Toner for developing electrostatic images and method for producing the same

The toner formulation addresses fogging and white streaks by minimizing coarse particles with specific size and circularity ranges, achieving stable image quality across varying environmental conditions.

JP7593104B2Active Publication Date: 2024-12-03ZEON CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2020218752
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-28
Publication Date
2024-12-03
Estimated Expiration
2040-12-28

AI Technical Summary

Technical Problem

Existing toners cause fogging and white streaks in high temperature and high humidity environments, and white streaks in low temperature and low humidity environments, due to the presence of coarse particles with varying circularity.

Method used

The toner is formulated to minimize coarse particles with relatively low circularity by passing through a 25 μm sieve, with specific ranges for equivalent circle diameter and circularity, and using a controlled air flow during sieving to remove coarse particles effectively.

Benefits of technology

The toner suppresses white streaks and fogging in both high temperature and high humidity, and low temperature and low humidity environments, ensuring high-quality image formation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007593104000003
    Figure 0007593104000003
  • Figure 0007593104000004
    Figure 0007593104000004
  • Figure 0007593104000005
    Figure 0007593104000005
Patent Text Reader

Abstract

To provide a toner for electrostatic charge image development that can prevent white streaks in both a high temperature and high humidity environment and a low temperature and low humidity environment, and can prevent the occurrence of fogging in a high temperature and high humidity environment.SOLUTION: A toner for electrostatic charge image development contains colored resin particles containing a binder resin, colorant, and mold release agent, and an external additive. When the toner is caused to pass through a sieve with an aperture of 25 μm by a wet method, of coarse particles not passing through the sieve, the number of coarse particles A with an equivalent circle diameter measured by a flow type particle image measuring device of 50 μm or more and less than 200 μm and a circularity of 0.20 or more and less than 0.97 is 1000 or more and 20000 or less in 1.0 g of toner, and the number of coarse particles B with an equivalent circle diameter measured by the flow type particle image measuring device of 50 μm or more and less than 200 μm and a circularity of 0.97 or more and 1.00 or less is less than 1000 in 1.0 g of toner.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a toner for developing electrostatic images formed by electrophotography, electrostatic recording, or the like, and a method for producing the toner. [Background technology]

[0002] In electrophotography, an electrostatic image formed on a photoreceptor is developed with toner to become a visible image, and the toner image is transferred to a transfer material such as paper or an OHP as necessary, and then the toner image is fixed on the transfer material to obtain a copy or print. In image forming devices using electrophotography, such as laser printers and copiers, there is a demand for reducing the frequency of replacing toner cartridges. On the other hand, when the toner cartridge is made larger in capacity and has a longer life in order to reduce the frequency of replacing the toner cartridge, if the toner contains coarse particles, the image quality is likely to deteriorate. In addition, since the market for electrophotography technology is rapidly expanding to emerging countries, there is a demand for toner that can obtain high-quality images in various usage environments, such as temperature and humidity.

[0003] For example, Patent Document 1 describes a method for producing toner that contains almost no coarse particles, in which a sieving process for removing coarse particles is performed using two sieves, one above the other, with the opening of the upper sieve set to W. 1 , the opening of the lower sieve is W 2 When W is 1.2 or less, 1 / W 2 Patent Document 1 discloses a method in which the toner obtained by this method is placed on a sieve with a mesh size of 25 μm and sucked from below the sieve, the number of coarse particles remaining on the sieve can be reduced to 200 or less per 2 g of toner, and specifically, the number of coarse particles remaining on the sieve is described as being 11 to 141 per 2 g of toner.

[0004] In Patent Document 2, a method for suppressing clogging of a mesh in a coarse particle removal process for removing coarse particles from a toner is described, in which a wind sieve is used and the flow rate F1 [m 3 / min] and the flow rate of the secondary air supplied from the coarse powder recovery port side F2 [m 3 / min] is in the range of 7≦(F1 / F2)≦ 17. Patent Document 2 describes that when 10 g of the toner obtained by this method was sieved through a 45 μm mesh sieve, the number of coarse particles remaining on the sieve was 2.2 to 11.2. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2008-76873 A [Patent Document 2] JP 2007-79444 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, it has been found that the toners disclosed in Patent Documents 1 and 2 are prone to fog when images are formed in a high-temperature and high-humidity environment. Furthermore, when coarse particles are contained in the toner, a problem occurs in that so-called white streaks appear in the image, which are vertical white streaks. White streaks are likely to occur when an image is formed in a low-temperature, low-humidity environment. An object of the present disclosure is to provide a toner for developing electrostatic images, which can suppress the occurrence of white streaks in both a high-temperature, high-humidity environment and a low-temperature, low-humidity environment, and further suppress the occurrence of fogging in a high-temperature, high-humidity environment, and a method for producing the same. [Means for solving the problem]

[0007] The present inventors have discovered that by reducing the content of coarse particles with a relatively high circularity among the coarse particles contained in the toner, it is possible to form an image in which the occurrence of white streaks is suppressed, even if a specific amount of coarse particles with a relatively low circularity is contained, and further discovered that by containing a specific amount of coarse particles with a relatively low circularity, the occurrence of fogging in a high temperature and high humidity environment can be suppressed.

[0008] The present disclosure relates to a toner for developing electrostatic images, the toner comprising a binder resin, colored resin particles containing a colorant and a release agent, and an external additive, The toner for developing electrostatic images is provided, in which, when the toner is passed through a sieve having an opening of 25 μm by a wet method, among the coarse particles that do not pass through the sieve, the number of coarse particles A having a circle-equivalent diameter of 50 μm or more and less than 200 μm and a circularity of 0.20 or more and less than 0.97 as measured by a flow type particle image measuring device is 1,000 to 20,000 particles per 1.0 g of toner, and the number of coarse particles B having a circle-equivalent diameter of 50 μm or more and less than 200 μm and a circularity of 0.97 or more and less than 1.00 as measured by a flow type particle image measuring device is less than 1,000 particles per 1.0 g of toner.

[0009] In the toner for developing electrostatic images of the present disclosure, the average circularity is preferably 0.98 or more and 1.00 or less.

[0010] The present disclosure relates to a method for producing a toner for developing an electrostatic image according to the present disclosure, comprising the steps of: A step of preparing a suspension in which droplets of a polymerizable monomer composition containing at least a polymerizable monomer, a colorant, and a release agent are dispersed in an aqueous dispersion medium; and subjecting the suspension to a polymerization reaction in the presence of a polymerization initiator to form colored resin particles.

[0011] The above-mentioned manufacturing method of the present disclosure further includes a step of removing a part of coarse particles contained in the particles by supplying the particles containing the colored resin particles to a sieve using an air flow, The sieve includes at least one mesh, and the mesh with the smallest opening among the meshes used in the sieve has an opening of 25 μm or more and 40 μm or less; The air flow is generated by primary air supplied together with the particles containing the colored resin particles, and secondary air supplied from the recovery port side of the coarse particles, and the flow rate F1 [m 3 / min] and the flow rate of the secondary air F2 [m 3 / min] is preferably 18 or more and 50 or less. Effect of the Invention

[0012] According to the present disclosure as described above, by setting the contents of the specific coarse particles A and the specific coarse particles B to the above-mentioned specific amounts, it is possible to provide a toner for developing electrostatic images that can suppress the occurrence of white streaks in both a high-temperature, high-humidity environment and a low-temperature, low-humidity environment and further suppress the occurrence of fogging in a high-temperature, high-humidity environment. [Brief description of the drawings]

[0013] [Figure 1] FIG. 2 is a schematic diagram of an example of a sieving system that can be used in the manufacture of the toner for developing electrostatic images of the present disclosure. [Diagram 2] FIG. 2 is a schematic diagram showing an example of an ejector that can be suitably used in the present disclosure. [Diagram 3] FIG. 1 is a schematic diagram showing a laminated wire mesh in which two wire meshes with different mesh sizes are arranged so that their meridians and latitudes are approximately parallel to each other. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] In this disclosure, the use of "to" in a numerical range means that the numerical values ​​before and after it are included as the lower limit and upper limit. In the present disclosure, (meth)acrylate refers to each of acrylate and methacrylate, (meth)acrylic refers to each of acrylic and methacrylic, and (meth)acryloyl refers to each of acryloyl and methacryloyl.

[0015] I. Toner for developing electrostatic images The toner for developing electrostatic images according to the present disclosure (sometimes simply referred to as "toner" in the present disclosure) is a toner for developing electrostatic images that contains a binder resin, colored resin particles containing a colorant and a release agent, and an external additive, The toner is characterized in that, when the toner is passed through a sieve with an opening of 25 μm by a wet method, among the coarse particles that do not pass through the sieve, the number of coarse particles A having a circle equivalent diameter of 50 μm or more and less than 200 μm and a circularity of 0.20 or more and less than 0.97 as measured by a flow type particle image measuring device is 1,000 to 20,000 particles per 1.0 g of toner, and the number of coarse particles B having a circle equivalent diameter of 50 μm or more and less than 200 μm and a circularity of 0.97 or more and less than 1.00 as measured by a flow type particle image measuring device is less than 1,000 particles per 1.0 g of toner.

[0016] In the present disclosure, the circle equivalent diameter is the diameter of a circle having the same projected area as the particle image. In the present disclosure, the circularity is the value obtained by dividing the perimeter of a circle having the same projected area as the particle image by the perimeter of the projected image of the particle. The more complex the surface shape of the particle, the smaller the circularity value, and when the particle is a perfect sphere, the circularity is 1. In the present disclosure, the arithmetic mean of the circularities of multiple particles contained in the measurement sample is defined as the average circularity, and the arithmetic mean of the circle equivalent diameters is defined as the average circle equivalent diameter. The equivalent circle diameter can be determined, for example, by taking a projected image of the particles in a sample liquid using a flow particle image analyzer (e.g., FPIA-3000, manufactured by CIMEX, etc.) and measuring the diameter of a circle equal to the projected area of ​​the particles from the projected image. The circularity can be determined by measuring the perimeter of a circle equal to the projected area of ​​the particles and the perimeter of the projected image of the particles from the projected image, and then using the following calculation formula 1. Calculation formula 1: (Circularity) = (Perimeter of a circle equal to the projected area of ​​a particle) / (Perimeter of the projected image of a particle)

[0017] When the toner of the present disclosure is passed through a sieve with an opening of 25 μm by a wet method, the coarse particles having a circle equivalent diameter of 50 μm or more and less than 200 μm that do not pass through the sieve are substantially the same as the coarse particles contained in the toner of the present disclosure having a circle equivalent diameter of 50 μm or more and less than 200 μm. This is because coarse particles having a circle equivalent diameter of 50 μm or more cannot usually pass through a sieve with an opening of 25 μm by a wet method. In addition, the coarse particles contained in the toner of the present disclosure usually have a circle equivalent diameter of less than 200 μm. Note that the amount of particles having a circle equivalent diameter of less than 50 μm in the toner of the present disclosure is not particularly limited. In the present disclosure, as the sieve with 25 μm mesh size, a mesh with 25 μm mesh size in which meridians and latitudes are arranged at equal intervals and the intervals between the meridians and latitudes are the same is used. The toner of the present disclosure can be passed through a sieve with a mesh size of 25 μm by a wet method, for example, as follows. First, a toner dispersion in which a pre-weighed amount of toner is dispersed in water containing a surfactant at a concentration of 0.1 to 1% by mass is passed through a sieve with a mesh size of 25 μm. Here, the concentration of the toner in the toner dispersion is usually about 1 to 5% by mass. Thereafter, the water containing the surfactant is further passed through the sieve until the water passing through the sieve does not have the color of the toner to the naked eye. Next, the coarse particles remaining on the sieve are collected with a small amount of water containing the surfactant to obtain a coarse particle dispersion. At that time, the mass of the obtained coarse particle dispersion is recorded. The particle size distribution of the coarse particle dispersion is measured using a flow-type particle image measuring device, and the particle count of the coarse particles A and the coarse particles B is measured. The particle count is measured for the coarse particle dispersion in the measurement cell. The number of coarse particles A contained in the coarse particle dispersion in the measurement cell is N A (pieces) and the number of coarse particles B N B (pieces), the capacity of the measurement cell C (g), and the total mass of the coarse particle dispersion W D (g), and the mass W of the toner used in the measurement T From (g), the number of coarse particles A contained in 1.0 g of toner can be calculated using the following calculation formula (A), and the number of coarse particles B contained in 1.0 g of toner can be calculated using the following calculation formula (B).

[0018]

number

[0019] In the toner of the present disclosure, the number of particles of the coarse particles A in 1.0 g of toner is 20,000 or less, and the number of particles of the coarse particles B in 1.0 g of toner is less than 1,000, so that the occurrence of white streaks and the deterioration of image quality can be suppressed in both high temperature and high humidity environments and low temperature and low humidity environments. It is considered that white streaks occur when coarse particles contained in the toner get caught in the nip between the developing roller and the layer regulating blade in the developing device, causing the toner layer on the developing roller to become uneven. In addition, white streaks are more likely to occur in a low temperature and low humidity environment than in a high temperature and high humidity environment. It is presumed that this is because the hardness of the developing roller increases in a low temperature and low humidity environment, making the toner more likely to get caught in the nip. The present inventors have found that among the coarse particles having a circularity of 50 μm or more and less than 200 μm, the coarse particles B having a circularity of 0.97 or more and 1.00 or less are likely to cause the generation of white streaks, and the coarse particles A having a circularity of 0.20 or more and less than 0.97 are unlikely to cause the generation of white streaks. In the toner of the present disclosure, the amount of the coarse particles B that are likely to cause the generation of white streaks is reduced to less than 1000 particles per 1.0 g of toner, while the amount of the coarse particles A that are unlikely to cause the generation of white streaks does not exceed 20000 particles per 1.0 g of toner, thereby suppressing the generation of white streaks in both high temperature and high humidity environments and low temperature and low humidity environments. The coarse particles A having a circularity of 0.20 or more and less than 0.97 are often flat and can slip through the nip portion, so they are unlikely to get caught in the developing device and are presumed to be unlikely to cause the generation of white streaks. In addition, in the toner of the present disclosure, the number of the coarse particles A in 1.0 g of toner is 1000 or more, so that the occurrence of fogging in a high-temperature, high-humidity environment can be suppressed. This is presumed to be because the coarse particles A contain aggregates of external additives such as silica. The coarse particles A have a large equivalent circle diameter of 50 μm or more, so they often contain aggregates of external additives such as silica. In addition, in a high-temperature, high-humidity environment, the toner is less likely to be charged than in a normal temperature and humidity environment, so that fogging is more likely to occur. In contrast, the toner of the present disclosure contains an appropriate amount of coarse particles A, so that the fluidity of the toner is improved, and it is presumed that the occurrence of fogging is suppressed even in a high-temperature, high-humidity environment. In this way, the toner of the present disclosure has the coarse particles B, which are prone to causing white streaks, sufficiently removed, and the amount of the coarse particles A is controlled to an extent that they do not cause white streaks and are effective in suppressing the occurrence of fogging in a high-temperature, high-humidity environment. This is believed to suppress the occurrence of white streaks in high-temperature, high-humidity environments and low-temperature, low-humidity environments, and further suppress the occurrence of fogging in a high-temperature, high-humidity environment.

[0020] From the viewpoint of suppressing the occurrence of white streaks, the number of the coarse particles A per 1.0 g of toner is preferably 19,000 or less, and the number of the coarse particles B per 1.0 g of toner is preferably 500 or less, more preferably 400 or less, and even more preferably 350 or less.

[0021] From the viewpoint of suppressing the occurrence of white streaks, the number of coarse particles A having a circularity of 0.95 or more and less than 0.97, among the coarse particles A having a circularity of 0.20 or more and less than 0.97, in 1.0 g of toner is preferably 500 or less, more preferably 400 or less, even more preferably 300 or less, and even more preferably 200 or less. The coarse particles contained in the toner of the present disclosure usually have a circularity in the range of 0.20 to 1.00. In addition, from the viewpoint of suppressing the occurrence of white streaks, the total number of coarse particles A having a circularity of 0.95 or more and less than 0.97, and the total number of coarse particles B, per 1.0 g of toner, is preferably 1,500 or less, more preferably 1,000 or less, and even more preferably 800 or less.

[0022] The toner of the present disclosure generally has an average equivalent circular diameter of 5 to 9 μm. Furthermore, the toner of the present disclosure is not particularly limited, but from the viewpoint of improving image reproducibility, the average circularity is preferably 0.98 to 1.00, and more preferably 0.99 to 1.00. The average circularity of the toner can be set within the above range by producing the colored resin particles contained in the toner by a wet method such as an emulsion polymerization aggregation method, a dispersion polymerization method, a suspension polymerization method, or a solution suspension method. Hereinafter, a method for producing the toner for developing electrostatic images according to the present disclosure will be described. The colored resin particles contained in the toner of the present disclosure contain at least a binder resin, a colorant, and a release agent. Each component contained in the colored resin particles is derived from each component in the polymerizable monomer composition used in the manufacturing method described below and the polymerizable monomer for shell. The polymerizable monomer used in the production of the colored resin particles is polymerized during the manufacturing process to become a polymer, and is contained in the colored resin particles as a binder resin. The external additive contained in the toner of the present disclosure is the same as the external additive used in the production method described below.

[0023] II. Method for producing toner for developing electrostatic images The toner for developing electrostatic images according to the present disclosure can be obtained, for example, by a production method including a step of preparing colored resin particles, a step of attaching an external additive to the surface of the colored resin particles (hereinafter, may be referred to as an external addition step), and a step of removing a portion of the coarse particles contained in the particles by supplying particles containing the colored resin particles to a sieve (hereinafter, may be referred to as a sieving step). In the present disclosure, the steps of the production method may be performed in a reverse order, as far as this is technically possible, and two or more steps may be performed simultaneously as one step.

[0024] 1.Preparing colored resin particles In general, the manufacturing method of colored resin particles is roughly classified into dry methods such as pulverization, and wet methods such as emulsion polymerization aggregation, dispersion polymerization, suspension polymerization, and dissolution suspension. Wet methods are preferred because they can easily produce toners with excellent printing performance such as fine line reproducibility. Among the wet methods, polymerization methods such as emulsion polymerization aggregation, dispersion polymerization, and suspension polymerization are preferred because they can easily produce toners with a relatively small particle size distribution on the order of microns, and among the polymerization methods, suspension polymerization is more preferred.

[0025] The emulsion polymerization aggregation method is a method in which an emulsified polymerizable monomer is polymerized to obtain fine resin particles, and the fine resin particles are aggregated with a colorant or the like to produce colored resin particles. The above-mentioned dissolution suspension method is a method in which a solution in which toner components such as a binder resin and a colorant are dissolved or dispersed in an organic solvent is formed into droplets in an aqueous medium, and the organic solvent is removed to produce colored resin particles, and any of the known methods can be used for the respective methods.

[0026] In the present disclosure, the colored resin particles can be produced by adopting a wet method or a dry method, but among the wet methods, it is preferable to produce them by a suspension polymerization method. As a method for producing colored resin particles by a suspension polymerization method, for example, a method having a step of preparing a suspension in which droplets of a polymerizable monomer composition containing at least a polymerizable monomer, a colorant, and a release agent are dispersed in an aqueous dispersion medium (hereinafter, sometimes referred to as a step of preparing a suspension), and a step of forming colored resin particles by subjecting the suspension to a polymerization reaction in the presence of a polymerization initiator (hereinafter, sometimes referred to as a polymerization step) can be suitably adopted. As the polymerizable monomer composition, a composition prepared in advance may be used, but a step of preparing a polymerizable monomer composition may also be further included. In addition, the materials of the polymerizable monomer composition may be simultaneously suspended while being introduced into an aqueous dispersion medium, so that the preparation of the polymerizable monomer composition and the preparation of the suspension may be simultaneously carried out in one step. In addition, the method for producing colored resin particles by a suspension polymerization method may further include other steps. An example of a method for producing colored resin particles by a suspension polymerization method including (1) a step of preparing a polymerizable monomer composition, (2) a step of preparing a suspension, and (3) a polymerization step will be described in detail below.

[0027] (1) A step of preparing a polymerizable monomer composition In this step, a polymerizable monomer composition is prepared that contains at least a polymerizable monomer, a colorant, and a release agent, and further contains other materials such as a charge control agent, a polar resin, and a molecular weight modifier, as necessary. The polymerizable monomer composition is prepared by mixing the respective materials, and a media type disperser, for example, is used for the mixing.

[0028] [Polymerizable monomer] In the present disclosure, the polymerizable monomer refers to a monomer having a functional group capable of addition polymerization. The polymerizable monomer is polymerized to become a binder resin. In the present disclosure, as the polymerizable monomer, a compound having an ethylenically unsaturated bond as a functional group capable of addition polymerization is generally used. As the main component of the polymerizable monomer, it is preferable to use a monovinyl monomer having only one polymerizable functional group. Examples of the monovinyl monomer include styrene, styrene derivatives such as vinyl toluene and α-methylstyrene, acrylic acid and methacrylic acid, acrylic acid esters such as methyl acrylate, ethyl acrylate, propyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, and 2-dimethylaminoethyl acrylate, methacrylic acid esters such as methyl methacrylate, ethyl methacrylate, propyl methacrylate, butyl methacrylate, 2-ethylhexyl methacrylate, and 2-dimethylaminoethyl methacrylate, nitrile compounds such as acrylonitrile and methacrylonitrile, amide compounds such as acrylamide and methacrylamide, and olefins such as ethylene, propylene, and butylene. These monovinyl monomers can be used alone or in combination of two or more. Among these, as the monovinyl monomer, at least one selected from the group consisting of styrene, styrene derivatives, acrylic acid, acrylic acid esters, methacrylic acid, and methacrylic acid esters is preferably used.

[0029] In order to improve the heat-resistant storage stability of the toner obtained, it is preferable to use a crosslinkable polymerizable monomer together with the monovinyl monomer. The crosslinkable polymerizable monomer is a monomer having two or more polymerizable functional groups, and is a polymerizable monomer that forms a crosslinked bond in the resin by a polymerization reaction. Examples of the crosslinkable polymerizable monomer include aromatic divinyl compounds such as divinylbenzene, divinylnaphthalene, and derivatives thereof; ester compounds in which two or more carboxylic acids are ester-bonded to an alcohol having two or more hydroxyl groups, such as ethylene glycol dimethacrylate and diethylene glycol dimethacrylate; other divinyl compounds such as N,N-divinylaniline and divinyl ether; and compounds having three or more vinyl groups. These crosslinkable polymerizable monomers can be used alone or in combination of two or more kinds. The crosslinkable polymerizable monomer is usually used in a proportion of 0.1 to 5 parts by mass, preferably 0.3 to 2 parts by mass, based on 100 parts by mass of the monovinyl monomer in the polymerizable monomer composition.

[0030] Furthermore, it is preferable to use a macromonomer as a part of the polymerizable monomer, since the resulting toner has a good balance between heat-resistant storage stability and low-temperature fixability. The macromonomer is a reactive oligomer or polymer having a polymerizable carbon-carbon unsaturated double bond at the end of the molecular chain, and usually has a number-average molecular weight of 1,000 to 30,000. The macromonomer is preferably one that gives a polymer having a glass transition temperature (Tg) higher than that of a polymer obtained by polymerizing a monovinyl monomer. The macromonomer is used in a proportion of preferably 0.03 to 5 parts by mass, more preferably 0.05 to 1 part by mass, based on 100 parts by mass of the monovinyl monomer in the polymerizable monomer composition.

[0031] The total amount of the polymerizable monomers contained in the polymerizable monomer composition is preferably 60 to 95 parts by mass, more preferably 70 to 90 parts by mass, based on 100 parts by mass of the total solid content contained in the polymerizable monomer composition. In the present disclosure, the solid content refers to everything other than the solvent, and for example, liquid monomers and the like are included in the solid content. In the toner of the present disclosure, the content of the polymer of the polymerizable monomer is preferably 60 to 95 parts by mass, and more preferably 70 to 90 parts by mass, based on 100 parts by mass of the colored resin particles.

[0032] [Coloring agent] The colorant contained in the polymerizable monomer composition is not particularly limited, and for example, black, cyan, yellow, and magenta colorants can be used. As the black colorant, for example, carbon black, titanium black, and magnetic powders such as zinc iron oxide and nickel iron oxide can be used. As the cyan colorant, for example, a copper phthalocyanine compound, a derivative thereof, an anthraquinone compound, etc. are used. Specific examples thereof include CI Pigment Blue 2, 3, 6, 15, 15:1, 15:2, 15:3, 15:4, 16, 17:1, and 60. As the yellow colorant, for example, azo pigments such as monoazo pigments and disazo pigments, and compounds such as condensed polycyclic pigments are used. Specific examples thereof include CI Pigment Yellow 3, 12, 13, 14, 15, 17, 62, 65, 73, 74, 83, 93, 97, 120, 138, 155, 180, 181, 185, 186, and 213. As the magenta colorant, for example, azo pigments such as monoazo pigments and disazo pigments, condensed polycyclic pigments, and other compounds are used. Specific examples thereof include CI Pigment Red 31, 48, 57:1, 58, 60, 63, 64, 68, 81, 83, 87, 88, 89, 90, 112, 114, 122, 123, 144, 146, 149, 150, 163, 170, 184, 185, 187, 202, 206, 207, 209, 237, 238, 251, 254, 255, 269, and CI Pigment Violet 19. In the present disclosure, these colorants may be used alone or in combination of two or more. The colorant is preferably used in an amount of 1 to 15 parts by mass, more preferably 1 to 10 parts by mass, based on 100 parts by mass of the polymerizable monomer in the polymerizable monomer composition. In the toner of the present disclosure, the content of the colorant is preferably 1 to 15 parts by mass, and more preferably 1 to 10 parts by mass, based on 100 parts by mass of the binder resin.

[0033] [Release agent] The polymerizable monomer composition contains a release agent from the viewpoint of improving the releasability of the toner from the fixing roll during fixing. The release agent is not particularly limited as long as it is a release agent generally used for toners, but a monoester compound is preferably used from the viewpoint of improving the low-temperature fixing property of the toner. As the monoester compound, for example, a monoester compound represented by the following formula (1) can be preferably used. R 1 -COO-R 2 Formula (1) In the formula (1), R 1 represents a linear alkyl group having 15 to 21 carbon atoms, and R 2 R represents a linear alkyl group having 16 to 22 carbon atoms. 1 and R 2 may be the same group or different groups. In the monoester compound shown in formula (1), the number of carbon atoms in the raw material fatty acid (i.e., R 1 The number of carbon atoms in the raw alcohol (i.e., R 2 The difference between the number of carbon atoms in the alkyl group and the alkyl group (the number of carbon atoms in the alkyl group) is preferably 0 to 6, and more preferably 4 to 6.

[0034] The monoester compound represented by the formula (1) is, for example, behenyl palmitate (C 15 H 31 -COO-C 22 H 45 ), Behenyl Stearate (C 17 H 35 -COO-C 22 H 45 ), Behenyl Eicosanoate (C 19 H 39 -COO-C 22 H 45 ), Behenyl behenate (C 21 H 43 -COO-C 22 H 45 ), eicosyl palmitate (C 15 H 31 -COO-C 20 H 41 ), eicosyl stearate (C 17 H 35 -COO-C 20 H 41 ), eicosanoic acid eicosyl (C 19 H 39 -COO-C 20 H 41 ), eicosyl behenate (C21 H 43 -COO-C 20 H 41 ), Stearyl stearate (C 17 H 35 -COO-C 18 H 37 ), Stearyl Eicosanoate (C 19 H 39 -COO-C 18 H 37 ), Stearyl Behenate (C 21 H 43 -COO-C 18 H 37 ), hexadecyl eicosanoate (C 19 H 39 -COO-C 16 H 33 ), Hexadecyl Behenate (C 21 H 43 -COO-C 16 H 33 Among these monoester compounds, behenyl stearate, behenyl palmitate, and stearyl behenate are more preferred.

[0035] The monoester compound represented by the formula (1) can be produced by, for example, a synthesis method using an oxidation reaction, synthesis from a carboxylic acid or its derivative, an ester group introduction reaction such as a Michael addition reaction, a method using a dehydration condensation reaction from a carboxylic acid compound and an alcohol compound, a reaction from an acid halide and an alcohol compound, an ester exchange reaction, or the like. A catalyst can also be used appropriately in the production of the monoester compound represented by the formula (1). As the catalyst, a general acidic or alkaline catalyst used in an esterification reaction, such as zinc acetate or a titanium compound, is preferable. After the esterification reaction, the target product may be purified by recrystallization, distillation, or the like.

[0036] Examples of the release agent that can be used in the present disclosure include, in addition to the monoester compound represented by formula (1), pentaerythritol ester compounds such as pentaerythritol tetrabehenate, pentaerythritol tetrapalmitate, pentaerythritol tetrastearate, pentaerythritol tetramyristate, and pentaerythritol tetralaurate, glycerin ester compounds such as hexaglycerin octabehenate, pentaglycerin heptabehenate, tetraglycerin hexabehenate, triglycerin pentabehenate, diglycerin tetrabehenate, and glycerin tribehenate, dipentaglycerin ester compounds such as hexaglycerin octabehenate, pentaglycerin heptabehenate, tetraglycerin hexabehenate, triglycerin pentabehenate, diglycerin tetrabehenate, and glycerin tribehenate, and dipentaglycerin ester compounds such as hexaglycerin octabehenate, pentaglycerin heptabehenate, tetraglycerin hexabehenate, triglycerin pentabehenate, diglycerin tetrabehenate, and glycerin tribehenate. Examples of suitable waxes include ester waxes such as polyhydric alcohol ester compounds, such as dipentaerythritol esters, e.g., dipentaerythritol hexamyristate, dipentaerythritol hexapalmitate, and dipentaerythritol hexalaurate; hydrocarbon waxes, e.g., polyolefin waxes, e.g., polyethylene wax, polypropylene wax; synthetic waxes, e.g., Fischer-Tropsch wax; and petroleum waxes, e.g., paraffin, microcrystalline, and petrolatum; natural waxes, e.g., candelilla, carnauba, rice, Japan wax, and jojoba; and mineral waxes, e.g., montan, ceresin, and ozokerite. These release agents may be used alone or in combination of two or more.

[0037] The release agent used in the present disclosure has a melting point of preferably 60 to 75° C., more preferably 63 to 72° C., and even more preferably 65 to 70° C. When the melting point of the release agent is equal to or higher than the lower limit, the heat-resistant storage stability of the toner can be improved, and when the melting point is equal to or lower than the upper limit, a decrease in the fixing temperature of the toner can be suppressed.

[0038] The acid value of the release agent used in the present disclosure is preferably 1.0 mgKOH / g or less, more preferably 0.6 mgKOH / g or less, and even more preferably 0.3 mgKOH / g or less. By making the acid value of the release agent equal to or less than the upper limit, the storage stability of the toner can be improved.

[0039] The hydroxyl value of the release agent used in the present disclosure is preferably 10 mgKOH / g or less, more preferably 6 mgKOH / g or less, and even more preferably 3 mgKOH / g or less. By making the hydroxyl value of the release agent equal to or less than the upper limit, the storage stability of the toner can be improved. In this disclosure, the acid value and hydroxyl value are values ​​measured in accordance with JIS K 0070, a standard method for analyzing fats and oils established by the Japanese Industrial Standards Committee (JICS). The release agent used in the present disclosure preferably has an acid value and a hydroxyl value both of which are equal to or less than the preferred upper limit values.

[0040] The release agent is used in an amount of usually 8 to 40 parts by mass, preferably 11 to 35 parts by mass, and more preferably 15 to 30 parts by mass, based on 100 parts by mass of the polymerizable monomer in the polymerizable monomer composition. In the toner of the present disclosure, the content of the release agent is usually 8 to 40 parts by mass, preferably 11 to 35 parts by mass, and more preferably 15 to 30 parts by mass, based on 100 parts by mass of the binder resin. When the content of the release agent is equal to or more than the lower limit, the releasability of the toner from the fixing roll can be improved, and when the content is equal to or less than the upper limit, deterioration of heat-resistant storage stability and durability can be suppressed.

[0041] [Charge control agent] The polymerizable monomer composition preferably contains a positively or negatively chargeable charge control agent in order to improve the chargeability of the toner. The charge control agent is not particularly limited as long as it is one that is generally used as a charge control agent for toners. Among charge control agents, positively or negatively charged charge control resins are preferably used because they have high compatibility with polymerizable monomers and can impart stable chargeability (charge stability) to toner particles.

[0042] As the positively or negatively charged charge control resin, a functional group-containing copolymer can be used. As the positively charged charge control resin, for example, a functional group-containing copolymer containing a structural unit containing a functional group such as an amino group, a quaternary ammonium group, or a quaternary ammonium salt-containing group can be used, and examples thereof include polyamine resins, quaternary ammonium group-containing copolymers, and quaternary ammonium base-containing copolymers. As the negatively charged charge control resin, for example, a functional group-containing copolymer containing a structural unit containing a functional group such as a sulfonic acid group, a sulfonate salt-containing group, a carboxylic acid group, or a carboxylate salt-containing group can be used, and examples thereof include sulfonic acid group-containing copolymers, sulfonate salt salt-containing copolymers, carboxylic acid group-containing copolymers, and carboxylate salt salt-containing copolymers. The functional group-containing copolymer used as the positively or negatively charged charge control resin is preferably one having a ratio of functional group-containing constitutional units of 10% by mass or less, more preferably 5% by mass or less, in terms of high compatibility with polymerizable monomers and excellent polymerization stability. On the other hand, in terms of improving the charge stability and storage stability of the toner, the ratio of functional group-containing constitutional units in the functional group-containing copolymer is preferably 0.5% by mass or more. It is presumed that the charge control resin contains a sufficient number of functional groups, which makes it easy for the charge control resin to be localized near the surface of the colored resin particles, and the charge control resin functions like a shell of the colored resin particles, thereby improving the storage stability of the toner.

[0043] The functional group-containing copolymer used as the positively or negatively charged charge control resin is preferably a styrene-acrylic resin, since it has high compatibility with the polymerizable monomer and the charge amount can be easily adjusted by the amount added.

[0044] The functional group-containing copolymer used as the positively or negatively charged charge control resin preferably has a glass transition temperature (Tg) of 50 to 110° C., more preferably 60 to 100° C. When the glass transition temperature (Tg) of the functional group-containing copolymer is within the above range, the storage stability of the toner can be improved. The functional group-containing copolymer is likely to be localized near the surface of the colored resin particles and can function like a shell. Therefore, when the Tg of the functional group-containing copolymer is within the above range, the Tg is sufficiently high, and therefore it is presumed that the storage stability of the toner is improved. In the present disclosure, the glass transition temperature (Tg) can be determined, for example, in accordance with ASTM D3418-82. Specifically, a sample is heated at a heating rate of 10° C. / min using a differential scanning calorimeter (Seiko Denshi Kogyo Co., Ltd.: SSC5200) or the like, and the temperature showing the maximum heat peak of the DSC curve obtained during the heating process can be determined as the glass transition temperature.

[0045] As the charge control agent, a charge control resin may be used in combination with a charge control agent other than the charge control resin. Other positively chargeable charge control agents include, for example, nigrosine dyes, quaternary ammonium salts, triaminotriphenylmethane compounds, imidazole compounds, and the like. Other negatively chargeable charge control agents include, for example, azo dyes containing metals such as Cr, Co, Al, and Fe, metal salicylate compounds, and metal alkylsalicylate compounds. The charge control agents can be used alone or in combination of two or more.

[0046] In the present disclosure, the charge control agent is usually used in an amount of 0.01 to 10 parts by mass, and preferably 0.03 to 8 parts by mass, based on 100 parts by mass of the polymerizable monomer in the polymerizable monomer composition. In the toner of the present disclosure, the content of the charge control agent is usually 0.01 to 10 parts by mass, and preferably 0.03 to 8 parts by mass, based on 100 parts by mass of the binder resin. When the content of the charge control agent is equal to or more than the lower limit, the occurrence of fog can be suppressed, and when the content is equal to or less than the upper limit, print smearing can be suppressed.

[0047] [Polar resin] The polymerizable monomer composition preferably contains a polar resin in order to suppress bleeding of the release agent. In the present disclosure, the polar resin is selected from the group consisting of polymers containing a repeating unit containing a heteroatom. Specific examples of the polar resin include acrylic resins, polyester resins, and vinyl resins containing heteroatoms. The polar resin may be a homopolymer or copolymer of a heteroatom-containing monomer, or a copolymer of a heteroatom-containing monomer and a non-heteroatom-containing monomer. When the polar resin is a copolymer of a heteroatom-containing monomer and a non-heteroatom-containing monomer, the ratio of the heteroatom-containing monomer unit in 100% by mass of all repeating units constituting the copolymer is preferably 50% by mass or more, more preferably 70% by mass or more, and even more preferably 90% by mass or more, from the viewpoint of easy control of the particle size of the colored resin particles and easy suppression of bleeding of the release agent in the obtained toner.

[0048] Examples of the heteroatom-containing monomer used in the polar resin include alkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, n-pentyl (meth)acrylate, sec-pentyl (meth)acrylate, isopentyl (meth)acrylate, neopentyl (meth)acrylate, n-hexyl (meth)acrylate, isohexyl (meth)acrylate, neohexyl (meth)acrylate, sec-hexyl (meth)acrylate, tert-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and lauryl (meth)acrylate; and 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxypropyl (meth)acrylate, 5-hydroxypropyl (meth)acrylate, 6-hydroxypropyl (meth)acrylate, 7-hydroxypropyl (meth)acrylate, 8-hydroxypropyl (meth)acrylate, 9-hydroxypropyl (meth)acrylate, 10-hydroxypropyl (meth)acrylate, 11-hydroxypropyl (meth)acrylate, 12-hydroxypropyl (meth)acrylate, 13-hydroxypropyl (meth)acrylate, 14-hydroxypropyl (meth)acrylate, 15-hydroxypropyl (meth)acrylate, 16-hydroxypropyl (meth)acrylate, 17-hydroxypropyl (meth)acrylate, 18-hydroxypropyl (meth)acrylate, 19-hydroxypropyl (meth)acrylate, 20-hydroxypropyl (meth)acrylate, 21-hydroxypropyl (meth)acrylate, 22-hydroxypropyl (meth)acrylate, 23-hydroxypropyl (meth)acrylate, 24-hydroxypropyl (meth)acrylate, 25-hydroxypropyl (meth)acrylate, 26-hydroxypropyl (meth)acrylate, 27-hydroxypropyl (meth)acrylate, 28-hydroxypropyl (meth)acrylate, 29-hydroxypropyl (meth)acrylate, 30-hydroxypropyl (meth)acrylate, 31-hydroxypropyl (meth Examples of the monomers include (meth)acrylic acid esters such as 4-hydroxybutyl acrylate (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, glycidyl (meth)acrylate, and 4-hydroxybutyl acrylate glycidyl ether, as well as monomers having a (meth)acryloyl group such as (meth)acrylic acid, i.e., (meth)acrylic monovinyl monomers; aromatic vinyl monomers containing heteroatoms such as halogenated styrene and styrenesulfonic acid; vinyl carboxylate ester monomers such as vinyl acetate; halogenated vinyl monomers such as vinyl chloride; halogenated vinylidene monomers such as vinylidene chloride; vinylpyridine monomers; carboxyl group-containing monomers such as ethylenically unsaturated carboxylic acid monomers such as crotonic acid, cinnamic acid, itaconic acid, fumaric acid, maleic acid, and butene tricarboxylic acid; and epoxy group-containing monomers such as allyl glycidyl ether. These heteroatom-containing monomers may be used alone or in combination of two or more.

[0049] Examples of the heteroatom-free monomer used in the polar resin include aromatic vinyl monomers not containing heteroatoms, such as styrene, vinyltoluene, α-methylstyrene, and p-methylstyrene; monoolefin monomers, such as ethylene, propylene, and butylene; and diene monomers, such as butadiene and isoprene. These heteroatom-free monomers can be used alone or in combination of two or more.

[0050] In the polar resin, it is preferable that the heteroatom-containing monomer contains a polar group-containing monomer unit containing at least one polar group selected from a carboxyl group, a hydroxyl group, a sulfonic acid group, an amino group, a polyoxyethylene group, and an epoxy group, because it is easy to control the particle size of the colored resin particles and easy to suppress bleeding of the release agent in the toner obtained. Among them, the polar group is preferably at least one selected from a carboxyl group and a hydroxyl group. Examples of polar group-containing monomers include carboxyl group-containing monomers such as ethylenically unsaturated carboxylic acid monomers such as acrylic acid, methacrylic acid, crotonic acid, cinnamic acid, itaconic acid, fumaric acid, maleic acid, and butene tricarboxylic acid; hydroxyl group-containing monomers such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate; sulfonic acid group-containing monomers such as styrenesulfonic acid; amino group-containing monomers such as dimethylaminoethyl (meth)acrylate and diethylaminoethyl (meth)acrylate; polyoxyethylene group-containing monomers such as methoxypolyethylene glycol (meth)acrylate; and epoxy group-containing monomers such as glycidyl (meth)acrylate, allyl glycidyl ether, and 4-hydroxybutyl acrylate glycidyl ether. These polar group-containing monomers can be used alone or in combination of two or more. When the polar resin contains a polar group-containing monomer unit, it is preferable that the polar group is located at the end of the main chain or a side chain, or is bonded in a pendant manner to the main chain or a side chain, because this makes it easier for the polar resin to be arranged on the surface of the droplets of the polymerizable monomer composition, making it easier to control the particle size of the colored resin particles, and making it easier to suppress bleeding of the release agent in the resulting toner.

[0051] When the polar resin does not contain the polar group-containing monomer unit, the heteroatom-containing monomer unit contained in the polar resin preferably contains a monomer unit derived from an alkyl(meth)acrylate, from the viewpoints of high compatibility with the polymerizable monomer, ease of control of the particle size of the colored resin particles, and ease of suppressing bleeding of the release agent in the obtained toner. Among them, from the viewpoint of high polarity, it is more preferable to contain a monomer unit derived from an alkyl(meth)acrylate having an alkyl group having 3 or less carbon atoms, further more preferable to contain a monomer unit derived from at least one selected from methyl(meth)acrylate and ethyl(meth)acrylate, and even more preferable to contain a monomer unit derived from methyl(meth)acrylate.

[0052] As the polar resin, a copolymer of at least one selected from acrylic acid esters and methacrylic acid esters and at least one selected from acrylic acid and methacrylic acid is preferred, and a copolymer of an acrylic acid ester, a methacrylic acid ester, and an acrylic acid is more preferred, because it has high compatibility with the polymerizable monomer, the particle size of the colored resin particles is easily controlled, and bleeding of the release agent in the resulting toner is easily suppressed. Note that in the present disclosure, such a copolymer of a (meth)acrylic acid ester and (meth)acrylic acid may be referred to as an acrylic copolymer. In the acrylic copolymer, the (meth)acrylic acid ester may be, for example, the same as the (meth)acrylic acid ester used in the heteroatom-containing monomer. In the acrylic copolymer, the (meth)acrylic acid ester may contain or not contain the polar group, but is preferably not containing the polar group, and among them, alkyl (meth)acrylate is preferable. The acrylic acid ester used in the acrylic copolymer is preferably at least one selected from the group consisting of ethyl acrylate, n-propyl acrylate, isopropyl acrylate, and n-butyl acrylate, and more preferably at least one selected from ethyl acrylate and n-butyl methacrylate. The methacrylic acid ester used in the acrylic copolymer is preferably at least one selected from the group consisting of methyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, and n-butyl methacrylate, and more preferably methyl methacrylate.

[0053] In the acrylic copolymer, the ratio of (meth)acrylic acid to the total amount (100% by mass) of the (meth)acrylic acid ester and (meth)acrylic acid used in the synthesis of the acrylic copolymer is preferably 0.05 to 1% by mass, more preferably 0.1 to 0.6% by mass, and even more preferably 0.3 to 0.5% by mass, from the viewpoints of high compatibility with the polymerizable monomer, ease of control of the particle size of the colored resin particles, and ease of suppression of bleeding of the release agent in the obtained toner.

[0054] The acrylic copolymer is preferably a copolymer of monomers containing 50.0% by mass or more of methyl methacrylate relative to 100% by mass of the total mass of monomers used in the synthesis of the copolymer, from the viewpoints of high compatibility with the polymerizable monomer, ease of control of the particle size of the colored resin particles, and ease of suppression of bleeding of the release agent in the obtained toner. The acrylic copolymer is more preferably a copolymer of a monomer containing 50.0 to 99.9 mass% of methyl methacrylate and 0.1 to 5.0 mass% of (meth)acrylic acid, even more preferably a copolymer of a monomer containing 50.0 to 99.0 mass% of methyl methacrylate and 0.1 to 5.0 mass% of (meth)acrylic acid, still more preferably a copolymer of a monomer containing 50.0 to 98.0 mass% of methyl methacrylate, 1.0 to 5.0 mass% of an alkyl (meth)acrylate different from methyl methacrylate, and 0.1 to 5.0 mass% of (meth)acrylic acid, and particularly preferably a copolymer of a monomer containing 50.0 to 98.0 mass% of methyl methacrylate, 1.0 to 5.0 mass% of an alkyl (meth)acrylate different from methyl methacrylate, and 0.2 to 3.0 mass% of (meth)acrylic acid. As the alkyl (meth)acrylate other than methyl methacrylate, at least one selected from ethyl acrylate and butyl acrylate is preferable since the glass transition temperature can be controlled.

[0055] The acrylic copolymer may contain a small amount of monomer units derived from other monomers different from both (meth)acrylic acid esters and (meth)acrylic acid. From the viewpoint of easy control of the particle size of the colored resin particles and easy suppression of bleeding of the release agent in the obtained toner, the content ratio of the other monomers is preferably 30% by mass or less, more preferably 20% by mass or less, and even more preferably 10% by mass or less, based on 100% by mass of the total amount of monomers used in the synthesis of the acrylic copolymer, and it is most preferable that the copolymer does not contain the other monomers. Examples of the other monomers include the heteroatom-free monomers and the heteroatom-containing monomers other than the (meth)acrylic monovinyl monomers.

[0056] The acid value of the polar resin is preferably 0.5 to 7.0 mgKOH / g, more preferably 1.0 to 5.0 mgKOH / g, and even more preferably 1.5 to 3.0 mgKOH / g. When the acid value of the polar resin is equal to or more than the lower limit, the heat-resistant storage stability, low-temperature fixability, and print durability of the toner can be improved. When the acid value of the polar resin is equal to or less than the upper limit, the particle size of the colored resin particles can be easily controlled.

[0057] The weight average molecular weight (Mw) of the polar resin is usually 6,000 to 50,000, preferably 8,000 to 45,000, more preferably 9,000 to 45,000, and even more preferably 10,000 to 40,000. When the weight average molecular weight (Mw) of the polar resin is at least the lower limit, the heat resistant storage stability and durability of the toner can be improved, and when it is at most the upper limit, an increase in the fixing temperature of the toner can be suppressed. In the present disclosure, the weight average molecular weight (Mw) of a polymer can be determined in terms of polystyrene by GPC using a sample dissolved in tetrahydrofuran (THF).

[0058] The glass transition temperature (Tg) of the polar resin is preferably 60 to 95°C, more preferably 65 to 90°C, even more preferably 65 to 85°C, and even more preferably 70 to 80°C. When the glass transition temperature of the polar resin is equal to or higher than the lower limit, the heat resistant storage stability of the toner can be improved, and when the glass transition temperature is equal to or lower than the upper limit, the low temperature fixability of the toner can be improved.

[0059] The polar resin may be a commercially available product, but may also be produced by polymerizing a monomer containing the heteroatom-containing monomer by a known method such as solution polymerization, aqueous solution polymerization, ionic polymerization, high-temperature high-pressure polymerization, or suspension polymerization. Furthermore, when the polar resin is a copolymer, the copolymer may be any of a random copolymer, a block copolymer, or a graft copolymer, but is preferably a random copolymer. In addition, the polar resin is preferably pulverized as finely as possible in order to improve the solubility.

[0060] The content of the polar resin is preferably 0.8 to 2.5 parts by mass, more preferably 1.0 to 2.2 parts by mass, and even more preferably 1.0 to 2.0 parts by mass, based on 100 parts by mass of the polymerizable monomer in the polymerizable monomer composition. In the toner of the present disclosure, the content of the polar resin is preferably 0.8 to 2.5 parts by mass, more preferably 1.0 to 2.2 parts by mass, and even more preferably 1.0 to 2.0 parts by mass, based on 100 parts by mass of the binder resin. By making the content of the polar resin equal to or more than the lower limit, the particle size of the colored resin particles can be easily controlled, and bleeding of the release agent in the obtained toner can be suppressed, and further, the balance between heat-resistant storage stability and low-temperature fixability can be improved, and print durability can be improved. On the other hand, by making the content of the polar resin equal to or less than the upper limit, an increase in the fixing temperature of the toner can be suppressed.

[0061] [Molecular weight regulator] The polymerizable monomer composition preferably further contains a molecular weight regulator. The molecular weight regulator is not particularly limited as long as it is generally used as a molecular weight regulator for toners, and examples thereof include mercaptans such as t-dodecyl mercaptan, n-dodecyl mercaptan, n-octyl mercaptan, and 2,2,4,6,6-pentamethylheptane-4-thiol; and thiuram disulfides such as tetramethylthiuram disulfide, tetraethylthiuram disulfide, tetrabutylthiuram disulfide, N,N'-dimethyl-N,N'-diphenylthiuram disulfide, and N,N'-dioctadecyl-N,N'-diisopropylthiuram disulfide. These molecular weight regulators may be used alone or in combination of two or more kinds. The molecular weight modifier is used in an amount of usually 0.01 to 10 parts by mass, preferably 0.1 to 5 parts by mass, based on 100 parts by mass of the polymerizable monomer in the polymerizable monomer composition.

[0062] (2) A step of preparing a suspension This step is a step of granulating the polymerizable monomer composition obtained by the above-mentioned step in an aqueous dispersion medium to prepare a suspension in which droplets of the polymerizable monomer composition are dispersed.

[0063] The aqueous dispersion medium used in this step includes at least an aqueous medium. In the present disclosure, the aqueous medium is a medium selected from the group consisting of water, hydrophilic solvents such as lower alcohols and lower ketones, and mixtures of water and hydrophilic solvents, and is preferably a medium mainly composed of water, or may be water alone. As water, ion-exchanged water is usually used. When a hydrophilic solvent is used, it is preferable to adjust the content of the hydrophilic solvent within a range that does not inhibit polymerization. The aqueous medium is usually used in an amount of 100 to 3,000 parts by mass, and preferably 200 to 2,000 parts by mass, per 100 parts by mass of the polymerizable monomer in the polymerizable monomer composition.

[0064] The aqueous dispersion medium preferably contains a dispersion stabilizer. Examples of the dispersion stabilizer include inorganic compounds such as sulfates, such as barium sulfate and calcium sulfate; carbonates, such as barium carbonate, calcium carbonate, and magnesium carbonate; phosphates, such as calcium phosphate; metal oxides, such as aluminum oxide and titanium oxide; metal hydroxides, such as aluminum hydroxide, magnesium hydroxide, and ferric hydroxide; and organic compounds such as water-soluble polymers, such as polyvinyl alcohol, methyl cellulose, and gelatin; anionic surfactants; nonionic surfactants; and amphoteric surfactants. These dispersion stabilizers can be used alone or in combination of two or more. Among the above dispersion stabilizers, inorganic compounds, particularly colloids of poorly water-soluble metal hydroxides, are preferred. By using inorganic compounds, particularly colloids of poorly water-soluble metal hydroxides, the particle size distribution of the colored resin particles can be narrowed, and the amount of the dispersion stabilizer remaining after washing can be reduced, so that the toner obtained can reproduce images clearly and has excellent environmental stability. In addition, it is preferred that the aqueous dispersion medium is a colloid in which a poorly water-soluble inorganic compound is dispersed in a solvent. In the present disclosure, the poorly water-soluble inorganic compound is preferably an inorganic compound having a solubility of 0.5 g or less in 100 g of water. The dispersion stabilizer is usually used in an amount of 0.1 to 20 parts by mass based on 100 parts by mass of the polymerizable monomer in the polymerizable monomer composition.

[0065] In this step, when the polymerizable monomer composition is granulated in the aqueous dispersion medium, it is preferable to add a polymerization initiator to a mixed liquid of the polymerizable monomer composition and the aqueous dispersion medium to form droplets of the polymerizable monomer composition. The polymerization initiator may be added after the polymerizable monomer composition is dispersed in the aqueous dispersion medium and before droplets are formed, or may be added to the polymerizable monomer composition before it is dispersed in the aqueous dispersion medium. Examples of the polymerization initiator include persulfates such as potassium persulfate and ammonium persulfate; azo compounds such as 4,4'-azobis(4-cyanovaleric acid), 2,2'-azobis(2-methyl-N-(2-hydroxyethyl)propionamide), 2,2'-azobis(2-amidinopropane)dihydrochloride, 2,2'-azobis(2,4-dimethylvaleronitrile), and 2,2'-azobisisobutyronitrile; and organic peroxides such as di-t-butyl peroxide, benzoyl peroxide, t-butylperoxy-2-ethylhexanoate, t-butylperoxydiethylacetate, t-hexylperoxy-2-ethylbutanoate, diisopropylperoxydicarbonate, di-t-butylperoxyisophthalate, and t-butylperoxyisobutyrate. These polymerization initiators can be used alone or in combination of two or more. Among these polymerization initiators, organic peroxides are preferred because they can reduce the amount of residual polymerizable monomers and improve the print durability of the toner. Among the organic peroxides, peroxyesters are preferred because they have good initiator efficiency and can reduce the amount of residual polymerizable monomers, and non-aromatic peroxyesters, i.e., peroxyesters without an aromatic ring, are more preferred.

[0066] In addition, in the step of preparing a suspension, a disperser having a combination of a rotor and a stator which are comb-tooth type concentric rings, and a stirring device having a dispersion supply tank are used, and the dispersion containing the aqueous dispersion medium and the polymerizable monomer composition is supplied from the dispersion supply tank to the disperser, stirred by the disperser, and then discharged into the dispersion supply tank, and is repeatedly circulated within the stirring device to prepare the suspension, and it is preferable that the peripheral speed of the rotor of the disperser is 15 to 40 m / s, and the circulation number of the dispersion calculated by the following formula (I) is 4 to 30. Formula (I) Dispersion circulation frequency = {Dispersion flow rate (liters / h) x Processing time (h)} / Dispersion charge (liters) Here, the circumferential speed of the rotor means the tip speed of the rotor. Also, the circulation frequency of the dispersion means the number of times the dispersion circulates inside the disperser. In other words, the total amount of the dispersion processed by the disperser is obtained by multiplying the flow rate (liters / h) of the dispersion in the disperser by the processing time (h) by the disperser. The circulation frequency of the dispersion can be calculated by dividing this total amount by the amount of the dispersion charged (liters). By setting the circumferential speed of the rotor to 15 m / s or more and the number of circulations to 4 or more, the particle size distribution of the colored resin particles can be narrowed. Furthermore, by setting the number of circulations to 30 or less, deterioration of toner productivity can be suppressed. From the viewpoint of convenience that allows the use of a general dispersing machine, the circumferential speed of the rotor is preferably 40 m / s or less. The peripheral speed of the rotor is preferably 15 to 35 m / s, more preferably 15 to 30 m / s, and further preferably 15 to 25 m / s. The number of circulations is more preferably 10 to 25, and further preferably 10 to 20.

[0067] In the dispersing machine of the stirring device, the rotor is rotated at high speed to circulate the dispersion from the inside of the rotor to the outside of the stator, and the dispersion is stirred in the gap between the rotor and the stator. The combination of the rotor and the stator in the dispersion may be one stage or two or more stages. From the viewpoint of narrowing the particle size distribution of the obtained colored resin particles, it is preferable that it is a multi-stage combination, more preferably two or three stages, and particularly preferably three stages. The number of layers of the rotor and the stator in the combination of the rotor and the stator, and the number of teeth of the rotor and the stator are appropriately selected according to the particle size of the toner to be produced, and are not particularly limited, but when the combination of the rotor and the stator is arranged in multiple stages, it is preferable that the number of teeth of the rotor and the stator closest to the injection port side of the dispersion is smaller than the number of teeth of the other rotors and stators. For example, it is preferable that the arrangement of the rotor and stator combinations in the disperser, from the dispersion liquid inlet side to the outlet side, be any one selected from three stages of coarse teeth, medium teeth, and fine teeth, three stages of coarse teeth, medium teeth, and medium teeth, three stages of coarse teeth, fine teeth, and fine teeth, two stages of coarse teeth and medium teeth, and two stages of coarse teeth and fine teeth.

[0068] In the stirring device, for example, when a dispersion containing the aqueous dispersion medium and the polymerizable monomer composition is injected into a dispersion supply tank, the dispersion is supplied from the dispersion supply tank to the disperser, stirred by the disperser, and then discharged into the dispersion supply tank, and this is repeated to circulate within the stirring device and then supplied to a polymerization reactor. The method of feeding the dispersion liquid is not particularly limited, and examples thereof include a method using a liquid feeding pump. The internal pressure of the disperser can be adjusted by adjusting the flow rate of the dispersion liquid discharged from the disperser. The internal pressure of the disperser is preferably 0.01 to 15 MPa, more preferably 0.05 to 10 MPa, and even more preferably 0.1 to 5 MPa. By setting the internal pressure of the disperser within the above range, it is possible to efficiently form fine droplets while suppressing the generation of bubbles due to cavitation.

[0069] The stirring device used in the production method of the present disclosure may be a horizontal type in which the rotation axis of the disperser extends along the horizontal direction, or a vertical type in which the rotation axis extends along the direction of gravity. In the manufacturing method of the present disclosure, a commercially available stirring device can be used, such as a horizontal multi-stage in-line disperser such as Milder (trade name) manufactured by Pacific Machinery Works, Ltd. or Cavitron (trade name) manufactured by Eurotech Co., Ltd., or a vertical multi-stage in-line disperser such as an in-line disperser manufactured by IKA (e.g., DISPAX-REACTOR (registered trademark) DRS (trade name)).

[0070] (3) Polymerization process In this step, the suspension obtained in the above step is subjected to a polymerization reaction to form colored resin particles. It is preferable to further add a water-soluble oxo acid salt to the suspension during the polymerization reaction. By adding a water-soluble oxo acid salt during polymerization, it is possible to suppress the aggregation of droplets and the generation of fine powder, and narrow the particle size distribution. Examples of the water-soluble oxo acid salt include borates, phosphates, sulfates, carbonates, silicates, nitrates, etc., and preferably at least one selected from the group consisting of borates and phosphates, more preferably borates. Examples of the borate salt include sodium tetrahydroborate, potassium tetrahydroborate, sodium tetraborate, sodium metaborate, sodium metaborate, sodium peroxoborate, potassium metaborate, and hydrates of these borates. Examples of phosphates include sodium phosphinate, sodium phosphonate, sodium hydrogen phosphonate, sodium phosphate, disodium hydrogen phosphate, disodium hydrogen phosphate, sodium dihydrogen phosphate, sodium hexametaphosphate, sodium hypophosphate, sodium diphosphate, disodium dihydrogen diphosphate, sodium triphosphate, cyclo-sodium phosphate, potassium phosphinate, potassium phosphonate, potassium hydrogen phosphonate, potassium phosphate, dipotassium hydrogen phosphate, potassium dihydrogen phosphate, potassium diphosphate, potassium metaphosphate, and hydrates of these phosphates, etc. Among borates, sodium tetraborate, sodium metaborate, sodium metaborate, and hydrates of these borates are preferred, and sodium tetraborate decahydrate is particularly preferred. The water-soluble oxo acid salt is usually used in a proportion of 0.1 to 1,000 parts by mass, and preferably 1 to 100 parts by mass, per 100 parts by mass of the inorganic compound used as a dispersion stabilizer.

[0071] The polymerization temperature when the suspension is subjected to the polymerization reaction is not particularly limited, but is preferably 50° C. or higher, and more preferably 60 to 95° C. The polymerization reaction time is preferably 1 to 20 hours, and more preferably 2 to 15 hours.

[0072] The colored resin particles obtained by subjecting the suspension to a polymerization reaction may be used as a polymerized toner by adding an external additive as it is, but it is preferable to use the colored resin particles as the core layer of so-called core-shell type (also called "capsule type") colored resin particles. Core-shell type colored resin particles have a structure in which the outside of the core layer is covered with a shell layer formed of a material different from the core layer. By covering the core layer made of a material having a low softening point with a material having a higher softening point, it is possible to achieve a balance between lowering the fixing temperature of the toner and preventing aggregation during storage.

[0073] The method for producing the core-shell type colored resin particles using the colored resin particles obtained by subjecting the suspension to a polymerization reaction is not particularly limited, and the particles can be produced by a conventionally known method. In terms of production efficiency, the in situ polymerization method and the phase separation method are preferred.

[0074] A method for producing core-shell type colored resin particles by in situ polymerization will be described below. The suspension is subjected to a polymerization reaction to obtain a dispersion in which colored resin particles are dispersed. To the dispersion, a polymerizable monomer for forming a shell layer (polymerizable monomer for shell) and a polymerization initiator are added, and polymerization is carried out to obtain core-shell type colored resin particles.

[0075] As the polymerizable monomer for the shell, the same polymerizable monomers as those described above can be used. Among them, it is preferable to use monomers such as styrene, acrylonitrile, and methyl methacrylate, which can give a polymer with a Tg exceeding 80° C., either alone or in combination of two or more kinds. The amount of the polymerizable monomer for the shell added is not particularly limited, but is usually 1 to 10 parts by mass relative to 100 parts by mass of the polymerizable monomer used in the core layer. The binder resin of the core-shell type colored resin particles includes the binder resin in the core layer and the binder resin in the shell layer.

[0076] Examples of the polymerization initiator used for polymerization of the shell polymerizable monomer include water-soluble polymerization initiators such as metal persulfates, such as potassium persulfate and ammonium persulfate; and azo initiators, such as 2,2'-azobis(2-methyl-N-(2-hydroxyethyl)propionamide) and 2,2'-azobis-(2-methyl-N-(1,1-bis(hydroxymethyl)2-hydroxyethyl)propionamide). These can be used alone or in combination of two or more. The amount of the polymerization initiator is preferably 0.1 to 30 parts by mass, more preferably 1 to 20 parts by mass, based on 100 parts by mass of the shell polymerizable monomer.

[0077] The polymerization temperature for the shell layer is preferably 50° C. or higher, and more preferably 60 to 95° C. The polymerization reaction time is preferably 1 to 20 hours, and more preferably 2 to 15 hours.

[0078] (4) Washing, filtering, dehydrating, and drying processes In the production method of the present disclosure, it is preferable to further include a step of repeating operations of washing, filtering, dehydrating, and drying the aqueous dispersion of colored resin particles obtained in the polymerization step according to a conventional method several times as necessary.

[0079] The washing is carried out in order to remove the poorly water-soluble inorganic compound from the aqueous dispersion of colored resin particles obtained by the polymerization step when the poorly water-soluble inorganic compound is used as a dispersion stabilizer. Examples of the washing method include a method in which an acid or an alkali is added to the aqueous dispersion of colored resin particles to dissolve the poorly water-soluble inorganic compound in water and remove it. Among them, it is preferable to add an acid to adjust the pH of the aqueous dispersion of colored resin particles to 6.5 or less. As the acid to be added, inorganic acids such as sulfuric acid, hydrochloric acid, and nitric acid, and organic acids such as formic acid and acetic acid can be used, but sulfuric acid is particularly suitable because of its high removal efficiency and its small burden on the production equipment.

[0080] The dehydration and filtration methods can be any of various known methods, and are not particularly limited. For example, centrifugal filtration, vacuum filtration, pressure filtration, etc. can be mentioned. The drying method is also not particularly limited, and various methods can be used. When the external addition process described below is carried out before the screening process, the external addition process can involve drying the colored resin particles in addition to adhering the external additives, so that the colored resin particles prior to the external addition process can be dried so that their moisture content is approximately 7 to 20%.

[0081] The colored resin particles obtained through the above process preferably have a volume average particle size (Dv) of 3 to 15 μm, more preferably 4 to 12 μm. By having Dv equal to or greater than the lower limit, the fluidity of the toner can be improved, and deterioration of transferability and decrease in image density can be suppressed. By having Dv equal to or less than the upper limit, decrease in resolution of the formed image can be suppressed.

[0082] The colored resin particles preferably have a ratio (Dv / Dn) of the volume average particle diameter (Dv) to the number average particle diameter (Dn) of 1.0 to 1.3, more preferably 1.0 to 1.2. By making Dv / Dn 1.3 or less, it is possible to suppress the deterioration of transferability, image density, and resolution. The volume average particle diameter and number average particle diameter of the colored resin particles can be measured, for example, using a particle size analyzer (manufactured by Beckman Coulter, product name: Multisizer) or the like.

[0083] From the viewpoint of image reproducibility, the average circularity of the colored resin particles is preferably from 0.96 to 1.00, more preferably from 0.97 to 1.00, and even more preferably from 0.98 to 1.00. The closer the average circularity of the colored resin particles is to 1.00, the more the reproducibility of thin lines in printing can be improved. The average circularity of the colored resin particles can be determined in the same manner as the average circularity of the toner.

[0084] 2. External addition process The external addition step is a step of attaching an external additive to the surface of the colored resin particles. The colored resin particles to which the external additive is attached may be colored resin particles before the sieving step described below, or may be colored resin particles obtained after the sieving step. Alternatively, a first external addition step of attaching a part of the external additive to the colored resin particles may be performed before the sieving step, and a second external addition step of attaching the external additive to the obtained particles after the sieving step may be performed. In the toner manufacturing method of the present disclosure, it is preferable to attach at least a part of the external additive to the surface of the colored resin particles before the sieving step in order to improve the fluidity of the particles supplied to the sieve in the sieving step described below.

[0085] The external addition step is carried out, for example, by mixing and stirring the colored resin particles together with the external additive to carry out an external addition treatment. The stirrer used for the external addition treatment is not particularly limited as long as it is a stirring device capable of adhering an external additive to the surface of colored resin particles. For example, the external addition treatment can be performed using a stirrer capable of mixing and stirring, such as a Henschel Mixer (product name, manufactured by Mitsui Mining Co., Ltd.), an FM Mixer (product name, manufactured by Nippon Coke and Engineering Co., Ltd.), a Super Mixer (product name, manufactured by Kawada Manufacturing Co., Ltd.), a Q Mixer (product name, manufactured by Nippon Coke and Engineering Co., Ltd.), a Mechanofusion System (product name, manufactured by Hosokawa Micron Corporation), and a Mechano Mill (product name, manufactured by Okada Seiko Co., Ltd.). In addition, in the external addition treatment carried out before the screening process, if the external addition treatment is carried out by mixing and stirring colored resin particles having a moisture content of about 7 to 20% and external additives using the above-mentioned stirrer while drying, the fluidity of the colored resin particles during drying is improved, which is preferable in that the drying time of the colored resin particles can be shortened.

[0086] Examples of the external additive include inorganic fine particles such as silica, titanium oxide, aluminum oxide, zinc oxide, tin oxide, barium titanate, strontium titanate, calcium carbonate, calcium phosphate, and cerium oxide; organic fine particles such as polystyrene resin, polymethyl methacrylate resin, and other (meth)acrylic acid ester resins, styrene-(meth)acrylate copolymers, silicone resins, melamine resins, zinc stearate, and calcium stearate; and the like. The organic fine particles may be, for example, core-shell type particles in which the core contains a (meth)acrylic acid ester resin and the shell contains a polystyrene resin. Among these, inorganic fine particles are preferred, and among inorganic fine particles, at least one fine particle selected from silica and titanium oxide is preferred, and silica fine particles are more preferred. These external additives may be used alone, but it is preferable to use two or more of them in combination. The external additive used in the present disclosure preferably contains hydrophobized fine particles, more preferably contains hydrophobized inorganic fine particles, and even more preferably contains hydrophobized silica fine particles.When drying colored resin particles is performed together with external additive treatment, from the viewpoint of improving drying efficiency, the external additive added during drying preferably contains hydrophobized fine particles, more preferably contains hydrophobized inorganic fine particles, and even more preferably contains hydrophobized silica fine particles. From the viewpoint of improving the charging characteristics, it is also preferable to use hydrophobic silica fine particles and organic fine particles in combination as the external additive.

[0087] The number average primary particle diameter of the external additive used in the present disclosure is not particularly limited, but is preferably 5 to 100 nm, and more preferably 5 to 50 nm, from the viewpoint of easily adjusting the number of the coarse particles A contained in the toner to the above specific amount. When drying the colored resin particles is carried out in conjunction with the external addition treatment, the number average primary particle size of the external additive added during drying is preferably 5 nm to 30 nm, and more preferably 5 nm to 15 nm, in order to improve drying efficiency.

[0088] Since the number of the coarse particles A contained in the toner can be easily adjusted to the specific amount, the amount of the external additive added is preferably 0.1 to 5 parts by mass, more preferably 0.2 to 4 parts by mass, relative to 100 parts by mass of the colored resin particles. When the amount of the external additive added is equal to or more than the lower limit, the occurrence of transfer residue can be suppressed, and when the amount is equal to or less than the upper limit, fogging can be suppressed. When drying the colored resin particles in conjunction with the external additive treatment, the amount of external additive added during drying is preferably 0.1 to 1 part by mass, more preferably 0.1 to 0.5 parts by mass, per 100 parts by mass of the colored resin particles, in order to improve drying efficiency.

[0089] 3. Sieving process The sieving process is a process in which, after obtaining the colored resin particles, particles containing the colored resin particles are fed to a sieve to remove some of the coarse particles contained in the particles. The sieving process makes it possible to control the particle numbers of the coarse particles A and the coarse particles B in the toner as described above.

[0090] The sieving step may be performed after the step of preparing the colored resin particles, and may be performed before or after the external addition step, or, as described above, the sieving step may be performed after the first external addition step, and then the second external addition step may be performed. When the sieving step is performed before the external addition step, the particles supplied to the sieve are particles containing at least the colored resin particles, and when the sieving step is performed after the external addition step, the particles supplied to the sieve are mixed particles containing at least the colored resin particles and an external additive.

[0091] As the sieve used in the sieving step, for example, a wire mesh such as a stainless steel mesh, or a resin mesh such as a nylon mesh, a polyester mesh, or a polypropylene mesh can be used. A metal mesh is preferable because the wire of the mesh is not easily stretched, and therefore the mesh size can be easily maintained even in long-term use. A resin mesh is preferable because the wire of the mesh is moderately stretched, and therefore coarse particles with a particle size close to the mesh size are not easily pierced by the mesh, and the processing capacity is not likely to decrease during use. In addition, it is preferable that the wire of the mesh is antistatically treated.

[0092] In the screening process, a mesh is used for the sieve in which meridians and latitude lines are arranged at equal intervals and the intervals between the meridians and latitude lines are the same. In a mesh in which meridians and latitude lines are arranged at equal intervals and the intervals between the meridians and latitude lines are the same, the mesh size based on the latitude lines and the mesh size based on the meridians are the same, so the mesh size is the same no matter where the mesh is measured, except for errors. The weave of the mesh used in the sieve is preferably such that the meridians and latitudes are perpendicular to each other, and may be, for example, a common weave such as plain weave, twill weave, ton-cap weave, etc. Among them, plain weave is preferred because it is easy to maintain the size of the mesh openings and can efficiently remove the desired coarse particles.

[0093] In the present disclosure, the sieving step is a step of removing a part of coarse particles contained in the particles by supplying the particles containing the colored resin particles to a sieve using an air flow, The sieve includes at least one mesh, and the mesh with the smallest opening among the meshes used in the sieve has an opening of 25 μm or more and 40 μm or less; The air flow is generated by primary air supplied together with the particles containing the colored resin particles, and secondary air supplied from the recovery port side of the coarse particles, and the flow rate F1 [m 3 / min] and the flow rate of the secondary air F2 [m 3 / min] (F1 / F2) is preferably 18 or more and 50 or less. By the preferred sieving step, the particle numbers of the coarse particles A and the coarse particles B in the toner can be easily adjusted to the above-mentioned particle numbers. When particles are supplied to a sieve using an air flow, the coarse particles caught in the sieve may be pushed by the air flow and pass through the sieve. In particular, since coarse particles with low circularity often have a flat shape, even if they are caught in the sieve, they are easily pushed by the air flow and pass through the sieve. In the above-mentioned preferred sieving step, in the method of supplying particles to a sieve using an air flow, by adjusting the mesh size of the sieve and the flow rate F1 of the primary air that generates the air flow and the flow rate F2 of the secondary air as described above, it is possible to allow the coarse particles A with a relatively low circularity to pass through the sieve appropriately and the coarse particles B with a relatively high circularity not to pass through the sieve, so that the coarse particles B can be efficiently removed and the coarse particles A can be appropriately left remaining, and the particle numbers of the coarse particles A and the coarse particles B in 1.0 g of toner can be easily controlled to the above-mentioned particle numbers.

[0094] The sieve capable of feeding the powder to be treated to the sieve using an air flow is not particularly limited, and examples thereof include a blow-through type sieve and an air sieving machine, etc. Among them, the blow-through type sieve is preferably used because it is easy to control the number of coarse particles A and coarse particles B in the toner to the above-mentioned particle numbers and has an excellent recovery rate. Examples of commercially available blow-through type sieves include Hi-Bolter (product name, manufactured by Toyo Hightec Co., Ltd.) and Spin Air Sheep (product name, manufactured by Seishin Enterprise Co., Ltd.). In order to generate an air flow by the primary air supplied together with the powder to be treated and the secondary air supplied from the recovery port side of the coarse particles, for example, a sifter equipped with a secondary air intake mechanism that introduces secondary air from the oversized product recovery port to the screen side may be used. The secondary air intake mechanism is a mechanism for lifting up the powder recovered as the oversized product to the screen side and sieving it again.

[0095] FIG. 1 is a schematic diagram of an example of a sieving system that can be used to manufacture the toner for developing electrostatic images of the present disclosure. In the sieving system shown in FIG. 1, particles are supplied to a sieve 13 by primary air supplied by a primary air intake mechanism 12 from a feeder 11 that supplies particles including colored resin particles. Among the particles supplied to the sieve 13, those that do not pass through a mesh 14 provided in the sieve 13 are either lifted up again to the mesh 14 side by secondary air introduced by a secondary air intake mechanism 16 on the way through a coarse particle drop port 15, or pass through the coarse particle drop port 15 and are collected in a coarse particle collection container 17. The secondary air intake mechanism 16 is provided with a flow rate adjustment valve 22 for adjusting the flow rate of air. Among the particles supplied to the sieve 13, those that pass through the mesh 14 are carried by an air flow generated by a blower 21, passed through a pipe 18 and a cyclone 19, and collected in a collection container 20.

[0096] In the sieving step, the particles containing the colored resin particles are preferably dispersed and supplied to a sieve via an ejector 1 as shown in Fig. 2. The ejector 1 is a dispersing machine that blows compressed air from an air blowing nozzle 2, creates a partial vacuum, and sucks in and disperses the powder 4 through a powder suction nozzle 3. By using the ejector 1, the particles containing the colored resin particles can be uniformly supplied to the sieve, and the life of the sieve can be extended.

[0097] In the above-mentioned preferred sieving step, the mesh size of the mesh with the smallest opening among the meshes used in the sieve is 25 μm or more and 40 μm or less. Here, the mesh with the smallest opening refers to the mesh when the sieve uses one mesh, and refers to the mesh with the smallest opening when the sieve uses multiple meshes. When the mesh size of the mesh with the smallest opening is within the above-mentioned range, the particle numbers of the coarse particles A and the coarse particles B in the toner can be easily controlled to the above-mentioned particle numbers. In addition, when the mesh size of the mesh with the smallest opening is equal to or more than the above-mentioned lower limit, clogging can be suppressed. The upper limit of the mesh size of the mesh with the smallest opening is preferably 38 μm or less.

[0098] In the preferred screening step, the flow rate F1 [m 3 / min] and the secondary air flow rate F2 [m 3 / min] is set to 18 or more and 50 or less. By setting the ratio (F1 / F2) within the above range, the particle numbers of coarse particles A and coarse particles B in the toner can be easily controlled to the above particle numbers. In addition, by setting the ratio (F1 / F2) to the above lower limit value or more, the coarse particles B can be efficiently removed and clogging can be suppressed. By setting the ratio (F1 / F2) to the above upper limit value or less, the coarse particles A can be appropriately left in the toner. In addition, by setting the ratio (F1 / F2) to the above upper limit value or less, a decrease in the recovery rate of the toner particles can be suppressed. The lower limit of the ratio (F1 / F2) is preferably 20 or more, more preferably 22 or more, and the upper limit of the ratio (F1 / F2) is preferably 48 or less, more preferably 46 or less. The above ratio (F1 / F2) is rounded to an integer in accordance with Rule B of JIS Z8401:1999. The blower air volume, which is the sum of the flow rate F1 of the primary air and the flow rate F2 of the secondary air, is not particularly limited and may be appropriately adjusted according to the area of ​​the sieve so that the ratio (F1 / F2) is within the above range.

[0099] As the mesh used as a sieve, a laminated wire mesh made of two or more wire meshes is preferable from the viewpoint of suppressing breakage and efficiently removing coarse particles, and a laminated wire mesh made of two or more wire meshes having different mesh openings is more preferable. Moreover, as the laminated wire mesh, a laminated wire mesh made of two or more wire meshes bonded together by sintering is preferable.

[0100] In the laminated wire mesh, it is preferable that the wire mesh with the smallest mesh size is placed on the supply side of the particles containing the colored resin particles, and the wire meshes are laminated in order of the size of the mesh size. In order to minimize the decrease in the aperture ratio, it is preferable to use a laminated wire mesh in which the meridians and latitudes of all the wire meshes constituting the laminated wire mesh are approximately parallel to each other, as shown in FIG.

[0101] The mesh size of the wire mesh in the laminated wire netting may be within the above-mentioned range, and the mesh size of the wire mesh other than the wire mesh with the smallest mesh size is not particularly limited. However, in two wire meshes selected arbitrarily from all wire meshes in the laminated wire netting, the mesh size ratio is preferably within the range of 2 to 30, more preferably within the range of 10 to 25, and even more preferably within the range of 12 to 20. Here, the mesh size ratio is the ratio of the mesh size of the wire mesh with the relatively large mesh size to the mesh size of the wire mesh with the relatively small mesh size among the two wire meshes. By setting the mesh size ratio within the above range, the reinforcing effect of the laminated wire netting can be improved and clogging can be suppressed. The mesh size ratio is rounded to an integer, as in the above F1 / F2.

[0102] There is no particular limit to the number of wire meshes in the laminated wire mesh, but it is preferably 4 or less, more preferably 3 or less, and most preferably 2.

[0103] It is also preferable that the mesh size of all the wire meshes in the laminated wire mesh is within the range of 25 to 850 μm. When the mesh size of the wire meshes in the laminated wire mesh is equal to or larger than the lower limit, breakage and clogging of the wire mesh can be suppressed, while when the mesh size is equal to or smaller than the upper limit, the strength of the laminated wire mesh can be improved.

[0104] The wire diameter of the net is not particularly limited, but the wire diameter of the wire netting having the smallest mesh size is preferably 20 to 90 μm, and more preferably 25 to 80 μm. In the laminated wire mesh, the ratio of the wire diameters of two wire meshes arbitrarily selected from the wire meshes contained in the laminated wire mesh is preferably within the range of 1.1 to 26, and more preferably within the range of 1.15 to 20. Here, the ratio of the wire diameters of two wire meshes refers to the ratio of the wire diameter of the wire mesh with a relatively large wire diameter to the wire diameter of the wire mesh with a relatively small wire diameter. Moreover, the wire diameters of all the wire meshes in the laminated wire mesh are preferably within the range of 20 to 550 μm, and more preferably within the range of 25 to 525 μm.

[0105] In the above-mentioned preferred sieving step, when the particles containing the colored resin particles are supplied to the sieve using an air flow, the solid-gas ratio of the particles to the air is preferably 0.05 to 0.37, more preferably 0.07 to 0.34, and even more preferably 0.10 to 0.30, calculated by mass. When the solid-gas ratio is equal to or greater than the above-mentioned lower limit, a sufficient amount of particles can be supplied to the sieve, improving productivity, and when the solid-gas ratio is equal to or less than the above-mentioned upper limit, the particles can be uniformly dispersed in the air flow, suppressing clogging and suppressing a decrease in the recovery rate.

[0106] In the present disclosure, the solid-gas ratio of particles to air in terms of mass is determined by the following formula (i):

[0107] Formula (i) Solid-gas ratio (kg / kg) = particle supply rate (kg / Hr) / air supply rate (kg / Hr)

[0108] In formula (i), the air supply rate is calculated by the following formula (ii).

[0109] Formula (ii) Air supply rate (kg / Hr) = Blower air volume (m 3 / Hr) × air density (kg / m 3 )

[0110] In this disclosure, the air density in formula (ii) is 1.293 kg / m, which is the density at 0°C and 1 atmospheric pressure. 3 It is calculated as follows.

[0111] In the sieving step, it is preferable to remove coarse particles by making the pressure difference before and after the sieve usually 3 kPa or less, preferably 2 kPa or less. By removing coarse particles by making the pressure difference before and after the sieve within the above range, clogging of the sieve can be suppressed.

[0112] In the present disclosure, in order to remove coarse particles or foreign matter having a circle equivalent diameter of 200 μm or more, a sieving step using a mesh with a larger mesh size than that used in the above-mentioned preferred sieving step may be further included. The sieving step for removing coarse particles or foreign matter having a circle equivalent diameter of 200 μm or more is not particularly limited, but is preferably performed after the external addition step.

[0113] In the present disclosure, the toner thus obtained may be used as a one-component developer, or may be further mixed and stirred with carrier particles to be used as a two-component developer. EXAMPLES

[0114] The present disclosure will be described in more detail below with reference to examples and comparative examples, but the present disclosure is not limited to these examples. Note that parts and % are by weight unless otherwise specified.

[0115] [Production Example 1: Production of Copolymer 1] 200 parts of toluene was added to the reaction vessel, and the inside of the reaction vessel was thoroughly replaced with nitrogen while stirring the toluene, and then the temperature was raised to 90°C. Then, a mixed solution of 96.2 parts of methyl methacrylate, 3.5 parts of ethyl acrylate, 0.4 parts of acrylic acid, and 2.8 parts of t-butylperoxy-2-ethylhexanoate (manufactured by NOF Corp., trade name: Perbutyl O) was dropped into the reaction vessel over 2 hours. Furthermore, the mixture was kept under toluene reflux for 10 hours to complete the polymerization, and then the solvent was distilled off under reduced pressure. In this way, copolymer 1 (Tg 77.8°C, acid value 2.4 mgKOH / g, weight average molecular weight Mw 12500) was obtained. The weight-average molecular weight Mw of the copolymer 1 was determined by polystyrene conversion using GPC. The sample for measurement was prepared by dissolving the polymer in tetrahydrofuran (THF) to a concentration of 2 mg / mL, subjecting it to ultrasonic treatment for 10 minutes, and passing it through a 0.45 μm membrane filter to obtain a sample. The measurement conditions were temperature: 40° C., solvent: tetrahydrofuran, flow rate: 1.0 mL / min, concentration: 0.2 wt%, sample injection amount: 100 μL, and the column used was a GPC TSKgel MultiporeHXL-M (30 cm x 2 columns) manufactured by Tosoh Corporation. In addition, the measurement was performed under conditions where the linear correlation equation of Log(Mw)-elution time between weight-average molecular weights Mw of 1,000 to 300,000 was 0.98 or more.

[0116] [Example 1] 1. Preparation of the sieve A laminated wire mesh was prepared by sintering a first wire mesh with a mesh size of 34 μm and a second wire mesh with a mesh size of 617 μm together with their meridians and latitudes parallel to each other. All wire meshes used in each example were wire meshes in which the meridians and latitudes were perpendicular to each other, and the meridians and latitudes were arranged at equal intervals, with the intervals between the meridians and latitudes being the same (the openings of the wire mesh were square). The ratio of the openings of the second wire mesh to the openings of the first wire mesh was 18. The laminated wire mesh was attached to a blow-through type sieve (product name: Hi-Bolter, model: NR-450S, manufactured by Toyo Hitec Co., Ltd.) so that particles were supplied from the first wire mesh side.

[0117] 2. Preparation of Colored Resin Particles (1) Preparation of polymerizable monomer composition for core 77 parts of styrene and 23 parts of n-butyl acrylate as monovinyl monomers, 7 parts of carbon black (manufactured by Mitsubishi Chemical Corporation, product name: #25B) as a colorant, 0.6 parts of divinylbenzene as a crosslinkable polymerizable monomer, 1.2 parts of t-dodecyl mercaptan as a molecular weight modifier, 0.3 parts of polymethacrylic acid ester macromonomer (manufactured by Toa Gosei Chemical Industry Co., Ltd., product name: AA6, Tg = 94 ° C.) as a macromonomer, and 1.0 parts of polar resin (copolymer 1 obtained in Production Example 1) were wet-ground using a media-type wet grinder to obtain a mixture. 1 part of charge control resin (styrene acrylic resin containing quaternary ammonium salt as functional group, copolymerization ratio of monomer containing quaternary ammonium salt functional group: 2 mass%) as a charge control agent and 20 parts of behenyl stearate (number average molecular weight Mn: 592) as a mold release agent were added to this mixture and mixed to obtain a polymerizable monomer composition for cores.

[0118] (2) Preparation of aqueous dispersion medium Separately, in a stirring tank at room temperature, an aqueous solution of 4.1 parts of sodium hydroxide (alkali metal hydroxide) in 50 parts of ion-exchanged water was gradually added to an aqueous solution of 7.4 parts of magnesium chloride (water-soluble polyvalent metal salt) in 250 parts of ion-exchanged water while stirring, to prepare a magnesium hydroxide colloid (poorly water-soluble inorganic hydroxide colloid) dispersion.

[0119] (3) Preparation of polymerizable monomer for shell On the other hand, 2 parts of methyl methacrylate and 65 parts of ion-exchanged water were subjected to a fine dispersion treatment using an ultrasonic emulsifier to prepare an aqueous dispersion of a polymerizable monomer for the shell.

[0120] (4) Preparation of suspension The core polymerizable monomer composition was added to the magnesium hydroxide colloidal dispersion and stirred, and 6 parts of t-butyl peroxyisobutyrate (manufactured by NOF Corp., product name: Perbutyl IB) was added thereto as a polymerization initiator. Thereafter, using an in-line type emulsifying disperser (manufactured by Pacific Machinery Works, Ltd., product name: Milder), the rotor peripheral speed was set to 23.6 m / s, the number of revolutions was set to 15,000 rpm, and a dispersion treatment was performed while circulating the dispersion until the circulation number of the dispersion calculated by the formula (I) reached 10, thereby preparing a suspension in which droplets of the core polymerizable monomer composition were dispersed in an aqueous dispersion medium.

[0121] (5) Formation of colored resin particles To the suspension prepared above, 1 part of sodium tetraborate decahydrate was added. The suspension to which sodium tetraborate decahydrate was added was placed in a reactor equipped with an agitator, and the temperature was raised to 85°C to carry out a polymerization reaction. After the polymerization conversion rate reached almost 100%, the aqueous dispersion of the shell polymerizable monomer prepared above and 0.3 parts of 2,2'-azobis(2-methyl-N-(2-hydroxyethyl)-propionamide) (manufactured by Wako Pure Chemical Industries, Ltd., trade name: VA-086, water-soluble) as a shell polymerization initiator were added to the reactor. After further continuing the polymerization for 4 hours, the reaction was stopped by cooling with water to obtain an aqueous dispersion of colored resin particles having a core-shell structure.

[0122] (6) Post-processing The aqueous dispersion of the colored resin particles was washed with dilute sulfuric acid (25°C, 10 minutes) to adjust the pH to 4.5 or less. Next, the water was separated by filtration, and 200 parts of ion-exchanged water was added to reslurry the mixture, followed by a water washing treatment in which washing, filtration, and dehydration were repeated several times at room temperature (25°C). The solid content thus obtained was separated by filtration to obtain colored resin particles with a water content of 10%. The water content of the colored resin particles was determined by the weight loss when the particles were dried in an oven at 105°C for 2 hours.

[0123] 3. First external addition process To 100 parts of the obtained colored resin particles, 0.2 parts of hydrophobic silica microparticles having a number-average primary particle size of 7 nm and having been hydrophobized with cyclic silazane were added as an external additive, and the mixture was mixed and stirred at 45°C for 10 hours using a conical mixer (manufactured by Hosokawa Micron Corporation, product name: Nauta Mixer) and dried.

[0124] 4. Sieving process Using the blow-through sieve, the blower volume was set at 14 m 3 / min, primary air flow rate F1 is 13.4m 3 / min, secondary air flow rate F2 is 0.6m 3 / min, and the particles obtained in the first external addition step were supplied to a sieve by an air flow for 1 hour, thereby sieving the particles.

[0125] 5. Second external addition process To the mixed particles (100 parts of colored resin particles, 0.2 parts of hydrophobic silica microparticles) obtained by the above sieving process, 1 part of hydrophobic silica microparticles having a number average primary particle size of 35 nm that had been hydrophobized with amino-modified silicone oil was added as an external additive, and the mixture was mixed and stirred using a high-speed mixer (manufactured by Nippon Coke & Engineering Co., Ltd., product name: FM Mixer) to perform external addition treatment, thereby producing the toner for developing electrostatic images of Example 1.

[0126] [Examples 2 to 6 and Comparative Examples 1 to 4] In Example 1, the first and second wire meshes used in the laminated wire mesh were made of wire meshes with the mesh sizes shown in Table 1, and the flow rates F1 and F2 of the primary air and secondary air in the sieving process were changed according to Table 1. Except for this, the toners for developing electrostatic images of Examples 2 to 6 and Comparative Examples 1 to 4 were prepared in the same manner as in Example 1.

[0127] [Comparative Example 5] The toner for developing electrostatic images of Comparative Example 5 was prepared in the same manner as in Example 1, except that a vibrating sieve (a circular vibrating sieve made by Kowa Kogyo Co., Ltd.) was used as the sieve instead of the blow-through sieve, and the first and second wire meshes used in the laminated wire mesh had the mesh openings shown in Table 1.

[0128] [Comparative Example 6] 1. Preparation of the sieve The same sieve as that used in Example 1 was used.

[0129] 2. Preparation of Colored Resin Particles <Preparation of Resin Particle Dispersion> 320 parts of styrene, 80 parts of n-butyl acrylate, 9 parts of β-carboxyethyl acrylate, 1.5 parts of 1,10-decanediol diacrylate, and 2.7 parts of dodecanethiol were mixed and dissolved. The resulting mixture was dissolved in 550 parts of ion-exchanged water containing 4 parts of anionic surfactant, and further dispersed and emulsified in a stirring tank, and 50 parts of ion-exchanged water in which 6 parts of ammonium persulfate were dissolved was added while gradually stirring and mixing for 10 minutes. Next, after sufficient nitrogen replacement in the system, the stirring tank jacket was heated while stirring the inside of the stirring tank until the temperature inside the tank reached 70 ° C., and emulsion polymerization was continued for 5 hours to obtain a resin particle dispersion.

[0130] <Preparation of Colorant Particle Dispersion> 90 parts of a phthalocyanine pigment (PVFASTBLUE, manufactured by Dainichi Seiyaku Co., Ltd.), 10 parts of an anionic surfactant (Neogen R, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.), and 240 parts of ion-exchanged water were mixed in a stirring tank, and the mixture was dispersed using an Ultimizer HJP-25070 (manufactured by Sugino Machine Ltd.) set to a dispersion pressure of 196 MPa to prepare a colorant particle dispersion liquid.

[0131] <Preparation of release agent dispersion> 30 parts of paraffin wax, 2.5 parts of anionic surfactant, and 67.5 parts of ion-exchanged water were heated to 95° C. and dispersed using a homogenizer, and then dispersed using a Dyno-Mill to obtain a release agent dispersion.

[0132] <Preparation of colored resin particles> 400 parts of ion-exchanged water, 240 parts of resin particle dispersion, 44 parts of colorant dispersion, 56 parts of release agent dispersion, 12 parts of inorganic fine particle dispersion (Nissan Chemical Industries, Snowtex OL) and 10 parts of inorganic fine particle dispersion (Nissan Chemical Industries, Snowtex OS) were added to a stirring tank and thoroughly mixed and dispersed with a homogenizer. A mixture of 0.5 parts of coagulant (Asada Chemical Industries, polyaluminum chloride) and 100 parts of ion-exchanged water was added to the obtained dispersion over 10 minutes while stirring the stirring tank, and after the addition was completed, the mixture was slowly heated to 40°C and held for 30 minutes, and then heated to 49°C. After holding at 49°C for 40 minutes, the temperature was further increased to 52°C and held for 40 minutes. To the dispersion, 65 parts of the above resin particle dispersion was slowly added, and the temperature was further increased to 53° C. and maintained for 1 hour. Next, 1 mol / L aqueous sodium hydroxide solution was added so that the pH became 6.0, and then the mixture was slowly heated to 85°C while continuing stirring and held for 60 minutes, then heated to 96°C, 1 mol / L aqueous nitric acid solution was added until the pH became 5.0, and held for 5 hours. Thereafter, the obtained toner slurry was cooled to 40° C., sieved through a mesh with 15 μm openings, and then filtered through a filter press (manufactured by Tokyo Engineering Co., Ltd.) to obtain colored resin particles.

[0133] For 100 parts of the obtained colored resin particles, 500 parts of ion-exchanged water was passed through the toner in a filter press device, followed by passing an acid washing solution prepared by adding 1 mol / L of nitric acid aqueous solution to 300 parts of ion-exchanged water until the pH reached 3.0, and then passing another 400 parts of ion-exchanged water through the toner. After squeezing and dehydrating, a wet toner was obtained. This wet toner was crushed with a Randel Mill RM-1 (manufactured by Tokuju Kogyosho) to obtain a wet toner as a dry raw material.

[0134] Drying was performed using a loss-in-weight feeder (602 model, manufactured by Kuma Engineering Co., Ltd.) as the wet toner feeder and a flash jet dryer (manufactured by Seishin Enterprise Co., Ltd.) as the airflow dryer. A Henschel mixer (manufactured by Mitsui Mining Co., Ltd.) was used as the external additive mixer. Toner particles were obtained by mixing 1.5 parts of hydrophobic silica (volume average particle size 0.1 μm), 0.55 parts of cerium oxide (volume average particle size 0.7 μm), and 0.3 parts of zinc stearate (volume average particle size 7.69 μm) as external additives with 100 parts of toner.

[0135] 3. Sieving process Using the blow-through sieve, the blower volume was set at 14 m 3 / min, primary air flow rate F1 is 12.8m 3 / min, secondary air flow rate F2 is 1.2m 3 The toner particles obtained were supplied to a sieve for 1 hour by air flow to sieve the particles, thereby preparing the toner for developing electrostatic images of Comparative Example 6.

[0136] [evaluation] The electrostatic image developing toners obtained in the respective Examples and Comparative Examples were measured or evaluated by the following methods.

[0137] 1. Average equivalent circle diameter and average circularity of toner A dispersion liquid in which 10 g of toner was dispersed in 300 g of water containing 0.3% surfactant was used as the sample liquid, and a flow type particle image analyzer (manufactured by CIMEX, product name: FPIA-3000) was used to take a projection image of the particles in the sample liquid, and the diameter of a circle equivalent to the projected area of ​​the particle was measured from the projection image to obtain the equivalent circle diameter of each toner particle. The circularity of each toner particle was obtained by measuring the perimeter of a circle equivalent to the projected area of ​​the particle and the perimeter of the projected particle image from the projection image, and using the above calculation formula 1. The arithmetic mean of the equivalent circle diameters of each toner particle contained in the sample liquid was calculated to obtain the average equivalent circle diameter, and the arithmetic mean of the circularities was calculated to obtain the average circularity.

[0138] 2. Number of coarse particles in toner A toner dispersion liquid in which 10 g of toner was dispersed in 300 g of water containing 0.3% surfactant was passed through a sieve with a mesh size of 25 μm. The water containing the surfactant was then passed through the sieve again until the water passing through the sieve no longer had the color of the toner to the naked eye. The coarse particles remaining on the sieve were then collected with water containing 0.3% surfactant to obtain a coarse particle dispersion liquid, and the mass of the obtained dispersion liquid was recorded. The particle size distribution of the coarse particle dispersion liquid was measured using a flow-type particle image measuring device, and the number of coarse particles A having a circle-equivalent diameter of 50 μm or more and less than 200 μm and a circularity of 0.20 to 0.97, and the number of coarse particles B having a circle-equivalent diameter of 50 μm or more and less than 200 μm and a circularity of 0.97 to 1.00 were measured. The number of particles N of coarse particles A contained in the coarse particle dispersion liquid in the measurement cell A (pieces) and the number of coarse particles B N B (pieces), the capacity of the measurement cell C (g), and the total mass of the coarse particle dispersion W D (g), and the mass W of the toner used in the measurement T From (g), the number of coarse particles A and the number of coarse particles B contained in 1.0 g of toner were calculated using the above-mentioned calculation formulas (A) and (B). In addition, by using a similar method, the number of coarse particles A having a circularity of 0.95 or more and less than 0.97 was determined.

[0139] 3. Recovery rate In each Example and Comparative Example, after sieving, the weight A of the particles in the coarse particle recovery container and the weight B of the particles in the recovery container that passed through the sieve were measured, and the recovery rate was calculated using the following formula. Recovery rate (%) = {B / (A+B)} x 100

[0140] 4. Evaluation of white streaks under L / L or H / H conditions A commercially available non-magnetic single-component development printer (printing speed: 20 sheets / min) and the toner to be evaluated were left for 24 hours in a low temperature and low humidity (L / L) environment (temperature: 10°C, relative humidity: 20% RH) or a high temperature and high humidity (H / H) environment (temperature: 32.5°C, relative humidity: 80% RH). After that, a print test was performed in the same environment with a print density of 5%, and a solid black print (print density 100%) was performed every 1,000 sheets to check for the occurrence of white vertical streaks (white streaks). The number of sheets when a white vertical streak was first observed on a solid black image (number of sheets with white streaks) was counted, and the print test was performed up to a maximum of 10,000 sheets. If no white streaks occurred in the printing test up to 10,000 sheets, it will be indicated as ">10000" in Table 1.

[0141] 5. Fog evaluation under H / H environment A printing test similar to the above white streak evaluation was performed under a high temperature and high humidity (H / H) environment (temperature: 32.5°C, relative humidity: 80% RH), and a solid black print (print density 100%) was performed every 1,000 sheets, followed by a solid white print (print density 0%). The printer was stopped in the middle of printing the solid white, and the toner in the non-image area on the photoreceptor after development was attached to an adhesive tape, which was then attached to a print paper. Next, the whiteness (B) of the print paper to which the adhesive tape was attached was measured with a whiteness meter, and in the same manner, only an unused adhesive tape was attached to the print paper, and its whiteness (A) was measured, and the difference in whiteness (BA) was taken as the fog value. The number of sheets (number of sheets with fog) when the fog value first reached 2.0 or more was counted, and the print test was performed up to a maximum of 10,000 sheets. In addition, if the fog value is less than 2.0 in the printing test of up to 10,000 sheets, it is indicated as ">10000" in Table 1.

[0142] [Table 1]

[0143] [Consideration] In the toner obtained in Comparative Example 1, the number of coarse particles A exceeded 20,000 and the number of coarse particles B was 1,000 or more per 1.0 g of toner, so that white streaks occurred in the printing test in an L / L environment. In the toner obtained in Comparative Example 2, the number of coarse particles A and B in the toner was even greater than in Comparative Example 1, so that white streaks occurred earlier in the printing test in an L / L environment and also in the printing test in an H / H environment. In Comparative Examples 1 and 2, it is considered that the mesh openings of the screen used in the sieving process were too large, so that coarse particles A and B passed through in the sieving process, and the amounts of coarse particles A and B remaining in the toner were large. In Comparative Example 3, in the screening process, particles were supplied to the sieve with an air flow in which the ratio (F1 / F2) of the primary air flow rate F1 to the secondary air flow rate was 8, resulting in a sudden increase in differential pressure, which caused the process to be stopped midway. The toners obtained in Comparative Examples 4 to 6 had less than 1000 particles of coarse particles A per 1.0 g of toner, and thus fog occurred in the printing test under H / H environment. In Comparative Example 4, in the sieving step, the particles were supplied to the sieve with an air flow in which the ratio (F1 / F2) of the flow rate of the primary air F1 to the flow rate of the secondary air was 139, and since the ratio of F1 to F2 was too large, the opportunity for the coarse particles that did not pass through the sieve to be supplied again to the sieve by the secondary air was reduced, and it is considered that both the coarse particles A and the coarse particles B were difficult to pass through the sieve, and the coarse particles A could not be appropriately left in the toner. In Comparative Example 5, in the sieving step, the vibrating sieve machine used in Example 1 of Patent Document 1 was used, and the sieving step was performed without using an air flow, so it is considered that both the coarse particles A and the coarse particles B were difficult to pass through the sieve, and the coarse particles A could not be appropriately left in the toner. In Comparative Example 6, a toner was produced under conditions similar to those of Example 1 of Patent Document 2. That is, colored resin particles were produced by an emulsion aggregation method, and in the sieving process, the particles were supplied to a sieve in an air flow in which the ratio (F1 / F2) of the flow rate of the primary air to the flow rate of the secondary air was 11. It is considered that, in the production method of colored resin particles carried out in Comparative Example 6, coarse particles A and coarse particles B were hardly generated, and therefore the amount of both coarse particles A and coarse particles B in the toner was small.

[0144] In contrast, the toners obtained in Examples 1 to 6 had a particle count of 1,000 to 20,000 particles of coarse particles A and less than 1,000 particles of coarse particles B per 1.0 g of toner, so that no white streaks occurred in the above printing test in either an H / H environment or an L / L environment, and no fogging occurred in the above printing test in an H / H environment. In Examples 1 to 6, in the sieving step, the particles were supplied to a sieve using an air flow, the mesh size of the mesh with the smallest opening among the meshes used in the sieve was set to 25 μm to 40 μm, and the flow rate F1 of the primary air and the flow rate F2 of the secondary air that generate the air flow were set to 1000 μm. 3 / min] (F1 / F2) was set to 18 or more and 50 or less. As a result, it is considered that coarse particles B with a relatively high circularity were not allowed to pass through the sieve, while coarse particles A with a relatively low circularity were allowed to pass through the sieve to an appropriate extent, thereby enabling coarse particles B to be sufficiently removed while allowing coarse particles A to remain in the toner to an appropriate extent. [Explanation of symbols]

[0145] 1 Ejector 2 Air blowing nozzle 3 Powder suction nozzle 4 Powder 5 Air blowing direction 6 Powder intake direction 7 Direction of dispersed powder 11 Feeding machine 12 Primary air intake mechanism 13 Sieve machine 14 net 15 Coarse particle drop hole 16 Secondary air intake mechanism 17 Large particle collection container 18 Piping 19. Cyclone 20 Collection container 21 Blower 22 Flow Control Valve

Claims

1. A toner for developing electrostatic images, comprising a binder resin, colored resin particles containing a colorant and a release agent, and an external additive, The toner has an average equivalent circular diameter of 5 to 9 μm, a toner for developing an electrostatic image, the toner being passed through a sieve having an opening of 25 μm by a wet method, wherein, among the coarse particles that do not pass through the sieve, the number of coarse particles A having a circular equivalent diameter of 50 μm or more and less than 200 μm and a circularity of 0.20 or more and less than 0.97 as measured by a flow type particle image measuring device is 1,000 to 20,000 particles per 1.0 g of the toner passed through the sieve, and the number of coarse particles B having a circular equivalent diameter of 50 μm or more and less than 200 μm and a circularity of 0.97 or more and less than 1.00 as measured by a flow type particle image measuring device is less than 1,000 particles per 1.0 g of the toner passed through the sieve.

2. 2. The toner for developing electrostatic images according to claim 1, having an average circularity of 0.98 or more and 1.00 or less.

3. A method for producing the toner for developing electrostatic images according to claim 1 or 2, comprising the steps of: A step of preparing a suspension in which droplets of a polymerizable monomer composition containing at least a polymerizable monomer, a colorant, and a release agent are dispersed in an aqueous dispersion medium; and subjecting the suspension to a polymerization reaction in the presence of a polymerization initiator to form colored resin particles.

4. The method further includes a step of removing a part of coarse particles contained in the particles by feeding the particles containing the colored resin particles to a sieve using an air flow, The sieve includes at least one mesh, and the mesh with the smallest opening among the meshes used in the sieve has an opening of 25 μm or more and 40 μm or less; The air flow is generated by primary air supplied together with the particles containing the colored resin particles, and secondary air supplied from the recovery port side of the coarse particles, and the flow rate F1 [m 3 / min] and the flow rate of the secondary air F2 [m 3 4. The method for producing a toner for developing electrostatic images according to claim 3, wherein the ratio (F1 / F2) of the total mass of the toner to the total mass of the toner is 18 or more and 50 or less.

Citation Information

Patent Citations

  • Manufacturing method for toner

    JP2003043744A

  • Method for manufacturing electrostatic charge image developing toner

    JP2007079444A

  • Method for manufacturing electrophotographic toner, and electrophotographic toner

    JP2008076873A