Aluminized steel sheet, method for manufacturing aluminized steel sheet, and method for manufacturing hot stamped body

By controlling the oxide layer thickness and hydroxide ratio on Al-plated steel sheets, hydrogen embrittlement during hot stamping is suppressed, enhancing the reliability of the steel sheet and the molded article.

JP7594219B2Active Publication Date: 2024-12-04NIPPON STEEL CORPORATION
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2023534773
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-07-14
Filing Date
2022-07-08
Publication Date
2024-12-04
Estimated Expiration
2042-07-08

AI Technical Summary

Technical Problem

During the hot stamping process of Al-plated steel sheets, hydrogen penetrates into the steel material due to oxidation of the Al plating, leading to hydrogen embrittlement, which existing technologies have not adequately addressed.

Method used

An Al-plated steel sheet with a specific chemical composition and an oxide layer formed through a preliminary oxidation process, where the oxide layer thickness is controlled between 10 to 400 nm and the hydroxide layer to oxide layer ratio is 30% or less, reducing hydrogen penetration.

Benefits of technology

The solution effectively suppresses hydrogen embrittlement in the steel material during hot stamping, resulting in a highly reliable Al-plated steel sheet and a hot-stamped molded article with reduced hydrogen content.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007594219000003
    Figure 0007594219000003
  • Figure 0007594219000004
    Figure 0007594219000004
  • Figure 0007594219000005
    Figure 0007594219000005
Patent Text Reader

Abstract

Provided is an Al-plated steel sheet with which it is possible to suppress hydrogen embrittlement that progresses due to hydrogen entering a steel material with oxidation of Al plating during hot stamp molding. This Al-plated steel sheet (1) comprises a steel substrate having a prescribed chemical composition, an Al plating layer (20) that is formed on the steel substrate and that is a plating layer containing Al and Si, and an oxide layer (30) formed on the Al plating layer (20), the oxide layer (30) having a thickness d of 10-400 nm, the oxide layer (30) containing a hydroxide layer (31), and the ratio of the thickness d1 of the hydroxide layer (31) relative to the thickness d of the oxide layer (30) being 30% or less. The thickness d of the oxide layer (30) is deemed to be the depth from the surface at which, in a depth-direction analysis by X-ray photoelectron spectroscopy, the integrated intensity for oxide is 1 / 2 of the maximum value. The thickness d1 of the hydroxide layer 31 is deemed to be the depth from the surface at which, in a depth-direction analysis by X-ray photoelectron spectroscopy, the integrated intensity for hydroxide is 1 / 2 of the maximum value.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an aluminized steel sheet, a method for producing an aluminized steel sheet, and a hot stamped product, and more particularly to an aluminized steel sheet for hot stamping and a method for producing the same, and a method for producing a hot stamped product using the same. [Background technology]

[0002] Hot stamping is known as a technique for forming high-strength steel (especially ultra-high strength steel of 1500 MPa or more) with high dimensional accuracy, which is difficult to ensure formability in. The hot stamping method eliminates the formability issue by forming the steel sheet in a state where it is heated to a high temperature of 800°C or more, and obtains the desired high strength by cooling after forming.

[0003] Since the hot stamping method involves heating in the atmosphere, scale forms on the surface of the steel sheet, which must be removed in a later process. To improve this, a technology is known in which the steel sheet is plated with aluminum containing silicon to suppress oxidation.

[0004] JP 2003-193187 A describes that the occurrence of cracks during processing is suppressed by setting the Al content of the Fe-Al coating to 35% or less. WO 2019 / 160106 A describes an Fe-Al-plated hot stamp member in which the Fe-Al-plated layer has a predetermined structure in order to improve the corrosion resistance of the formed part and the corrosion resistance after painting.

[0005] In the hot stamping method, hydrogen penetrates into the steel material during heating, which is said to increase the susceptibility of the steel material to hydrogen embrittlement. International Publication No. 2012 / 120692 describes a method for improving delayed fracture resistance by forming an Fe-Mn composite oxide in the steel sheet and trapping hydrogen at the interface between the composite oxide and the steel matrix. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2003-193187 A [Patent Document 2] International Publication No. 2019 / 160106 [Patent Document 3] International Publication No. 2012 / 120692 [Patent Document 4] JP 2016-65312 A [Patent Document 5] JP 2022-31677 A [Patent Document 6] Special Publication No. 2022-513595 [Patent Document 7] Japanese Patent Application Publication No. 6-272017 Summary of the Invention [Problem to be solved by the invention]

[0007] When aluminized steel sheets are subjected to a hot stamping process, hydrogen may penetrate into the steel material due to oxidation of the aluminized coating.

[0008] An object of the present invention is to provide an aluminized steel sheet having high reliability and capable of suppressing hydrogen embrittlement caused by hydrogen penetrating into the steel material accompanying oxidation of the aluminization during hot stamp forming, and to provide a method for producing the same. Another object of the present invention is to provide a hot stamped product in which hydrogen embrittlement is suppressed. [Means for solving the problem]

[0009] An aluminized steel sheet according to one embodiment of the present invention is an aluminized steel sheet for hot stamping, comprising a steel base material, an aluminized layer that is a plating layer containing Al and Si and is formed on the steel base material, and an oxide layer that is formed on the aluminized layer, and the chemical composition of the steel base material is, in mass%, C: 0.1 to 0.6%, Si: 0.01 to 1.50%, Mn: 0.10 to 3.00%, P: 0.05% or less, S: 0.020% or less, Al: 0.1 to 0.6%, Si: 0.01 to 1.50%, Mn: 0.10 to 3.00%, P: 0.05% or less, S: 0.020% or less, and Al: 0.1 to 0.6%. 0.10% or less, Ti: 0.01-0.10%, B: 0.0001-0.0100%, N: 0.015% or less, Cr: 0-1.0%, Mo: 0-1.0%, Ni: 0-1.0%, Cu: 0-1.0%, Nb: 0-1.0%, balance: Fe and impurities, the thickness of the oxide layer is 10-400 nm, the oxide layer includes a hydroxide layer, and the ratio of the thickness of the hydroxide layer to the thickness of the oxide layer is 30% or less. Here, the thickness of the oxide layer is the depth from the surface when the integrated intensity of the oxide becomes 1 / 2 of the maximum value in a depth direction analysis by X-ray photoelectron spectroscopy, and the thickness of the hydroxide layer is the depth from the surface when the integrated intensity of the hydroxide becomes 1 / 2 of the maximum value in a depth direction analysis by X-ray photoelectron spectroscopy.

[0010] A method for producing an aluminized steel sheet according to one embodiment of the present invention is a method for producing the aluminized steel sheet described above, and includes a preliminary oxidation step of heating the aluminized steel sheet to a temperature of 120 to 600°C.

[0011] A hot stamped steel according to one embodiment of the present invention includes a step of hot stamping the above-mentioned Al-plated steel sheet. Effect of the Invention

[0012] According to the present invention, it is possible to obtain a highly reliable aluminized steel sheet capable of suppressing hydrogen embrittlement that progresses due to hydrogen penetrating into a steel material accompanying oxidation of the aluminized coating during hot stamp forming. Also, according to the present invention, it is possible to obtain a hot stamped product in which hydrogen embrittlement is suppressed. [Brief description of the drawings]

[0013] [Figure 1] FIG. 1 is a schematic cross-sectional view of an aluminized steel sheet according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic cross-sectional view showing an enlarged configuration of the oxide layer of FIG. [Diagram 3] FIG. 3 is an example of an O 1s spectrum measured by XPS. [Figure 4] FIG. 4 shows an example of the depth profile of the integrated intensity of oxide and hydroxide. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] The present inventors have investigated the relationship between the oxide layer formed on the surface of an aluminized steel sheet and the amount of hydrogen that penetrates into the steel material when the aluminized steel sheet is subjected to a hot stamping process. During the investigation, it was found that the amount of hydrogen that penetrates into the steel material is reduced when the aluminized steel sheet is subjected to a preliminary oxidation process in which the aluminized steel sheet is heated under specified conditions and then subjected to a hot stamping process.

[0015] Immediately after plating, aluminized steel sheets have an oxide layer (initial oxide layer) on the surface that is several nm thick. This initial oxide layer contains, from the surface side, a hydroxide layer that contains a large amount of hydroxide, and an oxide layer that contains less hydroxide. Here, hydroxides include those that contain OH groups (hydroxyl groups) in their structure, such as Al(OH)3 and AlOOH. On the other hand, oxides include those that contain OH groups (hydroxyl groups), such as Al2O3 and Al 2 FeO As shown in Figure 4, the initial oxidation layer is expressed by a chemical formula consisting only of metal and oxygen. In the initial oxidation layer, the ratio of the thickness of the hydroxide layer to the thickness of the oxide layer is relatively high. When a pre-oxidation process is performed on an aluminized steel sheet, the oxide layer becomes thicker and the ratio of the thickness of the hydroxide layer to the thickness of the oxide layer decreases.

[0016] The hydrogen that penetrates into the steel material during the hot stamping process is assumed to be hydrogen from the hydroxides on the steel material surface and hydrogen from the moisture in the atmosphere. The above-mentioned preliminary oxidation process is considered to contribute to reducing both of these hydrogens. That is, the preliminary oxidation process promotes the release of hydrogen from the hydroxides on the steel material surface, and the oxide layer with reduced hydroxides functions as a protective layer against further oxidation, suppressing the oxidation reaction during the hot stamping process and suppressing the dissociation reaction of moisture in the atmosphere.

[0017] The present invention has been completed based on the above findings. Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings. In the drawings, the same or corresponding parts are designated by the same reference numerals and their description will not be repeated. The dimensional ratios between the components shown in each drawing do not necessarily represent the actual dimensional ratios.

[0018] [Aluminum-plated steel sheet] 1 is a schematic cross-sectional view of an Al-plated steel sheet 1 according to one embodiment of the present invention. The Al-plated steel sheet 1 includes a steel substrate 10, an Al-plated layer 20 formed on the steel substrate 10, and an oxide layer 30 formed on the Al-plated layer 20. The Al-plated layer 20 and the oxide layer 30 may be formed on one side of the steel substrate 10, or on both sides of the steel substrate 10.

[0019] [Oxidation layer] The oxide layer 30 is a layer formed by oxidizing the surface of the Al plating layer 20, and contains oxides and hydroxides of Al. Examples of oxides of Al include Al2O3 and Al 2 FeO 4. Examples of hydroxides of Al include Al(OH)3 and AlOOH. The oxide layer 30 may contain oxides other than the oxide of Al, or hydroxides other than the hydroxide of Al.

[0020] 2 is a schematic cross-sectional view showing an enlarged configuration of the oxide layer 30. The oxide layer 30 includes a hydroxide layer 31, which is a layer containing a large amount of hydroxide, and an oxide layer 32, which is a layer containing a small amount of hydroxide. The hydroxide contained in the oxide layer 30 is distributed in large amounts on the surface side of the oxide layer 30. Therefore, the hydroxide layer 31 is formed on the surface side, and the oxide layer 32 is formed on the substrate side.

[0021] In this embodiment, the thickness d of the oxide layer 30 is 10 to 400 nm, and the ratio of the thickness d1 of the hydroxide layer 31 to the thickness d of the oxide layer 30 is 30% or less.

[0022] The oxide layer 30 functions as a protective layer against further oxidation of the Al-plated steel sheet 1. That is, by forming the oxide layer 30 of a predetermined thickness in advance on the Al-plated steel sheet 1, it is possible to suppress the oxidation reaction in the hot stamping process. This makes it possible to reduce the amount of hydrogen that penetrates into the steel base material 10 during the hot stamping process. If the thickness d of the oxide layer 30 is less than 10 nm, this effect cannot be sufficiently obtained. On the other hand, if the thickness d of the oxide layer 30 exceeds 400 nm, the influence of hydrogen in the hydroxide contained in the oxide layer 30 becomes large. The lower limit of the thickness d of the oxide layer 30 is preferably 20 nm. The upper limit of the thickness d of the oxide layer 30 is preferably 300 nm, more preferably 200 nm, more preferably 100 nm, and more preferably 50 nm.

[0023] The hydroxide contained in the oxide layer 30 can be a source of hydrogen that penetrates into the steel substrate 10. By setting the ratio of the thickness d1 of the hydroxide layer 31 to the thickness d of the oxide layer 30 to 30% or less, the amount of hydrogen that penetrates from the hydroxide into the steel material can be reduced. The ratio of the thickness d1 of the hydroxide layer 31 to the thickness d of the oxide layer 30 is preferably 25% or less, more preferably 20% or less, and even more preferably 15% or less.

[0024] The thickness d of the oxide layer 30 and the thickness d1 of the hydroxide layer 31 are measured by depth profile analysis using X-ray photoelectron spectroscopy (XPS) as follows.

[0025] Figure 3 is an example of an O 1s spectrum measured by XPS. The O 1s spectrum contains oxide and hydroxide peaks. The background is subtracted from this O 1s spectrum, and the oxide and hydroxide peaks are waveform separated to determine their respective integrated intensities. The background is processed using the Shirley method, which is a typical method for processing XPS data. The ratio of the integrated intensities obtained here corresponds to the abundance ratio of oxide and hydroxide at the depth being measured.

[0026] Ar + While performing ion sputtering, sputtering and XPS measurement are repeated to obtain a depth profile of the integrated intensity of oxides and hydroxides. Figure 4 shows an example of a depth profile of the integrated intensity of oxides and hydroxides.

[0027] Here, the position where the hydroxide integrated intensity is half of the maximum value is defined as the layer boundary between the hydroxide layer 31 and the oxide layer 32. Also, the position where the oxide integrated intensity is half of the maximum value is defined as the layer boundary between the oxide layer 32 and the Al plating layer 20.

[0028] That is, the thickness d1 of the hydroxide layer 31 is the depth from the surface when the integrated intensity of the hydroxide is half of its maximum value. The thickness d of the oxide layer 30 is the depth from the surface when the integrated intensity of the oxide is half of its maximum value. The thickness d2 of the oxide layer 32 is the thickness d of the oxide layer 30 minus the thickness d1 of the hydroxide layer 31.

[0029] [Aluminum plating layer] The Al plating layer 20 is a plating layer containing Al and Si. In the Al plating layer 20, intermetallic compounds of Al, Fe, and Si may be formed. The chemical composition of the Al plating layer 20 (average composition in the thickness direction; the same applies hereinafter in this paragraph) is, but is not limited to, for example, Al: 20 to 100 mass%, Si: 1 to 20 mass%, and Fe: 0 to 60 mass%. The lower limit of the Al content of the Al plating layer 20 is preferably 25 mass%. The upper limit of the Al content of the Al plating layer 20 is preferably 95 mass%, more preferably 90 mass%, more preferably 70 mass%, and more preferably 55 mass%. The lower limit of the Si content of the Al plating layer 20 is preferably 2 mass%, and more preferably 5 mass%. The upper limit of the Si content of the Al plating layer 20 is preferably 15 mass%, and more preferably 12 mass%. The lower limit of the Fe content of the Al plating layer 20 is preferably 20 mass%. The upper limit of the Fe content in the Al plating layer 20 is preferably 50 mass %, and more preferably 40 mass %.

[0030] The Al plating layer 20 may contain elements other than Al, Si, and Fe. Specifically, Be, Mg, Ca, Sr, Ba, Sc, Ti, V, Cr, Mn, Co, Ni, Cu, Zn, Zr, Y, Nb, Ce, Ta, etc. may be added. The total content of elements other than Al, Si, and Fe is preferably 10 mass% or less, more preferably 5 mass% or less, even more preferably 3 mass% or less, and even more preferably 1 mass% or less.

[0031] The thickness of the Al plating layer 20 is not particularly limited, but is, for example, 1 to 100 μm. The lower limit of the thickness of the Al plating layer 20 is preferably 5 μm, more preferably 10 μm, and even more preferably 15 μm. The upper limit of the thickness of the Al plating layer 20 is preferably 50 μm, more preferably 40 μm, and even more preferably 30 μm.

[0032] [Steel base material] The steel base material 10 is, for example, a hot-rolled steel sheet or a cold-rolled steel sheet. The chemical composition of the steel base material 10 will be described below. In the following description, "%" for the content of an element means mass %.

[0033] C: 0.1 to 0.6% Carbon (C) is contained to ensure the desired mechanical strength. If the C content is less than 0.1%, sufficient improvement in mechanical strength cannot be obtained. On the other hand, if the C content exceeds 0.6%, elongation and reduction of area tend to decrease. The upper limit of the C content is preferably 0.5%.

[0034] Silicon: 0.01 to 1.50% Silicon (Si) is an element that improves mechanical strength, and is contained to ensure the desired mechanical strength, similar to C. If the Si content is less than 0.01%, sufficient improvement in mechanical strength cannot be obtained. On the other hand, if the Si content exceeds 1.50%, the Si oxide formed on the surface layer of the steel substrate may cause a decrease in wettability during plating, resulting in the risk of non-plating. The upper limit of the Si content is preferably 0.60%.

[0035] Mn: 0.10-3.00% Manganese (Mn) is one of the elements that strengthen steel and also one of the elements that improve hardenability. Mn is also effective in preventing hot embrittlement caused by S, one of the impurities. If the Mn content is less than 0.10%, these effects cannot be sufficiently obtained. On the other hand, if the Mn content exceeds 3.00%, there is a risk that the amount of retained austenite becomes too large, resulting in a decrease in strength. The lower limit of the Mn content is preferably 0.50%. The upper limit of the Mn content is preferably 2.00%.

[0036] P:0.05% or less Phosphorus (P) is an impurity contained in the steel substrate. P contained in the steel substrate may segregate at the grain boundaries of the steel substrate and reduce the toughness of the steel substrate. It is preferable to keep the P content as low as possible.

[0037] S: 0.020% or less Sulfur (S) is an impurity contained in a steel substrate. S contained in a steel substrate may form sulfides and reduce the toughness of the steel substrate. It is preferable to reduce the S content as much as possible.

[0038] Al: 0.10% or less Aluminum (Al) is generally used for the purpose of deoxidizing steel. However, if the Al content is high, the Ac3 point of the steel substrate rises, so that it is necessary to increase the heating temperature required to ensure the hardenability of the steel during the hot stamping process. Therefore, the Al content is preferably 0.10% or less. The Al content is more preferably 0.05% or less, and further preferably 0.01% or less.

[0039] Ti: 0.01 to 0.10% Titanium (Ti) is one of the strength-enhancing elements. If the Ti content is less than 0.01%, the strength and oxidation resistance are not sufficiently improved. On the other hand, if the Ti content exceeds 0.10%, carbides and nitrides are formed, which may soften the steel.

[0040] B: 0.0001 to 0.0100% Boron (B) acts during hardening to improve strength. If the B content is less than 0.0001%, the strength improvement effect is not sufficient. On the other hand, if the B content exceeds 0.0100%, inclusions are formed, which embrittles the steel base material and may reduce fatigue strength.

[0041] N: 0.015% or less Nitrogen (N) is an impurity contained in the steel substrate. N contained in the steel substrate may form nitrides and reduce the toughness of the steel substrate. Furthermore, N contained in the steel substrate may combine with B to reduce the amount of solute B, thereby reducing the effect of B in improving hardenability. It is preferable to keep the N content as low as possible. The upper limit of the N content is preferably 0.010%.

[0042] The steel substrate 10 may contain one or more of Cr, Mo, Ni, Cu, and Nb. Cr, Mo, Ni, Cu, and Nb are all optional elements. That is, the steel substrate 10 may not contain any or all of Cr, Mo, Ni, Cu, and Nb.

[0043] Cr: 0~1.0% Chromium (Cr) improves hardenability and increases temper softening resistance by forming carbides. It also improves corrosion resistance and is effective in improving high-temperature strength. Therefore, it may be added as necessary. The lower limit of the Cr content is preferably 0.01%. On the other hand, if it is added in excess of 1.0%, the effect saturates and costs increase.

[0044] Mo: 0-1.0% Molybdenum (Mo) easily forms carbides and increases temper softening resistance. The effect is enhanced by adding it in combination with Cr. A small amount of Mo also improves hardenability, increases the crystal grain coarsening temperature, and is highly effective in preventing temper embrittlement. Therefore, it may be added as necessary. The lower limit of the Mo content is preferably 0.01%. On the other hand, if the content exceeds 1.0%, the effect saturates and the cost increases.

[0045] Ni: 0-1.0% Nickel (Ni) significantly lowers the A1 transformation point and improves strength, toughness, and hardenability. When added in combination with Cr or Mo, a synergistic effect is likely to occur. It also improves corrosion resistance and suppresses low-temperature embrittlement. Therefore, it may be added as necessary. The lower limit of the Ni content is preferably 0.01%. On the other hand, if it is added in excess of 1.0%, the effect saturates and costs increase.

[0046] Cu: 0-1.0% Copper (Cu) improves hardenability and corrosion resistance. Therefore, it may be contained as necessary. The lower limit of the Cu content is preferably 0.01%. On the other hand, even if it is contained in excess of 1.0%, the effect is saturated and the cost increases.

[0047] Nb: 0-1.0% Niobium (Nb) improves hardenability. Since Nb has a larger metal radius and higher density than Fe, the main component of steel, it is difficult to dissolve in the Fe matrix, and by precipitating at the grain boundaries of steel, it plays a role in preventing the grains from becoming coarse. It also suppresses temper embrittlement. Therefore, it may be contained as necessary. The lower limit of the Nb content is preferably 0.01%. On the other hand, even if it is contained in an amount exceeding 1.0%, the effect is saturated and the cost increases.

[0048] The balance of the chemical composition of the steel substrate 10 is Fe and impurities. The impurities referred to here are elements mixed in from ores or scraps used as raw materials for steel, or elements mixed in from the environment during the manufacturing process. Examples of impurities include Zn, Co, Sn, V, As, Zr, Ca, Mg, etc. in addition to the elements listed above.

[0049] [Manufacturing method of aluminized steel sheets] Next, an example of a method for producing the aluminized steel sheet 1 will be described.

[0050] [Plating process] An Al plating layer 20 is formed on the surface of the steel substrate 10 by hot-dip plating. The temperature of the plating bath is preferably 600 to 700°C. If the temperature of the plating bath is lower than 600°C, the viscosity of the plating bath becomes low, making it difficult to achieve uniform plating. If the temperature of the plating bath is higher than 700°C, the components change in a short time due to volatilization, making process control difficult.

[0051] The plating bath contains Si in addition to Al. The Si content in the plating bath is, for example, 1 to 20 mass%, preferably 5 to 15 mass%. The plating bath may contain elements other than Al and Si. Specifically, in addition to Fe, Al, Si, O, and H, Be, Mg, Ca, Sr, Ba, Sc, Ti, V, Cr, Mn, Co, Ni, Cu, Zn, Zr, Y, Nb, Ce, Ta, and the like may be added to the plating bath. The metal component ratio of the Al plating layer 20 and the oxide layer 30 is modulated by the chemical composition of the plating bath, but is applicable as long as the plating layer formed in the plating process is a layer mainly composed of Al. The lower limit of the Al content in the plating bath is preferably 70 mass%, preferably 80 mass%, more preferably 85 mass%, and even more preferably 88 mass%.

[0052] The steel substrate 10 is maintained at, for example, 700 to 800°C, and then immersed in a plating bath. The plating process is preferably performed in a non-oxidizing atmosphere (including a reducing atmosphere) throughout. In an oxidizing atmosphere, the surface of the steel substrate 10 may be oxidized, resulting in non-uniform plating, and the plating bath may be oxidized, resulting in loss. The thickness of the Al plating layer 20 can be adjusted by the temperature, viscosity, immersion time, gas spraying, etc. of the plating bath.

[0053] Although the above describes the case where the plating layer is formed by hot-dip plating, the plating layer may be formed by vapor deposition or thermal spraying instead of hot-dip plating. In this case, an Al alloy may be used, or Al and the additive element may be vapor-deposited or thermally sprayed separately.

[0054] [Pre-oxidation process] A preliminary oxidation step is performed in which the Al-plated steel sheet is heated under predetermined conditions. Specifically, the Al-plated steel sheet is heated to a temperature of 120 to 600°C (any temperature within the range of 120°C to 600°C).

[0055] If the temperature of the preliminary oxidation is lower than 120°C, the dehydration from the initial oxidation layer proceeds slowly, and the ratio of the thickness d1 of the hydroxide layer 31 to the thickness d of the oxide layer 30 may not be sufficiently reduced. On the other hand, if the temperature of the preliminary oxidation exceeds 600°C, it may be difficult to appropriately control the thickness d of the oxide layer 30. In addition, the Al plating layer 20 may form an alloy with the steel substrate 10, or the steel substrate 10 may be altered, resulting in a decrease in workability and making the steel unsuitable for hot stamping. The lower limit of the temperature of the preliminary oxidation is preferably 150°C, more preferably 180°C. The upper limit of the temperature of the preliminary oxidation is preferably 400°C, more preferably 300°C, and more preferably 250°C.

[0056] The retention time depends on the temperature and other conditions, but is, for example, 1 minute to 48 hours. The lower limit of the retention time is preferably 20 minutes, and more preferably 40 minutes. The upper limit of the retention time is preferably 24 hours, and more preferably 12 hours, and more preferably 4 hours, and more preferably 2 hours.

[0057] The pre-oxidation step is preferably carried out in an oxidizing atmosphere, and particularly in the air, from the viewpoint of cost. However, the pre-oxidation step can be carried out in any atmosphere that is not excessively non-oxidizing, and even if the pre-oxidation step is carried out in, for example, a reduced pressure atmosphere, a reducing atmosphere, an inert gas atmosphere, or a high dew point environment, the desired oxide layer 30 can be formed depending on the conditions. The pre-oxidation step atmosphere preferably has a dew point of -70°C or higher, more preferably -30°C or higher, and even more preferably 0°C or higher. The pre-oxidation step atmosphere preferably has an oxygen partial pressure of 0.001 MPa or higher, and even more preferably 0.01 MPa or higher.

[0058] The heating method in the preliminary oxidation step may be any method, for example, a high-temperature furnace or electrical heating may be used. The temperature increase rate and temperature decrease rate may be any method, for example, 10 to 1000° C. / s.

[0059] The preliminary oxidation step can be carried out at any timing after the plating step and before the plated steel sheet is subjected to the hot stamping step. For example, the preliminary oxidation step may be carried out at any timing during the winding step after the plating step, during roll storage after winding, and during roll unfolding before the hot stamping step.

[0060] The above steps produce an aluminized steel sheet 1. In the aluminized steel sheet 1, the thickness d of the oxide layer 30 is 10 to 400 nm, and the ratio of the thickness d1 of the hydroxide layer 31 to the thickness d of the oxide layer 30 is 30% or less. This makes it possible to obtain a highly reliable aluminized steel sheet that can suppress hydrogen embrittlement that progresses due to hydrogen that enters the steel material in association with the oxidation of the aluminization during hot stamping.

[0061] The Al-plated steel sheet 1 can be suitably used as a steel sheet for hot stamping. The hot stamping process performed on the Al-plated steel sheet 1 is not particularly limited, but an example is as follows. The Al-plated steel sheet 1 is heated after being shaped to a predetermined size. The heating method may be either a high-temperature furnace or electric heating. The holding temperature is preferably 850 to 950°C, and the holding time is preferably 2 minutes or more. After heating, the sheet is shaped in a die and simultaneously cooled in the die.

[0062] [Method of manufacturing hot stamped compact] A method for producing a hot stamped steel according to one embodiment of the present invention includes a step of hot stamping an Al-plated steel sheet 1. The Al-plated steel sheet 1 can suppress hydrogen embrittlement that progresses due to hydrogen that enters the steel material accompanying oxidation of the Al plating during hot stamping. Therefore, according to the method for producing a hot stamped steel according to this embodiment, a hot stamped steel in which hydrogen embrittlement is suppressed can be obtained. EXAMPLES

[0063] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0064] Steel sheets having the chemical compositions shown in Table 1 were coated with aluminum layers on both sides by hot-dip galvanizing.

[0065] [Table 1]

[0066] The chemical composition of the plating bath was Al-10% by mass Si-2% by mass Fe. The Fe in the plating bath was inevitably supplied from the plating equipment and the steel sheet. The temperature of the plating bath during hot-dip plating was 700°C. After immersing the steel sheet in the plating bath, the coating weight was reduced to 70 g / m per side by gas wiping. 2 was adjusted to.

[0067] Thereafter, a pre-oxidation step was carried out under the conditions shown in Table 2 below to prepare aluminized steel sheets. A plurality of aluminized steel sheets were produced by carrying out the pre-oxidation step under the same conditions, and some of them were subjected to surface analysis by XPS.

[0068] [Surface analysis by XPS] XPS measurements were performed using a PHI Quantera SXM manufactured by ULVAC-PHI, Inc. The X-ray source used was monochromatic Al Kα radiation (1486.6 eV), and the X-ray irradiation area was set to a diameter of approximately 100 μm.

[0069] Short sputtering and XPS measurements were repeated to obtain depth profiles of the integrated intensity of oxides and hydroxides. + The ion sputtering was performed at an acceleration voltage of 4 kV in a sputtering area of ​​1 mm x 1 mm. The sputtering rate was 75.1 nm / min in terms of SiO2.

[0070] From the depth profile of the integrated intensity of the oxide and hydroxide, the thickness d of the oxide layer 30 and the thickness d1 of the hydroxide layer 31 were determined by the method described above.

[0071] [Hot stamping process and hydrogen analysis] The aluminized steel sheet after the preliminary oxidation step was heated in an electric resistance furnace at a furnace temperature of 900° C. for a soaking time of 5 minutes, then formed in a die and cooled in the die at the same time to obtain a hot stamped body.

[0072] The hot stamped compact was stored in liquid nitrogen and subjected to thermal desorption analysis to quantify the amount of hydrogen. The integrated hydrogen amount up to 250°C was calculated. Note that a hydrogen amount exceeding 0.7 ppm by mass is considered unsuitable for 1.5 GPa class steel, and a hydrogen amount exceeding 0.5 ppm by mass is considered unsuitable for 1.8 GPa class steel.

[0073] Table 2 shows the conditions of the preliminary oxidation step, the results of the surface analysis by XPS, and the results of the hydrogen analysis.

[0074] [Table 2]

[0075] As shown in Table 2, the aluminized steel sheets A01 to A11 had oxide layer thicknesses d in the range of 10 to 400 nm, and the ratio of hydroxide layer thickness d1 to oxide layer thickness d was 30% or less. The hydrogen amounts of the hot stamped products produced from these aluminized steel sheets were all 0.2 ppm by mass or less.

[0076] In contrast, the hydrogen amounts of the hot stamped products produced from the aluminized steel sheets designated by symbols a1 to a8 were all 0.5 ppm by mass or more.

[0077] The Al-plated steel sheet with reference symbol a1 is an example in which the preliminary oxidation step was not performed. In the Al-plated steel sheet with reference symbol a1, the thickness d of the oxide layer was less than 10 nm, and the ratio of the thickness d1 of the hydroxide layer to the thickness d of the oxide layer was higher than 30%.

[0078] In the aluminized steel sheets having the symbols a2, a4, and a6, the oxide layer thickness d was within the range of 10 to 400 nm, but the ratio of the hydroxide layer thickness d1 to the oxide layer thickness d was higher than 30%.

[0079] In the Al-plated steel sheet of substitute code a3, the ratio of the hydroxide layer thickness d1 to the oxide layer thickness d was 30% or less, but the oxide layer thickness d was greater than 400 nm. In the Al-plated steel sheets of substitute codes a5 and a7, the ratio of the hydroxide layer thickness d1 to the oxide layer thickness d was 30% or less, but the oxide layer thickness d was smaller than 10 nm. In the Al-plated steel sheet of substitute code a8, the ratio of the hydroxide layer thickness d1 to the oxide layer thickness d was higher than 30%, and the oxide layer thickness d was also smaller than 10 nm.

[0080] Although the embodiment of the present invention has been described above, the above-mentioned embodiment is merely an example for carrying out the present invention. Therefore, the present invention is not limited to the above-mentioned embodiment, and the above-mentioned embodiment can be appropriately modified and carried out without departing from the spirit of the present invention. [Explanation of symbols]

[0081] 1. Aluminum-plated steel sheet 10 Steel base material 20 Al plating layer 30 Oxide layer 31 Hydroxide layer 32 Oxide layer

Claims

1. An Al-plated steel sheet for hot stamping, A steel substrate; an Al plating layer that is a plating layer containing Al and Si formed on the steel base material; and an oxide layer formed on the Al plating layer, The chemical composition of the steel substrate is, in mass%, C: 0.1 to 0.6%, Si: 0.01-1.50%, Mn: 0.10-3.00%, P: 0.05% or less, S: 0.020% or less, Al: 0.10% or less, Ti: 0.01 to 0.10%, B: 0.0001 to 0.0100%, N: 0.015% or less, Cr: 0-1.0%, Mo: 0-1.0%, Ni: 0-1.0%, Cu: 0 to 1.0%, Nb: 0 to 1.0%, The balance is Fe and impurities. The thickness of the oxide layer is 10 to 400 nm; The aluminum-plated steel sheet, wherein the oxide layer includes a hydroxide layer, and a ratio of a thickness of the hydroxide layer to a thickness of the oxide layer is 30% or less. Here, the thickness of the oxide layer is defined as the depth from the surface at which the integrated intensity of the oxide becomes half of its maximum value in a depth profiling analysis by X-ray photoelectron spectroscopy, and the thickness of the hydroxide layer is defined as the depth from the surface at which the integrated intensity of the hydroxide becomes half of its maximum value in a depth profiling analysis by X-ray photoelectron spectroscopy.

2. A method for producing an Al-plated steel sheet according to claim 1, A method for producing an Al-plated steel sheet, comprising a pre-oxidation step of heating an Al-plated steel sheet to a temperature of 120 to 600°C.

3. A method for producing a hot stamped product, comprising a step of hot stamping the Al-plated steel sheet according to claim 1.

Citation Information

Patent Citations

  • Production of aluminum alloy coated heat resistant material

    JP1994272017A

  • High strength aluminum based plated steel sheet having excellent workability and corrosion resistance in worked part and high strength automotive parts

    JP2003193187A

  • Steel structure for hydrogen

    JP2016065312A

  • Plated sheet steel, and production method of painted plated sheet steel

    JP2018162508A

  • Steel sheet for hot press-formed components with excellent resistance to delayed hydrogen fracture and manufacturing method thereof

    JP2022031677A