Method and apparatus for manufacturing binary compound semiconductors
The method and apparatus automatically adjust gas flow rates to stabilize the in-plane thickness distribution and dopant profiles in binary compound semiconductor manufacturing, addressing the complexity of existing methods by maintaining consistent atom numbers and ratios, thus simplifying the film formation process.
Patent Information
- Application Number
- JP2021005180
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-01-15
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2041-01-15
AI Technical Summary
Existing methods for manufacturing binary compound semiconductors, such as SiC and GaN, require complex experiments to stabilize the in-plane thickness distribution and dopant uptake efficiency of epitaxial films due to variations in raw material gas cylinder concentrations, making it difficult to fix a consistent film formation recipe.
A method and apparatus that automatically corrects the gas flow rates of raw material gases after cylinder replacement to maintain consistent atom numbers and ratios, using diluent gases to stabilize the in-plane thickness distribution and dopant profiles by creating a recipe based on test values and target concentrations.
Enables the stabilization of in-plane thickness distribution and dopant uptake efficiency without complex experiments, allowing for a stable and easy fixation of the epitaxial film deposition recipe.
Smart Images

Figure 0007593124000001 
Figure 0007593124000002 
Figure 0007593124000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method and an apparatus for producing binary compound semiconductors such as silicon carbide (hereinafter referred to as SiC) and gallium nitride (hereinafter referred to as GaN). [Background technology]
[0002] Conventionally, as one of the methods for manufacturing binary compound semiconductors, Patent Document 1 proposes a method for manufacturing a compound semiconductor device in which an epitaxial film is grown on a semiconductor substrate made of SiC or the like. In this manufacturing method, an epitaxial film is formed using a recipe having a step of a temperature rise period accompanied by pre-doping in which a dopant gas is introduced in advance, a step of a transition period in which the introduction of a raw material gas starts and gradually increases, and a step of a steady growth period in which the amount of the raw material gas introduced is kept constant. When forming an epitaxial film of SiC, silane (SiH4) and propane (C3H8) are used as raw material gases, and a carrier gas such as hydrogen (H2) is introduced together with the raw material gas to stably supply the raw material gas to grow the epitaxial film. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2017-152487 A Summary of the Invention [Problem to be solved by the invention]
[0004] Generally, the raw gas cylinder containing the raw gas is diluted with a dilution gas and has a predetermined gas concentration tolerance with respect to the target gas concentration. For example, if the target gas concentration is a gas concentration where the volume ratio of the raw gas to the total volume of the mixed gas of the raw gas and the dilution gas is 10%, the allowable tolerance is ±5%. Therefore, even if the target concentration of the raw gas is 10%, a raw gas cylinder with a gas concentration of 9.5 to 10.5% is used to form an epitaxial film.
[0005] In the formation of epitaxial films on two-dimensional compound semiconductors such as SiC, it is known that the efficiency of dopant incorporation, such as aluminum (Al) or nitrogen (N), is highly dependent on the element ratio of Si and C contained in the Si-based material and the C-based material, but this ratio changes every time the raw gas cylinder is replaced. For this reason, every time the raw gas cylinder is replaced, a semiconductor substrate is prepared as a reference sample, an epitaxial film is formed on it, and then the in-plane distribution of the epitaxial film thickness on the semiconductor substrate, an experiment to grasp the dopant incorporation efficiency, and a concentration profile are measured. Then, a calibration curve is obtained based on the results, and the raw gas concentration is controlled when forming the epitaxial film.
[0006] However, starting from the flow rate under the epitaxial film growth conditions before the raw gas cylinder is replaced, the flow rate is gradually changed, and experiments are performed until the in-plane distribution of the epitaxial film thickness, the dopant incorporation efficiency, and the concentration profile reach the target values to obtain a calibration curve. This requires complicated experiments, and it is difficult to fix the epitaxial film growth recipe. Therefore, it is desired to be able to easily fix the epitaxial film growth recipe without having to perform complicated experiments.
[0007] Here, we have explained not only the in-plane distribution of the epitaxial film thickness, but also the experiment to grasp the dopant incorporation efficiency and the measurement of the concentration profile. However, as mentioned above, the dopant incorporation efficiency and the concentration profile are highly dependent on the element ratio of Si and C in the Si-based material and C-based material, and affect the in-plane distribution of the thickness of the obtained epitaxial film. Therefore, if it is possible to control at least the in-plane distribution of the epitaxial film thickness to be stable and reach the target value, it will be possible to eliminate the need for complicated experiments and easily fix the epitaxial film formation recipe.
[0008] In view of the above, an object of the present invention is to provide a method and an apparatus for manufacturing a binary compound semiconductor that can easily fix a deposition recipe for an epitaxial film without the need for complicated experiments. [Means for solving the problem]
[0009] In order to achieve the above object, the invention described in claim 1 provides a method for manufacturing a binary compound semiconductor by supplying a first raw material gas containing a first raw material and a second raw material gas containing a second raw material to grow an epitaxial film (2) on a substrate (1) of the binary compound semiconductor, the method comprising the steps of: preparing a first raw material gas cylinder (41) containing a first raw material dilution gas obtained by diluting the first raw material gas with a dilution gas to a first gas concentration; preparing a second raw material gas cylinder (42) containing a second raw material dilution gas obtained by diluting the second raw material gas with a dilution gas that is the same as or different from the dilution gas; and preparing a reaction furnace (20) constituting a growth chamber for accommodating and heating the substrate. When replacing at least one of the first raw material gas cylinder and the second raw material gas cylinder, an inspection value of the gas concentration of the gas cylinder to be replaced, one of the first gas concentration and the second gas concentration, is obtained, and the inspection value is input to an apparatus control unit (90). Then, the apparatus control unit automatically corrects the gas flow rate of the first raw material dilution gas introduced from the first raw material gas cylinder into the reactor and the gas flow rate of the second raw material dilution gas introduced from the second raw material gas cylinder into the reactor based on the test values so that the number of atoms of the first raw material when the first gas concentration is a target value and the number of atoms of the second raw material when the second gas concentration is a target value are obtained, and a recipe for growing an epitaxial film is created, and the first raw material dilution gas and the second raw material dilution gas are introduced into the reactor containing the substrate at the automatically corrected gas flow rates according to the recipe to grow an epitaxial film.
[0010] In this way, when replacing the cylinders, the gas flow rates of the first and second raw material dilution gases are automatically corrected to create a recipe so that the target number of atoms is maintained even for the first and second gas concentrations after the cylinder replacement. For example, the gas concentration of the first raw material dilution gas in the first raw material gas cylinder and the gas concentration of the second raw material dilution gas in the second raw material gas cylinder after the cylinder replacement are inspected, and the ratio of the inspection value to the target gas concentration is calculated. Then, based on the calculated ratio, the gas flow rates of the first and second raw material dilution gases are automatically corrected so that the number of atoms of the first and second raw materials before and after the replacement are the same, and a recipe is created based on this.
[0011] By growing an epitaxial film according to the recipe obtained in this way, the atomic numbers of the first and second raw materials can be kept constant and stabilized before and after changing the cylinder, and the in-plane distribution of the epitaxial film thickness can be stably set to the target value. Therefore, it is possible to easily fix the epitaxial film formation recipe without having to carry out complicated experiments.
[0012] According to an eighth aspect of the present invention, there is provided an apparatus for manufacturing a binary compound semiconductor for growing an epitaxial film (2) on a binary compound semiconductor substrate (1) by supplying a first source gas containing a first source and a second source gas containing a second source, the apparatus including a first source gas cylinder (41) containing a first source dilution gas obtained by diluting the first source gas with a dilution gas to a first gas concentration, a second source gas cylinder (42) containing a second source dilution gas obtained by diluting the second source gas with a dilution gas that is the same as or different from the dilution gas, a reaction furnace (20) constituting a growth chamber for accommodating and heating the substrate, and a first source gas when the first gas concentration is a target value. and an apparatus control unit (90) which stores the gas flow rate of the second raw material when the second gas concentration is a target value, and when replacing at least one of the first raw material gas cylinder and the second raw material gas cylinder, inputs an inspection value of the gas concentration of the gas cylinder to be replaced, out of the first gas concentration and the second gas concentration, and automatically corrects the gas flow rate of the first raw material dilution gas introduced from the first raw material gas cylinder to the reaction furnace and the gas flow rate of the second raw material dilution gas introduced from the second raw material gas cylinder to the reaction furnace based on the inspection value so as to obtain the number of atoms of the first raw material when the first gas concentration is the target value and the number of atoms of the second raw material when the second gas concentration is the target value, thereby creating a recipe for growing an epitaxial film.
[0013] In this way, it is possible to provide a manufacturing apparatus that realizes the epitaxial film manufacturing method described in claim 1. By providing such a manufacturing apparatus, it becomes possible to easily fix the film formation recipe of the epitaxial film without having to perform complicated experiments.
[0014] The reference symbols in parentheses attached to each component indicate an example of the correspondence between the component and specific components described in the embodiments described below. [Brief description of the drawings]
[0015] [Figure 1] FIG. 1 is a diagram showing a schematic configuration of an epitaxial film manufacturing apparatus according to a first embodiment. [Diagram 2] FIG. 1 is a diagram showing a conventional manufacturing flow of an epitaxial film. [Diagram 3] FIG. 13 is a diagram showing the results of investigating the susceptor radius, which is the distance from the center of the susceptor part, and the p-type impurity concentration of the epitaxial film at that location. [Figure 4] FIG. 1 is a diagram showing the results of investigating the relationship between the depth in the thickness direction of an epitaxial film and the p-type impurity concentration. [Diagram 5] FIG. 2 is a diagram showing a manufacturing flow based on the manufacturing method according to the first embodiment. [Figure 6] 3 is a table showing an example of a recipe created in the manufacturing method according to the first embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] Hereinafter, embodiments of the present invention will be described with reference to the drawings. In the following embodiments, parts that are the same or equivalent to each other will be denoted by the same reference numerals.
[0017] (First embodiment) A method and an apparatus for manufacturing a binary compound semiconductor according to a first embodiment of the present invention will be described. Here, an example will be described in which an epitaxial film of SiC is formed on a SiC substrate as a binary compound semiconductor, but this embodiment can also be applied to binary compound semiconductors other than SiC. This embodiment can also be applied to a case in which an epitaxial film is further formed on an epitaxial film or an ion-implanted layer formed on a SiC substrate.
[0018] First, an epitaxial film manufacturing apparatus, which is a binary compound semiconductor manufacturing apparatus according to this embodiment, will be described with reference to FIG.
[0019] The epitaxial film growth apparatus 10 shown in Fig. 1 is an apparatus for growing an epitaxial film 2 on the surface of a substrate 1 made of SiC. As shown in Fig. 1, the epitaxial film growth apparatus 10 of this embodiment is configured to include a furnace body 20, a gas inlet 30, various gas cylinders 40, a gas inlet path 50, a gas outlet 60, a susceptor unit 70, a heating unit 80, and an apparatus control unit 90.
[0020] The furnace body 20 corresponds to a reaction furnace, and is configured such that a heat insulating material 22 and a heated portion 23 are arranged in this order inside a cover 21 made of quartz or the like, and is cylindrical with a hollow portion that constitutes a growth chamber 24 in which a substrate 1 for growing an epitaxial film 2 is placed. The heated portion 23 is a portion that is induction heated by a heating portion 80, which will be described later, and is arranged so as to substantially surround the growth chamber 24 in this embodiment. The heated portion 23 is made of, for example, carbon or the like.
[0021] The gas inlet 30 is an inlet for introducing various gases for growing the epitaxial film 2 into the growth chamber 24 of the furnace body 20, and is provided on one end side of the cylindrical furnace body 20. Various gas cylinders 40 are connected to the gas inlet 30 through gas introduction paths 50. As a result, a Si raw material gas containing a Si raw material, a C raw material gas containing a C raw material, a dopant raw material gas containing a dopant raw material, and the like are introduced into the growth chamber 24 from the gas inlet 30.
[0022] The various gas cylinders 40 include a Si source gas cylinder 41, a C source gas cylinder 42, and a dopant gas cylinder 43. The various gas cylinders 40 are each individually replaceable, and when the gas runs out, they are replaced with new ones.
[0023] The Si raw material gas cylinder 41 contains the Si raw material gas, and contains the Si raw material diluted gas obtained by diluting the Si raw material gas with a dilution gas to a predetermined gas concentration. As the Si raw material gas contained in the Si raw material diluted gas, for example, SiH4 (silane) gas is used, but a chlorine-based Si raw material gas (chloride-based raw material) containing Cl having an etching effect, such as SiH2Cl2, SiHCl3, or SiCl4, can also be used. In addition, as the Si raw material diluted gas, for example, a gas in which H2 is added to silane can also be used.
[0024] The C raw material gas cylinder 42 contains the C raw material gas and contains a C raw material diluted gas obtained by diluting the C raw material gas with a dilution gas to a predetermined gas concentration. As the C raw material gas contained in the C raw material diluted gas, for example, C3H8 (propane) gas or the like is used.
[0025] The dopant gas cylinder 43 contains a dopant raw material gas, and contains a dopant raw material diluted gas obtained by diluting the dopant raw material gas with a dilution gas to a predetermined gas concentration. The dopant raw material diluted gas is a gas for controlling the conductivity type of the epitaxial film 2, and contains a dopant raw material gas corresponding to the conductivity type of the epitaxial film 2 to be formed. When epitaxially growing N-type SiC, for example, a dopant raw material diluted gas containing N2 (nitrogen) is used as the dopant raw material gas. When epitaxially growing P-type SiC, for example, a dopant raw material diluted gas containing TMA (trimethylaluminum) is used as the dopant raw material gas.
[0026] As the dilution gas in the various gas cylinders 40, a gas that does not contain Si or C is used, such as H2 gas or an inert gas (rare gas) such as Ar or He. By using such a gas that does not contain Si or C, it is possible to suppress the diffusion of the source gas and also to suppress the formation of unnecessary Si, C, or SiC products, which do not become a particle source.
[0027] The gas concentration of the source gas in each gas cylinder 40, that is, the volume ratio of the source gas to the total volume of the mixed gas of the dilution gas and the source gas, is adjusted to a predetermined target value. However, the actual gas concentration has a predetermined gas concentration tolerance with respect to the target gas concentration. In the case of the Si source gas cylinder 41, for example, the target gas concentration is set to 10%, and the allowable tolerance is ±5%. Therefore, the actual gas concentration in the Si source gas cylinder 41 varies in the range of 9.5 to 10.5%. In the case of the C source gas cylinder 42, for example, the target gas concentration is set to 30%, and the allowable tolerance is ±5%. Therefore, the actual gas concentration in the C source gas cylinder 42 varies in the range of 28.5 to 31.5%. In the case of the dopant gas cylinder 43, if N2 is used as the dopant source gas, for example, the target gas concentration is set to 1.0%, and the allowable tolerance is ±5%. Therefore, the actual gas concentration in the dopant gas cylinder 43 varies within the range of 0.95 to 1.05%.
[0028] The gas inlet passage 50 constitutes a gas flow path connecting the various gas cylinders 40 and the furnace body 20. The gas inlet passage 50 has a first passage 51 connected to the Si raw material gas cylinder 41, a second passage 52 connected to the C raw material gas cylinder 42, and a third passage 53 connected to the dopant gas cylinder 43, and the first to third passages 51 to 53 are provided with flow rate control valves 54 to 56, respectively. The flow rate control valves 54 to 56 can adjust the opening degree based on a control signal from the device control unit 90, and the flow rate control valves 54 to 56 are individually controlled to adjust the flow rate of gas supplied from the various gas cylinders 40 to the first to third passages 51 to 53.
[0029] The gas exhaust port 60 is disposed on the opposite side of the furnace body 20 to the gas inlet port 30, and exhausts unreacted gases and the like that have passed through the growth chamber 24. The gas exhaust port 60 is also connected to a suction unit (not shown) or the like so that the atmospheric pressure in the growth chamber 24 can be appropriately adjusted, and the growth chamber 24 can be evacuated.
[0030] The susceptor section 70 is disk-shaped and has a mounting section 71 that constitutes a mounting surface on which the substrate 1 is placed, and a support shaft 72 that extends downward from the center of the mounting section 71, and is disposed so that the mounting section 71 is located between the gas inlet 30 and the gas outlet 60. The susceptor section 70 is made rotatable by connecting the support shaft 72 to a rotation mechanism (not shown).
[0031] Although the figure shows a plurality of substrates 1 arranged on the installation surface of the susceptor section 70, the number of substrates 1 arranged on the installation surface is arbitrary. For example, in the case of a single substrate, the substrate 1 is arranged so that the center of the susceptor section 70 and the center of the substrate 1 coincide with each other, and in the case of a plurality of substrates, the substrates 1 are arranged in a circumferential direction around the center of the susceptor section 70.
[0032] The heating unit 80 is composed of a coil arranged to surround the furnace body 20. The heating unit 80 inductively heats the heated portion 25 by applying an alternating current thereto, thereby maintaining the inside of the growth chamber 24 at a predetermined temperature.
[0033] The device control unit 90 controls the aperture of each of the flow rate adjustment valves 54-56, thereby controlling the gas flow rates of the diluted Si raw material gas from the Si raw material gas cylinder 41, the diluted C raw material gas from the C raw material gas cylinder 42, and the diluted dopant raw material gas from the dopant gas cylinder 43. For example, the device control unit 90 controls the flow rates of each gas by transmitting control signals for controlling the aperture of each of the flow rate adjustment valves 54-56.
[0034] More specifically, when at least one of the Si raw material gas cylinder 41 and the C raw material gas cylinder 42 is replaced, the device control unit 90 controls the flow rate of each gas so that the epitaxial film 2 can be grown under the same conditions as when the gas concentration is the target value, even if the gas concentration is different from the predetermined target value. That is, the device control unit 90 stores a recipe for each gas flow rate when the gas concentration is the target value, and automatically corrects the gas flow rate after replacement based on this and the inspection value of the actual gas concentration so that the number of gas molecules, in other words the number of Si and C atoms, is the same as when the gas concentration is the target value. Also, when the dopant gas cylinder 43 is replaced, the gas flow rate is automatically corrected so that the gas molecular weight, in other words the number of dopant atoms, is the same as when the gas concentration of the dopant raw material dilution gas is the target value after replacement. Then, a recipe after replacement is created based on the result of the automatic correction, and the opening of each flow rate control valve 54 to 56 is controlled according to the recipe during the growth process of the epitaxial film 2 to adjust the gas flow rate. The method of automatic correction and creating a recipe after replacement will be described in detail later.
[0035] The above is the configuration of the epitaxial film growth apparatus 10 in this embodiment. Next, a method for manufacturing a SiC semiconductor in this embodiment will be described with reference to a conventional manufacturing method.
[0036] In the conventional manufacturing method, an epitaxial film is grown according to the manufacturing flow shown in Fig. 2. First, in step S100, various gas cylinders are replaced, and then in step S110, an epitaxial film is grown on a SiC substrate, which serves as a reference sample, and various parameters are measured. Specifically, experiments are performed to measure the in-plane distribution of the film thickness, the dopant incorporation efficiency, and the concentration profile.
[0037] At this time, the flow rate is first changed from the flow rate under the epitaxial film growth conditions before the exchange of the various gas cylinders, and the flow rate is gradually changed until the parameters of the in-plane distribution of the epitaxial film thickness, the dopant incorporation efficiency, and the concentration profile reach their target values. Then, in step S120, a calibration curve is obtained in which each parameter reaches the target value.
[0038] Thereafter, in step S130, a recipe is created based on the calibration curve obtained above so that each parameter has a target value, and then, in step S140, an epitaxial film is grown according to the created recipe to obtain an epitaxial film in which each parameter has a target value.
[0039] In this way, in order to ensure that each parameter of the epitaxial film reaches the target value, it is necessary to conduct experiments by starting from the flow rates that were in the epitaxial film growth conditions before the various gas cylinders were replaced, and then gradually changing the flow rates.
[0040] As described above, for example, the gas concentration of the Si raw material dilution gas is targeted to 10%, with a tolerance of ±5%, so even if the target concentration of the Si raw material dilution gas is 10%, the gas concentration in the Si raw material gas cylinder is 9.5 to 10.5%. Because of this variation in gas concentration, each parameter of the grown epitaxial film varies, and various experiments are conducted by changing the flow rates of each gas.
[0041] For example, the susceptor radius, which is the distance from the center of the susceptor part 70, and the p-type impurity concentration of the epitaxial film at that location were investigated for the case where the gas concentration of the C raw material dilution gas was the target value (ref.) and the case where the gas concentration varied by +5% and -5% from the target value. In addition, the relationship between the depth in the thickness direction of the epitaxial film and the p-type impurity concentration was investigated. Figures 3 and 4 show these results.
[0042] As shown in Fig. 3, the p-type impurity concentration with respect to the susceptor radius is significantly different from the target value in both cases of +5% and -5%. Also, as shown in Fig. 4, the p-type impurity concentration for each depth of the epitaxial film is significantly different from the target value in both cases of +5% and -5%. For this reason, every time the raw gas cylinder is replaced, it is necessary to prepare a SiC substrate as a reference sample, form an epitaxial film on it, and then repeatedly perform experiments to determine the in-plane distribution of the epitaxial film thickness, the dopant incorporation efficiency, and the concentration profile measurement. Therefore, experiments must be performed until each parameter reaches the target value to obtain a calibration curve, which not only requires complicated experiments but also makes it difficult to fix the epitaxial film formation recipe.
[0043] Therefore, in this embodiment, in order to eliminate the need for complicated experiments and to easily fix the deposition recipe for the epitaxial film, the epitaxial film 2 is grown on the substrate 1 while controlling the concentrations of the raw material gas and the dopant gas according to the manufacturing flow shown in FIG. 5.
[0044] First, in step S200, the various gas cylinders 41 to 43 are prepared, and the various gas cylinders 41 to 43 are replaced. At this time, only those of the various gas cylinders 41 to 43 that are empty or nearly empty of gas may be replaced.
[0045] Next, in step S210, the gas concentrations in the Si source gas cylinder 41, the C source gas cylinder 42, and the dopant gas cylinder 43 are inspected to obtain inspection values.
[0046] The gas concentration of the Si raw material diluted gas in the Si raw material gas cylinder 41 may be, for example, 10% as a target value, and may vary in the range of 9.5 to 10.5%, but the gas concentration may be specified and distributed. In that case, the inspection is performed by confirming the specified gas concentration. Similarly, the gas concentration of the C raw material diluted gas in the C raw material gas cylinder 42 may be, for example, 30% as a target value, and may vary in the range of 28.5 to 31.5%, but the gas concentration may be specified and distributed. In that case, the inspection is also performed by confirming the specified gas concentration. Furthermore, the gas concentration of the dopant gas in the dopant gas cylinder 43 may be, for example, 1.0% as a target value, and may vary in the range of 0.95 to 1.05%, but the gas concentration may be specified and distributed. In that case, the inspection is also performed by confirming the specified gas concentration.
[0047] Next, in step S220, the device control unit 90 calculates the ratio of the test value to the target value. For example, in the case of the Si raw material gas cylinder 41, if the target value of the gas concentration of the diluted Si raw material gas is 10% and the test value of the actual gas concentration is 10.5%, the ratio of the test value to the target value is 1.05. Similarly, in the case of the C raw material gas cylinder 42, if the target value of the gas concentration of the diluted C raw material gas is 30% and the test value of the actual gas concentration is 29.0%, the ratio of the test value to the target value is 0.967.
[0048] Then, in step S230, the gas flow rate is automatically corrected based on the calculated ratio so that the number of gas molecules, in other words the number of Si and C atoms, is the same as the target value even after the replacement, and a recipe for this is created and stored in the device control unit 90.
[0049] That is, a recipe is created in which correction is made based on the inspection value calculated from the actual gas concentration in response to the recipe in which the gas concentration is the target value. As an example, a recipe as shown in FIG. 6 is created. FIG. 6 shows a case where the Si raw material gas cylinder 41 and the C raw material gas cylinder 42 are replaced, and when at least one of the Si raw material gas cylinder 41 and the C raw material gas cylinder 42 is replaced, the gas flow rate of the replaced side is automatically corrected. Also, FIG. 6 shows a case where the dopant gas cylinder 43 is not replaced, but when it is replaced, automatic correction can be made in the same way as the Si raw material dilution gas and the C raw material dilution gas described later. Note that this figure shows the flow rates when each gas is introduced into the furnace body 20 under standard conditions, for example, 27° C. and 1 atm, but when applied to the growth of the epitaxial film 2, the flow rates are converted to the temperature and atmospheric pressure during the growth of the epitaxial film 2.
[0050] FIG. 6 shows two recipes: recipe 1, in which the epitaxial film 2 is grown at a relatively slow growth rate (hereinafter referred to as slow growth), and recipe 2, in which the epitaxial film 2 is grown at a faster growth rate than recipe 1 (hereinafter referred to as fast growth).
[0051] Recipe 1 includes step 1, in which epitaxial film 2 is grown at a slower growth rate than the slow growth rate during the initial growth, and step 2, in which epitaxial film 2 is grown at a faster growth rate than the initial growth rate.
[0052] For example, when the gas concentrations of various gases are as targeted, the gas flow rates and gas introduction times of each step are set so that the number of Si and C atoms is the desired value based on the target value. When the gas concentration of the Si raw material dilution gas is 10%, the gas concentration of the C raw material dilution gas is 30%, and the gas concentration of the dopant gas is 1.0%, the flow rates and introduction times of various gases in each of steps 1 and 2 are set to the values shown in the figure. At this time, the flow rates of the Si raw material dilution gas and the C raw material dilution gas are set so that the number of Si and C atoms introduced into the furnace body 20 is a predetermined number. In the case of step 1, the Si raw material dilution gas is 80.0 sccm, and the C raw material dilution gas is 60.0 sccm. In addition, in the case of step 2, the Si raw material dilution gas is 240.0 sccm, and the C raw material dilution gas is 180.0 sccm.
[0053] The number of Si and C atoms introduced into the furnace body 20 is a predetermined number determined by the gas concentration of the Si raw material dilution gas and the gas concentration of the C raw material dilution gas and the flow rate of each gas. That is, the number of Si atoms in SiH4 is 1, and the number of C atoms in C3H8 is 3. Since each gas concentration represents the content of SiH4 or C3H8 per unit volume, the number of Si and C atoms introduced into the furnace body 20 per unit time is determined by each gas concentration and gas flow rate.
[0054] For example, in step 1, the number of Si atoms per unit time introduced into the furnace body 20 is 1 [number of Si atoms] × 0.1 [gas concentration] × 80.0 [sccm: flow rate] × K, and the number of C atoms is 3 [number of C atoms] × 0.3 [gas concentration] × 60.0 [sccm: flow rate] × K. In step 2, the number of Si atoms per unit time is 1 [number of Si elements] × 0.1 [gas concentration] × 240.0 [sccm: flow rate] × K, and the number of C atoms is 3 [number of C elements] × 0.3 [gas concentration] × 180.0 [sccm: flow rate] × K. K is a coefficient equivalent to the number of molecules contained per unit volume.
[0055] In contrast, when the Si raw material gas cylinder 41 and the C raw material gas cylinder 42 are replaced, the gas concentration of the diluted Si raw material gas is 10.5% and the gas concentration of the diluted C raw material gas is 29.0%, as shown in Fig. 6. In this case as well, the flow rates of the diluted Si raw material gas and the diluted C raw material gas are set so that the number of atoms becomes equal to the number of atoms when the gas concentrations are the target values.
[0056] That is, in step 1, the number of Si atoms per unit time is 1 [number of Si elements] × 0.105 [gas concentration] × 76.2 [sccm: flow rate] × K, and the number of C atoms is 3 [number of C elements] × 0.29 [gas concentration] × 62.1 [sccm: flow rate] × K. The number of Si atoms is approximately equal to 1 [number of Si atoms] × 0.1 [gas concentration] × 80.0 [sccm: flow rate] × K before the replacement and 1 [number of Si elements] × 0.105 [gas concentration] × 76.2 [sccm: flow rate] × K after the replacement, and is maintained as a predetermined number. In addition, the number of C atoms is approximately equal to 3 [number of C atoms] × 0.3 [gas concentration] × 60.0 [sccm: flow rate] × K before the replacement and 3 [number of C elements] × 0.29 [gas concentration] × 62.1 [sccm: flow rate] × K after the replacement, and is maintained as a predetermined number.
[0057] Also, in step 2, the number of Si atoms per unit time is 1 [number of Si elements] × 0.105 [gas concentration] × 228.6 [sccm: flow rate] × K, and the number of C atoms is 3 [number of C elements] × 0.29 [gas concentration] × 186.2 [sccm: flow rate] × K. The number of Si atoms is approximately equal to 1 [number of Si atoms] × 0.1 [gas concentration] × 240.0 [sccm: flow rate] × K before the replacement and 1 [number of Si elements] × 0.105 [gas concentration] × 228.6 [sccm: flow rate] × K after the replacement, and is maintained as a predetermined number. The number of C atoms is approximately equal to 3 [number of C atoms] × 0.3 [gas concentration] × 180 [sccm: flow rate] × K before the replacement and 3 [number of C elements] × 0.29 [gas concentration] × 186.2 [sccm: flow rate] × K after the replacement, and is maintained as a predetermined number.
[0058] In this way, the gas flow rate is controlled so that the number of atoms of Si and C contained in each gas is maintained at a predetermined number before and after the replacement of the gas cylinder. Furthermore, by controlling the gas flow rate in this way, the element ratios of Si and C after the replacement of the gas cylinder can also be made to reach the target values.
[0059] That is, one Si element is contained in SiH4, and three C elements are contained in C3H8. Therefore, in step 1, the element ratio of Si and C per unit time is 1 [number of Si elements] x 0.1 [gas concentration] x 80.0 [sccm: flow rate]: 3 [number of C elements] x 0.3 [gas concentration] x 60.0 [sccm: flow rate] = 8:54 = 4:27. Also, in step 2, the element ratio of Si and C per unit time is 1 [number of Si elements] x 0.1 [gas concentration] x 240.0 [sccm: flow rate]: 3 [number of C elements] x 0.3 [gas concentration] x 180.0 [sccm: flow rate] = 24:162 = 4:27.
[0060] On the other hand, even when the Si raw material gas cylinder 41 and the C raw material gas cylinder 42 are replaced, the flow rates of the Si raw material dilution gas and the C raw material dilution gas are set so that the element ratio is equal to the element ratio when the gas concentration is the target value. That is, in step 1, the element ratio of Si and C per unit time is set to 1 [number of Si elements] × 0.105 [gas concentration] × 76.2 [sccm: flow rate]: 3 [number of C elements] × 0.29 [gas concentration] × 62.1 [sccm: flow rate] ≒ 8:54 = 1: 9. Also, in step 2, the element ratio of Si and C per unit time is set to 1 [number of Si elements] × 0.105 [gas concentration] × 228.6 [sccm: flow rate]: 3 [number of C elements] × 0.29 [gas concentration] × 186.2 [sccm: flow rate] ≒ 24: 162 = 4: 27.
[0061] In this way, the flow rates of the diluted Si raw material gas and the diluted C raw material gas are set and a recipe is created so that the numbers of Si and C atoms are maintained at predetermined values even after the Si raw material gas cylinder 41 and the C raw material gas cylinder 42 are replaced.
[0062] Here, the method of creating recipe 1 has been described, but the same is true for recipe 2. Recipe 1 is applied, for example, when low-speed growth is desired, and recipe 2 is applied, for example, when high-speed growth is desired. An example of a case where low-speed growth is desired is when the epitaxial film 2 is grown on an ion-implanted layer in which the underlying SiC is ion-implanted with impurities. In such a case, high-speed growth would result in more significant inheritance of damage during ion implantation, so low-speed growth is desirable in which the inheritance of damage is suppressed. An example of a case where high-speed growth is desirable is when a drift layer is formed on a SiC substrate 1. In such a case, the epitaxial film 2 is grown on an underlying substrate with a good surface condition that is not damaged by ion implantation on the SiC substrate 1, so the possibility of crystal defects is relatively low. For this reason, high-speed growth that can increase the growth rate is desirable. In addition, recipes 1 and 2 have been given as examples, but these are merely given as examples of cases where low-speed growth and high-speed growth are performed, and other recipes can be created.
[0063] In addition, although N2, which is an n-type dopant, is used as the dopant gas, other dopant gases may be used. For example, NH4 containing N, which is an n-type dopant, or TMA (trimethylaluminum) containing Al, which is a p-type dopant, may be used. In the case of NH4 or TMA, these are diluted with dilution gas such as H2 and stored in the dopant gas cylinder 43. In this case, when the dopant gas cylinder 43 is replaced, if a recipe is created by performing automatic correction in the same manner as the above-mentioned Si raw material dilution gas and C raw material dilution gas, the dopant intake efficiency and concentration profile can be stably set to the target value.
[0064] Once the recipe is created in this manner, in step S240, a growth process of the epitaxial film 2 is performed according to the recipe created in step S230. That is, an epitaxial film growth apparatus 10 having a furnace body 20 equivalent to a reactor as shown in Fig. 1 is prepared, and a substrate 1 made of SiC is placed therein. Then, the epitaxial film 2 is grown on the surface of the substrate 1 according to the created recipe.
[0065] This makes it possible to keep the number of Si and C atoms, in other words, the element ratio, constant and stable before and after replacement of the Si source gas cylinder 41 and the C source gas cylinder 42, thereby making it possible to stably achieve a target value for the in-plane distribution of the film thickness of the epitaxial film 2. Furthermore, it is possible to stably achieve the target values for the dopant incorporation efficiency and concentration profile in the epitaxial film 2 as well.
[0066] The manufacturing flow as shown in FIG. 5 is performed every time the cylinder is replaced, and each time, a recipe is created so that the number of Si and C atoms, in other words, the element ratio, is approximately the same as the target value as the deposition conditions of the epitaxial film 2.
[0067] As described above, when replacing the cylinders, the gas flow rates of the Si raw material dilution gas and the C raw material dilution gas are automatically corrected to create a recipe so that the target number of atoms is maintained even for the gas concentrations of the Si raw material dilution gas and the C raw material dilution gas after the cylinder replacement. Specifically, the gas concentration of the Si raw material dilution gas in the Si raw material gas cylinder 41 and the gas concentration of the C raw material dilution gas in the C raw material gas cylinder 42 after the cylinder replacement are inspected, and the ratio of the inspection value to the target gas concentration is calculated. Then, based on the calculated ratio, the gas flow rates of the Si raw material dilution gas and the C raw material dilution gas are automatically corrected so that the numbers of Si and C atoms are the same before and after the replacement, and a recipe is created based on that.
[0068] By growing the epitaxial film 2 according to the recipe thus obtained, the number of Si and C atoms, in other words, the element ratio, can be made constant and stabilized before and after replacement of the Si source gas cylinder 41 and the C source gas cylinder 42. This makes it possible to stably set the in-plane distribution of the film thickness of the epitaxial film 2 to a targeted value. Furthermore, the dopant incorporation efficiency and concentration profile in the epitaxial film 2 can also be stably set to the targeted values.
[0069] 6, the dopant gas cylinder 43 is not replaced, but when the dopant gas cylinder 43 is replaced, a recipe can be created by automatically correcting the gas flow rate of the dopant gas so that the number of dopant atoms remains constant before and after the replacement. This allows the dopant uptake efficiency and concentration profile in the epitaxial film 2 to be stable and reach the target values before and after the replacement.
[0070] (Other embodiments) Although the present disclosure has been described based on the above-described embodiment, it is not limited to the embodiment, and includes various modifications and modifications within the equivalent range. In addition, various combinations and forms, and other combinations and forms including only one element, more than one element, or less than one element, are also within the scope and concept of the present disclosure.
[0071] For example, in each of the above embodiments, as an example of a method for inspecting the gas concentration when the cylinder is replaced, a case where the gas concentration is specified and distributed is given as an example. However, this is merely one example. For example, the Si raw material diluted gas or the C raw material diluted gas may be discharged from the replaced Si raw material gas cylinder 41 or the C raw material gas cylinder 42, and the gas concentration may be measured with a gas concentration measuring device such as an in-situ monitor to obtain the inspection value. In this way, if the gas concentration during discharge is measured to obtain the inspection value, it is possible to deal with the case where the gas concentration changes during the flow into the furnace body 20.
[0072] Although the present invention has been described by taking SiC as an example of a binary compound semiconductor, the present invention can also be applied to other binary compound semiconductors, such as GaN, AsGa, and InP, when replacing a raw material gas cylinder or a dopant gas cylinder. That is, a first raw material gas cylinder containing a first raw material diluted gas obtained by diluting a first raw material gas with a dilution gas to a first gas concentration, and a second raw material gas cylinder containing a second raw material diluted gas obtained by diluting a second raw material gas with a dilution gas to a second gas concentration are prepared. The present invention can be applied to setting the gas flow rate when replacing the gas cylinder when manufacturing a binary compound semiconductor using these first raw material gas cylinder and second raw material gas cylinder. Also, for the dopant raw material, a dopant gas cylinder containing a dopant raw material diluted gas obtained by diluting with a dilution gas to a third gas concentration is prepared, and the present invention can be applied to setting the gas flow rate when replacing this gas cylinder. However, in the case of SiC, the cylinder needs to be replaced frequently and the absolute value of the impurity concentration and the in-plane distribution are highly dependent on the C / Si ratio, so that the effect of applying the present invention is greater than in the case of other binary compound semiconductors.
[0073] Although H2 is used as an example of the dilution gas, a dilution gas other than H2, for example, a rare gas such as Ar or an etching gas such as HCl, may be used. In this case, the gas species of the dilution gas used in the various gas cylinders 41 to 43 may be the same or different.
[0074] In the above embodiment, the number of Si and C atoms is equalized before and after the gas cylinder replacement by calculating the ratio of the test value to the target value of the gas concentration and automatically correcting the gas flow rate after the gas cylinder replacement. However, the present invention is not limited to this, and it is also possible to obtain the number of Si and C atoms at the target value supplied to the furnace body 20 per unit time and set the gas flow rate so that the number of Si and C atoms in the test value is equal to the number of Si and C atoms at the target value.
[0075] In the above embodiment, the present invention has been described as a method and an apparatus for manufacturing a binary compound semiconductor. However, the present invention can also be understood as a program for manufacturing a binary compound semiconductor, including automatic correction of gas flow rates, which is applied to the manufacture of a binary compound semiconductor. In this case, (1) a step of storing the gas flow rates of the first raw material at the gas concentration of the first raw material dilution gas at the target value and the second raw material at the gas concentration of the second raw material dilution gas is performed. Then, when the cylinder is replaced, (2) a step of inputting that the cylinder has been replaced and (3) a step of inputting the inspection value of the gas concentration are performed. After that, (4) a step of creating a recipe in which the gas flow rates of the first raw material dilution gas and the second raw material dilution gas are automatically corrected so that the atomic numbers of the first raw material and the second raw material at the inspection value become the atomic numbers at the target value is performed. Then, (5) a step of forming the epitaxial film 2 according to the created recipe is performed. A program for manufacturing a binary compound semiconductor having each of these steps can be obtained. [Explanation of symbols]
[0076] 1 Board 2 Epitaxial film 10 Epitaxial film growth equipment 20 Furnace body 41 Silicon gas cylinder 42 C raw gas cylinder 43 Dopant Gas Cylinder 70 Susceptor part
Claims
1. A method for manufacturing a binary compound semiconductor, comprising the steps of: supplying a first source gas containing a first source and a second source gas containing a second source to grow an epitaxial film (2) on a substrate (1) of the binary compound semiconductor, the method comprising the steps of: preparing a first raw material gas cylinder (41) for accommodating a first raw material dilution gas obtained by diluting the first raw material gas with a dilution gas to a first gas concentration, and a second raw material gas cylinder (42) for accommodating a second raw material dilution gas obtained by diluting the second raw material gas with a dilution gas that is the same as or different from the dilution gas, Providing a reactor (20) constituting a growth chamber for containing and heating the substrate; When replacing at least one of the first source gas cylinder and the second source gas cylinder, an inspection value of the gas concentration of the gas cylinder to be replaced is obtained, out of the first gas concentration and the second gas concentration; inputting the test value into a device control unit (90); the apparatus control unit automatically corrects a gas flow rate of the first raw material dilution gas introduced from the first raw material gas cylinder into the reactor and a gas flow rate of the second raw material dilution gas introduced from the second raw material gas cylinder into the reactor based on the test value so that the number of atoms of the first raw material when the first gas concentration is a target value and the number of atoms of the second raw material when the second gas concentration is a target value are obtained, and creates a recipe for growing the epitaxial film; growing the epitaxial film by introducing the first dilution source gas and the second dilution source gas into the reactor containing the substrate at the automatically corrected gas flow rates according to the recipe; A method for producing a binary compound semiconductor, comprising:
2. 2. The method for manufacturing a binary compound semiconductor according to claim 1, wherein, in obtaining the inspection values, the first diluted raw material gas is discharged from the first raw material gas cylinder and the second diluted raw material gas is discharged from the second raw material gas cylinder using a gas concentration measuring instrument to obtain the inspection values of the first gas concentration and the second gas concentration.
3. A silicon carbide substrate (1) is used as the substrate, 3 . The method for producing a binary compound semiconductor according to claim 1 , wherein the first source gas containing Si is used as the first source material, and the second source gas containing C is used as the second source material.
4. The first source dilution gas is SiH 4 H, which is a diluent gas of the first diluent gas 2 Dilute with The second raw material dilution gas is C which becomes the second raw material gas. 3 H 8 The dilution gas of the second dilution gas is H 2 4. The method for producing a binary compound semiconductor according to claim 3, wherein the diluted solution is one containing
5. preparing a dopant gas cylinder (43) for storing a diluted dopant source gas obtained by diluting a dopant source gas containing a dopant source with a third gas concentration; obtaining a test value of the third gas concentration when replacing the dopant gas cylinder; inputting the test value of the third gas concentration into the device controller; and automatically correcting, by the apparatus control unit, a gas flow rate of the diluted dopant source gas introduced from the dopant gas cylinder into the reactor based on the inspection value of the third gas concentration so that the number of atoms of the dopant source is equal to a target value for the third gas concentration, and creating the recipe for growing the epitaxial film; 5. The method for manufacturing a binary compound semiconductor according to claim 1, wherein, in growing the epitaxial film, the dopant source gas is introduced in addition to the first dilution source gas and the second dilution source gas according to the recipe to grow the epitaxial film.
6. The dopant source dilution gas is N 2 , N.H. 3 or trimethylaluminum, which is a diluent gas for the dopant source diluent gas. 2 6. The method for producing a binary compound semiconductor according to claim 5, wherein the diluted solution is one containing
7. 7. The method for manufacturing a binary compound semiconductor according to claim 1, wherein, in creating the recipe, a ratio of the gas concentration of the inspection value to a case where the first gas concentration and the second gas concentration are target values is calculated, and the automatic correction is performed based on the ratio.
8. An apparatus for manufacturing a binary compound semiconductor, which supplies a first source gas containing a first source and a second source gas containing a second source to grow an epitaxial film (2) on a substrate (1) of the binary compound semiconductor, comprising: a first raw material gas cylinder (41) for accommodating a first raw material diluted gas obtained by diluting the first raw material gas with a dilution gas to a first gas concentration; a second raw material gas cylinder (42) for accommodating a second raw material diluted gas obtained by diluting the second raw material gas to a second gas concentration with a dilution gas that is the same as or different from the dilution gas; a reactor (20) constituting a growth chamber for accommodating and heating the substrate; an apparatus control unit (90) which stores gas flow rates of the first raw material when the first gas concentration is a target value and the second raw material when the second gas concentration is a target value, and when replacing at least one of the first raw material gas cylinder and the second raw material gas cylinder, inputs an inspection value of the gas concentration of the gas cylinder to be replaced, out of the first gas concentration and the second gas concentration, and automatically corrects the gas flow rate of the first raw material dilution gas introduced from the first raw material gas cylinder to the reactor and the gas flow rate of the second raw material dilution gas introduced from the second raw material gas cylinder to the reactor based on the inspection value so as to obtain the number of atoms of the first raw material when the first gas concentration is the target value and the number of atoms of the second raw material when the second gas concentration is the target value, and creates a recipe for growing the epitaxial film; The manufacturing apparatus for binary compound semiconductors includes:
Citation Information
Patent Citations
Vapor growth device
JP1995193014A
Silicon carbide semiconductor, its manufacturing method and manufacturing apparatus
JP2006261612A
Epitaxial silicon carbide single-crystal substrate and method for producing the same
JP2011236085A
Vapor deposition apparatus and vapor deposition method
JP2014187113A
Method for producing silicon carbide epitaxial substrate, method for producing semiconductor device, and semiconductor device
JP2015179781A