Gypsum-based investment composition for casting and method for producing the same

The gypsum-based casting investment material composition with fine particles and low-water content moisturizing agents addresses cracking issues in rapid heating type materials, enabling efficient production with reduced standing times and improved thermal shock resistance.

JP7594267B2Active Publication Date: 2024-12-04YOSHINO GYPSUM CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2019546707
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2017-10-05
Filing Date
2018-10-01
Publication Date
2024-12-04
Estimated Expiration
2038-10-01

AI Technical Summary

Technical Problem

Rapid heating type gypsum-based investment materials used in dental applications are prone to cracking due to thermal shock when placed in high-temperature incinerators, which affects work efficiency and product quality.

Method used

A gypsum-based casting investment material composition with calcined gypsum, quartz, and cristobalite, incorporating a pulverized product with a particle size of 30 μm or less and a low-water content moisturizing component, such as glycerin, to reduce the standing time before high-temperature processing.

Benefits of technology

The composition effectively suppresses cracking from thermal shock while maintaining fluidity, allowing for a shorter standing time of 8 to 15 minutes, thus enhancing work efficiency and product quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007594267000004
    Figure 0007594267000004
  • Figure 0007594267000001
    Figure 0007594267000001
  • Figure 0007594267000002
    Figure 0007594267000002
Patent Text Reader

Abstract

To provide a gypsum-based investment material composition for casting, which is useful as a rapid heating type gypsum-based investment material and enables the provision of a product with a shortened leaving time, which has not been realized with conventional products, and a method for producing the same. The present invention provides a gypsum-based powdered casting investment composition for use as a rapid-heating investment in which a kneading liquid is added, the mixture is kneaded, and then hardened, and the hardened product is then placed in a high-temperature furnace. The gypsum-based casting investment composition has an average particle size of 30 μm or less and is mainly composed of calcined gypsum, quartz, and cristobalite. The composition contains at least one co-ground product selected from the group consisting of a co-ground product of calcined gypsum and quartz, a co-ground product of calcined gypsum and cristobalite, and a co-ground product of calcined gypsum, quartz, and cristobalite, and a powder or liquid moisturizing component with a low moisture content. The present invention also provides a method for producing the same.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a gypsum-based investment material composition for rapid heating type investment material and a method for producing the gypsum-based investment material composition for rapid heating type investment material. More specifically, the present invention relates to a technology for providing a gypsum-based investment material composition for rapid heating type investment material, which is useful as a dental investment material, and which contributes to improving work efficiency and can shorten the time required for making a slurry by adding a mixing liquid, embedding a wax pattern or a resin pattern as a core in the slurry, hardening the slurry, and then putting the hardened body into a high-temperature furnace, compared to conventional investment material compositions, and a method for producing the same. [Background technology]

[0002] The casting investment composition is a mold material used for casting when producing a prosthesis such as a silver tooth through the following steps, taking a dental investment material as an example. First, a mold prototype (hereinafter referred to as a pattern) for the prosthesis is made from wax, resin, etc. On the other hand, a kneading liquid is added to a powdered dental investment material and kneaded to prepare a slurry with high fluidity. The pattern obtained above is used as a core and embedded in the prepared slurry, and the pattern is left embedded. After a certain period of time, the slurry hardens to become a hardened body in which the pattern is embedded as a core. Then, the obtained hardened body is heated under appropriate conditions. In this heating step (burning step), only the pattern of the core is burned and disappears, and the part becomes a cavity, and a mold is obtained in which a hollow part having the shape of a prosthesis such as a silver tooth is formed inside. Then, a molten metal is cast into the cavity part of the mold to form a metal prosthesis such as a silver tooth having a desired shape.

[0003] Dental investment materials are classified into gypsum-based investment materials and phosphate-based investment materials according to the type of binder, and gypsum-based investment materials are widely used as casting molds (gypsum molds) when casting metals with a melting point of 1000°C or less. Gypsum-based investment materials use cristobalite or quartz as the refractory material and gypsum as the binder, and generally use water as the mixing liquid. Below, a case where water is used as the mixing liquid will be explained as a representative example, and the mixing liquid in that case is called mixing water. Gypsum-based investment materials are also classified into normal heating type and rapid heating type according to the heating conditions in the above-mentioned incineration process. In the normal heating type, the temperature is gradually increased from room temperature to incinerate the buried core pattern, while in the rapid heating type, the hardened body is put into an incinerator that has been heated to a high temperature of 700°C or 750°C to incinerate the pattern. This makes it possible to achieve higher workability than that of the normal heating type.

[0004] In particular, in the case of dental investment materials, the cavity of the resulting mold (plaster mold) is required to have high dimensional stability and surface smoothness due to the intended use. For this reason, various proposals have been made from the viewpoint of obtaining a mold that satisfies the above-mentioned characteristics for such applications (for example, see Patent Document 1). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2002-87918 A Summary of the Invention [Problem to be solved by the invention]

[0006] In the above situation, the present inventors have conducted intensive research into rapid heating gypsum-based investment materials, which are widely used as dental investment materials, from the viewpoint of further improving work efficiency. Rapid heating gypsum-based investment materials, which are highly workable, have a problem in that the hardened body is easily cracked in the mold because it is put into an incinerator heated to a high temperature. If a crack occurs in the mold (gypsum mold), burrs or the like will occur in the resulting casting such as a prosthesis, and in some cases, it may be necessary to start over from the preparation of the pattern. As described below, it is known that the problem of cracks occurring in the mold is related to the hardened state of the hardened body when it is put into an incinerator.

[0007] In general, the rapid heating type gypsum-based investment material is required to be kneaded with mixing water to make a slurry, and after a series of operations, the slurry must be left to harden until it can withstand the thermal shock when it is put into a high-temperature incinerator. It is known that the occurrence of cracks in the above-mentioned casting mold (gypsum mold) is related to the hardening state of the slurry when it is put into a high-temperature incinerator, that is, the time left to promote the above-mentioned hardening (called the "left-standing time"). Specifically, the shorter the left-standing time, the more the work efficiency can be improved, but if the hardened body is put into an incinerator heated to a high temperature without being left-standing for a sufficient time, cracks will occur in the casting mold, causing casting defects.

[0008] For the above reasons, dental investment products, which are rapid heating gypsum-based investment materials, are designed for this purpose before being sold on the market, and the required leaving time for each product is determined. Specifically, in the case of gypsum-based dental investment products, the leaving time is determined, which means that the product is one in which the hardened body can be put into a high-temperature incinerator 20 minutes or 30 minutes after starting the measurement from the time when mixing with the mixing water begins (the time when the dental investment material comes into contact with the mixing water). For this reason, when using a 20-minute type gypsum-based dental investment material, for example, the worker needs to start the measurement from the time when the material comes into contact with the mixing water and then put the hardened body into the incinerator, which has been heated to a high temperature, at least 20 minutes after the measurement. In other words, the worker needs to stop working for a while after mixing and embedding the core in the slurry. In the present invention, the time measured from the time when the mixing water is added until the hardened body becomes in a state where rapid heating can be started is defined as the "leaving time".

[0009] In view of the above-mentioned current situation, the inventors have come to realize that if a product could be provided that shortened the above-mentioned exposure time, work could be completed in a shorter time than with conventional products, and that if a variety of such products were available, it would broaden the range in which products with different exposure times could be appropriately selected and designed to suit the desired work conditions, which would be useful in improving work efficiency.

[0010] Therefore, the object of the present invention is to provide a gypsum-based investment material composition for casting that is useful as a rapid heating type gypsum-based investment material and that can provide a product with a shorter standing time than conventional products, which has not been realized with conventional products. Another object of the present invention is to provide a technology that can provide a product with a suitably designed standing time in a gypsum-based investment material composition for casting. [Means for solving the problem]

[0011] The above object can be achieved by the present invention, which provides the following gypsum-based investment material composition for casting. [1] A gypsum-based powdered casting investment material composition for use as a rapid heating type investment material in which a mixing liquid is added, the mixture is mixed, and then hardened, and the hardened body is placed in a high-temperature furnace. The gypsum-based casting investment material composition has an average particle size of 30 μm or less and is mainly composed of calcined gypsum, quartz, and cristobalite, and contains at least one co-ground product selected from a co-ground product of calcined gypsum and quartz, a co-ground product of calcined gypsum and cristobalite, or a co-ground product of calcined gypsum, quartz, and cristobalite, and a powder or liquid moisturizing component with a low moisture content.

[0012] Preferred embodiments of the gypsum-based casting investment composition of the present invention include the following: [2] The moisture-retaining component contains a component selected from polyhydric alcohols; [3] The polyhydric alcohol of [2] is at least one selected from the group consisting of glycerin, propylene glycol, ethylene glycol, 1,3-butylene glycol, and polymers or copolymers thereof; [4] The glycerin in [3] above has a purity of 98.5% or more; [5] In any one of [1] to [4] above, the time from when the mixing liquid is poured until the hardened body is in a state in which rapid heating can be started is 8 to 15 minutes; [6] The time period for leaving the mixture in [5] above is 8 to 10 minutes; [7] The standing time of [5] above is 8 minutes; [8] In any one of the items [1] to [7], the moisturizing component is contained in an amount of 0.05 to 1.0 part by mass per 100 parts by mass of the main component; [9] In any of the above items [1] to [8], the product is for dental use;

[10] In any one of [1] to [9] above, further containing gypsum dihydrate;

[11] The gypsum of

[10] is contained as the co-ground product;

[12] In any one of [1] to

[11] above, the setting expansion rate 2 hours after the mixing liquid is added is 0.2% or more and 3.0% or less;

[13] In any one of the above [1] to

[12] , the total expansion coefficient is 1.3% or more and 3.0% or less.

[0013] As another embodiment, the present invention provides the following method for producing a gypsum-based casting investment material composition.

[14] A method for producing a rapid heating type gypsum-based casting investment material composition, which is used by adding a kneading liquid, kneading, and hardening the resulting hardened body, and then putting it into a high-temperature furnace, wherein when mixing the main components, calcined gypsum, quartz, and cristobalite, at least one co-ground product selected from the group consisting of a co-ground product of calcined gypsum and quartz, a co-ground product of calcined gypsum and cristobalite, and a co-ground product of calcined gypsum, quartz, and cristobalite is used, and further, a powder or liquid moisturizing component with a low moisture content is mixed to prepare a powdered gypsum-based casting investment material composition having an average particle size of 30 μm or less.

[0014] A preferred embodiment of the method for producing the gypsum-based casting investment composition of the present invention is as follows.

[15] The method for producing a gypsum-based casting investment material composition according to

[14] , wherein the moisturizing component is mixed in an amount of 0.05 to 1.0 part by mass per 100 parts by mass of the main component.

[16] The method for producing a gypsum-based investment composition for casting according to

[14] or

[15] , further comprising blending gypsum dihydrate.

[17] The method for producing a gypsum-based investment composition for casting according to

[14] or

[15] , wherein each of the co-ground substances used in mixing the main components, calcined gypsum, quartz and cristobalite, is a co-ground substance further containing gypsum dihydrate and co-ground. Effect of the Invention

[0015] According to the present invention, it is possible to provide a useful gypsum-based investment material composition for casting, which can shorten the standing time, which could not be realized with conventional rapid heating type gypsum-based investment material products, and can obtain a good casting mold (gypsum mold) in which the occurrence of cracks due to heat shock is suppressed even if the standing time is shortened. Also, according to the present invention, a technology is provided that can appropriately design the standing time for the gypsum-based investment material composition for casting. [Brief description of the drawings]

[0016] [Figure 1] FIG. 1 is a schematic diagram of a T-shaped wax pattern used in the study example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] The present invention will be described in more detail below with reference to preferred embodiments. The present inventors have conducted intensive research to solve the problems of the prior art described above, and have found that a rapid heating type gypsum-based investment material has an extremely simple structure, yet can shorten the standing time compared to conventional products, and that the mold obtained by putting it into a high-temperature incinerator is a good one in which the occurrence of cracks due to heat shock is suppressed. For example, in a conventional commercially available rapid heating type dental investment material product, the standing time from the time when the dental investment material is poured with kneading water and brought into contact with the water to the time when the hardened body in which the pattern is embedded as a core is put into a high-temperature incinerator after a series of operations is 20 minutes or 30 minutes, and these times are required at the shortest. In contrast, by using the gypsum-based casting investment material composition of the present invention (hereinafter simply referred to as the "composition of the present invention"), even if the standing time is shortened to about 8 to 15 minutes, about 8 to 10 minutes, or even if it is shortened to about 8 minutes, a good mold in which the occurrence of cracks due to heat shock is suppressed can be obtained.

[0018] The composition of the present invention is composed of a binder containing calcined gypsum as the main component, and quartz and cristobalite as the refractory material, similar to the conventional gypsum-based investment composition. The composition of the present invention further contains these components as at least one of a dry co-ground product of calcined gypsum and quartz, a dry co-ground product of calcined gypsum and cristobalite, or a dry co-ground product of calcined gypsum, quartz, and cristobalite, and is configured so that the average particle size of the composition is 30 μm or less. In addition to this main component configuration, the composition is characterized by containing a powder or liquid moisture-retaining component with a low moisture content. The present inventors have surprisingly found that by using the above-mentioned co-ground product in the main component configuration and containing the moisture-retaining component, the "standing time" can be shortened without impairing the performance such as fluidity in the conventional product, and the mold (gypsum mold) formed in a short time has excellent thermal shock resistance with suppressed crack generation.

[0019] Specifically, the composition of the present invention is mixed with water to form a slurry, a pattern is embedded with the slurry, and the time for hardening is shortened compared to conventional products. Even when the mold is placed in a high-temperature incinerator at 700°C or 750°C, the mold formed is found to be one in which the occurrence of cracks caused by heat shock is effectively suppressed. Furthermore, the present inventors have found, as a result of their investigations, a surprising fact that the main component containing calcined gypsum is composed of a co-ground product, and the gypsum-based casting investment material composition is made into a powder having an average particle size of 30 μm or less, which contributes to the realization of the effect of shortening the above-mentioned standing time without impairing the quality obtained by conventional products. This point will be described later with examples.

[0020] In the present invention, the reason why the standing time can be shortened by using a co-ground product obtained by co-grounding at least calcined gypsum with other main components in a main component containing calcined gypsum and other main components in a dry manner and by making the average particle size 30 μm or less is unclear. The average particle size specified in the present invention is a volume average diameter measured by a laser diffraction / scattering method. According to the inventors' study, one of the factors that obtained the above-mentioned effect is that the particle size of calcined gypsum can be made fine by the above-mentioned composition. On the other hand, it was found that if the particle size of calcined gypsum is only made fine, another problem occurs in that the flow value decreases and the fluidity during mixing is poor. In response to this problem, the inventors found that it can be improved by co-grounding calcined gypsum with other main components. For this reason, in the present invention, a co-ground product of a main component containing calcined gypsum is used and the average particle size is made 30 μm or less, thereby achieving both the effect of shortening the standing time and the effect of suppressing the problem of the decrease in the flow value caused by making the particle size of calcined gypsum fine.

[0021] The composition of the present invention, which forms a mold (plaster mold) that is effectively inhibited from cracking due to heat shock, was used to measure the setting expansion rate two hours after the mixing liquid (mixing water) was added and the overall expansion rate described below, and an investigation was conducted to determine at what values ​​these values ​​would provide good results. As a result, it was confirmed that good results could be obtained when the setting expansion rate two hours after the mixing water was added was 0.2% or more and 3.0% or less, and when the overall expansion rate was 1.3% or more and 3.0% or less.

[0022] The setting expansion rate after 2 hours from the time of putting the mixing water in was measured by putting the gypsum-based casting investment material composition to be measured in 15 seconds into a silicone rubber cup containing the mixing water, stirring for 1 minute, and pouring it into a mold for measuring the setting expansion rate, and using this as a test specimen, measuring it as follows. That is, the size of the composition mixed with the mixing water immediately after pouring it into the mold was used as the standard, specifically, the gauge installed in the mold at this point was set to zero, and the value of the gauge after 2 hours was read, and the setting expansion rate after 2 hours from the time of putting the mixing water into the cup was measured.

[0023] The total expansion coefficient used in the present invention is the sum of the "setting expansion coefficient after the elapse of the standing time" and the "thermal expansion coefficient" measured as follows. First, the gypsum-based casting investment material composition to be measured was poured into a silicone rubber rubber cup containing mixing water for 15 seconds, and after stirring for 1 minute, it was poured into a mold for measuring the setting expansion coefficient and a mold for measuring the thermal expansion coefficient, and each was used as a test specimen and measured as follows.

[0024] The "setting expansion coefficient after the elapse of the standing time" is based on the size of the composition mixed with the mixing water immediately after it is poured into a mold for measuring the setting expansion coefficient, and specifically, the gauge in the mold is set to zero at this point, and the gauge value at the time of the standing time to be confirmed is read and measured. The "thermal expansion coefficient" is measured by taking a sample after the standing time has elapsed and heating it as described below. Specifically, the test piece (sample) taken out above is set in a thermal dilatometer (manufactured by Bruker, product name: TD5000SA), and the temperature is raised from room temperature at a rate of 10°C per minute, and the thermal expansion coefficient when it reaches 700°C is measured. The thermal expansion coefficient is measured based on the sample size after the standing time used for heating, and the amount of expansion relative to this standard is measured.

[0025] [Powder or liquid moisturizing ingredient with low water content] The composition of the present invention has the above-mentioned basic constitution and is characterized by containing a moisturizing component in the form of powder or liquid having a low water content.

[0026] In order to solve the problems of the conventional technology described above, the present inventors conducted intensive research to find a useful component that, when contained in a gypsum-based casting investment material composition, uses a component other than the main component described above and can suppress the occurrence of cracks due to heat shock in the mold formed even if the standing time is shortened. In the course of the research, the present inventors found that when glycerin with a purity of 98.5% or more and a low water content is contained, the mold formed can suppress the occurrence of cracks caused by heat shock even if the standing time is shortened.

[0027] As a result of further investigation, it was found that the same effect can be obtained by adding not only glycerin having a purity of 98.5% or more, but also a powder or liquid moisturizing ingredient having a low water content.

[0028] The powder or liquid moisturizing component with a low water content constituting the composition of the present invention includes polyhydric alcohols, such as the above-mentioned glycerin having a purity of 98.5% or more (called refined glycerin), other glycerins, propylene glycol, ethylene glycol, 1,3-butylene glycol, and polymers or copolymers thereof.

[0029] According to the study by the present inventors, the amount of the moisturizing component is preferably within the range of 0.05 to 1.0 parts by mass relative to 100 parts by mass of the main component. More preferably, it is contained within the range of 0.1 to 1.0 parts by mass, and even more preferably 0.2 to 1.0 parts by mass, depending on the balance with the intended effect of shortening the standing time. If it is less than the above range, even if the standing time can be shortened, the effect of suppressing the occurrence of cracks in the mold formed by rapid heating may not be fully exhibited. In addition, if it is more than the above range, it is not preferable because it becomes sticky when mixed with the main component by co-grinding, etc. Hereinafter, glycerin having a purity of 98.5% or more will be used as a representative example of the moisturizing component, but the present invention is not limited thereto.

[0030] In addition, although the present invention has been described with a focus on dental investment materials, the scope of use of the composition of the present invention is not limited thereto, and the composition can be used without distinction in the case of efficiently and with a high yield casting of jewelry, arts and crafts, metal parts, and the like, which require precise shapes without burrs.

[0031] Next, the main components constituting the composition of the present invention will be described. [Main component] The main components constituting the composition of the present invention are calcined gypsum, quartz and cristobalite, similar to conventional gypsum-based investment compositions, and the blending ratio of each may be about 1 / 3, similar to conventional compositions. More specifically, for example, when the total amount of the main components is 100 parts by mass, the calcined gypsum may be about 25 to 50 parts by mass, the cristobalite may be about 10 to 35 parts by mass, and the quartz may be about 40 to 65 parts by mass.

[0032] (plaster of Paris) The calcined gypsum constituting the composition of the present invention is calcium sulfate 1 / 2 hydrate [CaSO4·1 / 2H2O] and anhydrate [CaSO4], and examples thereof include β-type hemihydrate gypsum, α-type hemihydrate gypsum, III-type anhydrous gypsum, and mixtures thereof. Any type of calcined gypsum can be used in the present invention. According to the study by the inventors, in consideration of the strength of the mold required for casting, it is more preferable to use α-type hemihydrate gypsum (α-gypsum). Calcined gypsum is used as a binder because it chemically reacts with water and easily changes to gypsum dihydrate.

[0033] The slurry obtained by adding an appropriate amount of water to the composition of the present invention and kneading it is quickly solidified when poured into a mold with a pattern as a core. The composition of the present invention has a configuration in which the state of the hardened body formed by the solidification of the calcined gypsum is excellent in thermal shock resistance, making the mold (plaster mold) less susceptible to heat shock, in a shorter standing time than that of conventional products. As a result, the mold formed by burning off the core pattern in a high-temperature incinerator after the hardened body that has been left for a shorter standing time has effectively suppressed the occurrence of cracks, and the castings such as prosthetics obtained using the mold are good and free of burrs.

[0034] As described above, the composition of the present invention uses calcined gypsum as a binder, and therefore has excellent fluidity when the slurry is poured into the composition. The resulting mold (gypsum mold) has the advantages of being less prone to deformation due to residual stress after burning, allowing the casting to be easily removed after casting, and being less susceptible to change over time.

[0035] (Quartz, Cristobalite) The composition of the present invention contains quartz and cristobalite as refractory materials, and in this respect, is not different from the prior art. Therefore, these materials can be any of the known materials used in the conventional "gypsum-based investment materials."

[0036] As mentioned above, the composition of the present invention is characterized in that the calcined gypsum, quartz, and cristobalite are used as main components in a state in which the calcined gypsum and other main components are co-ground. By configuring in this way, when the composition of the present invention is placed in a high-temperature incinerator after shortening the standing time compared to the conventional product, the mold (gypsum mold) formed has excellent thermal shock resistance and is less susceptible to heat shock. In addition, as described later, by using such a co-ground product, the problem of a decrease in flow value, i.e., a decrease in the fluidity of the slurry, observed in a composition composed of only pulverized calcined gypsum can be suppressed.

[0037] (gypsum dihydrate) The composition of the present invention can be added with gypsum dihydrate. This can increase the setting expansion coefficient and thermal expansion coefficient of the composition of the present invention. The method of adding gypsum dihydrate to the composition of the present invention is not particularly limited. For example, the composition may be configured to add gypsum dihydrate when co-grinding the main component, co-grind with the main component, and add as a co-grind product, or to add gypsum dihydrate to the main component after co-grinding. However, gypsum dihydrate is not an essential component of the composition of the present invention, but is an optional component.

[0038] [Method for producing gypsum-based investment composition for casting] Next, the manufacturing method of the gypsum-based casting investment material composition of the present invention, which can obtain the composition of the present invention, will be described. The manufacturing method of the present invention is characterized in that when blending the main components of the composition, calcined gypsum, quartz and cristobalite, at least one co-ground product selected from the group consisting of a co-ground product of calcined gypsum and quartz, a co-ground product of calcined gypsum and cristobalite, and a co-ground product of calcined gypsum, quartz and cristobalite is used, and further, a powder or liquid moisture-retaining component with a low moisture content is blended to prepare a powdered gypsum-based casting investment material composition having an average particle size of 30 μm or less. That is, the manufacturing method of the present invention is characterized in that a co-ground product containing at least calcined gypsum is used as the main component raw material, a powder or liquid moisture-retaining component with a low moisture content is blended, and the average particle size is 30 μm or less, and otherwise it is the same as the manufacturing method of the conventional gypsum-based powdered casting investment material composition. EXAMPLES

[0039] The present invention will now be described in more detail with reference to the following examples. In the following, parts and percentages are by weight unless otherwise specified.

[0040] [Study Example 1] (Addition of glycerin) (Preparation of gypsum-based investment composition for casting) As the main component, a co-ground product with an average particle size of 15 μm was used, which was composed of 30 parts of α-gypsum, 20 parts of cristobalite, and 50 parts of quartz powder. When these components were co-ground in a dry manner, purified glycerin (manufactured by Kao Corporation) with a purity of 98.5% or more was added to each of the concentrations of 0.05 parts, 0.1 parts, 0.2 parts, 0.5 parts, 1.0 parts, and 1.2 parts per 100 parts of the main component in terms of active ingredient, to obtain six types of gypsum-based investment material compositions for casting with different amounts of glycerin. The conditions for co-grounding in a dry manner were the same.

[0041] (evaluation) The compositions obtained above, each containing different amounts of glycerin, were used, and the following series of procedures were carried out. The hardened bodies were left for three different periods of time, and then placed in a high-temperature incinerator to form molds (plaster molds). The thermal shock resistance of the molds obtained was compared using the following method.

[0042] Several stainless steel casting rings with an inner diameter of 40 mm and a height of 50 mm were prepared in advance by wrapping a single layer of ceramic liner (Yoshino Gypsum Sales Co., Ltd., product name: YS Liner 48) around the inner wall surface, and then inserting a T-shaped wax pattern as shown in Figure 1 into the liner. In Figure 1, A indicates the diameter of the cylindrical part that will become the mold, and B indicates the diameter of the cylinder that will become the introduction path for introducing molten metal into the mold. A is 6 mm, and B is 2.5 mm.

[0043] Water was added to 100 parts of the previously prepared gypsum-based casting investment material composition and mixed to obtain slurries with different amounts of glycerin. For comparison, a composition consisting of only the co-ground product of the main component that does not contain glycerin was used to obtain a slurry under the same conditions as described above. Next, the obtained slurry was poured into a casting ring prepared in advance, and the T-shaped wax pattern of the above shape was embedded inside. At this time, six test specimens each consisting of a composition with the same composition were obtained.

[0044] Then, the curing time of the slurry before being put into the high-temperature incinerator was changed so that the left-standing time was 8 minutes, 10 minutes, and 15 minutes, and then the hardened body was rapidly heated to obtain a gypsum mold (casting mold). Then, each of the obtained gypsum molds was used to produce a casting. The state of these gypsum molds and castings was observed to investigate the influence on thermal shock resistance of using each gypsum-based casting investment material composition with different blending amounts of glycerin. Specifically, first, two test pieces each, which had been cured under different conditions of left-standing time, were put into an electric furnace (incinerator) previously set at 700°C, at 8 minutes, 10 minutes, and 15 minutes after the mixing water was added to the composition to obtain the slurry. Then, after 30 minutes, one of the test pieces was taken out of the furnace, and the presence or absence of cracks in the taken-out gypsum mold was visually observed. The other plaster mold was used as it was for casting using a gold-silver-palladium alloy (gold 12%) (GC Corporation, product name: Castwell), and the surface condition of the resulting casting was visually observed.

[0045] From the results of the visual observation, the thermal shock resistance of the gypsum molds (casting molds) obtained from each gypsum-based casting investment composition with different blending amounts of glycerin and the castings cast with the gypsum molds was evaluated according to the following three-level criteria. The results are summarized in Table 1. ○: No cracks in the plaster mold △: Cracks are observed on the surface of the plaster mold (not reaching the inside), but there is no effect on the casting. ×: There was a crack in the plaster mold that reached the hollow inside, causing a casting defect in the casting.

[0046] TIFF0007594267000001.tif44170

[0047] From the results of Table 1, it was confirmed that by adding glycerin to the composition of the investment material for gypsum-based casting, even if the time (standing time) from contact with water to being put into a high-temperature incinerator is shortened, the casting mold (gypsum mold) obtained using the composition has excellent thermal shock resistance in which the occurrence of cracks due to heat shock is suppressed. In addition, when 1.2 parts of glycerin were added to the composition of the investment material for gypsum-based casting, the powder material became sticky, so it was found that the amount of glycerin to be added to the composition is preferably in the range of 0.05 parts to 1.0 parts. In addition, a T-shaped resin pattern was used instead of the T-shaped wax pattern used in the above study, and the same test as above was performed, and the same results as above were obtained.

[0048] [Study Example 2] (Gypsum particle size) From the results of the study example 1, the amount of glycerin to be mixed in the gypsum-based casting investment material composition was set to 0.2 parts, and the main components were mixed in the same manner as in the study example 1, with 30 parts of α-gypsum, 20 parts of cristobalite, and 50 parts of quartz powder. In the study example 2, unlike the case of the study example 1, these main components were not co-ground, but were stirred and mixed to obtain the gypsum-based casting investment material composition for study. As the α-gypsum used for stirring and mixing, commercially available 40 μm α-gypsum (manufactured by Yoshino Gypsum Co., Ltd.) was ground to obtain particles with average particle sizes of 25 μm, 30 μm, and 35 μm, respectively, and these were used. For the cristobalite, commercially available 20 μm powder was used, and for the quartz, commercially available 20 μm powder was used. Then, four types of compositions for study were obtained that had the same composition except for the average particle size of the α-gypsum. The average particle size of the α-gypsum was measured by a laser diffraction and scattering method (volume average diameter).

[0049] The influence of the four types of gypsum-based investment material compositions for casting, which were obtained by stirring and mixing the above-mentioned α-gypsum and had different average particle sizes, on the thermal shock resistance of the mold (gypsum mold) was evaluated in the same manner as in Study Example 1, and the results are shown in Table 2. Furthermore, the flow value of the slurry obtained by adding mixing water was measured to examine its fluidity. The results are summarized in Table 2.

[0050] TIFF0007594267000002.tif50170

[0051] From the results shown in Table 2, it was confirmed that the finer particle size of the alpha gypsum used as a binder contributes to the suppression of the occurrence of cracks due to heat shock in the resulting mold (plaster mold) when the leaving time is shortened. However, it was confirmed that the flow value tends to decrease when the particle size of the alpha gypsum used for stirring and mixing is made finer, and it was found that when the alpha gypsum is made finer, another problem occurs in that the fluidity of the slurry decreases.

[0052] [Study Example 3] (Co-grinding of main components) From the results of Study Example 2, it was confirmed that the effect of suppressing the occurrence of cracks due to heat shock occurring in the formed casting mold (plaster mold) can be obtained by grinding α-gypsum to make the particle size fine. However, in this case, it was recognized that another problem occurs, that is, the fluidity of the slurry decreases. Therefore, as shown below, the effect of co-grinding α-gypsum with other main components instead of grinding it alone was studied. The main components were blended with 30 parts of α-gypsum, 20 parts of cristobalite, and 50 parts of quartz, and a gypsum-based casting investment material composition was obtained using three types of co-grinding products, namely, a co-grinding product of α-gypsum and quartz, a co-grinding product of α-gypsum and cristobalite, and a co-grinding product of α-gypsum, quartz, and cristobalite. At that time, the main components not contained in the co-grinding product were ground alone to have the same average particle size as the co-grinding product, and added to the co-grinding product to obtain compositions mainly composed of α-gypsum, cristobalite, and quartz. In addition, three types of gypsum-based casting investment compositions with different particle sizes were obtained by co-grinding the average particle sizes of the co-ground products to 25 μm, 30 μm, and 35 μm. In each case, glycerin was mixed in an amount of 0.2 parts in terms of pure content to 100 parts of the main component during co-grinding.

[0053] The gypsum-based casting investment material compositions obtained above, which were different in type and average particle size from the co-ground products, were used to examine the thermal shock resistance of the obtained gypsum molds (casting molds) in the same manner as in Study Example 1. The results are shown in Table 3. The average particle sizes in Table 3 are the measurement results for the obtained gypsum-based casting investment material compositions.

[0054] TIFF0007594267000003.tif62170

[0055] As mentioned above, in the study example 2 in which α-gypsum was pulverized alone, as shown in Table 2, the pulverization suppressed the occurrence of cracks due to heat shock in the formed casting mold (gypsum mold), but the flow value decreased, and another problem occurred that the fluidity of the slurry decreased. In contrast, as shown in Table 3, by co-pulverizing α-gypsum with other main components and making the average particle size of the obtained gypsum-based casting investment material composition 30 μm or less, it was confirmed that the effect of suppressing the occurrence of cracks due to heat shock in the casting mold (gypsum mold) and casting can be realized while ensuring sufficient fluidity during mixing without significantly decreasing the flow value.

[0056] The expansion coefficient of each sample of the gypsum-based casting investment material composition having an average particle size of 30 μm and 25 μm in Table 3 was measured as follows. The setting expansion coefficient was measured 2 hours after the mixing water was added using the method described above. In addition, for each sample, the setting expansion coefficient of the test piece (hardened body) after each leaving time and the thermal expansion coefficient when the test piece after each leaving time was heated to 700 ° C. were measured, and the total expansion coefficient, which is the sum of these values, was calculated. As a result, the setting expansion coefficient was within the range of 0.2% to 3.0%. It was also confirmed that the total expansion coefficient was within the range of 1.3% to 3.0%. [Explanation of symbols]

[0057] A: The diameter (6 mm) of the part that will serve as the mold for the T-shaped wax pattern. B: The diameter (2.5 mm) of the part that serves as the introduction path for the T-shaped wax pattern mold.

Claims

1. A gypsum-based powdered casting investment composition for rapid heating investment material in which a mixing liquid is added, the mixture is mixed, the mixture is hardened, and the hardened product is placed in a high-temperature furnace. The main components are calcined gypsum, quartz, and cristobalite, and the main components include at least one co-ground product selected from the group consisting of a co-ground product of calcined gypsum and quartz, a co-ground product of calcined gypsum and cristobalite, and a co-ground product of calcined gypsum, quartz, and cristobalite, A gypsum-based investment material composition for casting, which contains 0.05 parts by mass or more of polyhydric alcohols, which are powder or liquid moisturizing components with a low water content, relative to 100 parts by mass of the main component, and which contains the main component and the moisturizing component, is characterized in that the average particle diameter of the gypsum-based investment material composition for casting containing the main component and the moisturizing component is 30 μm or less.

2. The gypsum-based casting investment material composition according to claim 1, wherein the polyhydric alcohol is at least one selected from the group consisting of glycerin, propylene glycol, ethylene glycol, 1,3-butylene glycol, and polymers or copolymers thereof.

3. The gypsum-based casting investment material composition according to claim 2, wherein the glycerin has a purity of 98.5% or more.

4. The gypsum-based casting investment material composition according to any one of claims 1 to 3, wherein the time until the hardened body is in a state in which rapid heating can be started, measured from the time when the kneading liquid is poured, is 8 to 15 minutes.

5. The gypsum-based casting investment material composition according to claim 4, wherein the leaving time is 8 to 10 minutes.

6. The gypsum-based casting investment material composition according to claim 4, wherein the leaving time is 8 minutes.

7. The gypsum-based casting investment material composition according to any one of claims 1 to 6, comprising 0.05 to 1.0 parts by mass of the moisture-retaining component relative to 100 parts by mass of the main component.

8. The gypsum-based casting investment material composition according to any one of claims 1 to 7, which is for dental use.

9. The gypsum-based casting investment material composition according to any one of claims 1 to 8, further comprising gypsum dihydrate.

10. The gypsum-based casting investment material composition according to claim 9, wherein the gypsum dihydrate is contained as the co-ground product.

11. The gypsum-based casting investment material composition according to any one of claims 1 to 10, wherein the setting expansion coefficient 2 hours after the mixing liquid is added is 0.2% or more and 3.0% or less.

12. The gypsum-based casting investment material composition according to any one of claims 1 to 11, wherein the overall expansion coefficient is 1.3% or more and 3.0% or less.

13. A method for producing a rapid heating type gypsum-based casting investment material composition, in which a kneading liquid is added, kneaded, and then hardened to obtain a hardened body, which is then put into a high-temperature furnace for use, A method for producing a gypsum-based investment material composition for casting, comprising the steps of: mixing the main components, calcined gypsum, quartz, and cristobalite; using at least one co-ground product selected from the group consisting of a co-ground product of calcined gypsum and quartz, a co-ground product of calcined gypsum and cristobalite, and a co-ground product of calcined gypsum, quartz, and cristobalite; and further mixing 0.05 parts by mass or more of a polyhydric alcohol, which is a powder or a liquid moisturizing component having a low moisture content, relative to 100 parts by mass of the main components, to prepare a powdered gypsum-based investment material composition for casting having an average particle diameter of 30 μm or less, the powdered gypsum-based investment material composition for casting containing the main components and the moisturizing component.

14. The method for producing a gypsum-based casting investment material composition according to claim 13, wherein the polyhydric alcohol is at least one selected from the group consisting of glycerin, propylene glycol, ethylene glycol, 1,3-butylene glycol, and polymers or copolymers thereof.

15. The method for producing a gypsum-based casting investment material composition according to claim 13 or 14, wherein the moisturizing component is blended so that the moisturizing component is contained in an amount of 0.05 to 1.0 part by mass relative to 100 parts by mass of the main component.

16. The method for producing a gypsum-based casting investment material composition according to any one of claims 13 to 15, further comprising blending dihydrate gypsum.

17. The method for producing a gypsum-based casting investment material composition according to any one of claims 13 to 15, wherein each of the co-ground products used when blending the main components, calcined gypsum, quartz, and cristobalite, is a co-ground product further containing dihydrate gypsum and co-ground.

Citation Information

Patent Citations

  • Gypsum composition

    JP1978096027A

  • Gypsum type embedding material composition for dentistry

    JP1999076270A

  • Plaster bonding investment material for dental casting

    JP2001353166A

  • Dental implant material and method of preparation for dental template

    JP2002087918A

  • Dental gypsum-based embedding material powder

    WO2016043131A1