Thermosetting binder composition and inorganic fiber product

The use of hydrogenated sugar and crosslinking agents in a thermosetting binder composition addresses the curability and strength issues of non-formaldehyde binders, ensuring rapid curing and enhanced mechanical strength in inorganic fiber products while minimizing formaldehyde release.

JP7593780B2Active Publication Date: 2024-12-03GUN EI CHEM IND
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2020181557
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-10-29
Publication Date
2024-12-03
Estimated Expiration
2040-10-29

AI Technical Summary

Technical Problem

Existing non-formaldehyde thermosetting binders for inorganic fiber products exhibit inferior curability and mechanical strength compared to phenolic resin binders, and emit less formaldehyde but at a slower curing rate.

Method used

A thermosetting binder composition comprising hydrogenated sugar, particularly maltotriitol, and a crosslinking agent, such as polycarboxylic acids, with optional catalysts, to enhance curability and mechanical strength without using formaldehyde-containing raw materials.

Benefits of technology

The binder composition achieves rapid curing and superior mechanical strength in inorganic fiber products, reducing formaldehyde emission and improving productivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007593780000009
    Figure 0007593780000009
  • Figure 0007593780000001
    Figure 0007593780000001
  • Figure 0007593780000002
    Figure 0007593780000002
Patent Text Reader

Abstract

To provide a thermosetting binder composition exhibiting good binder performance without using a raw material containing formaldehyde and excellent in curability.SOLUTION: A thermosetting binder composition contains a hydrogenated sugar and a crosslinking agent, the hydrogenated sugar contains maltotriitol, and the ratio of the maltotriitol to the total mass of the hydrogenated sugar is 20 mass% or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a thermosetting binder composition and an inorganic fiber product. [Background technology]

[0002] Conventionally, inorganic fiber products formed by binding inorganic fibers such as glass wool, rock wool, and ceramic fibers with a binder are used for heat insulation materials, sound absorbing materials, and various other molded products (such as automobile roofs and hood liners). Inorganic fiber products are generally manufactured by attaching a thermosetting binder to inorganic fibers, accumulating them to form an aggregate having the shape of the desired inorganic fiber product, and then heating the binder to harden the thermosetting binder. Thermosetting binders that are mainly composed of phenolic resin (hereinafter also referred to as "phenolic resin-based binders") are widely used because they are relatively inexpensive and can produce products with excellent performance such as mechanical strength.

[0003] However, phenolic resin binders have a problem in that they tend to emit formaldehyde during the manufacturing process of inorganic fiber products, etc. The causes of this include the fact that formaldehyde used as a raw material in the manufacture of phenolic resin remains unreacted, and that formaldehyde is generated during thermal curing of phenolic resin binders. Therefore, so-called non-formaldehyde type binders, which do not use raw materials containing formaldehyde, are being investigated.

[0004] Patent Document 1 proposes a mineral wool sizing agent composition that contains monosaccharides and / or polysaccharides and an organic polycarboxylic acid having a molecular weight of 1,000 or less. Patent Document 2 proposes a sizing agent composition for mineral wool that contains a specific hydrogenated sugar and a multifunctional crosslinking agent such as a non-polymer organic polycarboxylic acid. Patent Document 3 proposes a sizing agent composition for mineral wool, which contains a hydrogenated sugar mixture containing maltitol at a specific ratio and a polyfunctional crosslinking agent. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent No. 5575658 [Patent Document 2] Patent No. 5694166 [Patent Document 3] Patent No. 6141840 Summary of the Invention [Problem to be solved by the invention]

[0006] However, the compositions of Patent Documents 1 to 3 have lower formaldehyde emissions than phenolic resin binders, but are inferior in curability. For example, when the curing temperature is the same, the curing time of the compositions described in Patent Documents 1 to 3 is about 1.5 times that of the phenolic resin binder. In addition, inorganic fiber products using the compositions described in Patent Documents 1 to 3 may have inferior mechanical strength compared to inorganic fiber products using phenolic resin binders.

[0007] An object of the present invention is to provide a thermosetting binder composition that exhibits good binder performance without using raw materials containing formaldehyde and has excellent curing properties, and an inorganic fiber product using the same. [Means for solving the problem]

[0008] The present invention has the following aspects. [1] A method for producing a composition comprising: A thermosetting binder composition, wherein the hydrogenated sugar contains maltotriitol, and the ratio of the maltotriitol to the total mass of the hydrogenated sugar is 20 mass% or more. [2] The thermosetting binder composition according to [1] above, wherein the crosslinking agent is at least one selected from the group consisting of polycarboxylic acids, their salts, and acid anhydrides. [3] The thermosetting binder composition according to [1] or [2] above, further comprising a catalyst. [4] An inorganic fiber product having a molded body in which inorganic fibers are bound with a binder, The binder is a cured product of the thermosetting binder composition according to any one of [1] to [3] above. [5] The inorganic fiber product according to [4], wherein the inorganic fiber is glass wool or rock wool. Effect of the Invention

[0009] According to the present invention, it is possible to provide a thermosetting binder composition that exhibits good binder performance without using raw materials containing formaldehyde and has excellent curing properties, and an inorganic fiber product using the same. [Brief description of the drawings]

[0010] [Figure 1] DMA charts for Examples 6 to 9 and Comparative Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] [Thermosetting binder composition] A thermosetting binder composition according to one embodiment of the present invention (hereinafter, also simply referred to as a "binder composition") contains a hydrogenated sugar and a crosslinking agent. The binder composition may further comprise a catalyst. The binder composition may further comprise other ingredients in addition to the hydrogenated sugar, the crosslinking agent and the catalyst.

[0012] <Hydrogenated sugar> The term "hydrogenated sugar" refers to a product produced by reduction of at least one type of sugar selected from the group consisting of monosaccharides, oligosaccharides (disaccharides to decasaccharides), and polysaccharides, and a mixture of these products. In this embodiment, the hydrogenated sugar comprises maltotriitol. Maltotriitol is a reduced form of maltotriose and is also known as 4-O-(4-O-α-D-glucopyranosyl-α-D-glucopyranosyl)-D-glucitol.

[0013] The hydrogenated sugar may consist of only maltotriitol, or may be a mixture of maltotriitol and other hydrogenated sugars. Other hydrogenated sugars include, for example, erythritol, arabitol, xylitol, sorbitol, mannitol, iditol, maltitol, isomaltitol, lactitol, cellobitol, palatinitol, and hydrogenated products of starch hydrolysates. These other hydrogenated sugars may be used alone or in combination of two or more.

[0014] The ratio of maltotriitol to the total mass of hydrogenated sugar is 20% by mass or more, preferably 35% by mass or more, and more preferably 50% by mass or more. When the ratio of maltotriitol is 20% by mass or more, the binder composition has excellent curability and the inorganic fiber product using the binder composition has excellent mechanical strength. There is no particular upper limit on the proportion of maltotriitol, but when the hydrogenated sugar is a mixture of maltotriitol and other hydrogenated sugars, from the standpoint of ease of availability, the proportion of maltotriitol to the total mass of the hydrogenated sugar is preferably 75% by mass or less, and more preferably 60% by mass or less.

[0015] In terms of viscosity, it is preferable that the mixture of maltotriitol and other hydrogenated sugars contains at least maltitol as the other hydrogenated sugar. The proportion of maltitol in the total mass of the mixture of maltotriitol and other hydrogenated sugars is preferably from 1 to 80% by mass, more preferably from 20 to 50% by mass.

[0016] <Crosslinking agent> The cross-linking agent cross-links the hydrogenated sugars. The crosslinking agent is typically a polyfunctional compound having two or more functional groups capable of reacting with a hydroxyl group under the action of heat, such as a carboxyl group, an acid anhydride group, or a formyl group. Examples of the crosslinking agent include polycarboxylic acids, their salts and acid anhydrides, and polyaldehydes.

[0017] The polycarboxylic acid has two or more carboxy groups. The polycarboxylic acid can be a polycarboxylic acid polymer or a polycarboxylic acid monomer. In order to reduce the viscosity of the binder composition, the number average molar mass of the polycarboxylic acid is preferably 50,000 or less, more preferably 10,000 or less, and even more preferably 5,000 or less.

[0018] Examples of polycarboxylic acid polymers include homopolymers and copolymers of monomers having at least one carboxy group, such as (meth)acrylic acid, crotonic acid, isocrotonic acid, maleic acid, cinnamic acid, 2-methylmaleic acid, fumaric acid, itaconic acid, 2-methyltaconic acid, α,β-methylene glutaric acid, and unsaturated dicarboxylic acid monoesters. Examples of comonomers in copolymers include vinyl monomers such as vinyl acetate, styrene, and styrene substituted with an alkyl group, a hydroxyl group, a sulfonyl group, or a halogen atom; C1-C 10 Examples of (meth)acrylic monomers include alkyl (meth)acrylates (for example, methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, and isobutyl (meth)acrylate), (meth)acrylonitrile, and (meth)acrylamide. Here, (meth)acrylic acid refers to acrylic acid or methacrylic acid, and (meth)acrylate refers to acrylate or methacrylate. The same applies to (meth)acrylonitrile and (meth)acrylamide.

[0019] Examples of polycarboxylic acid monomers include dicarboxylic acids, tricarboxylic acids, and tetracarboxylic acids. Dicarboxylic acids include, for example, oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, malic acid, tartaric acid, tartronic acid, aspartic acid, glutamic acid, fumaric acid, itaconic acid, maleic acid, traumatic acid, camphoric acid, phthalic acid and derivatives thereof (e.g., those containing at least one boron or chlorine atom), tetrahydrophthalic acid and derivatives thereof (e.g., those containing at least one chlorine atom, such as chlorendic acid), isophthalic acid, terephthalic acid, mesaconic acid, and citraconic acid. Tricarboxylic acids include, for example, citric acid, tricarballylic acid, 1,2,4-butanetricarboxylic acid, aconitic acid, hemimellitic acid, trimellitic acid, and trimesic acid. Tetracarboxylic acids include, for example, 1,2,3,4-butanetetracarboxylic acid and pyromellitic acid. The number average molar mass of the polycarboxylic acid monomer is preferably 1,000 or less, more preferably 750 or less, and even more preferably 500 or less.

[0020] Examples of the salt of polycarboxylic acid include alkali metal salts such as sodium salts and potassium salts. Examples of the acid anhydrides of polycarboxylic acids include the anhydrides of the above dicarboxylic acids.

[0021] The polyaldehyde has two or more formyl groups. Examples of the polyaldehyde include dialdehydes such as glyoxal, glutaraldehyde, 1,6-hexanedial, and 1,4-terephthalaldehyde.

[0022] As the crosslinking agent, in terms of curing speed, at least one selected from the group consisting of polycarboxylic acid polymers, salts thereof, and acid anhydrides is preferred, and in terms of low viscosity, at least one selected from the group consisting of polycarboxylic acid monomers, salts thereof, and acid anhydrides is preferred.

[0023] <Catalyst> Examples of the catalyst include Lewis bases, Lewis acids, phosphorus-containing compounds, fluorine- and boron-containing compounds. Lewis bases or acids include, for example, clays, colloidal or non-colloidal silica, organic amines, quaternary ammonium, metal oxides, metal sulfates, metal chlorides, urea sulfates, urea chlorides, and silicate-based catalysts. Examples of the phosphorus-containing compound include alkali metal hypophosphites, alkali metal phosphates, alkali metal polyphosphates, alkali metal hydrogen phosphates, phosphoric acid, and alkylphosphonic acids. The alkali metal is preferably sodium or potassium. Examples of compounds containing fluorine and boron include tetrafluoroboric acid or a salt thereof (e.g., a tetrafluoroborate of an alkali metal such as sodium or potassium, a tetrafluoroborate of an alkaline earth metal such as calcium or magnesium, zinc tetrafluoroborate, and ammonium tetrafluoroborate). Among these, sodium hypophosphite and potassium hypophosphite are preferred, particularly when it is desired to improve the hue of inorganic fiber products, because they have the effect of making the hue of the cured product lighter through their reducing action.

[0024] <Other ingredients> The other components can be appropriately selected from those known to be blended in a thermosetting binder composition, and examples thereof include water, sugars other than hydrogenated sugars, surfactants, silane coupling agents, water repellents, dust-preventing oils, hardening regulators, hardening accelerators, urea, melamine, etc. These may be used alone or in combination of two or more.

[0025] Examples of the surfactant include cationic surfactants, amphoteric surfactants, and nonionic surfactants. Examples of the cationic surfactant include alkyl trimethyl ammonium salts and dialkyl dimethyl ammonium salts. Examples of the amphoteric surfactant include alkylamino fatty acid sodium salts, alkyl betaines, and alkyl amine oxides. Examples of the nonionic surfactant include sucrose fatty acid esters, sorbitan fatty acid esters, polyoxyethylene sorbitan fatty acid esters, fatty acid alkanolamides, polyoxyethylene alkyl ethers, polyoxyethylene alkyl phenyl ethers, and alkyl polyglucosides. Any one of these surfactants may be used alone, or two or more may be used in combination.

[0026] Examples of the silane coupling agent include an amino group-containing silane coupling agent, an epoxy group-containing silane coupling agent, a vinyl group-containing silane coupling agent, a methacryloyl group-containing silane coupling agent, an acryloyl group-containing silane coupling agent, a ureido group-containing silane coupling agent, an isocyanate group-containing silane coupling agent, etc. Examples of the amino group-containing silane coupling agent include N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-triethoxysilyl-N-(1,3-dimethyl-butylidene)propylamine, N-phenyl-3-aminopropyltrimethoxysilane, and hydrochloride salt of N-(vinylbenzyl)-2-aminoethyl-3-aminopropyltrimethoxysilane. Examples of epoxy group-containing silane coupling agents include 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, and 3-glycidoxypropyltriethoxysilane. Examples of vinyl group-containing silane coupling agents include vinyltriethoxysilane. Examples of methacryloyl group-containing silane coupling agents include 3-methacryloxypropyltrimethoxysilane. Examples of acryloyl group-containing silane coupling agents include 3-acryloxypropyltrimethoxysilane. Examples of ureido group-containing silane coupling agents include 3-ureidopropyltriethoxysilane. Examples of isocyanate group-containing silane coupling agents include 3-isocyanatepropyltriethoxysilane. These silane coupling agents may be used alone or in combination of two or more.

[0027] Examples of the water repellent include silicone-based water repellents, fluorine-based water repellents, hydrocarbon-based water repellents, etc. These water repellents may be used alone or in combination of two or more. The dust-preventing oil may be a mineral oil-based oil emulsion. The hardening regulator is preferably a water-soluble high boiling point solvent, and examples of such hardening regulators include ethylene glycol, diethylene glycol, triethylene glycol, polyethylene glycol, propylene glycol, 1,4-butylene glycol, glycerin, diglycerin (also called diglycerol), polyglycerin, etc. Any one of these hardening regulators may be used alone, or two or more of them may be used in combination. As the hardening accelerator, a phosphoric acid compound is preferable. Examples of the phosphoric acid compound include alkali metal hypophosphites, alkali metal phosphites, alkali metal polyphosphates, alkali metal hydrogen phosphates, and alkyl phosphates. Examples of the alkali metal salts include sodium salts and potassium salts, and examples of the alkali metal salts include sodium hypophosphite, sodium phosphite, potassium hypophosphite, and potassium phosphite.

[0028] The binder composition of this embodiment can exhibit good binder performance without using a raw material containing formaldehyde. Therefore, it is preferable that the binder composition of this embodiment does not contain a raw material containing formaldehyde (for example, formaldehyde, phenolic resin obtained by reacting phenols with formaldehyde). If the binder composition does not contain a raw material containing formaldehyde, the amount of formaldehyde emitted during the production of inorganic fiber products or from inorganic fiber products can be reduced.

[0029] <Composition> In the binder composition of this embodiment, the ratio of the hydrogenated sugar to the total of the hydrogenated sugar and the crosslinking agent (100% by mass) is preferably 10 to 90% by mass, more preferably 20 to 80% by mass, and even more preferably 30 to 70% by mass. If the ratio of the hydrogenated sugar is equal to or higher than the lower limit, the moisture resistance is superior, and if it is equal to or lower than the upper limit, the curability is superior.

[0030] The catalyst content is preferably 1 to 10 mass% relative to the total of the hydrogenated sugar and the crosslinking agent (100 mass%), more preferably 2 to 8 mass%, and even more preferably 3 to 7 mass%. When the catalyst content is equal to or more than the lower limit, the binder composition has better curability, and when it is equal to or less than the upper limit, the binder composition has better moisture resistance.

[0031] The total proportion of the hydrogenated sugar, crosslinking agent, and catalyst relative to the total solid content (100% by mass) of the binder composition is preferably 5% by mass or more, more preferably 10% by mass or more, and may be 100% by mass.

[0032] When the binder composition contains water, the content of water is set according to the solids concentration of the binder composition. The solids concentration of the binder composition can be appropriately set taking into consideration the solubility of the hydrogenated sugar and the crosslinking agent, the form in which the binder composition is used, and the like, and may be, for example, 5 to 95% by mass relative to the total mass of the binder composition.

[0033] The solid content of the binder composition refers to the non-volatile content. The non-volatile content is the residue remaining after drying at 135°C for 60 minutes. The solid content concentration (mass %) of the binder composition is calculated as the ratio of the mass of the non-volatile content to the total mass of the binder composition, as described in detail in the Examples below. The moisture content (mass %) of the binder composition is calculated by subtracting the solid content concentration (mass %) from 100.

[0034] The binder composition of this embodiment can be prepared by mixing the hydrogenated sugar, the crosslinking agent, optionally a catalyst, and optionally other components. The components may be mixed together at once or sequentially.

[0035] The binder composition of this embodiment has thermosetting properties, that is, it is cured by heating. The thermosetting mechanism of the binder composition of this embodiment is thought to be a mechanism in which the hydrogenated sugar is polymerized by a reaction (esterification, etc.) between the hydrogenated sugar and the crosslinking agent.

[0036] [Inorganic fiber products] An inorganic fiber product according to one aspect of the present invention includes a molded body in which inorganic fibers are bound with a binder. This binder is a cured product of the binder composition described above. The inorganic fiber is not particularly limited, and examples thereof include glass wool, rock wool, ceramic fiber, etc. These may be used alone or in combination of two or more. As the inorganic fiber, glass wool or rock wool is preferred in terms of versatility and heat insulating performance. The inorganic fiber product may be made of the molded body, or may further include other members other than the molded body, such as a skin material for packaging. Inorganic fiber products can be used, for example, as heat insulating materials, sound absorbing materials, and various other molded products (such as automobile roofs and bonnet liners).

[0037] <Manufacturing method of inorganic fiber products> The inorganic fiber product can be produced by a production method including a step of forming inorganic fibers using the binder composition to obtain a formed product. For the production of inorganic fiber products, a known method conventionally used for the production of inorganic fiber products can be used, except that the above-mentioned binder composition is used as a binder. An example of a method for producing an inorganic fiber product is a method that sequentially performs a step of adhering a binder composition to inorganic fibers (hereinafter, the adhering step), a step of accumulating the inorganic fibers to which the binder composition is adhered to form an aggregate having a shape corresponding to the inorganic fiber product to be produced, and a step of heating the aggregate to harden the binder composition and obtain a molded product (hereinafter, the molding step). Each step will be described in more detail below.

[0038] (Attachment process) The inorganic fibers used in the adhesion step include the same ones as those mentioned above. The fiber length and fiber diameter of the inorganic fibers are not particularly limited and may be appropriately set depending on the inorganic fiber product to be manufactured. Usually, fibers having a fiber diameter within the range of 3 to 10 μm are used. The inorganic fibers may be commercially available or may be produced by a known method. Inorganic fibers are generally produced by fiberizing raw materials (waste glass, basalt, iron furnace slag, etc.). Examples of fiberization methods include the flame method and the centrifugal method. Fiberization by these various methods can be carried out using a corresponding fiberization device.

[0039] Examples of methods for attaching the binder composition to the inorganic fibers include a method of spraying the binder composition onto the inorganic fibers using a spray device or the like, and a method of impregnating the inorganic fibers with the binder composition. Any method may be used. The amount of the binder composition to be applied to the inorganic fibers is not particularly limited, but is usually within the range of 0.5 to 20 mass% as the solid content of the binder composition relative to the inorganic fibers (100 mass%). This amount affects the physical properties (mechanical strength, etc.) of the resulting molded product. For example, the more the amount of the binder composition to be applied to the inorganic fibers, the higher the mechanical strength of the resulting molded product tends to be.

[0040] (molding process) Next, the inorganic fibers to which the binder composition is attached are accumulated to form an aggregate having a shape corresponding to the inorganic fiber product to be manufactured, and the aggregate is then heated to harden the binder composition. The molding step can be carried out by a known method. For example, in the case of producing a plate-shaped inorganic fiber product, inorganic fibers are piled up on a conveyor, and the pile is compressed by pressing from above and below the conveyor to form an aggregate, and the aggregate is sent to a heating furnace (curing furnace) and heated to cure the binder composition, thereby obtaining a plate-shaped molded product.

[0041] The amount of inorganic fibers used (the amount of inorganic fibers deposited on the conveyor) and the compression conditions are set according to the thickness, bulk density, etc. of the inorganic fiber product to be manufactured. The heating conditions (heating temperature, heating time) of the aggregate are not particularly limited as long as they are within a range in which the binder composition in the aggregate is cured, but the heating temperature is preferably 200 to 300°C, and more preferably 240 to 280°C. When the heating temperature is equal to or higher than the lower limit, the time required for curing can be shortened, and the productivity of inorganic fiber products is excellent. When the heating temperature is equal to or lower than the upper limit, decomposition of the binder composition and the associated decrease in yield and decrease in mechanical strength can be suppressed. The heating time varies depending on the size of the aggregate, the heating temperature, etc., and is not particularly limited.

[0042] The obtained molded product may be used as an inorganic fiber product as it is, or may be further subjected to processing such as cutting and packaging with a skin material, if necessary. EXAMPLES

[0043] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. "Parts" and "%" refer to "parts by mass" and "% by mass" respectively unless otherwise specified. The materials used in each example are shown below.

[0044] <Materials used> Citric acid: white powder, manufactured by Iwata Chemical Co., Ltd. Sodium hypophosphite: Sodium hypophosphite, white powder, manufactured by Nippon Chemical Industry Co., Ltd. Hydrogenated sugar A: "Sweet G3" manufactured by Bussan Food Science Co., Ltd. Hydrogenated sugar B: Maltitol (powder), manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. Hydrogenated sugar C: maltotriitol (33.1% solids in aqueous solution, column fractionated from sweet G3). The properties of hydrogenated sugar A (moisture, solids, viscosity, pH, sugar composition) are shown in Table 1, and the sugar compositions of hydrogenated sugars B and C are shown in Table 2. The sugar composition is the ratio of sorbitol (G1), maltitol (G2), maltotriitol (G3), and sugars above maltotetratol (G4 and above).

[0045] [Table 1]

[0046] [Table 2]

[0047] In Table 1, the moisture content was measured using a Karl Fischer moisture meter. The solid content was calculated by subtracting the moisture content (%) from the solid content (100). The viscosity was measured at a measurement temperature of 25°C using an E-type viscometer (manufactured by Toki Sangyo Co., Ltd.). The pH was measured at 25° C. in accordance with the provisions of JIS K6910, 5.4. The sugar composition was measured using an HPLC apparatus ("Waters Alliance 2695" manufactured by Japan Waters) under the following measurement conditions. Column: ULTRON PS-80N (8 mm x 300 mm): manufactured by Shinwa Kako Co., Ltd. Solvent: ultrapure water, Temperature: 60℃, Flow rate: 0.6mL / min, Detection: RI.

[0048] <Examples 1 to 9, Comparative Examples 1 to 2> (1. Preparation of Binder Composition) The materials were mixed according to the formulations shown in Tables 3 and 4 to obtain sugar binder compositions.

[0049] [Table 3]

[0050] [Table 4]

[0051] (2. Measurement of basic characteristics) The following properties were measured for the binder compositions of Examples 1 to 5 and Comparative Example 1. The results are shown in Table 5.

[0052] "viscosity" The viscosity of the binder composition was measured at a measurement temperature of 25° C. using an E-type viscometer (manufactured by Toki Sangyo Co., Ltd.).

[0053] "pH" The pH of the binder composition was measured at a measurement temperature of 25° C. in accordance with the provisions of JIS K6910, 5.4.

[0054] "Solids (non-volatile content) concentration" The mass C1 (g) of an aluminum foil dish (inner diameter 50 mm, height 15 mm) was measured, and 1.5 g of the sample (binder composition) was precisely weighed thereon, and the specific mass of the sample was taken as the sample mass S1 (g) before drying. The aluminum foil dish was placed in a thermostatic chamber previously kept at 135°C, and dried for 60 minutes, then cooled in a desiccator, and its mass C2 (g) was measured. From the results, the sample mass D1 after drying (mass of the sample remaining on the aluminum foil dish after drying, non-volatile content) (g) was calculated using the following formula (1), and the solid content concentration was calculated using the following formula (2). D1 = C2 - C1 (1) Solids concentration (%) = D1 / S1 × 100 (2)

[0055] "Gelation time" The gelation time of the binder composition was measured at a measurement temperature of 170° C. in accordance with the provisions of JIS K6910, 5.14.1 (gelation time method A).

[0056] [Table 5]

[0057] Among the binder compositions shown in Table 5, the binder compositions of Examples 1 to 5 had shorter gelation times than the binder composition of Comparative Example 1.

[0058] (3. Measurement of degree of cure) The degree of cure was measured by the following procedure for the binder compositions of Examples 1 to 5 and Comparative Example 1. The results are shown in Table 6. The mass C1 (g) of an aluminum foil dish (inner diameter 50 mm, height 15 mm) was measured, and 1 g of the sample (binder composition) was precisely weighed thereon. The aluminum foil dish was heated at 150°C for 10 minutes to harden the sample, and then cooled, and its mass C2 (g) was measured. From the results, the mass A (g) of the hardened product was calculated using the following formula (3). A = C2 - C1 (3) Next, about 50 g of water was placed in the aluminum foil dish, and the aluminum foil dish was left to stand at room temperature for 30 minutes, after which the water was discarded. The aluminum foil dish was placed in a thermostatic chamber previously kept at 135°C, and dried for 60 minutes, then cooled in a desiccator, and its mass C3 was measured. From the results, the mass B (g) of the cured product that remained undissolved in water was calculated using the following formula (4), and the degree of curing was calculated using the following formula (5). B = C3 - C1 (4) Curing degree (%)=100-(B / A×100) ···(5)

[0059] [Table 6]

[0060] As shown in Table 6, the binder compositions of Examples 1 to 5 tended to have a higher degree of hardening than the binder composition of Comparative Example 1.

[0061] (4. Measurement of tensile strength and water absorption rate) For the binder compositions of Examples 1 to 5 and Comparative Example 1, test pieces were prepared by the following procedure, and the tensile strength (normal strength, wet strength) and water absorption were measured. In addition, the strength retention was calculated from the normal strength and wet strength obtained by the following formula. The results are shown in Table 7. Strength retention rate (%) = Moisture resistance strength (MPa) / Normal strength (MPa) x 100

[0062] "Preparation of test specimens" A Whatman glass filter paper (GF / A) was cut to 90 mm x 25 mm, and its mass E (g) was measured. The glass filter paper was impregnated with the binder composition, and the excess binder composition was absorbed and removed with a Kimtowel. Release paper was placed on a punching metal, and the glass filter paper impregnated with the binder composition was placed on top of the release paper, and dried at 100°C for 30 minutes. The dried glass filter paper was then heat cured at 150°C for 15 minutes. The mass F (g) of the cured glass filter paper was measured, and the amount of binder attached was calculated by FE. In this test, the binder was adjusted to about 75%. Both ends of the hardened glass filter paper were cut with a cutter to give test pieces measuring 90 mm x 20 mm.

[0063] Six test pieces were prepared for each condition when the binder composition of each example was cured. Of the six test pieces, three were used to measure the normal strength and the remaining three were used to measure the moisture resistance. The test pieces used to measure the normal strength were also used to measure the water absorption rate. The test pieces for moisture resistance were subjected to moist heat pretreatment before the tensile test. The moist heat pretreatment conditions were a temperature of 60°C and a humidity of 90% for 6 hours. Immediately after the moist heat pretreatment, the mass of the test pieces was measured.

[0064] "Measurement of tensile strength" In a tensile tester, both ends (20 mm) of a test piece (for normal strength, no moist heat pretreatment was performed, for moist strength, moist heat pretreatment was performed) were clamped in a chuck and pulled at 5 mm / min, and the strength (N) at that time was measured. The tensile strength (normal strength or moist strength) was calculated from the measurement results using the following formula. In the formula, the cross-sectional area of ​​the test piece in this test was 20 mm x 0.3 mm = 6 mm 2 The tensile strength was measured for two test pieces, and the average value was calculated. Tensile strength (MPa) = measured strength (N) / cross-sectional area of ​​test piece (mm 2 )

[0065] "Water absorption measurement" The water absorption rate was calculated from the mass of the test piece for moisture resistance before and after the moist heat pretreatment according to the following formula. Water absorption rate (%) = mass of test piece after moist heat pretreatment (g) / mass of test piece before moist heat pretreatment (g) × 100

[0066] [Table 7]

[0067] As shown in Table 7, the test pieces using the binder compositions of Examples 1 to 5 were superior in normal strength, wet strength, and strength retention rate, and also had lower water absorption rates, compared to the test piece using the binder composition of Comparative Example 1.

[0068] (5. Measurement of Curing Speed) For the binder compositions of Examples 6 to 9 and Comparative Example 2, test pieces for dynamic viscoelasticity measurement (DMA) were prepared in the following manner, and DMA measurements were carried out under the following measurement conditions.

[0069] "Preparation of test specimens for DMA" Glass paper (100g / m 2 ) was cut into 10 mm x 50 mm pieces. The binder composition was diluted with water to a solid content of 5%, and the glass paper was impregnated with the diluted solution, which was then dried at room temperature for one day and night to prepare a test piece for DMA.

[0070] "DMA measurement conditions" Measuring equipment: Hitachi High-Techno Science DMA7100, Measurement temperature range: 30~240℃ Frequency: 1Hz, Heating rate: 4℃ / min, Mode: Film shear mode.

[0071] FIG. 1 shows the DMA charts of Examples 6 to 9 and Comparative Example 2. The rise (curing start) and convergence (curing convergence) of the elastic modulus were obtained from the tangent line in the DMA chart, and the curing time was calculated. The curing start temperature, curing convergence temperature, difference ΔT between the curing start temperature and the curing convergence temperature, curing time, and the relative curing time of Examples 6 to 9 when the curing time of Comparative Example 2 is set to 100 are shown in Table 8.

[0072] [Table 8]

[0073] As shown by the above results, the binder compositions of Examples 6 to 9 had a lower curing convergence temperature (curing end temperature) and a shorter curing time than the binder composition of Comparative Example 2. [Industrial Applicability]

[0074] The thermosetting binder composition of the present invention exhibits good binder performance without using raw materials containing formaldehyde. For example, inorganic fiber products using the thermosetting binder composition of the present invention have excellent tensile strength. In addition, the thermosetting binder composition of the present invention has excellent curing properties, and therefore, by using the thermosetting binder composition of the present invention, the productivity of inorganic fiber products and the like can be improved.

[0075] Because of the above-mentioned effects, the thermosetting binder composition of the present invention is useful for producing inorganic fiber products. However, the uses of the binder composition of the present invention are not limited thereto, and it can be used in various applications in which thermosetting binders such as phenolic resin binders have been used in the past, such as casting, friction materials, grinding wheels, filter paper, molding materials, plywood processing, decorative panels, laminates, etc.

Claims

1. comprising a hydrogenated sugar and a cross-linking agent, A thermosetting binder composition, in which the ratio of maltitol to the total mass of the hydrogenated sugar is 1 to 75.6 mass%, the ratio of maltotriitol is 20 to 94.4 mass%, and the ratio of hydrogenated sugars having tetrasaccharides or more is 0.8 to 16.7 mass%, based on the total mass of the hydrogenated sugar.

2. 2. The thermosetting binder composition according to claim 1, wherein the crosslinking agent is at least one selected from the group consisting of polycarboxylic acids, their salts, and acid anhydrides.

3. The thermosetting binder composition according to claim 1 or 2, further comprising a catalyst.

4. An inorganic fiber product comprising a molded body formed by binding inorganic fibers with a binder, The binder is a cured product of the thermosetting binder composition according to any one of claims 1 to 3.

5. The inorganic fiber product according to claim 4 , wherein the inorganic fiber is glass wool or rock wool.

Citation Information

Patent Citations

  • Component inspection unit

    JP1980075658A

  • Refrigerator

    JP1981094166A

  • Temperature detecting device for air conditioner

    JP1986041840A

  • Sizing composition for mineral wool based on hydrogenated sugars and the resulting insulating product

    JP2012502199A

  • Binder composition on an oligoester basis, production thereof, and use thereof for binding organic or mineral fibres