Laminate and electrochromic device
A gel electrolyte with a peeling index of 5.5 mm^-1 to 7.5 mm^-1, using polymethyl methacrylate chains and high ionic liquid content, addresses deformation and peeling issues, ensuring optical uniformity and stability in electrochemical devices.
Patent Information
- Application Number
- JP2021039826
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-12
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2041-03-12
AI Technical Summary
Gel electrolytes face issues with optical distortion due to deformation during transportation and storage, and difficulty in peeling off protective films during use, which affects their adhesion and stability in electrochemical devices.
A gel electrolyte composition containing a binder resin and a supporting electrolyte, with a specific peeling index value of 5.5 mm^-1 to 7.5 mm^-1, ensuring self-adhesion during transportation and easy peelability during use, achieved through the use of a polymer with polymethyl methacrylate chains and high ionic liquid content.
The solution provides a gel electrolyte that maintains optical uniformity by preventing deformation and peeling, suitable for electrochemical devices like electrochromic elements, lithium ion secondary batteries, solar cells, and fuel cells, with enhanced buckling resistance and peelability.
Smart Images

Figure 0007593173000008 
Figure 0007593173000009 
Figure 0007593173000010
Abstract
Description
[Technical field]
[0001] The present invention relates to a gel electrolyte and an electrochromic device. [Background technology]
[0002] In electrochromic elements using electrochromic materials, when obtaining a transparent display device, and when constructing a device having three laminated color-developing layers of cyan (C), magenta (M), and yellow (Y), it is important that the device is made of a material that is colorless and transparent, and that each layer is free of optical distortion such as wrinkles and unevenness and has excellent optical uniformity.
[0003] Liquid electrolytes, in which a supporting electrolyte is dissolved in water or an organic solvent, are used as the electrolyte for many electrochemical elements. However, liquid electrolytes have problems such as deterioration over time during long-term storage of electrochemical elements, leakage of electrolyte due to damage, and difficulty in making them smaller and thinner. For this reason, active research and development is being conducted on solidified electrolytes, solid thin-film electrolyte materials that are easy to handle, highly safe, and have high ionic conductivity.
[0004] There are two main approaches to the study of polymer solid electrolytes: one is gel electrolytes, which contain a liquid electrolyte in a mesh-like polymer matrix, and the other is polymer solid electrolytes, which consist of a supporting electrolyte dissolved in a polymer with a polyether structure, such as polyethylene oxide or polypropylene oxide.
[0005] The gel electrolyte is prepared by carrying out a polymerization reaction in a liquid electrolyte containing a monomer to form a polymer swollen with the liquid electrolyte, or by immersing a prepolymerized polymer matrix in the liquid electrolyte to swell the polymer.
[0006] In the gel electrolyte, the polymer matrix basically only has the function of containing the liquid electrolyte and does not contribute to ion conduction, and it is the liquid electrolyte in the polymer matrix that is mainly responsible for ion conduction. Since ions can move relatively freely in the polymer matrix, the ionic conductivity of the gel electrolyte can relatively easily be made to be as high as that of the liquid electrolyte.
[0007] Since such gel electrolytes have a high liquid electrolyte content, they are unlikely to exhibit self-adhesiveness, and the protective film may peel off from the gel electrolyte during transportation in the roll-to-roll process used for mass film formation and during storage in a rolled state, causing deformation and damage to the gel electrolyte.
[0008] Therefore, for example, in the case of a gel electrolyte that does not have self-adhesive properties, a method has been proposed in which both sides of the gel electrolyte are sandwiched between protective films having adhesive layers as a means for preventing the occurrence of wrinkles and unevenness in the electrolyte membrane during transportation and storage and for peeling off the protective film from the gel electrolyte during use (see, for example, Patent Document 1).
[0009] On the other hand, a polymer solid electrolyte in which a supporting electrolyte is dissolved in a polymer with a polyether structure can dissolve one monovalent cation per four oxygen atoms in the ether structure, and this cation conducts ions by hopping through the ether structure of the polymer chain. This type of polymer solid electrolyte does not contain a liquid electrolyte, so it has the characteristic of easily exhibiting self-adhesiveness. Summary of the Invention [Problem to be solved by the invention]
[0010] The present invention aims to provide a gel electrolyte having self-adhesiveness that does not peel off from a non-adhesive protective film during transportation and storage, and can be easily peeled off from the non-adhesive protective film when in use, in order to prevent the occurrence of optical distortion due to deformation of the gel electrolyte. [Means for solving the problem]
[0011] The gel electrolyte of the present invention as a means for solving the above problems is a gel electrolyte comprising a cured product of an electrolyte composition containing a binder resin and a supporting electrolyte, and is measured by a probe tack test in which a stainless steel probe having a diameter of 5 mm is brought into contact with a gel electrolyte having an average thickness of 700 μm from above at a speed of 120 mm / sec under an environmental condition of 25° C., a pressing load is set to 40 gf, and the pressing load is held for 5 seconds, and the probe is peeled off in the vertical direction at a speed of 400 mm / sec., and the stress, peel distance, and maximum stress are measured. The peel index value obtained by dividing the maximum stress by an integral value obtained by integrating the stress over the peel distance is 5.5 mm. -1 More than 7.5mm -1 The following is the result. Effect of the Invention
[0012] According to the present invention, it is possible to provide a gel electrolyte having self-adhesiveness that does not peel off from the non-adhesive protective film during transportation and storage, and can be easily peeled off from the non-adhesive protective film when in use, in order to prevent the occurrence of optical distortion due to deformation of the gel electrolyte. [Brief description of the drawings]
[0013] [Figure 1] FIG. 1 is a graph showing an example of the measurement results of the tack strength of the gel electrolyte of the present invention. [Diagram 2] FIG. 2 is a graph showing the relationship between peel distance and stress. [Diagram 3] FIG. 3 is a schematic diagram showing an example of the electrochromic element of the present invention. [Figure 4] FIG. 4 shows an example of a graph showing a waveform obtained by measuring impedance at a measurement temperature of 25° C. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] (Gel electrolyte) The gel electrolyte of the present invention is a gel electrolyte comprising a cured product of an electrolyte composition containing a binder resin and a supporting electrolyte, and is measured by a probe tack test in which a stainless steel probe having a diameter of 5 mm is brought into contact with a gel electrolyte having an average thickness of 700 μm from above at a speed of 120 mm / sec under an environmental condition of 25° C., a pressing load of 40 gf is applied, and the pressing load is maintained for 5 seconds. The probe is then peeled off in the vertical direction at a speed of 400 mm / sec under the following conditions: stress, peel distance, and maximum stress are measured; and a peel index value obtained by dividing the maximum stress by an integral value obtained by integrating the stress over the peel distance is 5.5 mm. -1 More than 7.5mm -1 The following is the result.
[0015] The conventional technology (JP Patent Publication 2011-253753 A) has problems such as the adhesive layer transferring to the electrolyte membrane and insufficient adhesion being obtained when transferring to a receiving body, making it difficult to stably peel off the protective film. In addition, in the conventional method of sandwiching a soft fluorine-based polymer solid electrolyte between non-adhesive protective films to prevent the occurrence of wrinkles and unevenness during transportation and storage, there are problems in that since the mobility of a fluorine-based polymer solid electrolyte is lower than that of a liquid electrolyte, in order to achieve high ionic conductivity, the carrier needs to be a proton with a small ionic radius, and there are many other constraints, such as the need to use the electrolyte in a high-humidity environment.
[0016] Therefore, in the present invention, a probe tack test is performed under environmental conditions of 25°C, in which a gel electrolyte with an average thickness of 700 μm is contacted from above with a SUS304 probe with a diameter of 5 mm at a speed of 120 mm / sec, the pressure load is set to 40 gf, the pressure load is held for 5 seconds, and the probe is peeled off in the vertical direction at a speed of 400 mm / sec., and the stress and peel distance are measured, resulting in the peaks shown in Figure 1. Then, the maximum stress 8 (unit: gf) in Figure 1 and the integral value 9 (unit: gf mm) obtained by integrating the stress over the peel distance are obtained. The value obtained by dividing the maximum stress 8 by the integral value 9 is the peel index value (unit: mm -1The probe tack test can be performed, for example, using a tack testing machine (TAC-II, manufactured by Rhesca Corporation). The gel electrolyte having an average thickness of 700 μm may be a laminate of gel electrolytes laminated to have an average thickness of 700 μm.
[0017] The peel index value is 5.5 mm -1 More than 7.5mm -1 By satisfying the following range, it is possible to achieve two seemingly contradictory properties: (1) adhesion that does not peel off from the non-adhesive protective film during roll-to-roll transportation and storage, and (2) releasability that allows the film to be easily peeled off from the non-adhesive protective film when in use. As shown in FIG. 2, the peeling index value is the ratio of the maximum stress (maximum load) 8 to the integral value 9, and is a numerical representation of the curve shape of the peeling distance profile of stress. Therefore, the larger the peeling index value, the sharper the peak will be, and the smaller the peeling index value, the lower the peak will be and the gentler it will be. The peak B of an appropriate size (a peeling index value of 6.3 mm) can achieve both the above characteristics (1) and (2). -1 The low and gentle peak C, which satisfies only the above (1), is difficult to peel off (peel index value 4.0 mm -1 The sharp and large peak A, which satisfies only the above (2), is prone to peeling (peel index value 7.6 mm -1 ). Therefore, as shown in FIG. 2, in the present invention, in order to achieve both the above characteristics (1) and (2), the peel index value is 5.5 mm. -1 More than 7.5mm -1 It is important to meet the following ranges:
[0018] The peel index value is the reciprocal of the amount of strain when the gel electrolyte is stretched with the maximum stress in the probe tack test, i.e., the difficulty of deformation. Therefore, the peel index value shows a high correlation with the amount of strain calculated by dividing the maximum stress from the elastic modulus calculated by dynamic viscoelasticity measurement based on Hooke's law.
[0019] The peeling of gel electrolytes sandwiched between protective films on both sides during transportation and storage is believed to be caused by a buckling phenomenon that occurs when the compressive stress generated at the interface between the gel electrolyte and the protective film due to bending, twisting, etc. exceeds the allowable buckling stress. When the protective film conditions are fixed, the compressive stress generated at the interface between the gel electrolyte and the protective film is determined by the rigidity calculated from the elastic modulus and thickness of the gel electrolyte, and it is expected that the smaller the rigidity, the stronger the resistance to buckling. In addition, the greater the tack strength of the gel electrolyte, the greater the allowable buckling stress, and the greater the expected buckling resistance. On the other hand, when the protective film is warped and peeled off from the gel electrolyte during processing, it is preferable that the gel electrolyte does not follow the warped protective film, that is, the gel electrolyte has high rigidity. Therefore, in order to achieve both buckling resistance during transportation and storage and good releasability during processing, the balance between the tackiness and rigidity of the gel electrolyte is extremely important, and the above-mentioned peel index value, which indicates the resistance of the gel electrolyte to deformation when stretched, is suitable for evaluating this balance.
[0020] During mass film formation, when the conveying direction is changed at the conveying roller in the roll-to-roll process, and when the film is wound around a roller core for storage, compressive stress that causes buckling is applied to the gel electrolyte and protective film. -1 For these, excellent buckling resistance can be achieved.
[0021] The peelability of the protective film during processing is good when the peel index value is 5.5 mm. -1 If the peel index value is 5.5 mm or more, the peel index value can be sufficiently achieved. -1 If the gel electrolyte is less than this, the frequency with which it undergoes plastic deformation or breakage due to fingering instability becomes significantly higher.
[0022] The gel electrolyte of the present invention has the above peeling index value of 7.5 mm -1or less, deformation or damage of the polymer membrane due to peeling of the non-adhesive protective film during transportation and storage can be prevented. This is based on the fact that the compressive stress generated when the gel electrolyte is bent is suppressed to the allowable buckling stress level or less, which is reinforced by the self-adhesiveness of the gel electrolyte.
[0023] The "peel-off of the non-adhesive protective film during transportation and storage" means that when a gel electrolyte sandwiched between non-adhesive protective films on both sides is transported by a commonly used conveying roller, or stored in a wound state around a roller-shaped core, the protective film peels off from the gel electrolyte due to a buckling phenomenon.
[0024] The gel electrolyte of the present invention has a peeling index value of 5.5 mm. -1 The above provides good peelability of the non-adhesive protective film, enabling transfer to a transferee without deformation or damage. This is because the resultant force of the adhesive force to the transferee and the resistance force generated by the rigidity of the gel electrolyte when the non-adhesive protective film is warped and peeled off exceeds the adhesive force between the non-adhesive protective film and the gel electrolyte.
[0025] The "good peelability of the non-adhesive protective film" means that when the non-adhesive protective film is peeled off from the electrolyte membrane as needed, the electrolyte membrane is prevented from deforming or being damaged by following the non-adhesive protective film on the side to be peeled off.
[0026] In the present invention, the shear storage modulus of the gel electrolyte is preferably 0.02 MPa or more, and more preferably 0.04 MPa or more. When the shear storage modulus of the gel electrolyte is 0.02 MPa or more, it is possible to obtain a gel electrolyte that exhibits an excellent peel index value in the above-mentioned probe tack test. A gel electrolyte membrane having a shear storage modulus of less than 0.02 MPa is relatively easily deformed, and therefore may be deformed due to other factors (e.g., excessive pressure, etc.) even if the above-mentioned peel index value is satisfied. When transferring a gel electrolyte membrane to a target object, this is often done under vacuum conditions to prevent air bubbles from getting in. For example, transfer using a vacuum laminator is one example of this, in which case the gel electrolyte membrane is pressurized to atmospheric pressure (0.101 MPa), but if the gel electrolyte membrane has a shear storage modulus of 0.04 MPa or more, it will not deform even under this pressure. The shear storage modulus of the gel electrolyte can be measured, for example, by a dynamic viscoelasticity measuring device (Rheosol-G5000, manufactured by UBM Corporation).
[0027] The electrolyte composition constituting the gel electrolyte of the present invention contains a binder resin and a supporting electrolyte, and further contains other components as required.
[0028] <Supporting electrolyte> The supporting electrolyte is not particularly limited and can be appropriately selected depending on the purpose. Examples of the supporting electrolyte include solid electrolytes that are solid at room temperature and are composed of a combination of a cation and an anion, and ionic liquids.
[0029] -Solid electrolyte- The cation of the solid electrolyte is not particularly limited and can be appropriately selected depending on the purpose. Examples of the cation include metal ion-based cations such as Li salt, Na salt, K salt, and Mg salt; imidazole derivatives such as N,N-dimethylimidazole salt, N,N-methylethylimidazole salt, N,N-methylpropylimidazole salt, N,N-methylbutylimidazole salt, and N,N-allylbutylimidazole salt; pyridinium derivatives such as N,N-dimethylpyridinium salt and N,N-methylpropylpyridinium salt; pyrrolidinium derivatives such as N,N-dimethylpyrrolidinium salt, N-ethyl-N-methylpyrrolidinium salt, N-methyl-N-propylpyrrolidinium salt, N-butyl-N-methylpyrrolidinium salt, N-methyl-N-pentylpyrrolidinium salt, and N-hexyl-N-methylpyrrolidinium salt; and aliphatic quaternary ammonium-based cations such as trimethylpropylammonium salt, trimethylhexylammonium salt, and triethylhexylammonium salt.
[0030] The anion of the solid electrolyte is not particularly limited and can be appropriately selected depending on the purpose. For example, a chloride anion, a bromide anion, an iodide anion, BF4 - , BF3CF3 - , BF3C2F5 - , PF6 - , NO3 - , CF3CO2 - , CF3SO3 - , (CF3SO2)2N - , (FSO2)2N - , (CF3SO2)(FSO2)N - , (CN)2N - , (CN)3C - , (CN)4B - , (CF3SO2)3C - , (C2F5SO2)2N - , (C2F5)3PF3 - , AlCl4 - , Al2Cl7 - etc. The above cations and anions can be used in any combination, and each of them may be used alone or in combination of two or more kinds.
[0031] The solid electrolyte may be directly dissolved in the binder resin. However, when the solubility of the solid electrolyte in the binder resin is low, a solution in which the solid electrolyte is dissolved in a small amount of a solvent may be mixed with the binder resin.
[0032] The solvent is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include propylene carbonate, acetonitrile, γ-butyrolactone, ethylene carbonate, sulfolane, dioxolane, tetrahydrofuran, 2-methyltetrahydrofuran, dimethyl sulfoxide, 1,2-dimethoxyethane, 1,2-ethoxymethoxyethane, polyethylene glycol, alcohols, etc. These may be used alone or in combination of two or more.
[0033] The supporting electrolyte is preferably a combination of anions and cations whose melting point is below room temperature. That is, it is preferable to use an ionic liquid as the supporting electrolyte. The ionic liquid provides good liquid retention of the binder resin, which makes it easier for tackiness to be expressed, and even when a high concentration of ionic liquid is contained, it is possible to obtain a gel electrolyte that shows an excellent peel index value in the probe tack test.
[0034] -Ionic liquid- Examples of the ionic liquid include ethylmethylimidazolium tetracyanoborate (manufactured by Merck), ethylmethylimidazolium bistrifluoromethanesulfonimide (manufactured by Kanto Chemical Co., Ltd.), ethylmethylimidazolium tripentafluoroethyl trifluorophosphate (manufactured by Merck), ethylmethylimidazolium bis(fluorosulfonyl)imide (manufactured by Kanto Chemical Co., Ltd.), ethylmethylimidazolium diethylphosphate (manufactured by Tokyo Chemical Industry Co., Ltd.), butylmethylimidazolium hexafluorophosphate (manufactured by Tokyo Chemical Industry Co., Ltd.), ethylmethylimidazolium trifluoromethanesulfonate (manufactured by Tokyo Chemical Industry Co., Ltd.), and ethylmethylimidazolium acetate (manufactured by Tokyo Chemical Industry Co., Ltd.). ), ethylmethylimidazolium tricyanomethanide (manufactured by Tokyo Chemical Industry Co., Ltd.), ethylmethylimidazolium dicyanamide (manufactured by Tokyo Chemical Industry Co., Ltd.), methyloctylimidazolium hexafluorophosphate (manufactured by Tokyo Chemical Industry Co., Ltd.), methylpropylpyrrolidinium bisfluorosulfonimide (manufactured by Kanto Chemical Industry Co., Ltd.), butylmethylimidazolium tetrafluoroborate (manufactured by Tokyo Chemical Industry Co., Ltd.), butylmethylimidazolium bis(trifluoromethanesulfonyl)imide (manufactured by Tokyo Chemical Industry Co., Ltd.), hexylmethylimidazolium bis(trifluoromethylsulfonyl)imide (manufactured by Kanto Chemical Industry Co., Ltd.), allylbutylimidazolium tetrafluoroborate (manufactured by Kanto Chemical Industry Co., Ltd.), etc. These may be used alone or in combination of two or more. Among these, ethylmethylimidazolium bisfluorosulfonimide, ethylmethylimidazolium tetracyanoborate, ethylmethylimidazolium bistrifluoromethanesulfonimide, ethylmethylimidazolium tripentafluoroethyl trifluorophosphate, and allylbutylimidazolium tetrafluoroborate are preferred, with ethylmethylimidazolium bisfluorosulfonimide being particularly preferred.
[0035] The content of the ionic liquid is preferably 70% by mass or more, more preferably 80% by mass or more, based on the total amount of the electrolyte composition constituting the gel electrolyte. When the content of the ionic liquid is 70% by mass or more, a gel electrolyte exhibiting higher ionic conductivity can be obtained.
[0036] <Binder resin> The binder resin is not particularly limited and can be appropriately selected according to the purpose, and examples thereof include acrylic resin, polyester resin, urethane resin, polyether resin, polyamide resin, polysaccharide resin such as cellulose derivative, polyacrylamide resin, polyvinyl ester resin, and resin obtained by polymerizing photopolymerizable monomer and photopolymerizable oligomer. These may be used alone or in combination of two or more. Among these, resin obtained by polymerizing photopolymerizable monomer and photopolymerizable oligomer is particularly preferred from the viewpoint of ease of production. As the photopolymerizable monomer, a monofunctional photopolymerizable monomer, a difunctional photopolymerizable monomer, or a polyfunctional photopolymerizable monomer having three or more functional groups can be used.
[0037] Examples of monofunctional photopolymerizable monomers include 2-(2-ethoxyethoxy)ethyl acrylate, methoxypolyethylene glycol monoacrylate, methoxypolyethylene glycol monomethacrylate, methyl methacrylate, phenoxypolyethylene glycol acrylate, 2-acryloyloxyethyl succinate, acryloylmorpholine, 2-ethylhexyl acrylate, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, tetrahydrofurfuryl acrylate, 2-ethylhexyl carbitol acrylate, 3-methoxybutyl acrylate, benzyl acrylate, cyclohexyl acrylate, isoamyl acrylate, isobutyl acrylate, methoxytriethylene glycol acrylate, phenoxytetraethylene glycol acrylate, cetyl acrylate, isostearyl acrylate, stearyl acrylate, or styrene monomer. These may be used alone or in combination of two or more.
[0038] Examples of bifunctional photopolymerizable monomers include 1,3-butanediol diacrylate, 1,4-butanediol diacrylate, 1,4-butanediol dimethacrylate, 1,6-hexanediol diacrylate, 1,6-hexanediol dimethacrylate, diethylene glycol diacrylate, polyethylene glycol diacrylate, neopentyl glycol diacrylate, EO-modified bisphenol A diacrylate, EO-modified bisphenol F diacrylate, and neopentyl glycol diacrylate. These may be used alone or in combination of two or more. In the above, "EO-modified" refers to ethyleneoxy-modified, and "PO-modified" refers to propyleneoxy-modified.
[0039] Examples of photopolymerizable monomers with three or more functionalities include trimethylolpropane triacrylate (TMPTA), trimethylolpropane trimethacrylate, EO-modified trimethylolpropane triacrylate, PO-modified trimethylolpropane triacrylate, caprolactone-modified trimethylolpropane triacrylate, HPA-modified trimethylolpropane trimethacrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate (PETTA), glycerol triacrylate, ECH-modified glycerol triacrylate, EO-modified glycerol triacrylate, PO-modified glycerol triacrylate, tris Examples of the acrylate include (acryloxyethyl) isocyanurate, dipentaerythritol hexaacrylate (DPHA), caprolactone-modified dipentaerythritol hexaacrylate, dipentaerythritol hydroxypentaacrylate, alkyl-modified dipentaerythritol pentaacrylate, alkyl-modified dipentaerythritol tetraacrylate, alkyl-modified dipentaerythritol triacrylate, dimethylolpropane tetraacrylate (DTMPTA), pentaerythritol ethoxy tetraacrylate, EO-modified phosphoric acid triacrylate, and 2,2,5,5-tetrahydroxymethylcyclopentanone tetraacrylate. These may be used alone or in combination of two or more.
[0040] Examples of photopolymerizable oligomers include urethane acrylate, epoxy acrylate, acrylic acrylate, polyester acrylate, polyethylene glycol acrylate, methyl methacrylate, ethyl methacrylate, butyl methacrylate, and various reactive polymers. As the photopolymerizable oligomer, commercially available products can be used. Examples of the commercially available products include Blenmar(R) DA-800AU (manufactured by NOF Corporation), Blenmar(R) TA-604AU (manufactured by NOF Corporation), CN9030 (manufactured by Tomoe Engineering Co., Ltd.), CN9010 NS (manufactured by Tomoe Engineering Co., Ltd.), CN9029 (manufactured by Tomoe Engineering Co., Ltd.), CN8885 NS (manufactured by Tomoe Engineering Co., Ltd.), CN9013 NS (manufactured by Tomoe Engineering Co., Ltd.), CN970 (manufactured by Tomoe Engineering Co., Ltd.), CN971 (manufactured by Tomoe Engineering Co., Ltd.), CN972 (manufactured by Tomoe Engineering Co., Ltd.), and CN975. NS (Tomoe Engineering Co., Ltd.), UX-3204 (Nippon Kayaku Co., Ltd.), UX-4101 (Nippon Kayaku Co., Ltd.), UXT-6100 (Nippon Kayaku Co., Ltd.), UX6101 (Nippon Kayaku Co., Ltd.), UX8101 (Nippon Kayaku Co., Ltd.), UX0937 (Nippon Kayaku Co., Ltd.), UXF-4001-M35 (Nippon Kayaku Co., Ltd.), UXF-4002 (Nippon Kayaku Co., Ltd.), UX-5000 (Nippon Kayaku Co., Ltd.) (manufactured by Shin-Nakamura Chemical Co., Ltd.), UA-4200 (manufactured by Shin-Nakamura Chemical Co., Ltd.), UA-160TM (manufactured by Shin-Nakamura Chemical Co., Ltd.), UA-290TM (manufactured by Shin-Nakamura Chemical Co., Ltd.), UA-7100 (manufactured by Shin-Nakamura Chemical Co., Ltd.), UA-W2A (manufactured by Shin-Nakamura Chemical Co., Ltd.), UV-3000B (manufactured by Mitsubishi Chemical Co., Ltd.), UV-3200B (manufactured by Mitsubishi Chemical Co., Ltd.), UV-3300B (manufactured by Mitsubishi Chemical Co., Ltd.) urethane acrylates such as UV3640B (manufactured by Mitsubishi Chemical Corporation), UV-3640PE80 (manufactured by Mitsubishi Chemical Corporation), UA-306H (manufactured by Kyoeisha Chemical Co., Ltd.), UA-306T (manufactured by Kyoeisha Chemical Co., Ltd.), and UA-306I (manufactured by Kyoeisha Chemical Co., Ltd.); BAEA-100 (manufactured by KSM Co., Ltd.), BAEM-100 (manufactured by KSM Co., Ltd.), R-115F (manufactured by Nippon Kayaku Co., Ltd.), R Epoxy acrylates such as EA-130 (manufactured by Nippon Kayaku Co., Ltd.), R-381 (manufactured by Nippon Kayaku Co., Ltd.), EAM-2160 (manufactured by Nippon Kayaku Co., Ltd.), ZFA-266H (manufactured by Nippon Kayaku Co., Ltd.), EA-1010N (manufactured by Shin-Nakamura Chemical Co., Ltd.), EA-1010LC (manufactured by Shin-Nakamura Chemical Co., Ltd.), EA-1010NT2 (manufactured by Shin-Nakamura Chemical Co., Ltd.), and EA-1020LC3 (manufactured by Shin-Nakamura Chemical Co., Ltd.);Acrylic acrylates such as EBECRYL 303 (manufactured by Daicel-Ornecle Co., Ltd.), EBECRYL 1710 (manufactured by Daicel-Ornecle Co., Ltd.), and EBECRYL 767 (manufactured by Daicel-Ornecle Co., Ltd.); CN2203 (manufactured by Tomoe Engineering Co., Ltd.), CN2270 (manufactured by Tomoe Engineering Co., Ltd.), CN22073 (manufactured by Tomoe Engineering Co., Ltd.), CN2274 (manufactured by Tomoe Engineering Co., Ltd.), EBECRYL Polyester acrylates such as 820 (manufactured by Daicel-Ornecle Co., Ltd.); polyethylene glycol acrylates such as AM-90G (manufactured by Shin-Nakamura Chemical Co., Ltd.), AM-130G (manufactured by Shin-Nakamura Chemical Co., Ltd.), and AM-450G (manufactured by Shin-Nakamura Chemical Co., Ltd.); methyl methacrylates such as AM45%AA-6 (manufactured by Toagosei Co., Ltd.), AA-6SR (manufactured by Toagosei Co., Ltd.), and AA-6 (manufactured by Toagosei Co., Ltd.); butyl methacrylates such as AN-6S (manufactured by Toagosei Co., Ltd.), AB-6 (manufactured by Toagosei Co., Ltd.), and AW-6S (manufactured by Toagosei Co., Ltd.); reactive polymers such as RP-274S (manufactured by KSM Co., Ltd.), and RP-310 (manufactured by KSM Co., Ltd.). These may be used alone or in combination of two or more types.
[0041] The binder resin is preferably a polymer having a polymethyl methacrylate (PMMA) chain, which is likely to exhibit tackiness even when it contains a large amount of ionic liquid, making it possible to obtain a gel electrolyte that exhibits an excellent peel index value in the above-mentioned probe tack test. Examples of polymers having a PMMA chain include MB-1 (manufactured by Toagosei Co., Ltd.), MB-1P (manufactured by Toagosei Co., Ltd.), and Hyperl M4501 (manufactured by Negami Chemical Industry Co., Ltd.).
[0042] The binder resin is preferably a crosslinked polymer having a polymethyl methacrylate (PMMA) chain. The crosslinked polymer having a PMMA chain can use a low molecular weight PMMA-based monomer having better compatibility than linear PMMA at the stage of the electrolyte composition, so that the content can be increased and tackiness can be more easily exhibited. Examples of crosslinked polymers having PMMA include those obtained by crosslinking reactive oligomers or reactive polymers having PMMA chains. The reactive oligomer having a PMMA chain is not particularly limited and can be appropriately selected depending on the purpose. For example, macromonomer AA-6 (manufactured by Toagosei Co., Ltd.) can be mentioned.
[0043] <Other ingredients> The other components are not particularly limited and can be appropriately selected depending on the purpose. Examples of the other components include a polymerization initiator.
[0044] The polymerization initiator is not particularly limited and can be appropriately selected depending on the purpose. Examples of the polymerization initiator include radical polymerization initiators. Examples of the radical polymerization initiator include a thermal polymerization initiator and a photopolymerization initiator.
[0045] Examples of the thermal polymerization initiator include azo compounds such as 2,2'-azobisisobutyronitrile, dimethyl-2,2'-azobisisobutyrate, 2,2'-azobis(2,4-dimethylvaleronitrile), and 2,2'-azobis[2-(2-imidazolin-2-yl)propane]; and organic peroxides such as 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane and di(4-tert-butylcyclohexyl)peroxydicarbonate. These may be used alone or in combination of two or more.
[0046] Examples of the photopolymerization initiator include ketal-based photopolymerization initiators such as 2,2-dimethoxy-1,2-diphenylethan-1-one, acetophenone-based photopolymerization initiators such as 1-hydroxycyclohexyl phenyl ketone, 2,2-diethoxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 4-phenoxydichloroacetophenone, and 4-(t-butyl)dichloroacetophenone, and benzoin ether-based photopolymerization initiators such as benzoin methyl ether, benzoin ethyl ether, benzoin propyl ether, benzoin isopropyl ether, and benzoin isobutyl ether. These may be used alone or in combination of two or more.
[0047] The content of the polymerization initiator is not particularly limited and can be appropriately selected depending on the purpose, but is preferably from 0.001 to 5 parts by mass, more preferably from 0.01 to 2 parts by mass, and particularly preferably from 0.01 to 1 part by mass, relative to 100 parts by mass of the total monomer components.
[0048] <Method of manufacturing gel electrolyte membrane> The gel electrolyte membrane of the present invention can be produced by first mixing the electrolyte composition, the binder resin, and, if necessary, a polymerization initiator to prepare an electrolyte composition, and then sandwiching the prepared electrolyte composition between two types of films having different peel strengths and polymerizing them. The polymerization reaction is preferably a radical polymerization reaction, and more preferably a thermal radical polymerization reaction or a photoradical polymerization reaction.
[0049] Among the above films, those having a small peel strength are not particularly limited and can be appropriately selected depending on the purpose. Examples thereof include polyethylene films with release layers, polypropylene films, polyethylene terephthalate films, polyethylene naphthalate films, polybutylene terephthalate films, liquid crystal polyester films, polyether ketone films, polyimide films, polyamideimide films, polyamide films, aramid films, and polytetrafluoroethylene films. The lower limit of the peel strength of the film is not particularly limited, but it is preferable that the peel strength is 0.15 N / 50 mm or more in a 90° peel test according to JIS Z0237: 2009. The other film having a higher peel strength is not particularly limited and can be appropriately selected depending on the purpose, but it is preferable that the peel strength is 1.5 times or more higher than that of the film on the lighter peel side.
[0050] The average thickness of the gel electrolyte of the present invention is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 10 μm or more and 100 μm or less. When the average thickness of the gel electrolyte is 10 μm or more and 100 μm or less, the buckling resistance during transportation and storage and the good peelability during processing become more remarkable.
[0051] <Applications of gel electrolytes> The gel electrolyte of the present invention has self-adhesiveness that prevents it from peeling off from the non-adhesive protective film during transportation and storage, and allows it to be easily peeled off from the non-adhesive protective film when in use, in order to prevent the occurrence of optical distortion due to deformation of the gel electrolyte. Therefore, the gel electrolyte of the present invention can be suitably used in various electrochemical devices such as electrochromic elements, lithium ion secondary batteries, solar cells, fuel cells, and ion conductive actuators, but is particularly suitable for use in the electrolyte layer of the electrochromic elements described below.
[0052] (Electrochromic element) The electrochromic element of the present invention has a first electrode, a second electrode, and, between the first electrode and the second electrode, an electrochromic layer containing an electrochromic compound and an electrolyte layer, and may further have other components as necessary.
[0053] <Electrolyte layer> The electrolyte layer uses the gel electrolyte of the present invention. The average thickness of the electrolyte layer made of the gel electrolyte is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 1 μm or more and 1,000 μm or less.
[0054] <Electrochromic layer> The electrochromic layer is a functional layer that contains an electrochromic compound and exhibits electrochromism. The electrochromic layer may be formed by combining an electrochromic compound with a conductive or semiconductive nanostructure, or may be formed by polymerizing the electrochromic compound, which is a radical polymerizable compound, into a layer.
[0055] -Electrochromic Compounds- The electrochromic compound is a material that changes color by an oxidation reaction or a reduction reaction, and examples thereof include radical polymerizable compounds and polymer-based compounds. The electrochromic compound is not particularly limited, and any known electrochromic compound can be appropriately selected depending on the purpose. Examples of the electrochromic compound include dye-based compounds, metal complex-based compounds, and metal oxide-based compounds. Examples of the dye-based compound include low molecular weight organic electrochromic compounds such as azobenzene-based, anthraquinone-based, diarylethene-based, dihydroprene-based, styryl-based, styrylspiropyran-based, spirooxazine-based, spirothiopyran-based, thioindigo-based, tetrathiafulvalene-based, terephthalic acid-based, triphenylmethane-based, triphenylamine-based, naphthopyran-based, viologen-based, pyrazoline-based, phenazine-based, phenylenediamine-based, phenoxazine-based, phenothiazine-based, phthalocyanine-based, fluoran-based, fulgide-based, benzopyran-based, and metallocene-based compounds; and conductive polymer compounds such as polyaniline and polythiophene. Examples of the metal complex compounds and metal oxide compounds include inorganic electrochromic compounds such as titanium oxide, vanadium oxide, tungsten oxide, indium oxide, iridium oxide, nickel oxide, and Prussian blue.
[0056] -Conductive and semiconducting nanostructures- The conductive or semiconductive nanostructure means a nanostructure having nanoscale irregularities, such as nanoparticles or a nanoporous structure. When the electrochromic compound has a phosphonic acid group, a phosphoric acid group, or a carboxyl group as a bond or adsorption structure, the electrochromic compound is easily combined with the nanostructure to form an electrochromic composition having excellent color image retention properties, and an electrochromic layer can be formed from the electrochromic composition.
[0057] The material constituting the conductive or semiconductive nanostructure is not particularly limited and can be appropriately selected depending on the purpose, but metal oxides are preferred from the viewpoints of transparency and conductivity. Examples of the metal oxide include those mainly composed of titanium oxide, zinc oxide, tin oxide, zirconium oxide, cerium oxide, yttrium oxide, boron oxide, magnesium oxide, strontium titanate, potassium titanate, barium titanate, calcium titanate, calcium oxide, ferrite, hafnium oxide, tungsten oxide, iron oxide, copper oxide, nickel oxide, cobalt oxide, barium oxide, strontium oxide, vanadium oxide, indium oxide, aluminosilicate, calcium phosphate, aluminosilicate, etc. These may be used alone or in combination of two or more. Among these, titanium oxide, zinc oxide, tin oxide, zirconium oxide, iron oxide, magnesium oxide, indium oxide, and tungsten oxide are preferred in terms of electrical properties such as electrical conductivity, physical properties such as optical properties, and response speed of color development and fading.
[0058] <First electrode and second electrode> The first electrode and the second electrode are not particularly limited as long as at least one of the first electrode and the second electrode is transparent, and a known conductor can be appropriately selected depending on the purpose.
[0059] The transparent electrode is not particularly limited as long as it is a transparent material having electrical conductivity and can be appropriately selected depending on the purpose. Examples of the transparent electrode include tin-doped indium oxide (hereinafter also referred to as "ITO"), fluorine-doped tin oxide (hereinafter also referred to as "FTO"), antimony-doped tin oxide (hereinafter also referred to as "ATO"), and inorganic materials such as ITO, InSnO, GaZnO, SnO, In2O3, and zinc oxide (ZnO).
[0060] In addition, an electrode may be used that has improved conductivity while maintaining transparency by forming transparent carbon nanotubes or other highly conductive non-transparent materials such as Au, Ag, Pt, and Cu into a fine network shape.
[0061] <Other materials> The other members are not particularly limited and can be appropriately selected depending on the purpose. Examples of the other members include a support, a sealing material, an insulating porous layer, a deterioration prevention layer, and a protective layer.
[0062] -Support- As the support, any known organic or inorganic material can be used as it is, so long as it is a transparent material capable of supporting each layer.
[0063] Examples of the support include glass substrates such as alkali-free glass, borosilicate glass, float glass, and soda-lime glass; and resin substrates such as polycarbonate resin, acrylic resin, polyethylene, polyvinyl chloride, polyester, epoxy resin, melamine resin, phenol resin, polyurethane resin, and polyimide resin.
[0064] The surface of the support may be coated with a transparent insulating layer, a UV-cut layer, an anti-reflection layer, or the like in order to improve water vapor barrier properties, gas barrier properties, ultraviolet resistance, and visibility.
[0065] The shape of the support is not particularly limited and may be appropriately selected depending on the purpose, and examples of the shape include rectangular and round.
[0066] The support may be a laminate of a plurality of substrates. For example, by using a structure in which an electrochromic element is sandwiched between two glass substrates, the water vapor barrier property and gas barrier property can be improved.
[0067] -Sealing material- The sealing material seals the side surfaces of the bonded electrochromic elements and has a function of preventing the intrusion of unnecessary substances such as moisture and oxygen in the air, which are necessary for the electrochromic elements to operate stably. The sealing material is not particularly limited and can be appropriately selected depending on the purpose. Examples of the sealing material include ultraviolet-curable and thermosetting resins, and specific examples thereof include acrylic resins, urethane resins, and epoxy resins.
[0068] -Insulating porous layer- The insulating porous layer serves to separate the first electrode and the second electrode so as to be electrically insulated from each other, and also serves to retain an electrolyte. The material for the insulating porous layer is not particularly limited as long as it is porous, and it is preferable to use an organic material, an inorganic material, or a composite material thereof that has high insulating properties, durability, and excellent film-forming properties.
[0069] Examples of methods for forming the insulating porous layer include a sintering method (using holes generated between particles by partially fusing polymer fine particles or inorganic particles with the addition of a binder or the like), an extraction method (forming a constituent layer with organic or inorganic substances soluble in a solvent and a binder or the like that is insoluble in the solvent, and then dissolving the organic or inorganic substances with a solvent to obtain pores), a foaming method, a phase inversion method in which a mixture of polymer compounds or the like is phase-separated by manipulating a good solvent and a poor solvent, and a radiation irradiation method in which various types of radiation are radiated to form pores.
[0070] -Protective layer- The protective layer has functions such as protecting the electrochromic element from external stress and chemicals used in the cleaning process, preventing leakage of the gel electrolyte, and preventing the intrusion of substances unnecessary for stable operation of the electrochromic element, such as moisture and oxygen in the air.
[0071] The material for the protective layer is not particularly limited, but examples thereof include ultraviolet-curable and thermosetting resins, and specific examples thereof include acrylic resins, urethane resins, and epoxy resins.
[0072] FIG. 3 is a schematic diagram showing an example of the electrochromic device of the present invention having the gel electrolyte of the present invention. As shown in FIG. 3, the electrochemical cell has a first electrode 3, a second electrode 2, and a gel electrolyte 6 between the first electrode 3 and the second electrode 2. The first electrode 3 and the second electrode 2 are sandwiched by a support 1. The first electrode 3 may have an electrochromic layer 5 on its surface, and the second electrode 2 may have an electrochromic layer 7 on its surface. It is preferable that the electrochromic layers 5 and 7 contain an electrochromic compound 4.
[0073] <Applications of electrochromic elements> The electrochromic element of the present invention has high transparency and excellent color development response, and can therefore be suitably used for, for example, electrochromic displays, large display panels such as stock price display panels, anti-glare mirrors, light control elements such as light control glass, low-voltage drive elements such as touch panel key switches, optical switches, optical memories, electronic paper, electronic albums, etc. EXAMPLES
[0074] Examples of the present invention will be described below, but the present invention is not limited to these examples.
[0075] Example 1 <Preparation of electrolyte membrane> A monomer solution was obtained by dissolving irgacure184 (manufactured by BASF) as a polymerization initiator in urethane acrylate (product name: UXF4002, manufactured by Nippon Kayaku Co., Ltd.) as a binder resin such that the mass ratio (binder resin / polymerization initiator) was 99.5 / 0.5. Next, a 1 mol / L solution of tributylammonium perchlorate (TBAP, manufactured by Tokyo Chemical Industry Co., Ltd.) in propylene carbonate (PC, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was mixed and dissolved as a supporting electrolyte in the obtained monomer solution at a mass ratio of 20% to prepare an electrolyte composition. Next, 500 μL of the obtained electrolyte composition was dropped onto a non-adhesive protective film 1 with a release layer (product name: SPPET-50-O1BU, manufactured by Mitsui Tohcello Co., Ltd.) on the light release side, and then covered with a non-adhesive protective film 2 with a release layer (product name: SPPET-50-O3BU, manufactured by Mitsui Tohcello Co., Ltd.) on the heavy release side to spread the electrolyte composition, and then irradiated with a UV (wavelength 250 nm) device (manufactured by Eye Graphics Co., Ltd.) at 2 J / cm. 2 Irradiation was performed to obtain a laminate of non-adhesive protective film 1 / gel electrolyte / non-adhesive protective film 2.
[0076] Next, the peel index value and the shear storage modulus were determined as follows, and the buckling resistance and peelability were evaluated. The results are shown in Table 1-2.
[0077] <Measurement of shear storage modulus> A gel electrolyte with an average thickness of 700 μm processed into a cylindrical shape with a diameter of 5 mm was sandwiched between parallel plates made of SUS304 with a diameter of 5 mm, and the shear storage modulus was measured using a dynamic viscoelasticity measuring device (Rheosol-G5000, manufactured by UBM Corporation) in an environment of 25°C under the conditions of an amount of strain within a range in which the gel electrolyte does not undergo plastic deformation and a frequency of 1 Hz.
[0078] <Measurement of peeling index value> A probe made of SUS304 and having a diameter of 5 mm was brought into contact with a gel electrolyte having an average thickness of 700 μm from above at a speed of 120 mm / sec, and the probe was peeled off vertically at a speed of 400 mm / sec using a tack testing machine (manufactured by Rhesca Corporation, TAC-II) under the conditions of a pressure load of 40 gf and a pressure load holding time of 5 seconds in an environment of 25° C. As shown in FIG. 1, the peel index value was calculated by dividing the maximum stress 8 under the above measurement conditions by the integral value 9 obtained by integrating the stress over the peel distance.
[0079] <Evaluation of buckling resistance> The buckling resistance was evaluated using a laminate of non-adhesive protective film 1 / gel electrolyte / non-adhesive protective film 2, in which the gel electrolyte had a thickness of 50 μm. Specifically, the laminate was wrapped around the side surface of a cylindrical rod having an outer diameter of 20 mm by 1 / 4 of the circumference so that the non-adhesive protective film 1 was on the outer periphery, and the non-adhesive protective film 1 was observed to see whether it peeled off from the gel electrolyte, and was evaluated according to the following criteria. [Judgment criteria] ◯: Buckling resistance is present, and peeling of the non-adhesive protective film 1 from the gel electrolyte is not visible. ×: No buckling resistance, and the non-adhesive protective film 1 was visibly peeled off from the gel electrolyte. The above criteria are based on the knowledge that if no peeling occurs using the above evaluation method, the non-adhesive protective film will not peel off during transportation using a 100 mm outer diameter transport roller that is generally used in roll-to-roll processes, or during storage wrapped around a 100 mm outer diameter core.
[0080] <Evaluation of peelability> The peelability was evaluated using the laminate of the non-adhesive protective film 1 / gel electrolyte / non-adhesive protective film 2, in which the thickness of the gel electrolyte was 50 μm. Specifically, the laminate was placed on a flat stage with the non-adhesive protective film 1 facing up, and when the non-adhesive protective film 1 was peeled off using an adhesive roller with an outer diameter of 30 mm, it was evaluated according to the following criteria as to whether the gel electrolyte was deformed or damaged. [Judgment criteria] ◯: The peelability is good, and the gel electrolyte is not visible to follow the non-adhesive protective film to be peeled off, and no deformation or damage is visible. ×: The peelability is poor, and the gel electrolyte is visibly attached to the non-adhesive protective film to be peeled off, or deformation or damage is visibly observed.
[0081] (Examples 2 to 27 and Comparative Examples 1 to 26) The gel electrolytes of Examples 2 to 27 and Comparative Examples 1 to 26 were prepared in the same manner as in Example 1, except that the binder resin and supporting electrolyte used in the gel electrolyte membrane in Example 1 were prepared based on the compositions and mass ratios shown in Tables 1-1 and 1-2. Next, for the obtained gel electrolytes of Examples 2 to 27 and Comparative Examples 1 to 26, the peel index value, shear storage modulus, buckling resistance, and peelability were evaluated in the same manner as in Example 1. The results are shown in Table 1-2.
[0082] [Table 1-1]
[0083] [Table 1-2]
[0084] Details of the abbreviations in Tables 1-1 and 1-2 are as follows: -Polymethylmethacrylate (PMMA) acrylate (polymer with PMMA chains)- ·AA-6 (manufactured by Toagosei Co., Ltd.)
[0085] -Other binder resins- ·UXF4002 (manufactured by Nippon Kayaku Co., Ltd.) UV3640PE80 (Mitsubishi Chemical Corporation) UV3000B (Mitsubishi Chemical Corporation) AM-90G (manufactured by Shin-Nakamura Chemical Co., Ltd.) A-BPE-30 (manufactured by Shin-Nakamura Chemical Co., Ltd.) ACMO (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.)
[0086] --Non-polymerizable polymer-- ·M4501 (manufactured by Negami Chemical Industries Co., Ltd.) ·M5000 (manufactured by Negami Chemical Industries Co., Ltd.) ·M5001 (manufactured by Negami Chemical Industries Co., Ltd.)
[0087] -Supporting electrolyte- · TBAP (Tributylammonium perchlorate, manufactured by Tokyo Chemical Industry Co., Ltd.) PC (propylene carbonate, Fujifilm Wako Pure Chemical Industries, Ltd.) EMIMFSI (Ethylmethylimidazolium bisfluorosulfonimide, manufactured by Kanto Chemical Co., Ltd.) ·EMIMTCB (Ethyl methylimidazolium tetracyanoborate, Merck) EMIMTFSI (Ethylmethylimidazolium bistrifluoromethanesulfonimide, manufactured by Kanto Chemical Co., Ltd.) EMIMFAP (Ethyl methyl imidazolium tripentafluoroethyl trifluorophosphate, Merck) ABIMBF4 (allylbutylimidazolium tetrafluoroborate, manufactured by Kanto Chemical Co., Ltd.) P13FSI (methylpropylpyrrolidinium bisfluorosulfonimide, manufactured by Kanto Chemical Co., Ltd.)
[0088] From the results of Tables 1-1 and 1-2, the gel electrolytes of Examples 1 to 27 had a peel index value of 5.5 mm in the above-mentioned probe tack test. -1 More than 7.5mm -1 The results are within the following ranges, and all of them were found to exhibit good buckling resistance and peeling resistance. From the results of Examples 2 to 27, by using an ionic liquid as a supporting electrolyte, the peel index value in the above-mentioned probe tack test was 5.5 mm even when the content of the supporting electrolyte was high. -1 More than 7.5mm -1 below 1 It was found that a gel electrolyte having good buckling resistance and peelability could be obtained. From the results of Examples 4 to 18 and 20 to 22, when the binder resin is a polymer having a polymethyl methacrylate (PMMA) chain, even if the content of the ionic liquid is 70 mass % or more, the peel index value in the above-mentioned probe tack test is 5.5 mm or less. -1 More than 7.5mm -1 It was found that a gel electrolyte having good buckling resistance and peelability could be obtained, falling within the following ranges. From the results of Examples 8 to 18 and 20 to 22, when the binder resin contains a crosslinked product obtained by crosslinking a polymer having a polymethyl methacrylate (PMMA) chain, the compatibility with the ionic liquid is excellent, so the PMMA content relative to the binder resin can be increased, and even if the content of the ionic liquid is 80 mass % or more, the peel index value in the above-mentioned probe tack test is 5.5 mm. -1 More than 7.5mm -1 It has been found that gel electrolytes falling within the following ranges are more readily obtainable:
[0089] (Example 28) The same electrolyte composition as in Example 2 was injected between the opposing platinum electrodes and irradiated with 2 J / cm 2 UV (wavelength 250 nm) by a UV irradiation device (manufactured by Eye Graphics Co., Ltd.). 2 The impedance of the gel electrolyte obtained by irradiation was measured as follows.
[0090] <Evaluation of ionic conductivity> The impedance of the device was measured by the AC impedance method. The measurement was performed using a modular electrochemical measurement system (device name: Modulab, manufactured by Toyo Technica Corporation) under the following conditions: applied AC voltage: 10 mV, measurement frequency range: 1 Hz to 1,000,000 Hz, and measurement temperature: 25°C. As a result of the measurement, an impedance waveform with the shape shown in Figure 4 was obtained. The length of the chord of the circular arc at this time was measured as the ionic conductivity of the gel electrolyte. The results are shown in Table 2.
[0091] (Examples 29 to 37 and Comparative Examples 27 to 28) The gel electrolytes of Examples 29 to 37 and Comparative Examples 27 to 28 were prepared in the same manner as in Example 28, except that the binder resin and supporting electrolyte in the electrolyte composition were prepared based on the compositions shown in Table 2. Next, the impedance of the obtained gel electrolytes of Examples 29 to 37 and Comparative Examples 27 to 28 was measured in the same manner as in Example 28. The results are shown in Table 2.
[0092] [Table 2] The results in Table 2 show that in Examples 32 to 33 and 36 to 37, when the ionic liquid content was 70% by mass or more, the gel electrolyte exhibited a high ionic conductivity of 1 mS / cm or more, and in particular, when the ionic liquid content was 80% by mass or more, the gel electrolyte exhibited an extremely high ionic conductivity of 5 mS / cm or more.
[0093] (Example 38) <Example of electrochromic element production> - Formation of an electrochromic layer on the surface of the first electrode - A solution of polyethylene glycol diacrylate (product name: PEG-400DA, manufactured by Nippon Kayaku Co., Ltd.), irgacure184 (manufactured by BASF), a compound represented by the following structural formula (1), and 2-butanone mixed in a mass ratio of (57 / 3 / 140 / 800) was applied by spin coating onto an ITO glass substrate (40 mm × 40 mm, average thickness: 0.7 mm, ITO film thickness: approximately 100 nm) serving as a first electrode, and cured with UV light in a nitrogen atmosphere to form an electrochromic layer containing the compound represented by the structural formula and having an average thickness of 1.1 μm on the first electrode.
[0094] [Compound represented by structural formula (1)] [ka]
[0095] <Formation of electrochromic layer on second electrode> A titanium oxide nanoparticle dispersion (product name: SP210, manufactured by Showa Titanium Co., Ltd., average particle size: about 20 nm) was applied by spin coating onto an ITO glass substrate (40 mm x 40 mm, average thickness: 0.7 mm, ITO film thickness: about 100 nm) as a second electrode, and an annealing treatment was performed at 120°C for 15 minutes to form a titanium oxide particle film. A 2 mass% 2,2,3,3-tetrafluoropropanol solution of a compound represented by the following structural formula (2) was applied as a coating liquid by spin coating onto this titanium oxide particle film, and an annealing treatment was performed at 120°C for 10 minutes to form an electrochromic layer with an average thickness of 1.0 μm on the second electrode, in which the compound represented by structural formula (2) was adsorbed onto the titanium oxide particle surface.
[0096] [Structural formula (2)] [ka]
[0097] <Cell Preparation> The same gel electrolyte as in Example 2 was attached to the second electrode on which the electrochromic layer was formed, and the first electrode on which the electrochromic layer was formed was further attached to it. The ends were sealed with a UV adhesive (Photolec E, low moisture permeability type, manufactured by Sekisui Chemical Co., Ltd.) to prepare a cell.
[0098] <Haze value> As a simple evaluation of optical distortion, the haze value of the cell was measured using a haze meter (NDH-5000, manufactured by Nippon Denshoku Industries Co., Ltd.) The results are shown in Table 3-2.
[0099] (Examples 39 to 48 and Comparative Examples 29 to 31) The gel electrolytes of Examples 39 to 48 and Comparative Examples 29 to 31 were prepared in the same manner as in Example 38, except that the binder resin and supporting electrolyte in the electrolyte composition were prepared based on the compositions shown in Tables 3-1 and 3-2. Next, for the obtained gel electrolytes of Examples 39 to 48 and Comparative Examples 29 to 31, the haze value was measured in the same manner as in Example 38. The results are shown in Table 3-2.
[0100] [Table 3-1]
[0101] [Table 3-2]
[0102] From the results in Tables 3-1 and 3-2, it was found that Examples 38 to 48, which showed good buckling resistance and good peelability, had no optical distortion in the gel electrolyte, and therefore no voids were generated at the interface between the gel electrolyte and the electrochromic layer during the preparation of the electrochromic element, and thus showed excellent haze values.
[0103] For example, aspects of the present invention are as follows. <1> A gel electrolyte comprising a cured product of an electrolyte composition containing a binder resin and a supporting electrolyte, Under environmental conditions of 25°C, a stainless steel probe having a diameter of 5 mm was brought into contact with a gel electrolyte having an average thickness of 700 μm from above at a speed of 120 mm / sec, and the pressure load was set to 40 gf. The pressure load was held for 5 seconds. The probe was then peeled off in the vertical direction at a speed of 400 mm / sec to measure stress, peel distance, and maximum stress. The peel index value, which was calculated by dividing the maximum stress by the integral obtained by integrating the stress over the peel distance, was 5.5 mm. -1 More than 7.5mm -1 The gel electrolyte is characterized in that: <2> The supporting electrolyte comprises an ionic liquid. <1> The gel electrolyte is as described in the above. <3> The ionic liquid is ethylmethylimidazolium bisfluorosulfonimide. <2> The gel electrolyte is as described in the above. <4> The binder resin includes a polymer having a polymethyl methacrylate chain. <1> from <3> The gel electrolyte according to any one of claims 1 to 5, <5> The binder resin includes a crosslinked product obtained by crosslinking a polymer having a polymethyl methacrylate chain. <4> The gel electrolyte is as described in the above. <6> The content of the ionic liquid is 70% by mass or more. <2> from <5> The gel electrolyte according to any one of claims 1 to 5, <7> The content of the ionic liquid is 80% by mass or more. <6> The gel electrolyte is as described in the above. <8> The shear storage modulus is 0.02 MPa or more. <1> from <7> The gel electrolyte according to any one of claims 1 to 5, <9> The above-mentioned electrochromic device <1> from <8> The gel electrolyte according to any one of claims 1 to 5, <10> An electrochromic element having a first electrode, a second electrode, and an electrochromic layer containing an electrochromic compound and an electrolyte layer between the first electrode and the second electrode, The electrolyte layer is <1> from <9> 1. An electrochromic device comprising the gel electrolyte according to claim 1.
[0104] The above <1> from <9> The gel electrolyte according to any one of the preceding claims, <10> According to the electrochromic element described in the above, the conventional problems can be solved and the object of the present invention can be achieved. [Explanation of symbols]
[0105] 1 Support 2 Second electrode 3 First electrode 4. Electrochromic Compounds 5 Electrochromic Layer 6. Gel Electrolytes 7 Electrochromic Layer [Prior art documents] [Patent documents]
[0106] [Patent Document 1] JP 2011-253753 A
Claims
1. A laminate comprising: a gel electrolyte membrane including a cured product of an electrolyte composition containing a binder resin and a supporting electrolyte; and non-adhesive protective film layers disposed on both sides of the gel electrolyte membrane, The gel electrolyte membrane was subjected to a probe tack test in which a stainless steel probe having a diameter of 5 mm was brought into contact with the gel electrolyte membrane having an average thickness of 700 μm from above at a speed of 120 mm / sec under an environmental condition of 25° C., and the probe was peeled off in the vertical direction at a speed of 400 mm / sec under the conditions of a pressing load of 40 gf and a pressing load holding time of 5 seconds, and the stress, peel distance and maximum stress were measured. The peel index value obtained by dividing the maximum stress by an integral value obtained by integrating the stress over the peel distance was 5.5 mm. -1 More than 7.5 mm -1 A laminate characterized in that:
2. The laminate of claim 1 , wherein the supporting electrolyte comprises an ionic liquid.
3. The laminate according to claim 2 , wherein the ionic liquid is ethylmethylimidazolium bisfluorosulfonimide.
4. The laminate according to claim 1 , wherein the binder resin comprises a polymer having a polymethyl methacrylate chain.
5. The laminate according to claim 4 , wherein the binder resin comprises a crosslinked product obtained by crosslinking a polymer having a polymethyl methacrylate chain.
6. A laminate as described in claim 2 or 3, wherein the content of the ionic liquid in the gel electrolyte membrane is 70 mass% or more.
7. The laminate described in claim 6, wherein the content of the ionic liquid in the gel electrolyte membrane is 80 mass% or more.
8. A laminate described in any one of claims 1 to 7, wherein the shear storage modulus of the gel electrolyte membrane is 0.02 MPa or more.
9. An electrochromic element having a first electrode, a second electrode, and an electrochromic layer containing an electrochromic compound and an electrolyte layer between the first electrode and the second electrode, the electrolyte layer is a gel electrolyte membrane, The gel electrolyte membrane is an electrochromic element characterized in that a peel index value obtained by dividing the maximum stress by an integral value obtained by integrating the stress over the peel distance is 5.5 mm -1 or more and 7.5 mm -1 or less, obtained by a probe tack test in which a stainless steel probe having a diameter of 5 mm is brought into contact with the gel electrolyte membrane having an average thickness of 700 μm from above at a speed of 120 mm / sec under environmental conditions of 25°C, a pressing load of 40 gf is applied, and the pressing load is held for 5 seconds, and the probe is peeled off in the vertical direction at a speed of 400 mm / sec.
Citation Information
Patent Citations
Polymer solid electrolytic film stack
JP2011253753A
Tacky hydrogel, and tacky gel sheet and electrode pad using the same
JP2013075979A
Gel electrolyte and electrochromic device
JP2017090677A
Curable resin composition, method for producing curable resin composition, and method for measuring tackiness of viscoelastic material surface
JP2017226782A
Gel polymer electrolyte, method for producing gel polymer electrolyte, and electrochromic device including the same
JP2019534934A