Thermal insulation waterproof paper

A coating layer with synthetic resin and thermally expandable microcapsules or hollow particles simplifies the process of achieving both heat retention and water resistance in cardboard boxes, ensuring effective performance and stability.

JP7594484B2Active Publication Date: 2024-12-04NIPPON PAPER IND CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2021056432
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-30
Publication Date
2024-12-04
Estimated Expiration
2041-03-30

AI Technical Summary

Technical Problem

Existing methods for imparting heat retention and water resistance to cardboard boxes are complex, often requiring separate processes and may not achieve both properties effectively, leading to manufacturing challenges and compromised performance.

Method used

A coating layer containing synthetic resin and thermally expandable microcapsules or hollow particles is applied to paper, providing both heat retention and water resistance through a simplified coating process.

Benefits of technology

The solution achieves both heat retention and water resistance in a single step, ensuring stable papermaking and effective performance without separate lamination, maintaining temperature and preventing water ingress.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007594484000002
    Figure 0007594484000002
  • Figure 0007594484000003
    Figure 0007594484000003
  • Figure 0007594484000001
    Figure 0007594484000001
Patent Text Reader

Abstract

To provide a heat-insulating waterproof paper manufactured by a method easier than conventional methods and having both of heat-insulating property and waterproof property.SOLUTION: A heat-insulating waterproof paper is provided with a coating layer involving a waterproof agent and a heat-insulating material on a paper substrate; the waterproof agent involves at least one selected from a styrenic resin, an acrylic resin, and a polyolefin-based resin, and, the heat-insulating material involves at least one selected from a hollow particle and a thermal expansion microcapsule. The heat-insulating waterproof paper is manufactured by a method that includes applying and drying a coating liquid which is a blend of a waterproof agent and a heat-insulating agent.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a heat-insulating, waterproof paper, and more specifically to a heat-insulating, waterproof paper suitable for transporting food and the like which require waterproofing and heat insulation / heat retention properties. [Background technology]

[0002] Styrofoam shipping boxes are widely used as a packaging means for transporting refrigerated and frozen foods such as fresh fish, and heated foods such as boxed lunches while keeping them warm. Styrofoam shipping boxes have the advantages of being lightweight yet highly water-resistant and insulating and heat-retaining, but because they are manufactured using forms, they require a lot of work to disassemble and dismantle after use, making it difficult to reduce their weight when discarded.

[0003] In recent years, the movement to eliminate plastic has been gaining momentum from the perspective of environmental protection, and the packaging and transportation industry is also seeking to develop alternatives to polystyrene foam. One such alternative is paper-made cardboard boxes.

[0004] Corrugated cardboard boxes can be given various functions depending on the application, one of which is heat insulation and heat retention. Methods of giving heat insulation and heat retention functions to corrugated cardboard boxes include using internal additives mainly during papermaking, coating the paper surface with heat-retaining materials, and making the cardboard box into a heat-retaining structure during processing. Patent Document 1 discloses that heat-retaining cardboard base paper is given heat insulation and heat retention performance by adding thermally expandable particle aggregates to at least the middle layer to form a foamed layer. Patent Document 2 discloses that heat-retaining cardboard base paper is given heat insulation and heat retention by applying a coating liquid containing hollow inorganic particles, thermally expandable particles, and a binder to a base paper to provide a coating layer. Patent Document 3 further discloses a cardboard box having a heat retention function by providing an inner box inside an outer box and a U-shaped opening of the inner box in the outer box so that the opening is opposite to the U-shaped opening of the outer box.

[0005] Another function that can be imparted to cardboard boxes is water resistance. Methods for imparting water resistance include coating the paper surface with a water-resistant material or covering the surface with a laminate film, such as the method of imparting water resistance by applying a water-resistant coating liquid disclosed in Patent Document 4, or the method of imparting water resistance by covering with a laminate film disclosed in Patent Document 5. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2009-133030 A [Patent Document 2] JP 2008-127703 A [Patent Document 3] JP 2018-111521 A [Patent Document 4] Japanese Patent Application Publication No. 05-025796 [Patent Document 5] JP 2002-284140 A Summary of the Invention [Problem to be solved by the invention]

[0007] These techniques have problems with the manufacturing process and process management. When manufacturing the heat-retaining base paper for cardboard described in Reference 1, which provides heat retention, the addition of a thermally expandable particle suspension makes it easier for dirt to accumulate in the papermaking system, and cumbersome management is required to ensure stable papermaking. The cardboard box described in Reference 3 can use existing paper, but the box itself has a double structure to improve heat retention, making the processing process and handling when storing items cumbersome. Furthermore, the technology described in Patent Document 5, which focuses on providing water resistance, requires a separate lamination process.

[0008] In addition, in conventional technologies, it is common to impart heat retention and water resistance separately, and when attempting to impart these functions using only coating technology, it is often impossible to ensure the desired water resistance and heat retention. The technology described in Patent Document 2 can impart heat retention by applying a coating liquid containing a heat-retaining material, but does not provide water resistance. Furthermore, the technology described in Patent Document 4 imparts water resistance to the coating liquid, but does not provide heat retention.

[0009] In view of the above circumstances, an object of the present invention is to provide paper that has both heat retention and water resistance by a method simpler than those of the prior art. [Means for solving the problem]

[0010] As a result of ingenuity, the inventors have discovered a technology for simultaneously imparting heat retention and water resistance with only a coating layer, which was previously difficult to achieve, and have arrived at the present invention. The present invention includes, but is not limited to, the following aspects. (1) A thermally insulating and waterproof paper having a paper base material and a coating layer containing at least one synthetic resin selected from the group consisting of styrene-based resin, acrylic-based resin, and polyolefin-based resin, and containing at least one type of hollow particles and thermally expandable microcapsules. (2) The coating weight of the coating layer is 4 g / m 2 The above is the heat-insulating waterproof paper described in (1). (3) The Cobb water absorption of the thermal insulation waterproof paper is 3 g / m in 120 seconds. 2 or less, or 25 g / m2 in 30 minutes 2 A thermal insulation waterproof paper according to (1) or (2) below. (4) The heat-insulating waterproof paper according to any one of (1) to (3), wherein the thermally expandable microcapsules have an outer shell of a thermoplastic resin and encapsulate a low-boiling point hydrocarbon as an expansion agent inside. (5) The heat-insulating waterproof paper according to any one of (1) to (4), characterized in that the expansion temperature of the thermally expandable microcapsules is 60° C. or higher and 120° C. or lower. (6) The heat-insulating, waterproof paper according to any one of (1) to (5), wherein the hollow particles contain an inorganic element in their outer shells. (7) The heat-insulating waterproof paper according to any one of (1) to (6), characterized in that the inside of the hollow particles is in a vacuum state. (8) The heat-insulating, waterproof paper according to any one of (1) to (7), wherein the paper base material is a multilayer paperboard. (9) A method for producing heat-retaining, waterproof paper, characterized in that a coating liquid containing a waterproofing agent containing at least one synthetic resin selected from the group consisting of styrene-based resin, acrylic-based resin, and polyolefin-based resin, and a heat-retaining agent containing at least one type of hollow particles and thermally expandable microcapsules is applied and then dried. Effect of the Invention

[0011] According to the present invention, it is possible to provide paper having a coating layer that achieves both heat retention and water resistance by a method that is simpler than conventional methods, such as a coating step alone. [Brief description of the drawings]

[0012] [Figure 1] FIG. 1 is a photograph showing the back side of a polystyrene foam lid into which a mold in which a sheet has been set is fitted, as a method for evaluating the heat retention of the sheet of the present invention. [Diagram 2] 1 is a general photograph showing a method for evaluating the heat retention of a sheet of the present invention. BEST MODE FOR CARRYING OUT THEINVENTION

[0013] The present invention relates to a heat-insulating waterproof paper. In the present invention, heat-insulating waterproof paper refers to paper that can keep the packaged contents warm and does not allow water to seep in even when exposed to water for a long period of time. In a preferred embodiment of the present invention, the heat-insulating waterproof paper of the present invention refers to a paper container that maintains the temperature inside the container even when ice is placed in the container and left for 20 hours or more, and that does not seep out of the container or deform the shape of the container even when water is placed in the container and left for three weeks, or the container shape is maintained with some deformation.

[0014] The uses of the thermal insulation waterproof paper of the present invention are not particularly limited, and it can be used, for example, as shipping boxes such as cardboard boxes with thermal insulation and cold insulation functions, individual packaging boxes for hygroscopic contents such as detergents, etc. The basis weight of the thermal insulation waterproof paper of the present invention is not particularly limited, and it can be, for example, 30 to 800 g / m 2 When the paper base material is a single-ply paper, the basis weight of the thermal insulation waterproof paper can be, for example, 30 to 350 g / m 2 50~300g / m 2 In addition, when the paper base material is a multi-layer paperboard having two or more paper layers, the basis weight of the thermal insulation waterproof paper is 75 to 800 g / m 2 200~600g / m 2 It can be said that:

[0015] In a preferred embodiment, the heat-insulating waterproof paper of the present invention has a surface Cobb water absorbency of 3 g / m 2 Less than or equal to 2 g / m 2 Less than 1 g / m is more preferable. 2 The absorbency may be less than 1 g / m when the 120-second Cobb water absorbency is measured. 2 In a preferred embodiment, the 30-minute Cobb water absorbency of the surface of the paper is less than 25 g / m2 (including the case where the paper does not absorb water and is less than the measurement limit). 2 Less than 20 g / m 2 Less than 10 g / m is more preferable. 2 In the present invention, the Cobb water absorbency is measured according to JIS P8140 (Cobb method), in which 100 ml of distilled water is brought into contact with a coating layer, and the weight of water absorbed per unit area after a specified time is measured. The lower the Cobb water absorbency is, even under conditions in which the measurement time is extended, the lower the water absorbency of the coating layer is.

[0016] (Paper base material) The thermal insulation waterproof paper of the present invention has at least a paper base material and a thermal insulation waterproof coating layer provided on at least one side of the paper base material. In the present invention, the basis weight of the paper base material is not particularly limited, and is, for example, 10 to 800 g / m 2 When the paper base material is a single-ply paper, the basis weight is 10 to 300 g / m 2For example, when the paper base material is kraft paper, the basis weight is 30 to 250 g / m 2 In addition, when the paper base material is a multi-layer paperboard having two or more paper layers, the basis weight is 70 to 800 g / m 2 For example, in the case of a cardboard liner, the basis weight is set to 80 to 600 g / m 2 The range can be set as follows:

[0017] The paper substrate used in the present invention is not particularly limited in terms of the 120-second Cobb water absorbency of the surface on which the thermal insulation and waterproof coating layer is to be formed, as long as the thermal insulation coating layer can be provided. However, it is preferably 25 g / m 2 Less than 20 g / m 2 Less than 15 g / m, more preferably 2 The paper substrate used in the present invention preferably has a 120-second Cobb water absorbency of 5 g / m 2 More preferably, 7 g / m 2 More preferably, 10 g / m 2 In the present invention, the 120-second Cobb water absorbency of the paper base material can be adjusted by applying a water repellent such as wax, and by having the 120-second Cobb water absorbency of the paper base material be in the above-mentioned range, a decrease in paper strength due to excessive penetration of the moisture contained in the solvent of the heat-retaining and waterproof paint can be prevented, and the solid content in the heat-retaining and waterproof paint can be retained on the surface of the paper layer to provide a reliable coating, thereby improving heat retention, waterproofness, and moisture resistance.

[0018] The physical properties of the paper base material are not particularly limited and can be appropriately set according to the application of the thermal insulation and waterproof paper. In the present invention, for example, the longitudinal elongation is 1.0 to 15.0%, the transverse elongation is 2.0 to 12.0%, and the specific compressive strength is 100 to 350 N·m 2 / g, specific burst strength is 2.80~5.00kPa m 2 / g, and the water contact angle of the surface on which the waterproof coating layer is to be formed is 75 degrees or more, more preferably 77 degrees or more. In a preferred embodiment, the Oken smoothness of the surface on which the coating layer is to be formed may be 13 seconds or more, more preferably 15 seconds or more, and even more preferably 17 seconds or more. There is no particular upper limit, but it is preferably 100 seconds or less, more preferably 90 seconds or less, even more preferably 80 seconds or less, and most preferably 70 seconds or less. Furthermore, the moisture permeability measured from the side on which the waterproof coating layer is to be formed may be 1500 g / m 2 - 24h or more, preferably 1750g / m 2 24h or more, preferably 2000g / m 2 The upper limit of the moisture permeability is not particularly limited, but in a preferred embodiment, it is 5000 g / m 2 - 24h or less, preferably 4500g / m 2 24h or less, more preferably 4000g / m 2 -24 hours or less is acceptable.

[0019] The raw material pulp for the paper base material can be any known one without any particular limitation.Specific examples of the raw material pulp include various pulps derived from wood fibers, such as bleached softwood kraft pulp (NBKP), bleached hardwood kraft pulp (LBKP), unbleached softwood kraft pulp (NUKP), unbleached hardwood kraft pulp (LUKP), groundwood pulp (GP), refiner ground pulp (RGP), chemical pulp (CP), thermomechanical pulp (TMP), and chemi-thermomechanical pulp (CTMP), and non-wood pulps obtained from kenaf, bagasse, bamboo, hemp, straw, etc.

[0020] The paper base material may contain recycled paper pulp or may not contain recycled paper pulp. When recycled paper pulp is contained, for example, when the paper base material is a single-layer paper, the recycled paper pulp content of the total pulp can be preferably 10% by mass or more, more preferably 25% by mass or more, even more preferably 50% by mass or more, and most preferably 70% by mass or more, and can be 100% by mass (consisting only of recycled paper-derived pulp). In addition, kraft pulp may be blended as a pulp other than recycled paper pulp, and the total amount may be kraft pulp. In addition, when the paper base material is a multi-layer paperboard having two or more paper layers, the recycled paper pulp content per layer can be as described above, and the recycled paper pulp content in each layer may be different.

[0021] Examples of waste paper pulp that can be used include waste paper pulp obtained by disintegrating unprinted waste paper such as cardboard, white, extra white, medium white, and white damage; waste paper printed on fine paper, fine coated paper, medium quality paper, medium quality coated paper, and recycled paper; and written waste paper, papers such as discarded confidential documents, waste magazines, and waste newspapers that have been disintegrated and then deinked (DIP).

[0022] In addition, in the papermaking process of the paper base material, sizing agents and water repellents can be added internally or externally, and further, a paper strength enhancing agent can be added internally to improve strength. Examples of sizing agents include rosin-based sizing agents, rosin emulsion-based sizing agents, α-carboxymethyl saturated fatty acids, neutral rosin-based sizing agents, alkyl ketene dimers (AKD), alkenyl succinic anhydrides (ASA), cationic polymer-based sizing agents, and the like. Examples of water repellents include fluorine-based resins, polyamide-based resins, waxes, and the like. Examples of paper strength enhancing agents include conventionally used paper strength enhancing agents such as polyacrylamide (PAM) and modified starch. In the present invention, it is preferable to externally add a water repellent containing wax to the side where the waterproof layer is provided, and it is more preferable to externally add a water repellent containing paraffin-based wax. The coating amount when the water repellent is externally added is 3 g / m. 2 Less than 2 g / m is preferred. 2 The following is more preferred:

[0023] If necessary, known fillers can be added to the paper base material, such as inorganic fillers such as kaolin, calcined kaolin, delaminated kaolin, clay, calcined clay, delaminated clay, illite, heavy calcium carbonate, light calcium carbonate, light calcium carbonate-silica composite, magnesium carbonate, barium carbonate, titanium dioxide, zinc oxide, silicon oxide, amorphous silica, aluminum hydroxide, calcium hydroxide, magnesium hydroxide, zinc hydroxide, and organic fillers such as urea-formaldehyde resin, polystyrene resin, and phenol resin.

[0024] Furthermore, aluminum sulfate, aluminum chloride, sodium aluminate, basic aluminum compounds, water-soluble aluminum compounds, polyvalent metal compounds, silica sol, etc. may be added internally within the limits that do not affect the quality of the paper base material.

[0025] The paper base material is produced by a known papermaking method, for example, using a Fourdrinier papermaking machine, a gap former type papermaking machine, a hybrid former type papermaking machine, an on-top former type papermaking machine, a cylinder papermaking machine, etc., but is not limited thereto.

[0026] In addition, in order to adjust the smoothness of the paper base material of the present invention, a smoothing treatment may be performed as necessary. For the smoothing treatment, a smoothing treatment device such as a normal calender, a super calender, a gloss calender, a soft calender, a thermal calender, or a shoe calender may be used. The smoothing treatment device may be appropriately adjusted in terms of the shape of the pressure device, the number of pressure nips, heating, line pressure, etc.

[0027] (Insulation and waterproof coating layer) The heat-insulating, waterproof paper of the present invention is characterized by having a heat-insulating, waterproof coating layer provided on a paper base material, and the heat-insulating, waterproof coating layer in the present invention contains a heat-insulating material, a synthetic resin, and a wax. This makes it possible to easily impart a function that combines heat-insulating and waterproof properties to the paper base material with a simpler structure than in the prior art.

[0028] The heat-insulating material used in the present invention is preferably a thermally expandable microcapsule or hollow particles. The thermally expandable microcapsule has a thermoplastic resin shell and contains a low-boiling point hydrocarbon as an expansion agent inside. The thermoplastic synthetic resin constituting the shell is not particularly limited, and examples thereof include acrylonitrile, methacrylonitrile, acrylamide, methacrylic acid or its salt, isobornyl methacrylate, dicyclopentenyl acrylate, vinylidene chloride, acrylic acid ester, etc. In addition, the low-boiling point solvent enclosed in the shell is not particularly limited, and examples thereof include isobutane, normal butane, normal pentane, isopentane, hexane, cyclohexane, heptane, petroleum ether, neopentane, propane, propylene, butene, halides of methane (methyl chloride, methylene chloride, etc.), tetraalkylsilane, etc., and two or more of them may be appropriately selected. In the present invention, when a thermally expandable microcapsule is used as a heat retaining material, it is preferable to select the foaming start temperature and maximum expansion temperature of the thermally expandable microcapsule according to the drying temperature condition of the waterproofing agent described later, and it is more preferable to select one within the range of the optimum drying temperature for expressing waterproofing performance. Specifically, the foaming start temperature of the microcapsule is preferably in the range of 60 to 120°C, more preferably 70 to 110°C, and even more preferably 75 to 105°C.

[0029] Moreover, the hollow particles are fine particles having a solid shell and a void inside (so-called balloon structure). The substance constituting the shell is not particularly limited as long as it does not impede the implementation and effects of the present invention, but is preferably an inorganic element or an inorganic compound, for example, aluminum and its compounds, silicon and its compounds, alkali metals and their compounds, Group 2 elements and their compounds, Group 4 elements and their compounds, boron and its compounds, etc., and one or more of these groups can be used. In addition, in order to enhance the effect of improving the heat retention effect, it is preferable to use hollow particles with a vacuum balloon structure in which the voids are in a vacuum state. The average particle size of the hollow particles and the average thickness of the particle shell are also not particularly limited as long as it does not impede the implementation and effects of the present invention, but hollow particles with an average particle size of 5 to 200 μm and an average shell thickness of 0.1 to 20 μm can be used.

[0030] In the present invention, when hollow particles are used as a heat retaining material, it is preferable to select a heat resistant temperature according to the drying temperature conditions of the waterproofing agent described later, and it is more preferable to select a temperature exceeding the optimum drying temperature for exhibiting waterproof performance. Specifically, the heat resistant temperature of the hollow particles is preferably 120°C or higher, more preferably 130°C or higher, and even more preferably 140°C or higher.

[0031] The synthetic resin used in the present invention preferably contains at least one of a styrene-based resin, an acrylic-based resin, and a polyolefin-based resin, and is particularly preferably a styrene-based resin and / or an acrylic-based resin.

[0032] The styrene-based resin that can be contained in the heat-retaining and waterproof coating layer constituting the present invention preferably has a copolymerization ratio of 50 mass% or more of a styrene-based monomer having a styrene skeleton in its structure, and may be composed only of a polymer of a styrene-based monomer.

[0033] Examples of the styrene monomer include styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, 2,4-dimethylstyrene, ethylstyrene, p-tert-butylstyrene, α-methylstyrene, and α-methyl-p-methylstyrene.

[0034] Examples of monomers copolymerizable with the styrene monomer include alkyl methacrylates such as methyl methacrylate, cyclohexyl methacrylate, and methylphenyl methacrylate, alkyl acrylates such as methyl acrylate, ethyl acrylate, butyl acrylate, and cyclohexyl acrylate, unsaturated carboxylic acids such as methacrylic acid and acrylic acid, unsaturated dicarboxylic anhydrides such as maleic acid and itaconic acid, unsaturated nitriles such as acrylonitrile and methacrylonitrile, and conjugated dienes such as 1,3-butadiene and 2-methyl-1,3-butadiene. These can be used alone or in combination of two or more.

[0035] The acrylic resin that can be contained in the heat-retaining and waterproof coating layer of the present invention is a resin in which the copolymerization ratio of acrylic monomers, such as acrylic acid, methacrylic acid, and their derivatives, is 50 mass% or more, and may be composed only of polymers of acrylic monomers.

[0036] Examples of the acrylic monomer include methacrylic acid esters such as cyclohexyl methacrylate, t-butylcyclohexyl methacrylate, and methyl methacrylate, and acrylic acid esters such as methyl acrylate, ethyl acrylate, butyl acrylate, and isopropyl acrylate. The acrylic resin may be a polymer of one or more monomers selected from these acrylic monomers.

[0037] Examples of monomers copolymerizable with acrylic monomers include aromatic vinyl compounds such as styrene, o-methylstyrene, p-methylstyrene, 2,4-dimethylstyrene, ethylstyrene, p-tert-butylstyrene, α-methylstyrene, and α-methyl-p-methylstyrene, unsaturated nitriles such as acrylonitrile and methacrylonitrile, maleimides such as N-phenylmaleimide and N-cyclohexylmaleimide, unsaturated dicarboxylic anhydrides such as maleic anhydride, and unsaturated carboxylic acids such as methacrylic acid and acrylic acid. These can be used alone or in combination of two or more.

[0038] In the present invention, the heat-retaining waterproof coating layer may contain wax. Examples of the wax contained in the heat-retaining waterproof coating layer include synthetic waxes such as polyethylene wax, Fischer-Tropsch wax, oil-based synthetic waxes (fatty acid esters, fatty acid amides, ketones and amines), hydrogenated oil, and natural waxes such as beeswax, wood wax, paraffin wax, and microcrystalline wax. These waxes may be used alone or in combination of two or more, and paraffin-containing hydrocarbon waxes are particularly suitable.

[0039] In the present invention, from the viewpoint of achieving both heat retention and waterproofness, it is preferable to add 0.1 to 100 parts by weight of the heat retaining material to 100 parts by weight of the waterproofing agent. The number of parts of the heat retaining material added may be more preferably 75 parts by weight or less, and further preferably 50 parts by weight or less. When 0.1 parts by weight or less of the heat retaining material is added, the heat retaining property is lost, and when 100 parts by weight or more of the heat retaining material is added, the waterproofing property is lost.

[0040] In the present invention, in order to improve the whiteness, a pigment may be contained in the heat-retaining waterproof coating layer within a range that does not impair the heat-retaining and waterproof properties. In this case, it is preferable that the whiteness of the surface of the heat-retaining and waterproof coating layer is 1% or more higher than the whiteness of the paper substrate by containing the pigment. Examples of such pigments include inorganic pigments such as calcium carbonate, titanium oxide, kaolin, clay, engineered kaolin, delaminated clay, talc, barium sulfate, calcium sulfate, zinc oxide, silicic acid, silicate salts, colloidal silica, satin white, mica, and montmorillonite, and these pigments can be used alone or in combination of two or more. Among these pigments, kaolin, calcium carbonate, or mica, which have flat particles, are particularly suitable in that they do not easily impair the moisture resistance and waterproof properties of the heat-retaining and waterproof coating layer. It is preferable that such flat inorganic pigments have an aspect ratio of 10 or more. The pigment content in the waterproof coating layer can be 5% by mass or more and 40% by mass or less, preferably 10% by mass or more and 35% by mass or less. If the pigment content is less than 5% by mass, the whiteness improvement effect is not sufficiently obtained, and if it exceeds 40% by mass, the moisture-proof and waterproof functions of the heat-retaining waterproof coating layer, which are possessed by the synthetic resin component, may not be fully exhibited, which is not preferable. In addition, other coating agents such as binders, stabilizers, defoamers, viscosity improvers, water retention agents, preservatives, colorants, etc. may be contained.

[0041] In the present invention, the heat-retaining waterproof coating layer can be formed by applying a coating agent containing the above-mentioned components onto a paper substrate and drying it. The coating amount of the heat-retaining waterproof coating layer is 4 to 20 g / m 2 It is preferable to set the thickness to 20 g / m 2 If the thickness exceeds this range, further improvements in heat retention and waterproofness cannot be expected, while the production cost may increase.

[0042] The heat-insulating waterproof paper of the present invention can be produced by coating at least one side of a paper substrate with a heat-insulating waterproof agent and drying the coated heat-insulating waterproof agent. The heat-insulating waterproof coating layer can be formed by coating the coating agent using a known coating method, and for example, coating methods such as air knife coating, curtain coating, blade coating, gate roll coating, and die coating can be used. The coating layer may be a single layer or multiple layers, and multiple coating layers may be coated sequentially, or two or more layers may be coated simultaneously by curtain coating or the like. When drying the coating layer, the coating layer temperature at the drying step outlet is preferably adjusted to be less than 120°C. The coating speed when coating the coating agent can be appropriately set in consideration of the viscosity of the coating agent and the target coating amount.

[0043] In a preferred embodiment, the coating agent is applied to the paper substrate by a contour coating method such as air knife coating or curtain coating, which allows the amount of coating agent applied to the paper substrate surface to be uniform, thus resulting in a uniform coating thickness, and suppressing the occurrence of blisters in the coating layer in the subsequent drying process. In addition, the amount of coating agent used can be reduced compared to contact coating methods, thereby reducing production costs.

[0044] The coating agent applied to the paper substrate is dried to form a coating layer. In this drying process, the coating layer temperature at the exit must be set to a drying condition that allows both thermal expansion of the heat-insulating material and suppression of blistering of the waterproofing agent. The preferred range of the coating layer temperature at the exit of the drying process is preferably 120°C or less, and may be adjusted to 100°C or less. If the coating layer temperature at the exit exceeds 120°C, the occurrence rate of blisters in the coating layer may increase, and blocking may occur in the heat-insulating waterproof paper wound up after the coating layer is formed. On the other hand, the coating layer temperature at the exit is preferably 60°C or more, more preferably 70°C, and can also be 80°C or more. If the coating layer temperature at the exit is less than 60°C, not only may blocking occur in the heat-insulating waterproof paper wound up after the coating layer is formed, but the thermal expansion of the heat-insulating material may be inhibited, and the coating layer may not be dried sufficiently to fully exhibit heat-insulating, waterproof, and moisture-proof performance. In addition, in order to achieve a balance between heat retention, waterproofness, and moisture resistance, when using thermally expandable microcapsules as the heat-retaining material, as described above, it is preferable to use thermally expandable microcapsules with a foaming start temperature of 60 to 120°C. When using microcapsules with a foaming start temperature of more than 120°C, the occurrence rate of blisters in the coating layer may increase, and waterproofness and moisture resistance, which should be compatible with heat retention, may be poor. When using hollow particles as the heat-retaining material, the heat-resistant temperature is preferably 120°C or higher, more preferably 130°C or higher, and even more preferably 140°C or higher. If the heat-resistant temperature is lower than 120°C, the heat-retaining material may be destroyed by heat during the drying process, resulting in poor heat-retaining performance.

[0045] The coating temperature at the exit of the drying process can be set in consideration of the basis weight and thickness of the paper substrate. For example, in the case of a cardboard liner in which the paper substrate is a multi-layered paperboard and has a large basis weight and thickness, blisters tend to occur more easily on the surface of the coating layer than in the case of a single-layered paper, kraft paper, which has a relatively small basis weight and thickness. The reason is not limited, but in the case of a cardboard liner, the basis weight and thickness are often larger and the air permeability is lower than that of kraft paper, and even if the moisture content of the paper is the same as that of kraft paper, it is considered that blisters tend to occur more easily on the surface of the coating layer because a large amount of moisture evaporated inside the paper substrate during the drying process cannot escape sufficiently. For this reason, the larger the basis weight and thickness of the paper substrate, the lower the coating temperature at the exit of the drying process is preferably adjusted within the above range.

[0046] Here, the outlet of the drying step refers to the outlet of the drying zone when there is one drying zone in the drying step, and refers to the outlet of the drying zone on the most downstream side when there are multiple drying zones in the drying step.

[0047] The temperature of the coating layer at the exit of the drying process can be adjusted by adjusting the drying time and the temperature of the drying zone. The drying time is determined by the feed speed of the paper substrate, the number and length of the drying zones, the equipment capacity of the drying zone (air volume, infrared output), etc. In addition, the drying method can be a known drying method, such as a steam cylinder heating drying method, a hot air drying method, a gas-type infrared drying method, an electric infrared drying method, etc., and any one of these can be used or a combination of two or more of them can be used.

[0048] The above-mentioned heat-insulating waterproof paper may be used as a cardboard liner to make cardboard boxes for storing and transporting fresh fish that require refrigerated storage. When transporting fresh fish, a large amount of ice is packed into the box together with the frozen or refrigerated fresh fish and then transported. A transport box using the heat-insulating waterproof paper obtained by the present invention has good heat retention properties, so the ice does not melt easily, and because it is waterproof, the cargo does not easily collapse even during long transports, so it is expected to contribute to saving resources and improving transport efficiency. EXAMPLES

[0049] The present invention will be illustrated by the following examples, but is not intended to limit the present invention. [Preparation of paper substrate] The paper is made of 63% softwood unbleached kraft pulp (NUKP) and 37% recycled paper pulp by mass, and has a basis weight of 280g / m2 in a three-ply papermaking process. 2 A paperboard for the liner was produced so as to have the above-mentioned shape and used as the paper base material (paper base material sample).

[0050] [Example 1]

[0051] A coating solution was prepared by mixing hollow particles (MFL-100MCA, manufactured by Matsumoto Yushi Seiyaku Co., Ltd., heat resistance temperature 150-160°C) with a waterproofing material (VAPORCOAT2200.S, manufactured by Michaelman Co., Ltd.), a mixture of styrene-based resin, acrylic-based resin, and hydrocarbon wax containing paraffin, in a solid weight ratio of 1:9. The prepared coating solution was applied using a Mayer bar at a coating amount of 10 g / m2. 2 After coating the paper substrate so as to obtain the above composition, the coating was dried in a blower dryer at 105° C. for 1 minute to obtain a heat-retaining, waterproof paper (Sample 1).

[0052] [Example 2] A coating solution was prepared by mixing ceramic vacuum balloon particles (Heatcut Powder, Toa System Create, melting point 1800°C) with a waterproofing agent (VAPORCOAT2200.S, Michaelman, Inc.), a mixture of styrene resin, acrylic resin, and hydrocarbon wax containing paraffin, in a solid weight ratio of 1:9. The coating solution was applied at a coating rate of 10 g / m2 using a Mayer bar. 2 After coating the paper substrate so as to obtain the composition as above, it was dried at 105°C for 1 minute in a blower dryer to obtain a heat-retaining, waterproof paper (Sample 2).

[0053] [Example 3] A coating solution was prepared by mixing a thermally expandable microcapsule (F-35D, manufactured by Matsumoto Yushi Seiyaku Co., Ltd.) with a waterproofing agent (VAPORCOAT2200.S, manufactured by Michaelman Co., Ltd.) in a solid weight ratio of 1:9. The coating solution was applied at a coating weight of 10 g / m2 using a Mayer bar. 2 After coating the paper substrate so as to obtain the above composition, the coating was dried in a blower dryer at 140° C. for 3 minutes to obtain a heat-retaining, waterproof paper (Sample 3).

[0054] [Example 4] A coating solution was prepared by mixing thermally expandable microcapsules (F-48D, manufactured by Matsumoto Yushi Seiyaku Co., Ltd.) with a waterproofing agent (VAPORCOAT2200.S, manufactured by Michaelman Co., Ltd.) in a solid weight ratio of 1:9. The coating solution was applied at a coating rate of 10 g / m2 using a Mayer bar. 2 After coating the paper substrate so as to obtain the above composition, the coating was dried in a blower dryer at 160° C. for 3 minutes to obtain a heat-retaining, waterproof paper (Sample 4).

[0055] [Example 5] A coating solution was prepared by mixing thermally expandable microcapsules (F-78D, manufactured by Matsumoto Yushi Seiyaku Co., Ltd.) with a waterproofing agent (VAPORCOAT2200.S, manufactured by Michaelman Co., Ltd.) in a solid weight ratio of 1:9. The coating solution was applied at a coating weight of 10 g / m2 using a Mayer bar. 2 After coating the paper substrate so as to obtain the above composition, the coating was dried in a blower dryer at 180° C. for 3 minutes to obtain a heat-retaining, waterproof paper (Sample 5).

[0056] [Comparative Example 1] A coating liquid was prepared by mixing hollow particles (MFL-100MCA, manufactured by Matsumoto Yushi Seiyaku Co., Ltd., expansion temperature: 105°C) with a coating liquid containing polyvinyl alcohol (PVA117, manufactured by Kuraray Co., Ltd.) in a solid content weight ratio of 1:9. The prepared coating liquid was applied with a Mayer bar at a coating amount of 10 g / m2. 2After coating the paper substrate so as to obtain the above composition, it was dried in a blower dryer at 105°C for 1 minute to obtain a thermal insulation cardboard base paper (Sample 6).

[0057] [Comparative Example 2] A waterproofing agent (Michaelman VAPORCOAT2200.S) made of a mixture of styrene-based resin, acrylic resin, and hydrocarbon wax containing paraffin was applied at a rate of 10 g / m using a Mayer bar. 2 After coating the paper substrate with the above composition, the coating was dried at 105° C. for 1 minute in a blower dryer to obtain waterproof paper (Sample 7).

[0058] [Evaluation method] The obtained samples were subjected to the following tests and evaluated. (1) Cobb absorbency The measurement was carried out by the Cobb method in accordance with JIS P 8140. That is, 100 ml of distilled water was brought into contact with the coating layer, and the weight of water absorbed per unit area after a specified time was measured. The measurement time was not only the usual specified time of 120 seconds (2 minutes), but also 30 minutes.

[0059] (2) Thermal conductivity The sample was cut to 50 mm x 50 mm, and eight sheets were stacked and sandwiched between graphite paper to prepare a measurement sample. The heat flux measurement sensor and the measurement sample were placed on the lower heater of the heat flux meter, and then the upper heater was lowered to press the sample. The lower heater was set to 18°C ​​and the upper heater to 42°C so that the surface of the sample was 30°C. Using the measured thermal resistance, the thermal conductivity of the sample was calculated using the following formula: Thermal conductivity (W / mK) = sample thickness (m) / thermal resistance (m 2 K / W)

[0060] (3) Heat retention The prepared samples were left to stand for 3 hours in an environment of 25°C and 50% RH, then cut to 200mm length x 150mm width, stacked on 5mm thick A-flute cardboard, fitted into a form as shown in Figure 1, and then fitted into a polystyrene foam lid with a thermometer on the top so that the sample faced the inside of the box. 2kg of chunky crushed ice was placed into the polystyrene foam container, which was then sealed with the lid fitted with the sample, and the temperature inside the box was measured every 10 minutes in an environment of 23°C and 50% humidity. (See Figure 2.) The evaluation results are shown in Table 1.

[0061] [Table 1]

[0062] From the above results, it is clear that the heat-insulating waterproof paper of the present invention (samples 1 to 5) has excellent heat-insulating and waterproof properties compared to other samples. The heat-insulating waterproof paper of the present invention can be suitably used as paper for manufacturing boxes and bags that require heat-insulating properties for food and the like and that do not leak liquids.

Claims

1. A thermal insulation waterproof paper having a coating layer containing a waterproofing agent and a thermal insulation agent provided on a paperboard, The above heat-insulating waterproof paper, wherein the waterproofing agent contains at least one synthetic resin selected from the group consisting of styrene-based resin, acrylic-based resin, and polyolefin-based resin, the heat-retaining agent contains at least one of hollow particles and thermally expandable microcapsules, and the coating layer does not contain a pigment.

2. The coating weight of the coating layer is 4 g / m 2 The heat-insulating, waterproof paper according to claim 1, wherein the weight ratio of the heat-insulating agent to the waterproof agent contained in the coating layer (heat-insulating agent / waterproof agent) is 1 / 9 or more.

3. The Cobb water absorption of the thermal insulation waterproof paper is 3 g / m in 120 seconds. 2 or less, or 25 g / m 2 The heat-insulating waterproof paper according to claim 1 or 2, which is as follows:

4. The heat-insulating waterproof paper according to any one of claims 1 to 3, wherein the Cobb water absorbency of the paperboard is 25 g / m 2 or less at 120 seconds.

5. 5. The heat-insulating waterproof paper according to claim 1, wherein the thermally expandable microcapsules have an outer shell of a thermoplastic resin and encapsulate therein a low-boiling point hydrocarbon as an expansion agent.

6. The thermally expandable microcapsules have an expansion temperature of 60° C. or higher and 120° C. or lower.

7. The heat-insulating waterproof paper according to any one of claims 1 to 6, wherein the outer shell of the hollow particle contains an inorganic element, and the inside of the hollow particle is in a vacuum state.

8. The heat-insulating and waterproof paper according to any one of claims 1 to 7, wherein the paperboard is a multi-layer paperboard.

9. A method for producing the thermal insulation waterproof paper according to any one of claims 1 to 8, comprising the steps of: The above method includes coating a coating liquid containing a waterproofing agent and a heat-retaining agent on a paperboard and then drying the coating liquid.

Citation Information

Patent Citations

  • Readily disaggregating, moisture-proof and water-proof paper and production thereof

    JP1993025796A

  • Moistureproof composition for paper coating and moistureproof paper

    JP2000129594A

  • Functional tape and panel

    JP2002052652A

  • Carton and paper box with watertightness and heat insulation

    JP2002284140A

  • Packaging method for cold / hot food container, and carton box used for packaging

    JP2004051130A