electrode for a non-aqueous electrolyte secondary battery, comprising: a current collector, a first active material layer, and a second active material layer in this order; the first active material layer includes a first binder and a graphite material; the second active material layer includes a second binder and a silicon-containing material, the first binder and the second binder contain different resin components, The BET specific surface area of ​​the graphite material is 1.6 m 2 / g or less, A negative electrode, wherein the resin component in the second binder contains only polyacrylamide.

2. 2. The negative electrode of claim 1, wherein the silicon-containing material is the only active material in the second active material layer.

3. 3. The negative electrode of claim 1 or 2, wherein the active material in the first active material layer is the graphite material alone or is the graphite material and a silicon-containing material.

4. 3. The negative electrode according to claim 1, wherein a mass ratio of the total silicon-containing material to the total active materials contained in the first active material layer and the second active material layer is 40% or less.

5. The negative electrode according to claim 1 or 2, wherein the first binder does not include polyacrylamide.

6. A non-aqueous electrolyte secondary battery comprising the negative electrode according to claim 1 or 2, a positive electrode, and a non-aqueous electrolyte.

Citation Information

Patent Citations

  • Negative plate and lithium ion battery

    CN110148708A

  • Negative electrode for secondary battery, manufacturing method of secondary battery and negative electrode for secondary battery

    JP2003249211A

  • Negative electrode for nonaqueous electrolyte secondary batteries, method for manufacturing the same, and nonaqueous electrolyte secondary battery

    JP2015179575A

  • Device and method for forming the device

    JP2015537347A

  • Binder composition for electrochemical device

    JP2020077620A