High-strength hot-rolled steel sheet, hot-rolled plated steel sheet and manufacturing method thereof
A high-strength hot-rolled steel sheet with controlled composition and cooling processes, combined with zinc or aluminum coatings, addresses the need for lightweight, economical structural materials by enhancing strength and formability.
Patent Information
- Application Number
- JP2023528466
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-11-17
- Filing Date
- 2021-11-10
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2041-11-10
AI Technical Summary
Existing high-strength hot-rolled steel sheets and plated steel sheets lack suitable physical properties for use as structural materials, particularly in terms of strength and weight reduction, and current manufacturing methods require expensive alloying elements that hinder the production of thin materials.
A hot-rolled steel sheet composition comprising specific elements (C, Mn, Si, Al, P, S, N, Ti, B, Nb, Mo, V) with controlled microstructures (bainite and ferrite fractions) and cooling processes to achieve high strength and formability, along with a plated steel sheet option using zinc or aluminum coatings.
The solution enables high-strength steel sheets that are thinner and more economical, with improved deformation resistance and corrosion resistance, suitable for structural applications.
Smart Images

Figure 0007594109000004 
Figure 0007594109000001 
Figure 0007594109000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a high-strength hot-rolled steel sheet, a hot-rolled plated steel sheet, and a manufacturing method thereof, and more particularly to a hot-rolled steel sheet, a hot-rolled plated steel sheet, and a manufacturing method thereof, which have physical properties suitable for use as steel building materials. [Background technology]
[0002] High-strength hot-rolled steel sheets and hot-rolled galvanized steel sheets are mainly used as structural support materials. In particular, high-strength hot-rolled galvanized steel sheets have excellent deformation resistance and corrosion resistance, and are more economical than cold-rolled galvanized steel sheets, and are therefore widely used as steel building materials such as construction scaffolding, vinyl greenhouse structures, and solar support platforms.
[0003] However, although there is an increasing trend for such hot-rolled steel sheets or hot-rolled plated steel sheets to have high strength and light weight, the reality is that up to now, no practical method has been provided for providing a hot-rolled steel sheet or hot-rolled plated steel sheet having physical properties suitable for use as a structural material.
[0004] Patent Documents 1 to 4 disclose techniques for ensuring the strength of steel sheets by precipitation strengthening through the addition of alloying elements. These techniques use the manufacturing method of ordinary HSLA steel (High Strength Low Alloy Steel), and require the addition of alloying elements such as Ti, Nb, V, and Mo. This requires the addition of expensive alloying elements, which is undesirable in terms of manufacturing costs, and there is a problem in that such alloying elements increase the rolling load and make it impossible to manufacture thin materials.
[0005] Patent Documents 5 to 7 disclose techniques for ensuring strength by utilizing a dual phase structure of ferrite and martensite or a composite structure of ferrite, bainite, martensite, and retained austenite. However, although ferrite and retained austenite have advantages in terms of workability, they are disadvantageous in terms of yield strength, and there are technical difficulties in ensuring strength suitable for use as a structural material.
[0006] Therefore, there is an urgent need to develop hot-rolled steel sheets and hot-rolled galvanized steel sheets that have high strength properties suitable for use as supporting structural materials, but can also be made thinner to reduce weight. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Korean Patent Publication No. 10-2005-0113247 (Published on December 1, 2005) [Patent Document 2] Japanese Patent Publication No. 2002-322542 (published on November 8, 2002) [Patent Document 3] Japanese Patent Publication No. 2006-161112 (Published on June 22, 2006) [Patent Document 4] Korean Patent Publication No. 10-2006-0033489 (Published on April 19, 2006) [Patent Document 5] Japanese Patent Publication No. 2005-298967 (published on October 27, 2005) [Patent Document 6] U.S. Patent Publication No. 2005-0155673 (published July 21, 2005) [Patent Document 7] European Patent Publication No. 1396549 (Published on March 10, 2004) Summary of the Invention [Problem to be solved by the invention]
[0008] According to one aspect of the present invention, there are provided a high-strength thin hot-rolled steel sheet, a hot-rolled plated steel sheet, and methods for producing the same.
[0009] The object of the present invention is not limited to the above-mentioned contents, and a person skilled in the art will have no difficulty in understanding further object of the present invention from the entire contents of this specification. [Means for solving the problem]
[0010] A hot-rolled steel sheet according to one aspect of the present invention contains, by weight, 0.1 to 0.25% carbon (C), 0.2 to 2.0% manganese (Mn), 0.3% or less silicon (Si), 0.05% or less aluminum (Al), 0.05% or less phosphorus (P), 0.03% or less sulfur (S), 0.01% or less nitrogen (N), 0.005 to 0.05% titanium (Ti), 0.0005 to 0.005% boron (B), 0.01% or less niobium (Nb), 0.1% or less molybdenum (Mo), 0.1% or less vanadium (V), and the remainder iron (Fe) and unavoidable impurities, and contains, by volume fraction, 55 to 90% bainite and 10 to 45% ferrite as a microstructure, and the number of carbides present in the bainite having a major axis length of 25 to 500 nm per unit area is 3×10 6 pieces / mm 2 The average aspect ratio (major axis / minor axis) of carbides present in the bainite can be set to 2.0 or less.
[0011] The above-mentioned hot-rolled steel sheet may contain, by volume fraction, one or more of the following microstructures: 10% or less (including 0%) pearlite, 1% or less (including 0%) martensite, and 1% or less (including 0%) retained austenite.
[0012] The average packet size of the bainite may be 50 to 200% of the average crystal grain size of the ferrite.
[0013] The above-mentioned hot-rolled steel sheet can satisfy the following relational expression 1. [Equation 1] 30*[Ti]+100*[Nb]+5*[V]≦1.65 In the above Relational Formula 1, [Ti], [Nb] and [V] respectively represent the contents (wt%) of titanium (Ti), niobium (Nb) and vanadium (V) contained in the above heat-rolled steel sheet.
[0014] The hot-rolled steel sheet may further contain, by weight percent, chromium (Cr): 0.2% or less.
[0015] The bendability (R / t) of the hot-rolled steel sheet can be set to 1.0 or less.
[0016] The hot-rolled steel sheet may have a yield strength (YS) of 550 MPa or more and a tensile strength (TS) of 650 MPa or more.
[0017] The thickness of the hot-rolled steel sheet may be 3 mm or less (excluding 0 mm).
[0018] A hot-rolled plated steel sheet according to one aspect of the present invention comprises a base steel sheet and a plating layer formed on at least one surface of the base steel sheet, wherein the base steel sheet is the hot-rolled steel sheet, and the plating layer may be any one plating layer selected from zinc, aluminum, a zinc-based alloy, and an aluminum-based alloy.
[0019] A method for producing a hot rolled steel sheet according to one aspect of the present invention includes a slab heating step of heating a slab containing, by weight, 0.1 to 0.25% carbon (C), 0.2 to 2.0% manganese (Mn), 0.3% or less silicon (Si), 0.05% or less aluminum (Al), 0.05% or less phosphorus (P), 0.03% or less sulfur (S), 0.01% or less nitrogen (N), 0.005 to 0.05% titanium (Ti), 0.0005 to 0.005% boron (B), 0.01% or less niobium (Nb), 0.1% or less molybdenum (Mo), 0.1% or less vanadium (V), with the remainder being iron (Fe) and unavoidable impurities; fm) to provide a steel sheet; a first cooling step of cooling the hot-rolled steel sheet at a first cooling rate to a first cooling stop temperature (T1) satisfying the following relational expression 4; a second cooling step of cooling the first-cooled steel sheet at a second cooling rate of 50 to 500°C / s which is faster than the first cooling rate to a second cooling stop temperature (T2) satisfying the following relational expression 5; a third cooling step of cooling the second-cooled steel sheet at a third cooling rate which is slower than the second cooling rate to a third cooling stop temperature (T3) satisfying the following relational expression 6; a coiling step of coiling the third-cooled hot-rolled steel sheet at the third cooling stop temperature (T3); and a heat treatment step of heat-treating the coiled steel sheet at a temperature range of 450 to 720°C. [Equation 3] T fm (℃)≧800+3000*[Ti]+10000*[Nb]-20*t^ (1 / 2) In the above Relational Formula 3, [Ti] and [Nb] respectively represent the titanium (Ti) and niobium (Nb) contents (wt%) contained in the slab, and t represents the thickness (mm) of the hot-rolled steel sheet. [Equation 4] T fm (℃)-80℃≦T1(℃)≦T fm (℃)-5℃ In the above relational expression 4, T fm is the rolling end temperature (T fm ) [Equation 5] T2(℃)≦750-270*[C]-90*[Mn] In the above Relational Formula 5, [C] and [Mn] respectively represent the contents (wt%) of carbon (C) and manganese (Mn) contained in the slab. [Equation 6] 540-423*[C]-30.4*[Mn]≦T3(℃) <T2(℃) In the above Relational Formula 6, T2 means the second cooling stop temperature (T2) of the second cooling stage, and [C] and [Mn] mean the contents (wt%) of carbon (C) and manganese (Mn) contained in the slab, respectively.
[0020] The first cooling rate may be from 5 to 50° C. / s, and the third cooling rate may be from 5 to 50° C. / s.
[0021] The slab can satisfy the following relational expression 1. [Equation 1] 30*[Ti]+100*[Nb]+5*[V]≦1.65 In the above Relational Formula 1, [Ti], [Nb] and [V] respectively represent the contents (wt%) of titanium (Ti), niobium (Nb) and vanadium (V) contained in the slab.
[0022] The slab may further include, by weight, chromium (Cr): 0.2% or less.
[0023] The hot rolled steel sheet may have a thickness of 3 mm or less.
[0024] A method for manufacturing a hot-rolled plated steel sheet according to one aspect of the present invention includes the steps of: preparing a base steel sheet; and forming a plating layer on at least one surface of the base steel sheet by any one method selected from a hot-dip plating method, an electroplating method, and a plasma method, wherein the base steel sheet is provided by the method for manufacturing a hot-rolled steel sheet, and the plating layer may be any one plating layer selected from zinc, aluminum, a zinc-based alloy, and an aluminum-based alloy.
[0025] The above solutions to the problems are not intended to be exhaustive, and the various features of the present invention and their associated advantages and benefits can be understood in more detail with reference to the following specific examples. Effect of the Invention
[0026] According to one aspect of the present invention, it is possible to provide a hot-rolled steel sheet, a hot-rolled plated steel sheet, and a manufacturing method thereof that have high strength properties suitable for use as a high-strength supporting structural material while being capable of being thinned to reduce weight.
[0027] The effects of the present invention are not limited to the above, and can be interpreted as including effects that a person skilled in the art can infer from the description below. [Brief description of the drawings]
[0028] [Figure 1] 1 is a photograph of the microstructure of test piece 1 observed using a scanning electron microscope (SEM). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0029] The present invention relates to a hot-rolled steel sheet, a hot-rolled plated steel sheet, and a manufacturing method thereof, and preferred embodiments of the present invention will be described below. The embodiments of the present invention can be modified in various ways, and the scope of the present invention should not be interpreted as being limited to the embodiments described below. The embodiments of the present invention are provided to further explain the present invention in detail to those skilled in the art to which the invention pertains.
[0030] The hot-rolled steel sheet of the present invention will be described in more detail below.
[0031] A hot-rolled steel sheet according to one aspect of the present invention contains, by weight, 0.1 to 0.25% carbon (C), 0.2 to 2.0% manganese (Mn), 0.3% or less silicon (Si), 0.05% or less aluminum (Al), 0.05% or less phosphorus (P), 0.03% or less sulfur (S), 0.01% or less nitrogen (N), 0.005 to 0.05% titanium (Ti), 0.0005 to 0.005% boron (B), 0.01% or less niobium (Nb), 0.1% or less molybdenum (Mo), 0.1% or less vanadium (V), and the remainder iron (Fe) and unavoidable impurities, and contains, by volume fraction, 55 to 90% bainite and 10 to 45% ferrite as a microstructure, and the number of carbides present in the bainite having a major axis length of 25 to 500 nm per unit area is 3×10 6 pieces / mm 2 The average aspect ratio (major axis / minor axis) of the carbides present in the bainite can be set to 2.0 or less.
[0032] The steel composition of the present invention will be described in more detail below. Unless otherwise specified, % representing the content of each element is based on weight.
[0033] A hot-rolled steel sheet according to one aspect of the present invention contains, by weight, 0.1 to 0.25% carbon (C), 0.2 to 2.0% manganese (Mn), 0.3% or less silicon (Si), 0.05% or less aluminum (Al), 0.05% or less phosphorus (P), 0.03% or less sulfur (S), 0.01% or less nitrogen (N), 0.005 to 0.05% titanium (Ti), 0.0005 to 0.005% boron (B), 0.01% or less niobium (Nb), 0.1% or less molybdenum (Mo), 0.1% or less vanadium (V), the balance being iron (Fe) and unavoidable impurities, and may further contain 0.2% or less by weight of chromium (Cr).
[0034] Carbon (C): 0.1~0.25% Carbon (C) is an element that effectively contributes to improving the strength of steel plate. Carbon (C) is also an element that needs to be appropriately added in order to secure the microstructure to be realized in the present invention. Therefore, in order to secure the desired level of strength and the desired level of bainite fraction during cooling after hot rolling, the present invention can add 0.1% or more of carbon (C). The preferred lower limit of the carbon (C) content can be 0.12%, and the more preferred lower limit of the carbon (C) content can be 0.14%. However, if carbon (C) is added excessively, a large amount of carbides are formed, which may reduce the formability, or when used in steel building materials, the weldability may be reduced, so the present invention can limit the carbon (C) content to 0.25% or less. The preferred upper limit of the carbon (C) content can be 0.24%, and the more preferred upper limit of the carbon (C) content can be 0.23%.
[0035] Manganese (Mn): 0.2-2.0% Manganese (Mn) is not only an element that improves the strength and hardenability of steel, but also an element that effectively contributes to suppressing crack generation due to sulfur (S) by combining with sulfur (S) that is inevitably contained during the steel manufacturing process to form MnS. Therefore, the present invention can contain manganese (Mn) of 0.2% or more. A preferable lower limit of the manganese (Mn) content can be 0.3%, and a more preferable lower limit of the manganese (Mn) content can be 0.4%. However, if manganese (Mn) is added excessively, not only the weldability is reduced but also it is not preferable from the economical point of view, so that the present invention can limit the manganese (Mn) content to 2.0% or less. A preferable upper limit of the manganese (Mn) content can be 1.9%, and a more preferable upper limit of the manganese (Mn) content can be 1.8%.
[0036] Silicon (Si): 0.3% or less Silicon (Si) is an element that not only acts as a deoxidizer but also effectively contributes to improving the strength of steel sheet, so in the present invention, silicon (Si) can be added to achieve such effects. A preferred lower limit of the silicon content can be 0.01%, and a more preferred lower limit of the silicon content can be 0.02%. However, if the silicon (Si) content exceeds a certain level, the surface quality may be deteriorated due to the scale formed on the steel sheet surface, and the weldability may be deteriorated, so in the present invention, the silicon (Si) content can be limited to 0.3% or less. A preferred upper limit of the silicon (Si) content can be 0.2%, and a more preferred upper limit of the silicon (Si) content can be 0.1%.
[0037] Aluminum (Al): 0.05% or less Aluminum (Al) is an element that combines with oxygen in steel to act as a deoxidizer, and the present invention can add aluminum (Al) for this effect. A preferred lower limit of the aluminum (Al) content can be 0.005%, and a more preferred lower limit of the aluminum (Al) content can be 0.01%. However, if aluminum (Al) is added excessively, not only will the number of inclusions in the steel sheet increase, but the workability of the steel sheet will also decrease, so the present invention can limit the aluminum (Al) content to 0.05% or less. A preferred upper limit of the aluminum (Al) content can be 0.04%.
[0038] Phosphorus (P): 0.05% or less Phosphorus (P) is an impurity element that is inevitably contained in steel, and is an element that segregates at grain boundaries and reduces the toughness of steel. Therefore, it is preferable to control its content as low as possible, and theoretically it is advantageous to limit the phosphorus (P) content to 0%. However, taking into consideration the content that is inevitably contained in the manufacturing process, the present invention can limit the phosphorus (P) content to 0.05% or less. A preferable upper limit of the phosphorus (P) content can be 0.04%, and a more preferable phosphorus (P) content can be 0.03%.
[0039] Sulfur (S): 0.03% or less Sulfur (S) is an impurity that is inevitably contained in steel, and is an element that reacts with manganese (Mn) to form MnS, increasing the content of precipitates and embrittling the steel. Therefore, it is preferable to control the content as low as possible, and theoretically it is advantageous to limit the sulfur (S) content to 0%. However, taking into consideration the content that is inevitably contained in the manufacturing process, the present invention can limit the sulfur (S) content to 0.03% or less. A preferable upper limit of the sulfur (S) content can be 0.02%, and a more preferable upper limit of the sulfur (S) content can be 0.01%.
[0040] Nitrogen (N): 0.01% or less Nitrogen (N) is an impurity that is inevitably contained in steel, and is an element that forms nitrides during continuous casting and causes cracks in the slab. Therefore, it is preferable to control its content as low as possible, and in theory, it is advantageous to limit the nitrogen (N) content to 0%. However, taking into consideration the content that is inevitably contained in the manufacturing process, the present invention can limit the nitrogen (N) content to 0.01% or less. The preferred nitrogen (N) content can be 0.008% or less, and the more preferred nitrogen (N) content can be 0.006% or less.
[0041] Titanium (Ti): 0.005-0.05% Titanium (Ti) is an element that combines with carbon (C) and nitrogen (N) to form carbides and nitrides. In the present invention, boron (B) is added to ensure hardening ability, and at this time, titanium (Ti) combines with nitrogen (N) before boron (B) combines with nitrogen (N), thereby improving the effect of adding boron (B). In the present invention, titanium (Ti) can be added in an amount of 0.005% or more to achieve such an effect. A preferable lower limit of the titanium (Ti) content can be 0.01%, and a more preferable lower limit of the titanium (Ti) content can be 0.015%. However, if titanium (Ti) is added excessively, it can cause a decrease in continuous castability in the slab production stage, and an increase in the rolling load during hot rolling can cause a decrease in rollability. Therefore, in the present invention, the titanium (Ti) content can be limited to 0.05% or less. A preferable lower limit of the titanium (Ti) content may be 0.04%, and a more preferable lower limit of the titanium (Ti) content may be 0.03%.
[0042] Boron (B): 0.0005-0.005% Boron (B) is an element that plays an important role in improving the hardening ability of steel sheet, and is an element that suppresses the transformation of ferrite and pearlite during cooling after rolling. In order to achieve such an effect, the present invention can add 0.0005% or more of boron (B). A preferred lower limit of the boron (B) content can be 0.0007%, and a more preferred lower limit of the boron (B) content can be 0.001%. However, if the amount of boron (B) added exceeds a certain level, there is a problem that excessively added boron (B) bonds with iron (Fe) to weaken the grain boundary, so the present invention can limit the boron (B) content to 0.005% or less. A preferred upper limit of the boron (B) content can be 0.004%, and a more preferred upper limit of the boron (B) content can be 0.003%.
[0043] Niobium (Nb): 0.01% or less, Molybdenum (Mo): 0.1% or less, Vanadium (V): 0.1% or less Niobium (Nb), molybdenum (Mo) and vanadium (V) are elements that react with carbon (C) and nitrogen (N) to form precipitates such as carbides and nitrides. However, since these are expensive elements, as the amount of addition increases, not only does the price increase, but the rolling load during hot rolling may increase, making it difficult to manufacture thin materials. Therefore, in the present invention, the addition of niobium (Nb), molybdenum (Mo) and vanadium (V) may be suppressed, and even if they are inevitably added, the contents of niobium (Nb), molybdenum (Mo) and vanadium (V) can be limited to 0.01% or less, 0.1% or less, and 0.01% or less, respectively. The upper limits of the preferred niobium (Nb) and molybdenum (Mo) contents can be 0.005% and 0.01%, respectively. The content of niobium (Nb), molybdenum (Mo) and vanadium (V) may each be 0%, and the lower limit thereof may each be 0.0005%.
[0044] On the other hand, the contents of titanium (Ti), niobium (Nb) and vanadium (V), which form precipitates and reduce rollability, preferably satisfy the following relational expression 1. [Equation 1] 30*[Ti]+100*[Nb]+5*[V]≦1.65 In the above Relational Formula 1, [Ti], [Nb] and [V] respectively represent the contents (wt%) of titanium (Ti), niobium (Nb) and vanadium (V) contained in the above heat-rolled steel sheet.
[0045] The above-mentioned relational expression 1 is a condition for providing a thin steel sheet material that ensures high strength and high formability properties. In other words, if the contents of titanium (Ti), niobium (Nb) and vanadium (V) do not satisfy the relational expression 1, not only is it necessary to unavoidably perform hot rolling at high temperatures to manufacture a thin steel sheet material, but the aspect ratio (major axis / minor axis) of carbides may exceed a desired level, resulting in a decrease in bending workability (R / t).
[0046] Chromium (Cr): 0.2% by weight or less Chromium (Cr) is an element that contributes to improving the hardenability of steel, so in the present invention, chromium (Cr) can be selectively added to achieve such an effect. However, since chromium (Cr) is an expensive element, adding excessive chromium (Cr) is not preferable from an economical point of view. Since excessive addition of chromium (Cr) may cause a decrease in weldability, the present invention can limit the chromium (Cr) content to 0.2% or less. The preferred upper limit of the chromium (Cr) content can be 0.15%, and the more preferred upper limit of the chromium (Cr) content can be 0.1%.
[0047] The hot-rolled steel sheet according to one aspect of the present invention may contain the remaining Fe and other inevitable impurities in addition to the above-mentioned components. However, since unintended impurities may be inevitably mixed in from raw materials or the surrounding environment in a normal manufacturing process, it is not possible to completely exclude them. Since these impurities are known to anyone having ordinary skill in the art, the entire contents of the impurities will not be specifically mentioned in this specification. Furthermore, the additional addition of effective components other than the above-mentioned components is not completely excluded.
[0048] The microstructure of the hot-rolled steel sheet according to one aspect of the present invention may contain 55 to 90 volume % bainite and 10 to 45 volume % ferrite, and may further contain one or more of 10 volume % or less (including 0%) pearlite, 1 volume % or less (including 0%) martensite, and 1 volume % or less (including 0%) retained austenite.
[0049] Since bainite is a microstructure effective for increasing strength, and ferrite is a microstructure effective for ensuring ductility, the bainite and ferrite fractions need to be appropriately controlled in order to achieve both high strength properties and excellent formability. Therefore, the present invention can control the bainite fraction to within a range of 55 to 90 volume %, and the ferrite fraction to within a range of 10 to 45%.
[0050] In addition, the hot-rolled steel sheet of the present invention may contain one or more of pearlite, martensite, retained austenite, and other precipitates as a microstructure, but the fraction may be limited to a certain range or less in order to achieve both high strength properties and excellent formability. When a large amount of pearlite is formed, the formability is reduced due to the formation of a composite structure, or the bainite fraction is reduced, making it difficult to ensure strength, so the present invention may limit the pearlite fraction to 10 volume % or less (including 0%). Martensite is advantageous in terms of ensuring strength but disadvantageous in terms of ensuring formability, so the present invention may limit the martensite fraction to 1% or less (including 0%). Retained austenite is advantageous in terms of ensuring formability but disadvantageous in terms of ensuring yield strength, so the present invention may limit the retained austenite fraction to 1% or less (including 0%).
[0051] Among the carbides present in bainite, the number of carbides with a major axis length of 25 to 500 nm per unit area is 3 × 10 6 pieces / mm 2It is preferable that the number of carbides present in bainite is equal to or greater than a certain amount. Carbides with too small a grain size among the carbides present in bainite increase the rolling load during hot rolling, making thin rolling difficult, while carbides with too large a grain size may act detrimentally in ensuring strength and ductility. In order to ensure strength, it is preferable that the number of carbides present in bainite is equal to or greater than a certain amount. Therefore, in the hot-rolled steel sheet of the present invention, the number of carbides with a major axis length of 25 to 500 nm per unit area among the carbides present in bainite is set to 3×10 6 pieces / mm 2 It is possible to control the above.
[0052] The shape of the carbides present in the bainite is also a factor that significantly affects the formability of the steel sheet, and the closer the shape of the carbides present in the bainite is to a spherical shape, the more advantageous it is for ensuring the formability of the steel sheet. Therefore, from the viewpoint of ensuring formability, the present invention can limit the average aspect ratio (major axis / minor axis) of the carbides present in the bainite to 2.0 or less.
[0053] On the other hand, the greater the difference in size between bainite and ferrite, the less preferable it is in terms of formability. Therefore, in the hot-rolled steel sheet of the present invention, the average packet size of bainite can be controlled to a level of 50 to 200% of the average crystal grain size of ferrite.
[0054] The hot-rolled steel sheet according to one aspect of the present invention can be a thin material having a thickness of 3 mm or less (excluding 0 mm), and can have a yield strength (YS) of 550 MPa or more, a tensile strength (TS) of 650 MPa or more, and a bending workability (R / t) of 1.0 or less.
[0055] In the hot-rolled steel sheet according to one aspect of the present invention, the yield strength and thickness of the steel sheet can satisfy the following Relational Expression 2 so as to meet the objectives of high strength and weight reduction through thinning. [Equation 2] YS-100*T≧350 In the above Relational Formula 2, YS means the yield strength (MPa) of the hot-rolled steel sheet, and t means the thickness (mm) of the hot-rolled steel sheet.
[0056] Meanwhile, the hot-rolled steel sheet according to one aspect of the present invention may be a hot-rolled plated steel sheet having a plating layer on at least one surface. The components of the plating layer of the hot-rolled plated steel sheet of the present invention are not particularly limited. As a non-limiting example, the plating layer may be any one selected from zinc, aluminum, zinc-based alloy, and aluminum-based alloy. As a non-limiting example, the zinc-based alloy plating layer may be a plating layer containing one or more selected from aluminum (Al), magnesium (Mg), nickel (Ni), and iron (Fe), and zinc (Zn) as the balance. The aluminum-based alloy plating layer may be a plating layer containing one or more selected from silicon (Si), magnesium (Mg), nickel (Ni), and iron (Fe), and aluminum (Al) as the balance.
[0057] Hereinafter, a method for producing a high strength hot rolled steel sheet according to one aspect of the present invention will be described in more detail.
[0058] A method for producing a hot rolled steel sheet according to another aspect of the present invention includes a slab heating step of heating a slab containing, by weight, 0.1 to 0.25% carbon (C), 0.2 to 2.0% manganese (Mn), 0.3% or less silicon (Si), 0.05% or less aluminum (Al), 0.05% or less phosphorus (P), 0.03% or less sulfur (S), 0.01% or less nitrogen (N), 0.005 to 0.05% titanium (Ti), 0.0005 to 0.005% boron (B), 0.01% or less niobium (Nb), 0.1% or less molybdenum (Mo), 0.1% or less vanadium (V), with the remainder being iron (Fe) and unavoidable impurities; fm) to provide a steel sheet; a first cooling step of cooling the hot-rolled steel sheet at a first cooling rate to a first cooling stop temperature (T1) satisfying the following relational expression 4; a second cooling step of cooling the first-cooled steel sheet at a second cooling rate of 50 to 500°C / s which is faster than the first cooling rate to a second cooling stop temperature (T2) satisfying the following relational expression 5; a third cooling step of cooling the second-cooled steel sheet at a third cooling rate which is slower than the second cooling rate to a third cooling stop temperature (T3) satisfying the following relational expression 6; a coiling step of coiling the third-cooled hot-rolled steel sheet at the third cooling stop temperature (T3); and a heat treatment step of heat-treating the coiled steel sheet at a temperature range of 450 to 720°C. [Equation 3] T fm (℃)≧800+3000*[Ti]+10000*[Nb]-20*t^ (1 / 2) In the above Relational Formula 3, [Ti] and [Nb] respectively represent the contents (wt%) of titanium (Ti) and niobium (Nb) contained in the slab, and t represents the thickness (mm) of the hot-rolled steel sheet. [Equation 4] T fm (℃)-80℃≦T1(℃)≦T fm (℃)-5℃ In the above relational expression 4, T fm is the rolling end temperature (T fm ) [Equation 5] T2(℃)≦750-270*[C]-90*[Mn] In the above Relational Formula 5, [C] and [Mn] respectively represent the contents (wt%) of carbon (C) and manganese (Mn) contained in the slab. [Equation 6] 540-423*[C]-30.4*[Mn]≦T3(℃)≦T2(℃) In the above Relational Formula 6, T2 means the second cooling stop temperature (T2) of the second cooling stage, and [C] and [Mn] mean the contents (wt%) of carbon (C) and manganese (Mn) contained in the slab, respectively.
[0059] Preparation and heating of steel slabs A steel slab having a predetermined composition is prepared. Since the steel slab of the present invention has an alloy composition corresponding to the alloy composition of the hot rolled steel sheet described above, the description of the alloy composition of the steel slab replaces the description of the alloy composition of the hot rolled steel sheet described above.
[0060] The prepared steel slab may be heated to a certain temperature range, and the heating method and heating temperature of the steel slab are not particularly limited. For example, the heating temperature of the steel slab may be in the range of 1100 to 1350°C. If the heating temperature of the steel slab is less than 1100°C, the hot rolling may be performed in a temperature range below the temperature range of the intended finish hot rolling. If the heating temperature of the steel slab exceeds 1350°C, excessive energy is input, resulting in additional costs, or a thick scale may be formed on the surface of the slab.
[0061] Hot rolling By hot rolling the heated steel slab, a hot-rolled steel sheet having a thickness of 3 mm or less (excluding 0 mm) can be provided. If the temperature of the heated steel slab is at a temperature at which normal hot rolling can be performed, hot rolling can be performed directly without reheating. If the temperature of the heated steel slab is lower than the temperature at which normal hot rolling can be performed, hot rolling can be performed after reheating.
[0062] At this time, the end temperature of hot rolling (T fm ) preferably satisfies the following relational expression 3. If the rolling temperature is excessively low, not only will the rolling load increase, reducing rollability, or surface roughness due to fatigue of the rolling rolls be induced, but the aspect ratio of carbides may deviate from the desired level due to low-temperature rolling. [Equation 3] T fm (℃)≧800+3000*[Ti]+10000*[Nb]-20*t^ (1 / 2) In the above Relational Formula 3, [Ti] and [Nb] respectively represent the titanium (Ti) and niobium (Nb) contents (wt%) contained in the slab, and t represents the thickness (mm) of the hot-rolled steel sheet.
[0063] 1st cooling The hot-rolled steel sheet is cooled at a first cooling rate (V C1 ) may be cooled. [Equation 4] T fm (℃)-80℃≦T1(℃)≦T fm (℃)-5℃ In the above relational expression 4, T fm is the rolling end temperature (T fm )
[0064] If the first cooling stop temperature (T1) is below a certain level, transformation to ferrite or pearlite occurs, making it impossible to obtain the microstructure that is the object of the present invention, and as a result, it is possible that the desired level of strength cannot be obtained. Therefore, the present invention sets the lower limit of the first cooling stop temperature (T1) at T fm (℃)-80℃. In addition, if the first cooling end temperature (T1) exceeds a certain level, the austenite grains may become coarse and not uniform, and the difference between the average packet size of bainite and the average grain size of ferrite may become too large. Therefore, the present invention sets the upper limit of the first cooling end temperature (T1) to T fm (℃) can be limited to -5℃.
[0065] 1st cooling rate (V C1 ) is not limited as long as it is a cooling rate applied to normal slow cooling, but can be limited to a range of 5 to 50° C. / s from the viewpoint of preventing defects in the steel sheet shape and ensuring the desired microstructure.
[0066] 2nd cooling The steel plate that has been first cooled is cooled at a second cooling rate (V C2 ) may be cooled. [Equation 5] T2(℃)≦750-270*[C]-90*[Mn] In the above Relational Formula 5, [C] and [Mn] respectively represent the contents (wt%) of carbon (C) and manganese (Mn) contained in the slab.
[0067] If the second cooling stop temperature (T2) exceeds a certain level, transformation to ferrite or pearlite occurs, making it impossible to obtain the microstructure targeted by the present invention, and as a result, it is possible that the targeted level of strength cannot be obtained. Therefore, the present invention can limit the upper limit of the second cooling stop temperature (T2) to 750-270*[C]-90*[Mn].
[0068] The second cooling is preferably performed at a rate faster than the first cooling, and more preferably the second cooling rate (V C2 The second cooling rate (V C2 If the cooling rate is less than 50°C / s, the transformation into ferrite or pearlite increases, which may cause a decrease in strength. In addition, a cooling rate of more than 500°C / s requires additional equipment, which is undesirable from an economical standpoint.
[0069] Third cooling and winding The steel plate that has been second-cooled is cooled at a third cooling rate (V C3 ), and then it can be wound up at the third cooling stop temperature (T3). [Equation 6] 540-423*[C]-30.4*[Mn]≦T3(℃) <T2(℃) In the above Relational Formula 6, T2 means the second cooling stop temperature (T2) of the second cooling stage, and [C] and [Mn] mean the contents (wt%) of carbon (C) and manganese (Mn) contained in the slab, respectively.
[0070] The third cooling is a cooling stage for controlling the coiling temperature, and the second cooling rate (V C2) the third cooling rate (V C3 ) to a third cooling stop temperature (T3) which is lower than the second cooling stop temperature (T2). C3 ) can be in the range of 5 to 50° C. / s.
[0071] However, if the third cooling end temperature (T3) is too low, low-temperature structures are formed excessively, making it impossible to ensure the desired microstructure and formability. Therefore, the present invention can limit the lower limit of the third cooling end temperature (T3) to 540-423*[C]-30.4*[Mn].
[0072] Heat Treatment The coiled steel sheet may be heated and maintained at a certain temperature for heat treatment. In order to ensure the temperature of the steel sheet in the subsequent coating process and to ensure stable carbide formation, the heat treatment may be performed at a temperature range of 450 to 720°C.
[0073] Plating After the heat treatment, a plating layer may be formed on at least one surface of the heat-treated steel sheet. The components and forming method of the plating layer of the present invention are not particularly limited, and may be interpreted as a concept including the components and forming methods of a plating layer typically provided for a hot-rolled plated steel sheet. As an example, the plating layer may be formed by any one method selected from a hot-dip plating method, an electroplating method, and a plasma method, and the plating layer may be any one plating layer selected from zinc, aluminum, a zinc-based alloy, and an aluminum-based alloy.
[0074] The hot-rolled steel sheet provided by the above-mentioned manufacturing method may contain, as a microstructure, 55 to 90 volume % of bainite and 10 to 45 volume % of ferrite, and may further contain one or more of 10 volume % or less (including 0%) of pearlite, 1 volume % or less (including 0%) of martensite, and 1 volume % or less (including 0%) of retained austenite. Of the carbides present in the bainite, the number of carbides with a major axis length of 25 to 500 nm per unit area is 3×10 6 pieces / mm2 or more, and the average aspect ratio (major axis / minor axis) of carbides present in the bainite may be 2.0 or less. Furthermore, the hot-rolled steel sheet provided by the above-mentioned manufacturing method may have an average packet size of bainite that is at the level of 50 to 200% of the average crystal grain size of ferrite.
[0075] The hot-rolled steel sheet provided by the above-mentioned manufacturing method has a thickness of 3 mm or less (excluding 0 mm) and can satisfy a yield strength (YS) of 550 MPa or more, a tensile strength (TS) of 650 MPa or more, and a bending workability (R / t) of 1.0 or less. In addition, the yield strength and thickness of the hot-rolled steel sheet provided by the above-mentioned manufacturing method can satisfy the following Relational Expression 2. [Equation 2] YS-100*t≧350 In the above Relational Formula 2, YS means the yield strength (MPa) of the hot-rolled steel sheet, and t means the thickness (mm) of the hot-rolled steel sheet. EXAMPLES
[0076] Hereinafter, the high strength hot rolled steel sheet and the manufacturing method thereof according to the present invention will be described in more detail with reference to specific examples. It should be noted that the following examples are for the purpose of understanding the present invention and are not intended to specify the scope of the present invention. The scope of the present invention is determined by the matters described in the claims and matters that can be reasonably inferred therefrom.
[0077] (Example) Hot-rolled steel sheets were manufactured from steel slabs having the alloy composition shown in Table 1 by applying the process conditions shown in Table 2. In Table 1, the remainder is iron (Fe) and unavoidable impurities, and the steel slab heating condition of 1200°C was commonly applied.
[0078] [Table 1]
[0079] [Table 2]
[0080] Thereafter, the microstructure of each test piece was observed, and the mechanical properties were measured and are listed in Table 3.
[0081] Each specimen was cut in a direction parallel to the rolling direction, and a specimen for microstructure observation was taken from the cut surface at 1 / 4 of the plate thickness. The samples thus taken were polished and etched with nital solution, and the microstructure of each specimen was observed using an optical microscope and a scanning electron microscope (SEM). The microstructure fraction was measured by image analysis. The average size of bainite packets and the average size of ferrite grains were measured at 1 / 4 of the plate thickness using electron backscatter diffraction (EBSD). The average size of bainite packets was measured by defining the position where the misorientation exceeded 15° as the grain boundary, and the average size of ferrite grains was measured using the Linear Intercept Method. In Table 3, F stands for ferrite, P stands for pearlite, B stands for bainite, M stands for martensite, and R-γ stands for retained austenite. A scanning electron microscope (SEM) was used at a magnification of 5000 times to obtain at least five electron microscope images of bainite in different regions of each sample, and a square region of 20 μm in width and length was calculated in each of the images obtained in this way to measure the size, number density, and average aspect ratio of carbides. In Table 3, the number density of carbides means the number density of carbides with a major axis length of 25 to 500 nm.
[0082] The tensile strength and yield strength were measured by performing a tensile test in the L direction for each test piece according to the DIN standard. The bending workability (R / t) was measured by applying a 90° V-bending test. After bending the test piece 90° with a V-shaped jig having different curvatures (R), the presence or absence of cracks in the bent part was measured.
[0083] [Table 3]
[0084] As shown in Tables 1 to 3, test pieces that satisfy all of the alloy compositions and process conditions of the present invention have a yield strength (YS) of 550 MPa or more, a tensile strength (TS) of 650 MPa or more, and a bending workability (R / t) of 1.0 or less. In contrast, it can be confirmed that test pieces that do not satisfy one or more of the alloy compositions or process conditions of the present invention do not simultaneously satisfy a yield strength (YS) of 550 MPa or more, a tensile strength (TS) of 650 MPa or more, and a bending workability (R / t) of 1.0 or less.
[0085] Although the present invention has been described in detail with reference to the embodiments, other embodiments are possible and the spirit and scope of the claims set forth below should not be construed as being limited to the embodiments.
Claims
1. A steel comprising, by mass%, carbon (C): 0.1-0.25%, manganese (Mn): 0.2-2.0%, silicon (Si): 0.3% or less, aluminum (Al): 0.05% or less, phosphorus (P): 0.05% or less, sulfur (S): 0.03% or less, nitrogen (N): 0.01% or less, titanium (Ti): 0.005-0.05%, boron (B): 0.0005-0.005%, niobium (Nb): 0.01% or less, molybdenum (Mo): 0.1% or less, and vanadium (V): 0.1% or less, with the remainder being iron (Fe) and unavoidable impurities; The microstructure contains, by volume fraction, 55 to 90% bainite and 10 to 45% ferrite; Among the carbides present in the bainite, the number of carbides having a major axis length of 25 to 500 nm per unit area is 3×10 6 pieces / mm 2 That's all. The average aspect ratio (major axis / minor axis) of carbides present in the bainite is 2.0 or less.
2. The hot-rolled steel sheet according to claim 1, wherein the hot-rolled steel sheet contains, by volume fraction, one or more of 10% or less (including 0%) pearlite, 1% or less (including 0%) martensite, and 1% or less (including 0%) retained austenite as a fine structure.
3. The hot-rolled steel sheet according to claim 1, wherein an average packet size of the bainite is 50 to 200% of an average crystal grain size of the ferrite.
4. The hot-rolled steel sheet according to claim 1, wherein the hot-rolled steel sheet satisfies the following relational expression 1. [Relationship 1] 30*[Ti]+100*[Nb]+5*[V]≦1.65 In the above Relational Formula 1, [Ti], [Nb] and [V] respectively represent the contents (mass%) of titanium (Ti), niobium (Nb) and vanadium (V) contained in the heat-rolled steel sheet.
5. The hot-rolled steel sheet according to claim 1, further comprising, by mass%, chromium (Cr): 0.2% or less.
6. The hot-rolled steel sheet according to claim 1, wherein the bendability (R / t) of the hot-rolled steel sheet is 1.0 or less.
7. The hot rolled steel sheet according to claim 1, wherein the hot rolled steel sheet has a yield strength (YS) of 550 MPa or more and a tensile strength (TS) of 650 MPa or more.
8. The hot-rolled steel sheet according to claim 1, wherein the thickness of the hot-rolled steel sheet is 3 mm or less (excluding 0 mm).
9. A steel sheet having a base steel sheet and a plating layer formed on at least one surface of the base steel sheet, The base steel sheet is a hot-rolled steel sheet according to any one of claims 1 to 8, The hot-rolled plated steel sheet, wherein the plating layer is any one selected from the group consisting of zinc, aluminum, a zinc alloy, and an aluminum alloy.
10. A slab heating step for heating a slab containing, by mass%, carbon (C): 0.1-0.25%, manganese (Mn): 0.2-2.0%, silicon (Si): 0.3% or less, aluminum (Al): 0.05% or less, phosphorus (P): 0.05% or less, sulfur (S): 0.03% or less, nitrogen (N): 0.01% or less, titanium (Ti): 0.005-0.05%, boron (B): 0.0005-0.005%, niobium (Nb): 0.01% or less, molybdenum (Mo): 0.1% or less, vanadium (V): 0.1% or less, with the remainder being iron (Fe) and unavoidable impurities; The heated slab is subjected to a rolling end temperature (T fm ) to provide a steel sheet; The hot-rolled steel sheet is cooled to a first cooling stop temperature (T 1 a first cooling stage of cooling to a temperature of 1000° C. at a first cooling rate; The steel sheet subjected to the first cooling is cooled to a second cooling stop temperature (T 2 a second cooling step of cooling the material at a second cooling rate of 50 to 500° C. / s which is faster than the first cooling rate; The second-cooled steel sheet is cooled to a third cooling stop temperature (T 3 a third cooling step of cooling the material at a third cooling rate slower than the second cooling rate to a temperature of 100° C.; The third-cooled hot-rolled steel sheet is cooled to the third cooling stop temperature (T 3 ) a winding step; and The method for producing a hot-rolled steel sheet according to claim 1, further comprising a heat treatment step of heat treating the coiled steel sheet at a temperature in the range of 450 to 720°C. [Relationship 3] T fm (℃)≧800+3000*[Ti]+10000*[Nb]-20*t (1/2) In the above Relational Formula 3, [Ti] and [Nb] respectively represent the contents (mass%) of titanium (Ti) and niobium (Nb) contained in the slab, and t represents the thickness (mm) of the hot-rolled steel plate. [Relationship 4] T fm (℃) -80℃≦T 1 (°C) ≦ T fm (℃) -5℃ In the above-mentioned Relational Formula 4, T fm is the rolling end temperature (T fm ) means [Relationship 5] T 2 (℃)≦750-270*[C]-90*[Mn] In the above Relational Formula 5, [C] and [Mn] respectively represent the contents (mass%) of carbon (C) and manganese (Mn) contained in the slab. [Relationship 6] 540-423*[C]-30.4*[Mn]≦T 3 (° C.) <T 2 (℃) In the above-mentioned Relational Formula 6, T 2 is the second cooling stop temperature (T 2 ), and [C] and [Mn] respectively represent the contents (mass%) of carbon (C) and manganese (Mn) contained in the slab.
11. The first cooling rate is 5 to 50° C. / s, The method for producing a hot-rolled steel sheet according to claim 10, wherein the third cooling rate is 5 to 50 ° C. / s.
12. The method for producing a hot-rolled steel sheet according to claim 10, wherein the slab satisfies the following relational expression 1. [Relationship 1] 30*[Ti]+100*[Nb]+5*[V]≦1.65 In the above Relational Formula 1, [Ti], [Nb] and [V] respectively represent the contents (mass%) of titanium (Ti), niobium (Nb) and vanadium (V) contained in the slab.
13. The method for producing a hot-rolled steel sheet according to claim 10, wherein the slab further contains, in mass%, chromium (Cr): 0.2% or less.
14. The method for producing a hot-rolled steel sheet according to claim 10, wherein the thickness of the hot-rolled steel sheet is 3 mm or less.
15. Providing a base steel sheet; and The method includes forming a coating layer on at least one surface of the base steel sheet by any one of a hot-dip coating method, an electroplating method, and a plasma coating method, The base steel sheet is provided by the manufacturing method according to any one of claims 10 to 14, The method for producing a hot-rolled plated steel sheet, wherein the plating layer is any one plating layer selected from the group consisting of zinc, aluminum, a zinc alloy, and an aluminum alloy.
Citation Information
Patent Citations
Process for manufacturing hot rolled pearlite-free steel strip and hot strip obtained thereby
EP1396549A1
High tensile hot rolled steel sheet having excellent peeling strength, and working method therefor
JP2002322542A
Hot rolled steel sheet having excellent working hardenability and method for producing the same
JP2005298967A
High-strength hot rolled steel sheet and its production method
JP2006161112A
Plated steel sheet with excellent surface quality, strength, and ductility