Hexagonal boron nitride powder for fillers
By controlling primary particle thickness and diameter ratio and stabilizing the crystal structure of h-BN powder through specific manufacturing processes, the issues of boron elution and reduced thermal conductivity are addressed, resulting in enhanced filling properties and thermal conductivity in resin applications.
Patent Information
- Application Number
- JP2023549703
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-09-27
- Filing Date
- 2022-09-20
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2042-09-20
AI Technical Summary
Conventional hexagonal boron nitride (h-BN) powders exhibit insufficient filling properties and thermal conductivity when used as fillers due to increased boron elution from thick primary particles, which destabilizes the resin mixture and reduces thermal conductivity.
The development of h-BN powder with controlled primary particle thickness and diameter ratio, stabilized crystal structure, and reduced boron elution through specific manufacturing processes, including controlled nitriding and decarburization treatments, to enhance filling properties and thermal conductivity.
The solution effectively suppresses boron elution, increasing the density and thermal conductivity of h-BN-filled resins, ensuring stable adhesion and improved thermal performance.
Smart Images

Figure 0007592181000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a hexagonal boron nitride powder for use as a filler. [Background technology]
[0002] Hexagonal boron nitride powder (hereinafter referred to as h-BN powder) is used for various purposes such as solid lubricant, glass release agent, insulating heat dissipation material, and cosmetic material.
[0003] Conventionally, such hexagonal boron nitride powder has generally been produced by reacting a boron compound, such as boric acid or a borate salt, with a nitrogen compound, such as urea or an amine, at a relatively low temperature to produce crude h-BN powder with low crystallinity, and then heating the resulting crude h-BN powder at a high temperature to grow crystals, as described in Patent Document 1, for example.
[0004] h-BN powder has a layered structure similar to that of graphite and has the following excellent properties as an electrical material: (1) to (3). (1) High thermal conductivity and excellent heat dissipation properties. (2) It has high electrical insulation and excellent dielectric strength. (3) It has the smallest dielectric constant of all ceramics.
[0005] One application of h-BN powder that takes advantage of the above properties is as a filler. In other words, by adding h-BN powder as a filler to resin materials such as epoxy resin and silicone rubber, it is possible to manufacture sheets and tapes with excellent thermal conductivity (heat dissipation) and insulation properties.
[0006] When using h-BN powder for such applications, the substitution rate of the h-BN powder with the resin (filling) determines the thermal conductivity. Therefore, it is desirable to improve the filling rate of the h-BN powder to obtain higher thermal conductivity.
[0007] However, conventional h-BN powder does not have sufficient packing properties, and the thermal conductivity of sheets or tapes in which h-BN powder is added to resin does not necessarily satisfy the required characteristics.
[0008] In order to solve the above problems, the inventors previously developed a new hexagonal boron nitride powder in which h-BN powder is used as agglomerated particles, and the primary particle size, the average diameter / thickness ratio of the primary particles, the agglomerated particle size, etc. are specified within appropriate ranges, and disclosed this in Patent Document 2.
[0009] In recent years, insulating sheets have become thinner, and it is therefore desirable to minimize the presence of conductive substances that deteriorate the insulating properties. In addition, in order to prevent the aggregates of boron nitride powder from being destroyed when it is mixed with resin, high powder strength is required. Furthermore, if there are many pores in the material obtained by mixing boron nitride powder with resin, the thermal conductivity and dielectric strength will decrease, so it is also necessary to reduce the number of pores.
[0010] In order to solve the above problems, the inventors previously developed a new hexagonal boron nitride powder in which the diameter and thickness of the primary particles, the average diameter / thickness ratio, and the size of the agglomerated particles are specified within appropriate ranges, and the upper limit of the conductive material impurities is specified. This was disclosed in Patent Document 3. [Prior art documents] [Patent documents]
[0011] [Patent Document 1] Japanese Patent Application Publication No. 09-295801 [Patent Document 2] JP 2007-308360 A [Patent Document 3] JP 2011-98882 A Summary of the Invention [Problem to be solved by the invention]
[0012] The technology disclosed in the above-mentioned Patent Document 3 has made it possible to obtain hexagonal boron nitride powder that is excellent in insulation, has high powder strength, and is also excellent in thermal conductivity and dielectric strength.
[0013] However, it has been found that when this hexagonal boron nitride powder is used as a filler, the following problems arise.
[0014] That is, in order to increase the thermal conductivity when hexagonal boron nitride powder is used as a filler, it is desirable to increase the thickness of the primary particles (increase the ratio of thickness to diameter) to reduce the voids within the agglomerates and increase the density.
[0015] However, when the thickness of the primary particles was increased, the amount of B eluted from the hexagonal boron nitride powder increased, and as a result, the desired thermal conductivity could not be obtained.
[0016] The present invention advantageously solves the above problems, and aims to provide a hexagonal boron nitride powder for fillers that reduces the amount of eluted B even when the thickness of the primary particles is increased, thereby achieving high thermal conductivity. [Means for solving the problem]
[0017] The circumstances that led to the invention will now be described.
[0018] As a result of extensive research aimed at solving the above problems, the inventors have discovered that the elution of B from boron nitride powder occurs mainly from the edge faces of hexagonal boron nitride particles having a scale-like shape. They have also discovered that by appropriately controlling the conditions for producing hexagonal boron nitride powder, it is possible to stabilize the crystal structure of the edge faces and reduce the elution of B even if the thickness of the primary particles is large.
[0019] The present invention has been developed based on the above findings, and has the following gist and configuration.
[0020] 1. A hexagonal boron nitride powder for filler comprising primary particles of hexagonal boron nitride and agglomerates of the primary particles, The primary particles have an average equivalent circle diameter of 4 μm or more, The average thickness of the primary particles is 0.5 μm or more, a ratio of the average equivalent circular diameter to the average thickness is 1 or more and 10 or less, The average particle size is 5 μm or more and 100 μm or less, Bulk density is 0.5g / cm 3 More than 1.0g / cm 3 is less than Hexagonal boron nitride powder for fillers with eluted B content of 60 ppm or less. Effect of the Invention
[0021] According to the present invention, even when the thickness of the primary particles of hexagonal boron nitride is increased, an increase in the amount of eluted B can be effectively suppressed, and as a result, high thermal conductivity can be obtained. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] The present invention will be specifically described below.
[0023] [Primary particles] The hexagonal boron nitride powder for filler of the present invention is a hexagonal boron nitride powder consisting of primary particles of hexagonal boron nitride and aggregates of the primary particles. In the present invention, the shape of the primary particles is not particularly limited, and it is sufficient that the average equivalent circle diameter and the average value of the ratio of the equivalent circle diameter to the thickness satisfy the conditions described below. However, as described above, since hexagonal boron nitride has a crystal structure similar to graphite, the primary particles may typically have a scaly (plate-like) structure. Here, the term "scaly" also includes cases where the particles have a twin crystal structure. In addition, the term "aggregates of primary particles" is defined as secondary particles that exist in a state where two or more primary particles are aggregated.
[0024] Average circle equivalent diameter of primary particles: 4μm or more Average thickness of primary particles: 0.5 μm or more In the present invention, the primary particles have an average equivalent circular diameter of 4 μm or more and an average thickness of 0.5 μm or more. This makes it possible to increase the density of the aggregated particles. As a result, the filling property when the hexagonal boron nitride powder is added to a resin as a filler can be improved, and the thermal conductivity can be improved. The primary particles preferably have an average equivalent circular diameter of 5 μm or more. The primary particles preferably have an average thickness of 0.8 μm or more, and more preferably have an average thickness of 0.9 μm or more.
[0025] According to the study by the present inventors, in conventional hexagonal boron nitride powder, the amount of eluted B from the hexagonal boron nitride powder increases when the thickness of the primary particles is increased. When the amount of eluted B increases, the mixed state of the hexagonal boron nitride powder and the resin deteriorates and the adhesion decreases, so that the desired thermal conductivity cannot be obtained even if the thickness of the primary particles is increased. However, according to the present invention, by adopting the manufacturing method described below, the elution of boron from the end faces of the hexagonal boron nitride particles can be suppressed, so that the thickness of the primary particles can be made 0.5 μm or more without increasing the amount of eluted B.
[0026] On the other hand, the upper limit of the average equivalent circle diameter of the primary particles is not particularly limited, but if it is too large, the time required for firing increases and the productivity decreases. Therefore, the average equivalent circle diameter is preferably 20 μm or less, more preferably 15 μm or less, and even more preferably 13 μm or less.
[0027] Similarly, the upper limit of the average thickness of the primary particles is not particularly limited, but if it is too large, the time required for firing increases and the productivity decreases. Therefore, the average thickness is preferably 10 μm or less, more preferably 5.0 μm or less, even more preferably 2.0 μm or less, and even more preferably 1.7 μm or less.
[0028] The equivalent circle diameter and thickness of the primary particles can be measured by image analysis of an image of the hexagonal boron nitride powder taken with a scanning electron microscope (SEM). That is, the equivalent circle diameter and thickness of the primary particles in the present invention are defined as the apparent equivalent circle diameter and thickness under the field of view of a scanning electron microscope. More specifically, they can be measured by the method described in the Examples.
[0029] Ratio of average equivalent circle diameter to average thickness: 1 to 10 In the present invention, the ratio of the average equivalent circular diameter to the average thickness of the primary particles is set to 1 or more and 10 or less. This can increase the density of the aggregated particles and increase the packing rate in the resin sheet. In one embodiment of the present invention, the ratio of the average equivalent circular diameter to the average thickness of the primary particles may be 1.0 or more and 10.0 or less. The ratio of the average equivalent circular diameter to the average thickness of the primary particles is preferably 3.0 or more, and more preferably 5.0 or more. The ratio of the average equivalent circular diameter may be 9.5 or less, or may be 9.0 or less. The value of the ratio can be obtained by dividing the average equivalent circular diameter of the primary particles by the average thickness of the primary particles.
[0030] Average particle size: 5μm or more and 100μm or less Bulk density: 0.5g / cm 3 More than 1.0g / cm 3 less than Furthermore, in the present invention, the average particle size of the hexagonal boron nitride powder is 5 μm or more and 100 μm or less, and the bulk density is 0.5 g / cm 3 More than 1.0g / cm 3 This makes it possible to increase the packing property (packing density) when the hexagonal boron nitride powder is added as a filler to a resin, thereby improving the thermal conductivity. In one embodiment of the present invention, the bulk density is 0.50 g / cm or less. 3 More than 1.00g / cm 3 It may be less than.
[0031] If the average particle size is smaller than 5 μm, the adhesion between the resin and the boron nitride particles is weak, while if it is larger than 100 μm, it may become a foreign body in the resin sheet and lead to the destruction of the sheet. The average particle size is preferably 10 μm or more, and more preferably 20 μm or more. The average particle size is preferably 80 μm or less, and more preferably 70 μm or less.
[0032] In addition, the bulk density is 0.5 g / cm 3 If the bulk density is lower than 1.0 g / cm3, the amount that can be added to the resin decreases, and the filling property into the resin decreases. 3 If the bulk density is more than 0.60 g / cm, the filling property is improved, but the dispersibility when mixed into the resin is decreased, and it becomes difficult to disperse the powder uniformly in the resin. 3 It is preferable that the bulk density is 0.95 g / cm or more. 3 It is preferable that:
[0033] The average particle size of the hexagonal boron nitride powder in the present invention is the median diameter D on a volume basis in the particle size distribution measured by a laser diffraction scattering method. 50 Therefore, the average particle size is the average particle size of the entire hexagonal boron nitride powder, including both primary particles and agglomerated particles (secondary particles). More specifically, it can be measured by the method described in the examples.
[0034] The bulk density can be determined from the volume and weight of the hexagonal boron nitride powder after filling a container with the hexagonal boron nitride powder and tapping it. More specifically, it can be measured by the method described in the Examples.
[0035] The average particle size and bulk density of the hexagonal boron nitride powder can be adjusted by controlling the conditions for pulverizing and classifying the hexagonal boron nitride powder after the decarburization treatment, as described below.
[0036] Elution B amount: 60ppm or less In conventional hexagonal boron nitride powder, when the thickness of the primary particles is increased, the amount of eluted B from the BN particles increases, resulting in problems such as unstable hardness of the resin after mixing with the resin and poor adhesion between the resin and BN. In contrast, in the present invention, by adopting a manufacturing method described below, it is possible to reduce the amount of eluted B to 60 ppm or less. The amount of eluted B is preferably 50 ppm or less. On the other hand, since the amount of eluted B is preferably as small as possible, the lower limit may be 0 ppm. However, from the viewpoint of industrial production, the amount of eluted B may be 10 ppm or more, or may be 15 ppm or more.
[0037] The amount of eluted B from hexagonal boron nitride powder can be obtained by adding 2.5 g of the hexagonal boron nitride powder to be measured to a mixed solvent of 30 ml of water and 10 ml of ethanol, heating and stirring at 50° C. for 60 minutes, filtering through a membrane filter with a pore size of 0.2 μm, and measuring the B contained in the filtrate using ICP atomic emission spectrometry as specified in JIS K 0116: 2014. More specifically, it can be measured by the method described in the Examples.
[0038] The proportion of aggregated particles in the hexagonal boron nitride powder of the present invention is not particularly limited, but from the viewpoint of further improving the performance as a filler, it is preferable that the proportion of fine powder generated by the destruction of aggregated particles is low. Specifically, when the particle size distribution of the hexagonal boron nitride powder is measured by a laser diffraction scattering method, the proportion of particles having a particle size of 10 μm or less in the entire hexagonal boron nitride powder is preferably 30 vol.% or less, more preferably 20 vol.% or less. The lower limit of the proportion of particles having a particle size of 10 μm or less in the entire hexagonal boron nitride powder is not particularly limited, and may be 0 vol.%.
[0039] A preferred manufacturing process for the hexagonal boron nitride powder according to the present invention will be described below, along with a specific description of a method for increasing the thickness of the primary particles and a method for reducing the amount of eluted B.
[0040] The hexagonal boron nitride powder of the present invention can be produced by calcining boron carbide (B4C) in a nitrogen atmosphere, then subjecting it to a decarburization treatment, and optionally performing treatments such as pulverization and classification.
[0041] The boron carbide is not particularly limited and any boron carbide can be used. In general, commercially available boron carbide can be used. Boron carbide can also be produced from boric acid (H3BO3) by the reaction of the following formula (1). That is, boric acid is reacted with a carbon-containing material at high temperature in a non-oxidizing atmosphere, and then the resulting mixture is pulverized and classified to obtain boron carbide powder. 4H3BO3+ 7C → B4C + 6H2O + 6CO (1)
[0042] Boron carbide powder is sintered in a nitrogen atmosphere (nitriding treatment) to produce BN powder through the reaction of the following formula (2). (1 / 2)B4C + N2→ 2BN +(1 / 2)C ···(2)
[0043] If the nitrogen partial pressure during the nitriding treatment is less than 0.005 MPa, the nitriding reaction proceeds slowly, and the treatment takes a long time. Therefore, the nitrogen partial pressure during the nitriding treatment is set to 0.005 MPa or more. On the other hand, the upper limit of the nitrogen partial pressure is not particularly limited, but due to equipment restrictions, the nitrogen partial pressure may generally be 5 MPa or less.
[0044] Similarly, if the temperature during the nitriding treatment is less than 1800°C, the nitriding reaction proceeds slowly, and the treatment takes a long time. Therefore, the temperature during the nitriding treatment is set to 1800°C or higher, preferably 1900°C or higher. On the other hand, if the temperature exceeds 2200°C, a reverse reaction occurs, and the reaction rate decreases. Therefore, the temperature during the nitriding treatment is set to 2200°C or lower, preferably 2100°C or lower.
[0045] The product obtained by the nitriding process contains not only boron nitride but also carbon. Therefore, the product is subjected to a decarburization process to remove the C that is mixed in. This decarburization process is performed by mixing the product with diboron trioxide and / or its precursor (hereinafter referred to as diboron trioxide, etc.) and heating it under a nitrogen atmosphere. In the decarburization process, the C contained in the product is removed as CO (gas) by the reaction of the following formula (3), and BN is generated from the carbonized diboron trioxide, etc. 2BN+(1 / 2)C+(1 / 6)B2O3+(1 / 6)N2→(7 / 3)BN+(1 / 2)CO↑···(3)
[0046] The precursor of diboron trioxide is a boron compound that can become diboron trioxide by heating, and specific examples thereof include ammonium salts of boric acid, orthoboric acid, metaboric acid, and tetraboric acid. Among diboron trioxide and its precursors, diboron trioxide is particularly preferred.
[0047] The product to be subjected to the decarbonization treatment can be mixed with diboron trioxide and the like by any method. For example, a solvent can be added to a ball mill to perform wet mixing, but it is preferable to use a dry mixer such as a V-blender. The mixing is continued until a homogeneous state is reached. Specifically, it is sufficient if the mixture becomes a homogeneous gray color when visually observed.
[0048] The reaction of formula (3) above proceeds at 1500° C. or higher, but in order to evaporate and remove diboron trioxide as described below, the temperature during the decarburization treatment is set to 1800° C. or higher, preferably 1900° C. or higher. On the other hand, the upper limit of the temperature is not particularly limited, but may usually be 2200° C. or lower, preferably 2100° C. or lower.
[0049] In order to allow the reaction to proceed sufficiently, the time for carrying out the decarbonization treatment is set to 6 hours or more, and preferably 12 hours or more.
[0050] By mixing an appropriate amount of diboron trioxide or the like and carrying out the decarburization treatment under the above conditions, the amount of carbon contained in the product can be reduced to, for example, 0.2 mass % or less.
[0051] In the present invention, the concept and specific means for increasing the thickness of the primary particles are as follows.
[0052] [How to increase thickness] The inventors have studied the growth of hexagonal boron nitride particles in the above-mentioned decarburization treatment, and as a result, have found that an excess of diboron trioxide etc. promotes the growth of hexagonal boron nitride particles in the plane direction, and as a result, the growth in the thickness direction is suppressed. This is believed to be because, when there is an excess of diboron trioxide etc., diboron trioxide etc. remains even after C is removed by the reaction of the above-mentioned formula (3), and boron nitride particles come into contact with each other and grow by combining in the liquid phase of the remaining diboron trioxide etc. At that time, hexagonal boron nitride is prone to combining at the end faces with high activity due to its crystal structure, and as a result, growth in the plane direction occurs preferentially.
[0053] Therefore, in order to reduce the ratio of the equivalent circle diameter to the thickness of the primary particles, it is effective to suppress the growth in the planar direction by reducing the amount of excess diboron trioxide or the like.
[0054] For this reason, when diboron trioxide, etc. is mixed with the product (BN, C) obtained after calcining boron carbide in a nitrogen atmosphere and calcined to remove by-product carbon, it is important to perform decarburization by adding an amount of diboron trioxide, etc. corresponding to the reaction of equation (3) to the total amount of product (BN, C) obtained after calcining boron carbide in a nitrogen atmosphere, in other words, to perform decarburization with as little excess diboron trioxide, etc. as possible.
[0055] [Specific Means for Increasing Thickness] As described above, the reaction in the decarburization treatment can be expressed by formula (3). From the left side of the formula, the amount of diboron trioxide etc. required to decarburize 1 part by mass of C (stoichiometric equivalent) is approximately 2 parts by mass in terms of B2O3 (formula (4) below). (1 / 2)C:(1 / 6)B2O3≒1 / 2×12:1 / 6×70≒1:2 …(4)
[0056] If the amount of diboron trioxide, etc. used in the decarburization treatment is less than 1.0 times the stoichiometric equivalent, decarburization will be insufficient and C will remain. Therefore, the amount of diboron trioxide, etc. used in the decarburization treatment is set to 1.0 times or more the stoichiometric equivalent. On the other hand, if the amount of diboron trioxide, etc. used in the decarburization treatment is more than 3.2 times the stoichiometric equivalent, excess diboron trioxide will remain after decarburization, and the average value of the ratio of the circle equivalent diameter to the thickness of the primary particles cannot be set in the desired range. Therefore, the amount of diboron trioxide, etc. used in the decarburization treatment is set to 3.2 times or less, preferably 2.4 times or less, the stoichiometric equivalent.
[0057] Also, it is effective to set the decarburization temperature to a high temperature of 1800° C. or more, increase the evaporation rate of diboron trioxide after completion of decarburization, and reduce excess diboron trioxide, etc. Therefore, the decarburization temperature is set to 1800° C. or more, preferably 1900° C. or more, which is higher than the boiling point of boron trioxide.
[0058] Furthermore, by carrying out a decompression treatment after the decarburization treatment, the evaporation rate of diboron trioxide and the like can be increased, and excess diboron trioxide and the like can be reduced, thereby suppressing growth in the longitudinal direction of the long sides and promoting growth in the thickness direction.
[0059] Next, the concept and specific means for reducing elution of B will be described.
[0060] [How to reduce eluted B] In hexagonal boron nitride powder with thick primary particles, the amount of dissolved B is greater than in hexagonal boron nitride powder with thin primary particles, because, as mentioned above, the dissolution of B occurs mainly at the edge faces of the hexagonal boron nitride particles, which are the primary particles.
[0061] According to the inventors' study, it is estimated that in BN with an unstable crystal structure at the end face of the primary particle, the amount of B dissolved by hydrolysis is large. Therefore, in order to reduce the amount of dissolved B from thick BN primary particles, it is considered effective to reduce and stabilize the unstable crystal structure BN present in large amounts at the end face. Although it is not clear what the unstable crystal structure BN is, it is estimated that it is a structure in which an OH group is bonded to the B in the terminal structure and an H group is bonded to the N. It is estimated that the unstable crystal structure BN reacts with H2O to generate NH3, making it a structure that is easily hydrolyzed.
[0062] [Specific measures for reducing elution B] In order to reduce the amount of dissolved B, it is necessary to stabilize the crystal structure of the end faces of the primary particles of BN as described above, and to reduce the amount of B dissolved by hydrolysis. Therefore, the inventors conducted numerous experiments and studies to achieve this.
[0063] As a result, although the reason is unclear, it was found that the crystal structure at the end face of the primary particle can be stabilized and the amount of dissolved B can be reduced by setting the cooling rate after the decarburization treatment to 50°C / min or less in a furnace temperature range of 1600°C or less, and further setting the temperature when removing BN from the furnace after the decarburization treatment to 500°C or less. The cooling rate is preferably 20°C / min or less, more preferably 10°C / min or less, and even more preferably 5°C / min or less. The temperature when removing from the furnace is 500°C or less means that the boron nitride powder is removed from the furnace after the temperature of the boron nitride powder has dropped to 500°C or less. The temperature when removing from the furnace is preferably 300°C or less, more preferably 200°C or less. The temperature is the furnace temperature, and the measurement method is not particularly limited, but it can be measured using a thermocouple, an infrared radiation thermometer, or the like.
[0064] It is believed that when the cooling rate after decarburization is high and the BN is taken out of the furnace and rapidly cooled at a high temperature exceeding 500°C, as in the past, the crystal structure of the end faces of the primary particles of BN becomes highly unstable, resulting in an increase in the amount of eluted B.
[0065] In contrast, in the present invention, as described above, the cooling rate after the decarburization treatment is slowed down, and the temperature when the BN is removed from the furnace is lowered, thereby stabilizing the crystal structure of the end faces of the primary particles and reducing the amount of eluted B.
[0066] The hexagonal boron nitride obtained by the above process is crushed and classified as necessary to obtain the desired bulk density and average particle size.
[0067] (Example) Hexagonal boron nitride powder was produced by the following procedure, and its properties were evaluated.
[0068] A commercially available boron carbide powder with a purity of 98% by mass was sieved through a sieve with an opening of 44 μm, and 101.8 g of the boron carbide powder that passed through the sieve was used as a raw material powder. The raw material powder was placed in a carbon crucible with an inner diameter of 90 mm and a height of 100 mm, and sintered (nitriding treatment) in a nitrogen atmosphere with the furnace pressure maintained at a temperature of 2000° C. for 15 hours.
[0069] In some cases, a decompression treatment was carried out after the nitriding treatment. Specifically, in the temperature drop process after the completion of the nitriding treatment for 15 hours, a decompression treatment was started to maintain the furnace pressure at 60 kPa when the furnace temperature reached 1800°C. The holding time in the decompression treatment was 3 hours.
[0070] 69.3 g of the product obtained by the calcination was taken and mixed with 35.2 g of commercially available diboron trioxide to obtain a powder mixture. The mixing was carried out using a V-blender with an internal volume of 1 L by rotating at 1 Hz for 30 minutes.
[0071] The obtained powder mixture was placed in a carbon crucible with an inner diameter of 90 mm and a height of 100 mm, and subjected to a decarburization treatment at 2000°C for 10 hours in a nitrogen stream to obtain a second fired product. At this time, the cooling rate after the decarburization treatment and the temperature at which the product was removed from the furnace were the values shown in Table 1. In some cases, after the decarburization treatment, a reduced pressure treatment was performed in which the furnace temperature was 2000°C and the furnace pressure was kept at 60 kPa for 3 hours.
[0072] The second calcination product thus obtained was a white aggregate, which was crushed and subjected to X-ray diffraction, and was confirmed to be almost completely h-BN.
[0073] (Evaluation of primary particles) Next, the average equivalent circle diameter and average thickness of the primary particles were measured for each of the obtained hexagonal boron nitride powders. Specifically, the hexagonal boron nitride powders were photographed at a magnification of 5000 times using an SEM. From the obtained image, 5 to 10 particles in which the shape of the primary particles could be confirmed were randomly selected, and the apparent equivalent circle diameter and thickness in the microscope field of view were obtained by image analysis, and the average values of each were calculated. In addition, the ratio of the average equivalent circle diameter to the average thickness of the primary particles was calculated from the obtained values. The obtained results are also shown in Table 1.
[0074] (Evaluation of hexagonal boron nitride powder) Furthermore, the average particle size, bulk density, and amount of eluted B of each of the obtained hexagonal boron nitride powders were evaluated by the following procedures. The obtained results are shown in Table 1.
[0075] ·Average particle size The average particle size of the hexagonal boron nitride powder was measured by a dry method using a Malvern Mastersizer laser diffraction particle size distribution analyzer. In the measurement, a laser beam was irradiated onto the hexagonal boron nitride powder introduced into a cell at 0.1 bar, and the particle size distribution was obtained by analyzing the resulting light scattering pattern. The refractive index of boron nitride was set to 1.7. The median diameter D on a volume basis in the obtained particle size distribution was 50 was taken as the average particle size.
[0076] Bulk density The obtained hexagonal boron nitride powder was gently filled into a 100 ml polypropylene measuring cylinder until the volume reached 100 ml. The polypropylene measuring cylinder was then attached to a tapping machine and tapped 216 times. After tapping, the bulk density (g / ml) was calculated from the volume (ml) of the hexagonal boron nitride powder in the polypropylene measuring cylinder and the weight (g) of the hexagonal boron nitride powder.
[0077] ·Elution B amount The amount of eluted B was measured for each of the obtained hexagonal boron nitride powders by the following procedure. First, 2.5 g of the hexagonal boron nitride powder to be measured was added to a mixed solvent of 30 ml of water + 10 ml of ethanol, heated and stirred at 50 ° C for 60 minutes, and then filtered using a barrel filter equipped with a membrane filter with a pore size of 0.2 μm and a diameter of 47 mm. Next, the amount of B contained in the filtrate was measured using ICP atomic emission spectroscopy specified in JIS K 0116:2014 in accordance with the quasi-drug raw material standard, and the amount of eluted B was obtained. In addition, in the above measurement, all the instruments used were made of quartz or resin to prevent contamination of B.
[0078] (Thermal Conductivity) In order to evaluate the performance of the obtained hexagonal boron nitride powder as a filler, a resin sheet containing the hexagonal boron nitride powder was produced by the following procedure, and its thermal conductivity was evaluated.
[0079] First, 20 g of epoxy resin containing a curing agent and hexagonal boron nitride powder were added to 40 g of methyl cellosolve as a solvent, and the mixture was kneaded for 60 minutes in a rotary ball mill to uniformly disperse the mixture. The amount of the hexagonal boron nitride powder added was 60 mass% based on the total weight excluding the solvent. BisF liquid type epoxy resin jER807 (manufactured by Mitsubishi Chemical Corporation) was used as the epoxy resin, and modified alicyclic amine grade epoxy resin curing agent jER Cure 113 (manufactured by Mitsubishi Chemical Corporation) was used as the curing agent.
[0080] Next, the resin containing the kneaded hexagonal boron nitride powder was applied to the polyimide film using a hand coater so as to give a film thickness of 200 μm. The applied resin was dried at 130° C. for 10 minutes, and then two sheets were stacked so that the resin surfaces were in contact with each other, and the two sheets were then heated at a temperature of 170° C. and a pressure of 80 kgf / cm. 2 The mixture was subjected to heat press molding at 400° C. for 30 minutes to obtain a resin sheet.
[0081] A test piece having a diameter of 10 mm and a thickness of 2 mm was cut out from the obtained resin sheet, and the thermal conductivity of the test piece was measured by laser flash.
[0082] As can be seen from the results shown in Table 1, the hexagonal boron nitride powder satisfying the conditions of the present invention had excellent thermal conductivity. This is believed to be due to the improved filling ability, adhesion, and contact resistance of the hexagonal boron nitride powder into resin. In particular, the hexagonal boron nitride powder of the present invention has a reduced amount of eluted B even when the average thickness of the primary particles is increased to 0.5 μm or more, and as a result, a high thermal conductivity can be achieved. Therefore, the hexagonal boron nitride powder of the present invention can be extremely suitably used as a filler to be added to insulating sheets and the like.
[0083] [Table 1]
Claims
[Claim 1] A hexagonal boron nitride powder for filler comprising primary particles of hexagonal boron nitride and aggregates of the primary particles, The average equivalent circular diameter of the primary particles is 4 μm or more, The average thickness of the primary particles is 0.5 μm or more, a ratio of the average equivalent circular diameter to the average thickness is 1 or more and 10 or less, The average particle size is 5 μm or more and 100 μm or less, Bulk density is 0.5 g / cm 3 1.0g / cm or more 3 is less than A hexagonal boron nitride powder for fillers, having an amount of eluted B of 60 ppm or less.
Citation Information
Patent Citations
Production of hexagonal boron nitride powder
JP1997295801A
Hexagonal boron nitride powder
JP2007308360A
Hexagonal boron nitride and manufacturing method thereof
JP2010047450A
Hexagonal boron nitride powder and method for producing the same
JP2011098882A