Boron diffusion method suitable for HBC batteries
The boron diffusion method with controlled gas injection and horizontal diffusion addresses the shallow junction and high concentration issues, resulting in improved efficiency and uniformity of N-type HBC batteries by forming a deep PN junction with reduced surface recombination.
Patent Information
- Application Number
- JP2023528697
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-02-02
- Filing Date
- 2021-05-27
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2041-05-27
AI Technical Summary
Existing boron diffusion processes for silicon wafers in solar cells result in shallow junction depth and high surface concentration, leading to reduced efficiency due to high-temperature oxidation and gas decomposition, which affects the quality of the PN junction.
A boron diffusion method involving controlled temperature and gas injection sequences, including nitrogen and oxygen alternation, to form a deep PN junction with reduced surface concentration, using a horizontal diffusion process with gravitational compression.
The method achieves a deeper junction depth and lower surface concentration, enhancing the front field effect and reducing surface recombination, thereby improving the efficiency and uniformity of N-type HBC batteries.
Smart Images

Figure 0007594110000004 
Figure 0007594110000005 
Figure 0007594110000006
Abstract
Description
[Technical field]
[0001] The present invention specifically relates to a boron diffusion method suitable for HBC batteries. [Background technology]
[0002] Silicon solar cells are the most widely used solar cells commercially among all solar cells. Photovoltaic solar cells can directly convert solar energy into electrical energy, and their power generation principle is the photovoltaic effect based on the PN junction of semiconductors.
[0003] P-type silicon wafers need to diffuse phosphorus elements to obtain PN junctions, and N-type silicon wafers need to diffuse boron elements to obtain PN junctions. In the production process of battery sheets, some steps require diffusing or depositing some elements on the silicon wafer to form a certain kind of thin layer structure, such as boron diffusion process, phosphorus diffusion process, low pressure boron diffusion process, low pressure phosphorus diffusion process, etc.
[0004] The diffusion process is one of the most important processes in manufacturing solar cells. The quality of the diffusion result directly affects the cell efficiency, and the criteria for evaluating the quality of the diffusion are sheet resistance, surface concentration and junction depth. When boron diffusion does not have a large effect on the contact resistance, the lower the surface concentration, the better, which can reduce the surface recombination rate and increase the on-voltage and current. The deep junction depth can increase the front field effect of N-type batteries, which is favorable for increasing FF.
[0005] The driving and bonding steps of the currently available boron diffusion process adopt a single high-temperature oxidation driving, which can rapidly reduce the surface concentration, and can precipitate boron on the silicon wafer surface by utilizing the interface displacement caused by the reaction of silicon and oxygen to produce silicon dioxide, thereby reducing the total doping amount of boron in silicon while driving at high temperature, and finally achieving the requirement of low surface concentration. However, this leads to a shallow junction depth and a weak front electric field effect.Is . Summary of the Invention [Problem to be solved by the invention]
[0006] In view of the above circumstances, in order to solve the existing technical deficiencies, the present invention provides a boron diffusion method suitable for HBC batteries. [Means for solving the problem]
[0007] In order to achieve the above objectives, the present invention provides the following technical solutions:
[0008] The boron diffusion method suitable for HBC batteries includes the following steps (1) to (8).
[0009] In the boat inserting step (1), silicon wafers are placed in the boat to perform the boat inserting step. During the boat inserting step, the furnace temperature is 700-750° C., and 2000 sccm of N2 is maintained to perform continuous purging.
[0010] In the heating and leak detection step (2), after the boat enters the furnace tube, it is heated to increase the temperature, the target temperature is 800-850°C, while the temperature is increased, vacuum is drawn, after the vacuum is completed, the vacuum pump is closed and vacuum leak detection is performed, the leak detection requirement is <5mbar / min, after the leak detection is completed, the vacuum pump is opened and the pressure of the furnace tube is adjusted, the target vacuum degree is 100-500mbar.
[0011] In the pre-oxidation step (3), after the target temperature and the target vacuum level are reached, oxygen is injected at 2000sccm to 10000sccm to perform pre-oxidation. The injection time is 10 to 30 minutes. A thin silicon oxide layer is grown on the silicon wafer surface by the pre-oxidation. This thin silicon oxide acts as a barrier layer to prevent damage to the silicon wafer surface by chlorides generated by the decomposition of BCl3 gas.
[0012] In the evacuation step (4), after the oxidation is completed, the furnace tube is evacuated, the evacuation time is 3-10 min, and the target pressure is <200 mabr.
[0013] In the step (5) of injecting and depositing boron source, BCl3 gas and O2 are injected at a gas volume ratio of BCl3:O2=1:1-1:3, and the injection time is 5-20 min. If the ratio is low, BCl3 cannot react with O2 completely, which causes the excess BCl3 to self-decompose, and a large amount of elemental boron is deposited on the surface of the silicon wafer to form a loss layer, and the decomposed Cl2 is likely to corrode the surface of the silicon wafer. If the ratio is high, the concentration of BCl3 will be insufficient, which will lead to uneven distribution of the gas source in the quartz furnace tube, resulting in poor uniformity throughout the tube.
[0014] In the heating step (6), after the boron source injection and deposition steps are completed, the quartz furnace tube is evacuated, and after the evacuation is completed, it is heated to increase the temperature, with the target temperature being 1000°C.
[0015] In the propulsion step (7), after the target temperature is reached, alternate injection and propulsion of N2 and O2 is used, and the N2 propulsion time:oxygen propulsion time for each time is 1:2 to 1:3, and preferably the N2 propulsion time for each time is 10 min to 25 min.
[0016] Preferably, N2 with a flow rate of 3 SLM to 10 SLM and O2 with a flow rate of 5 SLM to 20 SLM are used for each drive, and the number of drives is 2 to 5. By repeating the drive cycle, the amount of B source in the BSG can be significantly reduced while effectively guaranteeing a low surface concentration and a deep PN junction depth, and the minority carrier lifetime after B diffusion can be significantly improved, and the difficulty of subsequent processing steps can be reduced.
[0017] The O2 drive can ensure that the oxide layer continues to grow, and B atoms are continuously driven into the silicon body to ensure the doping concentration, but at the same time, the solubility of B atoms in silicon oxide is greater than that in silicon, and the continued growth of silicon oxide will cause a large amount of B to be absorbed into the silicon oxide layer, resulting in a high concentration of boron in the BSG, forming a boron-rich layer, and the reaction between the boron-rich layer and the acid will be slow, which is unfavorable for the subsequent cleaning operation. Therefore, the present invention needs to introduce N2 to drive and alternate with oxygen drive, so as to avoid that the long-term N2 drive will cause a high concentration of B atoms in the silicon wafer body, a high proportion of inactive B, and a dead layer will be formed, which will lead to severe surface recombination, a decrease in minority carrier life, and a decrease in cell efficiency.
[0018] In step (8) of decreasing the temperature and removing the boat, the temperature is decreased to 800° C. and the boat is removed to complete the diffusion process.
[0019] Furthermore, in step (2), the temperature increase rate is 10° C. / min.
[0020] Furthermore, in step (7), after the target temperature of 1000° C. is reached, nitrogen is injected at 3000 sccm / min for 10 minutes, oxygen is injected at 5000 sccm / min for 25 minutes, nitrogen is injected at 3000 sccm / min for 10 minutes, and oxygen is injected at 5000 sccm / min for 25 minutes. Effect of the Invention
[0021] The beneficial effects of the present invention are as follows:
[0022] (1) The present invention changes the driving step to a method of driving with a mixture of nitrogen and oxygen, and extends the driving time, which can effectively increase the junction depth and reduce the surface concentration. And by increasing the driving time of nitrogen, the concentration of B in BSG decreases, making it easier to completely remove BSG. The ECV results show that the junction depth is increased and the surface concentration is lower than that of the general boron diffusion method by using the method of the present invention.
[0023] (2) In the present invention, the concentration of B in BSG decreases due to the increase in the time of propelling nitrogen, and BSG can be more easily and completely removed. During cleaning, the concentration of the chemical solution is HO:HF=20:1 (volume ratio), the temperature is room temperature, and the cleaning time of BSG is reduced from the conventional 600 s to 500 s, a reduction of 100 s.
[0024] (3) The method of the present invention has excellent front doping ability, low dead layer and good light absorption ability for N-type batteries. In addition, the present invention adopts a horizontal diffusion method and has good single-sidedness, and utilizes a gravity compression method (gravity compression is a method of diffusing boron by placing sheets horizontally, stacking two adjacent sheets together, and the upper sheet presses the lower one by gravity) to place silicon wafers back to back in a horizontal groove, and the silicon wafers are compressed by the gravity of the upper silicon wafer, so that the deformation amount after high-temperature heating is very small, and the occurrence of rolling-up is effectively prevented, and even during diffusion, the diffusion of B to the back side is reduced, and the rolling-up on the back side is greatly reduced, which is particularly important for high-efficiency batteries with high requirements for single-sidedness.
[0025] (4) The diffusion method of the present invention is particularly suitable for N-type HBC high-efficiency batteries. The back surface process of HBC batteries is complicated. The excellent single-sidedness and excellent BSG layer can greatly reduce the difficulty of subsequent processing steps, which is favorable for the industrialization of HBC products. [Brief description of the drawings]
[0026] [Figure 1]FIG. 2 is an ECV diagram of boron diffusion in the method of the present invention and the method of Comparative Example 1. [Diagram 2] 1 is a PL photograph of a photovoltaic cell after adopting the boron diffusion method in Comparative Example 1 and Example 1. [Diagram 3] This is the test position at the time of sampling detection. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0027] Hereinafter, the technical solution of the present invention will be described in more detail with reference to the drawings. The specific embodiments are merely detailed descriptions of the present invention and should not be regarded as limiting the present invention.
[0028] Example 1 The boron diffusion method suitable for HBC batteries includes steps (1) to (8).
[0029] In the boat loading step (1), the silicon wafers after felting and cleaning are placed in a horizontal sheet-insertion type quartz boat, and the silicon wafers are inserted back-to-back into a horizontal quartz groove to perform the boat loading step. During the boat loading, the temperature of the quartz furnace tube is 700°C, and 2000 sccm of N2 is maintained for continuous purging.
[0030] In the heating and leak detection step (2), the silicon wafers and the quartz boat are placed in a quartz furnace tube, and then heated at a heating rate of 10°C / min to increase the temperature, with the target temperature being 850°C. During the heating, the furnace tube is evacuated using a vacuum pump. After the evacuation is completed, the vacuum pump is closed to perform vacuum leak detection, with the leak detection requirement being <5mbar / min. After the leak detection is completed, the vacuum pump is opened to adjust the pressure in the furnace tube, with the target vacuum being 200mbar.
[0031] In the pre-oxidation step (3), after the target temperature and the target vacuum are reached, 2000 sccm of oxygen is injected to perform pre-oxidation. The injection time is 10 minutes. A thin silicon oxide layer is grown on the silicon wafer surface by the pre-oxidation. This thin silicon oxide acts as a barrier layer to prevent the chloride generated by the decomposition of BCl3 gas from damaging the silicon wafer surface.
[0032] (4) After the oxidation is completed, a vacuum is pulled on the furnace tube to extract the oxygen in the furnace tube, with a target pressure of <200 mabr to prevent excess oxygen remaining in the furnace tube to consume the BCl3 source when the boron source is injected in the next step.
[0033] In the step (5) of injecting and depositing the boron source, BCl3 gas and oxygen are injected at a certain rate, the gas volume ratio is BCl3:O2=1:1, and the injection time is 20 min. If the rate is low, BCl3 cannot react with O2, which causes the excess BCl3 to self-decompose, and a large amount of elemental boron is deposited on the surface of the silicon wafer to form a loss layer, and the decomposed Cl2 is likely to corrode the surface of the silicon wafer. If the rate is high, the concentration of BCl3 will be insufficient, which will lead to uneven distribution of the gas source in the quartz furnace tube, resulting in poor uniformity throughout the tube.
[0034] In the heating step (6), after the step of injecting and depositing the boron source is completed, the quartz furnace tube is subsequently evacuated to extract BCl3 and oxygen from the furnace tube, the target pressure is <100 mbar, and after the evacuation is completed, the temperature is increased by heating, the target temperature is 1000°C.
[0035] In the propulsion step (7), after the target temperature is reached, the process proceeds to the propulsion step, in which alternate injection and propulsion of N2 and O2 is used, with nitrogen injected at 3000 sccm / min for 10 min, oxygen injected at 5000 sccm / min for 25 min, nitrogen injected at 3000 sccm / min for 10 min, and oxygen injected at 5000 sccm / min for 25 min.
[0036] In step (8) of decreasing the temperature and removing the boat, the temperature is decreased to 800° C. and the boat is removed to complete the diffusion process.
[0037] Example 2 The boron diffusion method suitable for HBC batteries includes steps (1) to (8).
[0038] In the boat loading step (1), the silicon wafers after felting and cleaning are placed in a horizontal sheet-loading quartz boat, and the silicon wafers are inserted back-to-back into a horizontal quartz groove to perform the boat loading step. During the boat loading, the temperature of the quartz furnace tube is 750°C, and 2000 sccm of N2 is maintained for continuous purging.
[0039] In the heating step (2), the silicon wafers and the quartz boat are placed in a quartz furnace tube, and then heated at a heating rate of 10°C / min to increase the temperature, with the target temperature being 800°C. During the heating, the furnace tube is evacuated using a vacuum pump. After the evacuation is completed, the vacuum pump is closed to perform vacuum leak detection, with the leak detection requirement being <5mbar / min. After the leak detection is completed, the vacuum pump is opened to adjust the pressure in the furnace tube, with the target vacuum being 500mbar.
[0040] In the pre-oxidation step (3), after the target temperature and the target vacuum are reached, 5000 sccm of oxygen is injected to perform pre-oxidation for 20 minutes. A thin silicon oxide layer is grown on the silicon wafer surface by the pre-oxidation. This thin silicon oxide acts as a barrier layer to prevent the chloride generated by the decomposition of BCl3 gas from damaging the silicon wafer surface.
[0041] (4) After the oxidation is completed, a vacuum is applied to the furnace tube to extract the oxygen in the furnace tube, with a target pressure of <200 mabr to prevent excess oxygen from remaining in the furnace tube and consuming the BCl3 source when the boron source is injected in the next step.
[0042] In the step (5) of injecting and depositing the boron source, BCl3 gas and oxygen are injected at a certain rate, the volume ratio of the gas is BCl3:O2=1:3, and the injection time is 10 min. If the rate is low, BCl3 cannot react with O2, which causes the excess BCl3 to self-decompose, and a large amount of elemental boron is deposited on the surface of the silicon wafer to form a loss layer, and the decomposed Cl2 is likely to corrode the surface of the silicon wafer. If the rate is high, the concentration of BCl3 will be insufficient, which will lead to uneven distribution of the gas source in the quartz furnace tube, resulting in poor uniformity throughout the tube.
[0043] (6) After the step of injecting and depositing the boron source is completed, the quartz furnace tube is subsequently evacuated to extract the BCl3 and oxygen in the furnace tube, with the target pressure being <100 mbar. After the evacuation is completed, the furnace tube is heated to increase the temperature, with the target temperature being 1000°C.
[0044] (7) After the target temperature is reached, proceed to the propulsion step, in which N2 and O2 alternate injection and propulsion is used, injecting 4000 sccm of nitrogen for 10 min, injecting 6000 sccm of oxygen for 30 min, injecting 4000 sccm of nitrogen for 10 min, and injecting 6000 sccm of oxygen for 30 min.
[0045] Example 3 The boron diffusion method suitable for HBC batteries includes steps (1) to (8).
[0046] In the boat loading step (1), the silicon wafers after felting and cleaning are placed in a horizontal sheet-loading quartz boat, and the silicon wafers are inserted back-to-back into a horizontal quartz groove to perform the boat loading step. During the boat loading, the temperature of the quartz furnace tube is 720°C, and 2000 sccm of N2 is maintained for continuous purging.
[0047] In the heating and leak detection step (2), the silicon wafers and the quartz boat are placed in a quartz furnace tube, and then heated at a heating rate of 10°C / min to increase the temperature, with the target temperature being 820°C. As the temperature increases, the furnace tube is evacuated using a vacuum pump. After the evacuation is completed, the vacuum pump is closed to perform vacuum leak detection, with the leak detection requirement being <5mbar / min. After the leak detection is completed, the vacuum pump is opened to adjust the pressure in the furnace tube, with the target vacuum being 100mbar.
[0048] In the pre-oxidation step (3), after the target temperature and the target vacuum are reached, 6000 sccm of oxygen is injected to perform pre-oxidation. The injection time is 10 minutes. A thin silicon oxide layer is grown on the silicon wafer surface by pre-oxidation. This thin silicon oxide acts as a barrier layer to prevent the chloride generated by the decomposition of BCl3 gas from damaging the silicon wafer surface.
[0049] (4) After the oxidation is completed, a vacuum is pulled on the furnace tube to extract the oxygen in the furnace tube, with a target pressure of <200 mabr to prevent excess oxygen remaining in the furnace tube to consume the BCl3 source when the boron source is injected in the next step.
[0050] In the step (5) of injecting and depositing boron source, BCl3 gas and oxygen are injected at a certain ratio, the gas volume ratio is BCl3:O2=1:2, and the injection time is 15 min. If the ratio is low, BCl3 cannot react with O2, which causes the excess BCl3 to self-decompose, and a large amount of elemental boron is deposited on the surface of the silicon wafer to form a loss layer, and the decomposed Cl2 is very likely to corrode the surface of the silicon wafer. If the ratio is high, the concentration of BCl3 will be insufficient, which will lead to uneven distribution of the gas source in the quartz furnace tube, and therefore poor uniformity throughout the tube.
[0051] In the heating step (6), after the step of injecting and depositing the boron source is completed, the quartz furnace tube is subsequently evacuated to extract BCl3 and oxygen from the furnace tube, the target pressure is <100 mbar, and after the evacuation is completed, the temperature is increased by heating, the target temperature is 1000°C.
[0052] In the propulsion step (7), after the target temperature is reached, the process proceeds to the propulsion step, in which N2 and O2 are alternately injected and propelled, with nitrogen injected at 3000 sccm / min for 10 min, oxygen injected at 5000 sccm / min for 30 min, nitrogen injected at 3000 sccm / min for 10 min, and oxygen injected at 5000 sccm / min for 30 min.
[0053] In step (8) of decreasing the temperature and removing the boat, the temperature is decreased to 800° C. and the boat is removed to complete the diffusion process.
[0054] Comparative Example 1 In this comparative example, the specific steps of boron diffusion are as shown in Table 1.
[0055] As can be seen from Figure 1, the results obtained using the diffusion method of the present invention show that the junction depth is increased and the surface concentration is lower than that of the boron diffusion in the comparative example, as can be seen from the ECV (electrochemical differential capacitance voltage) results. In Figure 1, the difference in the latter stages of the two methods is mainly due to the difference in junction depth, and the surface concentration mainly refers to the concentration at a position of 0 to 0.05 μm deep on the surface.
[0056] [Table 1] [Table 2]
[0057] [Table 3]
[0058] As can be seen from Table 2 and FIG. 1, by adopting the novel boron diffusion method of the present invention, a deep PN junction and a low surface doping concentration can be obtained. The low surface doping concentration can reduce the surface recombination velocity of the solar cell and improve the on-state voltage and current. The deep junction depth can enhance the front field effect of the N-type HBC cell and is favorable for improving the FF.
[0059] Before unloading the sheet (i.e. unloading the silicon wafer from the quartz boat), sampling detection was performed on the silicon wafer at different positions on the quartz boat, the test positions are shown in Figure 3, and the test results are as shown in Table 3. As can be seen from the data in Table 3, the method of the present invention has excellent intra-sheet and inter-sheet diffusion uniformity, can further improve the conformity of the PN junction, and is favorable for lateral carrier transport. Figure 2 is a photograph of the PL (photoluminescence) of a photovoltaic cell after boron diffusion using the methods in Comparative Example 1 and Example 1. As can be seen from Figure 2, the example corresponding to the present invention has better PL brightness and uniformity.
[0060] Apparently, the described embodiments are only some of the embodiments of the present invention, but not all of the embodiments. Based on the embodiments of the present invention, all other embodiments made by those skilled in the art without inventive efforts fall within the protection scope of the present invention.
Claims
1. A boron diffusion method suitable for an HBC battery, comprising the following steps (1) to (8): In the boat loading step (1), the silicon wafer is placed in the boat to perform the boat loading step. When the boat is loaded, the temperature of the furnace tube is 700-750° C., and 2000 sccm of N 2 To maintain the pressure, purge continuously. In the heating and leak detection step (2), the boat is heated after entering the furnace tube to raise the temperature, the target temperature is 800-850°C, while the temperature is raised, vacuum drawing is performed, after the vacuum drawing is completed, the vacuum pump is closed to perform vacuum leak detection, the leak detection requirement is <5mbar / min, after the leak detection is completed, the vacuum pump is opened to adjust the pressure of the furnace tube, the target vacuum degree is 100-500mbar; In the pre-oxidation step (3), after the target temperature and the target vacuum are reached, oxygen is injected at 2000 sccm to 10000 sccm to perform pre-oxidation, and the injection time is 10 to 30 minutes. In the evacuation step (4), after the oxidation is completed, the furnace tube is evacuated, the evacuation time is 3-10 min, and the target pressure is <200 mbar; In the step (5) of injecting and depositing a boron source, BCl 3 :O 2 = BCl at a gas volume ratio of 1:1 to 1:3 3 Gas and O 2 is injected, the injection time is 5 to 20 minutes, In the heating step (6), after the step of injecting and depositing the boron source is completed, the furnace tube is evacuated to a target pressure of <100 mbar, and after the evacuation is completed, the furnace tube is heated to a target temperature of 1000° C.; In the promotion step (7), after the target temperature is reached, N 2 Injection and promotion of O 2 The injection and thrust of N 2 was alternated, and each injection and thrust of N 2 and each injection and thrust of O 2 were counted as one time. 2 Propulsion time: Oxygen propulsion time = 1:2 to 1:3, and N with a flow rate of 3 SLM to 10 SLM each time it is propelled 2 , O flow rate of 5 SLM to 20 SLM 2 The cycle is repeated 2 to 4 times. In step (8) of reducing the temperature and releasing the boat, the temperature is reduced and the boat is released to complete the diffusion process. A boron diffusion method suitable for an HBC battery, comprising:
2. 2. The boron diffusion method suitable for HBC batteries according to claim 1, wherein in step (2), the temperature rise rate is 10° C. / min.
3. In step (7), after the target temperature of 1000° C. is reached, 3000 sccm of nitrogen is injected for 10 min, 5000 sccm of oxygen is injected for 25 min, 3000 sccm of nitrogen is injected for 10 min, and 5000 sccm of oxygen is injected for 25 min.
2. A boron diffusion method suitable for an HBC battery according to claim 1.
Citation Information
Patent Citations
Multi-step boron diffusion process for N-type solar cell
CN109545893A
N-type solar cell boron diffusion method
CN111341649A
Process method for depositing and doping surface of silicon wafer
CN111403271A
Method for diffusing impurity in semiconductor wafer, semiconductor wafer and silicon epitaxial wafer
JP2003017428A
Boron doping of silicon wafers
JP2012523127A