Display sealants
The display encapsulant using urethane (meth)acrylate with an aromatic ring and additional components achieves flexibility and low moisture permeability, addressing the balance of properties in flexible and curved displays.
Patent Information
- Application Number
- JP2021116482
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-07-29
- Filing Date
- 2021-07-14
- Publication Date
- 2024-12-04
- Estimated Expiration
- 2041-07-14
AI Technical Summary
Existing display encapsulants struggle to balance flexibility with low moisture permeability and adhesive strength, particularly in flexible and curved displays, as reducing crosslink density for flexibility often compromises moisture barrier properties.
A display encapsulant comprising urethane (meth)acrylate with a polyol component having an aromatic ring, combined with curable compounds, organic fillers, and specific initiators, to achieve both flexibility and low moisture permeability while maintaining excellent adhesive properties.
The encapsulant exhibits elastic moduli within preferred ranges, low moisture permeability, and high adhesive strength, suitable for flexible and curved displays, reducing peeling and damage from impact.
Smart Images

Figure 0007594503000001 
Figure 0007594503000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a sealant for displays that can be applied to flexible displays and curved displays. This sealant for displays can achieve both flexibility and low moisture permeability, and is therefore particularly useful as a sealant for flexible displays and curved displays. Furthermore, the highly flexible sealant of the present invention has excellent adhesiveness to the adherend, and is therefore useful in applications where high adhesive strength is required. [Background technology]
[0002] Examples of sealants for displays include sealants for liquid crystal displays, sealants for organic EL displays, adhesives for touch panels, etc. What these materials have in common is that they are required to have excellent curing properties, little outgassing, and no damage to display elements. Recently, displays with curved shapes and displays with high flexibility have been developed and commercialized. The substrates used in these displays are flexible, such as plastic films, instead of the conventional rigid substrates such as glass (Patent Document 1). In view of this, display sealants are increasingly being required to have the property of conforming to the bending of the substrate, etc., that is, to remain flexible even after curing.
[0003] Furthermore, a sealant having excellent flexibility is also advantageous in terms of adhesive strength. For example, peeling or damage to equipment caused by impact can be reduced. From this perspective, there is an increasing demand for sealants that have flexibility.
[0004] On the other hand, reducing the crosslink density of the cured product is an effective way to increase its flexibility. However, reducing the crosslink density usually leads to a decrease in moisture permeability. This is thought to be because moisture penetrates through the loose parts of the crosslink network of the cured product. Therefore, in order to ensure low moisture permeability, it is necessary to achieve the contradictory properties of increasing flexibility without reducing the crosslink density, or reducing the crosslink density without decreasing moisture permeability.
[0005] Conventionally, flexible adhesives for display elements have been developed from the viewpoint of improving adhesive strength (Patent Document 2). However, no adhesives having sufficient performance to be applicable to the above-mentioned flexible substrates have yet been realized. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2012-238005 A [Patent Document 2] JP 2016-24240 A Summary of the Invention [Problem to be solved by the invention]
[0007] The present invention relates to a sealant for displays that can be applied to flexible displays and curved displays. More specifically, the present invention relates to a sealant for displays that uses a urethane (meth)acrylate composed of a polyol component having an aromatic ring, and aims to provide a sealant for displays that has both flexibility and low moisture permeability and is also excellent in adhesion. [Means for solving the problem]
[0008] As a result of extensive research, the inventors discovered that a display sealant containing a urethane (meth)acrylate made of a polyol component having an aromatic ring has excellent flexibility and low moisture permeability, and thus arrived at the present invention. In this specification, "(meth)acrylate" means "acrylate" and / or "methacrylate".
[0009] That is, the present invention relates to the following [1] to
[12] . [1] A sealant for displays, comprising (A) a urethane (meth)acrylate obtained by reacting (a) a polyol having an aromatic ring, (b) an organic polyisocyanate, and (c) a hydroxyl group-containing (meth)acrylate. [2] The display sealant according to the above item [1], wherein the component (a) is a polyester polyol having an aromatic ring. [3] The sealant for displays according to the above item [2], wherein the polyester polyol having an aromatic ring comprises (a-1) a polyol and (a-2) a dibasic acid having an aromatic ring or an anhydride thereof. [4] The sealant for displays according to any one of the above [1] to [3], further comprising a component (B) a curable compound. [5] The display sealant according to the above item [4], wherein the component (B) is a partial epoxy (meth)acrylate. [6] The sealant for displays according to any one of the above [1] to [5], further comprising a component (C) an organic filler. [7] The sealant for displays according to item [6] above, wherein the component (C) is one or more organic fillers selected from the group consisting of urethane fine particles, acrylic fine particles, styrene fine particles, styrene olefin fine particles, and silicone fine particles. [8] The display sealant according to any one of items [1] to [7], further comprising a component (D) a heat curing agent. [9] The sealant for displays according to any one of items [1] to [8] above, further comprising a component (E) of a photoradical polymerization initiator.
[10] The sealant for displays according to any one of items [1] to [9] above, further comprising a component (F) of a thermal radical polymerization initiator.
[11] The sealant for displays according to item
[10] above, wherein the component (F) is a thermal radical polymerization initiator that does not contain an oxygen-oxygen bond (-OO-) or a nitrogen-nitrogen bond (-N=N-) in the molecule.
[12] The sealant for a display according to any one of items [1] to
[11] , which is a liquid crystal sealant for a liquid crystal dropping method.
[13] A liquid crystal display sealed with the liquid crystal sealant for the liquid crystal dropping method described in the preceding paragraph
[12] . Effect of the Invention
[0010] The sealant for displays of the present invention can provide a sealant for displays that has both flexibility and low moisture permeability and is also excellent in adhesion. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The display sealant of the present invention contains (A) a urethane (meth)acrylate (hereinafter also referred to simply as “component (A)”) consisting of (a) a polyol having an aromatic ring, (b) an organic polyisocyanate, and (c) a hydroxyl group-containing (meth)acrylate.
[0012] Component (A) has a flexible skeleton specific to a urethane structure, and furthermore the polyol component has an aromatic ring, so that the cured product has the characteristics of flexibility and low moisture permeability, and has high adhesive strength not only on glass substrates but also on alignment films.
[0013] The flexibility can be measured by the elastic modulus of the cured product. 2The elastic modulus of a 100 μm-thick cured product cured at 130° C. for 40 minutes after irradiation (measurement wavelength: 365 nm) is preferably 100 to 3000 MPa at room temperature (25° C.), more preferably 300 to 1900 MPa, and particularly preferably 400 to 1500 MPa. A display adhesive in the above range is preferable because it can conform to the stress applied to the display. The moisture permeability is 60g / m for a cured product with a thickness of 300μm. 2 *24h or less is preferable, 55g / m 2 *24h or less is more preferable, and 50g / m 2 *24 hours or less is especially preferred.
[0014] Component (A) can be obtained by synthesizing (a) a polyol having an aromatic ring, (b) an organic polyisocyanate, and (c) a hydroxyl group-containing (meth)acrylate in a conventional manner. It is preferable to react 1.1 to 2.0 equivalents, and particularly preferable to react 1.3 to 2.0 equivalents, of isocyanate groups in component (b) with 1 equivalent of hydroxyl groups in component (a). The reaction temperature is preferably room temperature (25°C) to 100°C. It is preferable to react 0.95 to 1.1 equivalents of hydroxyl groups in component (c) with 1 equivalent of isocyanate groups in the reaction product of component (a) and component (b). The reaction temperature is preferably room temperature (25°C) to 100°C.
[0015] Component (a) is a polyol component having an aromatic ring, and examples of the aromatic ring include aromatic hydrocarbon rings such as benzene ring, naphthalene ring, anthracene ring, and phenanthroline ring; aromatic heterocycles such as furan ring, pyrrole ring, thiophene ring, pyridine ring, thiazole ring, and benzothiazole ring; and preferably benzene ring or naphthalene ring. Component (a) is preferably a polyester polyol, and more preferably a polyester polyol consisting of (a-1) a polyol and (a-2) a dibasic acid having an aromatic ring or its anhydride. The urethane (meth)acrylate of the present invention may be used in combination with a polyol other than the component (a).
[0016] Specific examples of polyols that can be used as component (a-1) include hydrogenated polybutadiene polyol, ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, dipropylene glycol, tripropylene glycol, 1,4-butanediol, neopentyl glycol, 1,6-hexanediol, 1,8-octanediol, 1,9-nonanediol, 2-methyl-1,8-octanediol, 3-methyl-1,5-pentanediol, 2,4-diethyl-1,5-pentanediol, cyclohexane-1,4-dimethanol, polyethylene glycol, polypropylene glycol, bisphenol A poly(n≒2-20)ethoxydiol, and bisphenol A poly(n≒2-20)propoxydiol.
[0017] Examples of dibasic acids or anhydrides thereof having an aromatic ring that can be used as component (a-2) include isophthalic acid, terephthalic acid, orthophthalic acid or anhydrides thereof, etc. The urethane (meth)acrylate of the present invention may be used in combination with a dibasic acid or anhydride thereof other than component (a-2).
[0018] Specific examples of (b) organic polyisocyanates include tolylene diisocyanate, isophorone diisocyanate, 1,6-hexamethylene diisocyanate, trimethylhexamethylene diisocyanate, xylylene diisocyanate, 4,4'-diphenylmethane diisocyanate, 4,4'-cyclohexylmethane diisocyanate, xylylene diisocyanate, 1,3-bis(isocyanatomethyl)cyclohexane, trimethylhexamethylene diisocyanate, dimeryl diisocyanate, 1,5-naphthalene diisocyanate, 3,3'-dimethyl-4,4'-diphenylene diisocyanate, etc. Preferred are tolylene diisocyanate, isophorone diisocyanate, 1,6-hexamethylene diisocyanate, and trimethylhexamethylene diisocyanate, and particularly preferred is tolylene diisocyanate having an aromatic ring.
[0019] Specific examples of (c) hydroxyl group-containing (meth)acrylates include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 1,4-butanediol (meth)acrylate, polyethylene glycol mono(meth)acrylate, polypropylene glycol mono(meth)acrylate, pentaerythritol tri(meth)acrylate, ε-caprolactone adduct of 2-hydroxyethyl (meth)acrylate, 2-hydroxy-3-phenyloxypropyl (meth)acrylate, etc. Preferable examples include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, and polyethylene glycol mono(meth)acrylate.
[0020] The content of the component (A) is preferably from 5 to 50 mass %, more preferably from 10 to 40 mass %, and further preferably from 20 to 30 mass %, based on the total amount of the sealant for displays. The content of component (A) is preferably 10 to 60 mass %, more preferably 20 to 50 mass %, and further preferably 25 to 40 mass %, of the total amount of component (A) and component (B) described below.
[0021] [(B) Curable compound] The display sealant of the present invention contains a curable compound as component (B) (hereinafter, also simply referred to as "component (B)"). Component (B) is not particularly limited as long as it is a compound that is cured by light, heat, or the like, but is preferably a (meth)acrylate, such as (meth)acrylic ester, epoxy (meth)acrylate, or epoxy resin.
[0022] [(Meth)acrylate] Specific examples of (meth)acrylic esters include N-acryloyloxyethylhexahydrophthalimide, acryloylmorpholine, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, cyclohexane-1,4-dimethanol mono(meth)acrylate, tetrahydrofurfuryl (meth)acrylate, phenoxyethyl (meth)acrylate, phenylpolyethoxy (meth)acrylate, 2-hydroxy-3-phenyloxypropyl (meth)acrylate, and o-phenylphenol mono. Ethoxy (meth)acrylate, o-phenylphenol polyethoxy (meth)acrylate, p-cumylphenoxyethyl (meth)acrylate, isobornyl (meth)acrylate, tribromophenyloxyethyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate acrylate, tricyclodecane dimethanol (meth)acrylate, bisphenol A polyethoxy di(meth)acrylate, bisphenol A polypropoxy di(meth)acrylate, bisphenol F polyethoxy di(meth)acrylate, ethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, tris(acryloxyethyl)isocyanurate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, dipentaerythritol penta(meth)acrylate )acrylate, tripentaerythritol hexa(meth)acrylate, tripentaerythritol penta(meth)acrylate, trimethylolpropane tri(meth)acrylate, trimethylolpropane polyethoxytri(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, ester diacrylate of neopentyl glycol and hydroxypivalic acid, and diacrylate of an ε-caprolactone adduct of an ester of neopentyl glycol and hydroxypivalic acid.Preferred examples of the acrylates include N-acryloyloxyethylhexahydrophthalimide, phenoxyethyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, o-phenylphenol monoethoxy (meth)acrylate, and o-phenylphenol polyethoxy (meth)acrylate. Epoxy (meth)acrylate is obtained by a known method by reacting epoxy resin with (meth)acrylic acid. The epoxy resin as a raw material is not particularly limited, but is preferably a bifunctional or higher epoxy resin, such as resorcinol diglycidyl ether, bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol S type epoxy resin, phenol novolac type epoxy resin, cresol novolac type epoxy resin, bisphenol A novolac type epoxy resin, bisphenol F novolac type epoxy resin, alicyclic epoxy resin, aliphatic chain epoxy resin, glycidyl ester type epoxy resin, glycidyl amine type epoxy resin, hydantoin type epoxy resin, isocyanurate type epoxy resin, phenol novolac type epoxy resin having a triphenolmethane skeleton, and other diglycidyl etherified products of bifunctional phenols such as catechol and resorcinol, diglycidyl etherified products of bifunctional alcohols, and their halides and hydrogenated products. Among these, bisphenol A type epoxy resin and resorcinol diglycidyl ether are preferred from the viewpoint of liquid crystal contamination. Furthermore, the ratio of epoxy groups to (meth)acryloyl groups is not limited, and is appropriately selected from the viewpoint of process suitability. In addition, partial epoxy (meth)acrylates in which a portion of the epoxy groups is acrylic esterified are preferably used. In this case, the acrylic esterification rate is preferably 30 to 70%, and more preferably 40 to 60%. The (meth)acrylate may be used alone or in a mixture of two or more kinds. When the (meth)acrylate is used in the sealant for displays of the present invention, the content of the (meth)acrylate is preferably 20 to 70 mass %, more preferably 30 to 60 mass %, of the total amount of the sealant for displays.
[0023] [Epoxy resin] In a preferred embodiment of the present invention, the component (B) further contains an epoxy resin. The epoxy resin is not particularly limited, but is preferably a bifunctional or higher epoxy resin, such as resorcinol diglycidyl ether, bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol S type epoxy resin, phenol novolac type epoxy resin, cresol novolac type epoxy resin, bisphenol A novolac type epoxy resin, bisphenol F novolac type epoxy resin, alicyclic epoxy resin, aliphatic chain epoxy resin, glycidyl ester type epoxy resin, glycidyl amine type epoxy resin, hydantoin type epoxy resin, isocyanurate type epoxy resin, phenol novolac type epoxy resin having a triphenolmethane skeleton, and other diglycidyl ethers of bifunctional phenols such as catechol and resorcinol, diglycidyl ethers of bifunctional alcohols, and their halides and hydrogenated products. Among these, bisphenol A type epoxy resin and resorcinol diglycidyl ether are preferred from the viewpoint of liquid crystal contamination. The epoxy resin may be used alone or in combination of two or more kinds. When an epoxy resin is used in the sealant for displays of the present invention, the content of the epoxy resin is preferably 5 to 30 mass %, more preferably 5 to 20 mass %, of the total amount of the sealant for displays.
[0024] [(C) Organic filler] The display sealant of the present invention may contain an organic filler as component (C) (hereinafter, simply referred to as "component (C)"). Examples of the organic filler include urethane fine particles, acrylic fine particles, styrene fine particles, styrene olefin fine particles, and silicone fine particles. Examples of silicone fine particles include KMP-594, KMP-597, KMP-598 (manufactured by Shin-Etsu Chemical Co., Ltd.), Trefil RTME-5500, 9701, and EP-2001 (manufactured by Toray Dow Corning Co., Ltd.) are preferred, urethane fine particles are JB-800T and HB-800BK (manufactured by Negami Chemical Industries Co., Ltd.), and styrene fine particles are Rabalon. RTM T320C, T331C, SJ4400, SJ5400, SJ6400, SJ4300C, SJ5300C, and SJ6300C (manufactured by Mitsubishi Chemical) are preferred, and Septon is preferred as the styrene olefin fine particles. RTM SEPS2004 and SEPS2063 are preferred. These organic fillers may be used alone or in combination of two or more. Also, two or more may be used to form a core-shell structure. Among these, acrylic fine particles and silicone fine particles are preferred. When the above acrylic microparticles are used, it is preferable that the acrylic microparticles are of a core-shell structure consisting of two kinds of acrylic rubber, and it is particularly preferable that the core layer is made of n-butyl acrylate and the shell layer is made of methyl methacrylate. RTM It is sold by Aica Kogyo Co., Ltd. as F-351. Examples of the silicone fine particles include organopolysiloxane crosslinked powder and linear dimethylpolysiloxane crosslinked powder. Examples of the composite silicone rubber include the silicone rubber whose surface is coated with a silicone resin (for example, polyorganosilsesquioxane resin). Among these fine particles, particularly preferred are linear dimethylpolysiloxane crosslinked powder silicone rubber or silicone resin-coated linear dimethylpolysiloxane crosslinked powder composite silicone rubber fine particles. These may be used alone or in combination of two or more. The shape of the rubber powder is preferably spherical, which causes little increase in viscosity after addition. When component (C) is used in the display sealant of the present invention, it is preferably 1 to 30 mass % of the total amount of the display sealant, and more preferably 2 to 10 mass %.
[0025] [(D) Heat curing agent] The reactivity of the display sealant of the present invention can be improved by adding a heat curing agent as component (D) (hereinafter, also simply referred to as "component (D)"). Examples of component (D) include compounds having a carboxy group bonded to an aromatic ring in the molecule, polyamines, polyphenols, and organic acid hydrazides. However, the examples are not limited to these. Examples of the aromatic hydrazides include terephthalic acid dihydrazide, isophthalic acid dihydrazide, 2,6-naphthoic acid dihydrazide, 2,6-pyridine dihydrazide, 1,2,4-benzene trihydrazide, 1,4,5,8-naphthoic acid tetrahydrazide, and pyromellitic acid tetrahydrazide. In addition, examples of aliphatic hydrazides include formhydrazide, acetohydrazide, propionic acid hydrazide, oxalic acid dihydrazide, malonic acid dihydrazide, succinic acid dihydrazide, glutaric acid dihydrazide, adipic acid dihydrazide, pimelic acid dihydrazide, sebacic acid dihydrazide, 1,4-cyclohexane dihydrazide, tartaric acid dihydrazide, malic acid dihydrazide, iminodiacetic acid dihydrazide, N,N'-hexamethylenebissemicarbazide, citric acid trihydrazide, nitriloacetic acid trihydrazide, cyclohexanetricarboxylic acid trihydrazide, 1,3 Examples of the isocyanurate include dihydrazides having a hydantoin skeleton such as 5-bis(hydrazinocarbonoethyl)-5-isopropylhydantoin, preferably a valinehydantoin skeleton (a skeleton in which the carbon atoms of the hydantoin ring are substituted with isopropyl groups), tris(1-hydrazinocarbonylmethyl)isocyanurate, tris(2-hydrazinocarbonylethyl)isocyanurate, tris(1-hydrazinocarbonylethyl)isocyanurate, tris(3-hydrazinocarbonylpropyl)isocyanurate, and bis(2-hydrazinocarbonylethyl)isocyanurate. In view of the balance between curing reactivity and latency, preferred are isophthalic acid dihydrazide, malonic acid dihydrazide, adipic acid dihydrazide, tris(1-hydrazinocarbonylmethyl)isocyanurate, tris(1-hydrazinocarbonylethyl)isocyanurate, tris(2-hydrazinocarbonylethyl)isocyanurate, and tris(3-hydrazinocarbonylpropyl)isocyanurate, and particularly preferred is tris(2-hydrazinocarbonylethyl)isocyanurate. As component (D), it is preferable to use a compound having a carboxy group bonded to an aromatic ring in the molecule, such as 4-hydroxybenzoic acid, thiosalicylic acid, terephthalic acid, citrazinic acid, 4-aminobenzoic acid, 4-(aminomethyl)benzoic acid, and 2-mercaptonicotinic acid. Component (D) may be used alone or in combination of two or more kinds. When component (D) is used in the sealant for displays of the present invention, its content is preferably 0.1 to 10 mass %, more preferably 0.1 to 5 mass %, of the total amount of the sealant for displays.
[0026] The display sealant of the present invention can further improve its reactivity by adding a curing catalyst. Examples of the curing catalyst include amines and imidazoles, with imidazoles being particularly preferred. Examples of imidazoles include 2-methylimidazole, 2-phenylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-phenylimidazole, 1-benzyl-2-methylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole, 2,4-diamino-6(2'-methylimidazole(1'))ethyl-s-triazine, and 2,4-diamino-6(2'-undecylimidazole(1')). Ethyl-s-triazine, 2,4-diamino-6(2'-ethyl-4-methylimidazole(1'))ethyl-s-triazine, 2,4-diamino-6(2'-methylimidazole(1'))ethyl-s-triazine·isocyanuric acid adduct, 2-methylimidazole isocyanuric acid 2:3 adduct, 2-phenylimidazole isocyanuric acid adduct, 2-phenyl-3,5-dihydroxymethylimidazole, 2-phenyl-4-hydroxymethyl-5-methylimidazole, 1-cyanoethyl-2-phenyl-3,5-dicyanoethoxymethylimidazole, etc.
[0027] [(E) Photoradical polymerization initiator] The display sealant of the present invention may contain a photoradical polymerization initiator (hereinafter, simply referred to as "component (E)") as component (E). The photoradical polymerization initiator is not particularly limited as long as it is a compound that generates radicals or acids and initiates a chain polymerization reaction when irradiated with ultraviolet light or visible light, and examples of the photoradical polymerization initiator include benzyl dimethyl ketal, 1-hydroxycyclohexyl phenyl ketone, diethylthioxanthone, benzophenone, 2-ethylanthraquinone, 2-hydroxy-2-methylpropiophenone, 2-methyl-[4-(methylthio)phenyl]-2-morpholino-1-propane, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, camphorquinone, 9-fluorenone, and diphenyl disulfide. Specifically, IRGACURE RTM 651, 184, 2959, 127, 907, 369, 379EG, 819, 784, 754, 500, OXE01, OXE02, OXE03, OXE04, DAROCURE RTM 1173, LUCIRIN RTM TPO (both manufactured by BASF), Seikuol RTM Z, BZ, BEE, BIP, BBI (all manufactured by Seiko Chemical Co., Ltd.), Kayacure DETX-S (manufactured by Nippon Kayaku Co., Ltd.), etc. Among these, preferred are IRGACURE, an oxime ester initiator. RTM OXE01, OXE02, OXE03, OXE04, and the thioxanthone initiator Kayacure DETX-S. Furthermore, the combined use of an oxime ester initiator and a thioxanthone initiator is preferable because it is possible to achieve both immediate curing and curing in light-shielded areas and also to cure with visible light. When the component (E) is used in the sealant for displays of the present invention, its content is usually from 0.001 to 3 mass %, preferably from 0.01 to 2 mass %, based on the total amount of the sealant for displays.
[0028] [(F) Thermal radical polymerization initiator] The display sealant of the present invention contains a thermal radical polymerization initiator (F) (hereinafter, also simply referred to as "component (F)"), which can improve the curing speed and curing properties. The thermal radical polymerization initiator is not particularly limited as long as it is a compound that generates radicals by heating and initiates a chain polymerization reaction. Examples of the thermal radical polymerization initiator include organic peroxides, azo compounds, benzoin compounds, benzoin ether compounds, acetophenone compounds, and benzopinacol. Benzopinacol is preferably used. For example, an organic peroxide is KAYAMEK. RTM A, M, R, L, LH, SP-30C, Perkadox CH-50L, BC-FF, Kadox B-40ES, Perkadox 14, Trigonox RTM 22-70E, 23-C70, 121, 121-50E, 121-LS50E, 21-LS50E, 42, 42LS, Kayaester RTM P-70, TMPO-70, CND-C70, OO-50E, AN, Kayabutyl RTM B, Percadox 16, Kayacarvone RTM BIC-75, AIC-75 (manufactured by Kayaku Akzo Co., Ltd.), Permec RTM N, H, S, F, D, G, Perhexa RTM H,HC,TMH,C,V,22,MC,Percure RTM AH, AL, HB, Perbutyl RTM H, C, N.D., L, Park Mill RTM H.D. Perloyle RTM IB, IPP, Perocta RTM ND (manufactured by NOF Corporation) and other products are available commercially.
[0029] In addition, as azo compounds, VA-044, 086, V-070, VPE-0201, VSP-1001 (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), etc. are available as commercially available products.
[0030] The preferred component (F) is a thermal radical polymerization initiator that does not have an oxygen-oxygen bond (-OO-) or a nitrogen-nitrogen bond (-N=N-) in the molecule. Thermal radical polymerization initiators that have an oxygen-oxygen bond (-OO-) or a nitrogen-nitrogen bond (-N=N-) in the molecule emit a large amount of oxygen or nitrogen when radicals are generated, and therefore may harden while leaving air bubbles in the liquid crystal sealant, resulting in a decrease in adhesive strength, a decrease in moisture permeability, and a decrease in properties under humid and hot environments. Benzopinacol-based thermal radical polymerization initiators (including those chemically modified from benzopinacol) are particularly suitable. Specifically, benzopinacol, 1,2-dimethoxy-1,1,2,2-tetraphenylethane, 1,2-diethoxy-1,1,2,2-tetraphenylethane, 1,2-diphenoxy-1,1,2,2-tetraphenylethane, 1,2-dimethoxy-1,1,2,2-tetra(4-methylphenyl)ethane, 1,2-diphenoxy-1,1,2,2-tetra(4-methoxyphenyl)ethane, 1,2 -Bis(trimethylsiloxy)-1,1,2,2-tetraphenylethane, 1,2-bis(triethylsiloxy)-1,1,2,2-tetraphenylethane, 1,2-bis(t-butyldimethylsiloxy)-1,1,2,2-tetraphenylethane, 1-hydroxy-2-trimethylsiloxy-1,1,2,2-tetraphenylethane, 1-hydroxy-2-triethylsiloxy-1,1,2,2-tetraphenylethane Examples of the tert-butyldimethylsiloxy-1,1,2,2-tetraphenylethane include 1-hydroxy-2-trimethylsiloxy-1,1,2,2-tetraphenylethane, 1-hydroxy-2-triethylsiloxy-1,1,2,2-tetraphenylethane, 1-hydroxy-2-t-butyldimethylsiloxy-1,1,2,2-tetraphenylethane, and 1,2-bis(trimethylsiloxy)-1,1,2,2-tetraphenylethane. More preferred are 1-hydroxy-2-trimethylsiloxy-1,1,2,2-tetraphenylethane and 1,2-bis(trimethylsiloxy)-1,1,2,2-tetraphenylethane, and particularly preferred is 1,2-bis(trimethylsiloxy)-1,1,2,2-tetraphenylethane. The above-mentioned benzopinacol is commercially available from Tokyo Chemical Industry Co., Ltd., Fujifilm Wako Pure Chemical Industries, Ltd., and the like. The hydroxy group of benzopinacol can be easily etherified by a known method. The hydroxy group of benzopinacol can be silyl-etherified by heating the corresponding benzopinacol and various silylating agents under a basic catalyst such as pyridine. Examples of the silylating agent include commonly known trimethylsilylating agents such as trimethylchlorosilane (TMCS), hexamethyldisilazane (HMDS), and N,O-bis(trimethylsilyl)trifluoroacetamide (BSTFA), triethylchlorosilane (TECS) as a triethylsilylating agent, and t-butylmethylsilane (TBMS) as a t-butyldimethylsilylating agent. These reagents can be easily obtained from the market, such as silicon derivative manufacturers. The reaction amount of the silylating agent is preferably 1.0 to 5.0 times the moles per mole of the hydroxy group of the target compound. More preferably, it is 1.5 to 3.0 times the moles. If the molar ratio is less than 1.0, the reaction efficiency is poor and the reaction time is long, which promotes thermal decomposition, whereas if the molar ratio is more than 5.0, separation during recovery is poor and purification becomes difficult.
[0031] The content of the component (F) is preferably from 0.0001 to 10 mass %, more preferably from 0.0005 to 3 mass %, and particularly preferably from 0.001 to 1 mass %, based on the total amount of the display sealant of the present invention.
[0032] [(O) Other components] The display sealant of the present invention may further contain additives such as inorganic fillers, silane coupling agents, radical polymerization inhibitors, pigments, leveling agents, antifoaming agents, and solvents, if necessary.
[0033] [Inorganic filler] Examples of the inorganic filler include silica, silicon carbide, silicon nitride, boron nitride, calcium carbonate, magnesium carbonate, barium sulfate, calcium sulfate, mica, talc, clay, alumina, magnesium oxide, zirconium oxide, aluminum hydroxide, magnesium hydroxide, calcium silicate, aluminum silicate, lithium aluminum silicate, zirconium silicate, barium titanate, glass fiber, carbon fiber, molybdenum disulfide, asbestos, etc., and preferably includes fused silica, crystalline silica, silicon nitride, boron nitride, calcium carbonate, barium sulfate, calcium sulfate, mica, talc, clay, alumina, aluminum hydroxide, calcium silicate, and aluminum silicate, and more preferably silica, alumina, and talc. Two or more of these inorganic fillers may be mixed and used. If the average particle size of the inorganic filler is too large, it may cause defects such as poor gap formation when bonding upper and lower glass substrates together during the manufacture of narrow-gap liquid crystal display cells, so it is appropriate that the average particle size of the inorganic filler is 2000 nm or less, preferably 1000 nm or less, and more preferably 300 nm or less. The preferred lower limit is about 10 nm, and more preferably about 100 nm. The particle size can be measured using a laser diffraction / scattering type particle size distribution measuring device (dry type) (LMS-30, manufactured by Seishin Enterprise Co., Ltd.). In the display sealant of the present invention, when an inorganic filler is used, the inorganic filler is usually contained in an amount of 5 to 50 mass %, preferably 5 to 40 mass % of the total amount of the display sealant. If the content of the inorganic filler is less than 5 mass %, the adhesive strength to the glass substrate is decreased, and the moisture resistance reliability is also poor, so that the adhesive strength after moisture absorption may also be significantly decreased. If the content of the inorganic filler is more than 50 mass %, the filler content is too high, so that the liquid crystal cell may not be easily crushed and may not be able to form a gap.
[0034] [Silane coupling agents] Examples of the silane coupling agent include 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, N-phenyl-γ-aminopropyltrimethoxysilane, N-(2-aminoethyl)3-aminopropylmethyldimethoxysilane, N-(2-aminoethyl)3-aminopropylmethyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-mercaptopropyltrimethoxysilane, vinyltrimethoxysilane, N-(2-(vinylbenzylamino)ethyl)3-aminopropyltrimethoxysilane hydrochloride, 3-methacryloxypropyltrimethoxysilane, 3-chloropropylmethyldimethoxysilane, 3-chloropropyltrimethoxysilane, etc. These silane coupling agents are sold by Shin-Etsu Chemical Co., Ltd. and others as the KBM series, KBE series, etc., and are therefore easily available on the market. When a silane coupling agent is used in the sealant for displays of the present invention, the content thereof is preferably 0.05 to 3 mass % based on the total amount of the sealant for displays.
[0035] [Radical polymerization inhibitor] The radical polymerization inhibitor is not particularly limited as long as it is a compound that reacts with radicals generated from a photoradical polymerization initiator or a thermal radical polymerization initiator to prevent polymerization, and may be a quinone, piperidine, hindered phenol, nitroso, etc. Specifically, naphthoquinone, 2-hydroxynaphthoquinone, 2-methylnaphthoquinone, 2-methoxynaphthoquinone, 2,2,6,6-tetramethylpiperidine-1-oxyl, 2,2,6,6-tetramethyl-4-hydroxypiperidine-1-oxyl, 2,2,6,6-tetramethyl-4-methoxypiperidine-1-oxyl, 2,2,6,6-tetramethyl-4-phenoxypiperidine-1-oxyl, or hydroquinone. , 2-methylhydroquinone, 2-methoxyhydroquinone, parabenzoquinone, butylated hydroxyanisole, 2,6-di-t-butyl-4-ethylphenol, 2,6-di-t-butylcresol, stearyl β-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, 2,2'-methylenebis(4-ethyl-6-t-butylphenol), 4,4'-thiobis(3-methyl-6-t-butylpheno 4,4'-butylidenebis(3-methyl-6-t-butylphenol), 3,9-bis[1,1-dimethyl-2-[β-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy]ethyl], 2,4,8,10-tetraoxaspiro[5,5]undecane, tetrakis-[methylene-3-(3',5'-di-t-butyl-4'-hydroxyphenylpropionate)methane], 1,3,5-trimethylphenylpropionate, Examples of the aluminum salt of tris(3',5'-di-t-butyl-4'-hydroxybenzyl)-sec-triazine-2,4,6-(1H,3H,5H)trione, paramethoxyphenol, 4-methoxy-1-naphthol, thiodiphenylamine, N-nitrosophenylhydroxyamine, trade names Adeka STAB LA-81 and Adeka STAB LA-82 (manufactured by Adeka Corporation), but are not limited to these.Among these, naphthoquinone-based, hydroquinone-based, nitroso-based, and piperazine-based radical polymerization inhibitors are preferred, naphthoquinone, 2-hydroxynaphthoquinone, hydroquinone, 2,6-di-tert-butyl-p-cresol, and Polystop 7300P (manufactured by Hakuto Co., Ltd.) are more preferred, and Polystop 7300P (manufactured by Hakuto Co., Ltd.) is most preferred. The content of the radical polymerization inhibitor is preferably from 0.0001 to 1 mass %, more preferably from 0.001 to 0.5 mass %, and particularly preferably from 0.01 to 0.2 mass %, based on the total amount of the sealant for displays of the present invention.
[0036] An example of a method for obtaining the display sealant of the present invention is the following method. First, components (B) and (E) are heated and dissolved in component (A) as necessary. After cooling to room temperature, components (C), (D), and (F), an inorganic filler, a silane coupling agent, an antifoaming agent, a leveling agent, a solvent, and the like are added as necessary, and the mixture is mixed uniformly using a known mixing device such as a three-roll mill, a sand mill, or a ball mill, and filtered through a metal mesh to produce the display sealant of the present invention.
[0037] The display sealant of the present invention is also very useful as an adhesive for liquid crystal display cells, particularly as a liquid crystal sealant. An example of a liquid crystal display cell in which the display sealant of the present invention is used as a liquid crystal sealant is shown below.
[0038] The liquid crystal display cell manufactured by using the adhesive for liquid crystal display cells of the present invention is a cell in which a pair of substrates, each having a predetermined electrode formed thereon, are arranged facing each other at a predetermined interval, the periphery is sealed with the liquid crystal sealant of the present invention, and liquid crystal is sealed in the gap. The type of liquid crystal to be sealed is not particularly limited. Here, the substrate is composed of a combination of substrates made of glass, quartz, plastic, silicon, etc., at least one of which is optically transparent. The manufacturing method thereof is to add a spacer (gap control material) such as glass fiber to the liquid crystal sealant of the present invention, apply the liquid crystal sealant to one of the pair of substrates using a dispenser or a screen printing device, etc., and then temporarily cure at 80 to 120°C as necessary. Thereafter, liquid crystal is dropped on the inside of the dam of the liquid crystal sealant, and the other glass substrate is superimposed in a vacuum to form a gap. After the gap is formed, the liquid crystal display cell of the present invention can be obtained by curing at 90 to 130°C for 30 minutes to 2 hours. When used as a photothermal combined type, the liquid crystal sealant is irradiated with ultraviolet light by an ultraviolet irradiator to photocure it. The amount of ultraviolet light irradiation is preferably 500 to 6000 mJ / cm 2 , more preferably 1000 to 4000 mJ / cm 2 The irradiation dose is preferably 100 nm (measurement wavelength: 365 nm). Thereafter, if necessary, the liquid crystal display cell of the present invention can be obtained by curing at 90 to 130° C. for 30 minutes to 2 hours. The liquid crystal display cell of the present invention thus obtained is free from display defects due to liquid crystal contamination and has excellent adhesion and moisture resistance reliability. Examples of spacers include glass fiber, silica beads, polymer beads, etc. The diameter of the spacer varies depending on the purpose, but is usually 2 to 8 μm, preferably 4 to 7 μm. The amount of the spacer used is usually 0.1 to 4 parts by mass, preferably 0.5 to 2 parts by mass, and more preferably about 0.9 to 1.5 parts by mass, based on 100 parts by mass of the liquid crystal sealant of the present invention.
[0039] The display sealant of the present invention is very suitable for use as an adhesive in fields requiring curability, adhesion to different adherends, and reliable resistance to moisture and heat, such as liquid crystal sealants, organic electroluminescence sealants, and adhesives for touch panels. EXAMPLES
[0040] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. In the text, "parts" and "%" are by mass unless otherwise specified.
[0041] [Synthesis Example 1] In a flask equipped with a thermometer, a cooling tube, and a stirrer, 351.25 g of polyester polyol of 1,9-nonanediol, methyl octanediol, and adipic acid (O-1010 manufactured by Kuraray Co., Ltd., hydroxyl value 113.5 mg KOH / g), 347.88 g of polyester polyol of methyl pentanediol, adipic acid, and isophthalic acid (P-1012 manufactured by Kuraray Co., Ltd., hydroxyl value 114.6 mg KOH / g), and 197.99 g of toluene diisocyanate (Coronate T-100 manufactured by Tosoh Corporation, molecular weight 174.2) were charged and reacted at 80 ° C. The isocyanate content at this time was determined by adding an excess of amine and back titrating with hydrochloric acid, and it was confirmed that the value was within the range of plus or minus 2% of the residual amount of isocyanate determined from the calculated value. Next, 0.6 g of methoquinone (polymerization inhibitor), 101.98 g of 2-hydroxyethyl acrylate (molecular weight 116.1), and 0.3 g of dibutyltin dilaurate (catalyst) were added, and the mixture was stirred at 80°C. The absorption spectrum of the isocyanate group (2280 cm) was measured by infrared absorption spectroscopy. -1 The reaction was continued until the amine group 1 had disappeared, yielding a urethane acrylate oligomer having a weight average molecular weight of 6,900.
[0042] [Synthesis Example 2] A flask equipped with a thermometer, a cooling tube, and a stirrer was charged with 352.06 g of polycaprolactone diol (Daicel Corporation, Plaxel 210, hydroxyl value 113.1 mg KOH / g), 347.45 g of polyester polyol of methyl pentanediol, adipic acid, and isophthalic acid (Kuraray Corporation, P-1012, hydroxyl value 114.6 mg KOH / g), and 197.74 g of toluene diisocyanate (Tosoh Corporation, Coronate T-100, molecular weight 174.2), and reacted at 80 ° C. The isocyanate content at this time was determined by adding an excess of amine and back titrating with hydrochloric acid, and it was confirmed that the value was within the range of plus or minus 2% of the residual amount of isocyanate determined from the calculated value. Next, 0.6 g of methoquinone (polymerization inhibitor), 101.85 g of 2-hydroxyethyl acrylate (molecular weight 116.1), and 0.3 g of dibutyltin dilaurate (catalyst) were added, and the mixture was stirred at 80°C. The absorption spectrum of the isocyanate group (2280 cm) was measured by infrared absorption spectroscopy. -1 The reaction was continued until the amine group 1 had disappeared, yielding a urethane acrylate oligomer having a weight average molecular weight of 5,200.
[0043] [Synthesis Example 3] In a flask equipped with a thermometer, a cooling tube, and a stirrer, 776.99 g of polyester polyol (P-2012, manufactured by Kuraray Co., Ltd., hydroxyl value 54.6 mg KOH / g) of methyl pentanediol, adipic acid, and isophthalic acid, and 131.68 g of toluene diisocyanate (Coronate T-100, manufactured by Tosoh Corporation, molecular weight 174.2) were charged and reacted at 80 ° C. The isocyanate content at this time was determined by adding an excess of amine and back titrating with hydrochloric acid, and it was confirmed that the value was within the range of ± 2% of the residual amount of isocyanate calculated from the calculated value. Next, 0.6 g of methoquinone (polymerization inhibitor), 90.43 g of 2-hydroxyethyl acrylate (molecular weight 116.1), and 0.3 g of dibutyltin dilaurate (catalyst) were added, and the mixture was stirred at 80 ° C., and the absorption spectrum of the isocyanate group (2280 cm) was measured by infrared absorption spectroscopy. -1 The reaction was continued until the amine group 1 had disappeared, yielding a urethane acrylate oligomer having a weight average molecular weight of 6,300.
[0044] [Synthesis Example 4] In a flask equipped with a thermometer, a cooling tube, and a stirrer, 654.56 g of polycaprolactone diol (Daicel Corporation, PLACCEL 210, hydroxyl value 113.1 mg KOH / g) and 241.97 g of isophorone diisocyanate (Evonik, VESTANAT IPDI, molecular weight 222.3) were charged and reacted at 80 ° C. The isocyanate content at this time was determined by adding an excess of amine and back titrating with hydrochloric acid, and it was confirmed that the value was within ± 2% of the residual amount of isocyanate calculated from the calculated value. Next, 0.6 g of methoquinone (polymerization inhibitor), 102.57 g of 2-hydroxyethyl acrylate (molecular weight 116.1), and 0.3 g of dibutyltin dilaurate (catalyst) were added, and the mixture was stirred at 80 ° C., and the absorption spectrum of the isocyanate group (2280 cm) was measured by infrared absorption spectroscopy. -1 The reaction was continued until the amine group 1 had disappeared, yielding a urethane acrylate oligomer having a weight average molecular weight of 5,600.
[0045] [Synthesis Example 5] A flask equipped with a thermometer, a condenser, and a stirrer was charged with 724.7 g of polyester polyol of methylpentanediol and sebacic acid (P-2050 manufactured by Kuraray Co., Ltd., hydroxyl value 58.1 mgKOH / g), 31.56 g of tricyclodecane dimethanol (TCD Alcohol DM manufactured by Celanese, molecular weight 196.3), and 178.73 g of isophorone diisocyanate (VESTANAT IPDI manufactured by Evonik, molecular weight 222.3), and reacted at 80° C. The isocyanate content at this time was determined by adding an excess of amine and back titrating with hydrochloric acid, and it was confirmed that the value was within the range of ±2% of the residual amount of isocyanate determined from the calculated value. Next, 0.6 g of methoquinone (polymerization inhibitor), 64.11 g of 2-hydroxyethyl acrylate (molecular weight 116.1), and 0.3 g of dibutyltin dilaurate (catalyst) were added, and the mixture was stirred at 80°C. The absorption spectrum of the isocyanate group (2280 cm) was measured by infrared absorption spectroscopy. -1 The reaction was continued until the amine group 11100 disappeared, to obtain a urethane acrylate oligomer having a weight average molecular weight of 11100.
[0046] [Synthesis Example 6] 100 parts (0.28 moles) of commercially available benzopinacol (Tokyo Chemical Industry Co., Ltd.) was dissolved in 350 parts of dimethylformaldehyde. 32 parts (0.4 moles) of pyridine as a base catalyst and 150 parts (0.58 moles) of BSTFA (Shin-Etsu Chemical Co., Ltd.) as a silylating agent were added to the mixture, which was then heated to 70°C and stirred for 2 hours. The resulting reaction solution was cooled and 200 parts of water was added while stirring to precipitate the product and deactivate the unreacted silylating agent. The precipitated product was separated by filtration and thoroughly washed with water. The resulting product was then dissolved in acetone, and recrystallized by adding water, followed by purification. 105.6 parts (yield 88.3%) of the desired 1,2-bis(trimethylsiloxy)-1,1,2,2-tetraphenylethane was obtained.
[0047] [Examples 1 to 6, Comparative Examples 1 to 4] Components (A), (B), and (O) were mixed in the ratios shown in Table 1 below, and component (E) was heated to 90°C to dissolve. The mixture was then cooled to room temperature, and components (C), (D), (F), and (O) were added and stirred. The mixture was then dispersed using a three-roll mill and filtered through a metal mesh (635 mesh) to prepare a sealant for displays.
[0048] [evaluation] [Adhesive strength] An alignment film liquid (Nissan Chemical Co., Ltd.: NRB-U738) was spin-coated on a glass substrate, pre-baked on a hot plate at 80°C for 3 minutes, and then baked in an oven at 230°C for 30 minutes. Furthermore, this substrate with the alignment film was irradiated with a UV irradiator at 500 mJ / cm 2 The material was then irradiated with ultraviolet light (measurement wavelength: 254 nm) and baked in an oven at 230° C. for 30 minutes. 100 g of the sealant for displays manufactured in the examples and comparative examples is mixed and stirred with 1 g of 5 μm glass fiber as a spacer. This sealant for displays is applied to a glass substrate coated with an alignment film in a shape reproducing a 1 cm x 1 cm corner area, and the opposing alignment film-coated substrate is bonded together, and the substrate is irradiated with 3000 mJ / cm by a UV irradiator. 2After irradiating with ultraviolet light (measurement wavelength: 365 nm), the glass substrate was placed in an oven and thermally cured at 130°C for 40 minutes. The peel adhesion strength of the alignment film-coated glass substrate was measured by pressing the corners with a bond tester (SS-30WD, manufactured by Seishin Shoji Co., Ltd.). The strength is shown in Table 1. [Moisture permeability] The display sealants produced in the examples and comparative examples were sandwiched between polyethylene terephthalate (PET) films to form thin films with a thickness of 300 μm, and then irradiated with a UV irradiator at 3000 mJ / cm. 2 After irradiating with ultraviolet light (measurement wavelength: 365 nm), the sample was placed in an oven and thermally cured at 130°C for 40 minutes. After curing, the PET film was peeled off to obtain a sample. The moisture permeability of the sample at 60°C and 90% humidity was measured using a moisture permeability measuring device (Lessy: L80-5000). The results are shown in Table 1. Elasticity Modulus The display sealants produced in the examples and comparative examples were sandwiched between polyethylene terephthalate (PET) films to form thin films with a thickness of 100 μm, and then irradiated with a UV irradiator at 3000 mJ / cm 2 After irradiating with ultraviolet light (measurement wavelength: 365 nm), the sample was placed in an oven and thermally cured at 130°C for 40 minutes. After curing, the PET film was peeled off to obtain a sample. The sample was subjected to a tensile test at room temperature (25°C) at a test speed of 5 mm / min using a Tensilon universal testing machine (manufactured by A&D Co., Ltd., RTG-1210) and measured. The results are shown in Table 1.
[0049] [Table 1]
[0050] TIFF0007594503000002.tif103153
[0051] From the results in Table 1, it was confirmed that the sealant for displays of the present invention has both flexibility and low moisture permeability, and also has excellent adhesive strength. [Industrial Applicability]
[0052] The sealant for displays of the present invention has excellent adhesive strength with an adherend and is compatible with flexibility and low moisture permeability, and is therefore useful as a sealant for displays, flexible displays, and curved displays, which require particularly good adhesion to organic films.
Claims
1. A sealant for displays, comprising (A) a urethane (meth)acrylate obtained by reacting (a) a polyol having an aromatic ring, (b) an organic polyisocyanate, and (c) a hydroxyl group-containing (meth)acrylate, a partial epoxy (meth)acrylate, and (F) a thermal radical polymerization initiator, The sealant for displays, wherein the (a) polyol having an aromatic ring is a polyester polyol made of methylpentanediol, adipic acid, and isophthalic acid.
2. The sealant for displays according to claim 1, wherein the moisture permeability of the cured product, when measured at 60°C and 90%, is 60 g / m 2 ·24 h or less when the film thickness is 300 μm.
3. The sealant for displays according to claim 1 or 2, further comprising a component (C) an organic filler.
4. 4. The display sealant according to claim 3, wherein the component (C) is one or more organic fillers selected from the group consisting of urethane fine particles, acrylic fine particles, styrene fine particles, styrene olefin fine particles, and silicone fine particles.
5. The sealant for displays according to claim 1 , further comprising a component (D) a heat curing agent.
6. The sealant for displays according to claim 1 , further comprising a component (E) a photoradical polymerization initiator.
7. 7. The display sealant according to claim 1, wherein the component (F) is a thermal radical polymerization initiator that does not contain an oxygen-oxygen bond (-O-O-) or a nitrogen-nitrogen bond (-N=N-) in the molecule.
8. The sealant for a display according to claim 1 , which is a liquid crystal sealant for a liquid crystal dropping method.
9. A liquid crystal display sealed with the liquid crystal sealant for the liquid crystal dropping method according to claim 8.
Citation Information
Patent Citations
Liquid crystal sealant and liquid crystal display cell using the same
JP2009015129A
Display device
JP2012238005A
Liquid crystal sealant and liquid crystal cell using the same
JP2016024240A
Liquid crystal sealant and liquid crystal cell using the same
JP2016024243A