Toner and its manufacturing method, image forming apparatus, and image forming method

The toner design with controlled embedding of resin and external additives addresses the challenge of achieving low-temperature fixability and cleanability by maintaining additive functionality and preventing adhesion, ensuring stable image quality and cleaning efficiency.

JP7593007B2Active Publication Date: 2024-12-03RICOH CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020138651
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-08-19
Publication Date
2024-12-03
Estimated Expiration
2040-08-19

AI Technical Summary

Technical Problem

Existing toners struggle to achieve both low-temperature fixability and cleanability at a high level, with previous solutions either failing to provide sufficient resistance to embedding and detachment of external additives under stress or not maintaining image quality over time.

Method used

A toner design where fine resin particles and external additives are attached to the surface of toner base particles, with a specific degree of embedding (15% to 40%) achieved through a rocking mill simulation of machine stress, using hydrophobized silica or titania particles and adjusting the average primary particle diameter and surface hardness to enhance spacer function and prevent adhesion.

Benefits of technology

The toner achieves both low-temperature fixability and cleanability by maintaining the external additives' functionality under stress, preventing contamination and adhesion issues, thereby ensuring stable image quality and efficient cleaning.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007593007000004
    Figure 0007593007000004
  • Figure 0007593007000005
    Figure 0007593007000005
  • Figure 0007593007000001
    Figure 0007593007000001
Patent Text Reader

Abstract

To provide a toner that can achieve both low temperature fixability and a cleaning property at a high level.SOLUTION: A toner includes a toner base particle containing at least a binder resin, a colorant, and wax, and resin fine particles and an external additive attached to the surface of the toner base particle. The storage elastic modulus G' at 70°C of the toner is 4.0×105 or less, and the degree of embedment of the external additive in the toner after execution of processing according to the following condition is 15%-40%. (Condition) 10 g of the toner and 20 g of carrier are introduced into a 50 mL bottle, and subsequently the toner is stirred at 67 Hz for 60 minutes by using a rocking mill.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a toner and a method for producing the toner, a toner storage unit, an image forming apparatus, and an image forming method. [Background technology]

[0002] An image forming method using electrophotography with toner involves forming an electrostatic latent image on the surface of a photoconductor, developing the electrostatic latent image to form a toner image, transferring the toner image to a medium, and fixing the toner image.

[0003] In recent years, toners are required to have smaller particle size and high-temperature offset resistance for improving the quality of output images, low-temperature fixability for energy saving, and heat-resistant storage stability capable of withstanding high temperatures and high humidity during storage and transportation after production. In particular, since the power consumption during fixation accounts for a large portion of the power consumption in the image forming process, improving low-temperature fixability is extremely important.

[0004] In addition, the toner is required to prevent adhesion between the toner and the paper caused by the pressure due to the weight of the paper when the toner is fixed on the paper surface and stacked in the paper output tray and the residual heat during fixing, which is called paper discharge blocking.Furthermore, it is required to prevent a situation in which the toner is subjected to stress in the developing device, causing external additives to be embedded in the toner matrix and increasing the adhesive force between the toner and components, making it difficult to remove the toner with a cleaning blade.

[0005] Therefore, a toner has been proposed in which inorganic particles are arranged on the surface of a core particle of a toner base, and the inorganic particles are further covered with a shell of a thermosetting resin (see, for example, Patent Document 1). This proposal makes it possible to suppress embedding and detachment of external additives against stress at high temperatures and stress in a developing machine, and to form images with a desired image density over a long period of time. In addition, a toner has been proposed that achieves both durability and fluidity by appropriately controlling the mixing order of silica particles with different particle sizes in the external addition process, and controls the embedding property of the external additives, thereby providing low-temperature fixability and heat resistance (see, for example, Patent Document 2). However, even these proposals have not yet been able to achieve both low-temperature fixability and cleanability at a high level. Summary of the Invention [Problem to be solved by the invention]

[0006] An object of the present invention is to provide a toner which is capable of achieving both low-temperature fixing property and cleaning property at a high level. [Means for solving the problem]

[0007] The toner of the present invention as a means for solving the above problems is a toner in which resin fine particles and an external additive are attached to the surface of toner base particles containing at least a binder resin, a colorant, and a wax, The storage modulus G' of the toner at 70° C. is 4.0×10 5 is as follows: The toner is characterized in that the embedding degree of the external additive after the treatment under the following conditions is 15% to 40%. (conditions) 10 g of the toner and 20 g of the carrier are placed in a 50 mL bottle, and then stirred at 67 Hz for 60 minutes using a rocking mill. Effect of the Invention

[0008] According to the present invention, it is possible to provide a toner which is capable of achieving both low-temperature fixing property and cleaning property at a high level. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is a schematic view showing an example of a process cartridge which is a toner storage unit of the present invention. [Diagram 2] FIG. 2 is a schematic diagram showing an example of an image forming apparatus according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] (toner) The toner of the present invention contains toner base particles and further contains other components as required. The toner base particles have resin particles and external additives attached to their surfaces.

[0011] Up to now, various attempts have been made to achieve both low-temperature fixability and cleanability. For example, JP2015-087597A proposes a toner in which inorganic particles are arranged on the surface of a core particle of a toner base, and the inorganic particles are further covered with a shell layer of a thermosetting resin. However, although the proposed toner exhibits excellent functions in terms of resistance to embedding and release of external additives, the resin used for the shell layer is a material that exhibits high thermal properties from the viewpoint of stress resistance, and the low-temperature fixability required in recent years is not obtained. And, JP2013-105153A proposes a toner in which the embedding property of external additives is controlled. However, the embedding property of external additives is controlled only in the initial state, and the effect is not sufficient against the stress in an actual developing machine.

[0012] As a result of intensive research by the inventors, it was found that stirring for 60 minutes in a rocking mill roughly reproduces the stress in a developing machine. In other words, if the external additive has resistance to embedding against the stirring stress in a rocking mill, it was found that the external additive also has resistance to embedding against the stress over time in the developing unit of an actual machine, and this led to the completion of the present invention.

[0013] <External additives> The embedding degree of the external additive in the surface of the toner base particle is 15% to 40%, preferably 18% to 30%. The embedding degree of less than 15% indicates that the external additive is hardly fixed to the toner base particle and is free on the toner surface. Therefore, if the embedding degree is 15% or more, the problem that the free external additive contaminates the carrier and the image carrier, and a stable image cannot be obtained can be prevented. The embedding degree of more than 40% indicates that the external additive is almost embedded in the toner base particle. Therefore, if the embedding degree is 40% or less, the spacer function of the external additive is not fully exerted, which leads to an increase in the adhesion force between the exposed base and the members of the image forming apparatus, and the problem that cleaning failure occurs can be prevented.

[0014] The embedding degree of the external additive in the present invention is a value measured by the following measurement. This value indicates the embedding degree of the external additive after applying the assumed stress in the actual machine. 10 g of the obtained toner and 20 g of a carrier described below are placed in a 50 mL glass bottle and stirred at 67 Hz for 60 minutes using a rocking mill (product name: RM05S, manufactured by Seiwa Giken Co., Ltd.). After the toner is mixed, it is embedded in epoxy resin and fixed, and then the toner is cut using a FIB-SEM (SU-8230, Hitachi High-Technologies Corporation) and the cross-section SEM image is observed. The acceleration voltage is 30 kV and the current value is 100-500 pA. From the obtained toner cross-section SEM image, the embedding degree of the external additive is quantified using image analysis software as follows. (1) Observe using SEM in topographical image mode. The value obtained from the observed data is called A. (2) Observe using an SEM in compositional image mode. The value obtained from the observed data is called B. (3) In the shape image mode, the contrast of the external additive is strong, so binarization is performed based on this contrast. (4) The shape of the toner base particles is captured using a SEM in composition image mode. (5) The volume (a) of the external additive present on the surface of the toner base particle and the volume (b) of the external additive buried in the surface of the toner base particle are calculated by combining A and B. From these values, the buried degree (%) of the external additive can be calculated by (b / a)×100.

[0015] Examples of methods for adjusting the embedding degree of the external additive include a method for adjusting the average primary particle size of the external additive, and a method for adjusting the surface hardness of the toner base particles. The smaller the average primary particle size of the external additive, the easier it is to embed the external additive in the surface of the toner base particle due to stress over time (use) in the process, and the larger the average primary particle size, the more the external additive can be prevented from embedding in the surface of the toner base particle. Therefore, the degree of embedding of the external additive can be adjusted by adjusting the average primary particle size of the external additive. The term "adjusting the hardness of the toner base particle surface" means disposing a material (such as styrene acrylic resin) that can maintain elasticity in the temperature range expected in the actual machine on the surface of the toner base particle. By disposing this material, it is possible to prevent the external additive from being embedded even under the stress in the actual machine.

[0016] The external additive is not particularly limited and can be appropriately selected depending on the purpose. Examples of the external additive include silica fine particles, hydrophobic silica, fatty acid metal salts (e.g., zinc stearate, aluminum stearate, etc.), metal oxide fine particles (e.g., titania, alumina, tin oxide, antimony oxide, etc.), and fluoropolymers. These may be used alone or in combination of two or more. Among these, silica fine particles and titania fine particles are preferred. The external additive is preferably subjected to a hydrophobization treatment.

[0017] Commercially available products of the silica fine particles include, for example, R972, R974, RX200, RY200, R202, R805, and R812 (all manufactured by Nippon Aerosil Co., Ltd.). Commercially available examples of the titanium oxide (titania) microparticles include P-25 (manufactured by Nippon Aerosil Co., Ltd.), STT-30, STT-65C-S (all manufactured by Titanium Kogyo Co., Ltd.), TAF-140 (manufactured by Fuji Titanium Kogyo Co., Ltd.), MT-150W, MT-500B, MT-600B, MT-150A (all manufactured by Teika Corporation).

[0018] Commercially available hydrophobically treated titanium oxide (titania) microparticles include, for example, T-805 (manufactured by Nippon Aerosil Co., Ltd.), STT-30A, STT-65S-S (all manufactured by Titanium Kogyo Co., Ltd.), TAF-500T, TAF-1500T (all manufactured by Fuji Titanium Kogyo Co., Ltd.), MT-100S, MT-100T (all manufactured by Teika Corporation), and IT-S (manufactured by Ishihara Sangyo Co., Ltd.).

[0019] Hydrophobized oxide particles, hydrophobized silica particles, hydrophobized titania particles, and hydrophobized alumina particles can be obtained by treating hydrophilic particles with a silane coupling agent such as methyltrimethoxysilane, methyltriethoxysilane, octyltrimethoxysilane, etc. Silicone oil-treated oxide particles and inorganic particles, which are treated with silicone oil by heating if necessary, are also suitable.

[0020] Examples of the silicone oil include dimethyl silicone oil, methylphenyl silicone oil, chlorophenyl silicone oil, methylhydrogen silicone oil, alkyl-modified silicone oil, fluorine-modified silicone oil, polyether-modified silicone oil, alcohol-modified silicone oil, amino-modified silicone oil, epoxy-modified silicone oil, epoxy-polyether-modified silicone oil, phenol-modified silicone oil, carboxyl-modified silicone oil, mercapto-modified silicone oil, methacryl-modified silicone oil, and α-methylstyrene-modified silicone oil.

[0021] The average particle size (number average primary particle size) of the primary particles of the external additive is not particularly limited and may be appropriately selected depending on the purpose, but is preferably 70 nm to 220 nm. If the average particle size of the primary particles of the external additive is 70 nm or more, the external additive is easily embedded in the base particles, and the spacer effect is small, so that the problem of insufficient cleaning properties being obtained can be prevented. If the average particle size of the primary particles of the external additive exceeds 220 nm, the external additive is difficult to fix to the base particles and is easily released, so that the external additive is detached during the development or transfer process in the actual machine, so that the problem of insufficient spacer function being exhibited can be prevented. The external additive preferably contains two types of silica particles, and when the silica particles having the largest average primary particle diameter are designated as silica particles A, the average primary particle diameter of the silica particles A is preferably 70 nm to 220 nm. When the external additive uses a plurality of types of particles, the average primary particle diameter is measured as the average value of all particles.

[0022] The method for measuring the primary number average particle diameter of the external additive is not particularly limited and may be appropriately selected depending on the purpose. For example, a method for measuring the primary number average particle diameter using a TEM image of the toner may be used.

[0023] The content of the external additive is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 0.1 parts by mass to 5 parts by mass, and more preferably 0.3 parts by mass to 3 parts by mass, relative to 100 parts by mass of the toner.

[0024] <Resin fine particles> The resin particles are attached to the surfaces of the toner base particles.

[0025] The volume average primary particle diameter of the resin fine particles is more than 5 nm and not more than 60 nm, and preferably more than 10 nm and not more than 50 nm. If the volume average primary particle diameter is 5 nm or less, the heat resistance storage stability may be deteriorated, and if the volume average primary particle diameter is more than 60 nm, the low temperature fixability may be deteriorated. The volume average primary particle size can be measured using an SEM image as described below.

[0026] The volume average primary particle diameter of the resin fine particles is measured by removing as much of the external additives as possible by ultrasonic liberation treatment to bring the particles into a state close to that of toner base particles, and observing the particles with a scanning electron microscope (SEM) as described below. -How to separate external additives- [1] Add 50 mL of a 5% aqueous solution containing a surfactant (product name: Noigen ET-165, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) to a 100 mL screw tube, add 3 g of toner to the mixture, and gently move it up and down and left and right. Then, mix it with a ball mill for 30 minutes so that the toner blends into the dispersion solution. [2] Then, using an ultrasonic homogenizer (product name homogenizer, model VCX750, CV33, manufactured by SONICS & MATERIALS LLC), set the output to 40 W and apply ultrasonic energy for 60 minutes. -Ultrasonic conditions- Vibration time: 60 minutes continuous ·Amplitude: 40W ·Vibration start temperature: 23±1.5℃ ·Temperature during vibration: 23±1.5℃ [3](1) The dispersion liquid is suction filtered using filter paper (product name: Qualitative Filter Paper (No. 2, 110 mm), manufactured by Advantec Toyo Co., Ltd.), washed twice again with ion-exchanged water, filtered, and the liberated additives are removed, and the toner particles are then dried. (2) The toner obtained in (1) is observed with a scanning electron microscope (SEM). First, external additives and fillers containing Si are detected by observing the backscattered electron image. (3) The image of (1) is binarized using image processing software (ImageJ) to remove the external additives and fillers. Next, a secondary electron image is observed at the same position as in (1). Since the resin fine particles cannot be observed in the reflected electron image, but can only be observed in the secondary electron image, the image obtained in (3) is compared, and the fine particles present in the areas other than the remaining external additives and filler (areas other than those removed in (3)) are determined to be resin fine particles, and the distance between the resin fine particles (the distance connecting the centers of the particles) is measured using the image processing software. [Shooting conditions] Scanning electron microscope: SU-8230 (Hitachi High-Technologies Corporation) Magnification: 35,000x Image capture: SE(L): Secondary electrons, BSE (backscattered electrons) Acceleration voltage: 2.0kV ·Acceleration current: 1.0μA ·Probe current:Normal Focus mode: UHR WD:8.0mm The above measurement is carried out for 100 binarized images (one toner particle per image), and the average value is taken as the measurement result.

[0027] The resin fine particles (hereinafter, sometimes referred to as "resin fine particles (B)") preferably have a core resin (core portion) and a shell resin (outer shell portion) that covers at least a part of the surface of the core resin, more preferably consist of a core resin and a shell resin, and further preferably contain a vinyl-based unit consisting of resin (b1) and resin (b2). The shell resin (hereinafter also referred to as "resin (b1)") and the core resin (hereinafter also referred to as "resin (b2)") are preferably polymers obtained by homopolymerizing or copolymerizing vinyl monomers.

[0028] Examples of the vinyl monomer include the following (1) to (10). (1) Vinyl hydrocarbons Examples of vinyl hydrocarbons include (1-1) aliphatic vinyl hydrocarbons, (1-2) alicyclic vinyl hydrocarbons, and (1-3) aromatic vinyl hydrocarbons. (1-1) Aliphatic vinyl hydrocarbons Examples of the aliphatic vinyl hydrocarbon include alkenes and alkadienes. Specific examples of the alkenes include ethylene, propylene, and α-olefins. Specific examples of the alkadienes include butadiene, isoprene, 1,4-pentadiene, 1,6-hexadiene, and 1,7-octadiene. (1-2) Alicyclic vinyl hydrocarbons The alicyclic vinyl hydrocarbons include mono- or di-cycloalkenes and alkadienes, and specific examples thereof include (di)cyclopentadiene and terpene. (1-3) Aromatic vinyl hydrocarbons The aromatic vinyl hydrocarbons include styrene and its hydrocarbyl (alkyl, cycloalkyl, aralkyl and / or alkenyl) substituted products, and specific examples thereof include α-methylstyrene, 2,4-dimethylstyrene and vinylnaphthalene.

[0029] (2) Carboxyl-containing vinyl monomers and their salts Examples of the carboxyl group-containing vinyl monomer and its salt include unsaturated monocarboxylic acids (salts) having 3 to 30 carbon atoms, unsaturated dicarboxylic acids (salts), and anhydrides (salts) thereof, and monoalkyl (carbon number 1 to 24) esters thereof or salts thereof. Specific examples thereof include carboxyl group-containing vinyl monomers such as (meth)acrylic acid, (anhydride) maleic acid, maleic acid monoalkyl esters, fumaric acid, fumaric acid monoalkyl esters, crotonic acid, itaconic acid, itaconic acid monoalkyl esters, itaconic acid glycol monoether, citraconic acid, citraconic acid monoalkyl esters, and cinnamic acid, and metal salts thereof.

[0030] In the present invention, "(salt)" means an acid or a salt thereof. For example, an unsaturated monocarboxylic acid (salt) having 3 to 30 carbon atoms means an unsaturated monocarboxylic acid or a salt thereof. In the present invention, "(meth)acrylic" means methacrylic acid or acrylic acid. In the present invention, "(meth)acryloyl" means methacryloyl or acryloyl. In the present invention, "(meth)acrylate" means methacrylate or acrylate.

[0031] (3) Sulfonic acid-containing vinyl monomers, vinyl sulfate monoesters, and their salts Examples of the sulfone group-containing vinyl monomer, vinyl sulfate monoester, and salts thereof include alkene sulfonic acids (salts) having 2 to 14 carbon atoms, alkyl sulfonic acids (salts) having 2 to 24 carbon atoms, sulfo(hydroxy)alkyl-(meth)acrylates (salts), (meth)acrylamides (salts), and alkylarylsulfosuccinic acids (salts). Specifically, an example of an alkene sulfonic acid having 2 to 14 carbon atoms is vinyl sulfonic acid (salt), an example of an alkyl sulfonic acid (salt) having 2 to 24 carbon atoms is α-methylstyrene sulfonic acid (salt), and an example of a sulfo(hydroxy)alkyl-(meth)acrylate (salt) or (meth)acrylamide (salt) is sulfopropyl(meth)acrylate (salt), sulfuric acid ester (salt), or a sulfonic acid group-containing vinyl monomer (salt).

[0032] (4) Phosphate-containing vinyl monomers and their salts Examples of the phosphoric acid group-containing vinyl monomer and its salt include (meth)acryloyloxyalkyl (carbon number 1 to 24) phosphoric acid monoester (salt), (meth)acryloyloxyalkyl (carbon number 1 to 24) phosphonic acid (salt), and the like. Specific examples of the (meth)acryloyloxyalkyl (carbon number 1 to 24) phosphate monoester (salt) include 2-hydroxyethyl (meth)acryloyl phosphate (salt), phenyl-2-acryloyloxyethyl phosphate (salt), and the like. Specific examples of the (meth)acryloyloxyalkyl (carbon number: 1 to 24)phosphonic acid (salt) include 2-acryloyloxyethylphosphonic acid (salt).

[0033] Examples of the salts of (2) to (4) above include alkali metal salts (sodium salts, potassium salts, etc.), alkaline earth metal salts (calcium salts, magnesium salts, etc.), ammonium salts, amine salts, and quaternary ammonium salts.

[0034] (5) Hydroxyl group-containing vinyl monomer Examples of the hydroxyl group-containing vinyl monomer include hydroxystyrene, N-methylol (meth)acrylamide, hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, polyethylene glycol mono(meth)acrylate, (meth)allyl alcohol, crotyl alcohol, isocrotyl alcohol, 1-buten-3-ol, 2-buten-1-ol, 2-butene-1,4-diol, propargyl alcohol, 2-hydroxyethyl propenyl ether, and sucrose allyl ether.

[0035] (6) Nitrogen-containing vinyl monomers Examples of the nitrogen-containing vinyl monomer include (6-1) amino group-containing vinyl monomers, (6-2) amide group-containing vinyl monomers, (6-3) nitrile group-containing vinyl monomers, (6-4) quaternary ammonium cation group-containing vinyl monomers, and (6-5) nitro group-containing vinyl monomers. (6-1) Examples of amino group-containing vinyl monomers include aminoethyl (meth)acrylate. (6-2) Examples of amide group-containing vinyl monomers include (meth)acrylamide and N-methyl(meth)acrylamide. (6-3) Examples of nitrile group-containing vinyl monomers include (meth)acrylonitrile, cyanostyrene, and cyanoacrylate. (6-4) Examples of the vinyl monomer containing a quaternary ammonium cation group include quaternized products of tertiary amine group-containing vinyl monomers such as dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, dimethylaminoethyl (meth)acrylamide, diethylaminoethyl (meth)acrylamide, and diallylamine (which are quaternized with a quaternizing agent such as methyl chloride, dimethyl sulfate, benzyl chloride, or dimethyl carbonate). (6-5) Examples of nitro group-containing vinyl monomers include nitrostyrene.

[0036] (7) Epoxy group-containing vinyl monomer Examples of the epoxy group-containing vinyl monomer include glycidyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, and p-vinylphenyl phenyl oxide.

[0037] (8) Halogen-containing vinyl monomers Examples of the halogen-containing vinyl monomer include vinyl chloride, vinyl bromide, vinylidene chloride, allyl chloride, chlorostyrene, bromostyrene, dichlorostyrene, chloromethylstyrene, tetrafluorostyrene, and chloroprene.

[0038] (9) Vinyl esters, vinyl (thio)ethers, vinyl ketones Examples of the vinyl ester include vinyl acetate, vinyl butyrate, vinyl propionate, vinyl butyrate, diallyl phthalate, diallyl adipate, isopropenyl acetate, vinyl methacrylate, methyl 4-vinyl benzoate, cyclohexyl methacrylate, benzyl methacrylate, phenyl (meth)acrylate, vinyl methoxyacetate, vinyl benzoate, ethyl α-ethoxyacrylate, alkyl (meth)acrylate having an alkyl group having 1 to 50 carbon atoms [methyl ( (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, dodecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, octadecyl (meth)acrylate, eicosyl (meth)acrylate, behenyl (meth)acrylate, etc.)], dialkyl fumarate (wherein the two alkyl groups are linear, branched or alicyclic groups having 2 to 8 carbon atoms), dialkyl fumarates (wherein the two alkyl groups are linear, branched or alicyclic groups having 2 to 8 carbon atoms), vinyl monomers having polyalkylene glycol chains such as poly(meth)allyloxyalkanes [diallyloxyethane, triallyloxyethane, tetraallyloxyethane, tetraallyloxypropane, tetraallyloxybutane, tetramethallyloxyethane, etc.]; alcohol ethylene oxide 10 mol adduct (meth)acrylate, lauryl alcohol ethylene oxide 30 mol adduct (meth)acrylate, etc.], poly(meth)acrylates [poly(meth)acrylates of polyhydric alcohols: ethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, polyethylene glycol di(meth)acrylate, etc.]. The vinyl (thio)ethers include, for example, vinyl methyl ether. The vinyl ketone may, for example, be vinyl methyl ketone.

[0039] (10) Other vinyl monomers Examples of the other vinyl monomers include tetrafluoroethylene, fluoroacrylate, isocyanatoethyl (meth)acrylate, and m-isopropenyl-α,α-dimethylbenzyl isocyanate.

[0040] In the synthesis of the resin (b1), the vinyl monomers (1) to (10) may be used alone or in combination of two or more. As the resin (b1), from the viewpoint of low-temperature fixability, a styrene-(meth)acrylic acid ester copolymer and a (meth)acrylic acid ester copolymer are preferred, and a styrene-(meth)acrylic acid ester copolymer is more preferred. When the resin (b1) has a carboxylic acid, an acid value is imparted to the resin, and it becomes easy to form toner particles in which the fine resin particles (B) are adhered to the surface of the toner particles.

[0041] The vinyl monomer used in the resin (b2) may be the same as that used in the resin (b1). In synthesizing the resin (b2), the vinyl monomers (1) to (10) listed in the above resin (b1) may be used alone or in combination of two or more. As the resin (b2), from the viewpoint of low-temperature fixability, a styrene-(meth)acrylic acid ester copolymer and a (meth)acrylic acid ester copolymer are preferred, and a styrene-(meth)acrylic acid ester copolymer is more preferred.

[0042] The viscoelastic loss modulus G'' of the resin (b1) at 100° C. and a frequency of 1 Hz is preferably from 1.5 MPa to 100 MPa, more preferably from 1.7 MPa to 30 MPa, and even more preferably from 2.0 MPa to 10 MPa. The loss modulus G" of the viscoelastic properties of the resin (b2) at 100° C. and a frequency of 1 Hz is preferably 0.01 MPa to 1.0 MPa, more preferably 0.02 MPa to 0.5 MPa, and even more preferably 0.05 MPa to 0.3 MPa. When the viscoelastic characteristic loss modulus G″ is within this range, it is easy to form toner particles in which the resin fine particles (B) containing the resin (b1) and the resin (b2) as constituent components in the same particle are adhered to the surface of the toner particle.

[0043] The loss modulus G″ of the viscoelastic properties of the resins (b1) and (b2) at a frequency of 1 Hz and 100° C. can be adjusted by changing the types and composition ratio of the constituent monomers or by adjusting the polymerization conditions (types and amounts of initiator and chain transfer agent, reaction temperature, etc.). Specifically, for example, by using the following composition, it is possible to adjust each G'' to be within the above-mentioned range. (1) Regarding the glass transition temperature (Tg1) calculated from the constituent monomers of the resin (b1), and the glass transition temperature (Tg2) calculated from the constituent monomers of the resin (b2), Tg1 is preferably 0°C to 150°C, more preferably 50°C to 100°C, and Tg2 is preferably -30°C to 100°C, more preferably 0°C to 80°C, and most preferably 30°C to 60°C. The glass transition temperature (Tg) calculated from the constituent monomers is a value that can be calculated by the Fox method. Here, the Fox method [TGFox, Phys. Rev., 86, 652 (1952)] is a method for estimating the Tg of a copolymer from the Tg of each homopolymer represented by the following formula. 1 / Tg=W1 / Tg1+W2 / Tg2++Wn / Tgn [In the formula, Tg is the glass transition temperature (expressed in absolute temperature) of the copolymer, Tg1, Tg2...Tgn are the glass transition temperatures (expressed in absolute temperature) of the homopolymers of each monomer component, and W1, W2...Wn are the weight fractions of each monomer component.] (2) Regarding the calculated acid value (AV1) of the resin (b1) and the calculated acid value (AV2) of the resin (b2), (AV1) is preferably 75 mgKOH / g to 400 mgKOH / g, more preferably 150 mgKOH / g to 300 mgKOH / g, and (AV2) is 0 mgKOH / g to 50 mgKOH / g, more preferably 0 mgKOH / g to 20 mgKOH / g, and most preferably 0 mgKOH / g. The calculated acid value is a theoretical acid value calculated from the molar amount of acidic groups contained in the constituent monomers and the total weight of the constituent monomers.

[0044] As for the resin (b1), an example of a constituent monomer that satisfies the conditions (1) and (2) is a resin that contains, as a constituent monomer, preferably 10% by mass to 80% by mass, and more preferably 30% by mass to 60% by mass of styrene, and preferably 10% by mass to 60% by mass in total, and more preferably 30% by mass to 50% by mass of methacrylic acid and / or acrylic acid, based on the total weight of the resin (b1). Furthermore, the resin (b2) may, for example, be a resin containing, as a constituent monomer, preferably 10% by mass to 100% by mass, and more preferably 30% by mass to 90% by mass of styrene, based on the total weight of the resin (b2), and containing, in total, preferably 0% by mass to 7.5% by mass, and more preferably 0% by mass to 2.5% by mass of methacrylic acid and / or acrylic acid, based on the total weight of the resin (b2).

[0045] (3) Polymerization conditions (types and amounts of initiator and chain transfer agent, reaction temperature, etc.) are adjusted. Specifically, with respect to the number average molecular weights (Mn1) and (Mn2) of the resin (b1) and the resin (b2), (Mn1) is preferably set to 2,000 to 2,000,000, more preferably 20,000 to 200,000, and (Mn2) is preferably set to 1,000 to 1,000,000, more preferably 10,000 to 100,000.

[0046] The loss modulus G″ of the viscoelastic properties in the present invention is measured, for example, by using the following viscoelasticity measuring device. Equipment: ARES-24A (Rheometrics) Fixture: 25mm parallel plate Frequency: 1Hz Distortion rate: 10% Heating rate: 5℃ / min

[0047] The acid value (AVb1) of the resin (b1) is preferably from 75 mgKOH / g to 400 mgKOH / g, and more preferably from 150 mgKOH / g to 300 mgKOH / g. If the acid value is within this range, the fine resin particles (B) containing a vinyl-based unit in which the resin (b1) and the resin (b2) are contained as constituents in the same particle are likely to form particles adhered to the surface of the toner. Resin (b1) having an acid value within this range is a resin that contains methacrylic acid and / or acrylic acid in a total amount of preferably 10% by mass to 60% by mass, and more preferably 30% by mass to 50% by mass, based on the total weight of resin (b1).

[0048] From the viewpoint of low-temperature fixability, the acid value (AVb2) of the resin (b2) is preferably from 0 mgKOH / g to 50 mgKOH / g, more preferably from 0 mgKOH / g to 20 mgKOH / g, and even more preferably 0 mgKOH / g. Resin (b2) having an acid value within this range is a resin that contains methacrylic acid and / or acrylic acid in a total amount of preferably 0% to 7.5% by mass, and more preferably 0% to 2.5% by mass, based on the total weight of resin (b2). The acid value in the present invention is measured by the method of JIS K0070:1992.

[0049] The glass transition temperature of the resin (b1) is preferably higher than the glass transition temperature of the resin (b2), more preferably 10° C. or more higher, and even more preferably 20° C. or more higher. Within this range, the ease of forming toner particles in which the resin fine particles (B) are adhered to the surface of the toner and the low-temperature fixability of the toner particles of the present invention are well balanced.

[0050] The glass transition temperature (hereinafter abbreviated as Tg) of the resin (b1) is preferably from 0°C to 150°C, and more preferably from 50°C to 100°C. When the glass transition temperature is 0° C. or higher, the heat-resistant storage stability can be improved, and when the glass transition temperature is 150° C. or lower, the low-temperature fixability is less hindered. The Tg of the resin (b2) is preferably −30° C. to 100° C., more preferably 0° C. to 80° C., and even more preferably 30° C. to 60° C. If the glass transition temperature is −30° C. or higher, the heat-resistant storage stability can be improved, and if the glass transition temperature is 100° C. or lower, there is little inhibition of low-temperature fixability.

[0051] In the present invention, Tg is measured by the method (DSC) specified in ASTM D3418-82 using "DSC20, SSC / 580" [manufactured by a subsidiary of Seiko Electronics Industries].

[0052] From the viewpoint of ease of forming toner particles, the solubility parameter (hereinafter abbreviated as SP value) of the resin (b1) is set to 9 (cal / cm 3 ) 1 / 2 ~13(cal / cm 3 ) 1 / 2 is preferable, and 9.5 (cal / cm 3 ) 1 / 2 ~12.5(cal / cm 3 ) 1 / 2 More preferably, 10.5 (cal / cm 3 ) 1 / 2 ~11.5(cal / cm 3 ) 1 / 2 is more preferred. The SP value of the resin (b1) can be adjusted by changing the types and composition ratio of the constituent monomers. From the viewpoint of ease of forming toner particles, the SP value of the resin (b2) is set to 8.5 (cal / cm 3 ) 1 / 2 ~12.5(cal / cm 3 ) 1 / 2 is preferable, and 9 (cal / cm 3 ) 1 / 2 ~12(cal / cm 3 ) 1 / 2More preferably, 10 (cal / cm 3 ) 1 / 2 ~11(cal / cm 3 ) 1 / 2 is more preferred. The SP value of the resin (b2) can be adjusted by changing the types and composition ratio of the constituent monomers.

[0053] The SP value in the present invention is calculated by the method by Fedors [Polym. Eng. Sci. 14(2)152, (1974)].

[0054] From the viewpoint of Tg of the resin (b1) and copolymerizability with other monomers, the resin (b1) preferably contains 10% by mass to 80% by mass, and more preferably 30% by mass to 60% by mass of styrene as a constituent monomer, based on the total mass of the resin (b1). From the viewpoint of Tg of the resin (b2) and copolymerizability with other vinyl monomers, the resin (b2) preferably contains 10% by mass to 100% by mass, and more preferably 30% by mass to 90% by mass of styrene as a constituent monomer, based on the total mass of the resin (b2).

[0055] The number average molecular weight (Mn) of the resin (b1) is preferably 2,000 to 2,000,000, and more preferably 20,000 to 200,000. When the number average molecular weight is 2,000 or more, the heat-resistant storage stability is improved, and when it is 2,000,000 or less, the low-temperature fixability of the toner is less hindered.

[0056] The weight average molecular weight of the resin (b1) is preferably larger than that of the resin (b2), more preferably 1.5 times or more larger than that of the resin (b2), and even more preferably 2.0 times or more larger than that of the resin (b2). Within this range, the balance between the ease of forming toner particles and low-temperature fixability is excellent.

[0057] The weight average molecular weight (Mw) of the resin (b1) is preferably 20,000 to 20,000,000, and more preferably 200,000 to 2,000,000. When the weight average molecular weight is 20,000 or more, the heat resistant storage stability is improved, and when it is 20,000,000 or less, the low temperature fixability is less hindered.

[0058] The Mn of the resin (b2) is preferably 1,000 to 1,000,000, and more preferably 10,000 to 100,000. When the Mn is 1,000 or more, the heat-resistant storage stability of the toner is improved, and when it is 1,000,000 or less, the low-temperature fixability of the toner is less hindered.

[0059] The Mw of the resin (b2) is preferably 10,000 to 10,000,000, and more preferably 100,000 to 1,000,000. When the Mw is 10,000 or more, the heat-resistant storage stability of the toner is improved, and when it is 10,000,000 or less, the low-temperature fixability of the toner is less hindered.

[0060] Among these, it is preferred that the Mw of the resin (b1) is 200,000 to 2,000,000, the Mw of the resin (b2) is 100,000 to 500,000, and the "Mw of (b1)" is greater than the "Mw of (b2)".

[0061] In the present invention, Mn and Mw can be measured by gel permeation chromatography (GPC) under the following conditions. Equipment (example): "HLC-8120" [manufactured by Tosoh Corporation] Column (example): "TSK GEL GMH6" [Tosoh Corporation] x 2 Measurement temperature: 40℃ Sample solution: 0.25% by weight tetrahydrofuran solution (undissolved matter was removed by filtration using a glass filter) Solution injection volume: 100μl Detector: Refractive index detector Reference material: 12 standard polystyrenes (TSKstandard POLYSTYRENE) (molecular weight: 500, 1,050, 2,800, 5,970, 9,100, 18,100, 37,900, 96,400, 190,000, 355,000, 1,090,000, 2,890,000) [manufactured by Tosoh Corporation]

[0062] The weight ratio of the resin (b1) to the resin (b2) in the resin fine particles (B) is preferably 5 / 95 to 95 / 5, more preferably 25 / 75 to 75 / 25, and even more preferably 40 / 60 to 60 / 40. When the weight ratio of the resin (b1) to the resin (b2) is 5 / 95 or more, the toner has excellent heat-resistant storage stability, and when the weight ratio of the resin (b1) to the resin (b2) is 95 / 5 or less, the toner particles in which the resin fine particles (B) are attached to the surfaces of the toner resin particles are easily formed.

[0063] The resin fine particles (B) can be produced by known methods, such as the following production methods (I) to (V). (I) A method of seed polymerization of constituent monomers of resin (b2) using fine particles of resin (b1) in an aqueous dispersion as seeds. (II) A method of carrying out seed polymerization of constituent monomers of resin (b1) using fine particles of resin (b2) in an aqueous dispersion as seeds. (III) A method in which a mixture of resin (b1) and resin (b2) is emulsified in an aqueous medium to obtain an aqueous dispersion of resin fine particles. (IV) A method in which a mixture of resin (b1) and constituent monomers of resin (b2) is emulsified in an aqueous medium, and then the constituent monomers of resin (b2) are polymerized to obtain an aqueous dispersion of resin fine particles. (V) A method in which a mixture of resin (b2) and constituent monomers of resin (b1) is emulsified in an aqueous medium, and then the constituent monomers of resin (b1) are polymerized to obtain an aqueous dispersion of resin fine particles.

[0064] The fact that the resin microparticles (B) contain the shell resin (b1) and the core resin (b2) as constituent components within the same particle can be confirmed by observing an element mapping image of a cut surface of the resin microparticles (B) using a known surface elemental analysis device (TOF-SIMSEDX-SEM, etc.) and by observing an electron microscope image of a cut surface of the resin microparticles (B) stained with a stain corresponding to the functional groups contained in the resin (b1) and the resin (b2). Furthermore, the resin microparticles obtained by this method may be obtained as a mixture containing resin microparticles whose only constituent resin component is resin (b1) and resin microparticles whose only constituent resin component is resin (b2), in addition to resin microparticles (B) containing resin (b1) and resin (b2) as constituent components within the same particle. In the composite process described below, the mixture may be used as is, or only the resin microparticles (B) may be isolated and used.

[0065] Specific examples of (I) include a method in which the constituent monomers of (b1) are polymerized by dropwise polymerization to produce an aqueous dispersion of resin microparticles containing (b1), and then the constituent monomers of (b2) are polymerized using this as a seed; and a method in which (b1) produced in advance by solution polymerization or the like is emulsified and dispersed in water, and then the constituent monomers of (b2) are polymerized using this as a seed.

[0066] Specific examples of (II) include a method in which the constituent monomer of (b2) is polymerized by dropwise polymerization to produce an aqueous dispersion of resin microparticles containing (b2), and then the constituent monomer of (b1) is polymerized using this as a seed; and a method in which (b2) produced in advance by solution polymerization or the like is emulsified and dispersed in water, and then the constituent monomer of (b1) is polymerized using this as a seed.

[0067] A specific example of (III) is a method in which solutions or melts of (b1) and (b2) previously prepared by solution polymerization or the like are mixed together, and the mixture is then emulsified and dispersed in an aqueous medium.

[0068] Specific examples of (IV) include a method in which (b1), which has been produced in advance by solution polymerization or the like, is mixed with constituent monomers of (b2), the mixture is emulsified and dispersed in an aqueous medium, and then the constituent monomers of (b2) are polymerized; and a method in which (b1) is produced in the constituent monomers of (b2), the mixture is emulsified and dispersed in an aqueous medium, and then the constituent monomers of (b2) are polymerized.

[0069] Specific examples of (V) include a method in which (b2), which has been produced in advance by solution polymerization or the like, is mixed with the constituent monomers of (b1), the mixture is emulsified and dispersed in an aqueous medium, and then the constituent monomers of (b1) are polymerized; and a method in which (a2) is produced in the constituent monomers of (b1), the mixture is emulsified and dispersed in an aqueous medium, and then the constituent monomers of (b1) are polymerized.

[0070] In the present invention, any of the above production methods (I) to (V) is suitable.

[0071] The resin fine particles (B) are preferably used in the form of an aqueous dispersion. The substance (aqueous medium) used in the aqueous dispersion is not particularly limited as long as it dissolves in water, and can be appropriately selected depending on the purpose, and examples thereof include a surfactant (D), a buffering agent, a protective colloid, etc. These may be used alone or in combination of two or more. The aqueous medium used in the aqueous dispersion is not particularly limited as long as it is a liquid essentially containing water, and examples thereof include an aqueous solution containing water.

[0072] Examples of the surfactant (D) include nonionic surfactants (D1), anionic surfactants (D2), cationic surfactants (D3), amphoteric surfactants (D4), and other emulsifying dispersants (D5).

[0073] Examples of the nonionic surfactant (D1) include AO (alkylene oxide) addition type nonionic surfactants and polyhydric alcohol type nonionic surfactants. Examples of the AO-addition type nonionic surfactant include EO adducts of aliphatic alcohols having 10 to 20 carbon atoms, EO adducts of phenols, EO (ethylene oxide) adducts of nonylphenols, EO adducts of alkylamines having 8 to 22 carbon atoms, and EO adducts of poly(oxypropylene) glycols. Examples of the polyhydric alcohol type nonionic surfactant include fatty acid (having 8 to 24 carbon atoms) esters of polyhydric (tri- to octahydric or higher) alcohols (having 2 to 30 carbon atoms) (e.g., glycerin monostearate, glycerin monooleate, sorbitan monolaurate, sorbitan monooleate, etc.), alkyl (having 4 to 24 carbon atoms) poly(degree of polymerization 1 to 10) glycosides, and the like.

[0074] Examples of the anionic surfactant (D2) include ether carboxylic acids or salts thereof having a hydrocarbon group having 8 to 24 carbon atoms, sulfate esters or ether sulfate esters and salts thereof having a hydrocarbon group having 8 to 24 carbon atoms, sulfonates having a hydrocarbon group having 8 to 24 carbon atoms, sulfosuccinates having one or two hydrocarbon groups having 8 to 24 carbon atoms, phosphate esters or ether phosphate esters and salts thereof having a hydrocarbon group having 8 to 24 carbon atoms, fatty acid salts having a hydrocarbon group having 8 to 24 carbon atoms, and acylated amino acid salts having a hydrocarbon group having 8 to 24 carbon atoms. Examples of the ether carboxylic acid or salt thereof having a hydrocarbon group having 8 to 24 carbon atoms include sodium lauryl ether acetate, (poly)oxyethylene (number of moles added: 1 to 100) sodium lauryl ether acetate, and the like. Examples of the sulfate ester or ether sulfate ester having a hydrocarbon group having 8 to 24 carbon atoms and salts thereof include sodium lauryl sulfate, (poly)oxyethylene (number of moles added: 1 to 100) sodium lauryl sulfate, (poly)oxyethylene (number of moles added: 1 to 100) triethanolamine lauryl sulfate, (poly)oxyethylene (number of moles added: 1 to 100) sodium coconut oil fatty acid monoethanolamide sulfate, and the like. Examples of the sulfonate having a hydrocarbon group having 8 to 24 carbon atoms include sodium dodecylbenzenesulfonate. Examples of the phosphate ester or ether phosphate ester having a hydrocarbon group having 8 to 24 carbon atoms and salts thereof include sodium lauryl phosphate, and sodium (poly)oxyethylene (addition mole number 1 to 100) lauryl ether phosphate. Examples of the fatty acid salt having a hydrocarbon group having 8 to 24 carbon atoms include sodium laurate and triethanolamine laurate. Examples of the acylated amino acid salts having a hydrocarbon group having 8 to 24 carbon atoms include sodium methyl coconut taurate, sodium coconut sarcosine, triethanolamine coconut sarcosine, N-triethanolamine coconut acyl-L-glutamate, sodium N-sodium coconut acyl-L-glutamate, and sodium lauroylmethyl-β-alanine.

[0075] Examples of the cationic surfactant (D3) include quaternary ammonium salt types and amine salt types. Examples of the quaternary ammonium salt type include stearyl trimethyl ammonium chloride, behenyl trimethyl ammonium chloride, distearyl dimethyl ammonium chloride, lanolin fatty acid aminopropyl ethyl dimethyl ammonium ethyl sulfate, and the like. Examples of the amine salt type include stearic acid diethylaminoethylamide lactate, dilaurylamine hydrochloride, and oleylamine lactate.

[0076] Examples of the amphoteric surfactant (D4) include betaine-type amphoteric surfactants and amino acid-type amphoteric surfactants. Examples of the betaine type amphoteric surfactant include coconut oil fatty acid amidopropyl dimethylaminoacetic acid betaine, lauryl dimethylaminoacetic acid betaine, 2-alkyl-N-carboxymethyl-N-hydroxyethyl imidazolinium betaine, and lauryl hydroxysulfobetaine. Examples of the amino acid type amphoteric surfactant include sodium β-laurylaminopropionate.

[0077] Other emulsifying dispersants (D5) include, for example, reactive activators. The reactive activator is not particularly limited as long as it has radical reactivity and can be appropriately selected depending on the purpose. Examples of the reactive activator include ADEKA REASOAP (registered trademark) SE-10N, SR-10, SR-20, SR-30, ER-20, and ER-30 (all manufactured by ADEKA CORPORATION), AQUALON (registered trademark), HS-10, KH-05, KH-10, and KH-1025 (all manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd.), ELEMINOL (registered trademark) JS-20 (manufactured by SANYO CHEMICAL INDUSTRIES, LTD.), LATEMUL (registered trademark) D-104, PD-420, and PD-430 (all manufactured by ADEKA CORPORATION), and the like. Examples of suitable emulsifying dispersants include, for example, polycaprolactone polyol and polyether diol linked together via polyisocyanate, and the like. Examples of suitable emulsifying dispersants include, for example, polycaprolactone polyol and polyether diol linked together via polyisocyanate, and the like. Examples of suitable emulsifying dispersing agents include, for example, polycaprolactone polyol and polyether diol linked together via polyisocyanate, and the like.

[0078] As the surfactant (D), from the viewpoint of stabilizing oil droplets during emulsification and dispersion, obtaining a desired shape, and sharpening the particle size distribution, (D1), (D2), (D5), and combinations of these are preferred, and a combination of (D1) and (D5), and a combination of (D2) and (D5) are more preferred.

[0079] Examples of the buffer include sodium acetate, sodium citrate, and sodium bicarbonate. Examples of the protective colloid include water-soluble cellulose compounds and alkali metal salts of polymethacrylic acid.

[0080] The resin microparticles (B) may contain, in addition to the shell resin (b1) and the core resin (b2), other resin components, an initiator (and its residue), a chain transfer agent, an antioxidant, a plasticizer, a preservative, a reducing agent, an organic solvent, etc.

[0081] Examples of the other resin components include vinyl resins other than the resins used for the shell resin (b1) and the core resin (b2), polyurethane resins, epoxy resins, polyester resins, polyamide resins, polyimide resins, silicon resins, phenol resins, melamine resins, urea resins, aniline resins, ionomer resins, polycarbonate resins, and the like.

[0082] The initiator (and its residue) includes known radical polymerization initiators, and specific examples thereof include persulfate initiators such as potassium persulfate and ammonium persulfate; azo initiators such as azobisisobutyronitrile; organic peroxides such as benzoyl peroxide, cumene hydroperoxide, tertiary butyl hydroperoxide, tertiary butyl peroxyisopropyl monocarbonate, and tertiary butyl peroxybenzoate; and hydrogen peroxide.

[0083] Examples of the chain transfer agent include n-dodecyl mercaptan, tert-dodecyl mercaptan, n-butyl mercaptan, 2-ethylhexyl thioglycolate, 2-mercaptoethanol, β-mercaptopropionic acid, and α-methylstyrene dimer.

[0084] Examples of the antioxidant include phenol compounds, paraphenylenediamine, hydroquinone, organic sulfur compounds, and organic phosphorus compounds.

[0085] Examples of the phenol compound include 2,6-di-t-butyl-p-cresol, butylated hydroxyanisole, 2,6-di-t-butyl-4-ethylphenol, stearyl-β-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, 2,2′-methylene-bis-(4-methyl-6-t-butylphenol), 2,2′-methylene-bis-(4-ethyl-6-t-butylphenol), 4,4′-thiobis-(3-methyl-6-t-butylphenol), 4,4′-butylidenebis-(3-methyl-6-t-butylphenol), and 4,4′-butylidenebis-(3-methyl-6-t-butylphenol). methyl-6-t-butylphenol), 1,1,3-tris-(2-methyl-4-hydroxy-5-t-butylphenyl)butane, 1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene, tetrakis-[methylene-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate]methane, bis[3,3'-bis(4'-hydroxy-3'-t-butylphenyl)butyric acid]glycol ester, tocopherol, etc.

[0086] Examples of the paraphenylenediamine include N-phenyl-N'-isopropyl-p-phenylenediamine, N,N'-di-sec-butyl-p-phenylenediamine, N-phenyl-N-sec-butyl-p-phenylenediamine, N,N'-di-isopropyl-p-phenylenediamine, and N,N'-dimethyl-N,N'-di-t-butyl-p-phenylenediamine.

[0087] Examples of the hydroquinone include 2,5-di-t-octylhydroquinone, 2,6-didodecylhydroquinone, 2-dodecylhydroquinone, 2-dodecyl-5-chlorohydroquinone, 2-t-octyl-5-methylhydroquinone, and 2-(2-octadecenyl)-5-methylhydroquinone.

[0088] Examples of the organic sulfur compound include dilauryl-3,3'-thiodipropionate, distearyl-3,3'-thiodipropionate, and ditetradecyl-3,3'-thiodipropionate.

[0089] Examples of the organic phosphorus compound include triphenylphosphine, tri(nonylphenyl)phosphine, tri(dinonylphenyl)phosphine, tricresylphosphine, and tri(2,4-dibutylphenoxy)phosphine.

[0090] Examples of the plasticizer include phthalic acid esters, aliphatic dibasic acid esters, trimellitic acid esters, phosphate esters, and fatty acid esters. Examples of the phthalate ester include dibutyl phthalate, dioctyl phthalate, butyl benzyl phthalate, and diisodecyl phthalate. Examples of the aliphatic dibasic acid ester include di-2-ethylhexyl adipate and 2-ethylhexyl sebacate. Examples of the trimellitic acid ester include tri-2-ethylhexyl trimellitate and trioctyl trimellitate. Examples of the phosphate ester include triethyl phosphate, tri-2-ethylhexyl phosphate, and tricresyl phosphate. The fatty acid ester may, for example, be butyl oleate.

[0091] Examples of the preservatives include organic nitrogen sulfur compound preservatives and organic sulfur halide preservatives.

[0092] Examples of the reducing agent include reducing organic compounds such as ascorbic acid, tartaric acid, citric acid, glucose, and formaldehyde sulfoxylate metal salts; and reducing inorganic compounds such as sodium thiosulfate, sodium sulfite, sodium bisulfite, and sodium metabisulfite.

[0093] Examples of the organic solvent include ketone solvents such as acetone and methyl ethyl ketone (hereinafter abbreviated as MEK); ester solvents such as ethyl acetate and γ-butyrolactone; ether solvents such as THF (tetrahydrofuran); amide solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone and N-methylcaprolactam; alcohol solvents such as isopropyl alcohol; and aromatic hydrocarbon solvents such as toluene and xylene.

[0094] The content of the resin particles is preferably 0.2% by mass to 5% by mass relative to the toner. When the sum of the resins (b1) and (b2) is in this range, the low-temperature fixability and heat-resistant storage stability are improved. When the content is 0.2 wt% or more relative to the toner, the problem of the heat-resistant storage stability being deteriorated can be prevented, and when it is 5 wt% or less, the problem of the low-temperature fixability being reduced can be prevented.

[0095] <Toner base particles> The toner base particles (hereinafter, sometimes referred to as "toner base" or "base particles") contain a binder resin, a colorant, and a wax, and further contain other components as required.

[0096] <<Binding resin>> The binder resin is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include polyester resin, styrene-acrylic resin, polyol resin, vinyl resin, polyurethane resin, epoxy resin, polyamide resin, polyimide resin, silicon resin, phenol resin, melamine resin, urea resin, aniline resin, ionomer resin, polycarbonate resin, etc. These may be used alone or in combination of two or more. Among these, polyester resin is preferred because it can impart flexibility to the toner.

[0097] <<<Polyester resin>>> The polyester resin is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include crystalline polyester resins, amorphous polyester resins, modified polyester resins, etc. These may be used alone or in combination of two or more.

[0098] -Amorphous polyester resin- The amorphous polyester resin (hereinafter, also referred to as "amorphous polyester", "amorphous polyester", "amorphous polyester resin", "unmodified polyester resin", or "polyester resin component A") is not particularly limited and can be appropriately selected depending on the purpose. For example, there is an amorphous polyester resin obtained by reacting a polyol with a polycarboxylic acid. In the present invention, the amorphous polyester resin refers to a resin obtained by reacting a polyol with a polycarboxylic acid as described above. Modified polyester resins, such as prepolymers described below, and modified polyester resins obtained by subjecting the prepolymers to a crosslinking and / or elongation reaction, are not included in the amorphous polyester resins in the present invention, and are treated as modified polyester resins. The amorphous polyester is a polyester resin component that is soluble in tetrahydrofuran (THF). The amorphous polyester (polyester resin component A) is preferably a linear polyester resin.

[0099] The polyol includes, for example, a diol. Examples of the diol include alkylene (carbon number 2 to 3) oxide (average number of moles added: 1 to 10) adducts of bisphenol A such as polyoxypropylene(2.2)-2,2-bis(4-hydroxyphenyl)propane and polyoxyethylene(2.2)-2,2-bis(4-hydroxyphenyl)propane; ethylene glycol, propylene glycol; hydrogenated bisphenol A, and alkylene (carbon number 2 to 3) oxide (average number of moles added: 1 to 10) adducts of hydrogenated bisphenol A. These may be used alone or in combination of two or more. Among these, the polyol preferably contains 40 mol % or more of alkylene glycol.

[0100] The polycarboxylic acid may, for example, be a dicarboxylic acid. Examples of the dicarboxylic acid include adipic acid, phthalic acid, isophthalic acid, terephthalic acid, fumaric acid, maleic acid, dodecenylsuccinic acid, octylsuccinic acid, and other alkyl groups having 1 to 20 carbon atoms; and succinic acid substituted with an alkenyl group having 2 to 20 carbon atoms. These may be used alone or in combination of two or more. Among these, it is preferable that the polycarboxylic acid contains 50 mol % or more of terephthalic acid.

[0101] The polyester resin component A may contain a trivalent or higher carboxylic acid and / or a trivalent or higher alcohol, a trivalent or higher epoxy compound, or the like at the end of the resin chain in order to adjust the acid value and hydroxyl value. Among these, it is preferable to contain a trihydric or higher aliphatic alcohol, from the viewpoint of preventing unevenness and obtaining sufficient gloss and image density. Examples of the trivalent or higher carboxylic acid include trimellitic acid, pyromellitic acid, and acid anhydrides thereof. Examples of the trihydric or higher alcohol include glycerin, pentaerythritol, and trimethylolpropane.

[0102] The molecular weight of the polyester resin component A is not particularly limited and can be appropriately selected depending on the purpose, but is preferably in the following range. The weight average molecular weight (Mw) of the polyester resin component A is preferably from 3,000 to 10,000, and more preferably from 4,000 to 7,000. The number average molecular weight (Mn) of the polyester resin component A is preferably from 1,000 to 4,000, and more preferably from 1,500 to 3,000. The molecular weight ratio (Mw / Mn) of the polyester resin component A is preferably from 1.0 to 4.0, and more preferably from 1.0 to 3.5. The molecular weight can be measured by GPC (gel permeation chromatography). The reason why the molecular weight is preferably within the above range is that if the molecular weight is too low, the toner may be inferior in heat resistant storage stability and durability against stress such as stirring in a developing machine, while if the molecular weight is too high, the viscoelasticity of the toner when melted may increase and the low-temperature fixability may be inferior. Also, if the amount of the component having a molecular weight of 600 or less is too large, the toner may be inferior in heat resistant storage stability and durability against stress such as stirring in a developing machine, while if the amount of the component having a molecular weight of 600 or less is too small, the low-temperature fixability may be inferior.

[0103] The THF soluble component having a molecular weight of 600 or less is preferably 2% by mass to 10% by mass. As a method for adjusting the content of this component, there may be mentioned a method in which polyester resin component A is extracted with methanol, and components having a molecular weight of 600 or less are removed, followed by purification.

[0104] The acid value of the polyester resin component A is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 1 mgKOH / g to 50 mgKOH / g, more preferably 5 mgKOH / g to 30 mgKOH / g. When the acid value is 1 mgKOH / g or more, the toner tends to be negatively charged, and furthermore, the affinity between the paper and the toner is improved when fixed to the paper, and low-temperature fixability can be improved. On the other hand, when the acid value is 50 mgKOH / g or less, the problem of a decrease in charging stability, particularly charging stability against environmental changes, can be prevented.

[0105] The hydroxyl value of the polyester resin component A is not particularly limited and may be appropriately selected depending on the purpose, but is preferably 5 mgKOH / g or more.

[0106] The Tg of the polyester resin component A is preferably 40° C. to 65° C., more preferably 45° C. to 65° C., and even more preferably 50° C. to 60° C. When the Tg is 40° C. or higher, the toner has improved heat-resistant storage stability and durability against stress such as stirring in a developing machine, and also has improved filming resistance. On the other hand, when the Tg is 65° C. or lower, the toner is less susceptible to deformation due to heat and pressure during fixing, and low-temperature fixing ability is improved.

[0107] The content of the polyester resin component A is preferably 80 parts by mass to 90 parts by mass with respect to 100 parts by mass of the toner.

[0108] -Modified polyester- The modified polyester resin (hereinafter sometimes referred to as "modified polyester" or "polyester resin component C") is not particularly limited and can be appropriately selected depending on the purpose. For example, a reaction product of an active hydrogen group-containing compound and a polyester resin (in this specification, sometimes referred to as a "prepolymer" or "polyester prepolymer") having a site capable of reacting with the active hydrogen group-containing compound can be mentioned. The modified polyester is a polyester resin insoluble in tetrahydrofuran (THF). The polyester resin component insoluble in tetrahydrofuran (THF) lowers Tg and melt viscosity, and ensures low-temperature fixability, while having a branched structure in the molecular skeleton and a three-dimensional network structure in the molecular chain, and thus has rubber-like properties in that it deforms but does not flow at low temperatures. Since the polyester resin component C has an active hydrogen group-containing compound and a site capable of reacting with the active hydrogen group-containing compound, these sites behave like pseudo-crosslinking points, and the rubber-like properties of the amorphous polyester resin A are enhanced, making it possible to produce a toner having excellent heat-resistant storage stability and high-temperature offset resistance.

[0109] --Compounds containing active hydrogen groups-- The active hydrogen group-containing compound is a compound that reacts with a polyester resin having a site capable of reacting with the active hydrogen group-containing compound.

[0110] The active hydrogen group is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include a hydroxyl group (alcoholic hydroxyl group and phenolic hydroxyl group), an amino group, a carboxyl group, a mercapto group, etc. These may be used alone or in combination of two or more kinds.

[0111] The active hydrogen group-containing compound is not particularly limited and can be appropriately selected depending on the purpose. However, when the polyester resin having a site capable of reacting with the active hydrogen group-containing compound is a polyester resin containing an isocyanate group, amines are preferred in that the polyester resin can be polymerized by an elongation reaction, a crosslinking reaction, or the like with the polyester resin. The amines are not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include diamines, trivalent or higher amines, amino alcohols, amino mercaptans, amino acids, blocked amino groups of these, etc. These may be used alone or in combination of two or more. Among these, diamines and mixtures of diamines with small amounts of trivalent or higher amines are preferred.

[0112] The diamine is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include aromatic diamines, alicyclic diamines, and aliphatic diamines. The aromatic diamine is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include phenylenediamine, diethyltoluenediamine, and 4,4'-diaminodiphenylmethane. The alicyclic diamine is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include 4,4'-diamino-3,3'-dimethyldicyclohexylmethane, diaminocyclohexane, and isophoronediamine. The aliphatic diamine is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include ethylenediamine, tetramethylenediamine, and hexamethylenediamine.

[0113] The trivalent or higher amine is not particularly limited and can be appropriately selected depending on the purpose. Examples thereof include diethylenetriamine and triethylenetetramine.

[0114] The amino alcohol is not particularly limited and can be appropriately selected depending on the purpose. Examples of the amino alcohol include ethanolamine and hydroxyethylaniline.

[0115] The amino mercaptan is not particularly limited and can be appropriately selected depending on the purpose. Examples of the amino mercaptan include aminoethyl mercaptan and aminopropyl mercaptan.

[0116] The amino acid is not particularly limited and can be appropriately selected depending on the purpose. Examples of the amino acid include aminopropionic acid and aminocaproic acid.

[0117] The blocked amino group is not particularly limited and can be appropriately selected depending on the purpose. Examples of the blocked amino group include ketimine compounds and oxazoline compounds obtained by blocking the amino group with ketones such as acetone, methyl ethyl ketone, and methyl isobutyl ketone.

[0118] --Polyester resin having a site capable of reacting with an active hydrogen group-containing compound-- The polyester resin having a site capable of reacting with the active hydrogen group-containing compound is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include a polyester resin containing an isocyanate group (hereinafter, sometimes referred to as a "polyester prepolymer having an isocyanate group"). The polyester resin having an isocyanate group is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include a reaction product of a polyester resin having an active hydrogen group obtained by polycondensing a polyol and a polycarboxylic acid with a polyisocyanate.

[0119] The polyol is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include diols, trihydric or higher alcohols, mixtures of diols and trihydric or higher alcohols, etc. These may be used alone or in combination of two or more. Among these, diols and mixtures of diols with a small amount of trihydric or higher alcohols are preferred.

[0120] The diol is not particularly limited and can be appropriately selected depending on the purpose. Examples of the diol include linear alkylene glycols, diols having an oxyalkylene group, alicyclic diols, bisphenols, alkylene oxide adducts of alicyclic diols, and alkylene oxide adducts of bisphenols. Examples of the chain alkylene glycol include ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butanediol, and 1,6-hexanediol. Examples of the diol having an oxyalkylene group include diethylene glycol, triethylene glycol, dipropylene glycol, polyethylene glycol, polypropylene glycol, and polytetramethylene glycol. Examples of the alicyclic diol include 1,4-cyclohexanedimethanol and hydrogenated bisphenol A. Examples of the bisphenols include bisphenol A, bisphenol F, and bisphenol S. Examples of the alkylene oxide include ethylene oxide, propylene oxide, and butylene oxide. The number of carbon atoms of the chain alkylene glycol is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 2 to 12. Among these, at least any one of a chain alkylene glycol having 2 to 12 carbon atoms and an alkylene oxide adduct of a bisphenol is preferred, and an alkylene oxide adduct of a bisphenol and a mixture of an alkylene oxide adduct of a bisphenol and a chain alkylene glycol having 2 to 12 carbon atoms are more preferred.

[0121] The trihydric or higher alcohol is not particularly limited and can be appropriately selected depending on the purpose. Examples of the trihydric or higher alcohol include aliphatic trihydric or higher alcohols, trihydric or higher polyphenols, and alkylene oxide adducts of trihydric or higher polyphenols. The trihydric or higher aliphatic alcohol is not particularly limited and can be appropriately selected depending on the purpose. Examples thereof include glycerin, trimethylolethane, trimethylolpropane, pentaerythritol, and sorbitol. The trivalent or higher polyphenols are not particularly limited and can be appropriately selected depending on the purpose. Examples thereof include trisphenol PA, phenol novolac, and cresol novolac. Examples of the alkylene oxide adducts of trivalent or higher polyphenols include those obtained by adding alkylene oxides such as ethylene oxide, propylene oxide, and butylene oxide to trivalent or higher polyphenols. When the diol and the trihydric or higher alcohol are used in combination, the mass ratio of the trihydric or higher alcohol to the diol (trihydric or higher alcohol / diol) is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 0.01% by mass to 10% by mass, and more preferably 0.01% by mass to 1% by mass.

[0122] The polycarboxylic acid is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include dicarboxylic acids, trivalent or higher carboxylic acids, mixtures of dicarboxylic acids and trivalent or higher carboxylic acids, etc. These may be used alone or in combination of two or more. Among these, dicarboxylic acids and mixtures of dicarboxylic acids with a small amount of trivalent or higher polycarboxylic acids are preferred.

[0123] The dicarboxylic acid is not particularly limited and can be appropriately selected depending on the purpose. Examples of the dicarboxylic acid include divalent alkanoic acids, divalent alkenoic acids, and aromatic dicarboxylic acids. The divalent alkanoic acid is not particularly limited and can be appropriately selected depending on the purpose. Examples of the divalent alkanoic acid include succinic acid, adipic acid, and sebacic acid. The divalent alkenoic acid is not particularly limited and can be appropriately selected depending on the purpose, but is preferably a divalent alkenoic acid having 4 to 20 carbon atoms. The divalent alkenoic acid having 4 to 20 carbon atoms is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include maleic acid and fumaric acid. The aromatic dicarboxylic acid is not particularly limited and can be appropriately selected depending on the purpose, but is preferably an aromatic dicarboxylic acid having 8 to 20 carbon atoms. The aromatic dicarboxylic acid having 8 to 20 carbon atoms is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include phthalic acid, isophthalic acid, terephthalic acid, and naphthalenedicarboxylic acid.

[0124] The tri- or higher carboxylic acid is not particularly limited and can be appropriately selected depending on the purpose. Examples of the tri- or higher carboxylic acid include aromatic tri- or higher carboxylic acids. The trivalent or higher aromatic carboxylic acid is not particularly limited and can be appropriately selected depending on the purpose, but is preferably a trivalent or higher aromatic carboxylic acid having 9 to 20 carbon atoms. The trivalent or higher aromatic carboxylic acid having 9 to 20 carbon atoms is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include trimellitic acid and pyromellitic acid.

[0125] As the polycarboxylic acid, an acid anhydride or a lower alkyl ester of any of a dicarboxylic acid, a tri- or higher carboxylic acid, and a mixture of a dicarboxylic acid and a tri- or higher carboxylic acid can also be used. The lower alkyl ester is not particularly limited and can be appropriately selected depending on the purpose. Examples of the lower alkyl ester include methyl ester, ethyl ester, and isopropyl ester. When the dicarboxylic acid and the tri- or higher carboxylic acid are used in combination, the mass ratio of the tri- or higher carboxylic acid to the dicarboxylic acid (tri- or higher carboxylic acid / dicarboxylic acid) is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 0.01% by mass to 10% by mass, and more preferably 0.01% by mass to 1% by mass.

[0126] When the polyol and the polycarboxylic acid are polycondensed, the equivalent ratio of the hydroxyl groups of the polyol to the carboxyl groups of the polycarboxylic acid (hydroxyl groups of the polyol / carboxyl groups of the polycarboxylic acid) is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 1 to 2, more preferably 1 to 1.5, and particularly preferably 1.02 to 1.3.

[0127] The content of the polyol-derived structural unit in the polyester prepolymer having an isocyanate group is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 0.5% by mass to 40% by mass, more preferably 1% by mass to 30% by mass, and particularly preferably 2% by mass to 20% by mass. If the content is less than 0.5% by mass, the hot offset resistance decreases, and it may be difficult to achieve both the heat resistant storage stability and the low-temperature fixability of the toner. If the content exceeds 40% by mass, the low-temperature fixability may decrease.

[0128] The polyisocyanate is not particularly limited and can be appropriately selected depending on the purpose. Examples of the polyisocyanate include aliphatic diisocyanates, alicyclic diisocyanates, aromatic diisocyanates, araliphatic diisocyanates, isocyanurates, and those blocked with phenol derivatives, oximes, caprolactam, etc. The aliphatic diisocyanate is not particularly limited and can be appropriately selected depending on the purpose. Examples of the aliphatic diisocyanate include tetramethylene diisocyanate, hexamethylene diisocyanate, methyl 2,6-diisocyanatocaproate, octamethylene diisocyanate, decamethylene diisocyanate, dodecamethylene diisocyanate, tetradecamethylene diisocyanate, trimethylhexane diisocyanate, and tetramethylhexane diisocyanate. The alicyclic diisocyanate is not particularly limited and can be appropriately selected depending on the purpose. Examples of the alicyclic diisocyanate include isophorone diisocyanate and cyclohexylmethane diisocyanate. The aromatic diisocyanate is not particularly limited and can be appropriately selected depending on the purpose. Examples of the aromatic diisocyanate include tolylene diisocyanate, diisocyanatodiphenylmethane, 1,5-naphthylene diisocyanate, 4,4'-diisocyanatodiphenyl, 4,4'-diisocyanato-3,3'-dimethyldiphenyl, 4,4'-diisocyanato-3-methyldiphenylmethane, and 4,4'-diisocyanato-diphenyl ether. The aromatic aliphatic diisocyanate is not particularly limited and may be appropriately selected depending on the purpose. For example, α,α,α',α'-tetramethylxylylene diisocyanate is exemplified. The isocyanurates are not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include tris(isocyanatoalkyl)isocyanurate, tris(isocyanatocycloalkyl)isocyanurate, etc. These may be used alone or in combination of two or more kinds.

[0129] When the polyisocyanate is reacted with a polyester resin having a hydroxyl group, the equivalent ratio (NCO / OH) of the isocyanate group of the polyisocyanate to the hydroxyl group of the polyester resin is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 1 to 5, more preferably 1.2 to 4, and particularly preferably 1.5 to 2.5. If the equivalent ratio is less than 1, the hot offset resistance may decrease, and if it exceeds 5, the low-temperature fixability may decrease.

[0130] The content of the polyisocyanate-derived structural unit in the polyester prepolymer having an isocyanate group is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 0.5% by mass to 40% by mass, more preferably 1% by mass to 30% by mass, and particularly preferably 2% by mass to 20% by mass. If the content is less than 0.5% by mass, the hot offset resistance may decrease, and if it exceeds 40% by mass, the low-temperature fixability may decrease.

[0131] The average number of isocyanate groups in the polyester prepolymer having isocyanate groups per molecule is not particularly limited and may be appropriately selected depending on the purpose, but is preferably at least 1, more preferably 1.5 to 3, and particularly preferably 1.8 to 2.5. If the average number is less than 1, the molecular weight of the modified polyester resin may be low, and the hot offset resistance may be reduced.

[0132] The modified polyester resin can be produced by a one-shot method, etc. As an example, a method for producing a urea-modified polyester resin will be described. First, a polyol and a polycarboxylic acid are heated to 150°C to 280°C in the presence of a catalyst such as tetrabutoxy titanate or dibutyltin oxide, and the water generated is removed while reducing the pressure as necessary to obtain a polyester resin having hydroxyl groups. Next, the polyester resin having hydroxyl groups is reacted with a polyisocyanate at 40°C to 140°C to obtain a polyester prepolymer having an isocyanate group. Furthermore, the polyester prepolymer having an isocyanate group is reacted with amines at 0°C to 140°C to obtain a urea-modified polyester resin.

[0133] The number average molecular weight (Mn) of the modified polyester resin is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 1,000 to 10,000, more preferably 1,500 to 6,000, as measured by GPC (gel permeation chromatography). The weight average molecular weight of the modified polyester resin is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 20,000 or more and 1,000,000 or less as measured by GPC (gel permeation chromatography). If the weight average molecular weight is 20,000 or more, the toner becomes easily fluid at low temperatures, which can prevent problems such as poor heat-resistant storage stability and low viscosity when melted, which can prevent problems such as reduced high-temperature offset properties.

[0134] When a polyester resin having a hydroxyl group is reacted with a polyisocyanate, and when a polyester prepolymer having an isocyanate group is reacted with an amine, a solvent can be used as necessary. The solvent is not particularly limited and can be appropriately selected depending on the purpose. Examples of the solvent include aromatic solvents, ketones, esters, amides, ethers, and other solvents that are inactive against isocyanate groups. Examples of the aromatic solvent include toluene and xylene. Examples of the ketones include acetone, methyl ethyl ketone, and methyl isobutyl ketone. Examples of the esters include ethyl acetate. Examples of the amides include dimethylformamide and dimethylacetamide. Examples of the ethers include tetrahydrofuran.

[0135] The glass transition temperature of the modified polyester resin is preferably from -60°C to 0°C, and more preferably from -40°C to -20°C. If the glass transition temperature is -60°C or higher, the flow of the toner at low temperatures cannot be suppressed, and the problems of deterioration of heat-resistant storage stability and deterioration of filming resistance can be prevented. When the glass transition temperature is 0° C. or lower, the toner cannot be sufficiently deformed by the application of heat and pressure during fixing, and the problem of insufficient low-temperature fixing property can be prevented.

[0136] The content of the modified polyester is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 1 to 15 parts by mass, and more preferably 5 to 10 parts by mass, per 100 parts by mass of the toner. The molecular structures of the polyester resin components A and C can be confirmed by NMR measurement of a solution or solid, as well as X-ray diffraction, GC / MS, LC / MS, IR measurement, and the like. In the infrared absorption spectrum, the -1 and 990±10cm -1 One method is to detect amorphous polyester resins that do not have absorption due to olefin δCH (out-of-plane bending vibration).

[0137] -Crystalline polyester- The crystalline polyester resin (hereinafter also referred to as "crystalline polyester" or "polyester resin component D") is not particularly limited and can be appropriately selected depending on the purpose. For example, there is a crystalline polyester resin obtained by reacting a polyol with a polycarboxylic acid.

[0138] The crystalline polyester resin has high crystallinity and therefore exhibits heat melting characteristics in which the viscosity drops sharply near the fixing start temperature. By using the crystalline polyester resin having such characteristics together with the amorphous polyester resin, the heat-resistant storage stability is good due to the crystallinity until just before the melting start temperature, and at the melting start temperature, the crystalline polyester resin melts and causes a sudden viscosity drop (sharp melt), which causes it to become compatible with the amorphous polyester resin, and both of them rapidly drop in viscosity to be fixed, resulting in a toner that has both good heat-resistant storage stability and low-temperature fixing ability. Also, good results are shown in terms of the release width (the difference between the minimum fixing temperature and the high-temperature offset-resistant temperature). In the present invention, the crystalline polyester resin refers to a resin obtained by reacting a polyol with a polycarboxylic acid as described above, and modified polyester resins, such as the prepolymer and resins obtained by subjecting the prepolymer to a crosslinking and / or elongation reaction, do not belong to the crystalline polyester resin.

[0139] --Polyol-- The polyol is not particularly limited and can be appropriately selected depending on the purpose. Examples of the polyol include diols and trihydric or higher polyols.

[0140] The diol includes, for example, saturated aliphatic diols. The saturated aliphatic diol may be a linear saturated aliphatic diol or a branched saturated aliphatic diol. These may be used alone or in combination of two or more. Among these, linear saturated aliphatic diols are preferred, and linear saturated aliphatic diols having a carbon number of 2 to 12 are more preferred, because they can improve crystallinity and prevent a decrease in melting point.

[0141] Examples of the saturated aliphatic diol include ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,13-tridecanediol, 1,14-tetradecanediol, 1,18-octadecanediol, and 1,14-eicosanediol. Among these, ethylene glycol, 1,4-butanediol, 1,6-hexanediol, 1,8-octanediol, 1,10-decanediol, and 1,12-dodecanediol are preferred because the crystalline polyester resin has high crystallinity and excellent sharp melting properties.

[0142] Examples of the trihydric or higher alcohol include glycerin, trimethylolethane, trimethylolpropane, and pentaerythritol.

[0143] --Polycarboxylic acids-- The polycarboxylic acid is not particularly limited and can be appropriately selected depending on the purpose. Examples of the polycarboxylic acid include divalent carboxylic acids and trivalent or higher carboxylic acids.

[0144] Examples of the divalent carboxylic acid include saturated aliphatic dicarboxylic acids such as oxalic acid, succinic acid, glutaric acid, adipic acid, suberic acid, azelaic acid, sebacic acid, 1,9-nonanedicarboxylic acid, 1,10-decanedicarboxylic acid, 1,12-dodecanedicarboxylic acid, 1,14-tetradecanedicarboxylic acid, and 1,18-octadecanedicarboxylic acid; and aromatic dicarboxylic acids such as dibasic acids such as phthalic acid, isophthalic acid, terephthalic acid, naphthalene-2,6-dicarboxylic acid, malonic acid, and mesaconic acid; and further, anhydrides of these acids and lower (carbon number: 1 to 3) alkyl esters of these acids.

[0145] Examples of the trivalent or higher carboxylic acid include 1,2,4-benzenetricarboxylic acid, 1,2,5-benzenetricarboxylic acid, 1,2,4-naphthalenetricarboxylic acid, and anhydrides and lower (carbon number 1 to 3) alkyl esters of these.

[0146] The polycarboxylic acid may contain a dicarboxylic acid having a sulfonic acid group in addition to the saturated aliphatic dicarboxylic acid or aromatic dicarboxylic acid. Furthermore, the polycarboxylic acid may contain a dicarboxylic acid having a double bond in addition to the saturated aliphatic dicarboxylic acid or aromatic dicarboxylic acid. These may be used alone or in combination of two or more.

[0147] The crystalline polyester resin is preferably composed of a linear saturated aliphatic dicarboxylic acid having 4 to 12 carbon atoms and a linear saturated aliphatic diol having 2 to 12 carbon atoms. That is, the crystalline polyester resin preferably has a structural unit derived from a saturated aliphatic dicarboxylic acid having 4 to 12 carbon atoms and a structural unit derived from a saturated aliphatic diol having 2 to 12 carbon atoms. This is preferable in that the resin has high crystallinity and excellent sharp melting properties, and can therefore exhibit excellent low-temperature fixability.

[0148] The presence or absence of crystallinity of the crystalline polyester resin in the present invention can be confirmed by a crystal analysis X-ray diffraction device (for example, X'Pert Pro MRD Philips). The measurement method is described below. First, the target sample is ground in a mortar to prepare a powdered sample, and the powdered sample is evenly applied to a sample holder.Then, the sample holder is set in the diffraction device, and measurements are performed to obtain a diffraction spectrum. If the half-width of the peak with the highest intensity among the obtained diffraction peaks in the range of 20°<2θ<25° is 2.0 or less, it is judged to have crystallinity. In contrast to crystalline polyester resins, polyester resins that do not exhibit the above-mentioned state are referred to as amorphous polyester resins in the present invention. The conditions for the X-ray diffraction measurements are as follows. [Measurement conditions] Tension kV: 45kV Current: 40mA MPSS Upper Gonio Scan mode: continuous Start angle: 3° End angle: 35° Angle Step: 0.02° Lucident beam optics Divergence slit: Div slit 1 / 2 Diffraction beam optics Anti scatter slit: As fixed 1 / 2 Receiving slit: Prog rec slit

[0149] The melting point of the crystalline polyester resin is not particularly limited and may be appropriately selected depending on the purpose, but is preferably from 60° C. to 80° C. If the melting point is 60° C. or higher, the crystalline polyester resin is easily melted at low temperatures, and the problem of the heat-resistant storage stability of the toner decreasing can be prevented, whereas if the melting point is 80° C. or lower, the problem of the crystalline polyester resin not melting sufficiently due to heating during fixing, and the problem of the low-temperature fixability decreasing can be prevented.

[0150] The molecular weight of the crystalline polyester resin is not particularly limited and can be appropriately selected depending on the purpose. The orthodichlorobenzene soluble portion of the crystalline polyester resin preferably has a weight average molecular weight (Mw) of 3,000 to 30,000, more preferably 5,000 to 15,000, as measured by GPC. The orthodichlorobenzene soluble portion of the crystalline polyester resin preferably has a number average molecular weight (Mn) of 1,000 to 10,000, more preferably 2,000 to 10,000, as measured by GPC. The molecular weight ratio Mw / Mn of the crystalline polyester resin is preferably from 1.0 to 10, and more preferably from 1.0 to 5.0. This is because a toner having a sharp molecular weight distribution and a low molecular weight has excellent low-temperature fixability, and the high heat-resistant storage stability is reduced when there are a lot of low-molecular weight components.

[0151] The acid value of the crystalline polyester resin is not particularly limited and can be appropriately selected depending on the purpose, but from the viewpoint of affinity between paper and resin, in order to achieve the desired low-temperature fixability, it is preferably 5 mgKOH / g or more, more preferably 10 mgKOH / g or more, while in order to improve high-temperature offset resistance, it is preferably 45 mgKOH / g or less.

[0152] The hydroxyl value of the crystalline polyester resin is not particularly limited and may be appropriately selected depending on the purpose. In order to achieve the desired low-temperature fixability and good charging characteristics, the hydroxyl value is preferably 0 mgKOH / g to 50 mgKOH / g, and more preferably 5 mgKOH / g to 50 mgKOH / g.

[0153] The molecular structure of the crystalline polyester resin can be confirmed by NMR measurement of a solution or solid, as well as X-ray diffraction, GC / MS, LC / MS, IR measurement, etc. -1 Or 990±10cm -1 One method is to detect a crystalline polyester resin that has absorption based on the δCH (out-of-plane bending vibration) of olefin.

[0154] The content of the crystalline polyester resin is not particularly limited and can be appropriately selected according to the purpose, but is preferably 4 parts by mass to 12 parts by mass, more preferably 5 parts by mass to 11 parts by mass, relative to 100 parts by mass of the toner. When the content is 4 parts by mass or more, the problem of poor low-temperature fixability due to insufficient sharp melting by the crystalline polyester resin can be prevented. Also, when the content is 12 parts by mass or less, the problem of poor cohesion and adhesion at high temperatures can be prevented.

[0155] <<Coloring agent>> The colorant is not particularly limited and can be appropriately selected depending on the purpose. Examples of the colorant include carbon black, nigrosine dye, iron black, naphthol yellow S, Hansa yellow (10G, 5G, G), cadmium yellow, yellow iron oxide, yellow ocher, yellow lead, titanium yellow, polyazo yellow, oil yellow, Hansa yellow (GR, A, RN, R), pigment yellow L, benzidine yellow (G, GR), permanent yellow (NCG), Balkan fast yellow (5G, R), tartrazine lake, quinoline yellow lake, and anthrazan yellow BG. L, Isoindolinone Yellow, Bengala, Red Lead, Cinnabar, Cadmium Red, Cadmium Mercury Red, Antimony Vermilion, Permanent Red 4R, Para Red, Phaysee Red, Parachlor Orthonitroaniline Red, Lithol Fast Scarlet G, Brilliant Fast Scarlet, Brilliant Kanmin BS, Permanent Red (F2R, F4R, FRL, FRLL, F4RH), Fast Scarlet VD, Belkan Fast Rubin B, Brilliant Scarlet G, Lithol Rubin GX, Permanent Red F5R, Brilliant Antcarmine 6B, Pigment Scarlet 3B, Bordeaux 5B, Toluidine Maroon, Permanent Bordeaux F2K, Helio Bordeaux BL, Bordeaux 10B, Bon Maroon Light, Bon Maroon Medium, Eosin Lake, Rhodamine Lake B, Rhodamine Lake Y, Alizarin Lake, Thioindigo Red B, Thioindigo Maroon, Oil Red, Quinacridone Red, Pyrazolone Red, Polyazo Red, Chrome Vermilion, Benzidine Orange, Perinone Orange, Oil Orange, Cobalt Blue, Cerulean Blue, Alkaline Blue - Lake, Peacock Blue Lake, Victoria Blue Lake, Metal-free Phthalocyanine Blue, Phthalocyanine Blue, Fast Sky Blue, Indanthrene Blue (RS, BC), Indigo, Ultramarine Blue, Prussian Blue, Anthraquinone Blue, Fast Violet B, Methyl Violet Lake, Cobalt Purple, Manganese Purple, Dioxane Violet, Anthraquinone Violet, Chrome Green, Zinc Green, Chromium Oxide, Pyridian, Emerald Green, Pigment Green B, Naphthol Green B, Green Gold, Acid Green Lake,Examples include malachite green lake, phthalocyanine green, anthraquinone green, titanium oxide, zinc oxide, and lithopone.

[0156] The content of the colorant is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 1 part by mass to 15 parts by mass, and more preferably 3 parts by mass to 10 parts by mass, relative to 100 parts by mass of the toner.

[0157] The colorant can also be used as a masterbatch composited with a resin. Examples of resins to be used in the preparation of the masterbatch or kneaded with the masterbatch include, in addition to the other polyester resins, styrene or its substituted polymers such as polystyrene, poly-p-chlorostyrene, and polyvinyltoluene; styrene-p-chlorostyrene copolymer, styrene-propylene copolymer, styrene-vinyltoluene copolymer, styrene-vinylnaphthalene copolymer, styrene-methyl acrylate copolymer, styrene-ethyl acrylate copolymer, styrene-butyl acrylate copolymer, styrene-octyl acrylate copolymer, styrene-methyl methacrylate copolymer, styrene-ethyl methacrylate copolymer, styrene-butyl methacrylate copolymer, and styrene-α-chloromethyl methacrylate copolymer. styrene-based copolymers such as styrene-acrylonitrile copolymers, styrene-vinyl methyl ketone copolymers, styrene-butadiene copolymers, styrene-isoprene copolymers, styrene-acrylonitrile-indene copolymers, styrene-maleic acid copolymers, and styrene-maleic acid ester copolymers; polymethyl methacrylate, polybutyl methacrylate, polyvinyl chloride, polyvinyl acetate, polyethylene, polypropylene, polyester, epoxy resins, epoxy polyol resins, polyurethanes, polyamides, polyvinyl butyral, polyacrylic acid resins, rosin, modified rosin, terpene resins, aliphatic or alicyclic hydrocarbon resins, aromatic petroleum resins, chlorinated paraffins, and paraffin waxes. These may be used alone or in combination of two or more.

[0158] The master batch can be obtained by mixing and kneading the resin for the master batch and the colorant under high shear force. In this case, an organic solvent can be used to enhance the interaction between the colorant and the resin. In addition, a method called the flushing method, in which an aqueous paste containing water of the colorant is mixed and kneaded with the resin and the organic solvent, the colorant is transferred to the resin side, and the water and organic solvent components are removed, is also preferably used because the wet cake of the colorant can be used as it is and does not need to be dried. A high shear dispersion device such as a three-roll mill is preferably used for mixing and kneading.

[0159] <<Wax>> The wax (releasing agent) is not particularly limited and can be appropriately selected from known waxes, for example, natural waxes, synthetic waxes, etc. These may be used alone or in combination of two or more kinds.

[0160] Examples of the natural waxes include vegetable waxes such as carnauba wax, cotton wax, and wood wax; animal waxes such as beeswax and lanolin; mineral waxes such as ozokerite and cerusin; and petroleum waxes such as paraffin, microcrystalline, and petrolatum. Examples of the synthetic wax include synthetic hydrocarbon waxes such as Fischer-Tropsch wax, polyethylene, and polypropylene; fatty acid amide compounds such as esters, ketones, ethers, 12-hydroxystearic acid amide, stearic acid amide, phthalic anhydride imide, and chlorinated hydrocarbons; low molecular weight crystalline polymer resins, such as polyacrylate homopolymers and copolymers (e.g., n-stearyl acrylate-ethyl methacrylate copolymers); and crystalline polymers having long alkyl groups in their side chains. Among these, hydrocarbon waxes such as paraffin wax, microcrystalline wax, Fischer-Tropsch wax, polyethylene wax, and polypropylene wax are preferred.

[0161] The melting point of the release agent is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 60° C. or more and 80° C. or less. When the melting point is 60° C. or more, the release agent is easily melted at low temperatures, and the problem of poor heat resistance storage stability can be prevented. When the melting point is 80° C. or less, even when the resin is melted and in the fixing temperature range, the release agent does not melt sufficiently, causing fixing offset and preventing defects in the image.

[0162] The content of the release agent is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 2 to 10 parts by mass, more preferably 3 to 8 parts by mass, relative to 100 parts by mass of the toner. When the content is 2 parts by mass or more, problems such as poor high-temperature offset resistance and poor low-temperature fixability during fixing can be prevented, and when the content is 10 parts by mass or less, problems such as reduced heat-resistant storage stability and image fogging can be prevented.

[0163] The toner base particles are not particularly limited as long as they are used in ordinary toner base particles, and may contain other components appropriately selected depending on the purpose. The content of the other components is not particularly limited as long as it does not impair the properties of the toner, and can be appropriately selected depending on the purpose.

[0164] <Other ingredients> The other components are not particularly limited as long as they are used in ordinary toners and can be appropriately selected depending on the purpose. Examples of the other components include a charge control agent, an external additive, a flowability improver, a cleaning property improver, and a magnetic material.

[0165] -Charge control agent- The charge control agent is not particularly limited and can be appropriately selected depending on the purpose. Examples of the charge control agent include nigrosine dyes, triphenylmethane dyes, chromium-containing metal complex dyes, molybdic acid chelate pigments, rhodamine dyes, alkoxy amines, quaternary ammonium salts (including fluorine-modified quaternary ammonium salts), alkylamides, phosphorus simple substance or compounds, tungsten simple substance or compounds, fluorine-based activators, metal salicylic acid salts, and metal salts of salicylic acid derivatives.

[0166] Examples of commercially available charge control agents include the nigrosine dye Bontron 03, the quaternary ammonium salt Bontron P-51, the metal-containing azo dye Bontron S-34, the oxynaphthoic acid metal complex E-82, the salicylic acid metal complex E-84, and the phenol condensate E-89 (all manufactured by Orient Chemical Industry Co., Ltd.), the quaternary ammonium salt molybdenum complexes TP-302 and TP-415 (all manufactured by Hodogaya Chemical Co., Ltd.), LRA-901, and the boron complex LR-147 (all manufactured by Nippon Carlit Co., Ltd.).

[0167] The content of the charge control agent is determined by the type of the binder resin, the presence or absence of additives used as necessary, and the toner production method including the dispersion method, and is not uniquely limited, but is preferably 0.1 to 10 parts by mass, more preferably 0.2 to 5 parts by mass, relative to 100 parts by mass of the binder resin. If the content exceeds 10 parts by mass, the chargeability of the toner is too high, the effect of the main charge control agent is reduced, and the electrostatic attraction force with the developing roller increases, which may lead to a decrease in the fluidity of the developer and a decrease in image density. These charge control agents can be melt-kneaded with the master batch and resin and then dissolved and dispersed, or of course, they can be added when directly dissolved or dispersed in an organic solvent, or they can be fixed on the toner surface after the toner particles are produced.

[0168] -Flow improver- The flow improver is not particularly limited as long as it is capable of performing a surface treatment to increase hydrophobicity and prevent deterioration of flow characteristics and charging characteristics even under high humidity conditions, and may be appropriately selected depending on the purpose. Examples of the flow improver include silane coupling agents, silylating agents, silane coupling agents having a fluorinated alkyl group, organic titanate coupling agents, aluminum coupling agents, silicone oils, and modified silicone oils. It is particularly preferable that the silica and titanium oxide are surface-treated with such a flowability improving agent and used as hydrophobic silica and hydrophobic titanium oxide.

[0169] -Cleaning improver- The cleaning property improver is not particularly limited as long as it is added to the toner in order to remove the developer remaining on the photoconductor or the primary transfer medium after transfer, and may be appropriately selected depending on the purpose. Examples of the cleaning property improver include fatty acid metal salts such as zinc stearate, calcium stearate, and stearic acid, polymer fine particles produced by soap-free emulsion polymerization, such as polymethyl methacrylate fine particles and polystyrene fine particles. The polymer fine particles preferably have a relatively narrow particle size distribution, and the volume average particle size is preferably 0.01 μm to 1 μm.

[0170] -Magnetic materials- The magnetic material is not particularly limited and may be appropriately selected depending on the purpose, and examples thereof include iron powder, magnetite, ferrite, etc. Among these, those that are white in color are preferred.

[0171] The glass transition temperature (Tg1st) of the toner at the first temperature rise in differential scanning calorimetry (DSC) is preferably 40°C to 65°C. The glass transition temperature (Tg1st) at the first temperature rise in DSC of the component of the toner that is insoluble in tetrahydrofuran (THF) is preferably from -45°C to 5°C. The glass transition temperature (Tg2nd) of the THF-soluble component of the toner at the second temperature rise in DSC is preferably 20°C to 65°C. It is preferable that the glass transition temperature (Tg1st) during the first temperature rise and the glass transition temperature (Tg2nd) during the second temperature rise in differential scanning calorimetry (DSC) of the toner satisfy Tg1st-Tg2nd≧10[°C], since this improves the low-temperature fixability and heat-resistant storage stability.

[0172] Here, the glass transition temperature of the toner can be measured, for example, by using a differential scanning calorimeter (DSC-60, manufactured by Shimadzu Corporation). For example, a DSC curve is measured using the above-mentioned differential scanning calorimeter. From the obtained DSC curves, a DSC curve at the first heating is selected using an analysis program, and the glass transition temperature Tg1st at the first heating is obtained using the endothermic shoulder temperature in the analysis program. A DSC curve at the second heating is selected, and the glass transition temperature Tg2nd at the second heating is obtained using the endothermic shoulder temperature.

[0173] The storage modulus G' of the toner at 70°C is 4.0 x 10 5 is less than or equal to 3.0 x 10 5 Storage modulus G' is preferably 4.0×10 or less. 5 If it exceeds this value, the low-temperature fixing property may deteriorate. The storage modulus G' of the toner at 70° C. indicates the storage modulus in the temperature range during fixing in the low-temperature fixing property that is required in recent years. The method for measuring the storage modulus G' of the toner at 70° C. is not particularly limited, and may be appropriately selected depending on the purpose.

[0174] The average circularity of the toner is preferably 0.965 to 0.985, and more preferably 0.978 to 0.985. When the average circularity is 0.965 or more, the toner has excellent cleaning properties in a low-temperature, low-humidity environment, but at high temperatures, the toner has a large uneven shape, so that the toner is not sufficiently coated with external additives, and the toner cannot be sufficiently cleaned. When the average circularity is 0.985 or less, the toner has high coating properties and excellent cleaning properties at high temperatures, but the toner cannot be scraped off by a cleaning blade at low temperatures and low humidity, so that the toner cannot be sufficiently cleaned. The method for measuring the average circularity of the toner is not particularly limited, and can be appropriately selected depending on the purpose.

[0175] (Developer) The developer of the present invention contains at least the toner of the present invention, and contains other components, such as a carrier, which are appropriately selected as necessary. The developer may be a one-component developer or a two-component developer, but when used in a high-speed printer or the like that corresponds to the recent improvement in information processing speed, a two-component developer is preferred because of its improved lifespan.

[0176] <Career> The carrier is not particularly limited and may be appropriately selected depending on the purpose, but it is preferable that the carrier has a core material and a resin layer that covers the core material.

[0177] -Core material- The material of the core material is not particularly limited and can be appropriately selected according to the purpose, and examples thereof include manganese-strontium-based materials of 50 to 90 emu / g and manganese-magnesium-based materials of 50 to 90 emu / g. In order to ensure image density, it is preferable to use high magnetization materials such as iron powder of 100 emu / g or more and magnetite of 75 to 120 emu / g. In addition, it is preferable to use low magnetization materials such as copper-zinc-based materials of 30 to 80 emu / g, since it can reduce the impact of the developer in a standing state on the photoconductor and is advantageous for improving image quality. These may be used alone or in combination of two or more.

[0178] The volume average particle diameter of the core material is not particularly limited and can be appropriately selected according to the purpose, but is preferably 10 to 150 μm, more preferably 40 to 100 μm. If the volume average particle diameter is less than 10 μm, the amount of fine powder in the carrier increases, the magnetization per particle decreases, and the carrier may scatter. On the other hand, if it exceeds 150 μm, the specific surface area decreases, the toner may scatter, and in full color with many solid parts, the reproduction of the solid parts may be particularly poor.

[0179] The toner of the present invention can be mixed with the above-mentioned carrier and used in a two-component developer. The content of the carrier in the two-component developer is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 90 to 98 parts by mass, and more preferably 93 to 97 parts by mass, relative to 100 parts by mass of the two-component developer. The developer of the present invention can be suitably used for image formation by various known electrophotographic methods such as a magnetic one-component development method, a non-magnetic one-component development method, and a two-component development method.

[0180] (Toner manufacturing method) The toner production method of the present invention is a method for producing the above-mentioned toner. The toner manufacturing method includes a composite particle forming step and a removing step, and may further include other steps as necessary.

[0181] <Composite particle formation process> The composite particle forming step is a step of forming composite particles by adhering resin fine particles to the surfaces of toner base particles. The composite particles can be formed, for example, by a known dissolution suspension method in which an oil phase containing components of the toner base particles, such as the binder resin, colorant, and wax, is dispersed in an aqueous medium containing resin fine particles to form granules.

[0182] As an example of the dissolution suspension method, a method of forming composite particles while generating a polyester resin by an elongation reaction and / or a crosslinking reaction between the prepolymer and the curing agent will be described. In this method, an aqueous medium is prepared, an oil phase containing a toner base particle material is prepared, the toner base particle material is emulsified or dispersed, and the organic solvent is removed.

[0183] - Preparation of aqueous medium (aqueous phase) - The aqueous medium can be prepared, for example, by dispersing resin fine particles in the aqueous medium. The amount of the resin fine particles added to the aqueous medium is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 0.5 to 10 parts by mass relative to 100 parts by mass of the aqueous medium. The aqueous medium is not particularly limited and can be appropriately selected according to the purpose, and examples thereof include water, a solvent miscible with water, and a mixture thereof. These may be used alone or in combination of two or more. Among these, water is preferred.

[0184] The water-miscible solvent is not particularly limited and may be appropriately selected depending on the purpose, and examples thereof include alcohol, dimethylformamide, tetrahydrofuran, cellosolves, lower ketones, etc. Examples of the alcohol include methanol, isopropanol, ethylene glycol, etc. Examples of the lower ketones include acetone, methyl ethyl ketone, etc.

[0185] - Preparation of oil phase - The oil phase can be prepared by dissolving or dispersing the toner base particle material, which contains a binder resin, a colorant, and a wax, and further contains a hardener, etc., as required, in an organic solvent.

[0186] The organic solvent is not particularly limited and can be appropriately selected depending on the purpose, but an organic solvent having a boiling point of less than 150° C. is preferred in terms of ease of removal.

[0187] Examples of the organic solvent having a boiling point of less than 150° C. include toluene, xylene, benzene, carbon tetrachloride, methylene chloride, 1,2-dichloroethane, 1,1,2-trichloroethane, trichloroethylene, chloroform, monochlorobenzene, dichloroethylidene, methyl acetate, ethyl acetate, methyl ethyl ketone, and methyl isobutyl ketone. These may be used alone or in combination of two or more. Among these, ethyl acetate, toluene, xylene, benzene, methylene chloride, 1,2-dichloroethane, chloroform, carbon tetrachloride, etc. are preferable, and ethyl acetate is more preferable.

[0188] -Emulsification or dispersion- The toner materials can be emulsified or dispersed by dispersing an oil phase containing the toner materials in the aqueous medium, and when the toner materials are emulsified or dispersed, the curing agent and the prepolymer can undergo an elongation reaction and / or a crosslinking reaction.

[0189] The reaction conditions (reaction time, reaction temperature) for producing the prepolymer are not particularly limited and can be appropriately selected depending on the combination of the curing agent and the prepolymer. The reaction time is preferably 10 minutes to 40 hours, more preferably 2 to 24 hours. The reaction temperature is preferably 0°C to 150°C, more preferably 40°C to 98°C.

[0190] The method for stably forming a dispersion liquid containing the prepolymer in the aqueous medium is not particularly limited and can be appropriately selected depending on the purpose. For example, there is a method in which an oil phase prepared by dissolving or dispersing a toner material in a solvent is added to an aqueous medium phase, and the mixture is dispersed by shear force.

[0191] The dispersing machine for the dispersion is not particularly limited and can be appropriately selected according to the purpose. For example, low-speed shear dispersing machine, high-speed shear dispersing machine, friction dispersing machine, high-pressure jet dispersing machine, ultrasonic dispersing machine, etc. can be mentioned. Among these, high-speed shear dispersing machine is preferable because it can control the particle size of the dispersion (oil droplets) to 2 to 20 μm.

[0192] When using the high-speed shear type disperser, the conditions such as the rotation speed, dispersion time, and dispersion temperature can be appropriately selected depending on the purpose. The rotation speed is preferably 1,000 rpm to 30,000 rpm, and more preferably 5,000 rpm to 20,000 rpm. In the case of a batch method, the dispersion time is preferably 0.1 minutes to 5 minutes. The dispersion temperature is preferably 0°C to 150°C under pressure, and more preferably 40°C to 98°C. Generally, the higher the dispersion temperature, the easier the dispersion.

[0193] The amount of the aqueous medium used when emulsifying or dispersing the toner materials is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 50 parts by mass to 2,000 parts by mass, more preferably 100 parts by mass to 1,000 parts by mass, relative to 100 parts by mass of the toner materials. If the amount of the aqueous medium used is less than 50 parts by mass, the dispersion state of the toner materials may become poor and toner base particles of the specified particle size may not be obtained, and if it exceeds 2,000 parts by mass, the production cost may become high.

[0194] When the oil phase containing the toner materials is emulsified or dispersed, it is preferable to use a dispersant from the viewpoints of stabilizing the dispersion such as oil droplets, forming a desired shape, and sharpening the particle size distribution. The dispersant is not particularly limited and can be appropriately selected according to the purpose, and examples thereof include surfactants, poorly water-soluble inorganic compound dispersants, polymer-based protective colloids, etc. These may be used alone or in combination of two or more. Among these, surfactants are preferred.

[0195] The surfactant is not particularly limited and can be appropriately selected depending on the purpose, and for example, anionic surfactants, cationic surfactants, nonionic surfactants, amphoteric surfactants, etc. can be used. Examples of the anionic surfactant include alkylbenzene sulfonates, α-olefin sulfonates, and phosphate esters. Among these, those having a fluoroalkyl group are preferred.

[0196] -Removal of organic solvents- The method for removing the organic solvent from the dispersion liquid such as the emulsified slurry is not particularly limited and can be appropriately selected depending on the purpose. Examples of the method include a method in which the temperature of the entire reaction system is gradually increased to evaporate the organic solvent in the oil droplets, and a method in which the dispersion liquid is sprayed in a dry atmosphere to remove the organic solvent in the oil droplets. Once the organic solvent is removed, composite particles are formed.

[0197] <Removal process> The removing step is a step of removing at least a part of the resin fine particles from the composite particles, and it is preferable to remove a part or the whole of the shell resin (resin (b1)) in the resin fine particles. An example of the step of removing at least a portion of the resin fine particles is a washing step of washing the composite particles. For this reason, the removing step can also be called a washing step.

[0198] In the washing step, the method for removing a part or all of the resin (b1) includes a method for removing a part or all of (b1) by a chemical method. The chemical method may, for example, be a step of washing the composite particles with a basic aqueous solution, which can dissolve a part or all of the shell resin (b1). By carrying out the washing step, a toner that satisfies the above-mentioned (Formula 3) can be obtained.

[0199] The basic aqueous solution is not particularly limited as long as it is basic and can be appropriately selected depending on the purpose, and examples thereof include aqueous solutions of hydroxides of alkali metals such as potassium hydroxide and sodium hydroxide, ammonia, etc. These may be used alone or in combination of two or more. Among these, potassium hydroxide and sodium hydroxide are preferred from the viewpoint of easiness in dissolving the shell resin (b1). The pH of the basic aqueous solution is preferably 8 to 14, and more preferably 10 to 12.

[0200] In the washing step, the composite particles and the alkaline aqueous solution can be mixed by, for example, dropping the basic aqueous solution into the composite slurry under stirring. After the basic aqueous solution has been added dropwise, an acidic aqueous solution may be added dropwise to neutralize the mixture.

[0201] <Other processes> The other steps are not particularly limited and can be appropriately selected depending on the purpose. Examples of the other steps include a drying step and a classification step. The drying step is not particularly limited as long as it can remove the solvent from the composite particles, and can be appropriately selected depending on the purpose. The classification step may be carried out by removing fine particles in a liquid using a cyclone, decanter, centrifugal separation, or the like, or the classification operation may be carried out after drying.

[0202] The obtained composite particles may be mixed with particles of the external additive, the charge control agent, etc. In this case, by applying a mechanical impact force, it is possible to suppress the particles of the external additive, etc. from being detached from the surface of the toner base particle. The method of applying the mechanical impact force is not particularly limited and can be appropriately selected depending on the purpose. Examples of the method include a method of applying an impact force to the mixture using a blade rotating at high speed, a method of introducing the mixture into a high-speed air stream and accelerating it to collide the particles with each other or with a suitable collision plate, etc.

[0203] The apparatus used in the above method is not particularly limited and can be appropriately selected depending on the purpose. Examples include Angmill (manufactured by Hosokawa Micron Corporation), an apparatus obtained by modifying I-type mill (manufactured by Japan Pneumatic Co., Ltd.) to reduce the grinding air pressure, Hybridization System (manufactured by Nara Machinery Works), Cryptron System (manufactured by Kawasaki Heavy Industries, Ltd.), and automatic mortar.

[0204] (Toner storage unit) The toner storage unit in the present invention refers to a unit having a function of storing toner and storing the toner. Examples of the toner storage unit include a toner storage container, a developing unit, and a process cartridge. The toner storage container refers to a container that stores the toner of the present invention. The developing device has a means for storing toner and developing the toner. The process cartridge is a cartridge which integrates at least an image carrier and a developing means, contains toner, and is detachably mountable to an image forming apparatus. The process cartridge may further include at least one selected from a charging means, an exposure means, and a cleaning means.

[0205] Next, one embodiment of the process cartridge is shown in Fig. 2. As shown in Fig. 2, the process cartridge of this embodiment has a built-in latent image carrier 101, a charging device 102, a developing device 104, and a cleaning unit 107, and further has other means as necessary. In Fig. 2, reference numeral 103 denotes exposure from an exposure device, and reference numeral 105 denotes recording paper. The latent image carrier 101 may be the same as an electrostatic latent image carrier in an image forming apparatus described later. The charging device 102 may be any charging member. In the image forming process using the process cartridge shown in FIG. 2, while the latent image carrier 101 rotates in the direction of the arrow, an electrostatic latent image corresponding to the exposed image is formed on its surface by charging the latent image carrier 101 with a charging device 102 and exposing the latent image carrier 101 to light with light 103 by an exposure means (not shown). This electrostatic latent image is developed with toner by a developing device 104, and the toner development is transferred to a recording paper 105 by a transfer roller 108 and printed out. Next, the surface of the latent image carrier after the image transfer is cleaned by a cleaning unit 107, and further discharged by a discharge means (not shown), and the above operations are repeated again.

[0206] (Image forming apparatus and image forming method) The image forming apparatus of the present invention has the above-mentioned toner containing unit, and at least has an electrostatic latent image carrier, an electrostatic latent image forming means, and a developing means, and preferably further has other means as necessary. The image forming method according to the present invention includes at least an electrostatic latent image forming step and a development step, and further includes other steps as necessary.

[0207] <Electrostatic latent image carrier> The material, structure, and size of the electrostatic latent image bearing member are not particularly limited and may be appropriately selected from known materials, and examples of the material include inorganic photoconductors such as amorphous silicon and selenium, and organic photoconductors such as polysilane and phthalopolymethine, etc. Among these, amorphous silicon is preferred in terms of long life. The linear speed of the electrostatic latent image bearing member is preferably 300 mm / s or more.

[0208] <Electrostatic latent image forming means and electrostatic latent image forming process> The electrostatic latent image forming means is not particularly limited as long as it is a means for forming an electrostatic latent image on the electrostatic latent image carrier, and may be appropriately selected depending on the purpose. For example, there may be mentioned a means having at least a charging member that charges the surface of the electrostatic latent image carrier, and an exposure member that exposes the surface of the electrostatic latent image carrier to light in an imagewise manner.

[0209] The electrostatic latent image forming step is not particularly limited as long as it is a step of forming an electrostatic latent image on the electrostatic latent image bearing member, and can be appropriately selected depending on the purpose. For example, the electrostatic latent image forming step can be performed by charging the surface of the electrostatic latent image bearing member and then exposing it to light in an imagewise manner, using the electrostatic latent image forming means.

[0210] <<Charging materials and charging>> The charging member is not particularly limited and can be appropriately selected depending on the purpose. Examples of the charging member include a contact charger known per se having a conductive or semiconductive roller, brush, film, rubber blade, or the like, and a non-contact charger utilizing corona discharge such as a corotron or scorotron.

[0211] The charging can be carried out, for example, by applying a voltage to the surface of the electrostatic latent image bearing member using the charging member. The shape of the charging member may be any shape, such as a roller, a magnetic brush, a fur brush, etc., and can be selected according to the specifications and shape of the image forming apparatus.

[0212] The charging member is not limited to the contact-type charging member, but it is preferable to use a contact-type charging member because an image forming apparatus in which the amount of ozone generated from the charging member is reduced can be obtained.

[0213] <<Exposure materials and exposure>> The exposing member is not particularly limited and may be appropriately selected depending on the purpose as long as it can expose the surface of the electrostatic latent image carrier charged by the charging member in the form of an image to be formed, and examples of the exposing member include various exposing members such as a copying optical system, a rod lens array system, a laser optical system, and a liquid crystal shutter optical system.

[0214] The light source used in the exposure member is not particularly limited and can be appropriately selected depending on the purpose. For example, fluorescent lamps, tungsten lamps, halogen lamps, mercury lamps, sodium lamps, light-emitting diodes (LEDs), semiconductor lasers (LDs), electroluminescence (EL), and other light-emitting materials in general can be mentioned.

[0215] In order to irradiate only light in a desired wavelength range, various filters such as a sharp cut filter, a band pass filter, a near infrared cut filter, a dichroic filter, an interference filter, and a color temperature conversion filter can be used.

[0216] The exposure can be carried out, for example, by exposing the surface of the electrostatic latent image bearing member imagewise using the exposure member. In the present invention, a light back system may be adopted in which exposure is performed imagewise from the back side of the electrostatic latent image bearing member.

[0217] <Developing means and developing process> The developing unit is not particularly limited as long as it is a developing unit that develops the electrostatic latent image formed on the electrostatic latent image carrier to form a toner image, which is a visible image, and is equipped with a toner, and can be appropriately selected depending on the purpose. The developing step is not particularly limited as long as it is a step of developing the electrostatic latent image formed on the electrostatic latent image carrier with a toner to form a toner image, which is a visible image, and can be appropriately selected depending on the purpose. For example, the developing step can be performed by the developing means. The developing means is preferably a developing device having an agitator that frictionally stirs the toner to charge it, a magnetic field generating means fixed inside, and a developer carrier that can rotate and carries a developer containing the toner on its surface.

[0218] <Other means and other steps> Examples of the other means include a transfer means, a fixing means, a cleaning means, a discharging means, a recycling means, and a control means. Examples of the other steps include a transfer step, a fixing step, a cleaning step, a discharging step, a recycling step, and a control step.

[0219] <<Transfer means and transfer process>> The transfer means is not particularly limited as long as it is a means for transferring a visible image onto a recording medium, and can be appropriately selected depending on the purpose. However, a preferred embodiment has a primary transfer means for transferring the visible image onto an intermediate transfer body to form a composite transfer image, and a secondary transfer means for transferring the composite transfer image onto a recording medium. The transfer step is not particularly limited as long as it is a step of transferring a visible image onto a recording medium, and may be appropriately selected depending on the purpose. However, a preferred embodiment is one in which an intermediate transfer body is used, a visible image is primarily transferred onto the intermediate transfer body, and then the visible image is secondarily transferred onto the recording medium. The transfer step can be carried out, for example, by charging the visible image on the photoconductor using a transfer charger, and can be carried out by the transfer unit.

[0220] Here, when the image to be secondarily transferred onto the recording medium is a color image made up of toners of multiple colors, the transfer means can be configured to sequentially overlay toners of each color on the intermediate transfer body to form an image on the intermediate transfer body, and the intermediate transfer means can be configured to secondarily transfer the image on the intermediate transfer body onto the recording medium all at once. The intermediate transfer body is not particularly limited and can be appropriately selected from known transfer bodies depending on the purpose. For example, a transfer belt is preferably used.

[0221] The transfer means (the primary transfer means and the secondary transfer means) preferably has at least a transfer device that peels and charges the visible image formed on the photoreceptor onto the recording medium. Examples of the transfer device include a corona transfer device that uses corona discharge, a transfer belt, a transfer roller, a pressure transfer roller, and an adhesive transfer device. The recording medium is typically plain paper, but is not particularly limited as long as it is capable of transferring an unfixed image after development, and can be appropriately selected according to the purpose. A PET base for overhead projectors can also be used.

[0222] <<Fixing means and fixing process>> The fixing means is not particularly limited as long as it is a means for fixing the transferred image transferred to the recording medium, and can be appropriately selected according to the purpose. For example, a known heating and pressing member is preferable. Examples of the heating and pressing member include a combination of a heating roller and a pressing roller, and a combination of a heating roller, a pressing roller, and an endless belt. The fixing step is not particularly limited as long as it is a step of fixing the visible image transferred to the recording medium, and can be appropriately selected according to the purpose. For example, the fixing step may be performed for each color toner transferred to the recording medium, or may be performed simultaneously for each color toner in a laminated state.

[0223] The fixing step can be carried out by the fixing means. The heating temperature in the heating and pressing member is preferably 80°C to 200°C. In the present invention, depending on the purpose, for example, a known optical fixing device may be used together with or instead of the fixing means. The surface pressure in the fixing step is not particularly limited and can be appropriately selected depending on the purpose. 2 ~80N / cm 2 It is preferable that:

[0224] <<Cleaning means and cleaning process>> The cleaning means is not particularly limited as long as it can remove the toner remaining on the photoreceptor, and can be appropriately selected depending on the purpose, for example, a magnetic brush cleaner, an electrostatic brush cleaner, a magnetic roller cleaner, a blade cleaner, a brush cleaner, a web cleaner, etc. The cleaning step is not particularly limited as long as it can remove the toner remaining on the photoconductor, and can be appropriately selected depending on the purpose. For example, the cleaning step can be performed by the cleaning unit.

[0225] <<Static charge removal means and static charge removal process>> The charge removing means is not particularly limited as long as it is a means for removing electricity by applying a charge removing bias to the photoconductor, and may be appropriately selected depending on the purpose. For example, a charge removing lamp may be used. The charge removing step is not particularly limited as long as it is a step of removing electricity by applying a charge removing bias to the photoconductor, and may be appropriately selected depending on the purpose. For example, the charge removing step may be performed by the charge removing unit.

[0226] <<Recycling methods and processes>> The recycling means is not particularly limited as long as it is a means for recycling the toner removed in the cleaning step to the developing device, and can be appropriately selected depending on the purpose. For example, a known transport means can be used. The recycling process is not particularly limited as long as it is a process for recycling the toner removed by the cleaning process back into the developing device, and can be appropriately selected depending on the purpose. For example, the recycling process can be performed by the recycling means.

[0227] Next, one embodiment of a method for forming an image by the image forming apparatus of the present invention will be described with reference to Fig. 3. Although a printer is shown as an example of the image forming apparatus of this embodiment, the image forming apparatus is not particularly limited as long as it is capable of forming an image using toner, such as a copier, facsimile, or multifunction machine. The image forming apparatus includes a paper feed section 210, a conveying section 220, an image creating section 230, a transfer section 240, and a fixing unit 250. The paper feed section 210 includes a paper feed cassette 211 in which the paper P to be fed is stacked, and a paper feed roller 212 that feeds the paper P stacked in the paper feed cassette 211 one sheet at a time.

[0228] The conveying section 220 includes a roller 221 that conveys the paper P fed by the paper feed roller 212 toward the transfer section 240, a pair of timing rollers 222 that hold the leading end of the paper P conveyed by the roller 221 and wait to send the paper to the transfer section 240 at a predetermined timing, and a paper discharge roller 223 that discharges the paper P with the color toner image fixed thereto onto a paper discharge tray 224.

[0229] The image creating section 230 includes, spaced at a predetermined interval from left to right in the figure, an image forming unit Y that forms an image using a developer containing yellow toner, an image forming unit C that uses a developer containing cyan toner, an image forming unit M that uses a developer containing magenta toner, an image forming unit K that uses a developer containing black toner, and an exposure device 233. Incidentally, when referring to any one of the image forming units (Y, C, M, K), it is referred to as an image forming unit.

[0230] The developer contains toner and carrier. The four image forming units (Y, C, M, K) have substantially the same mechanical configuration, except for the developer used in each unit.

[0231] The transfer unit 240 includes a drive roller 241 and a driven roller 242, an intermediate transfer belt 243 that can rotate counterclockwise in the figure as the drive roller 241 is driven, primary transfer rollers (244Y, 244C, 244M, 244K) arranged opposite the photosensitive drum 231 across the intermediate transfer belt 243, and secondary opposing roller 245 and secondary transfer roller 246 arranged opposite each other across the intermediate transfer belt 243 at the transfer position of the toner image to paper.

[0232] The fixing unit 250 has a heater installed inside and is equipped with a pressure roller 252 that forms a nip by rotatably pressing a fixing belt 251, which heats the paper P, against the fixing belt 251. This applies heat and pressure to the color toner image on the paper P, fixing the color toner image. The paper P with the fixed color toner image is discharged to a paper discharge tray 224 by a paper discharge roller 223, completing a series of image formation processes. EXAMPLES

[0233] Examples of the present invention will be described below, but the present invention is not limited to these examples. In the following, unless otherwise specified, "parts" means parts by mass, and "%" means % by mass.

[0234] Example 1 <Synthesis of amorphous polyester resin A-1> In a four-neck flask equipped with a nitrogen inlet tube, a dehydration tube, a stirrer, and a thermocouple, bisphenol A ethylene oxide side 2 mole adduct, bisphenol A propylene oxide 3 mole adduct, terephthalic acid, adipic acid, and trimethylolpropane were added. The molar ratio of bisphenol A ethylene oxide side 2 mole adduct and bisphenol A propylene oxide 3 mole adduct was 85 / 15 (bisphenol A ethylene oxide side 2 mole adduct / bisphenol A propylene oxide 3 mole adduct), and the molar ratio of terephthalic acid and adipic acid was 1.0:1. The monomers were charged so that the molar ratio (terephthalic acid / adipic acid) was 75 / 25, the amount of trimethylolpropane in the total monomers was 1 mol%, and the molar ratio of hydroxyl groups to carboxyl groups, OH / COOH, was 1.2, and reacted with titanium tetraisopropoxide (500 ppm relative to the resin components) at normal pressure and 230°C for 8 hours, and then reacted for a further 4 hours at a reduced pressure of 10 mmHg to 15 mmHg. After that, trimellitic anhydride was added to the reaction vessel so that the amount was 1 mol% relative to the total resin components, and reacted at 180°C and normal pressure for 3 hours to obtain [Amorphous Polyester Resin A-1]. The tg2nd of the amorphous polyester resin A-1 was 55°C.

[0235] <Synthesis of dispersion of resin fine particles (B1) (resin fine particle dispersion B1)> In a reaction vessel equipped with a stirrer, a heating and cooling device, and a thermometer, 3,710 parts of water and 200 parts of polyoxyethylene-1-(allyloxymethyl) alkyl ether sulfate ammonium (Aqualon KH-1025, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) were charged and homogenized by stirring at 200 rpm. The homogenized mixture was heated to raise the temperature inside the system to 75°C, after which 90 parts of 10% ammonium persulfate aqueous solution was added, and then a mixture of 450 parts of styrene, 250 parts of butyl acrylate, and 300 parts of methacrylic acid was added dropwise over 4 hours. After the dropwise addition, the mixture was aged at 75°C for 4 hours to obtain a fine particle dispersion (W0-1) containing a shell resin (b1-1), which is a polymer in which the monomer and polyoxyethylene-1-(allyloxymethyl) alkyl ether sulfate ammonium were copolymerized. A reaction vessel equipped with a stirrer, a heating / cooling device, and a thermometer was charged with 667 parts of the microparticle dispersion (W0-1) and 248 parts of water, and 0.267 parts of tertiary butyl hydroperoxide (Perbutyl H, NOF Corp.) was added, and the temperature in the system was raised to 70° C. by heating, and then 43.3 parts of styrene, 23.3 parts of butyl acrylate, and 18.0 parts of a 1% by mass aqueous ascorbic acid solution were dropped over 2 hours. After the dropping, the mixture was aged at 70° C. for 4 hours to obtain a microparticle dispersion of resin microparticles (B1) containing resin (b2-1) and resin (b1-1), which are polymers in which the monomers are copolymerized using the microparticles in (W0-1) as seeds, as constituents in the same particle. The volume average particle size of the resin fine particles (B1) was 17.2 nm when measured by dynamic light scattering (light scattering electrophoresis apparatus: ELS-8000, manufactured by Otsuka Electronics Co., Ltd.).

[0236] It was confirmed by the following method using a transmission electron microscope that the fine particle dispersion contained resin fine particles (B1) containing resin (b1-1) and resin (b2-1) as constituent components in the same particle. Specifically, 2 parts of gelatin (Cook Gelatin, Morinaga Milk Industry Co., Ltd.) was dissolved in 15 parts of water heated to 95°C to 100°C, and the gelatin solution was cooled to 40°C by air cooling. The solution was then mixed with the microparticle dispersion (B1) in a 1:1 ratio, thoroughly stirred, and then cooled to 10°C for 1 hour to produce a hardened gel. This gel was sliced ​​into 80 nm-thick sections using an ultramicrotome (Ultramicrotome UC7, FC7, Leica Microsystems) while maintaining the temperature at -80°C. The sections were then stained with a 2% aqueous solution of ruthenium tetroxide for 5 minutes and then observed with a transmission electron microscope (Hitachi Technologies, H-7100) to confirm the sections.

[0237] <Synthesis of dispersion of resin fine particles (B2) (resin fine particle dispersion B2)> In a reaction vessel equipped with a stirring rod and a thermometer, 683 parts of water, 11 parts of sodium salt of methacrylic acid ethylene oxide adduct sulfate (Eleminol RS-30, manufactured by Sanyo Chemical Industries, Ltd.), 138 parts of styrene, 138 parts of methacrylic acid, and 1 part of ammonium persulfate were charged and stirred at 400 rpm for 15 minutes, resulting in a white emulsion. The resulting emulsion was heated to an internal temperature of 75°C and reacted for 5 hours. Furthermore, 30 parts of a 1% aqueous ammonium persulfate solution was added, and the mixture was aged at 75°C for 5 hours to obtain an aqueous dispersion of resin fine particles (B2) which is a vinyl resin (a copolymer of styrene-methacrylic acid-sodium salt of methacrylic acid ethylene oxide adduct sulfate) [resin fine particle dispersion B2].

[0238] <Synthesis of Prepolymer C-1 (Modified Polyester Resin C-1)> Into a reaction vessel equipped with a cooling tube, a stirrer, and a nitrogen inlet tube, 3-methyl-1,5-pentanediol, isophthalic acid, adipic acid, and trimellitic anhydride were added together with titanium tetraisopropoxide (1,000 ppm relative to the resin component) so that the molar ratio of hydroxyl groups to carboxyl groups, OH / COOH, was 1.5, the diol component was 100 mol% 3-methyl-1,5-pentanediol, the dicarboxylic acid component was 40 mol% isophthalic acid and 60 mol% adipic acid, and the amount of trimellitic anhydride in all monomers was 1 mol%. Thereafter, the temperature was raised to 200°C over about 4 hours, and then to 230°C over 2 hours, and the reaction was continued until no water was discharged. Thereafter, the mixture was further reacted for 5 hours under a reduced pressure of 10 mmHg to 15 mmHg to obtain [intermediate polyester C-1]. Next, into a reaction vessel equipped with a cooling tube, a stirrer, and a nitrogen inlet tube, [Intermediate polyester A-1] and isophorone diisocyanate (IPDI) were added in a molar ratio (isocyanate group of IPDI / hydroxyl group of intermediate polyester) of 2.0, and after diluting with ethyl acetate to make a 50% ethyl acetate solution, the mixture was reacted at 100°C for 5 hours to obtain [Prepolymer C-1].

[0239] In addition, from [prepolymer C-1], [polyester resin component C-1] corresponding to polyester resin component A of the present invention is generated during the process of producing the toner in the examples and comparative examples described below. The tg2nd of the prepolymer C-1 was -40°C.

[0240] <Synthesis of crystalline polyester resin D-1> Dodecanedioic acid and 1,6-hexanediol were charged into a 5 L four-neck flask equipped with a nitrogen inlet tube, a dehydration tube, a stirrer, and a thermocouple so that the molar ratio of hydroxyl groups to carboxyl groups, OH / COOH, was 0.9, and reacted with titanium tetraisopropoxide (500 ppm relative to the resin component) at 180°C for 10 hours, then heated to 200°C and reacted for 3 hours, and further reacted at a pressure of 8.3 kPa for 2 hours to obtain [Crystalline Polyester Resin D-1]. The melting point (mp) of the crystalline polyester resin was 70 °C.

[0241] <Preparation of Crystalline Polyester Resin Dispersion> Into a container equipped with a stirrer and a thermometer, 50 parts of [Crystalline Polyester Resin D-1] and 450 parts of ethyl acetate were charged. The temperature was raised to 80 °C with stirring, and after holding at 80 °C for 5 hours, it was cooled to 30 °C in 1 hour. Using a bead mill (Ultraviscomill, manufactured by Imex Co., Ltd.), dispersion was carried out under the conditions of a liquid feeding rate of 1 kg / hr, a disk peripheral speed of 6 m / sec, 80% by volume filling of zirconia beads with a diameter of 0.5 mm, and 3 passes to obtain [Crystalline Polyester Resin Dispersion 1].

[0242] <Preparation of Masterbatch (MB)> 1,200 parts of water, 500 parts of carbon black (Printex 35, manufactured by Degussa Co., Ltd.) [DBP oil absorption = 42 mL / 100 mg, pH = 9.5], and 500 parts of [Amorphous Polyester Resin A-1] were added and mixed with a Henschel mixer (manufactured by Mitsui Mining Co., Ltd.). The mixture was kneaded at 150 °C for 30 minutes using two rolls, then rolled and cooled and pulverized with a pelletizer to obtain [Masterbatch 1].

[0243] <Preparation of WAX Dispersion> Into a container equipped with a stirrer and a thermometer, 50 parts of paraffin wax as a mold release agent 1 (manufactured by Nippon Seiro Co., Ltd., HNP-9, hydrocarbon wax, melting point 75 °C, SP value 8.8) and 450 parts of ethyl acetate were charged. The temperature was raised to 80 °C with stirring, and after holding at 80 °C for 5 hours, it was cooled to 30 °C in 1 hour. Using a bead mill (Ultraviscomill, manufactured by Imex Co., Ltd.), dispersion was carried out under the conditions of a liquid feeding rate of 1 kg / hr, a disk peripheral speed of 6 m / sec, 80% by volume filling of zirconia beads with a diameter of 0.5 mm, and 3 passes to obtain [WAX Dispersion 1].

[0244] <Synthesis of Ketimine Compound> In a reaction vessel equipped with a stirring bar and a thermometer, 170 parts of isophoronediamine and 75 parts of methyl ethyl ketone were charged and reacted at 50° C. for 5 hours to obtain [Ketimine Compound 1]. The amine value of [Ketimine Compound 1] was 418.

[0245] <Preparation of oil phase> 500 parts of [WAX Dispersion 1], 956 parts of [Crystalline Polyester Dispersion 1], 76 parts of [Prepolymer C-1], 152 parts of [Prepolymer C-1], 836 parts of [Amorphous Polyester Resin A-1], 100 parts of [Masterbatch 1], and 2 parts of [Ketimine Compound 1] as a curing agent were placed in a container and mixed at 5,000 rpm for 60 minutes with a TK Homomixer (manufactured by Primix Corporation) to obtain [Oil Phase 1].

[0246] <Preparation of aqueous phase> 990 parts of water, 83 parts of [Resin fine particle dispersion B1], 37 parts of a 48.5% aqueous solution of sodium dodecyl diphenyl ether disulfonate (Eleminol MON-7: manufactured by Sanyo Chemical Industries, Ltd.), and 90 parts of ethyl acetate were mixed and stirred to obtain a milky white liquid. This was designated as [Aqueous phase 1].

[0247] <Emulsification / solvent removal> 1,200 parts of [water phase 1] was added to the container containing [oil phase 1], and mixed with a TK homomixer at 13,000 rpm for 20 minutes to obtain [emulsified slurry 1]. Next, [emulsified slurry 1] was placed in a container equipped with a stirrer and thermometer, and the solvent was removed at 30°C for 8 hours, and then aged at 45°C for 4 hours to obtain [dispersed slurry 1].

[0248] <Washing and drying> 100 parts of [Dispersion Slurry 1] was filtered under reduced pressure, and the following operations were then carried out. (1) 100 parts of ion-exchanged water was added to the filter cake, mixed with a TK homomixer (at 12,000 rpm for 10 minutes), and then filtered. (2): 100 parts of a 10% aqueous sodium hydroxide solution was added to the filter cake of (1), mixed with a TK homomixer (at 12,000 rpm for 30 minutes), and then filtered under reduced pressure. (3): 100 parts of 10% hydrochloric acid was added to the filter cake of (2), and the mixture was mixed with a TK homomixer (at 12,000 rpm for 10 minutes) and then filtered. (4) 300 parts of ion-exchanged water was added to the filter cake of (3), mixed with a TK homomixer (at 12,000 rpm for 10 minutes), and then filtered. The above operations (1) to (4) were repeated twice to obtain a filter cake. The filtered cake was dried in a circulating air dryer at 45° C. for 48 hours, and sieved through a 75 μm mesh to obtain toner base particles 1.

[0249] <External Addition Treatment> 100 parts of [toner base particles 1] were mixed with 2.2 parts of hydrophobic silica 1 having an average particle size of 160 nm, 1.0 part of titanium oxide having an average particle size of 20 nm, and 0.8 parts of hydrophobic silica fine powder having an average particle size of 15 nm in a Henschel mixer to obtain [toner 1].

[0250] Example 2 [Toner base particles 2] were obtained in the same manner as in Example 1, except that in the preparation of the oil phase in Example 1, the amount of [Crystalline polyester dispersion 1] added was changed to 224 parts. [Toner 2] was produced using this [Toner base particles 2].

[0251] Example 3 In the preparation of the oil phase in Example 1, except that the amount of [Crystalline Polyester Dispersion 1] added was changed to 1,791 parts, [Toner Base Particles 3] was obtained in the same manner as in Example 1. [Toner 3] was produced using this [Toner Base Particles 2].

[0252] Example 4 Toner 4 was prepared in the same manner as in Example 1, except that in the external addition treatment of Example 1, hydrophobic silica 1 was replaced with hydrophobic silica 2 having an average primary particle size of 70 nm.

[0253] Example 5 Toner 5 was prepared in the same manner as in Example 1, except that in the external addition treatment of Example 1, hydrophobic silica 1 was replaced with hydrophobic silica 3 having an average primary particle size of 220 nm.

[0254] Example 6 Toner 6 was prepared in the same manner as in Example 1, except that in the external addition treatment of Example 1, hydrophobic silica 1 was replaced with hydrophobic silica 4 having an average primary particle size of 50 nm.

[0255] Example 7 Toner 7 was prepared in the same manner as in Example 1, except that in the external addition treatment of Example 1, hydrophobic silica 1 was replaced with hydrophobic silica 5 having an average primary particle size of 240 nm.

[0256] Example 8 Toner 8 was prepared in the same manner as in Example 1, except that in the emulsification and desolvation step of Example 1, the stirring time with the TK homomixer was changed to 30 minutes.

[0257] Example 9 Toner 9 was prepared in the same manner as in Example 1, except that in the emulsification and desolvation step of Example 1, the stirring time with the TK homomixer was changed to 10 minutes.

[0258] Example 10 [Toner 10] was prepared in the same manner as in Example 1, except that in the preparation of the oil phase in Example 1, the amount of [Crystalline Polyester Dispersion 1] added was changed to 1,500 parts, in the emulsification / desolvation process, the stirring time in the TK Homomixer was changed to 30 minutes, and in the external addition treatment, Hydrophobic Silica 1 was replaced with Hydrophobic Silica 2 having an average primary particle size of 70 nm.

[0259] Example 11 [Toner 11] was prepared in the same manner as in Example 1, except that in the preparation of the oil phase in Example 1, the amount of [Crystalline Polyester Dispersion 1] added was changed to 458 parts, the stirring time in the TK Homomixer in the emulsification / desolvation step was changed to 10 minutes, and in the external addition treatment, Hydrophobic Silica 1 was replaced with Hydrophobic Silica 3 having an average primary particle size of 220 nm.

[0260] Comparative Example 1 [Toner 12] was prepared in the same manner as in Example 1, except that in the preparation of the oil phase in Example 1, [Crystalline Polyester Dispersion 1] was not added.

[0261] Comparative Example 2 [Toner 13] was prepared in the same manner as in Example 1, except that [Resin particle dispersion B1] in Example 1 was replaced with [Resin particle dispersion B2].

[0262] Comparative Example 3 Toner 14 was prepared in the same manner as in Example 1, except that sodium hydroxide was not added in the washing and drying step (2) of Example 1.

[0263] Comparative Example 4 [Toner 15] was prepared in the same manner as in Example 1, except that in the preparation of the oil phase in Example 1, the amount of [Crystalline Polyester Dispersion 1] added was changed to 1,791 parts, the stirring time in the TK Homomixer in the emulsification / desolvation step was changed to 30 minutes, and in the external addition treatment, Hydrophobic Silica 1 was changed to Hydrophobic Silica 4 having an average primary particle size of 50 nm.

[0264] <Measurement of embedding depth of external additives> 10 g of the obtained toner and 20 g of a carrier described below were placed in a 50 mL glass bottle and stirred at 67 Hz for 60 minutes using a rocking mill (product name: RM05S, manufactured by Seiwa Giken Co., Ltd.). After the stirring, the toner was embedded and fixed in epoxy resin, and then the toner was cut using a FIB-SEM (SU-8230, Hitachi High-Technologies Corporation) and the cross-section SEM image was observed. The acceleration voltage was 30 kV and the current value was 100-500 pA. From the obtained toner cross-section SEM image, the embedding degree of the external additive was quantified using image analysis software as follows. The measurement results are shown in Table 1. (1) Observed using SEM in topographical image mode. The value obtained from the observed data is designated as A. (2) Observed using SEM in compositional image mode. The value obtained from the observed data is designated as B. (3) In the shape image mode, the contrast of the external additive is strong, so binarization is performed based on this contrast. (4) The shape of the toner base particles was captured using a SEM in composition image mode. (5) The volume (a) of the external additive present on the surface of the toner base particle and the volume (b) of the external additive buried in the surface of the toner base particle can be calculated by combining A and B. From this value, (b / a) x 100 was calculated to measure the buried degree (%) of the external additive.

[0265] <Number average primary particle size of external additives> The silica particles were observed using a transmission electron microscope (magnification 100,000 times), and the average value was calculated from measurements of 20 or more appropriately selected silica particles. The average value was taken as the average primary particle size of the external additive. The calculation results are shown in Table 1.

[0266] <Measurement of storage modulus G' at 70℃> The storage modulus was measured using the following device and under the following conditions. The measurement results are shown in Table 1. Equipment: ARES-24A (Rheometrics) Fixture: 25mm parallel plate Frequency: 1Hz Distortion rate: 10% Heating rate: 5℃ / min

[0267] <Measurement of average circularity> The average circularity was measured using a flow particle image analyzer (FPIA-3000, manufactured by SYSMEX Co., Ltd.) as follows. The measurement results are shown in Table 1. A 1% NaCl aqueous solution was prepared using primary sodium chloride and passed through a 0.45 μm filter. 0.1 mL to 5 mL of alkylbenzene sulfonate was added as a dispersant to 50 mL to 100 mL of this aqueous solution, and 1 mg to 10 mg of the resulting toner was added. This was dispersed for 1 minute using an ultrasonic disperser, and the particle concentration was adjusted to 5,000 to 15,000 particles / μL. The diameter of a circle having the same area as the two-dimensional image area captured by the CCD camera was taken as the equivalent circle diameter, and a circle equivalent diameter of 0.6 μm or more was considered valid based on the accuracy of the CCD pixels and used to calculate the average circularity. The average circularity was obtained by calculating the circularity of each particle, adding up the circularity of each particle, and dividing by the total number of particles.

[0268] [Table 1]

[0269] <Measurement of toner Tg1st, toner Tg2nd, Tg1st of THF insoluble matter, and Tg of polyester resin components A-1, C-1 and D-1> 1 g of toner was put into 100 mL of THF, and Soxhlet extraction was performed to obtain a THF soluble fraction and an insoluble fraction. This was dried in a vacuum dryer for 24 hours, and polyester resin component C-1 (a mixture with crystalline polyester resin D-1 in Examples 9 to 11) was obtained from the THF soluble fraction, and a mixture of polyester resin component A-1 and polyester resin component B-1 was obtained from the THF insoluble fraction. These were used as the target samples. In addition, the toner was used as the target sample when measuring the toner Tg1st and toner Tg2nd.

[0270] Next, about 5.0 mg of the target sample was placed in an aluminum sample container, the sample container was placed on a holder unit, and set in an electric furnace. Next, under a nitrogen atmosphere, the sample was heated from -80°C to 150°C at a heating rate of 1.0°C / min (first heating). After that, the sample was cooled from 150°C to -80°C at a heating rate of 1.0°C / min, and further heated to 150°C at a heating rate of 1.0°C / min (second heating). In each of the first and second heating, a DSC curve was measured using a differential scanning calorimeter ("Q-200", manufactured by TA Instruments). From the obtained DSC curves, the DSC curve at the first heating was selected using the analysis program in the Q-200 system, and the glass transition temperature Tg1st at the first heating of the target sample was calculated. Similarly, the DSC curve at the second heating was selected, and the glass transition temperature Tg2nd at the second heating of the target sample was calculated.

[0271] From the obtained DSC curves, the DSC curve at the first heating was selected using the analysis program in the Q-200 system, and the glass transition temperature Tg1st at the first heating of the target sample was obtained. Similarly, the DSC curve at the second heating was selected, and the glass transition temperature Tg2nd at the second heating of the target sample was obtained.

[0272] From the obtained DSC curves, the analysis program in the Q-200 system was used to select the DSC curve during the first heating, and the endothermic peak top temperature during the first heating of the target sample was determined as the melting point. Similarly, the DSC curve during the second heating was selected, and the endothermic peak top temperature during the second heating of the target sample was determined as the melting point.

[0273] Unless otherwise specified, the melting points and glass transition temperatures Tg of the polyester resin components A-1, C-1, and D-1 and other constituent components were determined as the endothermic peak top temperature and glass transition temperature Tg2nd during the second heating, respectively, of each target sample.

[0274] For the toner components insoluble in THF, the toner was heated from -80°C to 150°C at a temperature rise rate of 1.0°C / min while applying a modulation temperature amplitude of ±1.0°C / min using the modulation mode (first temperature rise). The obtained DSC curve was obtained by plotting "Reversing Heat Flow" on the vertical axis using the analysis program in the Q-200 system as described above, and the onset value was taken as Tg. This allowed the Tg1st to be calculated. The results of measuring the toner Tg1st, toner Tg2nd, and Tg1st of the THF insoluble matter are shown in Table 2.

[0275] <Mass Ratio of Polyester Resin Components A-1, C-1, and D-1> The mass ratio of polyester resin component A-1 and crystalline polyester resin D-1 was calculated from the THF soluble matter obtained by the above Soxhlet extraction, and the composition ratio of polyester resin component A-1 and crystalline polyester resin D-1 was calculated. In addition, the mass ratio of polyester resin component C-1 was calculated from the THF insoluble matter obtained by the above Soxhlet extraction, and the composition ratio of polyester resin component C-1 was calculated. The measurement results are shown in Table 2.

[0276] [Table 2]

[0277] <Preparation of carrier> 100 parts of silicone resin (organo straight silicone), 5 parts of γ-(2-aminoethyl)aminopropyltrimethoxysilane, and 10 parts of carbon black were added to 100 parts of toluene, and dispersed for 20 minutes with a homomixer to prepare a resin layer coating solution. The resin layer coating solution was applied to the surface of 1,000 parts of spherical magnetite with an average particle size of 50 μm using a fluidized bed type coating device to prepare a [carrier].

[0278] <Preparation of developer> 5 parts of each of the toners obtained and 95 parts of the carrier were mixed in a ball mill to prepare a developer. The obtained developers were evaluated as follows. The evaluation results are shown in Table 3.

[0279] <Cleaning ability> Each of the obtained developers was set in a color multifunction printer (imagio MP C4500, manufactured by Ricoh Co., Ltd.), and 50,000 sheets (A4 size landscape) of a chart with an image area ratio of 5% was output in a laboratory environment of 21° C. and 65% RH, with 3 prints / job. Thereafter, in a laboratory environment of 32°C and 54% RH, 100 sheets of A4 size landscape charts with a vertical stripe pattern (relative to the paper travel direction) of 43 mm width were printed as evaluation images, and the resulting images and photoreceptor were visually observed, and the cleaning properties were evaluated based on the following evaluation criteria. Note that if the evaluation result was △ or better, there was no problem in practical use. -Evaluation criteria- ◎: The toner that has slipped through due to poor cleaning cannot be visually confirmed on the printed paper or on the photoconductor, and no streaks of toner can be confirmed even when observing the photoconductor longitudinally with a microscope. ○: No toner that has slipped through due to poor cleaning is visible on the printed paper or on the photoconductor. △: Toner that has slipped through due to poor cleaning can be visually confirmed slightly on the photoconductor, but cannot be confirmed on the printed paper. ×: Toner that has slipped through due to poor cleaning can be visually confirmed on the printed paper and on the photoconductor.

[0280] <Low temperature fixability> Each of the obtained developers was loaded into a color multifunction printer (imagio MP C4500, manufactured by Ricoh Co., Ltd.) and a rectangular solid image of 2 cm × 15 cm was printed in monochrome mode on PPC paper type 6000<70W>A4 T (manufactured by Ricoh Co., Ltd.) with a toner adhesion amount of 0.40 mg / cm 2 At this time, the surface temperature of the fixing roller was changed, and it was observed whether offset occurred, in which the development residual image of the solid image was fixed in a place other than the desired place, and the fixing temperature at which cold offset occurred was measured, and the low-temperature fixability was evaluated based on the following evaluation criteria. The solid image was created on the transfer paper at a position 3.0 cm from the leading edge in the paper feed direction, and the speed passing through the nip portion of the fixing device was 300 mm / s.

[0281] -Evaluation criteria for low temperature fixability- ◎: Minimum fixing temperature is 130℃ or less ○: The minimum fixing temperature is greater than 130°C and less than or equal to 135°C. △: The minimum fixing temperature is greater than 135°C and less than 140°C ×: The minimum fixing temperature is higher than 140° C.

[0282] <Overall rating> ⊚: The evaluation result of low temperature fixability is "good" or "good", and the evaluation result of cleaning ability is "good". ◯: There is one or more "△" in the evaluation results of low temperature fixability or cleaning ability. ×: One or more "×" marks were given in the evaluation results of low-temperature fixability or cleaning property.

[0283] [Table 3]

[0284] For example, aspects of the present invention are as follows. <1> A toner in which resin fine particles and an external additive are attached to the surface of a toner base particle containing at least a binder resin, a colorant, and a wax, The storage modulus G' of the toner at 70° C. is 4.0×10 5 is as follows: The toner is characterized in that the embedding degree of the external additive after the toner is subjected to the treatment under the following conditions is 15% to 40%. (conditions) 10 g of the toner and 20 g of the carrier are placed in a 50 mL bottle, and then stirred at 67 Hz for 60 minutes using a rocking mill. <2> The resin fine particles have a core resin (b2) and a shell resin (b1) that covers at least a part of the surface of the core resin. <1> The toner is as described above. <3> The shell resin contains a styrene-(meth)acrylic acid ester copolymer. <2> The toner is as described above. <4> The degree of embedment of the external additive in the surface of the toner base particle is 18% to 30%. <1> from <3> The toner according to any one of claims 1 to 5, <5> The external additive has an average primary particle diameter of 70 nm to 220 nm. <1> from <4> The toner according to any one of claims 1 to 5, <6> The toner has an average circularity of 0.978 to 0.985. <1> from <5> The toner according to any one of claims 1 to 5, <7> the toner has a glass transition temperature (Tg1st) in a first temperature rise measured by differential scanning calorimetry (DSC) of 40° C. to 65° C.; The toner has a tetrahydrofuran (THF)-insoluble component, and the glass transition temperature (Tg1st) at the first temperature rise in DSC is −45° C. to 5° C.; The toner has a THF-soluble component having a glass transition temperature (Tg2nd) of 20° C. to 65° C. in the second heating step of DSC. <1> from <6> The toner according to any one of claims 1 to 5, <8> The glass transition temperature (Tg1st) during the first temperature rise and the glass transition temperature (Tg2nd) during the second temperature rise in differential scanning calorimetry (DSC) of the toner are The above-mentioned, wherein Tg1st-Tg2nd≧10[° C.] <1> from <7> The toner according to any one of claims 1 to 5, <9> The binder resin contains an amorphous polyester. <1> from <8> The toner according to any one of claims 1 to 5, <10> The binder resin contains a modified polyester. <1> from <9> The toner according to any one of claims 1 to 5, <11> The modified polyester is a polyester having a trivalent or tetravalent aliphatic polyhydric alcohol having 3 to 10 carbon atoms as a constituent. <10> The toner is as described above. <12> The modified polyester has a diol as a constituent component, The diol has an odd carbon number of 3 to 9 in the main chain and has an alkyl group in the side chain. <10> from <11> The toner according to any one of claims 1 to 5, <13> The modified polyester has at least one of a urethane bond and a urea bond. <10> from <12> The toner according to any one of claims 1 to 5, <14> The binder resin contains a crystalline polyester. <1> from <13> The toner according to any one of claims 1 to 5, <15> The above <1> from <14> and a carrier. <16> The above <1> from <14> 13. A toner storage unit comprising the toner according to claim 12. <17> The above <16> 2 is a diagram showing a toner storage unit according to an embodiment of the present invention; <18> The above <1> from <14> An image forming method using the toner according to any one of an electrostatic latent image forming step of forming an electrostatic latent image on an electrostatic latent image carrier; a developing step of developing the electrostatic latent image formed on the electrostatic latent image carrier with the toner to form a toner image; a transfer step of transferring the toner image formed on the electrostatic latent image carrier onto a medium; and a fixing step of fixing the toner image transferred onto the medium. <19> The above <1> from <14> A method for producing the toner according to any one of the preceding claims, comprising the steps of: a composite particle forming step of forming composite particles by adhering resin fine particles to the surfaces of toner base particles; and removing at least a part of the resin fine particles from the composite particles. <20> The removing step is a step of washing with a basic aqueous solution. <19> The present invention relates to a method for producing a toner according to the present invention.

[0285] The above <1> from <14> The toner according to any one of the preceding claims. <15> The developer according to <16> The toner storage unit according to <17> The image forming apparatus according to the <18> The image forming method according to claim 1, <19> from <20> According to the toner production method described above, the conventional problems can be solved and the object of the present invention can be achieved. [Explanation of symbols]

[0286] 10 Photoconductor drum 40 Developer 58 Corona charger 80 Transfer roller 90 Cleaning Equipment 110 Process cartridge 210 Paper feed section 211 Paper feed cassette 212 Paper feed roller 220 Conveyor 221 Lola 222 Timing roller 223 Paper ejection roller 224 Paper output tray 230 Image creation section 233 Exposure device 240 Transcription Unit 241 Drive roller 242 Driven roller 243 Intermediate transfer belt 244 Primary transfer roller 245 Secondary opposing roller 246 Secondary transfer roller 250 Fixing unit 251 Fixing belt 252 Pressure roller [Prior art documents] [Patent documents]

[0287] [Patent Document 1] JP 2015-087597 A [Patent Document 2] JP 2013-105153 A

Claims

1. A toner in which resin fine particles and an external additive are attached to the surface of a toner base particle containing at least a binder resin, a colorant, and a wax, the resin fine particles have a core resin and a shell resin that coats at least a part of the surface of the core resin, The storage modulus G' of the toner at 70° C. is 4.0×10 5 is as follows: The toner is characterized in that the embedding degree of the external additive in the toner after the treatment under the following conditions is 15% to 40%. (conditions) 10 g of the toner and 20 g of the carrier are placed in a 50 mL bottle, and then stirred at 67 Hz for 60 minutes using a rocking mill.

2. 2. The toner according to claim 1, wherein the degree of embedment of the external additive in the surface of the toner base particle is 18% to 30%.

3. 3. The toner according to claim 1, wherein the average primary particle size of the external additive is from 70 nm to 220 nm.

4. 4. The toner according to claim 1, wherein the toner has an average circularity of 0.978 to 0.

985.

5. 5. The toner according to claim 1, further comprising a crystalline polyester resin in an amount of 4 parts by mass to 12 parts by mass based on 100 parts by mass of the toner.

6. 6. An image forming apparatus comprising a toner storage unit that stores the toner according to claim 1.

7. An image forming method using the toner according to any one of claims 1 to 4, an electrostatic latent image forming step of forming an electrostatic latent image on an electrostatic latent image carrier; a developing step of developing the electrostatic latent image formed on the electrostatic latent image carrier with a toner to form a toner image; a transfer step of transferring the toner image formed on the electrostatic latent image carrier onto a medium; a fixing step of fixing the toner image transferred onto the medium.

8. A method for producing the toner according to any one of claims 1 to 4, comprising the steps of: a composite particle forming step of forming composite particles by adhering resin fine particles to the surfaces of toner base particles; a removing step of removing at least a part of the resin fine particles from the composite particles.

9. The method for producing a toner according to claim 8, wherein the removing step is a step of washing with a basic aqueous solution.

Citation Information

Patent Citations

  • Toner for dry electrostatic charge image development, and image forming apparatus

    JP2013101264A

  • Toner for electrostatic charge image development and method for manufacturing toner

    JP2013105153A

  • Toner, developer, and image forming device

    JP2014063117A

  • Full-color image forming apparatus

    JP2014194528A

  • Toner for electrostatic latent image development, image forming apparatus, and process cartridge

    JP2014197090A