Heat dissipation member made of copper material and its manufacturing method

By oxidizing copper surfaces with an alkaline solution to form a copper oxide layer, the heat dissipation member achieves improved emissivity and thermal radiation efficiency, addressing the limitations of conventional treatments and enhancing cooling performance.

JP7593588B2Active Publication Date: 2024-12-03NAGASAKI PREFECTURAL GOVERNMENT
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
JP2020159900
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-24
Publication Date
2024-12-03
Estimated Expiration
2040-09-24

AI Technical Summary

Technical Problem

Existing heat dissipation members made of copper materials do not effectively enhance emissivity and thermal radiation due to high emissivity requirements, and conventional surface treatments are either ineffective or require high temperatures and complex processes.

Method used

A method involving oxidation of the copper material surface with an alkaline aqueous solution to form a copper oxide layer with increased emissivity, which can be done at low temperatures and without specialized equipment, creating a porous structure that enhances thermal radiation.

Benefits of technology

The copper oxide layer significantly improves emissivity, leading to enhanced heat dissipation efficiency with reduced thermal resistance and film peeling concerns, suitable for complex shapes and electronic equipment applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007593588000005
    Figure 0007593588000005
  • Figure 0007593588000006
    Figure 0007593588000006
  • Figure 0007593588000007
    Figure 0007593588000007
Patent Text Reader

Abstract

To provide a heat radiation member made of a copper material, having improved emissivity, and manufacturable by surface treatment at a temperature near a room temperature; and to provide a manufacturing method thereof.SOLUTION: An alkali aqueous solution is brought into contact with a prescribed heat radiation area used for heat radiation, in a surface of a raw material made of a copper material, to thereby apply oxidation treatment thereto, and to change a surface layer of the heat radiation area into a layer made of copper oxide. Thus, a heat radiation member having a heat radiation area with high emissivity is obtained.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a heat dissipation member made of a copper material and a method for manufacturing the same. [Background technology]

[0002] In recent years, the heat density of electronic devices has increased as they have become lighter and smaller. Properly dissipating the heat generated by electronic devices is necessary and important for properly utilizing the functions of the electronic devices.

[0003] Heat is transferred by conduction, convection, and radiation. Conventional heat dissipation components use materials with high thermal conductivity to quickly transfer heat from the heat source, and structures that increase the contact area with the air, such as fins, have been adopted to promote heat transfer to the air by convection. Meanwhile, with regard to radiation, there has been growing attention over the past decade in response to demands for improved heat dissipation characteristics.

[0004] Silver (422 W m -1 ·K -1 ), copper (395W m -1 ·K -1 ), gold (313W m -1 ·K -1 ), Aluminum (240W m -1 ·K -1 ) are known. Conventionally, aluminum has been generally used as a material for heat dissipation members from the viewpoint of cost. Copper is also used as a material for heat dissipation members and heat exchange members in places where high thermal conductivity is required.

[0005] Generally, metal materials have high thermal conductivity but low emissivity, and heat transfer from the surface by radiation is hardly expected. Therefore, in the past, a layer of oxide or the like with high emissivity was formed on the surface (surface layer) of a metal material to improve heat transfer by radiation. For example, in Patent Document 1, a surface treatment is performed on an aluminum substrate to form an aluminum hydroxide layer on the surface of the substrate, thereby improving the emissivity of the substrate. However, the invention in Patent Document 1 focuses solely on aluminum, and does not focus on copper at all. In addition, the immersion time described is very short, and surface treatment to the extent that a film can be formed on copper cannot be performed.

[0006] On the other hand, for copper surface treatment, an example has been reported in which an oxide film is formed by using an oxidizing agent such as sodium chlorite and sodium hydroxide (for example, Patent Document 2). However, the surface treatment in the invention of Patent Document 2 is targeted at copper circuits (circuit patterns) formed on printed circuit boards, and aims to "provide a copper surface treatment method that has excellent chemical resistance and adhesion between the copper circuit surface and insulating resin," and does not aim to improve radiation. In addition, in the invention of Patent Document 2, the surface treatment temperature is high at 50 to 95°C, and the treatment is performed for a short time (15 seconds or more), so that even if such a surface treatment is applied to a heat dissipation component made of a copper material, it is considered that it is very difficult to form a film that fully exhibits radiation.

[0007] As another surface treatment for copper, for example, in the invention of Patent Document 3, the surface area of ​​copper is increased to improve heat dissipation. In the invention of Patent Document 3, a method is adopted in which the workpiece is immersed in an NaOH aqueous solution or NaClO2 aqueous solution at 60 to 100°C for up to 10 minutes to form fine wires with a length of 0.1 to 100 μm and a width of 1 to 100 nm. In the invention of Patent Document 3, a method is adopted in which the workpiece is immersed in a copper electrolyte, current is passed through, and the copper generated on the heat sink is oxidized to form fine wires.

[0008] The invention of Patent Document 3 is not an invention in which a copper base material is directly treated, and does not mention improving the emissivity, but rather aims to improve heat dissipation characteristics only by increasing the surface area. In addition, in the invention of Patent Document 3, like the invention of Patent Document 2, the surface treatment temperature of copper is 50°C or higher, which is relatively high. As described above, the invention of Patent Document 3 does not disclose a method that can be performed at a low temperature below 50°C and that can sufficiently improve the emissivity. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] Patent No. 5083578 [Patent Document 2] Patent No. 4618466 [Patent Document 3] JP 2005-317962 A Summary of the Invention [Problem to be solved by the invention]

[0010] The object of the present invention is to provide a heat dissipation component made of a copper material that can be manufactured by surface treatment at a low temperature near room temperature and has an improved emissivity, and to provide a method for manufacturing the heat dissipation component. [Means for solving the problem]

[0011] As a result of intensive research into achieving the above-mentioned object, the inventors discovered that by oxidizing the surface of a copper material component with an alkaline aqueous solution and transforming the surface layer into a layer made of copper oxide, the treated surface and surface layer have a higher emissivity than the original surface and surface layer, thereby improving heat dissipation efficiency, and thus completed the present invention.

[0012] That is, the main configuration of the present invention is as follows. [1] A heat dissipation component made of a copper material, wherein a surface layer of a specified heat dissipation area of ​​the surface of the heat dissipation component used for heat dissipation is subjected to an oxidation treatment by contact with an alkaline aqueous solution to become a surface layer made of copper oxide material, thereby increasing the emissivity of the heat dissipation area. [2] The heat dissipation member according to [1] above, wherein the copper oxide is one or both of Cu2O and CuO. [3] The heat dissipation member according to [1] or [2] above, wherein the copper oxide has a porous structure. [4] A method for manufacturing a heat dissipation member made of a copper material, comprising the steps of: a step of subjecting a surface of a copper material for forming the heat dissipation member to an oxidation treatment by contacting the copper material with an alkaline aqueous solution in a predetermined heat dissipation region used for heat dissipation, thereby forming a surface layer of the heat dissipation region into a layer made of copper oxide material by the oxidation treatment; The manufacturing method. [5] The manufacturing method according to [4] above, wherein the treatment of contacting the heat dissipation area with an alkaline aqueous solution is a treatment of immersing the copper material in the alkaline aqueous solution. [6] The method according to [5] above, wherein air or oxygen is passed through the alkaline aqueous solution during the immersion to promote oxidation of the heat dissipation region. Effect of the Invention

[0013] The present invention provides the following effects. (i) By contacting the surface of a component made of a versatile copper material, which has an extremely high thermal conductivity (especially a specific heat dissipation area used for heat dissipation), with an alkaline aqueous solution and subjecting it to oxidation treatment, the emissivity from the surface is increased, making it possible to provide a heat dissipation component with a higher cooling effect (heat dissipation effect) than conventional products. (ii) In dissipating heat from electronic devices and the like, the cooling efficiency can be improved compared to the case where a heat dissipation member made of a simple copper material is used as is. (iii) The surface layer made of the copper oxide material formed in the present invention has a high emissivity, but is a thin film having a thickness of only a few μm. This reduces the risk of the surface layer falling off, and also reduces the increase in thermal resistance caused by the surface layer made of the copper oxide material. (iv) The desired surface layer made of copper oxide material can be formed by simply immersing the material in a general-purpose alkaline aqueous solution or by bubbling the material in the aqueous solution, so no special equipment is required. The oxidation treatment can be performed on any copper material having a complex shape or on a conventional heat dissipation component made of copper material (which has not been oxidized), and the heat dissipation component according to the present invention can be produced. [Brief description of the drawings]

[0014] [Figure 1] FIG. 1 is a cross-sectional view showing a schematic example of the structure of a heat dissipation member according to the present invention. [Diagram 2] FIG. 2 is a schematic diagram showing an example of a method for producing a heat dissipation member according to the present invention. [Diagram 3] Fig. 3 is a diagram showing the outline of the configuration of a heat dissipation characteristic evaluation device for measuring the temperature change of a heater, which was produced in the present invention. The figure is an end view of a stand 210 (thermometer 211), a stand 220 (insulating material 221, heater 222, sample S), and a stand 230 (sensor 231), which are arranged in a line at a predetermined interval, cut by a common plane passing through the center of each. Hatching and shading are appropriately applied for the purpose of distinguishing regions. [Figure 4] FIG. 4 is a diagram showing the structure of a stand in the heat radiation characteristic evaluation apparatus shown in FIG. 3, and is a diagram showing stand 210 shown in FIG. 3 as viewed from the right side of the figure. [Diagram 5] FIG. 5 is a graph showing the relationship between differences in oxidation treatment by immersion and spectral emissivity curves in the present invention. [Figure 6] FIG. 6 is a graph showing the relationship between the spectral emissivity curve and different concentrations of solutions for oxidation treatment in the present invention. [Figure 7]FIG. 7 is a graph showing the relationship between the temperature of the solution for the oxidation treatment and the spectral emissivity curve in the present invention. [Figure 8] FIG. 8 is a graph showing X-ray diffraction (XRD) patterns of a test piece made of a copper material that has been subjected to an oxidation treatment and a test piece made of a copper material that has not been subjected to an oxidation treatment. [Figure 9] FIG. 9 is a scanning electron microscope (SEM) photograph showing the surface state of a surface layer made of a copper oxide material obtained by oxidation treatment in an example of the present invention. [Figure 10] FIG. 10 is a graph showing a temperature rise curve in a heat dissipation test carried out in an example of the present invention. [Figure 11] FIG. 11 is a SEM photograph showing the surface state of a copper oxide surface layer obtained by subjecting a brass test piece to an oxidation treatment in an example of the present invention. [Figure 12] FIG. 12 is an SEM photograph showing the surface state of a surface layer made of a copper oxide material obtained by heat treating a copper plate sample in Comparative Example 1 of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] The heat dissipating member according to the present invention will be described in detail below together with the manufacturing method according to the present invention.

[0016] As shown in FIG. 1, the heat dissipation member 1 according to the present invention is made of a copper material, and the surface layer of a predetermined heat dissipation region 10e used for heat dissipation among the surfaces of the heat dissipation member 1 is oxidized by contact with an alkaline aqueous solution to become a surface layer 11 made of a copper oxide material. For example, if the surface layer of the heat dissipation region 10e is a layer made of high-purity metallic copper before the oxidation treatment, the surface layer of the heat dissipation region 10e becomes a layer made of copper oxide after the oxidation treatment. Since the surface layer 11 of the heat dissipation region 10e is made of a copper oxide material, the heat dissipation region 10e has a higher emissivity than before the oxidation treatment, and as a result, the heat dissipation member 1 has improved heat dissipation efficiency compared to the conventional one. Hereinafter, the surface layer made of a copper oxide material in the present invention is also called a "coating".

[0017] A manufacturing method according to the present invention is a method for manufacturing a heat dissipation member, which includes a step of bringing an alkaline aqueous solution into contact with a predetermined heat dissipation area used for heat dissipation on the surface of a copper blank 10 for forming the heat dissipation member, as an example of the manufacturing process being shown in FIG.

[0018] In the example of FIG. 2, as shown in FIG. 2(a), all surfaces (upper surface 10a and all side surfaces 10c in the figure) other than the lower surface 10b covered with the masking material 20 are the predetermined heat dissipation area. In the example of FIG. 2, as shown in FIG. 2(b), the oxidation treatment for the predetermined heat dissipation area (10a, 10c) of the copper material blank 10 is a treatment of contacting the heat dissipation area with an alkaline aqueous solution, and in a more specific example, the copper material blank 10 is immersed in an alkaline aqueous solution 110 contained in a container 100. By this oxidation treatment, the surface layer of the heat dissipation area (10a, 10c) becomes a layer 11 made of copper oxide. FIG. 2(c) shows an example of a heat dissipation member from which the masking material has been removed after the oxidation treatment, and the surface layer of the predetermined heat dissipation area of ​​the surface of the copper material blank 10 becomes a surface layer (i.e., a film) 11 made of copper oxide material. By this film, the heat dissipation area has a higher emissivity, making it a preferable heat dissipation member 1.

[0019] (Specifying the surface layer according to the manufacturing method) In the heat dissipation member according to the invention, the composition of the surface layer is defined by the manufacturing method, as stated in the provision that "the surface layer is formed by oxidation treatment through contact with an alkaline aqueous solution and is made of a copper oxide material." This provision is intended to indicate that the surface layer is not formed by adding a separately formed copper oxide member, nor is it formed by heat treatment at high temperature, but is a surface layer made of a copper oxide material obtained by contacting the original copper material of the surface layer with an alkaline aqueous solution. This provision is based on the fact that it is practically not possible to directly identify the state of the unique copper oxide material formed by contact with an alkaline aqueous solution from the structure or characteristics of the product, and is defined in the form of a manufacturing method.

[0020] The surface layer made of the copper oxide material obtained by contacting with an alkaline aqueous solution is homogeneous, as shown in the SEM image in Figure 9(a) (the diagonal parallel stripes on the surface are traces of machining), and as shown in the SEM images in Figures 9(b) and (c), it is a copper oxide layer with a unique porous structure that is formed only by contact with an alkaline aqueous solution.

[0021] (Emissivity) Emissivity (also called emissivity) is a value that indicates the characteristic of converting thermal energy into far infrared rays. Spectral emissivity can be calculated by measuring the radiation intensity (vs. wavelength) from a black body and a sample at the same temperature and calculating the ratio. The ratio of the values ​​obtained by integrating the spectral radiation intensity of the sample and the black body in a specific wavelength range is called integral emissivity. The integral emissivity (wavelength 3.33 to 20 μm) of a high-purity copper material (shiny surface) is about 6%, but when a copper oxide film is formed on the surface by oxidation treatment through contact with an alkaline aqueous solution, the integral emissivity of the surface can reach 50% or more, and in a more specific example, about 80 to 85% (described in the examples of the present invention).

[0022] (Copper heat dissipation material) The "copper material" in the "copper material heat dissipation member" of the present invention may be not only a high-purity copper material, but also a copper alloy material, a copper material containing impurities, etc. However, the copper alloy material and the copper material containing impurities are materials that contain a sufficiently large amount of copper so that the emissivity after the surface of the material is oxidized is higher than that before the oxidation treatment due to the high emissivity of the copper oxide formed by the oxidation treatment. The copper content (mass fraction) will be described later.

[0023] The heat dissipation component of the present invention contains a copper oxide material, which is formed by oxidizing and changing the original copper material, as a surface layer (coating) of the heat dissipation area, and the entire component including the original copper material and the changed copper oxide material is referred to as a "heat dissipation component made of copper material."

[0024] (copper material) Among copper materials, high purity copper materials are not particularly limited, but examples thereof include oxygen-free copper (C1020) and tough pitch copper (C1100) specified in JIS H3100, and oxygen-free copper for electronic devices (C1011) specified in JIS H 3510. Examples of general copper materials include various copper elongated products (rolled copper and copper alloy sheets and strips) specified in JIS H3100, copper and copper alloy castings specified in JIS H5120, and recycled copper elongated products.

[0025] (Copper alloy materials, other copper materials) As described above, in the present invention, if the emissivity after oxidation is higher than that before oxidation due to the high emissivity of copper oxide, the copper alloy material may be used. However, if the copper content (mass fraction, the same applies below) in the copper alloy material or the copper material containing impurities is excessively low, even if it is a copper alloy material, the effect of improving the emissivity due to copper oxide is not significantly obtained. Therefore, the copper content in the copper alloy material or the copper material containing impurities that can be used in the present invention is preferably 65% ​​or more, more preferably 80% or more, and particularly preferably 90% or more. As an example, the copper content of tough pitch copper (C1100), which is a preferred general copper material, is specified to be 99.90% or more. The upper limit of the copper content is not particularly limited, and may be any value up to the copper content in a high-purity copper material (ideally 100%). For example, as described in the Examples below, when a brass foil made of 65% copper and 35% zinc is immersed in a 0.5N-NaOH aqueous solution at room temperature while bubbling, the integral emissivity of the foil is improved from 5% before the immersion treatment to 30% after the immersion treatment. It was also found that the oxide film in this case is mainly composed of CuO.

[0026] Preferred copper alloy materials are not particularly limited, but examples thereof include red brass, brass, bronze, cupronickel, and nickel silver.

[0027] Comparing high purity copper material with copper alloy material, high purity copper material has a higher copper oxide content after oxidation treatment and therefore a higher emissivity, and is therefore preferable as a material for copper material.

[0028] The form of the copper material may be not only a refined copper material such as a copper roll product, but also a green compact obtained by compressing copper powder, a sintered body made of copper, a copper plating layer (electrolytic or electroless), a copper material film formed by various vapor deposition or deposition methods, etc. Even if a copper plating layer or a copper material film is in close contact with the surface of a base (the surface of an electronic component) and difficult to peel off, it is a heat dissipation member of the present invention if it is formed for the purpose of heat dissipation and a predetermined area of ​​its surface is oxidized.

[0029] The heat dissipation member may be not only a dedicated heat dissipation item intended solely for heat dissipation, but also a structure intended for other functions (e.g., a housing, a substrate, a protective wall, a conductive member, a tubular object (e.g., a pipe-shaped member used in the piping of a heat exchanger, etc.)).

[0030] (Shape of the heat dissipation member) The shape of the heat dissipation member is not particularly limited, and may be determined according to the object to be dissipated, and may be the same shape as a conventionally known heat dissipation member. For example, in the case of a simple plate-shaped heat dissipation member (with the outer shape of the main surface being rectangular or square) used for dissipating heat from electronic components, the length of one side is about 10 to 50 mm, and the thickness is about 5 to 30 mm. These shapes and dimensions are merely examples. For example, when dissipating heat from large equipment such as cooling components for automobiles or heat exchange components for the outdoor unit of an air conditioner, the shape may have an outer shape and thickness appropriate for the equipment.

[0031] (Copper material) In the manufacturing method of the present invention, a predetermined heat dissipation area of ​​a copper material for forming a heat dissipation member is oxidized. That is, the heat dissipation member of the present invention is a copper material having a predetermined heat dissipation area oxidized. The copper material may have the same shape as the finished product (heat dissipation member) except that it is not oxidized, or may be various blank materials that require shape processing such as punching, bending, and hole processing in addition to the oxidation treatment. The location of the predetermined heat dissipation area is predetermined by design. For example, when a heat dissipation member is formed from a copper hoop material by punching, secondary processing, etc., the oxidation treatment may be performed at the stage of the initial hoop material, the stage of the blank material that has been punched, or the stage of the material before the finished product that has been further processed such as deformed. The oxidation treatment may be performed at an appropriate stage in consideration of production efficiency, but a later stage is preferable in terms of not damaging the coating.

[0032] (heat radiation area) The predetermined heat dissipation area in the heat dissipation member may be an area of ​​any size at any position where heat dissipation is intended, depending on the object to which the heat dissipation member is applied. For example, the area may be the entire surface area of ​​the heat dissipation member, an area other than the surface that contacts the object to be dissipated (such as electronic components), or an area that can contribute to heat dissipation among the areas other than the surface that contacts the object. In the example of FIG. 1, the heat dissipation member 1 is a plate-like object, and the heat dissipation area 10e is located at the center of one surface (upper surface in the figure) 10a of the plate-like object, and the remaining area of ​​the surface 10a, the side surface 10c, and the other surface (lower surface in the figure) 10b remain the original copper material. In the example of FIG. 2, the heat dissipation member 1 is a plate-like object, and the heat dissipation area is all oxidized except for the lower surface 10b of the plate-like object as the heat dissipation area. Note that the outer periphery of the lower surface 10b of the plate-like object in the example of FIG. 2 is affected by the oxidation treatment on the side surface 10c, and becomes copper oxide only in a small amount.

[0033] Of the entire heat dissipation component of the present invention, it is preferable that the portion that comes into contact with the object to be cooled (e.g., an electronic component that serves as a heat source) remain in the original copper material without other components such as copper oxide, in order not to impede thermal conduction.

[0034] The thickness of the surface layer which is copper oxide in the heat dissipation region (for example, dimension t11 in the example of FIG. 1) is about 1 to 10 μm, preferably about 2 to 10 μm or about 1 to 5 μm, and more preferably about 2 to 5 μm. If the thickness of the surface layer is less than 1 μm, the emissivity drops drastically, and more effective radiative heat dissipation cannot be expected. On the other hand, if the thickness of the surface layer exceeds 10 μm, the possibility of the coating falling off increases, which is not preferable.

[0035] (Oxidation treatment) In the present invention, the copper material exposed in a predetermined heat dissipation area of ​​the surface of the copper material is brought into contact with an alkaline aqueous solution to convert the copper material into a copper oxide material. This type of oxidation treatment is preferable because it does not require high temperatures, can be performed at low temperatures around room temperature, and can be performed with simple equipment and easy handling.

[0036] The method for contacting the heat dissipation area with the alkaline aqueous solution is not particularly limited, and may be, for example, a method of pouring or spraying the alkaline aqueous solution onto the heat dissipation area. However, as shown in Figure 2(b), a method of immersing a copper material in an alkaline aqueous solution in a container requires a simple device and is easy to operate.

[0037] (Masking material when immersed) When the copper material is immersed in the alkaline aqueous solution, the copper material may be covered with a masking material other than the heat dissipation area. Any known masking material may be used.

[0038] (Alkaline aqueous solution) Examples of alkaline aqueous solutions capable of oxidizing the copper material in the heat dissipation region include NaOH aqueous solution, KOH aqueous solution, NH3 aqueous solution, etc. In particular, NaOH aqueous solution is preferable because it is inexpensive, has no odor, and is easy to handle.

[0039] (Concentration of alkaline aqueous solution) The concentration of the alkaline aqueous solution usable for the oxidation treatment is not particularly limited, but for example, in the case of an NaOH aqueous solution, it is preferably about 0.3 to 2.0 N, more preferably about 0.4 to 0.8 N. The concentrations of other alkaline aqueous solutions are generally similar to that of the NaOH aqueous solution, but the optimum concentration for each type of alkaline aqueous solution may be determined by experiment. If the concentration is below the lower limit, the formation of the film is deteriorated, and if the concentration is above the upper limit, the formation of the film is also deteriorated.

[0040] (Temperature of alkaline aqueous solution) The temperature of the alkaline aqueous solution during the oxidation treatment is not particularly limited, but for example, in the case of an NaOH aqueous solution, it is preferably about 5 to 40°C, more preferably about 10 to 30°C. The temperature of other alkaline aqueous solutions is generally similar to that of the NaOH aqueous solution, but the optimal temperature for each type of alkaline aqueous solution may be determined by experiment. If the temperature is below the lower limit, the reaction rate will be slow, and if the temperature is above the upper limit, the formation of the coating will be suppressed due to a decrease in dissolved oxygen.

[0041] (Oxidation treatment time) The time for the oxidation treatment is not particularly limited and varies depending on the temperature and concentration, but for example, in the case of immersion in a 0.5N NaOH aqueous solution at a temperature of 20° C., the time is preferably about 12 to 120 hours, and more preferably about 24 to 48 hours. The immersion time in other alkaline aqueous solutions is generally similar to the immersion time in the NaOH aqueous solution, but the optimal immersion time for each type of alkaline aqueous solution may be determined by experiment.

[0042] (Bubbling during immersion) When the copper material is immersed in an alkaline solution for contact with the alkaline solution, air and / or oxygen is pumped into the alkaline solution during the immersion so that the air and / or oxygen passes through the alkaline solution, accelerating the oxidation reaction of the surface layer of the heat dissipation area. This effect is achieved by actively dissolving oxygen in the NaOH solution to promote the oxidation reaction.

[0043] The size of the bubbles in the bubbling and the configuration of the bubbling device can be referred to in the publicly known art. The flow rate of the gas fed in the bubbling varies depending on the amount of the alkaline aqueous solution, but is preferably about 0.1 to 2 (L / min) for 1 liter of the alkaline aqueous solution (L stands for liters).

[0044] (Copper Oxide) The copper oxide formed by the oxidation treatment of the copper material in the heat dissipation region is one or both of Cu2O and CuO. In the embodiment of the present invention, it has been confirmed that Cu2O and CuO are mixed in the same film. For example, the generation ratio of CuO and Cu2O differs when the treatment temperature is different. That is, when the treatment temperature is low, the XRD peak of Cu2O is high, and when the treatment temperature is high, the XRD peak of CuO is high. Differences in the spectral emissivity curves are confirmed due to differences in the products (Figure 7). In other words, it has been confirmed that the emissivity tends to be low at about 13 μm or more in the treatment on the low temperature side where there is a lot of Cu2O, and the emissivity tends to be low at about 13 μm or less in the treatment on the high temperature side where there is a lot of CuO. In this way, the generation status of CuO and Cu2O affects the emissivity.

[0045] (Copper oxide structure) In the present invention, the structure of the copper oxide material formed by oxidizing the copper material in the heat dissipation region exhibits a specific porous shape when the copper material is brought into contact with an alkaline aqueous solution, as shown in the SEM photographs of Figures 9(b) and (c). It is generally known that optical properties such as radiation can be controlled and specific wavelengths can be amplified by controlling the periodic structure of the surface microstructure. On the other hand, in the present invention, a porous structure is formed on the surface of the copper, and it is presumed that the porous structure amplifies radiation as a pseudo-fine periodic structure. It is also considered that when the copper material is brought into contact with an alkaline aqueous solution, the copper is dissolved by the alkaline aqueous solution and reacts with dissolved oxygen to precipitate as an oxide. In particular, in the immersion method, it is considered that a precipitate is formed on the surface of the substrate made of the copper material, and the substrate becomes more porous. Therefore, it can be said that the porous structure shown in the SEM photographs of Figures 9(b) and (c) is a specific structure when the copper material is brought into contact with an alkaline aqueous solution (especially a structure that becomes more pronounced in immersion). EXAMPLES

[0046] Below are shown examples of the heat dissipating member of the present invention produced according to the production method of the present invention, comparative examples, an apparatus for evaluating the performance of the heat dissipating member, and the evaluation results.

[0047] (Oxidation treatment method) In this example, the oxidation treatment method involved immersing a copper material in an alkaline aqueous solution. The alkaline aqueous solution (hereinafter, treatment solution) was an NaOH aqueous solution, prepared by dissolving a reagent (NaOH) in distilled water. The treatment solution had various concentrations selected from a normality range of 0.1 to 2N, treatment times selected from a range of 0 to 165 hours, and treatment temperatures selected from a range of 5 to 60°C, and the heat dissipation members were manufactured by combining these conditions. A treatment time of "0" refers to an untreated comparative example. In the above normality, 1N is the concentration (1 normal) when 1 gram equivalent of solute (NaOH) is contained in 1 liter of NaOH aqueous solution.

[0048] (Copper material) A copper plate was used as the copper material. The copper plate was a plate material (length 50 mm, width 50 mm, thickness 2 mm) made of tough pitch copper (C1100), and the entire surface of the copper plate was subjected to an oxidation treatment.

[0049] (Other conditions) The above copper plate was immersed in 0.25 liters of the treatment solution and left as it was (static method), and the copper plate was immersed in 0.25 liters of the treatment solution while air was introduced into the treatment solution using an air pump (bubbling method). The bubbling flow rate was about 0.56 (L / min). After the specified immersion time, the sample was taken out, washed with water, washed with ethanol, and air-dried.

[0050] The samples were evaluated by spectral emissivity, film thickness, crystal phase, structure observation, and heat dissipation test. The spectral emissivity was measured with a far-infrared spectroemissometer (Thermo Fisher Scientific, FIR-1002) at a heater temperature of 100°C. The integral emissivity was calculated in the wavelength range of 3.33 to 20 μm. The thickness of the coating was measured at 10 points using an eddy current thickness gauge (SWT-9000, probe NFe3.0, manufactured by Sanko Electronics Laboratory) and the average value was calculated. The crystal phase was measured using an X-ray diffractometer (EMPYREAN, manufactured by PANalytical). The microstructure was observed using a scanning electron microscope (JEOL, JSM-7100F) at an accelerating voltage of 10 kV.

[0051] (Sample for heat dissipation test) The sample for the heat dissipation test was a plate material (length 50 mm, width 70 mm, thickness 1 mm) made of tough pitch copper (JIS C1100). The central region of one side of the copper plate, which was 50 mm long and 50 mm wide, was set as the heat dissipation region, and the region was subjected to oxidation treatment under the same conditions as above. In order to treat only the heat dissipation region, masking tape (adhesive tape with a PET base material) was attached tightly to the untreated surface. After the oxidation treatment, the sample was taken out, the masking tape was removed, and the sample was washed with water.

[0052] (Heat dissipation test equipment) The heat dissipation test was carried out using a heat dissipation test device shown in FIG. 3, the heat dissipation test device has a sealed acrylic box (housing) 200, and inside the box are arranged a thermometer (temperature sensor for measuring the ambient temperature Ta inside the box) 211 attached to a stand 210 with a bolt, a silicon rubber heater 222 for heating the sample and a sample S fixed to the heater via a fixing substrate 220e attached to the stand 220 with a bolt, and a radiation sensor (sensor for measuring the amount of radiation) 231 attached to a stand 230 with a bolt. A 70 mm thick heat insulating material 221 made of silicone sponge is fixed to the other surface of the silicon rubber heater 222, and most of the heat of the silicon rubber heater is conducted to the sample S through the fixing substrate 220e.

[0053] The stands 210, 220, and 230 all have the same structure, and as shown in the structure of the stand 210 representatively shown in Fig. 4, a rectangular pillar 210b is fixed to the upper surface of a base plate 210a having a rectangular outer periphery, a square frame 210c is fixed to the upper end of the pillar 210b, and a 1 mm thick aluminum fixing substrate 210e is suspended by four tension springs 210d in a square through hole surrounded by the frame 210c. The purpose of suspending the fixing substrate by tension springs is to minimize the thermal conduction between the fixing substrate and the frame, which allows the heat of the silicon rubber heater 222 to be conducted to the sample without loss, and also makes it possible to more accurately measure the temperature and radiant heat inside the box.

[0054] The heater 222 is a silicone rubber heater that is a flexible planar heating element, and is equipped with a temperature sensor (not shown), so that the temperature can be controlled by an external control device (not shown). The external control device is also configured to receive output values ​​from the thermometer and each sensor, and perform necessary calculation processing and control. In FIG. 3, the wiring connecting the thermometer and each sensor to the external control device is omitted.

[0055] A silicon rubber heater 222 is attached to one surface (the left surface in FIG. 3) of a fixing substrate 220e suspended from a central stand 220, and a sample S is fixed to the other surface of the fixing substrate 220e via a thermally conductive gel having a thickness of approximately 1 mm. The power input to the silicon rubber heater was 7.21 W (voltage 70 V, current 0.103 A), and the temperature rise of the heater was measured. The temperature rise is the difference between the heater temperature (Th) and the atmospheric temperature (Ta) in the acrylic box.

[0056] The acrylic box 200 is a rectangular parallelepiped formed by combining acrylic plates with a thickness of 25 mm, and the outer shape of the inner bottom surface is a rectangle of 340 mm x 240 mm, the length of the long side of which is the dimension L10 in FIG. 3. The inner height L20 is 375 mm. The stands 210, 220, and 230 are arranged in a row in the center of the inner bottom surface, and the fixing boards 210e, 220e, and 230e are arranged so that the board surfaces are parallel to each other. The distance L3 between the inner wall surface on the left side of FIG. 3 of the box 200 and the front surface of the support column of the stand 210 (the surface on the left side of the figure) is 50 mm, the interval L2 between the front surface of the support column of the stand 210 and the front surface of the support column of the stand 220 is 150 mm, the interval L1 between the surface of the heat dissipation area of ​​the sample and the surface of the radiation amount sensor 231 is 100 mm, and the height H1 of the centers of the thermometers, samples, and sensors is 155 mm.

[0057] Example 1 In this example, it was investigated how the coating formed differs depending on the immersion conditions of the sample (copper plate). The concentration of the treatment solution was 0.5N, the temperature of the treatment solution was 20°C, and the immersion time was 24 hours. The thickness and integrated emissivity of the film for a sample made by immersing the copper plate in the treatment solution and leaving it as is (static method) and a sample made by introducing air into the treatment solution with an air pump while the copper plate was immersed (bubbling method) are shown in Table 1 below, and the spectral emissivity curves are shown in the graph of Figure 5.

[0058] [Table 1]

[0059] As is clear from Table 1 and the graph in Figure 5, the integral emissivity of the sample that was not subjected to oxidation treatment was 5.9% (about 6%), whereas the integral emissivity of the samples with the coating formed by the static method and the bubbling method was 38.7% (about 40%) and 79.2% (about 80%), respectively, indicating that they were improved. In particular, it was confirmed that the effect of improving the emissivity was even greater with the bubbling method.

[0060] Example 2 In this example, it was investigated how the film formed differs depending on the concentration of the treatment liquid. The immersion method was the bubbling method, the temperature of the treatment solution was 20°C, and the immersion time was 24 hours. The film thickness and integral emissivity for each concentration are shown in Table 2 below, and the spectral emissivity curve is shown in the graph of Figure 6.

[0061] [Table 2]

[0062] As is clear from Table 2 and the graph in Figure 6, the thickness of the film increases as the concentration of the treatment liquid increases, but when the concentration becomes 1.0 N or more, the thickness starts to decrease, and it was found that the film is not formed favorably. Also, the integral emissivity changes according to the thickness of the film, and there is a tendency for the integral emissivity to be highest at a concentration of 0.5 N. It was also found that when the treatment liquid is highly concentrated (2.0 N), the emissivity at wavelengths of 10 μm or more is not high, so the integral emissivity does not improve.

[0063] Example 3 In this example, it was investigated how the coating formed differs depending on the immersion time. The immersion method was the bubbling method, the concentration of the treatment liquid was 0.5N, and the temperature of the treatment liquid was 20° C. The film thickness and integral emissivity for each immersion time are shown in Table 3 below.

[0064] [Table 3]

[0065] As is clear from Table 3, the thickness of the film increases with increasing immersion time, but the thickness is limited to about 4 to 5 μm, and it was found that the thickness does not increase even if the immersion time is increased beyond that. On the other hand, the integral emissivity is also limited to about 80 to 85%, and it was found that the integral emissivity does not improve even if the immersion time is increased beyond that. Therefore, in the case of immersion involving the bubbling method, it is judged that an immersion time of 24 hours is generally sufficient.

[0066] Example 4 In this example, it was investigated how the film formed differs depending on the temperature of the treatment liquid. The immersion method was the bubbling method, the concentration of the treatment liquid was 0.5 N, and the immersion time was 24 hours. The thickness and integral emissivity of the film at each treatment temperature are shown in Table 4 below, and the spectral emissivity curve is shown in the graph of Figure 7.

[0067] [Table 4]

[0068] As is clear from Table 4, even if the temperature of the treatment solution during immersion changes, the thickness of the film formed does not change significantly, being approximately 3 to 4 μm, but the integrated emissivity decreases when the temperature exceeds 30° C. Furthermore, as is clear from the graph in Fig. 7, it was found that when the temperature is low, such as 5° C., the emissivity at wavelengths longer than about 15 μm decreases, and when the temperature is high, such as 60° C., the emissivity at wavelengths shorter than about 15 μm decreases, showing a tendency to do so.

[0069] From the results of Examples 1 to 4 above, it was found that for the samples used, the optimum conditions for oxidation treatment were to blow air into a 0.5N NaOH aqueous solution while performing the oxidation treatment at a treatment temperature of 20°C for a dipping time of 24 hours, allowing a coating with a high emissivity to be formed. The XRD pattern of the coating produced under the above optimum conditions is shown in the graph of Figure 8. Two types of copper oxide (CuO and Cu2O) were confirmed in the coating.

[0070] FIG. 9 shows an SEM photograph of the surface of the coating of the sample obtained under the conditions in Example 1 (treatment solution concentration 0.5N, treatment solution temperature 20°C, immersion time 24 hours, with bubbling). As shown in the photograph in FIG. 9(a), the coating is formed uniformly over the entire plate surface. Also, as shown in the photographs in FIG. 9(b) and (c), the coating is composed of a collection of crystals with an outer diameter (Feret diameter) of several μm, and is porous with dispersed cavities with an opening diameter (Feret diameter) of about 2 μm or less. The Feret diameter (also called the unidirectional diameter) is the distance (distance) between two parallel lines in a fixed direction that sandwich the measurement target portion (the crystals or openings) in a surface image of the coating obtained by an electron microscope photograph such as an SEM photograph. In addition, by immersing the copper material to be oxidized in an alkaline aqueous solution, preferably by bubbling it, the alkaline aqueous solution can be brought into contact with the surface of the copper material under constantly uniform conditions (similarly changing concentration and temperature) over time, and a similar porous coating of copper oxide material can be obtained over the entire treatment surface.

[0071] A sample obtained under the conditions in Example 1 above (treatment solution concentration 0.5N, treatment solution temperature 20°C, immersion time 24 hours, bubbling performed) and a sample that was not surface-treated were each set in the heat dissipation test device of Figure 3 and used as a heat dissipation member, and the difference in heater temperature rise (i.e., the difference in cooling capacity of both samples as heat dissipation members) is shown in the graph of Figure 10. As is clear from the graph, there is no significant difference in temperature rise from the time power (7.21 W) is applied to the heater until about 10 minutes, but after 10 minutes, it was found that the surface-treated sample gradually suppressed the heater temperature rise by about 11°C.

[0072] Example 5 Brass foil (65% copper, 35% zinc) was immersed in a 0.5N NaOH aqueous solution at 20°C and bubbled for 24 hours to perform a surface treatment, after which the surface was observed under an SEM. The structure of the formed coating is shown in the SEM photograph in Figure 11. As can be seen from the structure shown in the SEM photograph, it was a homogeneous porous structure consisting of an aggregate of granular products with an average particle size (average Feret diameter) of about 0.5 μm.

[0073] From the elemental analysis by SEM-EDX, mainly copper and oxygen were detected, and zinc was very small. Also, from the result of XRD, the film contained CuO as the main phase, and a small amount of Cu2O. The integral emissivity was about 30%. The integral emissivity of untreated brass foil was about 6%. Although the surface treatment was performed under the same conditions as the optimal treatment conditions for pure copper, the integral emissivity was significantly lower than the surface treatment result for pure copper. It was presumed that one of the reasons for this was the significant change in the porous state due to the crystal form. From this, it is considered that although a film (copper oxide surface layer) is formed even in copper alloys, high purity copper is more desirable. Even if the copper content in the copper alloy is below 65%, the integral emissivity is improved by oxidation treatment by contact with an alkaline aqueous solution. However, in the present invention, from the above results, the preferable copper content in the copper alloy is set to 65% or more in order to improve the integral emissivity to a useful level.

[0074] Comparative Example 1 Heat treatment is a method for forming an oxide film on the surface of a copper plate. In this comparative example, a sample of the same copper plate as in the above example was heated in air at 500°C for 3 hours using an electric furnace to form an oxide film on the sample. The thickness of the oxide film was about 8 μm, and the integral emissivity was about 42%. From this result, it can be seen that the oxide film obtained by heat treatment is thicker than the film of the heat dissipation member of the present invention obtained in the above example, but the integral emissivity is very low at about 42%.

[0075] FIG. 12 is an SEM photograph showing the surface of the oxide film formed by the heat treatment. As shown in FIG. 12(a), the oxide film formed by the heat treatment is densely formed, unlike the film formed by contact with an alkaline aqueous solution in the present invention. In addition, the oxide film formed by the heat treatment is chipped as shown in FIG. 12(b) and turned over as shown in FIG. 12(c), and is clearly different from the film formed by contact with an alkaline aqueous solution. As shown in these FIGS. 12(a) to (c), the oxide film obtained by the heat treatment is visually seen to be mottled, and it is clear that it is not homogeneous. In addition, it was confirmed from the SEM photograph in FIG. 12 that the structure of the oxide film formed by heating is denser than the oxide film obtained by the present invention. From this, it was found that the oxidation treatment by contact with an alkaline aqueous solution is effective in improving the emissivity. [Industrial Applicability]

[0076] The present invention relates to a copper material heat dissipation member having an increased emissivity and improved heat dissipation effect, and can be used as a heat dissipation member (cooling member) for electronic devices, etc. The coating formed by the present invention is as thin as a few μm, so there is less concern that the coating will fall off, and since the coating is porous, it can reduce an increase in thermal resistance and can function more effectively as a heat dissipation member. In addition, since the coating can be formed simply by contacting the copper material with an alkaline aqueous solution, it is possible to easily perform oxidation treatment on copper material of any complex shape. [Explanation of symbols]

[0077] 1. Copper heat dissipation components 10 Copper material 10e heat dissipation area 11 Surface of heat dissipation area

Claims

1. A heat dissipation member made of a copper material, a surface layer of a predetermined heat dissipation region of the surface of the heat dissipation member used for heat dissipation is subjected to an oxidation treatment by contact with an alkaline aqueous solution to become a surface layer made of a copper oxide material, thereby increasing the emissivity of the heat dissipation region; The copper oxide is Cu 2 O and CuO, and The heat dissipation member, wherein the surface layer made of the copper oxide material has an integrated emissivity of 80 to 85%.

2. The heat dissipation member according to claim 1 , wherein the copper oxide has a porous structure.

3. A method for manufacturing a heat dissipation member made of a copper material, comprising the steps of: a step of subjecting a predetermined heat dissipation region used for heat dissipation among a surface of a copper material for forming the heat dissipation member to an oxidation treatment by contacting with an alkaline aqueous solution, thereby forming a surface layer of the heat dissipation region into a layer made of copper oxide material by the oxidation treatment; the treatment of bringing the heat dissipation region into contact with an alkaline aqueous solution is a treatment of immersing the copper material in an alkaline aqueous solution; During the immersion, air or oxygen is passed through the alkaline aqueous solution to promote oxidation of the heat dissipation region; the alkaline aqueous solution is an aqueous NaOH solution, The concentration of the NaOH aqueous solution is 0.4 to 0.8 N; and The temperature of the NaOH aqueous solution is 10 to 30° C. The manufacturing method.

Citation Information

Patent Citations

  • JP1975083578A

  • Process for treating selective absorption surface

    JP1977058025A

  • Method of manufacturing insulated electric wire

    JP1981069723A

  • Heat pipe and its manufacture

    JP1982204794A

  • Treating liquid for forming copper oxide coating on surface of copper

    JP1983055573A