Substrate for semiconductor device, method for manufacturing substrate for semiconductor device, and method for manufacturing wireless communication device

The semiconductor device substrate with reinforcing wires stabilizes FET characteristics on flexible substrates by controlling expansion and contraction, addressing manufacturing challenges and ensuring stable operation.

JP7593107B2Active Publication Date: 2024-12-03TORAY INDUSTRIES INC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2020547150
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-04-28
Filing Date
2020-09-03
Publication Date
2024-12-03
Estimated Expiration
2040-09-03

AI Technical Summary

Technical Problem

Existing methods for manufacturing RFID tags on flexible substrates fail to adequately suppress variations in field-effect transistor (FET) characteristics due to substrate expansion and contraction caused by temperature and humidity, leading to unstable circuit operation and manufacturing challenges.

Method used

A semiconductor device substrate with a resin base material and reinforcing wires made of the same material as the electrode layers, surrounding individual semiconductor devices to stabilize the substrate and control expansion and contraction, using a roll-to-roll manufacturing process.

Benefits of technology

The solution effectively suppresses variations in FET characteristics and maintains stable circuit operation by controlling substrate expansion and contraction, enhancing manufacturing consistency and reducing mechanical stress on the devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007593107000005
    Figure 0007593107000005
  • Figure 0007593107000006
    Figure 0007593107000006
  • Figure 0007593107000007
    Figure 0007593107000007
Patent Text Reader

Abstract

A substrate for a semiconductor device according to an aspect of the present invention has a resin base material, a plurality of semiconductor devices provided on the resin base material, and a reinforcement wire provided to surround the plurality of semiconductor devices. The reinforcement wire is made of the same material as a material constituting at least one of electrode layers included in the plurality of semiconductor devices. A plurality of regions in which one or more of the plurality of semiconductor devices are surrounded by the reinforcement wire are present on the resin base material. A plurality of semiconductor devices such as a wireless communication device can be obtained from said substrate for a semiconductor device.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a substrate for a semiconductor device, a method for manufacturing a substrate for a semiconductor device, and a method for manufacturing a wireless communication device. [Background technology]

[0002] In recent years, wireless communication systems using RFID (Radio Frequency IDentification) technology have been attracting attention. An RFID tag has an IC chip with a circuit composed of field effect transistors (hereinafter referred to as FETs) and an antenna for wireless communication with a reader / writer. The antenna installed in the RFID tag receives a carrier wave transmitted from the reader / writer, and the driving circuit in the IC chip operates.

[0003] RFID tags are expected to be used in a variety of applications, including logistics management, product management, and shoplifting prevention, and have begun to be introduced in some applications, such as IC cards for transportation cards and product tags. In order for RFID tags to be used in all products in the future, it is necessary to reduce the manufacturing cost of RFID tags. Therefore, in the field of RFID technology, a method has been proposed in which RFID tag circuits and antennas are manufactured on flexible substrates using coating and printing techniques (see, for example, Patent Document 1).

[0004] In the FETs that make up the circuits in RFID tags, if there is variation in characteristics (for example, variation in drive current value), it becomes difficult to achieve stable circuit operation according to the design specifications. In particular, when an inexpensive plastic film is used as the substrate, the substrate expands and contracts significantly due to temperature and humidity, and this expansion and contraction causes pattern misalignment of the materials that make up the FET. This makes it impossible to stably manufacture the FETs, and the variation in the FET characteristics becomes large.

[0005] As a technique for suppressing the above-mentioned pattern misalignment, a method has been considered in which an alignment mark is provided on a substrate, the alignment mark is detected, and the temperature and humidity of the substrate are controlled based on the magnitude of the positional misalignment of the detected alignment mark, thereby controlling the expansion and contraction of the substrate (see, for example, Patent Document 2).In addition, a method has been considered in which a gate electrode formed on a substrate is used as a photomask for patterning source and drain electrodes, and exposure is performed from the back side of the substrate to suppress positional misalignment between the electrodes (see, for example, Patent Document 3). [Prior art documents] [Patent documents]

[0006] [Patent Document 1] International Publication No. 2017 / 030070 [Patent Document 2] International Publication No. 2015 / 133391 [Patent Document 3] International Publication No. 2018 / 051860 Summary of the Invention [Problem to be solved by the invention]

[0007] However, the method described in Patent Document 2 can correct the positional deviation of each FET, but cannot suppress the characteristic variation of the FET within the substrate, and has the problem that it is difficult to control the positional deviation of the FET when the substrate is nonuniform (i.e., the distortion is difficult to predict because there is no regularity in the direction or amount of deformation).In addition, the method described in Patent Document 3 can suppress the variation in the electrode formation position of each FET, but cannot suppress the variation between FETs caused by the expansion and contraction of the substrate.

[0008] In addition, both of the methods in Patent Documents 2 and 3 take into consideration suppression of characteristic variations due to the manufacturing process, such as correcting positional misalignment of FETs, but do not take into consideration control of characteristics variations between FETs due to expansion and contraction variations in the substrate due to changes in temperature and humidity after FET formation, or the influence of misalignment of the substrate when FETs are continuously formed on consecutive substrates and wound into a roll.

[0009] The present invention has been made in light of the above-mentioned problems, and aims to provide a substrate for a semiconductor device, a method for manufacturing a substrate for a semiconductor device, and a method for manufacturing a wireless communication device, which are capable of suppressing variations in the characteristics of the semiconductor devices even after a plurality of semiconductor devices such as FETs are formed on the substrate. [Means for solving the problem]

[0010] In order to solve the above problems and achieve the object, the substrate for semiconductor device of the present invention comprises a resin base material and a plurality of semiconductor devices provided on the resin base material, and has a reinforcing wire arranged on the resin base material so as to surround the plurality of semiconductor devices, the reinforcing wire is made of the same material as a material constituting at least one of the electrode layers included in the plurality of semiconductor devices, and there are a plurality of areas on the resin base material in which one or more of the plurality of semiconductor devices are surrounded by the reinforcing wire.

[0011] In addition, in the substrate for semiconductor device according to the present invention, the reinforcing wire is provided so as to surround the plurality of semiconductor devices individually.

[0012] In addition, the substrate for a semiconductor device according to the present invention is characterized in that, in the above invention, the thickness of the reinforcing wire is the same as the thickness of each of the plurality of semiconductor devices or is thinner than the thickness of each of the plurality of semiconductor devices.

[0013] In addition, the substrate for semiconductor device according to the present invention is characterized in that, in the above invention, the resin base material has a longitudinal direction and a transverse direction, the plurality of semiconductor devices are formed in a row in the longitudinal direction on the resin base material, and a portion of the reinforcing wire is provided approximately continuously in the longitudinal direction of the resin base material.

[0014] In addition, the substrate for semiconductor device according to the present invention is characterized in that, in the above invention, the resin base material has a longitudinal direction and a transverse direction, the plurality of semiconductor devices are formed in a row in the longitudinal direction on the resin base material, and a portion of the reinforcing wire is provided approximately continuously in the longitudinal direction of the resin base material at both outer edge portions of the row of the plurality of semiconductor devices.

[0015] Furthermore, in the substrate for semiconductor device according to the present invention, in the above-mentioned invention, the plurality of semiconductor devices each include a field effect transistor, and the field effect transistor has a source electrode, a drain electrode and a gate electrode, a semiconductor layer in contact with the source electrode and the drain electrode, respectively, and a gate insulating layer that insulates the source electrode, the drain electrode and the semiconductor layer from the gate electrode.

[0016] In addition, the substrate for a semiconductor device according to the present invention is characterized in that, in the above-mentioned invention, the semiconductor layer contains carbon nanotubes.

[0017] In addition, the substrate for semiconductor device according to the present invention is characterized in that, in the above invention, the plurality of semiconductor devices each include a field effect transistor, and the reinforcing wire is provided in the same layer as the substrate side electrode and the substrate side electrode, which are located closer to the resin substrate, of the source electrode, drain electrode and gate electrode included in the field effect transistor, and made of the same material as the substrate side electrode and the substrate side electrode.

[0018] In addition, the substrate for semiconductor device according to the present invention is characterized in that, in the above invention, the plurality of semiconductor devices each include a field effect transistor having a bottom gate structure, and the reinforcing wire is provided in the same layer as the gate electrode and made of the same material as that constituting the gate electrode included in the field effect transistor.

[0019] In addition, the substrate for a semiconductor device according to the present invention is characterized in that, in the above invention, at least some of the field effect transistors have a second insulating layer in contact with the semiconductor layer on the side opposite to the gate insulating layer with respect to the semiconductor layer of the field effect transistor, and have second reinforcing wires on the resin base material made of the same material as the material constituting the second insulating layer.

[0020] In addition, the substrate for a semiconductor device according to the present invention is characterized in that, in the above invention, the gate electrode of the field effect transistor and the reinforcing line have the same thickness, and the thickness is 30 nm or more and 500 nm or less.

[0021] In addition, the substrate for a semiconductor device according to the present invention is characterized in that, in the above-mentioned invention, the field effect transistor is a field effect transistor having a top contact structure.

[0022] In addition, in the substrate for semiconductor device according to the present invention, in the above invention, each of the plurality of semiconductor devices is a wireless communication device.

[0023] In addition, the manufacturing method of a substrate for a semiconductor device according to the present invention is a manufacturing method of a substrate for a semiconductor device described in any one of the above-mentioned inventions, characterized in that the formation of any one of the constituent components of the plurality of semiconductor devices and the formation of the reinforcing wire on the resin base material are performed in the same process.

[0024] In addition, the method for manufacturing a substrate for a semiconductor device according to the present invention is characterized in that, in the above-mentioned invention, the formation of the plurality of semiconductor devices and the reinforcing wires is carried out while the resin base material is transported by a roll-to-roll system.

[0025] In addition, the manufacturing method of a substrate for a semiconductor device according to the present invention is characterized in that, in the above invention, the formation of at least one of the electrode layers included in each of the plurality of semiconductor devices and the formation of the reinforcing wire are performed in the same process.

[0026] In addition, the manufacturing method for a substrate for a semiconductor device according to the present invention is characterized in that, in the above invention, the plurality of semiconductor devices are each formed to include a field effect transistor, and among the source electrode, drain electrode and gate electrode included in the field effect transistor, the formation of the substrate side electrode located closer to the resin substrate and the formation of the reinforcing wire are performed in the same process.

[0027] In addition, the manufacturing method of a substrate for a semiconductor device according to the present invention is characterized in that, in the above invention, the multiple semiconductor devices are each formed to include a field effect transistor having a bottom gate structure, and the formation of a gate electrode included in the field effect transistor and the formation of the reinforcing line are performed in the same process.

[0028] In addition, the manufacturing method for a substrate for a semiconductor device according to the present invention is characterized in that, in the above invention, at least a portion of the plurality of field effect transistors are formed to have a second insulating layer that is in contact with the semiconductor layer of the field effect transistor on the side opposite to the gate insulating layer, and the formation of a second reinforcing line made of the same material as that of the second insulating layer and the formation of the second insulating layer on the resin base material are performed in the same process.

[0029] In addition, the manufacturing method for a substrate for a semiconductor device according to the present invention is characterized in that, in the above invention, a reinforcing line forming process in which the gate electrode and the reinforcing line are formed in the same process includes a patterning process in which a metal film formed on the resin base material by sputtering or vacuum deposition is processed into a pattern corresponding to the gate electrode and the reinforcing line.

[0030] In addition, in the manufacturing method for a substrate for a semiconductor device according to the present invention, in the above invention, the reinforcing line formation process, in which the formation of the gate electrode and the formation of the reinforcing line are performed in the same process, includes a film formation process of forming a coating film on the resin base material using a photosensitive paste containing conductive particles and a photosensitive organic component, and a patterning process of processing the coating film into a pattern corresponding to the gate electrode and the reinforcing line by a photolithography method.

[0031] In addition, the method for manufacturing a substrate for semiconductor device according to the present invention is characterized in that, in the above invention, the reinforcing wire is provided so as to surround the plurality of semiconductor devices individually.

[0032] In addition, the manufacturing method for a substrate for a semiconductor device according to the present invention is characterized in that, in the above invention, the resin base material has a longitudinal direction and a transverse direction, the plurality of semiconductor devices are formed in a row in the longitudinal direction on the resin base material, and a portion of the reinforcing wire is provided approximately continuously in the longitudinal direction of the resin base material.

[0033] In addition, the manufacturing method for a substrate for a semiconductor device according to the present invention is characterized in that, in the above invention, the resin base material has a longitudinal direction and a transverse direction, the plurality of semiconductor devices are formed in a row in the longitudinal direction on the resin base material, and a portion of the reinforcing wire is provided approximately continuously in the longitudinal direction of the resin base material at both outer edge portions of the row of the plurality of semiconductor devices.

[0034] In addition, in the method for manufacturing a substrate for a semiconductor device according to the present invention, in the above invention, each of the plurality of semiconductor devices is a wireless communication device or a circuit for a wireless communication device.

[0035] In addition, a method for manufacturing a wireless communication device according to the present invention is characterized by including a step of cutting the substrate for a semiconductor device obtained by the method for manufacturing a substrate for a semiconductor device according to the above invention into individual wireless communication devices.

[0036] In addition, the manufacturing method of a wireless communication device according to the present invention is characterized in that it includes a step of cutting a substrate for a semiconductor device obtained by the manufacturing method of a substrate for a semiconductor device described in the above invention into individual circuits of the wireless communication device, and a step of attaching the cut-out circuits of the wireless communication device to an antenna.

[0037] In addition, the manufacturing method of a wireless communication device according to the present invention is characterized in that it includes a step of bonding a circuit of the wireless communication device of the substrate for a semiconductor device obtained by the manufacturing method of a substrate for a semiconductor device described in the above invention to an antenna, and a step of cutting the substrate for a semiconductor device after the circuit of the wireless communication device and the antenna are bonded together into individual wireless communication devices each including the circuit of the wireless communication device and the antenna. Effect of the Invention

[0038] According to the present invention, it is possible to provide a substrate for a semiconductor device, a manufacturing method for a substrate for a semiconductor device, and a manufacturing method for a wireless communication device, which are capable of suppressing variation in the characteristics of the semiconductor devices even after a plurality of semiconductor devices are formed on the substrate. [Brief description of the drawings]

[0039] [Figure 1] FIG. 1 is a schematic diagram showing a configuration example of a substrate for a semiconductor device according to a first embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic diagram showing a configuration example of a substrate for a semiconductor device according to a modified example of the first embodiment of the present invention. [Diagram 3] FIG. 3 is a schematic diagram showing a configuration example of a substrate for a semiconductor device according to a second embodiment of the present invention. [Figure 4]FIG. 4 is a schematic diagram showing a configuration example of a substrate for a semiconductor device according to a third embodiment of the present invention. [Diagram 5] FIG. 5 is a schematic diagram showing a configuration example of a substrate for a semiconductor device according to a fourth embodiment of the present invention. [Figure 6] FIG. 6 is a schematic diagram showing a configuration example of a substrate for a semiconductor device according to a fifth embodiment of the present invention. [Figure 7] FIG. 7 is a schematic diagram showing a configuration example of a substrate for a semiconductor device according to a first modification of the fifth embodiment of the present invention. [Figure 8] FIG. 8 is a schematic diagram showing a configuration example of a substrate for a semiconductor device according to a second modification of the fifth embodiment of the present invention. [Figure 9] FIG. 9 is a perspective view showing a part of the substrate for a semiconductor device according to the first embodiment of the present invention. [Figure 10] FIG. 10 is a schematic cross-sectional view taken along line II' of the substrate for the semiconductor device shown in FIG. [Figure 11] FIG. 11 is a schematic cross-sectional view showing a first modified example of the substrate for a semiconductor device shown in FIG. [Figure 12] FIG. 12 is a schematic cross-sectional view showing a second modified example of the substrate for a semiconductor device shown in FIG. [Figure 13] FIG. 13 is a schematic diagram showing an example of a configuration of a substrate for a semiconductor device according to a sixth embodiment of the present invention. [Figure 14] FIG. 14 is a schematic cross-sectional view of the substrate for the semiconductor device shown in FIG. 13 taken along line II-II'. [Figure 15] FIG. 15 is a schematic cross-sectional view showing a first modified example of the substrate for a semiconductor device shown in FIG. [Figure 16] FIG. 16 is a schematic cross-sectional view showing a second modified example of the substrate for a semiconductor device shown in FIG. [Figure 17] FIG. 17 is a perspective view for explaining an example of a method for manufacturing a substrate for a semiconductor device according to the fifth embodiment of the present invention. [Figure 18A] FIG. 18A is a partial enlarged schematic view showing an example of a first step of a method for manufacturing a substrate for a semiconductor device according to a fifth embodiment of the present invention. [Figure 18B] FIG. 18B is a partial enlarged schematic view showing an example of a second step in the method for manufacturing a substrate for a semiconductor device according to the fifth embodiment of the present invention. [Figure 19A] FIG. 19A is a partial enlarged schematic view showing an example of a first step of a method for manufacturing a substrate for a semiconductor device according to a sixth embodiment of the present invention. [Figure 19B] FIG. 19B is a partial enlarged schematic view showing an example of a second step in the method for manufacturing a substrate for a semiconductor device according to the sixth embodiment of the present invention. [Figure 20] FIG. 20 is a schematic diagram showing a first configuration example of a wireless communication device to which the present invention is applied. [Figure 21] FIG. 21 is a schematic diagram showing a second configuration example of a wireless communication device to which the present invention is applied. [Figure 22A] FIG. 22A is a schematic view showing an example of a first step of the method for manufacturing a substrate for a semiconductor device according to Example 1 of the present invention. [Figure 22B] FIG. 22B is a schematic view showing a second example of a process of the method for manufacturing the substrate for the semiconductor device according to the first embodiment of the present invention. [Diagram 23] FIG. 23 is a schematic diagram showing an example of a substrate sample obtained from the substrate for semiconductor device of Example 2. As shown in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0040] Hereinafter, preferred embodiments of a substrate for a semiconductor device, a method for manufacturing a substrate for a semiconductor device, and a method for manufacturing a wireless communication device according to the present invention will be described in detail with reference to the drawings as appropriate. Note that the present invention is not limited to these embodiments, and various modifications are possible within the scope of the present invention as long as the object of the invention can be achieved and the gist of the invention is not deviated from.

[0041] <Substrate for semiconductor device> A substrate for a semiconductor device according to an embodiment of the present invention is a substrate for a semiconductor device, comprising a resin base material and a plurality of semiconductor devices provided on the resin base material, a reinforcing wire provided on the resin base material so as to surround the semiconductor devices, the reinforcing wire being made of the same material as a material constituting at least one of the electrode layers included in the semiconductor devices, and the reinforcing wire being provided so as to surround each region including one or more semiconductor devices. In other words, a substrate for a semiconductor device according to an embodiment of the present invention is a substrate for a semiconductor device, comprising a resin base material and a plurality of semiconductor devices provided on the resin base material, a reinforcing wire provided on the resin base material so as to surround the plurality of semiconductor devices, the reinforcing wire being made of the same material as a material constituting at least one of the electrode layers included in the plurality of semiconductor devices, and there are a plurality of regions on the resin base material in which one or more of the plurality of semiconductor devices are surrounded by the reinforcing wire.

[0042] (Embodiment 1) FIG. 1 is a schematic diagram showing a configuration example of a substrate for a semiconductor device according to the first embodiment of the present invention. As shown in FIG. 1, a substrate for a semiconductor device 50 according to the first embodiment of the present invention has a resin base material 1 and has a plurality of semiconductor devices, for example, nine semiconductor devices 10, on the resin base material 1. The substrate for a semiconductor device 50 also has a plurality of (for example, four) reinforcing wires 11a-11d extending in the lateral direction of the resin base material 1 and a plurality of (for example, four) reinforcing wires 12a-12d extending in the vertical direction of the resin base material 1 on the resin base material 1. The reinforcing wires 11a-11d and the reinforcing wires 12a-12d are arranged so as to intersect each other at right angles, and surround the plurality of semiconductor devices 10 individually. At this time, there are a plurality of regions (nine in the first embodiment as illustrated in FIG. 1) on the resin base material 1 in which the semiconductor devices 10 are surrounded by the reinforcing wires 11a-11d and the reinforcing wires 12a-12d. In addition, when the resin base material 1 has edges parallel to the lateral direction thereof, the reinforcing wires 11a to 11d are preferably arranged parallel to the parallel edges of the resin base material 1.

[0043] The horizontal and vertical directions of the resin substrate 1 are perpendicular to each other and perpendicular to the thickness direction of the resin substrate 1. The thickness direction of the resin substrate 1 is perpendicular to the plane of the drawing (the plane of FIG. 1 in the first embodiment). The definitions of the thickness direction, horizontal direction, and vertical direction of the resin substrate 1 are common to all the embodiments of the present invention.

[0044] In the first embodiment, the resin base material 1 is a base material having a longitudinal direction and a lateral direction. For example, in the resin base material 1 shown in FIG. 1, the longitudinal direction of the resin base material 1 is the lateral direction of the resin base material 1, and the lateral direction of the resin base material 1 is the vertical direction of the resin base material 1. Nine semiconductor devices 10 are formed in rows in the longitudinal direction on the resin base material 1. In the example shown in FIG. 1, the rows of the semiconductor devices 10 include three semiconductor devices 10 in each row, and are rows lined up in the lateral direction (vertical direction). The number of rows of the semiconductor devices 10 is three. Some of the reinforcing wires 11a to 11d, for example, the reinforcing wires 11a and 11d located at both ends of the lateral direction of the resin base material 1 among these reinforcing wires 11a to 11d, are continuously provided in the longitudinal direction of the resin base material 1 at the outer edge of the row of the semiconductor devices 10 (a total of three rows in FIG. 1). That is, the reinforcing wires 11a and 11d are reinforcing wires provided continuously on both outer edge portions of the row of the semiconductor devices 10. Note that both outer edge portions of the row of the semiconductor devices 10 can also be referred to as both outer edge portions extending in the longitudinal direction of the resin base material 1, and this point is common to all of the embodiments described below.

[0045] Since the substrate 50 for a semiconductor device has the reinforcing wires 11a-11d and the reinforcing wires 12a-12d, the substrate 50 for a semiconductor device can suppress in-plane expansion and contraction of the resin base 1 when exposed to environmental changes such as humidity and temperature. Therefore, the variation in characteristics among the nine semiconductor devices 10 caused by the variation in expansion and contraction of the substrate 50 for a semiconductor device can be suppressed.

[0046] The material used for the resin base material 1 is not particularly limited, but it is sufficient that at least the substrate surface on which the semiconductor device 10 is disposed is an insulating material. As the material for such a resin base material 1, for example, a resin such as polyimide (PI) resin, polyester resin, polyamide resin, epoxy resin, polycarbonate resin, cellulose-based resin, polyamideimide resin, polyetherimide resin, polyetherketone resin, polysulfone resin, polyphenylene sulfide (PPS) resin, cycloolefin resin, or a sheet containing polypropylene (PP) is preferably used. However, the material used for the resin base material 1 is not limited to these.

[0047] Among these, at least one resin selected from polyethylene terephthalate (PET), polyethylene naphthalate, PPS, polyphenylene sulfone, cycloolefin polymer, polyamide, and PI is preferably used as the material for the resin substrate 1. From the viewpoint of low cost, a PET film is preferable as the material for the resin substrate 1.

[0048] From the viewpoint of adhesion between the resin base material 1 and the electrodes and wiring, polysulfone resin and PPS resin are also preferred materials for the resin base material 1. This is presumably because metal atoms in the electrodes and wiring strongly interact with sulfur atoms contained in these resins.

[0049] The thickness of the resin base 1 is preferably 25 μm or more and 100 μm or less. When the thickness of the resin base 1 is within this range, the substrate 50 for a semiconductor device can have high durability and appropriate flexibility.

[0050] The reinforcing wires 11a-11d and the reinforcing wires 12a-12d are preferably all made of the same material and have the same thickness. The thicknesses of the reinforcing wires 11a-11d and the reinforcing wires 12a-12d are preferably the same as the thicknesses of the semiconductor devices 10 or thinner than the thicknesses of the semiconductor devices 10. If the reinforcing wires are thicker than the thicknesses of the semiconductor devices 10, the reinforcing wires are likely to become charged due to friction between the resin base material 1 and the reinforcing wires when the semiconductor device substrate 50 is stacked or wound into a roll, and as a result, the semiconductor device 10 is likely to be damaged.

[0051] In the present invention, the "thickness of the semiconductor device" refers to the thickness, in a cross section of the semiconductor device formed on the resin base material, from the interface between the resin base material and the semiconductor device to the highest point of the semiconductor device in the vertical direction (thickness direction) of the resin base material.

[0052] Furthermore, the reinforcing wires 11a-11d and the reinforcing wires 12a-12d are each made of the same material as the material constituting at least one of the electrode layers included in the plurality of semiconductor devices 10. That is, the material used for the reinforcing wires 11a-11d and the reinforcing wires 12a-12d is the same material as the material for at least one of the electrode layers, which is one of the layers constituting the semiconductor device 10. This makes it possible to reduce the manufacturing cost of the substrate 50 for a semiconductor device.

[0053] In the present invention, "the reinforcing wire and at least one of the electrode layers constituting the semiconductor device are made of the same material" means that the elements contained in the "reinforcing wire" and "at least one of the electrode layers constituting the semiconductor device" have the same element content with the highest molar ratio. The types and content ratios of the elements in the "reinforcing wire" and "at least one of the electrode layers constituting the semiconductor device" can be identified by elemental analysis such as X-ray photoelectron spectroscopy (XPS) or secondary ion mass spectrometry (SIMS).

[0054] In addition, the multiple (nine in the first embodiment) semiconductor devices 10 may all be the same, or some or all of them may be different, but it is preferable that the materials constituting the semiconductor devices 10, the layer configuration, and the thickness of each layer are the same. Details of the semiconductor device 10 will be described later.

[0055] (Modification of the first embodiment) FIG. 2 is a schematic diagram showing a configuration example of a substrate for a semiconductor device according to a modification of the first embodiment of the present invention. In the first embodiment described above, all of the semiconductor devices 10 are individually surrounded by the reinforcing wires 11a-11d and the reinforcing wires 12a-12d, but this is not limited thereto, and a group of the semiconductor devices 10 may be surrounded by the reinforcing wires. For example, as shown in FIG. 2, a substrate for a semiconductor device 50A according to this modification has reinforcing wires 11a, 11b, 11d and reinforcing wires 12a, 12b, 12d on a resin base material 1. In the substrate for a semiconductor device 50A, four regions are formed in which one or more of the semiconductor devices 10 are surrounded by these reinforcing wires 11a, 11b, 11d and the reinforcing wires 12a, 12b, 12d. As shown in FIG. 2, the regions in this modification include a region including one semiconductor device 10, a region including a group of two semiconductor devices 10, and a region including a group of four semiconductor devices 10.

[0056] In this modification, the shape of the area surrounded by the reinforcing wires 11a, 11b, 11d and the reinforcing wires 12a, 12b, 12d, the number of groups of semiconductor devices 10 surrounded by these reinforcing wires, and the number of semiconductor devices 10 included in the group are not limited to those shown in FIG. 2. For example, the configuration of the reinforcing wire on the resin base material 1 may be a configuration in which three semiconductor devices 10 arranged in the vertical direction of the resin base material 1 are grouped together, and three such groups are formed. However, regarding the configuration of the reinforcing wire, a configuration in which the reinforcing wire is provided so as to surround the plurality of semiconductor devices 10 individually is preferable to a configuration in which the reinforcing wire is provided so as to surround the group of semiconductor devices 10. This is because the reinforcing wire is more likely to reduce the in-plane expansion and contraction variation of the resin base material 1 when the reinforcing wire surrounds the individual semiconductor devices 10 than when the reinforcing wire surrounds the group of semiconductor devices 10.

[0057] In the above-described first embodiment, the reinforcing wires 11a-11d and 12a-12d, and the semiconductor device 10 are formed on the same surface of the resin base material 1, but the present invention is not limited to this. For example, the reinforcing wires 11a-11d and 12a-12d, and the semiconductor device 10 may be formed on opposite surfaces of the resin base material 1.

[0058] In the above-mentioned first embodiment and its modified example, nine semiconductor devices 10 are provided on the resin base material 1, but the present invention is not limited to this. For example, the number of semiconductor devices 10 arranged on the resin base material 1 is not limited to the above-mentioned nine, and may be two or more and less than nine, or may be nine or more. In the above-mentioned first embodiment and its modified example, the semiconductor devices 10 are arranged on the resin base material 1 in three rows and three columns, but the present invention is not limited to this. For example, the above-mentioned reinforcing wires and semiconductor devices can be arranged on the resin base material 1 in any number of rows and columns within a range in which the reinforcing wires and the semiconductor devices can be formed on the resin base material 1.

[0059] The above-described modifications of the first embodiment and its variations can be similarly made to each of the embodiments described below.

[0060] (Embodiment 2) FIG. 3 is a schematic diagram showing a configuration example of a substrate for a semiconductor device according to the second embodiment of the present invention. As shown in FIG. 3, the substrate for a semiconductor device 50B according to the second embodiment of the present invention has a resin base material 1, and has a plurality of semiconductor devices, for example, 12 semiconductor devices 10, on the resin base material 1. The substrate for a semiconductor device 50B also has a plurality of reinforcing wires 13 (for example, 12 wires, the same number as the number of semiconductor devices 10) on the resin base material 1, which surround the semiconductor devices 10 individually. Each of these reinforcing wires 13 is formed in a substantially circular shape, and is arranged so that the reinforcing wires 13 contact each other. For example, there are a plurality of substantially circular regions (12 in FIG. 3) on the resin base material 1 in which the plurality of semiconductor devices 10 are individually surrounded by the reinforcing wires 13. The role of the reinforcing wires 13 in the substrate for a semiconductor device 50B is the same as that in the first embodiment described above.

[0061] In the above-mentioned second embodiment, the reinforcing wires 13 are arranged so as to be in contact with each other, but the present invention is not limited to this, and the reinforcing wires 13 may be arranged so as to be spaced apart from each other. However, it is advantageous to arrange the reinforcing wires 13 so as to be in contact with each other, since this makes it easier to suppress deformation of the entire resin film 1.

[0062] (Embodiment 3) FIG. 4 is a schematic diagram showing a configuration example of a substrate for a semiconductor device according to the third embodiment of the present invention. As shown in FIG. 4, the substrate for a semiconductor device 50C according to the third embodiment of the present invention has a resin base material 1 and has a plurality of semiconductor devices, for example, 18 semiconductor devices 10, on the resin base material 1. The substrate for a semiconductor device 50C also has a plurality of reinforcing wires 14, 15 extending in a direction inclined with respect to the vertical and horizontal directions of the resin base material 1, and a reinforcing wire 16 extending in the horizontal direction of the resin base material 1, on the resin base material 1. A plurality of reinforcing wires 14 (five in FIG. 4) are formed on the resin base material 1 so as to be inclined in a predetermined direction (for example, a direction from the upper left side to the lower right side of the paper surface of FIG. 4) with respect to the horizontal reinforcing wire 16. A plurality of reinforcing wires 15 (four in FIG. 4) are formed on the resin base material 1 so as to be inclined in a direction different from the reinforcing wire 15 with respect to the horizontal reinforcing wire 16 (for example, a direction from the upper right side to the lower left side of the paper surface of FIG. 4). The reinforcing wire 16 is disposed parallel to at least one of both ends of the resin film 1 in the longitudinal direction.

[0063] 4, the reinforcing wires 14-16 intersect with each other on the surface of the resin base material 1 to form triangular regions that individually surround the multiple semiconductor devices 10. There are multiple triangular regions on the resin base material 1, in which the multiple semiconductor devices 10 are individually surrounded by these reinforcing wires 14-16. The roles of the reinforcing wires 14-16 in the substrate 50C for a semiconductor device are similar to those in the first embodiment described above.

[0064] (Embodiment 4) FIG. 5 is a schematic diagram showing a configuration example of a substrate for a semiconductor device according to the fourth embodiment of the present invention. As shown in FIG. 5, the substrate for a semiconductor device 50D according to the fourth embodiment of the present invention has a resin base material 1, and has a plurality of semiconductor devices, for example, 13 semiconductor devices 10, on the resin base material 1. The substrate for a semiconductor device 50D also has reinforcing wires 17 on the resin base material 1, which surround the plurality of semiconductor devices 10 individually. The reinforcing wires 17 are formed to form a plurality of hexagons adjacent to each other, and are arranged on the resin base material 1 to form a so-called honeycomb structure. For example, there are a plurality of hexagonal regions on the resin base material 1 in which the plurality of semiconductor devices 10 are individually surrounded by the reinforcing wires 17. The role of the reinforcing wires 17 in the substrate for a semiconductor device 50D is the same as that in the first embodiment described above.

[0065] (Embodiment 5) FIG. 6 is a schematic diagram showing a configuration example of a substrate for a semiconductor device according to a fifth embodiment of the present invention. As shown in FIG. 6, the substrate for a semiconductor device 50E according to the fifth embodiment of the present invention has a long film-like resin base material 1 that can be continuously unwound from a rolled state and wound into a roll. The substrate for a semiconductor device 50E has a plurality of designs including a plurality of semiconductor devices and reinforcing wires along the longitudinal direction of the resin base material 1 on the resin base material 1 that continues from the rolled state to the rolled state again. The design is a structural part that is configured by combining at least a plurality of semiconductor devices and reinforcing wires on the resin base material 1 and is repeated along the longitudinal direction of the resin base material 1. For example, as shown in FIG. 6, the substrate for a semiconductor device 50E has a design D1 having a plurality of semiconductor devices and reinforcing wires, and a design D2 having a structure similar to that of the design D1.

[0066] As shown in FIG. 6, the design D1 is a structure having nine semiconductor devices 10 described in the above-mentioned first embodiment, four horizontal reinforcing wires 11a-11d, and four vertical reinforcing wires 12a-12d. The design D2 repeats the same structure as the design D1. That is, the nine semiconductor devices included in the design D2 are the same semiconductor devices 10 as the design D1. The four horizontal reinforcing wires 11e-11h included in the design D2 are the same as the reinforcing wires 11a-11d of the design D1, and the four vertical reinforcing wires 12e-12h are the same as the reinforcing wires 12a-12d of the design D1. On the resin base material 1 of the substrate 50E for semiconductor device, these designs D1 and D2 are arranged substantially continuously in the longitudinal direction of the resin base material 1.

[0067] In the fifth embodiment, as shown in FIG. 6, the resin base material 1 is a long base material having a longitudinal direction and a lateral direction, and capable of being continuously transported from a state in which it is wound in a roll to a state in which it is wound up in a roll. That is, the resin base material 1 can be continuously transported in its longitudinal direction by a roll-to-roll method. A plurality of semiconductor devices 10 are formed in a row in the longitudinal direction on the resin base material 1. In the example shown in FIG. 6, the rows of the semiconductor devices 10 are three (three rows) arranged in the lateral direction (vertical direction) of the resin base material 1. That is, the number of rows of the semiconductor devices 10 is three.

[0068] A plurality of reinforcing wires 11a-11h and a part of the reinforcing wires 12a-12h, for example, the reinforcing wires 11a-11h, are provided substantially continuously in the longitudinal direction of the resin base material 1. The reinforcing wires 11a, 11d and the reinforcing wires 11e, 11h are provided substantially continuously in the longitudinal direction of the resin base material 1 at both outer edge portions of the row of the semiconductor device 10. That is, the reinforcing wire 11a in the design D1 and the reinforcing wire 11e in the design D2 are formed continuously in the longitudinal direction of the resin base material 1, except for the gaps between the designs on the resin base material 1. Similarly, the reinforcing wire 11d in the design D1 and the reinforcing wire 11h in the design D2 are formed continuously in the longitudinal direction of the resin base material 1, except for the gaps between the designs on the resin base material 1. By forming the reinforcing wires 11a-11h substantially continuously in the longitudinal direction of the resin base material 1, the bending stress when the resin base material 1 is wound can be periodically (periodically) alleviated, compared to the case where the reinforcing wires are formed continuously. As a result, breakage of the reinforcing wires 11a to 11h can be suppressed.

[0069] In the present invention, the term "provided substantially continuously in the longitudinal direction" refers to a concept including both a state in which the reinforcing line formed in the longitudinal direction on the resin substrate having a longitudinal direction and a lateral direction is continuous in the longitudinal direction of the resin substrate, and a state in which the reinforcing line has small gaps at regular or irregular intervals. An example of the latter is a state in which the reinforcing line is formed at intervals in the longitudinal direction on the resin substrate, such as the reinforcing line 11a in design D1 and the reinforcing line 11e in design D2. When the reinforcing line has a plurality of intervals, it is preferable that each of the reinforcing lines divided by the intervals has a constant length and that the plurality of intervals are also constant. This allows the reinforcing line to be continuously formed at a constant transport feed rate of the resin substrate by photolithography or printing in the manufacturing process of the substrate for the semiconductor device, thereby preventing the manufacturing process from becoming complicated.

[0070] Since the substrate 50E for a semiconductor device has the reinforcing wires 11a-11h and the reinforcing wires 12a-12h, the substrate 50E for a semiconductor device can control the expansion and contraction in the plane of the resin base material 1 for each design when the substrate 50E is exposed to environmental changes such as humidity and temperature. This makes it possible to suppress the variation in characteristics among the nine semiconductor devices 10 in a design and the variation in characteristics among the semiconductor devices 10 for each design formed substantially continuously, which are caused by the variation in expansion and contraction of the substrate 50E for a semiconductor device.

[0071] Moreover, the resin base material 1 has a longitudinal direction and a lateral direction, and the reinforcing wires 11a-11h are preferably arranged parallel to the ends of the resin base material 1 extending in the longitudinal direction (i.e., at least one of both ends of the lateral direction of the resin base material 1). Moreover, the multiple semiconductor devices 10 are preferably arranged in a row parallel to the ends of the resin base material 1 extending in the longitudinal direction. This allows the distortion of the resin base material 1 to be controlled in a direction parallel to the longitudinal direction of the resin base material 1, stabilizing the winding state of the resin base material 1 in the substrate 50E for a semiconductor device, and making it easier to reduce winding misalignment of the resin base material 1 (and thus winding misalignment of the substrate 50E for a semiconductor device) caused by external impacts or changes in temperature or humidity.

[0072] The thickness of the resin base material 1 is preferably 25 μm to 100 μm even if the resin base material 1 is a long base material that can be rolled up. When the thickness of the resin base material 1 is within this range, the substrate 50E for a semiconductor device can have high durability and appropriate flexibility.

[0073] It is preferable that the reinforcing wires 11a-11h and the reinforcing wires 12a-12h are all made of the same material and have the same thickness. In addition, it is preferable that the material used for the reinforcing wires 11a-11h and the reinforcing wires 12a-12h is the same material as that used for at least one of the electrode layers that constitute the semiconductor device 10. This reduces the manufacturing cost of the semiconductor device substrate 50E and improves mechanical impact resistance due to friction when the continuous resin base material 1 is wound into a roll.

[0074] In the above-mentioned fifth embodiment, the reinforcing wires 11a-11h and 12a-12h and the semiconductor device 10 are formed on the same surface of the resin base material 1, but the present invention is not limited to this. For example, the reinforcing wires 11a-11h and 12a-12h and the semiconductor device 10 may be formed on opposite surfaces of the resin base material 1. However, forming these reinforcing wires and the semiconductor device on the same surface of the resin base material 1 is advantageous because it is possible to prevent the reinforcing wires and the semiconductor device from directly rubbing against each other when the continuous resin base material 1 is wound into a roll.

[0075] (First modification of the fifth embodiment) 7 is a schematic diagram showing one configuration example of a substrate for a semiconductor device according to a first modified example of the fifth embodiment of the present invention. In the fifth embodiment described above, a design D1 having nine semiconductor devices 10, four reinforcing wires 11a-11d in the horizontal direction and four reinforcing wires 12a-12d in the vertical direction, and a design D2 having a similar structure are arranged substantially continuously in the longitudinal direction of the resin base material 1 on the resin base material 1 that is continuously wound in a roll shape and wound up in a roll shape, but the configuration of the substrate for a semiconductor device according to the present invention is not limited to this. For example, as shown in FIG. 7, a substrate for a semiconductor device 50F according to a first modified example of the fifth embodiment has a repeating structure of designs D1a and D2a instead of the repeating structure of designs D1 and D2 described above on a resin base material 1 similar to that of the fifth embodiment.

[0076] As shown in FIG. 7, the design D1a is a structure having the nine semiconductor devices 10, three horizontal reinforcing wires 11a-11c, and four vertical reinforcing wires 12a-12d. The design D2a repeats the same structure as the design D1a. That is, the nine semiconductor devices included in the design D2a are the same semiconductor devices 10 as the design D1a. The three horizontal reinforcing wires 11e-11g included in the design D2a are the same as the reinforcing wires 11a-11c of the design D1a, and the four vertical reinforcing wires 12e-12h are the same as the reinforcing wires 12a-12d of the design D1a. On the resin base material 1 of the substrate 50F for semiconductor device, these designs D1a and D2a are arranged substantially continuously in the longitudinal direction of the resin base material 1.

[0077] In the first modification of the fifth embodiment, as shown in FIG. 7, the resin base material 1 has a longitudinal direction and a lateral direction similar to the fifth embodiment. The semiconductor devices 10 are formed in a row in the longitudinal direction on the resin base material 1 similar to the fifth embodiment. The reinforcing wires 11a-11c and the reinforcing wires 11e-11g are formed parallel to the row of the semiconductor devices 10 and are provided substantially continuously in the longitudinal direction of the resin base material 1. That is, the reinforcing wires 11a-11c in the design D1a and the reinforcing wires 11e-11g in the design D2a are formed continuously in the longitudinal direction of the resin base material 1 except for the gaps between the designs on the resin base material 1. In the substrate 50F for semiconductor device according to the first modification, unlike the fifth embodiment, the reinforcing wires 11d and 11h are not formed. Therefore, the reinforcing wires are not provided substantially continuously in the longitudinal direction of the resin base material 1 on one of the outer edge parts of the row of the semiconductor devices 10.

[0078] (Modification 2 of the fifth embodiment) FIG. 8 is a schematic diagram showing a configuration example of a substrate for a semiconductor device according to Modification 2 of the fifth embodiment of the present invention. As shown in FIG. 8, the substrate for a semiconductor device 50G according to Modification 2 has a repeating structure of designs D1b and D2b instead of the repeating structure of designs D1 and D2 described above on a resin base material 1 that is continuous from a state where it is wound in a roll to a state where it is wound up in a roll. Design D1b is a structure portion having the nine semiconductor devices 10 described above, three reinforcing wires 11a, 11c, and 11d in the horizontal direction, and four reinforcing wires 12a to 12d in the vertical direction. Design D2b repeats a structure similar to that of design D1b described above. That is, the nine semiconductor devices included in design D2b are semiconductor devices 10 similar to design D1b described above. Moreover, the three horizontal reinforcing wires 11e, 11g, and 11h included in design D2b are similar to the reinforcing wires 11a, 11c, and 11d of design D1b, and the four vertical reinforcing wires 12e to 12h are similar to the reinforcing wires 12a to 12d of design D1b. On the resin base material 1 of the substrate 50G for a semiconductor device, these designs D1b and D2b are arranged substantially continuously in the longitudinal direction of the resin base material 1.

[0079] In the second modification of the fifth embodiment, as shown in FIG. 8, the resin base material 1 has a longitudinal direction and a lateral direction similar to the fifth embodiment. The semiconductor devices 10 are formed in a row in the longitudinal direction on the resin base material 1 similar to the fifth embodiment. The reinforcing wires 11a, 11c, 11d and the reinforcing wires 11e, 11g, 11h are formed in parallel to the row of the semiconductor devices 10 and are provided substantially continuously in the longitudinal direction of the resin base material 1. That is, the reinforcing wires 11a, 11c, 11d in the design D1b and the reinforcing wires 11e, 11g, 11h in the design D2b are formed continuously in the longitudinal direction of the resin base material 1, except for the gaps between the designs on the resin base material 1.

[0080] In the substrate 50G for semiconductor device according to the second modification, the reinforcing wires 11a, 11d and the reinforcing wires 11e, 11h are provided substantially continuously in the longitudinal direction of the resin base material 1 at both outer edge portions of the row of the plurality of semiconductor devices 10, as in the fifth embodiment. That is, the reinforcing wires 11a and 11d in the design D1b and the reinforcing wires 11e and 11h in the design D2b are formed continuously in the longitudinal direction of the resin base material 1, except for the gaps between the designs on the resin base material 1. In addition, unlike the fifth embodiment, the substrate 50G for semiconductor device does not have the reinforcing wires 11b and 11f. Therefore, the reinforcing wires are not provided substantially continuously in the longitudinal direction of the resin base material 1 in all the rows of the plurality of semiconductor devices 10.

[0081] The arrangement of the reinforcing wires formed substantially continuously on the resin base material 1 is not limited to the above, but it is preferable that all reinforcing wires extending in the longitudinal direction of the resin base material 1 are formed substantially continuously and that the reinforcing wires are provided on both outer edge portions of the row of the plurality of semiconductor devices 10, as in the fifth embodiment and its second modification. This is because, when the resin base material 1 is wound into a roll, it becomes easier to reduce the winding misalignment of the resin base material 1 (and thus the winding misalignment of the substrate for the semiconductor device) caused by external impacts and changes in temperature and humidity. In addition, this effect is enhanced when the reinforcing wires are formed on both outer edge portions of the row of the plurality of semiconductor devices 10 and all between each row, so it is particularly preferable to form the reinforcing wires in this manner.

[0082] <Semiconductor device> Next, a detailed description will be given of semiconductor devices suitable for use in each of the above-mentioned embodiments of the present invention, focusing on a portion of the substrate 50 for a semiconductor device according to the first embodiment as a representative example. As described above, a plurality of semiconductor devices (e.g., the semiconductor device 10 shown in FIG. 1) are used in the substrate for a semiconductor device according to the present invention. For example, each of these plurality of semiconductor devices is a field effect transistor (FET), an IC for various electronic devices equipped with a FET, a TFT array for a display, a TFT memory, a sensor, or a wireless communication device such as an RFID tag. In the present invention, the semiconductor device is not limited to these specific examples.

[0083] Fig. 9 is a perspective view showing an extracted part of the substrate for a semiconductor device according to the first embodiment of the present invention. Fig. 10 is a schematic cross-sectional view taken along line II' of the substrate for a semiconductor device shown in Fig. 9. Figs. 9 and 10 illustrate a case where the semiconductor device 10 (see Fig. 1) of the substrate for a semiconductor device 50 according to the first embodiment is a FET 20, and explain a number of semiconductor devices that are applied to the substrate for a semiconductor device of the present invention. Although not particularly shown, the configuration of the FET 20 is the same when the semiconductor device 10 is a device including the FET 20.

[0084] 9 and 10, the FET 20 has a gate electrode 2 formed on a resin base material 1, a gate insulating layer 3 covering the gate electrode 2, a source electrode 5 and a drain electrode 6 provided thereon, and a semiconductor layer 4 provided between these electrodes. Also, as shown in FIGS. 9 and 10, a substrate 50 for a semiconductor device has a plurality of reinforcing wires 11, 12 on the resin base material 1. The reinforcing wires 11 collectively refer to the horizontal reinforcing wires 11a to 11d in the first embodiment described above. The reinforcing wires 12 collectively refer to the vertical reinforcing wires 12a to 12d in the first embodiment described above.

[0085] 10, the FET 20 has a so-called bottom gate structure in which the gate electrode 2 is disposed below the semiconductor layer 4. When the FET 20 has a bottom gate structure, it is possible to make it difficult for the characteristics of the FET 20 to change due to the material of the resin base material 1.

[0086] In addition, the structure of the FET 20 is not limited to the bottom gate structure illustrated in FIG. 10. FIG. 11 is a schematic cross-sectional view showing a first modified example of the substrate for a semiconductor device shown in FIG. 10. The structure of the FET 20 may be a bottom gate structure in which a gate insulating layer 3 common to a plurality of FETs 20 is formed, as illustrated in FIG. 11. In this case, the reinforcing wire 12 may be covered by the gate insulating layer 3 as illustrated in FIG. 11. Although not particularly illustrated in FIG. 11, the reinforcing wire 11 may also be covered by the gate insulating layer 3, similar to the reinforcing wire 12.

[0087] The reinforcing wires 11 and 12 are made of the same material as that constituting at least one of the electrode layers included in a plurality of semiconductor devices (for example, FET 20). In Figs. 9 and 10, the reinforcing wires 11 and 12 and the gate electrode 2 are formed in the same layer by the same material. Fig. 12 is a schematic cross-sectional view showing a second modification of the substrate for semiconductor device shown in Fig. 10. The reinforcing wires 11 and 12 may be formed in the same layer as the source electrode 5 and the drain electrode 6 by the same material as these electrodes. In that case, the structure of the FET 20 may be a bottom gate structure in which a gate insulating layer 3 common to the plurality of FETs 20 is formed, as exemplified in Fig. 12. In the bottom gate structure of these FETs 20, the reinforcing wires 11 and 12 and the source electrode 5 and the drain electrode 6 are formed on the gate insulating layer 3.

[0088] The fact that the reinforcing wires 11, 12 and the gate electrode 2 are formed in the same layer, or that the reinforcing wires 11, 12 and the source electrode 5 and drain electrode 6 are formed in the same layer, can be confirmed by observing a cross section of the substrate 50 for a semiconductor device using a scanning electron microscope (SEM) or a transmission electron microscope (TEM) or the like.

[0089] 10, the FET 20 has a so-called top-contact structure in which the source electrode 5 and the drain electrode 6 are disposed on the upper surface of the semiconductor layer 4. However, the structure applicable to the FET 20 is not limited to this, and the FET 20 may have a bottom-contact structure.

[0090] 10 and 11 is a so-called bottom gate structure in which the gate electrode 2 is disposed below the semiconductor layer 4 (on the side of the resin base material 1), but is not limited thereto. For example, the FET 20 may be a so-called top gate structure in which the gate electrode 2 is disposed above the semiconductor layer 4 (on the side opposite the resin base material 1). Although not particularly shown, when the FET 20 has a top gate structure, the reinforcing wires 11 and 12 are preferably provided in the same layer as the source electrode 5 and drain electrode 6 located below the semiconductor layer 4, and made of the same material as these source electrode 5 and drain electrode 6.

[0091] From the above, regardless of whether the FET 20 has a bottom gate structure or a top gate structure, it is easier to suppress deformation of the resin base material 1 when the reinforcing wires 11, 12 are provided in the same layer as the electrodes (i.e., the electrodes on the base material side) of the source electrode 5, drain electrode 6, and gate electrode 2 included in the FET 20 that are located closer to the resin base material 1 (e.g., the lower side of the semiconductor layer 4) and made of the same material as the electrodes on the base material side. When the FET 20 has a bottom gate structure, the electrode on the base material side is the gate electrode 2 (see FIGS. 10 and 11). When the FET 20 has a top gate structure, the electrodes on the base material side are the source electrode 5 and the drain electrode 6.

[0092] However, when the FET 20 has a bottom gate structure, the characteristics of the FET 20 are less likely to change due to the material of the resin base material 1 compared to when the FET 20 has a top gate structure.

[0093] (Embodiment 6) Fig. 13 is a schematic diagram showing a configuration example of a substrate for a semiconductor device according to a sixth embodiment of the present invention. Fig. 13 shows a perspective view of a part of a substrate for a semiconductor device 50H according to the sixth embodiment of the present invention. Fig. 14 is a schematic cross-sectional view taken along line II-II' of the substrate for a semiconductor device shown in Fig. 13. In the sixth embodiment of the present invention, a case in which the substrate for a semiconductor device 50H includes a plurality of FETs 20 and FETs 30 as the above-mentioned plurality of semiconductor devices 10 will be illustrated to explain the configuration of the substrate for a semiconductor device according to the present invention and a plurality of semiconductor devices applied thereto.

[0094] As shown in FIG. 13, the semiconductor device substrate 50H has a resin base material 1, and has a plurality of FETs 20, 30, a plurality of reinforcing wires 11, 12, and a plurality of second reinforcing wires 41, 42 on the resin base material 1. The plurality of FETs 20, 30, one set of the FET 20 and the FET 30, constitutes the above-mentioned semiconductor device 10. The reinforcing wires 11, 12 form a plurality of regions on the resin base material 1 surrounding each set of the plurality of FETs 20, 30. The second reinforcing wires 41, 42 are provided on the resin base material 1 along the reinforcing wires 11, 12, respectively. For example, the second reinforcing wire 41 is formed so as to overlap the reinforcing wire 11 in the horizontal direction (the long direction of the resin base material 1). The second reinforcing wire 42 is formed so as to overlap the reinforcing wire 12 in the vertical direction (the short direction of the resin base material 1).

[0095] As shown in FIGS. 13 and 14, the FET 20 and the FET 30 have a gate electrode 2 formed on a resin base material 1, a gate insulating layer 3 covering the gate electrode 2, a source electrode 5 and a drain electrode 6 provided thereon, and a semiconductor layer 4 provided between these electrodes. The FET 30 further has a second insulating layer 7 in contact with the semiconductor layer 4 on the side opposite to the gate insulating layer 3. By forming such a second insulating layer 7 on the semiconductor layer 4, for example, a CNT-FET that normally exhibits p-type semiconductor characteristics can be converted into a semiconductor element that exhibits n-type semiconductor characteristics. The "CNT-FET" is a FET having a semiconductor layer formed of carbon nanotubes (hereinafter referred to as CNTs). For example, in the present embodiment 6, the FET 20 and the FET 30 are each a CNT-FET, and each semiconductor layer 4 of the FET 20 and the FET 30 contains CNTs.

[0096] 14, the FETs 20 and 30 have a so-called bottom gate structure in which the gate electrode 2 is disposed below the semiconductor layer 4. When the FETs 20 and 30 have a bottom gate structure, changes in the characteristics of the FETs 20 and 30 due to the material of the resin base material 1 can be made less likely to occur.

[0097] In addition, the structure of the FETs 20 and 30 is not limited to the bottom gate structure illustrated in FIG. 14. FIG. 15 is a schematic cross-sectional view showing a first modified example of the substrate for a semiconductor device shown in FIG. 13. The structure of the FETs 20 and 30 may be a bottom gate structure in which a gate insulating layer 3 is formed continuously between the multiple FETs 20 and 30, as illustrated in FIG. 15. In this case, the reinforcing wire 12 may be covered by the gate insulating layer 3 as shown in FIG. 15. Although not particularly illustrated in FIG. 15, the reinforcing wire 11 may also be covered by the gate insulating layer 3, similar to the reinforcing wire 12.

[0098] The reinforcing wires 11 and 12 are made of the same material as that constituting at least one of the electrode layers included in a plurality of semiconductor devices (e.g., FETs 20 and 30). In Figs. 13 and 14, the reinforcing wires 11 and 12 and the gate electrode 2 are formed in the same layer by the same material. Fig. 16 is a schematic cross-sectional view showing a second modification of the substrate for semiconductor device shown in Fig. 13. The reinforcing wires 11 and 12 may be formed in the same layer as the source electrode 5 and the drain electrode 6 by the same material as these electrodes. In that case, the structure of the FETs 20 and 30 may be a bottom gate structure in which a gate insulating layer 3 common to the plurality of FETs 20 and 30 is formed, as exemplified in Fig. 16. In the bottom gate structure of these FETs 20 and 30, the reinforcing wires 11 and 12 and the source electrode 5 and the drain electrode 6 are formed on the gate insulating layer 3.

[0099] Moreover, the second reinforcing wires 41, 42 are preferably made of the same material as the second insulating layer 7, regardless of the type of bottom gate structure of the above-mentioned FETs 20, 30. This makes it possible to suppress shaving of the resin base material 1 caused by the second insulating layer 7 that is locally formed.

[0100] 13 and 14, the second reinforcing wire 41 and the second reinforcing wire 42 are formed so as to overlap the reinforcing wire 11 and the reinforcing wire 12, respectively, but they may be formed so as to overlap only a part of the reinforcing wires 11, 12, or so as not to overlap the reinforcing wires 11, 12. Also, in the example shown in Fig. 13, the second reinforcing wire 41 and the second reinforcing wire 42 are formed so as to be continuous with each other, but they may be formed discontinuously.

[0101] 15, the gate insulating layer 3 may be formed to have a structure common to a plurality of FETs 20 and a plurality of FETs 30. In this case, the reinforcing lines 11 and 12 may be covered by the gate insulating layer 3, and second reinforcing lines 41 and 42 may be formed on the gate insulating layer 3.

[0102] The fact that the reinforcing wires 11, 12 and the gate electrode 2 are formed in the same layer, or that the reinforcing wires 11, 12 and the source electrode 5 and drain electrode 6 are formed in the same layer, can be confirmed by observing a cross section of the semiconductor device substrate 50H using a scanning electron microscope (SEM) or a transmission electron microscope (TEM).

[0103] 14, the structure of FET20 and FET30 is a so-called top contact structure in which the source electrode 5 and the drain electrode 6 are disposed on the upper surface of the semiconductor layer 4. However, the structure applicable to FET20 and FET30 is not limited to this, and a bottom contact structure may also be used.

[0104] (gate electrode) The gate electrode 2 may be any material containing a conductive material that can be used as an electrode. Examples of the conductive material of the gate electrode 2 include conductive metal oxides such as tin oxide, indium oxide, and indium tin oxide (ITO). Examples of the conductive material of the gate electrode 2 include metals such as platinum, gold, silver, copper, iron, tin, zinc, aluminum, indium, chromium, lithium, sodium, potassium, cesium, calcium, magnesium, palladium, molybdenum, amorphous silicon, and polysilicon, alloys of a plurality of metals selected from these, and inorganic conductive materials such as copper iodide and copper sulfide. Examples of the conductive material of the gate electrode 2 include polythiophene, polypyrrole, polyaniline, a complex of polyethylenedioxythiophene and polystyrenesulfonic acid, and a conductive polymer whose conductivity is improved by doping with iodine or the like. Examples of the conductive material of the gate electrode 2 include a carbon material, and a material containing an organic component and a conductor.

[0105] When a material containing the organic component and a conductor is used as the material of the gate electrode 2, the flexibility of the gate electrode 2 increases, the adhesion of the gate electrode 2 is good even when bent, and the electrical connection of the gate electrode 2 is good. The organic component contained in such a material is not particularly limited, and examples thereof include monomers, oligomers or polymers, photopolymerization initiators, plasticizers, leveling agents, surfactants, silane coupling agents, defoamers, and pigments. Among these, oligomers or polymers are preferable from the viewpoint of improving the bending resistance of the gate electrode 2. However, the conductive materials of the gate electrode 2 and the wiring are not limited to these. These conductive materials may be used alone, or multiple materials may be stacked or mixed.

[0106] Moreover, the width, thickness, and interval between the gate electrodes 2 are arbitrary. Specifically, the width of the gate electrode 2 is preferably 5 μm or more and 1 mm or less. By setting the width of the gate electrode 2 within this range, it becomes easier to control the overlap between the gate electrode 2 and the source electrode 5 and the drain electrode 6, and to control the FET characteristics by controlling the channel length. When the FET (for example, the above-mentioned FETs 20 and 30) has a bottom gate structure, the thickness of the gate electrode 2 is the same as that of the reinforcing wires 11 and 12, and is preferably 30 nm or more and 500 nm or less. The fact that the thickness of the reinforcing wires 11 and 12 is the same as that of the gate electrode 2 can be confirmed by observing a cross section of the substrate for a semiconductor device using a scanning electron microscope (SEM) or a transmission electron microscope (TEM).

[0107] (Gate insulation layer) The material used for the gate insulating layer 3 is not particularly limited, but may be inorganic materials such as silicon oxide and alumina; organic polymer materials such as polyimide, polyvinyl alcohol, polyvinyl chloride, polyethylene terephthalate, polyvinylidene fluoride, polysiloxane, and polyvinylphenol; or a mixture of inorganic material powder and organic material. Among them, the material for the gate insulating layer 3 preferably contains an organic compound having a bond between a silicon atom and a carbon atom. In addition, the material for the gate insulating layer 3 more preferably contains a metal compound having a bond between a metal atom and an oxygen atom.

[0108] The gate insulating layer 3 may be a single layer or multiple layers. The gate insulating layer 3 may be one layer formed from multiple insulating materials, or multiple insulating layers may be formed by stacking multiple insulating materials.

[0109] (Source and drain electrodes) The source electrode 5 and the drain electrode 6 (hereinafter, appropriately abbreviated as source and drain electrodes) may be any material containing a conductive material that can be used as an electrode. Examples of the conductive material of the source and drain electrodes include conductive metal oxides such as tin oxide, indium oxide, and indium tin oxide (ITO). Examples of the conductive material of the source and drain electrodes include metals such as platinum, gold, silver, copper, iron, tin, zinc, aluminum, indium, chromium, lithium, sodium, potassium, cesium, calcium, magnesium, palladium, molybdenum, amorphous silicon, and polysilicon, alloys of a plurality of metals selected from these, and inorganic conductive materials such as copper iodide and copper sulfide. Examples of the conductive material of the source and drain electrodes include polythiophene, polypyrrole, polyaniline, a complex of polyethylenedioxythiophene and polystyrenesulfonic acid, and a conductive polymer whose conductivity is improved by doping with iodine or the like. Examples of the conductive material of the source and drain electrodes include carbon materials and materials containing an organic component and a conductor.

[0110] When a material containing the organic component and a conductor is used as the conductive material of the source and drain electrodes, the flexibility of the source and drain electrodes is increased, and the adhesion of the source and drain electrodes is good even when bent, and the electrical connection of the source and drain electrodes is good. The organic components contained in such materials are not particularly limited, but include monomers, oligomers or polymers, photopolymerization initiators, plasticizers, leveling agents, surfactants, silane coupling agents, defoamers, pigments, etc. Among these, oligomers or polymers are preferable from the viewpoint of improving the bending resistance of the source and drain electrodes. However, the conductive materials of the source and drain electrodes and wiring are not limited to these. These conductive materials may be used alone, or multiple materials may be laminated or mixed.

[0111] The distance between the source electrode 5 and the drain electrode 6 is preferably 1 μm or more and 500 μm or less. Furthermore, the width and thickness of the wiring connected to the source and drain electrodes are also arbitrary. Specifically, the thickness of the wiring is preferably 0.01 μm or more and 100 μm or less. The width of the wiring is preferably 5 μm or more and 500 μm or less. However, these dimensions are not limited to those mentioned above.

[0112] (Semiconductor layer) The material used for the semiconductor layer 4 is not particularly limited as long as it exhibits semiconductivity, and a material with high carrier mobility is preferably used. In addition, the material for the semiconductor layer 4 is preferably one that can be applied to a simple coating process at low cost, and preferred examples include organic semiconductors and carbon materials.

[0113] As the organic semiconductor used in the semiconductor layer 4, pentacene, polythiophenes, compounds containing a thiophene unit in the main chain, polypyrroles, poly(p-phenylenevinylenes), polyanilines, polyacetylenes, polydiacetylenes, polycarbazoles, polyfurans, polyheteroaryls having a nitrogen-containing aromatic ring as a structural unit, condensed polycyclic aromatic compounds, heteroaromatic compounds, aromatic amine derivatives, biscarbazole derivatives, pyrazoline derivatives, stilbene compounds, hydrazone compounds, metal phthalocyanines such as copper phthalocyanine, metal porphyrins such as copper porphyrin, distyrylbenzene derivatives, aminostyryl derivatives, aromatic acetylene derivatives, condensed ring tetracarboxylic acid diimides, organic dyes, and other known ones can be used. The above organic semiconductors may contain two or more of these.

[0114] Examples of carbon materials used in the semiconductor layer 4 include carbon nanotubes (CNTs), graphene, and fullerenes. Among them, CNTs are preferred as the carbon material because they can be formed at low temperatures of 200°C or less when a roll-to-roll method is used as the transport method for the resin substrate 1, and they are highly suitable for coating processes. Furthermore, unlike organic semiconductors, they do not require crystallization, and high mobility can be achieved by the network structure between CNTs, so that high mobility can be easily maintained even if the sheet substrate expands and contracts due to external factors such as heat and tension. Therefore, CNTs are preferred as the carbon material.

[0115] As the CNT, any of single-walled CNTs in which one carbon film (graphene sheet) is wound in a cylindrical shape, double-walled CNTs in which two graphene sheets are wound concentrically, and multi-walled CNTs in which multiple graphene sheets are wound concentrically may be used, or two or more of these may be used. Among them, from the viewpoint of exhibiting semiconductor properties, it is preferable to use single-walled CNTs, and in particular, it is more preferable that the single-walled CNTs contain 90% by weight or more of semiconducting single-walled CNTs. It is even more preferable that the single-walled CNTs contain 95% by weight or more of semiconducting single-walled CNTs.

[0116] Furthermore, CNTs having a conjugated polymer attached to at least a portion of their surface (hereinafter referred to as a CNT composite) are particularly preferable as the carbon material for the semiconductor layer 4, since they have excellent dispersion stability in a solution and can obtain high mobility. Here, the conjugated polymer refers to a compound whose repeating unit has a conjugated structure and has a degree of polymerization of 2 or more. Furthermore, by using a solution in which CNTs are uniformly dispersed, a film in which CNTs are uniformly dispersed (the film that constitutes the semiconductor layer 4) can be formed by a coating method such as an inkjet method.

[0117] "A state in which a conjugated polymer is attached to at least a part of the surface of a CNT" means a state in which the conjugated polymer covers a part or the entire surface of the CNT. It is presumed that the reason why a conjugated polymer can cover a CNT is because the π-electron clouds derived from each conjugated structure overlap and interact with each other. Whether a CNT is covered with a conjugated polymer can be determined by checking whether the reflected color of the target CNT approaches the color of the conjugated polymer from the color of the uncovered CNT. Quantitatively, the presence of the deposit and the mass ratio of the deposit to the CNT can be identified by elemental analysis such as X-ray photoelectron spectroscopy (XPS).

[0118] The conjugated polymer to be attached to the CNT can be used regardless of its molecular weight, molecular weight distribution, or structure. From the viewpoint of ease of attachment to the CNT, the conjugated polymer preferably has a weight average molecular weight of 1000 or more.

[0119] Examples of methods for attaching a conjugated polymer to CNT include the following first to fourth methods. The first method includes a method of adding CNT to a molten conjugated polymer and mixing it. The second method includes a method of dissolving a conjugated polymer in a solvent, adding CNT to the solution, and mixing it. The third method includes a method of adding a conjugated polymer to a solution in which CNT has been preliminarily dispersed in a solvent using ultrasonic waves or the like, and mixing it. The fourth method includes a method of putting a conjugated polymer and CNT in a solvent, and irradiating the mixture with ultrasonic waves to mix it. In the present invention, these methods may be combined.

[0120] In the present invention, the length of the CNT is preferably shorter than the distance (channel length) between the source electrode 5 and the drain electrode 6. The average length of the CNT depends on the channel length, but is preferably 2 μm or less, more preferably 0.5 μm or less. Generally, commercially available CNTs have a distribution in length, and may contain CNTs longer than the channel length. For this reason, it is preferable to add a step of shortening the CNTs to be shorter than the channel length to the step of forming the semiconductor layer 4. As a method for shortening the CNTs to be shorter than the channel length, for example, a method of cutting the CNTs into short fibers by acid treatment with nitric acid, sulfuric acid, or the like, ultrasonic treatment, or a freeze-pulverization method is effective. In addition, it is more preferable to use separation by a filter in combination from the viewpoint of improving the purity of the CNTs. In addition, the diameter of the CNTs is not particularly limited, but is preferably 1 nm or more and 100 nm or less, and more preferably 50 nm or less.

[0121] Examples of the conjugated polymers that coat the CNTs include polythiophene polymers, polypyrrole polymers, polyaniline polymers, polyacetylene polymers, poly-p-phenylene polymers, poly-p-phenylenevinylene polymers, and thiophene-heteroarylene polymers having thiophene units and heteroaryl units in the repeating units. The conjugated polymers may be made of two or more of these. The conjugated polymers may be made of a single monomer unit arranged in a row, a block copolymer of different monomer units, a random copolymer, or a graft polymer.

[0122] A mixture of a CNT composite and an organic semiconductor may be used as the semiconductor layer 4. By uniformly dispersing the CNT composite in the organic semiconductor, it is possible to achieve high mobility while maintaining the properties of the organic semiconductor itself.

[0123] The semiconductor layer 4 may further include an insulating material. Examples of the insulating material used here include the insulating material composition of the present invention and polymer materials such as poly(methyl methacrylate), polycarbonate, and polyethylene terephthalate, but are not limited to these.

[0124] The semiconductor layer 4 may be a single layer or multiple layers. The thickness of the semiconductor layer 4 is preferably 1 nm or more and 200 nm or less, and more preferably 100 nm or less. By making the semiconductor layer 4 have a thickness within this range, it becomes easy to form a uniform thin film, and furthermore, it is possible to suppress the current between the source and drain electrodes that cannot be controlled by the gate voltage, and to increase the on / off ratio of the FET. The thickness of the semiconductor layer 4 can be measured by an atomic force microscope, an ellipsometry method, or the like.

[0125] An orientation layer can also be provided between the gate insulating layer 3 and the semiconductor layer 4. As the material for this orientation layer, known materials such as silane compounds, titanium compounds, organic acids, and heteroorganic acids can be used, and in particular, organic silane compounds are preferred.

[0126] In the present invention, a second insulating layer (for example, second insulating layer 7 shown in FIG. 14) may be formed on at least some of the semiconductor layers 4 of the multiple FETs, in contact with the semiconductor layers 4 on the side opposite to the gate insulating layer 3. This makes it possible to protect the semiconductor layers 4 from the external environment, such as oxygen and moisture.

[0127] The material used for the second insulating layer is not particularly limited, but specific examples include inorganic materials such as silicon oxide and alumina, polymer materials such as polyimide and its derivatives, polyvinyl alcohol, polyvinyl chloride, polyethylene terephthalate, polyvinylidene fluoride, polysiloxane and its derivatives, polyvinylphenol and its derivatives, and the like, or a mixture of inorganic material powder and a polymer material, or a mixture of an organic low molecular weight material and a polymer material.

[0128] The formed FET (for example, FETs 20 and 30 shown in FIG. 14 and the like) can control the current flowing between the source electrode 5 and the drain electrode 6 by changing the gate voltage. The mobility, which is an index of the performance of the FET, can be calculated using the following formula (a). Mobility μ=(δId / δVg)L·D / (W·εr·ε·Vsd)(a)

[0129] In the formula (a), Id is the current between the source and drain electrodes, Vsd is the voltage between the source and drain electrodes, Vg is the gate voltage, D is the thickness of the gate insulating layer 3, L is the channel length, and W is the channel width. εr is the relative dielectric constant of the gate insulating layer 3, and ε is the dielectric constant of a vacuum (8.85×10 -12 F / m).

[0130] The above FET has high mobility, and the relative positions of the gate electrode 2, the source electrode 5 and the drain electrode 6 are controlled with high precision.

[0131] (Second insulating layer) The second insulating layer 7 is formed on the side opposite to the side on which the gate insulating layer 3 is formed with respect to the semiconductor layer 4. "The side opposite to the side on which the gate insulating layer 3 is formed with respect to the semiconductor layer 4" refers to the upper side of the semiconductor layer 4, for example, when the gate insulating layer 3 is located on the lower side of the semiconductor layer 4. By forming the second insulating layer, a CNT-FET that normally exhibits p-type semiconductor characteristics can be converted into a semiconductor element that exhibits n-type semiconductor characteristics.

[0132] The second insulating layer 7 preferably contains an organic compound having a bond between a carbon atom and a nitrogen atom. Any organic compound may be used as such an organic compound, and examples of such an organic compound include amide-based compounds, imide-based compounds, urea-based compounds, amine-based compounds, imine-based compounds, aniline-based compounds, and nitrile-based compounds. Furthermore, it is believed that the second insulating layer 7 contains a polymer, which makes it possible to stably maintain the field where the organic compound having a bond between a carbon atom and a nitrogen atom interacts with the CNT, and therefore it is presumed that more stable n-type semiconductor characteristics can be obtained. Examples of the polymer contained in the second insulating layer 7 include acrylic resin, methacrylic resin, olefin polymer, cycloolefin polymer, polystyrene, polysiloxane, polyimide, polycarbonate, vinyl alcohol resin, and phenol resin.

[0133] The second insulating layer 7 may contain other compounds in addition to the organic compound or polymer. Examples of such other compounds include a thickener or a thixotropic agent for adjusting the viscosity or rheology of the solution when the second insulating layer 7 is formed by coating. The second insulating layer 7 may be a single layer or multiple layers.

[0134] The method for forming the second insulating layer 7 is not particularly limited, and dry methods such as resistance heating deposition, electron beam, sputtering, and CVD can be used, but from the viewpoint of manufacturing costs and suitability for large areas, it is preferable to use a coating method. Specific examples of the coating method that can be preferably used include spin coating, blade coating, slit die coating, screen printing, bar coater, casting, print transfer, immersion and pulling, inkjet, and drop casting. The coating method for the second insulating layer 7 can be selected depending on the coating film properties to be obtained, such as coating film thickness control and orientation control.

[0135] <Method of manufacturing a substrate for a semiconductor device> Next, a detailed description will be given of a method for manufacturing a substrate for a semiconductor device according to the present invention, focusing on the method for manufacturing the substrate for a semiconductor device 50E according to the fifth embodiment described above as a representative example. The method for manufacturing a substrate for a semiconductor device according to the present invention is for manufacturing any one of the substrates for a semiconductor device according to each of the above-mentioned embodiments. In the manufacturing method for manufacturing any one of the substrates for a semiconductor device according to each of the above-mentioned embodiments, it is preferable that the formation of any one of the components of the semiconductor device and the formation of the reinforcing wires on the resin film 1 are performed in the same process. This makes it possible to reduce the number of types of materials and the number of processes required for manufacturing the substrate for a semiconductor device.

[0136] FIG. 17 is a perspective view for explaining an example of a method for manufacturing a substrate for a semiconductor device according to the fifth embodiment of the present invention. FIG. 18A is a partially enlarged schematic view showing a first step example of the method for manufacturing a substrate for a semiconductor device according to the fifth embodiment of the present invention. FIG. 18B is a partially enlarged schematic view showing a second step example of the method for manufacturing a substrate for a semiconductor device according to the fifth embodiment of the present invention. In FIGS. 18A and 18B, a part (a part surrounded by a dashed line III) of the substrate for a semiconductor device 50E shown in FIG. 17 is extracted, and each step of the method for manufacturing the substrate for a semiconductor device 50E is shown. In manufacturing the substrate for a semiconductor device 50E, the following steps are performed while the long resin base material 1 is transported by a roll-to-roll method. In the transport by the roll-to-roll method, the transport direction of the resin base material 1 is the same as the longitudinal direction of the resin base material 1 (see the thick arrow in FIG. 17).

[0137] In the method for manufacturing the substrate 50E for a semiconductor device, first, as shown in state S1 in FIG. 18A, a reinforcing line forming step is performed in which the gate electrode 2 and the reinforcing lines 31-38 are formed on the surface of the resin base material 1. In this reinforcing line forming step, the gate electrode 2 and the reinforcing lines 31-38 are formed on the resin base material 1 in the same step. Note that the same step here does not only mean forming the gate electrode 2 and the reinforcing lines 31-38 at the same time, but also means forming one of the gate electrode 2 or the reinforcing lines 31-38 first, and then forming the other (the gate electrode 2 or the reinforcing lines 31-38 that have not yet been formed) before the step of forming the next gate insulating layer. Among these, it is preferable to form the gate electrode 2 and the reinforcing lines 31-38 at the same time.

[0138] The method of forming the gate electrode 2 and the reinforcing wires 31 to 38 in the reinforcing wire forming step includes a method using a known technique such as vacuum deposition, electron beam, sputtering, plating, CVD, ion plating coating, inkjet, and printing, and a method of applying a paste containing an organic component and conductive particles to an insulating substrate by a known technique such as a blade coating method, a slit die coating method, a screen printing method, a bar coater method, a mold method, a print transfer method, and a dip and pull method, and drying the paste using an oven, a hot plate, infrared rays, etc. The method of forming the gate electrode 2 and the reinforcing wires 31 to 38 is not particularly limited as long as the gate electrode 2 and the wiring (not shown) can be electrically connected. In the reinforcing wire forming step, the reinforcing wires 31 to 38 are formed from the same material as the material constituting the gate electrode 2.

[0139] In the reinforcing line forming step, the patterning method for forming the gate electrode 2 and the reinforcing lines 31 to 38 in a pattern may be a method of patterning the electrode thin film produced by the above method into a desired shape by a known photolithography method or a method of forming a pattern through a mask of a desired shape during vacuum deposition or sputtering of the electrode and wiring material. The patterning method may also be a method of directly forming a pattern using an inkjet method or a printing method.

[0140] Among these methods, the reinforcing line forming step preferably includes a patterning step of processing a metal film formed on the resin substrate 1 by sputtering or vacuum deposition, and processing the metal film into a pattern corresponding to the gate electrode 2 and the reinforcing lines 31 to 38. The reinforcing line forming step also preferably includes a film forming step of forming a coating film on the resin substrate 1 using a photosensitive paste containing conductive particles and a photosensitive organic component, and a patterning step of processing the coating film into a pattern corresponding to the gate electrode 2 and the reinforcing lines 31 to 38 by a photolithography method. By using these methods (steps) in the reinforcing line forming step, the gate electrode 2 and the reinforcing lines 31 to 38 can be formed with high flatness and uniform thickness and pattern shape. Therefore, the leakage rate of the FET to be manufactured can be reduced, and the characteristic variation of the FET can be reduced. Examples of preferred embodiments of the photosensitive paste used in the present invention include those described in International Publication No. 2018 / 051860 and International Publication No. 2017 / 030070.

[0141] When the resin base material 1, which is continuously transported by the roll-to-roll method, is wound into a roll, the portions of the resin base material 1 corresponding to the reinforcing wires 31-34 become thicker due to their overlap, and a gauge-shaped band is formed for each row of the reinforcing wires 31-34. If the reinforcing wires 31-34 have a uniform thickness, the thickness of each band becomes uniform, and thus the winding misalignment of the resin base material 1 can be reduced. In addition, by making the thickness of the reinforcing wires 31-38 and the thickness of the gate electrode 2 uniform, in the resin base material 1 wound into a roll, the thickness of the reinforcing wires 31-34 that are accumulated in an overlapping manner becomes thicker than the thickness of the gate electrode 2 that is accumulated in an overlapping manner. This makes it possible to reduce the occurrence of breaks in the gate electrode 2 that occur when the roll of the resin base material 1 is tightly wound and rubbed.

[0142] The thickness of the resin base material 1 is preferably 25 μm or more and 100 μm or less. By setting the thickness of the resin base material 1 within this range, the resin base material 1 can have high durability and appropriate flexibility, and therefore, it is possible to prevent the resin base material 1 from meandering during transport and winding deviation in the roll-to-roll method. As a result, the efficiency of forming a semiconductor device on the resin base material 1 is improved.

[0143] The term "uniform thickness" means that the standard deviation of the average thickness measured at any five locations is within 5%. The term "electrode thickness such as a gate electrode" and the reinforcing wire thickness are the same means that the difference between the average thicknesses of the electrodes and reinforcing wires formed within the surface of the resin base material 1 measured at any five locations is within 10% of the larger average thickness.

[0144] Next, as shown in state S2 of FIG. 18A, a first insulating layer forming step is performed to form a gate insulating layer 3. In this first insulating layer forming step, the gate insulating layer 3 is formed on the above-mentioned gate electrode 2 (see state S1 of FIG. 18A). Methods for forming the gate insulating layer 3 include known techniques such as vacuum deposition, electron beam, sputtering, plating, CVD, ion plating coating, inkjet, printing, spin coating, blade coating, slit die coating, bar coater, casting, printing transfer, and immersion and pulling. However, the method for forming the gate insulating layer 3 is not limited to these.

[0145] Although not shown in FIG. 18A, the gate insulating layer 3 may be formed also on the reinforcing lines 31 to 38, or may be formed over the entire surface of the resin base material 1 on which the gate electrode 2 and the reinforcing lines 31 to 38 are formed.

[0146] Next, as shown in state S3 of FIG. 18B, a semiconductor layer forming step is performed to form a semiconductor layer 4. In this semiconductor layer forming step, a solution containing CNT is applied onto the gate insulating layer 3 (see state S2 of FIG. 18A) described above to form the semiconductor layer 4. As a method for forming the semiconductor layer 4, a coating method is preferably used from the viewpoint of manufacturing cost and suitability for large areas. Examples of the coating method include known coating methods such as spin coating, blade coating, slit die coating, screen printing, bar coating, mold method, print transfer method, immersion and pulling method, and inkjet method. Among them, the coating method is preferably any one selected from the group consisting of an inkjet method, a dispenser method, and a spray method. Furthermore, from the viewpoint of efficiency in using raw materials, the inkjet method is more preferable. As the coating method, an appropriate one can be selected from these coating methods according to the coating film characteristics to be obtained, such as coating film thickness control and orientation control. In addition, in this semiconductor layer forming step, the formed coating film may be annealed under air, reduced pressure, or in an inert gas atmosphere (nitrogen or argon atmosphere).

[0147] Next, as shown in state S4 of FIG. 18B, an electrode formation process is carried out to form source and drain electrodes. In this electrode process, a source electrode 5 and a drain electrode 6 are formed on the gate insulating layer 3 and the semiconductor layer 4 (see state S3 of FIG. 18B) described above. The source electrode 5 and the drain electrode 6 can be formed by using a known technique such as vacuum deposition, electron beam, sputtering, plating, CVD, ion plating coating, inkjet, or printing, or by applying a paste containing an organic component and conductive particles onto an insulating substrate by a known technique such as spin coating, blade coating, slit die coating, screen printing, bar coater, casting, printing transfer, or immersion and pulling method, and then drying the paste using an oven, a hot plate, or infrared rays. However, the method of forming these electrodes is not particularly limited as long as the source electrode 5 and the drain electrode 6 can be electrically connected to the wiring (not shown).

[0148] In addition, in the manufacturing method of the substrate 50E for a semiconductor device, instead of forming the gate electrode 2 and the reinforcing wires 31-38 in the same process as described above, a reinforcing wire forming step may be performed in which the source electrode 5, the drain electrode 6, and the reinforcing wires 31-38 are formed in the same process. In this case, the material of the reinforcing wires 31-38 is the same material as the material constituting the source electrode 5 and the drain electrode 6. In the reinforcing wire forming step, the pattern forming method for forming the source electrode 5, the drain electrode 6, and the reinforcing wires 31-38 in a pattern may be a method of forming a pattern of the electrode thin film produced by the above method into a desired shape by a known photolithography method or the like, or a method of forming a pattern through a mask of a desired shape during deposition or sputtering of the electrode and wiring material. In addition, the pattern forming method may be a method of directly forming a pattern using an inkjet method or a printing method.

[0149] Next, a modified example of the method for manufacturing a substrate for a semiconductor device according to the present invention will be described by exemplifying the substrate for a semiconductor device 50H (see FIG. 13) according to the sixth embodiment described above. FIG. 19A is a partially enlarged schematic diagram showing a first step example of the method for manufacturing a substrate for a semiconductor device according to the sixth embodiment of the present invention. FIG. 19B is a partially enlarged schematic diagram showing a second step example of the method for manufacturing a substrate for a semiconductor device according to the sixth embodiment of the present invention. In FIGS. 19A and 19B, a part of the substrate for a semiconductor device 50H according to the sixth embodiment is extracted and each step of the method for manufacturing the substrate for a semiconductor device 50H is shown. The part of the substrate for a semiconductor device 50H shown in FIGS. 19A and 19B is the same as the part surrounded by the dashed line III of the substrate for a semiconductor device 50E shown in FIG. 17. In the method for manufacturing the substrate for a semiconductor device 50H, the resin base material 1 is a long resin base material, as in the method for manufacturing the substrate for a semiconductor device 50E according to the fifth embodiment described above (see FIG. 17). In addition, in manufacturing the substrate for a semiconductor device 50H, the following steps are performed while the long resin base material 1 is transported by a roll-to-roll method. At this time, the conveying direction of the resin base material 1 is the same as the conveying direction in the above-mentioned fifth embodiment (see the thick arrow in FIG. 17).

[0150] In the method for manufacturing the semiconductor device substrate 50H, first, as shown in FIG. 19A, a reinforcing wire forming step (state S11) in which the gate electrode 2 and the reinforcing wires 31 to 38 are formed, a first insulating layer forming step (state S12) in which the gate insulating layer 3 is formed, and a semiconductor layer forming step (state S13) in which the semiconductor layer 4 is formed are performed. In the reinforcing wire forming step of the present embodiment 6, the gate electrode 2 and the reinforcing wires 31 to 38 are formed on the resin base material 1 in the same step by the same method as in the above-mentioned embodiment 5 except for the number of gate electrodes 2 formed. In the first insulating layer forming step of the present embodiment 6, the gate insulating layer 3 is formed on the gate electrode 2 by the same method as in the above-mentioned embodiment 5 except for the number of gate electrodes 2 covered by the gate insulating layer 3. At this time, the gate insulating layer 3 may be formed so as to cover a pair of gate electrodes 2 as shown in FIG. 19A, may be formed on the reinforcing wires 31 to 38, or may be formed on the entire surface of the resin base material 1 on which the gate electrodes 2 and the reinforcing wires 31 to 38 are formed. In the semiconductor layer formation step of the sixth embodiment, the semiconductor layer 4 is formed on the gate insulating layer 3 in the same manner as in the fifth embodiment, except for the formation pattern of the semiconductor layer 4.

[0151] Next, as shown in state S14 in FIG. 19B, an electrode formation step is performed to form source and drain electrodes. In the electrode formation step of the sixth embodiment, the source electrode 5 and the drain electrode 6 are formed on the gate insulating layer 3 and the semiconductor layer 4 by the same method as in the fifth embodiment except for the number of source and drain electrodes formed. At this time, instead of forming the gate electrode 2 and the reinforcing wires 31 to 38 in the same step in the reinforcing wire formation step described above, the source electrode 5, the drain electrode 6 and the reinforcing wires 31 to 38 may be formed in the same step. In this step, the material of the reinforcing wires 31 to 38 is the same as the material constituting the source electrode 5 and the drain electrode 6.

[0152] 19B, a second reinforcing wire forming step is performed to form the second insulating layer 7 and the second reinforcing wires 51-58. In this second reinforcing wire forming step, the step of forming the second insulating layer 7 on some of the semiconductor layers 4 out of the plurality of semiconductor layers 4 described above and the step of forming the second reinforcing wires 51-58 on the reinforcing wires 31-38 described above are performed in the same step. At this time, the material of the second reinforcing wires 51-58 is the same as the material constituting the second insulating layer 7.

[0153] The method for forming the second insulating layer 7 and the second reinforcing wires 51-58 is not particularly limited, and a dry method such as resistance heating deposition, electron beam, sputtering, or CVD can be used. However, from the viewpoint of manufacturing cost and suitability for large areas, it is preferable to use a coating method. Specifically, the coating method can be preferably a spin coating method, a blade coating method, a slit die coating method, a screen printing method, a bar coater method, a mold method, a print transfer method, a dip and pull method, an inkjet method, or a drop casting method. The coating method for the second insulating layer 7 and the second reinforcing wires 51-58 can be selected according to the coating film characteristics to be obtained, such as coating film thickness control and orientation control. In addition, in the second reinforcing wire forming step, the formed coating film may be annealed in air, under reduced pressure, or in an inert gas atmosphere (nitrogen or argon atmosphere).

[0154] When the resin base material 1, which is continuously transported by the roll-to-roll method, is wound into a roll, the portions of the resin base material 1 corresponding to the second reinforcing wires 51-54 (second reinforcing wires extending in the longitudinal direction of the resin base material 1) become thicker due to the overlapping of the second reinforcing wires. This makes it possible to prevent localized and uneven thickness variations that occur within the rolled resin base material 1 when wound up. As a result, it is possible to suppress peeling of the second insulating layer 7 due to friction between the rolled resin base material 1 and the second insulating layer 7.

[0155] According to the manufacturing method of the substrate for semiconductor device according to the fifth and sixth embodiments described above, a plurality of semiconductor devices are formed on the resin base material so as to each include a field effect transistor having a bottom gate structure, and the gate electrode and the reinforcing wire included in the field effect transistor are formed in the same process, so that the expansion and contraction in the resin base material can be controlled by the reinforcing wire immediately after the gate electrode is formed. Therefore, in the subsequent insulating layer forming process and source electrode and drain electrode forming process, the alignment accuracy is improved, and the characteristic variation in the plurality of field effect transistors in the resin base material surface can be suppressed.

[0156] In addition, a resin base material having a longitudinal direction and a lateral direction is formed such that a row of multiple semiconductor devices is formed on the resin base material in the longitudinal direction, and a part of the reinforcing wire is provided substantially continuously in the longitudinal direction of the resin base material at both outer edge portions of the row of semiconductor devices. As a result, the resin base material is wound up while the substantially continuously formed reinforcing wires overlap, and as a result, the wound shape of the resin base material is strengthened and the winding deviation of the rolled resin base material can be suppressed. In addition, since a plurality of regions surrounding the semiconductor devices are formed on the resin base material surface by the substantially continuously formed reinforcing wires, when the semiconductor device substrate is exposed to environmental changes such as humidity and temperature, the variation in expansion and contraction within the resin base material surface can be controlled for each region surrounded by the substantially continuous reinforcing wire. Therefore, when a plurality of semiconductor devices are formed substantially continuously, the positioning accuracy can be improved for each region of the substantially continuous resin base material surface, and the characteristic variation of the plurality of semiconductor devices on the resin base material surface can be suppressed.

[0157] The method for manufacturing a substrate for a semiconductor device of the present invention is not limited to the manufacturing methods of the fifth and sixth embodiments described above, and may be, for example, a method in which a resin base material is continuously or intermittently transported by a method other than the roll-to-roll method, and a plurality of semiconductor devices and reinforcing lines are formed on the resin base material. It is also preferable that at least one of the electrode layers included in the semiconductor device and the reinforcing lines are formed in the same process. That is, the source and drain electrodes and the reinforcing lines may be formed in the same process.

[0158] 18A, 18B and 19A, 19B are so-called bottom gate structures in which the gate electrode 2 is disposed below the semiconductor layer 4 (on the side of the resin base material 1), but are not limited thereto. For example, the FET may be so-called top gate structures in which the gate electrode 2 is disposed above the semiconductor layer 4 (on the side opposite the resin base material 1). Although not particularly shown, when the FET has a top gate structure, the reinforcing wires 31 to 38 are preferably provided in the same layer as the source electrode 5 and drain electrode 6 located below the semiconductor layer 4, and made of the same material as these source electrode 5 and drain electrode 6.

[0159] From the above, regardless of whether the FET has a bottom gate structure or a top gate structure, it is preferable that the reinforcing wires 31 to 38 are provided in the same layer as the electrodes on the substrate side, which are located closer to the resin substrate 1 (for example, the lower side of the semiconductor layer 4) among the source electrode 5, drain electrode 6, and gate electrode 2 included in the FET, and made of the same material as the electrodes on the substrate side, since this makes it easier to suppress deformation of the resin substrate 1. Among these, it is preferable that the FET has a bottom gate structure. This is because deformation of the resin substrate 1 can be suppressed from the time of forming the gate electrode 2, and therefore it is easier to suppress pattern misalignment of the members constituting the FET in the element structure, such as in the subsequent alignment of the gate electrode 2 with the source electrode 5 and the drain electrode 6.

[0160] <Wireless communication device> Next, a case will be described where the semiconductor device used in the present invention (for example, the semiconductor device 10 shown in FIG. 1) is a wireless communication device. This wireless communication device is a device that communicates information using wireless waves, such as a product tag, an anti-shoplifting tag, various tickets, and a smart card. This wireless communication device is a device that performs electrical communication by receiving a wireless signal (carrier wave) transmitted from an antenna mounted on an external reader / writer, such as an RFID tag.

[0161] A specific operation of an RFID tag as an example of a wireless communication device is, for example, as follows. The antenna of the RFID tag receives a wireless signal transmitted from an antenna mounted on a reader / writer. The FET in the RFID tag obtains a command based on the received wireless signal and performs an operation according to this command. The RFID tag then transmits a response to this command as a wireless signal from its own antenna to the antenna of the reader / writer. The operation according to the command is performed by a known demodulation circuit, an operation control logic circuit, a modulation circuit, etc., which are composed of FETs.

[0162] A preferred embodiment of the wireless communication device used in the present invention includes at least the above-mentioned FET and an antenna. FIG. 20 is a schematic diagram showing a first configuration example of the wireless communication device applied to the present invention. FIG. 21 is a schematic diagram showing a second configuration example of the wireless communication device applied to the present invention. As a more specific configuration of the wireless communication device in the present invention, an example shown in FIG. 20 or FIG. 21 can be given. That is, as shown in FIG. 20 or FIG. 21, the wireless communication device 110, 110A includes a substrate 100, and on the substrate 100, an antenna pattern 101, a circuit 102 including a FET, and a connection wiring 103 connecting the circuit 102 and the antenna pattern 101 are provided. In these wireless communication devices 110, 110A, the substrate 100 is formed by cutting the resin base material (for example, the resin base material 1 shown in FIG. 1, etc.) of the above-mentioned semiconductor device substrate of the present invention into individual semiconductor devices.

[0163] In the method for manufacturing a substrate for a semiconductor device of the present invention, when each of the multiple semiconductor devices is a wireless communication device, a substrate for a semiconductor device having multiple wireless communication devices formed thereon can be obtained. The method for manufacturing a wireless communication device of the present invention includes a cutting step of cutting the substrate for a semiconductor device into individual wireless communication devices. Specifically, in the method for manufacturing a wireless communication device, the cutting step cuts the substrate for a semiconductor device into individual wireless communication devices, thereby allowing individual wireless communication devices to be obtained.

[0164] In addition, in the manufacturing method of the substrate for semiconductor device of the present invention, when each of the plurality of semiconductor devices is a circuit (for example, the circuit 102 shown in Figs. 20 and 21) of a wireless communication device, a substrate for semiconductor device in which the plurality of circuits 102 are formed on a resin base material can be obtained. The manufacturing method of the wireless communication device according to the present invention includes a cutting step of cutting the substrate for semiconductor device into individual circuits of the wireless communication device, and a bonding step of bonding the circuits of the wireless communication device cut by the cutting step to an antenna. Specifically, in the manufacturing method of the wireless communication device, the substrate for semiconductor device is cut into individual circuits 102 by the cutting step, and then the obtained plurality of circuits 102 are bonded to the antenna by the bonding step. As a result, the circuits 102 and the antenna (for example, the antenna pattern 101 shown in Figs. 20 and 21) are connected by wiring such as the above-mentioned connection wiring 103. As a result, a wireless communication device can be obtained.

[0165] Alternatively, the manufacturing method of the wireless communication device according to the present invention includes a bonding step of bonding the circuit 102 of the wireless communication device formed on the substrate for semiconductor device as described above to an antenna, and a cutting step of cutting the substrate for semiconductor device after bonding the circuit 102 and the antenna in the bonding step into individual wireless communication devices (including these circuits 102 and antennas). Specifically, in the manufacturing method of the wireless communication device, the circuit portion of the substrate for semiconductor device on which the multiple circuits 102 are formed is bonded to the antenna in the bonding step, and then the wireless communication devices including the circuits 102 and the antennas are individually cut out in the cutting step. In the bonding step, these circuits 102 and the antennas are connected by wiring. As a result, a wireless communication device can be obtained.

[0166] In the above-mentioned method for manufacturing a wireless communication device, the antenna material and the connection wiring material may be any conductive material. Specifically, the conductive material may be the same as the gate electrode material. Among them, a paste material containing a conductor and a binder is preferable because it increases flexibility, has good adhesion even when bent, and provides good electrical connection. From the viewpoint of reducing manufacturing costs, it is preferable that the antenna material and the connection wiring material are the same material.

[0167] Pattern forming methods for forming an antenna pattern and a connection wiring pattern include a method of processing a metal foil such as copper foil or aluminum foil using a punching blade and transferring it to a resin substrate, a method of etching a metal foil attached to a resin substrate using a resist layer formed on the metal foil as a mask, a method of forming a pattern of a conductive paste on a resin substrate by a coating method and curing the pattern by heat or light, etc. Among them, from the viewpoint of reducing manufacturing costs, the method of forming the pattern by coating a conductive paste on a resin substrate is preferred.

[0168] In addition, when a paste containing a conductor and a binder is used as the conductive material, a method of applying the paste onto a resin substrate using a known technique such as a spin coating method, a blade coating method, a slit die coating method, a screen printing method, a bar coater method, a mold method, a printing transfer method, or a dip and pull method, and then drying using an oven, a hot plate, infrared rays, etc., is also an example of the pattern formation method. In addition, the antenna pattern and the connection wiring pattern may be formed by patterning the conductive film produced by the above method into a desired shape using a known photolithography method, or may be formed through a mask of a desired shape during vacuum deposition or sputtering.

[0169] Furthermore, it is preferable that the antenna pattern and the connection wiring pattern are made of the same material as the gate electrode and wiring of the FET, because this reduces the number of types of materials required for manufacturing the wireless communication device, and by fabricating the antenna pattern and the connection wiring pattern and the gate electrode and wiring of the FET in the same process, the number of manufacturing steps for the wireless communication device can be reduced, which results in a reduction in the manufacturing cost of the wireless communication device.

[0170] "The antenna pattern and the connection wiring pattern, and the gate electrode and wiring of the FET are made of the same material" means that the elements contained in the antenna pattern and the connection wiring pattern and the gate electrode and wiring of the FET that have the highest molar ratios are the same. The types and content ratios of the elements contained in the antenna pattern and the connection wiring pattern and the gate electrode and wiring of the FET can be identified by elemental analysis such as X-ray photoelectron spectroscopy (XPS) and secondary ion mass spectrometry (SIMS).

[0171] When the antenna pattern, the connection wiring pattern, the gate electrode of the FET, and the wiring are produced in the same process, the connection between the antenna pattern and the connection wiring pattern, and the connection between the connection wiring pattern and the wiring for the gate electrode of the FET are each formed in a continuous phase. From the viewpoint of adhesion and reduction in manufacturing cost, it is preferable that the antenna pattern, the connection wiring pattern, the gate electrode of the FET, and the wiring are formed to form a continuous phase. "The antenna pattern, the connection wiring pattern, the gate electrode of the FET, and the wiring pattern are continuous phases" means that the patterns are integrated and there is no connection interface at the connection portion. The fact that the connection portion is a continuous phase can be confirmed by observing the cross section of the connection portion with a scanning electron microscope (SEM) or a transmission electron microscope (TEM).

[0172] In the present invention, the width and thickness of the connection portion between the antenna pattern and the connection wiring pattern, and the width and thickness of the connection portion between the connection wiring pattern and the wiring for the gate electrode of the FET are each arbitrary. EXAMPLES

[0173] The present invention will now be described in more detail with reference to examples, although the present invention is not limited to the following examples.

[0174] (Preparation of photosensitive paste) (Synthesis Example 1) In Synthesis Example 1, compound P1 was synthesized as a photosensitive organic component. The copolymerization ratio in the synthesis of this compound P1 is as follows. Copolymerization ratio (by mass): ethyl acrylate (hereinafter, "EA") / 2-ethylhexyl methacrylate (hereinafter, "2-EHMA") / styrene (hereinafter, "St") / glycidyl methacrylate (hereinafter, "GMA") / acrylic acid (hereinafter, "AA") = 20 / 40 / 20 / 5 / 15

[0175] Specifically, first, 150 g of diethylene glycol monoethyl ether acetate (hereinafter, "DMEA") was charged into a reaction vessel in a nitrogen atmosphere, and the temperature was raised to 80°C using an oil bath. A mixture consisting of 20 g of EA, 40 g of 2-EHMA, 20 g of St, 15 g of AA, 0.8 g of 2,2'-azobisisobutyronitrile, and 10 g of DMEA was added dropwise over 1 hour. After the dropwise addition was completed, the polymerization reaction was carried out for another 6 hours. Then, 1 g of hydroquinone monomethyl ether was added to stop the polymerization reaction. Subsequently, a mixture consisting of 5 g of GMA, 1 g of triethylbenzylammonium chloride, and 10 g of DMEA was added dropwise over 0.5 hours. After the dropwise addition was completed, the addition reaction was carried out for another 2 hours. The obtained reaction solution was purified with methanol to remove unreacted impurities, and further vacuum dried for 24 hours to obtain compound P1.

[0176] (Synthesis Example 2) In Synthesis Example 2, compound P2 was synthesized as the photosensitive organic component. The copolymerization ratio in the synthesis of compound P2 is as follows. Copolymerization ratio (by mass): 2-functional epoxy acrylate monomer (Epoxy Ester 3002A; Kyoeisha Chemical Co., Ltd.) / 2-functional epoxy acrylate monomer (Epoxy Ester 70PA; Kyoeisha Chemical Co., Ltd.) / GMA / St / AA = 20 / 40 / 5 / 20 / 15

[0177] Specifically, 150 g of diethylene glycol monoethyl ether acetate (hereinafter, "DMEA") was first charged into a reaction vessel in a nitrogen atmosphere, and the temperature was raised to 80°C using an oil bath. A mixture consisting of 20 g of epoxy ester 3002A, 40 g of epoxy ester 70PA, 20 g of St, 15 g of AA, 0.8 g of 2,2'-azobisisobutyronitrile, and 10 g of DMEA was added dropwise to the reaction vessel over 1 hour. After the dropwise addition, the polymerization reaction was carried out for another 6 hours. Then, 1 g of hydroquinone monomethyl ether was added to stop the polymerization reaction. Subsequently, a mixture consisting of 5 g of GMA, 1 g of triethylbenzylammonium chloride, and 10 g of DMEA was added dropwise over 0.5 hours. After the dropwise addition, the addition reaction was carried out for another 2 hours. The resulting reaction solution was purified with methanol to remove unreacted impurities, and further vacuum dried for 24 hours to obtain compound P2.

[0178] (Synthesis Example 3) In Synthesis Example 3, compound P3 was synthesized as a photosensitive organic component. Compound P3 is a urethane-modified compound of compound P2 in Synthesis Example 2 above.

[0179] Specifically, 100 g of DMEA was first charged into a reaction vessel in a nitrogen atmosphere, and the temperature was raised to 80° C. using an oil bath. A mixture consisting of 10 g of compound P2 (photosensitive component of Synthesis Example 2), 3.5 g of n-hexyl isocyanate, and 10 g of DMEA was added dropwise to the reaction vessel over 1 hour. After the addition was completed, the reaction was continued for another 3 hours. The resulting reaction solution was purified with methanol to remove unreacted impurities, and further dried in vacuum for 24 hours to obtain compound P3 having a urethane bond.

[0180] (Preparation Example 1) In Preparation Example 1, photosensitive paste A was prepared. Specifically, first, in a 100 mL clean bottle, compound P1 (16 g) obtained in Synthesis Example 1, compound P3 (4 g) obtained in Synthesis Example 3, light acrylate BP-4EA (2 g) manufactured by Kyoeisha Chemical Co., Ltd., photopolymerization initiator OXE-01 (4 g) manufactured by BASF Japan Ltd., acid generator SI-110 (0.6 g) manufactured by Sanshin Chemical Industry Co., Ltd., and γ-butyrolactone (10 g) manufactured by Mitsubishi Gas Chemical Co., Ltd. were placed and mixed with a rotation-revolution vacuum mixer "Awatori Rentaro" (registered trademark) (ARE-310; manufactured by Thinky Corporation). As a result, a photosensitive resin solution (solid content 78.5 mass%) of Preparation Example 1 was obtained. At this time, the mass of the photosensitive resin solution was 34.6 g. The photosensitive resin solution (8.0 g) obtained was mixed with Ag particles (42.0 g) having an average particle size of 0.06 μm, and kneaded using a three-roller “EXAKT M-50” (product name, manufactured by EXAKT Co., Ltd.) to obtain 50 g of photosensitive paste A.

[0181] (Preparation Example 2) In Preparation Example 2, photosensitive paste B was prepared. Specifically, 25.0 g of an alkali-soluble resin solution (40% by mass), 1.5 g of Irgacure (registered trademark) OXE02 (oxime ester compound; manufactured by BASF) as a photopolymerization initiator, 5.5 g of Light Acrylate (registered trademark) PE-4A (manufactured by Kyoeisha Chemical Co., Ltd.), and 2.0 g of DISPERBYK (registered trademark) 140 (manufactured by BYK Japan Co., Ltd.) (amine value: 146 mg KOH / g) as a dispersant were placed in a clean bottle, and mixed with a planetary centrifugal mixer "Awatori Rentaro" (registered trademark) (ARE-310; manufactured by Thinky Corporation). As a result, a photosensitive resin solution of Preparation Example 2 was obtained. The photosensitive resin solution (8.0 g) obtained in Preparation Example 2 was mixed with Ag particles (42.0 g) having an average particle size of 0.06 μm, and DMEA was added so that the solid content ratio became 80 mass %, and then the mixture was kneaded using a three-roller "EXAKT M-50" (product name, manufactured by EXAKT Co., Ltd.) to obtain photosensitive paste B.

[0182] (Preparation Example 3) In Preparation Example 3, photosensitive paste C was prepared. Specifically, photosensitive paste C was obtained by carrying out preparation in the same manner as in Preparation Example 2 described above, except that Ag particles having an average particle diameter of 0.15 μm were used.

[0183] (Preparation of semiconductor solution) In preparing the semiconductor solution, first, 1.0 mg of CNT (CNI, single-walled CNT, purity 95%) was added to a chloroform solution (10 mL) containing 2.0 mg of P3HT (Aldrich, poly(3-hexylthiophene)), and the mixture was ultrasonically stirred for 4 hours at 20% output using an ultrasonic homogenizer (Tokyo Rikakikai, VCX-500) while cooling on ice. This resulted in CNT dispersion A11 (CNT composite concentration in solvent: 0.96 g / l).

[0184] Next, the CNT dispersion A11 was filtered using a membrane filter (pore size 10 μm, diameter 25 mm, Millipore Omnipore Membrane) to remove CNT composites with a length of 10 μm or more. 5 mL of o-DCB (Wako Pure Chemical Industries, Ltd.) was added to the filtrate obtained by this, and then the low boiling point solvent chloroform was distilled off using a rotary evaporator, thereby replacing the solvent with o-DCB to obtain CNT dispersion B11. 3 mL of o-DCB was added to CNT dispersion B11 (1 mL), thereby obtaining semiconductor solution A10 (CNT composite concentration relative to the solvent is 0.03 g / l).

[0185] (Example of gate insulating layer fabrication) In the example of preparing the gate insulating layer, a gate insulating layer solution A20 was prepared. Specifically, first, methyltrimethoxysilane (61.29 g (0.45 mol)), 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane (12.31 g (0.05 mol)), and phenyltrimethoxysilane (99.15 g (0.5 mol)) were dissolved in 203.36 g of propylene glycol monobutyl ether (boiling point 170°C). Water (54.90 g) and phosphoric acid (0.864 g) were added to this while stirring. The solution obtained in this manner was heated at a bath temperature of 105°C for 2 hours, and the internal temperature was raised to 90°C to distill off a component mainly consisting of by-produced methanol. Next, the solution was heated at a bath temperature of 130°C for 2 hours, and the internal temperature was raised to 118°C to distill off a component mainly consisting of water and propylene glycol monobutyl ether. After that, the mixture was cooled to room temperature to obtain a polysiloxane solution A3 having a solid content of 26.0% by weight. The weight average molecular weight of the polysiloxane in the obtained polysiloxane solution A3 was 6,000.

[0186] Next, 10 g of the obtained polysiloxane solution A3 was weighed out, and 54.4 g of propylene glycol monoethyl ether acetate (hereinafter referred to as PGMEA) was mixed with this, and the mixture was stirred at room temperature for 2 hours. In this way, a gate insulating layer solution A20 was obtained.

[0187] (Example of creating the second insulating layer) In the example of preparing the second insulating layer, a second insulating layer solution A30 was prepared. Specifically, first, 2.5 g of polymethyl methacrylate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was dissolved in 7.5 g of N,N-dimethylformamide to prepare a polymer solution A31. Next, 1 g of N,N,N',N'-tetramethyl-1,4-phenylenediamine (manufactured by Tokyo Chemical Industry Co., Ltd.) was dissolved in 9.0 g of N,N-dimethylformamide to prepare a compound solution A32. After that, the compound solution A32 (0.30 g) was added to the polymer solution A31 (0.68 g), thereby obtaining a second insulating layer solution A30.

[0188] Example 1 In Example 1, a substrate for a semiconductor device was fabricated as a specific example of substrate 50 for a semiconductor device (see FIG. 1) according to the first embodiment of the present invention. The substrate for a semiconductor device in Example 1 is a substrate for a semiconductor device of a type having a field effect transistor with a bottom gate-top contact structure as a semiconductor device. FIG. 22A is a schematic diagram showing a first example of a process of a method for manufacturing a substrate for a semiconductor device according to Example 1 of the present invention. FIG. 22B is a schematic diagram showing a second example of a process of a method for manufacturing a substrate for a semiconductor device according to Example 1 of the present invention.

[0189] Specifically, first, 100 nm of copper was vacuum-deposited on the entire surface of a resin substrate 1 (width 300 mm, length 420 mm, film thickness 50 μm) made of a PET film by resistance heating. Photoresist (product name "LC100-10cP", manufactured by Rohm and Haas) was printed on the entire surface by slit coating, and then heated and dried in a hot air drying oven at 100°C for 4 minutes. The photoresist film thus produced was exposed to light at a dose of 60 mJ / cm through a photomask with an effective mask size of 280 mm × 400 mm on which a gate electrode 2 was designed. 2 A full line exposure (converted to a wavelength of 365 nm) was performed. The gate electrode width designed on this photomask was 100 μm. After exposure, the substrate was developed with a 2.38% by weight aqueous solution of tetramethylammonium hydroxide for 30 seconds, and then washed with water for 1 minute. Then, the substrate was etched with mixed acid (product name SEA-5, manufactured by Kanto Chemical Co., Ltd.) for 30 seconds, and then washed with water for 30 seconds. Next, the substrate was immersed in AZ Remover 100 (product name, manufactured by AZ Electronic Materials Co., Ltd.) for 2 minutes to peel off the photoresist film, washed with water for 30 seconds, and then the water droplets were removed with an air knife, and then heated and dried in a hot air drying oven at 80° C. for 60 seconds. As a result, nine gate electrodes 2 were formed on the surface of the resin substrate 1 (state S21) as shown in FIG. 22A.

[0190] Thereafter, a gate insulating layer solution A20 to become the gate insulating layer 3 was continuously printed over the entire surface by slit coating, and heat-treated in a hot air drying oven at 100°C for 3 minutes in an air atmosphere, and then heat-treated in an IR drying oven at 150°C for 20 minutes in a nitrogen atmosphere. As a result, as shown in Fig. 22A, a gate insulating layer 3 having a thickness of 500 nm was formed on the resin base material 1 (state S22).

[0191] On the resin substrate 1 on which the gate insulating layer 3 was formed as described above, 100 pL of the semiconductor solution A10 was applied by an inkjet method to each of the portions of the gate insulating layer 3 corresponding to the positions where the nine gate electrodes 2 were projected, and heat treatment was performed in an IR drying furnace under a nitrogen gas flow at 150°C for 30 minutes. As a result, semiconductor layers 4 were formed in nine places on the gate insulating layer 3 (state S23), as shown in Fig. 22A.

[0192] Next, photosensitive paste A was applied by screen printing onto the resin substrate 1 made of a PET film on which the gate insulating layer 3 was formed. At this time, the photosensitive paste A was applied so as to overlap the exposed area when the gate electrode 2 and the reinforcing lines 31 to 38 were formed with a printing size of 280 mm × 400 mm. Next, the applied photosensitive paste A was pre-baked at 100 °C for 4 minutes in a hot air drying furnace. After that, a light exposure of 80 mJ / cm was applied to the area overlapping the area where the photosensitive paste A was applied through a photomask with an effective mask size of 280 mm × 400 mm on which the source electrode 5 and the drain electrode 6 were designed. 2 After exposure, the film was exposed to 0.5% Na 2 CO 3 The substrate was developed with the solution for 30 seconds, washed with ultrapure water for 60 seconds, and then cured in an IR drying furnace at 150° C. for 10 minutes. As a result, as shown in FIG. 22B, nine source electrodes 5 and drain electrodes 6 were formed on the gate insulating layer 3 (state S24). The width of the source electrodes 5 and the drain electrodes 6 was 100 μm, and the distance between these electrodes was 20 μm.

[0193] Next, a paste obtained by diluting the photosensitive paste B by two times with DMEA was applied by inkjet coating onto the resin substrate 1 made of a PET film on which the source electrode 5 and the drain electrode 6 were formed, to form a pattern of the reinforcing lines 31 to 38, and the pattern was then heat-treated in a hot air drying oven at 100°C for 4 minutes in an air atmosphere. 2 After the exposure, the coating was cured in an IR drying furnace at 150° C. for 10 minutes, thereby forming reinforcing lines 31 to 38 as shown in FIG. 22B (state S25).

[0194] In the above manner, the semiconductor device substrate of Example 1 was obtained. The obtained semiconductor device substrate was subjected to measurement of the current-voltage characteristics of the current (Id) between the source and drain electrodes and the voltage (Vsd) between the source and drain electrodes when the gate voltage (Vg) of the FET was changed. For this measurement, a semiconductor characteristic evaluation system 4200-SCS type (manufactured by Keithley Instruments) was used to measure the above characteristics under air. In Example 1, the value of Id at Vsd=-5V when Vg was changed from +5V to -5V was measured. Thereafter, the sample was placed in a constant temperature and humidity chamber at 85°C and 85% RH for 24 hours, and after removing the sample, the value of Id at Vsd=-5V when Vg was changed from +5V to -5V was measured again. This measurement was performed on all 9 FETs, and the average value and standard deviation of these 9 FETs were calculated and evaluated according to the following criteria. The results of Example 1 are shown in Table 1 below. A (Good): The standard deviation is within 15% of the average value. B (Acceptable): The standard deviation is greater than 15% and less than 30% of the average value. C (Fail): The standard deviation is greater than 30% from the mean.

[0195] Comparative Example 1 In Comparative Example 1, the same evaluation as in Example 1 was performed in the same manner as in Example 1, except that the step of forming the reinforcing wires 31 to 38 in Example 1 was not performed. The evaluation results of Comparative Example 1 are shown in Table 1.

[0196] [Table 1]

[0197] Example 2 In Example 2, a substrate for a semiconductor device was produced as a specific example of substrate 50E for a semiconductor device according to the fifth embodiment of the present invention (see FIG. 6). The substrate for a semiconductor device in Example 2 is a type having a field effect transistor with a bottom gate-top contact structure as the semiconductor device, and was produced continuously by conveying resin base material 1 using a roll-to-roll method (see FIGS. 17, 18A, and 18B).

[0198] Specifically, first, 100 nm of copper was vacuum-deposited on the entire surface of a resin substrate 1 (width 300 mm, length 50 m, film thickness 50 μm) made of a PET film by resistance heating. Photoresist (product name "LC100-10cP", manufactured by Rohm and Haas) was continuously printed on the entire surface by slit coating, and then heated and dried in a hot air drying oven at 100°C for 4 minutes. The photoresist film thus produced was exposed to light at an exposure dose of 60 mJ / cm through a photomask with an effective mask size of 280 mm × 400 mm on which the gate electrode 2 and reinforcing lines 31 to 38 were designed. 2(converted to wavelength 365 nm) and the feed length of the resin substrate 1 was 420 mm, and 100 shots of full line exposure were performed. The gate electrode width designed in this photomask was 100 μm, the width of the reinforcing lines 31 to 38 was 1 mm, the length of the reinforcing lines 31 to 34 was 370 mm, and the length of the reinforcing lines 35 to 38 was 280 mm. After exposure, the substrate was developed for 30 seconds with a 2.38% by weight aqueous solution of tetramethylammonium hydroxide, and then washed with water for 1 minute. Then, the substrate was etched for 30 seconds with mixed acid (trade name SEA-5, manufactured by Kanto Chemical Co., Ltd.), and then washed with water for 30 seconds. Next, the substrate was immersed in AZ Remover 100 (trade name, manufactured by AZ Electronic Materials Co., Ltd.) for 2 minutes to peel off the photoresist film, washed with water for 30 seconds, and then water droplets were removed with an air knife, and then heated and dried in a hot air drying oven at 80° C. for 60 seconds. As a result, as shown in FIG. 18A, nine gate electrodes 2 and reinforcing lines 31 to 38 were formed per exposure area on the surface of the resin base material 1 (state S1).

[0199] Thereafter, the gate insulating layer solution A20 that would become the gate insulating layer 3 was continuously printed over the entire surface by slit coating, and heat-treated in a hot air drying oven at 100°C for 3 minutes in an air atmosphere, and then heat-treated in an IR drying oven at 150°C for 20 minutes in a nitrogen atmosphere. As a result, as shown in Fig. 18A, a gate insulating layer 3 with a thickness of 500 nm was formed on the resin base material 1 (state S2).

[0200] On the resin substrate 1 on which the gate insulating layer 3 was formed as described above, 100 pL of the semiconductor solution A10 was applied by the inkjet method to each of the nine portions of the gate insulating layer 3 where the gate electrodes 2 were projected, and then heat treatment was performed in an IR drying furnace under a nitrogen gas flow at 150°C for 30 minutes. As a result, as shown in Fig. 18B, the semiconductor layer 4 was formed in nine portions on the gate insulating layer 3 (state S3).

[0201] Next, photosensitive paste A was applied by screen printing onto the resin substrate 1 made of a PET film on which the gate insulating layer 3 was formed. At this time, the photosensitive paste A was applied 100 shots with a feed length of 420 mm for the resin substrate 1 so that the photosensitive paste A had a print size of 280 mm x 400 mm and overlapped with the exposed area when the gate electrode 2 and reinforcing lines 31 to 38 were formed. Next, the applied photosensitive paste A was pre-baked at 100°C for 4 minutes in a hot air drying furnace. Thereafter, the photosensitive paste A was exposed to light at an exposure dose of 80 mJ / cm 2 through a photomask with an effective mask size of 280 mm x 400 mm on which the source electrode 5 and drain electrode 6 were designed so that the photosensitive paste A overlapped with the area applied. 2 (Equivalent to a wavelength of 365 nm) and full line exposure was performed with a feed rate of 420 mm for the resin substrate 1. After exposure, 0.5% Na 2 CO 3 The substrate was developed with the solution for 30 seconds, washed with ultrapure water for 60 seconds, and then cured in an IR drying furnace at 150°C for 10 minutes. As a result, as shown in Fig. 18B, nine source electrodes 5 and drain electrodes 6 were formed on the gate insulating layer 3 (state S4). The width of the source electrodes 5 and drain electrodes 6 was 100 μm, and the distance between these electrodes was 20 μm.

[0202] In this manner, a substrate for a semiconductor device of Example 2 was obtained. The obtained substrate for a semiconductor device was subjected to the evaluations described in the following items 1 to 4. The results of the evaluations of items 1 and 2 are shown in Table 2, the results of the evaluation of item 3 are shown in Table 3, and the results of the evaluation of item 4 are shown in Table 4.

[0203] (Item 1: Winding misalignment test) In the first section, a winding misalignment test of a substrate for a semiconductor device is described. In the winding misalignment test of the first section, a substrate for a semiconductor device having a width of 300 mm and a length of 50 m was wound into a roll with an accuracy of ±1 mm around an ABS core having a width of 320 mm and a diameter of 3 inches. The rolled substrate for a semiconductor device was then dropped from a height of 10 cm in a direction perpendicular to the width direction of the ABS core, and the rolled width was measured with a digital caliper. Based on the measured value of the rolled width, the winding misalignment was evaluated according to the following criteria. A (Good): The roll winding width is within 301 mm. B (Acceptable): The roll winding width is greater than 301 mm and less than 305 mm. C (Not acceptable): The roll winding width is greater than 305 mm.

[0204] (Item 2: Film thickness measurement) In the second section, the measurement of the film thickness of the substrate for semiconductor device is described. In the measurement of the film thickness in the second section, each part (substrate sample) from the 1st shot to the 100th shot was cut out in the form of a sheet from the substrate for semiconductor device having a length of 50 m at the feed pitch implemented in the above-mentioned exposure process. Of these cut-out substrate samples, the cross section of each of the substrate samples for the 10th shot, 50th shot, and 90th shot was observed using a scanning electron microscope (SEM), and the thickness (film thickness) was measured at five arbitrary points from the gate electrode and five arbitrary points from the reinforcing line. The average value and standard deviation were calculated for each of the measured gate electrode film thickness and reinforcing line film thickness.

[0205] (Item 3: Evaluation of FET Id variation) In the third item, an evaluation of Id variation of FETs formed on a substrate for semiconductor device will be described. FIG. 23 is a schematic diagram showing an example of a substrate sample obtained from the substrate for semiconductor device of Example 2. FIG. 23 shows a projection view of substrate samples (samples used for measurement) cut from a continuous substrate for semiconductor device in a roll shape, stacked in the thickness direction. In the evaluation of the third item, the 10th, 50th, and 90th shot substrate samples were used among a plurality of substrate samples cut from the substrate for semiconductor device in the same manner as in the evaluation of the second item, and the current-voltage characteristics of the current (Id) between the source-drain electrodes and the voltage (Vsd) between the source-drain electrodes when the gate voltage (Vg) was changed were measured for each of the nine FETs 21 to 29 shown in FIG. 23. For this measurement, a semiconductor characteristic evaluation system 4200-SCS type (manufactured by Keithley Instruments) was used and the measurement was performed under atmospheric pressure. The average value and standard deviation of Id at Vsd=-5V when Vg=-5V was changed from +5V to -5V were calculated for nine FETs 21 to 29 for each of the substrate samples for each shot. Based on the average value and standard deviation of Id obtained, the Id variation of the FETs was evaluated according to the following criteria. A (Good): The standard deviation is within 15% of the average value of Id. B (Acceptable): The standard deviation of Id is greater than 15% and less than 30% of the average value. C (Fail): The standard deviation of Id is greater than 30% of the mean value.

[0206] (Item 4: Coordinate measurement of gate electrode patterns) In the fourth item, coordinate measurement of the gate electrode pattern of the semiconductor device substrate will be described. In the measurement of the fourth item, the coordinates of each gate electrode of nine FETs 21 to 29 (see FIG. 23) were measured for each of the 10th, 50th, and 90th shot substrate samples among a plurality of substrate samples cut out from the semiconductor device substrate in the same manner as in the evaluation of the second item above, using a coordinate measuring machine SMIC-800 (manufactured by Shinto S Precision Co., Ltd.), and the standard deviations in the longitudinal and lateral directions of the semiconductor device substrate were calculated as the coordinate variation for each gate electrode between shots. The larger of the obtained standard deviations in the longitudinal and lateral directions was used as the evaluation target, and the evaluation of the coordinate variation of the gate electrode pattern was performed according to the following criteria. In Table 4 described later, the numerical values ​​"21" to "29" are numerical values ​​(codes) that identify each FET to be evaluated. A (good): The standard deviation is 20 μm or less. B (Acceptable): The standard deviation is greater than 20 μm and less than 40 μm. C (Fail): Standard deviation is greater than 40 μm.

[0207] Example 3 In Example 3, evaluations similar to those of items 1 to 3 of Example 2 were performed in the same manner as in Example 2, except that aluminum was vacuum-deposited to a thickness of 60 nm over the entire surface instead of copper in the resistance heating method for forming the gate electrode 2 and the reinforcing lines 31 to 38. The evaluation results of Example 3 are shown in Tables 2 and 3.

[0208] Example 4 In Example 4, a substrate for a semiconductor device was produced as a specific example of the substrate for a semiconductor device 50 (see FIG. 1) according to the first embodiment of the present invention. The substrate for a semiconductor device in Example 4 is a substrate for a semiconductor device of a type having a field effect transistor as the semiconductor device, and was continuously produced by conveying the resin base material 1 by the roll-to-roll method in the same manner as in the fifth embodiment described above.

[0209] Specifically, first, the photosensitive paste B was continuously printed over the entire surface of a resin substrate 1 (width 300 mm, length 50 m, film thickness 50 μm) made of a PET film by slit coating, and then heat-treated in a hot air drying oven at 100°C for 4 minutes in an air atmosphere. The coating film thus produced was exposed to light with an exposure dose of 80 mJ / cm through a photomask with an effective mask size of 280 mm × 400 mm on which the gate electrode 2 and reinforcing lines 31 to 38 were designed. 2 (converted into a wavelength of 365 nm) and the feed rate of the resin base material 1 was 420 mm pitch, and full line exposure was performed. After exposure, the resin base material 1 was developed with a 2.38% TMAH solution for 30 seconds, washed with ultrapure water for 60 seconds, and then cured in an IR drying furnace at 150°C for 10 minutes. As a result, nine gate electrodes 2 and reinforcing lines 31 to 38 were formed per exposed area on the surface of the resin base material 1. The steps after the gate insulating layer 3 were performed in the same manner as in Example 2, and evaluations were performed in the same manner as in Example 2. The evaluation results of Example 4 are shown in Tables 2 to 4.

[0210] Example 5 In Example 5, a substrate for a semiconductor device was produced in the same manner as in Example 4, except that photosensitive paste C was used in place of photosensitive paste B for slit coating when forming the gate electrode 2 and reinforcing lines 31 to 38, and evaluations were performed in the same manner as in the evaluations for items 1 to 3 of Example 2. The evaluation results of Example 5 are shown in Tables 2 and 3.

[0211] Example 6 In Example 6, a substrate for a semiconductor device was fabricated as a specific example of the semiconductor device substrate (see FIG. 2) according to the modified example of the first embodiment of the present invention. The substrate for a semiconductor device in Example 6 is a substrate for a semiconductor device of a type having a field effect transistor with a bottom gate-top contact structure as the semiconductor device, and was continuously fabricated while conveying the resin base material 1 by a roll-to-roll method (see FIG. 6). Specifically, the substrate for a semiconductor device in Example 6 was fabricated in the same manner as in Example 1, except that a photomask with a design excluding the reinforcing wires 33 and 37 from the design of the photomask used in Example 1 was used. In Example 6, the same evaluations as those for the first to third items in Example 2 were performed. The evaluation results of Example 6 are shown in Tables 2 and 3.

[0212] Example 7 In Example 7, a substrate for a semiconductor device was fabricated as a specific example of the substrate for a semiconductor device 50D (see FIG. 5) according to the fourth embodiment of the present invention. The substrate for a semiconductor device in Example 7 is a substrate for a semiconductor device of a type having a field effect transistor with a bottom gate-top contact structure as a semiconductor device, and was continuously fabricated while conveying the resin base material 1 by a roll-to-roll method (see FIG. 6). Specifically, the substrate for a semiconductor device in Example 7 was fabricated in the same manner as in Example 2, except that the photomask used in the step of forming the gate electrode 2 and the reinforcing wires 31-38 in Example 2 and the step of forming the source electrode 5 and the drain electrode 6 was a photomask designed so that the layout design of the reinforcing wires 31-38 and the semiconductor device 10 (FET in Example 7) was the layout design in the fourth embodiment of the present invention shown in FIG. 5. In Example 7, the same evaluations as those in the first to third items in Example 2 were performed. In the evaluation of the third item in Example 7, 9 FETs out of 13 FETs in each substrate sample were measured, and the same evaluations as those in Example 2 were performed. The evaluation results of Example 7 are shown in Tables 2 and 3.

[0213] Example 8 In Example 8, a substrate for a semiconductor device was fabricated as a specific example of the substrate for a semiconductor device according to Modification 1 of the fifth embodiment of the present invention (see FIG. 6 and FIG. 7). The substrate for a semiconductor device in Example 8 is a substrate for a semiconductor device of a type having a field effect transistor with a bottom gate-top contact structure as a semiconductor device, and was continuously fabricated while conveying the resin base material 1 by a roll-to-roll method. Specifically, the substrate for a semiconductor device in Example 8 was fabricated in the same manner as in Example 2, except that the photomask used in the step of forming the gate electrode 2 and the reinforcing lines 31-38 in Example 2 was a photomask designed so that the layout design of the reinforcing lines 31-38 and the semiconductor device 10 (FET in Example 8) was the layout design in Modification 1 of the fifth embodiment of the present invention shown in FIG. 7. In Example 8, the same evaluations as those in the first to third items of Example 2 were performed. In the evaluation of the third item in Example 7, 9 FETs of the 13 FETs in each substrate sample were measured, and the same evaluations as those in Example 2 were performed. The evaluation results of Example 8 are shown in Tables 2 and 3.

[0214] Comparative Example 2 In Comparative Example 2, evaluations were performed in the same manner as in Example 2, except that a photomask on which the reinforcing lines 31 to 38 were not designed was used as the photomask used in the step of forming the gate electrode 2 and the reinforcing lines 31 to 38 in Example 2. The evaluation results of Comparative Example 2 are shown in Tables 2 to 4.

[0215] Comparative Example 3 In Comparative Example 3, evaluations were performed in the same manner as in Example 4 and Example 2, except that a photomask on which the reinforcing lines 31 to 38 were not designed was used as the photomask used in the step of forming the gate electrode 2 and the reinforcing lines 31 to 38 in Example 4. The evaluation results of Comparative Example 3 are shown in Tables 2 to 4.

[0216] [Table 2]

[0217] [Table 3]

[0218] [Table 4]

[0219] Example 9 In Example 9, a substrate for a semiconductor device was produced as a specific example of the substrate for a semiconductor device 50F according to Modification 1 of Embodiment 5 of the present invention. The substrate for a semiconductor device in Example 9 is a type having a field effect transistor with a bottom gate-top contact structure as the semiconductor device, and was continuously produced by conveying the resin base material 1 by a roll-to-roll method.

[0220] Specifically, first, 100 nm of copper was vacuum-deposited on the entire surface of a resin substrate 1 (width 300 mm, length 50 m, film thickness 50 μm) made of a PET film by resistance heating. Photoresist (product name "LC100-10cP", manufactured by Rohm and Haas) was continuously printed on the entire surface by slit coating, and then heated and dried in a hot air drying oven at 100°C for 4 minutes. The photoresist film thus produced was exposed to light at an exposure dose of 60 mJ / cm through a photomask with an effective mask size of 280 mm × 400 mm on which the gate electrode 2 and reinforcing lines 31 to 38 were designed. 2(converted to wavelength 365 nm) and the feed length of the resin substrate 1 was 420 mm, and 100 shots of full line exposure were performed. The gate electrode width designed in this photomask was 100 μm, the width of the reinforcing lines 31 to 38 was 1 mm, the length of the reinforcing lines 31 to 34 was 370 mm, and the length of the reinforcing lines 35 to 38 was 280 mm. After exposure, the substrate was developed for 30 seconds with a 2.38% by weight aqueous solution of tetramethylammonium hydroxide, and then washed with water for 1 minute. Then, the substrate was etched for 30 seconds with mixed acid (trade name SEA-5, manufactured by Kanto Chemical Co., Ltd.), and then washed with water for 30 seconds. Next, the substrate was immersed in AZ Remover 100 (trade name, manufactured by AZ Electronic Materials Co., Ltd.) for 2 minutes to peel off the photoresist film, washed with water for 30 seconds, and then water droplets were removed with an air knife, and then heated and dried in a hot air drying oven at 80° C. for 60 seconds. As a result, the gate electrodes 2 and the reinforcing lines 31 to 38 were formed at 18 locations per exposure area on the surface of the resin base material 1 (see state S11 in FIG. 19A).

[0221] Thereafter, a gate insulating layer solution A20 that would become the gate insulating layer 3 was continuously printed over the entire surface by slit coating, and heat-treated in a hot air drying oven at 100°C for 3 minutes in an air atmosphere, and then heat-treated in an IR drying oven at 150°C for 20 minutes in a nitrogen atmosphere. As a result, a gate insulating layer 3 with a thickness of 500 nm was formed on the resin substrate 1 (see state S12 in FIG. 19A).

[0222] On the resin substrate 1 on which the gate insulating layer 3 was formed as described above, 100 pL of the semiconductor solution A10 was applied by an inkjet method to each of the portions of the gate insulating layer 3 corresponding to the positions where the 18 gate electrodes 2 were projected, and heat treatment was performed in an IR drying furnace under a nitrogen gas flow at 150°C for 30 minutes. As a result, the semiconductor layer 4 was formed in 18 places on the gate insulating layer 3 (see state S13 in FIG. 19A).

[0223] Next, photosensitive paste A was applied by screen printing onto the resin substrate 1 made of a PET film on which the gate insulating layer 3 was formed. At this time, the photosensitive paste A was applied 100 shots with a feed length of 420 mm of the resin substrate 1 so as to overlap with the exposed area when the gate electrode 2 and the reinforcing lines 31 to 38 were formed with a printing size of 280 mm x 400 mm. Next, the applied photosensitive paste A was pre-baked at 100°C for 4 minutes in a hot air drying furnace. Thereafter, the photosensitive paste A was exposed to light at an exposure dose of 80 mJ / cm 2 through a photomask with an effective mask size of 280 mm x 400 mm on which the source electrode 5 and drain electrode 6 were designed so as to overlap with the area on which the photosensitive paste A was applied. 2 (Equivalent to a wavelength of 365 nm) and full line exposure was performed with a feed rate of 420 mm for the resin substrate 1. After exposure, 0.5% Na 2 CO 3 The substrate was developed with the solution for 30 seconds, washed with ultrapure water for 60 seconds, and then cured in an IR drying furnace at 150° C. for 10 minutes. As a result, source electrodes 5 and drain electrodes 6 were formed at 18 locations on the gate insulating layer 3 (see state S14 in FIG. 19B). The width of the source electrodes 5 and drain electrodes 6 was 100 μm, and the distance between these electrodes was 20 μm.

[0224] Example 10 In Example 10, a substrate for a semiconductor device was produced as a specific example of the substrate for a semiconductor device 50H (see FIG. 13) according to the sixth embodiment of the present invention. The substrate for a semiconductor device in Example 10 is a type having a field effect transistor with a bottom gate-top contact structure as the semiconductor device, and was continuously produced by conveying the resin base material 1 by a roll-to-roll method (see FIGS. 19A and 19B).

[0225] Specifically, first, 100 nm of copper was vacuum-deposited on the entire surface of a resin substrate 1 (width 300 mm, length 50 m, film thickness 50 μm) made of a PET film by resistance heating. Photoresist (product name "LC100-10cP", manufactured by Rohm and Haas) was continuously printed on the entire surface by slit coating, and then heated and dried in a hot air drying oven at 100°C for 4 minutes. The photoresist film thus produced was exposed to light at an exposure dose of 60 mJ / cm through a photomask with an effective mask size of 280 mm × 400 mm on which the gate electrode 2 and reinforcing lines 31 to 38 were designed. 2 (converted to wavelength 365 nm) and the feed length of the resin substrate 1 was 420 mm, and 100 shots of full line exposure were performed. The gate electrode width designed in this photomask was 100 μm, the width of the reinforcing lines 31 to 38 was 1 mm, the length of the reinforcing lines 31 to 34 was 370 mm, and the length of the reinforcing lines 35 to 38 was 280 mm. After exposure, the substrate was developed for 30 seconds with a 2.38% by weight aqueous solution of tetramethylammonium hydroxide, and then washed with water for 1 minute. Then, the substrate was etched for 30 seconds with mixed acid (trade name SEA-5, manufactured by Kanto Chemical Co., Ltd.), and then washed with water for 30 seconds. Next, the substrate was immersed in AZ Remover 100 (trade name, manufactured by AZ Electronic Materials Co., Ltd.) for 2 minutes to peel off the photoresist film, washed with water for 30 seconds, and then water droplets were removed with an air knife, and then heated and dried in a hot air drying oven at 80° C. for 60 seconds. As a result, as shown in FIG. 19A, the gate electrodes 2 and the reinforcing lines 31 to 38 were formed at 18 locations per exposure area on the surface of the resin base material 1 (state S11).

[0226] Thereafter, a gate insulating layer solution A20 that would become the gate insulating layer 3 was continuously printed over the entire surface by slit coating, and heat-treated in a hot air drying oven at 100°C for 3 minutes in an air atmosphere, and then heat-treated in an IR drying oven at 150°C for 20 minutes in a nitrogen atmosphere. As a result, as shown in Fig. 19A, a gate insulating layer 3 with a thickness of 500 nm was formed on the resin base material 1 (state S12).

[0227] On the resin base material 1 on which the gate insulating layer 3 was formed as described above, 100 pL of the semiconductor solution A10 was applied by an inkjet method to each of the portions of the gate insulating layer 3 corresponding to the positions where the 18 gate electrodes 2 were projected, and heat treatment was performed in an IR drying furnace under a nitrogen gas flow at 150°C for 30 minutes. As a result, as shown in Fig. 19A, the semiconductor layer 4 was formed in 18 places on the gate insulating layer 3 (state S13).

[0228] Next, photosensitive paste A was applied by screen printing onto the resin substrate 1 made of a PET film on which the gate insulating layer 3 was formed. At this time, the photosensitive paste A was applied 100 shots with a feed length of 420 mm of the resin substrate 1 so as to overlap with the exposed area when the gate electrode 2 and the reinforcing lines 31 to 38 were formed with a printing size of 280 mm x 400 mm. Next, the applied photosensitive paste A was pre-baked at 100°C for 4 minutes in a hot air drying furnace. Thereafter, the photosensitive paste A was exposed to light at an exposure dose of 80 mJ / cm 2 through a photomask with an effective mask size of 280 mm x 400 mm on which the source electrode 5 and drain electrode 6 were designed so as to overlap with the area on which the photosensitive paste A was applied. 2 (Equivalent to a wavelength of 365 nm) and full line exposure was performed with a feed rate of 420 mm for the resin substrate 1. After exposure, 0.5% Na 2 CO 3 The substrate was developed with the solution for 30 seconds, washed with ultrapure water for 60 seconds, and then cured in an IR drying furnace at 150° C. for 10 minutes. As a result, as shown in FIG. 19B, source electrodes 5 and drain electrodes 6 were formed at 18 locations on the gate insulating layer 3 (state S14). The width of the source electrodes 5 and drain electrodes 6 was 100 μm, and the distance between these electrodes was 20 μm.

[0229] Next, on the resin base material 1 made of a PET film on which the semiconductor layer 4 was formed, the second insulating layer solution A30 (5 μL) was dropped onto some of the semiconductor layers 4 (18 locations in FIG. 19B) by a drop cast method so as to cover the semiconductor layers 4. In addition, the second insulating layer solution A30 was continuously dropped by the same method so as to surround the semiconductor device. In Example 10, the second insulating layer solution A30 was continuously dropped onto the reinforcing wires 31 to 38. Then, the dropped second insulating layer solution A30 was heat-treated at 110° C. for 30 minutes under a nitrogen gas flow. As a result, the second insulating layer 7 and the second reinforcing wires 51 to 58 were formed on the resin base material 1 (state S15) as shown in FIG. 19B. The thickness of the second insulating layer 7 and the second reinforcing wires 51 to 58 was 20 μm.

[0230] In the manner described above, the substrates for semiconductor devices of Examples 9 and 10 were obtained. The obtained substrates for semiconductor devices were evaluated in the same manner as the evaluation of the first item of Example 2, and the evaluation results of Examples 9 and 10 were both "A" (good). Furthermore, the substrates for semiconductor devices of Examples 9 and 10 (length: 50 m) were cut into sheets of paper into each part from the 1st shot to the 100th shot at the feed pitch implemented in the exposure process, and the appearance of each obtained substrate sample was checked. As a result, there were no parts where the second insulating layer 7 had peeled off.

[0231] Comparative Example 5 In Comparative Example 5, the same evaluation as in Example 10 was performed in the same manner as in Example 10, except that the second reinforcing wires 51-58 were not formed in the step of forming the second insulating layer 7 and the second reinforcing wires 51-58 in Example 10. In Comparative Example 5, an evaluation similar to the evaluation of the first item in Example 2 was performed, and the evaluation result of the first item in Comparative Example 5 was "C" (fail). Furthermore, peeling of the second insulating layer 7 also occurred in the substrate for a semiconductor device in Comparative Example 5. [Industrial Applicability]

[0232] As described above, the substrate for semiconductor device, the method for manufacturing a substrate for semiconductor device, and the method for manufacturing a wireless communication device according to the present invention are suitable for a substrate for semiconductor device, a method for manufacturing a substrate for semiconductor device, and a method for manufacturing a wireless communication device that can suppress variation in the characteristics of the semiconductor devices even after a plurality of semiconductor devices are formed on a substrate. [Explanation of symbols]

[0233] 1 Resin substrate 2. Gate electrode 3 Gate insulation layer 4 Semiconductor layer 5. Source Electrode 6 Drain electrode 7 Second insulating layer 10 Semiconductor device 11, 11a~11h, 12, 12a~12h, 13~17, 31~38 Reinforcement wire 20~30 FET 41, 42, 51~58 Second reinforcement line 50, 50A, 50B, 50C, 50D, 50E, 50F, 50G, 50H Substrates for semiconductor device 100 Substrates 101 Antenna Pattern 102 Circuit 103 Connection Wiring 110, 110A wireless communication equipment D1, D1a, D1b, D2, D2a, D2b Design

Claims

1. A method for manufacturing a semiconductor device comprising: a long resin substrate; and a plurality of semiconductor devices provided on the resin substrate, the method comprising the steps of: providing a reinforcing wire on the resin substrate so as to surround the plurality of semiconductor devices; the reinforcing wire is made of the same material as a material constituting at least one of the electrode layers included in the plurality of semiconductor devices; a plurality of regions are present on the resin base material, in which one or more of the plurality of semiconductor devices are surrounded by the reinforcing wire; 2. A substrate for a semiconductor device comprising:

2. A semiconductor device comprising: a resin substrate; and a plurality of semiconductor devices provided on the resin substrate, the plurality of semiconductor devices being surrounded by reinforcing wires provided on the resin substrate; the reinforcing wire is made of the same material as a material constituting at least one of the electrode layers included in the plurality of semiconductor devices; a plurality of regions are present on the resin base material, in which one or more of the plurality of semiconductor devices are surrounded by the reinforcing wire; Each of the plurality of semiconductor devices includes a field effect transistor, the field effect transistor has a source electrode, a drain electrode, and a gate electrode, a semiconductor layer in contact with the source electrode and the drain electrode, respectively, and a gate insulating layer that insulates the source electrode, the drain electrode, and the semiconductor layer from the gate electrode; At least some of the plurality of field effect transistors have a second insulating layer in contact with the semiconductor layer on a side opposite to the gate insulating layer with respect to the semiconductor layer of the field effect transistor, a second reinforcing wire formed on the resin base material and made of the same material as the material forming the second insulating layer; 2. A substrate for a semiconductor device comprising:

3. A semiconductor device comprising: a resin substrate; and a plurality of semiconductor devices provided on the resin substrate; and a reinforcing wire provided on the resin substrate so as to surround the plurality of semiconductor devices; the reinforcing wire is made of the same material as a material constituting at least one of the electrode layers included in the plurality of semiconductor devices; a plurality of regions are present on the resin base material, in which one or more of the plurality of semiconductor devices are surrounded by the reinforcing wire; Each of the plurality of semiconductor devices is a wireless communication device.

2. A substrate for a semiconductor device comprising:

4. The reinforcing wire is provided so as to surround each of the semiconductor devices.

4. The substrate for a semiconductor device according to claim 1, wherein the substrate is a metal.

5. a thickness of the reinforcing wire is equal to or smaller than a thickness of each of the plurality of semiconductor devices; 5. The substrate for a semiconductor device according to claim 1, wherein the substrate is a metal.

6. The resin substrate has a longitudinal direction and a transverse direction, the plurality of semiconductor devices are formed in a row in a longitudinal direction on the resin base material, A portion of the reinforcing wire is provided substantially continuously in the longitudinal direction of the resin base material.

6. The substrate for a semiconductor device according to claim 1,

7. The resin substrate has a longitudinal direction and a transverse direction, the plurality of semiconductor devices are formed in a row in a longitudinal direction on the resin base material, a part of the reinforcing wire is provided substantially continuously in a longitudinal direction of the resin base material at both outer edge portions of the row of the plurality of semiconductor devices; 7. The substrate for a semiconductor device according to claim 1,

8. Each of the plurality of semiconductor devices includes a field effect transistor, The field effect transistor has a source electrode, a drain electrode, and a gate electrode, a semiconductor layer in contact with the source electrode and the drain electrode, respectively, and a gate insulating layer that insulates the source electrode, the drain electrode, and the semiconductor layer from the gate electrode.

8. The substrate for a semiconductor device according to claim 1, wherein the substrate is a metal.

9. The semiconductor layer contains carbon nanotubes.

9. The substrate for a semiconductor device according to claim 2 or 8.

10. Each of the plurality of semiconductor devices includes a field effect transistor, the reinforcing wire is provided in the same layer as an electrode on a substrate side, which is located closer to the resin substrate, of a source electrode, a drain electrode, and a gate electrode included in the field effect transistor, and is made of the same material as the electrode on the substrate side.

10. The substrate for a semiconductor device according to claim 1.

11. Each of the plurality of semiconductor devices includes a field effect transistor having a bottom gate structure, the reinforcing wire is made of the same material as a material constituting a gate electrode included in the field effect transistor, and is provided in the same layer as the gate electrode.

11. The substrate for a semiconductor device according to claim 1.

12. At least some of the plurality of field effect transistors have a second insulating layer in contact with the semiconductor layer on a side opposite to the gate insulating layer with respect to the semiconductor layer of the field effect transistor, a second reinforcing wire formed on the resin base material and made of the same material as the material forming the second insulating layer; 12. The substrate for a semiconductor device according to claim 8, wherein the substrate is a substrate for a semiconductor device.

13. the gate electrode of the field effect transistor and the reinforcing line have the same thickness; The thickness is 30 nm or more and 500 nm or less.

13. The substrate for a semiconductor device according to claim 11 or 12.

14. The field effect transistor is a field effect transistor having a top contact structure.

14. The substrate for a semiconductor device according to claim 2, wherein the substrate is a metal substrate.

15. Each of the plurality of semiconductor devices is a wireless communication device.

15. The substrate for a semiconductor device according to claim 1, 2, or 4 to 14.

16. A method for manufacturing a substrate for a semiconductor device according to any one of claims 1 to 15, comprising the steps of: forming any one of the plurality of components of the semiconductor device and forming the reinforcing wire on the resin base material in the same process; 2. A method for manufacturing a substrate for a semiconductor device comprising the steps of:

17. A method for manufacturing a substrate for semiconductor device comprising: a resin substrate; and a plurality of semiconductor devices provided on the resin substrate, the resin substrate having reinforcing wires arranged to surround the plurality of semiconductor devices, the reinforcing wires being made of the same material as a material constituting at least one of the electrode layers included in the plurality of semiconductor devices, and the resin substrate having a plurality of regions in which one or more of the plurality of semiconductor devices are surrounded by the reinforcing wires, forming any one of the plurality of components of the semiconductor device and forming the reinforcing wire on the resin base material in the same process; Each of the plurality of semiconductor devices is formed to include a field effect transistor having a bottom gate structure, forming a gate electrode included in the field effect transistor and forming the reinforcing line in the same process; At least some of the plurality of field effect transistors are formed to have a second insulating layer in contact with the semiconductor layer on the opposite side of the semiconductor layer of the field effect transistor from the gate insulating layer, forming a second reinforcing wire made of the same material as that of the second insulating layer on the resin base material and forming the second insulating layer in the same process; 2. A method for manufacturing a substrate for a semiconductor device comprising the steps of:

18. The formation of the plurality of semiconductor devices and the reinforcing wires is carried out while the resin base material is transported by a roll-to-roll method.

18. The method for manufacturing a substrate for a semiconductor device according to claim 16 or 17.

19. forming at least one of the electrode layers included in each of the plurality of semiconductor devices and forming the reinforcing wire in the same process; 19. The method for manufacturing a substrate for a semiconductor device according to claim 16,

20. each of the plurality of semiconductor devices is formed to include a field effect transistor; Among the source electrode, the drain electrode and the gate electrode included in the field effect transistor, the electrode on the substrate side located closer to the resin substrate and the reinforcing wire are formed in the same process.

20. The method for manufacturing a substrate for a semiconductor device according to claim 16,

21. Each of the plurality of semiconductor devices is formed to include a field effect transistor having a bottom gate structure, forming a gate electrode included in the field effect transistor and forming the reinforcing line in the same process; 21. The method for manufacturing a substrate for a semiconductor device according to claim 16, or any one of claims 18 to 20.

22. At least some of the plurality of field effect transistors are formed to have a second insulating layer in contact with the semiconductor layer on the opposite side of the semiconductor layer of the field effect transistor from the gate insulating layer, forming a second reinforcing wire made of the same material as that of the second insulating layer on the resin base material and forming the second insulating layer in the same process; 22. The method for manufacturing a substrate for a semiconductor device according to claim 21.

23. The reinforcing line forming step in which the gate electrode and the reinforcing line are formed in the same step includes a patterning step in which a metal film formed on the resin base material by sputtering or vacuum deposition is processed into a pattern corresponding to the gate electrode and the reinforcing line.

23. The method for manufacturing a substrate for a semiconductor device according to claim 17, 21 or 22.

24. The reinforcing line forming step of forming the gate electrode and the reinforcing line in the same step includes: a film-forming step of forming a coating film on the resin substrate using a photosensitive paste containing conductive particles and a photosensitive organic component; a patterning step of processing the coating film into a pattern corresponding to the gate electrode and the reinforcing line by a photolithography method; 23. The method for manufacturing a substrate for a semiconductor device according to claim 17, 21 or 22, comprising:

25. The reinforcing wire is provided so as to surround each of the semiconductor devices. The method for manufacturing a substrate for a semiconductor device according to any one of claims 16 to 24.

26. The resin substrate has a longitudinal direction and a transverse direction, forming the plurality of semiconductor devices in a row in a longitudinal direction on the resin base material; A part of the reinforcing wire is provided substantially continuously in the longitudinal direction of the resin base material. The method for manufacturing a substrate for a semiconductor device according to any one of claims 16 to 25.

27. The resin substrate has a longitudinal direction and a transverse direction, forming the plurality of semiconductor devices in a row in a longitudinal direction on the resin base material; a part of the reinforcing wire is provided substantially continuously in a longitudinal direction of the resin base material at both outer edge portions of the row of the plurality of semiconductor devices; The method for manufacturing a substrate for a semiconductor device according to any one of claims 16 to 26.

28. A method for manufacturing a substrate for a semiconductor device according to any one of claims 1 to 15, comprising the steps of: forming any one of the plurality of components of the semiconductor device and forming the reinforcing wire on the resin base material in the same process; Each of the plurality of semiconductor devices is a wireless communication device or a circuit of a wireless communication device.

2. A method for manufacturing a substrate for a semiconductor device comprising the steps of:

29. A method for manufacturing a substrate for semiconductor device comprising: a resin substrate; and a plurality of semiconductor devices provided on the resin substrate, the resin substrate having reinforcing wires arranged to surround the plurality of semiconductor devices, the reinforcing wires being made of the same material as a material constituting at least one of the electrode layers included in the plurality of semiconductor devices, and the resin substrate having a plurality of regions in which one or more of the plurality of semiconductor devices are surrounded by the reinforcing wires, forming any one of the plurality of components of the semiconductor device and forming the reinforcing wire on the resin base material in the same process; Each of the plurality of semiconductor devices is a wireless communication device or a circuit of a wireless communication device.

2. A method for manufacturing a substrate for a semiconductor device comprising the steps of:

30. a step of cutting the substrate for a semiconductor device obtained by the method for manufacturing a substrate for a semiconductor device according to claim 28 or 29 into individual substrates for the wireless communication devices; 4. A method for manufacturing a wireless communication device comprising the steps of:

31. A step of cutting the substrate for a semiconductor device obtained by the method for manufacturing a substrate for a semiconductor device according to claim 28 or 29 into individual circuits for the wireless communication device; A step of attaching the cut-out circuit of the wireless communication device to an antenna; A method for manufacturing a wireless communication device, comprising:

32. A step of bonding a circuit of the wireless communication device of the substrate for a semiconductor device obtained by the method for manufacturing a substrate for a semiconductor device according to claim 28 or 29 to an antenna; a step of cutting the semiconductor device substrate after the wireless communication device circuit and the antenna are bonded together into individual wireless communication devices each including the wireless communication device circuit and the antenna; A method for manufacturing a wireless communication device, comprising:

Citation Information

Patent Citations

  • Reinforcing method of flexible substrate and flexible substrate

    JP1997283889A

  • Flexible display apparatus, organic light emitting display apparatus, and mother substrate for flexible display apparatus

    US20130248826A1

  • Transistor manufacturing method

    WO2015133391A1

  • Production method for antenna substrate, production method for antenna substrate with wiring and electrode, and production method for RFID element

    WO2017030070A1

  • Method for manufacturing field effect transistor and method for manufacturing wireless communication device

    WO2018051860A1