Steel materials
A steel material with controlled elemental composition addresses surface peeling and shape stability challenges in large bearings by promoting fine V precipitates and optimizing machinability, enhancing performance under high pressure and foreign object conditions.
Patent Information
- Application Number
- JP2020147896
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-09-02
- Publication Date
- 2024-12-04
- Estimated Expiration
- 2040-09-02
AI Technical Summary
Medium- and large-sized bearing parts used in mining and construction machinery face challenges with surface peeling life and shape stability due to exposure to foreign objects and high surface pressures, which existing technologies do not adequately address.
A steel material with a specific chemical composition and controlled content of elements (C, Si, Mn, Cr, Mo, V, Al, Ca, P, S, N, O, and optionally Ni, B, Nb, Ti) that satisfies formulas (1) to (3), promoting fine V precipitates and suppressing coarse ones, ensuring excellent machinability, surface-originated flaking life, and shape stability.
The steel material exhibits enhanced machinability, surface-originated flaking life, and shape stability under high surface pressures, effectively addressing deformation and noise issues in bearing components.
Smart Images

Figure 0007594169000003 
Figure 0007594169000001 
Figure 0007594169000002
Abstract
Description
[Technical field]
[0001] The present disclosure relates to steel materials, and more particularly to steel materials that are used as raw materials for bearing components. [Background technology]
[0002] Small bearing parts are used in automobiles, while medium and large bearing parts are used in mining and construction machinery. As steel materials for such medium and large bearing parts, bearing steels such as SUJ3 and SUJ5 specified in JIS G 4805 (2019) and case hardened steels such as SNCM815 specified in JIS G 4053 (2016) are used. These steel materials are manufactured into bearing parts by the following method. Hot processing (hot forging) is performed on the steel material, and spheroidizing annealing is performed on the hot processed steel material. Cutting processing or the like is performed on the steel material after spheroidizing annealing to manufacture an intermediate product of a desired shape. Heat treatment is performed on the intermediate product to adjust the hardness and microstructure of the steel material. The heat treatment is, for example, quenching and tempering, carburizing quenching and tempering, carburizing nitriding quenching and tempering, or nitriding quenching and tempering. Through the above process, bearing parts having desired bearing performance (surface initiated spalling life, etc.) are manufactured using the above-mentioned steel material. As described above, in the manufacturing process of bearing parts, cutting is performed after hot working and spheroidizing annealing. Therefore, the steel material is required to have excellent machinability.
[0003] Furthermore, in the manufacturing process of bearing parts manufactured using steel as a raw material, the above-mentioned heat treatments (quenching and tempering, carburizing, quenching and tempering, carbonitriding, quenching and tempering, nitriding, quenching and tempering, etc.) are carried out in order to obtain bearing performance, particularly surface initiated spalling life, etc. In the heat treatment, a hardened layer, such as a quenched layer, a carburized layer, a carbonitrided layer, or a nitrided layer, is formed on the surface layer of the steel. This hardened layer improves bearing performance, such as an improvement in the surface initiated spalling life.
[0004] Techniques relating to improving bearing performance are disclosed in Japanese Patent Laid-Open Publication No. 8-49057 (Patent Document 1) and Japanese Patent Laid-Open Publication No. 2008-280583 (Patent Document 2).
[0005] The rolling bearing disclosed in Patent Document 1 is composed of raceways and rolling elements. At least one of the raceways and rolling elements is made of a low-carbon low-alloy steel containing 0.1-0.7% by weight of C, 0.5-3.0% by weight of Cr, 0.3-1.2% by weight of Mn, 0.3-1.5% by weight of Si, and 3% by weight or less of Mo, and contains 0.8-2.0% by weight of V. A carburizing or carbonitriding process is performed during heat treatment of a product formed using the material, so that the carbon concentration of the product surface is 0.8-1.5% by weight and the V / C concentration ratio of the surface satisfies the relationship of 1-2.5. As a result, in the rolling bearing of Patent Document 1, VC carbides are precipitated on the product surface. Patent Document 1 states that the rolling bearing of Patent Document 1 therefore enhances wear resistance, which is one of the bearing performances.
[0006] The case-hardened steel disclosed in Patent Document 2 contains, by mass%, C: 0.1 to 0.4%, Si: 0.5% or less, Mn: 1.5% or less, P: 0.03% or less, S: 0.03% or less, Cr: 0.3 to 2.5%, Mo: 0.1 to 2.0%, V: 0.1 to 2.0%, Al: 0.050% or less, O: 0.0015% or less, N: 0.025% or less, V + Mo: 0.4 to 3.0%, with the balance being Fe and unavoidable impurities. In this case-hardened steel, the surface layer C concentration after tempering is 0.6 to 1.2%, the surface hardness is HRC58 or more but less than 64, and the number ratio of fine V-based carbides with a grain size of less than 100 nm among the V-based carbides dispersed and precipitated in the surface layer is 80% or more. Patent Document 2 describes that by finely dispersing V-based carbides in components such as bearings to serve as hydrogen trapping sites, hydrogen embrittlement resistance is improved and the surface fatigue life, which is one aspect of bearing performance, is increased. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Japanese Patent Application Publication No. 8-49057 [Patent Document 2] JP 2008-280583 A Summary of the Invention [Problem to be solved by the invention]
[0008] Meanwhile, medium-sized and large-sized bearing parts applied to mining machinery and construction machinery are used in environments containing soil and rocks. Therefore, parts of soil and rocks may enter the bearing as foreign matter during use of the bearing parts. Even in a state where such foreign matter is mixed in, an excellent surface initiated spalling life is required. Patent Documents 1 and 2 do not disclose any technology for improving the surface initiated spalling life due to the above-mentioned foreign matter mixing in.
[0009] Furthermore, in the case of medium-sized and large-sized bearing parts for mining and construction machinery, a significantly higher surface pressure is repeatedly applied during use compared to small-sized bearing parts for automobiles. Recently, in order to further improve fuel efficiency, the viscosity of the lubricating oil has been reduced to reduce frictional resistance and transmission resistance, and the amount of lubricating oil used to circulate has been reduced. The reduction in the viscosity of the lubricating oil and the reduction in the amount of lubricating oil used reduces the thickness of the lubricating oil film on the contact surfaces between the bearing parts. In this case, the pressure applied per unit area of the bearing parts (hereinafter also referred to as surface pressure) becomes higher compared to when the viscosity of the lubricating oil is high and when the amount of lubricating oil used is large. When such a high surface pressure is repeatedly applied, the bearing parts may be deformed by the surface pressure. For example, if the deformation amount of the rolling surface of the bearing increases, the gap between the rolling elements (balls, rollers) and the inner and outer rings increases. In this case, the bearing cannot support the rotating member (shaft, etc.) so that it can rotate at an accurate position. As a result, vibration occurs in the bearing and the members supported by the bearing, and this vibration causes noise. Therefore, bearing parts for these applications are particularly required to have the property of being resistant to deformation and change in shape even when high surface pressure is repeatedly applied during use (hereinafter referred to as shape stability).
[0010] An object of the present disclosure is to provide a steel material that has excellent machinability and, when made into a bearing component, has excellent surface initiated spalling life and shape stability. [Means for solving the problem]
[0011] The steel material according to the present disclosure is Chemical composition, in mass%, C: 0.50-0.80%, Si: 0.30-1.50%, Mn: 0.20-0.40%, Cr: 0.30~1.25%, Mo: 0.10-0.30%, V: 0.20-0.40%, Al: 0.005 to 0.100%, Ca: 0.0002 to 0.0010%, P: 0.020% or less, S: 0.005% or less, N: 0.0300% or less, O: 0.0015% or less, and The balance is Fe and impurities, and satisfies the formulas (1) to (3). 1.20<0.4Cr+0.4Mo+4.5V<2.40 (1) 75C+35Si+150Mn+30Ni+60Cr+115Mo+50(V+Ti+Nb)≦255 (2) 30C+18Si+20Cr+35Mn+15Ni≦85 (3) Here, the content (mass%) of the corresponding element is substituted for each element symbol in formulas (1) to (3). When the corresponding element is not contained, "0" is substituted for the element symbol. Effect of the Invention
[0012] The steel material according to the present disclosure has excellent machinability, and when made into a bearing component, has excellent surface initiated spalling life and shape stability. [Brief description of the drawings]
[0013] [Figure 1] FIG. 1 is a schematic diagram of a thrust-type rolling fatigue testing machine. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The inventors investigated and examined the machinability of steel, which is the material for bearing components, the surface-initiated spalling life of bearing components when the steel is machined into bearing components, and the shape stability of the bearing components when they are in use.
[0015] First, the inventors investigated a steel material that has excellent machinability, surface initiated spalling life, and shape stability when used as a bearing part from the viewpoint of chemical composition. As a result, the chemical composition was found to be, in mass%, C: 0.50-0.80%, Si: 0.30-1.50%, Mn: 0.20-0.40%, Cr: 0.30-1.25%, Mo: 0.10-0.30%, V: 0.20-0.40%, Al: 0.005-0.100%, Ca: 0.0002-0.0010%, P: 0.020% or less, S: 0.005% or less, N: 0.005% or less, and Si: 0.005% or less. The inventors considered that a steel material containing C12: 0.0300% or less, O: 0.0015% or less, Ni: 0-2.00%, B: 0-0.0100%, Nb: 0-0.1000%, and Ti: 0-0.1000%, with the balance being Fe and impurities, would have excellent machinability and, when made into a bearing part, would likely have excellent surface initiated spalling life and shape stability.
[0016] However, it was found that even if the elements in the chemical composition of the steel material are within the above-mentioned ranges, the above-mentioned properties (machinability, surface initiated spalling life when used as a bearing part, and shape stability) may not be fully obtained. Therefore, the present inventors conducted further studies. As a result, the following findings were obtained.
[0017] [Regarding formula (1)] As described above, when manufacturing bearing parts using steel as a raw material, quenching and tempering, carburizing, quenching and tempering, carbo-nitriding, quenching and tempering, or nitriding, quenching and tempering are performed on the steel (intermediate product) that has been subjected to hot working and cutting. In the following explanation, quenching and tempering, carburizing, quenching and tempering, carbo-nitriding, quenching and tempering, and nitriding, quenching and tempering are collectively referred to as "heat treatment." In order to increase the surface initiated spalling life of the bearing part obtained by performing heat treatment on the steel, it is effective to disperse fine precipitates in the surface layer of the bearing part.
[0018] V forms precipitates such as carbides and carbonitrides. Hereinafter, precipitates containing V are referred to as "V precipitates". V precipitates include V carbides and V carbonitrides. If V precipitates are formed during heat treatment, they are fine. If fine V precipitates are formed on the surface layer of a bearing part, the surface layer of the bearing part becomes hard due to precipitation strengthening. As a result, the surface initiated spalling life of the bearing part is increased. However, coarse V precipitates (V carbides) may be formed during heating in hot working. In this case, coarse V precipitates remain in the bearing part. Coarse V precipitates are likely to become the starting point of fatigue fracture during use of the bearing part, and rather reduce the surface initiated spalling life of the bearing part. Furthermore, since coarse V precipitates are hard, when cutting steel (intermediate product) after hot working, the machinability of the steel decreases.
[0019] Therefore, the present inventors have investigated means for generating fine V precipitates and suppressing the generation of coarse V precipitates, and as a result, have obtained the following findings.
[0020] In order to generate fine V precipitates, it is effective to increase the number of precipitation nucleation sites. Cr and Mo increase the number of precipitation nucleation sites for generating fine V precipitates during heat treatment. As a result, Cr and Mo promote the dispersion and generation of fine V precipitates during heat treatment. However, V precipitates already exist in the steel material that is the material for the bearing part. Therefore, if the V precipitates in the steel material are not sufficiently dissolved during heating in the hot working process that precedes the heat treatment process in the manufacturing process of the bearing part, the V precipitates in the steel material will become coarse due to heating. In this case, even if the heat treatment process is performed, coarse V precipitates will remain in the bearing part. If the V content, Cr content, and Mo content are too high, many V precipitates already exist in the steel material that is the material for the bearing part, so that coarse V precipitates are likely to remain when the bearing part is made. Therefore, in order to disperse fine V precipitates in a bearing component while suppressing the remaining of coarse V precipitates in the bearing component, it is effective to appropriately adjust the V content, Cr content, and Mo content in the chemical composition of the steel material.
[0021] Based on the above findings, the inventors investigated the relationship between the V content, the Cr content, and the Mo content and the surface initiated spalling life. As a result, they found that in a steel material in which the contents of each element in the chemical composition are within the above-mentioned ranges, if the V content, the Cr content, and the Mo content further satisfy the following formula (1), a sufficient surface initiated spalling life can be obtained when the steel material is used as a bearing part, on the premise that the later-described formulas (2) and (3) are satisfied. 1.20<0.4Cr+0.4Mo+4.5V<2.40 (1) Here, the content (mass %) of each element in formula (1) is substituted for the corresponding element symbol.
[0022] [Regarding formula (2)] In the manufacturing process of the bearing parts, as described above, cutting is performed on the steel material after hot working and spheroidizing annealing to manufacture an intermediate product. Therefore, the present inventors have further studied the machinability of the steel material. The strength of the steel material affects the machinability. Specifically, if the strength of the steel material is high, the machinability decreases. Therefore, in order to improve the machinability of the steel material, it is effective to prevent the strength of the steel material from becoming excessively high. Among the elements in the above-mentioned chemical composition, C, Si, Mn, Ni, Cr, Mo, V, Ti, and Nb are elements that particularly increase the strength of the steel material. Therefore, the present inventors have focused on these elements and studied the improvement of the machinability of the steel material. As a result, it has been found that if the content of each element in the chemical composition is within the above-mentioned range and C, Si, Mn, Ni, Cr, Mo, V, Ti, and Nb satisfy the following formula (2), the machinability of the steel material is further improved, assuming that formula (1) and formula (3) described later are satisfied. 75C+35Si+150Mn+30Ni+60Cr+115Mo+50(V+Ti+Nb)≦255 (2) Here, the content (mass%) of the corresponding element is substituted for each element symbol in formula (2). When the corresponding element is not contained, "0" is substituted for the element symbol.
[0023] [Regarding formula (3)] As described above, in medium-sized and large-sized bearing parts for mining and construction machinery, a significantly high surface pressure is repeatedly applied during use. As a result, the bearing parts may be deformed due to the surface pressure. Therefore, the bearing parts are required to have excellent shape stability during use.
[0024] Therefore, the present inventors investigated factors that affect the shape stability of bearing parts manufactured using steel as a material, and found that when retained austenite remains in the core of a bearing part after heat treatment, the bearing part may be deformed by repeatedly applying high surface pressure.
[0025] Based on the above findings, the present inventors investigated elements that particularly affect the generation of retained austenite in the core when a bearing part is manufactured using a steel material having the above-mentioned chemical composition as a raw material. As a result, it was found that, when the content of each element in the chemical composition is within the above-mentioned range, C, Si, Cr, Mn, and Ni in particular affect the amount of retained austenite generated in the core of a bearing part obtained by performing hot working, cutting, and heat treatment using a steel material as a raw material. Therefore, the present inventors further investigated the relationship between the C content, Si content, Cr content, Mn content, and Ni content, and the shape stability of the bearing part when made into a bearing part. As a result, it was found that, if the content of each element in the chemical composition is within the above-mentioned range and C, Si, Cr, Mn, and Ni satisfy the following formula (3), the steel material has excellent machinability, and when made into a bearing part, the bearing part not only has excellent surface-initiated spalling life, but also has excellent shape stability, provided that formulas (1) and (2) are satisfied. 30C+18Si+20Cr+35Mn+15Ni≦85 (3) Here, the content (mass%) of the corresponding element is substituted for each element symbol in formula (3). When the corresponding element is not contained, "0" is substituted for the element symbol.
[0026] The steel material of this embodiment has been completed based on the above technical concept. Specifically, the steel material of this embodiment is a steel material that can be used as a material for bearing parts, and has the following configuration.
[0027] [1] Chemical composition, in mass%, C: 0.50-0.80%, Si: 0.30-1.50%, Mn: 0.20-0.40%, Cr: 0.30~1.25%, Mo: 0.10-0.30%, V: 0.20-0.40%, Al: 0.005 to 0.100%, Ca: 0.0002 to 0.0010%, P: 0.020% or less, S: 0.005% or less, N: 0.0300% or less, O: 0.0015% or less, and the remainder being Fe and impurities and satisfying formulas (1) to (3); Steel material. 1.20<0.4Cr+0.4Mo+4.5V<2.40 (1) 75C+35Si+150Mn+30Ni+60Cr+115Mo+50(V+Ti+Nb)≦255 (2) 30C+18Si+20Cr+35Mn+15Ni≦85 (3) Here, the content (mass%) of the corresponding element is substituted for each element symbol in formulas (1) to (3). When the corresponding element is not contained, "0" is substituted for the element symbol.
[0028] [2] The steel material according to [1], The chemical composition further contains, in place of a portion of Fe, Ni: 2.00% or less, B: 0.0100% or less, Nb: 0.1000% or less, and Ti: 0.1000% or less, containing one or more selected from the group consisting of Steel material.
[0029] The steel material of this embodiment will be described in detail below. "%" for elements means mass % unless otherwise specified.
[0030] [Chemical composition of steel] The steel material of this embodiment is suitable as a material for bearing parts manufactured by carrying out heat treatment. The heat treatments referred to here include quenching and tempering, carburizing, quenching and tempering, carbo-nitriding, quenching and tempering, and nitriding, quenching and tempering, etc. The chemical composition of the steel material of this embodiment contains the following elements.
[0031] C: 0.50-0.80% Carbon (C) increases the strength of the steel material. Furthermore, when the steel material is used as a bearing part, C forms fine V precipitates, and increases the surface-initiated spalling life of the bearing part. If the C content is less than 0.50%, the above effect cannot be sufficiently obtained even if the contents of other elements are within the range of this embodiment. On the other hand, if the C content exceeds 0.80%, even if the contents of other elements are within the range of this embodiment, the strength of the steel material becomes excessively high, and the machinability of the steel material decreases. If the C content exceeds 0.80%, furthermore, when the steel material is used as a bearing part, coarse V precipitates remain in the bearing part. In this case, the surface-initiated spalling life of the bearing part is rather reduced. Therefore, the C content is 0.50 to 0.80%. The preferable lower limit of the C content is 0.55%, and more preferably 0.60%. The preferable upper limit of the C content is 0.77%, and more preferably 0.75%.
[0032] Silicon: 0.30 to 1.50% Silicon (Si) increases the strength of a steel material and increases the surface-initiated spalling life of a bearing part when the steel material is used as a bearing part. If the Si content is less than 0.30%, the above effect cannot be sufficiently obtained even if the contents of other elements are within the range of this embodiment. On the other hand, if the Si content exceeds 1.50%, the strength of the steel material becomes excessively high and the machinability of the steel material decreases even if the contents of other elements are within the range of this embodiment. Therefore, the Si content is 0.30 to 1.50%. The preferred lower limit of the Si content is 0.35%, more preferably 0.40%, and more preferably 0.50%. The preferred upper limit of the Si content is 1.35%, more preferably 1.00%, and more preferably 0.90%.
[0033] Mn: 0.20~0.40% Manganese (Mn) improves the hardenability of steel and increases the surface initiated spalling life of a bearing part when the steel is used as a bearing part. If the Mn content is less than 0.20%, the above effects cannot be sufficiently obtained even if the contents of other elements are within the range of this embodiment. On the other hand, if the Mn content exceeds 0.40%, the strength of the steel becomes excessively high and the machinability of the steel decreases even if the contents of other elements are within the range of this embodiment. Therefore, the Mn content is 0.20 to 0.40%. The lower limit of the Mn content is preferably 0.22%, more preferably 0.25%. The upper limit of the Mn content is preferably 0.38%, more preferably 0.35%.
[0034] Cr: 0.30~1.25% Chromium (Cr) improves the hardenability of steel. Furthermore, when the steel is used as a bearing part, Cr promotes the formation of fine V precipitates during heat treatment. Therefore, the surface-initiated spalling life of the bearing part is increased. If the Cr content is less than 0.30%, the above effect cannot be sufficiently obtained even if the contents of other elements are within the range of this embodiment. On the other hand, if the Cr content exceeds 1.25%, the strength of the steel becomes excessively high even if the contents of other elements are within the range of this embodiment. In this case, the machinability of the steel decreases. Therefore, the Cr content is 0.30 to 1.25%. The preferred lower limit of the Cr content is 0.40%, more preferably 0.50%, and even more preferably 0.80%. The preferred upper limit of the Cr content is 1.20%, and even more preferably 1.15%.
[0035] Mo: 0.10-0.30% Molybdenum (Mo) improves the hardenability of steel. Furthermore, when the steel is used as a bearing part, Mo promotes the formation of fine V precipitates during heat treatment. Therefore, the surface-initiated spalling life of the bearing part is increased. If the Mo content is less than 0.10%, the above effect cannot be sufficiently obtained even if the contents of other elements are within the range of this embodiment. On the other hand, if the Mo content exceeds 0.30%, the strength of the steel becomes excessively high even if the contents of other elements are within the range of this embodiment. In this case, the machinability of the steel decreases. Therefore, the Mo content is 0.10 to 0.30%. The preferred lower limit of the Mo content is 0.13%, and more preferably 0.15%. The preferred upper limit of the Mo content is 0.28%, and more preferably 0.27%, and more preferably 0.25%.
[0036] V: 0.20~0.40% Vanadium (V) improves the hardenability of steel. Furthermore, when the steel is used as a bearing component, V forms fine V precipitates in the bearing component. Therefore, the surface initiated spalling life of the bearing component is increased. If the V content is less than 0.20%, the above effect cannot be sufficiently obtained even if the contents of other elements are within the range of this embodiment. On the other hand, if the V content exceeds 0.40%, the machinability of the steel and the surface initiated spalling life of the bearing component are reduced even if the contents of other elements are within the range of this embodiment. Specifically, if the V content exceeds 0.40%, coarse V precipitates are formed during heating before the hot working process in the manufacturing process of the bearing component using the steel. The coarse V precipitates reduce the machinability of the steel when the steel after hot working is cut. The coarse V precipitates further remain in the bearing component after the heat treatment process. The coarse V precipitates become the starting points of fatigue. Therefore, the surface initiated spalling life of the bearing component is reduced. Therefore, the V content is 0.20 to 0.40%. The lower limit of the V content is preferably 0.22%, and more preferably 0.25%. The upper limit of the V content is preferably 0.38%, and more preferably 0.35%.
[0037] Al: 0.005 to 0.100% Aluminum (Al) deoxidizes steel. Furthermore, Al forms AlN, which inhibits the coarsening of austenite grains in the steel material during heating at the time of quenching in the manufacturing process of the bearing part. As a result, the surface initiated spalling life of the bearing part is increased. If the Al content is less than 0.005%, the above effect cannot be sufficiently obtained even if the contents of other elements are within the range of this embodiment. On the other hand, if the Al content exceeds 0.100%, coarse alumina-based oxides are generated even if the contents of other elements are within the range of this embodiment. The coarse alumina-based oxides become the starting point of fatigue. Therefore, the surface initiated spalling life of the bearing part is reduced. Therefore, the Al content is 0.005 to 0.100%. The preferred lower limit of the Al content is 0.010%, more preferably 0.015%, and more preferably 0.025%. The preferred upper limit of the Al content is 0.080%, more preferably 0.050%, and more preferably 0.045%. In this embodiment, the Al content means the total Al content (Total Al).
[0038] Ca: 0.0002~0.0010% Calcium (Ca) dissolves in sulfide-based inclusions in steel material to spheroidize the sulfide-based inclusions. Ca also increases the deformation resistance of sulfide-based inclusions at high temperatures, and maintains the spheroidization of the sulfide-based inclusions even after hot working. Ca also dissolves in alumina-based oxides to suppress the aggregation of alumina-based oxides in molten steel. That is, it suppresses the generation of coarse alumina-based oxides. As a result, when the steel material is used as a bearing part, the surface-initiated spalling life of the bearing part is increased. If the Ca content is less than 0.0002%, the above effect cannot be sufficiently obtained even if the contents of other elements are within the range of this embodiment. On the other hand, if the Ca content exceeds 0.0010%, coarse oxides are generated even if the contents of other elements are within the range of this embodiment. In this case, when the steel material is used as a bearing part, the surface-initiated spalling life of the bearing part is reduced. Therefore, the Ca content is 0.0002 to 0.0010%. The lower limit of the Ca content is preferably 0.0003%, and more preferably 0.0004%.The upper limit of the Ca content is preferably 0.0009%, and more preferably 0.0008%.
[0039] P:0.020% or less Phosphorus (P) is an impurity that is inevitably contained. That is, the P content is more than 0%. P segregates to the grain boundary. As a result, the grain boundary strength is reduced. If the P content exceeds 0.020%, even if the contents of other elements are within the range of this embodiment, P will excessively segregate to the grain boundary, and the grain boundary strength will be significantly reduced. As a result, when the steel material is used as a bearing part, the surface-initiated spalling life of the bearing part will be reduced. Therefore, the P content is 0.020% or less. The preferred upper limit of the P content is 0.015%, and the more preferred upper limit is 0.012%. The P content is preferably as low as possible. However, excessive reduction of the P content increases the manufacturing cost. Therefore, in consideration of normal industrial production, the preferred lower limit of the P content is 0.001%, more preferably 0.002%, and even more preferably 0.004%.
[0040] S: 0.005% or less Sulfur (S) is an impurity that is inevitably contained. That is, the S content is more than 0%. S generates sulfide-based inclusions. The coarse sulfide-based inclusions become the starting point of fatigue of the bearing component. If the S content exceeds 0.005%, even if the contents of other elements are within the range of this embodiment, when the steel material is used as a bearing component, coarse sulfide-based inclusions remain in the bearing component. As a result, the surface-initiated spalling life of the bearing component decreases. Therefore, the S content is 0.005% or less. The preferred upper limit of the S content is 0.004%, more preferably 0.003%. The S content is preferably as low as possible. However, excessive reduction of the S content increases the manufacturing cost. Therefore, in consideration of normal industrial production, the preferred lower limit of the S content is 0.001%, more preferably 0.002%.
[0041] N: 0.0300% or less Nitrogen (N) is an unavoidably contained impurity. That is, the N content is more than 0%. N dissolves in the steel material and reduces the hot workability of the steel material. If the N content exceeds 0.0300%, the hot workability of the steel material is significantly reduced even if the contents of other elements are within the range of this embodiment. Therefore, the N content is 0.0300% or less. The preferred upper limit of the N content is 0.0250%, more preferably 0.0200%. The N content is preferably as low as possible. However, excessive reduction of the N content increases the manufacturing cost. Therefore, in consideration of normal industrial production, the preferred lower limit of the N content is 0.0001%, more preferably 0.0030%, and even more preferably 0.0050%.
[0042] O (oxygen): 0.0015% or less Oxygen (O) is an impurity that is inevitably contained. That is, the O content is more than 0%. O combines with other elements in the steel to generate coarse oxides. The coarse oxides become the starting point of fatigue of the bearing part. If the O content exceeds 0.0015%, even if the contents of other elements are within the range of this embodiment, when the steel material is used as a bearing part, coarse oxides remain in the bearing part. As a result, the surface-initiated spalling life of the bearing part is reduced. Therefore, the O content is 0.0015% or less. The preferred upper limit of the O content is 0.0013%, more preferably 0.0011%. The O content is preferably as low as possible. However, excessive reduction of the O content increases the manufacturing cost. Therefore, in consideration of normal industrial production, the preferred lower limit of the O content is 0.0001%, more preferably 0.0005%.
[0043] The balance of the chemical composition of the steel material according to the present embodiment is composed of Fe and impurities. Here, the term "impurities" refers to substances that are mixed in from raw materials such as ore and scrap, or from the manufacturing environment, during industrial production of the steel material, and that are permissible within a range that does not adversely affect the steel material according to the present embodiment.
[0044] [About optional elements] The chemical composition of the steel material of this embodiment may further contain, instead of a portion of Fe, one or more elements selected from the group consisting of Ni: 2.00% or less, B: 0.0100% or less, Nb: 0.1000% or less, and Ti: 0.1000% or less. These elements are optional elements, and any of them increases the surface initiated spalling life of a bearing component when the steel material is used as the bearing component.
[0045] Ni: 2.00% or less Nickel (Ni) is an optional element and may not be contained. That is, the Ni content may be 0%. When contained, Ni enhances the hardenability of the steel material and enhances the strength of the steel material. As a result, when the steel material is used as a bearing part, the surface-initiated spalling life of the bearing part is increased. If even a small amount of Ni is contained, the above effect can be obtained to a certain extent. However, if the Ni content exceeds 2.00%, the strength of the steel material becomes excessively high. In this case, even if the contents of other elements are within the range of this embodiment, the machinability of the steel material decreases. Therefore, the Ni content is 0 to 2.00%, and if contained, the Ni content is 2.00% or less. That is, if contained, the Ni content is more than 0 to 2.00%. The preferable lower limit of the Ni content is 0.01%, more preferably 0.05%, more preferably 0.10%, and more preferably 0.30%. The preferable upper limit of the Ni content is 1.80%, and more preferably 1.50%.
[0046] B: 0.0100% or less Boron (B) is an optional element and may not be contained. In other words, the B content may be 0%. When contained, B improves the hardenability of the steel material and increases the strength of the steel material. B further suppresses the segregation of P and S at the austenite grain boundary during hardening. As a result, when the steel material is used as a bearing part, the surface initiated spalling life of the bearing part is increased. If even a small amount of B is contained, the above effect can be obtained to a certain extent. However, if the B content exceeds 0.0100%, B nitride (BN) is generated even if the contents of other elements are within the range of this embodiment. In this case, when the steel material is used as a bearing part, the surface initiated spalling life of the bearing part is reduced. Therefore, the B content is 0 to 0.0100%, and when contained, the B content is 0.0100% or less. In other words, when contained, the B content is more than 0 to 0.0100%. The lower limit of the B content for effectively obtaining the above effects is preferably 0.0001%, more preferably 0.0003%, more preferably 0.0005%, more preferably 0.0010%, and more preferably 0.0040%. The upper limit of the B content is preferably 0.0080%, more preferably 0.0060%, and more preferably 0.0050%.
[0047] Nb: 0.1000% or less Niobium (Nb) is an optional element and may not be contained. That is, the Nb content may be 0%. When contained, Nb combines with C and N in the steel to form Nb precipitates (carbides or carbonitrides). These precipitates suppress the coarsening of crystal grains and increase the strength of the bearing part. As a result, the surface initiated spalling life of the bearing part is increased. If even a small amount of Nb is contained, the above effect can be obtained to some extent. However, if the Nb content exceeds 0.1000%, coarse Nb precipitates are formed. In this case, even if the contents of other elements are within the range of this embodiment, the surface initiated spalling life of the bearing part is reduced. Therefore, the Nb content is 0 to 0.1000%, and when contained, the Nb content is 0.1000% or less. That is, when contained, the Nb content is more than 0 to 0.1000%. The lower limit of the Nb content is preferably 0.0001%, more preferably 0.0010%, more preferably 0.0050%, and even more preferably 0.0100%. The upper limit of the Nb content is preferably 0.0800%, and even more preferably 0.0700%.
[0048] Ti:0.1000% or less Titanium (Ti) is an optional element and may not be contained. In other words, the Ti content may be 0%. When contained, Ti combines with C and N in the steel to generate Ti precipitates (carbides, carbonitrides, or nitrides). These precipitates suppress the coarsening of crystal grains and increase the strength of the bearing part. As a result, the surface initiated spalling life of the bearing part is increased. If even a small amount of Ti is contained, the above effect can be obtained to some extent. However, if the Ti content exceeds 0.1000%, coarse Ti precipitates are generated. In this case, even if the contents of other elements are within the range of this embodiment, the surface initiated spalling life of the bearing part is reduced. Therefore, the Ti content is 0 to 0.1000%, and when contained, the Ti content is 0.1000% or less. In other words, when contained, the Ti content is more than 0 to 0.1000%. The lower limit of the Ti content is preferably 0.0001%, more preferably 0.0010%, more preferably 0.0100%, and even more preferably 0.0300%. The upper limit of the Ti content is preferably 0.0800%, and even more preferably 0.0750%.
[0049] [Regarding formulas (1) to (3)] The chemical composition of the steel material of this embodiment further has each element content within the above-mentioned range and satisfies the following formulas (1) to (3). 1.20<0.4Cr+0.4Mo+4.5V<2.40 (1) 75C+35Si+150Mn+30Ni+60Cr+115Mo+50(V+Ti+Nb)≦255 (2) 30C+18Si+20Cr+35Mn+15Ni≦85 (3) Here, the content (mass%) of the corresponding element is substituted for each element symbol in formulas (1) to (3). When the corresponding element is not contained, "0" is substituted for the element symbol.
[0050] [Regarding formula (1)] F1 is defined as 0.4Cr+0.4Mo+4.5V. F1 is an index of precipitation nucleation sites for fine V precipitates during the heat treatment process when manufacturing bearing parts using steel as the raw material. As mentioned above, Cr and Mo promote the formation of precipitation nucleation sites for V precipitates. Specifically, Cr forms Fe-based carbides such as cementite or Cr carbides in a temperature range lower than the temperature range in which V precipitates form. Mo forms Mo carbides (Mo 2 As the temperature increases, Fe-based carbides, Cr carbides, and Mo carbides dissolve and become nucleation sites for V precipitates.
[0051] If F1 is 1.20 or less, even if the contents of each element are within the range of this embodiment and formula (2) and formula (3) are satisfied, any one of V, Cr, and Mo is insufficient. In this case, the precipitation nucleation sites of V precipitates are insufficient. Or, the V content itself necessary for the generation of V precipitates is insufficient relative to the Cr content and Mo content. Therefore, fine V precipitates are not sufficiently generated during the heat treatment process. As a result, a sufficient surface initiated spalling life is not obtained in the bearing component. On the other hand, if F1 is 2.40 or more, even if the contents of each element are within the range of this embodiment and formula (2) and formula (3) are satisfied, precipitation nucleation sites are excessively generated. In this case, excessive V precipitates are generated in the steel material. As a result, when a bearing component is manufactured using the steel material as a raw material, V precipitates do not dissolve and become coarse during heating in hot working. The coarse V precipitates remain in the bearing component after the heat treatment process. As a result, the surface initiated spalling life of the bearing component is reduced.
[0052] If F1 is greater than 1.20 and less than 2.40, the generation of coarse V precipitates is suppressed in the steel material and the bearing component, provided that the content of each element is within the range of this embodiment and formulas (2) and (3) are satisfied. Furthermore, fine V precipitates are sufficiently generated in the surface layer of the bearing component. As a result, the surface-initiated spalling life of the bearing component is increased.
[0053] The lower limit of F1 is preferably 1.30, more preferably 1.35, and even more preferably 1.40. The upper limit of F1 is preferably 2.38, more preferably 2.36, more preferably 2.34, more preferably 2.30, more preferably 2.25, and even more preferably 2.20. The numerical value of F1 is a value obtained by rounding off to two decimal places.
[0054] [Regarding formula (2)] F2 is defined as 75C+35Si+150Mn+30Ni+60Cr+115Mo+50(V+Ti+Nb). The elements in F2 (C, Si, Mn, Ni, Cr, Mo, V, Ti, and Nb) are the main elements that increase the hardenability of steel among the elements in the above chemical composition. F2 is an index of the machinability of steel.
[0055] If F2 is higher than 255, even if the content of each element is within the range of this embodiment and formula (1) and formula (3) are satisfied, the strength of the steel material will be too high. In this case, the machinability of the steel material will be insufficient.
[0056] If F2 is 255 or less, sufficient machinability can be obtained in the steel material, provided that the content of each element is within the range of this embodiment and formulas (1) and (3) are satisfied.
[0057] The upper limit of F2 is preferably 250, more preferably 245, and even more preferably 240. The lower limit of F2 is not particularly limited. However, taking into consideration the lower limits of the contents of each element in the chemical composition of this embodiment, the lower limit of F2 is preferably 118, more preferably 120, more preferably 150, and even more preferably 180. The numerical value of F2 is a value obtained by rounding off to one decimal place.
[0058] [Regarding formula (3)] It is defined as F3 = 30C + 18Si + 20Cr + 35Mn + 15Ni. F3 is an index of the shape stability of a bearing part during use when the steel is used as a bearing part. Among the elements in the above-mentioned chemical composition, C, Si, Cr, Mn and Ni in particular affect the amount of retained austenite produced in a bearing part obtained by performing hot working, cutting and heat treatment on the steel material.
[0059] If F3 is greater than 85, even if the content of each element is within the range of this embodiment and formula (1) and formula (2) are satisfied, a large amount of retained austenite remains in the bearing component after heat treatment. Therefore, the shape stability of the bearing component during use is reduced. If F3 is 85 or less, the shape stability of the bearing component during use is sufficiently improved, provided that the content of each element is within the range of this embodiment and formula (1) and formula (2) are satisfied.
[0060] The upper limit of F3 is preferably 83, more preferably 80, and even more preferably 78. The lower limit of F3 is not particularly limited. However, taking into consideration the lower limits of the contents of each element in the chemical composition of this embodiment, the lower limit of F3 is preferably 35, and even more preferably 40. The numerical value of F3 is a value obtained by rounding off to one decimal place.
[0061] [About the microstructure] The microstructure of the steel material in this embodiment is not particularly limited. In this embodiment, the machinability of the steel material is a property required for a steel material that has been subjected to a hot working process and then spheroidized annealing when the steel material is used for a bearing part. c3 Therefore, the microstructure of the steel material is not particularly limited.
[0062] The steel material of this embodiment having the above configuration has a chemical composition in which the content of each element falls within the range of this embodiment, and F1 to F3 satisfy formulas (1) to (3). Therefore, the steel material of this embodiment has excellent machinability. Furthermore, when the steel material of this embodiment is used as a bearing part, the bearing part has excellent surface initiated spalling life and shape stability.
[0063] [Steel use] As described above, the steel material of this embodiment is suitable as a material for bearing parts. The steel material of this embodiment is particularly suitable for medium-sized and large-sized bearing parts for mining and construction machinery applications. Medium-sized and large-sized bearing parts are repeatedly subjected to significantly higher surface pressure during use than small-sized bearing parts for automotive applications. As a result, the bearing parts may be deformed due to the surface pressure. When the steel material of this embodiment is used as a bearing part, it has excellent shape stability. Therefore, the steel material of this embodiment is suitable as a material for medium-sized and large-sized bearing parts. It is of course possible to use the steel material of this embodiment for small-sized bearing parts for automotive applications.
[0064] [Steel manufacturing method] An example of a method for manufacturing the steel material of this embodiment will be described. The method for manufacturing the steel material described below is one example for manufacturing the steel material of this embodiment. Therefore, the steel material having the above-mentioned configuration may be manufactured by a manufacturing method other than the manufacturing method described below. However, the manufacturing method described below is a preferred example of the method for manufacturing the steel material of this embodiment.
[0065] An example of the method for manufacturing a steel material according to the present embodiment includes a material preparation step of preparing a material, and a hot working step of hot working the material to manufacture a steel material. Each step will be described below.
[0066] [Material preparation process] In the material preparation step, a material for the steel material of this embodiment is prepared. Specifically, molten steel is produced in which the content of each element in the chemical composition is within the range of this embodiment and F1 to F3 satisfy formulas (1) to (3). The refining method is not particularly limited, and a well-known method may be used. For example, molten pig iron produced by a well-known method is refined in a converter (primary refining). The molten steel tapped from the converter is subjected to well-known secondary refining. In the secondary refining, alloy elements are added to the molten steel to adjust the composition, and molten steel is produced in which the content of each element is within the range of this embodiment and F1 to F3 satisfy formulas (1) to (3).
[0067] The molten steel produced by the above-mentioned refining method is used to produce a material by a well-known casting method. For example, the molten steel may be used to produce an ingot by an ingot casting method. Alternatively, the molten steel may be used to produce a bloom or billet by a continuous casting method. By the above-mentioned methods, a material (ingot, bloom, or billet) is produced.
[0068] [Hot processing process] In the hot working process, hot working is performed on the material (ingot, bloom or billet) prepared in the material preparation process to produce the steel material of this embodiment. The steel material is a steel bar or a wire rod. The hot working process includes a blooming process and a finish rolling process. Each process will be described below.
[0069] [Bulking rolling process] In the blooming process, the material is hot rolled to produce billets. Specifically, in the blooming process, the material is hot rolled (blooming) by a blooming mill to produce billets. If a continuous rolling mill is arranged downstream of the blooming mill, the billet after blooming may be further hot rolled by the continuous rolling mill to produce a smaller billet. In the continuous rolling mill, horizontal stands having a pair of horizontal rolls and vertical stands having a pair of vertical rolls are alternately arranged in a row. As described above, in the blooming process, the material is produced into billets by using the blooming mill, or by using the blooming mill and the continuous rolling mill.
[0070] The heating temperature in the heating furnace in the blooming process is not particularly limited. For example, the heating temperature is 1150 to 1300°C. The holding time at the furnace temperature of 1150 to 1300°C is not limited. For example, the holding time at the furnace temperature of 1150 to 1300°C may be 2 to 30 hours.
[0071] [Finish rolling process] In the finish rolling process, first, the billet is heated using a heating furnace, and then the heated billet is hot-rolled using a continuous rolling mill to produce a steel material, such as a bar or wire rod.
[0072] The heating temperature in the heating furnace in the finish rolling step is not particularly limited. For example, the heating temperature is 1000 to 1300°C. The holding time in the heating furnace at a furnace temperature of 1000 to 1300°C is not limited. For example, the holding time in the heating furnace at a furnace temperature of 1000 to 1300°C may be 1 to 10 hours.
[0073] The steel material after the finish rolling step is cooled at a cooling rate equal to or slower than natural cooling to produce the steel material of this embodiment.
[0074] The steel material according to the present embodiment having the above-mentioned configuration can be manufactured by the above-mentioned manufacturing process. Note that the steel material after the hot working process may be subjected to a known normalizing treatment or a known spheroidizing annealing treatment.
[0075] [Bearing parts] Bearing parts refer to parts of rolling bearings. Bearing parts include, for example, races, races, The raceway may be an inner or outer ring, and the raceway may be a shaft raceway or a hub raceway. The bearing may be a housing race, a central race, or an aligning housing race. The rolling elements are not particularly limited as long as they have a raceway surface. The rolling elements may be balls or rollers. Examples of the rollers include cylindrical rollers, rod-shaped rollers, needle rollers, tapered rollers, convex rollers, and the like.
[0076] The steel material of this embodiment is suitable as a material for bearing parts. Bearing parts using the steel material of this embodiment are manufactured by a well-known manufacturing method. For example, bearing parts using the steel material of this embodiment as a material are manufactured by the following manufacturing method.
[0077] The manufacturing method of the bearing part includes, for example, a hot working step, a spheroidizing annealing step, a cutting step, and a heat treatment step. In the hot working step, hot working is performed on the steel material of the present embodiment. The hot working is, for example, the well-known hot forging. In the hot working step, the steel material is A c3 After heating to a temperature above the hot working point, the steel is processed. Therefore, the microstructure of the steel is reset during the heating in the hot working process. The heating temperature is a well-known temperature, for example, 1000 to 1300°C. After the hot working, the steel is air-cooled.
[0078] The steel material after the hot working process is subjected to a well-known spheroidizing annealing process. The steel material after the spheroidizing annealing process is then subjected to a cutting process to manufacture an intermediate product of a predetermined shape. During this cutting process, high machinability of the steel material is required. In the cutting process, well-known cutting is performed. Through the above steps, an intermediate product is manufactured.
[0079] A heat treatment process is performed on the intermediate product after the cutting process. In this embodiment, "heat treatment" means quenching and tempering, carburizing quenching and tempering, carbonitriding quenching and tempering, or nitriding quenching and tempering, as described above. Any of the heat treatments may be performed under well-known conditions. It is a technical matter well-known to those skilled in the art that the surface hardness and core hardness of the bearing part, the surface carbon concentration of the bearing part, and the surface nitrogen concentration of the bearing part can be appropriately adjusted by appropriately adjusting the quenching conditions, carburizing quenching conditions, carbonitriding quenching conditions, nitriding quenching conditions, and tempering conditions. The above-mentioned well-known heat treatment is performed on the intermediate product to manufacture the bearing part.
[0080] The bearing component made of the steel material of this embodiment has an excellent surface initiated spalling life, and further has excellent shape stability during use.
[0081] In the manufacturing process of the bearing part, the intermediate product after the heat treatment process may be subjected to a finishing process (cutting process, polishing process, etc.). By performing the finishing process, the surface roughness of the intermediate product after the surface hardening process can be adjusted. The finishing process may be performed by a well-known method. EXAMPLES
[0082] Two tons of molten steel having the chemical composition shown in Table 1 was produced by vacuum melting.
[0083] [Table 1]
[0084] The blank spaces in Table 1 mean that the content of the corresponding element was below the detection limit.
[0085] The molten steel in Table 1 was continuously cast to produce a cast piece (bloom) as the raw material. The bloom as the raw material was subjected to a hot working process. Specifically, the bloom was heated to 1250°C and held at that temperature for 10 hours. The bloom was then bloomed using a blooming mill to produce a billet. The cross section of the billet perpendicular to the longitudinal direction was a rectangle measuring 160 mm x 160 mm. The produced billet was allowed to cool to room temperature.
[0086] The billet was subjected to a finish rolling process to produce a round bar with a diameter of 80 mm. Specifically, the billet was heated to 1200°C and held at that temperature for 3 hours. The heated billet was subjected to hot rolling using a continuous rolling mill to produce a round bar with a diameter of 80 mm. The round bar after hot rolling was allowed to cool to room temperature. Through the above manufacturing process, steel materials (round bars) of each test number were produced. Note that test number 49 was a steel material having a chemical composition equivalent to SUJ2, a conventional steel material, specified in JIS G 4805 (2019), as a comparative reference steel material.
[0087] [Evaluation test] The steel materials manufactured by the above manufacturing process were subjected to a machinability evaluation test, a surface initiated spalling life evaluation test, and a shape stability evaluation test.
[0088] [Machinability evaluation test] Heat treatment simulating hot working was performed on the steel material (round bar with a diameter of 80 mm) of each test number. In the heat treatment, the steel material was held at 1000°C for 1 hour, and then allowed to cool (air-cool) to room temperature. The steel material after cooling was subjected to well-known spheroidizing annealing. Specifically, in the spheroidizing annealing, the steel material was held at 760°C for 6 hours. Then, it was slowly cooled to 600°C at a cooling rate of 10 to 15°C / hour. Then, the steel material was allowed to cool (air-cool) to room temperature. Through the above steps, a steel test piece simulating hot working and spheroidizing annealing of a bearing part was produced.
[0089] The steel test pieces thus produced were subjected to peripheral turning to evaluate the machinability of the steel. Specifically, peripheral turning was performed on the steel test pieces of each test number under the following conditions. The cutting tool used was an uncoated cemented carbide equivalent to P20 as specified in JIS B 4053 (2013). The cutting speed was 200 m / min, the feed rate was 0.30 mm / rev, and the cutting depth was 1.0 mm. Water-soluble cutting oil was used during turning.
[0090] The steel test pieces were subjected to peripheral turning for 10 minutes under the above-mentioned cutting conditions. The flank wear amount (mm) of the cutting tool after peripheral turning was measured. The flank wear amount ratio (%) for the case of using the steel of each test number was calculated using the following formula, based on the flank wear amount of the comparative reference steel of test number 49. Flank wear ratio (%) = Flank wear when using steel with each test number (mm) / Flank wear when using standard steel (mm) x 100
[0091] The obtained flank wear ratio (%) is shown in the "Wear ratio (%)" column in Table 2. If the obtained flank wear ratio was 80% or less, it was determined that the machinability was excellent (indicated by "E" in the "Machinability evaluation" column in Table 2). On the other hand, if the flank wear ratio exceeded 80%, it was determined that the machinability was poor (indicated by "NA" in the "Machinability evaluation" column in Table 2).
[0092] [Table 2]
[0093] [Surface initiated peeling life evaluation test] Heat treatment simulating hot working was performed on the steel material (round bar with a diameter of 80 mm) of each test number. In the heat treatment, the steel material was held at 1000°C for 1 hour, and then cooled (air-cooled) to room temperature. The steel material after cooling was subjected to well-known spheroidizing annealing. Specifically, in the spheroidizing annealing, the steel material was held at 760°C for 6 hours. Then, it was slowly cooled to 600°C at a cooling rate of 10 to 15°C / hour. Then, the steel material was cooled (air-cooled) to room temperature. Cutting (periphery turning) and slicing were performed on the steel material (round bar) with a diameter of 80 mm after the spheroidizing annealing, and a disk-shaped rough test piece (rough test piece simulating an intermediate product) with a diameter of 60 mm and a thickness of 6 mm was taken. Ten rough test pieces were taken from each steel material of each test number.
[0094] The rough test pieces with each test number were subjected to one of the following heat treatments to produce test pieces simulating bearing parts. The type of heat treatment performed is shown in the "Heat treatment conditions" column of Table 2.
[0095] [Carburizing, quenching and tempering (referred to as "Carburizing" in Table 2)] The rough test pieces were held at 870°C for 4 hours in an atmosphere with a carbon potential CP of 0.8%. Then, they were quenched in oil at 60°C. After oil quenching, the rough test pieces were tempered at a tempering temperature of 150°C for a holding time of 120 minutes. [Carbonitriding, quenching and tempering (referred to as "carbonitriding" in Table 2)] The crude test pieces were held at 870°C for 4 hours in an atmosphere with a carbon potential CP of 0.8%. They were then continuously held at 830°C for 5 hours for nitriding. Ammonia gas was used for the nitriding, and the flow rate was adjusted so that the nitrogen concentration on the surface of the crude test pieces was 0.3%. They were then quenched by oil cooling in 60°C oil. After oil cooling, the crude test pieces were tempered at a tempering temperature of 150°C for a holding time of 120 minutes. [Nitriding, quenching and tempering (referred to as "nitriding" in Table 2)] The crude test pieces were subjected to nitriding treatment by holding them at 830°C for 5 hours. Ammonia gas was used for the nitriding treatment, and the flow rate was adjusted so that the nitrogen concentration on the surface of the crude test pieces was 0.3%. After that, they were quenched by oil cooling at 60°C. After oil cooling, the crude test pieces were tempered at a tempering temperature of 150°C for a holding time of 120 minutes. [Quenching and tempering (referred to as "Quenching" in Table 2)] The rough test pieces were held at 830°C for 2 hours, and then quenched by oil cooling at 60°C. The rough test pieces after oil cooling were tempered at a tempering temperature of 150°C for a holding time of 120 minutes.
[0096] After the heat treatment, the circular surface of each test piece, 60 mm in diameter, was polished by 30 μm on each side to prepare a test piece that was a simulated bearing part. One surface of the polished circular surface of each test piece was then lapped to prepare a rolling fatigue test piece.
[0097] A rolling fatigue test was carried out using a thrust type rolling fatigue tester. Specifically, as shown in FIG. 1, a rolling fatigue test piece 100 was immersed in a lubricating oil 102. The rolling fatigue test piece 100 was arranged so that the lapped surface of the rolling fatigue test piece 100 was in contact with three steel balls 101. The jig 103 was rotated around a central axis C1 while pressing the three steel balls 101 against the rolling fatigue test piece 100. The maximum contact surface pressure during the test was 4.0 GPa, and the repetition rate was 2500 cpm (cycles per minute). The lubricating oil 102 used during the test was mixed with gas atomized high-speed steel powder classified into a Vickers hardness of 750 (HV) and a particle size of 100 to 180 μm as a foreign matter. The amount of gas atomized powder mixed in was 0.02 mass% relative to the lubricating oil 102. The steel ball 101 used in the test had a diameter of 9.525 mm and was made of SUJ2 tempered material specified in JIS G 4805 (2019).
[0098] The rolling fatigue test results were plotted on a Weibull probability chart, and the L10 life, which indicates a 10% probability of failure, was defined as the "surface-initiated spalling life." Under the harsh operating environment of foreign matter contamination (main test), the L10 life was 1.0 x 10 7If the L10 life was 1.0×10 or more, it was judged to be excellent in surface initiated spalling life (indicated by "E" in the "Surface initiated spalling life" column in Table 2). 7 If it was less than this, it was determined that the surface initiated peeling life was short (indicated as "NA" in the "Surface initiated peeling life" column in Table 2).
[0099] [Shape stability evaluation test] In rolling fatigue tests, the L10 life was 1.0×10 7 For the rolling fatigue test pieces after the rolling fatigue test in the case where the rolling fatigue test was performed, a stylus roughness meter was used to measure the cross-sectional curve that crosses the rolling and non-rolling parts of the surface of the test piece at the same time. Then, the difference ΔH (μm) between the average height of the non-rolling part and the average height of the rolling part was calculated. The rolling part means the part where the test piece and the steel ball contacted each other in the rolling fatigue test. The non-rolling part means the part where the test piece and the steel ball did not contact each other in the rolling fatigue test. The cross-sectional curve was measured at four points for each test piece. The arithmetic mean value of the difference ΔH at the four points was defined as the deformation amount of the rolling part. If the deformation amount of the rolling part was less than 25 μm, it was judged to have excellent shape stability (indicated by "E" in the "shape stability" column in Table 2). On the other hand, if the deformation amount of the rolling part was 25 μm or more, it was judged to have insufficient shape stability (indicated by "NA" in the "shape stability" column in Table 2).
[0100] [Test Results] The test results are shown in Table 2. Referring to Table 2, the steel materials with test numbers 1 to 20 had appropriate elemental contents in the chemical composition. Furthermore, F1 to F3 satisfied formulas (1) to (3). Therefore, the wear volume ratio of the steel materials was 80% or less, and excellent machinability was obtained. Furthermore, in the rolling fatigue test, the L10 life was 1.0×10 7 In the rolling fatigue test, the L10 life was 1.0×10 7 In the rolling fatigue test pieces after the rolling fatigue test when the above condition was met, the deformation amount of the rolling portion was less than 25 μm, and the shape stability was excellent.
[0101] On the other hand, in test number 21, F1 was too low, and therefore the surface initiated spalling life was short.
[0102] Test No. 22 had too high F1 and F2, which resulted in a short surface initiated spalling life and poor machinability.
[0103] In test number 23, F1 was too high, which resulted in a short surface initiated spalling life.
[0104] Test No. 24 had too high F2, which resulted in poor machinability.
[0105] Test No. 25 had a too low C content, which resulted in a short surface initiated spalling life.
[0106] Test No. 26 had too high a C content and F2, which resulted in a short surface initiated spalling life and poor machinability.
[0107] Test No. 27 had a too low Si content, which resulted in a short surface initiated spalling life.
[0108] Test No. 28 had too high a Si content and F2, which resulted in poor machinability.
[0109] Test No. 29 had a too low Mn content, which resulted in a short surface initiated spalling life.
[0110] Test No. 30 had too high a Mn content and F2, which resulted in poor machinability.
[0111] Test No. 31 had a too low Cr content, which resulted in a short surface initiated spalling life.
[0112] Test No. 32 had too high a Cr content and F2, which resulted in poor machinability.
[0113] Test No. 33 had a too low Mo content, which resulted in a short surface initiated spalling life.
[0114] Test No. 34 had too high a Mo content and F2, which resulted in poor machinability.
[0115] Test No. 35 had a too low Al content, which resulted in a short surface initiated spalling life.
[0116] Test No. 36 had too high an Al content, which resulted in a short surface initiated spalling life.
[0117] In test number 37, the V content and F1 were too low, and therefore the surface initiated spalling life was short.
[0118] In test number 38, the V content, F1 and F2 were too high, which resulted in a short surface initiated spalling life and poor machinability.
[0119] Test No. 39 had a too low Ca content, which resulted in a short surface initiated spalling life.
[0120] Test No. 40 had too high a Ca content, which resulted in a short surface initiated spalling life.
[0121] Test No. 41 had too high a P content, which resulted in a short surface initiated spalling life.
[0122] Test No. 42 had too high a S content, which resulted in a short surface initiated spalling life.
[0123] Test No. 43 had too high Ni content, F2 and F3, which resulted in poor machinability and insufficient shape stability.
[0124] Test No. 44 had too high a Ti content, which resulted in a short surface initiated spalling life.
[0125] Test No. 45 had too high a Nb content, which resulted in a short surface initiated spalling life.
[0126] Test No. 46 had too high a B content, which resulted in a short surface initiated spalling life.
[0127] Test Nos. 47 and 48 had too high F3 values, which resulted in insufficient shape stability.
[0128] The embodiments of the present disclosure have been described above. However, the above-described embodiments are merely examples for implementing the present disclosure. Therefore, the present disclosure is not limited to the above-described embodiments, and can be implemented by appropriately modifying the above-described embodiments without departing from the spirit of the present disclosure.
Claims
1. The chemical composition, in mass%, is C: 0.50-0.80%, Si: 0.30-1.50%, Mn: 0.20-0.40%, Cr: 0.30-1.25%, Mo: 0.10-0.30%, V: 0.20-0.40%, Al: 0.005-0.100%, Ca: 0.0002-0.0010%, P: 0.020% or less, S: 0.005% or less, N: 0.0300% or less, O: 0.0015% or less, and The balance is Fe and impurities, and satisfies formulas (1) to (3). Steel material. 1.20<0.4Cr+0.4Mo+4.5V<2.40 (1) 75C+35Si+150Mn+30Ni+60Cr+115Mo+50(V+Ti+Nb)≦255 (2) 30C+18Si+20Cr+35Mn+15Ni≦85 (3) Here, the content (mass%) of the corresponding element is substituted for each element symbol in formulas (1) to (3). When the corresponding element is not contained, "0" is substituted for the element symbol.
2. The steel material according to claim 1, The chemical composition further contains, instead of a part of Fe, Ni: 2.00% or less, B: 0.0100% or less, Nb: 0.1000% or less, and Ti: 0.1000% or less; Steel material.
Citation Information
Patent Citations
Machine-structural carbon steel excellent in machinability
JP1995188849A
Rolling bearing excellent in wear resistance
JP1996049057A
Low alloy steel
JP2004002978A
Case-hardening steel excellent in surface fatigue strength due to hydrogen embrittlement
JP2008280583A
Surface layer hardening steel and surface layer-hardened part
JP2020100897A