Method for preparing copper-based hydrogenation catalyst, catalyst prepared therefrom and use thereof
A copper-based catalyst using activated carbon and lithium improves bonding strength and dispersion, addressing catalyst deactivation and by-product formation issues, achieving high activity and selectivity for α-phenylethyl alcohol production.
Patent Information
- Application Number
- JP2023501600
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-07-13
- Filing Date
- 2021-03-11
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2041-03-11
AI Technical Summary
Existing hydrogenation catalysts for acetophenone suffer from low bonding strength between the catalyst active component and the support, catalyst deactivation due to active component loss, non-uniform dispersion, and high formation of by-products such as ethylbenzene and styrene, particularly at elevated temperatures.
A copper-based catalyst is prepared using activated carbon as a carrier and metallic lithium as an auxiliary agent through an ion exchange method, enhancing the catalyst's skeletal strength, pore size distribution, and active component dispersion, while suppressing side reactions with the addition of lithium to improve alkalinity and stability.
The catalyst exhibits high activity, long-term stability, and reduced formation of by-products, with excellent low-temperature performance and improved selectivity for α-phenylethyl alcohol production.
Smart Images

Figure 0007594082000001 
Figure 0007594082000002
Abstract
Description
[Technical field]
[0001] The present application relates to the technical field of catalytic hydrogenation, specifically to a catalyst for hydrogenating acetophenone liquid phase to prepare α-phenylethyl alcohol, its preparation method and use. [Background technology]
[0002] α-Phenylethyl alcohol is an important chemical intermediate and is widely used in pharmaceutical, fragrance, cosmetics, food, fine chemicals, etc. Current methods for synthesizing α-phenylethyl alcohol mainly include microbial fermentation and acetophenone reduction / catalytic hydrogenation.
[0003] Microbial fermentation generally uses phenylalanine and fluorophenylalanine as raw materials to prepare α-phenylethyl alcohol by microbial fermentation conversion. The raw materials used in microbial fermentation are expensive, and the production cost is high. At present, the acetophenone hydrogenation method is generally used to prepare industrial α-phenylethyl alcohol, which has the advantages of low production cost, few by-products, high product yield, high product purity, etc., and is suitable for mass production of α-phenylethyl alcohol.
[0004] Acetophenone hydrogenation catalysts mainly include platinum palladium precious metal catalysts, nickel catalysts and copper catalysts, and precious metal catalysts and nickel catalysts are expensive, prone to aromatic ring saturation and hydrogenolysis of phenylethyl alcohol, and poor selectivity for α-phenylethyl alcohol. Compared with precious metal catalysts and nickel catalysts, copper catalysts have the advantages of high activity, selectivity, and low cost when used in the hydrogenation reaction of acetophenone, but still have problems such as low catalytic strength, poor stability, easy to lose active components, and easy to cause hydrogenolysis / dehydration side reactions (hydrogenolysis / dehydration side reactions of α-phenylethyl alcohol occur during the hydrogenation of acetophenone, which is easy to generate ethylbenzene / styrene, and the rate of hydrogenolysis and dehydration reaction both increases rapidly with the increase in reaction temperature).
[0005] In Patent Document 1, Ni-Sn-B / SiO2 catalyst is prepared by the impregnation method, and after low-temperature calcination, KBH4 is reduced as a reducing agent. During the catalytic reaction, the maximum selectivity of phenylethyl alcohol reaches 97.5%, but the interaction between the active component Ni and the support SiO2 is weak and it is easily washed away.
[0006] Patent Document 2 discloses a Pd-C catalyst, but the catalyst has poor stability and requires constant increase in reaction temperature during application.
[0007] Patent Document 3 discloses a reduced copper catalyst and a method for preparing α-phenylethyl alcohol using the same, but the method requires a liquid-phase reduction method to improve the stability of the catalyst, which makes the process complicated and expensive.
[0008] Patent Document 4 discloses a method for preparing α-phenylethyl alcohol using Raney nickel as a catalyst. However, in the hydrogenation product of acetophenone in this method, the aromatic ring hydrogenation product α-cyclohexylethanol is present in large amounts, and the selectivity for α-phenylethyl alcohol is low.
[0009] Therefore, it is of great significance to solve the problems in the prior art, such as the low binding strength between the catalytic active component and the support, the deactivation of the catalyst due to the loss of the active component, and the uneven dispersion of the active component, to improve the low-temperature activity of the copper-based hydrogenation catalyst, to improve the dispersibility of copper in the catalyst, to reduce the loss of the active component, to improve the strength of the catalyst, to suppress the production of by-products, and to prepare a highly active and highly selective acetophenone hydrogenation catalyst. [Prior art documents] [Patent documents]
[0010] [Patent Document 1] China Patent Application Publication No. 1557545 [Patent Document 2] U.S. Pat. No. 4,996,374 [Patent Document 3] China Patent Publication No. 1315226 [Patent Document 4] China Patent Publication No. 1911883 Summary of the Invention [Problem to be solved by the invention]
[0011] The following is a summary of the subject matter described in detail in the present text, which is not intended to limit the scope of protection of the claims.
[0012] The object of the present application is to solve the above problems in the prior art and provide a method for preparing a copper-based catalyst for hydrogenating acetophenone in liquid phase to prepare α-phenylethyl alcohol, and the prepared catalyst. [Means for solving the problem]
[0013] The copper catalyst of the present invention is prepared by ion exchange method using activated carbon as a carrier and metallic lithium as an auxiliary agent. The obtained catalyst has excellent skeletal strength and pore size distribution, good mass transfer and heat transfer effects, and also has the advantages of high activity, high dispersion of active components, high sintering resistance, and low loss of active components.
[0014] When the catalyst described in the present application is used for preparing α-phenylethyl alcohol by hydrogenating acetophenone in liquid phase, the catalyst has better low-temperature activity and can significantly reduce the generation of by-products. In particular, by adding lithium element, Cu-Li, as an auxiliary agent to the composition, the alkalinity of the catalyst can be improved, and the hydrogenolysis / dehydration side reaction can be effectively inhibited, and the catalyst has the advantages of long-term stability.
[0015] In one aspect of the present application to achieve the above object, the following technical solution is adopted. The method for preparing the catalyst is as follows: (1) a step of immersing activated carbon in an acid solution, followed by separation and washing; Step (2) of immersing the activated carbon treated in step (1) in an alkaline solution, then separating, washing and drying; The activated carbon treated in step (2) is immersed in an ethanol-water mixed solution containing a copper salt and a lithium salt for aging, and then separated, washed, dried and calcined to obtain a copper-based hydrogenation catalyst (3).
[0016] In step (1) of the preparation method of the present application, the acid solution is an aqueous solution of acid, the concentration of which is 0.5-2 mol / L, preferably 0.8-1.5 mol / L, and the acid is one or more selected from nitric acid, hydrochloric acid, and sulfuric acid, preferably nitric acid. A low acid concentration directly affects the number of groups on the support surface. In addition, the acid solution can also remove impurities present in the support itself, so a low acid concentration will leave impurities behind, which will affect the activity and selectivity of the catalyst. Conversely, a high acid concentration will destroy the support and affect the service life of the support.
[0017] In step (1) of the preparation method of the present application, the activated carbon is either coconut shell charcoal or wood charcoal, and its iodine value is 600-1500, preferably 800-1300, and its particle size is 4-60 mesh, preferably 8-16 mesh. The iodine value of the activated carbon is considered through experiments. A reasonable iodine value range in the present application is advantageous for promoting the progress of the hydrogenation reaction, but is disadvantageous to the reaction performance and physical performance of the catalyst.
[0018] In step (1) of the preparation method of the present application, the conditions of the immersion treatment are atmospheric pressure excess immersion, the immersion temperature is 80-140°C, preferably 90-130°C, and the time is 2-8h, preferably 3-6h. In the immersion treatment process, there is no specific requirement for the amount of acid solution used in this step, as long as the activated carbon carrier is completely immersed. The immersion temperature mainly promotes the formation of organic functional groups on the carrier surface, and a low or high temperature is disadvantageous.
[0019] In step (1) of the preparation method of the present application, the subsequent separation and washing after the soaking treatment can be performed by normal operating methods, and there are no specific requirements. In some embodiments, the separation can be performed by centrifugal separation, and the washing can be performed by water washing. The soaking treatment of the activated carbon carrier with an acid solution in step (1) can remove impurities from the activated carbon, while the purpose is to modify the oxygen-containing functional groups on the surface of the activated carbon. The activated carbon itself is an inert material with few surface functional groups. After high-temperature oxidation treatment in the acid solution, the oxygen-containing groups, such as functional groups such as -COOH, are increased on the surface of the activated carbon, which is then modified and ready for the next modification.
[0020] In step (2) of the preparation method of the present application, the alkaline solution is an alkaline water solvent containing an ammonium salt, the concentration of which is 2-10 wt%, preferably 3-8 wt%, and the ammonium salt is selected from ammonium carbonate and / or ammonium hydrogen carbonate.
[0021] In step (2) of the preparation method of the present application, the immersion treatment is carried out under normal pressure overdose conditions, the temperature is 20-60°C, preferably 30-50°C, and the immersion time is 2-8h, preferably 3-6h. In the immersion treatment process, the amount of alkaline solution used in this step is not specifically required as long as the activated carbon carrier is completely immersed, but it is necessary to ensure that the solution has a sufficient content of ions to exchange the functional groups generated by the acid-treated carrier in step (1). In step (2), the surface of the activated carbon carrier is modified using an ammonium salt to form NH 4+ The oxygen-containing functional groups modified in the first step are replaced with ions, e.g., -COOH is converted to -COONH4, and the purpose of the modification is to prepare for the next copper ion exchange, which would otherwise be unfavorable to the copper ion exchange reaction.
[0022] In step (2) of the preparation method of the present application, the drying temperature is 90-150°C, preferably 100-130°C, and the drying time is 2-8h, preferably 3-6h. The separation and washing in this step can be performed by a normal operation method, and there is no specific requirement. In some examples, the separation can be performed by a centrifugation method, and the washing can be performed by water washing.
[0023] In step (3) of the preparation method of the present application, the ethanol water mixed solution containing the copper salt and the lithium salt has a copper salt concentration of 10 to 45 wt%, preferably 15 to 30 wt%, a lithium salt concentration of 10 to 40 wt%, preferably 20 to 30 wt%, and an ethanol concentration of 2 to 8 wt%, preferably 3 to 6 wt%, based on the total weight of the mixed solution; Preferably, the copper salt is one or more of copper nitrate, copper chloride or copper acetate; Preferably, the lithium salt is one or both of lithium nitrate or lithium chloride.
[0024] In step (3) of the preparation method of the present application, the immersion-aging process is preferably isovolumic immersion-aging under normal pressure conditions, at a temperature of 20-60°C, preferably 30-50°C, for a time of 2-8 hours, preferably 3-6 hours.
[0025] In step (3) of the preparation method of the present application, the drying is performed at a temperature of 90 to 150° C., preferably 100 to 130° C., for 2 to 8 hours, preferably 3 to 6 hours; The firing temperature is 300 to 600° C., preferably 400 to 500° C., and the firing time is 2 to 8 hours, preferably 3 to 6 hours.
[0026] The separation and washing in this step can be performed by normal operating methods, and there are no specific requirements. In some embodiments, the separation can be performed by filtration, and the washing can be performed by water washing.
[0027] The preparation method of the present application controls the pretreatment step for the carrier, combines with the ion exchange method, and supports the active component by chemical bonding, so that the component is less likely to be washed away, and the prepared catalyst has stronger bonding strength between the active component and the carrier and better stability than the catalyst prepared by the conventional impregnation method.
[0028] In the present application, the copper-based hydrogenation catalyst prepared by the above method has a composition of 3-10 wt %, preferably 5-8 wt %, copper oxide, 0.3-3 wt %, preferably 0.5-2 wt %, lithium oxide, and the remainder is activated carbon, based on the total weight of the catalyst, to obtain a supported hydrogenation catalyst, and the active component shows an eggshell-type distribution.
[0029] In another aspect, the present application further provides the use of the above copper-based hydrogenation catalyst in the preparation of α-phenylethyl alcohol by liquid phase hydrogenation of acetophenone.
[0030] The method for preparing α-phenylethyl alcohol by hydrogenating acetophenone involves preparing α-phenylethyl alcohol by an acetophenone hydrogenation reaction under the action of the above-mentioned copper-based hydrogenation catalyst.
[0031] Preferably, the conditions of the hydrogenation reaction are a reaction pressure of 2 to 5 MPa (gauge pressure), preferably 2.5 to 4 MPa (gauge pressure), a reaction temperature of 60 to 100°C, preferably 70 to 90°C, a H2 / HPA (acetophenone) molar ratio of 2 to 20:1, preferably 5 to 15:1, and a catalyst usage amount of 0.2~0.6gHPA·gcat -1 ·h -1 , preferably 0.3 to 0.5 gHPA·gcat -1 ·h -1 It is.
[0032] Preferably, the hydrogenation raw material further contains a solvent, the solvent is ethylbenzene, and the concentration of acetophenone in the solvent is 10 to 15 wt %.
[0033] Those skilled in the art should understand that the catalyst has the corresponding catalytic activity after reductive activation, and preferably the reduced copper-based hydrogenation catalyst is used for the preparation of α-phenylethyl alcohol by hydrogenation of acetophenone.
[0034] The reductive activation of the hydrogenation catalyst is a common operation in the art. In a preferred embodiment, the reductive activation method of the catalyst described in the present application is carried out by adjusting the volumetric space velocity of the mixed gas of hydrogen and nitrogen to 300 to 1000 h -1 Preferably, the reactor temperature is first raised to 160-180°C, and the physical water adsorbed on the catalyst is desorbed at a constant temperature for 1-2 hours. Then, a mixed gas containing hydrogen and nitrogen with a volume fraction of 10v% H2 or less, for example (5v%±2v%) H2, is introduced to pre-reduce the catalyst for at least 0.5 hours, for example, 1 hour, 1.5 hours or 2 hours, and then the ratio of hydrogen in the mixed gas of hydrogen and nitrogen is increased stepwise, for example, to 10v%, 20v%, 50v%, 100v%, and the hot spot temperature of the catalyst bed layer during this process is controlled to be 220°C or less. Finally, the temperature is raised to 200-220°C, and reduction is performed in a pure hydrogen atmosphere for 2-5 hours, for example, 3 or 4 hours, to obtain an activated catalyst.
[0035] Compared with the prior art, the beneficial effects of the technical solution of the present application are as follows: In the present application, activated carbon is used as a catalyst carrier, and copper-lithium bimetallic acts synergistically. The catalyst is prepared by using ion exchange method, so that the dispersion degree of active components is improved, and the catalyst activity is high, and the catalyst has good low-temperature activity compared with conventional copper-based catalysts, and the active components are not easily washed away, the long-term stability of the catalyst is improved, and the sintering resistance of the catalyst is also improved. In addition, the catalyst adopts a carrier such as coconut shell charcoal, which has excellent skeletal strength and pore size distribution, which is favorable for the diffusion of reactants, and has good mass transfer and heat transfer effects. When the catalyst is used in the preparation of α-phenylethyl alcohol by hydrogenating acetophenone, it can effectively improve the hydrogenation ability of the catalyst and inhibit side reactions such as dehydration of phenylethyl alcohol, and has the advantages of high activity and high selectivity.
[0036] Other aspects may be appreciated after reading and understanding the detailed description. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0037] The method of the present invention will now be described in detail with reference to examples, but is not limited to these examples.
[0038] 1. Main raw materials used in the examples and comparative examples Coconut shell charcoal has a particle size of 8-16 mesh, an iodine value of 800-1300, and a pore volume of 0.38 cm 3 / g, purchased from Woody Alloys Co., Ltd. The alumina carrier has a particle size of 8 to 30 mesh and a specific surface area of 274 m 2 / g, pore volume 0.86 cm 3 / g, purchased from Shandong Aluminum Industry, Unless otherwise specified, all other raw materials are common commercial products, and all reagents are analytical reagents.
[0039] II. Analytical methods for products in the examples and comparative examples The element contents in the catalysts were measured using an X-ray fluorescence spectrum analyzer (XRF). The copper ions in the hydrogenation solution were measured using an inductively coupled plasma mass spectrometer (ICP). The catalyst side pressure strength was measured using a D-III type strength measuring instrument for 50 samples, and the average value was calculated.
[0040] The moles of acetophenone contained in the raw material, the moles of phenylethyl alcohol produced, and the moles of ethylbenzene and styrene produced by side reactions were analyzed and then calculated using an Agilent 7820A gas chromatograph. The measurement conditions include using a DB-5 column and an FID detector, the vaporizer temperature is 260°C, the detector temperature is 260°C, the carrier gas is high-purity N2, and the flow rate is 30ml / min.
[0041] Acetophenone conversion rate = (1 - moles of acetophenone remaining in the reaction solution / moles of acetophenone contained in the raw material) * 100%, Selectivity of phenylethyl alcohol=moles of phenylethyl alcohol produced / moles of acetophenone converted*100%; The calculation method for the selectivity of ethylbenzene and styrene is the same as that for the selectivity of phenylethyl alcohol. EXAMPLES
[0042] Example 1 On the preparation of copper-based hydrogenation catalysts (1) 50 ml of an aqueous solution of nitric acid with a concentration of 1 mol / L was prepared, 15 g of activated carbon was added to the aqueous solution of nitric acid, and the solution was heated to 90°C and soaked at a constant temperature for 4 hours, after which it was centrifuged and washed with water.
[0043] (2) 50 g of an aqueous solution of ammonium carbonate with a concentration of 5 wt % was prepared, and the activated carbon treated in step (1) was added to the aqueous solution of ammonium carbonate and soaked in excess at room temperature of 25°C for 4 hours, then centrifuged, washed with water, and dried at 100°C for 4 hours.
[0044] (3) 9.13 g of a mixed solution of copper nitrate and lithium nitrate in ethanol and water was prepared. The total weight of the mixed solution was 11.6 wt% copper nitrate, 22.7 wt% lithium nitrate, and 5 wt% ethanol. The activated carbon treated in step (2) was then added, and aged by immersing in an equal volume at room temperature of 25°C for 4 hours. The catalyst was then dried at 100°C for 4 hours and calcined at 400°C for 4 hours to obtain catalyst A having a copper oxide content of 3 wt% and a lithium oxide content of 3 wt%.
[0045] Example 2 On the preparation of copper-based hydrogenation catalysts (1) 50 ml of a hydrochloric acid solution with a concentration of 1.5 mol / L was prepared, 15 g of activated carbon was added to the hydrochloric acid solution, and the solution was heated to 90°C and soaked in excess at a constant temperature for 4 hours, after which it was centrifuged and washed with water.
[0046] (2) 50 g of an aqueous solution of ammonium bicarbonate with a concentration of 8 wt % was prepared, and the activated carbon treated in step (1) was added to the aqueous solution of ammonium bicarbonate and soaked in excess at room temperature of 25°C for 4 hours, then centrifuged, washed with water, and dried at 90°C for 5 hours.
[0047] (3) 7.4 g of an ethanol-water mixed solution of copper nitrate and lithium nitrate was prepared, and the total weight of the mixed solution was 14.3 wt% copper nitrate, 4.7 wt% lithium nitrate, and 5 wt% ethanol. The activated carbon treated in step (2) was then added, and aged by immersing in an equal volume at room temperature of 25°C for 4 hours, followed by drying at 100°C for 4 hours and calcining at 450°C for 4 hours to obtain catalyst B having a copper oxide content of 3 wt% and a lithium oxide content of 0.5 wt%.
[0048] Example 3 On the preparation of copper-based hydrogenation catalysts (1) 50 ml of an aqueous sulfuric acid solution with a concentration of 0.5 mol / L was prepared, 15 g of activated carbon was added to the aqueous sulfuric acid solution, and the solution was heated to 90°C and soaked in excess at a constant temperature for 4 hours, after which it was centrifuged and washed.
[0049] (2) 50 g of an aqueous solution of ammonium carbonate with a concentration of 5 wt % was prepared, and the activated carbon treated in step (1) was added to the ammonium carbonate solution and soaked in excess at room temperature of 45°C for 4 hours, then centrifuged, washed with water, and dried at 90°C for 5 hours.
[0050] (3) 10.6 g of a mixed solution of copper nitrate and lithium nitrate in ethanol and water was prepared, and the total weight of the mixed solution was 33.4 wt% copper nitrate, 9.8 wt% lithium nitrate, and 5 wt% ethanol. The activated carbon treated in step (2) was then added, and aged by immersing in an equal volume at room temperature of 30°C for 4 hours, followed by drying at 100°C for 4 hours and calcining at 400°C for 4 hours to obtain catalyst C having a copper oxide content of 10 wt% and a lithium oxide content of 1.5 wt%.
[0051] Example 4 On the preparation of copper-based hydrogenation catalysts (1) 50 ml of an aqueous solution of nitric acid with a concentration of 2 mol / L was prepared, 15 g of activated carbon was added to the aqueous solution of nitric acid, and the solution was heated to 80°C and soaked in excess at a constant temperature for 4 hours, after which it was centrifuged and washed.
[0052] (2) 50 g of an aqueous solution of ammonium carbonate with a concentration of 10 wt % was prepared, and the activated carbon treated in step (1) was added to the ammonium carbonate solution and soaked in excess at room temperature of 20°C for 4 hours, then centrifuged, washed with water, and dried at 90°C for 5 hours.
[0053] (3) 10.6 g of a mixed solution of copper nitrate and lithium nitrate in ethanol and water was prepared. The total weight of the mixed solution was 33.4 wt% copper nitrate, 9.8 wt% lithium nitrate, and 5 wt% ethanol. The activated carbon treated in step (2) was then added, and aged by immersing in an equal volume at room temperature of 30°C for 4 hours. The catalyst was then dried at 100°C for 4 hours and calcined at 400°C for 4 hours to obtain catalyst D having a copper oxide content of 10 wt% and a lithium oxide content of 1.5 wt%.
[0054] Example 5 On the preparation of copper-based hydrogenation catalysts (1) 50 ml of an aqueous solution of nitric acid with a concentration of 2 mol / L was prepared, 15 g of activated carbon was added to the aqueous solution of nitric acid, and the solution was heated to 80°C and soaked in excess at a constant temperature for 4 hours, after which it was centrifuged and washed.
[0055] (2) 50 g of an aqueous solution of ammonium carbonate with a concentration of 10 wt % was prepared, and the activated carbon treated in step (1) was added to the ammonium carbonate solution and soaked in excess at room temperature of 20°C for 4 hours, then centrifuged, washed with water, and dried at 90°C for 5 hours.
[0056] (3) 9.1 g of a mixed solution of copper nitrate and lithium nitrate in ethanol and water was prepared. The total weight of the mixed solution was 31.3 wt% copper nitrate, 2.3 wt% lithium nitrate, and 2 wt% ethanol. The activated carbon treated in step (2) was then added, and aged by immersing in an equal volume at room temperature of 30°C for 4 hours. The catalyst was then dried at 100°C for 4 hours and calcined at 400°C for 4 hours to obtain catalyst E having a copper oxide content of 8 wt% and a lithium oxide content of 0.3 wt%.
[0057] Comparative Example 1 The preparation method of Example 1 was repeated except that the alkaline solution immersion treatment in step (2) was omitted, and catalyst F was obtained with a copper content of 3 wt % and a lithium oxide content of 3 wt %.
[0058] Comparative Example 2 With reference to the preparation method of Example 2, the only difference was that the acid immersion treatment in step (1) was not carried out, and catalyst G was obtained, which had a copper oxide content of 3 wt % and a lithium oxide content of 0.5 wt %.
[0059] Comparative Example 3 Referring to the preparation method of Example 1, the only difference is that lithium nitrate is not added in step (3), and catalyst H with a copper oxide content of 3 wt% was obtained.
[0060] Comparative Example 4 Referring to the preparation method of Example 2, the only difference was that in step (3), lithium nitrate was replaced with 0.43 g of sodium nitrate, to obtain catalyst I with a copper oxide content of 3 wt % and a sodium oxide content of 0.5 wt %.
[0061] Comparative Example 5 Referring to the preparation method of Example 2, the only difference was that in step (3), activated carbon was replaced with an equal mass of alumina carrier, and catalyst J was obtained with a copper oxide content of 3 wt% and a lithium oxide content of 0.5 wt%.
[0062] Comparative Example 6 Referring to the preparation method of Example 1, the only difference is that the order of steps (1) and (2) is exchanged, and the alkaline solution immersion treatment of step (2) is carried out before the acid solution immersion treatment of step (1), thereby obtaining catalyst K having a copper oxide content of 3 wt% and a lithium oxide content of 3 wt%.
[0063] Comparative Example 7 8.07 g of a mixed solution of copper nitrate and lithium nitrate in ethanol and water was prepared. The total weight of the mixed solution was 13.4 wt% copper nitrate, 25.7 wt% lithium nitrate, and 3.7 wt% ethanol. Untreated activated carbon was added to the above solution, aged by immersing in an equal volume at room temperature of 25°C for 4 hours, dried at 100°C for 4 hours, and calcined at 400°C for 4 hours to obtain catalyst L with a copper oxide content of 3 wt% and lithium oxide content of 3 wt%.
[0064] Catalyst Use Examples The copper-based hydrogenation catalysts prepared in Examples 1 to 5 and Comparative Examples 1 to 7 were respectively used in the preparation of α-phenylethyl alcohol by the hydrogenation reaction of acetophenone, and the steps are as follows: Catalyst reduction: The catalyst was placed in a fixed-bed hydrogenation reactor with a catalyst loading of 20 ml. Before use, the catalyst was reduced under a mixture of nitrogen and hydrogen gas. During the reduction process, the volumetric space velocity of the mixture gas was 300 h -1 First, the temperature of the reactor was raised to 160°C and the physical water adsorbed on the catalyst was desorbed at a constant temperature for 2 hours. Then, a mixed gas containing hydrogen and nitrogen with a volume fraction of 5v% H2 was introduced and pre-reduced for 1 hour. After that, the hydrogen ratio in the hydrogen and nitrogen mixed gas was gradually increased to 10v%, 20v%, 50v%, and 100v%, and the hot spot temperature of the catalyst bed layer during this process was controlled to be below 220°C. Finally, the temperature was raised to 220°C and reduction was performed in a pure hydrogen atmosphere for 3 hours.
[0065] The reaction was carried out under the conditions of a pressure of 2.5 MPa (gauge pressure), a temperature of 70°C, a H2 / HPA molar ratio of 5:1, and a catalyst throughput of 0.3 gHPA / gcat / h, using an ethylbenzene solution of 15 wt% acetophenone as the hydrogenation feedstock.
[0066] The hydrogenated liquid was sampled at 24-hour intervals and the copper ion content in the hydrogenated liquid was measured. After 1000 hours of reaction, the catalyst was removed from the reactor and sieved using a stainless steel classification sieve with a pore size of 2 mm. The proportion of catalyst particle mass with a particle size of <1 mm to the total catalyst mass was calculated, and this was taken as the catalyst breakage rate.
[0067] The catalytic performance, hydrogenation reaction results, and average copper ion content in the hydrogenation liquid are shown in Table 1.
[0068] [Table 1]
[0069] From Table 1, it can be seen that no copper was detected in the hydrogenation liquid when catalyst A~catalyst E, catalyst H, I and J were used, and the ICP analysis of catalyst F, G, K and L showed that the copper content in the hydrogenation liquid was high, which indicated that the catalyst was obviously washed away. In addition, catalyst A~catalyst E have high activity and can effectively inhibit side reactions such as the production of ethylbenzene by hydrogenolysis and the production of styrene by dehydration, while the activity of the catalyst in Comparative Example 1~Comparative Example 7 is low. At the same time, after 1000 hours of long-term stable operation, the acetophenone conversion rate of catalyst A~catalyst E is more than 99%, and the selectivity of α-phenylethyl alcohol is more than 99%.
[0070] Example 6 The copper hydrogenation catalyst B prepared in Example 2 was used to prepare α-phenylethyl alcohol by hydrogenation of acetophenone, and the reaction temperature was adjusted according to the method of Example 4. The hydrogenation results are shown in Table 2.
[0071] [Table 2]
[0072] From Table 2, it can be seen that when the hydrogenation temperature is 60-100°C, a high acetophenone conversion can be obtained in all cases, and the acetophenone conversion increases with increasing temperature, but the selectivity of α-phenylethyl alcohol decreases. The optimum condition is 70-80°C, and the selectivity of α-phenylethyl alcohol is above 99% in all cases, which indicates that the catalyst has good low-temperature activity.
Claims
1. A method for preparing a copper-based hydrogenation catalyst, comprising the steps of: (1) a step of immersing activated carbon in an acid solution, followed by separation and washing; Step (2) of immersing the activated carbon treated in step (1) in an alkaline solution, followed by separation, washing and drying; and (3) adding the activated carbon treated in step (2) to an ethanol-water mixed solution containing a copper salt and a lithium salt, immersing the activated carbon in the mixed solution for aging, and then isolating, washing, drying and calcining the activated carbon to obtain a copper-based hydrogenation catalyst. The alkaline liquid is an alkaline aqueous solution containing an ammonium salt, The copper-based hydrogenation catalyst is used in the hydrogenation reaction of acetophenone.
2. In step (1), the acid solution is an aqueous solution of an acid, and the concentration is 0.5 to 2 mol / L, and the acid is one or more selected from nitric acid, hydrochloric acid, and sulfuric acid; The preparation method according to claim 1, wherein the activated carbon is either coconut shell charcoal or wood charcoal, and its iodine value is 600-1500, and its particle size is 4-60 mesh.
3. In step (1), the concentration of the acid solution is 0.8 to 1.5 mol / L, and the acid is selected from nitric acid; 3. The preparation method according to claim 1 or 2, wherein the iodine value of the activated carbon is 800-1300, and the particle size of the activated carbon is 8-16 mesh.
4. The method according to any one of claims 1 to 3, wherein in step (1), the immersion treatment is performed at a immersion temperature of 80 to 140°C for a time of 2 to 8h.
5. The method according to any one of claims 1 to 4, wherein in step (1), the immersion treatment is performed at a immersion temperature of 90 to 130°C for a time of 3 to 6h.
6. The preparation method according to any one of claims 1 to 5, wherein in step (2), the concentration of the alkaline solution is 2 to 10 wt %, and the ammonium salt is selected from ammonium carbonate and / or ammonium hydrogen carbonate.
7. The preparation method according to any one of claims 1 to 6, wherein in step (2), the concentration of the alkaline liquid is 3 to 8 wt%.
8. The method according to any one of claims 1 to 7, wherein in step (2), the immersion treatment is carried out at a immersion temperature of 20 to 60°C for a immersion time of 2 to 8 h.
9. The method according to any one of claims 1 to 8, wherein in step (2), the immersion treatment is carried out at a immersion temperature of 30 to 50°C for a immersion time of 3 to 6 h.
10. In step (3), the ethanol water mixed solution containing the copper salt and the lithium salt has a copper salt concentration of 10-45 wt %, a lithium salt concentration of 10-40 wt %, and an ethanol concentration of 2-8 wt %, based on the total weight of the mixed solution; the copper salt being one or more of copper nitrate, copper chloride, or copper acetate; The preparation method according to any one of claims 1 to 9, wherein the lithium salt is one or both of lithium nitrate or lithium chloride.
11. In step (3), the immersion and aging process is carried out at a temperature of 20 to 60° C. for 2 to 8 hours; The drying is performed at a temperature of 90 to 150° C. for 2 to 8 hours. The preparation method according to any one of claims 1 to 10, wherein the calcination is performed at a temperature of 300 to 600°C for a time of 2 to 8h.
12. A copper-based hydrogenation catalyst, the composition of which, based on the total weight of the catalyst, is 3-10 wt % copper oxide, 0.3-3 wt % lithium oxide, and the remainder is activated carbon; The copper-based hydrogenation catalyst is used in the hydrogenation reaction of acetophenone.
13. 13. The copper-based hydrogenation catalyst of claim 12, wherein the copper oxide in the catalyst is 5-8 wt % based on the total weight of the catalyst.
14. The copper-based hydrogenation catalyst according to claim 12 or 13, wherein the lithium oxide in the catalyst is 0.5-2 wt % based on the total weight of the catalyst.
15. Use of a copper-based hydrogenation catalyst prepared by the preparation process according to any one of claims 1 to 11 or of a copper-based hydrogenation catalyst according to any one of claims 12 to 14 in the preparation of α-phenylethyl alcohol by liquid phase hydrogenation of acetophenone.
16. A method for preparing α-phenylethyl alcohol by hydrogenating acetophenone, comprising: preparing α-phenylethyl alcohol by hydrogenation reaction of acetophenone under the action of a copper-based hydrogenation catalyst prepared by the preparation method according to any one of claims 1 to 11 or a copper-based hydrogenation catalyst according to any one of claims 12 to 14; The conditions of the hydrogenation reaction are a reaction pressure of 2 to 5 MPa (gauge pressure), a reaction temperature of 60 to 100° C., and H 2 / HPA molar ratio is 2-20:1, catalyst usage amount is 0.2-0.6gHPA·gcat -1 ・h -1 That is, the method.
17. The reaction pressure is 2.5 to 4 MPa (gauge pressure). The reaction temperature is 70 to 90° C. H 2 / HPA molar ratio is 5-15:1; The catalyst usage amount is 0.3 to 0.5 g HPA / gcat -1 ・h -1 and 17. The method according to claim 16, wherein the raw material for the hydrogenation reaction further comprises a solvent, the solvent being ethylbenzene, and the concentration of acetophenone in the solvent is 10 to 15 wt %.
Citation Information
Patent Citations
Copper-based catalyst, preparation method thereof and method for preparing etherified grade ethylene glycol using copper-based catalyst
CN109092310A
Reduction treated copper-base catalyst and process for preparing alpha-phenylethyl alcohol therefrom
CN1315226A
Amorphous nickel boron catalyst for hypnone hydrogenation and its preparation method
CN1557545A
Synthesis method of alpha phenyl ethanol
CN1911883A
Supported catalyst composition, processes for the preparation thereof and use of the supported catalyst composition
EP1288188A1