Electrolyte sealing material
The ethylene-propylene copolymer rubber composition with PTFE and/or titanium dioxide addresses the challenges of maintaining high gas shielding and electrolyte resistance, ensuring effective insulation and preventing compound extraction in electrolyte sealing materials for batteries and capacitors.
Patent Information
- Application Number
- JP2024507670
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-03-16
- Filing Date
- 2023-02-27
- Publication Date
- 2024-12-04
- Estimated Expiration
- 2043-02-27
AI Technical Summary
Existing electrolyte sealing materials for batteries and capacitors face challenges in maintaining high gas shielding properties, electrical insulation, and resistance to electrolytes, while also preventing the extraction of compounds into the electrolyte, which can adversely affect battery operation.
A composition of ethylene-propylene copolymer rubber blended with PTFE and/or titanium dioxide, combined with MT carbon black, is used to create an electrolyte sealing material with a filler concentration of 10% by weight or more, ensuring excellent insulation properties and resistance to electrolyte extraction.
The sealing material achieves effective insulation and prevents adverse effects on battery operation by maintaining high gas shielding and electrolyte resistance, meeting the required insulation properties and low compound extraction standards.
Smart Images

Figure 0007594709000001
Abstract
Description
[Technical field]
[0001] The present invention relates to an electrolyte sealing material, and more particularly to an electrolyte sealing material suitable for use as a sealing material in batteries, electrolytic capacitors, electric double layer capacitors, etc. [Background technology]
[0002] Ethylene-propylene copolymer rubber (EPM) or ethylene-propylene-non-conjugated diene copolymer rubber (EPDM) has excellent heat resistance, cold resistance, water resistance, and oil resistance, and is therefore widely used in various sealing parts (O-rings, gaskets, etc.).
[0003] Recently, in automotive electrical equipment applications and lighting applications, the environments in which batteries, capacitors, etc. are used are becoming hotter, and so heat resistance is being required for the batteries, capacitors, etc. themselves. The main factor that determines the lifespan of batteries, capacitors, etc. is the deterioration of their characteristics due to the evaporation of the internal electrolyte in gas form from the rubber seal, and the higher the temperature of the atmosphere, the greater the amount of electrolyte that evaporates. Therefore, in order to improve the heat resistance and extend the lifespan of batteries, capacitors, etc., rubber materials with excellent gas barrier properties are required.
[0004] Currently, electrolyte sealing materials used in lithium-ion batteries and the like are required to have high gas barrier properties, excellent electrical insulation, resistance to electrolyte, and no adverse effects on battery operation caused by the extraction of compounds in the rubber by the electrolyte. Specifically, the allowable amount of rubber compound extraction is an extremely small amount, such as 5 ppm. Therefore, only MT carbon black, which is chemically stable and does not extract free sulfur, can be used as a rubber filler.
[0005] In addition, to prevent short circuits in batteries and other circuits, the volume resistivity must be less than 10 14An insulation property of at least Ω·cm is required, and since EPDM polymer can meet this value, it is used as the rubber material for electrolyte seals in lithium-ion batteries, etc.
[0006] On the other hand, there are two types of fillers that can be mixed into rubber: conductive and insulating. Although silica and the like are commonly used as insulating fillers that can be mixed into rubber, they cannot be used as electrolyte sealing materials because they dissolve in the hydrogen fluoride generated from the electrolyte and have poor chemical stability. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2002-069254 A Summary of the Invention [Problem to be solved by the invention]
[0008] The present invention has been made in view of the above-mentioned problems, and has an object to provide an electrolyte sealing material which solves the problems of not allowing compounds in the rubber to be extracted by the electrolyte, in addition to having high gas barrier properties, excellent electrical insulation properties, and resistance to electrolytic solutions, and which is suitable for use in lithium ion batteries and the like. [Means for solving the problem]
[0009] The object of the present invention is achieved by an electrolyte sealing material which is an ethylene-propylene copolymer rubber composition comprising an ethylene-propylene copolymer rubber blended with PTFE and / or titanium dioxide, wherein the blending amount of PTFE and / or titanium dioxide in the total amount of filler is 10% by weight or more. Effect of the Invention
[0010] The electrolyte sealing material of the present invention is obtained by compounding a specified proportion of PTFE and / or titanium dioxide, which have electrical insulation properties, resistance to electrolyte and resistance to electrolyte extraction, as a rubber filler in an ethylene-propylene copolymer rubber, thereby achieving the excellent effect of satisfying the desired insulation properties and preventing any adverse effects on battery operation. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] As the ethylene-propylene copolymer rubber, ethylene-propylene-non-conjugated diene ternary copolymer rubber polymer (EPDM) is preferably used. As the non-conjugated diene, a small amount of dicyclopentadiene, 1,4-hexadiene, dicyclooctadiene, methylenenorbornene, vinylnorbornene, ethylidenenorbornene, etc. is copolymerized. Its Mooney viscosity ML 1+4 (125° C.) is about 25 to 80, preferably about 25 to 70. As the EPDM, commercially available products such as EP331 made by JSR and EPT-4010M made by Mitsui Chemicals can be used as they are or in the form of a blend.
[0012] As the electrically insulating filler to be mixed with the ethylene-propylene copolymer rubber, at least one of PTFE (polytetrafluoroethylene) and titanium dioxide is mixed and used in a proportion of 10% by weight or more of the total amount of the filler, preferably 45% by weight or more from the viewpoint of ensuring the normal physical properties of the sealing material. If the electrically insulating filler is used in a proportion of less than 10% by weight of the total amount of the filler, the volume resistivity becomes low, and even if the electrically insulating filler is used in a predetermined proportion of the total amount of the filler, when a filler other than PTFE or titanium dioxide, such as barium sulfate or mica, is mixed, the resistance to extraction by water cannot be satisfied, as shown in Comparative Examples 1 and 2 described later. Here, the total amount of the filler refers to the total amount of the electrically insulating filler and the conductive filler.
[0013] In the ethylene-propylene copolymer rubber, MT carbon black, which is chemically stable and does not extract free sulfur, can also be used as a conductive filler in a ratio of generally 150 parts by weight or less, preferably 50 to 150 parts by weight, and more preferably 75 to 125 parts by weight per 100 parts by weight of the ethylene-propylene copolymer rubber. By blending a predetermined amount of MT carbon black, the normal physical properties of the resulting sealing material can be ensured, so in this case, it is sufficient to blend PTFE and / or titanium dioxide in a ratio of about 10 to 30% by weight of the total amount of the filler. If the MT carbon black is used in a ratio greater than this, it may be difficult to ensure the sealing properties.
[0014] In rubber compositions containing the above components as essential components, organic peroxides are generally used as crosslinking agents. Examples of organic peroxides include tertiary butyl peroxide, dicumyl peroxide, 2,5-dimethyl-2,5-di-tertiary butyl peroxyhexane, 2,5-dimethyl-2,5-di-tertiary butyl peroxyhexyne-3, tertiary butyl cumyl peroxide, 1,3-di-tertiary butyl peroxy isopropyl benzene, 2,5-dimethyl-2,5-dibenzoyl peroxyhexane, peroxy ketals, and peroxy esters.
[0015] Examples of peroxyketals that can be used include n-butyl-4,4-di(tert-butylperoxy)valerate, 2,2-di(tert-butylperoxy)butane, 2,2-di[4,4-di(tert-butylperoxy)cyclohexyl]propane, 1,1-di(tert-butylperoxy)cyclohexane, di(3,5,5-trimethylhexanoyl)peroxide, 1,1-di(tert-hexylperoxy)cyclohexane, 1,1-di(tert-hexylperoxy)-3,3,5-trimethylcyclohexane, and 1,1-di(tert-butylperoxy)-2-methylcyclohexane.
[0016] As peroxy esters, for example, tert-butyl peroxybenzoate, tert-butyl peroxy acetate, tert-hexyl peroxy benzoate, tert-butyl peroxy-2-ethylhexyl monocarbonate, tert-butyl peroxy laurate, tert-butyl peroxy isopropyl monocarbonate, tert-butyl peroxy-3,5,5-trimethylhexanoate, tert-butyl peroxy maleic acid, tert-hexyl peroxy isopropyl monocarbonate, etc. may be used.
[0017] The crosslinking agent can be added in a ratio of about 0.5 to 10 parts by weight, preferably about 0.8 to 5 parts by weight, per 100 parts by weight of ethylene-propylene copolymer rubber. By adding the crosslinking agent in this range, foaming during crosslinking that makes it impossible to mold the rubber can be prevented, and the crosslinking density becomes good, making it easier to obtain sufficient physical properties.
[0018] Furthermore, a crosslinking accelerator may be contained as necessary. Examples of the crosslinking accelerator that can be used include triallyl isocyanurate, triallyl cyanurate, liquid polybutadiene, N,N'-m-phenylenedimaleimide, and trimethylolpropane trimethacrylate. The crosslinking accelerator can be added in an appropriate amount to improve crosslinking efficiency and further improve heat resistance and mechanical properties.
[0019] In addition to the above-mentioned components, compounding agents generally used in the rubber industry, such as acid acceptors, processing aids, plasticizers, lubricants, and antioxidants, may be added to the rubber composition as necessary, so long as they do not impair the object of the present invention.
[0020] The rubber composition can be prepared by kneading various materials using a kneading machine such as a single screw extruder, a twin screw extruder, an open roll, a Banbury mixer, a kneader, or a high shear mixer.
[0021] The crosslinking molding is carried out by a primary crosslinking process at about 150 to 220°C for about 1 to 60 minutes, and an oven crosslinking (secondary crosslinking) process at about 120 to 200°C for about 1 to 24 hours, which is carried out as necessary. EXAMPLES
[0022] The present invention will now be described in detail with reference to examples. However, the present invention, including its effects, is not limited to these examples.
[0023] Example 1 EPDM (JSR product EP331) 60 parts by weight EPDM (Mitsui Chemicals EPT-4010M) 36.5 〃 MT Carbon Black (Cancarb Thermax N990) 84 Same Titanium dioxide (Ishihara Sangyo Co., Ltd. Product Type A-100) 10 Same Peroxide crosslinking agent (NOF product Percumyl D) 3.5 Same The above components were kneaded in an internal kneader and open roll, compression molded at 180°C for 6 minutes, and then oven crosslinked at 150°C for 1 hour to obtain a test piece with a thickness of 2 mm. Using the obtained test piece, normal physical properties and volume resistivity were measured, and a water extraction test and an electrolyte immersion test were performed. Normal state physical properties: JIS K6251 corresponding to ISO 37, 6253 compliant to ISO 7619-1 Volume resistivity: Compliant with ISO 14309 JIS K6271 Compliance Measured using the double ring electrode method with an applied voltage of 500V To prevent short circuits in batteries and other circuits, 10 14 Insulation resistance of Ω·cm or more is required Water extraction test: Immerse the test piece in ion-exchanged water at 90°C for 70 hours. The aqueous extract was subjected to ion chromatography. Quantitative analysis of anions was performed using the immersed test Sum of all detected anions versus piece weight Evaluate the metric Electrolyte seals require water extractables of 5 ppm or less Electrolyte immersion test: Ethylene carbonate / Dimethyl carbonate / Ethyl methyl carbonate= The volume ratio of the mixture is 3 / 4 / 3, and the LiPF4 concentration is 1 mol / L. LiPF4 was mixed so that the test liquid was Test pins are compliant with JIS K6258, which corresponds to ISO1817. The volume change rate was evaluated by immersing the sample in a 90℃ bath for 250 hours. The electrolyte seal is required to have a volume change rate of 10% or less. Can
[0024] Example 2 In Example 1, the amount of MT carbon black was changed to 70 parts by weight, and the amount of titanium dioxide was changed to 16.7 parts by weight.
[0025] Example 3 In Example 1, the amount of MT carbon black was changed to 52.5 parts by weight, and the amount of titanium dioxide was changed to 25 parts by weight.
[0026] Example 4 In Example 1, MT carbon black was not used, the amount of titanium dioxide was changed to 50 parts by weight, and the amount of peroxide vulcanizing agent was changed to 4.5 parts by weight.
[0027] Example 5 In Example 1, 14 parts by weight of PTFE (Lubron L-5F, a product of Daikin Industries) was used in place of titanium dioxide.
[0028] Comparative Example 1 In Example 1, 10 parts by weight of barium sulfate (Sakai Chemical Industry Co., Ltd. product Variace B-54) was used in place of titanium dioxide.
[0029] Comparative Example 2 In Example 1, 10 parts by weight of mica (FNS mica, a product of Sanshin Kogyo) was used in place of titanium dioxide.
[0030] Comparative Example 3 In Example 1, the amount of MT carbon black was changed to 92 parts by weight, and the amount of titanium dioxide was changed to 6.3 parts by weight.
[0031] Comparative Example 4 In Example 1, titanium dioxide was not used, and the amount of MT carbon black was changed to 105 parts by weight.
[0032] Comparative Example 5 In Example 5, the amount of PTFE was changed to 6.3 parts by weight.
[0033] The results obtained in the above examples and comparative examples are shown in the following table together with the proportion of the insulating filler. TIFF0007594709000001.tif137158 [Industrial Applicability]
[0034] The sealing material obtained from the electrolyte sealing material of the present invention exhibits electrolyte resistance and resistance to electrolyte extraction, and is therefore suitably used as a sealing material for various batteries such as lithium ion batteries and nickel-metal hydride batteries, electrolytic capacitors, electric double layer capacitors, etc.
Claims
1. An electrolyte sealing material comprising an ethylene-propylene copolymer rubber composition containing PTFE and / or titanium dioxide in an ethylene-propylene copolymer rubber, the amount of PTFE and / or titanium dioxide being 10% by weight or more of the total amount of the filler.
2. 2. The electrolyte sealing material according to claim 1, wherein the content of PTFE and / or titanium dioxide in the total amount of the filler is 45% by weight or more.
3. 2. The electrolyte sealing material according to claim 1, wherein the ethylene-propylene copolymer rubber composition is an ethylene-propylene copolymer rubber blended with PTFE and / or titanium dioxide and MT carbon black.
4. 4. The electrolyte sealing material according to claim 3, wherein the MT carbon black is mixed in an amount of 150 parts by weight or less per 100 parts by weight of the ethylene-propylene copolymer rubber.
5. 4. The electrolyte sealing material according to claim 1, wherein the ethylene-propylene copolymer rubber is EPDM.
6. 2. The electrolyte sealing material according to claim 1, which is a molding material for a sealing material used in a battery.
7. An electrolyte seal which is a cross-linked molded product of the electrolyte seal material according to claim 6.
Citation Information
Patent Citations
Peroxide crosslinkable rubber composition
JP2002069254A
Sealed secondary battery
JP2004079469A
Electrolyte sealing material
JP2005093656A
Power storage device
JP2017091769A
Material for formation of seal for battery electrolyte
WO2004105160A1