Reactive hot melt adhesive, adhesive body and manufacturing method thereof, and clothing

A urethane prepolymer-based reactive hot melt adhesive with optimized carbon atom ratios in C-NMR analysis achieves superior adhesive strength and elasticity, addressing the balance issue in conventional adhesives.

JP7593395B2Active Publication Date: 2024-12-03RESONAC CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2022511403
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-03-31
Publication Date
2024-12-03
Estimated Expiration
2040-03-31

AI Technical Summary

Technical Problem

Conventional reactive hot melt adhesives lack sufficient adhesive strength and elasticity, failing to balance these properties effectively.

Method used

A reactive hot melt adhesive is developed with a urethane prepolymer that satisfies specific integral value ratios of carbon atoms in C-NMR analysis, enhancing adhesive strength and elasticity by adjusting the proportion of structural units derived from polyester polyols.

Benefits of technology

The adhesive exhibits excellent adhesive strength and elasticity, improving bonding performance in applications such as clothing and other adherends.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007593395000004
    Figure 0007593395000004
  • Figure 0007593395000005
    Figure 0007593395000005
  • Figure 0007593395000006
    Figure 0007593395000006
Patent Text Reader

Abstract

A reactive hot-melt adhesive that contains a urethane prepolymer. When C(A) is the integral value of the peak observed at 163–170 ppm during 13C-NMR analysis of the urethane prepolymer, and C(B) is the integral value of the peak observed at 171–176 ppm, C(A) and C(B) satisfy expression (X). (X) 0.36≤C(A) / (C(A)+C(B)).
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to reactive hot melt adhesives, adhesive bodies and methods for producing the same, and garments. [Background technology]

[0002] Hot melt adhesives are solvent-free, so they are less harmful to the environment and the human body, and can bond in a short time, making them suitable for improving productivity. Hot melt adhesives can be broadly divided into two types: those that use thermoplastic resins as the main component, and those that use reactive resins as the main component. Urethane prepolymers with isocyanate groups at the terminals are mainly used as reactive resins.

[0003] Reactive hot melt adhesives whose main component is urethane prepolymers exhibit a certain degree of adhesive strength in a short time after application, as the adhesive itself cools and hardens. The terminal isocyanate groups of the urethane prepolymer then react with moisture (in the air or on the surface of the adherend), increasing the molecular weight and causing crosslinking, which results in heat resistance. Such adhesives are called moisture-curing reactive hot melt adhesives. Reactive hot melt adhesives whose main component is urethane prepolymers exhibit good adhesive strength even when heated.

[0004] For example, Patent Document 1 discloses a reactive hot melt adhesive comprising a urethane prepolymer formed from polyisocyanate (a) and polyol (b) consisting of aromatic ring-containing polyether polyol (b1) and / or aromatic ring-containing polyester polyol (b2), and aliphatic polyester polyol (b3). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2008-063568 A Summary of the Invention [Problem to be solved by the invention]

[0006] In recent years, various reactive hot melt adhesives have been used with the diversification of wearable terminals and the like. However, in reactive hot melt adhesives, there is a trade-off between adhesive strength and elasticity, and it is extremely important to achieve both. However, conventional reactive hot melt adhesives have not yet achieved a sufficient balance between adhesive strength and elasticity, and there is room for further improvement.

[0007] Therefore, a main object of the present disclosure is to provide a reactive hot melt adhesive that has excellent adhesive strength and excellent elasticity. [Means for solving the problem]

[0008] In order to solve the above problems, the present inventors have 13 The inventors conducted a C-NMR analysis to examine the constituent units contained in the urethane prepolymer and found that a urethane prepolymer in which the integral values ​​of peaks observed in a specified range are in a specified ratio tends to have excellent adhesive strength and excellent elasticity, which led to the completion of the invention of the present disclosure.

[0009] One aspect of the present disclosure relates to a reactive hot melt adhesive. The reactive hot melt adhesive contains a urethane prepolymer. The urethane prepolymer comprises: 13 In the C-NMR analysis, when the integral value of the peak observed in the range of 163 to 170 ppm is C(A) and the integral value of the peak observed in the range of 171 to 176 ppm is C(B), C(A) and C(B) satisfy the following formula (X). Such a reactive hot melt adhesive has excellent adhesive strength and excellent elasticity. 0.36≦C(A) / (C(A)+C(B)) (X)

[0010] In this specification 13C-NMR analysis was performed using a nuclear magnetic resonance spectrometer (NMR) manufactured by Bruker Japan Co., Ltd., AVANCE NEO (probe: CryoProbe TM ) under the following measurement conditions. (Measurement conditions) · 13 C-NMR quantitative spectroscopy: inverse gate decoupling method ·Resonance frequency: 100MHz Waiting time (d1): 5 seconds Solvent: deuterated chloroform (CDCl3) Sample concentration: 100mg / 0.6ml-CDCl3, also containing 10mgCr(acac)3 as a relaxation reagent Chemical shift reference: Tetramethylsilane (TMS) peak set to 0.00 ppm ·Measurement temperature: 23℃ -Number of times: 400

[0011] Regarding the method of taking the integral value, for example, the integral value of each peak observed in the range of 163 to 170 ppm can be measured, and the sum of these integral values ​​can be taken as C(A). However, since it is easy to obtain the integral value and arbitrariness can be reduced, the integral value of the entire range of 163 to 170 ppm can be measured at once, and the integral value can be taken as C(A) (see, for example, Figures 2 and 3). The same applies to C(B) and C(C). That is, the integral value of the peak observed in the range of 163 to 170 ppm, the integral value of the peak observed in the range of 171 to 176 ppm, and the integral value of the peak observed in the range of 150 to 155 ppm can be the integral value of all peaks from 163 to 170 ppm, the integral value of all peaks from 171 to 176 ppm, and the integral value of all peaks from 150 to 155 ppm, respectively.

[0012] The urethane prepolymer may be, for example, a urethane prepolymer having an isocyanate group. The urethane prepolymer having an isocyanate group usually has a polymer chain including a structural unit derived from a polyol and a structural unit derived from a polyisocyanate, and an isocyanate group. The isocyanate group may be bonded to the end of the polymer chain.13 In the C-NMR analysis, the peak observed in the range of 160 to 180 ppm is mainly a peak attributable to the carbon atom of the carbonyl group of the ester bond of the structural unit derived from the polyester polyol in the structural unit derived from the polyol constituting the urethane prepolymer. The peak observed in the range of 163 to 170 ppm is a peak attributable to the carbon atom of the carbonyl group directly bonded to the carbon atom constituting the aromatic ring among the carbon atoms of the carbonyl group of the ester bond of the polyester polyol (hereinafter, the carbon atom may be referred to as "carbon atom (A)"). The peak observed in the range of 171 to 176 ppm is a peak attributable to the carbon atom of the carbonyl group directly bonded to the carbon atom constituting the aliphatic group among the carbon atoms of the carbonyl group of the ester bond of the polyester polyol (hereinafter, the carbon atom may be referred to as "carbon atom (B)". The carbon atom (A) may be, for example, a carbon atom represented by the following formula (1), and the carbon atom (B) may be, for example, a carbon atom represented by the following formula (2). The integral value of the peak attributable to the carbon atom of the carbonyl group of the ester bond of the structural unit derived from the polyester polyol (corresponding to the above (C(A)+C(B))) can be the sum of the integral value of the peak attributable to the carbon atom (A) (corresponding to the above C(A)) and the integral value of the peak attributable to the carbon atom (B) (corresponding to the above C(B)). Therefore, C(A) / (C(A)+C(B)) in the above formula (X) means the ratio of the total amount of carbon atoms (A) to the sum of the total amount of carbon atoms (A) and the total amount of carbon atoms (B) (total amount of carbon atoms (A) / sum of the total amount of carbon atoms (A) and the total amount of carbon atoms (B)). It can be said that the larger C(A) / (C(A)+C(B)), the larger the proportion of carbon atoms (A) in the structural unit derived from the polyester polyol constituting the urethane prepolymer (i.e., the larger the proportion of aromatic rings contained in the polyester polyol).

[0013] [ka]

[0014] The polyester polyol may be a polycondensation reaction product of a polyhydric alcohol and a polycarboxylic acid. In this case, the carbon atom (A) and the carbon atom (B) are carbon atoms derived from the polycarboxylic acid. The carbon atom (A) is a carbon atom of a carbonyl group (of the carboxylic acid) that is directly bonded to a carbon atom that constitutes an aromatic ring among the carbon atoms derived from the polycarboxylic acid. The carbon atom (B) is a carbon atom of a carbonyl group (of the carboxylic acid) that is directly bonded to a carbon atom that constitutes an aliphatic group among the carbon atoms derived from the polycarboxylic acid. C(A) / (C(A)+C(B)) in the formula (X) tends to be adjusted mainly by changing the type and content of the polycarboxylic acid that constitutes the structural unit derived from the polyester polyol, and the type and content of the polyester polyol derived from the polycarboxylic acid.

[0015] The urethane prepolymer is 13 In a C-NMR analysis, when the integral value of a peak observed in the range of 150 to 155 ppm is defined as C(C), C(A) and C(C) may satisfy the following formula (Y). 3.6≦C(A) / C(C) (Y)

[0016] 13In the C-NMR analysis, the peak observed in the range of 160 to 180 ppm is mainly a peak attributable to the carbon atom of the carbonyl group of the urethane bond formed by the reaction of the polyol of the urethane prepolymer with the polyisocyanate (hereinafter, the carbon atom may be referred to as "carbon atom (C)"). The carbon atom (C) may be, for example, a carbon atom represented by the following formula (3). In the above formula (Y), C(A) / C(C) means the ratio of the total amount of carbon atoms (A) to the total amount of carbon atoms (C) (total amount of carbon atoms (A) / total amount of carbon atoms (C)). It can be said that the larger the C(A) / C(C), the larger the proportion of carbon atoms (A) per carbon atom (C) in the urethane prepolymer (i.e., the larger the proportion of aromatic rings contained in the polyester polyol per urethane bond). C(A) / C(C) in formula (Y), like C(A) / (C(A)+C(B)) in formula (X), tends to be adjustable mainly by changing the type and content of the polycarboxylic acid constituting the structural unit derived from the polyester polyol, and the type and content of the polyester polyol derived from the polycarboxylic acid.

[0017] [ka]

[0018] Another aspect of the present disclosure relates to a reactive hot melt adhesive. The reactive hot melt adhesive contains a urethane prepolymer having a polymer chain including a structural unit derived from a polyol and a structural unit derived from a polyisocyanate, and an isocyanate group bonded to the end of the polymer chain. The urethane prepolymer is 13 In the C-NMR analysis, when the integral value of the peak observed in the range of 163 to 170 ppm is C(A) and the integral value of the peak observed in the range of 150 to 155 ppm is C(C), C(A) and C(C) satisfy the following formula (Y). Such a reactive hot melt adhesive has excellent adhesive strength and excellent elasticity. 3.6≦C(A) / C(C) (Y)

[0019] The structural unit derived from a polyol may include a structural unit derived from a polyester polyol having an aromatic ring.

[0020] The reactive hot melt adhesive may be used to bond a plurality of adherends selected from cloth and paper to each other. Here, the combination of adherends may be cloth and cloth, paper and paper, or cloth and paper. The present disclosure may further relate to the application of the composition containing the above-mentioned urethane prepolymer as a reactive hot melt adhesive used to bond a plurality of adherends selected from cloth and paper to each other, or to the application for the manufacture of a reactive hot melt adhesive used to bond a plurality of adherends selected from cloth and paper to each other.

[0021] Another aspect of the present disclosure relates to an adhesive structure comprising a first adherend, a second adherend, and an adhesive layer that bonds the first adherend and the second adherend to each other. The adhesive layer contains a cured product of the reactive hot melt adhesive.

[0022] Another aspect of the present disclosure relates to a garment. The garment includes the above-mentioned adhesive body, and the first adherend and the second adherend may be fabrics. The garment may be a seamless garment.

[0023] Another aspect of the present disclosure relates to a method for producing an adhesive body, which includes the steps of forming an adhesive layer by melting the reactive hot melt adhesive and applying it to a first adherend, arranging a second adherend on the adhesive layer and pressing the second adherend to obtain a laminate, and curing the adhesive layer in the laminate to obtain the adhesive body. Effect of the Invention

[0024] According to the present disclosure, there is provided a reactive hot melt adhesive having excellent adhesive strength and excellent elasticity. According to the present disclosure, there is also provided an adhesive body using such a reactive hot melt adhesive and a manufacturing method thereof. Furthermore, according to the present disclosure, there is provided a garment including the adhesive body. [Brief description of the drawings]

[0025] [Figure 1] FIG. 1 is a schematic diagram showing a method for producing a bonded body according to one embodiment, and FIGS. 1(a), (b), (c), and (d) are schematic diagrams showing the respective steps. [Diagram 2] FIG. 2 is a 13C-NMR spectrum of urethane prepolymer B of Production Example 2 in the range of 150 to 180 ppm. [Diagram 3] FIG. 3 is a 13C-NMR spectrum of urethane prepolymer E of Production Example 5 in the range of 150 to 180 ppm. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0026] Hereinafter, embodiments of the present disclosure will be described in detail. However, the present disclosure is not limited to the following embodiments.

[0027] As used herein, "polyol" refers to a compound having two or more hydroxy groups in the molecule.

[0028] In this specification, "polyisocyanate" means a compound having two or more isocyanate groups in the molecule.

[0029] In this specification, "amorphous" and "crystalline" can be judged based on the presence or absence of a melting point (Tm) (an endothermic peak associated with melting in DSC), and "crystalline" refers to a material having a melting point (Tm), and "amorphous" refers to a material not having a melting point (Tm). In this specification, "amorphous polyester polyol" refers to a polyester polyol not having a melting point (Tm), and "crystalline polyester polyol" refers to a polyester polyol having a melting point (Tm).

[0030] [Reactive hot melt adhesive] The reactive hot melt adhesive of one embodiment contains a urethane prepolymer. In general, reactive hot melt adhesives are polymerized by chemical reaction and can exhibit adhesive strength. In particular, since a urethane prepolymer having an isocyanate group reacts with moisture to harden (to form a hardened product), the urethane prepolymer alone can act as a reactive hot melt adhesive, but the reactive hot melt adhesive may contain components other than the urethane prepolymer.

[0031] <Urethane prepolymer> The urethane prepolymer may be, for example, a urethane prepolymer having an isocyanate group. The urethane prepolymer having an isocyanate group usually has a polymer chain containing a structural unit derived from a polyol and a structural unit derived from a polyisocyanate, and an isocyanate group. The isocyanate group may be bonded to the end of the polymer chain. The structural unit derived from a polyol may contain a structural unit derived from a polyester polyol. The urethane prepolymer having a structural unit derived from a polyester polyol can usually be obtained by reacting a polyol containing a polyester polyol with a polyisocyanate. That is, the urethane prepolymer may be a reaction product of a polyol containing a polyester polyol and a polyisocyanate. The content of the structural unit can be adjusted by changing the mixing ratio of the polyester polyol that provides the structural unit and the polyol other than the polyester polyol that provides the structural unit. In addition, since a urethane bond is formed by the reaction of a polyol with a polyisocyanate, the polymer chain of the urethane prepolymer may have a urethane bond. Also, by increasing the equivalent weight of polyisocyanate relative to the equivalent weight of polyol, an isocyanate group can be introduced at the end of the polymer chain.

[0032] The urethane prepolymer is 13 In the C-NMR analysis, when the integral value of the peak observed in the range of 163 to 170 ppm is C(A) and the integral value of the peak observed in the range of 171 to 176 ppm is C(B), C(A) and C(B) satisfy the following formula (X). A reactive hot melt adhesive containing such a urethane prepolymer has excellent adhesive strength and excellent elasticity. 0.36≦C(A) / (C(A)+C(B)) (X)

[0033] C(A) / (C(A)+C(B)) means the ratio of the total amount of carbon atoms (A) to the sum of the total amount of carbon atoms (A) and the total amount of carbon atoms (B) (total amount of carbon atoms (A) / sum of the total amount of carbon atoms (A) and the total amount of carbon atoms (B)). It can be said that the larger C(A) / (C(A)+C(B)) is, the larger the proportion of carbon atoms (A) in the structural units derived from the polyester polyol that constitutes the urethane prepolymer is (i.e., the larger the proportion of aromatic rings contained in the polyester polyol is).

[0034] C(A) / (C(A)+C(B)) is 0.36 or more, and may be 0.38 or more, or 0.40 or more. When C(A) / (C(A)+C(B)) is 0.36 or more, the reactive hot melt adhesive tends to have excellent adhesive strength and excellent elasticity. The upper limit of C(A) / (C(A)+C(B)) may be 1.00 or less, 0.95 or less, 0.90 or less, 0.85 or less, 0.80 or less, 0.75 or less, 0.70 or less, 0.65 or less, or 0.60 or less, since the adhesive strength is more excellent.

[0035] The urethane prepolymer is 13 In a C-NMR analysis, when the integral value of a peak observed in the range of 150 to 155 ppm is defined as C(C), C(A) and C(C) may satisfy the following formula (Y). 3.6≦C(A) / C(C) (Y)

[0036] C(A) / C(C) means the ratio of the total amount of carbon atoms (A) to the total amount of carbon atoms (C) (total amount of carbon atoms (A) / total amount of carbon atoms (C)). It can be said that the larger the C(A) / C(C), the higher the proportion of carbon atoms (A) per carbon atom (C) in the urethane prepolymer (i.e., the greater the proportion of aromatic rings contained in the polyester polyol per urethane bond).

[0037] C(A) / C(C) may be 3.6 or more, 3.8 or more, or 4.0 or more. When C(A) / C(C) is 3.6 or more, the reactive hot melt adhesive tends to have better adhesive strength and better stretchability. The upper limit of C(A) / C(C) may be 10 or less, 8 or less, 7 or less, 6.5 or less, or 6 or less, since the adhesive strength is even better.

[0038] C(A) / (C(A)+C(B)) in formula (X) and C(A) / C(C) in formula (Y) tend to be adjusted mainly by changing the type and content of the polycarboxylic acid constituting the structural unit derived from the polyester polyol, and the type and content of the polyester polyol derived from the polycarboxylic acid. The structural unit derived from the polyol is not particularly limited in type and content, as long as the urethane prepolymer satisfies formula (X) and further formula (Y). According to the study by the present inventors, it was found that the urethane prepolymer tends to easily satisfy formula (X) and formula (Y) when the structural unit derived from the polyol has a high ratio of structural units derived from the polyester polyol having an aromatic ring. In the following, the polyol and polyisocyanate constituting the urethane prepolymer will be described using the urethane prepolymer containing such structural units as an example.

[0039] Component (a): Polyol The constituent units derived from the component (a) include constituent units derived from a polyester polyol having an aromatic ring (hereinafter, may be referred to as "component (a1)"). The constituent units derived from the component (a) may further include constituent units derived from a polyol other than the polyester polyol having an aromatic ring (hereinafter, may be referred to as "component (a2)").

[0040] The polyester polyol having an aromatic ring may be a crystalline polyester polyol having a melting point (Tm) or an amorphous polyester polyol not having a melting point (Tm), but may be an amorphous polyester polyol.

[0041] The polymer chain contains a structural unit derived from the (a1) component, so that the solidification time and viscosity of the reactive hot melt adhesive can be adjusted. The (a1) component may be a polycondensation reaction product of a polyhydric alcohol and a polycarboxylic acid. The (a1) component may be a linear polyester diol produced from a diol and a dicarboxylic acid, or a branched polyester triol produced from a triol and a dicarboxylic acid. The branched polyester triol can also be obtained by the reaction of a diol and a tricarboxylic acid.

[0042] Examples of polyhydric alcohols include aliphatic or alicyclic diols such as ethylene glycol, 1,2-propanediol, 1,3-propanediol, isomers of butanediol, isomers of pentanediol, isomers of hexanediol, 2,2-dimethyl-1,3-propanediol, 2-methylpropanediol, 2,4,4-trimethyl-1,6-hexanediol, 2,2,4-trimethyl-1,6-hexanediol, 1,4-cyclohexanediol, and 1,4-cyclohexanedimethanol; and aromatic diols (diols having an aromatic ring) such as 4,4'-dihydroxydiphenylpropane, bisphenol A, bisphenol F, pyrocatechol, resorcinol, and hydroquinone. The polyhydric alcohol may be used alone or in combination of two or more. Among these, aliphatic diols are preferable, and aliphatic diols having 2 to 6 carbon atoms are more preferable.

[0043] Examples of polycarboxylic acids include polycarboxylic acids in which the carbon atom of the carbonyl group (of the carboxylic acid) is directly bonded to the carbon atom constituting the aromatic ring, such as phthalic acid, isophthalic acid, terephthalic acid, and 1,2,4-benzenetricarboxylic acid (hereinafter, sometimes referred to as "aromatic polycarboxylic acid"); and polycarboxylic acids in which the carbon atom of the carbonyl group (of the carboxylic acid) is directly bonded to the carbon atom constituting the aliphatic group, such as maleic acid, fumaric acid, aconitic acid, 1,2,3-propanetricarboxylic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, azelaic acid, sebacic acid, cyclohexane-1,2-dicarboxylic acid, and 1,4-cyclohexanediene-1,2-dicarboxylic acid (hereinafter, sometimes referred to as "aliphatic polycarboxylic acid"). The aromatic polycarboxylic acid may be a polycarboxylic acid in which the carbon atom of the carbonyl group (of the carboxylic acid) is directly bonded to the carbon atom constituting the benzene ring, and may be at least one selected from the group consisting of phthalic acid, isophthalic acid, and terephthalic acid. The polycarboxylic acid may be used alone or in combination of two or more. The C(A) / (C(A)+C(B)) in formula (X) and the C(A) / C(C) in formula (Y) can be adjusted by adjusting the proportion of the aromatic polycarboxylic acid.

[0044] Instead of polycarboxylic acid, polycarboxylic acid derivatives such as carboxylic acid anhydrides and compounds in which a part of the carboxyl group is esterified can be used. Examples of polycarboxylic acid derivatives include phthalic anhydride, dimethyl terephthalate, dodecyl maleic acid, and octadecenyl maleic acid.

[0045] The (a1) component may be a polycondensation reaction product of a polyhydric alcohol and a polycarboxylic acid, including an aromatic polycarboxylic acid.

[0046] In the polycondensation reaction product of a polyhydric alcohol and a polycarboxylic acid, the content of the structural unit derived from an aromatic polycarboxylic acid may be, for example, 10 to 60 mol% based on the total amount of the structural units constituting the component (a1) (polycondensation reaction product). The content of the structural unit derived from a compound having an aromatic ring may be 15 mol% or more, or 20 mol% or more, and may be 55 mol% or less, or 50 mol% or less, based on the total amount of the structural units constituting the component (a1).

[0047] When the component (a1) is a polycondensation reaction product of a polyhydric alcohol and a polycarboxylic acid including an aromatic polycarboxylic acid (a polycarboxylic acid having an aromatic ring, preferably at least one selected from the group consisting of phthalic acid, isophthalic acid, and terephthalic acid), the content of structural units derived from aromatic polycarboxylic acid may be 20 to 100 mol %, 25 to 100 mol %, or 30 to 100 mol % based on the total amount of structural units derived from polycarboxylic acid.

[0048] From the viewpoint of adhesive strength, the number average molecular weight (Mn) of the (a1) component may be 500 to 12000. The number average molecular weight (Mn) of the (a1) component may be 1000 or more, 1500 or more, or 1800 or more, and may be 11000 or less, 10000 or less, or 9000 or less. In this specification, Mn is a value measured by gel permeation chromatography (GPC) and converted into standard polystyrene.

[0049] In this specification, the GPC measurement for determining the number average molecular weight (Mn) can be carried out, for example, under the following conditions. Columns: "Gelpack GLA130-S", "Gelpack GLA150-S" and "Gelpack GLA160-S" (Hitachi Chemical Co., Ltd., HPLC packed columns) Eluent: Tetrahydrofuran Flow rate: 1.0mL / min Column temperature: 40℃ Detector: RI

[0050] The content of the (a1) component (constituent unit derived from the (a1) component) may be 50% by mass or more, 55% by mass or more, 60% by mass or more, 65% by mass or more, 70% by mass or more, or 75% by mass or more based on the total amount of the (a) component (constituent unit derived from the (a) component). When the content of the (a1) component is 50% by mass or more based on the total amount of the (a) component, the resulting urethane prepolymer (reactive hot melt adhesive) tends to have excellent initial adhesive strength. On the other hand, the upper limit of the content of the (a1) component (constituent unit derived from the (a1) component) may be 100% by mass or less, 95% by mass or less, or 90% by mass or less based on the total amount of the (a) component (constituent unit derived from the (a) component) from the viewpoint of workability.

[0051] The content of component (a1) (a constituent unit derived from component (a1)), which has superior adhesive strength and superior elasticity, may be 50 mol% or more, 55 mol% or more, 60 mol% or more, 65 mol% or more, 70 mol% or more, or 75 mol% or more, or may be 100 mol% or less, 95 mol% or less, or 90 mol% or less, when the total amount of component (a) (a constituent unit derived from component (a)) is taken as 100 mol%.

[0052] The component (a2) is a polyol other than a polyester polyol having an aromatic ring. Examples of the component (a2) include polyester polyols, polyether polyols, polyether ester polyols, polyurethane polyols, polycarbonate polyols, and polyolefin polyols having no aromatic ring.

[0053] The (a) component may contain a polyether polyol having an aromatic ring as the (a2) component from the viewpoint of improving the initial adhesive strength. The polyether polyol having an aromatic ring may be an amorphous polyether polyol. The polyether polyol having an aromatic ring may be a polyether polyol having a bisphenol skeleton, and the bisphenol skeleton may be a bisphenol A skeleton or a bisphenol F skeleton. The polyether polyol having a bisphenol A skeleton or a bisphenol F skeleton may be a polyether polyol obtained by modifying bisphenol A or bisphenol F with an alkylene oxide, more specifically, a polyether polyol obtained by modifying bisphenol A or bisphenol F with ethylene oxide or propylene oxide. The (a) component tends to have a better adhesive strength by containing such a polyether polyol having a bisphenol skeleton as the (a2) component.

[0054] The content of the polyether polyol having a bisphenol skeleton may be 0 to 10 mass% based on the total amount of component (a) (structural units derived from component (a)), and may be 1 mass% or more, 2 mass% or more, or 3 mass% or more, and may be 8 mass% or less, 6 mass% or less, or 5 mass% or less.

[0055] The content of the polyether polyol having an aromatic ring with a bisphenol skeleton may be 0 to 10 mol %, or may be 1 mol % or more, 2 mol % or more, or 3 mol % or more, and may be 8 mol % or less, 6 mol % or less, or 5 mol % or less, when the total amount of component (a) (structural units derived from component (a)) is taken as 100 mol %.

[0056] From the viewpoint of reducing the viscosity of the urethane prepolymer, the number average molecular weight (Mn) of the (a2) component may be 100 to 10,000. The number average molecular weight (Mn) of the (a2) component may be 400 or more or 1,000 or more, and may be 8,000 or less or 5,000 or less. In this specification, Mn is a value measured by gel permeation chromatography (GPC) and converted into standard polystyrene.

[0057] The content of component (a2) (structural unit derived from component (a2)) based on the total amount of component (a) (structural unit derived from component (a)) may be 0 to 50 mass%, may be 5 mass% or more, or 10 mass% or more, and may be 45 mass% or less, 40 mass% or less, 35 mass% or less, 30 mass% or less, or 25 mass% or less.

[0058] The content of the component (a2) (a structural unit derived from the component (a2)) may be 0 to 50 mol%, 5 mol% or more, or 10 mol% or more, or may be 45 mol% or less, 40 mol% or less, 35 mol% or less, 30 mol% or less, or 25 mol% or less, when the total amount of the component (a) (a structural unit derived from the component (a)) is taken as 100 mol%.

[0059] (b) Component: Polyisocyanate The polyisocyanate can be used without any particular limitation as long as it is a compound having two or more isocyanate groups. The polyisocyanate may be a compound (diisocyanate) having two isocyanate groups. Examples of the polyisocyanate include aromatic isocyanates such as diphenylmethane diisocyanate (4,4'-diphenylmethane diisocyanate), dimethyldiphenylmethane diisocyanate, tolylene diisocyanate, xylylene diisocyanate, and p-phenylene diisocyanate; alicyclic isocyanates such as dicyclohexylmethane diisocyanate and isophorone diisocyanate; and aliphatic isocyanates such as hexamethylene diisocyanate. From the viewpoint of reactivity and adhesive strength, the polyisocyanate preferably contains an aromatic diisocyanate, and more preferably contains diphenylmethane diisocyanate. The polyisocyanate may be used alone or in combination of two or more.

[0060] The urethane prepolymer can be synthesized by reacting the (a) component containing the (a1) component at a predetermined content with the (b) component. The urethane prepolymer has a polymer chain containing a structural unit derived from the (a) component containing a structural unit derived from the (a1) component, and a structural unit derived from the (b) component, and an isocyanate group bonded to the end of the polymer chain. When synthesizing such a urethane prepolymer, the equivalent ratio of the isocyanate group (NCO) of the (b) component to the hydroxyl group (OH) of the (a) component (isocyanate group (NCO) equivalent of the (b) component / hydroxyl group (OH) equivalent of the (a) component, NCO / OH) may be 1.1 or more, and may be 1.1 to 2.1. When the NCO / OH is 1.1 or more, the urethane prepolymer has an isocyanate group bonded to the end of the polymer chain, and the increase in the viscosity of the urethane prepolymer can be suppressed, which tends to further improve the workability. When the NCO / OH ratio is 2.1 or less, foaming is less likely to occur during the moisture curing reaction of the reactive hot melt adhesive, and a decrease in adhesive strength tends to be more easily suppressed.

[0061] The temperature and time for reacting the components (a) and (b) when synthesizing the urethane prepolymer are not particularly limited, but may be, for example, 85 to 120° C. and 0.1 minutes to 48 hours.

[0062] The urethane prepolymer may satisfy both of the following conditions (i) and (ii): A reactive hot melt adhesive containing such a urethane prepolymer has excellent initial adhesive strength and excellent workability. Condition (i): The melt viscosity at 120°C is 1 to 30 Pa·s. Condition (ii): The melt viscosity at 80°C is 100 Pa s or more.

[0063] Regarding condition (i), the melt viscosity of the urethane prepolymer at 120°C is 1 to 30 Pa·s. When the melt viscosity of the urethane prepolymer at 120°C is 1 to 30 Pa·s, the viscosity is sufficiently low, and the workability (dischargeability in coating, spinnability, etc.) is excellent. The melt viscosity at 120°C may be 3 Pa·s or more, 5 Pa·s or more, 7 Pa·s or more, or 10 Pa·s or more, or may be 28 Pa·s or less, 25 Pa·s or less, 20 Pa·s or less, or 15 Pa·s or less.

[0064] Regarding condition (ii), the melt viscosity of the urethane prepolymer at 80°C is 100 Pa·s or more. When the melt viscosity of the urethane prepolymer at 80°C is 100 Pa·s or more, the viscosity required for adhesive strength is developed early, resulting in excellent initial adhesive strength. The melt viscosity at 80°C may be 110 Pa·s or more, 120 Pa·s or more, 130 Pa·s or more, or 140 Pa·s or more. The upper limit of the melt viscosity at 80°C is not particularly limited, but may be, for example, 1000 Pa·s or less, 800 Pa·s or less, 600 Pa·s or less, 500 Pa·s or less, or 400 Pa·s or less. The melt viscosity at 120°C is measured using a rotational rheometer device.

[0065] The melt viscosities of the urethane prepolymer at 120°C and 80°C are measured using a rotational rheometer, for example, by the following method. Separate samples are prepared for measuring the melt viscosity at 120°C and at 80°C. The measuring device and conditions are as follows: Rotational rheometer: DHR-2 (TA Instruments Japan, Inc.) Geometry: Φ20mm(2°) cone plate GAP: 57μm Shear rate: 33 (1 / s) Melt viscosity at 120°C: Measured value obtained after incubating urethane prepolymer (reactive hot melt adhesive) at 120°C for 5 minutes Melt viscosity at 80°C: Measured value obtained after incubating urethane prepolymer (reactive hot melt adhesive) at 80°C for 5 minutes

[0066] The melt viscosity of the urethane prepolymer can be adjusted mainly by changing the type and content of the structural unit derived from the polyol. The structural unit derived from the polyol is not particularly limited in type and content, as long as the urethane prepolymer satisfies the conditions (i) and (ii). According to the study by the present inventors, it has been found that when the structural unit derived from the polyol contains a structural unit derived from a polyester polyol having an aromatic ring, the urethane prepolymer tends to easily satisfy the conditions (i) and (ii), and further, the urethane prepolymer that satisfies the conditions (i) and (ii) tends to easily satisfy the formula (X) and the formula (Y).

[0067] The reactive hot melt adhesive may further contain a catalyst from the viewpoint of promoting the curing of the urethane prepolymer and exhibiting higher adhesive strength. Examples of the catalyst include dibutyltin dilaurate, dibutylthione octate, dimethylcyclohexylamine, dimethylbenzylamine, trioctylamine, dimorpholinodiethyl ether (bis(2-morpholinoethyl)ether), etc. The content of the catalyst may be 0.001 to 0.5 mass% based on the total amount of the reactive hot melt adhesive.

[0068] The reactive hot melt adhesive may further contain a thermoplastic polymer from the viewpoint of increasing the rubber elasticity of the formed adhesive layer and further improving the impact resistance. Examples of the thermoplastic polymer include polyurethane, ethylene copolymer, propylene copolymer, vinyl chloride copolymer, acrylic copolymer, styrene-conjugated diene block copolymer, etc. The content of the thermoplastic polymer may be 0.1 to 50 mass% based on the total amount of the reactive hot melt adhesive.

[0069] The reactive hot melt adhesive may further contain a tackifier resin from the viewpoint of imparting stronger adhesive strength to the adhesive layer formed. Examples of the tackifier resin include rosin resin, rosin ester resin, hydrogenated rosin ester resin, terpene resin, terpene phenol resin, hydrogenated terpene resin, petroleum resin, hydrogenated petroleum resin, coumarone resin, ketone resin, styrene resin, modified styrene resin, xylene resin, and epoxy resin. The content of the tackifier resin may be 0.1 to 50 mass% based on the total amount of the reactive hot melt adhesive.

[0070] The reactive hot melt adhesive may further contain other components as necessary. Examples of the other components include antioxidants, pigments, ultraviolet absorbers, surfactants, flame retardants, fillers, photocoloring agents, thermal coloring inhibitors, fragrances, imaging agents, thermal crosslinking agents, etc. The content of the other components may be 0.001 to 10 mass% based on the total amount of the reactive hot melt adhesive.

[0071] The reactive hot melt adhesive may be composed of a urethane prepolymer alone or may contain other components in addition to the urethane prepolymer. When the reactive hot melt adhesive is composed of a urethane prepolymer alone, if the urethane prepolymer satisfies both conditions (i) and (ii), the reactive hot melt adhesive also satisfies both conditions (i) and (ii). Even when the reactive hot melt adhesive contains other components in addition to the urethane prepolymer, the reactive hot melt adhesive can be excellent in initial adhesive strength and excellent workability by containing a urethane prepolymer that satisfies both conditions (i) and (ii), and the reactive hot melt adhesive can satisfy both conditions (i) and (ii). Furthermore, a reactive hot melt adhesive containing any urethane prepolymer and other components can be excellent in initial adhesive strength and excellent workability by satisfying both conditions (i) and (ii).

[0072] That is, the reactive hot melt adhesive may satisfy both of the following conditions (i) and (ii): The reactive hot melt adhesive may contain a urethane prepolymer. Condition (i): The melt viscosity at 120°C is 1 to 30 Pa·s. Condition (ii): The melt viscosity at 80°C is 100 Pa s or more.

[0073] The preferred ranges of the melt viscosity of the reactive hot melt adhesive at 120°C and at 80°C are the same as the preferred ranges of the melt viscosity of the above-mentioned urethane prepolymer at 120°C and at 80°C. The measurement conditions of the melt viscosity of the reactive hot melt adhesive are also the same as the measurement conditions of the melt viscosity of the urethane prepolymer. Therefore, a duplicated description will be omitted here.

[0074] The content of the urethane prepolymer based on the total amount of the reactive hot melt adhesive may be 80% by mass or more, 85% by mass or more, 90% by mass or more, 92% by mass or more, 95% by mass or more, or 97% by mass or more, or may be 100% by mass. By adjusting the melt viscosity of the urethane prepolymer, it becomes easy to adjust the melt viscosity of the reactive hot melt adhesive to one that satisfies both conditions (i) and (ii). In addition, when the melt viscosity of the urethane prepolymer satisfies both conditions (i) and (ii), the melt viscosity of the reactive hot melt adhesive also easily satisfies both conditions (i) and (ii).

[0075] The reactive hot melt adhesive can be cured, for example, by leaving it for 24 hours (curing) at a temperature of 23°C and 50% RH (relative humidity) because the isocyanate group of the urethane prepolymer contained in the reactive hot melt adhesive reacts with moisture in the air or moisture on the surface of the adherend. In this way, a cured product of the reactive hot melt adhesive can be obtained.

[0076] The reactive hot melt adhesive can be used by, for example, melting at 60 to 130°C and then applying it to the adherend. The application method is not particularly limited, but examples thereof include methods using application devices such as a bar coater, a die coater, a roll coater, and a sprayer. A dispenser is suitable for application to small areas such as small parts. The application pattern of the reactive hot melt adhesive can be appropriately set, but examples thereof include application patterns such as dots, straight lines, zigzags, planes, and curves.

[0077] The reactive hot melt adhesive can bond various adherends via the cured product (adhesive layer) of the reactive hot melt adhesive. Examples of the adherend include metal substrates such as SUS and aluminum, and non-metal substrates such as cloth, paper, polycarbonate, polyamide, polyetherimide, glass, and carbon fiber. Among these, the adherend may be, for example, cloth or paper. The reactive hot melt adhesive can be suitably used to bond a plurality of adherends selected from cloth and paper to each other. In this case, the combination of adherends may be cloth and cloth, paper and paper, or cloth and paper. The reactive hot melt adhesive can be suitably used for clothing (apparel products) such as clothes, supporters, bags, wallets, interiors, various covers, cases, wearable devices, etc., and is particularly suitable for use in clothing.

[0078] The reactive hot melt adhesive may be formed into a film and used as an adhesive film. For example, the reactive hot melt adhesive may be applied to a support film such as a PET (polyethylene terephthalate) film to form an adhesive layer, thereby obtaining an adhesive film. The thickness of the adhesive layer (adhesive film) may be 10 μm or more, 20 μm or more, or 30 μm or more, and may be 300 μm or less, 250 μm or less, or 200 μm or less. When the film is thicker, the adhesive force tends to be more secure, and when the film is thinner, the stretchability tends to be more easily secured.

[0079] [Adhesive body and its manufacturing method] The adhesive article of one embodiment includes a first adherend, a second adherend, and an adhesive layer that adheres the first adherend and the second adherend to each other. The adhesive layer contains a cured product of the reactive hot melt adhesive. Examples of articles that include the adhesive article include clothing (particularly seamless clothing), semiconductor devices, electronic devices, and the like.

[0080] The first and second adherends can be exemplified by the same ones as those exemplified above. The first and second adherends can be, for example, cloth or paper, and the combination of the first and second adherends can be cloth and cloth, paper and paper, or cloth and paper. When the article having the adhesive is clothing, the first and second adherends are cloth.

[0081] The adhesive of this embodiment can be produced by a method comprising the steps of melting the reactive hot melt adhesive and applying it to a first adherend to form an adhesive layer, placing a second adherend on the adhesive layer and pressing the second adherend to obtain a laminate, and curing the adhesive layer to obtain the adhesive.

[0082] The temperature at which the reactive hot melt adhesive is melted may be, for example, 60 to 130° C. Examples of a method for applying the reactive hot melt adhesive to the first adherend include a method using an application device such as a die coater, a roll coater, or a sprayer. A dispenser is suitable for application to small areas such as small parts.

[0083] The second adherend may be pressure-bonded, for example, by using a pressure roll or the like.

[0084] The reactive hot melt adhesive in the adhesive layer can be cured, for example, by leaving it (curing) for 24 hours at a temperature of 23° C. and 50% RH (relative humidity). As a result, the adhesive layer can contain a cured product of the reactive hot melt adhesive.

[0085] Fig. 1 is a schematic diagram showing a method for producing an adhesive body of one embodiment, and Fig. 1(a), (b), (c), and (d) are schematic diagrams showing each step. Hereinafter, with reference to Fig. 1, a method for producing an adhesive body using a stretchable fabric as a first adherend and a second adherend will be described.

[0086] First, the elastic fabric 1 is placed along the jig 10 (see FIG. 1(a)). Next, the reactive hot melt adhesive of this embodiment is applied to a predetermined portion of the elastic fabric 1 to form an adhesive layer 4 (see FIG. 1(b)). The material and shape of the jig 10 are not particularly limited and can be appropriately selected according to the purpose. The reactive hot melt adhesive may be applied, for example, using a dispenser. Next, the elastic fabric 2 is placed on the adhesive layer 4, and the elastic fabric 1 and the elastic fabric 2 are bonded together via the adhesive layer 4 while applying pressure from above the elastic fabric 2 with a roll or the like to obtain a laminate 20 (see FIG. 1(c) and (d)). After that, the laminate 20 is left (cured) so that the reactive hot melt adhesive in the adhesive layer 4 is moisture-cured, and an adhesive body in which the elastic fabrics are bonded together can be obtained. The adhesive layer 4 in the adhesive body contains a cured product of the reactive hot melt adhesive.

[0087] 1(b), an adhesive film made of a reactive hot melt adhesive that has been formed in advance on a releasable substrate may be transferred onto the stretchable fabric 1 to form the adhesive layer 4. Alternatively, the adhesive may be provided on the stretchable fabric 2, which is then bonded to the stretchable fabric 1.

[0088] [clothing] In one embodiment, a garment includes the above-mentioned adhesive structure. In this case, the first adherend and the second adherend may be fabrics. The garment may be a seamless garment.

[0089] [analysis] The urethane prepolymer contained in the reactive hot melt adhesive of this embodiment can be identified by, for example, solution NMR measurement to identify the constituent components of the urethane prepolymer. When the reactive hot melt adhesive of this embodiment contains components other than the urethane prepolymer, the constituent components of the urethane prepolymer can be identified, for example, by isolating the urethane prepolymer using preparative liquid chromatography (known means such as GPC) and distilling off the solvent, followed by solution NMR measurement. In addition, by using a similar method, components other than the urethane prepolymer contained in the reactive hot melt adhesive can also be identified.

[0090] The cured product of the reactive hot melt adhesive of this embodiment can be identified by extracting only the uncured components using a solvent such as tetrahydrofuran, which dissolves the uncured components of the cured product but does not easily dissolve the cured product itself, and then decomposing the remaining undissolved components (cured product components) with pyridine to sever the urethane bonds. EXAMPLES

[0091] The present disclosure will be described in more detail below with reference to examples, although the present disclosure is not limited to these examples.

[0092] (Production Examples 1 to 5) <Preparation of urethane prepolymer (reactive hot melt adhesive)> The urethane prepolymers A to E of Production Examples 1 to 5 were prepared using the types and parts by mass of polyol and polyisocyanate shown in Table 1. More specifically, the polyisocyanate was added to a reaction vessel to a polyol previously dehydrated by a vacuum dryer so that the equivalent ratio ((NCO) equivalent / (OH) equivalent) of the isocyanate group of the polyisocyanate to the hydroxyl group of the polyol was the value shown in Table 1, and mixed at 110°C for 1 hour until uniform. Next, a urethane prepolymer was obtained by further degassing and stirring at 110°C for 1 hour. As shown in Table 1, since the (NCO) equivalent / (OH) equivalent is greater than 1, it is presumed that the obtained urethane prepolymer has a polymer chain containing a structural unit derived from a polyol and a structural unit derived from a polyisocyanate, and an isocyanate group bonded to the end of the polymer chain. In the following, the obtained urethane prepolymer was used as it is as a reactive hot melt adhesive.

[0093] Details of each component shown in Table 1 are as follows. (a) Polyol (a1) Polyester polyol having an aromatic ring (a1)-1: Amorphous polyester polyol having an aromatic ring, mainly composed of dicarboxylic acid (adipic acid and isophthalic acid) and diol (ethylene glycol and neopentyl glycol) (number of hydroxyl groups: 2, number average molecular weight: 2000, content of structural units derived from compounds having aromatic rings: 25 mol% (based on the total amount of structural units constituting the amorphous polyester polyol), 50 mol% (based on the total amount of structural units derived from dicarboxylic acid), melting point (Tm): none) (a1)-2: Amorphous polyester polyol having an aromatic ring, mainly composed of dicarboxylic acid (phthalic anhydride) and diol (ethylene glycol and diethylene glycol) (number of hydroxyl groups: 2, number average molecular weight: 2000, content of structural units derived from compounds having aromatic rings: 50 mol% (based on the total amount of structural units constituting the amorphous polyester polyol), 100 mol% (based on the total amount of structural units derived from dicarboxylic acid), melting point (Tm): none)

[0094] (a2) Polyol other than (a1) (a2)-1: Amorphous polyester polyol without aromatic rings, mainly composed of dicarboxylic acid (adipic acid) and diol (1,4-butanediol and neopentyl glycol) (number of hydroxyl groups: 2, number average molecular weight: 5000, melting point (Tm): none) (a2)-2: A crystalline polyester polyol without an aromatic ring, mainly composed of a dicarboxylic acid (adipic acid) and a diol (ethylene glycol and 1,4-butanediol) (number of hydroxyl groups: 2, number average molecular weight: 2038, melting point (Tm): 20°C) (a2)-3: Amorphous polyether polyol (bisphenol A·PO type) having an aromatic ring (manufactured by ADEKA Corporation, product name: BPX-11, number of hydroxyl groups: 2, melting point (Tm): none)

[0095] (b) Polyisocyanate (b)-1: Diphenylmethane diisocyanate (manufactured by Tosoh Corporation, product name: Millionate MT, number of isocyanate groups: 2)

[0096] < 13 C-NMR analysis> Regarding urethane prepolymers A to E, 13 C-NMR analysis was performed. 13 C-NMR analysis was performed using a nuclear magnetic resonance spectrometer (NMR) manufactured by Bruker Japan Co., Ltd., AVANCE NEO (probe: CryoProbe TM ) and the measurement was performed under the following conditions.

[0097] (Measurement conditions) · 13 C-NMR quantitative spectroscopy: inverse gate decoupling method ·Resonance frequency: 100MHz Waiting time (d1): 5 seconds Solvent: deuterated chloroform (CDCl3) Sample concentration: 100mg / 0.6ml-CDCl3, also containing 10mgCr(acac)3 as a relaxation reagent Chemical shift reference: Tetramethylsilane (TMS) peak set to 0.00 ppm ·Measurement temperature: 23℃ -Number of times: 400

[0098] FIG. 2 shows the results of the analysis of the urethane prepolymer B in Production Example 2 in the range of 150 to 180 ppm. 13 The C-NMR spectrum of Figure 2. 13 In the C-NMR spectrum, when the integral value (C(B)) of the peak observed in the range of 171 to 176 ppm was taken as 10.000, the integral value (C(A)) of the peak observed in the range of 163 to 170 ppm and the integral value (C(C)) of the peak observed in the range of 150 to 155 ppm were 33.039 and 5.081, respectively. 13 The C-NMR spectrum of Figure 3. 13 In the C-NMR spectrum, when the integral value (C(B)) of the peak observed in the range of 171 to 176 ppm was set to 10.000, the integral value (C(A)) of the peak observed in the range of 163 to 170 ppm and the integral value (C(C)) of the peak observed in the range of 150 to 155 ppm were 4.805 and 1.564, respectively. The results are shown in Table 1. Based on these values, C(A) / (C(A)+C(B)) and C(A) / C(C) were calculated. The results are shown in Table 1.

[0099] (Examples 1 to 3 and Comparative Examples 1 and 2) <Evaluation of reactive hot melt adhesives> Initial and final adhesive strength The reactive hot melt adhesives (urethane prepolymers A to E) of Examples 1 to 3 and Comparative Examples 1 and 2 were melted at 120°C and applied onto an elastic fabric (spandex, manufactured by Toray Oprontex Co., Ltd., Lycra (registered trademark)), and coated to a thickness of 80 μm using a bar coater to form an adhesive layer. The same elastic fabric was placed on the formed adhesive layer, and pressed at 120°C to obtain a pressed body. The adhesive strength of the pressed body 5 minutes after pressing was measured using a force gauge (manufactured by Imada Co., Ltd., DS250N), and this was taken as the initial adhesive strength of the reactive hot melt adhesive. Next, the above-mentioned pressed body was aged in a thermostatic chamber at 23°C and 50% RH for one day, and the adhesive layer was cured to produce an adhesive body. The adhesive strength of the bonded structure was measured by a T-peel strength test using a tensile tester (Shimadzu Corporation, EZ-Test EZ-SX) at a measurement temperature of 25°C and a tensile speed of 100 mm / min, and this was taken as the final adhesive strength. The results are shown in Table 1.

[0100] ·Elongation at break The reactive hot melt adhesives (urethane prepolymers A to E) of Examples 1 to 3 and Comparative Examples 1 and 2 were melted at 100°C to form a film having a thickness of 100 μm, and the formed film was then allowed to stand in a thermo-hygrostat at a temperature of 23°C and a humidity of 50% for 2 days to harden. The hardened film was punched out with a No. 1 dumbbell to prepare a test piece, and the breaking elongation (%) of the test piece was measured in accordance with JIS K-6251 using an autograph AGS-X (manufactured by Shimadzu Corporation). The results are shown in Table 1.

[0101] [Table 1]

[0102] Regarding urethane prepolymers A to E, 13When C-NMR analysis was performed, the urethane prepolymers A to C had a C(A) / (C(A)+C(B)) of 0.36 or more, and furthermore, a C(A) / C(C) of 3.6 or more. It was found that the reactive hot melt adhesives of Examples 1 to 3 using such urethane prepolymers tend to have excellent initial adhesive strength and final adhesive strength compared to the reactive hot melt adhesives of Comparative Examples 1 and 2 using urethane prepolymers that do not satisfy the specified requirements. It was also found that the reactive hot melt adhesives of Examples 1 to 3 tend to have a sufficiently high level of breaking elongation. From these results, it was confirmed that the reactive hot melt adhesive of the present disclosure has excellent adhesive strength (both initial adhesive strength and final adhesive strength) and excellent elasticity. [Explanation of symbols]

[0103] 1, 2...elastic fabric, 4...adhesive layer, 10...jig, 20...laminate.

Claims

1. Contains urethane prepolymer, the urethane prepolymer has a structural unit derived from a polyol and a structural unit derived from a polyisocyanate, the structural units derived from the polyol include structural units derived from a polyester polyol having an aromatic ring, The structural units derived from a polyisocyanate include structural units derived from a diisocyanate, the content of the structural units derived from the polyester polyol having an aromatic ring is 75 mass% or more based on the total amount of the structural units derived from the polyol; The urethane prepolymer is 13 In a C-NMR analysis, when an integral value of a peak observed in the range of 163 to 170 ppm is C(A) and an integral value of a peak observed in the range of 171 to 176 ppm is C(B), C(A) and C(B) satisfy the following formula (X): Reactive hot melt adhesive. 0.38≦C(A) / (C(A)+C(B))≦0.44 (X)

2. The urethane prepolymer is 13 In a C-NMR analysis, when an integral value of a peak observed in the range of 150 to 155 ppm is defined as C(C), the C(A) and the C(C) satisfy the following formula (Y): The reactive hot melt adhesive of claim 1. 3.6≦C(A) / C(C) (Y)

3. A reactive hot melt adhesive as described in claim 1 or 2, wherein the structural units derived from the polyisocyanate include structural units derived from an aromatic diisocyanate.

4. Used for bonding a plurality of adherends selected from cloth and paper to each other; The reactive hot melt adhesive according to any one of claims 1 to 3.

5. A first adherend; A second adherend; and an adhesive layer that bonds the first adherend and the second adherend to each other; Equipped with The adhesive layer contains a cured product of the reactive hot melt adhesive according to any one of claims 1 to 3. Adhesive body.

6. The adhesive body according to claim 5, The first adherend and the second adherend are fabrics. clothing.

7. A step of forming an adhesive layer by melting the reactive hot melt adhesive according to any one of claims 1 to 3 and applying it to a first adherend; a step of placing a second adherend on the adhesive layer and pressing the second adherend to obtain a laminate; a step of obtaining an adhesive body by curing the adhesive layer in the laminate; Equipped with A method for producing an adhesive body.

Citation Information

Patent Citations

  • Production of cleaning blade for electrophotographic copying machine

    JP1994035386A

  • Moisture curable polyurethane hot melt adhesive

    JP1996503513A

  • Reactive hot-melt adhesive and adhesive interlining cloth using the same

    JP2001026762A

  • Reactive hot-melt adhesive

    JP2008063568A

  • JPP7516816B