Honeycomb structure and electrically heated carrier
A ceramic honeycomb structure doped with group 13 or 15 elements and optimized silicon content addresses high resistivity and low thermal shock resistance issues, ensuring effective performance across diverse voltages and temperatures.
Patent Information
- Application Number
- JP2021042752
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-16
- Publication Date
- 2024-12-04
- Estimated Expiration
- 2041-03-16
AI Technical Summary
Existing honeycomb structures used in electrically heated catalysts face challenges with high volume resistivity for low-voltage applications and low thermal shock resistance, necessitating improvements for broader voltage compatibility and enhanced durability.
A ceramic honeycomb structure composed of silicon carbide, silicon nitride, or aluminum nitride particles, doped with group 13 or 15 elements, with a silicon content of 20-80% by mass and porosity of 30% or less, featuring electrode portions and a metal terminal configuration to manage resistance and thermal shock.
The solution provides a honeycomb structure with low resistance and good thermal shock resistance, effectively suppressing excessive current and maintaining structural integrity across varying voltages, including low voltages like 48V, while enhancing thermal conductivity.
Smart Images

Figure 0007594471000002 
Figure 0007594471000003 
Figure 0007594471000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a honeycomb structure and an electrically heated carrier. [Background technology]
[0002] An electrically heated catalyst (EHC) is a system in which electrodes are placed on a honeycomb structure made of conductive ceramics, and the honeycomb structure itself generates heat when electricity is passed through it, thereby raising the temperature of the catalyst supported on the EHC to its activation temperature before the engine is started.
[0003] Since various voltages are used for EHC power supplies, the resistance of the EHC substrate must be adjusted to the target resistance in order to match the voltage being used.
[0004] Patent Document 1 discloses an EHC using a honeycomb structure formed of a Si-SiC material. Si and SiC have a somewhat high volume resistivity. Therefore, even when the honeycomb structure described in Patent Document 1 is used in an EHC used under a high voltage of 200 to 500 V, the resistance can be adjusted to within a range of several Ωcm to 200 Ωcm. As a result, when used under a high voltage of 200 to 500 V, it is possible to suppress the flow of excessive current.
[0005] A very wide range of voltages is used for the power source of the EHC depending on the type of the vehicle in which it is installed. In particular, when a low voltage of 60 V or less, for example 48 V, is used for the power source of the EHC, it is necessary to adjust the resistance within a range of the order of 0.1 Ω cm in order to suppress the generation of excess current. In response to this problem, Patent Document 2 proposes a honeycomb structure that is formed of ceramics containing Si, and that can effectively suppress the generation of excess current even when used under low voltage by controlling the Si content in the ceramics and the dopant concentration in the Si. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Patent No. 5735428 [Patent Document 2] JP 2020-204300 A Summary of the Invention [Problem to be solved by the invention]
[0007] However, the Si-SiC material used in the honeycomb structure described in Patent Document 1 has a high volume resistivity and is therefore left to be improved for use in low-voltage EHCs. Also, the ceramic material containing Si with a given dopant concentration used in the honeycomb structure described in Patent Document 2 has low thermal shock resistance and is left to be improved.
[0008] The present invention has been made in consideration of the above problems, and an object of the present invention is to provide a honeycomb structure and an electrically heated carrier which have low resistance and good thermal shock resistance. [Means for solving the problem]
[0009] The above problems are solved by the present invention, which is specified as follows: A. A ceramic honeycomb structure having an outer peripheral wall and partition walls disposed inside the outer peripheral wall and defining a plurality of cells that form flow paths extending from one end face to the other end face, The honeycomb structure is (1) Particles including one or more selected from silicon carbide, silicon nitride, and aluminum nitride; (2) silicon doped with a dopant; the dopant is a Group 13 element or a Group 15 element, The honeycomb structure has a silicon content (B) of 20 to 80 mass % and a porosity of 30% or less. B. The honeycomb structure according to A, A pair of electrode portions provided on a surface of an outer peripheral wall of the honeycomb structure; Metal terminals provided on the pair of electrodes; An electrically heated carrier having Effect of the Invention
[0010] According to the present invention, it is possible to provide a honeycomb structure and an electrically heated carrier having low resistance and good thermal shock resistance. [Brief description of the drawings]
[0011] [Figure 1] 1 is a schematic external view of a honeycomb structure according to an embodiment of the present invention; [Diagram 2] 2 is a schematic cross-sectional view perpendicular to the extension direction of cells of an electrically heated carrier according to an embodiment of the present invention. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Hereinafter, with reference to the drawings, an embodiment of the honeycomb structure and the electrically heated carrier of the present invention will be described. However, the present invention should not be interpreted as being limited thereto, and various changes, modifications, and improvements can be made based on the knowledge of those skilled in the art without departing from the scope of the present invention.
[0013] <Honeycomb structure> Fig. 1 shows a schematic view of the appearance of a honeycomb structure 10 according to an embodiment of the present invention. The honeycomb structure 10 is made of ceramics, has an outer peripheral wall 12, and partition walls 13 disposed inside the outer peripheral wall 12 to partition and form a plurality of cells 15 that form flow paths extending from one end face to the other end face, and is formed in a columnar shape. The honeycomb structure 10 also has a pair of electrode parts 14a, 14b disposed on the surface of the outer peripheral wall 12 so as to face each other across the central axis of the honeycomb structure 10. The electrode parts 14a, 14b may not be provided.
[0014] The honeycomb structure 10 contains particles containing one or more selected from silicon carbide, silicon nitride, and aluminum nitride, and silicon doped with a dopant. The silicon carbide, silicon nitride, and aluminum nitride particles function as aggregate particles of the honeycomb structure 10, and can strengthen the honeycomb structure 10. In particular, it is preferable that the main component of the particles is silicon carbide, since it has a higher thermal conductivity and a smaller difference in thermal expansion coefficient with silicon. When it is said that the main component of the particles is silicon carbide, it means that the particles contain silicon carbide (total mass) in an amount of 80 mass% or more of the total, and more preferably 90 mass% or more of the total.
[0015] The dopant in the silicon contained in the honeycomb structure 10 is a Group 13 element or a Group 15 element. The Group 13 element or the Group 15 element has a concentration of 1×10 16 ~5×10 20 pieces / cm 3 In this case, the group 13 elements refer to boron (B), aluminum (Al), gallium (Ga), indium (In), etc., and the group 15 elements refer to nitrogen (N), phosphorus (P), arsenic (As), antimony (Sb), bismuth (Bi), etc. If the dopants in the silicon contained in the honeycomb structure 10 are elements of the same group, they can exhibit conductivity without being affected by counter doping, so they may contain multiple types of elements. In addition, it is more preferable that the dopant is one or two types selected from B and Al. It is also preferable that the dopant is one or two types selected from N and P. B, Al, N, and P are each 1×10 16 ~5×10 20 pieces / cm 3 In this concentration range, it can be more easily incorporated into silicon as a dopant.
[0016] The concentration of the dopant in the silicon contained in the honeycomb structure 10 is 1×10 16 ~5×10 20 pieces / cm 3It is preferable that the concentration of the dopant in the silicon contained in the honeycomb structure 10 is controlled within such a range, thereby making it possible to reduce the volume resistivity of the honeycomb structure 10. The concentration of the dopant in the silicon contained in the honeycomb structure 10 can be appropriately adjusted according to the desired volume resistivity of the honeycomb structure 10. In general, when the concentration of the dopant in the silicon is high, the volume resistivity of the honeycomb structure 10 is low, and when the concentration of the dopant in the silicon is low, the volume resistivity of the honeycomb structure 10 is high. The present inventors have found that the volume resistivity of the honeycomb structure 10 can be effectively reduced by doping silicon alone, rather than the above-mentioned compounds such as silicon carbide, silicon nitride, and aluminum nitride that function as aggregate particles. The concentration of the dopant in the silicon is more preferably 5×10 17 ~5×10 20 pieces / cm 3 It is.
[0017] The concentration of the dopant in the silicon contained in the honeycomb structure 10 can be measured, for example, by the following method. In the following, a case where boron is contained as a dopant will be described, but the same method can be used for measurement of dopants other than boron.
[0018] First, the honeycomb structure is cut along a plane perpendicular to the central axis to expose the cut surface. Next, the unevenness of the cross section of the honeycomb structure is filled with resin, and the surface filled with resin is polished. Next, the polished surface of the honeycomb structure is observed, and elemental analysis of the materials constituting the honeycomb structure is performed by energy dispersive X-ray spectroscopy (EDX analysis).
[0019] Next, for the portions of the polished surface that are determined to be "silicon," whether or not the silicon contains "other elements" is determined using the following method. First, for the portions where silicon element is detected, the portions where elements other than silicon are detected are determined to be "other components" by mapping using a cross-sectional structure photograph of the polished surface and an electron probe microanalyzer (EPMA analysis). Examples of "other elements" include boron, and metal borides and borides that exist in silicon as a boron source.
[0020] Next, for the portion where only silicon element or silicon and boron are detected by EPMA analysis and determined to be "silicon", the amount of boron in silicon is identified by the following method. First, the honeycomb structure including the portion determined to be "silicon" is cut into several millimeters thick, and the cut honeycomb structure is subjected to cross-section preparation using the broad ion beam method to prepare a sample for measuring the amount of boron. The broad ion beam method is a method for preparing a sample cross-section using an argon ion beam. Specifically, a shield plate is placed directly above the sample, and a broad ion beam of argon is irradiated from above to etch the sample, thereby preparing a cross-section of the sample along the end face of the shield plate. Next, the boron in silicon of the sample whose cross-section has been prepared is analyzed by time-of-flight secondary ion mass spectrometry (TOF-SIMS). In time-of-flight secondary ion mass spectrometry, a sample is first irradiated with a primary ion beam, causing secondary ions to be emitted from the surface of the sample. The emitted secondary ions are then introduced into a time-of-flight mass spectrometer to obtain a mass spectrum of the outermost surface of the sample. The sample is then analyzed using the obtained mass spectrum, and the concentration of boron in silicon (particles / cm) is determined. 3 ) is calculated by correlation between the spectral intensity of boron in silicon and a previously measured value (e.g., a calibration curve) for the concentration.
[0021] The silicon contained in the honeycomb structure 10 is preferably present as a continuous layer. With such a configuration, it is easy to control the volume resistivity to a low level. Here, the presence of silicon as a continuous layer refers to a matrix-domain structure in which the particles of silicon carbide or the like are domains and silicon is the matrix.
[0022] The honeycomb structure 10 has a silicon content of 20 to 80% by mass. When the honeycomb structure 10 has a silicon content of 20% by mass or more, it is easy to form a structure in which low-resistance doped silicon is arranged in series in a microstructure. As a result, the volume resistivity of the honeycomb structure 10 can be reduced, and the generation of excess current can be effectively suppressed even for a low voltage of 60V or less, such as 48V. Furthermore, such a configuration increases the ratio of strength to Young's modulus in the honeycomb structure 10, and improves thermal shock resistance. When the honeycomb structure 10 has a silicon content of 80% by mass or less, the honeycomb structure can have a shape stability. The silicon content in the honeycomb structure 10 is more preferably 30 to 80% by mass, and even more preferably 40 to 80% by mass.
[0023] The method for calculating the silicon content in the honeycomb structure includes, for example, the following method. In the following method, a calculation method when silicon and silicon carbide are used as ceramic raw materials will be described. When silicon and silicon carbide are used as ceramic raw materials, the composition after the formation of the honeycomb structure is composed of silicon (Si), silicon carbide (SiC) and silicon dioxide (SiO2). The composition amounts of Si, SiC and SiO2 in this honeycomb structure can be measured by measuring the silicon element amount and the oxygen element amount by the fluorescent X-ray method, and the carbon element amount by the resistance heating infrared absorption method. The SiC amount is calculated by assuming that all carbon elements are SiC and calculating the SiC amount in the honeycomb structure by molecular weight calculation. The SiO2 amount is calculated by assuming that all oxygen elements are SiO2 and calculating the SiO2 amount in the honeycomb structure by molecular weight calculation. The amount of Si can be calculated by subtracting the total amount of Si, which is the sum of the amount of Si in SiC and the amount of Si in SiO2, from the amount of silicon element determined by the X-ray fluorescence method and the amount of SiC and the amount of SiO2 calculated above from the total amount of silicon element. When a ceramic raw material other than silicon carbide is used, the amount of element can be calculated by measuring the amount of element by the X-ray fluorescence method or the resistance heating infrared absorption method after confirming the composition after the formation of the honeycomb structure.
[0024] It is preferable that 80 mass% or more of the total mass of the honeycomb structure 10 excluding the silicon content is particles containing one or more selected from the above-mentioned silicon carbide, silicon nitride, and aluminum nitride. With such a configuration, high thermal conductivity and good thermal shock resistance can be obtained. It is more preferable that 90 mass% or more of the total mass of the honeycomb structure 10 excluding the silicon content is such particles, and even more preferable that 95 mass% or more is such particles.
[0025] The silicon contained in the honeycomb structure 10 may contain impurities of Al and Fe. In this case, the content of the impurities Al and Fe in the silicon contained in the honeycomb structure 10 is preferably 2 mass% or less, respectively, relative to the silicon. When the content of the impurities Al and Fe in the silicon contained in the honeycomb structure 10 is 2 mass% or less, respectively, relative to the silicon, variation in the shape of the honeycomb structure 10 during manufacture can be effectively suppressed. The content of the impurities Al and Fe in the silicon contained in the honeycomb structure 10 is more preferably 1 mass% or less, and even more preferably 0.1 mass% or less.
[0026] In the embodiment of the present invention, when the silicon contained in the honeycomb structure 10 contains impurities, the impurities exist in a form attached to the silicon. In contrast, in the embodiment of the present invention, when the silicon contained in the honeycomb structure 10 contains a dopant, the dopant exists in the form dissolved in the silicon particles.
[0027] The porosity of the honeycomb structure 10 is controlled to 30% or less. When the porosity of the honeycomb structure 10 is 30% or less, the thermal conductivity of the honeycomb structure 10 is improved, thereby improving the thermal shock resistance. The porosity of the honeycomb structure 10 is preferably 20% or less, and more preferably 10% or less. The lower limit of the porosity of the honeycomb structure 10 is theoretically 0% or more. The porosity of the honeycomb structure 10 is a value measured by a mercury porosimeter.
[0028] The thermal conductivity of the honeycomb structure 10 is preferably 30 W / m·K or more. With such a configuration, good thermal shock resistance can be obtained in the honeycomb structure 10. The thermal conductivity of the honeycomb structure 10 is more preferably 50 W / m·K or more, and even more preferably 70 W / m·K or more.
[0029] The volume resistivity of the honeycomb structure 10 may be appropriately set according to the applied voltage, and is not particularly limited, but may be, for example, 0.001 to 100 Ω·cm. For high voltages of more than 60 V, the volume resistivity may be 2 to 100 Ω·cm, and typically 5 to 100 Ω·cm. For low voltages of 60 V or less, such as 48 V, the volume resistivity may be 0.001 to 2 Ω·cm, typically 0.001 to 1 Ω·cm, and more typically 0.01 to 1 Ω·cm. In particular, when the concentration of the dopant in silicon contained in the honeycomb structure 10 is 1×10 16 ~5×10 20 pieces / cm 3 In this case, the volume resistivity of the honeycomb structure 10 can be reduced so that excessive current does not occur even when used at a low voltage of 60V or less, such as 48V. The volume resistivity of the honeycomb structure may be 0.01 Ω·cm or more and 5 Ω·cm or less. A honeycomb structure having a volume resistivity of 5 Ω·cm or less can satisfactorily suppress the occurrence of excessive current even at a low voltage of 48V. On the other hand, a honeycomb structure having a volume resistivity of more than 5 Ω·cm cannot sufficiently suppress the occurrence of excessive current at a low voltage of 48V.
[0030] The outer shape of the honeycomb structure 10 is not particularly limited as long as it is columnar, and may be, for example, a columnar shape with a circular end face (cylindrical shape), a columnar shape with an oval end face, a columnar shape with a polygonal end face (quadragonal, pentagonal, hexagonal, heptagonal, octagonal, etc.), etc. The size of the honeycomb structure 10 is set to 2000 to 20000 mm2 in order to increase the heat resistance (suppress cracks in the circumferential direction of the outer peripheral wall). 2 It is preferable that the thickness is 5000 to 15000 mm. 2 It is more preferable that:
[0031] Although there is no limitation on the shape of the cells in a cross section perpendicular to the stretching direction of the cells 15, a square, a hexagon, an octagon, or a combination thereof is preferable. Among these, a square and a hexagon are preferable from the viewpoint of easily achieving both structural strength and heating uniformity.
[0032] The thickness of the partition walls 13 that define the cells 15 is preferably 0.1 to 0.3 mm, and more preferably 0.15 to 0.25 mm. In the present invention, the thickness of the partition walls 13 is defined as the length of a portion that passes through the partition wall 13, of a line segment connecting the centers of gravity of adjacent cells 15 in a cross section perpendicular to the stretching direction of the cells 15.
[0033] The honeycomb structure 10 has a cell density of 40 to 150 cells / cm in a cross section perpendicular to the flow direction of the cells 15. 2 Preferably, the cell density is 70 to 100 cells / cm. 2 It is more preferable that the cell density is within this range. By setting the cell density in this range, the purification performance of the catalyst can be improved while reducing the pressure loss when exhaust gas flows through the catalyst. The cell density is a value obtained by dividing the number of cells by the area of one bottom surface portion of the honeycomb structure 10 excluding the peripheral wall 12 portion.
[0034] Providing the outer peripheral wall 12 of the honeycomb structure 10 is useful from the viewpoint of ensuring the structural strength of the honeycomb structure 10 and suppressing leakage of the fluid flowing through the cells 15 from the outer peripheral wall 12. Specifically, the thickness of the outer peripheral wall 12 is preferably 0.05 mm or more, more preferably 0.1 mm or more, and even more preferably 0.2 mm or more. However, if the outer peripheral wall 12 is made too thick, the strength becomes too high, and the strength balance with the partition walls 13 is lost, resulting in a decrease in thermal shock resistance. Therefore, the thickness of the outer peripheral wall 12 is preferably 1.0 mm or less, more preferably 0.7 mm or less, and even more preferably 0.5 mm or less. Here, the thickness of the outer peripheral wall 12 is defined as the thickness in the normal direction to the tangent of the outer peripheral wall 12 at the measurement point when the portion of the outer peripheral wall 12 to be measured for thickness is observed in a cross section perpendicular to the extension direction of the cells.
[0035] The honeycomb structure 10 may have a pair of electrode parts 14a, 14b arranged on the surface of the outer peripheral wall 12 so as to face each other across the central axis of the honeycomb structure 10. Each electrode part 14a, 14b is electrically connected to the honeycomb structure 10. With this configuration, the honeycomb structure 10 can suppress bias in the current flowing through the honeycomb structure 10 when a voltage is applied, and can suppress bias in the temperature distribution within the honeycomb structure 10. The shape and size of the electrode parts 14a, 14b are not particularly limited, and can be appropriately designed depending on the size, current carrying performance, etc. of the honeycomb structure 10. For example, each electrode part 14a, 14b may be provided in a strip shape extending in the extension direction of the cells 15 of the honeycomb structure 10.
[0036] The electrode parts 14a and 14b are formed of a material having electrical conductivity. The electrode parts 14a and 14b are preferably oxide ceramics, or a mixture of a metal or a metal compound and an oxide ceramic. The metal may be either a single metal or an alloy, and for example, silicon, aluminum, iron, stainless steel, titanium, tungsten, Ni-Cr alloy, etc. can be preferably used. The metal compound is a material other than oxide ceramic, and includes metal oxides, metal nitrides, metal carbides, metal silicides, metal borides, and composite oxides, and for example, FeSi2, CrSi2, alumina, silica, titanium oxide, etc. can be preferably used. The metal and the metal compound may be either a single type or a combination of two or more types. Specific examples of oxide ceramics include glass, cordierite, and mullite. The glass may further contain an oxide of at least one component selected from B, Mg, Al, Si, P, Ti, and Zr. It is more preferable to further contain an oxide of the above-mentioned component in that the strength of the electrode parts 14a and 14b is further improved. The material constituting the electrode parts 14a, 14b is more preferably a material containing particles containing one or more selected from silicon carbide, silicon nitride, and aluminum nitride, and silicon doped with a dopant, similar to the material constituting the above-mentioned honeycomb structure 10. With such a configuration, the electrode parts 14a, 14b are made of the same material as the honeycomb structure 10, so there is no interface between the honeycomb base material and the electrode parts, improving strength. It is more preferable that the electrode parts 14a, 14b contain silicon carbide and silicon doped with a dopant.
[0037] <Manufacturing method of honeycomb structure> The honeycomb structure 10 can be manufactured in accordance with a method for manufacturing a honeycomb structure in a known method for manufacturing a honeycomb structure. For example, the honeycomb structure 10 can be manufactured in accordance with the method described below. For example, first, a binder, a surfactant, water, etc. are added to ceramic powder containing silicon carbide powder to prepare a forming raw material.
[0038] Examples of the binder include methyl cellulose, hydroxypropyl methyl cellulose, hydroxypropoxyl cellulose, hydroxyethyl cellulose, carboxymethyl cellulose, polyvinyl alcohol, etc. Among these, it is preferable to use methyl cellulose and hydroxypropoxyl cellulose in combination. The content of the binder is preferably 2.0 to 10.0 parts by mass when the mass of the ceramic powder containing silicon carbide powder is 100 parts by mass.
[0039] The content of water is preferably 20 to 60 parts by mass when the mass of the ceramic powder containing silicon carbide powder is taken as 100 parts by mass.
[0040] The surfactant may be ethylene glycol, dextrin, fatty acid soap, polyalcohol, etc. These may be used alone or in combination of two or more. The content of the surfactant is preferably 0.1 to 2.0 parts by mass when the mass of the ceramic powder containing silicon carbide powder is 100 parts by mass.
[0041] A pore former may be added to the extent that it does not affect the porosity of the present invention. Examples of the pore former include starch, foamed resin, and water-absorbent resin.
[0042] Next, the obtained molding raw material is kneaded to form a clay, and then the clay is extruded to produce a raw (unfired) honeycomb molded body. In the extrusion molding, a die having a desired overall shape, cell shape, partition wall thickness, cell density, etc. can be used.
[0043] Next, the obtained honeycomb molded body is dried and degreased to produce a honeycomb degreased body. The degreasing process is carried out at 400 to 500°C in an air atmosphere, an inert atmosphere, or a reduced pressure atmosphere. Thereafter, the honeycomb degreased body is impregnated with silicon (metallic silicon) in a reduced pressure inert gas or vacuum, and fired to obtain a honeycomb structure. As the dopant source, silicon to which a dopant has been added and / or a dopant source is added to the forming raw material, so that the concentration of the dopant in silicon in the honeycomb structure 10 is 1×10 16 ~5×10 20 pieces / cm 3 The ratio is appropriately adjusted according to the dopant element so as to satisfy the above.
[0044] As described above, a columnar honeycomb structure having cells partitioned by partition walls can be obtained by impregnating and firing the honeycomb degreased body with silicon doped with a dopant or a dopant source in the honeycomb degreased body in a reduced pressure inert atmosphere or vacuum. This impregnation and firing fills the pores in the honeycomb degreased body with molten silicon and solidifies it, making it possible to achieve a porosity of 30% or less in the honeycomb structure. Examples of the inert atmosphere include a nitrogen gas atmosphere, a rare gas atmosphere such as argon, or a mixed gas atmosphere of these. Examples of the method of impregnating and firing the silicon include a method in which a mass containing silicon and the honeycomb degreased body are placed so as to come into contact with each other and then fired.
[0045] In order to perform sufficient sintering, the firing temperature is preferably 1350° C. or higher, more preferably 1400° C. or higher, and even more preferably 1450° C. or higher. In order to reduce the manufacturing cost during firing, the firing temperature is preferably 2200° C. or lower, more preferably 1800° C. or lower, and even more preferably 1600° C. or lower.
[0046] In order to perform sufficient sintering, the heating time of the honeycomb degreased body at the above firing temperature is preferably 0.25 hours or more, more preferably 0.5 hours or more, and even more preferably 0.75 hours or more. In order to reduce the manufacturing cost during firing, the heating time of the honeycomb degreased body at the above firing temperature is preferably 5 hours or less, more preferably 4 hours or less, and even more preferably 3 hours or less.
[0047] After firing, in order to improve durability, it is preferable to carry out an oxidation treatment for 1 to 10 hours at 1000 to 1350° C. The oxidation treatment means a heat treatment in an oxidizing atmosphere (for example, in air).
[0048] Next, if necessary, a pair of electrode parts 14a, 14b may be disposed so as to face each other across the central axis of the honeycomb structure 10.
[0049] <Electrically heated carrier> 2 is a schematic cross-sectional view perpendicular to the cell extension direction of the electrically heated carrier 20 in the embodiment of the present invention. The electrically heated carrier 20 includes a honeycomb structure 10 and a pair of metal terminals 24a, 24b. The pair of metal terminals 24a, 24b are disposed so as to face each other across the central axis of the honeycomb structure 10, and are provided on a pair of electrode parts 14a, 14b, respectively, and are electrically connected. As a result, when a voltage is applied via the electrode parts 14a, 14b, the metal terminals 24a, 24b are energized, and the honeycomb structure 10 can generate heat by Joule heat. For this reason, the honeycomb structure 10 can also be suitably used as a heater.
[0050] The material of the metal terminals 24a and 24b is not particularly limited as long as it is a metal, and a single metal or an alloy can be used, but from the viewpoint of corrosion resistance, electrical resistivity, and linear expansion coefficient, it is preferable to use an alloy containing at least one selected from Cr, Fe, Co, Ni, and Ti, and stainless steel and an Fe-Ni alloy are more preferable. The shape and size of the metal terminals 24a and 24b are not particularly limited, and can be designed appropriately depending on the size and current carrying performance of the electrically heated carrier 20.
[0051] By supporting a catalyst on the electrically heated support 20, the electrically heated support 20 can be used as a catalyst body. A fluid such as automobile exhaust gas can be passed through the flow paths of the multiple cells 15. Examples of the catalyst include precious metal catalysts and other catalysts. Precious metal catalysts include three-way catalysts or oxidation catalysts in which precious metals such as platinum (Pt), palladium (Pd), and rhodium (Rh) are supported on the surface of alumina pores and include co-catalysts such as ceria and zirconia, or alkaline earth metals and platinum are used to reduce nitrogen oxides (NO x ) as a storage component of NO x Examples of catalysts that do not use precious metals include NOx storage reduction catalysts (LNT catalysts). x Examples include selective catalytic reduction catalysts (SCR catalysts). Two or more catalysts selected from these catalysts may be used. There is no particular restriction on the method of supporting the catalyst, and the method may be the same as the conventional method of supporting a catalyst on a honeycomb structure.
[0052] <Exhaust gas purification equipment> The electrically heated carrier 20 according to the embodiment of the present invention can be used in an exhaust gas purification device. The exhaust gas purification device has the electrically heated carrier 20 and a can body that holds the electrically heated carrier 20. In the exhaust gas purification device, the electrically heated carrier 20 is installed in the middle of an exhaust gas flow path for passing exhaust gas from an engine. As the can body, a metallic cylindrical member that houses the electrically heated carrier 20 can be used. EXAMPLES
[0053] The following examples are provided to better understand the present invention and its advantages, but the present invention is not limited to these examples.
[0054] [Example 1] <1. Preparation of honeycomb structure> Silicon carbide (SiC) powder with a bimodal particle size distribution was prepared as the silicon carbide raw material, and boron nitride powder was prepared as the dopant source. The silicon carbide powder and boron nitride powder were mixed to prepare a ceramic raw material. Next, methyl cellulose and hydroxypropoxyl cellulose were added as binders to the ceramic raw material, and a water-absorbent resin was added as a pore former, and water was added to prepare a molding raw material. The molding raw material was then kneaded using a vacuum kneader to prepare a cylindrical clay. The average particle size of the silicon carbide powder was 20 μm. The average particle size of the silicon carbide powder refers to the arithmetic mean diameter based on volume when the particle size frequency distribution was measured by a laser diffraction method.
[0055] The obtained cylindrical clay was molded using an extrusion molding machine with a checkerboard die structure to obtain a cylindrical honeycomb molded body in which each cell shape in the cross section perpendicular to the cell flow direction is hexagonal. This honeycomb molded body was dried by high-frequency dielectric heating, and then dried at 120°C for 2 hours using a hot air dryer to produce a dried honeycomb body.
[0056] After the dried honeycomb body was degreased, the honeycomb degreased body was impregnated with silicon (metallic silicon) doped with a dopant (boron: B) in a vacuum, and fired at 1500°C to obtain a fired honeycomb body. At this time, the concentration of the dopant in the silicon was adjusted to the values in Table 1. It was confirmed by cross-sectional observation with a scanning electron microscope (SEM) that the obtained honeycomb structure had a matrix-domain structure in which particles such as silicon carbide were domains and silicon was the matrix, and the silicon was present as a continuous layer.
[0057] <2. Formation of electrode part> Silicon carbide (SiC) powder, boron nitride powder, methyl cellulose, glycerin, and water were mixed with a centrifugal mixer to prepare an electrode forming paste. When the silicon carbide (SiC) powder was 100 parts by mass, the methyl cellulose was 0.5 parts by mass, the glycerin was 10 parts by mass, and the water was 38 parts by mass. The average particle diameter of the silicon carbide powder was 20 μm. These average particle diameters refer to the arithmetic mean diameter based on volume when the frequency distribution of particle size was measured by a laser diffraction method. Next, this electrode portion forming paste was applied to the honeycomb fired body in an appropriate area and thickness using a curved surface printing machine to prepare a honeycomb structure.
[0058] [Examples 2 to 6] A honeycomb structure was produced in the same manner as in Example 1, except that the concentration of the dopant in silicon was adjusted to the values shown in Table 1.
[0059] [Examples 7 to 14, Comparative Example 1] A honeycomb structure was prepared in the same manner as in Example 1, except that the mass ratio of silicon carbide (SiC) powder and silicon metal (Si) in the honeycomb structure was appropriately adjusted and the concentration of the dopant in the silicon was adjusted to the value in Table 1.
[0060] [Comparative Example 2] Silicon powder, silicon carbide powder, and boron nitride were mixed to prepare a ceramic raw material. Hydroxypropyl methylcellulose as a binder, a water-absorbent resin as a pore former, and water were added to the ceramic raw material to prepare a molding raw material. The molding raw material was then kneaded using a vacuum kneader to prepare a cylindrical clay. The water content was 42 parts by mass when the total of the silicon powder and silicon carbide powder was 100 parts by mass. The obtained cylindrical clay was molded using an extrusion molding machine to obtain an unfired columnar honeycomb structure part in which the cross section of each cell was a square. The unfired columnar honeycomb structure part was dried by high-frequency dielectric heating, and then dried at 120°C for 2 hours using a hot air dryer, and both bottom surfaces were cut off by a predetermined amount to obtain a honeycomb structure. Next, the dried honeycomb structure was degreased (calcined), fired, and further oxidized to obtain a honeycomb fired body. The degreasing conditions were 550°C for 3 hours. The firing conditions were 1400°C for 2 hours in an argon atmosphere. The oxidation treatment conditions were 1300°C for 1 hour.
[0061] <3.Porosity> The porosity of the honeycomb structure was measured by image analysis of the cross-sectional observation results by SEM. Specifically, from the cross-sectional observation photographs of multiple pieces (four pieces in this example and this comparative example) of the honeycomb structure obtained by SEM at a magnification of 500 times, the actual observation area was 0.08 mm 2 The above area (in this embodiment and this comparative example, 0.1 mm × 0.2 mm × 4 sheets = 0.08 mm 2 ) A total area S2 of pores in an area S1 of the honeycomb structure was determined, and the porosity of the honeycomb structure was calculated by the formula (S2 / S1)×100%.
[0062] <4.Si, SiC, SiO2 content> The composition amounts of Si, SiC, and SiO2 in the partition walls and the outer peripheral wall of the honeycomb structure were measured by the fluorescent X-ray method to measure the silicon element amount and the oxygen element amount, and the carbon element amount was measured by the resistance heating infrared absorption method. The SiC amount was calculated by assuming that all carbon elements were SiC, and calculating the SiC amount in the partition walls and the outer peripheral wall. The SiO2 amount was calculated by assuming that all oxygen elements were SiO2, and calculating the SiO2 amount in the partition walls and the outer peripheral wall. The Si amount was calculated by subtracting the total Si amount of the Si amount in SiC and the Si amount in SiO2 from the total silicon amount from the silicon amount calculated above from the SiC amount and the SiO2 amount calculated above from the silicon amount by the fluorescent X-ray method.
[0063] <5. Dopant species and amount in silicon> First, the honeycomb structure was cut along a plane perpendicular to the central axis to expose the cut surface. Next, the unevenness of the cross section of the honeycomb structure was filled with resin, and the surface filled with resin was polished. Next, the polished surface of the honeycomb structure was observed, and elemental analysis of the materials constituting the honeycomb structure was performed by energy dispersive X-ray spectroscopy (EDX analysis). Next, for the parts of the polished surface that were judged to be "silicon," whether or not the silicon contained boron was determined using the following method. First, for the parts where silicon element was detected, the parts where elements other than silicon were detected were determined to be boron by mapping using a cross-sectional structure photograph of the polished surface and an electron probe micro analyzer (EPMA analysis). Next, for the portion where only silicon element or silicon and boron were detected by EPMA analysis and determined to be "silicon", the amount of boron in silicon was identified by the following method. First, the honeycomb structure including the portion determined to be "silicon" was cut into several millimeters thick, and the cut honeycomb structure was subjected to cross-section preparation using the broad ion beam method to prepare a sample for measuring the amount of boron. The broad ion beam method is a method for preparing a sample cross-section using an argon ion beam. Specifically, a shield plate is placed directly above the sample, and a broad ion beam of argon is irradiated from above to etch the sample, thereby preparing a cross-section of the sample along the end face of the shield plate. Next, the boron in silicon of the sample whose cross-section was prepared was analyzed by time-of-flight secondary ion mass spectrometry (TOF-SIMS). In time-of-flight secondary ion mass spectrometry, a sample is first irradiated with a primary ion beam, causing secondary ions to be emitted from the surface of the sample. The emitted secondary ions are then introduced into a time-of-flight mass spectrometer to obtain a mass spectrum of the outermost surface of the sample. The sample is then analyzed using the obtained mass spectrum, and the concentration of boron in silicon [dopant amount] (particles / cm 3) was calculated by correlation between the spectral intensity of boron in silicon and a previously measured value (e.g., a calibration curve) for the concentration.
[0064] <6.Volume resistivity> The volume resistivity of the honeycomb structure was measured by a four-terminal method using a sample cut into a rod shape from the honeycomb structure, with silver paste and silver wires arranged at four positions in the axial direction.
[0065] <7. Thermal Conductivity> The thermal conductivity of the honeycomb structure was measured by measuring the thermal diffusivity using the optical AC method, the specific heat using a differential scanning calorimeter (DSC), and the true density using the Archimedes method. The product of the thermal diffusivity, specific heat, and true density measurements was taken as the thermal conductivity.
[0066] <8. Thermal shock resistance> A heating and cooling test of the honeycomb structure was carried out using a propane gas burner tester equipped with a metal case for housing the honeycomb structure and a propane gas burner capable of supplying heated gas into the metal case. The heated gas was a combustion gas generated by burning propane gas with a gas burner (propane gas burner). Then, by the heating and cooling test, it was confirmed whether or not cracks were generated in the honeycomb structure, and the thermal shock resistance was evaluated. Specifically, first, the obtained honeycomb structure was housed (canned) in the metal case of the propane gas burner tester. Then, gas (combustion gas) heated by the propane gas burner was supplied into the metal case so as to pass through the honeycomb structure. The temperature conditions (inlet gas temperature conditions) of the heated gas flowing into the metal case were as follows. First, the temperature was raised to a designated temperature in 5 minutes, and the designated temperature was held for 10 minutes, and then the temperature was cooled to 100°C in 5 minutes, and the temperature was held at 100°C for 10 minutes. This series of operations of heating, cooling, and holding is called "heating and cooling operation". After that, the honeycomb structure was checked for cracks. Then, the above "heating and cooling operation" was repeated while increasing the designated temperature from 825°C by 25°C each time. The thermal shock resistance of the honeycomb structure was evaluated based on the following evaluation criteria. Rating AA: No cracks occurred at the specified temperature of 1000°C. Rating A: No cracks occurred at the specified temperatures of 950℃ to 975℃, but cracks occurred at 1000℃. Rating B: No cracks occurred at the specified temperatures of 900℃ to 925℃, but cracks occurred at 950℃.
[0067] [Table 1]
[0068] <9. Consideration> The honeycomb structures according to Examples 1 to 14 all contained silicon carbide and silicon doped with a dopant (boron), and the porosity of the honeycomb structures was 30% or less, which resulted in low resistance and good thermal conductivity and thermal shock resistance. In Comparative Example 1, the Si content was as low as 5 mass %, resulting in high resistance. In addition, the thermal conductivity and thermal shock resistance were inferior to those of Examples 1-14. In Comparative Example 2, the porosity of the honeycomb structure exceeded 30%, so that the thermal conductivity and thermal shock resistance were inferior to those of Examples 1-14. [Explanation of symbols]
[0069] 10 Honeycomb structure 12 Peripheral wall 13 Bulkhead 14a, 14b electrode part 15 Cells 20 Electrically heated carrier 24a, 24b metal terminal 20 Electrically heated carrier
Claims
1. A ceramic honeycomb structure having an outer peripheral wall and partition walls disposed inside the outer peripheral wall and partitioning a plurality of cells that form flow paths extending from one end face to the other end face, The honeycomb structure is (1) Particles including one or more selected from silicon carbide, silicon nitride, and aluminum nitride; (2) silicon doped with a dopant; the dopant is a Group 13 element or a Group 15 element, The honeycomb structure has a silicon content (B) of 20 to 80 mass %, and the pores are filled with silicon, thereby controlling the porosity of the honeycomb structure to 30% or less.
2. 10. The honeycomb structure of claim 1, wherein the silicon is present as a continuous layer.
3. The amount of dopant (A) in the silicon is 1×10 16 ~5×10 20 pieces / cm 3 The honeycomb structure according to claim 1 or 2,
4. The honeycomb structure according to any one of claims 1 to 3, wherein 80 mass % or more of the total mass of the honeycomb structure excluding the silicon content (B) is the particles.
5. 5. The honeycomb structure according to claim 1, wherein the particles contain silicon carbide as a main component.
6. The honeycomb structure according to any one of claims 1 to 5, wherein the honeycomb structure has a volume resistivity of 0.001 to 100 Ω·cm.
7. The honeycomb structure according to any one of claims 1 to 6, wherein the honeycomb structure has a thermal conductivity of 30 W / m·K or more.
8. A honeycomb structure according to any one of claims 1 to 7, A pair of electrode portions provided on a surface of an outer peripheral wall of the honeycomb structure; Metal terminals provided on the pair of electrodes; An electrically heated carrier having
Citation Information
Patent Citations
Single side band radio receiver
JP1982035428A
Honeycomb structure, electric heating-type honeycomb structure, electric heating-type carrier and exhaust emission control device
JP2020204300A
Method for producing honeycomb structured body, method for producing si-sic-based composite material, and honeycomb structured body
WO2012132837A1
Honeycomb-type heating device and method for using same
WO2017086020A1