Porous ceramics for electrolytes in thin-layer electrochemical devices.

A porous inorganic layer electrolyte with a lithium ion-carrying phase in lithium ion batteries addresses resistance and safety issues, offering high conductivity, mechanical stability, and safety, enhancing battery performance.

JP7593570B2Active Publication Date: 2024-12-03I TEN
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020560782
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-05-07
Filing Date
2019-05-06
Publication Date
2024-12-03
Estimated Expiration
2039-05-06

AI Technical Summary

Technical Problem

Existing lithium ion batteries face issues with high resistance to lithium transport, mechanical fragility, and safety risks due to metallic lithium dendrite formation and organic binder flammability, leading to short circuits and thermal runaway.

Method used

A thin-layer electrolyte comprising a porous inorganic layer with interconnected mesopores, impregnated with a lithium ion-carrying phase, is used without organic binders, formed by depositing a colloidal suspension of nanoparticles and consolidating them through heat treatment or mechanical compression, ensuring high ionic conductivity and mechanical stability.

Benefits of technology

The solution provides a battery with enhanced ionic conductivity, mechanical robustness, thermal stability, and safety, enabling high power density and long service life without the risk of ignition, suitable for high-energy density storage and rapid energy restoration.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007593570000002
    Figure 0007593570000002
  • Figure 0007593570000003
    Figure 0007593570000003
  • Figure 0007593570000004
    Figure 0007593570000004
Patent Text Reader

Abstract

A thin layer electrolyte in an electrochemical device such as a lithium ion battery, the electrolyte comprising a porous inorganic layer impregnated with a lithium ion-carrying phase, the porous inorganic layer being characterized by having an interconnected network of open pores. [Selected Figure] Figure 1A
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the field of electrochemistry, more specifically to thin-layer electrochemical systems. More precisely, it relates to thin-layer electrolytes that can be used in electrochemical systems such as high-power batteries, in particular lithium-ion batteries, or supercapacitors. The present invention more particularly relates to an electrolyte comprising a porous inorganic layer impregnated with a phase carrying lithium ions, and to a method for preparing such a thin-layer electrolyte. The present invention also relates to a method for manufacturing an electrochemical device comprising at least one such electrolyte, and to the device obtained thereby. [Background technology]

[0002] A lithium-ion battery is an electrochemical component that allows the storage of electrical energy. In general, it is composed of one or more elementary cells, each cell consisting of two electrodes with different electrical potentials and an electrolyte. Various types of electrodes can be used in secondary lithium-ion batteries. A cell may consist of two electrodes separated by a polymeric porous membrane (also called "separator") or a ceramic porous membrane impregnated with a liquid electrolyte containing a lithium salt. For example, patent application JP2002-042792 describes the implementation of an electrolyte layer on the electrodes of a battery. The electrolyte in question is essentially a polymer membrane such as polyethylene oxide, polyacrylonitrile, poly(vinylidene fluoride), the pores of which are filled with an electrolyte such as LiPF 6 According to this document, the size of the particles deposited by electrophoresis is preferably less than 1 μm and the thickness of the layer formed is preferably less than 10 μm. In such a system, the liquid electrolyte migrates into the pores contained in the membrane and into the electrodes, thus providing ionic conduction between the electrodes.

[0003] In order to create high-power thin-layer batteries and reduce the resistance of the transport of lithium ions between the two electrodes, it has been sought to increase the porosity of the polymer membrane. However, increasing the porosity of the polymer membrane promotes the precipitation of metallic lithium dendrites in the pores of the polymer membrane during the charge and discharge cycles of the battery. These dendrites can cause internal short circuits in the cell and pose a risk of thermal runaway in the battery.

[0004] These polymer membranes impregnated with liquid electrolyte have a lower ionic conductivity than the liquid electrolyte used. To facilitate ionic conduction between the electrodes and the electrolyte, thin polymer membranes were used. However, these polymer membranes are mechanically fragile and their electrical insulation can change under the influence of strong electric fields, in the case of batteries with very thin electrolyte films, or under the influence of mechanical and vibrational stresses. These polymer membranes are prone to breakage during charge and discharge cycles, which can cause delamination of the anode and cathode particles, induce electrical insulation losses, and cause short circuits between the two positive and negative electrodes, leading to electrical breakdown. In batteries using porous electrodes, this phenomenon becomes even more pronounced.

[0005] To improve the mechanical resistance, Ohara, inter alia in EP 1 049 188 A1 and in patent EP 1 424 743 B1, has proposed the use of an electrolyte composed of a polymer membrane containing lithium ion conducting glass-ceramic particles.

[0006] Furthermore, it is known from Maunel et al. (Polymer 47 (2006) p. 5952-5964) that the incorporation of ceramic charges into the polymer matrix improves the morphological and electrochemical properties of the polymer electrolyte; these ceramic charges are active (Li 2 N, LiAl 2 O 3 ), in which case they are involved in the process of transporting lithium ions, or they can be passive (Al 2 O 3 , SiO 2, MgO, etc.), in which case they do not participate in the process of transporting lithium ions. The size of the particles and the characteristics of the ceramic charge affect the electrochemical properties of the electrolyte, see Zhang et al., "Flexible and ion-conducting membrane electrolytes for solid-state lithium batteries: Dispersions of garnet nanoparticles in insulating POE", NanoEnergy, 28 (2016) p. 447-454. However, these membranes are relatively brittle and easily destroyed under the influence of mechanical stresses induced during battery assembly. Summary of the Invention [Problem to be solved by the invention]

[0007] The present invention seeks to overcome at least some of the aforementioned disadvantages in the prior art.

[0008] More precisely, the problem that the present invention aims to solve is to propose an electrolyte that has high ionic conductivity, a stable mechanical structure, good thermal stability, a long life span and does not pose any safety hazards.

[0009] Another problem that the present invention aims to solve is to provide a method for producing such thin-layer electrolytes that is simple, safe, fast, easy to implement, easy to industrialize and inexpensive.

[0010] Another problem that the present invention seeks to solve is to provide an electrode for a battery that can operate reliably and without the risk of fire.

[0011] Another challenge is to provide an electrolyte that does not contain organic binders, as such binders can cause fires in the event of an internal short circuit in the battery.

[0012] Another object of the present invention is to provide a battery with a rigid structure having a high power density that is mechanically capable of withstanding shock and vibration.

[0013] Another object of the invention is to provide a method for the manufacture of an electronic, electrical or electrotechnical device, such as a battery, a capacitor or a supercapacitor, comprising an electrolyte according to the invention.

[0014] Another object of the invention is to propose devices such as batteries, lithium-ion battery cells, capacitors, supercapacitors, etc., that have improved reliability, have a longer lifetime and can be encapsulated by coatings deposited by atomic layer deposition techniques (ALD) at high temperature and reduced pressure.

[0015] Yet another object of the present invention is to propose devices such as batteries, lithium-ion battery cells, capacitors, supercapacitors, etc., that can store high energy density and recover this energy with very high power density (especially in capacitors and supercapacitors), withstand high temperatures, have long lifetimes, and can be encapsulated by coatings deposited by ALD at high temperature and reduced pressure. [Means for solving the problem]

[0016] Objective of the invention According to the invention, the problem is solved by using at least one thin layer electrolyte in an electrochemical device such as a lithium ion battery, said electrolyte comprising a porous inorganic layer having an interconnected network of open pores impregnated with a lithium ion carrying phase. Preferably, the porous inorganic layer has a mesoporous structure with a porosity of more than 25% by volume, preferably more than 30% by volume.

[0017] Advantageously, the open pores of said porous inorganic layer have an average diameter D 50 The thickness of the thin-layer electrolyte is less than 100 nm, preferably less than 80 nm, preferably 2 to 80 nm, more preferably 2 to 50 nm, and the volume of the thin-layer electrolyte is more than 25%, preferably more than 30% of the total volume of the thin-layer electrolyte.

[0018] Advantageously, the open pores of said porous inorganic layer have a volume between 30 and 50% of the total volume of said thin-layer electrolyte.

[0019] Preferably, the porous inorganic layer does not contain an organic binder.

[0020] Advantageously, the thickness of the porous inorganic layer is less than 10 μm, preferably between 3 and 6 μm, preferably between 2.5 and 4.5 μm.

[0021] Advantageously, said porous inorganic layer comprises an electronically insulating material, preferably Al 2 O 3 , SiO 2 , ZrO 2 and / or selected from a material selected from the group formed by: ·General formula Li d A 1 x A 2 y (TO 4 ) z Garnet, where A 1 is a cation in the oxidation state +II, preferably Ca, Mg, Sr, Ba, Fe, Mn, Zn, Y, Gd; and A 2 is a cation in the oxidation state +III, preferably Al, Fe, Cr, Ga, Ti, La; and ·(TO 4 ) is an anion, T is the atom in the center of a tetrahedron formed by oxygen atoms in the oxidation state +IV, and TO 4 advantageously represents a silicate or zirconate anion, in which the element T in oxidation state +IV is totally or partially replaced by an atom in oxidation state +III or +V, such as Al, Fe, As, V, Nb, In, Ta; d is 2 to 10, preferably 3 to 9, more preferably 4 to 8; x is 2.6 to 3.4 (preferably 2.8 to 3.2); y is 1.7 to 2.3 (preferably 1.9 to 2.1), and z is 2.9 to 3.1; Garnet, preferably selected from: Li 7 La 3 Zr 2 O 12 Li 6 La 2 BaTa 2 O 12 Li 5.5 La 3 Nb 1.75 In 0.25 O 12 Li 5 La 3 M 2 O 12 , M=Nb or Ta or a mixture of the two; Li 7-x Ba x La 3-x M 2 O 12 , 0≦x≦1 and M=Nb or Ta or a mixture of the two compounds; Li 7-x La 3 Zr 2-x M x O 12 , 0≦x≦2 and M=Al, Ga or Ta or a mixture of two or three of these compounds; Lithium phosphate, preferably selected from: NaSICON type phosphates, Li 3 PO 4 ;LiPO 3 ;Li called "LASP" 3 Al 0.4 Sc 1.6 (PO 4 ) 3 Li 1.2 Zr 1.9 Ca 0.1 (PO 4 ) 3 ;LiZr 2 (PO 4 ) 3 Li 1+3x Zr 2 (P 1-x S x O 4 ) 3 , 1.8 <x<2.3;Li 1+6x Zr 2 (P 1-x B x O 4) 3 , 0≦x≦0.25; Li 3 (Sc 2-x M x )(PO 4 ) 3 , M=Al or Y and 0≦x≦1; Li 1+x M x (Sc) 2-x (PO 4 ) 3 , M=Al, Y, Ga or a mixture of these three compounds and 0≦x≦0.8; Li 1+x M x (Ga 1-y Sc y ) 2-x (PO 4 ) 3 , 0≦x≦0.8; 0≦y≦1 and M=Al or Y or a mixture of the two compounds; Li 1+x M x (Ga) 2-x (PO 4 ) 3 , M=Al, Y or a mixture of the two compounds, 0≦x≦0.8; Li 1+x Al x Ti 2-x (PO 4 ) 3 , 0≦x≦1, referred to as "LATP"; or Li 1+x Al x Ge 2-x (PO 4 ) 3 , 0≦x≦1, referred to as "LAGP"; or Li 1+x+z M x (Ge 1-y Ti y ) 2-x S z P 3-z O 12 , 0≦x≦0.8 and 0≦y≦1.0 and 0≦z≦0.6 and M=Al, Ga or Y or a mixture of two or three of these compounds; Li 3+y (Sc 2-x M x )Q y P 3-y O 12 , M=Al and / or Y and Q=Si and / or Se, 0≦x≦0.8 and 0≦y≦1; or Li 1+x+y Mx Sc 2-x Q y P 3-y O 12 , M=Al, Y, Ga or a mixture of the three compounds and Q=Si and / or Se, 0≦x≦0.8 and 0≦y≦1; or Li 1+x+y+z M x (Ga 1-y Sc y ) 2-x Q z P 3-z O 12 , 0≦x≦0.8; 0≦y≦1; 0≦z≦0.6, M=Al or Y or a mixture of the two compounds and Q=Si and / or Se; or Li 1+x Zr 2-x B x (PO 4 ) 3 , 0≦x≦0.25; or Li 1+x Zr 2-x Ca x (PO 4 ) 3 , 0≦x≦0.25; or Li 1+x M 3 x M 2-x P 3 O 12 , 0≦x≦1 and M 3 = Cr, V, Ca, B, Mg, Bi and / or Mo, M = Sc, Sn, Zr, Hf, Se or Si or mixtures of these compounds; Lithium borate, preferably selected from: Li 3 (Sc 2-x M x )(BO 3 ) 3 , M=Al or Y, 0≦x≦1; Li 1+x M x (Sc) 2-x (BO 3 ) 3 M=Al, Y, Ga or a mixture of these three compounds; 0≦x≦0.8; Li 1+x M x (Ga 1-y Sc y ) 2-x (BO 3 ) 3, 0 ≤ x ≤ 0.8, 0 ≤ y ≤ 1 and M = Al or Y; Li 1+x M x (Ga) 2-x (BO 3 ) 3 , M = Al, Y or a mixture of two of their compounds, 0 ≤ x ≤ 0.8; Li 3 BO 3 , Li 3 BO 3 -Li 2 SO 4 , Li 3 BO 3 -Li 2 SiO 4 , Li 3 BO 3 -Li 2 SiO 4 -Li 2 SO 4 ; · Acid nitride, preferably Li 3 PO 4-x N 2x / 3 , Li 4 SiO 4-x N 2x / 3 , Li 4 GeO 4-x N 2x / 3 and 0 < x < 4 or Li 3 BO 3-x N 2x / 3 and 0 < x < 3, selected from; · A lithium compound based on lithium oxynitride and phosphorus, called "LiPON", with the general formula Li x PO y N z where x ~ 2.8 and 2y + 3z ~ 7.8 and 0.16 ≤ z ≤ 0.4, and especially Li 2.9 PO 3.3 N 0.46 , also Li w PO x N y S z and a compound where 2x + 3y + 2z = 5 = w or Li w PO x N y S z and a compound where 3.2 ≤ x ≤ 3.8, 0.13 ≤ y ≤ 0.4, 0 ≤ z ≤ 0.2, 2.9 ≤ w ≤ 3.3 or Li tP x Al y O u N v S w A compound where 5x+3y=5, 2u+3v+2w=5+t, 2.9≦t≦3.3, 0.84≦x≦0.94, 0.094≦y≦0.26, 3.2≦u≦3.8, 0.13≦v≦0.46, and 0≦w≦0.2; Lithium phosphorus or boron oxynitride based materials, referred to as "LiPON" and "LIBON" respectively, which may contain silicon, sulfur, zirconium, aluminum, or a combination of aluminum, boron, sulfur and / or silicon, and in the case of lithium phosphorus oxynitride based materials, boron; Lithium compounds based on lithium, phosphorus and silicon oxynitride, called "LiSiPON", especially Li 1.9 S 0.28 P 1.0 O 1.1 N 1.0 ; Lithium oxynitrides of the type LiBON, LiBSO, LiSiPON, LiSON, Thio-LiSiCON, LiPONB (where B, P and S stand for boron, phosphorus and sulfur, respectively); (1-x)LiBO 2 -xLi 2 SO 4 , LiBSO type lithium oxynitride, such as 0.4≦x≦0.8; Lithium oxide, preferably Li 7 La 3 Zr 2 O 12 Or Li 5+x La 3 (Zr x , A 2-x )O 12 , A=Sc, Y, Al, Ga and 1.4≦x≦2 or Li 0.35 La 0.55 TiO 3 Or Li 3x La 2 / 3-x TiO 3 , selected from 0≦x≦0.16(LLTO); Silicates, preferably Li2 Si 2 O 5 、Li 2 SiO 3 、Li 2 Si 2 O 6 、LiAlSiO 4 、Li 4 SiO 4 、LiAlSi 2 O 6 selected from; ·An anti-perovskite type solid electrolyte selected from the following: Li 3 OA, where A is a halogen atom or a mixture of halogen atoms, preferably at least one element selected from F, Cl, Br, I or a mixture of two, three or four of these elements; Li (3-x) M x / 2 OA where 0 < x ≦ 3, M is a divalent metal, preferably at least one of the elements Mg, Ca, Ba, Sr or a mixture of two, three or four of these elements, and A is a halogen atom or a mixture of halogen atoms, preferably at least one element selected from F, Cl, Br, I or a mixture of two, three or four of these elements; Li (3-x) M 3 x / 3 OA, 0 ≦ x ≦ 3, M 3 is a trivalent metal, A is a halogen atom or a mixture of halogen atoms, preferably at least one element selected from F, Cl, Br, I or a mixture of two, three or four of these elements; or, LiCOX z Y (1-z) 、X and Y are halogens as described above for A, 0 ≦ z ≦ 1, ·Compound La 0.51 Li 0.34 Ti 2.94 、Li 3.4 V 0.4 Ge 0.6 O 4 、Li 2 O-Nb 2 O 5 、LiAlGaSPO 4 ; ·Li 2 CO 3, B 2 O 3 , Li 2 O, Al(PO 3 ) 3 LiF, P 2 S 3 , Li 2 S., Li 3 N, Li 14 Zn(GeO 4 ) 4 , Li 3.6 Ge 0.6 V 0.4 O 4 , LiTi 2 (PO 4 ) 3 , Li 3.25 Ge 0.25 P 0.25 S 4 , Li 1,3 Al 0,3 Ti 1,7 (PO 4 ) 3 , Li 1+x Al x M 2-x (PO 4 ) 3 (where M=Ge, Ti and / or Hf, 0 <x<1)、Li 1+x+y Al x Ti 2-x S y P 3-y O 12 (where 0≦x≦1 and 0≦y≦1).

[0022] Advantageously, said pores of the thin-layer electrolyte are impregnated with a phase carrying lithium ions, such as an organic solvent or a solvent mixture in which at least one lithium salt is dissolved, and / or a polymer comprising at least one lithium salt, and / or an ionic liquid or a mixture of ionic liquids comprising at least one lithium salt, optionally diluted in a suitable solvent.

[0023] Advantageously, said pores are impregnated with a lithium ion carrying phase comprising at least 50% by weight of at least one ionic liquid.

[0024] The porous inorganic layer may be made of (or may contain) an electrolyte material, i.e. a material in which lithium ions have sufficient mobility. The porous inorganic layer may be made of (or may contain) a material that does not have electronic conductivity or sufficient ionic conductivity for lithium ions. In both cases, the electrolyte layer is formed by the porous inorganic layer and the lithium ion carrying phase with which it is impregnated. In the second case, only this lithium ion carrying phase ensures the ionic conductivity of the electrolyte, while in the first case, the mobility of the lithium ions in the material of the porous inorganic layer contributes to the ionic conductivity.

[0025] The lithium ion carrying phase must comprise lithium ions. To form this carrying phase, the lithium ions may be dissolved in any suitable solvent. For example, the lithium ion carrying phase may comprise an ionic liquid, which may be diluted in a suitable solvent. It may also comprise a liquid or a polymer that is soluble in a suitable solvent that is at least sufficiently viscous to penetrate the open porosity of the porous inorganic layer.

[0026] According to the invention, said porous inorganic layer may be deposited by electrophoresis, inkjet, doctor blade, roll coating, curtain coating or dip coating from a colloidal suspension of electrically insulating nanoparticles of a solid electrolyte material, preferably without a binder. According to an essential feature of the invention, this suspension comprises aggregates or agglomerates of primary nanoparticles.

[0027] The primary nanoparticles forming the aggregates or agglomerates are preferably monodisperse, i.e. the distribution of their primary diameters is narrow, which allows a better control of the porosity and even the mesoporosity.

[0028] The thermal treatment leads to a partial coalescence of the nanoparticles of the material (a phenomenon called necking). It is known that nanoparticles have a large surface energy, which is the driving force behind this structural change; this occurs at temperatures well below the melting point of the material and after short treatment times. Thus, a binder-free, homogeneous, three-dimensional mesoporous structure with an interconnected network of open pores is formed, in which the lithium ions have mobility that is not reduced by grain boundaries or binder layers. This partial coalescence of the agglomerated nanoparticles transforms into agglomerates. The partial coalescence of the agglomerated nanoparticles caused by the thermal treatment allows the consolidation of the three-dimensional mesoporous structure.

[0029] This structure also provides good mechanical resistance of the layer, even without a binder.

[0030] Aggregates and agglomerates, respectively, can also be obtained immediately after hydrothermal synthesis if the suspension is not sufficiently refined and the ionic strength of the suspension leads the primary nanoparticles to aggregate and agglomerate, respectively, into particles of larger size.

[0031] A second object of the invention is a method for producing a thin layer electrolyte deposited on an electrode, said layer preferably being free of organic binders and preferably having a porosity, preferably mesoporous, of more than 30% by volume, more preferably between 30 and 50% by volume, said layer having a mean diameter D 50 having pores of less than 100 nm, preferably less than 80 nm, preferably less than 50 nm, said method being characterized by: (a) providing a colloidal suspension comprising aggregates or agglomerates of nanoparticles of at least one inorganic material, the aggregates or agglomerates having an average diameter of 80 to 300 nm (preferably 100 to 200 nm); (b) preparing an electrode; (c) depositing on said electrode a porous inorganic layer from a suspension of particles of inorganic material obtained in step (a) by electrophoresis, inkjet, doctor blade, roll coating, curtain coating or dip coating; (d) drying the porous inorganic layer, preferably with an air stream, to obtain a porous inorganic layer; (e) subjecting the porous inorganic layer to mechanical compression and / or heat treatment; (f) impregnating the porous inorganic layer obtained in step (e) with a phase carrying lithium ions;

[0032] Another object of the invention is a method for the manufacture of a thin layer electrolyte deposited on an electrode, said layer preferably being free of organic binders and preferably having a porosity, preferably mesoporous, of more than 30% by volume, more preferably between 30 and 50% by volume, said layer having an average diameter D 50 having pores of less than 100 nm, preferably less than 80 nm, preferably less than 50 nm, said method being characterized by: (a1) Primary diameter D 50 preparing a colloidal suspension comprising nanoparticles of at least one inorganic material P having a particle size of 50 nm or less; (a2) destabilizing the nanoparticles present in said colloidal suspension to form particle aggregates or agglomerates having an average diameter of 80-300 nm, preferably 100-200 nm, said destabilization being preferably carried out by adding a destabilizing agent such as a salt, preferably LiOH, (b) preparing an electrode; (c) depositing on said electrode a porous inorganic layer from said suspension comprising aggregates or agglomerates of particles of at least one inorganic material obtained in step (a2) by electrophoresis, inkjet, doctor blade, roll coating, curtain coating or dip coating; (d) drying the porous inorganic layer, preferably with an air stream, to obtain a porous inorganic layer; (e) subjecting the porous inorganic layer to mechanical compression and / or heat treatment; (f) impregnating the porous inorganic layer obtained in step (e) with a phase carrying lithium ions;

[0033] Advantageously, the porous inorganic layer obtained in step (c) has a thickness of less than 10 μm, preferably less than 8 μm and more preferably between 1 and 6 μm.

[0034] Advantageously, the porous inorganic layer obtained in step (d) has a thickness of less than 10 μm, preferably between 3 and 6 μm, preferably between 2.5 and 4.5 μm.

[0035] Advantageously, the primary diameter of said nanoparticles is between 10 and 50 nm, preferably between 10 and 30 nm.

[0036] The average diameter of the pores is preferably 2 to 50 nm, more preferably 6 to 30 nm, and even more preferably 8 to 20 nm.

[0037] The electrodes are dense electrodes or porous electrodes, preferably mesoporous electrodes.

[0038] The method according to the invention is used for the manufacture of thin-layer electrolyte electronic, electrical or electrotechnical devices selected from the group consisting of: batteries, capacitors, supercapacitors, capacitors, resistors, inductances, transistors, solar cells.

[0039] Another object of the invention is a method for manufacturing a thin-layer battery according to the invention, comprising the following steps: -1- Preparing at least two conductive substrates pre-coated with layers of materials usable as an anode and as a cathode (respectively "anode layer" 12, "cathode layer" 22), -2- Providing a colloidal suspension containing aggregates or agglomerates of nanoparticles of at least one inorganic material, the aggregates or agglomerates having an average diameter of 80 to 300 nm (preferably 100 to 200 nm); -3- depositing a porous inorganic layer on the cathode and anode obtained in step-1-, respectively, from a suspension of agglomerated particles of inorganic material obtained in step-2- by electrophoresis, inkjet, doctor blade, roll coating, curtain coating or dip coating, -4- The layer obtained in step-3- is dried, preferably with an air stream, -5- stacking the cathode and anode layers, preferably laterally offset; -6- the stack of anode and cathode layers obtained in step -5- is subjected to a mechanical compression and / or a heat treatment in order to align and assemble the porous inorganic layers present in the anode and cathode layers, so as to obtain a rigid all-solid-state assembly, preferably free of organic binders, -7- The structure obtained in step-6- is impregnated with a lithium ion carrying phase, preferably with a lithium ion carrying phase comprising at least 50 wt. % of at least one ionic liquid, to obtain an assembled stack, preferably a battery.

[0040] The order of steps -1- and -2- is not important.

[0041] Advantageously, the cathode is a dense electrode or a porous electrode or, preferably, a mesoporous electrode. Advantageously, the anode is a dense electrode or a porous electrode or, preferably, a mesoporous electrode.

[0042] Advantageously, the dense electrode or the porous electrode or the mesoporous electrode is coated by ALD or by chemical solution deposition CSD with an electronically insulating, preferably ionically conductive, layer, preferably less than 5 nm thick. Advantageously, the cathode is a dense electrode or a porous electrode coated by ALD or by CSD with an electronically insulating layer, preferably with an electronically insulating and ionically conductive layer, or a porous electrode coated by ALD or by CSD with an electronically insulating layer, preferably with an electronically insulating and ionically conductive layer, or preferably a mesoporous electrode or a mesoporous electrode coated by ALD or by CSD with an electronically insulating layer, preferably with an electronically insulating and ionically conductive layer, and and / or alternatively the anode is a dense electrode, or a dense electrode coated by ALD or by CSD with an electronically insulating layer, preferably an electronically insulating and ionically conducting layer, or a porous electrode, or a porous electrode coated by ALD or by CSD with an electronically insulating layer, preferably an electronically insulating and ionically conducting layer, preferably a mesoporous electrode, or a mesoporous electrode coated by ALD or by CSD with an electronically insulating layer, preferably an electronically insulating and ionically conducting layer.

[0043] Advantageously, when the cathode and / or the anode are porous or mesoporous electrodes, the structure (i.e. the laminate treated by mechanical compression and / or heat treatment) is impregnated in step 7 with a lithium ion carrying phase, impregnating the porous inorganic layer of said cathode and / or said anode.

[0044] Advantageously, after step -7-, do the following: - depositing the following in alternating succession on the battery: at least one first layer of parylene and / or polyimide on said battery; at least one second layer made of an electrically insulating material by ALD (Atomic Layer Deposition) on said first layer of parylene and / or polyimide; and depositing, on the alternating succession of at least one first layer and at least one second layer, a layer, preferably made of silicone, epoxy resin or parylene or polyimide, making it possible to protect the battery from mechanical damage to the battery, to form a sealing system for the battery; - cutting the so sealed battery along two cut planes to expose the anode and cathode connections of the battery at each of the cut planes, such that the sealing system covers, preferably continuously, four of the six sides of the battery; - At and around these anode and cathode connections, the following are successively deposited: optionally depositing a first conductive layer, preferably a metal, preferably by ALD; Depositing a second layer of silver-filled epoxy resin on the first conductive layer; Depositing a nickel-based third layer on the second layer; A tin or copper based fourth layer is deposited on the third layer.

[0045] Advantageously, after step -6-, do the following: - depositing successively and alternately on the assembled stack a sealing system formed by a series of layers, i.e. by a sequence, preferably by a z-sequence, comprising: a first coating layer, preferably chosen from parylene, parylene type F, polyimide, epoxy resin, silicone, polyamide and / or mixtures thereof, deposited on the assembled stack, a second coating layer made of an electrically insulating material deposited on the first coating layer by atomic layer deposition; This sequence may be repeated z times, where z ≥ 1. - depositing, in this successive layer, a final coating layer of a material selected from epoxy resin, polyethylene naphthalate (PEN), polyimide, polyamide, polyurethane, silicone, sol-gel silica or organosilica, - cutting the assembled stack so sealed along two cut planes, exposing the anode and cathode connections of the assembled stack on each of said cut planes, such that the sealing system covers, preferably continuously, four of the six faces of said assembled stack, to obtain a basic battery, After step (7), do the following: At and around these anode and cathode junctions, the following are successively deposited: a first layer of graphite filled material, preferably graphite filled epoxy resin; a second layer comprising metallic copper obtained from an ink filled with copper nanoparticles deposited on the first layer; - heat treating the layer obtained, preferably by means of infrared flash lamps, in order to obtain a coating of the cathode and anode connections with a layer of metallic copper, - on and around this first stack of terminal ends, in succession, a second stack may be deposited comprising: A first layer of tin-zinc alloy, preferably deposited by immersion in a molten tin-zinc bath, to ensure hermeticity of the battery at minimal cost; A second layer based on pure tin, deposited by electrodeposition, or a second layer containing an alloy based on silver, palladium and copper, deposited on this first layer of a second laminate.

[0046] Advantageously, the anode and cathode connections 50 are on opposite sides of the stack.

[0047] Another object of the invention relates to a battery, preferably a lithium-ion battery, comprising at least one thin-layer electrolyte according to the invention.

[0048] Another object of the invention relates to a supercapacitor comprising at least one thin-layer electrolyte according to the invention. [Brief description of the drawings]

[0049] 1 and 2 are diagrams illustrating embodiments of the present invention that do not limit the scope of the invention. [Figure 1A] FIG. 1A shows the nanoparticles before heat treatment and illustrates the necking phenomenon. [Figure 1B] FIG. 1B shows the nanoparticles after heat treatment, demonstrating the necking phenomenon. [Figure 2A] FIG. 2A shows the diffractogram. [Figure 2B] FIG. 2B shows a snapshot obtained by electron microscopy of the primary nanoparticles used to deposit the porous electrode by electrophoresis. [Diagram 3] FIG. 3 shows diagrammatically a front view of a battery with an electrolyte according to the invention in an extracted state, illustrating the structure of the battery with an assembly of elementary cells covered by a sealing system and terminations. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0050] Table 1 lists the symbols used in the drawings.

[0051] [Table 1]

[0052] Detailed Description 1.Definition In the context of this specification, a particle size is defined by its largest dimension. "Nanoparticle" refers to any particle or object of nanometer size, at least one of whose dimensions is less than or equal to 100 nm.

[0053] In the framework of this specification, a material or electronically insulating layer, preferably an electronically insulating and ionically conductive layer, is defined as a material having an electrical resistance (resistance to the passage of electrons) of 10 5A material or layer with a resistivity of more than Ω·cm.

[0054] "Ionic liquid" means any liquid salt that can transport electricity and is distinct from all salts molten with a melting temperature below 100°C. Some of these salts remain liquid at ambient temperature and do not solidify even at very low temperatures. Such salts are referred to as "ambient temperature ionic liquids".

[0055] "Mesoporous material" refers to any solid that has in its structure pores called "mesopores", whose size is intermediate between micropores (less than 2 nm wide) and macropores (more than 50 nm wide), i.e. between 2 and 50 nm. This term corresponds to the term adopted by IUPAC (International Union of Pure and Applied Chemistry) as a reference for the skilled person. Thus, although mesopores as defined above have nanometer dimensions with respect to the definition of nanoparticles, the term "nanopores" is not used here. Pores with a size smaller than that of mesopores are known to be called "micropores" by those skilled in the art.

[0056] A presentation of the concept of porosity (and of the terms disclosed above) is given in the article "Texture des materiaux pulverulents ou poreux" by F. Rouquerol et al., published in "Techniques de l'Ingenieur", traite Analyse et Characterisation, fascicule P 1050; in this article techniques for characterising porosity are described, in particular the BET method.

[0057] In the context of the present invention, "mesoporous layer" refers to a layer having mesopores. As explained below, in these layers, the mesopores contribute significantly to the total porous volume; this condition is referred to in the following description using the expression "mesoporous layer having a mesoporous porosity of more than X% by volume", where "X%" is preferably more than 25%, preferably more than 30%, more preferably 30-50% of the total volume of the layer.

[0058] "Agglomerates" refers to weakly bound collections of primary particles, according to the UPAC definition, where these primary particles are nanoparticles with a diameter that can be measured by transmission electron microscopy. According to techniques known to the skilled person, aggregates of aggregated primary nanoparticles can be broken down and suspended in a liquid phase, i.e. resulting in primary nanoparticles, usually under the effect of ultrasound.

[0059] "Agglomerates" as defined by UPAC means strongly bound collections of primary particles or aggregates.

[0060] In the context of the present invention, the term "electrolyte layer" refers to a layer in an electrochemical device, which device may operate according to its intended purpose. For example, if the electrochemical device is a secondary lithium ion battery, the term "electrolyte layer" refers to a "porous inorganic layer" impregnated with a phase that carries lithium ions.

[0061] Said porous inorganic layer in an electrochemical device is also referred to herein as a "separator", as that term is used in the art.

[0062] According to the present invention, the "porous inorganic layer" is preferably mesoporous and can be deposited by electrophoresis, by dip coating, by inkjet, by roll coating, by curtain coating or by doctor blading from a suspension of nanoparticle aggregates or agglomerates, preferably from a concentrated suspension comprising nanoparticle agglomerates.

[0063] 2. Suspension Preparation The deposition of polydisperse nanoparticles results in porous structures with closed porosity, for this reason the use of these polydisperse nanoparticles should be avoided in the method according to the invention.

[0064] The method according to the invention uses electrophoresis, inkjet, doctor blade, roll coating, curtain coating or dip coating of nanoparticle suspensions as deposition techniques for these porous, preferably mesoporous, layers. Within the framework of the invention, it is preferred that these suspensions of nanoparticles are not prepared from dry nanopowders. They can be prepared by grinding powders or nanopowders in the liquid phase.

[0065] For example, the particles may be wet nano-milled in ethanol; the particles may be zirconia beads (e.g. 0.3 mm diameter) milled for several hours (e.g. 5 hours) until the primary particle size is greater than 50 nm, or greater than 80, more preferably 50-150 nm; this prevents uncontrolled sintering of the deposited layer, which would lead to the formation of a dense phase. The conductivity of the suspension remains low, around 20 μS / cm. A monomodal but rather broad size distribution can thus be obtained. A drawback of nano-milling is the partial amorphization of the particles in the region close to the surface, which may interfere with the processing of the layers deposited from these nanoparticles.

[0066] In another embodiment of the invention, the nanoparticles are prepared directly in the suspension by precipitation. The synthesis of nanoparticles by precipitation makes it possible to obtain primary nanoparticles of monomodal size, of very homogeneous size, i.e. very narrow monodispersity, with good crystallinity and purity. The use of these nanoparticles of very homogeneous size and narrow distribution makes it possible to obtain, after deposition, porous structures with controlled and open porosity. The porous structures obtained after deposition of these nanoparticles have few, preferably no, closed pores.

[0067] In a more preferred embodiment of the invention, the nanoparticles are prepared directly in their primary size by solvothermal or hydrothermal synthesis; this technique allows to obtain nanoparticles with a very narrow size distribution and a single distribution; these particles are called "monodisperse nanoparticles". Moreover, these particles have very good crystallinity. The size of these non-agglomerated particles is called the primary size, which in the present invention is preferably less than 100 nm, advantageously between 10 and 50 nm, preferably between 10 and 30 nm; this favors the formation of a porous, preferably mesoporous, interconnected network during the later steps of the method, due to the necking phenomenon.

[0068] This suspension of monodisperse nanoparticles may be purified to remove all ions that may interfere in the liquid phase. Depending on the degree of purification, it may then be specially treated to form aggregates or agglomerates of controlled size. More precisely, the formation of aggregates or agglomerates may result from the destabilization of the suspension caused by ions. When the suspension is completely purified, it is stable, and to destabilize it, usually in the form of salts, ions are added; these ions are preferably lithium ions (preferably added in the form of LiOH).

[0069] If the suspension is not fully refined, the formation of aggregates or agglomerates may proceed spontaneously or by aging. This process is simpler due to fewer purification steps, but the size of the aggregates or agglomerates is more difficult to control. One of the essential aspects for the production of the porous layer according to the invention consists of controlling the size of the primary particles used and their degree of aggregation or agglomeration.

[0070] This suspension of aggregates or agglomerates is then used for the deposition of the porous layer according to the invention by electrophoresis, ink jet, doctor blade, roll coating, curtain coating or dip coating.

[0071] In one embodiment, the material used for the manufacture of the porous layer according to the invention is selected from inorganic materials that have a low melting point, are electronically insulating and are stable in contact with the electrodes during the hot pressing step. The more heat-resistant the material, the more likely it is to be necessary to heat the electrode / electrolyte interface at high temperatures, with the risk of modifying the interface with the electrode material, especially by interdiffusion. This gives rise to parasitic reactions, producing depletion layers whose electrochemical properties differ from those found in the same material deeper from the interface. Lithium-containing materials are preferred, as they may prevent or even eliminate these lithium depletion phenomena.

[0072] The material used for the manufacture of the porous layer according to the invention is inorganic. In a particular embodiment, the material used for the manufacture of the porous layer according to the invention is an electrically insulating material. It is preferably Al 2 O 3 , SiO 2 , ZrO 2 may be selected from.

[0073] Alternatively, the material used in the manufacture of the porous inorganic layer according to the present invention may be an ionically conductive material, such as a lithium-containing solid electrolyte, to limit modification of the electrode / electrolyte interface.

[0074] According to the invention, the solid electrolyte material used for the manufacture of the porous inorganic layer may in particular be chosen from: · General formula Li d A 1 x A 2 y (TO 4 ) z Garnet, where A 1 represents a cation in the oxidation state +II, preferably Ca, Mg, Sr, Ba, Fe, Mn, Zn, Y, Gd; and A 2 represents a cation in the oxidation state +III, preferably Al, Fe, Cr, Ga, Ti, La; and (TO 4) represents an anion, T is an atom in oxidation state +IV, located at the center of a tetrahedron formed by oxygen atoms, and TO 4 advantageously represents the anion of silicate or zirconate, the element T in oxidation state +IV being replaceable in whole or in part by an atom in oxidation state +III or +V, such as Al, Fe, As, V, Nb, In, Ta; d is from 2 to 10, preferably from 3 to 9, more preferably from 4 to 8; x is from 2.6 to 3.4 (preferably from 2.8 to 3.2); y is from 1.7 to 2.3 (preferably from 1.9 to 2.1), and z is from 2.9 to 3.1; Garnet, preferably selected from: Li 7 La 3 Zr 2 O 12 Li 6 La 2 BaTa 2 O 12 Li 5.5 La 3 Nb 1.75 In 0.25 O 12 Li 5 La 3 M 2 O 12 where M=Nb or Ta or a mixture of these two compounds; Li 7-x Ba x La 3-x M 2 O 12 where 0≦x≦1 and M=Nb or Ta or a mixture of these two compounds; Li 7-x La 3 Zr 2-x M x O 12 where 0≦x≦2, M=Al, Ga, Ta or a mixture of two or three of these compounds; Lithium phosphate, preferably selected from: Lithium phosphate of the NaSICON type, Li 3 PO 4 ;LiPO 3 ;Li called "LASP" 3 Al 0.4 Sc 1.6 (PO4 ) 3 , Li 1.2 Zr 1.9 Ca 0.1 (PO 4 ) 3 ;LiZr 2 (PO 4 ) 3 Li 1+3x Zr 2 (P 1-x S x O 4 ) 3 and 1.8 <x<2.3;Li 1+6x Zr 2 (P 1-x B x O 4 ) 3 where 0≦x≦0.25; Li 3 (Sc 2-x M x )(PO 4 ) 3 , M=Al or Y and 0≦x≦1; Li 1+x M x (Sc) 2-x (PO 4 ) 3 , M=Al, Y, Ga or a mixture of these three compounds and 0≦x≦0.8; Li 1+x M x (Ga 1-y Sc y ) 2-x (PO 4 ) 3 where 0≦x≦0.8; 0≦y≦1 and M=Al or Y, or a mixture of these two compounds; Li 1+x M x (Ga) 2-x (PO 4 ) 3 where M=Al, Y or a mixture of the two compounds and 0≦x≦0.8; Li, called “LATP” 1+x Al x Ti 2-x (PO 4 ) 3 where 0≦x≦1, or Li, called "LAGP" 1+x Al x Ge 2-x (PO 4 ) 3where 0≦x≦1; or Li 1+x+z M x (Ge 1-y Ti y ) 2-x S z P 3-z O 12 , 0≦x≦0.8 and 0≦y≦1.0 and 0≦z≦0.6 and M=Al, Ga or Y or a mixture of two or three of these compounds; Li 3+y (Sc 2-x M x )Q y P 3-y O 12 where M=Al and / or Y and Q=Si and / or Se, 0≦x≦0.8 and 0≦y≦1; or Li 1+x+y M x Sc 2-x Q y P 3-y O 12 , M=Al, Y, Ga or a mixture of these three compounds, and Q=Si and / or Se, and 0≦x≦0.8 and 0≦y≦1; or Li 1+x+y+z M x (Ga 1-y Sc y ) 2-x Q z P 3-z O 12 where 0≦x≦0.8; 0≦y≦1; 0≦z≦0.6, M=Al or Y or a mixture of these two compounds, and Q=Si and / or Se; or Li 1+x Zr 2-x B x (PO 4 ) 3 where 0≦x≦0.25; or Li 1+x Zr 2-x Ca x (PO 4 ) 3 where 0≦x≦0.25; or Li 1+x M 3 x M 2-x P 3 O 12 where 0≦x≦1 and M 3= Cr, V, Ca, B, Mg, Bi and / or Mo, M = Sc, Sn, Zr, Hf, Se or Si or a mixture of these compounds; · Lithium borate, preferably selected from the following: Li 3 (Sc 2-x M x )(BO 3 ) 3 where M = Al or Y and 0 ≦ x ≦ 1; Li 1+x M x (Sc) 2-x (BO 3 ) 3 , M = Al, Y, Ga or a mixture of these three compounds and 0 ≦ x ≦ 0.8; Li 1+x M x (Ga 1-y Sc y ) 2-x (BO 3 ) 3 where 0 ≦ x ≦ 0.8, 0 ≦ y ≦ 1 and M = Al or Y; Li 1+x M x (Ga) 2-x (BO 3 ) 3 where M = Al, Y or a mixture of these two compounds and 0 ≦ x ≦ 0.8; Li 3 BO 3 , Li 3 BO 3 -Li 2 SO 4 , Li 3 BO 3 -Li 2 SiO 4 , Li 3 BO 3 -Li 2 SiO 4 -Li 2 SO 4 ; · Oxynitride, preferably Li 3 PO 4-x N 2x / 3 , Li 4 SiO 4-x N 2x / 3 , Li 4 GeO 4-x N 2x / 3 where 0 < x < 4 or Li 3BO 3-x N 2x / 3 which is selected from 0 < x < 3; · Li where x ~ 2.8 and 2y + 3z ~ 7.8 and 0.16 ≦ z ≦ 0.4 x PO y N z A lithium compound called "LiPON", based on lithium oxynitride and phosphorus, especially Li 2.9 PO 3.3 N 0.46 , also the compound Li w PO x N y S z where 2x + 3y + 2z = 5 = w or Li w PO x N y S z where 3.2 ≦ x ≦ 3.8, 0.13 ≦ y ≦ 0.4, 0 ≦ z ≦ 0.2, 2.9 ≦ w ≦ 3.3, or Li t P x Al y O u N v S w A compound in the form of, where 5x + 3y = 5, 2u + 3v + 2w = 5 + t, 2.9 ≦ t ≦ 3.3, 0.84 ≦ x ≦ 0.94, 0.094 ≦ y ≦ 0.26, 3.2 ≦ u ≦ 3.8, 0.13 ≦ v ≦ 0.46, 0 ≦ w ≦ 0.2; · Materials called "LiPON" and "LIBON", respectively, based on lithium phosphorus or boron oxynitride, and which may also contain silicon, sulfur, zirconium, aluminum, or a combination of aluminum, boron, sulfur and / or silicon, and boron in the case of materials based on lithium phosphorus oxynitride; · A lithium compound called "LiSiPON", based on lithium, phosphorus and silicon oxynitride, especially Li 1.9 Si 0.28 P 1.0 O 1.1 N 1.0 ; · LiBON, LiBSO, LiSiPON, LiSON, thio - LiSiCON, lithium oxynitrides of the LiPONB type (B, P and S represent boron, phosphorus and sulfur respectively); · (1 - x)LiBO 2 - xLi 2 SO 4 which is a LiBSO - type lithium oxynitride with 0.4 ≤ x ≤ 0.8; · A lithium oxide, preferably selected from the following: Li 7 La 3 Zr 2 O 12 or Li 5+x La 3 (Zr x , A 2-x )O 12 where A = Sc, Y, Al, Ga and 1.4 ≤ x ≤ 2, or Li 0.35 La 0.55 TiO 3 or Li 3x La 2 / 3-x TiO 3 where 0 ≤ x ≤ 0.16 (LLTO); · A silicate, preferably Li 2 Si 2 O 5 , Li 2 SiO 3 , Li 2 Si 2 O 6 , LiAlSiO 4 , Li 4 SiO 4 , LiAlSi 2 O 6 selected from; · An anti - perovskite - type solid electrolyte selected from the following: Li 3 OA where A is a halogen atom or a mixture of halogen atoms, preferably at least one of the elements selected from F, Cl, Br, I or a mixture of two or three or four of them; Li (3-x) M x / 2 OA, 0 < x ≤ 3, M is a divalent metal, preferably at least one of the elements Mg, Ca, Ba, Sr or a mixture of two or three or four of these elements, A is a halogen atom or a mixture of halogen atoms, preferably at least one of the elements F, Cl, Br, I or a mixture of two or three or four of these elements; Li(3-x) M 3 x / 3 OA, 0≦x≦3, M 3 is a trivalent metal, A is a halogen atom or a mixture of halogen atoms, preferably at least one of the elements F, Cl, Br, I or a mixture of two or three or four of these elements; or LiCOX z Y (1-z) X and Y are halogen atoms as described above for A, and 0≦z≦1. · Compound La 0.51 Li 0.34 Ti 2.94 , Li 3.4 V 0.4 Ge 0.6 O 4 , Li 2 O-Nb 2 O 5 , LiAlGaSPO 4 ; Li 2 CO 3 , B 2 O 3 , Li 2 O, Al(PO 3 ) 3 LiF, P 2 S 3 , Li 2 S., Li 3 N, Li 14 Zn(GeO 4 ) 4 , Li 3.6 Ge 0.6 V 0.4 O 4 , LiTi 2 (PO 4 ) 3 , Li 3.25 Ge 0.25 P 0.25 S 4 , Li 1.3 Al 0.3 Ti 1.7 (PO 4 ) 3 , Li 1+x Al x M 2-x (PO 4 ) 3 (M=Ge, Ti and / or Hf and 0 <x<1)、Li1+x+y Al x Ti 2-x S y P 3-y O 12 (0≦x≦1 and 0≦y≦1).

[0075] For the assembly of the battery, it is preferred that between the anode and the cathode there is a porous layer of a solid electrolyte based on lithium phosphate. These materials have a relatively low melting point and the particles fuse relatively well at moderate temperatures. Moreover, the fact that they already contain intercalated lithium makes it possible to prevent diffusion of the lithium within the material, which could lead to the formation of depleted areas at the surface.

[0076] The Applicants have observed that the average diameter of the nanoparticle aggregates or agglomerates in the later steps of the method is between 80 and 300 nm (preferably between 100 and 200 nm) and the average diameter of the pores in the layer having open porosity is less than 100 nm, preferably less than 80 nm, preferably between 2 and 80 nm, more preferably between 2 and 50 nm.

[0077] According to the present invention, the porous inorganic layer may be deposited by electrophoresis, ink jet, doctor blade, roll coating, curtain coating or dip coating.

[0078] 3. Deposition of porous inorganic layers by electrophoresis The method according to the invention can use electrophoresis of a suspension of nanoparticles as a deposition technique for the porous layer. Methods for depositing layers from a suspension of nanoparticles are known per se (see for example EP 2 774 208 B1). Deposition by electrophoresis is carried out by applying an electric field between the substrate on which the deposition takes place and a counter electrode, which mobilizes the charged particles in the colloidal suspension and deposits them on the substrate. To ensure the stability of the colloidal suspension, it is preferred to use polar nanoparticles and / or the colloidal suspension advantageously has a zeta potential of an absolute value greater than 25 mV.

[0079] Electrophoretic deposition is carried out on a substrate with sufficient electrical conductivity from a suspension of particles of inorganic material that can be used as the porous inorganic layer according to the invention. This can therefore be a metallic substrate, for example a metal foil (such as a stainless steel foil with a thickness of about 5 μm), or a polymeric or non-metallic foil with an electrically conductive surface (for example coated with a layer of metal or with a layer of an electrically conductive oxide, such as ITO, which has the advantage of also acting as a diffusion barrier). To produce a battery, the inorganic material can be electrophoretically deposited on a layer of electrode material (anode or cathode). Said layer of electrode material can be deposited on a conductive substrate, for example of the metal foil or polymer foil type coated with an electrically conductive layer. To carry out electrophoresis, a counter electrode is placed in the suspension and a voltage is applied between the conductive substrate and said counter electrode.

[0080] The electrophoretic deposition rate depends on the applied electric field and the electrophoretic mobility of the particles and can be very fast: at an applied voltage of 200 V, the deposition rate can reach about 10 μm / min.

[0081] The inventors have observed that this technique allows the deposition of very homogeneous layers (with uniform particle concentration and electric field at the surface of the substrate) over very large areas, and it is suitable for a continuous band process, and for batch processing on plates.

[0082] The porous, preferably mesoporous, inorganic layer is deposited on the anode 12 and / or cathode 22 layers, which are themselves formed by any suitable process onto a conductive substrate used as a current collector and / or directly onto a sufficiently conductive substrate used as a current collector.

[0083] The substrate used as a current collector may be, for example, a metal foil, or a polymer foil or a metallized non-metal (i.e., coated with a layer of metal). The substrate is preferably selected from foils composed of titanium, copper, nickel or stainless steel.

[0084] The metal foil may be coated with a layer of a precious metal, in particular chosen from gold, platinum, titanium or an alloy mainly containing at least one of these metals, or with a layer of an electrically conductive material of the ITO type, which has the advantage of also acting as a diffusion barrier.

[0085] In batteries using the porous inorganic layer and the porous electrode according to the invention, the liquid phase carrying the lithium ions that impregnate the pores is in direct contact with the current collector. However, if these liquid phases carrying the lithium ions are in contact with a metal substrate and polarized at a potential that is highly anodic with respect to the cathode and highly cathodic with respect to the anode, they may induce dissolution of the current collector. These parasitic reactions may shorten the life of the battery and accelerate its self-discharge. To prevent this, aluminum current collectors are used in the cathodes of all lithium-ion batteries. Aluminum has the particularity of anodizing at the very anode potential, and the oxide layer that forms on its surface protects it from dissolution. However, aluminum has a melting temperature close to 600° C. and cannot be used to manufacture batteries with the porous electrode and electrolyte according to the invention. The solidification process of the porous electrode and electrolyte according to the invention leads to the melting of the current collector. Therefore, to prevent parasitic reactions that may shorten the life of the battery and accelerate its self-discharge, a titanium foil is advantageously used as the current collector in the cathode. During the operation of the battery, the titanium foil is anodized like aluminum, and the oxide layer prevents the parasitic reaction of dissolving the titanium in contact with the liquid electrolyte. Moreover, because titanium has a much higher melting point than aluminum, the all-solid-state electrode according to the present invention can be fabricated directly on this type of foil.

[0086] The use of these massive materials, in particular foils made of titanium, copper or nickel, also makes it possible to protect the cut ends of the electrodes of the battery from corrosion phenomena.

[0087] Stainless steels can also be used as current collectors, especially if they contain titanium or aluminum as alloying elements or have a thin layer of a protective oxide on the surface.

[0088] Other substrates used as current collectors, such as base metal foils, may be used coated with a protective coating to prevent dissolution of these foils caused by the presence of electrolyte in contact with them.

[0089] These base metal foils may be copper, nickel or metal alloy foils such as stainless steel foils, Fe-Ni alloys, Be-Ni-Cr alloys, Ni-Cr alloys or Ni-Ti alloys.

[0090] The coating that can be used to protect the substrate used as the current collector can be of various nature. It can be: A thin layer of the same material as the electrodes, obtained by a sol-gel process, which is non-porous and therefore prevents contact between the electrolyte and the metal current collector; a thin layer obtained by vacuum deposition, in particular physical vapor deposition (PVD) or chemical vapor deposition (CVD), of the same material as the electrodes; A defect-free, dense thin metal layer, such as a thin metal layer of gold, titanium, platinum, palladium, tungsten or molybdenum. These metals have good electrical conductivity and can be used to protect the current collector because they are resistant to heat treatments in subsequent electrode manufacturing processes. This layer can be formed by electrochemistry, PVD, CVD, evaporation, ALD, among others. Thin layers of carbon, such as diamond-like carbon, graphite, deposited by ALD, PVD, CVD or by inking of sol-gel solutions, which can obtain a carbon-doped inorganic phase after heat treatment to make them conductive, or layers of conductive oxides, such as a layer of ITO (indium tin oxide), deposited only on the cathode substrate, since the oxide is reduced at low potentials; · A layer of conductive nitride, such as a layer of TiN, deposited only on the cathode substrate, since nitrides intercalate lithium at low potentials.

[0091] Coatings that can be used to protect substrates used as current collectors must be electronically conductive without becoming too resistive and impairing the operation of the electrode that is subsequently deposited on the coating.

[0092] Generally, to avoid unduly affecting the operation of the battery cell, the µA / cm2 measured at the substrate at the operating potential of the electrodes should be used. 2 The maximum dissolution current, expressed as μAh / cm 2 The capacitance must be 1 / 1000 of the surface capacitance of the electrode, expressed as

[0093] A porous, preferably mesoporous, inorganic layer is deposited on the anode layer 12 and / or the cathode layer 22. The electrophoretic deposition of the layer of material completely covers the electrode layer surface, regardless of the shape and the presence of rough defects. It can therefore guarantee the dielectric properties of the layer. In an advantageous embodiment, high-frequency current pulses are applied, for the reason that they prevent fluctuations of the electric field in the suspension during deposition and the formation of gas bubbles at the surface of the electrodes. The thickness of the porous inorganic layer thus deposited is advantageously less than 10 μm, preferably less than 8 μm, more preferably between 1 and 6 μm.

[0094] The compactness of the layer obtained by electrophoretic deposition and the absence of significant amounts of organic compounds in the layer may limit or prevent the risk of the layer cracking or the appearance of other defects during the drying step. According to an essential feature of the invention, the porous inorganic layer according to the invention does not comprise an organic binder.

[0095] 4. Deposition of porous inorganic layers by dip coating Regardless of the chemical nature of the nanoparticles used, a dip-coating method and thus the deposition of nanoparticles of inorganic material is possible. This deposition method preferably provides that the inorganic nanoparticles have little or no charge. The step of depositing the inorganic nanoparticles by dip-coating, followed by the step of drying the resulting layer, is repeated as many times as necessary to obtain a layer of the desired thickness.

[0096] Although this sequence of coating steps by dipping / drying is time consuming, the deposition method by dip coating is simple, safe, easy to implement and easy to industrialize, making it possible to obtain a homogeneous and compact final layer.

[0097] These nanoparticles are deposited in the anode 12 and / or cathode 22 layers, are themselves formed by suitable processes onto a conductive substrate to be used as a current collector, and / or directly onto a sufficiently conductive substrate to be used as a current collector as described in section 3 above.

[0098] 5. Processing and properties of the deposited layers After their deposition, the layers must be dried; drying must not lead to the formation of cracks, and for this reason drying is preferably carried out under controlled humidity and temperature conditions.

[0099] The dried layer can be solidified by a pressing and / or heat treatment step. In a highly advantageous embodiment of the invention, this mechanical (i.e. mechanical compression) and / or heat treatment leads to a partial coalescence of the primary nanoparticles in the aggregates or agglomerates and between adjacent aggregates or agglomerates; this phenomenon is called "necking" or "neck formation". It is characterized by two particles in contact partially coalescing and remaining separated, connected by a neck (shrinkage); this is illustrated in FIG. 1. In this way, a three-dimensional network of interconnected particles is formed, which comprises an open porosity formed by interconnected pores. The size of these pores is advantageously mesopores, i.e. in the range of 2 to 50 nm. Advantageously, the open pores of said porous inorganic layer have a volume of more than 25%, preferably more than 30%, of the total volume of said porous inorganic layer. If the pore volume of the porous inorganic layer is less than 25%, a three-dimensional network of interconnected particles is not obtained; in this case, the resulting layer has a closed porosity whose structure cannot be subsequently impregnated with a phase carrying lithium ions.

[0100] The temperature necessary to obtain "necking" varies from material to material; the duration of the treatment varies with the temperature, in light of the diffusive nature of the phenomenon that causes necking.

[0101] In some cases, this heat treatment, if carried out at a sufficient temperature, for example 350° C., also makes it possible to remove organic residues originating from the manufacturing process of the suspension of nanoparticles or solvent.

[0102] Heat treatment and / or pressing may be advantageously carried out during later steps of manufacture to be used for other purposes; this is explained in section 6 below, regarding the manufacture of batteries.

[0103] 6. Battery Assembly One of the aims of the present invention is to provide a new thin-layer electrolyte for secondary lithium-ion batteries. In the following, the implementation of a battery with an electrolyte containing a porous inorganic layer is described.

[0104] A nanoparticle suspension, which is the precursor of the porous inorganic layer, is prepared solvothermally, in particular hydrothermally, which directly gives nanoparticles with good crystallinity. The porous organic layer is deposited by electrophoresis, inkjet, doctor blade, roll coating, curtain coating or dip coating onto the cathode layer 22 covering the substrate 21 and / or the anode layer 12 covering the substrate 11; in both cases the substrates 11, 21 must be sufficiently conductive to function as cathode or anode current collectors, respectively.

[0105] The assembly of the cell composed of the anode layer, the porous inorganic layer and the cathode layer is preferably carried out by hot pressing under an inert atmosphere. The temperature is advantageously 300-500° C., preferably 350-450° C. The pressure is advantageously 40-100 MPa. The hot pressing is carried out, for example, at 350° C. and 100 MPa.

[0106] The completely solid, rigid, organic-free cell is then immersed and impregnated with a layer that carries lithium ions. 50 Due to the size of the LiFePO4 nanoparticles (<50 nm), the impregnation of the entire cell (electrodes and separator) is achieved by capillary action. A particularly preferred separator is a LiFePO4 nanoparticle with mesoporosity. 3 Al 0.4 Sc 1.6 (PO 4 ) 3 The details of the impregnation are explained in Section 7 below.

[0107] The phase carrying the lithium ions is, for example, LiPF dissolved in an aprotic solvent. 6 Or LiBF 4 or ionic liquids containing lithium salts. Ionic liquids may also be used dissolved in a suitable solvent and / or mixed with an organic electrolyte, for example 50 wt% LiPF dissolved in EC / DMC. 6 with an ionic liquid containing a lithium salt, of the type LiTFSI:PYR14TFSI (molar ratio 1:9). The mixture of ionic liquids may be composed of those that operate at low temperatures, for example a mixture of LiTFSI:PYR13FSI:PYR14TFSI (molar ratio 2:9:9).

[0108] EC is the common abbreviation for ethylene carbonate (CAS number: 96-49-1). DMC is the common abbreviation for dimethyl carbonate (CAS number: 616-38-6). LITFSI is the common abbreviation for lithium bistrifluoromethanesulfonimide (CAS number: 90076-65-6). PYR13FSI is the common abbreviation for N-propyl-N-methylpyrrolidinium bis(fluorosulfonyl)imide. PYR14TFSI is the common abbreviation for 1-butyl-1-methylpyrrolidinium bis(trifluoromethanesulfonyl)imide.

[0109] Another example of the manufacture of a lithium-ion battery according to the present invention is given below, which comprises the following steps: (1) providing at least two conductive substrates precoated with layers of materials usable as an anode and a cathode, respectively (these layers are referred to as "anode layers" and "cathode layers"); (2) Providing a colloidal suspension containing aggregates or agglomerates of nanoparticles of at least one inorganic material, and measuring the average diameter D of the aggregates or agglomerates. 50 is 80 to 300 nm (preferably 100 to 200 nm), (3) depositing a porous inorganic layer from said colloidal suspension on at least one of the cathode and anode obtained in step (1) by electrophoresis, inkjet, doctor blade, roll coating, curtain coating or dip coating; (4) The layer thus obtained is dried, preferably with an air current, (5) stacking the cathode and anode layers, preferably laterally offset; (6) subjecting the laminate of anode and cathode layers obtained in step (5) to mechanical compression and / or heat treatment in order to align and assemble the porous inorganic layers present in the cathode and cathode layers; (7) The structure obtained in step (6) is impregnated with a lithium ion carrying phase, preferably with a lithium ion carrying phase comprising at least 50% by weight of at least one ionic liquid, to obtain a battery.

[0110] The order of steps (1) and (2) is not important.

[0111] The resulting battery is completely rigid and, if at least one ionic liquid is used, this is nanoconfined in the pores of the porous layer.

[0112] The average primary diameter D of the nanoparticles that form aggregates or agglomerates 50 It may be less than 50 nm, in which case the suspension is prepared by precipitation or solvothermal synthesis, it may also be greater than 50 nm, preferably between 50 and 150 nm, in which case a suspension obtained by wet milling may be used.

[0113] Advantageously, the anode and cathode layers may be dense electrodes, i.e. electrodes with a volume porosity of less than 20%, porous electrodes, preferably having an interconnected network of open pores or mesoporous pores, preferably having an interconnected network of open mesopores.

[0114] The porous, preferably mesoporous, electrodes have such a high specific surface area that when used with a liquid electrolyte, parasitic reactions between the electrode and the electrolyte can occur; these reactions are at least partially irreversible. In an advantageous embodiment, a very thin layer of an electronically insulating, preferably ionically conductive, material is applied to the porous, preferably mesoporous, electrode layer to prevent these parasitic reactions.

[0115] In the framework of the high density electrode, and in another advantageous embodiment, a very thin layer of electronically insulating, preferably ionically conductive, material is applied to the electrode layer in order to reduce the interfacial resistance that exists between the high density electrode and the electrolyte.

[0116] This layer of electronically insulating, preferably ionically conductive, material is advantageously 10 -8 It has an electronic conductivity of less than 1.5 S / cm. Advantageously, this deposition is carried out on at least one face of the electrode, forming the interface between the electrode and the electrolyte, whether porous or dense. This layer may be composed, for example, of alumina, silica or zirconia. At the cathode, Li 4 Ti 5 O 12 You can use Li 4 Ti 5 O 12 Alternatively, another material may be used that has the property of not intercalating lithium at the operating voltage of the cathode and behaving as an electronic insulator, such as

[0117] Alternatively, the electronically insulating layer may be ionically conductive, advantageously at least 10 -8The material has an electronic conductivity of less than 1.5 S / cm. The material must be selected so that it does not insert lithium at the operating voltage of the battery, but only transports it. This includes, for example, Li 3 PO 4 , Li 3 BO 3 Or, Li 7 La 3 Zr 2 O 12 Lithium lanthanum zirconium oxides (LLZO) such as 3x La 2 / 3-x TiO 3 Lithium lanthanum titanium oxide (LLTO), lithium aluminum titanium phosphate (LATP), and lithium aluminum germanium phosphate (LAGP) have a limited range of operating potentials and can only be used in contact with a cathode; above that range, they can insert lithium into their crystal structure.

[0118] This deposition further improves the performance of lithium-ion batteries equipped with at least one electrode, whether porous or dense. In the case of impregnated porous electrodes, this deposition can suppress the interfacial faradaic reactions with the electrolyte. These parasitic reactions are more critical at high temperatures; they are responsible for reversible and / or irreversible losses of capacity. In the case of dense electrodes in contact with the electrolyte, it can limit the interfacial resistance related to the appearance of space charges.

[0119] Very advantageously, this deposition is carried out by a technique that allows a covering coating (also called conformal deposition), i.e. a deposition that faithfully reproduces the atomic topography of the substrate to which it is applied. The ALD (Atomic Layer Deposition) or CSD (Chemical Solution Deposition) techniques, as they are known, may be suitable. It may be carried out on the dense electrode before the deposition of the porous inorganic layer and before the assembly of the cell. It may be carried out on the porous, preferably mesoporous, electrode after its manufacture, before and / or after the deposition of the porous inorganic layer and before and / or after the assembly of the cell, preferably before the impregnation of the porous electrode with a phase that carries lithium ions. The deposition technique by ALD is carried out layer by layer in a cyclical manner and makes it possible to produce a sealing coating that truly reproduces the topography of the substrate; it follows the entire surface of the electrode. This covering coating typically has a thickness of 1 to 5 nm. The deposition technique by CSD makes it possible to produce a sealing coating that truly reproduces the topography of the substrate; it follows the entire surface of the electrode. This covering coating typically has a thickness of less than 5 nm, preferably of 1 to 5 nm.

[0120] If the electrode used is porous and coated with a nanolayer of an electronically insulating, preferably ionically conductive, material, the primary diameter D of the particles of the electrode material used to produce it should be taken into account in order to prevent the electronically insulating, preferably ionically conductive, layer of material from blocking the open porosity of the electrode layer. 50 is preferably at least 10 nm.

[0121] A layer of electronically insulating, preferably ionically conductive, material must only be deposited on electrodes that do not contain any organic binder. In fact, deposition by ALD is usually carried out at temperatures between 100 and 300 °C. At this temperature, there is a risk that the organic materials forming the binder (for example the polymers contained in electrodes produced by tape casting of inks) will decompose, contaminating the ALD reactor. Moreover, the presence of residual polymers in contact with the particles of active electrode material can prevent the ALD coating from covering the entire surface of the particles, which is detrimental to its effectiveness.

[0122] For example, a layer of alumina about 1.6 nm thick may be suitable.

[0123] If the electrode is a cathode, it may be constituted by a cathode material P selected from: - LiMn oxide 2 O 4 , Li 1+x Mn 2-x O 4 and 0 <x<0.15、LiCoO 2 , LiNiO 2 , LiMn 1.5 Ni 0.5 O 4 , LiMn 1.5 Ni 0.5-x X x O 4 and X is selected from Al, Fe, Cr, Co, Rh, Nd, and other rare earth elements such as Sc, Y, Lu, La, Ce, Pr, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, and Yb. <x<0.1、LiMn 2-x M x O 4 Where M=Er, Dy, Gd, Tb, Yb, Al, Y, Ni, Co, Ti, Sn, As, Mg or a mixture of these compounds. <x<0.4、LiFeO 2 , LiMn 1 / 3 Ni 1 / 3 Co 1 / 3 O 2 , LiNi 0.8 Co 0.15 Al 0.05 O 2 , LiAl x Mn 2-x O 4 where 0≦x<0.15, LiNi 1 / x Co 1 / y Mn 1 / z O 2 and x+y+z=10; - Phosphate LiFePO 4 , LiMnPO 4 , LiCoPO 4 , LiNiPO 4 , Li 3 V2 (PO 4 ) 3 ; a phosphate of the formula LiMM’PO 4 wherein M and M’ (M≠M’) are selected from Fe, Mn, Ni, Co, V; - all lithium forms of the following chalcogenides: V 2 O 5 , V 3 O 8 , TiS 2 , titanium oxysulfide (TiO y S z where z = 2 - y and 0.3 ≦ y ≦ 1), tungsten oxysulfide (WO y S z where 0.6 < y < 3 and 0.1 < z < 2), CuS, CuS 2 , preferably Li x V 2 O 5 where 0 < x ≦ 2, Li x V 3 O 8 where 0 < x ≦ 1.7, Li x TiS 2 where 0 < x ≦ 1, titanium oxysulfide and lithium oxysulfide Li x TiO y S z where z = 2 - y, 0.3 ≦ y ≦ 1, Li x WO y S z , Li x CuS, Li x CuS 2 .

[0124] When the electrode is an anode, it may be composed of an anode material P selected from the following: - carbon nanotubes, graphene, graphite; - lithium iron phosphate (of the general formula LiFePO 4 ); - oxynitrides of silicon and tin (of the general formula Si a Sn b O y N z where a > 0, b > 0, a + b ≦ 2, 0 < y ≦ 4, 0 < z ≦ 3) (also called SiTON), in particular SiSn0.87 O 1.2 N 1.72 Similarly, the general formula Si a Sn b C c O y N z Oxynitride-carbide, where a>0, b>0, a+b≦2, 0 <c<10、0<y<24、0<z<17; - Nitrides of the following types:Si x N y (especially x=3 and y=4), Sn x N y (especially x=3 and y=4), Zn x N y (especially x=3 and y=2), Li 3-x M x N (0≦x≦0.5 when M=Co, 0≦x≦0.6 when M=Ni, 0≦x≦0.3 when M=Cu); Si 3-x M x N 4 where M=Co or Fe and 0≦x≦3; - The following oxides: SnO 2 , SnO, Li 2 SnO 3 , SnSiO 3 , Li x SiO y (x>=0 and 2>y>0), Li 4 Ti 5 O 12 , TiNb 2 O 7 , Co 3 O 4 , SnB 0.6 P 0.4 O 2.9 and TiO 2 , - TiNb composite oxide containing 0-10% by weight of carbon 2 O 7 and preferably the carbon is selected from graphene and carbon nanotubes.

[0125] The electrolyte according to the invention may be implemented on dense, porous, preferably mesoporous, electrodes, whether or not coated with an electronically insulating, preferably ionically conducting, material, preferably by ALD or by chemical methods in solution, known under the acronym CSD.

[0126] To obtain a battery with high energy density and high power density, the battery advantageously comprises porous, preferably mesoporous, anode and cathode layers and an electrolyte according to the invention.

[0127] Advantageously, the anode and cathode layers, whether coated by ALD with a layer of electronically insulating, preferably ionically conducting, material, are then covered with a porous inorganic layer and hot pressed to facilitate cell assembly without inducing sintering: the deposit remains porous and can be later impregnated with electrolyte, preventing any risk of subsequent short circuits.

[0128] Advantageously, a battery comprising at least one porous, preferably mesoporous, electrode and electrolyte according to the invention has improved performance, in particular high power density.

[0129] An example of the manufacture of a lithium-ion battery according to the invention comprising at least one porous, preferably mesoporous, electrode is described below. The method comprises the following steps: (1) Primary diameter D 50 providing a colloidal suspension comprising nanoparticles of at least one cathode material having a diameter of 50 nm or less; (2) Average primary diameter D 50 providing a colloidal suspension comprising nanoparticles of at least one anode material having a diameter of 50 nm or less; (3) providing at least two conductive substrates, preferably metal, which can be used as current collectors in a battery; (4) depositing at least one thin layer of a cathode or an anode on said substrate obtained in step (3) from a suspension of nanoparticles of the material obtained in step (1) or (2), respectively, preferably by dip coating, inkjet, doctor blade, roll coating, curtain coating or electrophoresis, preferably by pulsed current constant current electrodeposition, (5) drying the layer obtained in step (4); (6) optionally depositing a layer of an electrically insulating material on the surface of the cathode and / or anode layers obtained in step (5) by ALD; (7) depositing a porous inorganic material from a colloidal suspension comprising aggregates or agglomerates of nanoparticles of at least one inorganic material onto the cathode and / or anode layers obtained in step (5) or step (6) by electrophoresis, inkjet, doctor blade, roll coating, curtain coating or dip coating to obtain a first and / or second intermediate structure; (8) drying the layer thus obtained in step (7), preferably with an air stream; (9) Producing a laminate from said first and / or second intermediate structures to obtain a laminate of the type "substrate / anode / porous inorganic layer / cathode / substrate" by either: depositing an anode layer on said first intermediate structure; or depositing a cathode layer on said second intermediate structure; or by superposing the first intermediate structure and the second intermediate structure so as to place one of the two layers of porous inorganic layer on top of the other, (10) hot pressing the laminate obtained in step (9); (11) Impregnating the structure obtained in step (10) or step (11) with a lithium ion carrying phase to obtain an impregnated structure, preferably a cell.

[0130] The order of steps (1), (2) and (3) is not important.

[0131] Advantageously, said aggregates or agglomerates of nanoparticles of at least one inorganic material have an average diameter between 80 and 300 nm, preferably between 100 and 200 nm.

[0132] Once the assembly of the stack forming the battery by hot pressing is complete, it can be impregnated with a phase carrying lithium ions. This phase may be a solution constituted by a lithium salt dissolved in an organic solvent or a mixture of organic solvents, and / or dissolved in a polymer containing at least one lithium salt, and / or dissolved in an ionic liquid (i.e. molten lithium salt) containing at least one lithium salt. This phase may also be a solution constituted by a mixture of these components. The porous, preferably mesoporous, electrode has a mean diameter D of its pores. 50 The liquid phase can be absorbed by simple capillarity when the pore diameter of these electrodes is between 2 and 80 nm, preferably between 2 and 50 nm, preferably between 6 and 30 nm, preferably between 8 and 20 nm. This completely unexpected effect is particularly advantageous when the pore diameter of these electrodes is small.

[0133] Advantageously, the porous, preferably mesoporous, electrode is impregnated with an electrolyte, preferably a phase carrying lithium ions, such as an ionic liquid comprising a lithium salt, optionally diluted with an organic solvent or a mixture of organic solvents comprising a lithium salt which may be different from the one dissolved in the ionic liquid.

[0134] In that way, a lithium-ion battery cell having a very high power density is obtained.

[0135] 7. Impregnation of porous inorganic layer As shown in the previous section, once the deposition and processing of the porous inorganic layer is completed, for example hot pressing during assembly of the stack to form the battery, it can be impregnated with a phase carrying lithium ions. This phase can be a solution constituted by a lithium salt dissolved in an organic solvent or a mixture of organic solvents and / or dissolved in a polymer containing at least one lithium salt and / or dissolved in an ionic liquid (i.e. molten lithium salt) containing at least one lithium salt. This phase can also be a solution constituted by a mixture of these components.

[0136] The inventors have found that the porous inorganic layers according to the invention are capable of absorbing a liquid phase by simple capillary action. This entirely unexpected effect is specific to the deposition of the porous inorganic layers according to the invention; it is due to the fact that the average diameter D 50 It is particularly advantageous when the thickness is 2 to 80 nm, preferably 2 to 50 nm, preferably 6 to 30 nm, and more preferably 8 to 20 nm.

[0137] In an advantageous embodiment of the invention, the porous inorganic layer has a porosity, preferably mesoporous, of more than 30% and an average diameter D 50 The diameter of the particles is less than 50 nm and the primary diameter of the particles is less than 30 nm. Its thickness is advantageously less than 10 μm, preferably between 3 and 6 μm, preferably between 2.5 and 4.5 μm, in order to reduce the final thickness of the battery without compromising its properties. No binder is included. Its pores are impregnated by an electrolyte, such as an ionic liquid containing a lithium salt, which may be diluted with an organic solvent or a mixture of organic solvents containing a lithium salt which may be different from the one dissolved in the ionic liquid.

[0138] In one particularly advantageous embodiment, the porosity, preferably mesoporous, is preferably between 35 and 50%, more preferably between 40 and 50%.

[0139] Liquids that are "nanoconfined" or "nanotrapped" in porosity, especially in mesoporosity, can no longer escape. This is related to a phenomenon called here "absorption in mesoporous structures" (which does not appear to be described in the literature in the context of lithium-ion batteries), and cannot escape even if the cell is placed in a vacuum. The battery is then considered quasi-solid.

[0140] The phase carrying the lithium ions may be an ionic liquid containing a lithium salt, diluted with an organic solvent or a mixture of organic solvents containing a lithium salt that may be different from the one dissolved in the ionic liquid.

[0141] Ionic liquids contain cations with anions; the anions and the cations are selected so that the ionic liquid is in a liquid state in the operating temperature range of the storage battery. Ionic liquids have the advantages of high thermal stability, low flammability, non-volatility, low toxicity and good wettability of ceramics, which are materials that can be used as electrode materials. Surprisingly, the weight percentage of ionic liquid in the phase carrying lithium ions can be more than 50%, preferably more than 60%, more preferably more than 70%, which is in contrast to conventional lithium ion batteries, where the weight percentage of ionic liquid in the electrolyte must be less than 50% by weight in order for the battery to maintain a high capacity and high voltage during discharge and good stability in cycling. As shown in application US2010 / 209783A1, above 50% by weight, the capacity of the prior art batteries is low. This can be explained by the presence of polymer binders in the electrolyte of the prior art batteries; these binders are only slightly wetted by the ionic liquid, which leads to insufficient ionic conduction in the phase carrying lithium ions, causing a decrease in the capacity of the battery.

[0142] Batteries using porous electrodes according to the invention are preferably binder-free, which allows them to use more than 50% by weight of at least one ionic liquid lithium-ion carrying phase without reducing the final capacity of the battery.

[0143] The lithium ion carrying phase may comprise a mixture of several ionic liquids.

[0144] Advantageously, the ionic liquid is of the 1-ethyl-3-methylimidazolium (also called EMI+) type and / or n-propyl-n-methylpyrrolidinium (PYR 13 + (also called) and / or n-butyl-n-methylpyrrolidinium (PYR 14 + It may be a cation of bis(trifluoromethanesulfonyl)imide (TFSI, also called - ) and / or bis(fluorosulfonyl)imide (FSI - To form the electrolyte, a lithium salt such as LiTFSI may be dissolved in the ionic liquid or a solvent such as γ-butyrolactone, which is used as the solvent. γ-butyrolactone prevents the ionic liquid from crystallizing and allows a wider operating range at the temperatures of the ionic liquid, especially at low temperatures.

[0145] The lithium ion carrying phase may be an electrolyte comprising PYR14TFSI and LiTFSI; these abbreviations are defined below.

[0146] Advantageously, when the porous anode or cathode comprises a surface passivation layer of lithium phosphate, the phase carrying the lithium ions is LiBH 4 , or LiBH 4 and one or more compounds selected from LiCl, LiI, and LiBr. 4 LiBH is an excellent conductor of lithium and has a low melting point, which makes it easy to impregnate porous electrodes, especially by immersion. 4LiBH is rarely used as an electrolyte because of its extremely strong reducing power. By using a protective film on the surface of the porous lithium phosphate electrode, 4 This prevents the reduction of the electrode materials, particularly the cathode materials, and prevents deterioration of the electrodes.

[0147] Advantageously, the phase carrying lithium ions comprises at least one ionic liquid, preferably at least one ionic liquid at ambient temperature, such as, for example, PYR14TFSI, optionally diluted with at least one solvent, such as γ-butyrolactone.

[0148] Advantageously, the phase carrying lithium ions comprises between 10 and 40% by weight of solvent, preferably between 30 and 40% by weight of solvent, more preferably between 30 and 40% by weight of γ-butyrolactone.

[0149] Advantageously, the lithium ion carrying phase comprises more than 50% by weight of at least one ionic liquid and less than 50% of a solvent, which reduces safety and fire risks in the event of failure of a battery comprising such a lithium ion carrying phase.

[0150] Advantageously, the phase carrying lithium ions comprises: - 30 to 40% by weight of a solvent, preferably 30 to 40% by weight of γ-butyrolactone, and - more than 50% by weight of at least one ionic liquid, preferably more than 50% by weight of PYR14TFSI.

[0151] The lithium ion carrying phase may be an electrolyte comprising PYR14TFSI, LiTFSI and γ-butyrolactone, preferably an electrolyte comprising about 90% by weight PYR14TFSI, 0.7M LiTFSI and 10% by weight γ-butyrolactone.

[0152] 8. Sealing The battery 1 or assembly, which is a multi-layered rigid system constituted by one or more assembled cells, which may be impregnated with a phase carrying lithium ions, must be sealed in a suitable manner to ensure protection from the ambient air. The sealing system comprises at least one layer, and is preferably a stack of several layers. If the sealing system consists of a single layer, it must be deposited by ALD or be composed of parylene and / or polyimide. These sealing layers must be chemically stable, resistant to high temperatures and impermeable to the ambient air (barrier layers). One of the methods described in patent applications WO2017 / 115032, WO2016 / 001584, WO2016 / 001588 or WO2014 / 131997 may be utilized.

[0153] Advantageously, the battery or assembly may be covered with a sealing system 30 formed by a stack of several layers, i.e. a sequence, preferably z sequences, including: a first coating layer, deposited on the anode and cathode foil stack, preferably chosen from parylene, parylene type F, polyimide, epoxy resin, silicone, polyamide and / or mixtures thereof; - a second coating layer made of an electrically insulating material and deposited on the first coating layer by atomic layer deposition; This sequence can be repeated z times, z≧1. This multi-layer sequence has a barrier effect. The more the sequence of the sealing system is repeated, the greater this barrier effect becomes. It is as effective as the number of thin layers deposited.

[0154] Advantageously, the first coating layer is a polymer layer, for example made of silicone (deposited for example by impregnation or plasma-assisted chemical vapor deposition from hexamethyldisiloxane (HMDSO)), or of epoxy resin, or of polyimide, polyamide, or of polyparaxylylene (more commonly known as parylene), preferably based on parylene and / or polyimide. This first coating layer makes it possible to protect sensitive elements of the battery from its surrounding environment. The thickness of said first coating layer is preferably between 0.5 and 3 μm.

[0155] Advantageously, the first coating layer may be parylene of type C, parylene of type D, parylene of type N (CAS number: 1633-22-3), parylene of type F or a mixture of parylenes of types C, D, N and / or F. Parylene (also called polyparaxylylene or poly(p-xylylene)) is a dielectric, transparent, semi-crystalline material with high thermodynamic stability, high resistance to solvents and very low permeability. Parylene also has barrier properties that allow the battery to be protected from the external environment. If this first coating layer is composed of parylene of type F, the protection of the battery is enhanced. It may be vacuum deposited by chemical vapor deposition techniques (CVD). This first sealing layer is advantageously obtained from the condensation of gaseous monomers deposited on the surface by chemical vapor deposition techniques (CVD), thereby allowing a conformal, thin and uniform coating of all accessible surfaces of the object. It makes it possible to track the changes in the volume of the battery during its operation and its elastic properties facilitate a specific cutting of the battery. The thickness of this first sealing layer is between 2 and 10 μm, preferably between 2 and 5 μm, more preferably about 3 μm. It covers all accessible surfaces of the laminate, closing the access to the pores of these accessible surfaces only at its surface, allowing the chemical nature of the substrate to be homogenized. The first covering layer does not enter the pores of the battery or assembly, since the size of the deposited polymer is too large to enter the pores of the laminate.

[0156] This first coating layer is advantageously rigid; it cannot be considered a flexible surface. Thus, sealing can be performed directly on the laminate and the coating can penetrate all accessible pores.

[0157] It should be noted here that due to the absence of binders in the pores of the electrolyte and / or electrodes according to the present invention, the battery can be subjected to vacuum processing.

[0158] In one embodiment, a first layer composed of parylene is deposited, such as a layer of parylene C, a layer of parylene D, a layer of parylene N (CAS number: 1633-22-3), or a layer comprising a mixture of parylenes C, D and / or N. Parylene (also called polyparaxylylene or poly(p-xylylene)) is a dielectric, transparent, semi-crystalline material with high thermodynamic stability, excellent resistance to solvents and very low permeability.

[0159] This layer of Parylene can protect sensitive elements of the battery from its surrounding environment, and this protection is enhanced when this first encapsulation layer is composed of Parylene N.

[0160] In another embodiment, a polyimide-based first layer is deposited, which protects sensitive elements of the battery from its surrounding environment.

[0161] In another embodiment, the first encapsulation layer is composed of a first encapsulation layer of polyimide, preferably 1 μm thick, on which a second layer of parylene, preferably 2 μm thick, is deposited. This protection is enhanced if this second layer is composed of parylene, preferably parylene N, about 2 μm thick. The layer of polyimide combined with the layer of parylene improves the protection of sensitive elements of the battery from its surrounding environment.

[0162] However, the inventors have observed that if this first layer is based on parylene, it is not stable enough in the presence of oxygen, and if this first layer is based on polyimide, it does not seal well, especially in the presence of water. For these reasons, a second layer is deposited that coats the first layer.

[0163] Advantageously, a second covering layer made of an electrically insulating material can be deposited on this first layer by a conformal deposition technique such as atomic layer deposition (ALD). Thus, a conformal coverage is obtained on all accessible surfaces of the stack previously covered with a first covering layer, preferably a first layer of parylene and / or polyimide; this second layer is preferably an inorganic layer. The growth of a layer deposited by ALD is influenced by the nature of the substrate. A layer deposited by ALD on a substrate having various regions of different chemical nature may show an uneven growth, which may lead to a loss of integrity of this second protective layer. The second covering layer deposited on this first layer of parylene and / or polyimide protects the first layer of parylene and / or polyimide from air and increases the lifetime of the sealed battery.

[0164] ALD deposition techniques are particularly suitable for covering very rough surfaces in a globally hermetic and conformal manner. They make it possible to achieve conformal layers that are defect-free, e.g. without holes (layers that are called "pinhole-free"), and that exhibit very good barrier properties. Their WVTR coefficients are very small. The WVTR coefficient (Water Vapor Transmission Rate) allows one to evaluate the vapor permeability of a sealing system. The smaller the WVTR coefficient, the more hermetic the sealing system. For example, a 100 nm thick Al deposited by ALD 2 O 3 The layer has a vapor permeability of 0.00034g / m 2 The second coating layer is made of a ceramic material, a glassy material or a glass-ceramic material, such as an oxide, Al 2 O 3This second coating layer may be of the nitride, phosphate, oxynitride or siloxane type, and has a thickness of less than 200 nm, preferably between 5 and 200 nm, more preferably between 10 and 100 nm, 10 and 50 nm, and even more preferably about 50 nm.

[0165] This second covering layer deposited by ALD makes it possible, on the one hand, to ensure hermeticity of the structure, i.e. to prevent the migration of water inside the structure, and, on the other hand, to protect the first covering layer, preferably a layer of parylene and / or polyimide, preferably of type F parylene, from the surrounding environment in order to prevent its degradation.

[0166] However, these layers deposited by ALD are mechanically very fragile and require a rigid supporting surface to ensure their protective role: if a fragile layer is deposited on a flexible surface, cracks will form and the integrity of this protective layer will be lost.

[0167] In one embodiment, to enhance the protection of the battery cell from the external environment, a third coating layer is deposited on the second coating layer or on the sealing system 30 constituted by a stack of several layers as described above, i.e. in a sequence of the sealing system, preferably in a z sequence, where z ≧ 1. Typically, this third layer is made of a polymer, for example a silicone (for example deposited by impregnation or plasma-assisted chemical vapor deposition from hexamethyldisiloxane (HMDSO, CAS number: 107-46-0)), or an epoxy resin, or a polyimide, or a parylene.

[0168] Additionally, the encapsulation system may include alternating successive layers of parylene and / or polyimide, preferably about 3 μm thick, and layers composed of an electrically insulating material, such as an inorganic layer conformally deposited by ALD as described above, to form a multi-layer encapsulation system. To improve the performance of the encapsulation, the encapsulation system may include a first layer of parylene and / or polyimide, preferably about 3 μm thick, a second layer conformally deposited by ALD on the first layer and composed of an electrically insulating material, preferably an inorganic layer, a third layer of parylene and / or polyimide, preferably about 3 μm thick, deposited on the second layer, and a fourth layer composed of an electrically insulating material conformally deposited by ALD on the third layer.

[0169] The battery or assembly thus sealed by this sequence of sealing systems, preferably by the z-sequence, may then be coated with a final coating layer to mechanically protect the stack thus sealed and, optionally, to provide an aesthetic aspect. This final coating layer protects the battery and prolongs its life. Advantageously, this final coating layer is also selected to be resistant to high temperatures and to have sufficient mechanical resistance to protect the battery during subsequent use. Advantageously, the thickness of this final coating layer is between 1 and 50 μm. Ideally, the thickness of this final coating layer is about 10 to 15 μm, such a thickness range allowing the battery to be protected from mechanical damage.

[0170] Advantageously, in order to enhance the protection of the battery cell from the external environment and to protect it from mechanical damage, this last covering layer is deposited on a sealing system constituted by a stack of several layers as described above, i.e. on a sequence of sealing systems, preferably on a z sequence with z≧1, on this alternating succession of inorganic layers, preferably of parylene and / or polyimide, preferably with a thickness of about 3 μm and conformally deposited by ALD. This last covering layer preferably has a thickness of about 10-15 μm. This last covering layer is preferably based on epoxy resin, polyethylene naphthalate (PEN), polyimide, polyamide, polyurethane, silicone, sol-gel silica or organosilica. Advantageously, this last covering layer is deposited by immersion. Typically, this last layer is composed of a polymer, for example of a silicone (for example deposited by immersion or by plasma-assisted chemical vapor deposition from hexamethyldisiloxane (HMDSO)), or of an epoxy resin, or of a parylene, or of a polyimide. For example, a layer of silicone (typically about 15 μm thick) may be deposited by injection to protect the battery from mechanical damage. These materials are resistant to high temperatures and allow the battery to be easily assembled by welding to an electronic substrate without glass transition. Advantageously, the battery is sealed on four of the six sides of the stack. The sealing layer surrounds the periphery of the stack, while protection from the ambient air for the rest is given by a layer obtained by the termination.

[0171] After the sealing step, the thus sealed laminate is then cut along the cut surfaces to obtain unit battery components with the battery anode and cathode connections 50 exposed on each of the cut surfaces. The sealing system 30 then covers, preferably continuously, four of the six sides of the battery, and the other two sides of the battery are subsequently covered by the terminations 40, so that the system can be assembled without welding.

[0172] In an advantageous embodiment, the laminate thus sealed and cut may be impregnated, in an anhydrous atmosphere, with a phase carrying lithium ions, such as an ionic liquid comprising a lithium salt, which may be diluted with an organic solvent or a mixture of organic solvents comprising a lithium salt which may be different from that dissolved in the ionic liquid, as indicated in paragraph 10 of the present application. The impregnation may be carried out by immersion in an electrolyte, such as an ionic liquid comprising a lithium salt, which may be diluted with an organic solvent or a mixture of organic solvents comprising a lithium salt which may be different from that dissolved in the ionic liquid. The ionic liquid immediately enters the pores by capillary action.

[0173] After the steps of sealing, cutting and optionally impregnating the battery, terminations 40 are added to provide the electrical contacts necessary for proper operation of the battery.

[0174] 9. Termination Advantageously, the battery comprises terminations 40 where the current collectors emerge, at the cathode and at the anode. Preferably, the anode and cathode connections are on opposite sides of the stack. A termination system 40 is deposited around these connections 50. The connections can be metallized using plasma deposition techniques known to those skilled in the art, preferably by ALD and / or by immersion in a molten bath of conductive epoxy resin (filled with silver) and / or tin. Preferably, the terminations are made up of a stack including, in succession, a first thin conductive coating layer, preferably metallic, deposited by ALD, a second layer of epoxy resin filled with silver deposited on this first layer, and a third layer based on tin deposited on this second layer. The first conductive layer deposited by ALD is used to protect that area of ​​the battery from moisture. This first conductive layer deposited by ALD is optional. It allows to extend the calendar life of the battery by reducing the WVTR at the termination. This first thin coating layer may in particular be metal or metal nitride based. The second layer, made of silver-filled epoxy resin, allows the connection to be "flexible" without breaking the electrical contact when the electrical circuit is subjected to thermal and / or vibration stresses.

[0175] A third metallized layer, based on tin, is used to ensure the weldability of the battery. In other embodiments, this third layer may consist of two layers of different materials. The first layer is in contact with a layer of silver-filled epoxy resin. This layer is made of nickel, by electrodeposition. This nickel layer is used as a thermal barrier to protect the rest of the component from diffusion during the assembly step, by remelting. The last layer deposited on this nickel layer is also a metallized layer, preferably made of tin, in order to make it compatible with the assembly of the interface, by remelting. This tin layer can be deposited by immersion in a molten tin bath or by electrodeposition; these techniques are known as such.

[0176] Certain assemblies on copper tracks with micro-wiring may require a final metallization layer of copper. Such a layer can be realized by electrodeposition instead of tin.

[0177] In another embodiment, termination 40 may be constructed from a laminate including, in sequence, a layer constructed from a silver-filled epoxy resin and a second layer of tin or nickel-based material deposited on the first layer.

[0178] In another embodiment, termination 40 may be constructed from a laminate including, in sequence, a layer of silver-filled epoxy resin, a nickel-based second layer deposited on the first layer, and a tin or copper-based third layer.

[0179] In another preferred embodiment, the termination 40 is made up of a first stack at the ends of the cathode and anode connections, comprising successively a first layer made of a graphite filled material, preferably a graphite filled epoxy resin, and a second layer comprising copper metal obtained from an ink filled with copper nanoparticles deposited on the first layer, and this first stack of terminations is then sintered by means of infrared flash lamps to obtain the coating of the cathode and anode connections with a layer of copper metal.

[0180] According to the final application of the battery, the termination part may further comprise a second laminate arranged on the first laminate of the termination part, which comprises in succession a first layer of a tin-zinc alloy, preferably deposited by immersion in a molten tin-zinc bath, to ensure hermeticity of the battery at minimal cost, and a second layer of pure tin-based material, deposited by electrodeposition, or a second layer comprising a silver, palladium and copper-based alloy, deposited on this first layer of the second laminate.

[0181] The terminations 40 allow for alternating positive and negative electrical connections at each of the ends of the battery. These terminations 40 allow for parallel electrical connections to be made between different elements of the battery. To this end, only the cathode connection 50 is present at one end, while the anode connection 50 is available at the other end.

[0182] In another preferred embodiment, a lithium ion battery is manufactured according to the present invention by a method comprising the following steps: (1) providing a colloidal suspension comprising aggregates or agglomerates of nanoparticles of at least one inorganic material, the aggregates or agglomerates having an average diameter of 80-300 nm (preferably 100-200 nm); (2) providing at least one electrode; (3) depositing at least one porous inorganic layer on said electrode from a suspension of particles of inorganic material obtained in step (1) by electrophoresis, inkjet, doctor blade, roll coating, curtain coating or dip coating; (4) drying the porous inorganic layer, preferably with an air stream, to obtain a porous inorganic layer; (5) subjecting the porous inorganic layer to mechanical compression and / or heat treatment; (6) optionally impregnating the porous inorganic layer obtained in step (5) with a phase carrying lithium ions; (7) carrying out a stacking of alternating thin cathode and anode layers, preferably laterally offset, such that at least one porous inorganic layer is disposed between the cathode and anode layers; (8) consolidating the laminate by mechanical compression and / or heat treatment to obtain an assembled laminate; (9) Optionally, the assembled stack obtained in step (8), including said porous inorganic layer, is impregnated with a phase carrying lithium ions.

[0183] After step (9) of the method for producing a lithium ion battery according to the present invention, the following is carried out: depositing on the assembled stack a sealing system constituted successively, alternatingly, by a series of layers, i.e. by a sequence, preferably by a z-sequence, comprising: a first coating layer, deposited on the assembled stack, preferably chosen from parylene, parylene type F, polyimide, epoxy resin, silicone, polyamide and / or mixtures thereof; a second coating layer made of an electrically insulating material and deposited on the first coating layer by atomic layer deposition; This sequence can be repeated z times, where z>=1. a final coating layer is deposited on this successive layer, the final coating layer being made of a material selected from the group consisting of epoxy resin, polyethylene naphthalate (PEN), polyimide, polyamide, polyurethane, silicone, sol-gel silica or organosilica; - cutting the assembled stack thus sealed along two cutting planes, exposing the anode and cathode connections of the assembled stack on each of said cutting planes, such that the sealing system covers, preferably continuously, four of the six faces of said assembled stack, to obtain a basic battery; - optionally impregnating the sealed and cut elementary battery with a phase carrying lithium ions, - on and around these anode and cathode connections the following are deposited in succession: a first layer of graphite filled material, preferably graphite filled epoxy resin; a second layer comprising metallic copper obtained from an ink filled with copper nanoparticles, deposited on the first layer; - heat treatment of the layer obtained, preferably by means of infrared flash lamps, so as to obtain the coating of the cathode and anode connections with a layer of metallic copper, - on and around this first stack of terminal portions, in succession, a second stack may be deposited, comprising: a first layer of tin-zinc alloy, preferably deposited by immersion in a molten tin-zinc bath, to ensure hermeticity of the battery at minimal cost; and A second layer based on pure tin, deposited by electrodeposition, or a second layer comprising a silver, palladium and copper based alloy, deposited on this first layer in a second stack.

[0184] In this method, the deposition, by ALD or chemical solution deposition CSD, of a layer of an electronically insulating, preferably ionically conductive, material can be carried out after treatment of the porous inorganic layer by mechanical compression and / or heat treatment, after solidification of the stack by mechanical compression and / or heat treatment so as to make it possible to obtain an assembled stack, or after cutting according to two cut planes so as to expose the anode and cathode connections of the assembled stack on each of the cut planes. This deposition of a layer of electronically insulating, preferably ionically conductive, material is advantageously carried out before an optional step of impregnating the porous inorganic layer with a phase carrying lithium ions. This deposit preferably has a thickness of less than 5 nm.

[0185] In this method, the impregnation of the porous inorganic layer with the phase carrying lithium ions may be carried out after treatment of the porous inorganic layer by mechanical compression and / or heat treatment, after solidification of the stack by mechanical compression and / or heat treatment so as to obtain an assembled stack, or after cutting of the assembled stack according to two cutting planes so as to expose the anode connection and the cathode connection on each of the cutting planes. In another preferred embodiment, a lithium ion battery is manufactured according to the invention by the same method as the one described above, except that step (1) comprises the following steps: (1a) Primary diameter D 50 preparing a colloidal suspension comprising nanoparticles of at least one inorganic material P having a particle size of 50 nm or less; (1b) destabilizing the nanoparticles present in said colloidal suspension to form particle aggregates or agglomerates having an average diameter of 80-300 nm, preferably 100-200 nm, said destabilization being preferably carried out by adding a destabilizing agent such as a salt, preferably LiOH.

[0186] Advantageously, the anode and cathode connections are on opposite sides of the stack.

[0187] All of the above-mentioned embodiments relating to the assembly of the battery, the impregnation of the porous inorganic layer, the sealing system and the deposition of the terminations may be combined independently of each other, if such combinations are practical for the skilled person. EXAMPLES

[0188] Example 1: Li deposited on the cathode layer 3 PO 4 Implementation of the mesoporous electrolyte layer based on a.Li 3 PO 4 Conducting a suspension of nanoparticles Two solutions were prepared: 11.44g of CH 3 COOLi, 2H 2 O was dissolved in 112 ml of water, and then 56 ml of water was added to the solvent under vigorous stirring to obtain solution A.

[0189] 4.0584g H 3 PO 4 was diluted with 105.6 ml of water, and then 45.6 ml of ethanol was added to this solution to obtain a second solution, hereafter referred to as solution B.

[0190] Solution B was then added to solution A with vigorous stirring.

[0191] The resulting solution becomes completely transparent after the disappearance of the air bubbles formed during mixing and the addition of an Ultraturrax to homogenize the solvent. TMThe mixture was added to 1.2 liters of acetone under the action of a type homogenizer. A white precipitate in the liquid phase suspension was immediately observed.

[0192] The reaction medium was homogenized for 5 minutes and then stirred with a magnetic stirrer for 10 minutes. It was decanted for 1-2 hours. The supernatant was then discarded and the remaining suspension was centrifuged at 6000 rpm for 10 minutes. Then 300 ml of water was added to bring the precipitate back into suspension (using a sonotrode, magnetic stirrer). To the colloidal suspension thus obtained, 125 ml of a solution of sodium tripolyphosphate 100 g / l was added, under vigorous stirring. In that way the suspension was more stabilized. Then the suspension was sonicated using a sonotrode. Then the suspension was centrifuged at 8000 rpm for 15 minutes. Then its main components were redispersed in 150 ml of water. Then the suspension obtained was again centrifuged at 8000 rpm for 15 minutes and the obtained main components were redispersed in 300 ml of ethanol, obtaining a suspension capable of carrying out electrophoretic deposition.

[0193] In this way, 10 nm Li 3 PO 4 Agglomerates of about 100 nm formed from primary particles of were obtained by suspending in ethanol.

[0194] b.Li 3 PO 4 Implementation of the porous inorganic layer according to the invention based on a suspension of nanoparticles of i.LiCoO 2 Implementation of the based mesoporous cathode LiCoO 2 A suspension of crystalline nanoparticles was prepared by hydrothermal synthesis. For 100 ml of suspension, 20 ml of a 0.5 M aqueous solution of cobalt nitrate hexahydrate was added to 20 ml of a 3 M solution of lithium hydroxide monohydrate under stirring, followed by addition of 50% H 2 O 2 The reaction mixture was added dropwise to 20 ml of 100 ml of 1.0 mL ...

[0195] A black precipitate was obtained in suspension in the solvent. This precipitate was subjected to a series of centrifugation-redispersion steps in water until a suspension was obtained with a conductivity of about 200 μS / cm and a zeta potential of -30 mV. The size of the primary particles was about 10-20 nm, and the size of the aggregates was 100-200 nm. The product was characterized by X-ray diffraction and electron microscopy.

[0196] These aggregates were electrophoretically deposited in aqueous solvent onto a 5 μm thick stainless steel foil by applying a pulsed current of 0.6 A peak and 0.2 A average; the applied voltage was about 4-6 V for 400 s. A deposit of about 4 μm thickness was thus obtained. The nanoparticles were welded together, improving their adhesion to the substrate and the LiCoO 2 For recrystallization, the mixture was solidified at 600°C in air for 1 hour.

[0197] ii. Li 4 Ti 5 O 12 Implementation of the mesoporous anode based on: Li 4 Ti 5 O 12 A suspension of nanoparticles of was prepared by glycothermal synthesis: 190 ml of 1,4-butanediol was poured into a beaker and 4.25 g of lithium acetate was added while stirring. The solution was kept stirred until the acetate was completely dissolved. 16.9 g of titanium butoxide was taken under an inert atmosphere and placed into the acetate solution. The solution was then stirred for a few minutes before being transferred to an autoclave pre-filled with an additional 60 ml of butanediol. The autoclave was then closed and purged with nitrogen for at least 10 minutes. The autoclave was then heated to 300 °C at a rate of 3 °C / min and maintained at this temperature for 2 hours while stirring. Finally, it was left to cool while stirring.

[0198] A white precipitate was obtained in suspension in the solvent. This precipitate underwent a series of centrifugation-redispersion in ethanol steps to obtain a pure colloidal suspension with low ionic conductivity. It contained approximately 150 nm aggregates formed from 10 nm primary particles. The zeta potential was approximately -45 mV. The product was characterized by X-ray diffraction and electron microscopy. Figure 2A shows the diffractogram and Figure 2B shows a snapshot of the primary nanoparticles obtained by transmission electron microscopy.

[0199] These aggregates were electrophoretically deposited in aqueous medium on a 5 μm thick stainless steel foil by passing a pulsed current of 0.6 A peak and 0.2 A average; the applied voltage was about 3-5 V for 500 s. In that way, a deposit of about 4 μm thickness was obtained. The nanoparticles were welded together, improving their adhesion to the substrate and Li 4 Ti 5 O 12 For recrystallization, the powder was solidified by RTA annealing in nitrogen at 40% power for 1 hour.

[0200] iii. Li as described in part a) above on the previously prepared anode and cathode layers. 3 PO 4 Implementation of porous inorganic layers from suspensions of nanoparticles Next, Li 3 PO 4 A thin porous layer of the Li obtained above was applied to the previously prepared anode and cathode surfaces. 3 PO 4 A suspension of nanoparticles was electrophoretically deposited by applying an electric field of 20 V / cm for 90 s to obtain a layer approximately 1.5 μm thick, which was then dried in air at 120 °C to remove traces of organic residues and then calcined in air at 350 °C for 1 h.

[0201] Example 2: Electrochemical Cell Implementation A previously prepared electrode (LiCoO 2 and Li 4 Ti 5 O 12 ) each of which was coated with 1.5 μm porous Li 3 PO4 After depositing Li 3 PO 4 The two subsystems were laminated together so that the membranes of the two subsystems were in contact with each other. The laminate was then vacuum hot pressed.

[0202] To do this, the laminate was placed under a pressure of 1.5 MPa and -3 The laminate was then vacuum dried at bar for 30 minutes. The press platens were then heated to 450° C. at a rate of 4° C. / s. At 450° C., the laminate was then hot pressed under a pressure of 45 MPa for 1 minute and the system was cooled to ambient temperature.

[0203] Assembly was performed to obtain a rigid multi-layer system composed of one or more assembled battery cells.

[0204] The assembly was then immersed in an electrolyte containing 0.7 M PYR14TFSI25 and LiTFSI. The ionic liquid immediately enters the porosity by capillary action. The system was left to soak for 1 min, and then the surface of the cell stack was covered with N 2 Drying on the curtain.

Claims

1. A thin layer electrolyte (13, 23) in an electrochemical device, the electrolyte comprises a porous inorganic layer impregnated with a lithium ion carrying phase; said porous inorganic layer having an interconnected network of open pores with an average diameter D50 of less than 100 nm and a volume of more than 25% of the total volume of said thin-layer electrolyte; The porous inorganic layer does not contain an organic binder, A thin-layer electrolyte, characterized in that the thickness of the thin-layer electrolyte is less than 10 μm.

2. A thin-layer electrolyte (13, 23) according to claim 1, A thin-layer electrolyte, wherein the open pores of the porous inorganic layer have a volume of 30-50% of the total volume of the thin-layer electrolyte.

3. A thin-layer electrolyte (13, 23) according to claim 1 or 2, The porous inorganic layer includes an electronic insulating material, and Al 2 O 3 , SiO 2 , ZrO 2 and / or a thin-layer electrolyte, characterized in that it is selected from a material selected from the group formed by: ・General formula Li d A 1 x A 2 y (TO 4 ) z Garnet, where ・A 1 is a cation in the oxidation state +II; and ・A 2 is a cation in the oxidation state +III; and ・(TO 4 ) is an anion, T is an atom in the oxidation state +IV, which is located at the center of a tetrahedron formed by oxygen atoms, and TO 4 preferably represents a silicate or zirconate anion, in which all or part of the element T in oxidation state +IV is replaced by an atom in oxidation state +III or +V; d is from 2 to 10; x is from 2.6 to 3.4; y is from 1.7 to 2.3, and z is from 2.9 to 3.1; Garnet, selected from: Li 7 La 3 Zr 2 O 12 Li 6 La 2 BaTa 2 O 12 Li 5.5 La 3 Nb 1.75 In 0.25 O 12 Li 5 La 3 M 2 O 12 , M=Nb or Ta or a mixture of the two compounds; Li 7-x Ba x La 3-x M 2 O 12 , 0≦x≦1 and M=Nb or Ta or a mixture of the two compounds; Li 7-x La 3 Zr 2-x M x O 12 , 0≦x≦2 and M=Al, Ga or Ta or a mixture of two or three of these compounds; Lithium phosphate, selected from: NaSICON type phosphates, Li 3 P.O. 4 LiPO 3 ; Li called "LASP" 3 A 0.4 S.C. 1.6 (P.O. 4 ) 3 Li 1.2 Zr 1.9 Ca 0.1 (P.O. 4 ) 3 LiZr 2 (P.O. 4 ) 3 Li 1+3x Zr 2 (P 1-x S x O 4 ) 3 , 1.8<x<2.3; Li 1+6x Zr 2 (P 1-x B x O 4 ) 3 , 0≦x≦0.25; Li 3 (Sc 2-x M x ) (PO 4 ) 3 , M=Al or Y and 0≦x≦1; Li 1+x M x (Sc) 2-x (P.O. 4 ) 3 M=Al, Y, Ga or a mixture of these three compounds and 0≦x≦0.8; Li 1+x M x (Ga 1-y S.C. y ) 2-x (P.O. 4 ) 3 , 0≦x≦0.8; 0≦y≦1 and M=Al or Y or a mixture of the two compounds; Li 1+x M x (Ga) 2-x (P.O. 4 ) 3 , M=Al, Y or a mixture of the two compounds, 0≦x≦0.8; Li 1+x A x Ti 2-x (P.O. 4 ) 3 , 0≦x≦1, referred to as "LATP"; or Li 1+x A x Ge 2-x (P.O. 4 ) 3 , 0≦x≦1, referred to as "LAGP"; or Li 1+x+z M x (Ge 1-y Ti y ) 2-x S z P 3-z O 12 , 0≦x≦0.8 and 0≦y≦1.0 and 0≦z≦0.6 and M=Al, Ga or Y or a mixture of two or three of these compounds; Li 3+y (Sc 2-x M x ) Q y P 3-y O 12 , M=Al and / or Y and Q=Si and / or Se, 0≦x≦0.8 and 0≦y≦1; or Li 1+x+y M x S.C. 2-x Q y P 3-y O 12 , M=Al, Y, Ga or a mixture of the three compounds and Q=Si and / or Se, 0≦x≦0.8 and 0≦y≦1; or Li 1+x+y+z M x (Ga 1-y S.C. y ) 2-x Q z P 3-z O 12 , 0≦x≦0.8; 0≦y≦1; 0≦z≦0.6, M=Al or Y or a mixture of the two compounds and Q=Si and / or Se; or Li 1+x Zr 2-x B x (P.O. 4 ) 3 , 0≦x≦0.25; or Li 1+x Zr 2-x Ca x (P.O. 4 ) 3 , 0≦x≦0.25; or Li 1+x M 3 x M 2-x P 3 O 12 , 0≦x≦1 and M 3 = Cr, V, Ca, B, Mg, Bi and / or Mo, M = Sc, Sn, Zr, Hf, Se or Si or mixtures of these compounds; Lithium borate, selected from: Li 3 (Sc 2-x M x ) (BO 3 ) 3 , M=Al or Y, 0≦x≦1; Li 1+x M x (Sc) 2-x (BO 3 ) 3 M=Al, Y, Ga or a mixture of these three compounds; 0≦x≦0.8; Li 1+x M x (Ga 1-y S.C. y ) 2-x (BO 3 ) 3 , 0≦x≦0.8, 0≦y≦1 and M=Al or Y; Li 1+x M x (Ga) 2-x (BO 3 ) 3 , M=Al, Y or a mixture of the two compounds, 0≦x≦0.8; Li 3 B.O. 3 , Li 3 B.O. 3 -Li 2 SO 4 , Li 3 B.O. 3 -Li 2 SiO 4 , Li 3 B.O. 3 -Li 2 SiO 4 -Li 2 SO 4 ; ・Oxynitride, Li 3 P.O. 4-x N 2x/3 , Li 4 SiO 4-x N 2x/3 , Li 4 GeO 4-x N 2x/3 and 0<x<4 or Li 3 B.O. 3-x N 2x/3 where 0<x<3; Lithium compounds based on lithium oxynitride and phosphorus, called "LiPON", having the general formula LixPOyNz, where x ~ 2.8 and 2y + 3z ~ 7.8 and 0.16 < z < 0.4, and Li w P.O. x N y S z and 2x + 3y + 2z = 5 = w, or Li w P.O. x N y S z and 3.2≦x≦3.8, 0.13≦y≦0.4, 0≦z≦0.2, 2.9≦w≦3.3, or Li t P x A y O u N v S w a compound in which 5x + 3y = 5, 2u + 3v + 2w = 5 + t, 2.9 < t < 3.3, 0.84 < x < 0.94, 0.094 < y < 0.26, 3.2 < u < 3.8, 0.13 < v < 0.46, and 0 < w < 0.2; - Lithium phosphorus or boron oxynitride based materials, referred to as "LiPON" and "LIBON" respectively, which may contain silicon, sulfur, zirconium, aluminum, or a combination of aluminum, boron, sulfur and / or silicon, and in the case of lithium phosphorus oxynitride based materials, boron; - a lithium compound based on an oxynitride of lithium, phosphorus and silicon, called "LiSiPON"; Lithium oxynitrides of type LiBON, LiBSO, LiSiPON, LiSON, thio-LiSiCON, LiPONB (B, P and S represent boron, phosphorus and sulfur, respectively); Lithium oxynitrides of the LiBSO type; Lithium oxide, Li 7 La 3 Zr 2 O 12 Or Li 5+x La 3 (Zr x , A 2-x ) O 12 , A=Sc, Y, Al, Ga, and 1.4≦x≦2 or Li 0.35 La 0.55 TiO 3 Or Li 3x La 2/3-x TiO 3 , selected from 0≦x≦0.16 (LLTO); Silicate, Li 2 S 2 O 5 , Li 2 SiO 3 , Li 2 S 2 O 6 , LiAlSiO 4 , Li 4 SiO 4 , LiAlSi 2 O 6 Selected from: Antiperovskite type solid electrolyte selected from the following: Li 3 OA, where A is a halogen atom or a mixture of halogen atoms and is at least one element selected from F, Cl, Br, I or a mixture of two, three or four of these elements; Li (3-x) M x/2 OA, 0<x≦3, M is a divalent metal and is at least one of the elements Mg, Ca, Ba, Sr or a mixture of two, three or four of these elements, A is a halogen atom or a mixture of halogen atoms and is at least one element selected from F, Cl, Br, I or a mixture of two, three or four of these elements; Li (3-x) M 3 x/3 OA, 0≦x≦3, M 3 is a trivalent metal, A is a halogen atom or a mixture of halogen atoms and is at least one element selected from F, Cl, Br, I or a mixture of two, three or four of these elements; or LiCOX z Y (1-z) X and Y are halogen atoms as described above for A, and 0≦z≦1; ・ Compound La 0.51 Li 0.34 Ti 2.94 、 Li 3.4 V 0.4 Ge 0.6 O 4 、 Li 2 O-Nb 2 O 5 、 LiAlGaSPO 4 ; Li 2 CO 3 , B 2 O 3 , Li 2 O, Al(PO 3 ) 3 LiF, P 2 S 3 , Li 2 S., Li. 3 N., Li 14 Zn(GeO 4 ) 4 , Li 3.6 Ge 0.6 V 0.4 O 4 , LiTi 2 (P.O. 4 ) 3 , Li 3.25 Ge 0.25 P 0.25 S 4 , Li 1.3 A 0.3 Ti 1.7 (P.O. 4 ) 3 , Li 1+x A x M 2-x (P.O. 4 ) 3 (wherein M=Ge, Ti and / or Hf, 0<x<1), Li 1+x+y A x Ti 2-x S y P 3-y O 12 (where 0≦x≦1 and 0≦y≦1).

4. A thin-layer electrolyte (13, 23) according to any one of claims 1 to 3, the pores are impregnated with a phase carrying lithium ions, said phase being an organic solvent or a mixture of solvents in which at least one lithium salt is dissolved, and / or a polymer comprising at least one lithium salt, and / or an ionic liquid or a mixture of ionic liquids, optionally diluted with a suitable solvent, comprising at least one lithium salt, A thin-layer electrolyte comprising:

5. The thin-layer electrolyte (13, 23) according to any one of claims 1 to 3, the pores are impregnated with a lithium ion carrying phase comprising at least 50% by weight of at least one ionic liquid; A thin-layer electrolyte comprising:

6. A method for producing a thin-layer electrolyte (13, 23) deposited on an electrode (12, 22), comprising the steps of: (a) providing a colloidal suspension comprising aggregates or agglomerates of nanoparticles of at least one inorganic material, said aggregates or agglomerates having an average diameter of 80 to 300 nm; (b) providing electrodes (12, 22); (c) depositing on said electrode a porous inorganic layer from a suspension of particles of inorganic material obtained in step (a) by electrophoresis, inkjet, doctor blade, roll coating, curtain coating or dip coating; (d) drying the porous inorganic layer to obtain a porous inorganic layer; (e) subjecting the porous inorganic layer to mechanical compression and / or heat treatment, the porous inorganic layer being free of organic binder; (f) impregnating the porous inorganic layer obtained in step (e) with a phase carrying lithium ions; A method for producing a thin-layer electrolyte.

7. A method for producing a thin-layer electrolyte (13, 23) deposited on an electrode, comprising the steps of: (a1) providing a colloidal suspension comprising nanoparticles of at least one inorganic material P having a primary diameter D50 of 50 nm or less; (a2) destabilizing the nanoparticles present in the colloidal suspension to form aggregates or agglomerates of particles having an average diameter of 80 to 300 nm; (b) providing an electrode; (c) depositing on said electrode a porous inorganic layer from said suspension comprising said aggregates or agglomerates of particles of at least one inorganic material obtained in step (a2) by electrophoresis, inkjet, doctor blade, roll coating, curtain coating or dip coating; (d) drying the porous inorganic layer to obtain a porous inorganic layer; (e) subjecting the porous inorganic layer to mechanical compression and / or heat treatment, the porous inorganic layer being free of organic binder; (f) impregnating the porous inorganic layer obtained in step (e) with a phase carrying lithium ions; A method for producing a thin-layer electrolyte.

8. The method for producing a thin-layer electrolyte according to claim 6 or 7, The method for producing a thin layer electrolyte, wherein the porous inorganic layer obtained in step (c) has a thickness of less than 10 μm.

9. The method for producing a thin-layer electrolyte according to any one of claims 6 to 8, The method for producing a thin layer electrolyte, wherein the porous inorganic layer obtained in step (d) has a thickness of less than 10 μm.

10. The method for producing a thin-layer electrolyte according to any one of claims 6 to 9, The method for producing a thin-layer electrolyte, wherein the primary diameter of said nanoparticles is between 10 and 50 nm.

11. The method for producing a thin-layer electrolyte according to any one of claims 6 to 10, The method for producing a thin-layer electrolyte, wherein the average diameter of the pores in the porous inorganic layer is 2 to 50 nm.

12. The method for producing a thin-layer electrolyte according to any one of claims 6 to 11, The method for producing a thin-layer electrolyte, wherein the electrode is a high-density electrode or a porous electrode.

13. Use of the method for producing a thin-layer electrolyte according to any one of claims 6 to 12, Use of the thin-layer electrolyte for the manufacture of a device selected from the group consisting of a battery, a capacitor, a supercapacitor, a capacitance, a resistor, an inductor, and a transistor.

14. A method for producing a thin-layer battery by implementing the method for producing a thin-layer electrolyte according to any one of claims 6 to 12, comprising the steps of: -1- providing at least two conductive substrates (11, 21) pre-coated with layers of materials usable as an anode and as a cathode (the "anode layer" and the "cathode layer", respectively); -2- Providing a colloidal suspension comprising aggregates or agglomerates of nanoparticles of at least one inorganic material, said aggregates or agglomerates having an average diameter between 80 and 300 nm; -3- depositing a porous inorganic layer on each of the cathode and anode layers obtained in step-1- from a suspension of agglomerated particles of inorganic material obtained in step-2- by electrophoresis, inkjet, doctor blade, roll coating, curtain coating or dip coating; -4- The layer obtained in step-3- is dried, -5- Laminating the cathode and anode layers; -6- mechanical compression and / or heat treatment of the stack of anode and cathode layers obtained in step-5 in order to align and assemble the porous inorganic layers present in the cathode and cathode layers; -7- The structure obtained in step-6- is impregnated with a lithium ion carrying phase to obtain an assembled stack.

15. 15. The method of claim 14, The cathode is high density electrode, or a high density electrode coated with an electronically insulating layer by ALD; Or a porous electrode, or a porous electrode coated with an electronically insulating layer by ALD; or a mesoporous electrode or a mesoporous electrode coated with an electronically insulating layer by ALD; and / or the anode is high density electrode, or a high density electrode coated with an electronically insulating layer by ALD; Or a porous electrode, or a porous electrode coated with an electronically insulating layer by ALD; Or a mesoporous electrode, or a mesoporous electrode coated with an electronically insulating layer by ALD; method.

16. 16. The method according to claim 14 or 15, After step 7, do the following: The battery is deposited in alternating succession with: at least one first layer of parylene and / or polyimide over the battery; At least one second layer composed of an electrically insulating material by ALD (Atomic Layer Deposition) on said first layer of parylene and / or polyimide; and depositing a layer on the alternating sequence of at least one first layer and at least one second layer, making it possible to protect said battery from mechanical damage, forming a sealing system for said battery; - cutting the battery so sealed along two cutting planes to expose the anode and cathode connections of the battery at each of said cutting planes, such that the sealing system covers four of the six sides of the battery; At and around these anode and cathode connections, the following are deposited in succession: Optionally, a first conductive layer is deposited by ALD; depositing a second layer of a silver-filled epoxy resin base on said first conductive layer; depositing a nickel-based third layer on said second layer; Depositing a fourth layer on said third layer, which may be tin or copper based.

17. 15. The method of claim 14, After step 6, do the following: - depositing, successively and alternately, on the assembled stack a sealing system (30) formed by a series of layers, i.e. a sequence, comprising: a first coating layer, deposited on the assembled stack, selected from parylene, F-type parylene, polyimide, epoxy resin, silicone, polyamide and / or mixtures thereof; a second coating layer made of an electrically insulating material deposited by atomic layer deposition on the first coating layer; depositing, in this successive layer, a final coating layer of a material chosen from epoxy resin, polyethylene naphthalate (PEN), polyimide, polyamide, polyurethane, silicone, sol-gel silica or organosilica, - cutting the assembled stack so sealed along two cutting planes, exposing the anode and cathode connections of the assembled stack on each of said cutting planes, such that the sealing system covers four of the six sides of the assembled stack, to obtain an elementary battery; After step 7, do the following: At and around these anode and cathode junctions (50), the following are deposited in succession: a first layer of graphite filled material; a second layer comprising metallic copper obtained from an ink filled with copper nanoparticles deposited on said first layer; - heat treatment of the layer obtained in order to obtain the coating of the cathode and anode connections (50) with a layer of metallic copper, In succession, on and around this first stack of terminal ends, a second stack may be deposited, comprising: a first layer of tin-zinc alloy deposited to ensure hermeticity of the battery at minimal cost; a second layer based on pure tin, deposited by electrodeposition, or a second layer comprising an alloy based on silver, palladium and copper, deposited on this first layer of said second stack.

18. 18. The method of claim 17, The method wherein the anode and cathode connections are on opposite sides of the stack.

19. Electrochemical device comprising at least one thin electrolyte layer according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • Battery using ceramic film

    JP1993211059A

  • Separator for electrochemical cells and method for manufacturing the same

    JP2010537387A

  • Separation membrane for electrochemical elements and method for manufacturing the same

    JP2015536031A

  • Lithium metal cell precursor, lithium metal cell and method for manufacturing the same

    JP2016122528A

  • Organic / inorganic composite porous film andelectrochemical device prepared thereby

    KR1020070082402A