Fluorene derivatives and their uses
Fluorene derivatives with specific structures address the challenges of charge transport and refractive index in organic EL devices, enhancing their efficiency and color reproducibility by forming high-quality thin films for hole injection layers.
Patent Information
- Application Number
- JP2021511886
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-03-29
- Filing Date
- 2020-03-26
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2040-03-26
AI Technical Summary
Existing organic electroluminescence (EL) devices face challenges in achieving high charge transport properties, high transparency, and appropriate refractive index, particularly in hole injection layers, which affect their efficiency and color purity.
The use of fluorene derivatives with specific structural formulas to form thin films that exhibit high charge transport properties, high transparency, and high refractive index, suitable for use in hole injection layers of organic EL devices, even when fired at low temperatures.
The fluorene derivatives enable the production of thin films with excellent charge-transporting properties, enhancing the performance of organic EL devices by improving their efficiency and color reproducibility.
Smart Images

Figure 0007593312000001 
Figure 0007593312000002 
Figure 0007593312000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a fluorene derivative and its use. [Background technology]
[0002] In organic electroluminescence (EL) devices, charge-transporting thin films made of organic compounds are used as the light-emitting layer and charge-injection layer. In particular, the hole-injection layer is responsible for the transfer of charges between the anode and the hole-transport layer or the light-emitting layer, and plays an important role in achieving low-voltage operation and high brightness of the organic EL device.
[0003] Up to now, various efforts have been made to improve the performance of organic EL elements, and efforts have been made to adjust the refractive index of the functional film used for the purpose of improving light extraction efficiency, etc. Specifically, attempts have been made to improve the efficiency of elements by using hole injection layers and hole transport layers with relatively high or low refractive indexes, taking into account the overall configuration of the element and the refractive indexes of other adjacent members (Patent Documents 1 and 2). Thus, the refractive index is an important factor in the design of organic EL elements, and the refractive index is also considered to be an important physical property value that should be taken into consideration for materials for organic EL elements.
[0004] Furthermore, because coloration of a charge-transporting thin film used in an organic EL element reduces the color purity and color reproducibility of the organic EL element, in recent years, it has been desired that a charge-transporting thin film for an organic EL element has high transmittance in the visible region and high transparency (see Patent Document 3).
[0005] The methods for forming the hole injection layer are roughly divided into dry processes, such as deposition, and wet processes, such as spin coating. Comparing these processes, wet processes can efficiently produce thin films with high flatness over a large area. Therefore, as organic EL displays are currently being made larger, there is a constant demand for wet process materials that can be formed by wet processes and provide charge transport thin films with excellent refractive index and transparency. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Special Publication No. 2007-536718 [Patent Document 2] Special Publication No. 2017-501585 [Patent Document 3] International Publication No. 2013 / 042623 Summary of the Invention [Problem to be solved by the invention]
[0007] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a compound that can provide a thin film having good charge transport properties, a high refractive index and high transparency by low-temperature baking, and that can realize an organic EL device having excellent characteristics when this thin film is used as a hole injection layer or the like. [Means for solving the problem]
[0008] As a result of extensive research to achieve the above-mentioned object, the inventors have found that a thin film obtained by using a specific fluorene derivative exhibits high charge transport properties, and is a thin film with high transparency and high refractive index, and that when this thin film is applied to a hole injection layer or the like, an organic EL device having excellent characteristics can be obtained, thereby completing the present invention.
[0009] That is, the present invention provides the following fluorene derivatives and uses thereof. 1. A fluorene derivative represented by the following formula (1): [ka] [In the formula, Z 1 and Z 2 are each independently a group represented by any one of the following formulas (2) to (7): [ka] (In the formula, the dashed lines represent bonds. Aand R B are each independently a hydrogen atom or an alkyl group having 1 to 20 carbon atoms. Ar 1 and Ar 2 each independently represents an aryl group having 6 to 20 carbon atoms or a heteroaryl group having 2 to 20 carbon atoms, which may be substituted with a cyano group, a chlorine atom, a bromine atom, an iodine atom, a nitro group, an alkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 3 to 20 carbon atoms, a bicycloalkyl group having 4 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an alkynyl group having 2 to 20 carbon atoms, or an alkoxy group having 1 to 20 carbon atoms; Ar 3 and Ar 4 are each independently a group represented by any one of the following formulas (8) to (11). [ka] (In the formula, the dashed line represents a bond, R 1 represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, or a cyano group, a nitro group, a halogen atom, an aryl group having 6 to 20 carbon atoms which may be substituted with an alkyl group having 1 to 20 carbon atoms or a halogenated alkyl group having 1 to 20 carbon atoms, or a heteroaryl group having 6 to 20 carbon atoms which may be substituted with an alkyl group having 1 to 20 carbon atoms or a halogenated alkyl group having 1 to 20 carbon atoms, or a group represented by any of the following formulas (12) to (14): R 2 ~R 52 are each independently a hydrogen atom, a cyano group, a nitro group, a halogen atom, an alkyl group having 1 to 20 carbon atoms, or a halogenated alkyl group having 1 to 20 carbon atoms. [ka] (In the formula, the dashed line represents a bond, D A is a diarylamino group in which each aryl group is independently an aryl group having 6 to 20 carbon atoms, R 53 ~R 76each independently represents a hydrogen atom, a cyano group, a nitro group, a halogen atom, an alkyl group having 1 to 20 carbon atoms, or a halogenated alkyl group having 1 to 20 carbon atoms. 2.Ar 1 and Ar 2 are each independently a phenyl group, a 1-naphthyl group or a 2-naphthyl group, or a group represented by the following formulae (T1-1) to (T11-4), (F1-1) to (F4-4), (N1-1) to (N10-7), or (M1-1) to (M4-3). [ka] (In the formula, the dashed lines represent bonds.) [ka] (In the formula, the dashed lines represent bonds.) [ka] (In the formula, the dashed lines represent bonds.) [ka] (In the formula, the dashed lines represent bonds.) [ka] (In the formula, the dashed lines represent bonds.) [ka] (In the formula, the dashed lines represent bonds.) 3.Ar 1 and Ar 2 Fluorene derivatives 1 or 2, each of which is the same group. 4.Z 1 and Z 2 is a group represented by formula (2). 5.R 1 A fluorene derivative according to any one of 1 to 4, wherein 6.R 2 ~R 76is a hydrogen atom. 7. A charge transporting substance comprising any one of the fluorene derivatives 1 to 6. A charge transporting varnish comprising the charge transporting material of 8.7 and an organic solvent. 9. Further, the charge transport varnish of 8 containing a dopant. A charge-transporting thin film obtained from the charge-transporting varnish of 10.8 or 9. 11. An organic electroluminescence device having the charge transporting thin film of 10. 12. A step of reacting a compound represented by formula (15) with a compound represented by formula (16-1) and a compound represented by formula (16-2) to obtain an intermediate represented by formula (17); reducing the intermediate of formula (17) to obtain an intermediate of formula (18); and A step of reacting the intermediate represented by formula (18) with a halide represented by formula (19-1) and a halide represented by formula (19-2). The present invention relates to a method for producing a fluorene derivative represented by the following formula (1): [ka] (In the formula, Z 1 , Z 2 , Ar 1 , Ar 2 , Ar 3 and Ar 4 is the same as above; and X is a halogen atom or a pseudohalogen group. Effect of the Invention
[0010] By using the charge-transporting varnish containing the fluorene derivative of the present invention, a thin film having high transparency and a high refractive index can be prepared, and a thin film having excellent charge transport properties can be prepared even when baked at a low temperature of 200° C. or less. The charge-transporting thin film obtained from the charge-transporting varnish of the present invention can be suitably used as a thin film for electronic devices such as organic EL devices, and by using it as a hole injection layer or hole transport layer, particularly a hole injection layer, an organic EL device having excellent characteristics can be obtained. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] [Fluorene derivatives] The fluorene derivative of the present invention is represented by the following formula (1). [ka]
[0012] Examples of the compound represented by formula (1) include, but are not limited to, those shown below. [ka]
[0013] In formula (1), Z 1 and Z 2 are each independently a group represented by any one of the following formulas (2) to (7). 1 and Z 2 When is a group represented by formula (4) or (5), a carbon atom contained in this group bonds to the nitrogen atom in formula (1). [ka]
[0014] In formulas (2) to (7), the dashed lines represent bonds. In formula (6), R A and R B are each independently a hydrogen atom or an alkyl group having 1 to 20 carbon atoms, and preferably a hydrogen atom.
[0015] R A and R BThe alkyl group having 1 to 20 carbon atoms represented by the formula (I) may be linear, branched, or cyclic, and specific examples thereof include linear or branched alkyl groups having 1 to 20 carbon atoms, such as a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, an n-pentyl group, an n-hexyl group, an n-heptyl group, an n-octyl group, an n-nonyl group, or an n-decyl group; and cyclic alkyl groups having 3 to 20 carbon atoms, such as a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, a cyclohexyl group, a cycloheptyl group, a cyclooctyl group, a cyclononyl group, a cyclodecyl group, a bicyclobutyl group, a bicyclopentyl group, a bicyclohexyl group, a bicycloheptyl group, a bicyclooctyl group, a bicyclononyl group, or a bicyclodecyl group.
[0016] Z 1 and Z 2 is preferably a group represented by formula (2), (3), (4), (5) or (6), more preferably a group represented by formula (2), (4) or (6), and even more preferably a group represented by formula (2).
[0017] In formula (1), Ar 1 and Ar 2 are each independently an aryl group having 6 to 20 carbon atoms or a heteroaryl group having 2 to 20 carbon atoms.
[0018] Ar 1 and Ar 2 Examples of the aryl group having 6 to 20 carbon atoms represented by the formula (I) include a phenyl group, a 1-naphthyl group, a 2-naphthyl group, a 1-anthryl group, a 2-anthryl group, a 9-anthryl group, a 1-phenanthryl group, a 2-phenanthryl group, a 3-phenanthryl group, a 4-phenanthryl group, and a 9-phenanthryl group.
[0019] Ar 1 and Ar 2Examples of the heteroaryl group having 2 to 20 carbon atoms and represented by the formula (T1-1) to (T11-4), (F1-1) to (F4-4), (N1-1) to (N10-7), and (M1-1) to (M4-3) include, but are not limited to, groups represented by the following formulae (T1-1) to (T11-4), (F1-1) to (F4-4), (N1-1) to (N10-7), and (M1-1) to (M4-3). Among these, from the viewpoint of realizing a higher refractive index, the heteroaryl group is preferably a sulfur-containing heteroaryl group or a nitrogen-containing heteroaryl group, and more preferably a sulfur-containing heteroaryl group. [ka] (In the formula, the dashed lines represent bonds.)
[0020] [ka] (In the formula, the dashed lines represent bonds.)
[0021] [ka] (In the formula, the dashed lines represent bonds.)
[0022] [ka] (In the formula, the dashed lines represent bonds.)
[0023] [ka] (In the formula, the dashed lines represent bonds.)
[0024] [ka] (In the formula, the dashed lines represent bonds.)
[0025] Ar 1 and Ar 2The aryl group having 6 to 20 carbon atoms or the heteroaryl group having 2 to 20 carbon atoms represented by the following formula (I) may be substituted with a cyano group, a chlorine atom, a bromine atom, an iodine atom, a nitro group, an alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an alkynyl group having 2 to 20 carbon atoms, or an alkoxy group having 1 to 20 carbon atoms.
[0026] The alkyl group having 1 to 20 carbon atoms may be linear, branched, or cyclic. Specific examples thereof include R A and R B Examples of the above-mentioned examples are the same as those described above.
[0027] The alkenyl group having 2 to 20 carbon atoms may be linear, branched, or cyclic, and specific examples thereof include an ethenyl group, an n-1-propenyl group, an n-2-propenyl group, a 1-methylethenyl group, an n-1-butenyl group, an n-2-butenyl group, an n-3-butenyl group, a 2-methyl-1-propenyl group, a 2-methyl-2-propenyl group, a 1-ethylethenyl group, a 1-methyl-1-propenyl group, a 1-methyl-2-propenyl group, an n-1-pentenyl group, an n-1-decenyl group, and an n-1-eicosenyl group.
[0028] The alkynyl group having 2 to 20 carbon atoms may be linear, branched, or cyclic, and specific examples thereof include an ethynyl group, an n-1-propynyl group, an n-2-propynyl group, an n-1-butynyl group, an n-2-butynyl group, an n-3-butynyl group, a 1-methyl-2-propynyl group, an n-1-pentynyl group, an n-2-pentynyl group, an n-3-pentynyl group, an n-4-pentynyl group, a 1-methyl-n-butynyl group, a 2-methyl-n-butynyl group, a 3-methyl-n-butynyl group, a 1,1-dimethyl-n-propynyl group, an n-1-hexynyl group, an n-1-decynyl group, an n-1-pentadecinyl group, and an n-1-eicosynyl group.
[0029] The alkoxy group having 1 to 20 carbon atoms may be linear, branched, or cyclic, and specific examples thereof include linear or branched alkoxy groups having 1 to 20 carbon atoms, such as a methoxy group, an ethoxy group, an n-propoxy group, an isopropoxy group, an n-butoxy group, an isobutoxy group, a sec-butoxy group, a tert-butoxy group, an n-pentyloxy group, an n-hexyloxy group, an n-heptyloxy group, an n-octyloxy group, an n-nonyloxy group, or an n-decyloxy group; Examples of cyclic alkoxy groups having 3 to 20 carbon atoms include a cyclopropyloxy group, a cyclobutyloxy group, a cyclopentyloxy group, a cyclohexyloxy group, a cycloheptyloxy group, a cyclooctyloxy group, a cyclononyloxy group, a cyclodecyloxy group, a bicyclobutyloxy group, a bicyclopentyloxy group, a bicyclohexyloxy group, a bicycloheptyloxy group, a bicyclooctyloxy group, a bicyclononyloxy group, and a bicyclodecyloxy group.
[0030] Of these, Ar 1 and Ar 2Examples of the alkylphenyl groups include phenyl groups; nitrophenyl groups; alkylphenyl groups such as methylphenyl groups, ethylphenyl groups, propylphenyl groups, dimethylphenyl groups, diethylphenyl groups, dipropylphenyl groups, trimethylphenyl groups, triethylphenyl groups, tripropylphenyl groups, and structural isomers thereof; alkenylphenyl groups such as vinylphenyl groups, 1-propenylphenyl groups, and 2-propenylphenyl groups; and alkenylphenyl groups such as ethynylphenyl groups, 1-propynylphenyl groups, and 2-propynylphenyl groups. alkynylphenyl group; 1-naphthyl group; nitro-1-naphthyl group; alkyl-1-naphthyl groups such as methyl-1-naphthyl group, ethyl-1-naphthyl group, propyl-1-naphthyl group, dimethyl-1-naphthyl group, diethyl-1-naphthyl group, dipropyl-1-naphthyl group, trimethyl-1-naphthyl group, triethyl-1-naphthyl group, tripropyl-1-naphthyl group, and structural isomers thereof; vinyl-1-naphthyl group, 1-propenyl-1-naphthyl group, 2-propenyl-1-naphthyl group, etc. alkenyl-1-naphthyl group; alkynyl-1-naphthyl groups such as ethynyl-1-naphthyl group, 1-propynyl-1-naphthyl group, and 2-propynyl-1-naphthyl group; 2-naphthyl group; nitro-2-naphthyl group; methyl-2-naphthyl group, ethyl-2-naphthyl group, propyl-2-naphthyl group, dimethyl-2-naphthyl group, diethyl-2-naphthyl group, dipropyl-2-naphthyl group, trimethyl-2-naphthyl group, triethyl-2-naphthyl group, and tripropyl-2-naphthyl group; Alkyl-2-naphthyl groups such as isomers; alkenyl-2-naphthyl groups such as vinyl-2-naphthyl group, 1-propenyl-2-naphthyl group, and 2-propenyl-2-naphthyl group; alkynyl-2-naphthyl groups such as ethynyl-2-naphthyl group, 1-propynyl-2-naphthyl group, and 2-propynyl-2-naphthyl group; 9-anthryl group, 1-phenanthryl group, 2-phenanthryl group, 3-phenanthryl group, and 9-phenanthryl group; and groups represented by formulae (T1-1) to (T11-4) are preferred. In addition, Ar 1 and Ar 2 are preferably the same group from the viewpoint of ease of synthesis of the fluorene derivative.
[0031] In formula (1), Ar3 and Ar 4 are each independently a group represented by any one of the following formulas (8) to (11). [ka]
[0032] In formulas (8) to (11), the dashed lines represent bonds. 1 is a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, or a cyano group, a nitro group, a halogen atom, an aryl group having 6 to 20 carbon atoms which may be substituted with an alkyl group having 1 to 20 carbon atoms or a halogenated alkyl group having 1 to 20 carbon atoms, or a heteroaryl group having 6 to 20 carbon atoms which may be substituted with an alkyl group having 1 to 20 carbon atoms or a halogenated alkyl group having 1 to 20 carbon atoms, or a group represented by any of the following formulas (12) to (14). [ka]
[0033] In formulas (12) to (14), the dashed lines represent bonds. A is a diarylamino group in which each aryl group is independently an aryl group having 6 to 20 carbon atoms.
[0034] R 1 The alkyl group having 1 to 20 carbon atoms represented by the formula (6) and the alkyl group having 1 to 20 carbon atoms which is the substituent include R A and R B The same as those mentioned in the explanation of R 1 The aryl group having 6 to 20 carbon atoms represented by the formula (1) is Ar 1 and Ar 2 The same as those mentioned in the explanation of R 1Examples of the heteroaryl group having 2 to 20 carbon atoms represented by the formula (I) include a 2-thienyl group, a 3-thienyl group, a 2-furanyl group, a 3-furanyl group, a 2-oxazolyl group, a 4-oxazolyl group, a 5-oxazolyl group, a 3-isoxazolyl group, a 4-isoxazolyl group, a 5-isoxazolyl group, a 2-thiazolyl group, a 4-thiazolyl group, a 5-thiazolyl group, a 3-isothiazolyl group, a 4-isothiazolyl group, a 5-isothiazolyl group, a 2-imidazolyl group, a 4-imidazolyl group, a 2-pyridyl group, a 3-pyridyl group, and a 4-pyridyl group.
[0035] Examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom. Examples of the halogenated alkyl group having 1 to 20 carbon atoms include the alkyl group having 1 to 20 carbon atoms in which a part or all of the hydrogen atoms are substituted with the halogen atom, and specifically, examples of the same as those described below in the explanation of formula (B) are included. Examples of the diarylamino group include a diphenylamino group, a dinaphthylamino group, a dianthrylamino group, an N-phenyl-N-naphthylamino group, an N-phenyl-N-anthrylamino group, and an N-naphthyl-N-anthrylamino group.
[0036] As the groups represented by the formulae (12) to (14), those represented by the following formulae (12-1) to (14-1) and the like are preferable. [ka]
[0037] Of these, R 1 is preferably a hydrogen atom, a phenyl group, a 1-naphthyl group, a 2-naphthyl group, a 1-anthryl group, a 2-anthryl group, a 9-anthryl group, a 1-phenanthryl group, a 2-phenanthryl group, a 3-phenanthryl group, a 4-phenanthryl group, a 9-phenanthryl group, a group represented by formula (12-1), a group represented by formula (13-1), or a phenyl group, more preferably a group represented by formula (12-1), a group represented by formula (13-1), or a phenyl group, and still more preferably a phenyl group.
[0038] In formulas (8) to (14), R 2 ~R 76 R are each independently a hydrogen atom, a cyano group, a nitro group, a halogen atom, an alkyl group having 1 to 20 carbon atoms, or a halogenated alkyl group having 1 to 20 carbon atoms. 2 ~R 76 As the alkyl group having 1 to 20 carbon atoms represented by the formula (6), A and R B Among these, R 2 ~R 76 is preferably a hydrogen atom, a cyano group, a nitro group, a halogen atom, an alkyl group having 1 to 10 carbon atoms, or a halogenated alkyl group having 1 to 10 carbon atoms, more preferably a hydrogen atom, a cyano group, a nitro group, a halogen atom, or a trifluoromethyl group, and even more preferably all of them are hydrogen atoms.
[0039] Examples of the groups represented by formulas (8) to (11) include, but are not limited to, the following. [ka] (In the formula, R 1 ~R 52 is the same as above. The dashed lines indicate bonds.)
[0040] As the groups represented by the formulae (8) to (11), the following are particularly preferred. [ka] (In the formula, the dashed lines represent bonds.)
[0041] [Method of synthesizing fluorene derivatives] The fluorene derivative of the present invention can be synthesized by the method shown in Scheme A below. [ka] (In the formula, Z 1 , Z 2 , Ar 1 , Ar 2 , Ar3 and Ar 4 is the same as above. X is a halogen atom or a pseudohalogen group.
[0042] Examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, etc. Examples of the pseudohalogen group include a fluoroalkylsulfonyloxy group such as a methanesulfonyloxy group, a trifluoromethanesulfonyloxy group, a nonafluorobutanesulfonyloxy group, etc.; an aromatic sulfonyloxy group such as a benzenesulfonyloxy group, a toluenesulfonyloxy group, etc.
[0043] The compound represented by formula (15) can be synthesized by a conventionally known method, for example, according to the method described in J. Mater. Chem. C, 2014, pp. 1068-1075.
[0044] In Scheme A, the first step is a step of obtaining an intermediate represented by formula (17) from a compound represented by formula (15), a compound represented by formula (16-1), and a compound represented by formula (16-2) by a coupling reaction. Although Scheme A shows a synthesis method using the Suzuki-Miyaura coupling reaction as an example, it is also possible to synthesize the compound by using other coupling reactions.
[0045] Catalysts used in the Suzuki-Miyaura coupling reaction include palladium catalysts such as [1,1'-bis(diphenylphosphino)ferrocene]palladium(II) dichloride (PdCl2(dppf)), tetrakis(triphenylphosphine)palladium (Pd(PPh3)4), bis(triphenylphosphine)dichloropalladium (Pd(PPh3)2Cl2), bis(benzylideneacetone)palladium (Pd(dba)2), tris(benzylideneacetone)dipalladium (Pd2(dba)3), bis(tri-tert-butylphosphine)palladium (Pd(Pt-Bu3)2), and palladium acetate (Pd(OAc)2). Among these, from the viewpoint of efficiently obtaining the target product, preferred catalysts are PdCl2(dppf), Pd(PPh3)4, Pd(PPh3)2Cl2, and Pd(Pt-Bu3)2, more preferably Pd(PPh3)4 and Pd(Pt-Bu3)2. The amount of the catalyst used is usually about 0.1 to 50 mol%, preferably 0.1 to 30 mol%, and more preferably 1 to 10 mol%, based on the compound represented by formula (15).
[0046] In addition, a base is also used in the Suzuki-Miyaura coupling reaction, and examples of the base include hydroxides such as sodium hydroxide, potassium hydroxide, and cesium hydroxide, alkoxides such as sodium tert-butoxide and potassium tert-butoxide, fluoride salts such as lithium fluoride, potassium fluoride, and cesium fluoride, carbonates such as lithium carbonate, sodium carbonate, potassium carbonate, cesium carbonate, sodium bicarbonate, and potassium bicarbonate, phosphates such as potassium phosphate, and amines such as trimethylamine, triethylamine, diisopropylamine, n-butylamine, and diisopropylethylamine. Among these, from the viewpoint of efficiently obtaining the target product, preferred bases are carbonates such as sodium carbonate, potassium carbonate, cesium carbonate, sodium bicarbonate, and potassium bicarbonate, and phosphates such as potassium phosphate, and more preferably potassium carbonate and cesium carbonate. The amount of the base used is usually about 2 to 20 equivalents, preferably 1 to 20 equivalents, and more preferably 2 to 8 equivalents, relative to the compound represented by formula (15).
[0047] The solvent used in the first step is not particularly limited as long as it does not adversely affect the reaction. Specific examples of the solvent include aliphatic hydrocarbons (pentane, n-hexane, n-octane, n-decane, decalin, etc.), halogenated aliphatic hydrocarbons (chloroform, dichloromethane, dichloroethane, carbon tetrachloride, etc.), aromatic hydrocarbons (benzene, nitrobenzene, toluene, o-xylene, m-xylene, p-xylene, mesitylene, etc.), ethers (diethyl ether, diisopropyl ether, tert-butyl ether, Examples of suitable solvents include ethyl ether, tetrahydrofuran (THF), dioxane, 1,2-dimethoxyethane, 1,2-diethoxyethane, etc.), amides (N,N-dimethylformamide (DMF), N,N-dimethylacetamide, etc.), lactams and lactones (N-methylpyrrolidone, γ-butyrolactone, etc.), urea derivatives (N,N-dimethylimidazolidinone, tetramethylurea, etc.), sulfoxides (dimethyl sulfoxide, sulfolane, etc.), and nitriles (acetonitrile, propionitrile, butyronitrile, etc.). Among these, from the viewpoint of efficiently obtaining the target substance, preferred solvents are aliphatic hydrocarbons (pentane, n-hexane, n-octane, n-decane, decalin, etc.), aromatic hydrocarbons (benzene, nitrobenzene, toluene, o-xylene, m-xylene, p-xylene, mesitylene, etc.), and ethers (diethyl ether, diisopropyl ether, tert-butyl methyl ether, THF, dioxane, 1,2-dimethoxyethane, 1,2-diethoxyethane, etc.), and more preferred are aromatic hydrocarbons (benzene, nitrobenzene, toluene, o-xylene, m-xylene, p-xylene, mesitylene, etc.), and ethers (diethyl ether, diisopropyl ether, tert-butyl methyl ether, THF, dioxane, 1,2-dimethoxyethane, 1,2-diethoxyethane, etc.).
[0048] The ratio of the compound represented by formula (15) to the compound represented by formula (16-1) and the compound represented by formula (16-2) is preferably 2 to 6 equivalents, more preferably 2 to 3 equivalents, of the total of the compound represented by formula (16-1) and the compound represented by formula (16-2) relative to the compound represented by formula (15). The compound represented by formula (16-1) and the compound represented by formula (16-2) may be the same or different from each other.
[0049] In the first step, the reaction temperature is appropriately set within the range from the melting point to the boiling point of the solvent while taking into consideration the type and amount of the raw material compounds and catalyst used, and is usually about 0 to 200° C., and preferably 0 to 50° C. The reaction time cannot be generally specified because it varies depending on the raw material compounds used and the reaction temperature, but is usually about 1 to 24 hours.
[0050] In the scheme A, the second step is a step of reducing the intermediate represented by formula (17) to obtain an intermediate represented by formula (18). Examples of the reduction method include known methods such as catalytic hydrogenation and chemical reduction using a metal and an acid.
[0051] When reduction is carried out by catalytic hydrogenation, it may be carried out using a known catalyst such as palladium on carbon, Raney nickel catalyst, platinum oxide, ruthenium on carbon, rhodium on carbon, platinum on carbon, etc. In addition, conditions for catalytic hydrogenation include, for example, a hydrogen pressure of 1 to 10 atm, a reaction temperature of 20 to 100° C., and a reaction time of 1 to 48 hours.
[0052] In Scheme A, the third step is a step of synthesizing the fluorene derivative represented by formula (1) by reacting the intermediate represented by formula (18) with the compound represented by formula (19-1) and the compound represented by formula (19-2).
[0053] In the third step, a base may be used. Examples of the base include the same bases as those usable in the first step. Among these, triethylamine, pyridine, diisopropylethylamine, etc. are particularly suitable because they are easy to handle.
[0054] The reaction solvent is preferably an aprotic organic solvent, such as N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, 1,3-dimethyl-2-imidazolidinone, dimethylsulfoxide, tetrahydrofuran, dioxane, etc. From the viewpoint of ease of removal of the reaction solvent after the reaction, N,N-dimethylformamide, N,N-dimethylacetamide, tetrahydrofuran, dioxane, toluene, xylene, mesitylene, etc. are preferred.
[0055] The ratio of the intermediate represented by formula (18) to the compound represented by formula (19-1) and the compound represented by formula (19-2) is preferably 2 to 6 equivalents, more preferably 2 to 3 equivalents, of the total of the compound represented by formula (19-1) and the compound represented by formula (19-2) relative to the intermediate represented by formula (18). The compound represented by formula (19-1) and the compound represented by formula (19-2) may be the same or different from each other.
[0056] In the third step, the reaction temperature is appropriately set within the range from the melting point to the boiling point of the solvent while taking into consideration the type and amount of the raw material compounds and catalyst used, and is usually about 0 to 200° C., and preferably 0 to 50° C. The reaction time cannot be generally specified because it varies depending on the raw material compounds used and the reaction temperature, but is usually about 1 to 24 hours.
[0057] After the reaction is completed, the reaction mixture is post-treated in a conventional manner to obtain the desired fluorene derivative.
[0058] The compound represented by formula (19-1) and the compound represented by formula (19-2) can be obtained by a known method or commercially available products.
[0059] [Charge transporting substance] The fluorene derivative of the present invention can be suitably used as a charge transporting material, particularly as a hole transporting material. In the present invention, charge transporting property is synonymous with electrical conductivity. A charge transporting material is a material that has charge transporting property by itself. In addition, a charge transporting varnish may be a material that has charge transporting property by itself, or a solid film obtained by the charge transporting varnish may have charge transporting property.
[0060] [Charge-transporting varnish] The charge transporting varnish of the present invention contains a charge transporting substance made of the fluorene derivative and an organic solvent. The charge transporting substance may be used alone or in combination of two or more kinds.
[0061] [Organic solvents] As the organic solvent, a highly polar solvent capable of dissolving the fluorene derivative well can be used. The fluorene derivative of the present invention can be dissolved in a solvent regardless of the polarity of the solvent. If necessary, a low polar solvent may be used because it has better process compatibility than a high polar solvent. In the present invention, a low polar solvent is defined as a solvent having a relative dielectric constant of less than 7 at a frequency of 100 kHz, and a high polar solvent is defined as a solvent having a relative dielectric constant of 7 or more at a frequency of 100 kHz.
[0062] Examples of the low polarity solvent include chlorine-based solvents such as chloroform and chlorobenzene; aromatic hydrocarbon-based solvents such as toluene, xylene, tetralin, cyclohexylbenzene, and decylbenzene; aliphatic alcohol-based solvents such as 1-octanol, 1-nonanol, and 1-decanol; ether-based solvents such as tetrahydrofuran, dioxane, anisole, 4-methoxytoluene, 3-phenoxytoluene, dibenzyl ether, diethylene glycol dimethyl ether, diethylene glycol butyl methyl ether, triethylene glycol dimethyl ether, and triethylene glycol butyl methyl ether; and ester-based solvents such as methyl benzoate, ethyl benzoate, butyl benzoate, isoamyl benzoate, bis(2-ethylhexyl) phthalate, dibutyl maleate, dibutyl oxalate, hexyl acetate, diethylene glycol monoethyl ether acetate, and diethylene glycol monobutyl ether acetate.
[0063] Examples of the highly polar solvent include amide-based solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, N,N-dimethylisobutyramide, N-methylpyrrolidone, and 1,3-dimethyl-2-imidazolidinone; ketone-based solvents such as ethyl methyl ketone, isophorone, and cyclohexanone; cyano-based solvents such as acetonitrile and 3-methoxypropionitrile; polyhydric alcohol-based solvents such as ethylene glycol, diethylene glycol, triethylene glycol, dipropylene glycol, 1,3-butanediol, and 2,3-butanediol; monohydric alcohol-based solvents other than aliphatic alcohols such as diethylene glycol monomethyl ether, diethylene glycol monophenyl ether, triethylene glycol monomethyl ether, dipropylene glycol monomethyl ether, benzyl alcohol, 2-phenoxyethanol, 2-benzyloxyethanol, 3-phenoxybenzyl alcohol, and tetrahydrofurfuryl alcohol; and sulfoxide-based solvents such as dimethyl sulfoxide.
[0064] The amount of the solvent used is such that the solid content concentration in the varnish of the present invention is generally about 0.1 to 20% by mass, preferably 0.5 to 10% by mass, from the viewpoint of ensuring a sufficient film thickness while suppressing the precipitation of the charge transporting material. The solid content here means the components contained in the varnish other than the solvent. The solvent may be used alone or in combination of two or more.
[0065] [Dopant (charge-accepting dopant)] The charge-transporting varnish of the present invention may contain a dopant for the purpose of improving the charge transportability of the thin film obtained from the charge-transporting varnish of the present invention. The dopant is not particularly limited as long as it is soluble in at least one solvent used in the composition, and both inorganic and organic dopants can be used. Furthermore, the dopant may be a substance in which a part of the molecule is removed by an external stimulus such as heating during baking in the process of obtaining a charge-transporting thin film, which is a solid film, from the composition, and the function as a dopant is first expressed or improved, for example, an arylsulfonic acid ester compound protected by a group from which the sulfonic acid group is easily removed.
[0066] The inorganic dopant is preferably a heteropolyacid, and specific examples thereof include phosphomolybdic acid, silicomolybdic acid, phosphotungstic acid, phosphotungstomolybdic acid, and silicotungstic acid.
[0067] Heteropolyacids are polyacids that have a structure in which a heteroatom is located at the center of the molecule, typically represented by the chemical structure of the Keggin type represented by the following formula (HPA1) or the Dawson type represented by the following formula (HPA2), and are formed by condensing an isopolyacid, which is an oxyacid of vanadium (V), molybdenum (Mo), tungsten (W), etc., with an oxyacid of a different element. Examples of such oxyacids of different elements include oxyacids of silicon (Si), phosphorus (P), and arsenic (As). [ka]
[0068] Examples of the heteropolyacid include phosphomolybdic acid, silicomolybdic acid, phosphotungstic acid, silicotungstic acid, and phosphotungstomolybdic acid. These may be used alone or in combination of two or more. The heteropolyacid used in the present invention is commercially available, and can also be synthesized by a known method. In particular, when one type of heteropolyacid is used, the one type of heteropolyacid is preferably phosphotungstic acid or phosphomolybdic acid, and phosphotungstic acid is the most suitable. When two or more types of heteropolyacids are used, one of the two or more types of heteropolyacids is preferably phosphotungstic acid or phosphomolybdic acid, and phosphotungstic acid is more preferable.
[0069] In addition, even if the heteropolyacid has a large or small number of elements in the structure represented by the general formula in a quantitative analysis such as elemental analysis, it can be used in the present invention as long as it is obtained as a commercially available product or is appropriately synthesized according to a known synthesis method.
[0070] For example, phosphotungstic acid is generally represented by the chemical formula H3(PW 12 O 40 )·nH2O, and phosphomolybdic acid has the chemical formula H3(PMo 12 O 40 )·nH2O, but in quantitative analysis, those having a large or small number of P (phosphorus), O (oxygen), W (tungsten), or Mo (molybdenum) in this formula can be used in the present invention as long as they are commercially available or appropriately synthesized according to a known synthesis method. In this case, the mass of the heteropolyacid specified in the present invention does not mean the mass of pure phosphotungstic acid (phosphotungstic acid content) in the synthesized or commercially available product, but the total mass including water of hydration and other impurities in a commercially available form or in a form that can be isolated by a known synthesis method.
[0071] Examples of the organic dopant include arylsulfonic acid, arylsulfonic acid esters, ionic compounds consisting of a specific anion and its counter cation, tetracyanoquinodimethane derivatives, and benzoquinone derivatives.
[0072] As the arylsulfonic acid compound, those represented by the following formula (A) or (B) are preferred from the viewpoint of the transparency of the thin film obtained from the charge transporting varnish of the present invention. [ka]
[0073] In formula (A), A 1 is -O- or -S-, with -O- being preferred. 2 is derived from naphthalene or anthracene (p 2 +1) valence group (i.e., from naphthalene or anthracene to p 2 + A group obtained by removing one hydrogen atom), but a group derived from naphthalene is preferred. 3 is a divalent to tetravalent perfluorobiphenyl group. 1 A 1 and A 3 is the number of bonds with p 1 An integer that satisfies ≦4, but A 3 is a divalent perfluorobiphenyl group, and p 1 is preferably 2. 2 A 2 The number of sulfonic acid groups bonded to p is 1≦p 2 An integer satisfying the condition ≦4, with 2 being preferred.
[0074] In formula (B), A 4 ~A 8 each independently represents a hydrogen atom, a halogen atom, a cyano group, an alkyl group having 1 to 20 carbon atoms, a halogenated alkyl group having 1 to 20 carbon atoms, or a halogenated alkenyl group having 2 to 20 carbon atoms; 4 ~A 8At least three of the groups are halogen atoms. q is the number of sulfonic acid groups bonded to the naphthalene ring and is an integer satisfying 1≦q≦4, preferably 2 to 4, and more preferably 2.
[0075] Examples of the halogenated alkyl group having 1 to 20 carbon atoms include a trifluoromethyl group, a 2,2,2-trifluoroethyl group, a perfluoroethyl group, a 3,3,3-trifluoropropyl group, a 2,2,3,3,3-pentafluoropropyl group, a perfluoropropyl group, a 4,4,4-trifluorobutyl group, a 3,3,4,4,4-pentafluorobutyl group, a 2,2,3,3,4,4,4-heptafluorobutyl group, a perfluorobutyl group, etc. Examples of the halogenated alkenyl group having 2 to 20 carbon atoms include a perfluoroethenyl group, a 1-perfluoropropenyl group, a perfluoroallyl group, a perfluorobutenyl group, etc.
[0076] Examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom, and a fluorine atom is preferable. Examples of the alkyl group having 1 to 20 carbon atoms include R A and R B Examples of the above-mentioned examples are the same as those described above.
[0077] Among these, A 4 ~A 8 is a hydrogen atom, a halogen atom, a cyano group, an alkyl group having 1 to 10 carbon atoms, a halogenated alkyl group having 1 to 10 carbon atoms, or a halogenated alkenyl group having 2 to 10 carbon atoms, and A 4 ~A 8 At least three of A are preferably fluorine atoms, and A is a hydrogen atom, a fluorine atom, a cyano group, an alkyl group having 1 to 5 carbon atoms, a fluorinated alkyl group having 1 to 5 carbon atoms, or a fluorinated alkenyl group having 2 to 5 carbon atoms. 4 ~A 8 At least three of A are preferably fluorine atoms, and A is preferably a hydrogen atom, a fluorine atom, a cyano group, a perfluoroalkyl group having 1 to 5 carbon atoms, or a perfluoroalkenyl group having 1 to 5 carbon atoms. 4 , A5 and A 8 It is more preferable that is a fluorine atom. Note that the perfluoroalkyl group is a group in which all hydrogen atoms of an alkyl group are substituted with fluorine atoms, and the perfluoroalkenyl group is a group in which all hydrogen atoms of an alkenyl group are substituted with fluorine atoms.
[0078] Specific examples of suitable arylsulfonic acids include, but are not limited to, those shown below. [ka]
[0079] Examples of the arylsulfonic acid ester compound include the arylsulfonic acid ester compounds disclosed in WO 2017 / 217455, the arylsulfonic acid ester compounds disclosed in WO 2017 / 217457, and the arylsulfonic acid ester compounds described in Japanese Patent Application No. 2017-243631, from the viewpoint of the transparency of the thin film obtained from the charge-transporting varnish of the present invention.
[0080] Specifically, from the viewpoint of solubility in a low polarity solvent, the arylsulfonic acid ester compound is preferably one represented by any one of the following formulas (C) to (E). [ka]
[0081] In the formulas (C) to (E), m is an integer satisfying 1≦m≦4, and is preferably 2. n is an integer satisfying 1≦n≦4, and is preferably 2.
[0082] In formula (C), A 11 is an m-valent group derived from perfluorobiphenyl (i.e., a group obtained by removing m fluorine atoms from perfluorobiphenyl). 12 is -O- or -S-, with -O- being preferred. 13R is a (n+1)-valent group derived from naphthalene or anthracene (i.e., a group obtained by removing n+1 hydrogen atoms from naphthalene or anthracene), with a group derived from naphthalene being preferred. s1 ~R s4 are each independently a hydrogen atom or a linear or branched alkyl group having 1 to 6 carbon atoms; R s5 is an optionally substituted monovalent hydrocarbon group having 2 to 20 carbon atoms.
[0083] R s1 ~R s4 Examples of the linear or branched alkyl group having 1 to 6 carbon atoms represented by the formula (1) include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, an n-hexyl group, etc. Among these, an alkyl group having 1 to 3 carbon atoms is preferred.
[0084] R s5 The monovalent hydrocarbon group having 2 to 20 carbon atoms represented by the formula (I) may be linear, branched, or cyclic, and specific examples thereof include alkyl groups such as an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, and a tert-butyl group; and aryl groups such as a phenyl group, a naphthyl group, and a phenanthryl group.
[0085] In particular, R s1 ~R s4 Of these, R s1 or R s3 is a linear alkyl group having 1 to 3 carbon atoms, and the rest are hydrogen atoms, or R s1 is a linear alkyl group having 1 to 3 carbon atoms, and R s2 ~R s4 is preferably a hydrogen atom. In this case, the linear alkyl group having 1 to 3 carbon atoms is preferably a methyl group. s5 As the alkyl group, a linear alkyl group having 2 to 4 carbon atoms or a phenyl group is preferable.
[0086] In formula (D), A 14is an m-valent hydrocarbon group having 6 to 20 carbon atoms, containing one or more aromatic rings, which may be substituted, and which is obtained by removing m hydrogen atoms from a hydrocarbon compound having 6 to 20 carbon atoms, containing one or more aromatic rings. Examples of the hydrocarbon compound include benzene, toluene, xylene, ethylbenzene, biphenyl, naphthalene, anthracene, and phenanthrene.
[0087] In addition, A 14 In the hydrocarbon group represented by the formula (I), some or all of the hydrogen atoms may be further substituted with a substituent, and examples of such a substituent include a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, a nitro group, a cyano group, a hydroxy group, an amino group, a silanol group, a thiol group, a carboxy group, a sulfonate group, a phosphoric acid group, a phosphoric acid ester group, an ester group, a thioester group, an amide group, a monovalent hydrocarbon group, an organooxy group, an organoamino group, an organosilyl group, an organothio group, an acyl group, and a sulfo group. 14 As the alkyl group, groups derived from benzene, biphenyl, etc. are preferred.
[0088] In formula (D), A 15 is -O- or -S-, with -O- being preferred.
[0089] In formula (D), A 16 is an aromatic hydrocarbon group having 6 to 20 carbon atoms and a valence of (n+1), which is obtained by removing (n+1) hydrogen atoms from an aromatic ring of an aromatic hydrocarbon compound having 6 to 20 carbon atoms. Examples of the aromatic hydrocarbon compound include benzene, toluene, xylene, biphenyl, naphthalene, anthracene, and pyrene. Among them, A 16 As the alkyl group, a group derived from naphthalene or anthracene is preferable, and a group derived from naphthalene is more preferable.
[0090] In formula (D), R s6 and R s7 are each independently a hydrogen atom or a linear or branched monovalent aliphatic hydrocarbon group; Rs8 is a linear or branched monovalent aliphatic hydrocarbon group, provided that R s6 , R s7 and R s8 The total number of carbon atoms in R is 6 or more. s6 , R s7 and R s8 The upper limit of the total number of carbon atoms is not particularly limited, but is preferably 20 or less, and more preferably 10 or less.
[0091] R s6 , R s7 and R s8 Specific examples of the linear or branched monovalent aliphatic hydrocarbon group represented by the formula (I) include alkyl groups having 1 to 20 carbon atoms, such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, n-hexyl, n-octyl, 2-ethylhexyl, and decyl groups; and alkenyl groups having 2 to 20 carbon atoms, such as vinyl, 1-propenyl, 2-propenyl, isopropenyl, 1-methyl-2-propenyl, 1-butenyl, 2-butenyl, 3-butenyl, and hexenyl groups. s6 is preferably a hydrogen atom, and R s7 and R s8 are each preferably an alkyl group having 1 to 6 carbon atoms.
[0092] In formula (E), R s9 ~R s13 are each independently a hydrogen atom, a nitro group, a cyano group, a halogen atom, an alkyl group having 1 to 10 carbon atoms, a halogenated alkyl group having 1 to 10 carbon atoms, or a halogenated alkenyl group having 2 to 10 carbon atoms.
[0093] R s9 ~R s13The alkyl group having 1 to 10 carbon atoms represented by the formula (I) may be linear, branched, or cyclic, and specific examples thereof include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, an n-pentyl group, a cyclopentyl group, an n-hexyl group, a cyclohexyl group, an n-heptyl group, an n-octyl group, an n-nonyl group, and an n-decyl group.
[0094] R s9 ~R s13 The halogenated alkyl group having 1 to 10 carbon atoms represented by the formula (I) is not particularly limited as long as it is a group in which some or all of the hydrogen atoms of an alkyl group having 1 to 10 carbon atoms are substituted with halogen atoms. Specific examples thereof include a trifluoromethyl group, a 2,2,2-trifluoroethyl group, a 1,1,2,2,2-pentafluoroethyl group, a 3,3,3-trifluoropropyl group, a 2,2,3,3,3-pentafluoropropyl group, a 1,1,2,2,3,3,3-heptafluoropropyl group, a 4,4,4-trifluorobutyl group, a 3,3,4,4,4-pentafluorobutyl group, a 2,2,3,3,4,4,4-heptafluorobutyl group, and a 1,1,2,2,3,3,4,4,4-nonafluorobutyl group.
[0095] R s9 ~R s13 The halogenated alkenyl group having 2 to 10 carbon atoms represented by the formula (I) is not particularly limited as long as it is a group in which some or all of the hydrogen atoms of an alkenyl group having 2 to 10 carbon atoms have been substituted with halogen atoms, and specific examples thereof include a perfluorovinyl group, a perfluoro-1-propenyl group, a perfluoro-2-propenyl group, a perfluoro-1-butenyl group, a perfluoro-2-butenyl group, and a perfluoro-3-butenyl group.
[0096] Among these, R s9R is preferably a nitro group, a cyano group, a halogenated alkyl group having 1 to 10 carbon atoms, or a halogenated alkenyl group having 2 to 10 carbon atoms, more preferably a nitro group, a cyano group, a halogenated alkyl group having 1 to 4 carbon atoms, or a halogenated alkenyl group having 2 to 4 carbon atoms, and even more preferably a nitro group, a cyano group, a trifluoromethyl group, or a perfluoropropenyl group. s10 ~R s13 As the group, a halogen atom is preferable, and a fluorine atom is more preferable.
[0097] In formula (E), A 17 is -O-, -S- or -NH-, with -O- being preferred.
[0098] In formula (E), A 18 is an aromatic hydrocarbon group having 6 to 20 carbon atoms and a valence of (n+1), which is obtained by removing (n+1) hydrogen atoms from an aromatic ring of an aromatic hydrocarbon compound having 6 to 20 carbon atoms. Examples of the aromatic hydrocarbon compound include benzene, toluene, xylene, biphenyl, naphthalene, anthracene, pyrene, etc. Among these, A 18 As the alkyl group, a group derived from naphthalene or anthracene is preferable, and a group derived from naphthalene is more preferable.
[0099] In formula (E), R s14 ~R s17are each independently a hydrogen atom or a linear or branched monovalent aliphatic hydrocarbon group having 1 to 20 carbon atoms. Examples of the monovalent aliphatic hydrocarbon group include alkyl groups having 1 to 20 carbon atoms, such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, n-pentyl, cyclopentyl, n-hexyl, cyclohexyl, n-heptyl, n-octyl, n-nonyl, n-decyl, n-undecyl, and n-dodecyl; and alkenyl groups having 2 to 20 carbon atoms, such as vinyl, 1-propenyl, 2-propenyl, isopropenyl, 1-methyl-2-propenyl, 1-butenyl, 2-butenyl, 3-butenyl, and hexenyl. Among these, alkyl groups having 1 to 20 carbon atoms are preferred, alkyl groups having 1 to 10 carbon atoms are more preferred, and alkyl groups having 1 to 8 carbon atoms are even more preferred.
[0100] In formula (E), R s18 represents a linear or branched monovalent aliphatic hydrocarbon group having 1 to 20 carbon atoms, or -OR s19 R s19 is an optionally substituted monovalent hydrocarbon group having 2 to 20 carbon atoms.
[0101] R s18 As the linear or branched monovalent aliphatic hydrocarbon group having 1 to 20 carbon atoms represented by the formula s14 ~R s17 The same as those mentioned in the explanation of R s18 is a monovalent aliphatic hydrocarbon group, R s18 is preferably an alkyl group having 1 to 20 carbon atoms, more preferably an alkyl group having 1 to 10 carbon atoms, and even more preferably an alkyl group having 1 to 8 carbon atoms.
[0102] R s19 Examples of the monovalent hydrocarbon group having 2 to 20 carbon atoms represented by the formula (I) include the above-mentioned monovalent aliphatic hydrocarbon groups other than the methyl group, as well as aryl groups such as phenyl, naphthyl, and phenanthryl groups. s19 is preferably a linear alkyl group having 2 to 4 carbon atoms or a phenyl group.
[0103] Examples of the substituent that the monovalent hydrocarbon group may have include a fluorine atom, an alkoxy group having 1 to 4 carbon atoms, a nitro group, and a cyano group.
[0104] Specific examples of suitable arylsulfonate compounds include, but are not limited to, those shown below.
[0105] [ka]
[0106] As the ionic compound consisting of the above-mentioned predetermined anion and its counter cation, from the viewpoint of the transparency of the thin film obtained from the charge transporting varnish of the present invention, the ionic compound represented by the following formula (F) is preferred. [ka]
[0107] In formula (F), E is an element of Group 13 of the long periodic table, and Ar 101 ~Ar 104 each independently represents an aryl group having 6 to 20 carbon atoms or a heteroaryl group having 2 to 20 carbon atoms, which may be substituted with a halogen atom such as a fluorine atom, a chlorine atom, or a bromine atom, an acyl group having 2 to 12 carbon atoms such as a cyano group, a nitro group, or an acetyl group, or a halogenated alkyl group having 1 to 10 carbon atoms such as a trifluoromethyl group.
[0108] The Group 13 element represented by E is preferably a boron atom, an aluminum atom, or a gallium atom, and more preferably a boron atom. 101 ~Ar 104 The aryl group having 6 to 20 carbon atoms represented by the formula (1) is Ar 1 and Ar 2 The same as those described in the description of Ar 101 ~Ar 104Examples of the heteroaryl group having 2 to 20 carbon atoms represented by the formula (I) include a 2-thienyl group, a 3-thienyl group, a 2-furanyl group, a 3-furanyl group, a 2-oxazolyl group, a 4-oxazolyl group, a 5-oxazolyl group, a 3-isoxazolyl group, a 4-isoxazolyl group, a 5-isoxazolyl group, a 2-thiazolyl group, a 4-thiazolyl group, a 5-thiazolyl group, a 3-isothiazolyl group, a 4-isothiazolyl group, a 5-isothiazolyl group, a 2-imidazolyl group, a 4-imidazolyl group, a 2-pyridyl group, a 3-pyridyl group, and a 4-pyridyl group.
[0109] In formula (F), M + is an onium ion. Examples of the onium ion include an iodonium ion, a sulfonium ion, an ammonium ion, and a phosphonium ion. In particular, an iodonium ion represented by the following formula (G) is preferred. [ka]
[0110] In formula (G), R 101 and R 102 each independently represents an alkyl group having 1 to 12 carbon atoms, an alkenyl group having 2 to 12 carbon atoms, an alkynyl group having 2 to 12 carbon atoms, an aryl group having 6 to 20 carbon atoms, or a heteroaryl group having 2 to 20 carbon atoms, which may be substituted with a halogen atom, a cyano group, a nitro group, an alkyl group having 1 to 12 carbon atoms, an alkenyl group having 2 to 12 carbon atoms, an alkynyl group having 2 to 12 carbon atoms, an aryl group having 6 to 20 carbon atoms, or a heteroaryl group having 2 to 20 carbon atoms.
[0111] Examples of the tetracyanoquinodimethane derivative include 7,7,8,8-tetracyanoquinodimethane (TCNQ), 2-fluoro-7,7,8,8-tetracyanoquinodimethane, 2,5-difluoro-7,7,8,8-tetracyanoquinodimethane, tetrafluoro-7,7,8,8-tetracyanoquinodimethane (F4TCNQ), tetrachloro-7,7,8,8-tetracyanoquinodimethane, 2-fluoro-7,7,8,8-tetracyanoquinodimethane, 2-chloro-7,7,8,8-tetracyanoquinodimethane, 2,5-difluoro-7,7,8,8-tetracyanoquinodimethane, and 2,5-dichloro-7,7,8,8-tetracyanoquinodimethane.
[0112] Examples of the benzoquinone derivatives include tetrachloro-1,4-benzoquinone (chloranil) and 2,3-dichloro-5,6-dicyano-1,4-benzoquinone (DDQ).
[0113] When the charge-transporting varnish of the present invention contains a dopant, the content cannot be generally specified since it varies depending on the type of dopant, the desired charge transport properties, etc., but is usually about 0.01 to 50, preferably about 0.1 to 10, and more preferably about 1.0 to 5.0, in mass ratio relative to 1 part of the charge-transporting substance.
[0114] The charge transport varnish of the present invention may further contain an organic silane compound for the purpose of adjusting the film properties of the resulting charge transport thin film. The organic silane compound may be a dialkoxysilane compound, a trialkoxysilane compound, or a tetraalkoxysilane compound. In particular, the organic silane compound is preferably a dialkoxysilane compound or a trialkoxysilane compound, and more preferably a trialkoxysilane compound. The organic silane compound may be used alone or in combination of two or more kinds.
[0115] When an organic silane compound is contained, the content thereof is usually about 0.1 to 50 mass % based on the total mass of the charge transporting substance and the dopant. However, in consideration of suppressing a decrease in the charge transporting property of the obtained thin film and enhancing the hole injection ability into a layer (e.g., a hole transporting layer or a light emitting layer) laminated on the opposite side of the anode so as to be in contact with the hole injection layer made of the charge transporting thin film of the present invention, the content is preferably about 0.5 to 40 mass %, more preferably about 0.8 to 30 mass %, and even more preferably about 1 to 20 mass %.
[0116] The method of preparing charge transporting varnish is not particularly limited, but for example, the method of adding the fluorene derivative and dopant etc. as required to organic solvent in any order or simultaneously can be mentioned.In addition, when there are multiple organic solvents, first, the fluorene derivative and dopant etc. as required can be dissolved in one solvent, and then other solvent can be added thereto, or the fluorene derivative and dopant etc. as required can be dissolved in the mixed solvent of multiple organic solvents in order or simultaneously.
[0117] In order to reproducibly obtain a thin film with higher flatness, it is desirable to dissolve the fluorene derivative and, if necessary, a dopant, etc. in an organic solvent and then filter the charge-transporting varnish of the present invention using a sub-micrometer-order filter, etc.
[0118] The viscosity of the charge-transporting varnish of the present invention is usually 1 to 50 mPa·s at 25° C. The surface tension of the charge-transporting varnish of the present invention is usually 20 to 50 mN / m at 25° C. The viscosity is a value measured using a TVE-25 viscometer manufactured by Toki Sangyo Co., Ltd. The surface tension is a value measured using an automatic surface tensiometer CBVP-Z manufactured by Kyowa Interface Science Co., Ltd. The viscosity and surface tension of the varnish can be adjusted by changing the types of solvents and their ratios, solids concentration, etc. described above, taking into consideration various factors such as the desired film thickness.
[0119] [Charge transporting thin film] The charge-transporting thin film of the present invention can be formed by applying the charge-transporting varnish of the present invention onto a substrate and baking the applied varnish.
[0120] Examples of the method for applying the varnish include, but are not limited to, a dip method, a spin coating method, a transfer printing method, a roll coating method, a brush coating method, an inkjet method, a spray method, a slit coating method, etc. It is preferable to adjust the viscosity and surface tension of the varnish according to the application method.
[0121] In addition, the atmosphere in which the charge-transporting varnish is baked after application is not particularly limited, and a thin film having a uniform film surface and high charge transportability can be obtained not only in an air atmosphere but also in an inert gas such as nitrogen or in a vacuum. Depending on the type of dopant used together, a thin film having charge transportability may be reproducibly obtained by baking the varnish in an air atmosphere.
[0122] The baking temperature is appropriately set within the range of about 100 to 260° C., taking into consideration the use of the resulting thin film, the degree of charge transportability imparted to the resulting thin film, the type and boiling point of the solvent, etc. When the resulting thin film is used as a hole injection layer of an organic EL device, the baking temperature is preferably about 140 to 250° C., more preferably about 145 to 240° C., but with the charge-transporting varnish of the present invention, a thin film having good charge transportability can be obtained even at a low baking temperature of 200° C. or less. In addition, during baking, two or more stages of temperature change may be applied for the purpose of expressing more uniform film formation properties or proceeding with the reaction on the substrate, and heating may be performed using an appropriate device such as a hot plate or oven.
[0123] The thickness of the charge transporting thin film is not particularly limited, but is preferably 5 to 300 nm when used as a hole injection layer, a hole transport layer, or a hole injection transport layer of an organic EL device. Methods for changing the thickness include changing the solid concentration in the varnish, changing the amount of liquid on the substrate during application, and the like.
[0124] The charge-transporting thin film of the present invention exhibits a refractive index of 1.6 or more and an extinction coefficient of 0.030 or less, averaged over a wavelength range of 400 to 800 nm; in one embodiment, the charge-transporting thin film exhibits a refractive index of 1.65 or more, in another embodiment, a refractive index of 1.70 or more, and in one embodiment, an extinction coefficient of 0.020 or less, and in another embodiment, an extinction coefficient of 0.005 or less.
[0125] [Organic EL element] The organic EL device of the present invention has a pair of electrodes and a functional layer made of the charge transporting thin film of the present invention between the electrodes.
[0126] Representative configurations of the organic EL element include, but are not limited to, the following (a) to (f). In the following configurations, an electron blocking layer or the like can be provided between the light-emitting layer and the anode, and a hole (positive hole) blocking layer or the like can be provided between the light-emitting layer and the cathode, if necessary. In addition, the hole injection layer, the hole transport layer, or the hole injection transport layer may also function as an electron blocking layer, etc., and the electron injection layer, the electron transport layer, or the electron injection transport layer may also function as a hole blocking layer, etc. Furthermore, an arbitrary functional layer can be provided between each layer, if necessary. (a) Anode / hole injection layer / hole transport layer / light emitting layer / electron transport layer / electron injection layer / cathode (b) Anode / hole injection layer / hole transport layer / light emitting layer / electron injection transport layer / cathode (c) Anode / hole injection transport layer / light emitting layer / electron transport layer / electron injection layer / cathode (d) Anode / hole injection transport layer / light emitting layer / electron injection transport layer / cathode (e) Anode / hole injection layer / hole transport layer / light emitting layer / cathode (f) Anode / hole injection transport layer / light emitting layer / cathode
[0127] The "hole injection layer", "hole transport layer" and "hole injection transport layer" are layers formed between the light-emitting layer and the anode, and have the function of transporting holes from the anode to the light-emitting layer. When only one layer of a hole transport material is provided between the light-emitting layer and the anode, it is the "hole injection transport layer", and when two or more layers of a hole transport material are provided between the light-emitting layer and the anode, the layer closest to the anode is the "hole injection layer" and the other layers are the "hole transport layers". In particular, the hole injection (transport) layer is a thin film that is excellent not only in terms of hole acceptance from the anode but also in terms of hole injection into the hole transport (light-emitting) layer.
[0128] An "electron injection layer", "electron transport layer" and "electron injection transport layer" are layers formed between a light-emitting layer and a cathode, and have the function of transporting electrons from the cathode to the light-emitting layer. When only one layer of an electron transporting material is provided between the light-emitting layer and the cathode, it is the "electron injection transport layer", and when two or more layers of an electron transporting material are provided between the light-emitting layer and the cathode, the layer closest to the cathode is the "electron injection layer" and the other layers are "electron transport layers".
[0129] The "light-emitting layer" is an organic layer having a light-emitting function, and contains a host material and a dopant material when a doping system is adopted. In this case, the host material mainly has a function of promoting the recombination of electrons and holes and confining excitons in the light-emitting layer, and the dopant material has a function of efficiently emitting the excitons obtained by the recombination. In the case of a phosphorescent element, the host material mainly has a function of confining the excitons generated by the dopant in the light-emitting layer.
[0130] The charge transporting thin film of the present invention can be suitably used as a functional layer provided between an anode and an emitting layer in an organic EL device, and can be more suitably used as a hole injection layer, a hole transport layer, or a hole injection transport layer, and can be even more suitably used as a hole injection layer.
[0131] When an organic EL device is produced using the charge transporting varnish of the present invention, the materials used and the production method thereof include, but are not limited to, those described below.
[0132] An example of a method for producing an organic EL device having a hole injection layer made of a charge transporting thin film obtained from the charge transporting varnish of the present invention is as follows. It is preferable to previously perform surface treatment of the electrodes, such as washing with alcohol, pure water, etc., or UV ozone treatment, oxygen plasma treatment, etc., within a range that does not adversely affect the electrodes.
[0133] A hole injection layer is formed on an anode substrate by the above-mentioned method using the charge transport varnish of the present invention. This is introduced into a vacuum deposition apparatus, and a hole transport layer, a light emitting layer, an electron transport layer / hole blocking layer, an electron injection layer, and a cathode metal are sequentially deposited. Alternatively, instead of forming the hole transport layer and the light emitting layer by deposition in the method, these layers are formed by a wet process using a hole transport layer forming composition containing a hole transport polymer and a light emitting layer forming composition containing a light emitting polymer. If necessary, an electron blocking layer may be provided between the light emitting layer and the hole transport layer.
[0134] The anode material may be a transparent electrode such as indium tin oxide (ITO) or indium zinc oxide (IZO), a metal such as aluminum, or an alloy thereof, and is preferably a metal anode that has been subjected to a planarization process. A polythiophene derivative or a polyaniline derivative having high charge transportability may also be used. Other metals that constitute the metal anode include, but are not limited to, gold, silver, copper, indium, and alloys thereof.
[0135] Examples of materials for forming the hole transport layer include triarylamines such as (triphenylamine) dimer derivatives, [(triphenylamine) dimer] spiro dimer, N,N'-bis(naphthalen-1-yl)-N,N'-bis(phenyl)-benzidine (α-NPD), 4,4',4''-tris[3-methylphenyl(phenyl)amino]triphenylamine (m-MTDATA), and 4,4',4''-tris[1-naphthyl(phenyl)amino]triphenylamine (1-TNATA), and oligothiophenes such as 5,5''-bis-{4-[bis(4-methylphenyl)amino]phenyl}-2,2':5',2''-terthiophene (BMA-3T).
[0136] Materials for forming the light-emitting layer include, but are not limited to, low molecular weight light-emitting materials such as metal complexes such as aluminum complexes of 8-hydroxyquinoline, metal complexes of 10-hydroxybenzo[h]quinoline, bisstyrylbenzene derivatives, bisstyrylarylene derivatives, metal complexes of (2-hydroxyphenyl)benzothiazole, and silole derivatives; and systems in which a light-emitting material and an electron transfer material are mixed with a polymer compound such as poly(p-phenylenevinylene), poly[2-methoxy-5-(2-ethylhexyloxy)-1,4-phenylenevinylene], poly(3-alkylthiophene), or polyvinylcarbazole.
[0137] In addition, when forming a light-emitting layer by vapor deposition, it may be co-deposited with a light-emitting dopant. Examples of the light-emitting dopant include, but are not limited to, metal complexes such as tris(2-phenylpyridine)iridium(III) (Ir(ppy)3), naphthacene derivatives such as rubrene, quinacridone derivatives, and condensed polycyclic aromatic rings such as perylene.
[0138] Examples of materials for forming the electron transport layer / hole block layer include, but are not limited to, oxydiazole derivatives, triazole derivatives, phenanthroline derivatives, phenylquinoxaline derivatives, benzimidazole derivatives, and pyrimidine derivatives.
[0139] Materials for forming the electron injection layer include, but are not limited to, metal oxides such as lithium oxide (Li2O), magnesium oxide (MgO), and alumina (Al2O3), and metal fluorides such as lithium fluoride (LiF) and sodium fluoride (NaF).
[0140] The cathode material includes, but is not limited to, aluminum, magnesium-silver alloy, aluminum-lithium alloy, and the like.
[0141] Examples of materials for forming the electron blocking layer include, but are not limited to, tris(phenylpyrazole)iridium.
[0142] Examples of the hole transporting polymer include poly[(9,9-dihexylfluorenyl-2,7-diyl)-co-(N,N'-bis{p-butylphenyl}-1,4-diaminophenylene)], poly[(9,9-dioctylfluorenyl-2,7-diyl)-co-(N,N'-bis{p-butylphenyl}-1,1'-biphenylene-4,4-diamine)], poly[(9,9-bis{1'-penten-5'-yl}fluorenyl-2,7-diyl)-co-(N,N'-bis{p-butylphenyl}-1,4-diaminophenylene)], and poly[N,N'-bis(4-butylphenyl)-N,N'-bis(phenyl)-benzidine]-endcapped with Examples thereof include polysilsesquioxane and poly[(9,9-dioctylfluorenyl-2,7-diyl)-co-(4,4'-(N-(p-butylphenyl))diphenylamine)].
[0143] Examples of the light-emitting polymer include polyfluorene derivatives such as poly(9,9-dialkylfluorene) (PDAF), polyphenylenevinylene derivatives such as poly(2-methoxy-5-(2'-ethylhexoxy)-1,4-phenylenevinylene) (MEH-PPV), polythiophene derivatives such as poly(3-alkylthiophene) (PAT), and polyvinylcarbazole (PVCz).
[0144] The materials constituting the anode, cathode and layers formed therebetween differ depending on whether an element having a bottom emission structure or a top emission structure is manufactured, and appropriate materials are selected taking this into consideration.
[0145] Typically, in bottom emission devices, a transparent anode is used on the substrate side and light is extracted from the substrate side, whereas in top emission devices, a reflective anode made of metal is used and light is extracted from the transparent electrode (cathode) side opposite the substrate. Therefore, for example, in terms of anode materials, transparent anodes such as ITO are used when manufacturing bottom emission devices, and reflective anodes such as Al / Nd are used when manufacturing top emission devices.
[0146] The organic EL element of the present invention may be sealed, if necessary, with a moisture scavenger or the like in accordance with a standard method in order to prevent deterioration of the characteristics.
[0147] As described above, the charge transport varnish of the present invention is suitably used for forming a functional layer of an organic EL device, but it can also be used for forming functional layers in electronic devices such as organic photoelectric conversion devices, organic thin-film solar cells, organic perovskite photoelectric conversion devices, organic integrated circuits, organic field-effect transistors, organic thin-film transistors, organic light-emitting transistors, organic optical inspectors, organic photoreceptors, organic field quenching devices, light-emitting electrochemical cells, quantum dot light-emitting diodes, quantum lasers, organic laser diodes, and organic plasmon light-emitting devices. EXAMPLES
[0148] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples. The apparatus used is as follows. (1) 1 H-NMR: AVANCE III HD 500MHz nuclear magnetic resonance spectrometer, manufactured by Bruker Biospin Corporation (2) Substrate cleaning: Substrate cleaning equipment (low pressure plasma method) manufactured by Choshu Sangyo Co., Ltd. (3) Coating of varnish: Spin coater MS-A100, manufactured by Mikasa Co., Ltd. (4) Film thickness measurement: Kosaka Laboratory Co., Ltd., micro shape measuring instrument Surfcorder ET-4000 (5) Preparation of EL elements: Multi-function deposition system C-E2L1G1-N manufactured by Choshu Sangyo Co., Ltd. (6) Measurement of luminance of EL elements: Multi-channel IVL measuring device manufactured by EHC Corporation (7) EL element lifetime measurement (luminance half-life measurement): EHC Corporation, Organic EL luminance lifetime evaluation system PEL-105S (8) Measurement of refractive index and extinction coefficient: Multi-angle spectroscopic ellipsometer VASE manufactured by J.A. Woollam Japan
[0149] [1] Synthesis of compounds [Synthesis Example 1] Synthesis of intermediate A [ka]
[0150] The synthesis was carried out according to the method described in J. Mater. Chem. C, 2014, pp. 1068-1075, to obtain intermediate A (2,7-dibromo-9,9-bis(4-nitrophenyl)-9H-fluorene).
[0151] [Example 1-1] Synthesis of fluorene derivative A [Example 1-1-1] Synthesis of intermediate B [ka]
[0152] The synthesis was carried out according to the method described in WO 2017 / 122649 to obtain intermediate B (4,4'-(9,9-bis(4-nitrophenyl)-9H-fluorene-2,7-diyl)bis(N,N-diphenylaniline)).
[0153] [Example 1-1-2] Synthesis of intermediate C [ka]
[0154] The synthesis was carried out according to the method described in WO 2017 / 122649 to obtain intermediate C (4,4'-(9,9-bis(4-aminophenyl)-9H-fluorene-2,7-diyl)bis(N,N-diphenylamine)).
[0155] [Example 1-1-3] Synthesis of fluorene derivative A [ka]
[0156] Intermediate C (1 g, 1.2 mmol), THF (2 mL), and trimethylamine (368 μL, 2.64 mmol) were placed in a reaction vessel and replaced with nitrogen. Then, 1-naphthoyl chloride (396 μL, 2.6 mmol) was added dropwise while cooling in an ice bath. After the dropwise addition, the mixture was stirred at room temperature for 1 hour. Ion-exchanged water (25 mL) was added to the reaction mixture, and the mixture was extracted with ethyl acetate (25 mL). The extraction operation was performed three times. The organic layer was dried over anhydrous magnesium sulfate, and the solvent was distilled off under reduced pressure. The concentrated liquid was added dropwise to 2-propanol (20 mL), and the suspension was stirred at room temperature. Filtration was performed and the residue was dried to obtain 1.16 g of the target fluorene derivative A (N,N'-(2,7-bis(4-(diphenylamino)phenyl-9H-fluorene-9,9-diyl)bis(4,1-phenylene))bis(1-naphthamide)) (yield: 85%). 1 The results of H-NMR are shown below. 1 H-NMR(500MHz, DMSO-d6) δ[ppm]: 7.05-7.07(m, 16H), 7.26-7.33(m, 12H), 7.56-7.60(m, 10H), 7.62-7.74(m, 10H), 7.99-8.06(m, 6H), 8.13-8.15(m, 2H), 10.58(brs, 2H).
[0157] [Example 1-2] Synthesis of fluorene derivative B Except for using benzoyl chloride (304 μL, 2.64 mmol) instead of 1-naphthoyl chloride, the same method as in Example 1-1-3 was used to obtain 1.07 g of the target fluorene derivative B (N,N'-(2,7-bis(4-(diphenylamino)phenyl-9H-fluorene-9,9-diyl)bis(4,1-phenylene))bisbenzamide) (yield: 85%). 1 The results of H-NMR are shown below. 1 H-NMR(500MHz, DMSO-d6) δ[ppm]: 7.03-7.07(m, 16H), 7.24(d, J=8.5Hz, 4H), 7.29-7.33(m, 8H), 7.49-7.52(m, 4H), 7.55-7.61(m, 6H), 7.69-7.73(m, 8H), 7.90(dd, J=1.5Hz, 8.5Hz, 4H), 8.20(d, J=7.5Hz, 2H), 10.24(brs, 2H). [ka]
[0158] [Example 1-3] Synthesis of fluorene derivative C [Example 1-3-1] Synthesis of intermediate D [ka]
[0159] The synthesis was carried out according to the method described in WO 2017 / 122649 to give intermediate D (3,3′-(9,9-bis(4-nitrophenyl)-9H-fluorene-2,7-diyl)bis(9-phenyl-9H-carbazole)).
[0160] [Example 1-3-2] Synthesis of intermediate E [ka]
[0161] The synthesis was carried out according to the method described in WO 2017 / 122649 to obtain intermediate E (4,4'-(2,7-bis(9-phenyl-9H-carbazol-3-yl)-9H-fluorene-9,9-diyl)dianiline).
[0162] [Example 1-3-3] Synthesis of fluorene derivative C [ka]
[0163] The same method as in Example 1-1-3 was used except that intermediate E (1.13 g, 1.36 mmol) was used instead of intermediate C, and 1.46 g of the target fluorene derivative C (N,N'-((2,7-bis(9-phenyl-9H-carbazol-3-yl)-9H-fluorene-9,9-diyl)bis(4,1-phenylene))bis(1-naphthamide)) was obtained (yield: 94%). 1 The results of H-NMR are shown below. 1 H-NMR(500MHz, DMSO-d6) δ[ppm]: 7.32(t, J=7.0Hz, 2H), 7.39-7.41(m, 6H), 7.46(t, J=7.5Hz, 4H), 7.54-7.58(m, 8H), 7.65-7.72(m, 10H), 7.78-7.80(m, 6H), 7.91-7.99(m, 6H), 8.04 (d, J=8.5Hz, 2H), 8.12-8.15(m, 4H), 8.41 (d, J=8.0Hz, 2H), 8.65(s, 2H), 10.59(brs, 2H).
[0164] [Example 1-4] Synthesis of fluorene derivative D [Example 1-4-1] Synthesis of intermediate F [ka]
[0165] In a reaction vessel, intermediate A (0.57 g, 1 mmol), 9-phenylcarbazole-2-boronic acid (0.63 g, 2.2 mmol), potassium carbonate (0.55 g, 4 mmol), 1,4-dioxane (11 mL), ion-exchanged water (2.8 mL), and Pd(PPh3)4 (57.8 mg, 0.05 mmol) were placed, and the atmosphere was replaced with nitrogen, followed by stirring at 90°C for 3 hours. After cooling to room temperature, ion-exchanged water (8.4 mL) was added to the reaction mixture, which was then filtered, and the residue was washed with ion-exchanged water (11 mL). Washing was performed twice. 1,4-dioxane (5.6 g) was added to the residue, followed by stirring at 90°C for 1 hour. After cooling to room temperature, filtration was performed, and the filter cake was washed with 1,4-dioxane (5.6 g) to obtain 0.68 g of the desired intermediate F (2,2'-(9,9-bis(4-nitrophenyl)-9H-fluorene-2,7-diyl)bis(9-phenyl-9H-carbazole)) (yield: 76%).
[0166] [Example 1-4-2] Synthesis of intermediate G [ka]
[0167] Intermediate F (3 g, 3.3 mmol), DMF (60 mL) and 5% Pd / C (0.3 g) were placed in a reaction vessel, and after hydrogen replacement, the mixture was stirred at room temperature for 48 hours. After nitrogen replacement, the mixture was filtered through Celite and washed with DMF (30 mL). The filtrate was distilled under reduced pressure, and the concentrated liquid was added dropwise to ethyl acetate (20 mL), and the suspension was stirred at room temperature. Filtration was performed, and the residue was dried to obtain 2.10 g of the desired intermediate G (4,4'-(2,7-bis(9-phenyl-9H-carbazol-2-yl)-9H-fluorene-9,9-diyl)dianiline) (yield: 77%).
[0168] [Example 1-4-3] Synthesis of fluorene derivative D [ka]
[0169] Except for using intermediate G (0.9 g, 1.08 mmol) instead of intermediate A and using benzoyl chloride (274 μL, 2.38 mmol) instead of 1-naphthoyl chloride, the same method as in Example 1-1-3 was used to obtain 0.86 g of the desired fluorene derivative D (N,N'-((2,7-bis(9-phenyl-9H-carbazol-2-yl)-9H-fluorene-9,9-diyl)bis(4,1-phenylene))bisbenzamide) (yield: 69%). 1 The results of H-NMR are shown below. 1 H-NMR(500MHz, DMSO-d6) δ[ppm]: 7.26-7.32(m, 6H), 7.40-7.42(m, 4H), 7.43-7.59(m, 12H), 7.68-7.77(m, 16H), 7.93-7.94(m, 4H), 8.04 (d, J=7.5Hz, 2H), 8.27 (d, J=7.5Hz, 2H), 8.32(d, J=8.0Hz, 2H), 10.26(brs, 2H).
[0170] [Example 1-5] Synthesis of fluorene derivative E [ka]
[0171] Except for using 2-thenoyl chloride (280 μL, 2.64 mmol) instead of 1-naphthoyl chloride, the same method as in Example 1-1-3 was used to obtain 1.02 g of the target fluorene derivative E (N,N'-(2,7-bis(4-(diphenylamino)phenyl-9H-fluorene-9,9-diyl)bis(4,1-phenylene))bis(thiophene-2-carboxamide)) (yield: 80%). 1 The results of H-NMR are shown below. 1H-NMR(500MHz, DMSO-d6) δ[ppm]: 7.02-7.07(m, 16H), 7.20(dd, J=4Hz, 4.5Hz, 2H), 7.23(d, J=9.0Hz, 4H), 7.30-7.33(m, 8H), 7.60(d, J=8.5Hz, 4H), 7.64(d, J=8.5Hz, 4H), 7.69(s, 2H), 7.72(d, J=8.0Hz, 2H), 7.83(d, J=5.0Hz, 2H), 7.97(d, J=3.5Hz, 2H), 8.01(d, J=8.5Hz, 2H), 10.21(brs, 2H).
[0172] [Examples 1-6] Synthesis of fluorene derivative F [ka]
[0173] The same method as in Example 1-1-3 was used except that benzo[b]thiophene-2-carbonyl chloride (517 mg, 2.64 mmol) was used instead of 1-naphthoyl chloride, and 1.14 g of the target fluorene derivative F (N,N'-(2,7-bis(4-(diphenylamino)phenyl-9H-fluorene-9,9-diyl)bis(4,1-phenylene))bis(benzo[b]thiophene-2-carboxamide)) was obtained (yield: 83%). 1 The results of H-NMR are shown below. 1 H-NMR(500MHz, DMSO-d6) δ[ppm]: 7.03-7.07(m, 16H), 7.26-7.33(m, 12H), 7.44-7.50(m, 4H), 7.61(d, J=8.5Hz, 4H), 7.69-7.74(m, 8H), 7.99(d, J=7.5Hz, 2H), 8.03(dd, J=6.5Hz, 8.0Hz, 4H), 8.32(s, 2H), 10.51(brs, 2H).
[0174] [2] Preparation of charge-transporting varnish [Example 2-1] Preparation of charge-transporting varnish A1 Fluorene derivative A (174 mg) and arylsulfonic acid ester A (0.189 g) represented by the following formula, which was synthesized according to the method described in WO 2017 / 217455, were dissolved in a mixed solvent of triethylene glycol butyl methyl ether (2 g), butyl benzoate (4 g) and dimethyl phthalate (4 g) by stirring at room temperature. The resulting solution was filtered using a polytetrafluoroethylene (PTFE) filter with a pore size of 0.2 μm to obtain charge transporting varnish A1. [ka]
[0175] [Example 2-2] Preparation of charge-transporting varnish B1 Fluorene derivative B (165 mg) and arylsulfonic acid ester A (0.198 g) were dissolved in a mixed solvent of triethylene glycol butyl methyl ether (2 g), butyl benzoate (4 g) and dimethyl phthalate (4 g) by stirring at room temperature. The resulting solution was filtered using a PTFE filter with a pore size of 0.2 μm to obtain charge transporting varnish B1.
[0176] [Example 2-3] Preparation of charge transport varnish C1 Fluorene derivative C (173 mg) and arylsulfonic acid ester A (0.190 g) were dissolved in a mixed solvent of triethylene glycol butyl methyl ether (2 g), butyl benzoate (4 g) and dimethyl phthalate (4 g) by stirring at room temperature. The resulting solution was filtered using a PTFE filter with a pore size of 0.2 μm to obtain charge transporting varnish C1.
[0177] [Example 2-4] Preparation of charge transport varnish D1 Fluorene derivative D (165 mg) and arylsulfonic acid ester A (0.198 g) were dissolved in a mixed solvent of triethylene glycol butyl methyl ether (2 g), butyl benzoate (4 g) and dimethyl phthalate (4 g) by stirring at room temperature. The resulting solution was filtered using a PTFE filter with a pore size of 0.2 μm to obtain charge transporting varnish D1.
[0178] [Example 2-5] Preparation of charge transport varnish E1 Fluorene derivative E (166 mg) and arylsulfonic acid ester A (0.197 g) were dissolved in a mixed solvent of triethylene glycol butyl methyl ether (2 g), butyl benzoate (4 g) and dimethyl phthalate (4 g) by stirring at room temperature. The resulting solution was filtered using a PTFE filter with a pore size of 0.2 μm to obtain charge transporting varnish E1.
[0179] [Example 2-6] Preparation of charge transport varnish F1 Fluorene derivative F (175 mg) and arylsulfonic acid ester A (0.188 g) were dissolved in a mixed solvent of triethylene glycol butyl methyl ether (2 g), butyl benzoate (4 g) and dimethyl phthalate (4 g) by stirring at room temperature. The resulting solution was filtered using a PTFE filter with a pore size of 0.2 μm to obtain a charge transporting varnish F1.
[0180] [Example 2-7] Preparation of charge transporting varnish A2 Fluorene derivative A (363 mg) was dissolved in a mixed solvent of triethylene glycol butyl methyl ether (2 g), butyl benzoate (4 g) and dimethyl phthalate (4 g) by stirring at room temperature. The resulting solution was filtered using a PTFE filter with a pore size of 0.2 μm to obtain charge transporting varnish A2.
[0181] [Examples 2-8 to 2-12] Preparation of charge-transporting varnishes B2, C2, E2, and F2 Charge-transporting varnishes B2, C2, E2 and F2 were obtained in the same manner as in Example 2-7, except that the fluorene derivative A was changed to the fluorene derivatives B, C, E and F, respectively.
[0182] [3] Evaluation of refractive index (n) and extinction coefficient (k) [Examples 3-1 to 3-5] Charge-transporting varnishes A1, B1, C1, E1 and F1 were each applied to a quartz substrate using a spin coater, and then pre-baked at 120°C for 1 minute in an air atmosphere, and then baked at 200°C for 15 minutes in an air atmosphere to form a uniform thin film of 50 nm on the quartz substrate. Using the obtained quartz substrate with the film, the average refractive index n in the visible range and the average extinction coefficient k in the visible range at wavelengths of 400 to 800 nm were measured. The results are shown in Table 1.
[0183] [Table 1]
[0184] As shown in Table 1, the charge transporting thin film of the present invention had a high refractive index of 1.65 or more and a low extinction coefficient of 0.03 or less.
[0185] [4] Fabrication and characterization of hole-only device (HOD)-1 In the following examples, the ITO substrate used was a 25 mm × 25 mm × 0.7 mm glass substrate with a 150 nm thick ITO pattern on the surface, and prior to use, impurities on the surface were removed using an O2 plasma cleaning device (150 W, 30 seconds).
[0186] [Preparation of hole injection layer solution] 0.137 g of an aniline derivative represented by the following formula (S1) synthesized according to the method described in WO 2013 / 084664 and 0.271 g of an arylsulfonic acid represented by the following formula (S2) synthesized according to the method described in WO 2006 / 025342 were dissolved in 6.7 g of 1,3-dimethyl-2-imidazolidinone under a nitrogen atmosphere. 10 g of cyclohexanol and 3.3 g of propylene glycol were added to the obtained solution in this order and stirred to prepare a hole injection layer solution. [ka]
[0187] [Example 4-1] The hole injection layer solution was applied onto an ITO substrate using a spin coater, and then pre-baked on a hot plate in an air atmosphere at 80°C for 1 minute, and then baked at 230°C for 15 minutes to form a hole injection layer (film thickness 30 nm). Next, charge transport varnish A2 was applied onto the hole injection layer using a spin coater, and the solvent was removed by vacuum drying at room temperature. The film was then baked in an air atmosphere at 130°C for 10 minutes to form a hole transport layer with a film thickness of 40 nm. On top of this, a deposition apparatus (vacuum degree 1.0×10 -5 A hole-only device (HOD) was fabricated by depositing an 80 nm aluminum thin film at 0.2 nm / sec using a 1000 keV laser.
[0188] [Examples 4-2 to 4-5] HOD was prepared in the same manner as in Example 4-1, except that the charge transporting varnish A2 was replaced with the charge transporting varnish B2, C2, E2 or F2.
[0189] For each of the HODs produced in Examples 4-1 to 4-5, the current density was measured at a driving voltage of 4 V. The results are shown in Table 2.
[0190] [Table 2]
[0191] As shown in Table 2, the thin film prepared from the charge-transporting varnish of the present invention exhibited good charge-transporting properties.
[0192] [5] Fabrication of single-layer element (SLD) [Example 5-1] The charge transport varnish A1 was applied onto an ITO substrate using a spin coater, and then pre-baked at 120°C for 1 minute in an air atmosphere, and then baked at 200°C for 15 minutes to form a hole injection layer (film thickness 50 nm). -5 A thin aluminum film with a thickness of 80 nm was formed at a rate of 0.2 nm / sec using a 1000 keV laser (1000 keV) and a single-layer element (SLD) was fabricated.
[0193] [Examples 5-2 to 5-6] An SLD was prepared in the same manner as in Example 5-1, except that charge transporting varnish B1, C1, D1, E1 or F1 was used instead of charge transporting varnish A1.
[0194] For each of the SLDs produced in Examples 5-1 to 5-6, the current density was measured at a driving voltage of 4 V. The results are shown in Table 3.
[0195] [Table 3]
[0196] As shown in Table 3, the thin film prepared from the charge-transporting varnish of the present invention exhibited good charge-transporting properties.
[0197] [6] Preparation and evaluation of HOD-2 [Example 6-1] The charge transport varnish A1 was applied to an ITO substrate using a spin coater, and then pre-baked at 120°C for 1 minute in an air atmosphere, and then baked at 200°C for 15 minutes to form a 50 nm thin film on the ITO substrate. -5 The HOD was fabricated by sequentially depositing thin films of α-NPD and aluminum using a vacuum evaporation method. The deposition rate was 0.2 nm / sec. The thicknesses of the thin films of α-NPD and aluminum were 30 nm and 80 nm, respectively.
[0198] [Examples 6-2 to 6-5] HOD was prepared in the same manner as in Example 6-1, except that charge transporting varnish B1, C1, E1 or F1 was used instead of charge transporting varnish A1.
[0199] The current density was measured for the HODs produced in Examples 6-1 to 6-5 at a driving voltage of 4 V. The results are shown in Table 4.
[0200] [Table 4]
[0201] As shown in Table 4, the thin films prepared from the charge-transporting varnish of the present invention exhibited good charge-transporting properties.
[0202] [7] Preparation and characterization of organic electroluminescence devices [Example 7-1] Charge transporting varnish A1 was applied to an ITO substrate using a spin coater, and then pre-baked in an air atmosphere at 120° C. for 1 minute, and then main-baked at 200° C. for 15 minutes to form a 50 nm thin film on the ITO substrate. Next, the ITO substrate on which the thin film was formed was placed in a deposition device (vacuum degree 1.0×10 -5 A 30 nm film of α-NPD was formed at 0.2 nm / sec using a 1000 sieve vacuum chamber (Pa). Next, a 10 nm film of an electron block material HTEB-01 manufactured by Kanto Chemical Co., Ltd. was formed. Next, an emitting layer host material NS60 manufactured by Nippon Steel & Sumikin Chemical Co., Ltd. and an emitting layer dopant material Ir(ppy)3 were co-deposited. The deposition rate of the co-deposition was controlled so that the concentration of Ir(ppy)3 was 6%, and 40 nm was laminated. Next, thin films of Alq3, lithium fluoride, and aluminum were sequentially laminated to prepare an organic EL device. At this time, the deposition rate was 0.2 nm / sec for Alq3 and aluminum, and 0.02 nm / sec for lithium fluoride, respectively, and the film thicknesses were 20 nm, 0.5 nm, and 80 nm, respectively. In order to prevent deterioration of characteristics due to the influence of oxygen, water, etc. in the air, the organic EL element was sealed with a sealing substrate before evaluating its characteristics. Sealing was performed as follows. In a nitrogen atmosphere with an oxygen concentration of 2 ppm or less and a dew point of -76°C or less, the organic EL element was placed between the sealing substrates, and the sealing substrates were bonded together with an adhesive (MORESCO Moisture Cut WB90US(P) manufactured by MORESCO Corporation). At this time, a moisture scavenger (HD-071010W-40 manufactured by DYNIC Co., Ltd.) was placed inside the sealing substrate together with the organic EL element. The bonded sealing substrates were irradiated with UV light (wavelength: 365 nm, irradiation dose: 6,000 mJ / cm2). 2 ), and then annealed at 80°C for 1 hour to harden the adhesive.
[0203] [Examples 7-2 to 7-5] An organic EL device was prepared in the same manner as in Example 7-1, except that charge transporting varnish B1, C1, E1 or F1 was used instead of charge transporting varnish A1.
[0204] The obtained organic EL device had a luminance of 5,000 cd / m 2 The driving voltage, current density, current efficiency, luminous efficiency, external luminescence quantum yield (EQE), and LT90 (initial luminance 5,000 cd / m 2 The time required for a 10% decrease in the concentration of the saturation gas was measured. The results are shown in Table 5.
[0205] [Table 5]
[0206] As shown in Table 5, all of the organic EL devices of the present invention exhibited high current efficiency and high EQE, and also exhibited good life characteristics.
Claims
1. A fluorene derivative represented by the following formula (1): 【Chemistry 1】 [In the formula, Z 1 and Z 2 are each independently a group represented by any one of the following formulas (2) to (7): 【Chemistry 2】 (In the formula, the dashed lines represent bonds. R A and R B are each independently a hydrogen atom or an alkyl group having 1 to 20 carbon atoms. Ar 1 and Ar 2 each independently represents a phenyl group, a 1-naphthyl group, a 2-naphthyl group, or a group represented by the following formulas (T1-1) to (T11-4); 【Chemistry 3】 【Chemistry 4】 Ar 3 and Ar 4 are each independently a group represented by any one of the following formulas (8) to (11). 【Chemistry 5】 (In the formula, the dashed lines represent bonds, R 1 is a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, or a cyano group, a nitro group, a halogen atom, an aryl group having 6 to 20 carbon atoms which may be substituted with an alkyl group having 1 to 20 carbon atoms or a halogenated alkyl group having 1 to 20 carbon atoms, or a heteroaryl group having 6 to 20 carbon atoms which may be substituted with an alkyl group having 1 to 20 carbon atoms or a halogenated alkyl group having 1 to 20 carbon atoms, or a group represented by any of the following formulas (12) to (14): R 2 ~R 52 each independently represents a hydrogen atom, a cyano group, a nitro group, a halogen atom, an alkyl group having 1 to 20 carbon atoms, or a halogenated alkyl group having 1 to 20 carbon atoms. 【Chemistry 6】 (In the formula, the dashed lines represent bonds, D A is a diarylamino group, each aryl group independently being an aryl group having 6 to 20 carbon atoms, R 53 ~R 76 are each independently a hydrogen atom, a cyano group, a nitro group, a halogen atom, an alkyl group having 1 to 20 carbon atoms, or a halogenated alkyl group having 1 to 20 carbon atoms.
2. Ar 1 and Ar 2 The fluorene derivative according to claim 1, wherein are the same group.
3. Z 1 and Z 2 The fluorene derivative according to claim 1 or 2, wherein is a group represented by formula (2):
4. R 1 The fluorene derivative according to any one of claims 1 to 3, wherein is a phenyl group.
5. R 2 ~R 76 The fluorene derivative according to any one of claims 1 to 4, wherein is a hydrogen atom.
6. A charge transporting material comprising the fluorene derivative according to any one of claims 1 to 5.
7. A charge transporting varnish comprising the charge transporting substance according to claim 6 and an organic solvent.
8. 8. The charge transporting varnish according to claim 7, further comprising a dopant.
9. A charge transporting thin film obtained from the charge transporting varnish according to claim 7 or 8.
10. An organic electroluminescence device comprising the charge transporting thin film according to claim 9.
11. The organic electroluminescence device according to claim 10, wherein the charge transporting thin film is a hole injection layer or a hole transport layer.
12. A step of reacting a compound represented by formula (15) with a compound represented by formula (16-1) and a compound represented by formula (16-2) to obtain an intermediate represented by formula (17); reducing the intermediate of formula (17) to obtain an intermediate of formula (18); and A step of reacting the intermediate represented by formula (18) with a halide represented by formula (19-1) and a halide represented by formula (19-2). A method for producing a fluorene derivative represented by the following formula (1): 【Chemistry 7】 [In the formula, Z 1 and Z 2 are each independently a group represented by any one of the following formulas (2) to (7): 【Chemistry 8】 (In the formula, the dashed lines represent bonds. R A and R B are each independently a hydrogen atom or an alkyl group having 1 to 20 carbon atoms. Ar 1 and Ar 2 each independently represents a phenyl group, a 1-naphthyl group, a 2-naphthyl group, or a group represented by the following formulas (T1-1) to (T11-4); 【Chemistry 9】 【Chemistry 10】 Ar 3 and Ar 4 are each independently a group represented by any one of the following formulas (8) to (11): 【Chemistry 11】 (In the formula, the dashed lines represent bonds, R 1 is a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, or a cyano group, a nitro group, a halogen atom, an aryl group having 6 to 20 carbon atoms which may be substituted with an alkyl group having 1 to 20 carbon atoms or a halogenated alkyl group having 1 to 20 carbon atoms, or a heteroaryl group having 6 to 20 carbon atoms which may be substituted with an alkyl group having 1 to 20 carbon atoms or a halogenated alkyl group having 1 to 20 carbon atoms, or a group represented by any of the following formulas (12) to (14): R 2 ~R 52 each independently represents a hydrogen atom, a cyano group, a nitro group, a halogen atom, an alkyl group having 1 to 20 carbon atoms, or a halogenated alkyl group having 1 to 20 carbon atoms. 【Chemistry 12】 (In the formula, the dashed lines represent bonds, D A is a diarylamino group, each aryl group independently being an aryl group having 6 to 20 carbon atoms, R 53 ~R 76 are each independently a hydrogen atom, a cyano group, a nitro group, a halogen atom, an alkyl group having 1 to 20 carbon atoms, or a halogenated alkyl group having 1 to 20 carbon atoms. X is a halogen atom or a pseudohalogen group.
Citation Information
Patent Citations
Electronic devices containing organic semiconductors
JP2007536718A
Organic Light Emitting Display Device and Top Emission Type OLED Device with Improved Viewing Angle Characteristics
JP2017501585A
Charge-transporting varnish
WO2013042623A1
Charge-transporting varnish and organic electroluminescent element
WO2016204079A1
Fluorine atom-containing compound and use thereof
WO2017122649A1
