Method for producing paint colorants

A method for producing paint coloring materials with core-shell structures using Fe and tannic acid mixing achieves durable and adjustable color development through pigment and structural colors, addressing the limitations of existing paints by enhancing stability and environmental friendliness.

JP7593589B2Active Publication Date: 2024-12-03JTEKT CORP +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2020178523
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-10-26
Publication Date
2024-12-03
Estimated Expiration
2040-10-26

AI Technical Summary

Technical Problem

Existing coloring materials for paints do not effectively utilize structural colors, which are less prone to fading and have a lower environmental impact, limiting the development of novel and durable color options.

Method used

A method involving the alternately mixing solutions containing Fe and tannic acid with core particles to form a core-shell structure, adjusting pH, and forming a dye layer around the core particles to achieve color development based on both pigment and structural colors, with specific molar ratios and pH adjustments to enhance dye layer formation and stability.

Benefits of technology

The resulting paint coloring material exhibits novel color development due to both pigment and structural colors, providing durability against sunlight fading and environmental impact, with adjustable color properties through liquid part properties and improved storage stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007593589000001
    Figure 0007593589000001
  • Figure 0007593589000002
    Figure 0007593589000002
  • Figure 0007593589000003
    Figure 0007593589000003
Patent Text Reader

Abstract

To provide a paint color material that exhibits novel coloration by means of a structural color and a pigment color.SOLUTION: A paint color material has a core part and a pigment layer including ferric tannate formed around the core part. The paint color material contains color material particles having a particle diameter corresponding to the wavelength of a structural color, and exhibits coloration by means of the pigment layer and the structural color.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a color material for paint and a method for producing a coating material. [Background technology]

[0002] Regarding paint colorants, colorants that exhibit structural colors, which are different from pigment colors due to light absorption, are known. Structural colors are generally colors that are produced by the interference and scattering of visible light caused by the structure of the colorant. Therefore, colorants that exhibit structural colors have the advantage that they are less susceptible to fading due to sunlight compared to general organic pigments and dyes, and are less likely to cause environmental load compared to general organic and inorganic pigments. For example, Patent Document 1 discloses a composition that contains particles with a core-shell structure and is capable of forming a film that exhibits structural colors. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2014-47231 A Summary of the Invention [Problem to be solved by the invention]

[0004] As described above, structural color has various advantages. Therefore, there has been a demand for technology that can obtain novel color development using structural color. [Means for solving the problem]

[0005] The present invention can be realized in the following forms. According to one embodiment of the present disclosure, a method for producing a paint coloring material that exhibits color development due to a pigment color and a structural color is provided. The method includes a first step of obtaining a mixed solution containing coloring material particles having a particle size corresponding to the wavelength of the structural color by alternately adding and mixing a solution containing Fe and a solution containing tannic acid, the mixed solution having a core part formed by the core particles and a pigment layer containing iron tannate formed around the core part, by which the mixed solution contains coloring material particles having a particle size corresponding to the wavelength of the structural color, a second step of washing the coloring material particles, and a step of adjusting the liquid property of the mixed solution obtained in the first step. In the step of adjusting the color development, when the color development is adjusted to be more blue, the liquid property is adjusted to be acidic, and when the color development is adjusted to be more red, the liquid property is adjusted to be neutral or basic. According to one embodiment of the present disclosure, there is provided a method for producing a paint color material that exhibits color development due to a pigment color and a structural color. This production method includes a first step of obtaining a mixed solution containing color material particles having a particle size corresponding to the wavelength of the structural color by alternately introducing a solution containing Fe and a solution containing tannic acid, and a core part formed by the core particles and a pigment layer containing iron tannate formed around the core part, by mixing the two solutions, a second step of washing the color material particles, and a step of adjusting the pH of the mixed solution obtained in the first step to 7.0 or more to adjust the color development. The step of adjusting the color development is carried out after the first step and before the second step.

[0006] (1) According to a first aspect of the present disclosure, there is provided a paint color material, which has a core and a pigment layer containing iron tannate formed around the core, contains colorant particles having a particle size according to the wavelength of a structural color, and exhibits color development due to the pigment layer and the structural color. According to such an embodiment, the paint color material exhibits a novel color development due to the pigment layer and the structural color. (2) The paint color material of the above embodiment may further contain a liquid part, and the color development may be adjustable by the liquid properties of the liquid part. According to such an embodiment, the paint color material exhibits a novel color development that can be adjusted by the liquid properties of the liquid part. (3) According to a second embodiment of the present disclosure, there is provided a method for producing a paint colorant that exhibits color development due to a pigment color and a structural color. This production method includes a first step of obtaining a mixed solution containing colorant particles having a particle diameter corresponding to the wavelength of the structural color, the mixed solution having a core part formed by the core particles and a pigment layer containing iron tannate formed around the core part by alternately adding and mixing a solution in which core particles having a uniform particle diameter are suspended in a solution containing Fe and a solution containing tannic acid into a solution mainly composed of water, and a second step of washing the colorant particles. According to this embodiment, a paint colorant that exhibits novel color development due to the pigment color of the pigment layer and the structural color can be produced. (4) In the manufacturing method of the above aspect, in the mixed solution, the ratio of the number of moles of the Fe to the number of moles of the core particles is 5.41×10 -4 or more, and the ratio of the number of moles of the tannic acid to the number of moles of the core particles is 3.61 × 10 -4 According to such an embodiment, a dye layer can be more effectively formed around the core particle. (5) In the manufacturing method of the above embodiment, the pH of the mixed liquid may be adjusted to 7.0 or more prior to the second step. According to such an embodiment, the color development by the pigment layer of the paint color material can be adjusted and the storage stability of the paint color material can be improved. (6) In the manufacturing method of the above embodiment, after the second step, a third step may be provided in which a liquid in which the colorant particles are suspended in a solution containing Fe and a liquid containing tannic acid are alternately poured into a liquid mainly composed of water and mixed to form an additional pigment layer around the colorant particles. According to this embodiment, the thickness of the pigment layer of the colorant particles can be increased. In addition, the thickness of the pigment layer of the colorant particles can be adjusted by adjusting the number of times the third step is performed. [Brief description of the drawings]

[0007] [Figure 1] 3A to 3C are diagrams showing an example of a method for producing a paint color material according to the present embodiment. [Diagram 2] FIG. 1 shows the sample prepared for the experiment. [Diagram 3] Second figure showing the sample prepared for the experiment. [Figure 4] FIG. 13 shows the reflectance spectra of Sample 1 and Sample 3 in a coated state. [Diagram 5] FIG. 13 shows the reflectance spectra of Sample 2 and Sample 4 in a coated state. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] A. Embodiment: The paint color material of the present disclosure has a core portion and a pigment layer containing iron tannate formed around the core portion, and contains color material particles having a particle size corresponding to the wavelength of the structural color. As a result, the paint color material exhibits color development due to the pigment layer and structural color. Note that structural color is a color that is produced by interference and scattering of visible light caused by the structure of the color material. Therefore, color materials that exhibit structural colors are less likely to fade due to sunlight compared to general organic pigments, dyes, etc.

[0009] The colorant particles contained in the paint colorant have a so-called core-shell shape, with the pigment layer as the shell. That is, the core and the pigment layer formed around the core are integrated to form the colorant particle. In this embodiment, spherical silica (SiO2) particles with uniform particle size are used as the core. It is preferable to use a transparent or translucent material with a low haze value as the core. The haze value is an index indicating the degree of cloudiness of a material and can be measured based on JIS K7136.

[0010] The pigment layer contains iron tannate and exhibits a pigment color due to iron tannate. A pigment color is a color that occurs when light in a certain wavelength range is absorbed in a certain substance and light in a wavelength range that is not absorbed is reflected. General organic or inorganic pigments and dyes exhibit this pigment color. It is known that iron tannate is produced by the reaction of iron salts such as iron chloride (III) with tannic acid. It is also known that iron tannate exhibits different colors depending on the liquid properties. Specifically, iron tannate dimerizes and exhibits a blue-purple color under conditions of pH 3.0 to 6.0, and trimers and exhibits a reddish brown color under conditions of pH 7.0 or higher. As a result, the pigment layer exhibits a strong bluish color under acidic conditions and a strong reddish color under neutral or basic conditions.

[0011] As described above, the colorant particles have a particle size corresponding to the wavelength of the structural color. For example, when a paint colorant is applied to a support, the colorant particles are arranged with periodicity on the support. Due to this arrangement of colorant particles, the paint colorant exhibits a structural color with a wavelength corresponding to the particle size of the colorant particles. For example, when a colloidal crystal of a face-centered cubic lattice is formed by the arrangement of colorant particles, the wavelength λ of the structural color and the average refractive index n of the colloidal crystal are a and the particle diameter D of the color material particles have the relationship expressed by the following formula (1). λ=1.633n a D … (1) Average refractive index n a is the refractive index n of the component i that composes the colloidal crystal. i and volume fraction Φi This is determined by the following equation (2). n a 2 =Σn i 2 Φ i … (2) In the following description, the state in which the paint color material is applied to the support is also referred to as the "applied state."

[0012] The particle size of the colorant particles is determined by the size of the core portion and the thickness of the dye layer. For example, in this embodiment, the particle size of the colorant particles is the sum of the particle size of the silica particles constituting the core portion and the thickness of the dye layer. Therefore, by adjusting the diameter of the core portion and the thickness of the dye layer, the particle size of the colorant particles can be adjusted, and a desired structural color can be expressed in the coated state.

[0013] In the case where the paint colorant expresses structural color by the arrangement of colorant particles as in the present embodiment, the period of the structure of the portion expressing the structural color becomes short, and the angle dependency of the colorant's coloring becomes low. In contrast, for example, when the colorant expresses structural color by a portion formed in a thin film or multilayer film having a uniform film, the period of the structure of the portion expressing the structural color becomes long. In this case, the structure of the portion expressing the structural color becomes close to the so-called thin film interference model or multilayer film interference model, so the angle dependency of the colorant becomes high. Note that when the angle dependency of the colorant is high, the color of the colorant is easily perceived differently depending on the angle at which the colorant is viewed or the direction of light irradiation on the colorant.

[0014] The paint colorant may further contain a liquid portion in addition to the above-mentioned colorant particles. The liquid portion may be any liquid such as water, but is preferably a liquid that does not cause the structural color of the paint colorant or the pigment color of the pigment layer to be lost due to, for example, a chemical reaction with the colorant particles or the pigment layer. When the paint colorant contains a liquid portion, the coloring of the iron tannate contained in the above-mentioned pigment layer can be changed by changing the liquid property of the liquid portion, thereby changing the coloring of the paint colorant. In addition, the paint colorant may contain, for example, an additive for improving the storage stability of the paint.

[0015] The paint colorant is applied to a support. For example, the paint colorant having a liquid portion is applied to a glass material as a support by spin coating, and then dried to obtain a coating in which the paint colorant is applied to the support. As the support, for example, in addition to glass materials, ceramic materials, metal materials, resin materials, paper, cloth, and other materials and shapes can be used. Furthermore, the coating of the paint colorant to the support may be performed by any method that allows the completed coating to exhibit a structural color, and may be performed by, for example, dropping or spraying the paint colorant onto the support, or by using a brush or paint brush, in addition to spin coating.

[0016] FIG. 1 is a diagram showing an example of a method for producing a paint color material according to the present embodiment. In this production method, first, in step S110, a first liquid and a second liquid are prepared. The first liquid is a suspension in which core particles such as silica forming a core part are suspended in a solution containing iron (Fe) as a solute. The second liquid is a solution containing tannic acid (TA). Next, in step S120, the first liquid and the second liquid are alternately poured into a third liquid mainly composed of water such as pure water and mixed. Note that the main component of a composition refers to a component that occupies 50% by mass or more of the composition. By executing step S120, a pigment layer is formed around the core particle to generate color material particles, and a mixed liquid containing the color material particles is obtained. Note that in this embodiment, the color material particles and the mixed liquid obtained in step S120 are also referred to as first color material particles and first mixed liquid, respectively. Thereafter, in step S130, the first color material particles obtained in step S120 are washed. In step S130, for example, the first color material particles are mixed with pure water, centrifuged, and the supernatant generated by the centrifugation is discarded. This operation is repeated to wash away impurities adhering to the first color material particles.

[0017] Further, in step S140, a fourth liquid and a fifth liquid are prepared. The fourth liquid is a suspension in which color material particles are suspended in a solution containing Fe as a solute. The fifth liquid is a solution containing tannic acid, similar to the second liquid. In step S140, specifically, a suspension in which the first color material particles washed in step S130 are suspended in a solution containing Fe is prepared as the fourth liquid. Then, in step S150, the fourth liquid and the fifth liquid are alternately poured into and mixed with a sixth liquid whose main component is water, similar to the third liquid. By executing step S150, a second mixed liquid containing second color material particles formed by adding a pigment layer around the first color material particles is obtained. Thereafter, in step S160, the second color material particles obtained in step S150 are washed in the same manner as the first color material particles are washed in step S130. Note that step S120 may be referred to as a first step, step S130 as a second step, step S150 as a third step, and step S160 as a fourth step.

[0018] For example, the production of the paint color material may be terminated when step S130 is completed without performing the steps from step S140 to step S160 shown in FIG. 1. In this case, the number of times the pigment layer of the color material particles contained in the paint color material is formed is one. In addition, after the completion of step S160, the same steps as steps S140 to S160 may be repeated again to form additional pigment layers around the color material particles two or more times. For example, if two additional pigment layers are formed around the color material particles, the number of times the pigment layer of the color material particles is formed is three times in total. In this case, a further pigment layer can be formed around the second color material particles by preparing, for example, a suspension in which the second color material particles are suspended in a solution containing Fe as the fourth liquid in the step similar to step S140 that is executed again.

[0019] In the first mixture obtained in step S120, the ratio of the number of moles of Fe to the number of moles of core particles is 5.41 × 10 -4 or more, and the ratio of the number of moles of tannic acid to the number of moles of core particles is 3.61 × 10 -4Therefore, in the present embodiment, in the first mixture liquid, the ratio of the number of moles of Fe to the number of moles of silica, Fe / SiO2, is preferably 5.41×10 -4 or more, and the ratio of the number of moles of tannic acid to the number of moles of silica, TA / SiO2, is 3.61 x 10 -4 It is preferable that the ratio is equal to or more than this. This allows the dye layer to be formed more effectively around the core particles. The Fe / SiO2 and TA / SiO2 ratios in the first mixed liquid can be adjusted, for example, by adjusting the number of moles of silica and Fe in the first liquid, the number of moles of tannic acid in the second liquid, and the mixing amount of the first liquid and the second liquid.

[0020] In the manufacturing method shown in FIG. 1, the pH of the first mixed liquid may be adjusted to 7.0 or more prior to the second step of step S130. In this case, for example, the pH of the first mixed liquid can be adjusted by adding a base such as sodium hydroxide or a phosphate-based pH 7.0 buffer solution to the mixed liquid after the completion of step S120. By adjusting the pH of the first mixed liquid prior to step S130, rather than after the second step of step S130, it is possible to change the color development by the pigment layer in the applied state and improve the preservation of the paint color material. Similarly, by adjusting the pH of the second mixed liquid prior to the fourth step of step S150, it is possible to change the color development by the pigment layer in the applied state and improve the preservation of the paint color material.

[0021] The paint color material of the present embodiment described above includes a core portion and a pigment layer made of iron tannate, and contains color material particles having a particle size according to the wavelength of the structural color. Therefore, the paint color material exhibits a novel color development due to the pigment layer and structural color. In addition, since the paint color material of the present embodiment exhibits color development due to the pigment layer and structural color, it is less likely to lose color due to sunlight, etc., compared to color materials that exhibit only pigment colors, such as general organic pigments and dyes. Furthermore, since the color development due to the pigment layer is more likely to fade due to sunlight, etc., compared to structural colors, for example, it is possible to enjoy the change in color development over time in the applied product, and the change in color development over time can be used as an indicator of aging. In addition, by using a material such as silica or glass mainly composed of silica as a material for forming the core portion, the environmental load caused by the color material can be reduced compared to general organic and inorganic pigments, and novel color development of the color material can be realized.

[0022] In the present embodiment, the paint color material contains a liquid portion, and the color development can be adjusted by the liquid properties of the liquid portion. Therefore, the paint color material exhibits a novel color development that can be adjusted by the liquid properties of the liquid portion.

[0023] The method for producing a paint color material of this embodiment includes a first step of obtaining a first mixed solution containing first color material particles by alternately adding and mixing a first liquid in which core particles forming a core part are suspended in a solution containing Fe and a second liquid containing tannic acid into a third liquid mainly composed of water, and a second step of washing the first color material particles. Therefore, a paint color material that exhibits novel color development due to a pigment layer and structural color can be produced.

[0024] In the method for producing a paint color material according to the present embodiment, the molar ratio of Fe to the core particles in the first mixture is 5.41×10 -4 or more, and the molar ratio of tannic acid to core particles is 3.61 × 10 -4 As a result, the dye layer can be more effectively formed around the core particle.

[0025] In the method for producing a paint color material of the present embodiment, the pH of the first mixed liquid is adjusted to 7.0 or more in the first step, so that the color development by the pigment layer of the paint color material can be adjusted and the storage stability of the paint color material can be improved.

[0026] The method for producing a paint colorant of this embodiment also includes a third step in which a fourth liquid in which colorant particles are suspended in a solution containing Fe and a fifth liquid containing tannic acid are alternately added to and mixed with a sixth liquid mainly composed of water to form an additional pigment layer around the colorant particles. This allows the thickness of the pigment layer of the colorant particles to be increased. The thickness of the pigment layer of the colorant particles can also be adjusted by adjusting the number of times the third step is performed.

[0027] B. Experimental results: FIG. 2 is a first diagram showing samples prepared for an experiment to verify the effect of the embodiment. FIG. 3 is a second diagram showing samples prepared for an experiment. As shown in FIG. 2 and FIG. 3, samples 1 to 24 were prepared as experimental samples. FIG. 2 shows the particle size of the core part, the number of times the dye layer was formed, the pH adjustment method, the molar concentration of silica, the molar concentration of Fe, the molar concentration of tannic acid, Fe / SiO2, and TA / SiO2 in the mixing process, the pH after washing, the color in the suspension state, and the color in the coating state for samples 16 to 24. FIG. 3 shows the particle size of the core part, the number of times the dye layer was formed, the pH adjustment method, the molar concentration of silica, the molar concentration of Fe, the molar concentration of tannic acid, Fe / SiO2, and TA / SiO2 in the mixing process, the pH after washing, and the color in the suspension state for samples 16 to 24.

[0028] Each sample was prepared by the following method. As the aqueous suspension of silica particles that is the raw material of the silica particles as the core particles, an aqueous suspension of silica particles manufactured by Fuji Chemical Co., Ltd. was used. Specifically, in preparing Sample 1 and Sample 2, an aqueous suspension of silica particles containing 26.3 mass% of silica particles having a particle diameter of 268.3 nm and a density of 1.168 g / cm3 was used. 3In the preparation of samples 16 and 17, the silica particle water suspension was prepared by adding 25.7 mass% of silica particles having a particle size of 268.3 nm and a density of 1.163 g / cm 3 In the preparation of Samples 5, 9, 10, 13, 14, and 24, the silica particle water suspension containing 20.5 mass% of silica particles having a particle size of 268.3n and a density of 1.125 g / cm 3 In the preparation of samples 6 to 8, 11, 12, 15, and 18 to 23, the silica particle water suspension contained 26.8 mass% of silica particles with a particle size of 322.4 nm and had a density of 1.171 g / cm 3 The silica particle aqueous suspensions of the above were used. The average particle size of these silica particles was calculated based on the results of particle size distribution measurement by dynamic light scattering. Specifically, the median diameter (D50) of the silica particles calculated from the results of measurement by dynamic light scattering was taken as the average particle size. The average particle size of the silica particles contained in the silica particle aqueous suspension used to prepare each color material was taken as the average particle size of the core part of each color material. As the second liquid, an aqueous tannic acid solution was used in which the concentration was adjusted by adding pure water to tannic acid (molecular weight 1701.19) manufactured by Kishida Chemical Co., Ltd., which is a raw material for tannic acid.

[0029] Sample 1, Sample 2, and Sample 7 to Sample 24 were prepared according to the manufacturing method of the paint color material shown in FIG. 1. First, 0.6 ml of the first liquid in step S110 was prepared by mixing an aqueous solution of iron (III) chloride hexahydrate (molecular weight 270.30) and an aqueous suspension of silica particles using a vortex. Prior to mixing the two, ultrasonic waves were irradiated to the aqueous suspension of silica particles for 90 minutes to improve the dispersibility of silica fine particles in the aqueous suspension of silica particles. In addition, 0.6 ml of the second liquid was prepared. Next, in step S120, a syringe was used to alternately add one drop (about 0.03 mL) of the first liquid and the second liquid, a total of 0.6 mL each, to pure water as the third liquid, and the mixture was mixed using a stirrer to obtain a first mixed liquid containing first color material particles. Thereafter, in step S130, the first mixed liquid was first centrifuged, and the supernatant generated by the centrifugation was discarded to obtain a residue containing first color material particles. Next, the residue was mixed with pure water by a vortex, the suspension obtained by mixing was further centrifuged, and the supernatant generated by centrifugation was discarded. This operation was repeated to wash the first colorant particles. In Sample 1, Sample 2, and Sample 7 to Sample 24, the molar concentration of silica, the molar concentration of Fe, the molar concentration of tannic acid, Fe / SiO2, and TA / SiO2 in the first mixed solution were set to the molar concentration of silica, the molar concentration of Fe, the molar concentration of tannic acid, Fe / SiO2, and TA / SiO2 shown in Figures 2 and 3, respectively. In Samples 8 to 24, in which the dye layer was formed once, the colorant particles obtained in step S130 were suspended in 5.0 ml of pure water, and the color of the colorant particles in this suspension was visually observed, and the observed color was set to the "color in suspension" shown in Figures 2 and 3. In addition, the pH of this suspension was measured, and the measured pH was set to the "pH after washing" shown in Figures 2 and 3.

[0030] In the preparation of Sample 2, Sample 14, and Sample 15, the pH of the first mixed solution was adjusted by adding 0.2 mL of 1 mol / L aqueous sodium hydroxide solution to the first mixed solution obtained in Step S120 prior to Step S130. The pH immediately after the addition of sodium hydroxide was 8.0 for Sample 2 and Sample 14, and 8.1 for Sample 15. In the preparation of Sample 13, the pH of the first mixed solution was adjusted by adding 0.5 mL of 0.1 mol / L phosphoric acid pH 7.0 buffer solution to the first mixed solution obtained in Step S120 prior to Step S130 and stirring. In Sample 13, the pH immediately after the addition of the buffer solution was 7.2. In the preparation of Sample 24, after Step S130, 0.5 mL of 0.1 mol / L phosphoric acid pH 7.0 buffer solution was added to the aqueous suspension of the colorant particles prior to measuring the above-mentioned "pH after washing". In Sample 24, the pH immediately after the addition of the buffer solution was 7.2. The pH 7.0 buffer solution was prepared by mixing 30.5 ml of 0.2 mol / L disodium hydrogen phosphate and 19.5 ml of 0.2 mol / L sodium dihydrogen phosphate, and then adding 50 ml of pure water.

[0031] In the preparation of Sample 1, Sample 2, and Sample 7, in which the dye layer was formed three times, the first colorant particles obtained in step S130 were further suspended in water to prepare a suspension, and the prepared suspension of colorant particles and the same iron (III) chloride hexahydrate solution as in step S110 were mixed using a vortex to prepare the fourth liquid in step S140. Thereafter, steps S150 and S160 were performed in the same manner as steps S120 and S130, and a dye layer was additionally formed around the first colorant particles. Note that the fifth liquid was a tannic acid aqueous solution similar to the second liquid, and the sixth liquid was pure water similar to the third liquid. In addition, after step S160, the same steps as steps S140 to S160 were performed again to form an additional dye layer, making the total number of dye layer formations three. In Sample 2, the pH of the mixture was adjusted to 8.0 in step S150 and in a process similar to step S150 executed again after step S160, as in the case of step S120. In Samples 1, 2, and 7, after the third dye layer formation was completed, the obtained colorant particles were suspended in 5.0 ml of water, and the color of the colorant particles in the suspension was observed visually, and the observed color was designated as the "color in suspension" shown in Figures 2 and 3. The pH of this suspension was also measured, and the measured pH was designated as the "pH after washing" shown in Figures 2 and 3.

[0032] Samples 3 and 4 were prepared by mixing an aqueous solution of iron (III) chloride hexahydrate with the second liquid. Specifically, 0.05 ml of an aqueous solution of iron (III) chloride hexahydrate with a concentration of 40 g / L and 0.6 ml of the second liquid with a concentration of tannic acid of 13 g / L were added to 25 ml of pure water and mixed by stirring using a stirrer to obtain an iron tannate liquid as a coloring material. Note that the Fe molar concentration and TA molar concentration of Samples 3 and 4 in FIG. 2 represent the molar concentration in this iron tannate liquid. In the preparation of Sample 4, after the preparation of the mixed liquid was completed, 0.2 ml of an aqueous solution of sodium hydroxide with a concentration of 1 mol / L was added to the mixed liquid to adjust the pH of the iron tannate liquid to 8.0. In Sample 3, the color of the iron tannate liquid was visually observed, and the observed color was designated as the "color in suspension" shown in FIG. 2. For Sample 4, the color of the iron tannate solution after pH adjustment was visually observed, and the observed color was recorded as the “color in suspension” shown in FIG.

[0033] Sample 5 contains 20.5 mass% silica particles with a particle size of 268.3 nm and has a density of 1.125 g / cm 3 As sample 6, a silica water suspension containing 26.8 mass% of silica particles with a particle size of 322.4 nm and a density of 1.171 g / cm3 was used. 3 In Sample 5 and Sample 6, the color of the silica particles in the silica water suspension was observed visually, and the observed color was recorded as the "color in suspension" shown in Figures 2 and 3.

[0034] The average particle size of the colorant particles contained in Samples 1, 7, and 8 was calculated in the same manner as for the average particle size of the core portion. The thickness of the dye layer formed around the core portion can be calculated by subtracting the particle size of the core portion from the average particle size of the measured colorant particles.

[0035] Samples 1 to 15 were suspended in pure water, and the suspension was applied to a support and dried to obtain coated products of Samples 1 to 15. In preparing the coated products, a plurality of coated products having different coating thicknesses were prepared by adjusting the amount of coloring material applied. In Samples 1 to 4, a white unglazed plate manufactured by Nikkato Corporation was used as the support. In Samples 5 to 15, a transparent glass slide manufactured by Matsunami Glass Industry Co., Ltd. was used as the support. The color of each sample in the coated state was visually observed.

[0036] The coating thickness of Sample 1 and Sample 2 was calculated using SEM (scanning electron microscope) images of the cross sections of the coatings. Specifically, four cross-sectional SEM images were observed for each coating, and the thickness of the part excluding the support was measured at two points for each SEM image, and the coating thickness of the coating was calculated by calculating the average thickness of the total eight measured points.

[0037] The reflection spectra of Samples 1 to 4 in the coated state were measured using a small fiber optic spectrometer, USB2000 Miniature Fiber Optic Spectrometer, manufactured by Ocean Optics. Specifically, white light was irradiated onto the sample at a perpendicular angle of incidence, and the relative reflection spectra were measured. A standard white plate made of PTFE was used as a reference sample in the measurement of the relative reflection spectra. A halogen lamp was used as the white light source.

[0038] The average particle size of the colorant particles in Sample 1 was 286.7 nm. The average particle size of the colorant particles in Sample 7 was 373.6 nm. The average particle size of the colorant particles in Sample 8 was 338.6 nm. In Samples 1, 7, and 8, it is believed that iron tannate was adsorbed around the silica particles, which are the core particles, to form a pigment layer containing iron tannate around the core, and colorant particles having an average particle size larger than that of the core were formed. In addition, the average particle size of the colorant particles in Samples 7 and 8 was larger than that of Sample 1. Since the average particle size of the core particles in Samples 7 and 8 is larger than that of Sample 1, it is believed that the average particle size of the colorant particles in Samples 7 and 8 was larger.

[0039] Furthermore, the average particle size of the colorant particles in Sample 7 was larger than that of Sample 8. Since the pigment layer of Sample 8 was formed once, while the pigment layer of Sample 7 was formed three times, it is considered that the pigment layer of Sample 7 was formed thicker than that of Sample 8. In this way, the thickness of the pigment layer of the paint colorant can be adjusted by adjusting the number of times the pigment layer was formed. Furthermore, the particle size of the colorant particles can be adjusted by adjusting the thickness of the pigment layer.

[0040] As shown in FIG. 2, in Sample 1 and Samples 7 to 12, in which the pH after washing was less than 7.0, i.e., the color of the colorant liquid part was acidic, the color in the suspension state was blue-purple. The color in the suspension state of Sample 3, in which the iron tannate liquid was acidic, was also blue-purple. On the other hand, in Sample 2 and Samples 13 to 15, in which the pH after washing was 7.0 or more, i.e., the color of the colorant liquid part was neutral or basic, the color due to the pigment layer was a reddish brown or reddish purple, which was a strong reddish color. The color in the suspension state of Sample 4, in which the iron tannate liquid was basic, was also a reddish brown with a strong reddish color. In Samples 5 and 6, the color in the suspension state was white. It is considered that in Samples 1, 2, and Samples 7 to 15, the color due to the iron tannate in the pigment layer according to the liquid property of the liquid part was observed in the suspension state. It is considered that Samples 5 and 6 did not show a color due to the pigment layer in the suspension state because they did not have a pigment layer.

[0041] In addition, in Sample 1, Sample 2, Sample 9, Sample 10, Sample 13, and Sample 14, in which the particle diameter of the core portion is 268.3 nm, the color in the applied state was greener than the color in the suspended state. In addition, in these samples, the greater the amount of coloring material applied, the greener the color in the applied state became. In contrast, in Sample 7, Sample 8, Sample 11, Sample 12, and Sample 15, in which the particle diameter of the core portion is 322.4 nm, the color in the applied state was redder than the color in the suspended state. In addition, in these samples, the greater the amount of coloring material applied, the redder the color in the applied state became. In Sample 5 and Sample 6, the color in the applied state was green and red, respectively. In Sample 3 and Sample 4, the color in the applied state was blue-purple and reddish brown, respectively, which were similar to the color in the suspended state.

[0042] In Samples 1, 2, and 7 to 15, the colorant particles are arranged periodically in the coated state, which is believed to have caused structural color in addition to the colorant color due to the dye layer. In addition, in these samples, the coating thickness increases as the amount of colorant applied increases, and the area in which the particles are arranged periodically increases in the thickness direction, which is believed to have caused the structural color to be relatively stronger than the dye color. Samples 5 and 6 do not have a dye layer, so they are believed to have only exhibited structural color. Samples 3 and 4 do not contain colorant particles, so they are believed to have not exhibited structural color in the coated state, but rather exhibited a color similar to that in the suspended state.

[0043] As described above, the particle size of the colorant particles contained in Sample 7 and Sample 8 is larger than that of the colorant particles contained in Sample 1. Furthermore, since the only difference between the preparation method of Sample 1 and the preparation method of Sample 2 is the presence or absence of pH adjustment, it is considered that the average particle size of the colorant particles in Sample 2 is approximately the same as that of the colorant particles in Sample 1. Therefore, it is considered that Sample 7 and Sample 8 exhibited a red structural color with a longer wavelength compared to the structural colors of Sample 1 and Sample 2, corresponding to the particle size of the colorant particles. Similarly, it is considered that the other samples with a core particle size of 322.4 nm also exhibited a red structural color because the particle size of the colorant particles was larger than that of the sample with a core particle size of 268.3 nm. Therefore, in the paint colorant, for example, the relationship between the wavelength of the structural color and the particle size of the colorant particles can be investigated in advance by experiment, and the particle size of the colorant particles can be adjusted so that the desired structural color is expressed, thereby expressing the desired structural color.

[0044] The color of Sample 5 and Sample 6 in the coated state was whiter than the color of Sample 1, Sample 2, and Sample 7 to Sample 15 in the coated state. Sample 5 and Sample 6 contain only silica particles without a dye layer, so it is believed that the reflected light of the structural color is multiple-scattered in the coated state of Sample 5 and Sample 6, and there is no coloring due to the dye layer, so the white color was observed. On the other hand, Sample 1, Sample 2, and Sample 7 to Sample 15 have a dye layer, so it is believed that the multiple scattering of the reflected light of the structural color is suppressed in the coated state of these samples, and coloring due to the reflected light of the dye color and the reflected light of the structural color that is stronger than that of Sample 5 and Sample 6 was observed.

[0045] FIG. 4 is a diagram showing the reflection spectra of Sample 1 and Sample 3 in their coated states. In Sample 1, green reflected light was observed at a wavelength of about 555 nm at each coating thickness. In Sample 1 and Sample 3, red to reddish brown pigment-colored reflected light was observed at wavelengths of 700 nm to 750 nm. Furthermore, in Sample 1, the intensity of red to reddish brown reflected light at wavelengths of about 700 to 750 nm was weaker than in Sample 3.

[0046] FIG. 5 is a diagram showing the reflection spectra of Sample 2 and Sample 4 in the coated state. In Sample 2, green reflected light was observed at a wavelength of about 555 nm at each coating thickness. In Sample 2 and Sample 4, blue pigment color reflected light was observed at a wavelength of about 480 nm, and red to reddish brown pigment color reflected light was observed at wavelengths of 700 nm to 750 nm. In Sample 2, the intensity of blue reflected light at a wavelength of about 480 nm and the intensity of red to reddish brown reflected light at wavelengths of about 700 nm to 750 nm were weaker than in Sample 4.

[0047] As shown in Figures 4 and 5, in Samples 1 and 2, the greater the coating thickness, the stronger the intensity of the reflected light of the structural color relative to the intensity of the reflected light of the pigment color. Also, in Samples 1 and 2, the greater the coating thickness, the stronger the greenish color of the coated state as confirmed by visual inspection. In Samples 1 and 2, the greater the coating thickness, the greater the area in which the particles are periodically arranged in the thickness direction, which is thought to have made the structural color appear stronger relative to the pigment color.

[0048] As shown in Fig. 3, the color of Samples 17 to 23 in the suspended state was bluish purple, and the color of Sample 24 in the suspended state was reddish purple. It is believed that these samples in the suspended state exhibited the dye color due to the dye layer formed around the core, similar to Samples 1, 2, and 7 to 15 shown in Fig. 2.

[0049] In Sample 16, the color of the suspension was white. In the preparation of Sample 16, the Fe / SiO2 and TA / SiO2 in the first mixed solution were smaller than those of the other samples, which is thought to have made it difficult for a dye layer to form around the silica particles that are the core particles. As shown in Figure 3, in order to effectively form a dye layer around the core particles, the Fe / SiO2 ratio needs to be 5.41×10 -4 or more, and TA / SiO2 is 3.61×10 -4 More preferably, it is equal to or greater than this.

[0050] As described above, the preparation method of Sample 13 and the preparation method of Sample 24 are similar in that the pH was adjusted by a buffer solution in both cases, but the timing of the pH adjustment is different. In Sample 24, the color in the suspended state after washing was reddish purple, but the pigment layer gradually peeled off from the core portion over time, and the color of the color material became white after 7 days. In Sample 13, the color in the suspended state after washing was reddish purple, similar to Sample 24, and the color of the color material remained reddish purple even after 7 days. Therefore, when adjusting the pH in the production of a paint color material, it is preferable to adjust the pH of the first mixed solution prior to the second step in order to improve the storage stability of the paint color material.

[0051] According to the experimental results described above, it has been confirmed that a paint color material containing particles having a core portion and a pigment layer containing iron tannate formed around the core portion exhibits novel color development due to the pigment layer and structural color.

[0052] The present disclosure is not limited to the above-mentioned embodiment, and can be realized in various configurations without departing from the spirit of the present disclosure. For example, the technical features of the embodiments corresponding to the technical features in each aspect described in the Summary of the Invention can be appropriately replaced or combined to solve some or all of the above-mentioned problems or to achieve some or all of the above-mentioned effects. Furthermore, if a technical feature is not described as essential in this specification, it can be appropriately deleted.

Claims

1. A method for producing a paint color material that exhibits color development due to a pigment color and a structural color, comprising the steps of: a first step of alternately introducing a liquid in which core particles having a uniform particle size are suspended in a solution containing Fe, and a liquid containing tannic acid into a liquid mainly composed of water, and mixing them to obtain a mixed liquid having core portions formed by the core particles and a pigment layer containing iron tannate formed around the core portions, the mixed liquid containing colorant particles having a particle size corresponding to the wavelength of the structural color; a second step of washing the colorant particles; and adjusting the color development by adjusting the liquid property of the mixed liquid, In the step of adjusting the color development, the liquid is adjusted to be acidic when the color development is adjusted to have a stronger blue tinge, and the liquid is adjusted to be neutral or basic when the color development is adjusted to have a stronger red tinge.

2. A method for producing a paint color material that exhibits color development due to a pigment color and a structural color, comprising the steps of: a first step of alternately introducing a liquid in which core particles having a uniform particle size are suspended in a solution containing Fe, and a liquid containing tannic acid into a liquid mainly composed of water, and mixing them to obtain a mixed liquid having core portions formed by the core particles and a pigment layer containing iron tannate formed around the core portions, the mixed liquid containing colorant particles having a particle size corresponding to the wavelength of the structural color; a second step of washing the colorant particles; and adjusting the color development by adjusting the pH of the mixture to 7.0 or more. A method for producing a paint color material, wherein the step of adjusting the color development is carried out after the first step and before the second step.

3. The method according to claim 1 or 2, In the mixture, the ratio of the number of moles of the Fe to the number of moles of the core particles is 5.41 × 10 -4 or more, and the ratio of the number of moles of the tannic acid to the number of moles of the core particles is 3.61 × 10 -4 The above is the method for producing a paint color material.

4. The method according to any one of claims 1 to 3, The method for producing a paint color material includes a third step of, after the second step, alternately adding and mixing a liquid in which the color material particles are suspended in a solution containing Fe and a liquid containing tannic acid into a liquid mainly composed of water, thereby forming an additional pigment layer around the color material particles.

Citation Information

Patent Citations

  • Temperature-controlled structural color dye, and preparation and application thereof

    CN110003882A

  • Method for preparing photonic crystal material through ordered self-assembly of emulsion

    CN111363189A

  • Structural color coating film-forming coating composition and method for forming multilayer coating film

    JP2009249527A

  • Coated film and resin composition

    JP2012214740A

  • Composition for structural color expression and structural color expression membrane

    JP2014047231A