Film forming method and electronic component manufacturing method
The film forming method for electronic components uses modified metal oxides and controlled hydrolysis in a solvent-containing reaction vessel to address coating quality inconsistencies, achieving uniform coating thickness and improved performance.
Patent Information
- Application Number
- JP2023052942
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2040-02-13
AI Technical Summary
The existing film forming method for electronic components using metal alkoxide-based coating agents results in variations in the degree of polymerization due to hydrolysis and dehydration condensation reactions, leading to inconsistent coating quality.
A film forming method involving a metal oxide modified with functional groups such as long-chain alkyl and epoxy groups, where the element body is charged before the catalyst and metal alkoxide, followed by controlled hydrolysis and dehydration in a solvent-containing reaction vessel, ensuring uniform coating formation.
The method suppresses variations in coating layer quality by ensuring uniform adherence and polymerization of the metal alkoxide, resulting in a more consistent coating thickness and improved electronic component performance.
Smart Images

Figure 0007593431000001 
Figure 0007593431000002 
Figure 0007593431000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a film forming method and a method for manufacturing an electronic component. [Background technology]
[0002] The electronic component described in Patent Document 1 includes an element body, an internal electrode disposed inside the element body, and an external electrode exposed to the outside of the element body and connected to the internal electrode. The surface of the element body is covered with a coating layer. In this electronic component, the coating layer is formed by applying a liquid or slurry coating agent to the element body. The coating agent is prepared by an alkoxide method containing aluminum, silicon, etc. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Application Publication No. 9-162452 Summary of the Invention [Problem to be solved by the invention]
[0004] In the film forming method for electronic components described in Patent Document 1, the coating agent is in the form of a sol or gel in which a metal alkoxide and a catalyst are mixed. Therefore, reactions such as hydrolysis and dehydration condensation of the metal alkoxide proceed between the preparation of the coating agent and the application to the element. As a result, in the coating agent, there are areas where the reaction has progressed and areas where the reaction has not progressed much, which may cause variation in the degree of polymerization of the metal alkoxide. If a coating layer is formed on the element using a coating agent with such variation in the degree of polymerization, the quality of the coating layer will also vary. [Means for solving the problem]
[0005] In order to solve the above problem, one aspect of the present disclosure is to provide a surface of an element body. , a metal oxide modified with one or more functional groups selected from a long-chain alkyl group and an epoxy group.A method for forming a coating layer, comprising: a step of introducing the element into a reaction vessel; Modified with the functional group Metal alkoxide or Modified with the functional group The film formation method includes a metal alkoxide introducing step of introducing a metal alkoxide precursor, a catalyst introducing step of introducing a catalyst that promotes hydrolysis of the metal alkoxide into the reaction vessel, and a film formation step of hydrolyzing and dehydrating condensing the metal alkoxide to form the coating layer on the surface of the element, the process being performed in this order: the catalyst introducing step, the element introducing step, and the metal alkoxide introducing step.
[0006] In order to solve the above problems, one aspect of the present disclosure includes a body and a coating material covering a surface of the body. The layer comprises a metal oxide modified with one or more functional groups selected from a long-chain alkyl group and an epoxy group. 1. A method for manufacturing an electronic component comprising: a coating layer; an internal electrode that is embedded within the element body and has a portion exposed from a surface of the element body; and an external electrode that is provided on the element body and is connected to the internal electrode via a through portion that passes through the coating layer, the method comprising the steps of: In the reaction vessel The internal electrode is embedded an element introduction step of introducing the element body, a metal alkoxide introduction step of introducing a metal alkoxide modified with the functional group or a metal alkoxide precursor modified with the functional group into the reaction vessel, a catalyst introduction step of introducing a catalyst that promotes hydrolysis of the metal alkoxide into the reaction vessel, and a step of hydrolyzing and dehydrating and condensing the metal alkoxide to cover the portion of the internal electrode exposed from the surface of the element body, a film forming step of forming the coating layer on a surface of the element body, a conductor applying step of applying a conductor paste onto the coating layer, and a hardening step of hardening the coating layer and firing the conductor paste to form the external electrodes on the element body, the element introduction step is carried out prior to at least one of the metal alkoxide introduction step and the catalyst introduction step, In the curing step, the through portion is formed so as to connect the internal electrode and the external electrode by the Kirkendall effect. Effect of the Invention
[0007] This makes it possible to suppress variation in the quality of the coating layer. [Brief description of the drawings]
[0008] [Figure 1] FIG. [Diagram 2] Cross-sectional view of an electronic component. [Diagram 3] 1 is an explanatory diagram of a manufacturing method for an electronic component. [Figure 4] FIG. [Diagram 5] FIG. [Figure 6] FIG. [Figure 7] FIG. [Figure 8] FIG. [Figure 9] 13 is a photograph showing a side view of an electronic component of a comparative example. [Figure 10] 4 is a photograph showing a side view of an electronic component according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The film forming method and the method for manufacturing an electronic component will be described below with reference to the drawings. Note that the drawings may show components enlarged for ease of understanding. The dimensional ratios of the components may differ from the actual ones or from those in other drawings.
[0010] First, the electronic components will be described. 1, the electronic component is, for example, a surface-mount type negative temperature coefficient thermistor component 10 that is mounted on a circuit board or the like. The negative temperature coefficient thermistor component 10 functions as an electronic component whose resistance value increases as the temperature increases. The negative temperature coefficient thermistor component 10 includes an element body 20.
[0011] The element body 20 has a regular rectangular prism shape, and the length in the direction of the central axis CA is longer than the length of one side of the square. The material of the element body 20 is ceramics obtained by firing oxides containing manganese, nickel, cobalt, and the like. In the following description, the direction of the central axis CA of the element body 20 is defined as the length direction Ld. In addition, the height direction Td and the width direction Wd perpendicular to the length direction Ld are defined as follows. That is, the height direction Td is a direction perpendicular to the length direction Ld, which is perpendicular to the main surface of the circuit board when the negative characteristic thermistor component 10 is mounted on the circuit board. The width direction Wd is a direction perpendicular to the length direction Ld, which is parallel to the main surface of the circuit board when the negative characteristic thermistor component 10 is mounted on the circuit board.
[0012] The surface of the element body 20 is roughly divided into a first end face 20A which is an end face on the first end side in the length direction Ld, a second end face 20B which is an end face on the second end side opposite the first end in the length direction Ld, and four side faces. The four side faces are composed of a first side face 20C located on the first end side in the width direction Wd, a second side face 20D located on the second end side opposite the first end in the width direction Wd, an upper side face 20E located on the upper side in the height direction Td, and a lower side face 20F located on the lower side in the height direction Td.
[0013] 2, two rectangular plate-shaped first internal electrodes 21 and two rectangular second internal electrodes 22 are built into the element body 20. The first internal electrodes 21 and the second internal electrodes 22 are made of silver. The first internal electrodes 21 and the second internal electrodes 22 are arranged such that both surfaces in the thickness direction are approximately parallel to the first side surface 20C and the second side surface 20D of the element body 20.
[0014] The dimension of the first internal electrode 21 in the length direction Ld, i.e., the dimension in the longitudinal direction of the first internal electrode 21, is smaller than the dimension in the length direction Ld of the element body 20. As shown in Fig. 1, the dimension of the first internal electrode 21 in the height direction Td, i.e., the dimension in the short direction of the first internal electrode 21, is approximately two-thirds of the dimension in the height direction Td of the element body 20. In addition, the second internal electrode 22 has the same shape as the first internal electrode 21.
[0015] 2, the first internal electrodes 21 and the second internal electrodes 22 are arranged alternately in the width direction Wd. That is, from the first end side in the width direction Wd, the first internal electrode 21, the second internal electrode 22, the first internal electrode 21, and the second internal electrode 22 are arranged in this order in the width direction Wd. In this embodiment, the distances between the internal electrodes 22 are equal.
[0016] The two first internal electrodes 21 and the two second internal electrodes 22 are both disposed in the center of the element body 20 in the height direction Td. On the other hand, the first internal electrode 21 is disposed closer to the first end in the length direction Ld, and the second internal electrode 22 is disposed closer to the second end in the length direction Ld.
[0017] Specifically, the end face of the first internal electrode 21 on the first end side in the length direction Ld is flush with the first end face 20A of the element body 20 in the length direction Ld and is exposed from the element body 20. On the other hand, the end face of the first internal electrode 21 on the second end side in the length direction Ld is embedded inside the element body 20 and is not exposed to the outside. On the other hand, the end face of the second internal electrode 22 on the second end side in the length direction Ld is flush with the second end face 20B of the element body 20 in the length direction Ld and is exposed from the element body 20. On the other hand, the end face of the second internal electrode 22 on the first end side in the length direction Ld is embedded inside the element body 20 and is not exposed to the outside.
[0018] As shown in Fig. 1, the surface of the element body 20 is covered with a coating layer 30. In this embodiment, the coating layer 30 covers the entire surface of the element body 20. The coating layer 30 is made of a metal oxide, and in this embodiment, the coating layer 30 is made of a ceramic of silicon dioxide. The thickness of the coating layer 30 is several tens of nm. Note that the thickness of the coating layer 30 is exaggerated in Fig. 2.
[0019] 1, a first external electrode 41 is laminated on a first end side portion in the longitudinal direction Ld of the element body 20. Specifically, the first external electrode 41 is a five-sided electrode that covers the first end face 20A of the element body 20 and parts of the first end side in the longitudinal direction Ld of the four side faces 20C to 20F. In this embodiment, the first external electrode 41 is laminated on the surface of the coating layer 30. The material of the first external electrode 41 is an alloy made of silver and palladium.
[0020] A second external electrode 42 is laminated on a portion of the element body 20 on the second end side in the longitudinal direction Ld. Specifically, the second external electrode 42 is a five-sided electrode that covers the second end face 20B of the element body 20 and parts of the second end side in the longitudinal direction Ld of the four side faces 20C to 20F. In this embodiment, the first external electrode 41 is laminated on the surface of the coating layer 30. The material of the second external electrode 42 is the same as that of the first external electrode 41, an alloy of silver and palladium.
[0021] The second external electrode 42 does not reach the first external electrode 41 on the four side surfaces 20C to 20F, and is disposed away from the first external electrode 41 in the direction of the central axis CA. In addition, in the center of the length direction Ld on the four side surfaces 20C to 20F of the element body 20, the first external electrode 41 and the second external electrode 42 are not laminated, and the coating layer 30 is exposed. In Fig. 1 and Fig. 2, the first external electrode 41 and the second external electrode 42 are illustrated by two-dot chain lines.
[0022] As shown in FIG. 2, the first external electrode 41 and the end face of the first internal electrode 21 at the first end in the length direction Ld are connected via a first through portion 51 penetrating the coating layer 30. The first through portion 51 is formed by the silver constituting the first internal electrode 21 extending toward the first external electrode 41 during the manufacturing process of the negative characteristic thermistor component 10, as will be described in detail later. The second external electrode 42 and the end face of the second internal electrode 22 at the second end in the length direction Ld are connected via a second through portion 52 penetrating the coating layer 30. The second through portion 52 is also formed by the silver constituting the second internal electrode 22 extending toward the second external electrode 42 during the manufacturing process of the negative characteristic thermistor component 10, similar to the first through portion 51. In FIG. 2, the first internal electrode 21 and the first through portion 51 are illustrated as separate members with a boundary, but in reality, there is no clear boundary between them. The same applies to the second through portion 52. Moreover, in FIG. 1, the first penetrating portion 51 is omitted.
[0023] Next, a method for manufacturing the NTC thermistor component 10 will be described. As shown in FIG. 3, the method for manufacturing the negative temperature coefficient thermistor component 10 includes a solvent introduction step S10, a catalyst introduction step S12, a body introduction step S14, a metal alkoxide introduction step S16, a film formation step S18, a drying step S20, a conductor application step S22, and a curing step S24.
[0024] Before forming the coating layer 30, the element body 20 is prepared in advance. Specifically, the ceramic layers are laminated while sandwiching the first internal electrode 21 and the second internal electrode 22 between a plurality of ceramic layers such that the ends of the first internal electrode 21 and the second internal electrode 22 have portions exposed from the surface of the element body 20. In this way, the first internal electrode 21 and the second internal electrode 22 are disposed inside the element body 20. Then, the plurality of ceramic layers and the first internal electrode 21 and the second internal electrode 22 are pressure-bonded to form an unfired ceramic laminate. Thereafter, the ceramic laminate is fired to form the element body 20. Then, formation of the coating layer 30 is started.
[0025] 4, in the solvent introduction step S10, 2-propanol is introduced into a reaction vessel 60 as a solvent 70.
[0026] As shown in Fig. 3, following the solvent introduction step S10, a catalyst introduction step S12 is performed. As shown in Fig. 5, in the catalyst introduction step S12, stirring of the solvent 70 in the reaction vessel 60 is started. Next, ammonia water is introduced into the reaction vessel 60 as an aqueous solution 80 containing a catalyst. In this embodiment, the catalyst is a hydroxide ion, and functions as a catalyst for promoting hydrolysis of a metal alkoxide 90, which will be described later.
[0027] 3, the catalyst introduction step S12 is followed by an element introduction step S14. As shown in FIG 6, in the element introduction step S14, a plurality of element bodies 20 prepared in advance as described above are introduced into a reaction vessel 60.
[0028] As shown in FIG. 3, the element introduction step S14 is followed by the metal alkoxide introduction step S16. As shown in FIG. 7, in the metal alkoxide introduction step S16, liquid tetraethyl orthosilicate is introduced into the reaction vessel 60 as the metal alkoxide 90. Note that tetraethyl orthosilicate is also called tetraethoxysilane. In this embodiment, the amount of the metal alkoxide 90 introduced in the metal alkoxide introduction step S16 is calculated based on the surface area of the element 20 introduced in the element introduction step S14. Specifically, the amount of the metal alkoxide 90 per element 20 required to form the coating layer 30 formed on the surface of the element 20 is multiplied by the number of element 20 introduced in the element introduction step S14 to calculate the amount.
[0029] As shown in FIG. 3, the film forming step S18 is performed after the metal alkoxide introduction step S16. Specifically, the stirring of the solvent 70 started in the catalyst introduction step S12 is continued for a predetermined time after the metal alkoxide 90 is introduced into the reaction vessel 60 in the metal alkoxide introduction step S16. As a result, the metal alkoxide 90 is hydrolyzed by the hydroxide ions serving as the catalyst. When the metal alkoxide 90 is hydrolyzed, the hydrolyzed metal alkoxide 90 adheres to the surface of the element body 20. Then, the metal alkoxides 90 adhered to the surface of the element body 20 are dehydrated and condensed with each other to form the coating layer 30. In addition, in the film forming step S18, since the element body 20 is submerged in the solution, the coating layer 30 is formed on the entire surface of the element body 20. At the stage of the film forming step S18, the coating layer 30 is in a sol state. In this embodiment, the film formation method for forming the coating layer 30 on the element 20 includes the solvent introduction step S10, the catalyst introduction step S12, the element introduction step S14, the metal alkoxide introduction step S16, and the film formation step S18.
[0030] Following the film-forming step S18, a drying step S20 is performed. In the drying step S20, after stirring is continued for a predetermined time in the film-forming step S18, the element body 20 is removed from the reaction vessel 60 and dried. As a result, the sol-like coating layer 30 is dried to become a gel-like coating layer 30.
[0031] Following the drying step S20, a conductor application step S22 is performed. As shown in Fig. 8, in the conductor application step S22, a conductor paste P is applied to two locations on the surface of the coating layer 30, namely, a first end portion and a second end portion in the longitudinal direction Ld of the element body 20. Specifically, the conductor paste P is applied so as to cover the entire first end face 20A and parts of the coating layer 30 on the four side faces 20C to 20F. The conductor paste P is also applied so as to cover the entire second end face 20B and parts of the coating layer 30 on the four side faces 20C to 20F.
[0032] As shown in FIG. 3, the conductor application step S22 is followed by a curing step S24. Specifically, in this embodiment, the curing step S24 is a heating step. In the curing step S24, the element body 20 on which the coating layer 30 and the conductor paste P are applied is heated. As a result, water is evaporated from the gel-like coating layer 30, and the coating layer 30 covering the surface of the element body 20 is baked and cured as shown in FIG. 1. At the same time, the first external electrode 41 and the second external electrode 42 are baked. In this way, the conductor application step S22 and the curing step S24 constitute an external electrode formation step. That is, in this embodiment, the curing step S24 is not only a step for curing the coating layer 30, but also serves as a part of the external electrode formation step.
[0033] In this embodiment, during heating in the curing step S24, the Kirkendall effect caused by the difference in diffusion speed between the first internal electrode 21 and the first external electrode 41 attracts silver contained in the first internal electrode 21 to the first external electrode 41 containing palladium. As a result, the first through portion 51 extends from the first internal electrode 21 toward the first external electrode 41 through the coating layer 30, thereby connecting the first internal electrode 21 to the first external electrode 41. The same applies to the second through portion 52 connecting the second internal electrode 22 to the second external electrode 42.
[0034] Next, the quality variation of the coating layer was evaluated for the negative temperature coefficient thermistor component 10 manufactured by the above-mentioned manufacturing method and a comparative negative temperature coefficient thermistor component based on the variation of the thickness of the coating layer. For the comparative negative temperature coefficient thermistor component shown in Fig. 9, a coating liquid in a state in which a catalyst-containing aqueous solution 80 and a metal alkoxide 90 were mixed in advance was applied to the surface of the element body 20, and the drying step S20, the conductor application step S22, and the curing step S24 were performed in the same manner as in the above-mentioned embodiment.
[0035] As shown in Fig. 9, when the NTC thermistor component of the comparative example was observed under a microscope while being irradiated with irradiation light, interference fringes were observed on the surface of the coating layer 30. When the thickness of the coating layer 30 was about several tens of nm, interference fringes were observed if the thickness of the coating layer 30 varied. In other words, interference fringes were visible on the coating layer 30 of the NTC thermistor component of the comparative example, which indicates that the thickness of the coating layer 30 varied.
[0036] On the other hand, as shown in Fig. 10, when the negative characteristic thermistor component 10 manufactured by the manufacturing method of the above embodiment was observed under a microscope while being irradiated with irradiation light, no interference fringes were observed on the surface of the coating layer 30. Therefore, it can be seen that the coating layer 30 of the negative characteristic thermistor component 10 in this embodiment has a smaller variation in thickness and is more uniform than the negative characteristic thermistor component of the comparative example.
[0037] Next, the operation and effects of the above embodiment will be described. (1) According to the above embodiment, in the metal alkoxide introduction step S16, hydrolysis of the metal alkoxide 90 is initiated by the catalyst while the element body 20 is in the reaction vessel 60. Therefore, the hydrolyzed metal alkoxide 90 is likely to adhere to the surface of the element body 20 before excessive dehydration condensation occurs. As a result, the coating layer 30 can be formed on the element body before the metal alkoxide 90 is in a part where the reaction has progressed and a part where the reaction has not progressed much, so that the variation in the quality of the coating layer 30 can be suppressed. Therefore, the variation in the film thickness of the coating layer 30 formed from the coating layer 30 can also be suppressed.
[0038] (2) According to the above embodiment, the solvent introduction step S10 is performed prior to both the catalyst introduction step S12 and the metal alkoxide introduction step S16. Therefore, when the metal alkoxide 90 and the aqueous solution 80 containing the catalyst are mixed, the solvent 70 is already contained in the reaction vessel 60. Therefore, the hydrolyzed metal alkoxide 90 is likely to adhere uniformly to the surface of the element body 20.
[0039] (3) According to the above embodiment, the inside of the reaction vessel 60 is stirred after the solvent introduction step S10. Then, the inside of the reaction vessel 60 is also stirred in the film formation step S18. Therefore, the metal alkoxide 90 and the aqueous solution 80 containing the catalyst can be mixed uniformly. As a result, the hydrolyzed metal alkoxide 90 is dehydrated and condensed at a uniform rate, and the degree of polymerization is likely to be the same.
[0040] (4) In the above embodiment, the reaction vessel 60 contains the solvent 70, and the metal alkoxide 90 can be dehydrated and condensed at a substantially uniform rate regardless of location by further stirring. In the above embodiment, a plurality of elements 20 are placed in the reaction vessel 60. Therefore, not only the variation in the thickness of the coating layer 30 within the element 20 but also the variation in the thickness of the coating layer 30 between the element bodies 20 can be suppressed.
[0041] (5) If the catalyst-containing aqueous solution 80 is introduced into the reaction vessel 60 while the metal alkoxide 90 is contained therein, there is a risk that the reaction of the metal alkoxide 90 will proceed locally at a location where the density of the catalyst is high when the aqueous solution 80 is introduced. According to the above embodiment, the catalyst introduction step S12 is performed prior to the metal alkoxide introduction step S16. Therefore, when the metal alkoxide 90 is introduced into the reaction vessel 60 in the metal alkoxide introduction step S16, the catalyst-containing aqueous solution 80 is already present in the reaction vessel 60. Therefore, the local reaction when the metal alkoxide 90 is introduced can be suppressed more effectively than when the catalyst-containing aqueous solution 80 is introduced when the metal alkoxide 90 is present in the reaction vessel 60.
[0042] (6) According to the above embodiment, tetraethyl orthosilicate is used as the metal alkoxide 90. The metal alkoxide 90 in which the metal is silicon has a relatively slow reaction rate, and therefore the reaction rate can be easily controlled to a constant value.
[0043] (7) According to the above embodiment, the metal alkoxide introducing step S16 is performed after the element body introducing step S14. Therefore, the amount of metal alkoxide 90 required to form the coating layer 30 on the element body 20 introduced in the element body introducing step S14 can be calculated before the metal alkoxide introducing step S16 is performed. For example, the amount of metal alkoxide 90 required to form the film thickness of the coating layer 30 to be formed can be calculated for the surface area of the element body 20 introduced in the element body introducing step S14. Therefore, it is possible to avoid consuming more metal alkoxide 90 than necessary.
[0044] The above embodiment can be modified as follows: The above embodiment and the following modifications can be combined and implemented within a range that does not cause technical contradiction. In the above embodiment, the electronic component to which the film formation method is applied as a manufacturing method for the electronic component is not limited to the negative temperature coefficient thermistor component 10. For example, it may be a thermistor component other than a negative temperature coefficient thermistor component, or it may be a multilayer capacitor component or an inductor component. As long as the electronic component has at least an element body 20 and a coating layer 30 covering the surface of the element body 20, the film formation method of the above embodiment can be applied as a manufacturing method for the electronic component.
[0045] In the above embodiment, the material of the element body 20 is not limited to the examples in the above embodiment. For example, the material of the element body 20 may be manganese-zinc ferrite or copper-zinc ferrite. The material of the element body 20 may also be resin.
[0046] In the above embodiment, the shape of the element body 20 is not limited to the example of the above embodiment, and may be cylindrical or polygonal. The element body 20 may also be the core of a wire-wound inductor component. For example, the core is composed of a columnar winding core portion and flange portions provided at each end of the winding core portion, and the core may have a so-called drum core shape. In the case of a wire-wound inductor component, the inductor component can be manufactured by further winding a conductive wire after the hardening step S24 in which the coating layer 30, the first external electrode 41, and the second external electrode 42 are formed on the core, which is the element body 20.
[0047] In the above embodiment, the thickness of the coating layer 30 is not limited to several tens of nm, but may be several tens of μm. When the thickness of the coating layer 30 is several tens of nm, it is easy to evaluate the variation in the thickness based on the presence or absence of interference fringes caused by the irradiated light. In order to increase the thickness of the coating layer 30, for example, the metal alkoxide introduction step S16 and the film formation step S18 may be repeated multiple times.
[0048] In the above embodiment, the first internal electrode 21 and the second internal electrode 22 may have any shape as long as they can ensure electrical conduction with the corresponding first external electrode 41 and second external electrode 42. Furthermore, the number of first internal electrodes 21 and second internal electrodes 22 does not matter, and the number of first internal electrodes 21 may be one, or three or more.
[0049] In the above embodiment, the combination of materials for the first internal electrode 21 and the first external electrode 41 is not limited to the example in the above embodiment. If one of the electrodes contains silver and the other contains palladium, the Kirkendall effect described above can be obtained. The same applies to the combination of materials for the second internal electrode 22 and the second external electrode 42.
[0050] In addition, the combination of materials for the first internal electrode 21 and the first external electrode 41 is not limited to silver and palladium, and the Kirkendall effect does not have to be obtained. In this case, after the film forming step S18, for example, the first end face 20A side of the element body 20 may be polished to physically remove a part of the coating layer 30 so that the first internal electrode 21 is exposed, and then the drying step S20 and the conductor application step S22 may be performed. This allows the conductor paste P to be directly applied to the first internal electrode 21, so that the first internal electrode 21 and the first external electrode 41 can be connected. The same applies to the combination of materials for the second internal electrode 22 and the second external electrode 42.
[0051] In the above embodiment, the location of the first external electrode 41 is not limited to the example in the above embodiment. For example, the first external electrode 41 may be arranged only on the lower surface 20F that serves as the mounting surface, or may be arranged from the lower surface 20F to the first end surface 20A. The same applies to the second external electrode 42.
[0052] In the above embodiment, the external electrode forming process is not limited to the example of the above embodiment. For example, after the film forming process S18, the coating layer 30 may be hardened by a heat treatment, and then the conductor applying process S22 and the hardening process S24 may be performed to form the first external electrode 41 and the second external electrode 42. Also, for example, as in the above-mentioned modified example, a part of the first internal electrode 21 may be exposed from the element body 20, and the first external electrode 41 may be formed on the exposed part by a plating method.
[0053] In the above embodiment, the curing step S24 is not limited to a step of simultaneously curing the coating layer 30 and the conductive paste P. For example, if the conductive paste P is a material that is cured by ultraviolet light irradiation, a heating step may be performed as the curing step for curing the coating layer 30, and ultraviolet light may be irradiated as the step for curing the conductive paste P.
[0054] In the above embodiment, the coating layer 30 may be hardened by sufficiently evaporating water in the drying step S20. In this case, the drying step S20 functions as a hardening step for hardening the coating layer 30.
[0055] In the above embodiment, the raw material introduction step S14 may be performed prior to the catalyst introduction step S12. Furthermore, when the raw material introduction step S14 is performed prior to the catalyst introduction step S12, the metal alkoxide introduction step S16 may be performed prior to the catalyst introduction step S12 and the raw material introduction step S14. The raw material introduction step S14 may be performed prior to at least one of the metal alkoxide introduction step S16 and the catalyst introduction step S12.
[0056] In the above embodiment, the solvent 70 introduced in the solvent introduction step S10 is not limited to the example in the above embodiment, and may be any liquid capable of dispersing the metal alkoxide 90 appropriately. In the above embodiment, the solvent introduction step S10 may be performed after the catalyst introduction step S12 or the matrix introduction step S14. The solvent introduction step S10 may be performed prior to at least one of the metal alkoxide introduction step S16 and the catalyst introduction step S12. The solvent introduction step S10 may also be omitted. In this case, for example, if the amount of water contained in the catalyst-containing aqueous solution 80 is appropriately large, the metal alkoxide 90 reacts in the liquid phase. The catalyst-containing aqueous solution 80 may also be introduced in a state where it is mixed with an organic solvent as the solvent 70.
[0057] In the above embodiment, stirring in the reaction vessel 60 is started during the catalyst introduction step S12, but as long as stirring in the reaction vessel 60 is performed at least in the film formation step S18, the reaction rate of the metal alkoxide 90 can be easily kept constant. Stirring in the reaction vessel 60 may be performed by rotating a stirring blade, or by rotating the reaction vessel 60 and mixing by turning it upside down. Furthermore, stirring in the reaction vessel 60 may be omitted. For example, if the ratio of the metal alkoxide 90 to the solvent 70 is appropriately small, the metal alkoxide 90 may be sufficiently dispersed and the reaction rate may be appropriately slow.
[0058] In the above embodiment, the aqueous solution 80 containing a catalyst is ammonia water, and the catalyst is hydroxide ions, but the catalyst is not limited to this. A basic aqueous solution can catalyze the hydrolysis of the metal alkoxide 90, similar to the ammonia water in the above embodiment, and even an acidic aqueous solution can catalyze the hydrolysis of the metal alkoxide 90. Furthermore, even a neutral aqueous solution can be used as long as it contains ions that can catalyze hydrolysis.
[0059] In the above embodiment, the catalyst is described as being added as an aqueous solution 80 containing the catalyst, but a solid compound containing the catalyst and water may be added separately to the reaction vessel 60, in which case the catalyst can be considered to have been added to the reaction vessel 60 by being generated in the reaction vessel 60. Also, for example, a solid compound containing the catalyst may be added to the reaction vessel 60, and moisture in the air may be used as the water required for hydrolysis.
[0060] In the above embodiment, the metal alkoxide 90 is not limited to tetraethyl orthosilicate. For example, the metal contained in the metal alkoxide 90 may be titanium, zirconium, aluminum, or the like. When the metal contained in the metal alkoxide 90 is silicon, the reaction rate is slower than other metals, so that the reaction rate of the metal alkoxide 90 is easily controlled to a constant value. The alkoxy group of the metal alkoxide 90 may be a methoxy group, a propoxy group, or the like, or may be modified with a functional group such as a long-chain alkyl group or an epoxy group as in a coupling agent. Furthermore, the coordination number for the metal contained in the metal alkoxide 90 is not limited to 4-coordination, and may be 3-coordination or 2-coordination.
[0061] In the above embodiment, in the metal alkoxide introduction step S16, a solution containing a precursor for generating the metal alkoxide 90 may be introduced instead of the metal alkoxide 90. The metal alkoxide 90 may be generated in the reaction vessel 60 instead of being introduced into the reaction vessel 60 after the metal alkoxide 90 is generated outside the reaction vessel 60. For example, the metal alkoxide 90 is generated by reacting a metal salt with an alcohol. Therefore, even when a metal salt and an alcohol, which are metal alkoxide precursors, are introduced into the reaction vessel 60 and the metal alkoxide 90 is generated by the reaction between them, the metal alkoxide 90 can be considered to have been introduced into the reaction vessel 60.
[0062] In the above embodiment, the film forming method forms a film on the element body 20 of the electronic component, but the element body on which the film is formed is not limited to one that constitutes an electronic component. For example, the element body may be a substrate. [Explanation of symbols]
[0063] 10...Negative characteristic thermistor 20…Base 30…Coating layer 41...First external electrode 42…Second external electrode 60…Reaction vessel 70...Solvent 80…Aqueous solution 90...Metal alkoxide S10: Solvent injection process S12...Catalyst injection process S14…Body input process S16…Metal alkoxide injection process S18…Film formation process S20…Drying process S22: Conductive coating process S24…Curing process
Claims
1. 1. A method for forming a coating layer on a surface of an element, the method comprising the steps of: an element introduction step of introducing the element into a reaction vessel; a metal alkoxide introduction step of introducing the metal alkoxide modified with the functional group or the metal alkoxide precursor modified with the functional group into the reaction vessel; a catalyst introduction step of introducing a catalyst for promoting hydrolysis of the metal alkoxide into the reaction vessel; and a film-forming step of forming the coating layer on the surface of the element body by hydrolysis and dehydration condensation of the metal alkoxide, The catalyst introduction step, the base material introduction step, and the metal alkoxide introduction step are carried out in this order. Film formation method.
2. A solvent introduction step of introducing a solvent into the reaction vessel, The solvent introduction step is carried out prior to at least one of the metal alkoxide introduction step and the catalyst introduction step. The film forming method according to claim 1 .
3. In the film forming step, the inside of the reaction vessel is stirred. The film forming method according to claim 1 or 2.
4. The metal alkoxide includes tetraethyl orthosilicate. The film forming method according to any one of claims 1 to 3.
5. A method for manufacturing an electronic component comprising: an element body; a coating layer covering a surface of the element body and containing a metal oxide modified with one or more functional groups selected from a long-chain alkyl group and an epoxy group; an internal electrode built into the element body and having a portion exposed from a surface of the element body; and an external electrode provided on the element body and connected to the internal electrode via a through portion that passes through the coating layer, the method comprising the steps of: an element introduction step of introducing the element having the internal electrode built therein into a reaction vessel; a metal alkoxide introduction step of introducing the metal alkoxide modified with the functional group or the metal alkoxide precursor modified with the functional group into the reaction vessel; a catalyst introduction step of introducing a catalyst for promoting hydrolysis of the metal alkoxide into the reaction vessel; a film formation step of forming the coating layer on the surface of the element body by hydrolyzing and dehydrating condensing the metal alkoxide so as to cover the portions of the internal electrodes exposed from the surface of the element body; a conductor coating step of coating a conductor paste on the coating layer; a curing step of curing the coating layer and firing the conductive paste to form the external electrodes on the element body; Equipped with the element introduction step is carried out prior to at least one of the metal alkoxide introduction step and the catalyst introduction step, In the curing step, the through portion is formed so as to connect the internal electrode and the external electrode by the Kirkendall effect. A method for manufacturing electronic components.
Citation Information
Patent Citations
Ceramic device and its production
JP1997162452A
Method for manufacturing graphene-based two-dimensional sandwich nanomaterials
JP2013530908A
JPP7256478B
Methods for forming coatings on MEMS devices
US20040071863A1