Polyimide resin composition, polyimide varnish and polyimide film
A polyimide resin composition with specific structural units and a crosslinking agent addresses the challenges of peeling polyimide films from substrates, ensuring high transparency, isotropy, and peelability, while maintaining excellent mechanical and thermal properties for use in image display devices.
Patent Information
- Application Number
- JP2021551705
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-10-11
- Filing Date
- 2020-10-08
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2040-10-08
AI Technical Summary
Existing methods for peeling polyimide films from substrates, such as glass or silicon, often damage the resin substrate, require expensive laser devices, limit the combination of release layers, are complex, and result in deteriorated optical properties like colorless transparency and optical isotropy due to the use of phenylenediamine-based polyimides.
A polyimide resin composition containing specific structural units and a crosslinking agent with oxazolyl groups, such as 1,3-bis(4,5-dihydro-2-oxazolyl)benzene, is used to form a film that maintains high colorless transparency and optical isotropy while ensuring easy and stable peeling from substrates.
The film exhibits excellent colorless transparency, optical isotropy, and peelability from substrates, with improved heat resistance and mechanical properties, making it suitable for use in image display devices like liquid crystal displays and OLED displays.
Smart Images

Figure 0007593325000001 
Figure 0007593325000002 
Figure 0007593325000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyimide resin composition, a polyimide varnish, and a polyimide film. [Background technology]
[0002] Various applications of polyimide resins are being considered in the fields of electric and electronic components, etc. For example, it is desirable to replace glass substrates used in image display devices such as liquid crystal displays and OLED displays with plastic substrates in order to make the devices lighter and more flexible, and research is being conducted on polyimide films suitable for such plastic substrates. In an image display device, when light emitted from a display element is emitted through a plastic substrate, the plastic substrate is required to be colorless and transparent. Furthermore, when light passes through a retardation film or a polarizing plate (for example, a liquid crystal display, a touch panel, etc.), in addition to colorless transparency, the substrate is also required to have high optical isotropy (i.e., low Rth).
[0003] When a polyimide film is used as a substrate, the desired electronic circuit is formed on the polyimide film through various processes such as a sputtering process and an etching process for forming an oxide semiconductor film such as an indium tin oxide (ITO) film depending on the application. When forming the desired electronic circuit on the polyimide film, it is necessary to ensure the flatness of the polyimide film. For this purpose, the polyimide film is adhered to a hard support such as a glass plate, and is obtained by peeling it off from the support after cooling.
[0004] Known methods for adhering a polyimide film to a support include adding an adhesive to the polyimide itself, and interposing a layer called a release layer between the polyimide film and the support to ensure adhesion during processing.
[0005] As a method for peeling off a polyimide film from a support, for example, the following method is known. (1) A method in which a structure containing a polyimide resin / support is obtained, and then a laser is irradiated from the support side to ablate the polyimide resin interface, thereby peeling off the polyimide resin (see, for example, Patent Document 1). Types of laser include solid (YAG) lasers and gas (UV excimer) lasers, and a spectrum of 308 nm or the like is used. (2) A method in which a release layer is formed on the support before the resin composition is applied to the support, and then a structure including a polyimide resin film / release layer / support is obtained, and the polyimide resin film is mechanically peeled off (see, for example, Patent Document 2). Examples of the release layer include a method using Parylene (registered trademark, manufactured by Nippon Parylene LLC) or tungsten oxide, and a method using a vegetable oil-based, silicone-based, fluorine-based, or alkyd-based release agent. Laser irradiation as described in (1) above may also be used in combination.
[0006] Patent Document 3 discloses a method for fixing a resin substrate to a support substrate via an adhesive layer, forming an electronic element on the resin substrate, and peeling an electronic device including the electronic element and the resin substrate from the support substrate, in which an adhesive layer containing a material whose adhesive strength with the support substrate decreases upon contact with moisture is used as a main component. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Special Publication No. 2007-512568 [Patent Document 2] JP 2010-067957 A [Patent Document 3] JP 2016-021384 A Summary of the Invention [Problem to be solved by the invention]
[0008] The method (1) above requires an expensive laser irradiation device, and the resin substrate formed on the base may be damaged during laser irradiation.The method (2) above may be limited in the combination of the release layer and the type of polyimide in order to exhibit performance. In the method of Patent Document 3, when forming an electronic element, it was necessary to form a sealing layer to seal the exposed portion of the adhesive layer in order to prevent the adhesive layer from coming into contact with moisture so as not to reduce the adhesive strength. On the other hand, when peeling off the electronic device after forming the electronic element, it was necessary to remove the sealing layer before peeling off in order to bring moisture into contact with the adhesive layer. Therefore, the method of Patent Document 3 was a complicated process overall. Furthermore, it was necessary to place the device in a high humidity environment of 90% or more in order to contact moisture, and there was a problem that it was difficult to control the moisture content and ensure stable peelability. Furthermore, the polyimide used in Patent Document 3 was prone to coloring because it used phenylenediamine with strong intramolecular charge transfer interaction, and therefore had low transparency, and also had a structure in which polymer molecules were easily arranged, so it had low optical isotropy. As described above, the above-mentioned methods tend to deteriorate the optical properties of the film, such as colorless transparency and optical isotropy, due to damage, the addition of a release layer, and the properties of the polymer, and also to deteriorate the yield.
[0009] Thus, there has been a demand for a polyimide resin that can easily and stably peel a polyimide film from a glass substrate or a silicon substrate while maintaining the optical properties, such as high colorless transparency and optical isotropy, of the resulting polyimide film. Therefore, an object of the present invention is to provide a polyimide resin composition capable of forming a film which is excellent in colorless transparency and optical isotropy and further in peelability from a substrate, and a polyimide varnish and a polyimide film each containing the polyimide resin composition. [Means for solving the problem]
[0010] The present inventors have found that the above-mentioned problems can be solved by a polyimide resin composition containing a polyimide resin having a specific combination of structural units and a specific crosslinking agent, and have completed the invention.
[0011] That is, the present invention provides the following <1> ~ <11> Regarding. <1> A polyimide resin composition comprising a polyimide resin and a crosslinking agent having at least two oxazolyl groups, the polyimide resin being a polyimide resin having a structural unit A derived from a tetracarboxylic dianhydride and a structural unit B derived from a diamine, the structural unit B comprising a structural unit (B-1) derived from a diamine having a sulfonyl group in its structure, and a structural unit (B-2) derived from a compound represented by the following formula (b-2): [ka] (In formula (b-2), X is a single bond, a substituted or unsubstituted alkylene group, a carbonyl group, an ether group, a group represented by the following formula (b-2-i), or a group represented by the following formula (b-2-ii); p is an integer of 0 to 2, m1 is an integer of 0 to 4, and m2 is an integer of 0 to 4. However, when p is 0, m1 is an integer of 1 to 4.) [ka] (In formula (b-2-i), m3 is an integer of 0 to 5; in formula (b-2-ii), m4 is an integer of 0 to 5. Note that m1+m2+m3+m4 is 1 or more, and when p is 2, each of the two Xs and the two m2 to m4 is independently selected.) <2> The structural unit (B-2) is a structural unit (B-21) derived from a compound represented by the following formula (b-21): <1> The polyimide resin composition according to claim 1 . [ka] <3> The structural unit (B-1) is at least one selected from the group consisting of a structural unit (B-11) derived from a compound represented by the following formula (b-11), a structural unit (B-12) derived from a compound represented by the following formula (b-12), and a structural unit (B-13) derived from a compound represented by the following formula (b-13): <1> or <2> The polyimide resin composition according to claim 1 . [ka] <4> The structural unit A includes at least one selected from the group consisting of a structural unit (A-1) derived from a compound represented by the following formula (a-1) and a structural unit (A-2) derived from a compound represented by the following formula (a-2): <1> ~ <3> 10. The polyimide resin composition according to claim 9, [ka] <5> The structural unit B further contains a structural unit (B-3) derived from a compound represented by the following formula (b-3): <1> ~ <4> 10. The polyimide resin composition according to claim 9, [ka] (In formula (b-3), Z 1 and Z 2 each independently represents a divalent aliphatic group or a divalent aromatic group which may contain an oxygen atom; R 1 and R 2 each independently represents a monovalent aromatic group or a monovalent aliphatic group; R 3 and R 4 each independently represents a monovalent aliphatic group; R 5 and R 6 each independently represents a monovalent aliphatic group or a monovalent aromatic group, m and n each independently represent an integer of 1 or more, and the sum of m and n represents an integer of 2 to 1000. 1 and R 2 At least one of represents a monovalent aromatic group. <6> The structural unit B further contains a structural unit (B-4) derived from a compound represented by the following formula (b-4): <1> ~ <5> 10. The polyimide resin composition according to claim 9, [ka] <7> The crosslinking agent is a compound containing an aromatic ring or an aromatic heterocycle to which at least two oxazolyl groups are bonded. <1> ~ <6> 10. The polyimide resin composition according to claim 9, <8> The crosslinking agent is a compound containing a benzene ring to which at least two oxazolyl groups are bonded. <1> ~ <7> 10. The polyimide resin composition according to claim 9, <9> The above, wherein the crosslinking agent is 1,3-bis(4,5-dihydro-2-oxazolyl)benzene. <1> ~ <8> 10. The polyimide resin composition according to claim 9, <10> the above <1> ~ <9> 2. A polyimide varnish obtained by dissolving the polyimide resin composition according to any one of claims 1 to 11 in an organic solvent. <11> the above <1> ~ <9> 2. A polyimide film, comprising the polyimide resin in the polyimide resin composition according to claim 1, crosslinked by the crosslinking agent. Effect of the Invention
[0012] According to the present invention, a film can be formed which is excellent in colorless transparency and optical isotropy, and further has excellent releasability from a substrate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] [Polyimide resin composition] The polyimide resin composition of the present invention contains a polyimide resin and a crosslinking agent. The polyimide resin and the crosslinking agent in the present invention will be described below. Incidentally, the reason why the polyimide resin composition of the present invention has excellent releasability while maintaining optical properties such as colorless transparency and optical isotropy is not clear; however, it is believed that the bent polymer molecular structure derived from the diamine monomer having a sulfonyl group in the main chain inhibits stacking between imides, resulting in excellent optical properties such as optical isotropy and reduced residual stress in the resulting polyimide film, which in turn results in excellent releasability.
[0014] <Polyimide resin> The polyimide resin contained in the polyimide resin composition of the present invention has a structural unit A derived from a tetracarboxylic dianhydride and a structural unit B derived from a diamine, and the structural unit B contains a structural unit (B-1) derived from a diamine having a sulfonyl group in its structure and a structural unit (B-2) derived from a compound represented by the following formula (b-2). [ka] (In formula (b-2), X is a single bond, a substituted or unsubstituted alkylene group, a carbonyl group, an ether group, a group represented by the following formula (b-2-i), or a group represented by the following formula (b-2-ii); p is an integer of 0 to 2, m1 is an integer of 0 to 4, and m2 is an integer of 0 to 4. However, when p is 0, m1 is an integer of 1 to 4.) [ka] (In formula (b-2-i), m3 is an integer of 0 to 5; in formula (b-2-ii), m4 is an integer of 0 to 5. Note that m1+m2+m3+m4 is 1 or more, and when p is 2, each of the two Xs and the two m2 to m4 is independently selected.)
[0015] (Structural unit A) The structural unit A is a structural unit derived from a tetracarboxylic dianhydride contained in the polyimide resin. The structural unit A preferably contains at least one selected from the group consisting of structural unit (A-1) derived from a compound represented by the following formula (a-1) and structural unit (A-2) derived from a compound represented by the following formula (a-2), and more preferably contains structural unit (A-2). By containing structural unit (A-2), it is possible to improve colorless transparency and optical isotropy, and also to reduce residual stress. On the other hand, particularly from the standpoint of colorless transparency and heat resistance, it is more preferable that the structural unit (A-1) is contained. [ka]
[0016] The compound represented by formula (a-1) is norbornane-2-spiro-α-cyclopentanone-α'-spiro-2″-norbornane-5,5″,6,6″-tetracarboxylic dianhydride. When the structural unit A contains the structural unit (A-1), the colorless transparency and heat resistance of the film can be improved.
[0017] The ratio of the structural unit (A-1) in the structural unit A is preferably 40 mol% or more, more preferably 50 mol% or more, and even more preferably 60 mol% or more. The upper limit of the ratio of the structural unit (A-1) is not particularly limited, that is, it is 100 mol%. The structural unit A may be composed of only the structural unit (A-1).
[0018] The compound represented by formula (a-2) is 1,2,4,5-cyclohexanetetracarboxylic dianhydride. By including the structural unit (A-2) in the structural unit A, the colorless transparency and optical isotropy of the film can be improved, and the residual stress can also be reduced.
[0019] The ratio of the structural unit (A-2) in the structural unit A is preferably 50 mol% or more, more preferably 70 mol% or more, and even more preferably 85 mol% or more. The upper limit of the ratio of the structural unit (A-2) is not particularly limited, that is, it is 100 mol%. The structural unit A may be composed of only the structural unit (A-2).
[0020] When the structural unit A contains the structural unit (A-1) and the structural unit (A-2), the total ratio of the structural units (A-1) and (A-2) in the structural unit A is preferably 50 mol% or more, more preferably 70 mol% or more, even more preferably 90 mol% or more, and particularly preferably 99 mol% or more. The upper limit of the total ratio of the structural units (A-1) and (A-2) is not particularly limited, that is, it is 100 mol%. The structural unit A may be composed of only the structural unit (A-1) and the structural unit (A-2).
[0021] The structural unit A may contain structural units other than the structural units (A-1) and (A-2). In addition to the structural units (A-1) and (A-2), the structural unit A may contain a structural unit (A-3) derived from a silicone modified with acid anhydrides at both ends. The silicone modified with acid anhydrides at both ends is preferably a compound represented by the following formula (a-3). [ka] (In formula (a-3), R 31 ~R 36 are each independently a monovalent hydrocarbon group having 1 to 20 carbon atoms, L 31 and L 32 each independently represents a single bond or a divalent hydrocarbon group having 1 to 20 carbon atoms, Z 31 and Z 32 are each independently a trivalent hydrocarbon group having 1 to 20 carbon atoms, n3 is 1 to 200.
[0022] R in formula (a-3) 31 ~R 36 are each independently a monovalent hydrocarbon group having 1 to 20 carbon atoms. Examples of monovalent hydrocarbon groups having 1 to 20 carbon atoms include alkyl groups having 1 to 20 carbon atoms, cycloalkyl groups having 3 to 20 carbon atoms, aryl groups having 6 to 20 carbon atoms, aralkyl groups having 7 to 20 carbon atoms, and alkenyl groups having 2 to 20 carbon atoms. The alkyl group having 1 to 20 carbon atoms is preferably an alkyl group having 1 to 10 carbon atoms, and examples thereof include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a t-butyl group, a pentyl group, and a hexyl group. The cycloalkyl group having 3 to 20 carbon atoms is preferably a cycloalkyl group having 3 to 10 carbon atoms, and examples thereof include a cyclopentyl group and a cyclohexyl group. The aryl group having 6 to 20 carbon atoms is preferably an aryl group having 6 to 10 carbon atoms, and examples thereof include a phenyl group and a naphthyl group. The aralkyl group having 7 to 20 carbon atoms is preferably an aralkyl group having 7 to 10 carbon atoms, and examples thereof include a benzyl group and a phenethyl group. The alkenyl group having 2 to 20 carbon atoms is preferably an alkenyl group having 2 to 10 carbon atoms, and examples thereof include a vinyl group, an allyl group, a propenyl group, an isopropenyl group, and a butenyl group.
[0023] R in formula (a-3) 31 ~R 36 are each independently preferably selected from the group consisting of an alkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 3 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, and an alkenyl group having 2 to 20 carbon atoms; more preferably selected from the group consisting of an alkyl group having 1 to 10 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, an aralkyl group having 7 to 10 carbon atoms, and an alkenyl group having 2 to 10 carbon atoms; and even more preferably selected from the group consisting of an alkyl group having 1 to 10 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, an aralkyl group having 7 to 10 carbon atoms, and an alkenyl group having 2 to 10 carbon atoms. is preferably selected from the group consisting of a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a t-butyl group, a pentyl group, a hexyl group, a phenyl group, a naphthyl group, a vinyl group, an allyl group, a propenyl group, an isopropenyl group, and a butenyl group; and is most preferably selected from the group consisting of a methyl group, an ethyl group, a phenyl group, and a vinyl group.
[0024] L in formula (a-3) 31 and L 32 are each independently a single bond or a divalent hydrocarbon group having 1 to 20 carbon atoms. Examples of the divalent hydrocarbon group having 1 to 20 carbon atoms include an alkylene group having 1 to 20 carbon atoms, a cycloalkylene group having 3 to 20 carbon atoms, and an arylene group having 6 to 20 carbon atoms. As the alkylene group having 1 to 20 carbon atoms, an alkylene group having 1 to 10 carbon atoms is preferable, and examples thereof include a methylene group, an ethylene group, a propylene group, a butylene group, a pentylene group, and a hexylene group. The cycloalkylene group having 3 to 20 carbon atoms is preferably a cycloalkylene group having 3 to 10 carbon atoms, and examples thereof include a cyclobutylene group, a cyclopentylene group, a cyclohexylene group, and a cycloheptylene group. As the arylene group having 6 to 20 carbon atoms, an arylene group having 6 to 10 carbon atoms is preferable, and examples thereof include a phenylene group and a naphthylene group.
[0025] L 31 and L 32 are each independently preferably selected from the group consisting of a single bond, an alkylene group having 1 to 20 carbon atoms, a cycloalkylene group having 3 to 20 carbon atoms, and an arylene group having 6 to 20 carbon atoms; more preferably selected from the group consisting of a single bond, an alkylene group having 1 to 10 carbon atoms, a cycloalkylene group having 3 to 10 carbon atoms, and an arylene group having 6 to 10 carbon atoms; still more preferably selected from the group consisting of a single bond, an alkylene group having 1 to 10 carbon atoms, and an arylene group having 6 to 10 carbon atoms; particularly preferably selected from the group consisting of a single bond, a methylene group, an ethylene group, a propylene group, a butylene group, a pentylene group, a hexylene group, a phenylene group, and a naphthylene group; and most preferably selected from the group consisting of a single bond, a methylene group, an ethylene group, a propylene group, and a phenylene group.
[0026] Z in formula (a-3) 31 and Z 32are each independently a trivalent hydrocarbon group having 1 to 20 carbon atoms. Z in formula (a-3) 31 and Z 32 are each independently preferably selected from the group consisting of a group represented by the following formula (a-3-i), a group represented by the following formula (a-3-ii), a group represented by the following formula (a-3-iii), and a group represented by the following formula (a-3-iv). [ka]
[0027] The group represented by formula (a-3-i) is a succinic acid residue, the group represented by formula (a-3-ii) is a phthalic acid residue, the group represented by formula (a-3-iii) is a 2,3-norbornanedicarboxylic acid residue, and the group represented by formula (a-3-iv) is a 5-norbornene-2,3-dicarboxylic acid residue. In formulas (a-3-i) to (a-3-iv), "*" indicates a bond position.
[0028] In the formula (a-3), n3 is an integer of 1 to 200. n3 is preferably an integer of 3 to 150, and more preferably an integer of 5 to 120.
[0029] Commercially available silicones modified with acid anhydrides at both ends include "X22-168AS", "X22-168A", "X22-168B", and "X22-168-P5-8" manufactured by Shin-Etsu Chemical Co., Ltd., and "DMS-Z21" manufactured by Gelest Pharmaceuticals.
[0030] When the structural unit A contains the structural unit (A-3), the proportion of the structural unit (A-3) in the structural unit A is preferably 1 to 50 mol %, more preferably 2 to 40 mol %, and even more preferably 3 to 30 mol %. When the structural unit A further contains the structural unit (A-3), the colorless transparency of the film can be improved while maintaining a low residual stress.
[0031] The structural units other than the structural units (A-1) and (A-2) optionally contained in the structural unit A are not limited to the structural unit (A-3). The tetracarboxylic dianhydride that gives such an optional structural unit is not particularly limited, but includes aromatic tetracarboxylic dianhydrides such as pyromellitic dianhydride, 9,9'-bis(3,4-dicarboxyphenyl)fluorene dianhydride, and 4,4'-(hexafluoroisopropylidene)diphthalic anhydride; alicyclic tetracarboxylic dianhydrides such as 1,2,3,4-cyclobutane tetracarboxylic dianhydride (excluding the compounds represented by formula (a-1) or (a-2)); and aliphatic tetracarboxylic dianhydrides such as 1,2,3,4-butane tetracarboxylic dianhydride. In this specification, the term "aromatic tetracarboxylic acid dianhydride" refers to a tetracarboxylic acid dianhydride containing one or more aromatic rings, the term "alicyclic tetracarboxylic acid dianhydride" refers to a tetracarboxylic acid dianhydride containing one or more alicyclic rings but no aromatic rings, and the term "aliphatic tetracarboxylic acid dianhydride" refers to a tetracarboxylic acid dianhydride containing neither an aromatic ring nor an alicyclic ring. The structural units other than the structural units (A-1) and (A-2) optionally contained in the structural unit A may be of one type, or of two or more types.
[0032] (Structural unit B) The structural unit B is a structural unit derived from a diamine contained in the polyimide resin, and includes a structural unit (B-1) derived from a diamine having a sulfonyl group in its structure, and a structural unit (B-2) derived from a compound represented by the following formula (b-2). [ka] (In formula (b-2), X is a single bond, a substituted or unsubstituted alkylene group, a carbonyl group, an ether group, a group represented by the following formula (b-2-i), or a group represented by the following formula (b-2-ii); p is an integer of 0 to 2, m1 is an integer of 0 to 4, and m2 is an integer of 0 to 4. However, when p is 0, m1 is an integer of 1 to 4.) [ka] (In formula (b-2-i), m3 is an integer of 0 to 5; in formula (b-2-ii), m4 is an integer of 0 to 5. Note that m1+m2+m3+m4 is 1 or more, and when p is 2, each of the two Xs and the two m2 to m4 is independently selected.) In the formulae (b-2-i) and (b-2-ii), "*" indicates the bond position.
[0033] The structural unit (B-1) derived from a diamine having a sulfonyl group in its structure is preferably at least one selected from the group consisting of a structural unit (B-11) derived from a compound represented by the following formula (b-11), a structural unit (B-12) derived from a compound represented by the following formula (b-12), and a structural unit (B-13) derived from a compound represented by the following formula (b-13). [ka] The compound represented by formula (b-11) is bis(3-aminophenyl)sulfone (3,3'-DDS), the compound represented by formula (b-12) is bis[4-(4-aminophenoxy)phenyl]sulfone (BAPS), and the compound represented by formula (b-13) is bis[4-(3-aminophenoxy)phenyl]sulfone (BAPS-M). When the polyimide resin used in the composition of the present invention contains at least one diamine-derived structural unit selected from the group consisting of compounds represented by formula (b-11), formula (b-12), and formula (b-13), the colorless transparency and optical isotropy of the obtained polyimide film are improved.
[0034] When the structural unit (B-1) contains the structural unit (B-12), it is preferable to use it in combination with the structural unit (B-13) from the viewpoint of optical isotropy. That is, from the viewpoint of optical isotropy, the structural unit (B-1) preferably contains the structural unit (B-12) and the structural unit (B-13). It is believed that the use of diamines having sulfonyl groups affects the flexibility of the polymer molecular chains and thus the peelability of the polyimide film. Furthermore, the sulfonyl groups in the diamines inhibit intramolecular charge transfer and inhibit the conjugation of electrons, which is believed to improve the colorless transparency and optical isotropy of the polyimide film.
[0035] Specific examples of the compound represented by formula (b-2) include compounds represented by any of the following formulas (b-21) to (b-27).
[0036] [ka]
[0037] A specific example of the compound represented by formula (b-21) is the compound represented by the following formula (b-211), that is, 3,5-diaminobenzoic acid. [ka]
[0038] The structural unit (B-2) is preferably a structural unit (B-21) derived from a compound represented by formula (b-21), and more preferably a structural unit (B-211) derived from a compound represented by formula (b-211).
[0039] When the structural unit B contains the structural unit (B-2), the heat resistance and chemical resistance of the film are improved.
[0040] The proportion of the structural unit (B-1) in the structural unit B is preferably 15 to 95 mol %, and from the viewpoint of heat resistance, is more preferably 20 to 95 mol %, even more preferably 50 to 90 mol %, and still more preferably 70 to 85 mol %. The proportion of the structural unit (B-2) in the structural unit B is preferably 5 to 85 mol %, more preferably 5 to 80 mol %, even more preferably 10 to 50 mol %, and still more preferably 15 to 30 mol %.
[0041] The molar ratio of the structural unit (B-1) to the structural unit (B-2) in the structural unit B [(B-1) / (B-2)] is preferably 15 / 85 to 95 / 5, and from the standpoint of reducing residual stress and improving elongation, is more preferably 15 / 85 to 70 / 30, even more preferably 15 / 85 to 50 / 50, and still more preferably 15 / 85 to 40 / 60. The total ratio of the structural units (B-1) and (B-2) in the structural unit B is preferably 50 mol% or more, more preferably 70 mol% or more, and even more preferably 90 mol% or more. The upper limit of the total ratio of the structural units (B-1) and (B-2) is not particularly limited, that is, it is 100 mol%. The structural unit B may be composed of only the structural unit (B-1) and the structural unit (B-2).
[0042] The structural unit B preferably contains a structural unit (B-3) derived from a compound represented by the following formula (b-3): When the structural unit B contains the structural unit (B-3), the colorless transparency and optical isotropy of the film are improved, and the residual stress is reduced. [ka]
[0043] In formula (b-3), Z 1 and Z 2 each independently represents a divalent aliphatic group or a divalent aromatic group which may contain an oxygen atom; R 1 and R 2 each independently represents a monovalent aromatic group or a monovalent aliphatic group; R 3 and R 4 each independently represents a monovalent aliphatic group; R 5 and R 6 each independently represents a monovalent aliphatic group or a monovalent aromatic group, m and n each independently represent an integer of 1 or more, and the sum of m and n represents an integer of 2 to 1000. 1 and R 2 At least one of these represents a monovalent aromatic group. In formula (b-3), the two or more different repeating units described in parallel in brackets [ ] may each be repeated in any form and order of random, alternating, or block.
[0044] In formula (b-3), Z 1 and Z 2 The divalent aliphatic group or divalent aromatic group in may be substituted with a fluorine atom. Examples of the divalent aliphatic group include a divalent saturated or unsaturated aliphatic group having 1 to 20 carbon atoms and an aliphatic group containing an oxygen atom. The divalent aliphatic group preferably has 3 to 20 carbon atoms. Examples of the divalent saturated aliphatic group include alkylene groups having 1 to 20 carbon atoms, such as a methylene group, an ethylene group, a propylene group, a trimethylene group, a tetramethylene group, a hexamethylene group, an octamethylene group, a decamethylene group, and a dodecamethylene group. The divalent unsaturated aliphatic group may be an alkylene group having 2 to 20 carbon atoms, such as a vinylene group, a propenylene group, or an alkylene group having an unsaturated double bond at a terminal. Examples of the aliphatic group containing an oxygen atom include an alkyleneoxy group and an aliphatic group having an ether bond. Examples of the divalent aromatic group include an arylene group having 6 to 20 carbon atoms and an aralkylene group having 7 to 20 carbon atoms. 1 and Z 2 Specific examples of the arylene group having 6 to 20 carbon atoms in the formula include an o-phenylene group, an m-phenylene group, a p-phenylene group, a 4,4'-biphenylylene group, and a 2,6-naphthylene group. Z in formula (b-3) 1 and Z 2 As the alkyl group, a trimethylene group or a p-phenylene group is particularly preferable, and a trimethylene group is more preferable.
[0045] In formula (b-3), R 1 ~R 6In the above, examples of the monovalent aliphatic group include monovalent saturated or unsaturated aliphatic groups. Examples of the monovalent saturated aliphatic group include alkyl groups having 1 to 22 carbon atoms, such as methyl, ethyl, and propyl groups. Examples of the monovalent unsaturated aliphatic group include alkenyl groups having 2 to 22 carbon atoms, such as vinyl and propenyl groups. These groups may be substituted with a fluorine atom. R in formula (b-3) 1 , R 2 , R 5 and R 6 Examples of the monovalent aromatic group in the formula (I) include an aryl group having 6 to 20 carbon atoms, an aryl group having 7 to 30 carbon atoms and substituted with an alkyl group, and an aralkyl group having 7 to 30 carbon atoms. As the monovalent aromatic group, an aryl group is preferable, and a phenyl group is more preferable. R in formula (b-3) 1 and R 2 At least one of R represents a monovalent aromatic group. 1 and R 2 are preferably both monovalent aromatic groups, and R 1 and R 2 More preferably, both are phenyl groups. R in formula (b-3) 3 and R 4 As the alkyl group, an alkyl group having 1 to 6 carbon atoms is preferable, and a methyl group is more preferable. R in formula (b-3) 5 and R 6 As the group, a monovalent aliphatic group is preferable, and a methyl group is more preferable.
[0046] As described above, among the compounds represented by formula (b-3), the compounds represented by the following formula (b-31) are preferred. [ka] (In formula (b-31), m and n have the same meanings as m and n in formula (b-3), respectively, and the preferred ranges are also the same.)
[0047] In formula (b-3), m represents the number of repeating siloxane units to which at least one monovalent aromatic group is bonded, and n in formula (b-3) represents the number of repeating siloxane units to which a monovalent aliphatic group is bonded. In formula (b-3), m and n each independently represent an integer of 1 or more, and the sum of m and n (m+n) represents an integer of 2 to 1000. The sum of m and n preferably represents an integer of 3 to 500, more preferably an integer of 3 to 100, and even more preferably an integer of 3 to 50. The ratio of m / n in the formula (b-3) is preferably from 5 / 95 to 50 / 50, more preferably from 10 / 90 to 40 / 60, and further preferably from 20 / 80 to 30 / 70.
[0048] The functional group equivalent (amine equivalent) of the compound represented by formula (b-3) is preferably 150 to 5,000 g / mol, more preferably 400 to 4,000 g / mol, and further preferably 500 to 3,000 g / mol. The functional group equivalent means the mass of the compound represented by formula (b-3) per mole of the functional group (amino group).
[0049] Among the compounds represented by formula (b-3), examples of commercially available products include “X-22-9409”, “X-22-1660B”, “X-22-161AS”, “X-22-161A”, and “X-22-161B” manufactured by Shin-Etsu Chemical Co., Ltd.
[0050] The proportion of the structural unit (B-3) in the structural unit B is preferably 1 to 25 mol %, more preferably 2 to 20 mol %, even more preferably 3 to 15 mol %, still more preferably 5 to 15 mol %, and even more preferably 7 to 15 mol %.
[0051] The structural unit B preferably contains a structural unit (B-4) derived from a compound represented by the following formula (b-4): When the structural unit B contains the structural unit (B-4), the colorless transparency of the film is improved. [ka]
[0052] The proportion of the structural unit (B-4) in the structural unit B is preferably 1 to 50 mol %, more preferably 5 to 45 mol %, even more preferably 5 to 40 mol %, still more preferably 10 to 40 mol %, and even more preferably 10 to 30 mol %.
[0053] The structural unit B may contain a structural unit other than the structural units (B-1) to (B-4). Diamines that provide such structural units are not particularly limited, but include 1,4-phenylenediamine, p-xylylenediamine, 1,5-diaminonaphthalene, 2,2'-dimethylbiphenyl-4,4'-diamine, 4,4'-diaminodiphenyl ether, 4,4'-diaminodiphenylmethane, 2,2-bis(4-aminophenyl)hexafluoropropane, 4,4'-diaminodiphenyl sulfone, 4,4'-diaminobenzanilide, 1-(4-aminophenyl)-2,3-dihydro-1,3,3-trimethyl-1H-inden-5-amine, α,α'-bis(4-aminophenyl)-1,4-diisopropylbenzene, N,N'-bis(4-aminophenyl)tetraamine, and the like. aromatic diamines such as benzophthalamide, 4,4'-bis(4-aminophenoxy)biphenyl, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 2,2-bis(4-(4-aminophenoxy)phenyl)hexafluoropropane, and 9,9-bis(4-aminophenyl)fluorene (excluding the compounds represented by any of formulas (b-1) to (b-4)); alicyclic diamines such as 1,3-bis(aminomethyl)cyclohexane and 1,4-bis(aminomethyl)cyclohexane; and aliphatic diamines such as ethylenediamine and hexamethylenediamine (excluding the compounds represented by formula (b-1) and formula (b-3)). In this specification, an aromatic diamine refers to a diamine containing one or more aromatic rings, an alicyclic diamine refers to a diamine containing one or more alicyclic rings but no aromatic rings, and an aliphatic diamine refers to a diamine containing neither an aromatic ring nor an alicyclic ring. The structural units other than the structural units (B-1) to (B-4) optionally contained in the structural unit B may be of one type, or of two or more types.
[0054] From the viewpoint of the mechanical strength of the resulting polyimide film, the number average molecular weight of the polyimide resin is preferably 5,000 to 100,000. The number average molecular weight of the polyimide resin can be determined, for example, from a standard polymethyl methacrylate (PMMA)-equivalent value measured by gel filtration chromatography.
[0055] The polyimide resin may contain a structure other than a polyimide chain (a structure formed by imide bonding between a structural unit A and a structural unit B). Examples of structures other than a polyimide chain that can be contained in a polyimide resin include a structure containing an amide bond. The polyimide resin preferably contains, as its main structure, a polyimide chain (a structure formed by imide bonding between the structural unit A and the structural unit B). Therefore, the ratio of the polyimide chain in the polyimide resin is preferably 50% by mass or more, more preferably 70% by mass or more, even more preferably 90% by mass or more, and particularly preferably 99% by mass or more.
[0056] The polyimide resin composition of the present invention containing the above polyimide resin can form a film that is excellent in colorless transparency, optical isotropy and releasability, and the suitable physical properties of the film are as follows.
[0057] The total light transmittance, when made into a film having a thickness of 10 μm, is preferably 88% or more, more preferably 89% or more, and further preferably 90% or more. The yellow index (YI) when made into a film having a thickness of 10 μm is preferably 5.0 or less, more preferably 4.0 or less, and further preferably 3.0 or less. The residual stress is preferably 25.0 MPa or less, more preferably 24.0 MPa or less, and further preferably 22.0 MPa or less. The absolute value of the thickness retardation (Rth) is preferably 100 nm or less, more preferably 60 nm or less, and even more preferably 35 nm or less, when the film has a thickness of 10 μm. When the absolute value is within this range, the optical isotropy is excellent.
[0058] Furthermore, a film that can be formed using the polyimide resin has good heat resistance and mechanical properties, and has the following preferable physical properties. The glass transition temperature (Tg) is preferably 250° C. or higher, more preferably 270° C. or higher, and further preferably 280° C. or higher. The tensile modulus is preferably 2.0 GPa or more, more preferably 2.5 GPa or more, and further preferably 2.6 GPa or more. The tensile elongation is preferably 5%, more preferably 6% or more, even more preferably 7% or more, and still more preferably 10% or more. When the tensile modulus and tensile elongation are within the above ranges, the film can be easily peeled from the substrate during processing. The above-mentioned physical properties in the present invention can be specifically measured by the methods described in the Examples.
[0059] <Method of manufacturing polyimide resin> In the present invention, the polyimide resin can be produced by reacting a tetracarboxylic acid component containing a compound that provides the above-mentioned structural unit A with a diamine component containing a compound that provides the above-mentioned structural unit (B-1) and a compound that provides the above-mentioned structural unit (B-2).
[0060] Compounds that provide the structural unit A include compounds represented by formula (a-1) and formula (a-2), but are not limited thereto and may be derivatives thereof as long as they provide the same structural unit. Examples of the derivatives include tetracarboxylic acids corresponding to the tetracarboxylic dianhydrides represented by formula (a-1) and formula (a-2) (i.e., norbornane-2-spiro-α-cyclopentanone-α'-spiro-2"-norbornane-5,5",6,6"-tetracarboxylic acid, 1,2,4,5-cyclohexanetetracarboxylic acid), and alkyl esters of the tetracarboxylic acids. Among these, the tetracarboxylic dianhydrides represented by formula (a-1) and formula (a-2) are preferred.
[0061] The tetracarboxylic acid component contains a compound that gives the structural unit (A-1) in an amount of preferably 40 mol% or more, more preferably 50 mol% or more, and even more preferably 60 mol% or more. The upper limit of the content of the compound that gives the structural unit (A-1) is not particularly limited, that is, it is 100 mol%. The tetracarboxylic acid component may be composed of only the compound that gives the structural unit (A-1).
[0062] The tetracarboxylic acid component contains a compound that gives the structural unit (A-2) in an amount of preferably 50 mol% or more, more preferably 70 mol% or more, and even more preferably 85 mol% or more. The upper limit of the content of the compound that gives the structural unit (A-2) is not particularly limited, that is, it is 100 mol%. The tetracarboxylic acid component may be composed of only the compound that gives the structural unit (A-2).
[0063] When the tetracarboxylic acid component contains a compound that gives the structural unit (A-1) and a compound that gives the structural unit (A-2), the tetracarboxylic acid component contains the compound that gives the structural unit (A-1) and the compound that gives the structural unit (A-2) in total preferably 50 mol% or more, more preferably 70 mol% or more, even more preferably 90 mol% or more, and particularly preferably 99 mol% or more. The upper limit of the compound that gives the structural unit (A-1) and the compound that gives the structural unit (A-2) is not particularly limited, that is, it is 100 mol%. The tetracarboxylic acid component may be composed of only the compound that gives the structural unit (A-1) and the compound that gives the structural unit (A-2).
[0064] The tetracarboxylic acid component may contain compounds other than the compound that provides the structural unit (A-1) and the compound that provides the structural unit (A-2).
[0065] The tetracarboxylic acid component may further contain a compound that provides the structural unit (A-3), in addition to the compound that provides the structural unit (A-1) and the compound that provides the structural unit (A-2). Examples of compounds that provide the structural unit (A-3) include silicones modified with acid anhydrides at both ends (for example, compounds represented by formula (a-3)), but are not limited thereto, and may be derivatives thereof as long as they provide the same structural unit. Examples of such derivatives include tetracarboxylic acids corresponding to the silicones modified with acid anhydrides at both ends and alkyl esters of the tetracarboxylic acids. Examples of compounds that provide the structural unit (A-3) include silicones modified with acid anhydrides at both ends (i.e., dianhydrides).
[0066] When the tetracarboxylic acid component contains a compound that provides the structural unit (A-3), the tetracarboxylic acid component preferably contains the compound that provides the structural unit (A-3) in an amount of 1 to 50 mol %, more preferably 2 to 40 mol %, and even more preferably 3 to 30 mol %.
[0067] Compounds other than the compound that gives the structural unit (A-1) and the compound that gives the structural unit (A-2) that are optionally contained in the tetracarboxylic acid component are not limited to the compound that gives the structural unit (A-3). Examples of such optional compounds include the above-mentioned aromatic tetracarboxylic acid dianhydrides, alicyclic tetracarboxylic acid dianhydrides, and aliphatic tetracarboxylic acid dianhydrides, as well as derivatives thereof (tetracarboxylic acids, alkyl esters of tetracarboxylic acids, etc.). The compounds optionally contained in the tetracarboxylic acid component other than the compound providing the structural unit (A-1) and the compound providing the structural unit (A-2) may be one type or two or more types.
[0068] Compounds that provide the structural unit (B-1) include compounds represented by formula (b-11), compounds represented by formula (b-12), and compounds represented by formula (b-13), but are not limited thereto, and may also be derivatives thereof as long as they provide the same structural unit. Examples of the derivatives include diisocyanates corresponding to the diamines represented by formula (b-11), diisocyanates corresponding to the diamines represented by formula (b-12), and diisocyanates corresponding to the diamines represented by formula (b-13). Among these, the diamines represented by formula (b-11), formula (b-12), and formula (b-13) are preferred. Similarly, the compound that gives the structural unit (B-2) may be a compound represented by formula (b-2), but is not limited thereto and may be a derivative thereof as long as it gives the same structural unit. The derivative may be a diisocyanate corresponding to the diamine represented by formula (b-2). The compound that gives the structural unit (B-2) is preferably a compound represented by formula (b-2) (i.e., a diamine).
[0069] The diamine component contains the compound that provides the structural unit (B-1) in an amount of preferably 15 to 95 mol %, more preferably 20 to 95 mol %, even more preferably 50 to 90 mol %, and even more preferably 70 to 85 mol %. The diamine component contains a compound that provides the structural unit (B-2) in an amount of preferably 5 to 85 mol %, more preferably 5 to 80 mol %, even more preferably 10 to 50 mol %, and even more preferably 15 to 30 mol %. The diamine component contains a compound that gives the structural unit (B-1) and a compound that gives the structural unit (B-2) in a total amount of preferably 50 mol% or more, more preferably 70 mol% or more, even more preferably 90 mol% or more, and particularly preferably 99 mol% or more. The upper limit of the total content of the compound that gives the structural unit (B-1) and the compound that gives the structural unit (B-2) is not particularly limited, that is, it is 100 mol%. The diamine component may be composed of only the compound that gives the structural unit (B-1) and the compound that gives the structural unit (B-2).
[0070] The diamine component may contain compounds other than the compound that provides the structural unit (B-1) and the compound that provides the structural unit (B-2).
[0071] The diamine component may further contain a compound that provides the structural unit (B-3), in addition to the compound that provides the structural unit (B-1) and the compound that provides the structural unit (B-2). Compounds that give the structural unit (B-3) include compounds represented by formula (b-3), but are not limited thereto, and may be derivatives thereof as long as they give the same structural unit. Examples of such derivatives include diisocyanates corresponding to the diamines represented by formula (b-3). Compounds that give the structural unit (B-3) are preferably compounds represented by formula (b-3) (i.e., diamines). The diamine component contains a compound that provides the structural unit (B-3) in an amount of preferably 1 to 25 mol %, more preferably 2 to 20 mol %, even more preferably 3 to 15 mol %, still more preferably 5 to 15 mol %, and even more preferably 7 to 15 mol %.
[0072] The diamine component may further contain a compound that provides the structural unit (B-4), in addition to the compound that provides the structural unit (B-1) and the compound that provides the structural unit (B-2). Compounds that give the structural unit (B-4) include compounds represented by formula (b-4), but are not limited thereto, and may be derivatives thereof as long as they give the same structural unit. Examples of such derivatives include diisocyanates corresponding to the diamines represented by formula (b-4). Compounds that give the structural unit (B-4) are preferably compounds represented by formula (b-4) (i.e., diamines). The diamine component contains a compound that provides the structural unit (B-4) in an amount of preferably 1 to 50 mol %, more preferably 5 to 45 mol %, even more preferably 5 to 40 mol %, still more preferably 10 to 40 mol %, and even more preferably 10 to 30 mol %. In particular, from the viewpoint of reducing residual stress, the compound contains preferably 1 to 50 mol %, more preferably 10 to 50 mol %, and even more preferably 20 to 40 mol %.
[0073] Compounds other than the compound that gives the structural unit (B-1) and the compound that gives the structural unit (B-2) that are optionally contained in the diamine component are not limited to the compound that gives the structural unit (B-3) and the compound that gives the structural unit (B-4). Such optional compounds include the above-mentioned aromatic diamines, alicyclic diamines, and aliphatic diamines, and their derivatives (diisocyanates, etc.). The compound optionally contained in the diamine component other than the compound providing the structural unit (B-1) and the compound providing the structural unit (B-2) may be one type or two or more types.
[0074] In the present invention, the ratio of the amounts of the tetracarboxylic acid component and the diamine component used in the production of the polyimide resin is preferably 0.9 to 1.1 mol of the diamine component per 1 mol of the tetracarboxylic acid component.
[0075] In the present invention, in addition to the above-mentioned tetracarboxylic acid component and diamine component, a terminal blocking agent may be used in the production of the polyimide resin. As the terminal blocking agent, monoamines or dicarboxylic acids are preferred. The amount of the terminal blocking agent to be introduced is preferably 0.0001 to 0.1 moles per mole of the tetracarboxylic acid component, and particularly preferably 0.001 to 0.06 moles. As the monoamine terminal blocking agent, for example, methylamine, ethylamine, propylamine, butylamine, benzylamine, 4-methylbenzylamine, 4-ethylbenzylamine, 4-dodecylbenzylamine, 3-methylbenzylamine, 3-ethylbenzylamine, aniline, 3-methylaniline, 4-methylaniline, etc. are recommended. Among these, benzylamine and aniline are preferably used. As the dicarboxylic acid terminal blocking agent, dicarboxylic acids are preferred, and a part of them may be ring-closed. For example, phthalic acid, phthalic anhydride, 4-chlorophthalic acid, tetrafluorophthalic acid, 2,3-benzophenonedicarboxylic acid, 3,4-benzophenonedicarboxylic acid, cyclohexane-1,2-dicarboxylic acid, cyclopentane-1,2-dicarboxylic acid, 4-cyclohexene-1,2-dicarboxylic acid, etc. are recommended. Of these, phthalic acid and phthalic anhydride are preferably used.
[0076] The method for reacting the tetracarboxylic acid component and the diamine component is not particularly limited, and any known method can be used. Specific reaction methods include (1) a method in which a tetracarboxylic acid component, a diamine component, and a reaction solvent are charged into a reactor, and the mixture is stirred at room temperature to 80°C for 0.5 to 30 hours, and then the temperature is raised to carry out the imidization reaction; (2) a method in which a diamine component and a reaction solvent are charged into a reactor and dissolved, and then a tetracarboxylic acid component is charged, and the mixture is stirred at room temperature to 80°C for 0.5 to 30 hours as necessary, and then the temperature is raised to carry out the imidization reaction; and (3) a method in which a tetracarboxylic acid component, a diamine component, and a reaction solvent are charged into a reactor, and the temperature is immediately raised to carry out the imidization reaction.
[0077] The reaction solvent used in the production of the polyimide resin may be any solvent that does not inhibit the imidization reaction and can dissolve the resulting polyimide. Examples of the solvent include aprotic solvents, phenolic solvents, ether solvents, and carbonate solvents.
[0078] Specific examples of aprotic solvents include amide-based solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone (NMP), N-methylcaprolactam, 1,3-dimethylimidazolidinone, and tetramethylurea; lactone-based solvents such as γ-butyrolactone (GBL) and γ-valerolactone; phosphorus-containing amide-based solvents such as hexamethylphosphoric amide and hexamethylphosphine triamide; sulfur-containing solvents such as dimethyl sulfone, dimethyl sulfoxide, and sulfolane; ketone-based solvents such as acetone, cyclohexanone, and methylcyclohexanone; amine-based solvents such as picoline and pyridine; and ester-based solvents such as 2-methoxy-1-methylethyl acetate.
[0079] Specific examples of phenol-based solvents include phenol, o-cresol, m-cresol, p-cresol, 2,3-xylenol, 2,4-xylenol, 2,5-xylenol, 2,6-xylenol, 3,4-xylenol, and 3,5-xylenol. Specific examples of ether solvents include 1,2-dimethoxyethane, bis(2-methoxyethyl)ether, 1,2-bis(2-methoxyethoxy)ethane, bis[2-(2-methoxyethoxy)ethyl]ether, tetrahydrofuran, and 1,4-dioxane. Specific examples of carbonate solvents include diethyl carbonate, methyl ethyl carbonate, ethylene carbonate, and propylene carbonate. Among the above reaction solvents, amide-based solvents and lactone-based solvents are preferred. The above reaction solvents may be used alone or in combination of two or more.
[0080] In the imidization reaction, it is preferable to carry out the reaction while removing water generated during the production using a Dean-Stark apparatus, etc. By carrying out such an operation, it is possible to further increase the degree of polymerization and the imidization rate.
[0081] In the above imidization reaction, a known imidization catalyst can be used, such as a base catalyst or an acid catalyst. Examples of the base catalyst include organic base catalysts such as pyridine, quinoline, isoquinoline, α-picoline, β-picoline, 2,4-lutidine, 2,6-lutidine, trimethylamine, triethylamine (TEA), tripropylamine, tributylamine, triethylenediamine, imidazole, N,N-dimethylaniline, and N,N-diethylaniline; and inorganic base catalysts such as potassium hydroxide, sodium hydroxide, potassium carbonate, sodium carbonate, potassium hydrogencarbonate, and sodium hydrogencarbonate. Examples of the acid catalyst include crotonic acid, acrylic acid, trans-3-hexenoic acid, cinnamic acid, benzoic acid, methylbenzoic acid, oxybenzoic acid, terephthalic acid, benzenesulfonic acid, paratoluenesulfonic acid, naphthalenesulfonic acid, etc. The above imidization catalysts may be used alone or in combination of two or more kinds. Among the above, from the viewpoint of handleability, it is preferable to use a base catalyst, more preferably an organic base catalyst, further preferably triethylamine, and particularly preferably a combination of triethylamine and triethylenediamine.
[0082] The temperature of the imidization reaction is preferably 120 to 250° C., more preferably 160 to 200° C., from the viewpoints of reaction rate and suppression of gelation, etc. The reaction time is preferably 0.5 to 10 hours after the start of distillation of the produced water.
[0083] <Crosslinking agent> In the present invention, the crosslinking agent has at least two oxazolyl groups, that is, the crosslinking agent in the present invention is a polyfunctional oxazoline compound having two or more oxazolyl groups (oxazoline rings) in the molecule. The oxazolyl group is reactive with the carboxyl group, and when the carboxyl group reacts with the oxazolyl group, an amide ester bond is formed as shown below. This reaction is particularly likely to proceed when heated to 80°C or higher. [ka]
[0084] Since the polyimide resin contained in the polyimide resin composition of the present invention has a carboxyl group, when the polyimide resin composition of the present invention is heated, the polyimide resins crosslink with each other via the crosslinking agent to form a crosslinked polyimide resin, which improves the chemical resistance of the film.
[0085] The crosslinking agent is not particularly limited as long as it is a polyfunctional oxazoline compound having two or more oxazolyl groups in the molecule. Specific examples thereof include 1,3-bis(4,5-dihydro-2-oxazolyl)benzene, 1,4-bis(4,5-dihydro-2-oxazolyl)benzene, 2,2'-bis(2-oxazoline), "K-2010E", "K-2020E", and "K-2030E" manufactured by Nippon Shokubai Co., Ltd., 2,6-bis(4-isopropyl-2-oxazolin-2-yl)pyridine, 2,6-bis(4-phenyl-2-oxazolin-2-yl)pyridine, 2,2'-isopropylidenebis(4-phenyl-2-oxazoline), and 2,2'-isopropylidenebis(4-tert-butyl-2-oxazoline).
[0086] The crosslinking agent is preferably a compound containing an aromatic ring or aromatic heterocycle to which at least two oxazolyl groups are bonded, more preferably a compound containing a benzene ring or pyridine ring to which at least two oxazolyl groups are bonded, even more preferably a compound containing a benzene ring to which at least two oxazolyl groups are bonded, and particularly preferably 1,3-bis(4,5-dihydro-2-oxazolyl)benzene. The crosslinking agent may be used alone or in combination of two or more kinds.
[0087] The polyimide resin composition of the present invention preferably contains a polyimide resin and a crosslinking agent in such a ratio that the molar ratio of the oxazolyl group in the crosslinking agent to the carboxyl group in the polyimide resin (oxazolyl group / carboxyl group) is in the range of 1 / 8 to 1 / 0.5, more preferably 1 / 6 to 1 / 1, and further preferably 1 / 4 to 1 / 2. The above molar ratio means the molar ratio between the oxazolyl group contained in the crosslinking agent and the carboxyl group contained in the compound that provides the structural unit (B-2) used in the production of the polyimide resin, and is calculated based on the amount of the crosslinking agent added and the amount of the compound that provides the structural unit (B-2) added.
[0088] [Polyimide varnish] A preferred embodiment of the polyimide resin composition of the present invention is a polyimide resin composition (hereinafter, also referred to as a "polyimide varnish") that further contains an organic solvent in addition to the above-mentioned polyimide resin and the above-mentioned crosslinking agent, and in which the polyimide resin is dissolved in the organic solvent. The organic solvent is not particularly limited as long as it dissolves the polyimide resin. However, it is preferable to use the above-mentioned compounds as reaction solvents used in the production of the polyimide resin, either alone or in combination of two or more kinds. The polyimide varnish may be prepared by adding a crosslinking agent to a solution in which a polyimide resin obtained by polymerization is dissolved in a reaction solvent, or by adding a dilution solvent and a crosslinking agent to the solution.
[0089] The polyimide varnish preferably contains 5 to 40 mass %, more preferably 7 to 30 mass %, and even more preferably 8 to 20 mass % of polyimide resin. The viscosity of the polyimide varnish is preferably 50 to 5000 Pa·s, more preferably 100 to 4000 Pa·s, and even more preferably 300 to 3500 Pa·s. The viscosity of the polyimide varnish is a value measured at 25°C using an E-type viscometer.
[0090] In addition, the polyimide varnish of the present invention may contain various additives such as inorganic fillers, adhesion promoters, release agents, flame retardants, UV stabilizers, surfactants, leveling agents, defoamers, fluorescent brightening agents, crosslinking agents, polymerization initiators, and photosensitizers, as long as the additives do not impair the required properties of the polyimide film. The method for producing the polyimide varnish of the present invention is not particularly limited, and any known method can be applied.
[0091] [Polyimide film] The polyimide film of the present invention is obtained by crosslinking the above-mentioned polyimide resin contained in the polyimide resin composition of the present invention with the above-mentioned crosslinking agent. That is, the polyimide film of the present invention contains a crosslinked polyimide resin which is a crosslinked product of polyimide resins via a crosslinking agent. Therefore, the polyimide film of the present invention is excellent in heat resistance, colorless transparency, and chemical resistance, and further has low residual stress. The preferable physical properties of the polyimide film of the present invention are as described above.
[0092] The method for producing the polyimide film of the present invention is not particularly limited as long as it includes a step of crosslinking at a temperature at which the crosslinking reaction between the polyimide resin and the crosslinking agent proceeds (preferably 80°C or higher, more preferably 100°C or higher, and even more preferably 150°C or higher). For example, the above-mentioned polyimide varnish is applied to a smooth support such as a glass plate, a metal plate, or a plastic, or formed into a film, and then heated. This heat treatment can remove organic solvents such as reaction solvents and dilution solvents contained in the polyimide varnish while proceeding with the crosslinking reaction between the polyimide resin in the polyimide varnish and the crosslinking agent. If necessary, a release agent may be applied in advance to the surface of the support.
[0093] The heat treatment is preferably performed by the following method. That is, it is preferable to first evaporate the organic solvent at a temperature of 120°C or less, and then further dry at a temperature equal to or higher than the boiling point of the organic solvent to produce a polyimide film. It is also preferable to dry under a nitrogen atmosphere. The pressure of the drying atmosphere may be reduced pressure, normal pressure, or increased pressure. By drying at two temperatures, a film having a smooth surface and free of defects can be obtained. The drying temperature in the second stage is not particularly limited, but is preferably 200 to 450°C, more preferably 300 to 430°C, and particularly preferably 350 to 400°C. By drying within this temperature range, the transparency and yellowness of the film become good, and further good solvent resistance can be obtained.
[0094] The polyimide film of the present invention can also be produced by using a polyamic acid varnish prepared by dissolving a polyamic acid and a crosslinking agent in an organic solvent. The polyamic acid contained in the polyamic acid varnish is a precursor of the polyimide resin of the present invention, and is a product of a polyaddition reaction between a tetracarboxylic acid component containing a compound that gives the above-mentioned structural unit A and a diamine component containing a compound that gives the above-mentioned structural unit (B-1) and a compound that gives the above-mentioned structural unit (B-2). The polyamic acid is imidized (dehydration ring closure) to obtain a polyimide resin. As the organic solvent contained in the polyamic acid varnish, the organic solvent contained in the polyimide varnish of the present invention can be used. In the present invention, the polyamic acid varnish may be a polyamic acid solution itself obtained by subjecting a tetracarboxylic acid component containing a compound that provides the above-mentioned structural unit A to a polyaddition reaction in a reaction solvent with a diamine component containing a compound that provides the above-mentioned structural unit (B-1) and a compound that provides the above-mentioned structural unit (B-2), or may be a polyamic acid solution to which a dilution solvent has been further added.
[0095] The method for producing a polyimide film using a polyamic acid varnish is not particularly limited as long as it includes a step of crosslinking at a temperature at which the crosslinking reaction between the polyimide resin and the crosslinking agent proceeds (preferably 80°C or higher, more preferably 100°C or higher, and even more preferably 150°C or higher), and a known method can be used. For example, the polyamic acid varnish is applied to a smooth support such as a glass plate, a metal plate, a silicon wafer, or a plastic, or formed into a film, and organic solvents such as reaction solvents and dilution solvents contained in the varnish are removed by heating to obtain a polyamic acid film, and the polyamic acid in the polyamic acid film is imidized by heating, and further crosslinked by reacting the polyimide resin with a crosslinking agent, thereby producing a polyimide film. The heating temperature when the polyamic acid varnish is dried to obtain a polyamic acid film is preferably 50 to 120° C. The heating temperature when the polyamic acid is imidized by heating is preferably 200 to 400° C. The imidization method is not limited to thermal imidization, and chemical imidization can also be applied.
[0096] The thickness of the polyimide film of the present invention can be appropriately selected depending on the application, etc., but is preferably in the range of 1 to 250 μm, more preferably 5 to 100 μm, and even more preferably 10 to 80 μm. When the thickness is 1 to 250 μm, practical use as a free-standing film becomes possible. The thickness of the polyimide film can be easily controlled by adjusting the solids concentration and viscosity of the polyimide varnish.
[0097] The polyimide film of the present invention is suitably used as a film for various members such as color filters, flexible displays, semiconductor parts, optical members, etc. The polyimide film of the present invention is particularly suitably used as a substrate for image display devices such as liquid crystal displays and OLED displays. EXAMPLES
[0098] The present invention will be described in detail below with reference to examples, although the present invention is not limited to these examples in any way. The solids concentration of the varnishes and the physical properties of the films obtained in the examples and comparative examples were measured by the methods described below.
[0099] (1) Solid content concentration The solids concentration of the varnish was measured by heating the sample at 320°C for 120 min in a small electric furnace "MMF-1" manufactured by AS ONE Corporation, and calculating from the mass difference of the sample before and after heating.
[0100] (2) Film thickness The film thickness was measured using a micrometer manufactured by Mitutoyo Corporation.
[0101] (3) Total light transmittance, yellow index (YI) The total light transmittance and YI were measured in accordance with JIS K7105:1997 using a color / turbidity simultaneous measuring instrument "COH7700" manufactured by Nippon Denshoku Industries Co., Ltd.
[0102] (4) Haze The measurements were performed in accordance with JIS K7361-1 using a color and turbidity simultaneous measuring device "COH400" manufactured by Nippon Denshoku Industries Co., Ltd.
[0103] (5)b * b * was measured in accordance with JIS Z8781:2013 using a color and turbidity simultaneous measuring device "COH7700" manufactured by Nippon Denshoku Industries Co., Ltd.
[0104] (6) In-plane retardation (Re) The in-plane retardation (Re) was measured using an ellipsometer "M-220" manufactured by JASCO Corporation. The in-plane phase difference value was measured at a measurement wavelength of 590 nm.
[0105] (7) Thickness phase difference (Rth) The thickness retardation (Rth) was measured using an ellipsometer "M-220" manufactured by JASCO Corporation. The thickness retardation value was measured at a measurement wavelength of 590 nm. Rth is expressed by the following formula, where the maximum in-plane refractive index of the polyimide film is nx, the minimum is ny, the refractive index in the thickness direction is nz, and the thickness of the film is d. Rth = [{(nx + ny) / 2}-nz] × d
[0106] (8) Peel strength The peel strength between the polyimide film and the glass interface was measured using a tensile tester "Strograph EII-L05" manufactured by Toyo Seiki Co., Ltd. The test piece used was a glass plate measuring 10 mm x 100 mm in size on which a polyimide film was formed. The test piece, one end of which had been peeled off, was placed horizontally in the device, the end of the film was clamped with a chuck, and the peel strength was determined by the stress when the peeled film and the glass were pulled at an angle of approximately 90°. The tensile test speed was 50 mm / min.
[0107] (9) Glass transition temperature (Tg) Using a thermomechanical analyzer "TMA / SS6100" manufactured by Hitachi High-Tech Science Corporation, the specimen was heated to a temperature sufficient to remove the residual stress under the following conditions: sample size 2mm x 20mm, load 0.1N, and heating rate 10℃ / min in tensile mode, and then cooled to room temperature. The specimen elongation was then measured under the same conditions as in the treatment for removing the residual stress, and the point at which an inflection point in the elongation was observed was determined as the glass transition temperature.
[0108] (10)1% weight loss temperature (Td 1%) The 1% weight loss temperature was measured using a thermogravimetric analyzer (TG / DTA6200 manufactured by Seiko Instruments Inc.) for a sample of about 10 mg. The temperature was measured at which the sample weight decreased by 1% by weight relative to 100% by weight at 100°C when the sample was heated from room temperature to 450°C at a heating rate of 10°C / min. The temperature was increased under the conditions of an air gas flow rate of 50 mL / min in an air atmosphere and a nitrogen gas flow rate of 100 mL / min in a nitrogen atmosphere.
[0109] (11) Residual stress Polyimide varnish or polyamic acid varnish was applied using a spin coater onto a 4-inch silicon wafer with a thickness of 525μm±25μm, the "warpage" of which had been measured in advance using a residual stress measurement device "FLX-2320" manufactured by KLA-Tencor Corporation, and the wafer was pre-baked. After that, a heat curing process was performed at 350-400℃ for 30 minutes in a nitrogen atmosphere using a hot air dryer, and a silicon wafer with a polyimide film with a thickness of 8-15μm after curing was produced. The amount of warpage of this wafer was measured using the aforementioned residual stress measurement device, and the residual stress generated between the silicon wafer and the polyimide film was evaluated.
[0110] (12) Chemical resistance 1 (PGMEA) A solvent was dropped onto a polyimide film formed on a glass plate at room temperature, and the film surface was checked for any changes. Propylene glycol monomethyl ether acetate (PGMEA) was used as the solvent. The evaluation criteria for solvent resistance were as follows. ○: No change was observed on the film surface. △: Slight cracks occurred on the film surface. ×: The film surface was cracked or dissolved.
[0111] (13) Chemical resistance 2 (acid resistance) The polyimide film formed on the glass plate was immersed in a mixed acid (a mixed solution of H3PO4 (70% by mass) + HNO3 (10% by mass) + CH3COOH (5% by mass) + H2O (15% by mass)) heated to 40°C for 4 minutes, and then washed with water. After washing with water, the water was wiped off and the film was heated on a hot plate at 240°C for 50 minutes and dried. * Measure the change (Δb * The table shows the b * and Δb *Here, b * The measurement was carried out in a state where a polyimide film was formed on a glass plate (a state of glass plate + polyimide film).
[0112] (14) Tensile modulus and tensile elongation (tensile breaking strain) The tensile modulus of elasticity and tensile elongation (tensile breaking strain) were measured in accordance with JIS K7161:2014 and JIS K7127:1999 using a tensile testing machine "Strograph VG-1E" manufactured by Toyo Seiki Co., Ltd. The chuck distance was 50 mm, the test piece size was 10 mm × 70 mm, and the test speed was 20 mm / min.
[0113] The tetracarboxylic acid components and diamine components used in the examples and comparative examples, and their abbreviations, are as follows:
[0114] <Diamine> 3,3'-DDS: 3,3'-bis(aminophenyl)sulfone (manufactured by Seika Corporation; compound represented by formula (b-11)) BAPS: bis[4-(4-aminophenoxy)phenyl]sulfone (manufactured by Seika Corporation; compound represented by formula (b-12)) BAPS-M: bis[4-(3-aminophenoxy)phenyl]sulfone (manufactured by Seika Corporation; compound represented by formula (b-13)) 3,5-DABA: 3,5-diaminobenzoic acid (manufactured by Nippon Junryo Pharmaceutical Co., Ltd.; compound represented by formula (b-2)) X-22-9409: Amino-modified silicone oil on both ends "X-22-9409" (manufactured by Shin-Etsu Chemical Co., Ltd.; compound represented by formula (b-3)) 6FODA: 4,4'-diamino-2,2'-bistrifluoromethyldiphenyl ether (manufactured by ChinaTech Chemical (Tianjin) Co., Ltd.; compound represented by formula (b-4))
[0115] <Tetracarboxylic acid component> CpODA: norbornane-2-spiro-α-cyclopentanone-α'-spiro-2″-norbornane-5,5″,6,6″-tetracarboxylic dianhydride (manufactured by JX Energy Corporation; compound represented by formula (a-1)) HPMDA: 1,2,4,5-cyclohexanetetracarboxylic dianhydride (manufactured by Mitsubishi Gas Chemical Company, Inc.; compound represented by formula (a-2))
[0116] <Crosslinking agent> 1,3-PBO: 1,3-bis(4,5-dihydro-2-oxazolyl)benzene (Mikuni Pharmaceutical Co., Ltd.)
[0117] <Other> GBL: γ-butyrolactone (manufactured by Mitsubishi Chemical Corporation) TEA: Triethylamine (Kanto Chemical Co., Ltd.)
[0118] Example 1 28.793 g (0.066 mol) of BAPS-M, 3.372 g (0.022 mol) of 3,5-DABA, and 125.425 g of GBL were placed in a 300 mL five-neck round-bottom flask equipped with a stainless steel half-moon shaped stirring blade, a nitrogen inlet tube, a Dean-Stark equipped cooling tube, a thermometer, and a glass end cap, and the mixture was stirred at a system temperature of 70°C under a nitrogen atmosphere at a rotation speed of 200 rpm to obtain a solution. To this solution, 35.026g (0.089mol) of CpODA and 35.026g of GBL were added all at once, and 0.784g of TEA was added as an imidization catalyst. The reaction system was heated with a mantle heater and the temperature was raised to 200°C over about 30 minutes. The components that were distilled off were collected, and the temperature in the reaction system was kept at 200°C while adjusting the rotation speed according to the increase in viscosity, and the mixture was refluxed for 4 hours. GBL was then added so that the solid content concentration became 20% by mass, and the temperature in the reaction system was cooled to 100°C, after which the mixture was stirred for about 1 hour to homogenize. Next, 0.755 g of 1,3-PBO (0.5 mol % relative to 1 mol % of 3,5-DABA) was added to 100 g of the obtained varnish, and the mixture was stirred for 30 minutes to homogenize, yielding a polyimide varnish. The resulting polyimide varnish was then applied to a glass plate and a silicon wafer by spin coating, and dried on a hot plate at 120°C for 15 minutes, followed by heating in a hot air dryer at 260°C for 60 minutes in the atmosphere to evaporate the solvent, yielding a film with a thickness of 10 μm.
[0119] Example 2 A 300 mL five-neck round-bottom flask equipped with a stainless steel half-moon stirring blade, a nitrogen inlet tube, a Dean-Stark equipped with a cooling tube, a thermometer, and a glass end cap was charged with 15.007 g (0.045 mol) of 6FODA, 5.564 g (0.022 mol) of 3,3'-DDS, 6.791 g (0.045 mol) of 3,5-DABA, 13.670 g (0.011 mol) of X-22-9409, and 127.679 g of GBL, and the mixture was stirred at 200 rpm under a nitrogen atmosphere at an internal temperature of 70°C to obtain a solution. To this solution, 27.368g (0.122 moles) of HPMDA and 31.920g of GBL were added all at once, and 0.730g of TEA was added as an imidization catalyst. The reaction system was heated with a mantle heater and the temperature was raised to 200°C over about 30 minutes. The components that were distilled off were collected, and the temperature in the reaction system was maintained at 200°C and refluxed for 4 hours while adjusting the rotation speed according to the increase in viscosity. GBL was then added so that the solid content concentration became 20% by mass, and the temperature in the reaction system was cooled to 100°C, after which the mixture was stirred for about 1 hour to homogenize. Next, 1.492 g of 1,3-PBO (0.5 mol % relative to 1 mol % of 3,5-DABA) was added to 100 g of the obtained varnish, and the mixture was stirred for 30 minutes to homogenize, yielding a polyimide varnish. The resulting polyimide varnish was then applied to a glass plate and a silicon wafer by spin coating, and dried on a hot plate at 120°C for 15 minutes, followed by heating in a hot air dryer at 260°C for 60 minutes in the atmosphere to evaporate the solvent, yielding a film with a thickness of 10 μm.
[0120] Example 3 Into a 300 mL five-neck round-bottom flask equipped with a stainless steel half-moon stirring blade, a nitrogen inlet tube, a Dean-Stark equipped with a cooling tube, a thermometer, and a glass end cap, 13.853 g (0.041 mol) of 6FODA, 8.921 g (0.021 mol) of BAPS-M, 6.269 g (0.041 mol) of 3,5-DABA, 13.610 g (0.011 mol) of X-22-9409, and 127.099 g of GBL were added, and the mixture was stirred at a system temperature of 70° C. under a nitrogen atmosphere at a rotation speed of 200 rpm to obtain a solution. To this solution, 25.436g (0.113 moles) of HPMDA and 31.775g of GBL were added all at once, and 0.678g of TEA was added as an imidization catalyst. The reaction system was heated with a mantle heater and the temperature was raised to 200°C over about 30 minutes. The components that were distilled off were collected, and the temperature in the reaction system was maintained at 200°C while adjusting the rotation speed according to the increase in viscosity, and the mixture was refluxed for 4 hours. GBL was then added so that the solid content concentration became 20% by mass, and the temperature in the reaction system was cooled to 100°C, after which the mixture was stirred for about 1 hour to homogenize. Next, 1.384 g of 1,3-PBO (0.5 mol % relative to 1 mol % of 3,5-DABA) was added to 100 g of the obtained varnish, and the mixture was stirred for 30 minutes to homogenize, yielding a polyimide varnish. The resulting polyimide varnish was then applied to a glass plate and a silicon wafer by spin coating, and dried on a hot plate at 120°C for 15 minutes, followed by heating in a hot air dryer at 260°C for 60 minutes in the atmosphere to evaporate the solvent, yielding a film with a thickness of 10 μm.
[0121] Example 4 Into a 300 mL five-neck round-bottom flask equipped with a stainless steel half-moon stirring blade, a nitrogen inlet tube, a Dean-Stark equipped with a cooling tube, a thermometer, and a glass end cap, 14.512 g (0.034 mol) of BAPS, 8.363 g (0.034 mol) of 3,3'-DDS, 2.552 g (0.017 mol) of 3,5-DABA, 6.616 g (0.005 mol) of X-22-9409, and 125.448 g of GBL were added, and the mixture was stirred at a system temperature of 70°C under a nitrogen atmosphere at a rotation speed of 200 rpm to obtain a solution. To this solution, 35.161g (0.089 moles) of CpODA and 31.362g of GBL were added all at once, and 0.619g of TEA was added as an imidization catalyst. The reaction system was heated with a mantle heater and the temperature was raised to 200°C over about 30 minutes. The components that were distilled off were collected, and the temperature in the reaction system was maintained at 200°C while adjusting the rotation speed according to the increase in viscosity, and the mixture was refluxed for 4 hours. After that, GBL was added so that the solid content concentration became 20 mass%, and the temperature in the reaction system was cooled to 100°C, and then the mixture was stirred for about 1 hour to be homogenized. Next, 0.571 g of 1,3-PBO (0.5 mol % relative to 1 mol % of 3,5-DABA) was added to 100 g of the obtained varnish, and the mixture was stirred for 30 minutes to be homogenized, thereby obtaining a polyimide varnish. The resulting polyimide varnish was then applied to a glass plate and a silicon wafer by spin coating, and dried on a hot plate at 120°C for 15 minutes, followed by heating in a hot air dryer at 260°C for 60 minutes in the atmosphere to evaporate the solvent, yielding a film with a thickness of 10 μm.
[0122] Example 5 Into a 300 mL five-neck round-bottom flask equipped with a stainless steel half-moon shaped stirring blade, a nitrogen inlet tube, a Dean-Stark equipped with a cooling tube, a thermometer, and a glass end cap, 17.235 g (0.040 mol) of BAPS, 17.252 g (0.040 mol) of BAPS-M, 3.031 g (0.020 mol) of 3,5-DABA, 6.771 g (0.005 mol) of X-22-9409, and 126.514 g of GBL were added, and the mixture was stirred at a system temperature of 70° C. under a nitrogen atmosphere at a rotation speed of 200 rpm to obtain a solution. To this solution, 23.486g (0.105 mol) of HPMDA and 31.629g of GBL were added all at once, and 0.731g of TEA was added as an imidization catalyst. The reaction system was heated with a mantle heater and the temperature was raised to 200°C over about 30 minutes. The components that were distilled off were collected, and the temperature in the reaction system was maintained at 200°C while adjusting the rotation speed according to the increase in viscosity, and the mixture was refluxed for 4 hours. GBL was then added so that the solid content concentration became 20% by mass, and the temperature in the reaction system was cooled to 100°C, after which the mixture was stirred for about 1 hour to homogenize. Next, 0.672 g of 1,3-PBO (0.5 mol % relative to 1 mol % of 3,5-DABA) was added to 100 g of the obtained varnish, and the mixture was stirred for 30 minutes to homogenize, yielding a polyimide varnish. The resulting polyimide varnish was then applied to a glass plate and a silicon wafer by spin coating, and dried on a hot plate at 120°C for 15 minutes, followed by heating in a hot air dryer at 260°C for 60 minutes in the atmosphere to evaporate the solvent, yielding a film with a thickness of 10 μm.
[0123] The obtained film was subjected to the above evaluations, and the results are shown in Table 1.
[0124] [Table 1]
[0125] As shown in Table 1, the polyimide films of Examples 1 to 5 were excellent in colorless transparency and optical isotropy, and also had excellent peelability from the substrate.
Claims
1. A polyimide resin composition comprising a polyimide resin and a crosslinking agent having at least two oxazolyl groups, the polyimide resin is a polyimide resin having a structural unit A derived from a tetracarboxylic dianhydride and a structural unit B derived from a diamine, The structural unit B includes a structural unit (B-1) derived from a diamine having a sulfonyl group in its structure, and a structural unit (B-2) derived from a compound represented by the following formula (b-2): The polyimide resin composition, wherein the structural unit (B-1) is at least one selected from the group consisting of a structural unit (B-12) derived from a compound represented by the following formula (b-12), and a structural unit (B-13) derived from a compound represented by the following formula (b-13): 【Chemistry 1】 (In formula (b-2), X is a single bond, a substituted or unsubstituted alkylene group, a carbonyl group, an ether group, a group represented by the following formula (b-2-i), or a group represented by the following formula (b-2-ii); p is an integer of 0 to 2; m1 is an integer of 0 to 4; and m2 is an integer of 0 to 4. However, when p is 0, m1 is an integer of 1 to 4.) 【Chemistry 2】 (In formula (b-2-i), m3 is an integer of 0 to 5; in formula (b-2-ii), m4 is an integer of 0 to 5. Note that, m1+m2+m3+m4 is 1 or more, and when p is 2, each of the two Xs and the two m2 to m4 is independently selected.) 【Chemistry 3】
2. The polyimide resin composition according to claim 1, wherein the structural unit (B-2) is a structural unit (B-21) derived from a compound represented by the following formula (b-21): 【Chemistry 4】
3. 3. The polyimide resin composition according to claim 1, wherein the structural unit A comprises at least one selected from the group consisting of a structural unit (A-1) derived from a compound represented by the following formula (a-1), and a structural unit (A-2) derived from a compound represented by the following formula (a-2): 【Chemistry 5】
4. The polyimide resin composition according to any one of claims 1 to 3, wherein the structural unit B further comprises a structural unit (B-3) derived from a compound represented by the following formula (b-3): 【Chemistry 6】 (In formula (b-3), Z 1 and Z 2 each independently represents a divalent aliphatic group or a divalent aromatic group which may contain an oxygen atom; R 1 and R 2 each independently represents a monovalent aromatic group or a monovalent aliphatic group; R 3 and R 4 each independently represents a monovalent aliphatic group; R 5 and R 6 each independently represents a monovalent aliphatic group or a monovalent aromatic group, m and n each independently represent an integer of 1 or more, and the sum of m and n represents an integer of 2 to 1000. 1 and R 2 At least one of represents a monovalent aromatic group.
5. The polyimide resin composition according to any one of claims 1 to 4, wherein the structural unit B further comprises a structural unit (B-4) derived from a compound represented by the following formula (b-4): 【Chemistry 7】
6. 6. The polyimide resin composition according to claim 1, wherein the crosslinking agent is a compound containing an aromatic ring or an aromatic heterocycle to which at least two oxazolyl groups are bonded.
7. 7. The polyimide resin composition according to claim 1, wherein the crosslinking agent is a compound containing a benzene ring having at least two oxazolyl groups bonded thereto.
8. The polyimide resin composition according to any one of claims 1 to 7, wherein the crosslinking agent is 1,3-bis(4,5-dihydro-2-oxazolyl)benzene.
9. A polyimide varnish obtained by dissolving the polyimide resin composition according to any one of claims 1 to 8 in an organic solvent.
10. A polyimide film obtained by crosslinking the polyimide resin in the polyimide resin composition according to any one of claims 1 to 8 with the crosslinking agent.
Citation Information
Patent Citations
Active matrix displays and other electronic devices with plastic substrates
JP2007512568A
Substrate structure applied in flexible electronic device and fabrication method thereof
JP2010067957A
Composition for forming resist overlay film for lithography
JP2015108644A
Method of manufacturing electronic device and electronic device
JP2016021384A
Polyimide resin composition
JP2016222797A
Cited By
Polyimide precursor for display substrate, polyimide film for display substrate and display substrate
KR1020240154650A
Polyimide precursor for display substrate, polyimide film for display substrate, and display substrate
KR103009685B1