Iodine complexes and their production method and use

Iodine complexes with polymer carriers address solubility and durability issues, providing low elution rates and adjustable iodine content for radiological markers and polarizing films.

JP7594297B2Active Publication Date: 2024-12-04NOVASHIN CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021502960
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-04-02
Filing Date
2020-03-11
Publication Date
2024-12-04
Estimated Expiration
2040-03-11

AI Technical Summary

Technical Problem

Existing iodine complexes are easily soluble in water and alcohol, limiting their use, and compound carriers for iodine have limited binding capacity and poor durability in high temperature and humidity environments.

Method used

Forming iodine complexes by complexing iodine with a polymer carrier that has good biocompatibility, allowing adjustable iodine content and improved binding properties through structural units represented by formulas (I), (II), (III), and (IV), utilizing ligand bonds and van der Waals forces.

Benefits of technology

The iodine complexes exhibit low elution rates, enabling their use as radiological markers and polarizing films with adjustable iodine content and enhanced durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

The present invention provides an iodine complex, a method for producing the same, and uses thereof. The iodine complex is a complex of a structural unit represented by formula (I) with an iodine molecule or a polyiodine ion in which an iodine molecule and an iodine ion are bonded. Complexation with iodine as a carrier to obtain iodine complexes: [Formula 1] JPEG2022525708000031.jpg104169 The iodine complex can be used as a radiological marker, in iodine therapeutic agents, or in polarizing films, and the polymer has excellent biocompatibility. The iodine content in the iodine complex can be adjusted as needed, and the iodine content can be adjusted between 0.001 and 60%. The iodine content affects the transmission resolution of the radiological marker.
Need to check novelty before this filing date? Find Prior Art

Description

Detailed Description of the Invention

[0001] This application claims priority from a prior patent application, bearing application number 201910263342.5, filed with the State Intellectual Property Office of China on April 2, 2019, for the invention "Iodine complex and its preparation method and use," the entire text of which is incorporated herein by reference. [Technical field] The present invention relates to the technical field of iodine complexes, and in particular to an iodine complex and its preparation and use as a radiation marker, or in an iodine therapeutic agent, or in a polarizing film. [Background technology] Iodine is one of the most important elements for the life of animals and plants, and is also a trace element essential for the human body. Iodine undergoes complexation reactions with many substances. For example, the complexes obtained by complexing amino acids with polyvinylpyrrolidone (PVP) are water-soluble and are often used as plant nutrients, disinfectants, and bactericides. However, the complexes obtained by complexing these substances with iodine are easily soluble in water and / or alcohol, limiting their scope of application.

[0002] In nature, starch and iodine form a complex that absorbs maximally at 620-680 nm and shows a violet color, so starch is used as an indicator in many chemical titrations with iodine. Amylose can swell and dissolve in water, but the helical structure formed by hydrogen bonds of the hydroxyl groups of glucose is destroyed, so the binding ability of starch with iodine in the dissolved state is greatly reduced.

[0003] Iodine and iodides are radiopaque and are therefore the main components of contrast media. 131 , iodine 125 and iodine 123By incorporating iodine into a compound carrier, radioactively labeled compounds can be produced and used for iodine labeling of proteins. However, existing compound carriers have limited binding capacity, so the amount of iodine that can be bound is limited. Therefore, finding an appropriate compound carrier remains one of the important research topics in these application fields.

[0004] When a polyvinyl alcohol (PVA) film is dyed with iodine and then stretched, the iodine molecules are arranged in an orderly manner in the PVA film, forming a polarizing film with uniform bidirectional absorption. Since PVA is obtained by hydrolysis of vinyl acetate polymer, the degree of polymerization during the manufacturing process, the degree of hydrolysis of ester groups, and the structure of the polymer affect the binding ability of PVA to iodine; PVA has strong water solubility; the binding ability between PVA and iodine molecules is weak, and the PVA-iodine film will lose iodine just by being heated. Increasing the durability of PVA-iodine film in high temperature and high humidity environments is a common technical challenge and research boom in polarizing films. [Contents of the invention] In order to improve the deficiencies of the prior art, the present invention aims to provide an iodine complex and its preparation and use, which can be used as a radioactive marker (e.g., a radiopaque marker), can be used to prepare iodine therapeutic drugs, and can even be used to prepare polarizing films; the iodine complex is formed by complexing iodine with a polymer carrier, and the polymer carrier has good biocompatibility. The iodine content in the iodine complex can be adjusted as needed, for example, the mass content of iodine can be adjusted within 0.001-60wt%.

[0005] The objective of the present invention is achieved by the following technical solutions: The present invention provides use of a polymer containing a structural unit represented by formula (I) and, optionally, at least one structural unit selected from the group consisting of structural units represented by formula (II), formula (III) and formula (IV) as an iodine carrier.

[0006] Such uses include: A polymer containing a structural unit represented by formula (I) and, if necessary, at least one selected from the structural units represented by formulas (II), (III) and (IV) was used as a carrier to complex with iodine to obtain an iodine complex:

[0007] [ka]

[0008] [ka]

[0009] [ka]

[0010] [ka]

[0011] In formula (I), R 1 , R 2 , R 3 , R 4 , R 5 and R 6 may be the same or different, and each independently represents H and C 1-8 an alkyl group and an unsubstituted or optionally one, two or more R a C replaced with 6-20 and an aryl group; each R a may be the same or different, and each independently C 1-12 selected from alkyl groups; a, b, c, d, e and f are each independently an integer greater than or equal to 0, but a and e cannot simultaneously be 0; In formula (II), R 19 H, cyano, and C 1-8 an alkyl group and an unsubstituted or optionally one, two or more R a Substituted groups: C 3-10 Cycloalkyl groups and C 6-20and an aryl group; each R a may be the same or different, and each independently C 1-12 selected from alkyl groups; g is an integer equal to or greater than 1; In formula (III), R 13 , R 16 , R 17 and R 18 may be the same or different, and each independently represents H and C 1-8 an alkyl group and an unsubstituted or optionally one, two or more R a C replaced with 6-20 and an aryl group; each R a may be the same or different, and each independently C 1-12 selected from alkyl groups; h, i, j, k and n' are each independently an integer greater than or equal to 1; In formula (IV), R 7 , R 8 , R 9 , R 10 , R 11 and R 12 may be the same or different, and each independently represents H and C 1-8 an alkyl group and an unsubstituted or optionally one, two or more R a C replaced with 6-20 and an aryl group; each R a may be the same or different, and each independently C 1-12 selected from alkyl groups; a', b', c', d', e', and f' are each independently an integer greater than or equal to 0, and are not all simultaneously 0.

[0012] The present invention further provides an iodine complex, which is obtained by complexing a polymer containing a structural unit represented by formula (I) and, optionally, at least one structural unit selected from the group consisting of structural units represented by formulas (II), (III) and (IV) with iodine as a carrier:

[0013] [ka]

[0014] [ka]

[0015] [ka]

[0016] [ka]

[0017] In formula (I), R 1 , R 2 , R 3 , R 4 , R 5 and R 6 may be the same or different, and each independently represents H and C 1-8 an alkyl group and an unsubstituted or optionally one, two or more R a C replaced with 6-20 and an aryl group; each R a may be the same or different, and each independently C 1-12 selected from alkyl groups; a, b, c, d, e and f are each independently an integer greater than or equal to 0, and a and e cannot simultaneously be 0; In formula (II), R 19 is H, a cyano group, and C 1-8 an alkyl group and an unsubstituted or optionally one, two or more R a C replaced with 3-10 A cycloalkyl group, unsubstituted or optionally containing one, two or more R a C replaced with 6-20 and an aryl group; each R a may be the same or different, and each independently C 1-12 selected from alkyl groups; g is an integer equal to or greater than 1; In formula (III), R 13 , R 16 , R 17 and R 18 may be the same or different, and each independently represents H and C 1-8 an alkyl group and an unsubstituted or optionally one, two or more R a C replaced with 6-20 and an aryl group; each R a may be the same or different, and each independently C 1-12 selected from alkyl groups; h, i, j, k and n' are each independently an integer greater than or equal to 1; In formula (IV), R 7 , R 8 , R 9 , R 10 , R 11 and R 12 may be the same or different, and each independently represents H and C 1-8 an alkyl group and an unsubstituted or optionally one, two or more R a C replaced with 6 - 20 an aryl group; Each R a may be the same or different, and each independently C 1-12 selected from alkyl groups; a', b', c', d', e', and f' are each independently an integer greater than or equal to 0, and are not all simultaneously 0.

[0018] In the present invention, the above-mentioned complexation includes, but is not limited to, the ligand bond and / or van der Waals bond formed between iodine and the polymer molecule. For example, the above-mentioned polymer is a complex formed by the bond between the lone pair of electrons provided by the oxygen atoms in the two pairs of o-hydroxyl groups and the vacant level provided by iodine; for example, the following bonding method is adopted:

[0019] [ka]

[0020] In the present invention, the iodine is one of an iodine molecule and a polyiodine ion in which an iodine molecule is bound to an iodine ion, or a mixture thereof.

[0021] In the present invention, the above polymer may be a homopolymer, a random copolymer, or a block copolymer.

[0022] In the present invention, R 1 , R 2 , R 3 , R 4 , R 5 and R 6 may be the same or different, and each independently represents H and C 1-4 an alkyl group and an unsubstituted or optionally one, two or more R a C replaced with 6-10 an aryl group; R a The definition of is the same as above. Preferably, R 1 , R 2 , R 3 , R 4 , R 5 and R 6 may be the same or different and are each independently selected from H, methyl, phenyl, and tolyl. More preferably, R 1 , R 2 , R 3 , R 4 , R 5 and R 6 may be the same or different and are each independently selected from H and a methyl group. Most preferably, R 1 , R 2 , R 3 , R 4 , R 5 and R 6 are the same and are selected from H.

[0023] In the present invention, R 19 is H, a cyano group, and C 1-4 an alkyl group and an unsubstituted or optionally one, two or more R a C replaced with 6-10an aryl group; R a The definition of is the same as above. Preferably, R 19 is selected from phenyl, tolyl, and cyano.

[0024] In the present invention, R 7 , R 8 , R 9 , R 10 , R 11 and R 12 may be the same or different, and each independently represents H and C 1-4 an alkyl group and an unsubstituted or optionally one, two or more R a C replaced with 6-10 an aryl group; R a The definition of is the same as above. Preferably, R 7 , R 8 , R 9 , R 10 , R 11 and R 12 may be the same or different and are each independently selected from H, methyl, phenyl, and tolyl; more preferably, R 7 , R 8 , R 9 , R 10 , R 11 and R 12 may be the same or different and are each independently selected from H and a methyl group; more preferably, R 7 , R 8 , R 9 , R 10 , R 11 and R 12 are the same and are selected from H.

[0025] In the present invention, R 13 , R 16 , R 17 and R 18 may be the same or different, and each independently represents H and C 1-4 an alkyl group and an unsubstituted or optionally one, two or more R a C replaced with 6-10 an aryl group; R aThe definition of is the same as above. Preferably, R 13 , R 16 , R 17 and R 18 may be the same or different and are each independently selected from H, methyl, phenyl, and tolyl; more preferably, R 13 , R 16 , R 17 and R 18 may be the same or different and are each independently selected from H and a methyl group. Most preferably, R 13 , R 16 , R 17 and R 18 are the same and are selected from H.

[0026] In the present invention, a is an integer of 0-20000, for example, a can be 1, 50, 500, 1000, 2000, 3000, 4000, 5000, 6000, 7000, 8000, 9000, 10000, 12000, 15000, 18000, 20000, for example, a can be an integer of 1-7000; preferably, a is an integer of 50-3000.

[0027] In the present invention, b is an integer of 0-2000, for example, 1, 5, 50, 100, 500, 1000, 1500 or 2000; c is an integer of 0-2000, for example, 1, 5, 50, 100, 500, 1000, 1500 or 2000; d is an integer of 0-2000, for example, 1, 5, 50, 100, 500, 1000, 1500 or 2000. e is an integer from 0 to 20000, for example 1, 50, 500, 1000, 2000, 3000, 4000, 5000, 6000, 7000, 8000, 9000, 10000, 12000, 15000, 18000 or 20000; f is an integer from 0 to 2000, for example 1, 5, 50, 100, 500, 1000, 1500 or 2000.

[0028] In the present invention, g is an integer from 1 to 10000, for example 1, 50, 500, 1000, 2000, 3000, 4000, 5000, 6000, 7000, 8000, 9000 or 10000.

[0029] In the present invention, a' is an integer of 1-20000, for example, 1, 50, 500, 1000, 2000, 3000, 4000, 5000, 6000, 7000, 8000, 9000, 10000, 12000, 15000, 18000 or 20000; b' is an integer of 0-2000, for example, 1, 5, 50, 100, 500, 1000, 1500 or 2000; c' is an integer of 0-2000, for example, 1, 5, 50, 100, 500, 100 d' is an integer between 0 and 2000, for example, 1, 5, 50, 100, 500, 1000, 1500 or 2000; e' is an integer between 0 and 10000, for example, 1, 50, 500, 1000, 2000, 3000, 4000, 5000, 6000, 7000, 8000, 9000 or 10000; f' is an integer between 0 and 2000, for example, 1, 5, 50, 100, 500, 1000, 1500 or 2000. Preferably, a' and e' are not 0 at the same time.

[0030] In the present invention, h is an integer of 0-2000, for example, 1, 5, 50, 100, 500, 1000, 1500 or 2000; i is an integer of 0-2000, for example, 1, 5, 50, 100, 500, 1000, 1500 or 2000; j is an integer of 0-2000, for example, 1, 5, 50, 100, 500, 1000, 1500 or 2000; k is an integer of 0-2000, for example, 1, 5, 50, 100, 500, 1000, 1500 or 2000.

[0031] In the present invention, n' is an integer from 1 to 10, for example, 1, 2, 3, 4, 5, 6, 7, 8, 9 or 10. Preferably, n' is 1 or 2.

[0032] In the present invention, the mass ratio of polymer to iodine in the iodine complex is 1:0.00001-1.5, for example, 1:0.00001, 1:0.0001, 1:0.001, 1:0.005, 1:0.01, 1:0.05, 1:0.1, 1:0.2, 1:0.3, 1:0.4, 1:0.5, 1:0.6, 1:0.7, 1:0.8, 1:0.9, 1:1, 1:1.2 or 1:1.5.

[0033] The present invention further provides a method for preparing the above iodine complex, the method comprising the steps of: The above iodine complex can be produced by reacting a polymer containing a structural unit represented by formula (I) and, optionally, at least one selected from the structural units represented by formulas (II), (III) and (IV) with iodine.

[0034] Wherein, the reaction may be a gas-solid reaction, a solid-liquid reaction, or a liquid-liquid single-phase reaction; The gas-solid reaction is a reaction in which a gas containing iodine is contacted with a polymer solid containing a structural unit represented by formula (I) and, optionally, at least one structural unit selected from the structural units represented by formulas (II), (III), and (IV); The solid-liquid reaction is a reaction of a solution containing iodine with a polymer solid containing a structural unit represented by formula (I) and, optionally, at least one structural unit selected from the structural units represented by formulas (II), (III), and (IV); The liquid-liquid single-phase reaction is a single-phase reaction in which a solution containing iodine is mixed with a solution of a polymer containing a structural unit represented by formula (I) and, optionally, at least one structural unit selected from the structural units represented by formulas (II), (III), and (IV).

[0035] In the present invention, those skilled in the art can reasonably adjust the above reaction temperature and the above reaction time to prepare an iodine complex with a required iodine content; for example, the above reaction temperature is -20°C to 110°C, and the reaction time is 0.5-250h.

[0036] In the present invention, the above reaction is carried out under a sealed condition.

[0037] In the present invention, the iodine-containing gas may be a gas obtained by sublimating solid iodine. The iodine-containing solution may be an iodine-containing solution consisting of solid iodine or a substance containing polyiodine ions and a solvent. The solvent may be, for example, water, dimethyl sulfoxide, acetic acid, ethanol, etc.; the iodine-containing solid may be iodine or a polyiodine ion-containing substance. The solution of the polymer containing the structural unit represented by the formula (I) and, if necessary, at least one selected from the structural units represented by the formulas (II), (III), and (IV) is a solution consisting of a polymer solid containing the structural unit represented by the formula (I) and at least one arbitrarily selected from the structural units represented by the formulas (II), (III), and (IV) and an organic solvent. The organic solvent may be, for example, dimethyl sulfoxide, acetic acid, ethanol, etc.

[0038] In the present invention, the polymer containing the structural unit represented by formula (I) can be produced by the following method.

[0039] (i) An epoxidized polymer can be produced by subjecting a polymer containing a structural unit represented by formula (V) to an oxidation reaction.

[0040] [ka]

[0041] In formula (V), x=a+b+c, y=d+e+f;R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , a, b, c, d, e and f are defined as above; (ii) The epoxidized polymer may be hydrolyzed, or first hydrolyzed and then catalytically hydrogenated, or first catalytically hydrogenated and then hydrolyzed to produce the polymer product.

[0042] In the present invention, the polymer containing the structural unit represented by formula (V) may further contain at least one of structural units represented by formula (II), formula (VI), and formula (VII):

[0043] [ka]

[0044] In formula (II), R 19 and g are defined as above;

[0045] [ka]

[0046] In formula (VI), n=h+i+j+k, R 13 , R 16 , R 17 , R 18 , h, i, j, k and n' are defined as above;

[0047] [ka]

[0048] In formula (VII), x'=a'+b'+c', y'=d'+e'+f';R 7 , R 8 , R 9 , R 10 , R 11 , R 12 , a', b', c', d', e' and f' are defined as above.

[0049] In the present invention, in step (i), the polymer containing the structural unit represented by formula (V) may be obtained by polymerization of a conjugated diene monomer, and the conjugated diene monomer may be, for example, 1,3-butadiene, 1,3-pentadiene or isoprene.

[0050] In step (i), the polymer comprising the structural unit represented by formula (V) and at least one of the structural units represented by formula (II) and / or formula (VI) is prepared by reacting a conjugated diene monomer with R 19 -CH=CH 2 and / or

[0051] [ka]

[0052] The conjugated diene monomer may be, for example, 1,3-butadiene, 1,3-pentadiene or isoprene, and the R 19 , R 13 , R 16 , R 17 , R 18 and n' is defined as above.

[0053] In step (i), the polymer containing the structural unit represented by formula (V) and at least one structural unit represented by formula (VII) is obtained by copolymerization of at least two conjugated diene monomers, and the conjugated diene monomer may be, for example, 1,3-butadiene, 1,3-pentadiene or isoprene.

[0054] In step (i), the polymer comprising the structural unit represented by formula (V), at least one structural unit represented by formula (VII), and at least one structural unit represented by formula (II) and / or formula (VI) is prepared by mixing at least two conjugated diene monomers with at least one R 19 -CH=CH 2 and / or

[0055] [ka]

[0056] The conjugated diene monomer may be, for example, 1,3-butadiene, 1,3-pentadiene or isoprene, and the R 19 , R 13 , R 16 , R 17 , R 18 and n' are defined as above.

[0057] Specifically, a method for producing a polymer containing a structural unit represented by formula (V) is as follows: A continuous solution polymerization method is adopted, in which a conjugated diene (e.g., 1,3-butadiene, 1,3-pentadiene, or isoprene) is mixed with a solvent such as an alkane, an aromatic hydrocarbon, or a mixture of the two (e.g., a toluene-heptane mixture), and the mixture is heated at 30-65°C with an initiator (e.g., nickel naphthenate-BF 3 -Et 3 Al) to initiate the reaction, and if necessary, a molecular weight regulator (e.g., an alcohol such as octanol) is added to adjust the molecular weight, and a polymerization terminator (e.g., ethanol) is added to terminate the polymerization, thereby producing a polymer containing a structural unit represented by formula (V).

[0058] In the present invention, the oxidation reaction in step (i) includes, but is not limited to, the chlorohydrin method, the peroxide epoxidation method, or the direct oxidation method with oxygen. The oxidation reaction is an epoxidation reaction, and the oxidation reaction may be partial epoxidation or complete epoxidation.

[0059] For example, the peroxide may be one or a mixture of more than one of hydrogen peroxide, performic acid, peracetic acid, perbenzoic acid, 3-chloroperbenzoic acid, and tert-butyl hydroperoxide.

[0060] For example, the oxidation reaction may be carried out in an organic solvent containing the polymer or in a water / organic solvent emulsion. The organic solvent may include, but is not limited to, aliphatic alkanes, halogenated aliphatic hydrocarbons, aromatic hydrocarbons, cyclic alkanes, petroleum-based solvents, etc. Preferably, hexane, cyclohexane, heptane, dichloromethane, benzene, toluene, petroleum-based solvents, etc. The temperature of the oxidation reaction is 0-120°C, preferably 20-80°C.

[0061] In the present invention, in the step (ii), the catalytic hydrogenation reaction can open the epoxy ring of the epoxidized polymer by a method such as catalytic hydrogenation to obtain a polymer containing a hydroxy group in the CC chain; the hydrolysis reaction can open the epoxy ring by hydrolyzing the epoxidized polymer with a general acidic or alkaline substance to obtain a polymer containing an o-bishydroxy group in the CC chain. The catalytic hydrogenation reaction can be partial catalytic hydrogenation or complete catalytic hydrogenation. The hydrolysis reaction can also be partial hydrolysis or complete hydrolysis. The specific reaction conditions and the mixing ratio of materials for the catalytic hydrogenation reaction and hydrolysis reaction described above are all selected from the general methods in the art, and are not particularly limited, but it is sufficient to produce a polymer having a structural unit represented by formula (I) of the present application.

[0062] Exemplary examples of the acidic substance include inorganic acids such as aqueous hydrogen halide solutions, sulfuric acid, and nitric acid; organic acids such as alkylsulfonic acids; solid acids; and heteropolyacids.

[0063] Exemplary alkaline substances include aqueous solutions of hydroxides and carbonates of alkali metals.

[0064] Exemplarily, the catalytic hydrogenation is carried out under the action of a catalyst such as Raney nickel, chlorotris(triphenylphosphine)rhodium, platinum, or palladium.

[0065] For example, the catalytic hydrogenation reaction can be carried out in an organic solvent containing a polymer or in a water / organic solvent emulsion, and the organic solvent includes, but is not limited to, an aliphatic alkane, a halogenated aliphatic hydrocarbon, a cyclic alkane, a petroleum solvent, a cyclic ether compound, an alcohol, etc. Preferably, hexane, cyclohexane, tetrahydrofuran, methanol, ethanol, etc. are used. The temperature of the catalytic hydrogenation reaction is 0 to 120°C, preferably 20 to 80°C.

[0066] For example, the hydrolysis reaction can be carried out in an organic solvent containing a polymer, or in a water / organic solvent emulsion, and the organic solvent includes, but is not limited to, an aliphatic alkane, a halogenated aliphatic hydrocarbon, an aromatic hydrocarbon, a cyclic alkane, a petroleum solvent, a cyclic ether compound, a sulfoxide, a sulfone, a pyrrolidinone, a methylpyrrolidinone, etc. Preferred are tetrahydrofuran, dimethyl sulfoxide, methylpyrrolidinone, etc. The temperature of the hydrolysis reaction is -20 to 150°C, preferably -10 to 80°C.

[0067] The present invention further provides the use of the above iodine complexes as radioactive markers, or in iodine therapeutic agents, or in polarizing films.

[0068] Preferably, the radioactive marker is a radiopaque marker. Terms and Interpretations: The term “C 1-12 "Alkyl" is understood to represent preferentially a linear or branched saturated monovalent hydrocarbon radical having 1 to 12 carbon atoms, preferably C 1-8 It is an alkyl group. 1-8"Alkyl" is to be understood as preferentially representing a linear or branched saturated monovalent hydrocarbon radical having 1, 2, 3, 4, 5, 6, 7 or 8 carbon atoms. Said alkyl is, for example, methyl, ethyl, propyl, butyl, pentyl, hexyl, isopropyl, isobutyl, sec-butyl, tert-butyl, isopentyl, 2-methylbutyl, 1-methylbutyl, 1-ethylpropyl, 1,2-dimethylpropyl, neopentyl, 1,1-dimethylpropyl, 4-methylpentyl, 3-methylpentyl, 2-methylpentyl, 1-methylpentyl, 2-ethylbutyl, 1-ethylbutyl, 3,3-dimethylbutyl, 2,2-dimethylbutyl, 1,1-dimethylbutyl, 2,3-dimethylbutyl, 1,3-dimethylbutyl or 1,2-dimethylbutyl, etc. or isomers thereof. In particular, said radicals are those having 1, 2, 3, 4, 5 or 6 carbon atoms ("C 1-6 The alkyl group "is, for example, methyl, ethyl, propyl, butyl, isopropyl, isobutyl, sec-butyl, tert-butyl, and more particularly, the groups have 1, 2 or 3 carbon atoms ("C 1-3 Alkyl ") is, for example, methyl, ethyl, n-propyl or isopropyl.

[0069] The term “C 6-20 The term "aryl group" is understood to represent preferentially a monovalent aromatic or partially aromatic monocyclic, bicyclic or tricyclic cyclic hydrocarbon having 6 to 20 carbon atoms, preferably C 6-14 The term "C" is an aryl group. 6-14 An "aryl group" is a monovalent aromatic or partially aromatic monocyclic, bicyclic or tricyclic cyclic hydrocarbon group having 6, 7, 8, 9, 10, 11, 12, 13 or 14 carbon atoms (C 6-14 It is to be understood that the present invention preferentially expresses a ring having six carbon atoms (C 6 aryl group), for example a phenyl or biphenyl group, or a ring having 9 carbon atoms (C 9aryl group), for example indanyl or indenyl, or a ring having 10 carbon atoms (C 10 aryl group), such as tetrahydronaphthyl, dihydronaphthyl or naphthyl, or a ring having 13 carbon atoms (C 13 aryl group), e.g., fluorenyl, or a ring having 14 carbon atoms (C 14 aryl groups), for example anthracenyl. [Effects of the Invention] The present invention provides an iodine complex and a method for producing the same, and the use of the same as a radiation marker, or in an iodine therapeutic agent, or in a polarizing film. The iodine complex is formed by complexing a polymer carrier with iodine, and the polymer carrier has good biocompatibility, while the iodine complex has a low iodine elution rate, so it can be used as a radiation marker, or in the production of an iodine therapeutic agent, or in the production of a polarizing film. In the production method provided by the present invention, the iodine content in the iodine complex can be adjusted as necessary, and the iodine content can be adjusted within the range of 0.001 to 60%. The difference in iodine content affects the transmission resolution as a radiation marker and the amount of iodine therapeutic agent used. [Explanation of attached diagram] FIG. 1 is an industrial CT scan of the iodine complex film of Example 5.

[0070] FIG. 2 is a TGA diagram of the iodine complex of Example 5. [Mode for carrying out the invention] The method of the present invention will be described in more detail below with reference to specific examples. It should be understood that the following examples are merely illustrative explanations and explanations of the present invention and should not be construed as limiting the scope of protection of the present invention. All technologies realized based on the above content of the present invention are intended to be included within the scope of protection of the present invention.

[0071] Unless otherwise specified, all experimental methods used in the following examples are conventional methods; all reagents, materials, etc. used in the following examples are commercially available products unless otherwise specified. Equipment and Facilities Measurement of material structure: 1 HNMR, 13 A 600MHz Fourier transform nuclear magnetic resonance analyzer from JOEL was used for CNMR; IR is measured by a Thermofisher Fourier transform infrared spectrometer nicolet is50; The Tg value is measured using a TA Q100 differential scanning calorimeter; TGA measurements are performed using a TA Q500 thermogravimetric analyzer; The molecular weight of the polymer is measured by Agilent PL-GPC50 (equipped with a differential refractive index detector and an evaporative light scattering detector); The degree of polarization is measured using a UV-visible spectrometer UV3600 (Shimadzu Corporation, Japan). [Production Example 1] Cis-polybutadiene: Cis-polybutadiene rubber block is commercially available (Sichuan Petrochemical Co., Ltd., among the structures shown in formula IV, the content of 1,4-cis structure is about 98%, and the content of 1,4-trans structure and 1,2-structure is about 2%; number average molecular weight M n =170,000) and sheared into rubber particles of approximately 2 mm.

[0072] Epoxidation: Add 7g of the above cis-polybutadiene rubber particles and 100ml of dichloromethane to a 250ml three-neck flask equipped with a stirrer and thermometer. Dissolve at room temperature in a thermostatic water bath, stir, and when completely dissolved and sticky, pass nitrogen through for several minutes. Add 9.90g of formic acid, and drop 21.40g of 30% aqueous hydrogen peroxide solution while stirring; continue to react while keeping warm for about 15 hours, then 1 HNMR (CDCl 3) analysis, but the signal of chemical shift specific to 1,4-cis double bond disappeared (epoxy group specific chemical shift δ = 2.98, 1,4-cis double bond specific chemical shift δ = 5.40). The reaction product was neutralized to pH = 7 with 10% sodium carbonate solution, the aqueous phase was removed, and after washing with water and separation, absolute ethanol was added to the separated rubber liquid, and when a precipitate was precipitated, the precipitate was separated and washed once with absolute ethanol, and the waste liquid was filtered to obtain wet rubber, which was dried at room temperature for 12 hours and then dried in a vacuum drying box at 40 ° C for 24 hours until it reached a constant weight, and 7.3 g of epoxidized cis-butadiene rubber was obtained.

[0073] Hydrolysis: 1 g of the epoxylated cis-butadiene rubber prepared above is weighed out and dissolved in 100 ml of tetrahydrofuran. A solution consisting of 5 ml of water and 1 ml of perchloric acid is added dropwise over 30 minutes while stirring at 25°C, and the mixture is then stirred at 25°C for 12 hours. 1 HNMR (DMSO) analysis showed that the signals of chemical shifts specific to epoxidized cisbutadiene rubber disappeared (chemical shift δ=2.98 specific to epoxy group, chemical shift δ=4.18 specific to o-bishydroxy group). The reaction solution was neutralized with sodium carbonate solution. 1000 ml of water was dropped into the reaction solution, and when a precipitate was precipitated, the precipitate was separated and immersed in 400 ml of water for 24 hours, and the polymeric substance obtained by filtering off the water was dried at room temperature for 24 hours and then further dried in a vacuum drying box at 40 °C until it reached a constant weight. 1.12 g of a translucent solid was obtained. The molecular weight of the product was Mn=146000, the molar content of o-bishydroxy group C4 units was 98%, and the Tg value was 56 °C. [Production Example 2] 2 g of the epoxylated cis-butadiene rubber prepared above is weighed out and dissolved in 200 ml of freshly distilled tetrahydrofuran, then added to a 500 ml stainless steel high-pressure reactor; 0.4 g of Raney nickel (covered with ethanol and washed three times with tetrahydrofuran before being added to the reactor) is added; the pressure in the high-pressure reactor is increased to 1 MPa with nitrogen gas and then released to normal pressure, and this nitrogen pressurization and release are repeated three times. Hydrogen gas is passed through while stirring at 50°C, and the pressure is increased to 1 MPa. The mixture is reacted with stirring for 12 hours while maintaining the hydrogen gas pressure. 1 The rate of ring-opening of the epoxy group was approximately 75% (mol) as determined by 1 HNMR (DMSO).

[0074] The reaction solution was cooled to 0°C and the pressure was removed. The catalyst was filtered off. A solution consisting of 5 ml of water, 1 ml of perchloric acid, and 5 ml of tetrahydrofuran was added dropwise to the reaction solution from which the catalyst had been removed by filtration over a period of 30 minutes. The reaction temperature was allowed to rise to 25°C, but the mixture was stirred for 12 hours while keeping the temperature constant. 1 HNMR (DMSO) measurement showed that the chemical shift signal specific to epoxidized cisbutadiene rubber disappeared. 0.37g of solid sodium carbonate was added to the reaction solution and stirred for 2 hours. Water was dropped into the reaction solution to precipitate, and the solution was immersed in water for 24 hours, after which the water was filtered off and the resulting polymeric material was dried at room temperature for 24 hours and then further dried in a vacuum drying box at 40°C until it reached a constant weight. 2.35g of a milky white solid was obtained. The number average molecular weight was 133,000, the molar content of o-bishydroxy C4 units was 24.7%, and the Tg value was 66°C. [Production Example 3] Butylbenzene rubber: Butylbenzene rubber block is commercially available (Qilu Petrochemical Co., Ltd., styrene unit / butadiene unit (S / B): 27 / 73, weight average molecular weight M w =320,000) and sheared into approximately 2 mm rubber particles.

[0075] Epoxidation: Add 6g of the above butylbenzene rubber granules and 550ml of toluene to a 1000ml three-neck flask equipped with a stirrer and thermometer. Dissolve at room temperature in a thermostatic water bath, stir, and when completely dissolved and sticky, pass nitrogen gas through for several minutes. Heat to 40°C, add 3.0g of formic acid, and drop 8.2g of 30% hydrogen peroxide solution while stirring; continue to keep warm and react for about 5 hours, then 1 HNMR (CDCl 3 ) analysis, but the chemical shift signal specific to the double bond disappeared. The reaction product was neutralized to pH=7 with 10% sodium carbonate solution, the aqueous phase was removed, and after washing with water and separation, absolute ethanol was added to the separated rubber liquid, and when a precipitate was precipitated, the precipitate was separated, washed once with absolute ethanol, and the waste liquid was filtered to obtain wet rubber, which was then dried at room temperature for 12 hours and then dried in a vacuum drying box at 40℃ for about 24 hours until it reached a constant weight, yielding 6.33g of epoxidized butylbenzene rubber.

[0076] Hydrolysis: 1 g of the epoxidized butylbenzene rubber prepared above is weighed out and dissolved in 100 ml of tetrahydrofuran. A solution consisting of 5 ml of water and 1 ml of perchloric acid is added dropwise over 30 minutes while stirring at 25°C, and the mixture is then stirred at 25°C for 12 hours. 1 HNMR (DMSO) analysis showed that the signal of the chemical shift specific to epoxidation disappeared. The reaction solution was neutralized with sodium carbonate. 1000 ml of water was dropped into the reaction solution, and when a precipitate was precipitated, the precipitate was separated and immersed in 500 ml of water for 24 hours, and the polymeric substance obtained by filtering off the water was dried at room temperature for 24 hours, and then further dried at 40°C in a vacuum drying box until it reached a constant weight. 1.1 g of a white solid was obtained, and the ratio of o-bishydroxy group C4 units was 62%. Example 1 1 g of the translucent solid produced by the method of Production Example 1 and 1.1 g of iodine particles were placed together in a 20 ml glass flask, sealed, and stored at 50°C for 24 hours to obtain an iodine complex through a gas-solid reaction. The iodine complex was a black hard lump weighing 2.0 g, and the mass percentage of iodine in the iodine complex was 50%. Example 2 1 g of the semi-transparent solid produced by the method of Production Example 1 was dissolved in 20 ml of dimethyl sulfoxide to produce a dimethyl sulfoxide solution of the polymer, to which 1.1 g of free iodine particles were added at 25°C and stirred, causing the reaction solution to turn brown due to the dissolution of iodine. After 2 hours, stirring was stopped, the liquid-liquid single-phase reaction was terminated, and 200 ml of methanol was added to precipitate a dark brown solid glutinous mass. The solid was vacuum-dried at 30°C for 24 hours to produce 1.48 g of a black solid mass, i.e., the iodine complex of the present invention, and the mass percentage of iodine in the iodine complex was 32%. Example 3 1 g of the translucent solid produced by the method of Production Example 1 was placed in a sealed glass bottle, and 20 ml of water and 2.0 g of elemental iodine were added. The elemental iodine dissolved in the water was adsorbed by the solid (i.e., liquid-solid reaction). After stirring at 25°C for 8 hours, the solid that did not dissolve or deform was black in color. The solid was taken out and dried in a vacuum drying box at 30°C for 24 hours to obtain a solid with a weight of 1.21 g, that is, the iodine complex of the present invention. The mass percentage of iodine in the iodine complex was 17.4%. Example 4 Iodine adsorption experiment: Related substances: solid products (approximately 3 mm particles) produced by the methods of Production Examples 1, 2, and 3; ethylene-vinyl alcohol polymer (EVOH, Kuraray F171B, Japan, ethylene content 32%, approximately 3 mm particles); polyvinyl alcohol (PVA, Shanghai Shinkai Chemical Technology Co., Ltd., polymerization degree 1680, alcoholysis degree 99%, molecular weight 81000, white powder); soluble pure starch of analytical purity, each of which was dried at 120°C to a constant weight before use.

[0077] Weigh out 2g each of the six solids (accuracy: 0.0001g) and place them in a 100ml glass bottle, then place an open vial containing 4g of elemental iodine (accuracy: 0.0001g) into the same glass bottle and leave it sealed at 20℃ for 100 hours. Remove the solids and weigh them to calculate the increase in weight.

[0078] [Table 1]

[0079] Example 5 1 g of the translucent solid obtained in Preparation Example 1 was dissolved in 20 ml of dimethyl sulfoxide, and the solution was transferred to a stainless steel palette (304 material, 27 x 20 x 2 cm) and allowed to naturally level. It was then dried to a constant weight to obtain a soft polymer film. The polymer film and iodine particles were placed in a sealed glass bottle and left at 50°C for 12 hours to obtain 1.2 g of a black complex film. The mass percentage of iodine in the iodine complex was 16.7%.

[0080] The iodine complex film obtained in Example 5 was imaged using an XTH225 series industrial CT scanner with a 225 kV microfocus X-ray source, and the results are shown in FIG.

[0081] As can be seen from the IR analysis of the graft of the iodine complex obtained in Example 5, compared with the translucent solid produced in Preparation Example 1, the value of the stretching vibration peak of the hydroxyl group gradually shifts to the higher frequency direction, and the so-called blue shift phenomenon appears, the hydrogen bond of the hydroxyl in the polymer structure is weakened, and the lone electron pair provided by the oxygen atoms in the two pairs of o-hydroxyl groups enters the vacant valence level provided by iodine, forming an iodine complex in the form of a ligand bond.

[0082] The results of the weightless analysis of the iodine complex obtained in Example 5 were as shown in FIG. 2. As the temperature increased, iodine continued to dissociate and volatilize, and at 350° C., iodine was completely volatilized. Example 6 For the saline immersion experiment, prepare the following materials: The iodine complex prepared in Example 1 (iodine content: 50.0%); Iodine-bound starch prepared in Example 4 (iodine content 19.4%); Commercially available povidone-iodine solid (iodine content 11.2%); Physiological saline was prepared according to the Chinese Pharmacopoeia standard.

[0083] 1 g of each of the above substances was accurately weighed, added to 100 ml of physiological saline, and soaked for 24 hours. The solid substances were removed and washed with a small amount of physiological saline, and the washings were returned to the soaking solution. The soaking solution was titrated with sodium thiosulfate standard solution to calculate the iodine dissolution rate.

[0084] Iodine elution rate % = (iodine content in immersion liquid (wt%) × weight of immersion liquid) / iodine content weight before immersion of solid object × 100.

[0085] [Table 2]

[0086] Example 7 The iodine-containing film produced in Example 5 was cut into a size of 5 cm x 4 cm and a thickness of 0.05 to 0.07 mm; it was stretched to a thickness of 0.02 mm using a stretching machine. The stretched iodine film was cut into two pieces of size 2 cm x 2 cm, and each was placed on a white glass plate (transmittance 100%). The transmittance Tsp (single transmittance, theoretical value is 50%), T⊥ (orthogonal transmittance when two polarizing films are arranged perpendicularly in the axial direction), and T∥ (parallel transmittance when two polarizing films are arranged parallel in the axial direction) of the film were measured using an ultraviolet-visible light spectrophotometer, and the polarization degree PE = (T∥-T⊥) / (T∥+T⊥) × 100% was calculated as the film polarization degree. The measurement and calculation result was polarization degree PE = 90%. When the iodine film after stretching was measured in the same manner as in Example 6, the iodine film immersed in saline did not deform, and the iodine elution rate was 0.09 wt %. Compared with PVA, which is highly water-soluble, the polarizing film produced from the polymer provided by the present invention had better moisture resistance than the PVA-based polarizing film.

[0087] The above describes the implementation method of the present invention. However, the present invention is not limited to the above implementation method. Any modifications, equivalent replacements, improvements, etc. made within the spirit and principle of the present invention shall be included within the protection scope of the present invention. [Brief description of the drawings]

[0088] [Figure 1] FIG. 1 is an industrial CT scan of the iodine complex film of Example 5. [Diagram 2] FIG. 2 is a TGA diagram of the iodine complex of Example 5.

Claims

1. An iodine complex obtained by complexing iodine with a polymer carrier comprising a structural unit represented by formula (I) and, as necessary, at least one structural unit selected from the group consisting of structural units represented by formula (II), formula (III) and formula (IV). 【Chemistry 1】 【Chemistry 2】 【Chemistry 3】 【Chemistry 4】 In formula (I), R 1 , R 2 , R 3 , R 4 , R 5 and R 6 may be the same or different, and each independently represents H and C 1-8 an alkyl group and an unsubstituted or optionally substituted group having one, two or more R a C replaced with 6-20 and an aryl group; each R a may be the same or different, and each independently C 1-12 Selected from alkyl groups; a is an integer greater than or equal to 50, e is an integer greater than or equal to 1, and b, c, d, and f are each independently an integer greater than or equal to 0; In formula (II), R 19 H, cyano, and C 1-8 an alkyl group and an unsubstituted or optionally substituted group having one, two or more R a C replaced with 3-10 A cycloalkyl group, unsubstituted or optionally containing one, two or more R a C replaced with 6-20 and an aryl group; each R a may be the same or different, and each independently C 1-12 Selected from alkyl groups; g is an integer equal to or greater than 1; In formula (III), R 13 , R 16 , R 17 and R 18 may be the same or different, and each independently represents H and C 1-8 an alkyl group and an unsubstituted or optionally substituted group having one, two or more R a C replaced with 6-20 and an aryl group; each R a may be the same or different, and each independently C 1-12 Selected from alkyl groups; h, i, j, k and n' are each independently an integer greater than or equal to 1; In formula (IV), R 7 , R 8 , R 9 , R 10 , R 11 and R 12 may be the same or different, and each independently represents H and C 1-8 an alkyl group and an unsubstituted or optionally substituted group having one, two or more R a Replaced by C 6-20 an aryl group; Each R a may be the same or different, and each independently C 1-12 Selected from alkyl groups; a', b', c', d', e' and f' are each independently an integer greater than or equal to 0, and are not all simultaneously 0.

2. R 1 , R 2 , R 3 , R 4 , R 5 and R 6 may be the same or different, and each independently represents H and C 1-4 an alkyl group and an unsubstituted or optionally substituted group having one, two or more R a C replaced with 6-10 aryl groups; and R a The iodine complex according to claim 1, wherein the definition of is as above.

3. R 1 , R 2 , R 3 , R 4 , R 5 and R 6 2. The iodine complex of claim 1, wherein may be the same or different and are each independently selected from H, a methyl group, phenyl, and tolyl.

4. 2. The iodine complex of claim 1, wherein a is an integer of 50-20000, b is an integer of 0-2000; c is an integer of 0-2000; d is an integer of 0-2000; e is an integer of 1-20000; and f is an integer of 0-2000.

5. 2. The iodine complex of claim 1, wherein a is an integer from 50 to 3000.

6. R 19 is H, a cyano group, and C 1-4 an alkyl group and an unsubstituted or optionally substituted group having one, two or more R a C replaced with 6-10 an aryl group; R a The iodine complex according to claim 1, wherein the definition of is as above.

7. R 19 is selected from phenyl, tolyl, and cyano; The iodine complex according to claim 1, wherein g is an integer from 1 to 10,000.

8. R 7 , R 8 , R 9 , R 10 , R 11 and R 12 may be the same or different, and each independently represents H and C 1-4 an alkyl group and an unsubstituted or optionally substituted group having one, two or more R a C replaced with 6-10 an aryl group; R a The iodine complex according to claim 6, wherein the definition of is as above.

9. 2. The iodine complex of claim 1, wherein a' is an integer of 0-20000; b' is an integer of 0-2000; c' is an integer of 0-2000; d' is an integer of 0-2000; e' is an integer of 0-10000; and f' is an integer of 0-2000.

10. a' and e' cannot be 0 at the same time; and / or R 7 , R 8 , R 9 , R 10 , R 11 and R 12 2. The iodine complex of claim 1, wherein: may be the same or different and are each independently selected from H, methyl, phenyl, and tolyl.

11. R 13 , R 16 , R 17 and R 18 may be the same or different, and each independently represents H and C 1-4 an alkyl group and an unsubstituted or optionally substituted group having one, two or more R a C replaced with 6-10 an aryl group; R a The definitions are the same as above; 2. The iodine complex of claim 1, wherein h is an integer from 0 to 2000; i is an integer from 0 to 2000; j is an integer from 0 to 2000; and k is an integer from 0 to 2000.

12. R 13 , R 16 , R 17 and R 18 may be the same or different and are each independently selected from H, methyl, phenyl, and tolyl; And / or n' is an integer from 1 to 10.

13. The iodine complex according to claim 1, wherein the iodine is one of an iodine molecule and a polyiodine ion in which an iodine molecule is bound to an iodine ion, or a mixture thereof.

14. The polymer is a homopolymer, a random copolymer or a block copolymer; And / or the mass ratio of polymer to iodine in the iodine complex is 1:0.00001-1.

5.

15. A method for preparing the iodine complex according to any one of claims 1 to 14, comprising the steps of: The iodine complex can be produced by reacting a polymer containing a structural unit represented by formula (I) and, if necessary, at least one structural unit selected from the structural units represented by formula (II), formula (III), and formula (IV) with iodine; Wherein, the reaction is a gas-solid reaction, a solid-liquid reaction, or a liquid-liquid single-phase reaction; The gas-solid reaction is a contact reaction between a gas containing iodine and a polymer solid containing a structural unit represented by formula (I) and, if necessary, at least one structural unit selected from the group consisting of structural units represented by formulas (II), (III), and (IV); The solid-liquid reaction is a reaction of a solution containing iodine with a polymer solid containing a structural unit represented by formula (I) and, if necessary, at least one structural unit selected from the group consisting of structural units represented by formulas (II), (III), and (IV); The liquid-liquid single-phase reaction is a single-phase reaction in which a solution containing iodine is mixed with a solution of a polymer containing a structural unit represented by formula (I) and, if necessary, at least one structural unit selected from the group consisting of structural units represented by formulas (II), (III), and (IV).

16. The method according to claim 15, wherein the reaction temperature is -20°C to 110°C, and the reaction time is 0.5-250h. Alternatively, a polymer comprising a structural unit represented by formula (I) can be prepared by the following method: (i) An epoxidized polymer can be produced by subjecting a polymer containing a structural unit represented by formula (V) to an oxidation reaction; 【Chemistry 5】 In formula (V), x=a+b+c, y=d+e+f;R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , a, b, c, d, e and f are as defined above; (ii) The epoxidized polymer can be hydrolyzed, or first hydrolyzed and then subjected to a hydrogenation catalysis, or first subjected to a hydrogenation catalysis and then hydrolyzed to produce a polymer containing structural units represented by formula (I) above.

17. The method of claim 16, wherein the polymer comprising the structural unit represented by formula (V) further comprises at least one of structural units represented by formula (II), formula (VI), and formula (VII). 【Chemistry 6】 In formula (II), R 19 and g are defined as above; 【Chemistry 7】 In formula (VI), n=h+i+j+k, R 13 , R 16 , R 17 , R 18 , h, i, j, k and n' are defined as above; 【Chemistry 8】 In formula (VII), x'=a'+b'+c', y'=d'+e'+f'; R 7 , R 8 , R 9 , R 10 , R 11 , R 12 The definitions of a', b', c', d', e' and f' are the same as above.

18. Use of the iodine complex according to any one of claims 1 to 14 in a radioactive marker.

19. The use according to claim 18, wherein the radioactive marker is a radiopaque marker.

20. Use of the iodine complex according to any one of claims 1 to 14 in an iodine therapeutic agent.

21. Use of an iodine complex according to any one of claims 1 to 14 in a polarising film.

Citation Information

Patent Citations

  • Shinkijushinoseizoho

    JP1976092888A

  • Modified rubber and method for producing it

    JP2009173727A

  • Manufacturing method of polarizing film

    JP2014119501A

  • Water-soluble highly syndiotactic polyvinyl alcohol

    JP2016505701A

  • Polarization film, polarization plate and manufacturing method of polarization film

    JP2019053279A