R-T-B permanent magnet
By controlling the distribution and spacing of R-rich phases between main phase particles in R-T-B magnets, the coercive force is enhanced, addressing the underperformance of conventional magnets, resulting in improved magnetic properties.
Patent Information
- Application Number
- JP2021143354
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-12-22
- Filing Date
- 2021-09-02
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2041-09-02
AI Technical Summary
Conventional R-T-B permanent magnets, despite having fine crystal grain sizes, fail to achieve the expected high coercive force due to the distribution of R-rich phases affecting the coercive force in the cross section parallel to the easy axis direction.
The R-T-B permanent magnet is designed with specific control over the distribution of R-rich phases, ensuring they are located between main phase particles, with an average spacing of 30 μm to 1000 μm perpendicular to the easy axis direction, and main phase particles with dimensions within certain ranges to enhance coercive force.
This design results in a permanent magnet with significantly higher coercive force, maintaining it at room and elevated temperatures, while also enhancing residual magnetic flux density and squareness ratio.
Smart Images

Figure 0007593903000002 
Figure 0007593903000003 
Figure 0007593903000004
Abstract
Description
[Technical field]
[0001] The present invention relates to an RTB based permanent magnet. [Background technology]
[0002] R-T-B permanent magnets contain rare earth elements R (Nd, etc.), transition metal elements T (Fe, etc.), and boron (B). R-T-B permanent magnets have excellent magnetic properties and are widely used. R-T-B permanent magnets include sintered magnets manufactured by powder metallurgy and hot-processed magnets manufactured by hot plastic processing. (See Patent Document 1, Non-Patent Documents 1 and 2 below.) The alloy ribbon, which is the raw material of the hot-processed magnet, is obtained by the super-rapid solidification method. In the super-rapid solidification method, the molten R-T-B alloy is rapidly cooled on the surface of a cooling roll. As a result, the molten metal solidifies to form an alloy ribbon. The alloy ribbon obtained by the super-rapid solidification method contains microcrystals (and amorphous alloy) of the alloy. Therefore, the crystal grains (main phase particles) constituting the hot-processed magnet are finer than those of the sintered magnet. It is known that the finer the crystal grain size of an R-T-B permanent magnet, the higher the coercive force (HcJ), as shown by the Kronmuller formula. Therefore, hot-processed magnets should have a higher coercive force than sintered magnets. However, the coercive force of conventional hot-processed magnets is equivalent to that of sintered magnets with similar compositions, and they do not achieve the high coercive force expected from a fine crystal grain size. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2016-96203 A [Non-patent literature]
[0004] [Non-Patent Document 1] M. Soderznik et al, Magnetization reversal process of anisotropic hot-deformed magnets observed by magneto-opticalKerr effect microscopy,Journal of Alloys and Compounds 771 (2019) 51 - 59. [Non-Patent Document 2] LAI Bin et al, Quasi-periodic layer structure of die-upset NdFeB magnets, JOURNAL OF RARE EARTHS, Vol. 31, No.7, July 2013, P. 679 - 684. Summary of the Invention [Problem to be solved by the invention]
[0005] Therefore, the inventors investigated and considered the reason why conventional R-T-B permanent magnets (e.g., hot-worked magnets) do not have a high coercive force commensurate with the fine crystal grain size. As a result, the inventors found that the distribution of the R-rich phase in the cross section of an R-T-B permanent magnet that is approximately parallel to the easy axis of magnetization affects the coercive force. Furthermore, the inventors found a method for obtaining an R-T-B permanent magnet with high coercive force by controlling the distribution of the R-rich phase in the cross section.
[0006] An object of the present invention is to provide an RTB based permanent magnet having high coercive force. [Means for solving the problem]
[0007] An R-T-B system permanent magnet according to one aspect of the present invention is an R-T-B system permanent magnet containing a rare earth element R and transition metal elements T and B, wherein the R-T-B system permanent magnet contains at least Nd as R, and the R-T-B system permanent magnet contains at least Fe as T, the R-T-B system permanent magnet comprises a plurality of main phase particles and a plurality of R-rich phases, the main phase particles contain at least R, T and B, and the R-rich phase contains at least R, the main phase particles observed in a cross section of the R-T-B system permanent magnet are flat, the cross section is approximately parallel to the direction of easy magnetization of the R-T-B system permanent magnet, the R-rich phase is located between the plurality of main phase particles, the average spacing between the R-rich phases in a direction approximately perpendicular to the direction of easy magnetization is 30 μm or more and 1000 μm or less, and the average length of the minor axes of the main phase particles observed in the cross section is 20 nm or more and 200 nm or less.
[0008] The R content in the R-T-B system permanent magnet may be 28 mass % or more and 33 mass % or less, and the B content in the R-T-B system permanent magnet may be 0.8 mass % or more and 1.1 mass % or less.
[0009] A plurality of flattened main phase grains may be stacked along the easy axis direction.
[0010] The R-T-B based permanent magnet may be a hot worked magnet.
[0011] The concentration of R in the R-rich phase may be higher than the average concentration of R in the cross section, and the unit of the concentration of R may be atomic %.
[0012] The concentration of R in the R-rich phase may be higher than the concentration of R in the main phase particles, and the unit of the concentration of R may be atomic %. Effect of the Invention
[0013] According to the present invention, an RTB based permanent magnet having high coercive force is provided. [Brief description of the drawings]
[0014] [Figure 1] (a) in Figure 1 is a schematic perspective view of an R-T-B system permanent magnet according to one embodiment of the present invention, and (b) in Figure 1 is a schematic diagram of a cross section of the R-T-B system permanent magnet shown in (a) in Figure 1 (viewed in the direction of the arrows along line b-b). [Diagram 2] FIG. 2 is an enlarged view of a part (region II) of the cross section shown in (b) of FIG. 1, and a brightness distribution of a backscattered electron image of region II. [Diagram 3] FIG. 3 is a backscattered electron image of a cross section of the RTB system permanent magnet of Example 2. [Figure 4] FIG. 4 is a backscattered electron image of a cross section of the RTB system permanent magnet of Comparative Example 8. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Preferred embodiments of the present invention will be described below with reference to the drawings. In the drawings, equivalent components are given the same reference numerals. The present invention is not limited to the following embodiments. The "permanent magnet" described below means an R-T-B system permanent magnet. The unit of concentration of each element in the permanent magnet described below is atomic %.
[0016] (Permanent magnet) The permanent magnet according to the present embodiment contains at least a rare earth element (R), a transition metal element (T) and boron (B). The permanent magnet according to the present embodiment is a hot worked magnet. However, the permanent magnet according to the present embodiment may be a sintered magnet.
[0017] The permanent magnet contains at least neodymium (Nd) as a rare earth element R. The permanent magnet may contain other rare earth elements R in addition to Nd. The other rare earth elements R contained in the permanent magnet may be at least one selected from the group consisting of scandium (Sc), yttrium (Y), lanthanum (La), cerium (Ce), praseodymium (Pr), samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), ytterbium (Yb), and lutetium (Lu).
[0018] The permanent magnet contains at least iron (Fe) as the transition metal element T. The permanent magnet may contain only Fe as the transition metal element T. The permanent magnet may contain both Fe and cobalt (Co) as the transition metal element T.
[0019] FIG. 1(a) is a perspective view of a permanent magnet 2 according to this embodiment. FIG. 1(b) is a schematic diagram of a cross section 2cs of the permanent magnet 2, which is approximately parallel to the magnetization easy axis direction C of the permanent magnet 2. The magnetization easy axis direction C is parallel to a line connecting a pair of magnetic poles of the permanent magnet 2. In other words, the magnetization easy axis direction C is a direction from the S pole of the permanent magnet 2 to the N pole of the permanent magnet 2. The magnetization easy axis direction C may be determined based on a measurement of the magnetic flux distribution of the permanent magnet 2. The magnetization easy axis direction C may be determined based on a measurement of the magnetic flux distribution of an analysis sample separated from the permanent magnet 2.
[0020] The permanent magnet 2 according to this embodiment is a rectangular parallelepiped (plate). However, the shape of the permanent magnet 2 is not limited to a rectangular parallelepiped. For example, the shape of the permanent magnet 2 may be, for example, a cube, a polygonal prism, an arc segment, an annular sector, a sphere, a disk, a cylinder, a tube, or a ring. The shape of the cross section 2cs of the permanent magnet 2 may be, for example, a polygon, an arc (circular chord), a bow, an arch, a C-shape, or a circle.
[0021] 2 is an enlarged view of a portion (region II) of the cross section 2cs shown in (b) of FIG. 1. As shown in FIG. 2, the permanent magnet 2 includes a plurality of main phase particles 4 and a plurality of R-rich phases 6. The R-rich phases 6 are located between the plurality of main phase particles 4. The R-rich phases 6 may be a type of grain boundary phase included in the grain boundaries between the plurality of main phase particles 4. The grain boundary including the R-rich phases 6 may be a grain boundary multiple point surrounded by three or more main phase particles 4, or may be a two-grain grain boundary between two main phase particles 4. The total volume ratio of the main phase particles 4 in the permanent magnet 2 is not particularly limited, and may be, for example, 80 volume % or more and less than 100 volume %, 90 volume % or more and less than 100 volume %, or 95 volume % or more and less than 100 volume %.
[0022] The main phase grains 4 contain at least Nd, T and B. The main phase grains 4 may be rephrased as single crystal grains (i.e., primary particles). 14 Includes crystals (single crystal or polycrystal) of B. R2T 14 B is a ternary intermetallic compound having ferromagnetic properties. The main phase particles 4 are R2T 14 It may consist of only B crystals. 14 The crystal of B may be tetragonal. That is, R2T 14 The crystal axes of B are the a-axis, the b-axis, and the c-axis, which are perpendicular to each other. 14 The lattice constant of B in the a-axis direction is R2T 14 B is equal to the lattice constant in the b-axis direction, and R2T 14 The lattice constant of B in the c-axis direction may be different from the lattice constants in the a-axis direction and the b-axis direction. 14 The c-axis direction of B may be approximately parallel to the magnetization easy axis direction C of the permanent magnet 2.
[0023] The main phase grains 4 may contain other elements in addition to Nd, T, and B. For example, R2T constituting the main phase grains 4 14 B is (Nd 1-x Pr x )2(Fe 1-y Co y ) 14B. x may be 0 or more and less than 1. y may be 0 or more and less than 1. The main phase grains 4 may contain heavy rare earth elements such as Tb and Dy as R in addition to the light rare earth elements. 14 A part of B in B may be substituted with another element such as carbon (C). The composition within the main phase particle 4 may be uniform. The composition within the main phase particle 4 may be non-uniform. For example, the concentration distribution of each of R, T and B in the main phase particle 4 may have a gradient.
[0024] The main phase particles 4 may be composed of a surface layer and a center portion covered by the surface layer. The surface layer may be referred to as a shell, and the center portion may be referred to as a core. The surface layer of the main phase particles 4 may contain at least one heavy rare earth element selected from Tb and Dy. The surface layer of each of all the main phase particles 4 may contain at least one heavy rare earth element selected from Tb and Dy. The surface layer of a part of all the main phase particles 4 may contain at least one heavy rare earth element selected from Tb and Dy. When the surface layer contains a heavy rare earth element, the anisotropic magnetic field is likely to increase locally in the vicinity of the grain boundary, and nuclei of magnetization reversal are unlikely to occur in the vicinity of the grain boundary. As a result, the coercive force of the permanent magnet 2 at high temperatures (for example, 100 to 200°C) is increased. Since the residual magnetic flux density (Br) and coercive force of the permanent magnet 2 are likely to be compatible, the total concentration of the heavy rare earth elements in the surface layer portion may be higher than the total concentration of the heavy rare earth elements in the central portion.
[0025] The R-rich phase 6 is a non-ferromagnetic phase. The R-rich phase 6 contains at least R. For example, the R-rich phase 6 may contain Nd as R. The R-rich phase 6 may further contain one or more other rare earth elements in addition to Nd as R. The R-rich phase 6 may further contain one or more elements other than R in addition to R. The R-rich phase 6 may contain at least one component selected from the group consisting of metals, alloys, intermetallic compounds, and oxides. For example, a part or all of the R-rich phase 6 may be composed of only at least one component selected from the group consisting of a simple substance of R, an alloy containing R, and a metal compound containing R. A part or all of the R-rich phase 6 may contain an oxide of R. For example, the oxide of R may be an oxide of Nd. The oxidized surface of the main phase particle 4 may be an oxide of R. A part of the R-rich phase 6 may be composed of only an oxide of R. The present inventors consider that the R-rich phase 6 containing an oxide of R can be formed by oxidation of R located in the vicinity of the surface of the alloy ribbon or alloy powder (precursor of the main phase particles 4) during the production process of the permanent magnet 2 (particularly, each transportation step described later).
[0026] The concentration of R in the R-rich phase 6 may be higher than the average value of the concentration of R in the cross section 2cs. The concentration of R in the R-rich phase 6 may be higher than the average value of the concentration of R in the main phase particles 4. When the permanent magnet 2 contains multiple types of R, the concentration of R may be the sum of the concentrations of the multiple types of R.
[0027] As shown in FIG. 2, each main phase particle 4 observed in the cross section 2cs is flat. In other words, each main phase particle 4 observed in the cross section 2cs may be plate-shaped. A plurality of flat main phase particles 4 may be stacked along the easy axis direction C. The permanent magnet 2 may further include secondary particles 4a composed of a plurality of main phase particles 4 bonded to each other. The permanent magnet 2 may include a plurality of secondary particles 4a. At least a portion of the R-rich phase 6 may be located at a grain boundary between the plurality of secondary particles 4a. The oxidized surface of the secondary particle 4a may be an oxide of R. The plurality of R-rich phases 6 are aligned along a direction substantially perpendicular to the easy axis direction C. In other words, the plurality of R-rich phases 6 may be scattered in the cross section 2cs along a direction substantially perpendicular to the easy axis direction C. Each of the plurality of R-rich phases 6 aligned along a direction substantially perpendicular to the easy axis direction C may be located between at least two main phase particles 4. A part of the R-rich phase 6 may be a layer extending in a direction substantially perpendicular to the magnetization easy axis direction C. A part of the R-rich phase 6 may be located between a plurality of flat main phase grains 4 stacked along the magnetization easy axis direction C.
[0028] The "AB direction" described below means a direction substantially perpendicular to the direction C of easy magnetization.
[0029] Average spacing of R-rich phase 6 in the AB direction i AVE is 30 μm or more and 1000 μm or less. The average value i of the interval between the R-rich phases 6 in the AB direction AVE may be 30.42 μm or more and 975.00 μm or less, 34 μm or more and 1000 μm or less, 34.89 μm or more and 975.00 μm or less, 34 μm or more and 38 μm or less, 34.89 μm or more and 37.77 μm or less, 34 μm or more and 36 μm or less, or 34.89 μm or more and 35.82 μm or less. AVE may be one value selected from the group consisting of 30 μm, 30.42 μm, 34.89 μm, 35.82 μm, 37.77 μm, 269.87 μm, 446.70 μm, 674.12 μm, 886.36 μm, and 975.00 μm, and the average value i AVEThe upper limit value of may be one value selected from the group consisting of 30.42 μm, 34.89 μm, 35.82 μm, 37.77 μm, 269.87 μm, 446.70 μm, 674.12 μm, 886.36 μm, 975.00 μm, and 1000 μm. AVE When the average value i of the spacing between the R-rich phases 6 in the AB direction is within the above range, the permanent magnet 2 can have a high coercive force at room temperature and at high temperatures. AVE may be approximately equal to the average value of the total width of one or more main phase grains 4 located between a pair of R-rich phases 6 in the AB direction. The average value of the spacing between the R-rich phases 6 in the AB direction is measured by the following method.
[0030] A backscattered electron image of a part (region II) of the cross section 2cs of the permanent magnet 2 is taken by a scanning electron microscope (SEM). The magnification of the backscattered electron image may be, for example, 300 times. As shown in FIG. 2, an arbitrary rectangular measurement region A in which a plurality of parts (6) with relatively high brightness are arranged along the AB direction is selected from the backscattered electron image. The width of the measurement region A in the AB direction is larger than the width of the measurement region A in the magnetization easy axis direction C. For example, the width of the measurement region A in the AB direction may be 400 μm, and the width of the measurement region A in the magnetization easy axis direction C may be 15 μm. The measurement region A is scanned with an electron beam along the AB direction, and the brightness of each measurement point in the measurement region A is continuously measured along the AB direction. As a result, a brightness distribution D of the measurement region A along the AB direction is obtained. The interval between the measurement points may be, for example, 1 μm or less. The brightness is the intensity of the backscattered electron beam at each measurement point (INTENSITY in FIG. 2). The unit of brightness is an arbitrary unit (au). The greater the atomic weight of an element, the higher the brightness of the measurement point where that element is present, and the higher the concentration of an element with a large atomic weight at the measurement point, the higher the brightness of the measurement point. Of all the elements contained in the permanent magnet 2, the atomic weight of R is relatively large. Therefore, a peak in the brightness distribution D suggests the presence of an R-rich phase. A moving average I of brightness is calculated from the brightness of an arbitrary measurement point X in the measurement area A, the brightness of each of the five measurement points measured immediately before the measurement of the brightness of the measurement point X, and the brightness of each of the five measurement points measured immediately after the measurement of the brightness of the measurement point X.AVE In other words, the moving average of the brightness I is calculated from the brightness of a total of 11 measurement points including the measurement point X. AVE is calculated from the luminance of the measurement point X. AVE The value obtained by subtracting I AVE If the luminance at the measurement point X is 7% or more of I AVE 107% or more, the position (POSITION in FIG. 2) of measurement point X (peak of brightness at measurement point X) is the position of the R-rich phase 6. The distance (distance in the AB direction) between two adjacent R-rich phases 6 is the interval between the R-rich phases 6 in the AB direction. Based on the above premise, the average value of the intervals between the R-rich phases 6 in the measurement area A is calculated. For example, there are four R-rich phases 6 in the measurement area A shown in FIG. 2, and i1, i2, and i3 are measured as the intervals between the R-rich phases 6. The average value of the intervals between the R-rich phases 6 in the measurement area A shown in FIG. 2 is (i1+i2+i3) / 3. A plurality of different measurement regions A are selected from the backscattered electron image, and the average value of the spacing between the R-rich phases 6 in each measurement region A is measured by the above-mentioned method. For example, five measurement regions A may be selected from the backscattered electron image. The average values of the spacing between the R-rich phases 6 in each of the plurality of measurement regions A are further averaged to obtain the above-mentioned average value i AVE It should be noted that the average line (100% line) of the luminance distribution D in FIG.
[0031] The R-rich phase 6 is the cause of the decrease in coercivity of the permanent magnet 2. However, the permanent magnet 2 according to this embodiment can have a higher coercivity than a conventional permanent magnet having a similar composition. In other words, the permanent magnet 2 according to this embodiment suppresses the decrease in coercivity caused by the R-rich phase 6. The mechanism by which the decrease in coercivity caused by the R-rich phase 6 is suppressed is described below. However, the technical scope of the present invention is not limited by the mechanism described below.
[0032] The coercivity mechanism of R-T-B permanent magnets is of the nucleation type, so the creation of reverse magnetic domains becomes the nucleus of magnetization reversal. In other words, the creation of reverse magnetic domains causes a decrease in coercivity. Reverse magnetic domains are created in places with large local demagnetizing fields. Places with large local demagnetizing fields include voids, the surfaces of main phase particles, and heterogeneous phases. <Hole> Both sintered magnets and hot-deformed magnets are densified to nearly true density, so voids are unlikely to exist. <Surface of main phase grains> The shape of the main phase particles that make up the sintered magnet reflects the shape of the alloy powder obtained by airflow pulverization, so the main phase particles that make up the sintered magnet have an irregular (distorted) shape. Since the surfaces of irregularly shaped main phase particles are not smooth, they are likely to become the starting points for the generation of reverse magnetic domains. On the other hand, the main phase grains that make up the hot-worked magnet are plate-like crystals that have undergone anisotropic crystal growth from extremely fine crystal grains. As a result, the shapes of the main phase grains that make up the hot-worked magnet are relatively uniform, and the surfaces of the main phase grains that make up the hot-worked magnet are smoother than the surfaces of the main phase grains that make up the sintered magnet. Therefore, the local demagnetizing field is small on the surfaces of the main phase grains that make up the hot-worked magnet, making it difficult for reverse magnetic domains to form. As a result, hot-worked magnets tend to have high coercivity. <Altered Phase> Sintered magnets are densified by the sintering process. In the sintering process, a compact formed from alloy powder is sintered. In the sintering process, the surface of the alloy powder becomes a liquid phase, and the liquid phase fills the gaps between the alloy powder particles to become a grain boundary phase (R-rich phase), resulting in a dense sintered body. The two-particle grain boundary phase is useful for magnetic separation that prevents the movement of domain walls between main phase particles. Excess grain boundary phase components other than the two-particle grain boundary phase are discharged from the surface of the sintered body, but the amount is small, and most of them segregate to grain boundary multiple points. The grain boundary phase segregated to grain boundary multiple points is not useful. This is because the grain boundary phase segregated to grain boundary multiple points becomes a different phase and becomes the starting point for the generation of reverse magnetic domains. However, as mentioned above, sintered magnets require a liquid phase for densification, so the segregation of the grain boundary phase (R-rich phase) to the grain boundary multiple points is inevitable. On the other hand, the densification of hot-worked magnets depends on the temperature and pressure of hot pressing and hot plastic working. Therefore, the densification of hot-worked magnets does not require as much grain boundary phase as sintered magnets. The grain boundary phase (R-rich phase), which is a liquid phase, is useful for the lubrication (grain boundary sliding) of the main phase particles when the anisotropically grown plate-like main phase particles are rearranged by hot plastic working. However, the amount of liquid phase required for the lubrication of the main phase particles is less than the amount of liquid phase required for the densification of sintered magnets. Therefore, the segregation and aggregation of the R-rich phase at the grain boundary multiple points of hot-worked magnets is less than that of sintered magnets. In other words, the heterogeneous phase in hot-worked magnets is less than that of sintered magnets. Therefore, hot-worked magnets tend to have high coercivity. However, hot-processed magnets also inevitably contain R-rich phases. When R-rich phases such as two-particle grain boundary phases cover the surface of each main phase particle, adjacent main phase particles are magnetically separated from each other, increasing the coercive force of the permanent magnet. On the other hand, R-rich phases that segregate and aggregate at grain boundary multiple points tend to generate reverse magnetic domains. In other words, R-rich phases that segregate and aggregate at grain boundary multiple points become nuclei of magnetization reversal. Starting from these nuclei of magnetization reversal, magnetization reversal of the main phase particles progresses, decreasing the coercive force of the permanent magnet. As described above, conventional sintered magnets and hot-deformed magnets suffer from a decrease in coercivity due to R-rich phases that segregate and aggregate at grain boundary multiple points. In contrast, in the case of the permanent magnet 2 according to the present embodiment, the average interval between the R-rich phases 6 in the AB direction i AVE is 30 μm or more, and the intervals of the R-rich phases 6 in the AB direction are relatively large. Therefore, segregation and aggregation (generation of nuclei for magnetization reversal) of the R-rich phases 6 in the AB direction are suppressed, and the frequency of generation of reverse magnetic domains in the AB direction is reduced. As a result, the decrease in coercivity caused by the segregation and aggregation of the R-rich phases 6 is suppressed. Average spacing of R-rich phase 6 in the AB direction i AVE When the diameter is 30 μm or more, the R-rich phase 6 segregated and aggregated at the grain boundary multiple points is small, and the R-rich phase 6 easily surrounds each main phase grain 4 without any spots. As a result, adjacent main phase grains are magnetically separated from each other, and the coercive force of the permanent magnet 2 is increased. However, the average interval of the R-rich phase 6 in the AB direction is i AVE As the width of each main phase grain 4 located between a pair of R-rich phases 6 in the AB direction increases, the width of each main phase grain 4 located between the pair of R-rich phases 6 in the AB direction tends to increase. In other words, the average value i AVE As the temperature increases, the grain size (crystal grain size) of the main phase grains 4 located between a pair of R-rich phases 6 in the AB direction tends to increase. Due to the increase in the grain size (crystal grain size) of the main phase grains 4, the coercivity of the permanent magnet 2 tends to decrease with increasing temperature, and the squareness ratio (Hk / HcJ) of the permanent magnet 2 also tends to decrease. (Hk is the strength of the demagnetizing field equivalent to 90% of the residual magnetic flux density in the second quadrant of the magnetization curve.) In addition, the coarse main phase grains 4 are difficult to rotate during hot plastic working and difficult to be oriented in the magnetization easy axis direction C, which is one of the causes of the decrease in residual magnetic flux density. However, according to the present embodiment, the average interval between the R-rich phases 6 in the AB direction i AVE is 1000 μm or less, main phase particles 4 with excessively large grain sizes (crystal grain sizes) are unlikely to be contained in the permanent magnet 2. As a result, the decrease in coercivity caused by an increase in the grain size (crystal grain size) of the main phase particles 4 is suppressed, the decrease in coercivity caused by an increase in temperature is suppressed, the decrease in squareness ratio is suppressed, and the decrease in residual magnetic flux density is suppressed.
[0033] The average value of the length of the minor axis of the main phase particles 4 (primary particles) observed in the cross section 2cs is, for example, 20 nm or more and 200 nm or less. When the average value of the length of the minor axis of the main phase particles 4 is less than 20 nm, each main phase particle 4 (R2T 14B) is insufficient, and the main phase grains 4 are difficult to orient in the easy axis direction C, and the coercivity, squareness ratio, and residual magnetic flux density are likely to decrease. When the average value of the short axis length of the main phase grains 4 is greater than 200 nm, the grain size (crystal grain size) of the main phase grains 4 is excessively large, and the main phase grains 4 are difficult to orient in the easy axis direction C, and the coercivity, squareness ratio, and residual magnetic flux density are likely to decrease. Since the decrease in coercivity, squareness ratio, and residual magnetic flux density is likely to be suppressed, the average value of the short axis length of the main phase grains 4 observed in the cross section 2cs may be 22 nm or more and 187 nm or less. For the same reason, the lower limit of the average value of the short axis length of the main phase grains 4 observed in the cross section 2cs may be one value selected from the group consisting of 20 nm, 22.00 nm, 86.00 nm, 92.00 nm, 122.00 nm, 157.00 nm, 164.00 nm, 172.00 nm, 187.00 nm, and 198.00 nm, and the upper limit of the average value of the short axis length of the main phase grains 4 observed in the cross section 2cs may be one value selected from the group consisting of 22.00 nm, 88.00 nm, 92.00 nm, 122.00 nm, 157.00 nm, 164.00 nm, 172.00 nm, 187.00 nm, 198.00 nm, and 200 nm. The average value of the length of the major axis of the main phase particles 4 (primary particles) observed in the cross section 2cs may be, for example, 100 nm or more and 1000 nm or less. When the average value of the length of the major axis of the main phase particles 4 is within the above range, the average value i of the interval between the R-rich phases 6 in the AB direction AVE The larger the average value of the length of the major axis of the main phase grains 4, the more easily the average value of the intervals between the R-rich phases 6 in the AB direction i AVE The smaller the average value of the length of the major axes of the main phase grains 4, the higher the coercive force of the permanent magnet 2 tends to be. The short axis of each main phase particle 4 observed in the cross section 2cs may be approximately parallel to the magnetization easy axis direction C. The long axis of each main phase particle 4 may be approximately perpendicular to the magnetization easy axis direction C. The shape of the main phase particle 4 in the cross section 2cs is not limited to a rectangle. The shape of the main phase particle 4 in the cross section 2cs may be distorted. The shape of the main phase particle 4 in the cross section 2cs may not be uniform. When the shape of the main phase particle 4 in the cross section 2cs is distorted, the shape of the main phase particle 4 may be approximated by a rectangle that has the smallest area among the rectangles circumscribing the main phase particle 4. The rectangle may be a rectangle. The length of the short side of this rectangle may be regarded as the length of the short axis of the main phase particle 4, and the length of the long side of the rectangle may be regarded as the length of the long axis of the main phase particle 4. The average value of the length of the short axis of the main phase particle 4 may be calculated from the measured values of the lengths of the short axes of all the main phase particles 4 present in a backscattered electron image of the cross section 2cs taken by a scanning electron microscope (SEM). The average value of the length of the major axis of the main phase particles 4 may also be calculated from the measured values of the length of the major axis of all the main phase particles 4 present in the backscattered electron image. However, the dimensions of the main phase particles 4 protruding from the backscattered electron image are excluded from the calculation of the average value. The maximum value of the size of the backscattered electron image used to measure the length of each of the minor and major axes of the main phase particles 4 may be, for example, 120 μm in length × 80 μm in width, or 80 μm in length × 120 μm in width. A plurality of representative locations may be selected from the backscattered electron images taken at these low magnifications, and the backscattered electron images of each location may be taken at a high magnification. Then, the average value of each of the major and minor axes may be calculated from the lengths of the major and minor axes of all the main phase particles 4 measured in the backscattered electron image at a high magnification. Commercially available image analysis software may be used to specify the shape (contour line) of the main phase particles 4 and to measure the size of the main phase particles 4 (rectangles circumscribing the main phase particles 4).
[0034] The width of each R-rich phase 6 in the easy axis direction C may be, for example, 100 nm or more and 20000 nm or less. The width of each R-rich phase 6 in the AB direction may be, for example, 100 nm or more and 20000 nm or less. When the width of the R-rich phase 6 is within the above range, the magnetization reversal of the main phase particles 4 due to the R-rich phase 6 is likely to be suppressed, and the permanent magnet 2 is likely to have a high coercive force. The width of the R-rich phase 6 in the easy axis direction C may be equal to or less than the length of the minor axis of the main phase particles 4 (primary particles). The width of the R-rich phase 6 in the easy axis direction C may be equal to or less than the length of the minor axis of the secondary particles 4a. The width of the R-rich phase 6 in the AB direction may be equal to or less than the length of the major axis of the main phase particles 4 (primary particles). The width of the R-rich phase 6 in the AB direction may be equal to or less than the length of the major axis of the secondary particles 4a.
[0035] The width of the permanent magnet 2 in the AB direction is the average value of the intervals between the R-rich phases 6 in the AB direction i AVE The width of the permanent magnet 2 in the AB direction may be, for example, several mm to several hundred mm, or several tens of mm to several hundred mm. The vertical width of the permanent magnet 2 in the direction perpendicular to the AB direction may also be, for example, several mm to several hundred mm, or several tens of mm to several hundred mm. The horizontal width of the permanent magnet 2 in the direction perpendicular to the AB direction may also be, for example, several mm to several hundred mm, or several tens of mm to several hundred mm.
[0036] The grain boundaries may include a grain boundary phase other than the R-rich phase 6. For example, the grain boundaries may include a grain boundary phase including an element introduced into the permanent magnet 2 by the grain boundary diffusion process described below. The element introduced into the permanent magnet 2 by the grain boundary diffusion process may be at least one heavy rare earth element selected from Tb and Dy. The element introduced into the permanent magnet 2 by the grain boundary diffusion process may be a heavy rare earth element and a light rare earth element, and the light rare earth element may be at least one of Nd and Pr. The element introduced into the permanent magnet 2 by the grain boundary diffusion process may be a heavy rare earth element, a light rare earth element, and copper.
[0037] The main phase particles 4 and the R-rich phase 6 can be identified based on the contrast of an image of the cross section 2cs of the permanent magnet 2 taken by a scanning electron microscope (SEM) or a scanning transmission electron microscope (STEM). The composition of each of the main phase particles 4 and the R-rich phase 6 may be analyzed by an electron probe microanalyzer (EPMA) equipped with an energy dispersive X-ray spectroscopy (EDS) device.
[0038] The overall composition of the permanent magnet 2 is described below. However, the composition of the permanent magnet 2 is not limited to the composition below. The content of each element in the permanent magnet 2 may be outside the range below.
[0039] The total content of rare earth elements R in permanent magnet 2 may be 25.00% by mass or more and 35.00% by mass or less, or 28.00% by mass or more and 33.00% by mass or less. When the content of R is within the above range, the residual magnetic flux density and coercive force of permanent magnet 2 are likely to increase. When the content of R is too low, the R2T constituting main phase particles 4 becomes too low. 14 B is difficult to form, and an α-Fe phase having soft magnetism is easily formed. As a result, the coercive force is easily reduced. On the other hand, if the content of R is too high, the volume ratio of the main phase particles 4 is reduced, and the residual magnetic flux density is easily reduced. Since the residual magnetic flux density and the coercive force are easily increased, the total ratio of Nd and Pr to the total rare earth elements R may be 80 atomic % or more and 100 atomic % or less, or 95 atomic % or more and 100 atomic % or less.
[0040] The total content of Tb and Dy in the permanent magnet 2 may be 0.20% by mass or more and 5.00% by mass or less. When the permanent magnet 2 contains at least one heavy rare earth element selected from Tb and Dy, the magnetic properties (particularly the coercive force at high temperatures) of the permanent magnet 2 tend to increase. However, the permanent magnet 2 does not necessarily need to contain Tb and Dy.
[0041] The B content in the permanent magnet 2 may be 0.70% by mass or more and 1.10% by mass or less, or 0.80% by mass or more and 1.10% by mass or less. When the B content is 0.70% by mass or more, the residual magnetic flux density is likely to increase. When the B content is 1.10% by mass or less, the coercive force of the permanent magnet 2 is likely to increase. When the B content is within the above range, the squareness ratio of the permanent magnet 2 is likely to approach 1.0. When the total content of the rare earth element R in the permanent magnet 2 is 28.00 mass% or more and 33.00 mass% or less, and the content of B in the permanent magnet 2 is 0.80 mass% or more and 1.10 mass% or less, the content of the rare earth element R in the permanent magnet 2 is R2T 14 As a result, in the hot plastic working process described later, the liquid phase is easily generated at the grain boundaries. 14 B) promotes anisotropic growth, grain boundary sliding, and grain rotation. As a result, the c-axes of the crystal grains tend to be oriented in the stress direction, and the packing rate of the crystal grains in the permanent magnet 2 tends to increase (in other words, the volume ratio of the main phase tends to increase), and the coercive force and residual magnetic flux density of the permanent magnet 2 tend to increase.
[0042] The permanent magnet 2 may contain gallium (Ga). The Ga content may be 0.03 mass% or more and 1.00 mass% or less, or 0.20 mass% or more and 0.80 mass% or less. When the Ga content is within the above range, the generation of subphases (e.g., phases containing R, T and Ga) is appropriately suppressed, and the residual magnetic flux density and coercive force of the permanent magnet 2 tend to increase. However, the permanent magnet 2 does not have to contain Ga.
[0043] The permanent magnet 2 may contain aluminum (Al). The Al content in the permanent magnet 2 may be 0.01% by mass or more and 0.2% by mass or less, or 0.04% by mass or more and 0.07% by mass or less. When the Al content is within the above range, the coercive force and corrosion resistance of the permanent magnet are likely to be improved. However, the permanent magnet 2 does not have to contain Al.
[0044] The permanent magnet 2 may contain copper (Cu). The Cu content in the permanent magnet 2 may be 0.01% by mass or more and 1.50% by mass or less, or 0.04% by mass or more and 0.50% by mass or less. When the Cu content is within the above range, the coercive force, corrosion resistance, and temperature characteristics of the permanent magnet 2 are likely to be improved. However, the permanent magnet 2 does not have to contain Cu.
[0045] The permanent magnet 2 may contain cobalt (Co). The content of Co in the permanent magnet may be 0.30% by mass or more and 6.00% by mass or less, or 0.30% by mass or more and 4.00% by mass or less. When the permanent magnet 2 contains Co, the Curie temperature of the permanent magnet 2 is likely to be improved. Furthermore, when the permanent magnet 2 contains Co, the corrosion resistance of the permanent magnet 2 is likely to be improved. However, the permanent magnet 2 does not have to contain Co.
[0046] The remainder, excluding the above elements from the permanent magnet 2, may be only Fe, or Fe and other elements. In order for the permanent magnet 2 to have sufficient magnetic properties, the total content of the elements other than Fe in the remainder may be 5 mass% or less with respect to the total mass of the permanent magnet 2.
[0047] The permanent magnet 2 may contain at least one element selected from the group consisting of silicon (Si), titanium (Ti), Mn (manganese), Zr (zirconium), vanadium (V), chromium (Cr), nickel (Ni), niobium (Nb), molybdenum (Mo), hafnium (Hf), tantalum (Ta), tungsten (W), bismuth (Bi), tin (Sn), calcium (Ca), carbon (C), nitrogen (N), oxygen (O), chlorine (Cl), sulfur (S) and fluorine (F) as other elements (for example, inevitable impurities). The total content of the other elements in the permanent magnet 2 may be 0.001% by mass or more and 0.50% by mass.
[0048] The composition of the entire permanent magnet 2 may be analyzed by, for example, X-ray fluorescence (XRF) analysis, high-frequency inductively coupled plasma (ICP) optical emission analysis, inert gas fusion-non-dispersive infrared absorption (NDIR) method, combustion in oxygen flow-infrared absorption method, and inert gas fusion-thermal conductivity method.
[0049] The permanent magnet 2 may be applied to a motor, a generator, an actuator, etc. For example, the permanent magnet 2 is used in various fields such as hybrid cars, electric cars, hard disk drives, magnetic resonance imaging devices (MRI), smartphones, digital cameras, flat-screen TVs, scanners, air conditioners, heat pumps, refrigerators, vacuum cleaners, washer-dryers, elevators, and wind power generators.
[0050] (Manufacturing method of permanent magnets) The method for producing a permanent magnet according to the present embodiment includes at least a ribbon production step, a first conveying step, a crushing / classifying step, a second conveying step, a hot compacting step, a third conveying step, and a hot plastic working step. The method for producing a permanent magnet may further include other steps, such as a grain boundary diffusion step, following the hot plastic working step. However, the grain boundary diffusion step is not essential.
[0051] The ribbon production process is a process in which alloy ribbons are produced from the raw alloy by the super-rapid solidification method. In the super-rapid solidification method, the molten metal in a container is sprayed onto the surface of a chill roll from a nozzle located at the tip of the container. The molten metal comes into contact with the surface of the chill roll and is instantly thrown off by the chill roll rotating at high speed, becoming numerous elongated ribbons. Upon contacting the surface of the chill roll, the molten metal is rapidly cooled and solidified. As a result, numerous elongated alloy ribbons are formed. A container is placed in the direction in which the alloy ribbons are thrown off by the chill roll, and the alloy ribbons are collected into the container.
[0052] The nozzle hole diameter may be, for example, 0.2 mm or more and 1.0 mm or less. When the nozzle hole diameter is 0.2 mm or more and 1.0 mm or less, alloy powder having an average aspect ratio of 1 to 2 or less is easily recovered in the pulverization / classification process.
[0053] The molten metal is a metal (raw metal) containing each element constituting the permanent magnet. The raw metal may be, for example, a rare earth element (metal element), an alloy containing a rare earth element, pure iron, ferroboron, or an alloy containing these. These raw metals are weighed out so as to match the composition of the desired permanent magnet.
[0054] The molten metal may be obtained by heating the raw metal in the container by high-frequency induction heating. The temperature of the molten metal sprayed from the nozzle (spraying temperature) may be, for example, about 1400° C. The rate of temperature rise until the temperature of the raw metal reaches the spraying temperature may be, for example, about 20 to 100° C. / sec.
[0055] The surface of the chill roll may be made of a metal with high thermal conductivity, such as Cu. The temperature of the surface of the chill roll may be controlled by a coolant flowing through the chill roll. For example, if the cooling rate of the molten metal on the surface of the chill roll is about 10 5 ~10 6 The surface temperature of the cooling roll may be controlled to be 100° C. / sec. The higher the cooling rate, the greater the crystals (R 14 B) particle size tends to be finer, and the coercive force of the permanent magnet tends to increase. The smaller the amount of molten metal sprayed onto the surface of the chill roll per unit time, the thinner the molten metal adhering to the surface of the chill roll, the higher the cooling rate, and the thinner the alloy ribbon. The higher the peripheral speed of the chill roll, the thinner the molten metal adhering to the surface of the chill roll, the higher the cooling rate, and the thinner the alloy ribbon. The thickness of the main phase particles in the direction of the easy magnetization axis (the length of the short axis of the main phase particles) depends on the thickness of the alloy ribbon (as well as the crushing and classification of the alloy ribbon). The thinner the alloy ribbon, the smaller the thickness (particle size) of the main phase particles, and the higher the coercive force of the permanent magnet tends to be. However, one cause of the R-rich phase is the oxidation of the surface of the alloy ribbon, and the thinner the alloy ribbon, the more easily thin main phase particles with oxidized surfaces are included in the permanent magnet, and the average interval i of the R-rich phase AVEtends to be small. The thickness of the alloy ribbon may be, for example, 20 μm or more and 60 μm or less, or 30 μm or more and 50 μm or less. The width of the alloy ribbon may be, for example, 1.0 mm or more and 5.0 mm or less. When the alloy ribbon has the above dimensions, alloy powder having an average aspect ratio of 1 or more and 2 or less is easily recovered in the crushing / classifying step.
[0056] In order to suppress oxidation of the molten metal, the atmosphere in the container for the molten metal may be replaced with an inert gas such as argon (Ar) gas. The air pressure in the container for the molten metal may be, for example, 100 kPa or more and 240 kPa or more.
[0057] The cooling roll is installed in the chamber. One cause of the R-rich phase is preferential oxidation of R contained in the surface vicinity of the alloy ribbon. In order to suppress the generation of the R-rich phase due to the oxidation of the molten metal and the alloy ribbon, the atmosphere in the chamber may be replaced with an inert gas such as argon (Ar) gas. For the same reason, the atmosphere in the chamber may contain a reducing gas such as hydrogen gas (H2) in addition to the inert gas. The concentration of hydrogen gas in the atmosphere in the chamber may be, for example, 0.1 mass% or more and 0.5 mass% or less. The reducing property of hydrogen in the atmosphere in the chamber further suppresses the oxidation of the molten metal and the alloy ribbon (the generation of the R-rich phase). Therefore, when the atmosphere in the chamber contains hydrogen, the intervals of the R-rich phases tend to become even larger, and the average interval of the R-rich phases i AVE As the hydrogen concentration in the atmosphere in the chamber increases, the spacing between the R-rich phases tends to become larger, and the average spacing between the R-rich phases i AVEThe pressure inside the chamber may be, for example, 60 kPa or more and 200 kPa or less. The molten metal is not immediately cooled to room temperature on the surface of the chill roll. The temperature of the alloy ribbon immediately after solidification is still high, and the alloy ribbon continues to cool by heat conduction to the housing of the ultra-rapid solidification apparatus and the atmosphere inside the chamber. When the pressure inside the chamber is low (for example, when the pressure inside the chamber is 20 kPa), the heat conduction from the alloy ribbon to the atmosphere inside the chamber is small, and the cooling rate of the alloy ribbon is slow. When the cooling rate is slow, R2T 14 Excessive R relative to the stoichiometric ratio of B is discharged from the inside of the alloy ribbon to the surface. As a result, R becomes excessive near the surface of the alloy ribbon, and oxides of R are likely to form on the surface of the alloy ribbon. The average interval between the R-rich phases i AVE tends to be less than 30 μm. The air pressure inside the container is higher than the air pressure inside the chamber. The difference between the air pressure inside the container and the air pressure inside the chamber is the pressure at which the molten metal is sprayed from the nozzle (the spray pressure differential).
[0058] After the ribbon preparation step, a first transport step is performed. The first transport step is a step of transporting the alloy ribbon produced by the ultra-rapid solidification method to a pulverization / classification device used in the pulverization / classification step. The atmosphere in the first transport step is a non-oxidizing atmosphere. That is, the alloy ribbon is maintained in a non-oxidizing atmosphere from the time when the alloy ribbon is formed to the time when the alloy ribbon reaches the pulverization / classification device. For example, the atmosphere in a transport path communicating from the ultra-rapid solidification device (a chamber in which a cooling roll is installed) to the pulverization / classification device may be a non-oxidizing atmosphere, and the alloy ribbon may be transported in this transport path. The alloy ribbon contained in a container filled with a non-oxidizing atmosphere may be transported from the chamber to the pulverization / classification device. The atmosphere in the first transport step (non-oxidizing atmosphere) may be, for example, an inert gas such as Ar gas. The oxygen concentration in the atmosphere in the first transport step is 0 mass ppm or more and 20 mass ppm or less. The lower the oxygen concentration in the atmosphere in the first conveying step, the less likely the surface of the alloy ribbon is to be oxidized in the first conveying step, and the less likely the R-rich phase originating from the oxidized surface of the alloy ribbon is to be contained in the permanent magnet. As a result, the spacing between the R-rich phases tends to become large, and the average spacing between the R-rich phases i AVE On the other hand, when the oxygen concentration in the atmosphere in the first transport step is higher than 20 mass ppm, the spacing between the R-rich phases tends to become small, and the average spacing between the R-rich phases i AVE tends to be less than 30 μm.
[0059] After the first conveying step, a pulverization / classification step is carried out. The pulverization / classification step is a step of pulverizing the alloy ribbon using a pulverizing device to prepare a coarse powder, and classifying the coarse powder to recover an alloy powder having a predetermined particle size and aspect ratio. The alloy powder is a precursor of the main phase particles contained in the permanent magnet. The shape of each alloy particle constituting the alloy powder may be plate-like or flake-like. The pulverization method of the alloy ribbon may be, for example, at least one method of a cutter mill and a propeller mill. The means for classifying the coarse powder is a sieve. The particle size and particle size distribution of the alloy powder obtained by classification may be measured, for example, by a laser diffraction scattering method. The particle size of the alloy powder obtained by classification may be, for example, 60 μm to 2800 μm, or 150 μm to 2800 μm.
[0060] The average aspect ratio of the alloy powder recovered in the pulverization / classification process is 1 or more and 2 or less. The smaller the average aspect ratio of the alloy powder, the more preferable, and the most preferable average aspect ratio of the alloy powder is 1. When the average aspect ratio of the alloy powder is 1 or more and 2 or less, segregation and aggregation of the R-rich phase are suppressed in the hot compaction process and the hot plastic working process, and the average spacing i of the R-rich phase is reduced. AVE In other words, as the average aspect ratio of the alloy powder decreases, segregation and aggregation of the R-rich phase are suppressed in the hot plastic working process, and the average spacing i AVE For the same reason, it is preferable that the standard deviation σ of the aspect ratio of the alloy powder is as small as possible. For example, the standard deviation σ of the aspect ratio of the alloy powder may be 0 or more and 2 or less.
[0061] If the average aspect ratio of the alloy powder is too large, the shape of each alloy particle is distorted, so that the forces acting on each alloy particle during the hot compaction process and the hot plastic processing process are non-uniform, and each alloy particle is likely to be crushed. At the grain boundaries where the cross sections of each alloy particle created by crushing are located, the liquid phase (R-rich phase) that seeps out from each alloy particle is likely to aggregate. As a result, a large number of R-rich phases are likely to be formed in the permanent magnet, and the average spacing between the R-rich phases i AVEIt is likely to be less than 30 μm. Also, due to the aggregated liquid phase (R-rich phase), abnormal growth of each alloy particle is likely to occur, and coarse primary phase particles are likely to be formed. Due to the dispersion of stress in the compact and the coarsening of the primary phase particles accompanying the aggregation of the liquid phase, it is difficult for the primary phase particles to rotate, and it is difficult for the primary phase particles to be oriented in the direction of the easy magnetization axis. Also, when the average value of the aspect ratio of the alloy powder is too large, since the shape of each alloy particle is distorted, it is difficult for each alloy particle to be densely filled in the compact in the hot forming process and the hot plastic working process, and gaps are likely to occur in the compact. As a result, the residual magnetic flux density is likely to decrease.
[0062] As follows, the average value of the aspect ratio of the alloy powder is controlled by the pore diameter of the nozzle and the sieve used for classifying the coarse powder. The length of the major axis of the flat alloy particles constituting the coarse powder is represented by l (lowercase L). The length of the minor axis of the alloy particle is represented by w. The thickness of the alloy particle is represented by t. l, w, and t satisfy t < w ≤ l. The aspect ratio AR of the alloy particle is represented by l / w. AR is a real number of 1 or more. l may be rephrased as the major diameter of the alloy particle in a direction substantially perpendicular to the thickness direction of the alloy particle. w may be rephrased as the minor diameter of the alloy particle in a direction substantially perpendicular to the thickness direction of the alloy particle. The thickness direction of the alloy particle may correspond to the direction of the minor axis of the primary phase particles in the cross section of the permanent magnet parallel to the easy magnetization axis. The thickness t of the alloy particle may be substantially the same as the thickness of the alloy ribbon, for example, 20 μm or more and 60 μm or less, or 30 μm or more and 50 μm or less. The length w of the minor axis of the alloy particle may be substantially the same as the width of the alloy ribbon, for example, 1.0 mm or more and 5.0 mm or less. In the classification of the coarse powder, a first sieve and a second sieve having a smaller inner diameter (hole diameter) of the opening than that of the first sieve are used. The inner diameter of the opening of the first sieve is represented as D1. In other words, the opening of the first sieve is a square, and the length of one side of the square is D1. The inner diameter of the opening of the second sieve is represented as D2. In other words, the opening of the second sieve is a square, and the length of one side of the square is D2. D2 is smaller than D1. Among the coarse powder obtained by pulverizing the alloy ribbon, the alloy powder that has passed through the first sieve but not the second sieve is collected and used as a material for a permanent magnet. In other words, alloy particles whose major axis length l is equal to or less than D1 and larger than D2 are easily collected between the first sieve and the second sieve. Therefore, each alloy particle constituting the alloy powder collected between the first sieve and the second sieve tends to satisfy the following inequality 1. Since the length l of the major axis of the alloy particle is expressed as w×AR, the following inequality 1 is equivalent to the following inequality 2. The following inequality 3 is derived from the following inequality 2. When the inner diameter D1 of the opening of the first sieve is constant, the following inequality 3 shows that the aspect ratio of the alloy particle tends to increase as the length w of the minor axis of the alloy particle decreases. When the length w of the minor axis of the alloy particle is constant, the following inequality 3 shows that the aspect ratio of the alloy particle tends to increase as the inner diameter D1 of the opening of the first sieve increases. Inequality 3 also shows that the range of the aspect ratio of the alloy particle narrows and the standard deviation σ of the aspect ratio tends to decrease as the difference (D1-D2) between D1 and D2 decreases. D2 <l≦D1 (1) D2 <w×AR≦D1 (2) (D2 / w) <AR≦(D1 / w) (3) For the following reasons, the length w of the minor axis of the alloy particle and the aspect ratio (l / w) of the alloy particle depend on the hole diameter of the nozzle used in the above-mentioned ultra-rapid solidification method. The size of the molten metal (droplets) sprayed from the nozzle is approximately equal to the nozzle hole diameter. The molten metal (droplets) sprayed from the nozzle onto the surface of the chill roll are instantly crushed and spread on the surface of the chill roll. As a result, a flat and elongated alloy ribbon is formed. Therefore, the width of the alloy ribbon tends to be larger than the nozzle hole diameter (droplet size), and the length w of the minor axis of the alloy particles formed by pulverizing the alloy ribbon also tends to be larger than the nozzle hole diameter (droplet size). As the nozzle hole diameter decreases, the droplets become smaller, the alloy ribbon formed from the droplets becomes elongated, and the length w of the minor axis of the alloy particles formed by pulverizing the alloy ribbon tends to decrease. Therefore, the length w of the minor axis of the alloy particle and the aspect ratio (l / w) of the alloy particle can be controlled by the nozzle hole diameter. The length l of the major axis of the alloy particle is less dependent on the nozzle hole diameter than the length w of the minor axis of the alloy particle. The length l of the major axis of the alloy particle can be easily controlled within a desired range by the method and conditions for pulverizing the alloy ribbon. As described above, the aspect ratio of the alloy powder recovered by classification is controlled based on the relationship between the nozzle hole diameter, the length of the minor axis w of the alloy particle, the length of the major axis l of the alloy particle, and the inner diameters of the openings of each sieve (D1 and D2). The alloy powder that does not pass through the first sieve may be reused. For example, the coarse powder that does not pass through the first sieve may be collected and re-pulverized together with the alloy ribbon. The alloy powder that passes through the second sieve may also be reused. For example, the alloy powder that passes through the second sieve may be collected and used as a raw material for the molten metal. The alloy powder that passes through the second sieve may be discarded.
[0063] The average aspect ratio of the alloy powder recovered in the pulverization / classification process may be measured by the following method. Each alloy particle constituting the alloy powder is placed on a flat surface so as not to overlap each other. The flat surface may have adhesiveness to fix each alloy particle. A large number of alloy particles placed on the flat surface are observed by a scanning electron microscope (SEM). The dimensions of the field of view observed by the SEM may be, for example, 1 mm in length x 1 mm in width. The number of alloy particles observed in the field of view observed by the SEM may be, for example, about 100 to 1000. Each alloy particle is plate-like or flake-like, and the thickness t of each alloy particle is smaller than the length l of the major axis and the length w of the minor axis of each alloy particle. Therefore, each alloy particle placed on the flat surface is observed as a two-dimensional shape including the major axis and the minor axis of each alloy particle. The shape of each alloy particle may be approximated by a rectangle that has the smallest area among the rectangles circumscribing each alloy particle. The quadrangle is a rectangle or a square. The length of the short side of this quadrangle is regarded as the length w of the short axis of the alloy particle. The length of the long side of the above quadrangle is regarded as the length l of the long axis of the alloy particle. Based on the above premise, the length l of the long axis and the length w of the short axis of each alloy particle are measured, and the aspect ratio (l / w) of each alloy particle is calculated. The average aspect ratio and the standard deviation of the aspect ratio of the alloy powder are calculated from the aspect ratios of all alloy particles present within the field of view observed by SEM. Commercially available image analysis software may be used to identify the shape (contour line) of each alloy particle and to measure the dimensions of the quadrangle circumscribing each alloy particle.
[0064] Since the specific surface area of the alloy powder is larger than that of the alloy ribbon, the alloy powder is more easily oxidized than the alloy ribbon. (Since the specific surface area of the alloy ribbon is larger than that of a compact formed from the alloy powder, the alloy ribbon is more easily oxidized than the compact.) Furthermore, the smaller the particle size of the alloy powder, the larger the specific surface area of the alloy powder, and the more easily the surface of the alloy powder is oxidized. Due to the oxidation of the alloy powder, a large number of R-rich phases originating from the oxidized surface of the alloy powder are more likely to be contained in the permanent magnet. Therefore, the smaller the particle size of the alloy powder, the more likely the spacing between the R-rich phases is to be smaller, and the average spacing between the R-rich phases i AVEIn other words, the larger the particle size of the alloy powder, the smaller the specific surface area of the alloy powder, and the more the oxidation of the surface of the alloy powder is suppressed. By suppressing the oxidation of the alloy powder, the number of R-rich phases contained in the permanent magnet is reduced. Therefore, the larger the particle size of the alloy powder, the more likely the spacing between the R-rich phases is to become large, and the average spacing between the R-rich phases i AVE tends to be 30 μm or more.
[0065] The atmosphere in the pulverization / classification process is a non-oxidizing atmosphere. By performing the pulverization / classification process in a non-oxidizing atmosphere, oxidation of the alloy ribbon, coarse powder, and alloy powder during the pulverization / classification process is suppressed. As a result, the spacing between the R-rich phases tends to become large, and the average spacing between the R-rich phases i AVE The atmosphere (non-oxidizing atmosphere) in the pulverization / classification process may be, for example, an inert gas such as Ar gas. The oxygen concentration in the atmosphere in the pulverization / classification process is 0 mass ppm or more and 20 mass ppm or less. The lower the oxygen concentration in the atmosphere in the pulverization / classification process, the larger the spacing between the R-rich phases tends to be, and the average spacing between the R-rich phases i AVE On the other hand, when the oxygen concentration in the atmosphere during the grinding / classification process is higher than 20 mass ppm, the spacing between the R-rich phases tends to become small, and the average spacing between the R-rich phases i AVE tends to be less than 30 μm.
[0066] After the pulverization / classification step, a second conveying step is carried out. The second conveying step is a step of conveying the alloy powder obtained by the pulverization / classification step to a forming device used in the hot forming step. The atmosphere of the second conveying step is a non-oxidizing atmosphere. That is, the alloy powder is maintained in a non-oxidizing atmosphere from the time when the alloy powder is formed to the time when the alloy powder reaches the forming device. For example, the atmosphere in the conveying path communicating from the pulverization / classification device to the forming device may be a non-oxidizing atmosphere, and the alloy powder may be conveyed in this conveying path. The alloy powder contained in a container filled with a non-oxidizing atmosphere may be conveyed from the pulverization / classification device to the forming device. The atmosphere of the second conveying step (non-oxidizing atmosphere) may be, for example, an inert gas such as Ar gas. The concentration of oxygen in the atmosphere of the second conveying step is 0 mass ppm or more and 20 mass ppm or less. The lower the oxygen concentration in the atmosphere in the second transport step, the less likely the surface of the alloy powder is oxidized during the second transport step, and the less likely the R-rich phase originating from the oxidized surface of the alloy powder is to be contained in the permanent magnet. As a result, the spacing between the R-rich phases tends to become large, and the average spacing between the R-rich phases i AVE On the other hand, when the oxygen concentration in the atmosphere in the second transport step is higher than 20 mass ppm, the spacing between the R-rich phases tends to become small, and the average spacing between the R-rich phases i AVE tends to be less than 30 μm.
[0067] After the second conveying step, a hot compacting step is carried out. The hot compacting step is a step of forming a compact by pressing the alloy powder while heating it. For example, the alloy powder may be compressed in a die while heating the alloy powder in the die. By pressing the alloy powder, the gaps between the alloy powder are reduced, and a dense compact is obtained. In addition, by heating the alloy powder with pressing, a liquid phase (R-rich phase such as Nd-rich phase) is formed from the surface of the alloy powder, and the liquid phase fills the gaps (grain boundaries) between the alloy powder, and the alloy powder is lubricated by the liquid phase, thereby obtaining a dense compact. A cold compacting step may be carried out before the hot compacting step. In the cold compacting step, a compact may be formed by pressing the alloy powder at room temperature (room temperature). The compact obtained by the cold compacting step may be densified by pressing the compact while heating it in the hot compacting step. The temperature of the alloy powder in the hot compacting step (hot compacting temperature) may be, for example, 700°C or more and 800°C or less. If the hot compaction temperature is too low, a sufficient liquid phase is not formed on the surface of the alloy powder, and the compact is difficult to densify. If the hot compaction temperature is too high, the crystals (R2T 14 B) grain growth proceeds excessively, and the coercive force of the permanent magnet is likely to decrease. The pressure applied to the alloy powder in the hot compacting step (hot compacting pressure) may be 50 MPa or more and 200 MPa or less. The time during which the combined hot compacting temperature and hot compacting pressure are maintained within the above ranges (hot compacting time) may be, for example, several tens of seconds or more and several hundreds of seconds or less.
[0068] In order to suppress oxidation of the alloy powder and the compact in the hot compacting step, the hot compacting step may be performed in a non-oxidizing atmosphere. The atmosphere in the hot compacting step (non-oxidizing atmosphere) may be, for example, an inert gas such as Ar gas. The oxygen concentration in the atmosphere in the hot compacting step may be, for example, 0 mass ppm or more and 20 mass ppm or less.
[0069] After the hot forming step, a third conveying step is carried out. The third conveying step is a step of conveying the compact obtained by the hot forming step to a forming device used in the hot plastic working step. In order to suppress oxidation of the compact, the atmosphere in the third conveying step may be a non-oxidizing atmosphere. That is, the compact may be maintained in a non-oxidizing atmosphere from the time when the compact is formed to the time when the compact reaches the forming device for hot plastic working. For example, the atmosphere in the conveying path communicating from the forming device for hot forming to the forming device for hot plastic working may be a non-oxidizing atmosphere, and the compact may be conveyed in this conveying path. The compact contained in a container filled with a non-oxidizing atmosphere may be conveyed from the forming device for hot forming to the forming device. The atmosphere in the third conveying step may be, for example, an inert gas such as Ar gas. Since the specific surface area of the compact formed from the alloy powder is significantly smaller than the specific surface areas of the alloy powder and the alloy ribbon, the compact (particularly the inside of the compact) is less likely to be oxidized than the alloy powder and the alloy ribbon. Therefore, even if the oxygen concentration in the atmosphere in the third conveying step is higher than the oxygen concentration in the atmosphere in each of the first conveying step and the second conveying step, the average interval i AVE For example, even when the atmosphere in the third conveying step is air, the average interval between the R-rich phases i can be controlled to 30 μm or more by reducing the oxygen concentration in the atmosphere in each of the first conveying step and the second conveying step. AVE The oxygen concentration in the atmosphere in the third transport step may be 0 ppm by mass or more and 200,000 ppm by mass or less, preferably 0 ppm by mass or more and 2,000 ppm by mass or less, and more preferably 0 ppm by mass or more and 20 ppm by mass or less.
[0070] After the third conveying step, a hot plastic working step is carried out. In the hot plastic working step, a plurality of main phase grains (R2T) whose c-axes (axis of easy magnetization) are oriented in a predetermined direction are formed by hot extrusion of the compact obtained by the hot forming step. 14This is a process for obtaining a magnet base material containing R-rich phase (crystal grains of R). For example, in the hot plastic working process, the compact is extruded from a die while being heated. In the die, the grain boundary phase in the heated compact liquefies to generate a liquid phase (R-rich phase), and stress acts on the compact in a predetermined direction, distorting each alloy particle constituting the compact. With the generation of the liquid phase and the distortion of the alloy particles, anisotropic growth of the crystal grains in a direction perpendicular to the c-axis of the crystal grains progresses. In addition, the liquid phase lubricates each crystal grain, and a force acts on each crystal grain according to the stress. As a result, the crystal grains rotate due to grain boundary sliding, and the c-axis of each crystal grain (main phase particle) is oriented approximately parallel to the stress direction. In other words, a plurality of flat main phase particles extending in a direction approximately perpendicular to the c-axis are stacked along the stress direction. The temperature of the formed body in the hot plastic working step (hot plastic working temperature) may be, for example, 700°C or more and less than 900°C, or 700°C or more and 850°C or less. If the hot plastic working temperature is too low, liquid phases (R-rich phases such as Nd-rich phases) are unlikely to form at the grain boundaries in the compact, crystal grains are unlikely to grow, and crystal grain rotation due to grain boundary sliding is unlikely to occur. As a result, the average length of the minor axis of the main phase grains is likely to be less than 20 nm, and the c-axis of each main phase grain (crystal grain) is unlikely to be oriented approximately parallel to the stress direction. If the hot plastic working temperature is too high (for example, if the hot plastic working temperature is 900°C or higher), the liquid phase (R-rich phase) will exude excessively from each alloy particle and segregate to the surface of each alloy particle and the interface between the alloy particles, and most of the liquid phase will be consumed for grain growth. As a result, the frequency of R-rich phase generation in the AB direction will decrease, and the average interval between the R-rich phases will decrease. AVE In addition, most of the liquid phase is consumed by the growth of the crystal grains, so that the grain growth of the main phase particles (crystal grains) proceeds abnormally, and coarse main phase particles are likely to be formed, with the average length of the minor axis of the main phase particles easily exceeding 200 nm. The coarse main phase particles are difficult to orient in the direction of the easy axis of magnetization. The extrusion speed for hot extrusion molding is 10 -2The extrusion speed may be from 10 mm / sec to 9.9 mm / sec. If the extrusion speed is too high (for example, if the extrusion speed is 10 mm / sec or higher), the anisotropic growth of the main phase particles (crystal grains) in the compact does not proceed sufficiently, and the average length of the minor axis of the main phase particles (primary particles) is likely to be less than 20 nm. In other words, if the extrusion speed is too high, the compact is extruded from the die before the anisotropic growth of the crystal grains in the compact proceeds sufficiently. As a result, it is difficult for the c-axis of each main phase particle (crystal grain) to be oriented approximately parallel to the stress direction. The pressure applied to the compact in the hot plastic working step (hot plastic working pressure) may be 50 MPa or more and 200 MPa or less. The time during which the hot plastic working temperature and the hot plastic working pressure are maintained within the above ranges (hot plastic working time) may be, for example, several tens of seconds.
[0071] In order to suppress oxidation of the compact and the magnet substrate in the hot plastic working process, the hot plastic working process may be performed in a non-oxidizing atmosphere. The atmosphere in the hot plastic working process (non-oxidizing atmosphere) may be, for example, an inert gas such as Ar gas. The oxygen concentration in the atmosphere in the hot plastic working process may be, for example, 0 ppm by mass or more and 20 ppm by mass or less.
[0072] The magnet base material obtained by the above steps may be a finished permanent magnet. The magnet base material that has been subjected to the grain boundary diffusion step described below may be a finished permanent magnet.
[0073] After the hot plastic working process, the following grain boundary diffusion process may be performed. The grain boundary diffusion process is a process in which a diffusion material containing a heavy rare earth element is attached to the surface of the magnet base material, and the diffusion material and the magnet base material are heated. By heating the magnet base material to which the diffusion material is attached, the heavy rare earth element in the diffusion material diffuses from the surface of the magnet base material to the inside of the magnet base material. Inside the magnet base material, the heavy rare earth element diffuses through the grain boundaries to the vicinity of the surface of the main phase particles. In the vicinity of the surface of the main phase particles, some of the light rare earth elements (Nd, etc.) are replaced with the heavy rare earth element. By localizing the heavy rare earth element in the vicinity of the surface and at the grain boundaries of the main phase particles, the anisotropic magnetic field becomes locally large in the vicinity of the grain boundaries, and nuclei of magnetization reversal are less likely to occur in the vicinity of the grain boundaries. As a result, a permanent magnet with high coercive force is obtained. In the grain boundary diffusion process, each element contained in the diffusion material is diffused uniformly to each grain boundary and each crystal grain surface in the magnet base material. In addition, the grain boundary phase formed by each element derived from the thermal diffusion material is finer than the R-rich phase caused by oxidation, and is difficult to detect during measurement of the spacing between the R-rich phases. Therefore, each element derived from the diffusion material is unlikely to affect the spacing between the R-rich phases.
[0074] In order to suppress oxidation of the magnet base material in the grain boundary diffusion step, the grain boundary diffusion step may be performed in a non-oxidizing atmosphere. The atmosphere in the grain boundary diffusion step (non-oxidizing atmosphere) may be, for example, an inert gas such as Ar gas. The oxygen concentration in the atmosphere in the grain boundary diffusion step may be, for example, 0 mass ppm or more and 20 mass ppm or less. The atmospheric pressure in the grain boundary diffusion step may be, for example, 50 kPa or more and 120 kPa or less. The temperature (diffusion temperature) of the diffusion material and the magnet base material in the grain boundary diffusion step may be, for example, 550°C or more and 900°C or less. The time (diffusion time) during which the diffusion temperature is held in the above range may be, for example, 1 minute or more and 1440 minutes or less.
[0075] The diffusion material may contain at least one heavy rare earth element selected from Tb and Dy. The diffusion material may further contain at least one light rare earth element selected from Nd and Pr in addition to the heavy rare earth element. The diffusion material may further contain Cu in addition to the heavy rare earth element and the light rare earth element. The diffusion material may be, for example, a metal consisting of one of the above elements, a hydride of one of the above elements, an alloy containing a plurality of the above elements, or a hydride of the alloy. The diffusion material may be a powder. In the grain boundary diffusion process, a slurry containing the diffusion material and an organic solvent may be applied to the surface of the magnet base material. In the grain boundary diffusion process, the surface of the magnet base material may be covered with a sheet containing the diffusion material and a binder. In the grain boundary diffusion process, the surface of the magnet base material may be covered with an alloy foil (ribbon) composed of the diffusion material.
[0076] In order to promote diffusion of the diffusion material, the surface of the magnet base material may be polished before the grain boundary diffusion step. In order to remove the diffusion material remaining on the surface of the magnet base material after the grain boundary diffusion step, the surface of the magnet base material may be polished after the grain boundary diffusion step.
[0077] The size and shape of the magnet substrate may be adjusted by cutting and polishing the magnet substrate. A passive layer may be formed on the surface of the magnet substrate by oxidation or chemical treatment of the surface of the magnet substrate. The surface of the magnet substrate may be covered with a protective film such as a resin film. The passive layer or protective film improves the corrosion resistance of the permanent magnet.
[0078] The present invention is not necessarily limited to the above-described embodiment. Various modifications of the present invention are possible without departing from the spirit of the present invention, and these modifications are also included in the present invention. EXAMPLES
[0079] The present invention will be described in detail with reference to the following examples and comparative examples, but the present invention is not limited to the following examples.
[0080] <Making permanent magnets> Example 1 In the ribbon production process, alloy ribbons were produced from the raw alloy by the ultra-rapid solidification method. The raw metal (molten metal) used in the ribbon production process contained Nd, Fe, Co, Ga, Al, and B. The Nd content in the raw material metal was 30.17 mass %. The Co content in the raw material metal was 3.96 mass %. The Ga content in the raw material metal was 0.59 mass %. The Al content in the raw material metal was 0.04 mass %. The B content in the raw material metal was 0.97 mass %. The balance of the raw material metals other than Nd, Co, Ga, Al and B was Fe.
[0081] The temperature of the molten metal sprayed from the nozzle (spray temperature) was 1400°C. The heating rate until the temperature of the raw metal reached the spray temperature was 100°C / sec. The cooling rate of the molten metal on the surface of the chill roll was about 10 5The temperature was controlled at 50° C. / sec. The peripheral speed of the cooling roll was 40 m / sec. The nozzle hole diameter was the value shown in Table 1 below.
[0082] The gas in the nozzle (the atmosphere in the container of the molten metal) was Ar. The pressure in the nozzle (the atmospheric pressure in the container of the molten metal) was 100 kPa.
[0083] The gas (atmosphere) in the chamber in which the cooling roll was placed was Ar. The concentration of hydrogen gas in the atmosphere in the chamber was 0.00 mass %. The pressure in the chamber (air pressure in the chamber) was 60 kPa. The injection differential pressure was 40 kPa.
[0084] In the first transport step after the ribbon preparation step, the alloy ribbon was transported from the ultra-rapid solidification device to the crushing / classifying device. The gas (atmosphere) in the first transport step was Ar. The oxygen concentration in the atmosphere in the first transport step was 20 ppm by mass.
[0085] In the crushing / classification step after the first conveying step, the alloy ribbon was crushed and classified to recover alloy powder having a predetermined aspect ratio. The inner diameter D1 of the opening of the first sieve used for classification was the value shown in Table 1 below. The inner diameter D2 of the opening of the second sieve used for classification was the value shown in Table 1 below. The average aspect ratio AR of the recovered alloy powder AVE The average aspect ratio of the recovered alloy powder, AR, was measured by the method described above. AVE The standard deviation σ of the aspect ratio of the alloy powder was the value shown in Table 1 below.
[0086] The gas (atmosphere) in the pulverization / classification process was Ar. The oxygen concentration in the atmosphere in the pulverization / classification process was 20 ppm by mass.
[0087] In the second conveying step after the pulverization / classification step, the alloy powder was conveyed from the pulverization / classification device to the molding device. The gas (atmosphere) in the second conveying step was Ar. The oxygen concentration in the atmosphere in the second conveying step was 20 mass ppm.
[0088] In the hot forming step after the second conveying step, the alloy powder was compressed in a die while the alloy powder in the die was heated, to produce a compact. The compact was a thin plate. The length of the compact was 80 mm, the width of the compact was 22 mm, and the thickness of the compact was 11 mm. The hot forming temperature was 750°C. The hot forming pressure was 100 MPa. The hot forming time was 300 seconds. The gas (atmosphere) in the hot forming step was Ar. The oxygen concentration in the atmosphere in the hot forming step was 20 ppm by mass.
[0089] In the third conveying step after the hot forming step, the compact was conveyed from the hot forming device to the hot plastic working device. The gas (atmosphere) in the third conveying step was Ar. The oxygen concentration in the atmosphere in the third conveying step was 20 mass ppm.
[0090] After the third conveying step, a hot plastic processing step was carried out. The die used in the hot plastic processing step (hot extrusion molding of the molded body) was cylindrical. That is, the cavity of the die penetrates the die from the end face (starting end face) of the die where the inlet for the molded body opens to the end face (terminal end face) of the die where the extrusion port for the molded body opens. The starting end face and the terminal end face are planes parallel to each other. The direction from the starting end face to the terminal end face is the extrusion direction of the molded body, and the extrusion direction is perpendicular to the starting end face and the terminal end face. The opening area of the extrusion port of the molded body is smaller than the opening area of the inlet of the molded body. The cavity is divided into an inlet region, an intermediate region, and an extrusion outlet region along the extrusion direction. The inlet region opens at the starting end face. The extrusion outlet region opens at the terminal end face. The intermediate region is located between the inlet region and the extrusion outlet region in the extrusion direction. The shape of the cavity in the cross section of the die perpendicular to the extrusion direction (the cross section of the die parallel to the starting and ending faces) is a quadrilateral with all four corners being right angles. A pair of opposing sides of this quadrilateral is referred to as the first sides, and the other pair of opposing sides of the quadrilateral is referred to as the second sides. The length of each of the first side and the second side in the inlet side region is constant. That is, the opening area of the inlet side region in the cross section perpendicular to the extrusion direction is constant. In the middle region, the length of the first side gradually decreases along the extrusion direction, and finally coincides with the length of the first side in the extrusion port side region. Therefore, the first side in the extrusion port side region is shorter than the first side in the inlet side region. Also, in the middle region, the length of the second side gradually increases along the extrusion direction, and finally coincides with the length of the second side in the extrusion port side region. Therefore, the second side in the extrusion port side region is longer than the second side in the inlet side region. Furthermore, the opening area of the middle region in the cross section perpendicular to the extrusion direction gradually decreases along the extrusion direction, and finally coincides with the opening area of the extrusion port side region in the cross section perpendicular to the extrusion direction. Therefore, the opening area of the extrusion port side region in the cross section perpendicular to the extrusion direction is smaller than the opening area of the inlet side region in the cross section perpendicular to the extrusion direction. The length of each of the first side and the second side in the extrusion port side region is constant. In other words, the opening area of the extrusion port side region in a cross section perpendicular to the extrusion direction is constant. The length of the first side in the inlet side region (starting end face) was 22 mm, and the length of the second side in the inlet side region (starting end face) was 11 mm. The length of the first side in the extrusion outlet side region (terminal end face) was 7 mm, and the length of the second side in the extrusion outlet side region (terminal end face) was 30 mm. The length of the inlet side region in the extrusion direction was 80 mm. The length of the intermediate region in the extrusion direction was 20 mm. The length of the extrusion outlet side region in the extrusion direction was 20 mm. As described above, the opening area of the extrusion port side region in a cross section perpendicular to the extrusion direction is smaller than the opening area of the inlet side region in a cross section perpendicular to the extrusion direction, and the first side in the outlet side region (terminal end face) is shorter than the second side in the extrusion port side region (terminal end face). Therefore, in the extrusion port side region, stress approximately parallel to the first side acts on the compact, causing grain boundary sliding and rotation of the main phase particles. As a result, the c-axes of the main phase particles are oriented along the stress direction (direction of the first side). In other words, the magnetization easy axis direction of the magnet base material obtained by hot extrusion molding is the direction of the first side in the extrusion port side region (terminal end face).
[0091] In the hot plastic working step, the above molded body was hot extrusion molded to produce a magnet base material. The temperature at the inlet of the mold was the value shown in Table 1 below. The temperature at the extrusion port (outlet) of the mold was the value shown in Table 1 below. The hot plastic working pressure was 100 MPa. The extrusion speed of the hot extrusion molding was the value shown in Table 1 below.
[0092] The gas (atmosphere) in the hot plastic working process was Ar. The oxygen concentration in the atmosphere in the hot plastic working process was 20 ppm by mass.
[0093] In the grain boundary diffusion process after the hot plastic working process, the magnet base material with the diffusion material attached thereto was heated. The diffusion material was a hydride powder of a eutectic alloy consisting of Nd, Tb, and Cu. In the grain boundary diffusion process, a slurry, which was a mixture of the diffusion material and an organic solvent, was applied to the entire surface of the magnet base material. The Nd content in the diffusion material was 60 mass %. The Tb content in the diffusion material was 20 mass %. The Cu content in the diffusion material was 20 mass %. The mass of the diffusion material attached to the magnet base material was adjusted so that the Tb content in the permanent magnet (magnet base material after the grain boundary diffusion process) was equal to 2 mass %.
[0094] The gas (atmosphere) in the grain boundary diffusion step was Ar. The pressure in the grain boundary diffusion step (atmospheric pressure in the grain boundary diffusion step) was 100 kPa. The diffusion temperature was 700° C. The diffusion time was 300 minutes.
[0095] By the above method, the permanent magnet of Example 1 was produced.
[0096] (Examples 2 to 9 and Comparative Examples 1 to 12) The nozzle hole diameters of Examples 2 to 9 and Comparative Examples 1 to 12 were the values shown in Table 1 below. The inner diameter D1 of the openings of the first sieve in each of Examples 2 to 9 and Comparative Examples 1 to 12 was the value shown in Table 1 below. The inner diameter D2 of the openings of the second sieve in each of Examples 2 to 9 and Comparative Examples 1 to 12 was the value shown in Table 1 below. The average aspect ratio AR of each of the alloy powders in Examples 2 to 9 and Comparative Examples 1 to 12 AVE The values were as shown in Table 1 below. The standard deviation σ of the aspect ratio of each of the alloy powders in Examples 2 to 9 and Comparative Examples 1 to 12 was the value shown in Table 1 below. The temperature at the inlet of the die in the hot plastic working step in each of Examples 2 to 9 and Comparative Examples 1 to 12 was the value shown in Table 1 below. The temperature of the extrusion port (outlet) of the die in the hot plastic working step in each of Examples 2 to 9 and Comparative Examples 1 to 12 was the value shown in Table 1 below. The extrusion speeds of the hot extrusion molding in each of Examples 2 to 9 and Comparative Examples 1 to 12 were the values shown in Table 1 below. The permanent magnets of Examples 2 to 9 and Comparative Examples 1 to 12 were each produced in the same manner as in Example 1, except for the various production conditions shown in Table 1 below.
[0097] <Analysis of permanent magnets> (Composition and microstructure of permanent magnets) The cross-sections of the permanent magnets of all the examples and comparative examples were observed by a scanning electron microscope (SEM). The cross-sections of the permanent magnets observed were parallel to the magnetization easy axis of each permanent magnet. The composition of the cross-sections of each permanent magnet was also analyzed by an electron probe microanalyzer (EPMA) and an energy dispersive X-ray spectroscopy (EDS) device. In all the examples and comparative examples, the permanent magnets were composed of a number of main phase particles (NdFe 14 In all the examples and comparative examples, each main phase grain observed in the cross section was flat, and multiple flat main phase grains were stacked along the easy axis direction. In all the examples and comparative examples, each R-rich phase was located between multiple main phase grains. At least a portion of the R-rich phase was located between multiple main phase grains aligned along the AB direction. In all the examples and comparative examples, a portion of the R-rich phase contained an oxide of Nd.
[0098] A backscattered electron image of a part of a cross section of the permanent magnet of Example 2 is shown in FIG. 3. The five backscattered electron images in FIG. 3 are identical. The backscattered electron images were taken by SEM. The cross section on which the backscattered electron images were taken was parallel to the easy axis direction of magnetization.
[0099] In each of the measurement regions A(a), A(b), A(c), A(d) and A(e) in FIG. 3, the luminance distribution was measured along the AB direction. The width of each measurement region in the AB direction was 400 μm. The width of each measurement region in the direction of the easy axis of magnetization C was 15 μm. In each measurement region, the average value of the spacing between the R-rich phases in the AB direction was measured based on the luminance distribution. The average values of the spacing between the R-rich phases in each of the five measurement regions were further averaged to obtain the average spacing between the R-rich phases in the AB direction, i AVE The details of the measurement method for the luminance distribution and the interval between the R-rich phases were as described in the above embodiment.
[0100] A backscattered electron image of a portion of the cross section of the permanent magnet of Comparative Example 8 is shown in FIG. 4. The five backscattered electron images in FIG. 4 are identical. The backscattered electron images were taken by SEM. The cross section on which the backscattered electron images were taken was parallel to the easy axis direction of magnetization. In each of the measurement areas A'(a), A'(b), A'(c), A'(d), and A'(e) in FIG. 4, the brightness distribution was measured along the AB direction. Then, in the same manner as in Example 2, the average spacing of the R-rich phase in Comparative Example 8, i AVE was obtained.
[0101] In the same manner as in Example 2, the average value i of the spacing between the R-rich phases in all the examples and comparative examples was AVE The average value i of the spacing between the R-rich phases in each of Examples 1 to 9 and Comparative Examples 11 to 12 was obtained. AVE is shown in Table 1 below.
[0102] (Main phase particle size) A backscattered electron image of the cross section of the permanent magnet of Example 2 was taken by SEM. The cross section on which the backscattered electron image was taken was parallel to the easy axis direction of magnetization. The dimensions of the backscattered electron image were 88 μm in length and 126 μm in width. A number of representative locations in the backscattered electron image were selected, and the backscattered electron images of each location were taken at high magnification. The lengths of the major and minor axes of the main phase particles (primary particles) present in the high-magnification backscattered electron image were measured. The shape of each main phase particle was approximated by a rectangle with the smallest area among the rectangles circumscribing the main phase particle. The length of the long side of this rectangle was considered to be the length of the major axis of the main phase particle, and the length of the short side of the rectangle was considered to be the length of the minor axis of the main phase particle. The average value Lab of the lengths of the major axes of all the main phase particles present in the high-magnification backscattered electron image was calculated. The average value Lc of the lengths of the minor axes of all the main phase particles present in the high-magnification backscattered electron image was calculated.
[0103] The lengths of the major and minor axes of the main phase particles of all the examples and comparative examples were measured in the same manner as in Example 2. The average values Lc of the minor axis lengths of the main phase particles (primary particles) of each of the examples 1 to 9 and comparative examples 11 to 12 are shown in Table 1 below.
[0104] The minimum value of the average major axis length Lab of the main phase particles (primary particles) in each Example was about 100 nm.The maximum value of the average major axis length Lab of the main phase particles (primary particles) in each Example was about 1000 nm.
[0105] (Magnetic properties of permanent magnets) The remanence (Br), coercivity (HcJ) and squareness (Hk / HcJ) of the permanent magnets of all the examples and comparative examples were measured. The remanence, coercivity and squareness were measured using a BH tracer. The coercivity was measured at 23°C and 150°C. Br was measured at room temperature. The squareness was measured at 23°C. The temperature coefficient β of the coercivity of each of the examples and comparative examples was calculated. The temperature coefficient β is defined by the following equation 4. HcJ in the following equation 4 150 is the coercive force at 150°C. 23 is the coercive force at 23°C. β = 100 × (HcJ150 -HcJ 23 ) / HcJ 23 (150-23) (4)
[0106] The measured magnetic properties of the permanent magnets described above are shown in Table 1 below.
[0107] [Table 1] [Industrial Applicability]
[0108] The R-T-B system permanent magnet according to the present invention is suitable, for example, as a material for motors mounted on electric vehicles or hybrid vehicles. [Explanation of symbols]
[0109] 2... R-T-B system permanent magnet, 2cs... cross section of permanent magnet, 4... main phase particle (primary particle), 4a... secondary particle, 6... R-rich phase, C... direction of easy magnetization axis, AB... direction approximately perpendicular to the direction of easy magnetization axis.
Claims
1. An R-T-B system permanent magnet containing a rare earth element R, a transition metal element T and B, The R-T-B system permanent magnet contains at least Nd as R, The R-T-B system permanent magnet contains at least Fe as T, The R-T-B system permanent magnet comprises a plurality of main phase grains and a plurality of R-rich phases, The main phase grains contain at least R, T, and B, The R-rich phase contains at least R, the main phase grains observed in a cross section of the R-T-B system permanent magnet are flat, the cross section is approximately parallel to the magnetization easy axis direction of the R-T-B system permanent magnet, The R-rich phase is located between a plurality of the main phase particles, an average spacing between the R-rich phases in a direction substantially perpendicular to the easy axis direction is 30 μm or more and 1000 μm or less; the average value of the length of the minor axis of the main phase grains observed in the cross section is 20 nm or more and 200 nm or less; R-T-B series permanent magnet.
2. The content of R is 28% by mass or more and 33% by mass or less, The content of B is 0.8% by mass or more and 1.1% by mass or less. The R-T-B system permanent magnet according to claim 1 .
3. A plurality of the flat main phase grains are stacked along the direction of the easy axis of magnetization. The R-T-B system permanent magnet according to claim 1 or 2.
4. Hot processed magnets, The R-T-B system permanent magnet according to any one of claims 1 to 3.
5. The concentration of R in the R-rich phase is higher than the average value of the concentration of R in the cross section, The unit of the concentration of R is atomic %. The R-T-B system permanent magnet according to any one of claims 1 to 4.
6. the concentration of R in the R-rich phase is higher than the concentration of R in the main phase grains, The unit of the concentration of R is atomic %. The R-T-B system permanent magnet according to any one of claims 1 to 5.
Citation Information
Patent Citations
Method of manufacturing r-t-b based rare earth magnet
JP2010027852A
Rare earth based alloy and method for manufacturing the same
JP2013111599A
JP2016‐96203A
Raw material alloy for r-t-b-based magnet
WO2014174795A1