Performance improving method suitable for copper-based shape memory alloy and product and application thereof

Through heat treatment and staging quenching heat treatment, the problem of martensite stabilization of copper-based shape memory alloys in high temperature environments is solved, and its shape memory effect and mechanical properties under high temperature conditions are improved, and effective application in oil wells is achieved.

CN119061335AActive Publication Date: 2024-12-03SOUTH CHINA UNIV OF TECH

Patent Information

Application Number
CN202411126305.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-12-03
Estimated Expiration
2044-08-16

AI Technical Summary

Technical Problem

Existing copper-based shape memory alloys are prone to martensite stabilization in high temperature environments, resulting in weakening of memory effects and high cost, making it difficult to effectively apply in high-temperature oil wells.

Method used

Improve the dilute crystallinity of copper-based shape memory alloy through heat treatment, reduce the number of trijunction grain boundaries, use hierarchical quenching heat treatment to prevent martensite stability, and regulate the phase transition temperature to make it have stable shape memory in the range of 100-350℃ Reply to respond.

Benefits of technology

It significantly improves the mechanical properties and shape memory effects of copper-based shape memory alloys, reduces costs, and achieves reliable and high recovery strain under high temperature conditions. It is suitable for sand prevention work in high-temperature oil wells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119061335A_ABST
    Figure CN119061335A_ABST
Patent Text Reader

Abstract

The invention discloses a performance improvement method suitable for a copper-based shape memory alloy and a product thereof, and the method comprises the following steps: adopting a copper-based shape memory alloy wire with proper wire diameter and composition to regulate the phase transition temperature and prevent martensite stabilization through thin crystal degree regulation and control heat treatment and step quenching heat treatment; the copper-based shape memory alloy with the improved performance is subjected to spiral winding, winding, weaving, cold press forming and other steps to prepare the screen pipe material, the screen pipe material has high thermal conductivity and a stable shape memory effect, has high recoverable strain at the high temperature, and is simple in preparation process, low in equipment cost and material cost requirement, high in reliability and suitable for industrial production. The invention further discloses a filter pipe assembly and a using method thereof. The filter pipe assembly has excellent application prospects in the technical field of oil and gas drilling well completion sand prevention.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of oil extraction, and specifically relates to a performance improvement method for copper-based shape memory alloys and a product thereof. The present invention also relates to a preparation method for a screen material suitable for operation in a high-temperature oil well, and a product and application thereof. Background Art

[0002] The process of oil extraction is generally divided into four steps: exploration-drilling-completion-extraction. Among them, the completion process is the last step before oil reservoir extraction. The goal is to connect the oil and gas reservoir and the wellbore of the drilling so that subsequent extraction work can proceed smoothly. However, during the production process, due to the changes in the mechanical properties of the rock and soil caused by the disturbance of the formation by drilling, the pressure difference between the inside and outside of the wellbore pipeline, and other factors, the formation sand will inevitably flow into the wellbore when oil is produced, resulting in equipment wear, pipeline blockage, and even the scrapping of the oil well.

[0003] Among the several mainstream completion technologies, the old-fashioned casing perforation completion method and open hole completion method basically do not prevent sand production, so both are only suitable for formations with less sand production. In the face of the sand production problem, the traditional solution is to use gravel packing, that is, to use gravel slurry to fill the wellbore annulus and create a gravel packing layer for the oil production pipeline to prevent the sand and gravel in the oil layer from flowing into the oil production pipeline. However, gravel packing still has many shortcomings. First, the gravel packing layer needs to be pumped from the ground to the gravel slurry, which is prone to problems such as stuck, fault, and deformation, making well repair operations difficult; secondly, the gravel packing process requires the use of a separately designed packer, and the process requires the string to be lowered twice, which is a complicated process; finally, the gravel packing process on the horizontal well pipeline is still immature. For horizontal wells, collapse is prone to occur during completion and perforation, damaging downhole equipment.

[0004] In response to the problem of sand production in oil and gas production pipelines, Baker Hughes Oilfield Technology Services Company of the United States has developed a smart screen material based on porous shape memory polymer (Shape Memory Polyurethane Foam for Downhole Sand Control Filtration Devices, US patent 7926565B2, 2011-04-19; Variable Tg Shape Memory Polyurethane for Wellboredevices US patent, 8365833B2. 2013-02-05). The smart screen is composed of an inner porous base pipe and an outer porous shape memory polymer. Before going down the well, the outer soft porous shape memory polymer is compressed (compressed by 50-80%), and then lowered into the well. The porous shape memory polymer will expand to the size before compression under the high temperature environment downhole and with the assistance of acid, filling wellbore annuli of different sizes, and will generate support force on the surrounding well walls, further preventing sand production from the bottom of the well.

[0005] However, the above-mentioned porous shape memory polymer has low recovery stress, and its shape recovery is not complete when encountering obstacles or complex pipelines. In addition, such materials require a large amount of acid to reduce their shape memory recovery transition temperature, resulting in high cost. Finally, such materials cannot be used in high temperature conditions, and the maximum operating temperature is only 93°C. Looking at the world's oil resources, more than 70% are heavy oil, extra heavy oil and asphalt. The exploitation of these oil and gas resources requires the use of thermal recovery, which makes the bottom hole temperature above 200°C. The performance of porous shape memory polymer screens is unstable in high temperature environments, and they are prone to creep and large stress relaxation, and even melting failure.

[0006] In order to solve the above problems, the patent document with publication number CN114352239A discloses an ultra-high strain recovery shape memory alloy screen material and its preparation method and application. The NiTi shape memory alloy screen material disclosed in the patent document can be used in high-temperature oil wells. However, the raw materials of the NiTi shape memory alloy screen material are expensive, and the molding pressure required for preparing the NiTi memory alloy wire screen material is relatively large. When the screen material is made, the cold pressing pressure is as high as 2 to 80 kN, which leads to a high cost of the screen material molding equipment. On the other hand, the thermal conductivity of the NiTi alloy does not exceed 20 W / (m·K). In the steam-driven oil production process, it is difficult to soften the bottom hole heavy oil. The prior art also discloses that its 50% compression stress is 49.79 MPa.

[0007] Copper-based shape memory alloys have relatively low costs and better thermal conductivity than NiTi alloys. They have obvious advantages as oil well screen materials. However, the memory effect of copper-based shape memory alloys comes from the thermoelastic martensitic phase transformation and its reversal, and martensite stabilization is prone to occur, that is, the thermoelastic martensite is not easy to reverse, the reversible amount of martensite is reduced, and even the thermoelasticity is lost, resulting in the loss of shape memory effect.

[0008] Based on the above, it can be seen that the martensite stabilization phenomenon will seriously damage the memory effect of the copper-based shape memory alloy. The present invention aims to prevent the martensite stabilization of the copper-based shape memory alloy and improve the reliability of the copper-based shape memory alloy during use, so that it can be used as a screen material for oil wells and can be used in high temperature environments. Summary of the invention

[0009] In view of the problems in the related art, the present invention proposes a performance improvement method applicable to copper-based shape memory alloys and its products and applications, so as to overcome the above-mentioned technical problems existing in the existing related art.

[0010] The technical solution of the present invention is achieved in this way:

[0011] A method for improving the performance of a copper-based shape memory alloy comprises the following steps:

[0012] (1) placing a copper-based shape memory alloy wire in a reaction device in a sand bath for heating, maintaining the temperature at 600 to 900° C. for 4 to 30 hours under a vacuum environment or an inert atmosphere, and then taking out the copper-based shape memory alloy wire for rapid cooling;

[0013] (2) placing the cooled copper-based shape memory alloy wire in the reaction device again for sand bath heating, keeping the temperature at 750-900° C. for 10-30 min under vacuum or inert atmosphere, and then taking out the copper-based shape memory alloy wire for rapid cooling;

[0014] (3) The cooled copper-based shape memory alloy wire is heated in an oil bath and kept at 120-160° C. for 0.5-2 h, and then the copper-based shape memory alloy wire is taken out and rapidly cooled; and the surface oil is removed by cleaning.

[0015] Compared with the prior art, firstly, the present invention improves the rarefaction degree of the copper-based shape memory alloy by heat treatment, reduces the number of triple grain boundaries inside the copper-based shape memory alloy, and thus significantly improves the mechanical properties and shape memory effect of the copper-based shape memory alloy;

[0016] Secondly, the regulation of the rarefaction of the present invention can also effectively improve the recovery performance of the screen material containing the copper-based shape memory alloy of the present invention, and can be made into different degrees of recoverable strain to cope with different needs corresponding to the complex and changeable conditions of high-temperature oil wells;

[0017] Thirdly, on the basis of the rarefaction control, the present invention adopts a special graded quenching heat treatment method to prevent the martensite stabilization, so that the copper-based shape memory alloy has excellent and stable shape memory recovery strain, and adjusts the phase transition temperature (A f The temperature) is in the range of 29.9-99.8°C, that is, it has a phase transition temperature suitable for underground high-temperature working conditions, thereby enabling the screen material containing the copper-based shape memory alloy of the present invention to be used with reliable high recovery strain under high temperature conditions (100-350°C).

[0018] Finally, the method for preparing copper-based shape memory alloy wire of the present invention is simple and easy to operate, and compared with the existing NiTi shape memory alloy, the raw material cost and processing cost are relatively low; on the other hand, the thermal conductivity of NiTi shape memory alloy at 200°C is about 13.2W / m·K, which is much lower than the copper-based shape memory alloy of the present invention (above 300W / m·K). Therefore, the copper-based shape memory alloy prepared by the present invention has significant advantages when used for steam-driven oil production to soften the viscosity of the bottom oil layer.

[0019] Preferably, in step (1), the copper-based shape memory alloy wire is CuZnAl, wherein the atomic percentage of Cu is 66.02-81.75%, the atomic percentage of Zn is 15.09-24.52%, and the atomic percentage of Al is 3.05-9.88%.

[0020] Preferably, the copper-based shape memory alloy wire has a wire diameter of 0.7-1.2 mm.

[0021] Preferably, in step (1) and step (2), the fine sand heated in the sand bath is Al2O3 pellets.

[0022] More preferably, the diameter of the Al2O3 ball is smaller than the diameter of the copper-based shape memory alloy wire; specifically, the diameter of the Al2O3 ball is 0.25 mm.

[0023] Preferably, in step (3), the oil used for oil bath heating is dimethyl silicone oil.

[0024] Preferably, in step (3), the specific operation of the cleaning is: ultrasonic cleaning with a 95% alcohol solution for 10 to 30 minutes.

[0025] Preferably, the present invention achieves rapid cooling of steps (1) to (3) by water quenching.

[0026] The present invention also discloses a copper-based shape memory alloy wire, which is made by the above-mentioned method for improving the performance of copper-based shape memory alloys. The made copper-based shape memory alloy wire is a single martensite phase at room temperature.

[0027] The average grain diameter of the copper-based shape memory alloy wire is 0.006-0.51 mm, and the dilution degree is 0.006-0.51.

[0028] The martensitic transformation completion temperature M of the copper-based shape memory alloy wire f ≤50.5℃, phase transition point A f <100℃.

[0029] Based on the above-mentioned copper-based shape memory alloy wire with improved performance, the present invention further studies how to make it into a screen tube material. Specifically, a porous copper-based shape memory alloy screen tube material is prepared by making the copper-based shape memory alloy wire into a spiral roll, winding it into a preform and cold pressing it. The screen tube material of the present invention is prepared by entanglement of copper-based shape memory alloy wires whose rarefaction and phase transition temperature are regulated. Different rarefactions bring different copper-based shape memory alloy wire properties, thereby regulating the recoverable strain of the screen tube material. The screen tube material preparation method of the present invention has high reliability and is easy to achieve mass production.

[0030] The present invention also discloses a method for preparing a screen tube material, comprising the following steps:

[0031] (1) preparing a cylindrical first mandrel, winding and stretching the copper-based shape memory alloy wire around the first mandrel, wherein the copper-based shape memory alloy wire is inclined relative to the axis of the first mandrel to form a spiral coil;

[0032] (2) The spiral coils obtained in step (1) are interlocked by winding, laying out and weaving to obtain a preform with a stable structure;

[0033] (3) placing the preform obtained in step (2) in a mold for cold pressing to obtain a screen tube material.

[0034] Preferably, in step (1), the ratio of the wire diameter of the copper-based shape memory alloy wire to the diameter of the first mandrel is 5 to 15:1.

[0035] Preferably, in step (1), the copper-based shape memory alloy wire is inclined relative to the axis of the first core shaft to form an angle of 40 to 60°, which is set as the helix angle.

[0036] Preferably, the specific operation of step (2) is: prepare a cylindrical second core shaft, the spiral roll obtained in step (1) is inclined relative to the axis of the second core shaft, the spiral roll is reciprocatingly wound around the second core shaft until the spiral roll is wound, and the end of the spiral roll is embedded inside for end sealing treatment to lock and prevent falling off, thereby obtaining a preform.

[0037] Preferably, the diameter of the second mandrel is smaller than that of the first mandrel; the diameter of the first mandrel is 3-10 mm, and the diameter of the second mandrel is 0.5-4 mm.

[0038] Preferably, in step (2), the spiral roll is inclined relative to the axis of the second core shaft to form an angle of 40 to 50°, which is set as the winding angle.

[0039] Preferably, in step 3), the loading rate of the cold pressing is 5 to 12 mm / min, displacement control loading is adopted during compression, the cold pressing pressure is at least 900 N, and the holding time is 2 to 15 min. It can be seen from the cold pressing pressure of this step that the cold pressing pressure required for molding the screen tube material of the present invention is small, and compared with the molding pressure of 2 to 80 kN of NiTi shape memory alloy, the processing cost of the screen tube material of the present invention is relatively low.

[0040] Preferably, the ratio of the length of the preform obtained in step (2) to the height of the cold-pressed screen tube material in the cold-pressing direction is 2 to 10:1.

[0041] Preferably, the first mandrel and the second mandrel are both mandrels made of metal materials such as stainless steel or carbon steel.

[0042] The invention also discloses a sieve tube material, which is made by the preparation method of the sieve tube material.

[0043] Specifically, the sieve tube material is composed of the above-mentioned copper-based shape memory alloy wires entangled with each other, and the gaps between the wires constitute the interconnected pores inside the sieve tube material. The porosity of the sieve tube material is 75-85%.

[0044] The stress of the screen tube material corresponding to a compression strain of 50% is 2.81-22.67 MPa, which is much lower than the stress of the NiTi shape memory alloy screen tube material in the prior art corresponding to a compression strain of 50% of 49.79 MPa.

[0045] The screen material has excellent high temperature tolerance and thermal conductivity, with a thermal conductivity of more than 300W / m·K, and can be used for sand control in oil and gas drilling and completion, and is particularly suitable for heavy oil wells with an ambient temperature of more than 200°C that require high thermal conductivity screen materials.

[0046] It can realize spontaneous shape recovery under high temperature conditions, and the recoverable strain can reach 33-50% at a temperature of 100-350°C, meeting the use requirement of not less than 20.4% recoverable strain in actual production; at the same time, the present invention adopts a simple and economical method of regulating the dilution degree to make the screen material have different recovery properties, which is particularly suitable for the complex and changeable high-temperature oil well exploitation needs.

[0047] The present invention also discloses a filter tube assembly suitable for operation in a high-temperature oil well, comprising a porous base tube jacketed on the outside of an oil production pipe, the porous base tube jacketed with a screen tube, the screen tube being a tube made by pressing the above-mentioned screen tube material;

[0048] The height of the screen tube material after cold pressing in the direction of cold pressing pressure is used as the thickness of the screen tube.

[0049] The invention also discloses a method for using the filter tube assembly, which comprises the following steps:.

[0050] 1) placing the screen tube on the porous base tube, wherein the initial thickness of the screen tube is H0;

[0051] 2) Control temperature T <M f , that is, in the low-temperature martensite phase state, a load is applied to the outer peripheral wall of the screen tube to deform and constrain its shape, so that the thickness of the screen tube after pressurization is H1 <H0;

[0052] 3) Ambient temperature T in the oil well a >A f , the filter tube assembly of step 2) is lowered into the oil well. Due to the coupling effect of the structural recovery (pore structure) and phase transformation recovery (martensitic phase transformation) of the screen material, the screen can achieve great strain recovery. The screen expands and recovers to a thickness of H2>H0, and the installation is completed.

[0053] The microstructure inside the screen material after shape recovery or expansion is still the entanglement of alloy wires, maintaining a stable through-hole pore structure. This stable and unique pore structure can ensure that oil and gas can smoothly pass through this embodiment into the oil production pipe, while effectively blocking sand and gravel. BRIEF DESCRIPTION OF THE DRAWINGS

[0054] Figure 1 The overall process flow chart of the copper-based shape memory alloy wire and the screen tube material of the present invention;

[0055] Figure 2 The metallographic photograph and grain diagram of Example 1 of the present invention;

[0056] Figure 3 The metallographic photograph and grain diagram of Example 3 of the present invention;

[0057] Figure 4 The metallographic photograph and grain diagram of Example 5 of the present invention;

[0058] Figure 5 It is a schematic diagram of the winding of the spiral coil of the present invention;

[0059] Figure 6 It is a schematic diagram of the structure of the spiral coil of the present invention;

[0060] Figure 7 It is a schematic diagram of winding of a preform of the present invention;

[0061] Figure 8 A physical diagram of the preform of the present invention;

[0062] Fig. 9 A physical picture of the screen material of the present invention;

[0063] Fig.10 is the DSC curve of Example 1 of the present invention;

[0064] Fig.11 It is the DSC curve of Example 3 of the present invention;

[0065] Fig.12 It is the DSC curve of Example 5 of the present invention;

[0066] Fig.13 is one of the cyclic compression curves of Example 2 of the present invention;

[0067] Fig.14 The second cyclic compression curve of Example 2 of the present invention;

[0068] Fig.15 It is a statistical diagram of the stress required when the embodiment 2, embodiment 4 and embodiment 6 of the present invention are compressed to 50% strain;

[0069] Fig.16 It is a statistical diagram of thermal recovery strain and structural recovery strain when the Example 2, Example 4 and Example 6 of the present invention are compressed by 50% strain;

[0070] Fig.17 It is a schematic diagram of the method of using the filter tube assembly of the present invention.

[0071] Reference numerals

[0072] 1. First mandrel; 2. Spiral roll; 3. Second mandrel; 4. Porous base pipe; 5. Screen pipe. DETAILED DESCRIPTION

[0073] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0074] In the description of the present invention, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present invention.

[0075] like Figure 1 As shown, Figure 1 The following is an overall process flow chart of copper-based shape memory alloy wire and screen tube materials.

[0076] Example 1

[0077] A method for preparing a copper-based shape memory alloy wire comprises the following steps:

[0078] (1) A CuZnAl (Cu at.% 67.85, Zn at.% 23.33, Al at.% 8.83) shape memory alloy wire with a wire diameter of 1.0 mm, a wire length of 5.40 m, and a mass of 34.12 g was selected and placed in a crucible;

[0079] The remaining gaps were then filled with Al2O3 balls with a diameter of 0.25 mm, placed in a vacuum tube furnace, kept at 760°C for 8 h, and then water quenched.

[0080] Record metallographic photos and grain images through a metallographic microscope, such as Figure 2 shown.

[0081] (2) placing the copper-based shape memory alloy wire heat-treated in step (1) in a crucible, filling the remaining gaps with Al2O3 balls with a diameter of 0.25 mm, placing the crucible in a vacuum tube furnace, keeping the temperature at 900°C for 10 min, and then cooling with water quenching;

[0082] (3) The wire was placed in an oil bath using dimethyl silicone oil for heating at 150°C for 1 hour, followed by water quenching. The wire was then placed in a 95% alcohol solution at 25°C and subjected to ultrasonic treatment for 10 minutes to remove oil stains on the wire surface.

[0083] Example 2

[0084] A method for preparing a screen tube material comprises the following steps:

[0085] (1)Reference Figure 5 The copper-based shape memory alloy wire prepared in Example 1 is tilted relative to the axis of the first mandrel 1, and then wound and stretched around the first mandrel 1, wherein the first mandrel 1 is a 304 stainless steel shaft with a diameter of 5 mm. Figure 6 As shown, a spiral coil 2 having a spiral angle α of 50° and a coil outer diameter Φ of 8.53 mm is obtained.

[0086] (2)Reference Figure 7 The spiral roll 2 obtained in step (1) is inclined relative to the axis of the second mandrel 3, the second mandrel 3 is a 304 stainless steel shaft with a diameter of 3 mm, the spiral roll 2 forms a winding angle β of 45° relative to the axis of the second mandrel 3, and then is reciprocatedly wound around the second mandrel 3;

[0087] The spiral roll 2 is wound from the middle of the second core shaft 3, and after the spiral roll 2 is wound unidirectionally to the edge of the second core shaft 3, it is wound back in the opposite direction, that is, it is wound back and forth in the directions of A→B→C→D→E→F and a→b→c→d→e→f in sequence until the spiral roll 2 is wound, and finally the end of the spiral roll 2 is embedded inside for end sealing treatment to lock and prevent it from falling off, so as to obtain a preform with a length of 18.85 cm and a diameter slightly less than 30 mm (such as Figure 8 shown).

[0088] (3) The preform prepared in step (2) is placed in a cylindrical mold with an inner diameter of 30 mm, and cold pressed at a loading rate of 8 mm / min. Displacement-controlled loading is adopted, the cold pressing pressure is 920 N and the pressure is maintained for 5 minutes to obtain a cylindrical sieve tube material (such as Fig. 9 shown).

[0089] Example 3

[0090] A method for preparing a copper-based shape memory alloy wire comprises the following steps:

[0091] (1) A CuZnAl (Cu at.% 67.85, Zn at.% 23.33, Al at.% 8.83) shape memory alloy wire with a wire diameter of 1.0 mm, a wire length of 5.40 m, and a mass of 34.12 g was selected and placed in a crucible;

[0092] The remaining gaps were then filled with Al2O3 balls with a diameter of 0.25 mm, placed in a vacuum tube furnace, kept at 760°C for 24 h, and then water quenched.

[0093] Record metallographic photos and grain images through a metallographic microscope, such as Figure 3 shown.

[0094] (2) placing the copper-based shape memory alloy wire heat-treated in step (1) in a crucible, filling the remaining gaps with Al2O3 balls with a diameter of 0.25 mm, placing the crucible in a vacuum tube furnace, keeping the temperature at 900°C for 10 min, and then cooling with water quenching;

[0095] (3) The wire was placed in an oil bath using dimethyl silicone oil for heating at 150°C for 1 hour, followed by water quenching. The wire was then placed in a 95% alcohol solution at 25°C and subjected to ultrasonic treatment for 10 minutes to remove oil stains on the wire surface.

[0096] Example 4

[0097] A method for preparing a screen tube material comprises the following steps:

[0098] (1)Reference Figure 5 The copper-based shape memory alloy wire prepared in Example 1 is tilted relative to the axis of the first mandrel 1, and then wound and stretched around the first mandrel 1, wherein the first mandrel 1 is a 304 stainless steel shaft with a diameter of 5 mm. Figure 6 As shown, a spiral coil 2 having a spiral angle α of 50° and a coil outer diameter Φ of 8.53 mm is obtained.

[0099] (2)Reference Figure 7 The spiral roll 2 obtained in step (1) is inclined relative to the axis of the second mandrel 3, the second mandrel 3 is a 304 stainless steel shaft with a diameter of 3 mm, the spiral roll 2 forms a winding angle β of 45° relative to the axis of the second mandrel 3, and then is reciprocatedly wound around the second mandrel 3;

[0100] The spiral roll 2 is wound from the middle of the second core shaft 3, and after the spiral roll 2 is wound unidirectionally to the edge of the second core shaft 3, it is wound back in the opposite direction, that is, it is wound back and forth in the directions of A→B→C→D→E→F and a→b→c→d→e→f in sequence until the spiral roll 2 is wound, and finally the end of the spiral roll 2 is embedded inside for end sealing treatment to lock and prevent it from falling off, so as to obtain a preform with a length of 20.64 cm and a diameter slightly less than 30 mm (such as Figure 8 shown).

[0101] (3) The preform prepared in step (2) is placed in a cylindrical mold with an inner diameter of 30 mm, and cold pressed at a loading rate of 8 mm / min. Displacement-controlled loading is adopted, the cold pressing pressure is 922 N and the pressure is maintained for 5 minutes to obtain a cylindrical sieve tube material (such as Fig. 9shown).

[0102] Example 5

[0103] A method for preparing a copper-based shape memory alloy wire comprises the following steps:

[0104] (1) A CuZnAl (Cu at.% 67.85, Zn at.% 23.33, Al at.% 8.83) shape memory alloy wire with a wire diameter of 1.0 mm, a wire length of 5.40 m, and a mass of 34.12 g was selected;

[0105] Record metallographic photos and grain images through a metallographic microscope, such as Figure 4 shown.

[0106] (2) placing the copper-based shape memory alloy wire of step (1) in a crucible, filling the remaining gap with Al2O3 balls with a diameter of 0.25 mm, placing the crucible in a vacuum tube furnace, keeping the temperature at 900°C for 10 min, and then cooling by water quenching;

[0107] (3) The wire was placed in an oil bath using dimethyl silicone oil for heating at 150°C for 1 hour, followed by water quenching. The wire was then placed in a 95% alcohol solution at 25°C and subjected to ultrasonic treatment for 10 minutes to remove oil stains on the wire surface.

[0108] Example 6

[0109] A method for preparing a screen tube material comprises the following steps:

[0110] (1)Reference Figure 5 The copper-based shape memory alloy wire prepared in Example 1 is tilted relative to the axis of the first mandrel 1, and then wound and stretched around the first mandrel 1, wherein the first mandrel 1 is a 304 stainless steel shaft with a diameter of 5 mm. Figure 6 As shown, a spiral coil 2 having a spiral angle α of 50° and a coil outer diameter Φ of 8.53 mm is obtained.

[0111] (2)Reference Figure 7 The spiral roll 2 obtained in step (1) is inclined relative to the axis of the second mandrel 3, the second mandrel 3 is a 304 stainless steel shaft with a diameter of 3 mm, the spiral roll 2 forms a winding angle β of 45° relative to the axis of the second mandrel 3, and then is reciprocatedly wound around the second mandrel 3;

[0112] The spiral roll 2 is wound from the middle of the second core shaft 3, and after the spiral roll 2 is wound unidirectionally to the edge of the second core shaft 3, it is wound back in the opposite direction, that is, it is wound back and forth in the directions of A→B→C→D→E→F and a→b→c→d→e→f in sequence until the spiral roll 2 is wound, and finally the end of the spiral roll 2 is embedded inside for end sealing treatment to lock and prevent it from falling off, so as to obtain a preform with a length of 19.84 cm and a diameter slightly less than 30 mm (such as Figure 8 shown).

[0113] (3) The preform prepared in step (2) is placed in a cylindrical mold with an inner diameter of 30 mm, and cold pressed at a loading rate of 8 mm / min. Displacement-controlled loading is adopted, the cold pressing pressure is 922 N and the pressure is maintained for 5 minutes to obtain a cylindrical sieve tube material (such as Fig. 9 shown).

[0114] Performance Testing

[0115] (1) Determination of crystallinity

[0116] The formula for calculating the rarefaction of the wire is d / D, where d represents the average grain size of the alloy and D represents the diameter of the wire. The average grain size d is calculated as the average value of all radial lines passing through the centroid of the grain.

[0117] According to the above method, statistics Figure 2 All the grains in the embodiment 1 are available, and the average grain diameter d of the embodiment 1 is 0.19 mm. The diameter D of the wire material prepared in the embodiment 1 is 1 mm, and the rarefaction d / D thereof is 0.19.

[0118] According to the above method, statistics Figure 3 All the grains in the embodiment 3 are available, and the average grain diameter d of the embodiment 3 is 0.51 mm. The diameter D of the wire material prepared in the embodiment 3 is 1 mm, and its rarefaction d / D is 0.51.

[0119] According to the above method, statistics Figure 4 All the crystal grains in the embodiment 5 are available, and the average crystal grain diameter d of the embodiment 5 is 0.006 mm, the diameter D of the crystal grains prepared in the embodiment 5 is 1 mm, and the dilution degree d / D thereof is 0.006.

[0120] (2) Differential scanning calorimetry analysis and thermal conductivity test

[0121] Differential scanning calorimetry (DSC) was performed on Example 1, Example 3 and Example 5. At the same time, the element distribution ratio of the samples was obtained by performing EDS test, and the thermal conductivity was calculated.

[0122] The DSC curve of Example 1 is as follows Fig.10 As shown, M of Example 1f 、M s , A s and A f The temperatures are 39.7℃, 67.8℃, 72.3℃ and 97.1℃ respectively; the thermal conductivity is 317.3W / m·K.

[0123] The DSC curve of Example 3 is as follows Fig.11 As shown, M of Example 3 f 、M s , A s and A f The temperatures are 49.5°C, 74.2°C, 73.2°C and 94.9°C respectively; the thermal conductivity is 320.0W / m·K.

[0124] The DSC curve of Example 5 is as follows Fig.12 As shown, M of Example 5 f 、M s , A s and A f The temperatures are 41.1°C, 56.8°C, 62.1°C and 86.6°C respectively; the thermal conductivity is 348.3W / m·K.

[0125] Through the DSC curves of Example 1, Example 3 and Example 5 and the above-mentioned dilution measurement, it can be found that by adjusting the dilution, the phase transition temperature of the copper-based shape memory alloy will also be adjusted to adapt to different usage requirements, and the A of Example 1, Example 3 and Example 5 f The temperature is less than 100°C, and the transformation is complete under high temperature conditions (100-350°C), and the phase change temperature is suitable for use in high temperature environments; on the other hand, through the special graded quenching heat treatment method of the present invention, copper-based shape memory alloys of different dilutions avoid martensite stabilization and can exhibit a stable shape memory effect under high temperature conditions (100-350°C), indicating that the screen material containing the copper-based shape memory alloy of the present invention can be used in a high-temperature oil well bottom environment and achieve spontaneous shape recovery, and is suitable for high-temperature heavy oil wells above 200°C that require high thermal conductivity screen materials.

[0126] (3) Porosity measurement

[0127] The mass m, diameter D and height H of Example 2, Example 4 and Example 6 are measured, where V is the apparent volume of the sample, and the density of the copper-based shape memory alloy wire is known to be ρ s =8.05g / cm 3 The porosity P of Example 2, Example 4 and Example 6 is calculated by the following formula: is the relative density.

[0128]

[0129]

[0130] Calculation shows that the porosity of Example 2 is 80.4%, the porosity of Example 4 is 80.9%, and the porosity of Example 6 is 75.2%. The appropriate porosity is combined with the shape memory effect of the wire to achieve the high recovery characteristics of the present invention. It also proves that the preparation process of the present invention can regulate the porosity to meet the filtration accuracy requirements in the oil and gas production process.

[0131] (4) Compression test

[0132] (4-1) Compression tests were performed at room temperature according to ASTM E9-89a standard. The testing equipment was an INSTRON 5984 universal material testing machine. Displacement-controlled loading was adopted with a loading rate of 0.5 mm / min. Compression performance tests were performed on Example 2 at 20%, 30%, 40% and 50% compressive strains, respectively. Loading and unloading tests at 50% compressive strain were directly performed on Example 4 and Example 6.

[0133] The test results of Example 2 are shown in Fig.13 and Fig.14 As can be seen from the figure, the stress values ​​of Example 2 at 20%, 30%, 40% and 50% strains are 3.50 MPa, 5.03 MPa, 7.95 MPa and 16.14 MPa, respectively.

[0134] After experiencing 20% ​​and 30% compressive strain loading, the shape of Example 2 can be completely restored to the unloaded state, indicating that the recoverable strain brought by the structure of Example 2 at room temperature reaches 30%, which is far beyond the maximum recoverable strain of the copper-based shape memory alloy itself, indicating that the present invention can effectively improve the comprehensive performance of the copper-based shape memory alloy.

[0135] The stress required for Example 2, Example 4 and Example 6 to compress to 50% strain is as follows: Fig.15 shown.

[0136] The corresponding stress of Example 2 at a compressive strain of 50% is 16.14 MPa, the corresponding stress of Example 4 at a compressive strain of 50% is 2.81 MPa, and the corresponding stress of Example 6 at a compressive strain of 50% is 22.67 MPa. That is, the stress (2.81-22.67 MPa) corresponding to the compressive strain of 50% of the screen tube material prepared by the present invention is much lower than the stress 49.79 MPa corresponding to the compressive strain of 50% of the NiTi shape memory alloy screen tube material in the prior art.

[0137] (4-2) After experiencing 50% compressive strain, Examples 2, 4 and 6 were placed in a 200° C. water bath for 8 hours, and the structural recovery strain and thermal recovery strain were tested.

[0138] The results are as follows Fig.16 As shown. Example 2 produced 21.3% of phase change driven rebound strain (phase change recovery, i.e., shape memory recovery strain), and its recoverable strain (i.e., the sum of structural recovery and phase change recovery) reached 33.2%; Example 4 produced 24.4% of phase change driven rebound strain, and its recoverable strain reached 48.7%; Example 6 produced 16.6% of phase change driven rebound strain, and its recoverable strain reached 35.2%, indicating that the screen tube materials prepared by the present invention have reached and far exceeded the actual production use requirement of 20.4% recoverable strain.

[0139] Example 7

[0140] like Fig.17 As shown, a filter tube assembly comprises a porous base tube 4 which is jacketed on the outside of an oil production tube. The porous base tube 4 is jacketed with a screen tube 5 which is a tube fitting pressed by Example 4.

[0141] The height of Example 4 in the pressure direction after cold pressing is the thickness of the screen tube 5.

[0142] The method for using the filter tube assembly comprises the following steps:

[0143] 1) placing a screen tube 5 on the porous base tube 4, wherein the initial thickness of the screen tube 5 is H0;

[0144] 2) Control temperature T <M f , that is, in the low-temperature martensite phase state, a load is applied to the outer peripheral wall of the screen tube 5 to deform and constrain its shape, so that the thickness of the pressurized screen tube 5 is H1 <H0;

[0145] 3) Ambient temperature T in the oil well a >A f , the filter tube assembly of step 2) is lowered into the oil well. Due to the coupling effect of the structural recovery (pore structure) and phase transformation recovery (martensitic phase transformation) of the screen tube material, the screen tube 5 can achieve great strain recovery. The screen tube 5 expands and recovers to a thickness of H2>H0, and the installation is completed.

[0146] The microstructure inside the screen material after shape recovery or expansion is still the entanglement of alloy wires, maintaining a stable through-hole pore structure. This stable and unique pore structure can ensure that oil and gas can smoothly pass through this embodiment into the oil production pipe, while effectively blocking sand and gravel.

[0147] According to the disclosure and teaching of the above description, those skilled in the art to which the present invention belongs may also change and modify the above implementation modes. Therefore, the present invention is not limited to the specific implementation modes disclosed and described above, and some modifications and changes to the present invention should also fall within the protection scope of the claims of the present invention. In addition, although some specific terms are used in this specification, these terms are only for the convenience of description and do not constitute any limitation to the present invention.

Claims

1. A method for improving the performance of a copper-based shape memory alloy, characterized in that: The steps include: (1) placing a copper-based shape memory alloy wire in a reaction device in a sand bath for heating, maintaining the temperature at 600 to 900° C. for 4 to 30 hours under a vacuum environment or an inert atmosphere, and then taking out the copper-based shape memory alloy wire for rapid cooling; (2) placing the cooled copper-based shape memory alloy wire in the reaction device again for sand bath heating, keeping the temperature at 750-900° C. for 10-30 min under vacuum or inert atmosphere, and then taking out the copper-based shape memory alloy wire for rapid cooling; (3) heating the cooled copper-based shape memory alloy wire in an oil bath, keeping the temperature at 120-160° C. for 0.5-2 h, then taking out the copper-based shape memory alloy wire for rapid cooling; and cleaning.

2. The method for improving the performance of copper-based shape memory alloy according to claim 1, characterized in that: In step (1), the copper-based shape memory alloy wire is CuZnAl, wherein the atomic percentage of Cu is 66.02-81.75%, the atomic percentage of Zn is 15.09-24.52%, and the atomic percentage of Al is 3.05-9.88%; The wire diameter of the copper-based shape memory alloy wire is 0.7-1.2 mm.

3. The method for improving the performance of a copper-based shape memory alloy according to claim 1 or 2, characterized in that: In step (1) and step (2), the fine sand heated in the sand bath is Al2O3 pellets; The diameter of the Al2O3 ball is smaller than the diameter of the copper-based shape memory alloy wire.

4. The method for improving the performance of a copper-based shape memory alloy according to claim 1 or 2, characterized in that: In step (3), the oil used for oil bath heating is dimethyl silicone oil.

5. A copper-based shape memory alloy wire, characterized in that: The invention is made by the performance improvement method for copper-based shape memory alloys as described in any one of claims 1 to 4.

6. A method for preparing a sieve tube material, characterized in that: The steps include: (1) preparing a cylindrical first mandrel, winding and stretching the copper-based shape memory alloy wire around the first mandrel, wherein the copper-based shape memory alloy wire is inclined relative to the axis of the first mandrel to form a spiral coil; (2) The spiral coils obtained in step (1) are interlocked by winding, laying out and weaving to obtain a preform with a stable structure; (3) placing the preform obtained in step (2) in a mold for cold pressing to obtain a screen tube material.

7. The method for preparing the sieve tube material according to claim 6, characterized in that: In step (1), the copper-based shape memory alloy wire is inclined relative to the axis of the first core shaft to form an angle of 45 to 55°, which is set as the helix angle; The specific operation of step (2) is as follows: a cylindrical second mandrel is prepared, the spiral roll obtained in step (1) is inclined relative to the axis of the second mandrel, the spiral roll is reciprocatedly wound around the second mandrel until the spiral roll is wound, and the end of the spiral roll is embedded inside and sealed to lock and prevent it from falling off, thereby obtaining a preform; In step (2), the spiral winding is inclined relative to the axis of the second mandrel to form an angle of 40 to 50 degrees, which is set as the winding angle; In step 3), the cold pressing loading rate is 5 to 12 mm / min, displacement-controlled loading is adopted during compression, the cold pressing pressure is at least 900 N, and the holding time is 2 to 15 min; The ratio of the length of the preform obtained in step (2) to the height of the cold-pressed screen tube material in the cold-pressing direction is 2 to 10:

1.

8. A screen material, characterized in that: The sieve tube material is made by the preparation method of the sieve tube material according to claim 6 or 7.

9. A filter tube assembly suitable for operation in a high-temperature petroleum well, characterized in that: It comprises a porous base pipe which is jacketed on the outside of the oil production pipe, the porous base pipe is jacketed with a screen pipe, and the screen pipe is a pipe fitting formed by pressing the screen pipe material according to claim 8; The height of the screen tube material after cold pressing in the direction of cold pressing pressure is used as the thickness of the screen tube.

10. The method for using the filter tube assembly according to claim 9, characterized in that: The steps include: (1) placing a screen tube on the porous base tube, wherein the initial thickness of the screen tube is H0; (2) Control temperature T <M f , a load is applied to the outer peripheral wall of the screen tube so that the thickness of the screen tube after pressurization is H1 <H0; (3) Ambient temperature T in the oil well a >A f , the filter tube assembly of step 2) is lowered into the oil well, and the screen tube expands and returns to a thickness of H2>H0, completing the installation.

Citation Information

Patent Citations

  • High-performance copper-based shape memory alloy material

    CN102400008A

  • Heat treatment process for improving friction and wear properties of copper-zinc-aluminum memory alloy

    CN104233131A

  • Novel self-expansion screen pipe

    CN105626001A

  • Damage patching and repairing method based on memory alloy and for expandable tubular

    CN108661585A

  • Cu SECTION SHAPE MEMORY ALLOY AND ITS FABRICATION METHOD

    KR1019900010029A

Cited By

  • Preparation method of supersonic speed cold spraying solid phase additive copper-based shape memory alloy

    CN120055285A

  • Preparation method of copper-based shape memory alloy by supersonic cold spraying solid-phase additive

    CN120055285B

  • Manufacturing method of composite metal rubber

    CN120396380A

  • A method for manufacturing composite metal rubber

    CN120396380B

  • Electric heating auxiliary steam injection oil extraction device for horizontal well

    CN122106517A