Toner for developing electrostatic images, electrostatic image developer, toner cartridge, process cartridge, image forming apparatus, and image forming method
A toner with amorphous and crystalline resins and controlled element intensities and domain configurations addresses the challenge of forming high-quality halftone images on uneven surfaces with low-temperature fixability and improved gradation.
Patent Information
- Application Number
- JP2020159126
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-09-23
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2040-09-23
AI Technical Summary
Existing toners struggle to form high-quality halftone images on recording media with uneven surfaces while maintaining low-temperature fixability, leading to deterioration in gradation and transfer efficiency.
The toner contains a binder resin composed of amorphous and crystalline resins, with controlled Mg and Cl element intensities and specific crystalline resin domain configurations, enhancing charge retention and uniform heat distribution for improved fixability and gradation on uneven surfaces.
The toner achieves low-temperature fixability and suppresses gradation deterioration on uneven surfaces by retaining charge and ensuring uniform melting, thereby improving image quality and transfer efficiency.
Smart Images

Figure 0007593022000005 
Figure 0007593022000006 
Figure 0007593022000007
Abstract
Description
[Technical field]
[0001] The present invention relates to a toner for developing an electrostatic image, an electrostatic image developer, a toner cartridge, a process cartridge, an image forming apparatus, and an image forming method. [Background technology]
[0002] Patent Document 1 proposes "a toner for developing electrostatic latent images, comprising toner particles containing at least a binder resin and a release agent, the toner particles having a core-shell structure in which the surfaces of core particles are coated with a shell layer, the binder resins containing an amorphous polyester resin and a crystalline resin, the amorphous polyester resin being contained as a main component of the resin contained in the toner particles, the crystalline resin being present in the toner particles as domains of thread-like crystal structures, and the average major axis of the thread-like crystal structures in the cross section of the toner particles being within a range of 300 to 2000 nm." [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2017-90828 A Summary of the Invention [Problem to be solved by the invention]
[0004] An object of the present invention is to provide a toner for developing electrostatic images, which comprises toner particles containing a binder resin, the binder resin containing an amorphous resin and a crystalline resin, and which has low-temperature fixability for a recording medium having an uneven surface and suppresses deterioration in gradation when a halftone image is formed on a recording medium having an uneven surface, compared to a case in which the net intensity of Mg element in the toner particles is less than 0.02 or exceeds 0.15, or the net intensity of Cl element in the toner particles is less than 0.02 or exceeds 0.60, as measured by fluorescent X-ray analysis. [Means for solving the problem]
[0005] The above problems are solved by the following means: <1> The toner particles include a binder resin. The binder resin contains an amorphous resin and a crystalline resin, The toner for developing electrostatic images, wherein the toner particles have a net intensity of Mg element of 0.02 or more and 0.15 or less, as measured by fluorescent X-ray analysis, and a net intensity of Cl element of 0.02 or more and 0.60 or less, as measured by fluorescent X-ray analysis. <2> The net intensity of the Mg element is 0.03 or more and 0.12 or less, and the net intensity of the Cl element is 0.03 or more and 0.40 or less. <1> 2. The toner for developing electrostatic images according to claim 1 . <3> The crystalline resin contains a polymer of an α,ω-linear aliphatic dicarboxylic acid and an α,ω-linear aliphatic diol. <1> or <2> 2. The toner for developing electrostatic images according to claim 1 . <4> The polymer of the α,ω-linear aliphatic dicarboxylic acid and the α,ω-linear aliphatic diol includes a polymer of 1,10-decanedicarboxylic acid and 1,6-hexanediol. <3> 2. The toner for developing electrostatic images according to claim 1 . <5> The toner particles (hereinafter also referred to as first toner particles) have at least two domains of the crystalline resin that satisfy the following conditions (A), (B1), (C), and (D) when a cross section of the toner particles is observed: <1> ~ <4> 10. The toner for developing an electrostatic image according to claim 9, Condition (A): The aspect ratio of the domain of the crystalline resin is 5 or more and 40 or less. Condition (B1): The length of the major axis of the domain of the crystalline resin is 0.5 μm or more and 1.5 μm or less. Condition (C): The angle between an extension line of the long axis of the domain of the crystalline resin and a tangent line at the contact point where the extension line contacts the surface of the toner particle is 60 degrees or more and 90 degrees or less. Condition (D): The crossing angle between the extension lines of the long axes of the two domains of the crystalline resin is 45 degrees or more and 90 degrees or less. <6> The toner particles (hereinafter also referred to as second toner particles) have at least two domains of the crystalline resin that satisfy the following conditions (A), (B2), (C), and (D) when a cross section of the toner particles is observed: <1> ~ <4> 10. The toner for developing an electrostatic image according to claim 9, Condition (A): The aspect ratio of the domain of the crystalline resin is 5 or more and 40 or less. Condition (B2): In at least one of the two domains of the crystalline resin, the ratio of the major axis length to the maximum diameter of the toner particle is 10% or more and 30% or less. Condition (C): The angle between an extension line of the long axis of the domain of the crystalline resin and a tangent line at the contact point where the extension line contacts the surface of the toner particle is 60 degrees or more and 90 degrees or less. Condition (D): The crossing angle between the extension lines of the long axes of the two domains of the crystalline resin is 45 degrees or more and 90 degrees or less. <7> the toner particles contain a release agent, The release agent is an ester wax. <1> ~ <6> 10. The toner for developing an electrostatic image according to claim 9, <8> the toner particles contain a release agent, and when a cross section of the toner particles is observed, a domain of the release agent is present at a depth of 50 nm or more from the surface of the toner particles; <7> 2. The toner for developing electrostatic images according to claim 1 . <9> The content of the toner particles is 40% by number or more of the total toner particles. <5> ~ <8> 10. The toner for developing an electrostatic image according to claim 9, <10> The content of the toner particles is 70% by number or more of the total toner particles. <9> 2. The toner for developing electrostatic images according to claim 1 . <11> The above <1> ~ <10> 2. An electrostatic image developer comprising the toner for developing electrostatic images according to claim 1. <12> The above <1> ~ <10> 13. A toner cartridge which contains the toner for developing electrostatic images according to any one of claims 1 to 12 and is detachably mountable to an image forming apparatus. <13> The above <11> and a developing means for developing an electrostatic image formed on a surface of an image carrier by using the electrostatic image developer into a toner image. <14> An image carrier; a charging means for charging the surface of the image carrier; an electrostatic image forming means for forming an electrostatic image on the charged surface of the image carrier; The above <11> a developing means for developing the electrostatic image formed on the surface of the image carrier into a toner image by using the electrostatic image developer; a transfer means for transferring the toner image formed on the surface of the image carrier to a surface of a recording medium; a fixing means for fixing the toner image transferred onto the surface of the recording medium; An image forming apparatus comprising: <15> a charging step of charging the surface of the image carrier; an electrostatic image forming step of forming an electrostatic image on the charged surface of the image carrier; The above <11> a developing step of developing the electrostatic image formed on the surface of the image carrier into a toner image by using the electrostatic image developer according to claim 1; a transfer step of transferring the toner image formed on the surface of the image carrier onto a surface of a recording medium; a fixing step of fixing the toner image transferred onto the surface of the recording medium; The image forming method according to claim 1, Effect of the Invention
[0006] <1> According to the invention related to the above, there is provided a toner for developing electrostatic images, which includes toner particles containing a binder resin, and the binder resin contains an amorphous resin and a crystalline resin, and which has low-temperature fixability for a recording medium having an uneven surface and suppresses deterioration in gradation when a halftone image is formed on a recording medium having an uneven surface, compared to a case in which the net intensity of Mg element in the toner particles is less than 0.02 or exceeds 0.15, or the net intensity of Cl element in the toner particles is less than 0.02 or exceeds 0.60, as measured by X-ray fluorescence analysis.
[0007] <2> According to the invention, there is provided a toner for developing electrostatic images which has low-temperature fixing ability for a recording medium having an uneven surface and suppresses deterioration in gradation when a halftone image is formed on a recording medium having an uneven surface, compared to a case in which the net intensity of the Mg element is less than 0.03 or exceeds 0.12, or the net intensity of the Cl element is less than 0.03 or exceeds 0.40.
[0008] <3> According to the invention, there is provided a toner for developing electrostatic images which has low-temperature fixability to a recording medium having an uneven surface and suppresses deterioration in gradation when a halftone image is formed on a recording medium having an uneven surface, compared to a case in which the crystalline resin is a polymer of an aromatic dicarboxylic acid other than a polymer of an α,ω-linear aliphatic dicarboxylic acid and an α,ω-linear aliphatic diol, and a diol having a double bond.
[0009] <4> According to the invention, there is provided a toner for developing electrostatic images which has low-temperature fixing properties for a recording medium having an uneven surface and suppresses deterioration in gradation when a halftone image is formed on a recording medium having an uneven surface, compared to when the crystalline resin is a polymer of 1,8-octanedicarboxylic acid and 1,7-heptanediol out of polymers of α,ω-linear aliphatic dicarboxylic acid and α,ω-linear aliphatic diol.
[0010] <5> According to the invention, there is provided a toner for developing electrostatic images, which has toner particles containing an amorphous resin and a crystalline resin, and which, when a cross section of the toner particle is observed, suppresses a decrease in uneven gloss of an image that occurs when an image with a large toner loading is formed, compared to a case in which at least two crystalline resin domains have only toner particles that do not satisfy the above condition (A), the above condition (B1), the above condition (C), and the above condition (D).
[0011] <6> According to the invention, there is provided a toner for developing electrostatic images, which has toner particles containing an amorphous resin and a crystalline resin, and which, when a cross section of the toner particle is observed, suppresses a decrease in uneven gloss of an image that occurs when an image with a large toner loading is formed, compared to a case in which at least two crystalline resin domains have only toner particles that do not satisfy the above condition (A), the above condition (B2), the above condition (C), and the above condition (D).
[0012] <7> According to the present invention, when the toner particles contain a release agent, there is provided a toner for developing electrostatic images which, compared to a case in which the release agent is paraffin wax, has low-temperature fixability for a recording medium having an uneven surface, while suppressing a decrease in gradation when a halftone image is formed on a recording medium having an uneven surface.
[0013] <8> According to the present invention, there is provided a toner for developing electrostatic images which suppresses the decrease in uneven gloss of an image that occurs when an image with a large toner loading is formed, compared to when the domain of the release agent is present at a depth of less than 50 nm from the surface of the toner particle.
[0014] <9> or <10> According to the present invention, there is provided a toner for developing electrostatic images which suppresses the decrease in uneven gloss of an image that occurs when an image with a large toner loading is formed, compared to when the content of the first toner particles and the second toner particles is less than 40% by number or less than 70% by number.
[0015] <11> ~ <15> According to the invention, there are provided an electrostatic image developing toner which includes toner particles containing a binder resin, the binder resin containing an amorphous resin and a crystalline resin, and which, compared to a case where an electrostatic image developing toner in which the toner particles have a net intensity of Mg element less than 0.02 or more than 0.15, or a net intensity of Cl element measured by fluorescent X-ray analysis less than 0.02 or more than 0.60, as measured by fluorescent X-ray analysis, is used, has the low-temperature fixing ability of the electrostatic image developing toner for a recording medium having an uneven surface, while suppressing a decrease in gradation when a halftone image is formed on a recording medium having an uneven surface, a toner cartridge, an image forming apparatus, and an image forming method. [Brief description of the drawings]
[0016] [Figure 1] 1 is a schematic configuration diagram illustrating an example of an image forming apparatus according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic diagram illustrating an example of a process cartridge according to the present embodiment. [Diagram 3] 2 is a schematic diagram showing a cross section of a toner particle in the electrostatic image developing toner according to the exemplary embodiment; FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Hereinafter, an embodiment of the present invention will be described in detail. In addition, in numerical ranges described in stages, the upper limit or lower limit value described in a certain numerical range may be replaced with the upper limit or lower limit value of another numerical range described in stages. In addition, in a numerical range, the upper limit or lower limit described in a certain numerical range may be replaced with a value shown in the examples. When a plurality of substances corresponding to each component are present in the composition, the amount of each component in the composition means the total amount of the plurality of substances present in the composition, unless otherwise specified. The term "process" includes not only an independent process, but also a process that cannot be clearly distinguished from other processes, as long as the intended purpose of the process is achieved.
[0018] <Toner for developing electrostatic images> The toner for developing electrostatic images according to the present embodiment (hereinafter, may be simply referred to as "toner") includes toner particles containing a binder resin, the binder resin contains an amorphous resin and a crystalline resin, and has a net intensity of Mg element measured by fluorescent X-ray analysis of 0.02 or more and 0.15 or less, and a net intensity of Cl element measured by fluorescent X-ray analysis of 0.02 or more and 0.60 or less.
[0019] The toner according to the present embodiment, due to the above-mentioned constitution, has low-temperature fixability to a recording medium having an uneven surface, while suppressing a decrease in gradation when a halftone image is formed on the recording medium having an uneven surface. The reason for this is presumed to be as follows.
[0020] In electrophotographic image formation, when a recording medium having an uneven surface, such as embossed paper, is used as the recording medium for the image, the fixing property of the toner may be reduced. A recording medium having an uneven surface may have a large thickness and a large heat capacity. Therefore, when a toner is fixed to a recording medium having an uneven surface, the recording medium tends to absorb a lot of heat, and the fixing property may be reduced. In order to improve the fixing property, it is necessary to increase the fixing temperature when fixing the toner to the recording medium, but this may increase the manufacturing cost. Therefore, there is a demand for a toner that is easily fixed to a recording medium even at a low fixing temperature.
[0021] In order to improve the low-temperature fixability of the toner to the recording medium, a toner containing toner particles in which the binder resin contains an amorphous resin and a crystalline resin may be used. By using such a binder resin, the amorphous resin and the crystalline resin become compatible with each other when the toner is fixed, and the toner becomes easy to melt. In other words, the toner becomes easy to melt at a low temperature. Therefore, when the toner is fixed to the recording medium, the toner melts at a low fixing temperature, and is easy to fix to the recording medium.
[0022] However, when the toner particles contain a crystalline resin, charge leakage from the toner may occur. This is because the crystalline resin has a property of being difficult to retain charge, and when the surface layer of the toner particles has a domain of the crystalline resin, charge leakage from the domain is likely to occur. Therefore, for example, in image formation by the secondary transfer method, when the toner is transferred from the intermediate transfer body to the recording medium during the secondary transfer, the charge amount of the toner may decrease, and the transfer efficiency may decrease. And, due to the decrease in transfer efficiency, the image formed on the recording medium may have image defects. The decrease in transfer efficiency due to the inclusion of a crystalline resin in the toner particles may be more likely to occur when a halftone image is formed on a recording medium having an uneven surface, and therefore, when a halftone image is formed on a recording medium having an uneven surface, the gradation of the halftone image may be decreased. In recent years, there has been a demand for the development of a technology for forming images with various color expressions on a recording medium having an uneven surface. In light of this background, there has been a demand for a toner including toner particles in which the binder resin contains an amorphous resin and a crystalline resin, which has low-temperature fixability for a recording medium having an uneven surface, while suppressing a decrease in gradation when a halftone image is formed on the recording medium having an uneven surface.
[0023] The toner according to the present embodiment has a net intensity of Mg element measured by fluorescent X-ray analysis of the toner particles of 0.02 or more and 0.15 or less. By setting the net intensity of Mg element within this range, Mg is contained in a large amount on the surface of the toner particles. Then, Mg bonds with carboxyl groups derived from the binder resin on the surface of the toner particles within a range that does not impair the fixability of the toner, and a structure is formed in which Mg covers the surface of the toner particles. Then, even if the surface layer of the toner particles has a domain of crystalline resin, the charge leakage from the domain is inhibited by Mg present on the surface of the toner particles. Therefore, the toner according to the present embodiment is easy to hold charge, and for example, in the case of image formation by the secondary transfer method, when the toner is transferred from the intermediate transfer body to the recording medium during the secondary transfer, the decrease in the transfer efficiency of the toner can be suppressed. Therefore, when a halftone image is formed on a recording medium having an uneven surface, the toner according to the present embodiment suppresses the decrease in the gradation of the halftone image. In addition, the toner according to the present embodiment has a net intensity of Cl element measured by fluorescent X-ray analysis of the toner particles of 0.02 to 0.60. By setting the net intensity of Cl element within this range, the amount of bond between Mg and the carboxyl group derived from the binder resin on the toner particle surface is adjusted to a level that does not impair the fixability of the toner. By including Cl on the toner particle surface so that the net intensity is within the above range, Mg bonds not only with the carboxyl group of the binder resin but also with Cl. Cl moderately inhibits the bond between Mg and the carboxyl group of the binder resin, thereby suppressing the formation of bonds between excess Mg and the carboxyl group derived from the binder resin on the toner particle surface. Therefore, even if bonds between Mg and the carboxyl group derived from the binder resin are formed on the toner particle surface, the decrease in fixability of the toner is suppressed.
[0024] As described above, the toner according to this embodiment has the above-mentioned configuration, which has low-temperature fixing properties for recording media having an uneven surface, while suppressing a decrease in gradation when a halftone image is formed on a recording medium having an uneven surface.
[0025] (Toner particles) The toner contains toner particles containing a binder resin. The toner particles may also contain a colorant, a release agent, and other additives. -Binding resin- The binder resin contains an amorphous resin and a crystalline resin. The binder resin may be an amorphous resin or a crystalline resin. However, the mass ratio of the amorphous resin to the crystalline resin (crystalline resin / amorphous resin) is preferably from 3 / 97 to 50 / 50, and more preferably from 7 / 93 to 30 / 70.
[0026] The content of the binder resin is, for example, preferably from 40% by mass to 95% by mass, more preferably from 50% by mass to 90% by mass, and even more preferably from 60% by mass to 85% by mass, based on the total amount of the toner particles.
[0027] Here, the term "amorphous resin" refers to a resin that, in a thermal analysis measurement using differential scanning calorimetry (DSC), has only a stepwise endothermic change rather than a clear endothermic peak, is a solid at room temperature, and is thermoplasticized at a temperature equal to or higher than the glass transition temperature. On the other hand, a crystalline resin is one that has a clear endothermic peak rather than a stepwise change in endothermic amount in differential scanning calorimetry (DSC). Specifically, for example, a crystalline resin means a resin whose half-width of an endothermic peak is within 10°C when measured at a heating rate of 10°C / min, and an amorphous resin means a resin whose half-width exceeds 10°C or a resin in which no clear endothermic peak is observed.
[0028] The amorphous resin will be described. Examples of the amorphous resin include known amorphous resins such as amorphous polyester resin, amorphous vinyl resin (e.g., styrene acrylic resin, etc.), epoxy resin, polycarbonate resin, polyurethane resin, etc. Among these, from the viewpoint of improving low-temperature fixability and facilitating bonding with Mg, amorphous polyester resin and amorphous vinyl resin (particularly styrene acrylic resin) are preferred, and amorphous polyester resin is more preferred. In addition, it is also a preferred embodiment to use an amorphous polyester resin and a styrene-acrylic resin in combination as the amorphous resin.
[0029] The amorphous polyester resin may be, for example, a condensation polymer of a polyvalent carboxylic acid and a polyhydric alcohol. The amorphous polyester resin may be a commercially available product or a synthesized product.
[0030] Examples of polyvalent carboxylic acids include aliphatic dicarboxylic acids (e.g., oxalic acid, malonic acid, maleic acid, fumaric acid, citraconic acid, itaconic acid, glutaconic acid, succinic acid, alkenylsuccinic acid, adipic acid, sebacic acid, etc.), alicyclic dicarboxylic acids (e.g., cyclohexanedicarboxylic acid, etc.), aromatic dicarboxylic acids (e.g., terephthalic acid, isophthalic acid, phthalic acid, naphthalenedicarboxylic acid, etc.), anhydrides thereof, and lower alkyl esters thereof (e.g., having 1 to 5 carbon atoms). Among these, aromatic dicarboxylic acids are preferable as polyvalent carboxylic acids. The polyvalent carboxylic acid may be a trivalent or higher carboxylic acid having a crosslinked or branched structure in combination with a dicarboxylic acid. Examples of the trivalent or higher carboxylic acid include trimellitic acid, pyromellitic acid, anhydrides thereof, and lower (e.g., carbon number 1 to 5) alkyl esters thereof. The polyvalent carboxylic acids may be used alone or in combination of two or more kinds.
[0031] Examples of polyhydric alcohols include aliphatic diols (e.g., ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, butanediol, hexanediol, neopentyl glycol, etc.), alicyclic diols (e.g., cyclohexanediol, cyclohexanedimethanol, hydrogenated bisphenol A, etc.), and aromatic diols (e.g., ethylene oxide adducts of bisphenol A, propylene oxide adducts of bisphenol A, etc.). Among these, examples of polyhydric alcohols include aromatic diols and alicyclic diols, and more preferably aromatic diols. As the polyhydric alcohol, a trihydric or higher polyhydric alcohol having a crosslinked or branched structure may be used in combination with the diol. Examples of the trihydric or higher polyhydric alcohol include glycerin, trimethylolpropane, and pentaerythritol. The polyhydric alcohols may be used alone or in combination of two or more kinds.
[0032] The amorphous polyester resin can be obtained by a known manufacturing method, for example, by carrying out the reaction while removing water and alcohol generated during condensation by setting the polymerization temperature to 180° C. or higher and 230° C. or lower, and reducing the pressure in the reaction system as necessary. If the raw material monomer is not soluble or compatible at the reaction temperature, a high boiling point solvent may be added as a solubilizing agent to dissolve it. In this case, the polycondensation reaction is carried out while distilling off the solubilizing agent. If a monomer with poor compatibility is present, it is recommended that the monomer with poor compatibility is condensed in advance with the acid or alcohol to be polycondensed, and then polycondensed with the main component.
[0033] Here, the amorphous polyester resin may be a modified amorphous polyester resin in addition to the unmodified amorphous polyester resin described above. The modified amorphous polyester resin is an amorphous polyester resin having a bond group other than an ester bond, or an amorphous polyester resin having a resin component different from the amorphous polyester resin component bonded by a covalent bond or an ionic bond. The modified amorphous polyester resin may be, for example, an amorphous polyester resin having a functional group such as an isocyanate group that reacts with an acid group or a hydroxyl group at the end introduced therein, and a resin having a modified end that is reacted with an active hydrogen compound.
[0034] The styrene-acrylic resin is a copolymer obtained by copolymerizing at least a styrene-based monomer (a monomer having a styrene skeleton) and a (meth)acrylic-based monomer (a monomer having a (meth)acrylic group, preferably a monomer having a (meth)acryloxy group). The styrene-acrylic resin includes, for example, a copolymer of a styrene monomer and a (meth)acrylic acid ester monomer. The acrylic resin portion of the styrene-acrylic resin is a partial structure formed by polymerizing either an acrylic monomer or a methacrylic monomer, or both. In addition, the term "(meth)acrylic" includes both "acrylic" and "methacrylic".
[0035] Specific examples of styrene-based monomers include styrene, alkyl-substituted styrenes (e.g., α-methylstyrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 2-ethylstyrene, 3-ethylstyrene, 4-ethylstyrene, etc.), halogen-substituted styrenes (e.g., 2-chlorostyrene, 3-chlorostyrene, 4-chlorostyrene, etc.), vinylnaphthalene, etc. The styrene-based monomers may be used alone or in combination of two or more. Of these, as the styrene-based monomer, styrene is preferred from the viewpoints of ease of reaction, ease of reaction control, and availability.
[0036] Specific examples of the (meth)acrylic monomer include (meth)acrylic acid and (meth)acrylic acid esters. Examples of the (meth)acrylic acid esters include (meth)acrylic acid alkyl esters (e.g., methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl acrylate, n-heptyl (meth)acrylate, n-octyl (meth)acrylate, n-decyl (meth)acrylate, n-dodecyl (meth)acrylate, n-lauryl (meth)acrylate, n-tetradecyl (meth)acrylate, n-hexadecyl (meth)acrylate, n-octadecyl (meth)acrylate, isopropyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, isopentyl (meth)acrylate, amyl (meth)acrylate, and (meth) Examples of the (meth)acrylic acid monomer include neopentyl acrylate, isohexyl (meth)acrylate, isoheptyl (meth)acrylate, isooctyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, cyclohexyl (meth)acrylate, t-butylcyclohexyl (meth)acrylate, etc.), aryl (meth)acrylate esters (e.g., phenyl (meth)acrylate, biphenyl (meth)acrylate, diphenylethyl (meth)acrylate, t-butylphenyl (meth)acrylate, terphenyl (meth)acrylate, etc.), dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, methoxyethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, β-carboxyethyl (meth)acrylate, and (meth)acrylamide. The (meth)acrylic acid monomer may be used alone or in combination of two or more. Among these (meth)acrylic esters among the (meth)acrylic monomers, from the viewpoint of fixation, (meth)acrylic acid esters having an alkyl group having 2 to 14 carbon atoms (preferably 2 to 10 carbon atoms, more preferably 3 to 8 carbon atoms) are preferred. Of these, n-butyl (meth)acrylate is preferred, and n-butyl acrylate is particularly preferred.
[0037] The copolymerization ratio of the styrene monomer to the (meth)acrylic monomer (mass basis, styrene monomer / (meth)acrylic monomer) is not particularly limited, but is preferably 85 / 15 to 70 / 30.
[0038] The styrene-acrylic resin may have a crosslinked structure. A preferred example of the styrene-acrylic resin having a crosslinked structure is a copolymer of at least a styrene-based monomer, a (meth)acrylic acid-based monomer, and a crosslinkable monomer.
[0039] The crosslinkable monomer may, for example, be a bifunctional or higher functional crosslinking agent. Examples of bifunctional crosslinking agents include divinylbenzene, divinylnaphthalene, di(meth)acrylate compounds (e.g., diethylene glycol di(meth)acrylate, methylene bis(meth)acrylamide, decanediol diacrylate, glycidyl (meth)acrylate, etc.), polyester type di(meth)acrylate, 2-([1'-methylpropylideneamino]carboxyamino)ethyl methacrylate, etc. Examples of polyfunctional crosslinking agents include tri(meth)acrylate compounds (e.g., pentaerythritol tri(meth)acrylate, trimethylolethane tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, etc.), tetra(meth)acrylate compounds (e.g., pentaerythritol tetra(meth)acrylate, oligoester (meth)acrylate, etc.), 2,2-bis(4-methacryloxy, polyethoxyphenyl)propane, diallyl phthalate, triallyl cyanurate, triallyl isocyanurate, triallyl trimellitate, diaryl chlorendate, etc. Among these, as the crosslinkable monomer, from the viewpoints of suppressing the occurrence of a decrease in image density and suppressing the occurrence of uneven image density, and of fixability, a bifunctional or higher (meth)acrylate compound is preferred, a bifunctional (meth)acrylate compound is more preferred, a bifunctional (meth)acrylate compound having an alkylene group with 6 to 20 carbon atoms is further preferred, and a bifunctional (meth)acrylate compound having a linear alkylene group with 6 to 20 carbon atoms is particularly preferred.
[0040] The copolymerization ratio of the crosslinkable monomer to the total monomers (mass basis, crosslinkable monomer / total monomers) is not particularly limited, but is preferably 2 / 1,000 to 20 / 1,000.
[0041] The method for producing the styrene-acrylic resin is not particularly limited, and various polymerization methods (e.g., solution polymerization, precipitation polymerization, suspension polymerization, bulk polymerization, emulsion polymerization, etc.) are applied. In addition, the polymerization reaction is carried out by a known operation (e.g., batchwise, semi-continuous, continuous, etc.).
[0042] The characteristics of the amorphous resin will be described. The glass transition temperature (Tg) of the amorphous resin is preferably 50°C or higher and 80°C or lower, and more preferably 50°C or higher and 65°C or lower. The glass transition temperature is determined from a DSC curve obtained by differential scanning calorimetry (DSC), more specifically, from the "extrapolated glass transition onset temperature" described in the method for determining glass transition temperature in JIS K 7121-1987 "Method for measuring transition temperature of plastics."
[0043] The weight average molecular weight (Mw) of the amorphous resin is preferably 5,000 or more and 1,000,000 or less, and more preferably 7,000 or more and 500,000 or less. The number average molecular weight (Mn) of the amorphous resin is preferably 2,000 or more and 100,000 or less. The molecular weight distribution Mw / Mn of the amorphous resin is preferably 1.5 or more and 100 or less, and more preferably 2 or more and 60 or less. The weight average molecular weight and number average molecular weight are measured by gel permeation chromatography (GPC). The molecular weight measurement by GPC is performed using a Tosoh GPC HLC-8120GPC as the measuring device, a Tosoh TSKgel SuperHM-M (15 cm) column, and THF solvent. The weight average molecular weight and number average molecular weight are calculated from the measurement results using a molecular weight calibration curve created with a monodisperse polystyrene standard sample.
[0044] The crystalline resin will now be described. Examples of the crystalline resin include known crystalline resins such as crystalline polyester resins and crystalline vinyl resins (e.g., polyalkylene resins, long-chain alkyl (meth)acrylate resins, etc.) Among these, crystalline polyester resins are preferred from the viewpoints of improving low-temperature fixability and facilitating bonding with Mg.
[0045] The crystalline polyester resin may be, for example, a polycondensate of a polyvalent carboxylic acid and a polyhydric alcohol. The crystalline polyester resin may be a commercially available product or a synthesized product. Here, the crystalline polyester resin is preferably a polycondensate using a polymerizable monomer having a linear aliphatic group rather than a polymerizable monomer having an aromatic group, since the crystalline polyester resin can easily form a crystalline structure.
[0046] Examples of polyvalent carboxylic acids include aliphatic dicarboxylic acids (e.g., oxalic acid, succinic acid, glutaric acid, adipic acid, suberic acid, azelaic acid, sebacic acid, 1,9-nonanedicarboxylic acid, 1,10-decanedicarboxylic acid, 1,12-dodecanedicarboxylic acid, 1,14-tetradecanedicarboxylic acid, 1,18-octadecanedicarboxylic acid, etc.), aromatic dicarboxylic acids (e.g., dibasic acids such as phthalic acid, isophthalic acid, terephthalic acid, naphthalene-2,6-dicarboxylic acid, etc.), anhydrides thereof, and lower alkyl esters thereof (e.g., having 1 to 5 carbon atoms). The polyvalent carboxylic acid may be a trivalent or higher carboxylic acid having a crosslinked or branched structure in combination with a dicarboxylic acid. Examples of the trivalent carboxylic acid include aromatic carboxylic acids (e.g., 1,2,3-benzenetricarboxylic acid, 1,2,4-benzenetricarboxylic acid, 1,2,4-naphthalenetricarboxylic acid, etc.), their anhydrides, and their lower alkyl esters (e.g., carbon number 1 to 5). As the polyvalent carboxylic acid, a dicarboxylic acid having a sulfonic acid group and a dicarboxylic acid having an ethylenic double bond may be used in combination with these dicarboxylic acids. The polyvalent carboxylic acids may be used alone or in combination of two or more kinds.
[0047] Examples of polyhydric alcohols include aliphatic diols (for example, straight-chain aliphatic diols having 7 to 20 carbon atoms in the main chain). Examples of aliphatic diols include ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,13-tridecanediol, 1,14-tetradecanediol, 1,18-octadecanediol, and 1,14-eicosanedecanediol. Among these, 1,8-octanediol, 1,9-nonanediol, and 1,10-decanediol are preferred as aliphatic diols. The polyhydric alcohol may be a trihydric or higher alcohol having a crosslinked or branched structure in combination with the diol. Examples of the trihydric or higher alcohol include glycerin, trimethylolethane, trimethylolpropane, and pentaerythritol. The polyhydric alcohols may be used alone or in combination of two or more kinds.
[0048] Here, the polyhydric alcohol has an aliphatic diol content of 80 mol % or more, preferably 90 mol % or more.
[0049] The crystalline polyester resin can be obtained by a known manufacturing method, for example, in the same manner as the amorphous polyester.
[0050] The characteristics of the crystalline resin will be described. The melting temperature of the crystalline resin is preferably 50°C or higher and 100°C or lower, more preferably 55°C or higher and 90°C or lower, and even more preferably 60°C or higher and 85°C or lower. The melting temperature is determined from a DSC curve obtained by differential scanning calorimetry (DSC) based on the "melting peak temperature" described in the method for determining melting temperature in JIS K7121-1987 "Method for measuring transition temperature of plastics."
[0051] The weight average molecular weight (Mw) of the crystalline resin is preferably 6,000 or more and 35,000 or less.
[0052] From the viewpoint of easily forming a crystal structure and having good compatibility with the amorphous polyester resin, which results in improved image fixing properties, it is preferable that the crystalline resin is a polymer of an α,ω-linear aliphatic dicarboxylic acid and an α,ω-linear aliphatic diol.
[0053] The α,ω-linear aliphatic dicarboxylic acid is preferably an α,ω-linear aliphatic dicarboxylic acid in which the alkylene group connecting the two carboxy groups has 3 or more and 14 or less carbon atoms, more preferably the alkylene group has 4 or more and 12 or less carbon atoms, and even more preferably the alkylene group has 6 or more and 10 or less carbon atoms. Examples of α,ω-linear aliphatic dicarboxylic acids include succinic acid, glutaric acid, adipic acid, 1,6-hexanedicarboxylic acid (commonly known as suberic acid), 1,7-heptanedicarboxylic acid (commonly known as azelaic acid), 1,8-octanedicarboxylic acid (commonly known as sebacic acid), 1,9-nonanedicarboxylic acid, 1,10-decanedicarboxylic acid, 1,12-dodecanedicarboxylic acid, 1,14-tetradecanedicarboxylic acid, and 1,18-octadecanedicarboxylic acid. Of these, 1,6-hexanedicarboxylic acid, 1,7-heptanedicarboxylic acid, 1,8-octanedicarboxylic acid, and 1,10-decanedicarboxylic acid are preferred. The α,ω-linear aliphatic dicarboxylic acids may be used alone or in combination of two or more kinds.
[0054] The α,ω-linear aliphatic diol is preferably an α,ω-linear aliphatic diol in which the alkylene group connecting the two hydroxy groups has 3 to 14 carbon atoms, more preferably the alkylene group has 4 to 12 carbon atoms, and further preferably the alkylene group has 6 to 10 carbon atoms. Examples of the α,ω-linear aliphatic diol include ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,12-dodecanediol, 1,14-tetradecanediol, and 1,18-octadecanediol. Of these, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, and 1,10-decanediol are preferred. The α,ω-linear aliphatic diols may be used alone or in combination of two or more kinds.
[0055] As the polymer of an α,ω-linear aliphatic dicarboxylic acid and an α,ω-linear aliphatic diol, from the viewpoint of easily forming a crystal structure and having good compatibility with an amorphous polyester resin, thereby improving the fixability of an image, a polymer of at least one selected from the group consisting of 1,6-hexanedicarboxylic acid, 1,7-heptanedicarboxylic acid, 1,8-octanedicarboxylic acid, 1,9-nonanedicarboxylic acid, and 1,10-decanedicarboxylic acid and at least one selected from the group consisting of 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, and 1,10-decanediol is preferred, and among these, a polymer of 1,10-decanedicarboxylic acid and 1,6-hexanediol is more preferred.
[0056] - Domain morphology of crystalline resin in toner particles - When a cross section of a toner particle is observed, it is preferable that at least two crystalline resin domains (preferably at least three crystalline resin domains) satisfy the conditions (A), (B1), (B2), (C) and (D), provided that the at least two crystalline resin domains only need to satisfy at least one of the conditions (B1) and (B2).
[0057] Condition (A): The aspect ratio of the domain of the crystalline resin is 5 or more and 40 or less. Condition (B1): The length of the major axis of the domain of the crystalline resin is 0.5 μm or more and 1.5 μm or less. Condition (B2): In at least one of the two domains of the crystalline resin, the ratio of the major axis length to the maximum diameter of the toner particle is 10% or more and 30% or less. Condition (C): The angle between an extension line of the long axis of the domain of the crystalline resin and a tangent line at the contact point where the extension line contacts the surface of the toner particle is 60 degrees or more and 90 degrees or less. Condition (D): The crossing angle between the extension lines of the long axes of the two domains of the crystalline resin is 45 degrees or more and 90 degrees or less.
[0058] The toner according to the present embodiment, by virtue of the above-mentioned constitution, suppresses the deterioration of uneven glossiness of an image that occurs when an image having a large amount of toner is formed. The reason for this is presumed to be as follows.
[0059] When a cross section of a toner particle is observed, a first toner particle in which at least two crystalline resin domains satisfy the following condition (A), the following condition (B1), the following condition (C), and the following condition (D) becomes more uniform throughout the toner particle, and heat is easily transferred therethrough, making it difficult for uneven melting of the toner particle to occur when a toner image is fixed. Here, the first toner particle satisfying the above conditions means that the first toner particle has an elliptical or needle shape with a large aspect ratio, and two crystalline resin domains with long major axes extend from the surface side of the toner particle toward the inside and are arranged in an intersecting manner (see Figure 3). When heat is applied to the first toner particles during fixing of a toner image having the first toner particles that satisfy the above conditions, the ellipsoidal or needle-shaped crystalline resin melts, and heat is easily and rapidly transferred from the surface to the inside of the first toner particles, whereby heat is transferred almost uniformly throughout the entire inside of the toner particles, and the entire inside of the toner particles is easily melted in an almost uniform manner.
[0060] When a cross section of a toner particle is observed, a second toner particle in which at least two crystalline resin domains satisfy the following condition (A), the following condition (B2), the following condition (C), and the following condition (D) becomes more uniform within the toner particle, and heat is easily transferred therethrough, making it difficult for uneven melting of the toner particle to occur when the toner image is fixed. Here, the second toner particles satisfying the above conditions means that, like the first toner particles, the second toner particles have elliptical or needle-like shapes with a large aspect ratio, and two crystalline resin domains with long major axes extend from the surface side of the toner particles toward the inside and are arranged to intersect (see FIG. 3). Therefore, like the first toner particles, when heat is applied to the first toner particles during fixing of a toner image having the first toner particles, the heat is transferred almost uniformly throughout the entire interior of the toner particles, and the entire interior of the toner particles is easily melted in an almost uniform state.
[0061] From the above, it is presumed that the toner according to the present embodiment, due to the above-mentioned configuration, suppresses the decrease in uneven gloss of an image that occurs when an image with a large amount of toner is formed.
[0062] Here, each symbol shown in FIG. TN: toner particles Amo: Amorphous resin Cry: Crystalline resin L cry : Long axis length of the domain of the crystalline resin L T : Maximum diameter of toner particles θ A The angle between the extension of the long axis of the crystalline resin domain and the tangent at the point where the extension touches the surface of the toner particle θ B : The crossing angle between the extension lines of the long axes of two crystalline resin domains Shows.
[0063] Each condition will be explained below.
[0064] Condition (A) The aspect ratio of the domain of the crystalline resin is 5 or more and 40 or less. From the viewpoint of suppressing uneven gloss of an image, the aspect ratio of the domain of the crystalline resin is preferably 10 or more and 40 or less. Here, the aspect ratio of a crystalline resin domain means the ratio of the long axis length to the short axis length (long axis length / short axis length) in the crystalline resin domain. The long axis length of the domain of the crystalline resin means the maximum length of the domain of the crystalline resin. The minor axis length of a domain of a crystalline resin means the maximum length among lengths in a direction perpendicular to an extension line of the major axis length of the domain of a crystalline resin.
[0065] ·Conditions (B1) The long axis length of the domain of the crystalline resin (L in Fig. 3) cry The particle size is between 0.5 μm and 1.5 μm. From the viewpoint of suppressing uneven gloss of an image, the major axis length of the domain of the crystalline resin is preferably 0.8 μm or more and 1.5 μm or less.
[0066] ·Conditions (B2) In at least one of the two domains of the crystalline resin, the major axis length (L in FIG. 3) relative to the maximum diameter (Lt in FIG. 3) of the toner particle is cry The proportion of those who are not eligible for the 2015 GAAP (see reference) is between 10% and 30%. From the viewpoint of suppressing uneven gloss of an image, the ratio of the major axis length of the crystalline resin domain to the maximum diameter of the toner particle is preferably 13% or more and 30% or less, and more preferably 17% or more and 30% or less. The maximum diameter of a toner particle means the maximum length of a straight line drawn between any two points on the contour line of the cross section of a toner particle (so-called major axis).
[0067] ·Condition (C) The angle between the extension line of the long axis of the crystalline resin domain and the tangent line at the point where the extension line touches the toner particle surface (i.e., the outer edge of the toner particle) (θ in FIG. 3) A (see reference) is between 60 degrees and 90 degrees. From the viewpoint of suppressing uneven gloss of an image, the angle between the extension line of the long axis of the crystalline resin domain and the tangent line at the contact point where the extension line contacts the toner particle surface is preferably 75 degrees or more and 90 degrees or less.
[0068] Condition (D) The crossing angle between the extension lines of the long axes of the two crystalline resin domains (θ B See reference) is between 45 degrees and 90 degrees. From the viewpoint of suppressing uneven gloss of the image, the crossing angle of the extension lines of the long axes of the two crystalline resin domains (θ B The angle θ is preferably between 60 degrees and 90 degrees.
[0069] From the viewpoint of suppressing uneven gloss of an image, the toner particles satisfying each of the conditions preferably account for 40% by number or more of the total toner particles, more preferably 70% by number or more, even more preferably 80% by number or more, and particularly preferably 90% by number or more. Ideally, the ratio of toner particles satisfying each of the above conditions is 100% by number. The more toner particles that satisfy the above conditions, the easier it is for the entire toner particles to melt in a nearly uniform state, and the easier it is to suppress uneven gloss in the image.
[0070] - Method for observing the cross section of a toner particle The method for observing the cross section of a toner particle to determine whether the toner particle satisfies the conditions (A), (B1), (B2), (C) and (D) is as follows. Toner particles (or toner particles with external additives) are mixed and embedded in epoxy resin, and the epoxy resin is solidified. The solidified material obtained is cut using an ultramicrotome device (Ultracut UCT manufactured by Leica) to prepare a thin section sample with a thickness of 80 nm to 130 nm. Next, the obtained thin section sample is stained with ruthenium tetroxide for 3 hours in a desiccator at 30°C. Then, an ultra-high resolution field emission scanning electron microscope (FE-SEM, S-4800 manufactured by Hitachi High-Technologies Corporation) is used to obtain a STEM observation image (accelerating voltage: 30 kV, magnification: 20,000 times) in the transmission image mode of the stained thin section sample. Among the toner particles, the crystalline polyester resin and the release agent are judged from the contrast and shape. In the SEM image, the crystalline resin stained with ruthenium is different from the amorphous resin, the release agent, etc., in that the binder resin other than the release agent has many double bond parts and is stained with ruthenium tetroxide, so the release agent part and the resin part other than the release agent can be distinguished. That is, with ruthenium dyeing, the release agent is the domain that is dyed the lightest, followed by the crystalline resin (e.g., crystalline polyester resin), and the amorphous resin (e.g., amorphous polyester resin) that is dyed the darkest. By adjusting the contrast, the release agent can be judged as a domain that is observed to be white, the amorphous resin as black, and the crystalline resin as light gray.
[0071] Then, the ruthenium-dyed crystalline resin region is subjected to image analysis to determine whether the toner particles satisfy the conditions (A), (B1), (B2), (C) and (D). In addition, when determining the ratio of toner particles that satisfy each of the above conditions, 100 toner particles are observed, and the ratio of toner particles that satisfy each of the above conditions is calculated.
[0072] In addition, since the SEM image contains toner particle cross sections of various sizes, a toner particle cross section whose diameter is 85% or more of the volume average particle diameter of the toner particle is selected as the toner particle to be observed. Here, the diameter of the toner particle cross section refers to the maximum length of a straight line drawn between any two points on the contour line of the toner particle cross section (the so-called major axis).
[0073] -Coloring agent- Examples of colorants include carbon black, chrome yellow, Hansa Yellow, benzidine yellow, threne yellow, quinoline yellow, pigment yellow, permanent orange GTR, pyrazolone orange, Balkan orange, watch young red, permanent red, brilliant carmine 3B, brilliant carmine 6B, DuPont oil red, pyrazolone red, lithol red, rhodamine B lake, lake red C, pigment red, rose bengal, aniline blue, ultramarine blue, and tetrahydrofuran. Examples of the dyes include various pigments such as phosphorus blue, chalcoil blue, methylene blue chloride, phthalocyanine blue, pigment blue, phthalocyanine green, and malachite green oxalate, and various dyes such as acridine-based, xanthene-based, azo-based, benzoquinone-based, azine-based, anthraquinone-based, thioindigo-based, dioxazine-based, thiazine-based, azomethine-based, indigo-based, phthalocyanine-based, aniline black-based, polymethine-based, triphenylmethane-based, diphenylmethane-based, and thiazole-based dyes. The colorant may be used alone or in combination of two or more kinds.
[0074] The colorant may be surface-treated as necessary, or may be used in combination with a dispersant. In addition, a plurality of types of colorants may be used in combination.
[0075] The content of the colorant is, for example, preferably from 1% by mass to 30% by mass, and more preferably from 3% by mass to 15% by mass, based on the total mass of the toner particles.
[0076] -Release agent- Examples of the release agent include hydrocarbon waxes; natural waxes such as carnauba wax, rice wax, and candelilla wax; synthetic or mineral / petroleum waxes such as montan wax; and ester waxes such as fatty acid esters and montan acid esters.
[0077] The melting temperature of the release agent is preferably 50°C or higher and 110°C or lower, and more preferably 60°C or higher and 100°C or lower. The melting temperature is determined from a DSC curve obtained by differential scanning calorimetry (DSC) based on the "melting peak temperature" described in the method for determining melting temperature in JIS K 7121-1987 "Method for measuring transition temperature of plastics."
[0078] The release agent is preferably an ester wax. When an ester wax is used as the releasing agent, it has good compatibility with the amorphous polyester resin and can improve the fixing property of the image.
[0079] The ester wax is a wax having an ester bond. The ester wax may be any of a monoester, diester, triester, and tetraester, and any known natural or synthetic ester wax can be used. Examples of ester waxes include ester compounds of higher fatty acids (such as fatty acids having 10 or more carbon atoms) and monohydric or polyhydric aliphatic alcohols (such as aliphatic alcohols having 8 or more carbon atoms), and have a melting temperature of 60°C or higher and 110°C or lower (preferably 65°C or higher and 100°C or lower, more preferably 70°C or higher and 95°C or lower). Examples of ester waxes include ester compounds of higher fatty acids (caprylic acid, capric acid, lauric acid, myristic acid, palmitic acid, stearic acid, arachidic acid, behenic acid, oleic acid, etc.) and alcohols (monohydric alcohols such as methanol, ethanol, propanol, isopropanol, butanol, capryl alcohol, lauryl alcohol, myristyl alcohol, cetyl alcohol, stearyl alcohol, oleyl alcohol, etc.; polyhydric alcohols such as glycerin, ethylene glycol, propylene glycol, sorbitol, pentaerythritol, etc.). Specific examples include carnauba wax, rice wax, candelilla wax, jojoba oil, Japan wax, beeswax, privet wax, lanolin, and montanic acid ester wax.
[0080] In toner particles in which at least two crystalline resin domains satisfy conditions (A), (B1), (B2), (C) and (D), it is preferable that the domain of the release agent exists at a depth of 50 nm or more from the surface of the toner particle when the cross section of the toner particle is observed. In other words, this means that when the cross section of the toner particle is observed, the shortest distance between the domain of the release agent existing in the toner particle and the surface (i.e., the outer edge) of the toner particle is 50 nm or more. The at least two crystalline resin domains need only satisfy at least one of the conditions (B1) and (B2).
[0081] The domain of the release agent is present at a depth of 50 nm or more from the surface of the toner particle, which means that the domain of the release agent is not exposed on the surface of the toner particle. If the domain of the release agent is exposed on the surface of the toner particle, the external additive is unevenly distributed and adhered to the release agent exposed position. Therefore, if the domain of the release agent is present at a depth of 50 nm or more from the surface of the toner particle, the external additive is easily adhered in a nearly uniform state, and melting unevenness of the toner particle during fixing is easily suppressed. As a result, gloss unevenness of the image is easily suppressed.
[0082] Whether the domain of the release agent is present inside the toner particle to a depth of 50 nm or more from the surface thereof is confirmed by the above-mentioned method for observing the cross section of the toner particle.
[0083] From the viewpoint of suppressing uneven gloss in an image, the ratio of toner particles in which at least two crystalline resin domains satisfy the above conditions and the release agent domain exists at a depth of 50 nm or more from the surface of the toner particles is preferably 40% by number or more, more preferably 70% by number or more, even more preferably 80% by number or more, and particularly preferably 90% by number or more, based on the total toner particles. Ideally, the ratio of toner particles satisfying each of the above conditions is 100% by number.
[0084] The content of the release agent is, for example, preferably from 1% by mass to 20% by mass, and more preferably from 5% by mass to 15% by mass, based on the total amount of the toner particles.
[0085] -Other additives- Examples of other additives include well-known additives such as magnetic materials, charge control agents, inorganic powders, etc. These additives are contained in the toner particles as internal additives.
[0086] -Net strength of Mg and Cl elements- In the toner according to the present embodiment, the net intensity of Mg element in the toner particles measured by fluorescent X-ray analysis is 0.02 to 0.15, and the net intensity of Cl element in the toner particles measured by fluorescent X-ray analysis is 0.02 to 0.60.
[0087] By setting the net strength of Mg element within the above range, the bond between Mg and the carboxyl group derived from the binder resin is formed within a range that does not impair the fixability of the toner. Therefore, the toner according to the present embodiment is easy to hold charge and can suppress the decrease in transfer efficiency. Therefore, when a halftone image is formed on a recording medium having an uneven surface, the toner according to the present embodiment suppresses the decrease in gradation of the halftone image. In addition, by setting the net strength of Cl element within the above range, the amount of bond between Mg and the carboxyl group derived from the binder resin on the toner particle surface is adjusted to a level that does not impair the fixability of the toner.
[0088] From the viewpoint of having low-temperature fixing ability for a recording medium having an uneven surface, while further suppressing the decrease in gradation when a halftone image is formed on a recording medium having an uneven surface, it is preferable that the net intensity of the Mg element is 0.03 to 0.12 and the net intensity of the Cl element is 0.03 to 0.40, it is more preferable that the net intensity of the Mg element is 0.03 to 0.10 and the net intensity of the Cl element is 0.03 to 0.30, it is even more preferable that the net intensity of the Mg element is 0.03 to 0.08 and the net intensity of the Cl element is 0.03 to 0.25.
[0089] The method for measuring the net intensity of Mg element and the net intensity of Cl element is as follows. Approximately 0.12 g of toner (toner containing external additives includes the external additives) is compressed with a compression molding machine under a load of 6 tons for 60 seconds to produce a disk with a diameter of 50 mm and a thickness of 2 mm. This disk is used as a sample to perform qualitative and quantitative elemental analysis under the following conditions using a scanning X-ray fluorescence analyzer (Rigaku ZSX PrimusII) to determine the net strength (unit: kilocounts per second, kcps) of each of the Na and Cl elements. Tube voltage: 40kV ·Tube current: 70mA ·Anti-cathode: Rhodium Measurement time: 15 minutes ·Analysis diameter: 10mm in diameter
[0090] Here, examples of sources of Mg element in the toner particles include magnesium chloride, magnesium sulfate, magnesium nitrate, and the like. Furthermore, examples of sources of Cl element in the toner particles include sodium chloride, potassium chloride, calcium chloride, and the like.
[0091] -Characteristics of toner particles, etc.- The toner particles may be toner particles having a single layer structure, or may be toner particles having a so-called core-shell structure composed of a core portion (core particle) and a coating layer (shell layer) that coats the core portion. Here, the toner particles having a core-shell structure may be composed of, for example, a core containing a binder resin and, if necessary, other additives such as a colorant and a release agent, and a coating layer containing the binder resin.
[0092] The volume average particle size (D50v) of the toner particles is preferably from 2 μm to 15 μm, and more preferably from 4 μm to 8 μm.
[0093] The volume average particle size of the toner particles and various particle size distribution indices are measured using a Coulter Multisizer II (manufactured by Beckman Coulter, Inc.), and the electrolyte is measured using an ISOTON-II (manufactured by Beckman Coulter, Inc.). For the measurement, 0.5 mg to 50 mg of the measurement sample is added to 2 ml of a 5% aqueous solution of a surfactant (preferably sodium alkylbenzene sulfonate) as a dispersant, and this is then added to 100 ml to 150 ml of the electrolyte. The electrolyte with the sample suspended in it is dispersed for 1 minute using an ultrasonic disperser, and the particle size distribution of particles with diameters in the range of 2 μm to 60 μm is measured using a Coulter Multisizer II with an aperture diameter of 100 μm. The number of particles sampled is 50,000. Based on the measured particle size distribution, cumulative distributions of volume and number are drawn for each divided particle size range (channel) from the smallest diameter side, and the particle size at 16% of the cumulative size is defined as the volume particle size D16v, the number particle size D16p, the particle size at 50% of the cumulative size as the volume average particle size D50v, the cumulative number average particle size D50p, and the particle size at 84% of the cumulative size as the volume particle size D84v and number particle size D84p. Using these, the volumetric particle size distribution index (GSDv) is (D84v / D16v) 1 / 2 The number size distribution index (GSDp) is (D84p / D16p) 1 / 2 It is calculated as:
[0094] The average circularity of the toner particles is preferably 0.94 or more and 1.00 or less, and more preferably 0.95 or more and 0.98 or less.
[0095] The average circularity of toner particles is calculated by (circular equivalent perimeter) / (perimeter) [(perimeter of a circle having the same projected area as the particle image) / (perimeter of the particle projected image)]. Specifically, it is a value measured by the following method. First, the toner particles to be measured are sucked and collected, flattened, and a still image of the particles is captured by instantaneous strobe light emission, and the particle image is analyzed by a flow-type particle image analyzer (FPIA-3000 manufactured by Sysmex Corporation). The number of samples to be taken in order to calculate the average circularity is 3,500. When the toner contains an external additive, the toner (developer) to be measured is dispersed in water containing a surfactant, and then ultrasonic treatment is performed to obtain toner particles from which the external additive has been removed.
[0096] (Toner characteristics) In the toner according to this embodiment, the maximum endothermic peak temperature during the first temperature rise measured by a differential scanning calorimeter (DSC) is preferably 58° C. or more and 75° C. or less. By setting the maximum endothermic peak temperature of the toner to 58° C. or more and 75° C. or less, the low-temperature fixability of the toner is improved.
[0097] The maximum endothermic peak temperature during the first temperature rise of the toner is measured by a differential scanning calorimeter (DSC) as follows. A PerkinElmer DSC-7 differential scanning calorimeter is used, and the melting points of indium and zinc are used to correct the temperature of the detector, and the heat of fusion of indium is used to correct the amount of heat. An aluminum pan is used for the sample, and an empty pan is set as a control, and the temperature is raised from room temperature to 150°C at a rate of 10°C / min. Then, the temperature at which the maximum endothermic peak is obtained in the obtained endothermic curve is determined.
[0098] (Toner manufacturing method) Next, a method for producing the toner according to the present embodiment will be described. The toner according to the exemplary embodiment is obtained by producing toner particles and then externally adding an external additive to the toner particles.
[0099] The toner particles may be produced by any of a dry production method (e.g., a kneading and pulverizing method, etc.) and a wet production method (e.g., an aggregation-coalescence method, a suspension polymerization method, a dissolution suspension method, etc.). The method for producing the toner particles is not particularly limited, and a well-known production method is adopted. Among these, from the viewpoint of ensuring that the net intensity of Mg element in the toner particles is 0.02 or more and 0.15 or less, and that the net intensity of Cl element is 0.02 or more and 0.60 or less, and from the viewpoint of ensuring that the domains of the crystalline resin satisfy the above conditions, it is preferable to obtain the toner particles by the aggregation and coalescence method.
[0100] Specifically, for example, when toner particles are produced by the aggregation and coalescence method, A step of preparing an amorphous resin particle dispersion liquid in which amorphous resin particles are dispersed, and a crystalline resin particle dispersion liquid in which crystalline resin particles are dispersed (a resin particle dispersion preparation step); a step of aggregating amorphous resin particles (and, as necessary, a colorant, a release agent, etc.) in an amorphous resin particle dispersion (in a dispersion obtained by mixing, as necessary, a colorant dispersion and a release agent dispersion) to form first aggregated particles (first aggregated particle forming step); a step of forming second aggregated particles by repeating an operation of mixing the aggregated particle dispersion with an amorphous resin particle dispersion and a crystalline resin particle dispersion (or mixing the aggregated particle dispersion with a mixed liquid of an amorphous resin particle dispersion and a crystalline resin particle dispersion) two or more times to further adhere the amorphous resin particles and the crystalline resin particles to the surfaces of the first aggregated particles (second aggregated particle step); a step of mixing the aggregated particle dispersion liquid with an amorphous resin particle dispersion liquid after obtaining the aggregated particle dispersion liquid in which the second aggregated particles are dispersed, and aggregating the second aggregated particles so that the amorphous resin particles are attached to the surfaces of the second aggregated particles to form third aggregated particles (third aggregated particle step); a step of heating the aggregated particle dispersion liquid in which the third aggregated particles are dispersed to fuse and coalesce the aggregated particles, and then sequentially performing rapid cooling, reheating, and slow cooling to form toner particles before surface treatment (fusion and coalescence step); a step of surface-treating the toner particles before the surface treatment with a solution containing a Mg element source and a solution containing a Cl element source (surface treatment step); The toner particles are produced through the above steps.
[0101] Each step will be described in detail below. In the following description, a method for obtaining toner particles containing a colorant and a release agent will be described, but the colorant and the release agent are used as necessary. Of course, additives other than the colorant and the release agent may be used.
[0102] -Resin particle dispersion preparation process- First, in addition to each resin particle dispersion liquid (amorphous resin particle dispersion liquid and crystalline resin particle dispersion liquid) in which each resin particle that will become the binder resin is dispersed, for example, a colorant particle dispersion liquid in which colorant particles are dispersed and a release agent particle dispersion liquid in which release agent particles are dispersed are prepared.
[0103] Here, the resin particle dispersion liquid is prepared, for example, by dispersing resin particles in a dispersion medium with the aid of a surfactant.
[0104] The dispersion medium used in the resin particle dispersion liquid is, for example, an aqueous medium. Examples of the aqueous medium include water such as distilled water and ion-exchanged water, alcohols, etc. These may be used alone or in combination of two or more kinds.
[0105] Examples of the surfactant include anionic surfactants such as sulfate salts, sulfonates, phosphates, and soaps; cationic surfactants such as amine salts and quaternary ammonium salts; and nonionic surfactants such as polyethylene glycols, alkylphenol ethylene oxide adducts, and polyhydric alcohols. Among these, anionic surfactants and cationic surfactants are particularly preferred. The nonionic surfactants may be used in combination with anionic surfactants or cationic surfactants. The surfactant may be used alone or in combination of two or more kinds.
[0106] In the resin particle dispersion, examples of the method for dispersing the resin particles in the dispersion medium include general dispersion methods using, for example, a rotary shear type homogenizer, a ball mill having a media, a sand mill, a dyno mill, etc. Depending on the type of resin particles, the resin particles may be dispersed in the resin particle dispersion using, for example, a phase inversion emulsification method. The phase inversion emulsification method is a method in which the resin to be dispersed is dissolved in a hydrophobic organic solvent in which the resin is soluble, a base is added to the organic continuous phase (O phase) to neutralize it, and then an aqueous medium (W phase) is added to effect conversion of the resin from W / O to O / W (so-called phase inversion), resulting in a discontinuous phase, and the resin is dispersed in particulate form in the aqueous medium.
[0107] The volume average particle size of the resin particles dispersed in the resin particle dispersion is, for example, preferably from 0.01 μm to 1 μm, more preferably from 0.08 μm to 0.8 μm, and even more preferably from 0.1 μm to 0.6 μm. The volume average particle size of the resin particles is measured by using a particle size distribution obtained by measurement using a laser diffraction particle size distribution measuring device (e.g., LA-700 manufactured by Horiba, Ltd.), subtracting the cumulative distribution from the small particle size side for the volume of the divided particle size range (channel), and measuring the particle size at which the cumulative distribution is 50% of all particles as the volume average particle size D50v. The volume average particle sizes of particles in other dispersions are also measured in the same manner.
[0108] The content of the resin particles in the resin particle dispersion is, for example, preferably from 5% by mass to 50% by mass, and more preferably from 10% by mass to 40% by mass.
[0109] In addition, for example, a colorant particle dispersion and a release agent particle dispersion are also prepared in the same manner as the resin particle dispersion. That is, the volume average particle size, dispersion medium, dispersion method, and particle content of the particles in the resin particle dispersion are the same for the colorant particles dispersed in the colorant particle dispersion and the release agent particles dispersed in the release agent particle dispersion.
[0110] -First agglomerated particle formation process- Next, the colorant particle dispersion and the release agent particle dispersion are mixed together with the amorphous resin particle dispersion. Then, in the mixed dispersion, the amorphous resin particles, the colorant particles, and the release agent particles are hetero-aggregated to form first aggregate particles containing the amorphous resin particles, the colorant particles, and the release agent particles and having a diameter close to that of the target toner particles.
[0111] Specifically, for example, an aggregating agent is added to the mixed dispersion, the pH of the mixed dispersion is adjusted to be acidic (e.g., pH 2 or more and 5 or less), a dispersion stabilizer is added as necessary, and then the mixed dispersion is heated to a temperature of the glass transition temperature of the resin particles (specifically, for example, a temperature of the glass transition temperature of the resin particles -30°C or more and the glass transition temperature -10°C or less), and the particles dispersed in the mixed dispersion are aggregated to form first aggregated particles. In the first aggregate particle formation step, for example, the above-mentioned aggregating agent may be added to the mixed dispersion at room temperature (e.g., 25°C) while stirring the mixed dispersion with a rotary shear homogenizer, the pH of the mixed dispersion may be adjusted to an acidic state (e.g., a pH of 2 or more and 5 or less), and a dispersion stabilizer may be added as necessary, followed by the above-mentioned heating.
[0112] Examples of the flocculant include a surfactant having a polarity opposite to that of the surfactant used as the dispersant added to the mixed dispersion, an inorganic metal salt, and a divalent or higher metal complex. In particular, when a metal complex is used as the flocculant, the amount of surfactant used is reduced and the charging characteristics are improved. If necessary, an additive that forms a complex or a similar bond with the metal ions of the flocculant may be used, and a chelating agent is preferably used as this additive.
[0113] Examples of inorganic metal salts include metal salts such as calcium chloride, calcium nitrate, barium chloride, magnesium chloride, zinc chloride, aluminum chloride, and aluminum sulfate, as well as inorganic metal salt polymers such as polyaluminum chloride, polyaluminum hydroxide, and calcium polysulfide. The chelating agent may be a water-soluble chelating agent, such as oxycarboxylic acid (e.g., tartaric acid, citric acid, gluconic acid, etc.), iminodiacetic acid (IDA), nitrilotriacetic acid (NTA), ethylenediaminetetraacetic acid (EDTA), etc. The amount of the chelating agent added is, for example, preferably 0.01 parts by mass or more and 5.0 parts by mass or less, and more preferably 0.1 parts by mass or more and less than 3.0 parts by mass, relative to 100 parts by mass of the amorphous resin particles.
[0114] -Second agglomerated particle formation process- Next, after obtaining an aggregated particle dispersion in which the first aggregated particles are dispersed, the aggregated particle dispersion is mixed with an amorphous resin particle dispersion and a crystalline resin particle dispersion, or the aggregated particle dispersion may be mixed with a mixture of the amorphous resin particle dispersion and the crystalline resin particle dispersion.
[0115] Then, in the dispersion liquid in which the first aggregated particles, the amorphous resin particles, and the crystalline resin particles are dispersed, the amorphous resin particles and the crystalline resin particles are aggregated on the surfaces of the first aggregated particles. Specifically, for example, in the first aggregated particle forming step, when the first aggregated particles reach a target particle size, a non-crystalline resin particle dispersion and a crystalline resin particle dispersion are added to the second aggregated particle dispersion, and the dispersion is heated at a temperature equal to or lower than the glass transition temperature of the non-crystalline resin particles. This aggregation operation is repeated two or more times to form the second aggregated particles.
[0116] -Third agglomerated particle formation process- After obtaining the aggregated particle dispersion in which the second aggregated particles are dispersed, the aggregated particle dispersion and the amorphous resin particle dispersion are mixed together.
[0117] Then, in the dispersion liquid in which the second aggregated particles and the amorphous resin particles are dispersed, the amorphous resin particles are aggregated on the surfaces of the second aggregated particles. Specifically, for example, in the second aggregate particle formation step, when the second aggregate particles reach a target particle size, a dispersion of amorphous resin particles is added to a dispersion of second aggregate particles, and this dispersion is heated at or below the glass transition temperature of the amorphous resin particles. The pH of the dispersion is then adjusted to stop the progression of aggregation.
[0118] -Fusion / unification process- Next, the third aggregate particle dispersion liquid in which the third aggregate particles are dispersed is heated, for example, to a temperature equal to or higher than the glass transition temperature of the amorphous resin particles (for example, a temperature 10 to 30° C. higher than the glass transition temperature of the amorphous resin particles) to fuse and coalesce the aggregated particles, thereby forming toner particles before surface treatment.
[0119] Here, after fusing and coalescing the aggregated particles by heating, it is advisable to cool them, for example, to 30°C at a cooling rate of 5°C / min to 40°C / min. By performing the second aggregation step and then rapid cooling, the toner particle surface is more likely to shrink, making it more likely to crack. It is presumed that by performing the rapid cooling step under the above conditions, cracks are more likely to form from the inside of the toner particle toward the toner surface. Next, the temperature is raised again at 0.1°C / min to 2°C / min, and the temperature is maintained at the melting temperature of the crystalline resin minus 5°C or higher for 10 minutes or more. After that, the temperature is gradually cooled at 0.1°C / min to 1°C / min, whereby the domains of the crystalline resin grow in the crack direction, from the inside of the toner particle toward the surface, and the domains of the crystalline resin satisfy the above conditions. In addition, for example, when the temperature is increased again, if the temperature is increased to the melting temperature of the release agent or higher, the domain of the release agent is likely to grow to the vicinity of the surface of the toner particles. Therefore, the heating temperature after the temperature is increased again is preferably set to a temperature higher than the melting temperature of the crystalline resin minus 5°C or higher and lower than the melting temperature of the release agent.
[0120] Through the above steps, toner particles before surface treatment are obtained. In addition to the above-mentioned aggregation-coalescence method, when the above-mentioned rapid cooling, reheating and slow cooling are carried out after the preparation of the toner particles, the domains of the crystalline resin tend to satisfy the above-mentioned conditions.
[0121] After the fusion and coalescence process, the toner particles formed in the solution before surface treatment are subjected to a known washing process and solid-liquid separation process. In the washing step, it is preferable to carry out sufficient replacement washing with ion-exchanged water from the viewpoint of electrostatic chargeability. In addition, the solid-liquid separation step is not particularly limited, but it is preferable to carry out suction filtration, pressure filtration, or the like from the viewpoint of productivity.
[0122] -Surface treatment process- Next, the toner particles before the surface treatment are surface-treated with a solution containing a source of Mg element and a solution containing a source of Cl element. As a method of the surface treatment, for example, a method in which a solution containing a source of Mg element and a solution containing a source of Cl element are added to toner particles before the surface treatment, and then the toner particles are dried to obtain toner particles in a dry state can be mentioned.
[0123] As the solution containing a source of Mg element, an aqueous solution obtained by dissolving the above-mentioned source of Mg element in water can be used. The concentration of the Mg element source in the solution containing the Mg element source is preferably 5 mass % or more and 30 mass % or less, more preferably 7 mass % or more and 20 mass % or less, and even more preferably 10 mass % or more and 15 mass % or less, based on the entire solution. The amount of the solution containing the Mg element source to be added to the toner particles before the surface treatment is not particularly limited, but is preferably 1 mass % or more and 12 mass % or less, more preferably 2 mass % or more and 10 mass % or less, and even more preferably 3 mass % or more and 8 mass % or less, based on the toner particles before the surface treatment.
[0124] As the solution containing a Cl element source, an aqueous solution obtained by dissolving the above-mentioned Cl element source in water can be used. The concentration of the Cl element source in the solution containing the Cl element source is preferably 5 mass % or more and 35 mass % or less, more preferably 10 mass % or more and 30 mass % or less, and even more preferably 15 mass % or more and 25 mass % or less, based on the entire solution. The amount of the solution containing the Cl element source to be added to the toner particles before the surface treatment is not particularly limited, but is preferably 1 mass % or more and 30 mass % or less, more preferably 2 mass % or more and 25 mass % or less, and even more preferably 3 mass % or more and 20 mass % or less, relative to the toner particles before the surface treatment.
[0125] The method for drying the toner particles is not particularly limited, but from the viewpoint of productivity, freeze drying, air flow drying, fluidized bed drying, vibration type fluidized bed drying, etc. are preferably used.
[0126] The toner according to the present embodiment is produced, for example, by adding an external additive to the obtained toner particles in a dry state and mixing them. The mixing may be performed, for example, by using a V blender, a Henschel mixer, a Loedige mixer, etc. Furthermore, if necessary, coarse particles of the toner may be removed using a vibration sieve, an air sieve, etc.
[0127] <Electrostatic image developer> The electrostatic image developer according to this embodiment contains at least the toner according to this embodiment. The electrostatic image developer according to the present embodiment may be a one-component developer containing only the toner according to the present embodiment, or may be a two-component developer in which the toner is mixed with a carrier.
[0128] The carrier is not particularly limited, and may be any known carrier, such as a coated carrier in which the surface of a core material made of magnetic powder is coated with a coating resin, a magnetic powder dispersion type carrier in which magnetic powder is dispersed and mixed in a matrix resin, or a resin impregnated type carrier in which porous magnetic powder is impregnated with a resin. The magnetic powder dispersion type carrier and the resin impregnated type carrier may be a carrier in which the constituent particles of the carrier are used as a core material and are coated with a coating resin.
[0129] Examples of the magnetic powder include magnetic metals such as iron, nickel, and cobalt, and magnetic oxides such as ferrite and magnetite.
[0130] Examples of the coating resin and matrix resin include polyethylene, polypropylene, polystyrene, polyvinyl acetate, polyvinyl alcohol, polyvinyl butyral, polyvinyl chloride, polyvinyl ether, polyvinyl ketone, vinyl chloride-vinyl acetate copolymer, styrene-acrylic acid ester copolymer, straight silicone resin containing an organosiloxane bond or a modified product thereof, fluororesin, polyester, polycarbonate, phenolic resin, and epoxy resin. The coating resin and the matrix resin may contain other additives such as conductive particles. Examples of the conductive particles include particles of metals such as gold, silver, and copper, carbon black, titanium oxide, zinc oxide, tin oxide, barium sulfate, aluminum borate, and potassium titanate.
[0131] Here, the method of coating the surface of the core material with the coating resin includes a method of coating with a solution for forming a coating layer in which the coating resin and, if necessary, various additives are dissolved in an appropriate solvent, etc. The solvent is not particularly limited and may be selected taking into consideration the coating resin to be used, the suitability for application, etc. Specific resin coating methods include an immersion method in which the core material is immersed in a solution for forming a coating layer, a spray method in which the solution for forming a coating layer is sprayed onto the surface of the core material, a fluidized bed method in which the solution for forming a coating layer is sprayed onto the core material while it is suspended in flowing air, and a kneader coater method in which the core material of a carrier and the solution for forming a coating layer are mixed in a kneader coater and the solvent is removed.
[0132] In the two-component developer, the mixture ratio (mass ratio) of the toner and the carrier is preferably toner:carrier=1:100 to 30:100, and more preferably 3:100 to 20:100.
[0133] <Image forming device / image forming method> An image forming apparatus / image forming method according to this embodiment will be described. The image forming apparatus according to the present embodiment includes an image carrier, a charging means for charging the surface of the image carrier, an electrostatic image forming means for forming an electrostatic image on the surface of the charged image carrier, a developing means for containing an electrostatic image developer and developing the electrostatic image formed on the surface of the image carrier as a toner image with the electrostatic image developer, a transfer means for transferring the toner image formed on the surface of the image carrier to the surface of a recording medium, and a fixing means for fixing the toner image transferred to the surface of the recording medium. The electrostatic image developer according to the present embodiment is used as the electrostatic image developer.
[0134] In the image forming apparatus according to this embodiment, an image forming method (the image forming method according to this embodiment) is carried out, which includes a charging step of charging the surface of an image carrier, an electrostatic image forming step of forming an electrostatic image on the surface of the charged image carrier, a developing step of developing the electrostatic image formed on the surface of the image carrier as a toner image using the electrostatic image developer according to this embodiment, a transfer step of transferring the toner image formed on the surface of the image carrier to the surface of a recording medium, and a fixing step of fixing the toner image transferred to the surface of the recording medium.
[0135] The image forming apparatus according to the present embodiment may be any of known image forming apparatuses, such as a direct transfer type apparatus in which a toner image formed on the surface of an image holder is directly transferred to a recording medium; an intermediate transfer type apparatus in which a toner image formed on the surface of an image holder is primarily transferred to the surface of an intermediate transfer body, and the toner image transferred to the surface of the intermediate transfer body is then secondarily transferred to the surface of a recording medium; an apparatus equipped with a cleaning means for cleaning the surface of the image holder before charging after the transfer of the toner image; and an apparatus equipped with a discharging means for irradiating the surface of the image holder with discharging light to discharge it before charging after the transfer of the toner image. In the case of an intermediate transfer type device, the transfer means has, for example, an intermediate transfer body onto whose surface a toner image is transferred, a primary transfer means which primarily transfers the toner image formed on the surface of the image carrier onto the surface of the intermediate transfer body, and a secondary transfer means which secondarily transfers the toner image transferred onto the surface of the intermediate transfer body onto the surface of a recording medium.
[0136] In the image forming apparatus according to the present embodiment, for example, a portion including the developing means may have a cartridge structure (process cartridge) that is detachably attached to the image forming apparatus. As the process cartridge, for example, a process cartridge including a developing means that contains the electrostatic image developer according to the present embodiment is preferably used.
[0137] An example of an image forming apparatus according to the present embodiment will be described below, but the present invention is not limited to this. Note that only the main parts shown in the drawings will be described, and descriptions of the rest will be omitted.
[0138] FIG. 1 is a schematic diagram showing the configuration of an image forming apparatus according to the present embodiment. The image forming apparatus shown in Fig. 1 includes first to fourth electrophotographic image forming units 10Y, 10M, 10C, and 10K (image forming means) that output images of each color of yellow (Y), magenta (M), cyan (C), and black (K) based on color-separated image data. These image forming units (hereinafter sometimes simply referred to as "units") 10Y, 10M, 10C, and 10K are arranged in parallel at predetermined distances from each other in the horizontal direction. These units 10Y, 10M, 10C, and 10K may be process cartridges that are detachable from the image forming apparatus.
[0139] Above each of the units 10Y, 10M, 10C, and 10K in the drawing, an intermediate transfer belt 20 is provided as an intermediate transfer body extending through each unit. The intermediate transfer belt 20 is provided wound around a drive roll 22 and a support roll 24 that are arranged from left to right in the drawing at a distance from each other and contact the inner surface of the intermediate transfer belt 20, and is adapted to run in a direction from the first unit 10Y to the fourth unit 10K. Note that a force is applied to the support roll 24 in a direction away from the drive roll 22 by a spring or the like (not shown), and tension is applied to the intermediate transfer belt 20 wound around them. In addition, an intermediate transfer body cleaning device 30 is provided on the image carrier side of the intermediate transfer belt 20, facing the drive roll 22. Further, the developing devices (developing means) 4Y, 4M, 4C, and 4K of the units 10Y, 10M, 10C, and 10K are supplied with toner including four colors of toner, yellow, magenta, cyan, and black, contained in toner cartridges 8Y, 8M, 8C, and 8K, respectively.
[0140] Since the first to fourth units 10Y, 10M, 10C, and 10K have the same configuration, the first unit 10Y that forms a yellow image and is disposed upstream in the direction in which the intermediate transfer belt travels will be described here as a representative example. Note that by assigning reference numerals of magenta (M), cyan (C), and black (K) instead of yellow (Y) to parts equivalent to those of the first unit 10Y, descriptions of the second to fourth units 10M, 10C, and 10K will be omitted.
[0141] The first unit 10Y has a photoconductor 1Y that acts as an image carrier. Around the photoconductor 1Y, a charging roll (an example of a charging means) 2Y that charges the surface of the photoconductor 1Y to a predetermined potential, an exposure device (an example of an electrostatic image forming means) 3 that exposes the charged surface to a laser beam 3Y based on a color-separated image signal to form an electrostatic image, a developing device (an example of a developing means) 4Y that supplies charged toner to the electrostatic image to develop it, a primary transfer roll 5Y (an example of a primary transfer means) that transfers the developed toner image onto an intermediate transfer belt 20, and a photoconductor cleaning device (an example of a cleaning means) 6Y that removes toner remaining on the surface of the photoconductor 1Y after the primary transfer are arranged in this order. The primary transfer roll 5Y is disposed inside the intermediate transfer belt 20 and is provided at a position facing the photoconductor 1Y. Furthermore, a bias power supply (not shown) that applies a primary transfer bias is connected to each of the primary transfer rolls 5Y, 5M, 5C, and 5K. Each bias power supply varies the transfer bias applied to each primary transfer roll under the control of a control unit (not shown).
[0142] Hereinafter, an operation of forming a yellow image in first unit 10Y will be described. First, prior to operation, the surface of the photoconductor 1Y is charged to a potential of −600V to −800V by the charging roll 2Y. The photoconductor 1Y has a conductivity (for example, a volume resistivity at 20° C. of 1×10 -6 The photosensitive layer is formed by laminating a photosensitive layer on a substrate having a resistivity of Ωcm or less. This photosensitive layer is usually highly resistive (the resistance of ordinary resins), but when irradiated with a laser beam 3Y, the resistivity of the portion irradiated with the laser beam changes. A laser beam 3Y is output to the charged surface of the photoreceptor 1Y via an exposure device 3 in accordance with image data for yellow sent from a control unit (not shown). The laser beam 3Y is irradiated onto the photosensitive layer on the surface of the photoreceptor 1Y, and an electrostatic charge image of a yellow image pattern is formed on the surface of the photoreceptor 1Y.
[0143] An electrostatic image is an image formed on the surface of the photoconductor 1Y by electrostatic charging. The laser beam 3Y reduces the resistivity of the irradiated parts of the photosensitive layer, causing the charged charges on the surface of the photoconductor 1Y to flow, while the charges remain in the parts not irradiated by the laser beam 3Y. This is a so-called negative latent image. The electrostatic image formed on the photoconductor 1Y is rotated to a predetermined developing position as the photoconductor 1Y travels. Then, at this developing position, the electrostatic image on the photoconductor 1Y is made visible as a toner image (developed image) by the developing device 4Y.
[0144] The developing device 4Y contains an electrostatic image developer including at least yellow toner and a carrier, for example. The yellow toner is triboelectrically charged by being stirred inside the developing device 4Y, and is held on a developer roll (an example of a developer holder) with a charge of the same polarity (negative polarity) as the charge on the photoconductor 1Y. As the surface of the photoconductor 1Y passes through the developing device 4Y, the yellow toner electrostatically adheres to the discharged latent image portion on the surface of the photoconductor 1Y, and the latent image is developed with the yellow toner. The photoconductor 1Y on which the yellow toner image has been formed continues to travel at a predetermined speed, and the toner image developed on the photoconductor 1Y is transported to a predetermined primary transfer position.
[0145] When the yellow toner image on the photoreceptor 1Y is transported to the primary transfer, a primary transfer bias is applied to the primary transfer roll 5Y, and an electrostatic force from the photoreceptor 1Y toward the primary transfer roll 5Y acts on the toner image, and the toner image on the photoreceptor 1Y is transferred onto the intermediate transfer belt 20. The transfer bias applied at this time has a polarity (+) opposite to the polarity (-) of the toner, and in the first unit 10Y, for example, it is controlled to +10 μA by a control unit (not shown). On the other hand, the toner remaining on the photoconductor 1Y is removed and collected by the photoconductor cleaning device 6Y.
[0146] Further, the primary transfer bias applied to the primary transfer rolls 5M, 5C, and 5K subsequent to the second unit 10M is also controlled in accordance with the first unit. In this manner, the intermediate transfer belt 20 onto which the yellow toner image has been transferred by the first unit 10Y is conveyed successively through the second to fourth units 10M, 10C, and 10K, where the toner images of the respective colors are transferred in a superimposed manner.
[0147] The intermediate transfer belt 20 onto which the four color toner images have been transferred in multiple layers through the first to fourth units reaches a secondary transfer section that is composed of the intermediate transfer belt 20, a support roll 24 that contacts the inner surface of the intermediate transfer belt, and a secondary transfer roll (an example of a secondary transfer means) 26 arranged on the image bearing surface side of the intermediate transfer belt 20. Meanwhile, a recording paper (an example of a recording medium) P is fed at a predetermined timing into the gap between the secondary transfer roll 26 and the intermediate transfer belt 20 via a supply mechanism, and a secondary transfer bias is applied to the support roll 24. The transfer bias applied at this time has a (-) polarity that is the same as the (-) polarity of the toner, and an electrostatic force from the intermediate transfer belt 20 toward the recording paper P acts on the toner image, so that the toner image on the intermediate transfer belt 20 is transferred onto the recording paper P. The secondary transfer bias at this time is determined according to the resistance detected by a resistance detection means (not shown) that detects the resistance of the secondary transfer section, and is voltage-controlled.
[0148] Thereafter, the recording paper P is sent to a pressure contact portion (nip portion) of a pair of fixing rolls in a fixing device (one example of a fixing means) 28, where the toner image is fixed onto the recording paper P, forming a fixed image.
[0149] The recording paper P onto which the toner image is transferred can be, for example, plain paper used in electrophotographic copying machines, printers, etc. In addition to the recording paper P, other examples of the recording medium include overhead projector sheets, etc. To further improve the smoothness of the image surface after fixing, it is preferable that the surface of the recording paper P is also smooth. For example, coated paper in which the surface of ordinary paper is coated with resin or the like, art paper for printing, or the like is preferably used.
[0150] After the color image has been fixed, the recording paper P is conveyed toward the discharge section, and the series of color image forming operations is completed.
[0151] <Process cartridge / toner cartridge> The process cartridge according to this embodiment will be described. The process cartridge according to this embodiment is a process cartridge that contains the electrostatic image developer according to this embodiment, is equipped with a developing means that develops an electrostatic image formed on the surface of an image carrier using the electrostatic image developer into a toner image, and is detachably attached to an image forming apparatus.
[0152] In addition, the process cartridge according to this embodiment is not limited to the above configuration, and may be configured to include a developing device and, as necessary, at least one other means selected from an image carrier, a charging means, an electrostatic image forming means, and a transfer means.
[0153] An example of a process cartridge according to the present embodiment will be described below, but the present invention is not limited to this example. Note that only the main parts shown in the drawings will be described, and descriptions of the rest will be omitted.
[0154] FIG. 2 is a schematic diagram showing the process cartridge according to the present embodiment. The process cartridge 200 shown in FIG. 2 is configured by, for example, a housing 117 having a mounting rail 116 and an opening 118 for exposure, and integrally combining and holding a photoconductor 107 (an example of an image carrier), a charging roll 108 (an example of a charging means) provided around the photoconductor 107, a developing device 111 (an example of a developing means), and a photoconductor cleaning device 113 (an example of a cleaning means), which are assembled into a cartridge. In FIG. 2, 109 denotes an exposure device (an example of an electrostatic image forming means), 112 denotes a transfer device (an example of a transfer means), 115 denotes a fixing device (an example of a fixing means), and 300 denotes recording paper (an example of a recording medium).
[0155] Next, the toner cartridge according to this embodiment will be described. The toner cartridge according to the present embodiment is a toner cartridge that contains the toner according to the present embodiment and is detachably attached to an image forming apparatus. The toner cartridge contains replenishment toner to be supplied to a developing unit provided in the image forming apparatus.
[0156] 1 is an image forming apparatus having a configuration in which toner cartridges 8Y, 8M, 8C, and 8K can be attached and detached, and the developing devices 4Y, 4M, 4C, and 4K are connected to the toner cartridges corresponding to the respective developing devices (colors) through toner supply pipes (not shown). When the toner contained in the toner cartridge becomes low, the toner cartridge is replaced. EXAMPLES
[0157] Examples will be described below, but the present invention is not limited to these examples. In the following description, unless otherwise specified, all "parts" and "%" are based on mass.
[0158] The present embodiment will be described in more detail below with reference to examples and comparative examples, but the present embodiment is not limited to these examples. Note that "parts" and "%" indicating amounts are based on mass unless otherwise specified.
[0159] <Preparation of amorphous resin particle dispersion> (Preparation of amorphous polyester resin particle dispersion (A1)) Terephthalic acid: 70 parts Fumaric acid: 30 parts Ethylene glycol: 41 parts 1,5-Pentanediol: 48 parts The above materials were charged into a 5-liter flask equipped with a stirrer, a nitrogen inlet tube, a temperature sensor, and a distillation column, and the temperature was raised to 220°C over 1 hour under a nitrogen gas flow, and 1 part of titanium tetraethoxide was added for 100 parts of the above materials. The temperature was raised to 240°C over 0.5 hours while distilling off the generated water, and the dehydration condensation reaction was continued at that temperature for 1 hour, and then the reactant was cooled. In this way, an amorphous polyester resin with a weight average molecular weight of 96,000 and a glass transition temperature of 61°C was synthesized. 40 parts of ethyl acetate and 25 parts of 2-butanol were added to a container equipped with a temperature control means and a nitrogen replacement means to prepare a mixed solvent, and then 100 parts of polyester resin were gradually added and dissolved, and a 10% aqueous ammonia solution (equivalent to 3 times the amount by mole relative to the acid value of the resin) was added and stirred for 30 minutes. Next, the inside of the container was replaced with dry nitrogen, the temperature was kept at 40°C, and 400 parts of ion-exchanged water was added dropwise at a rate of 2 parts / min while stirring the mixture, to emulsify it. After the dropwise addition was completed, the emulsion was returned to 25°C to obtain a resin particle dispersion in which resin particles having a volume average particle size of 190 nm were dispersed. Ion-exchanged water was added to the resin particle dispersion to adjust the solid content to 20%, to obtain amorphous polyester resin particle dispersion (A1).
[0160] <Preparation of Crystalline Polyester Resin Particle Dispersion> (Preparation of Crystalline Polyester Resin Particle Dispersion (B1)) 1,10-Decanedicarboxylic acid: 265 parts 1,6-Hexanediol: 168 parts Dibutyltin oxide (catalyst): 0.3 parts by weight The above components were placed in a heated and dried three-neck flask, and the air in the container was turned into an inert atmosphere with nitrogen gas by a pressure reduction operation, and stirring and refluxing were performed for 5 hours at 180°C by mechanical stirring. After that, the temperature was gradually raised to 230°C under reduced pressure and stirred for 2 hours, and when it became viscous, it was air-cooled to stop the reaction. The molecular weight measurement (polystyrene equivalent) showed that the weight average molecular weight (Mw) of the obtained "crystalline polyester resin 1" was 12700, and the melting temperature was 73°C. 90 parts by mass of the obtained resin, 1.8 parts by mass of ionic surfactant Neogen RK (Dai-ichi Kogyo Seiyaku), and 210 parts by mass of ion-exchanged water were heated to 120°C and thoroughly dispersed with an IKA Ultra-Turrax T50, and then dispersion treatment was performed for 1 hour with a pressure discharge type Gaulin homogenizer to obtain a crystalline polyester resin particle dispersion (B1) with a volume average particle size of 190 nm and a solid content of 20 parts by mass.
[0161] (Preparation of Crystalline Polyester Resin Particle Dispersion (B2)) Terephthalic acid: 250 parts 1,4-Butenediol: 115 parts Dibutyltin oxide (catalyst): 0.2 parts The above components were placed in a heated and dried three-neck flask, and the air in the container was made into an inert atmosphere with nitrogen gas by a decompression operation, and the mixture was stirred and refluxed at 175°C for 4 hours by mechanical stirring. The temperature was then gradually increased to 230°C under reduced pressure and stirred for 2 hours, and when the mixture became viscous, it was air-cooled to stop the reaction. The molecular weight measurement (polystyrene equivalent) showed that the weight average molecular weight (Mw) of the obtained "crystalline polyester resin (B2)" was 13,500, and the melting temperature was 69°C. 90 parts of the obtained resin, 1.5 parts of an ionic surfactant Neogen RK (Dai-ichi Kogyo Seiyaku), and 200 parts of ion-exchanged water were mixed, heated to 120°C, and thoroughly dispersed with an IKA Ultra Turrax T50, and then dispersed for 1 hour with a pressure discharge type Gaulin homogenizer to obtain a crystalline polyester resin particle dispersion (B2) with a volume average particle size of 210 nm and a solid content of 23 parts by mass.
[0162] (Preparation of Crystalline Polyester Resin Particle Dispersion (B3)) 1,8-octanedicarboxylic acid: 250 parts 1,7-heptanediol: 160 parts Dibutyltin oxide (catalyst): 0.2 parts The above components were placed in a heated and dried three-neck flask, and the air in the container was made into an inert atmosphere with nitrogen gas by a decompression operation, and the mixture was stirred and refluxed at 180°C for 5 hours by mechanical stirring. The temperature was then gradually increased to 220°C under reduced pressure and stirred for 3 hours, and when the mixture became viscous, it was air-cooled to stop the reaction. The weight average molecular weight (Mw) of the obtained "crystalline polyester resin (B3)" was 19,500 and the melting temperature was 66°C by molecular weight measurement (polystyrene equivalent). 88 parts of the obtained resin, 2 parts of ionic surfactant Neogen RK (Dai-ichi Kogyo Seiyaku), and 210 parts of ion-exchanged water were mixed, heated to 120°C, and thoroughly dispersed with an IKA Ultra Turrax T50, and then dispersed for 5 hours with a pressure discharge type Gaulin homogenizer to obtain a crystalline polyester resin particle dispersion (B3) with a volume average particle size of 160 nm and a solid content of 28 parts by mass.
[0163] (Preparation of Colorant Particle Dispersion) Carbon black (Cabot, Regal 330): 50 parts Ionic surfactant Neogen RK (Daiichi Kogyo Seiyaku): 5 parts Ion-exchanged water: 193 parts The above components were mixed and treated for 10 minutes at 240 MPa with an Ultimizer (manufactured by Sugino Machine Co., Ltd.) to prepare a colorant particle dispersion (solid content: 20%).
[0164] <Preparation of release agent particle dispersion> (Preparation of release agent particle dispersion (W1)) Ester wax (WEP-5, made by Nippon Oil & Fats Co., Ltd., melting temperature 82°C): 100 parts Anionic surfactant (Daiichi Kogyo Seiyaku Co., Ltd., Neogen RK): 1 part Ion-exchanged water: 350 parts The above materials were mixed and heated to 100°C, dispersed using a homogenizer (IKA Ultra Turrax T50), and then dispersed using a Manton-Gaulin high pressure homogenizer (Gaulin) to obtain a release agent particle dispersion (solid content 20%) in which release agent particles having a volume average particle size of 220 nm were dispersed.
[0165] (Preparation of release agent particle dispersion (W2)) Paraffin wax (HNP-0190, made by Nippon Seiro Co., Ltd., melting temperature 89°C): 100 parts Anionic surfactant (Daiichi Kogyo Seiyaku Co., Ltd., Neogen RK): 1 part Ion-exchanged water: 350 parts The above materials were mixed and heated to 100°C, dispersed using a homogenizer (IKA Ultra Turrax T50), and then dispersed using a Manton-Gaulin high pressure homogenizer (Gaulin) to obtain a release agent particle dispersion (solid content 20%) in which release agent particles having a volume average particle size of 220 nm were dispersed.
[0166] <Example 1> -Production of toner particles- Ion-exchanged water: 215 parts Amorphous polyester resin particle dispersion (A1): 228 parts Release agent dispersion (W1): 10 parts Colorant dispersion: 20 parts Anionic surfactant (Daiichi Kogyo Seiyaku Co., Ltd.: Neogen RK, 20%): 2.8 parts The above components were placed in a 3-liter reaction vessel equipped with a thermometer, pH meter, and stirrer, and the temperature was controlled from the outside with a mantle heater while maintaining the temperature at 30°C and the stirring speed at 150 rpm for 30 minutes. Then, a 0.3N aqueous nitric acid solution was added to adjust the pH to 3.0 in the flocculation process.
[0167] While dispersing with a homogenizer (IKA Japan: Ultra Turrax T50), a PAC aqueous solution in which 0.7 parts of PAC (Oji Paper Co., Ltd.: 30% powder product) was dissolved in 7 parts of ion-exchanged water was added. Then, while stirring, the temperature was raised to 50°C, and the particle size was measured with a Coulter Multisizer II (aperture diameter: 50 μm, Coulter Co.), and the volume average particle size was determined to be 4.5 μm. Then, a mixture of 30 parts of amorphous polyester resin particle dispersion (A1) and 15 parts of crystalline polyester resin particle dispersion (B1) was added. After 30 minutes, a mixture of 30 parts of amorphous polyester resin dispersion (A1) and 15 parts of crystalline polyester resin particle dispersion (B1) was added. This additional addition was repeated a total of four times, that is, the mixed liquid of 30 parts of the amorphous polyester resin particle dispersion (A1) and 15 parts of the crystalline polyester resin particle dispersion (B1) was additionally added four times. Finally, 47 parts of the amorphous polyester resin particle dispersion (A1) was further added to cause the amorphous polyester resin particles to adhere to the surfaces of the aggregated particles.
[0168] Next, 20 parts of 10% NTA (nitrilotriacetic acid) metal salt aqueous solution (Chilest 70: manufactured by Chelest Co., Ltd.) was added, and the pH was adjusted to 9.0 using 1N sodium hydroxide aqueous solution. Thereafter, the temperature was raised to 90°C at a temperature rise rate of 0.05°C / min, and after holding at 90°C for 3 hours, it was cooled to 30°C at a rate of 15°C / min (first cooling). Thereafter, it was heated again at a temperature rise rate of 0.2°C / min to 80°C, which is a temperature not lower than the melting temperature of the crystalline resin by 5°C, and after holding for 30 minutes, it was gradually cooled to 30°C at a rate of 0.5°C / min (second cooling), and then filtered to obtain crude toner particles. This was further redispersed in ion-exchanged water, filtered, and washed repeatedly until the electrical conductivity of the filtrate was 20μS / cm or less. To the washed and filtered crude toner particles, 5 parts of an aqueous solution in which 10 parts of magnesium chloride, a source of Mg element, was dissolved in 80 parts of ion-exchanged water, and 8 parts of an aqueous solution in which 20 parts of sodium chloride, a source of Cl element, was dissolved in 80 parts of ion-exchanged water were added. After that, the mixture was vacuum-dried in an oven at 40° C. for 5 hours to obtain toner particles having a volume average particle size of 6.1 μm.
[0169] - Toner production - 100 parts of the obtained toner particles were mixed with 1.5 parts of hydrophobic silica (RY50, manufactured by Nippon Aerosil Co., Ltd.) using a sample mill at 10,000 rpm for 30 seconds, and then sieved using a vibrating sieve with 45 μm openings to obtain a toner.
[0170] <Example 2> A toner was obtained in the same manner as in Example 1, except that the amount of the aqueous solution in which 10 parts of magnesium chloride were dissolved in 80 parts of ion-exchanged water was changed to 1.5 parts, and the amount of the aqueous solution in which 20 parts of sodium chloride, a Cl element source, were dissolved in 80 parts of ion-exchanged water was changed to 7 parts. <Example 3> A toner was obtained in the same manner as in Example 1, except that the amount of the aqueous solution in which 10 parts of magnesium chloride were dissolved in 80 parts of ion-exchanged water was changed to 7.5 parts, and the amount of the aqueous solution in which 20 parts of sodium chloride, which is a Cl element source, were dissolved in 80 parts of ion-exchanged water was changed to 6 parts. <Example 4> A toner was obtained in the same manner as in Example 1, except that the amount of the aqueous solution in which 10 parts of magnesium chloride were dissolved in 80 parts of ion-exchanged water was changed to 1.5 parts, and the amount of the aqueous solution in which 20 parts of sodium chloride, a Cl element source, were dissolved in 80 parts of ion-exchanged water was changed to 1 part. <Example 5> A toner was obtained in the same manner as in Example 1, except that the amount of the aqueous solution in which 10 parts of magnesium chloride were dissolved in 80 parts of ion-exchanged water was changed to 8 parts, and the amount of the aqueous solution in which 20 parts of sodium chloride, a Cl element source, were dissolved in 80 parts of ion-exchanged water was changed to 27 parts. <Example 6> A toner was obtained in the same manner as in Example 1, except that the amount of the aqueous solution in which 10 parts of magnesium chloride were dissolved in 80 parts of ion-exchanged water was changed to 6 parts, and the amount of the aqueous solution in which 20 parts of sodium chloride, a Cl element source, were dissolved in 80 parts of ion-exchanged water was changed to 5 parts. <Example 7> A toner was obtained in the same manner as in Example 1, except that the amount of the aqueous solution in which 10 parts of magnesium chloride were dissolved in 80 parts of ion-exchanged water was changed to 2 parts, and the amount of the aqueous solution in which 20 parts of sodium chloride, a Cl element source, were dissolved in 80 parts of ion-exchanged water was changed to 7 parts. <Example 8> A toner was obtained in the same manner as in Example 1, except that the amount of the aqueous solution in which 10 parts of magnesium chloride were dissolved in 80 parts of ion-exchanged water was changed to 5 parts, and the amount of the aqueous solution in which 20 parts of sodium chloride, a Cl element source, were dissolved in 80 parts of ion-exchanged water was changed to 29 parts. <Example 9> A toner was obtained in the same manner as in Example 1, except that the amount of the aqueous solution in which 10 parts of magnesium chloride were dissolved in 80 parts of ion-exchanged water was changed to 6 parts, and the amount of the aqueous solution in which 20 parts of sodium chloride, a Cl element source, were dissolved in 80 parts of ion-exchanged water was changed to 1 part. <Example 10> A toner was obtained in the same manner as in Example 1, except that the amount of the aqueous solution in which 10 parts of magnesium chloride were dissolved in 80 parts of ion-exchanged water was changed to 6 parts, and the amount of the aqueous solution in which 20 parts of sodium chloride, a Cl element source, were dissolved in 80 parts of ion-exchanged water was changed to 18 parts. <Example 11> A toner was obtained in the same manner as in Example 1, except that the amount of the aqueous solution in which 10 parts of magnesium chloride were dissolved in 80 parts of ion-exchanged water was changed to 3.5 parts, and the amount of the aqueous solution in which 20 parts of sodium chloride, a Cl element source, were dissolved in 80 parts of ion-exchanged water was changed to 1.2 parts. <Example 12> A toner was obtained in the same manner as in Example 1, except that the amount of the aqueous solution in which 10 parts of magnesium chloride were dissolved in 80 parts of ion-exchanged water was changed to 1 part, and the amount of the aqueous solution in which 20 parts of sodium chloride, a Cl element source, were dissolved in 80 parts of ion-exchanged water was changed to 2 parts. <Example 13> A toner was obtained in the same manner as in Example 1, except that the amount of the aqueous solution in which 10 parts of magnesium chloride were dissolved in 80 parts of ion-exchanged water was changed to 8 parts, and the amount of the aqueous solution in which 20 parts of sodium chloride, a Cl element source, were dissolved in 80 parts of ion-exchanged water was changed to 21 parts.
[0171] <Example 14> A toner was obtained in the same manner as in Example 1, except that the crystalline polyester resin particle dispersion (B2) was used instead of the crystalline polyester resin particle dispersion (B1).
[0172] <Example 15> A toner was obtained in the same manner as in Example 1, except that the crystalline polyester resin particle dispersion (B3) was used instead of the crystalline polyester resin particle dispersion (B1).
[0173] <Example 16> A toner was obtained in the same manner as in Example 1, except that the release agent particle dispersion (W2) was used instead of the release agent particle dispersion (W1).
[0174] <Comparative Example 1> A toner was obtained in the same manner as in Example 1, except that the aqueous solution in which 10 parts of magnesium chloride was dissolved in 80 parts of ion-exchanged water and the aqueous solution in which 20 parts of sodium chloride, which is a Cl element source, was dissolved in 80 parts of ion-exchanged water were not added. <Comparative Example 2> A toner was obtained in the same manner as in Example 1, except that the amount of the aqueous solution in which 10 parts of magnesium chloride were dissolved in 80 parts of ion-exchanged water was changed to 0.3 parts, and the amount of the aqueous solution in which 20 parts of sodium chloride, which is a source of Cl element, were dissolved in 80 parts of ion-exchanged water was changed to 0.5 parts. <Comparative Example 3> A toner was obtained in the same manner as in Example 1, except that the amount of the aqueous solution in which 10 parts of magnesium chloride were dissolved in 80 parts of ion-exchanged water was changed to 10 parts, and the amount of the aqueous solution in which 20 parts of sodium chloride, a Cl element source, were dissolved in 80 parts of ion-exchanged water was changed to 0.5 parts. <Comparative Example 4> A toner was obtained in the same manner as in Example 1, except that the amount of the aqueous solution in which 10 parts of magnesium chloride were dissolved in 80 parts of ion-exchanged water was changed to 2 parts, and the amount of the aqueous solution in which 20 parts of sodium chloride, a Cl element source, were dissolved in 80 parts of ion-exchanged water was changed to 0.5 parts. <Comparative Example 5> A toner was obtained in the same manner as in Example 1, except that the amount of the aqueous solution in which 10 parts of magnesium chloride were dissolved in 80 parts of ion-exchanged water was changed to 12 parts, and the amount of the aqueous solution in which 20 parts of sodium chloride, which is a Cl element source, were dissolved in 80 parts of ion-exchanged water was changed to 28 parts.
[0175] <Evaluation> (Preparation of developer) Using the toners of each example, developers were obtained as follows. After thoroughly stirring 500 parts of spherical magnetite powder particles (volume average particle diameter: 0.55 μm) in a Henschel mixer, 5.0 parts of a titanate coupling agent was added, the mixture was heated to 100° C., and mixed and stirred for 30 minutes to obtain spherical magnetite particles coated with a titanate coupling agent. Next, 6.25 parts of phenol, 9.25 parts of 35% formalin, 500 parts of the magnetite particles, 6.25 parts of 25% ammonia water, and 425 parts of water were mixed and stirred in a four-neck flask. Next, the mixture was reacted at 85°C for 120 minutes while stirring, then cooled to 25°C, 500 parts of water were added, the supernatant liquid was removed, and the precipitate was washed with water. This was dried under reduced pressure at 150°C to 180°C to obtain a carrier with an average particle size of 35μm. Then, the toner of each example and the obtained carrier were placed in a V blender in a ratio of toner:carrier=5:95 (mass ratio), and stirred for 20 minutes to obtain a developer.
[0176] (Low temperature fixability evaluation) A modified image forming device "ApeosPortIV C5575" manufactured by Fuji Xerox Co., Ltd. was prepared, and the developer was placed in the developing device. After leaving the image forming device for one day in an environment with a temperature of 25°C and a relative humidity of 15%, 100 halftone images with an image density of 10% were printed on embossed paper manufactured by Tokai Paper Co., Ltd. under the same environment. The mass of the first sheet and the 100th sheet of embossed paper on which a halftone image was formed was weighed, and the halftone image was rubbed with a Kimwipe (manufactured by Nippon Paper Crecia Co., Ltd.), and then the mass was weighed again. From the mass before and after rubbing, the mass retention rate (mass of the embossed paper on which a halftone image was formed after rubbing ÷ mass of the embossed paper on which a halftone image was formed before rubbing × 100, unit: %) was calculated. In addition, the difference in image density before and after rubbing was visually observed. The mass retention rate and image density difference were classified as follows. Note that up to G3 was considered to be within the acceptable range. G1: The mass retention rate was 99.5% or more on both the 1st and 100th sheets, and no difference in image density was observed before and after rubbing. G2: The mass retention rate was 99.5% or more on both the 1st and 100th sheets, and only a slight difference in image density was observed before and after rubbing. G3: The mass retention rate was 98.0% or more and less than 99.5% for both the 1st and 100th sheets, and a difference in image density before and after rubbing was visible. G4: The mass retention rate was 97.0% or more and less than 98.0% for both the 1st and 100th sheets, and a difference in image density before and after rubbing was visible. G5: The mass retention rate was less than 97.0% for both the 1st and 100th sheets, and a difference in image density before and after rubbing was visible.
[0177] (Halftone image gradation evaluation) The image density of the 100th image printed on the embossed paper on which the halftone image obtained in the low-temperature fixing evaluation was formed was measured using a reflection densitometer X-Rite938 (manufactured by X-Rite Co., Ltd.) The gradation was evaluated from the difference between the obtained image density and the density of the halftone image with the target image density. The evaluation criteria are as follows. Grades up to G3 are considered acceptable. -Evaluation criteria- G1: Image density difference is 0.1 or less G2: Image density difference is more than 0.1 and less than 0.2 G3: Image density difference is more than 0.2 and less than 0.3 G4: Image density difference is more than 0.3 and less than 0.4 G5: Image density difference exceeds 0.4
[0178] The abbreviations used in Table 1 are as follows: DDA: 1,10-decanedicarboxylic acid HDO: 1,6-Hexanediol
[0179] [Table 1]
[0180] From the above results, it can be seen that the toner of this embodiment has low-temperature fixing properties for recording media having an uneven surface, while suppressing the decrease in gradation when a halftone image is formed on a recording medium having an uneven surface.
[0181] <Preparation of amorphous resin> (Preparation of amorphous polyester resin (AA)) Terephthalic acid: 70 parts Fumaric acid: 30 parts Ethylene glycol: 41 parts 1,5-Pentanediol: 48 parts The above materials were charged into a 5-liter flask equipped with a stirrer, nitrogen inlet tube, temperature sensor, and distillation column, and the temperature was raised to 220°C over 1 hour under nitrogen gas flow, and 1 part of titanium tetraethoxide was added for 100 parts of the above materials. The temperature was raised to 240°C over 0.5 hours while distilling off the generated water, and the dehydration condensation reaction was continued at that temperature for 1 hour, after which the reactant was cooled. In this way, an amorphous polyester resin (AA) with a weight average molecular weight of 96,000 and a glass transition temperature of 61°C was synthesized.
[0182] <Preparation of amorphous resin particle dispersion> (Preparation of amorphous polyester resin particle dispersion (AA1)) In a vessel equipped with a temperature control means and a nitrogen substitution means, 40 parts of ethyl acetate and 25 parts of 2-butanol were added to prepare a mixed solvent, and then 100 parts of amorphous polyester resin (AA) were gradually added and dissolved, and a 10% aqueous ammonia solution (equivalent to 3 times the amount by mole relative to the acid value of the resin) was added thereto and stirred for 30 minutes. Next, the inside of the vessel was substituted with dry nitrogen, the temperature was kept at 40°C, and 400 parts of ion-exchanged water was dropped at a rate of 2 parts / min while stirring the mixed liquid, to perform emulsification. After the dropwise addition was completed, the emulsion was returned to 25°C, and a resin particle dispersion in which resin particles with a volume average particle size of 190 nm were dispersed was obtained. Ion-exchanged water was added to the resin particle dispersion to adjust the solid content to 20%, to obtain an amorphous polyester resin particle dispersion (AA1).
[0183] <Preparation of crystalline resin> (Preparation of crystalline polyester resin (BB)) 1,10-Decanedicarboxylic acid: 265 parts 1,6-Hexanediol: 168 parts Dibutyltin oxide (catalyst): 0.3 parts by weight The above ingredients were placed in a heated and dried three-neck flask, and the air in the container was turned into an inert atmosphere with nitrogen gas by reducing the pressure, and the mixture was stirred and refluxed for 5 hours at 180°C using mechanical stirring. The temperature was then gradually increased to 230°C under reduced pressure and stirred for 2 hours, and when the mixture became viscous, it was air-cooled to stop the reaction. Molecular weight measurements (polystyrene equivalent) showed that the weight average molecular weight (Mw) of the resulting "crystalline polyester resin (BB)" was 12,700, and the melting temperature was 73°C.
[0184] <Preparation of Crystalline Polyester Resin Particle Dispersion> (Preparation of Crystalline Polyester Resin Particle Dispersion (BB1)) 90 parts by mass of crystalline polyester resin (BB), 1.8 parts by mass of ionic surfactant Neogen RK (Dai-ichi Kogyo Seiyaku), and 210 parts by mass of ion-exchanged water were heated to 120°C and thoroughly dispersed using an IKA Ultra-Turrax T50. The mixture was then subjected to a dispersion process for 1 hour using a pressure-discharge type Gaulin homogenizer to produce a crystalline polyester resin particle dispersion (BB1) with a volume average particle size of 190 nm and a solid content of 20 parts by mass.
[0185] (Preparation of Colorant Particle Dispersion) Carbon black (Cabot, Regal 330): 50 parts Ionic surfactant Neogen RK (Daiichi Kogyo Seiyaku): 5 parts Ion-exchanged water: 193 parts The above components were mixed and treated for 10 minutes at 240 MPa with an Ultimizer (manufactured by Sugino Machine Co., Ltd.) to prepare a colorant particle dispersion (solid content: 20%).
[0186] <Preparation of release agent particle dispersion> (Preparation of release agent particle dispersion (WW1)) Ester wax (NOF Corp. WEP-5, melting temperature 85°C): 100 parts Anionic surfactant (Daiichi Kogyo Seiyaku Co., Ltd., Neogen RK): 1 part Ion-exchanged water: 350 parts The above materials were mixed and heated to 100°C, dispersed using a homogenizer (IKA Ultra Turrax T50), and then dispersed using a Manton-Gaulin high pressure homogenizer (Gaulin) to obtain a release agent particle dispersion (WW1) (solid content 20%) in which release agent particles having a volume average particle size of 220 nm were dispersed.
[0187] (Preparation of release agent particle dispersion (WW2)) Paraffin wax (HNP-0190, made by Nippon Seiro Co., Ltd., melting temperature 89°C): 100 parts Anionic surfactant (Daiichi Kogyo Seiyaku Co., Ltd., Neogen RK): 1 part Ion-exchanged water: 350 parts The above materials were mixed and heated to 100°C, dispersed using a homogenizer (IKA Ultra Turrax T50), and then dispersed using a Manton-Gaulin high pressure homogenizer (Gaulin) to obtain a release agent particle dispersion (WW2) (solid content 20%) in which release agent particles with a volume average particle size of 220 nm were dispersed.
[0188] (Preparation of release agent particle dispersion (WW3)) Polyethylene wax (HNP-0190, made by Nippon Seiro Co., Ltd., melting temperature 89°C): 100 parts Anionic surfactant (Daiichi Kogyo Seiyaku Co., Ltd., Neogen RK): 1 part Ion-exchanged water: 350 parts The above materials were mixed and heated to 100°C, dispersed using a homogenizer (IKA Ultra Turrax T50), and then dispersed using a Manton-Gaulin high pressure homogenizer (Gaulin) to obtain a release agent particle dispersion (WW3) (solid content 20%) in which release agent particles having a volume average particle size of 220 nm were dispersed.
[0189] <Example 101> -Production of toner particles- Ion-exchanged water: 215 parts Amorphous polyester resin particle dispersion (AA1): 167 parts Crystalline polyester resin particle dispersion (BB1): 27 parts Release agent dispersion (WW1): 40 parts Colorant dispersion: 20 parts Anionic surfactant (Daiichi Kogyo Seiyaku Co., Ltd.: Neogen RK, 20%): 2.8 parts The above components were placed in a 3-liter reaction vessel equipped with a thermometer, pH meter, and stirrer, and the temperature was controlled from the outside with a mantle heater while maintaining the temperature at 30°C and the stirring speed at 150 rpm for 30 minutes. Then, a 0.3N aqueous nitric acid solution was added to adjust the pH to 3.0 in the flocculation process.
[0190] While dispersing with a homogenizer (IKA Japan: Ultra Turrax T50), a PAC aqueous solution in which 0.7 parts of PAC (Oji Paper Co., Ltd.: 30% powder product) was dissolved in 7 parts of ion-exchanged water was added. Then, the temperature was raised to 50°C while stirring to prepare aggregated particles that would become the core (hereinafter also referred to as "core aggregated particles"). Here, the particle size of the core aggregated particles was measured with a Coulter Multisizer II (aperture diameter: 50 μm, Coulter Co., Ltd.), and the volume average particle size (D50v) was 4.9 μm. Then, a mixture of 10 parts of amorphous polyester resin particle dispersion (AA1) and 10 parts of crystalline polyester resin particle dispersion (BB1) was added. After 30 minutes, a mixture of 10 parts of amorphous polyester resin dispersion (AA1) and 10 parts of crystalline polyester resin particle dispersion (BB1) was added. This additional addition was repeated a total of four times, that is, the mixed liquid of 10 parts of the amorphous polyester resin particle dispersion (AA1) and 10 parts of the crystalline polyester resin particle dispersion (BB1) was additionally added four times. Finally, 20 parts of the amorphous polyester resin particle dispersion (AA1) was added to cause the amorphous polyester resin particles to adhere to the surfaces of the aggregated particles.
[0191] Next, 20 parts of 10% NTA (nitrilotriacetic acid) metal salt aqueous solution (Chilest 70: manufactured by Chelest Co., Ltd.) was added, and the pH was adjusted to 9.0 using 1N sodium hydroxide aqueous solution. Thereafter, the temperature was raised to 90°C at a temperature rise rate of 0.05°C / min, and after holding at 90°C for 3 hours, it was cooled to 30°C at a rate of 15°C / min (first cooling). Thereafter, it was heated again at a temperature rise rate of 0.2°C / min to 80°C, which is a temperature not lower than the melting temperature of the crystalline resin by 5°C, and after holding for 30 minutes, it was gradually cooled to 30°C at a rate of 0.5°C / min (second cooling), and then filtered to obtain crude toner particles. This was further redispersed in ion-exchanged water, filtered, and washed repeatedly until the electrical conductivity of the filtrate was 20μS / cm or less. To the washed and filtered crude toner particles, 5 parts of an aqueous solution in which 10 parts of magnesium chloride, a source of Mg element, was dissolved in 80 parts of ion-exchanged water, and 8 parts of an aqueous solution in which 20 parts of sodium chloride, a source of Cl element, was dissolved in 80 parts of ion-exchanged water were added. After that, the mixture was vacuum-dried in an oven at 40°C for 5 hours to obtain toner particles having a volume average particle size (D50v) of 5.8 μm.
[0192] - Toner production - 100 parts of the obtained toner particles were mixed with 1.5 parts of hydrophobic silica (RY50, manufactured by Nippon Aerosil Co., Ltd.) using a sample mill at 10,000 rpm for 30 seconds, and then sieved using a vibrating sieve with 45 μm openings to obtain a toner.
[0193] <Examples 102 to 127> Toner particles were prepared in the same manner as in Example 101, except that when the core aggregated particles reached the particle size shown in Table 2, the amorphous polyester resin particle dispersion (AA1) and the crystalline polyester resin particle dispersion (BB1) were added. However, the cooling rate for the first cooling, the holding temperature after reheating, and the cooling rate for the second cooling were as shown in Table 2. In Example 103, the release agent particle dispersion liquid (WW2) was used instead of the release agent particle dispersion liquid (WW1) used in Example 101 to prepare toner particles. In Example 104, the release agent particle dispersion liquid (WW3) was used instead of the release agent particle dispersion liquid (WW1) used in Example 101 to prepare toner particles.
[0194] <Example 128> 680 parts of amorphous polyester resin (AA), 200 parts of crystalline polyester resin (BB), 40 parts of carbon black (Regal 330), and 80 parts of ester wax (WEP-5) were thoroughly pre-mixed in a Henschel mixer, melt-kneaded in a two-axis roll mill, cooled, and then finely pulverized in a jet mill. The mixture was then classified twice in an air classifier to obtain coarse toner particles. The obtained coarse toner particles were dispersed in ion-exchanged water, and 6 parts of an aqueous solution in which 10 parts of magnesium chloride, a source of Mg element, was dissolved in 80 parts of ion-exchanged water, and 7.4 parts of an aqueous solution in which 20 parts of sodium chloride, a source of Cl element, was dissolved in 80 parts of ion-exchanged water, were added and held for 20 minutes.Then, the mixture was filtered and vacuum-dried in an oven at 40°C for 4 hours to obtain toner particles after surface treatment. The toner particles after the surface treatment were heated to 70°C, which is a temperature 5°C higher than the melting temperature of the crystalline resin, and held for 20 minutes.Then, they were rapidly cooled to 30°C by air cooling at a rate of 15°C / min.Then, they were heated again to 70°C, held for 30 minutes, and gradually cooled to 30°C by air cooling at a rate of 0.5°C / min to obtain toner particles.
[0195] - Toner production - 100 parts of the obtained toner particles were mixed with 1.5 parts of hydrophobic silica (RY50, manufactured by Nippon Aerosil Co., Ltd.) using a sample mill at 10,000 rpm for 30 seconds, and then sieved using a vibrating sieve with 45 μm openings to obtain a toner.
[0196] <Example 129> (Preparation of polyester prepolymer) Bisphenol A-ethylene oxide adduct: 182 parts Bisphenol A-propylene oxide adduct: 21 parts Terephthalic acid: 7 parts Isophthalic acid: 85 parts The above monomers were put into a well-dried three-neck flask that had been purged with N2, and dissolved by heating to 180°C while blowing in N2, and then thoroughly mixed. After adding 0.4 parts of dibutyltin oxide, the temperature in the system was raised to 205°C, and the reaction was allowed to proceed while maintaining that temperature. During the reaction, a small amount of sample was taken to measure the molecular weight, and the reaction progress was controlled by adjusting the temperature and recovering water under a reduced pressure atmosphere, thereby obtaining the desired condensation product. Next, the temperature was lowered to 175°C, and then 8 parts of phthalic anhydride was added, and the reaction was allowed to proceed with stirring for 3 hours under a reduced pressure atmosphere. Dry thoroughly and 2 Into another substituted three-neck flask, 330 parts of the condensate obtained above, 25 parts of isophorone diisocyanate, and 410 parts of ethyl acetate were placed, and this mixture was heated at 70°C for 5 hours while blowing in N2, to obtain a polyester prepolymer having an isocyanate group (hereinafter referred to as "isocyanate-modified polyester prepolymer").
[0197] (Preparation of ketimine compounds) Methyl ethyl ketone: 20 parts Isophoronediamine: 15 parts The above materials were placed in a vessel and stirred under heating at 58° C. to obtain a ketimine compound. (Preparation of black pigment dispersion for oil phase liquid) Carbon black (Cabot, Regal 330): 15 parts Ethyl acetate: 65 parts Solsperse 5000 (Zeneca): 1.2 parts The above components were mixed and dissolved / dispersed using a sand mill to obtain a black pigment dispersion for oil phase liquid. (Preparation of release agent dispersion for oil phase liquid) Ester wax (NOF Corp., WEP-5, melting temperature 85°C): 20 parts Ethyl acetate: 220 parts The above components were cooled to 18° C. and then wet-pulverized using a microbead type disperser (DCP mill) to obtain a dispersion of a release agent for the oil phase liquid.
[0198] (Preparation of oil phase liquid) Black pigment dispersion for oil phase: 32 parts Bentonite (Wako Pure Chemical Industries): 8 parts Ethyl acetate: 58 parts The above ingredients were added and thoroughly mixed. Amorphous polyester resin AA: 112 parts Crystalline polyester resin BB: 28 parts Release agent dispersion for oil phase: 75 parts The mixture was added and thoroughly stirred to prepare an oil phase liquid.
[0199] (Preparation of styrene acrylic resin particle dispersion (1)) Styrene: 75 parts n-Butyl acrylate: 115 parts Methacrylic acid: 75 parts Methacrylic acid polyoxyalkylene sulfate sodium ester (Eleminol RS-30, manufactured by Sanyo Chemical Industries, Ltd.): 8 parts Dodecanethiol: 4 parts The above components were added to a refluxable reaction vessel and thoroughly mixed. 800 parts of ion-exchanged water and 1.2 parts of ammonium persulfate were quickly added to the mixture, and the mixture was dispersed and emulsified with a homogenizer (Ultra Turrax T50, manufactured by IKA) while maintaining the temperature below room temperature to obtain a white emulsion. The temperature in the system was raised to 70°C while stirring and blowing in N2, and emulsion polymerization was continued for 5 hours. Furthermore, 18 parts of a 1% aqueous ammonium persulfate solution was gradually added dropwise, and the mixture was maintained at 70°C for 2 hours to complete the polymerization.
[0200] (Preparation of aqueous phase) Styrene acrylic resin particle dispersion (1): 50 parts 2% aqueous solution of Cellogen BS-H (CMC, Daiichi Kogyo Seiyaku Co., Ltd.): 170 parts Anionic surfactant (Dowfax2A1, manufactured by Dow): 3 parts Ion-exchanged water: 230 parts The above ingredients were thoroughly mixed and stirred to prepare an aqueous phase liquid.
[0201] ·Oil phase liquid: 370 parts Isocyanate-modified polyester prepolymer: 25 parts Ketimine compound: 1.5 parts The above ingredients were placed in a round-bottom stainless steel flask and stirred for 2 minutes with a homogenizer (Ultra Turrax, manufactured by IKA) to prepare a mixed oil phase liquid, after which 900 parts of the aqueous phase liquid was added to the flask and quickly emulsified for approximately 2 minutes with a homogenizer (8,500 rpm). Next, the emulsion was stirred with a paddle stirrer at room temperature or below and at normal pressure (1 atm) for approximately 15 minutes to allow particle formation and the urea modification reaction of the polyester resin to proceed. After that, 2 m of nitrogen was introduced into the suspension. 3 The mixture was stirred at 75° C. for 8 hours while blowing in the mixture at a rate of 1000 ml / h and distilling off the solvent under reduced pressure or removing the solvent under normal pressure, thereby completing the urea modification reaction. After that, it was rapidly cooled to 30°C at 15°C / min, heated again to 90°C and held there for 30 minutes, and then gradually cooled to 30°C at 0.5°C / min. After cooling, the suspension of the produced particles was taken out, thoroughly washed with ion-exchanged water, and separated into solid and liquid by Nutsche suction filtration. Next, the particles were redispersed in ion-exchanged water at 35°C and washed with stirring for 15 minutes. This washing operation was repeated several times, and then the particles were redispersed in ion-exchanged water at 30°C, to which 5.4 parts of an aqueous solution in which 10 parts of magnesium chloride, a source of Mg element, were dissolved in 80 parts of ion-exchanged water, and 8.4 parts of an aqueous solution in which 20 parts of sodium chloride, a source of Cl element, were dissolved in 80 parts of ion-exchanged water, were added, and the mixture was held for 15 minutes. Then, the mixture was separated into solid and liquid by Nutsche suction filtration, and freeze-dried under vacuum to obtain toner particles. 100 parts by mass of the obtained toner particles were mixed and blended with 1.5 parts by mass of hydrophobic silica (manufactured by Nippon Aerosil Co., Ltd., RY50) and 1.0 part by mass of hydrophobic titanium oxide (manufactured by Nippon Aerosil Co., Ltd., T805) using a sample mill at 10,000 rpm for 30 seconds. The mixture was then sieved using a vibrating sieve with 45 μm openings to prepare toner particles.
[0202] <Comparative Example 101: Normal Toner> -Production of toner particles- Ion-exchanged water: 215 parts Amorphous polyester resin particle dispersion (AA1): 127 parts Crystalline polyester resin particle dispersion (BB1): 67 parts Release agent dispersion (WW1): 40 parts Colorant dispersion: 20 parts Anionic surfactant (Daiichi Kogyo Seiyaku Co., Ltd.: Neogen RK, 20%): 2.8 parts The above components were placed in a 3-liter reaction vessel equipped with a thermometer, pH meter, and stirrer, and the temperature was controlled from the outside with a mantle heater while maintaining the temperature at 30°C and the stirring speed at 150 rpm for 30 minutes. Then, a 0.3N aqueous nitric acid solution was added to adjust the pH to 3.0 in the flocculation process.
[0203] While dispersing with a homogenizer (IKA Japan: Ultra Turrax T50), an aqueous PAC solution prepared by dissolving 0.7 parts of PAC (Oji Paper Co., Ltd.: 30% powder product) in 7 parts of ion-exchanged water was added. Then, while stirring, the temperature was raised to 50°C, and the particle size was measured with a Coulter Multisizer II (aperture diameter: 50 μm, Coulter Co.), and the volume average particle size was found to be 4.9 μm. Then, 100 parts of amorphous polyester resin particle dispersion (AA1) was added, and the amorphous polyester resin particles were attached to the surface of the aggregated particles.
[0204] Next, 20 parts of 10% NTA (nitrilotriacetic acid) metal salt aqueous solution (Chilest 70: manufactured by Chelest Co., Ltd.) was added, and the pH was adjusted to 9.0 using 1N sodium hydroxide aqueous solution. Thereafter, the temperature was raised to 90°C at a temperature rise rate of 0.05°C / min, and after holding at 90°C for 3 hours, it was cooled to 30°C at a rate of 15°C / min. Thereafter, the temperature was raised to 80°C, which is a temperature not lower than the melting temperature of the crystalline resin by 5°C, at a temperature rise rate of 0.2°C / min, and after holding for 30 minutes, it was rapidly cooled to 30°C at a rate of 15°C / min, and then filtered to obtain crude toner particles. This was further redispersed in ion-exchanged water, and filtered repeatedly, and washed until the electrical conductivity of the filtrate was 20 μS / cm or less, and then vacuum-dried in an oven at 40°C for 5 hours to obtain toner particles with a volume average particle size of 5.8 μm.
[0205] - Toner production - 100 parts of the obtained toner particles were mixed with 1.5 parts of hydrophobic silica (RY50, manufactured by Nippon Aerosil Co., Ltd.) using a sample mill at 10,000 rpm for 30 seconds, and then sieved using a vibrating sieve with 45 μm openings to obtain a toner.
[0206] <Comparative Example 102> 680 parts of amorphous polyester resin (AA), crystalline polyester resin (BB), 40 parts of carbon black (Regal 330), and 80 parts of ester wax (WEP-5) were thoroughly premixed in a Henschel mixer, and then melt-kneaded in a twin-screw roll mill. The melt-kneaded mixture was then discharged from a twin-screw extruder, and a sheet-like molten mixture was produced using a rolling roll installed near the twin-screw extruder, and cooled at 1°C / min. The sheet-like molten kneaded product was finely pulverized by a jet mill and further classified twice by an air classifier to obtain toner particles.
[0207] <Characteristics> For the toner of each example, the following properties were measured according to the methods already described. Aspect ratio of the domain of the crystalline resin (referred to as aspect ratio AR in the table) The long axis length of the domain of the crystalline resin (L cry (denoted as) The long axis length of the crystalline resin domain relative to the maximum diameter of the toner particle (L cry (denoted as "%)" The angle between the extension of the long axis of the crystalline resin domain and the tangent at the point where the extension touches the toner particle surface (in the table, the angle θ between the long axis and the tangent A (denoted as) The crossing angle of the extension lines of the long axes of the two crystalline resin domains (in the table, the crossing angle θ B (denoted as)
[0208] The shortest distance between the domain of the release agent present on the toner particle and the surface (i.e., the outer edge) of the toner particle (in the table, this is referred to as the shortest distance between the domain and the toner particle surface)
[0209] The ratio (number %) of first toner particles A that satisfy the following conditions to all toner particles Condition (A): The aspect ratio of the domain of the crystalline resin is 5 or more and 40 or less. Condition (B1): The major axis length of the domain of the crystalline resin is 0.5 μm or more and 1.5 μm or less. Condition (C): The angle between an extension line of the long axis of the crystalline resin domain and a tangent line at the point where the extension line touches the surface of the toner particle is 60 degrees or more and 90 degrees or less. Condition (D): The crossing angle between the extensions of the long axes of the two crystalline resin domains is 45 degrees or more and 90 degrees or less.
[0210] The ratio (number %) of the first toner particles A that further satisfies the following condition (E) to the total toner particles Condition (E): A domain of the release agent is present at a depth of 50 nm or more from the surface of the toner particle.
[0211] The ratio (number %) of first toner particles B that satisfy the following conditions to all toner particles Condition (A'): The aspect ratio of the domain of the crystalline resin is 10 or more and 40 or less. Condition (B1'): The major axis length of the domain of the crystalline resin is 0.8 μm or more and 1.5 μm or less. Condition (C'): The angle between an extension line of the long axis of the crystalline resin domain and a tangent line at the point where the extension line touches the surface of the toner particle is 75 degrees or more and 90 degrees or less. Condition (D'): The crossing angle between the extension lines of the long axes of the two crystalline resin domains is 60 degrees or more and 90 degrees or less.
[0212] The ratio (number %) of first toner particles B that further satisfies the following condition (E) to all toner particles Condition (E): A domain of the release agent is present at a depth of 50 nm or more from the surface of the toner particle.
[0213] The ratio (number %) of second toner particles A that satisfy the following conditions to the total toner particles Condition (A): The aspect ratio of the domain of the crystalline resin is 5 or more and 40 or less. Condition (B2): In at least one of the two domains of the crystalline resin, the ratio of the major axis length to the maximum diameter of the toner particle is 10% or more and 30% or less. Condition (C): The angle between an extension line of the long axis of the crystalline resin domain and a tangent line at the point where the extension line touches the surface of the toner particle is 60 degrees or more and 90 degrees or less. Condition (D): The crossing angle between the extensions of the long axes of the two crystalline resin domains is 45 degrees or more and 90 degrees or less.
[0214] The ratio (number %) of second toner particles A that further satisfies the following condition (E) to all toner particles Condition (E): A domain of the release agent is present at a depth of 50 nm or more from the surface of the toner particle.
[0215] The ratio (number %) of second toner particles B that meet the following conditions to the total toner particles Condition (A'): The aspect ratio of the domain of the crystalline resin is 10 or more and 40 or less. Condition (B2'): In at least one of the two domains of the crystalline resin, the ratio of the major axis length to the maximum diameter of the toner particle is 13% or more and 30% or less. Condition (C'): The angle between an extension line of the long axis of the crystalline resin domain and a tangent line at the point where the extension line touches the surface of the toner particle is 75 degrees or more and 90 degrees or less. Condition (D'): The crossing angle between the extension lines of the long axes of the two crystalline resin domains is 60 degrees or more and 90 degrees or less.
[0216] The ratio (number %) of second toner particles B that further satisfies the following condition (E) to all toner particles Condition (E): A domain of the release agent is present at a depth of 50 nm or more from the surface of the toner particle.
[0217] The morphology of domains A and B of the crystalline resin and domains of the release agent of a representative toner particle (hereinafter referred to as a representative toner) is shown in Table 3. Specifically, it is as follows. 100 toner particles of each example are observed, and among the 100 toner particles observed, the toner particle having the crystalline resin domain with the largest angle (condition (C)) between the extension line of the long axis of the crystalline resin domain and the tangent line at the point where the extension line touches the toner particle surface is determined to be the representative toner particle. In the representative toner particle, the crystalline resin domain having the largest angle (condition (C)) between the extension line of the long axis of the crystalline resin domain and the tangent line at the point where the extension line touches the toner particle surface is designated as crystalline resin domain A (see A in Figure 3), and the morphology of crystalline resin domain A is shown in Table 3. In the representative toner particle, the crystalline resin domain having the largest crossing angle (condition (D)) with respect to the extension line of the long axis of the crystalline resin domain A is designated as the crystalline resin domain B (see B in Figure 3), and the shape of the crystalline resin domain B is shown in Table 3. Table 3 shows the crossing angle of the extension lines of the major axes of the crystalline resin domains A and B in the representative toner particles. Table 3 shows the morphology of the domains of the release agent in the representative toner particles.
[0218] In addition, for the toners produced in Examples 101 to 129, the net intensity of Mg element and the net intensity of Cl element were measured in the toner particles by fluorescent X-ray analysis according to the described method. The net intensity of Mg element was 0.02 or more and 0.15 or less, and the net intensity of Cl element was 0.02 or more and 0.60 or less.
[0219] <Evaluation> (Preparation of developer) Using the toners of each example, developers were obtained as follows. After thoroughly stirring 500 parts of spherical magnetite powder particles (volume average particle diameter: 0.55 μm) in a Henschel mixer, 5.0 parts of a titanate coupling agent was added, the mixture was heated to 100° C., and mixed and stirred for 30 minutes to obtain spherical magnetite particles coated with a titanate coupling agent. Next, 6.25 parts of phenol, 9.25 parts of 35% formalin, 500 parts of the magnetite particles, 6.25 parts of 25% ammonia water, and 425 parts of water were mixed and stirred in a four-neck flask. Next, the mixture was reacted at 85°C for 120 minutes while stirring, then cooled to 25°C, 500 parts of water were added, the supernatant liquid was removed, and the precipitate was washed with water. This was dried under reduced pressure at 150°C to 180°C to obtain a carrier with an average particle size of 35μm. Then, the toner of each example and the obtained carrier were placed in a V blender in a ratio of toner:carrier=5:95 (mass ratio), and stirred for 20 minutes to obtain a developer.
[0220] (Uneven gloss) Using the resulting developer, uneven gloss was evaluated as follows. The developers obtained in each of the Examples and Comparative Examples were filled into the developing machine of an image forming apparatus "DocuCentrecolor 400 manufactured by Fuji Xerox Co., Ltd." Using this image forming apparatus, a solid image with an image density of 100% (toner applied amount (TMA) of 10.0 g / m2) was printed on OS coated paper (manufactured by Oji Paper Co., Ltd., product name:) at a process speed of 228 mm / s in an environment of a temperature of 28°C and a humidity of 85% RH, using the Electrophotographic Society Test Chart No. 5-1. 2 After that, a solid image with a density of 100% (toner coverage area (TMA) 14.4 g / m2) was printed on 1,000 sheets. 2 The image was printed on 1,000 sheets of OS coated paper at a fixing temperature of 190°C and a process speed of 90 m / s. The gloss of the black areas of Electrophotography Society Test Chart No. 5-1 when the first sheet of OS coated paper was printed and Electrophotography Society Test Chart No. 5-1 after 1,000 sheets were printed were measured by the following method. The gloss was measured at 60 degrees at five locations using a portable gloss meter (BYK Gardner Micro Trigloss, manufactured by Toyo Seiki Seisakusho Co., Ltd.). The difference between the measured gloss values was calculated and evaluated according to the following criteria. A: The difference between the maximum and minimum gloss values of the output image on 1,001 sheets is less than 3° B: The difference between the maximum and minimum gloss values of the output images on 1,001 sheets is less than 4° C: The difference between the maximum and minimum gloss values of the output images is less than 6° D: The difference between the maximum and minimum gloss values of the output images is less than 8° E: The difference between the maximum and minimum gloss values of the output images is less than 10°. F: 1,001 sheets Maximum-minimum gloss difference of output image is 10° or more
[0221] [Table 2]
[0222] [Table 3]
[0223] [Table 4]
[0224] From the above results, it is understood that the present embodiment suppresses the decrease in uneven gloss of an image that occurs when an image with a large amount of toner is formed, compared to the comparative example. [Explanation of symbols]
[0225] 1Y, 1M, 1C, 1K Photoconductor (an example of an image carrier) 2Y, 2M, 2C, 2K Charging roll (an example of a charging means) 3 Exposure device (an example of an electrostatic image forming means) 3Y, 3M, 3C, 3K laser beam 4Y, 4M, 4C, 4K developing device (an example of developing means) 5Y, 5M, 5C, 5K Primary transfer roll (an example of a primary transfer means) 6Y, 6M, 6C, 6K Photoconductor cleaning device (an example of a cleaning means) 8Y, 8M, 8C, 8K toner cartridges 10Y, 10M, 10C, 10K Image forming units 20 Intermediate transfer belt (an example of an intermediate transfer body) 22 Driving Roll 24 Support roll 26 Secondary transfer roll (an example of a secondary transfer means) 30 Intermediate transfer body cleaning device 107 Photoconductor (an example of an image carrier) 108 Charging roll (an example of charging means) 109 Exposure device (an example of electrostatic image forming means) 111 Developing device (an example of developing means) 112 Transfer device (an example of a transfer means) 113 Photoconductor cleaning device (an example of a cleaning means) 115 Fixing device (an example of fixing means) 116 Mounting Rail 118 Exposure Aperture 117 Cabinet 200 Process Cartridge 300 Recording paper (an example of a recording medium) P Recording paper (an example of a recording medium)
Claims
1. The toner particles include a binder resin. The binder resin contains an amorphous resin and a crystalline resin, In the toner particles, a net intensity of Mg element measured by fluorescent X-ray analysis is 0.02 or more and 0.15 or less, and a net intensity of Cl element measured by fluorescent X-ray analysis is 0.02 or more and 0.60 or less, A toner for developing an electrostatic image, comprising toner particles in which, when a cross section of the toner particle is observed, at least two domains of the crystalline resin satisfy the following condition (A), the following condition (B1), the following condition (C), and the following condition (D): Condition (A): the aspect ratio of the domain of the crystalline resin is 5 or more and 40 or less. Condition (B1): The length of the major axis of the domain of the crystalline resin is 0.5 μm or more and 1.5 μm or less. Condition (C): the angle between an extension line of the long axis of the domain of the crystalline resin and a tangent line at the contact point where the extension line contacts the surface of the toner particle is 60 degrees or more and 90 degrees or less. Condition (D): The crossing angle between the extensions of the long axes of the two domains of the crystalline resin is 45 degrees or more and 90 degrees or less.
2. The toner particles include a binder resin. The binder resin contains an amorphous resin and a crystalline resin, In the toner particles, a net intensity of Mg element measured by fluorescent X-ray analysis is 0.02 or more and 0.15 or less, and a net intensity of Cl element measured by fluorescent X-ray analysis is 0.02 or more and 0.60 or less, A toner for developing electrostatic images, comprising toner particles in which, when a cross section of the toner particle is observed, at least two domains of the crystalline resin satisfy the following condition (A), the following condition (B2), the following condition (C), and the following condition (D): Condition (A): the aspect ratio of the domain of the crystalline resin is 5 or more and 40 or less. Condition (B2): In at least one of the two domains of the crystalline resin, the ratio of the major axis length to the maximum diameter of the toner particle is 10% or more and 30% or less. Condition (C): the angle between an extension line of the long axis of the domain of the crystalline resin and a tangent line at the contact point where the extension line contacts the surface of the toner particle is 60 degrees or more and 90 degrees or less. Condition (D): The crossing angle between the extensions of the long axes of the two domains of the crystalline resin is 45 degrees or more and 90 degrees or less.
3. 3. The toner for developing electrostatic images according to claim 1, wherein the net strength of the Mg element is from 0.03 to 0.12, and the net strength of the Cl element is from 0.03 to 0.
40.
4. 4. The toner for developing electrostatic images according to claim 1, wherein the crystalline resin comprises a polymer of a linear α,ω-aliphatic dicarboxylic acid and a linear α,ω-aliphatic diol.
5. 5. The toner for developing electrostatic images according to claim 4, wherein the polymer of said α,ω-straight-chain aliphatic dicarboxylic acid and said α,ω-straight-chain aliphatic diol includes a polymer of 1,10-decanedicarboxylic acid and 1,6-hexanediol.
6. the toner particles contain a release agent, 6. The toner for developing electrostatic images according to claim 1, wherein the releasing agent is an ester wax.
7. 7. The toner for developing electrostatic images according to claim 6, wherein the toner particles contain a release agent, and when a cross section of the toner particles is observed, a domain of the release agent is present at a depth of 50 nm or more from the surface of the toner particles.
8. The toner for developing electrostatic images according to any one of claims 1 to 7, wherein the content of the toner particles is 40% by number or more based on the total number of toner particles.
9. 9. The toner for developing electrostatic images according to claim 8, wherein the content of the toner particles is 70% or more by number based on the total number of toner particles.
10. 10. An electrostatic image developer comprising the toner for developing electrostatic images according to claim 1.
11. A toner cartridge which contains the toner for developing electrostatic images according to any one of claims 1 to 9 and is detachably mountable to an image forming apparatus.
12. 11. A process cartridge detachably mounted to an image forming apparatus, comprising: a developing unit that contains the electrostatic image developer according to claim 10 and develops an electrostatic image formed on a surface of an image carrier by the electrostatic image developer into a toner image.
13. An image carrier; a charging means for charging the surface of the image carrier; an electrostatic image forming means for forming an electrostatic image on the charged surface of the image carrier; a developing unit that contains the electrostatic image developer according to claim 10 and develops the electrostatic image formed on the surface of the image carrier into a toner image by the electrostatic image developer; a transfer means for transferring the toner image formed on the surface of the image carrier to a surface of a recording medium; a fixing means for fixing the toner image transferred onto the surface of the recording medium; An image forming apparatus comprising:
14. a charging step of charging the surface of the image carrier; an electrostatic image forming step of forming an electrostatic image on the charged surface of the image carrier; a developing step of developing the electrostatic image formed on the surface of the image carrier into a toner image by using the electrostatic image developer according to claim 10; a transfer step of transferring the toner image formed on the surface of the image carrier onto a surface of a recording medium; a fixing step of fixing the toner image transferred onto the surface of the recording medium; The image forming method according to claim 1,
Citation Information
Patent Citations
Method for manufacturing toner for electrostatic charge image development
JP2014164079A
toner
JP2015121576A
Image forming method
JP2015206876A
Toner for electrostatic latent image development and manufacturing method of the same
JP2017090828A
Toner for two-component developer and image forming method using the same
JP2017167440A