Nonwoven fabrics and sanitary materials
By integrating amino-modified silicone and olefin polymers, nonwoven fabrics achieve enhanced moist feeling and reduced friction, addressing the texture issues in existing fabrics.
Patent Information
- Application Number
- JP2022539578
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-07-31
- Filing Date
- 2021-07-29
- Publication Date
- 2024-12-04
- Estimated Expiration
- 2041-07-29
AI Technical Summary
Nonwoven fabrics used in absorbent articles lack an optimal moist feeling, despite having adequate flexibility and strength.
Incorporation of amino-modified silicone with a nitrogen mass fraction of 2000 μg/g or more, along with specific friction coefficients and olefin polymer fibers, to enhance the moist feeling without compromising flexibility and strength.
The nonwoven fabrics exhibit improved moist feeling, reduced friction, and enhanced sliding properties, resulting in a smoother and more comfortable touch.
Smart Images

Figure 0007594594000001 
Figure 0007594594000002
Abstract
Description
[Technical field]
[0001] The present disclosure relates to nonwoven fabrics and sanitary materials. [Background technology]
[0002] In recent years, nonwoven fabrics have been widely used for various purposes due to their excellent breathability and flexibility. Representative uses of nonwoven fabrics include absorbent articles such as disposable diapers, sanitary napkins, and incontinence pads, sanitary masks, medical gauzes, and base fabrics for compresses.
[0003] For example, nonwoven fabrics used in absorbent articles are required to have flexibility, a pleasant feel when used such as a touch, strength such as resistance to breakage, etc. As a method for producing nonwoven fabrics that is unlikely to cause a decrease in the breaking strength of the nonwoven fabric and can stably produce nonwoven fabrics that are pleasant to the touch, a method for producing nonwoven fabrics that includes a step of applying a fabric softener to a spunbonded nonwoven fabric or a laminated nonwoven fabric of a spunbonded layer and a meltblown layer, and a step of partially stretching each of a plurality of positions of the nonwoven fabric at a temperature of 50° C. or less has been proposed (for example, see Patent Document 1). [Patent Document 1] Patent No. 5878309 Summary of the Invention [Problem to be solved by the invention]
[0004] The nonwoven fabric produced by the method disclosed in Patent Document 1 has room for improvement in terms of texture, such as moist feeling.
[0005] The present disclosure aims to provide a nonwoven fabric that has an excellent moist feeling, and a sanitary material that contains this nonwoven fabric. [Means for solving the problem]
[0006] Means for solving the above problems include the following embodiments. <1> A nonwoven fabric containing amino-modified silicone having a nitrogen mass fraction of 2000 (μg / g) or more. <2> The content of the amino-modified silicone is 10.00% by mass or less based on the total amount of the nonwoven fabric. <1> The nonwoven fabric described in <3> The content of the amino-modified silicone is 5.00% by mass or less based on the total amount of the nonwoven fabric. <2> The nonwoven fabric described in <4> A nonwoven fabric, in which the ratio of the coefficient of static friction between fibers (μs) to the coefficient of kinetic friction between fibers (μk), μs / μk, is 1.20 or less, and the coefficient of static friction between fibers is 0.40 or less. <5> Contains olefin polymer fibers <1> ~ <4> 13. The nonwoven fabric according to claim 12 . <6> The olefin-based polymer includes at least one selected from the group consisting of a propylene-based polymer and an ethylene-based polymer. <5> The nonwoven fabric described in <7> The olefin-based polymer includes the propylene-based polymer, and the propylene-based polymer includes at least one selected from the group consisting of a propylene homopolymer and a propylene / α-olefin copolymer. <6> The nonwoven fabric described in <8> It is a long fiber nonwoven fabric with a fineness of 0.5 denier to 3.0 denier. <1> ~ <7> 13. The nonwoven fabric according to claim 12 . <9> Contains amide compounds <1> ~ <8> 13. The nonwoven fabric according to claim 12 . <10> Contains crimped fibers <1> ~ <9> 13. The nonwoven fabric according to claim 12 . <11> <1> ~ <10> A sanitary material comprising the nonwoven fabric according to any one of the above items. Effect of the Invention
[0007] The present disclosure can provide a nonwoven fabric having an excellent moist feeling, as well as a sanitary material containing this nonwoven fabric. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] The present invention will be described in detail below. The following description of the configuration elements may be based on representative embodiments of the present invention, but the present disclosure is not limited to such embodiments.
[0009] In the present disclosure, the term "step" refers not only to an independent step, but also to a step that cannot be clearly distinguished from other steps, as long as the purpose of the step is achieved. In the present disclosure, the content of each component in a composition means, when multiple substances corresponding to each component are present in the composition, the total amount of those multiple substances present in the composition, unless otherwise specified.
[0010] In addition, in this disclosure, a numerical range expressed using "to" means a range that includes the numerical values before and after "to" as the lower limit and upper limit. In the numerical ranges described in the present disclosure in stages, the upper or lower limit value described in one numerical range may be replaced with the upper or lower limit value of another numerical range described in stages. In addition, in the numerical ranges described in the present disclosure, the upper or lower limit value of the numerical range may be replaced with a value shown in the examples. In the present disclosure, combinations of two or more preferred embodiments are more preferred embodiments.
[0011] [Nonwoven fabric] The nonwoven fabric of the present disclosure contains an amino-modified silicone having a nitrogen mass fraction of 2000 (μg / g) or more (hereinafter also referred to as "specific amino-modified silicone"), which gives the nonwoven fabric of the present disclosure an excellent moist feel.
[0012] In the nonwoven fabric of the present disclosure, the specific amino-modified silicone can function as a lubricant. Examples of the specific amino-modified silicone include side-chain type amino-modified silicone, both-end type amino-modified silicone, and both-end type side-chain amino-modified silicone. Examples of the side-chain type amino-modified silicone include monoamine type and diamine type. The specific amino-modified silicone may be used alone or in combination of two or more types.
[0013] From the viewpoint of obtaining a nonwoven fabric having an even more excellent moist feeling, the nitrogen mass fraction in the specific amino-modified silicone is preferably 2300 (μg / g) or more, more preferably 2500 (μg / g) to 8000 (μg / g), and even more preferably 3000 (μg / g) to 7000 (μg / g).
[0014] The nonwoven fabric of the present disclosure may or may not contain an amino-modified silicone other than the specific amino-modified silicone. In the nonwoven fabric of the present disclosure, the content of the specific amino-modified silicone contained in the amino-modified silicone is preferably 50% by mass to 100% by mass, more preferably 70% by mass to 100% by mass, and even more preferably 90% by mass to 100% by mass, from the viewpoint of obtaining a nonwoven fabric with an even more excellent moist feeling.
[0015] In the nonwoven fabric of the present disclosure, from the viewpoint of obtaining a nonwoven fabric with a more excellent moist feeling, the content of the specific amino-modified silicone is preferably 10.00 mass% or less, more preferably 5.00 mass% or less, even more preferably 1.00 mass% or less, particularly preferably 0.01 mass% to 0.80 mass%, and even more preferably 0.05 mass% to 0.70 mass%, based on the total amount of the nonwoven fabric. In particular, by having the content of the specific amino-modified silicone be 1.00 mass% or less, the stickiness of the surface of the nonwoven fabric tends to be suppressed.
[0016] From the viewpoint of moist feeling of the nonwoven fabric, the functional group equivalent of the specific amino-modified silicone is preferably 500 g / mol to 7000 g / mol, more preferably 1000 g / mol to 6000 g / mol, and even more preferably 1500 g / mol to 4000 g / mol. In the present disclosure, the term "functional group equivalent" refers to the molecular weight per amino group in a compound.
[0017] The kinetic viscosity of the specific amino-modified silicone at 25°C is set to 300 mm from the viewpoint of moisturizing the nonwoven fabric. 2 / s or more is preferable, and 1000 mm 2 / s~4000mm 2 / s is more preferable, and 1500 mm 2 / s~4000mm 2 The specific amino-modified silicone has a kinematic viscosity of 1000 mm / s at 25° C. 2 / s may be exceeded.
[0018] A nonwoven fabric means a fabric in which fibers are intertwined without being woven, and the nonwoven fabric of the present disclosure also contains fibers. The nonwoven fabric of the present disclosure preferably contains fibers of a thermoplastic polymer.
[0019] Examples of the thermoplastic polymer constituting the fibers include olefin-based polymers, polyester-based polymers, polyamide-based polymers, thermoplastic polymer compositions containing a plurality of these polymers, etc. The nonwoven fabric of the present disclosure preferably contains fibers of an olefin-based polymer.
[0020] An olefin-based polymer is a polymer that mainly contains structural units derived from an olefin, a polyester-based polymer is a polymer that contains polyester as a structural unit, and a polyamide-based polymer is a polymer that contains polyamide as a structural unit. In the present disclosure, the terms "mainly comprise" and "mainly comprise" mean that the target substance is contained in the largest amount relative to the whole. For example, the content of the target substance relative to the whole is 50% by mass or more.
[0021] The olefin-based polymer preferably contains at least one selected from the group consisting of propylene-based polymers and ethylene-based polymers. The olefin-based polymer may be a homopolymer of an olefin or a copolymer of two or more kinds of olefins. The copolymer of two or more kinds of olefins may be a block copolymer or a random copolymer.
[0022] The propylene-based polymer is a polymer mainly composed of structural units derived from propylene, and is a concept including propylene homopolymers and copolymers of propylene and α-olefins other than propylene (propylene / α-olefin copolymers). For example, it may be either a propylene homopolymer or a copolymer of propylene and α-olefins other than propylene, or it may include both. The propylene / α-olefin copolymer is preferably, for example, a copolymer of propylene and one or more α-olefins having 2 to 10 carbon atoms other than propylene, and more preferably a copolymer of propylene and one or more α-olefins having 2 to 8 carbon atoms other than propylene.
[0023] In terms of excellent flexibility, specific examples of preferred α-olefins to be copolymerized with propylene include ethylene, 1-butene, 1-pentene, 1-hexene, 1-octene, 1-decene, 3-methyl-1-butene, 3-methyl-1-pentene, 3-ethyl-1-pentene, 4-methyl-1-pentene, and 4-methyl-1-hexene. Examples of propylene / α-olefin copolymers include propylene-ethylene copolymers and propylene-ethylene-1-butene copolymers. The content of the structural unit derived from the α-olefin in the propylene / α-olefin copolymer is not particularly limited, and is preferably, for example, 1 mol% to 10 mol%, and more preferably 1 mol% to 5 mol%. The propylene-based polymer may be one type of propylene-based polymer, or a combination of two or more types of propylene-based polymers.
[0024] In the present disclosure, when a copolymer of propylene and an α-olefin other than propylene has an equal content of propylene-derived structural units and an equal content of ethylene-derived structural units, such a copolymer is classified as a propylene-based polymer.
[0025] The ethylene-based polymer is a polymer mainly composed of structural units derived from ethylene, and is a concept including ethylene homopolymers and copolymers of ethylene and α-olefins other than ethylene. For example, it may be either an ethylene homopolymer or a copolymer of ethylene and α-olefins other than ethylene (ethylene / α-olefin copolymer). The ethylene / α-olefin copolymer is preferably, for example, a copolymer of ethylene and one or more α-olefins having 2 to 10 carbon atoms other than ethylene.
[0026] From the viewpoint of excellent flexibility, specific examples of α-olefins copolymerized with ethylene include propylene, 1-butene, 1-pentene, 1-hexene, 1-octene, 1-decene, 3-methyl-1-butene, 3-methyl-1-pentene, 3-ethyl-1-pentene, 4-methyl-1-pentene, and 4-methyl-1-hexene. Examples of ethylene / α-olefin copolymers include ethylene-propylene copolymers and ethylene-1-butene copolymers. The content of the structural unit derived from α-olefin in the ethylene / α-olefin copolymer is not particularly limited, and is preferably, for example, 1 mol% to 10 mol%, and more preferably 1 mol% to 5 mol%. The ethylene-based polymer may be one type of ethylene-based polymer, or a combination of two or more types of ethylene-based polymers.
[0027] The olefin polymer preferably includes a propylene polymer. The melting point (Tm) of the propylene polymer is preferably 125° C. or higher, more preferably 125° C. to 165° C. From the viewpoint of spinnability, the melt flow rate (MFR) of the propylene polymer (ASTM D-1238, 230° C., load 2,160 g) is preferably 10 g / 10 min to 100 g / 10 min, more preferably 20 g / 10 min to 70 g / 10 min.
[0028] The melting point (Tm) of the propylene-based polymer can be measured using a differential scanning calorimeter (DSC). Using a differential scanning calorimeter (DSC), the sample is heated to a temperature about 50°C higher than the temperature at which the melting endothermic curve reaches its extreme value when the sample is heated at a rate of 10°C / min, and is then held at this temperature for 10 minutes. The sample is then cooled to 30°C at a rate of 10°C / min, and the melting curve is measured when the sample is heated again to a predetermined temperature at a rate of 10°C / min. From the melting curve, the temperature (Tp) at which the melting endothermic curve reaches its extreme value can be determined according to the method of ASTM D3418, and the endothermic peak at the peak temperature can be determined as the melting point (Tm).
[0029] The fibers contained in the nonwoven fabric of the present disclosure may be fibers containing one type of thermoplastic polymer, or may be composite fibers containing two or more types of thermoplastic polymers. Examples of composite fibers include islands-in-the-sea type, side-by-side type, concentric core-sheath type, and eccentric core-sheath type. Eccentric core-sheath type composite fibers may be exposed type in which the core is exposed on the surface, or non-exposed type in which the core is not exposed on the surface.
[0030] The fibers contained in the nonwoven fabric of the present disclosure may be crimped fibers or non-crimped fibers. The non-crimped fibers may be, for example, eccentric core-sheath type crimped composite fibers.
[0031] When the composite fiber is a concentric core-sheath type, an eccentric core-sheath type, or the like, the mass ratio of the sheath portion to the core portion (core portion / sheath portion) is, for example, preferably 95 / 5 to 5 / 95, more preferably 90 / 10 to 10 / 90, and further preferably 90 / 10 to 40 / 60.
[0032] The nonwoven fabric of the present disclosure is preferably a long-fiber nonwoven fabric having a fineness of 0.5 denier to 3.0 denier, more preferably a long-fiber nonwoven fabric having a fineness of 0.8 denier to 2.5 denier, and even more preferably a long-fiber nonwoven fabric having a fineness of 1.0 denier to 2.2 denier.
[0033] The nonwoven fabric of the present disclosure preferably has a ratio of μs / μk between the static friction coefficient between fibers (μs) and the kinetic friction coefficient between fibers (μk) of 1.20 or less. By reducing the ratio of the static friction coefficient between fibers to the kinetic friction coefficient between fibers, there is a tendency for snagging at the initial stage of sliding to be suppressed. Furthermore, when the skin touching the nonwoven fabric rubs against the nonwoven fabric and the relative positions of the two change, there is a tendency for a smooth nonwoven fabric to be obtained with less roughness and sliminess. Furthermore, due to the good sliding between the fibers of the nonwoven fabric, there is a tendency for the drapeability to be good.
[0034] In the nonwoven fabric of the present disclosure, μs / μk may be 1.18 or less, 1.15 or less, or 1.10 or less. The lower limit of μs / μk is not particularly limited, and may be 0.90 or more, 0.95 or more, or from the viewpoint of flexibility, 1.00 or more.
[0035] In the nonwoven fabric of the present disclosure, from the viewpoint of moist feeling, μs is preferably 0.40 or less, and from the viewpoint of softness, μs is preferably 0.37 or less, more preferably 0.35 or less, and even more preferably 0.33 or less.
[0036] In the nonwoven fabric of the present disclosure, μk is not particularly limited, and is, for example, preferably 0.40 or less, more preferably 0.35 or less, and even more preferably 0.30 or less.
[0037] From the viewpoint of softness, the nonwoven fabric of the present disclosure preferably has a lower value of at least one of μs and μk, and more preferably has a lower value of μs and μk, compared to a nonwoven fabric made of the same fibers that does not contain the specific amino-modified silicone (hereinafter also referred to as a "comparative nonwoven fabric"). The fact that the μs, μk, etc. of the nonwoven fabric containing the specific amino-modified silicone are lower than the μs, μk, etc. of the comparative nonwoven fabric may be confirmed, for example, by removing the specific amino-modified silicone by applying a solvent to the nonwoven fabric containing the specific amino-modified silicone.
[0038] The reduction rate of μs (μs1) of the nonwoven fabric of the present disclosure relative to μs (μs2) of the comparative nonwoven fabric ([(μs2-μs1) / μs2]×100) and the reduction rate of μk (μk1) of the nonwoven fabric of the present disclosure relative to μk (μk2) of the comparative nonwoven fabric ([(μk2-μk1) / μk2]×100) are each independently preferably from 10% to 70%, and more preferably from 19% to 47%.
[0039] The difference (μs2-μs1) between μs (μs2) of the comparative nonwoven fabric and μs (μs1) of the nonwoven fabric of the present disclosure, and the difference (μk2-μk1) between μk (μk2) of the comparative nonwoven fabric and μk (μk1) of the nonwoven fabric of the present disclosure are each independently preferably 0.05 to 0.3, and more preferably 0.07 to 0.2.
[0040] <Additives> The nonwoven fabric of the present disclosure may contain, as optional components, various known additives such as antioxidants, heat stabilizers, weather stabilizers, antistatic agents, slip agents, anti-fogging agents, dyes, pigments, natural oils, synthetic oils, waxes, and amide compounds, provided that the addition of these additives does not impair the object of the present invention.
[0041] The nonwoven fabric of the present disclosure may contain an amide compound. The amide compound may function as a lubricant. Examples of the amide compound include fatty acid amides, such as fatty acid amides having 15 to 22 carbon atoms. It is believed that the fatty acid amides having 15 to 22 carbon atoms adsorbed on the fiber surface of the nonwoven fabric modify the fiber surface, thereby improving flexibility, touch, blocking resistance, etc., and more effectively suppressing adhesion of the fibers to members such as various rotating devices in the device used in the embossing process, etc.
[0042] In the present disclosure, the number of carbon atoms in a fatty acid amide means the number of carbon atoms contained in the molecule, and the carbon atoms constituting the amide bond are also included in the above carbon number. The fatty acid amide preferably has 18 to 22 carbon atoms. Examples of fatty acid amides having 15 to 22 carbon atoms include fatty acid monoamide compounds, fatty acid diamide compounds, saturated fatty acid monoamide compounds, and unsaturated fatty acid diamide compounds. Among these, preferred examples include palmitic acid amide (number of carbon atoms: 16), stearic acid amide (number of carbon atoms: 18), oleic acid amide (number of carbon atoms: 18), erucic acid amide (number of carbon atoms: 22), etc.
[0043] The content of the amide compound is preferably 0.1 to 5.0% by mass, more preferably 0.1 to 3.0% by mass, and even more preferably 0.1 to 1.0% by mass, based on the total amount of the nonwoven fabric. The nonwoven fabric may contain only one type of amide compound, or may contain two or more types of amide compounds.
[0044] The basis weight of the nonwoven fabric of the present disclosure is not particularly limited. From the viewpoint of achieving both flexibility and strength, a basis weight of 30 g / m 2 It is preferable that the thickness is less than 25 g / m 2 More preferably, it is 5 g / m or less. 2 ~20g / m 2 It is even more preferable that:
[0045] The nonwoven fabric of the present disclosure may be a single-layer nonwoven fabric, a nonwoven fabric laminate consisting of two or more layers of nonwoven fabric, or a nonwoven fabric laminate including the nonwoven fabric of the present disclosure and a layer other than the nonwoven fabric of the present disclosure. The layer other than the nonwoven fabric of the present disclosure may be a single layer or two or more layers.
[0046] The type of nonwoven fabric of the present disclosure is not particularly limited, and examples thereof include various nonwoven fabrics such as spunbond nonwoven fabrics, meltblown nonwoven fabrics, carded air-through nonwoven fabrics, airlaid nonwoven fabrics, needle punched spunbond nonwoven fabrics, wet-laid nonwoven fabrics, dry pulp nonwoven fabrics, flash spun nonwoven fabrics, spread fiber nonwoven fabrics, etc. Among these, the nonwoven fabric of the present disclosure is preferably a spunbond nonwoven fabric.
[0047] Examples of layers other than the nonwoven fabric of the present disclosure include knitted fabrics, woven fabrics, nonwoven fabrics other than the nonwoven fabric of the present disclosure (hereinafter also referred to as "other nonwoven fabrics"), films, etc. Examples of other nonwoven fabrics include the various nonwoven fabrics described above.
[0048] The method for forming the nonwoven fabric laminate is not particularly limited, and various methods can be used, such as heat fusion methods such as thermal embossing and ultrasonic fusion, mechanical entanglement methods such as needle punching and water jet, methods using adhesives such as hot melt adhesives and urethane adhesives, and extrusion lamination.
[0049] The nonwoven fabric laminate is preferably partially heat-sealed. When a portion of the nonwoven fabric laminate is heat-sealed, various known heat-sealing methods (for example, a method using ultrasonic means, a heat embossing process using an embossing roll, or hot air through) can be used.
[0050] When a portion of the nonwoven fabric laminate is heat-fused by thermal embossing, the embossed area ratio is usually preferably 5% to 30%, and more preferably 5% to 20%. Examples of the stamp shape include a circle, an ellipse, an oval, a square, a diamond, a rectangle, a square, and a continuous shape based on these shapes.
[0051] When hot embossing is performed, the embossing temperature depends on the line speed, pressure during embossing, etc., but is generally preferably in the range of 85°C to 150°C.
[0052] (Modification) In a modified example, the nonwoven fabric of the present disclosure may have a ratio of μs / μk between the static friction coefficient (μs) and the kinetic friction coefficient (μk) between fibers of 1.20 or less, and the static friction coefficient between fibers of 0.40 or less.
[0053] In the nonwoven fabric according to the modified example, the ratio μs / μk between the static friction coefficient between fibers (μs) and the kinetic friction coefficient between fibers (μk) is 1.20 or less, and the static friction coefficient between fibers is 0.40 or less. As a result, the nonwoven fabric of the present disclosure has excellent moist feeling. The reason for this is presumed to be as follows. The value of the static friction coefficient between fibers is reduced, and the ratio of the static friction coefficient between fibers to the kinetic friction coefficient between fibers is also reduced, thereby suppressing snagging at the initial stage of sliding. Furthermore, when the skin touching the nonwoven fabric rubs against the nonwoven fabric and the relative positions of the two change, a smooth nonwoven fabric is obtained with little roughness or sliminess. Furthermore, the good sliding between the fibers of the nonwoven fabric tends to improve drapeability.
[0054] In the nonwoven fabric according to the modified example, μs / μk may be 1.20 or less, and may be, for example, 1.18 or less, 1.15 or less, or 1.10 or less. The lower limit of μs / μk is not particularly limited, and may be 0.90 or more, 0.95 or more, or from the viewpoint of flexibility, may be 1.00 or more.
[0055] In the nonwoven fabric according to the modified example, μs is 0.40 or less, and from the viewpoint of softness, μs is preferably 0.37 or less, more preferably 0.35 or less, and even more preferably 0.33 or less.
[0056] In the nonwoven fabric according to the modified example, μk is not particularly limited as long as μs / μk is 1.20 or less and μs is 0.40 or less. For example, μk is preferably 0.40 or less, more preferably 0.35 or less, and even more preferably 0.30 or less.
[0057] A preferred embodiment of the nonwoven fabric according to the modified example may be an appropriate combination of the configuration of the nonwoven fabric of the present disclosure and the preferred configuration of the nonwoven fabric of the present disclosure described above. For example, the nonwoven fabric according to the modified example may or may not contain the specific amino-modified silicone described above.
[0058] (Nonwoven fabric manufacturing method) The method for producing the nonwoven fabric of the present disclosure is not particularly limited, and the nonwoven fabric can be produced by a conventional method depending on the type of nonwoven fabric. For example, when the nonwoven fabric of the present disclosure is a spunbonded nonwoven fabric, it can be produced by the following method. The composition constituting the fibers is melted using an extruder, and the molten composition is melt-spun using a spunbonded nonwoven fabric molding machine having multiple spinnerets. The fibers are stretched using a blower or the like, and the long fibers formed by spinning are cooled as necessary. Thereafter, the fibers are deposited on the collecting surface of the spunbonded nonwoven fabric molding machine, and are heated and pressurized with an embossing roll.
[0059] [Hygiene materials] The sanitary material of the present disclosure includes the nonwoven fabric of the present disclosure described above. Examples of sanitary materials include absorbent articles such as disposable diapers, sanitary napkins, and incontinence pads, medical sanitary materials such as bandages, medical gauze, and towels, sanitary masks, etc. The sanitary material of the present disclosure is not limited to these, and may also be suitably used for other sanitary material applications. The sanitary material may include a nonwoven fabric laminate consisting of two or more layers of the nonwoven fabric of the present disclosure, or may include a nonwoven fabric laminate containing the nonwoven fabric of the present disclosure and a layer other than the nonwoven fabric of the present disclosure. EXAMPLES
[0060] Hereinafter, the embodiment of the present invention will be described in more detail based on examples. However, the present invention is not limited to these examples, which are one embodiment of the present invention. The physical properties of each of the examples and comparative examples were measured by the following methods. The evaluation results are shown in Tables 1 and 2.
[0061] (1) Weight [g / m 2 〕 Ten test pieces measuring 100 mm in the machine direction (MD) and 100 mm in the cross direction (CD) were taken from the nonwoven fabric laminate. The test pieces were taken from 10 locations in the CD direction. The mass (g) of each test piece was then measured using a top-pan electronic balance (Kensei Kogyo Co., Ltd.) in an environment of 23°C and 50% relative humidity. The average mass of each test piece was calculated. A 1m deviation was calculated from the calculated average.2 The weight per unit area of the spunbond nonwoven fabric is calculated by converting the weight per unit area (g) and rounding off to the nearest whole number. 2 〕.
[0062] (2) Nitrogen mass fraction The nitrogen mass fraction of approximately 3 mg to 5 mg of amino-modified silicone oil was measured using a TN-110 trace total nitrogen analyzer manufactured by Mitsubishi Chemical Analytech Co., Ltd. (currently Nitto Seiko Analytech Co., Ltd.) at a combustion furnace temperature of 900°C. The measurement was performed three times, and the average value of the results was used.
[0063] (3) Coefficient of static friction between fibers μs and coefficient of kinetic friction between fibers μk The friction tester TL201Ts manufactured by Trinity Lab Co., Ltd. was used to measure the inter-fiber static friction coefficient μs and inter-fiber dynamic friction coefficient μk in the nonwoven fabric laminate. A 40 mm (MD) × 12 mm (CD) test piece taken from the obtained nonwoven fabric laminate was attached to the attached urethane contact with a fingerprint pattern, and a 250 mm (MD) × 40 mm (CD) test piece was taken from the obtained nonwoven fabric laminate and placed on the stage so that the sliding direction was the MD of the test piece. The measurement conditions were a temperature of 23 ± 2 ° C, a humidity of 40 ± 5%, a load of 50 gf, and a sliding speed of 100 mm / sec, and the inter-fiber dynamic friction coefficient μk and the inter-fiber static friction coefficient μs corresponding to the peak of the friction coefficient at the beginning of sliding were obtained. The measurement was performed three times, and the average value of the obtained results was used.
[0064] (4) Texture evaluation Five researchers who handle nonwoven fabrics were gathered as sensory testers, and nonwoven fabric laminates (20 cm x 25 cm) of each Example and Comparative Example were prepared on a table. The sensory testers were asked to evaluate the tactile sensation of the nonwoven fabric laminates of each Example and Comparative Example based on the following evaluation criteria. At this time, the nonwoven fabric laminate of Comparative Example 5, which was not coated with a lubricant, was given a score of 1, which was used as the standard. The scores of the five sensory testers for each Example and Comparative Example were averaged to obtain the evaluation value for the tactile sensation. The moist feeling of the nonwoven fabric laminate was evaluated based on the feeling of little roughness, smoothness, and moderate sliminess. The temperature during the evaluation was 23°C to 23.5°C, and the humidity was 38% to 43%. -Evaluation criteria- Score 1: The feel was equivalent to that of the nonwoven fabric laminate of Comparative Example 5. 2 points: Slightly more moist than the nonwoven fabric laminate of Comparative Example 5. 3 points: The moist feeling is superior to that of the nonwoven fabric laminate of Comparative Example 5. 4 points: Much better moist feeling than the nonwoven fabric laminate of Comparative Example 5. 5 points: Much better moist feeling than the nonwoven fabric laminate of Comparative Example 5.
[0065] Example 1 <Nonwoven fabric manufacturing> A propylene homopolymer (h-PP) with a melt flow rate (ASTM D-1238, 230°C, load 2,160 g) of 60 g / 10 min and a melting point of 162°C was melt spun by the spunbond method and deposited on a collection surface to obtain a 7.5 g nonwoven web made of fibers. The average fiber diameter of this fiber was 2.0d (denier). Two layers of nonwoven fabric webs were stacked to form a laminated web having two nonwoven fabric web layers, and the first nonwoven fabric web layer was brought into contact with an elliptical embossing roll with an embossed convex area of 18% and the second nonwoven fabric layer was brought into contact with a mirror roll, and the layers were heat-pressed at 145°C to obtain a nonwoven fabric laminate. The total basis weight of the nonwoven fabric laminate was 15 g / m 2 It was.
[0066] A side-chain diaminosilicone with a nitrogen mass fraction of 3300 μg / g (Shin-Etsu Chemical Co., Ltd. KF869, kinematic viscosity at 25°C of 1500 mm 2 / s) was diluted with normal hexane to obtain an amino-modified silicone solution with a concentration of 0.25% by mass. The amino-modified silicone solution was applied uniformly to the obtained nonwoven fabric laminate. The physical properties of the nonwoven fabric laminate obtained by applying the amino-modified silicone solution were measured according to the methods described above. The amount of the amino-modified silicone applied to the nonwoven fabric laminate was calculated using the following formula (1) and was found to be 0.50 mass%. [(mass of nonwoven fabric after application (g) - mass of nonwoven fabric before application (g)) / mass of nonwoven fabric before application (g)] × concentration of amino-modified silicone solution (mass%) (1)
[0067] Example 2 In Example 1, the side-chain diamino silicone (Shin-Etsu Chemical Co., Ltd. KF869) was replaced with a side-chain diamino silicone having a nitrogen mass fraction of 6900 μg / g (Shin-Etsu Chemical Co., Ltd. KF861, kinematic viscosity at 25° C. of 3500 mm 2 A nonwoven fabric laminate having an amino-modified silicone attached thereto was obtained in the same manner as in Example 1, except that the composition was changed to (1 / s).
[0068] Example 3 In Example 1, the side-chain diamino silicone (Shin-Etsu Chemical Co., Ltd. KF869) was replaced with a side-chain diamino silicone having a nitrogen mass fraction of 3700 μg / g (Shin-Etsu Chemical Co., Ltd. KF864, kinematic viscosity at 25° C. of 1700 mm 2 A nonwoven fabric laminate having an amino-modified silicone attached thereto was obtained in the same manner as in Example 1, except that the composition was changed to (1 / s).
[0069] Example 4 A nonwoven fabric laminate was obtained in the same manner as in Example 2, except that the nonwoven fabric web layer was changed as follows. A mixture of propylene polymer (h-PP) (75% by mass) with MFR 60g / 10min and melting point 162°C and propylene-ethylene random copolymer (r-PP) (25% by mass) with MFR 60g / 10min, melting point 142°C, ethylene content 4% by mass, and erucic acid amide (2000 ppm) was melt spun by the spunbond method, and a first nonwoven fabric web (first layer) made of fibers was deposited on a moving collection surface. A mixture of propylene polymer (h-PP) (75% by mass) with MFR 60g / 10min and melting point 162°C and propylene-ethylene random copolymer (r-PP) (25% by mass) with MFR 60g / 10min, melting point 142°C and ethylene content of 4% by mass was melt spun by the spunbond method, and a second nonwoven fabric web (second layer) and a third nonwoven fabric web (third layer) made of fibers were laminated on the first nonwoven fabric web, respectively, to form a three-layer laminate web. The fibers had an average fiber diameter of 1.4d. The total weight of the three-layered laminated web is 15g / m 2 The basis weight of each layer was almost uniform. Next, the three-layer laminate web was brought into contact with an elliptical embossing roll with a convex area of 11% on the third nonwoven fabric web layer side, and with a mirror-finished roll on the first nonwoven fabric web layer side, and heat-pressed at 157°C to obtain a nonwoven fabric laminate. The total basis weight of the nonwoven fabric laminate was 15 g / m 2 It was.
[0070] Example 5 A nonwoven fabric laminate was obtained in the same manner as in Example 2, except that the nonwoven fabric web layer was changed as follows: The crimped conjugate fibers had an average fiber diameter of 1.3d. The following thermoplastic polymer was used as the core component and the following thermoplastic polymer was used as the sheath component, and composite melt spinning was performed by the spunbond method to deposit a first nonwoven fabric web (first layer) made of eccentric core-sheath type crimped composite fibers with a core component / sheath component mass ratio of 40 / 60 on a moving collection surface. Note that erucamide was contained in the above-mentioned thermoplastic polymer so that the erucamide content in the crimped composite fibers was 2000 ppm. -Core component- MFR: 60g / 10min, melting point: 162℃, propylene homopolymer (h-PP) -Sheath component- Propylene-ethylene random copolymer (r-PP) with MFR 60g / 10min, melting point 142℃, and ethylene content 4% by mass
[0071] In Example 5, a second nonwoven web of similar construction to the first nonwoven web was deposited onto the first nonwoven web. Next, a mixture of propylene polymer (h-PP) (60 mass%) with MFR 60g / 10min, melting point 162°C, and propylene-ethylene random copolymer (r-PP) (40 mass%) with MFR 60g / 10min, melting point 142°C, ethylene content 4 mass%, containing 1500 ppm of erucic acid amide was melt spun by the spunbond method to deposit a third nonwoven web (third layer) consisting of non-crimped fibers with an average fiber diameter of 1.3d on the second nonwoven web. The total weight of the three-layered laminated web is 17g / m 2 The basis weight of each layer was almost uniform. Next, the three-layer laminate web was brought into contact with an elliptical embossing roll with a convex area of 11% on the first nonwoven fabric web layer side, and with a mirror-finished roll on the third nonwoven fabric web layer side, and heat-pressed at 143°C to obtain a nonwoven fabric laminate. The total basis weight of the nonwoven fabric laminate was 17 g / m 2 It was.
[0072] Example 6 A nonwoven fabric laminate was obtained in the same manner as in Example 2, except that the nonwoven fabric web layer was changed as follows. A propylene polymer (h-PP) with MFR 60g / 10min and melting point 162°C was melt spun by the spunbond method to form a first nonwoven fabric web (first layer) made of fibers, which was then deposited on a moving collection surface. A second nonwoven fabric web (second layer) and a third nonwoven fabric web (third layer), each having the same structure as the first nonwoven fabric web, were laminated on the first nonwoven fabric web to form a three-layer laminate web. The fibers had an average fiber diameter of 1.4d. The total weight of the three-layered laminated web is 13g / m 2The basis weight of each layer was almost uniform. Next, the three-layer laminate web was brought into contact with an elliptical embossing roll with a convex area of 11% on the third nonwoven fabric web layer side, and with a mirror-finished roll on the first nonwoven fabric web layer side, and heat-pressed at 157°C to obtain a nonwoven fabric laminate. The total basis weight of the nonwoven fabric laminate was 13 g / m 2 It was.
[0073] (Examples 7 to 12) A nonwoven fabric laminate having an amino-modified silicone adhered thereto was obtained in the same manner as in Example 2, except that the coating amount of the amino-modified silicone adhered to the nonwoven fabric laminate was changed to the value shown in Table 1.
[0074] (Example 13) An emulsion containing 10% amino-modified silicone with a nitrogen mass fraction of 6700 μg / g (Toho Chemical Industry Co., Ltd., THS-3710) was diluted with ethanol, and a nonwoven fabric laminate having amino-modified silicone attached was obtained in the same manner as in Example 1, except that the amino-modified silicone solution diluted with ethanol was used instead of the amino-modified silicone solution diluted with normal hexane used in Example 1.
[0075] Example 14 An emulsion containing 30% amino-modified silicone with a nitrogen mass fraction of 5200 μg / g (Shin-Etsu Chemical Co., Ltd., POLON-MF-14EC) was diluted with water, and a nonwoven fabric laminate having amino-modified silicone attached was obtained in the same manner as in Example 1, except that the amino-modified silicone solution diluted with water was used instead of the amino-modified silicone solution diluted with normal hexane used in Example 1.
[0076] Example 15 In Example 1, a side-chain diamino silicone (Shin-Etsu Chemical Co., Ltd. KF869) was replaced with a both-end amino-modified silicone (Shin-Etsu Chemical Co., Ltd. KF8008) having a nitrogen mass fraction of 2200 μg / g, a kinetic viscosity at 25° C. of 450 mm 2 A nonwoven fabric laminate having an amino-modified silicone attached thereto was obtained in the same manner as in Example 1, except that the epoxy group was changed to 0.01 g / mol (functional group equivalent: 5700 g / mol).
[0077] Comparative Example 1 In Example 1, the side-chain diamino silicone (Shin-Etsu Chemical Co., Ltd. KF869) was replaced with a side-chain diamino silicone having a nitrogen mass fraction of 1800 μg / g (Shin-Etsu Chemical Co., Ltd. KF860, kinematic viscosity at 25° C. of 250 mm 2 A nonwoven fabric laminate having an amino-modified silicone attached thereto was obtained in the same manner as in Example 1, except that the composition was changed to (1 / s).
[0078] Comparative Example 2 A nonwoven fabric laminate having an amino-modified silicone adhered thereto was obtained in the same manner as in Comparative Example 1, except that the coating amount of the amino-modified silicone adhered to the nonwoven fabric laminate was changed to 2.00 mass %.
[0079] Comparative Example 3 A nonwoven fabric laminate having erucic acid amide adhered thereto was obtained in the same manner as in Example 1, except that erucic acid amide was adhered to the nonwoven fabric laminate instead of the amino-modified silicone in Example 1.
[0080] Comparative Example 4 A nonwoven fabric laminate having behenic acid adhered thereto was obtained in the same manner as in Example 1, except that behenic acid was adhered to the nonwoven fabric laminate instead of the amino-modified silicone in Example 1.
[0081] Comparative Example 5 The nonwoven fabric laminate of Example 1 to which no amino-modified silicone was applied was used as the nonwoven fabric laminate of Comparative Example 5.
[0082] The evaluation results of Examples 1 to 15 are shown in Table 1, and the evaluation results of Comparative Examples 1 to 5 are shown in Table 2.
[0083] [Table 1]
[0084] [Table 2]
[0085] As shown in Tables 1 and 2, the nonwoven fabric laminates of Examples 1 to 15, in which μs / μk was 1.20 or less and μs was 0.40 or less, had higher evaluation values in the tactile evaluation than the nonwoven fabric laminates of Comparative Examples 1 to 5, which had at least one of μs / μk greater than 1.20 and μs greater than 0.40, and were confirmed to have excellent moist feel.
[0086] The disclosure of Japanese Patent Application No. 2020-131012, filed on July 31, 2020, is incorporated herein by reference in its entirety. All publications, patent applications, and standards mentioned in this specification are herein incorporated by reference to the same extent as if each individual publication, patent application, or standard was specifically and individually indicated to be incorporated by reference.
Claims
1. Contains an amino-modified silicone having a nitrogen mass fraction of 2000 (μg / g) or more and 8000 (μg / g) or less, The content of the amino-modified silicone in the nonwoven fabric is 1.00 mass % or less based on the total amount of the nonwoven fabric (excluding nonwoven fabrics containing (A) amino.polyoxyalkylene group-containing organopolysiloxane and (B) polyoxyalkylene group-containing organopolysiloxane).
2. 2. The nonwoven fabric according to claim 1, wherein the ratio of the coefficient of static friction between fibers (μs) to the coefficient of kinetic friction between fibers (μk), μs / μk, is 1.20 or less, and the coefficient of static friction between fibers is 0.40 or less.
3. 3. The nonwoven fabric according to claim 1, which comprises fibers of an olefin polymer.
4. The nonwoven fabric according to claim 3 , wherein the olefin-based polymer comprises at least one selected from the group consisting of propylene-based polymers and ethylene-based polymers.
5. The nonwoven fabric according to claim 4, wherein the olefin-based polymer comprises the propylene-based polymer, and the propylene-based polymer comprises at least one selected from the group consisting of a propylene homopolymer and a propylene / α-olefin copolymer.
6. The nonwoven fabric according to any one of claims 1 to 5, which is a long-fiber nonwoven fabric having a fineness of 0.5 denier to 3.0 denier.
7. The nonwoven fabric according to any one of claims 1 to 6, which contains an amide compound.
8. The nonwoven fabric according to any one of claims 1 to 7, comprising crimped fibers.
9. A sanitary material comprising the nonwoven fabric according to any one of claims 1 to 8.
Citation Information
Patent Citations
Treating agent for synthetic fiber
JP1996302573A
Fiber having high smoothness, fabric-like material and molding
JP1997067772A
Production of staple fiber non-woven fabric
JP2000265350A
Abrasive
JP2004223701A
Softener composition for sanitation material
JP2006136351A