Stripping agent and method for stripping hard coating film
Inorganic powders with controlled properties are used to crush into sharp particles for efficient and scratch-free removal of hard coatings from PVC surfaces, addressing the inefficiencies and damage of conventional methods.
Patent Information
- Application Number
- JP2021143557
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-07-28
- Publication Date
- 2024-12-05
- Estimated Expiration
- 2041-07-28
AI Technical Summary
Conventional methods for removing hard coating films from PVC surfaces, such as using diamond grindstones or brushes, cause damage and require expensive tools, while alternative abrasive powders lack sufficient polishing power and efficiency.
A method using inorganic powders with controlled Vickers hardness (3 to 20 GPa), particle size (30 μm to 300 μm), and specific gravity (0.1 or more) that are crushed into finely sharp particles to effectively peel off hard coatings without scratching the surface.
The method improves peeling efficiency and reduces surface scratches, allowing for easy removal of hard coatings without damaging the PVC floor.
Smart Images

Figure 0007594721000009 
Figure 0007594721000010 
Figure 0007594721000011
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for peeling off a hard coating film (such as an inorganic glass coating film) having a hardness of 6H or more that is applied to the surface of a PVC floor or the like. Agent Specifically, the crushed abrasive becomes sharp, significantly improving the abrasive power and reducing the PV of the coating floor. C Peeling of hard coating film without leaving noticeable scratches on the surface Agent The present invention also relates to a peeling method. [Background technology]
[0002] Conventionally, wax and UV coating methods have been common methods for protecting PVC floors, and these methods have been widely used in various places, but there have been many issues in terms of quality, gloss retention, and environmental aspects. Therefore, a new method of maintenance for PVC floors using hard coating agents has been attracting attention as an alternative method. Once applied, this method maintains a high quality condition for a long time, and is excellent in water resistance, alcohol resistance, oil resistance, acid resistance, alkali resistance, and chemical resistance, so it can be maintained in a beautiful state forever, and it is also an environmentally friendly method because it does not need to be peeled off. Therefore, it has been attracting attention as a new maintenance method to replace the conventional wax and UV methods, but one issue is that it is not easy to peel off using chemicals. Therefore, although various companies have proposed various hard coating methods, they cannot be easily peeled off, so it is not possible to return to the original state, and from the perspective of risk management, they have not been put into practical use. It is also possible to use a diamond grinding wheel to remove the flooring, but this method has problems such as scraping the flooring itself and damaging it, and leaving noticeable scratches, making it difficult to put these removal methods into practical use.
[0003] Regarding release agents for hard coatings with a hardness of 6H or more; Conventionally, coatings have been removed using diamond grindstones or diamond brushes, but this method scrapes the PVC tile itself and requires expensive tools, making the cost of removal high. In addition, diamond brushes can take a long time to remove. Therefore, as an alternative method, the following method is used to remove hard coating agents using abrasives. Agent It is generally used as an industrial polishing method to replace the diamond grindstone and diamond brush mentioned above. Agent For example, colloidal silica powder, silica powder, alumina powder, GC (green carbide) powder, zirconia powder, B4C (boron carbide) powder, etc. are used. Agent Although it has high hardness, it is not suitable for removing hard coating agents. Agent It was found that the abrasive power was insufficient for removing the coating material. The reason for this is that if the hardness and particle size of the abrasive are not appropriate, it is not suitable for removing the coating material. Therefore, although it can be used to roughen the surface of hard coating materials, it is difficult to use it to remove the coating material.
[0004] In addition, it was assumed that using a high hardness abrasive as described above would improve the abrasive power and allow the abrasive to be used as an abrasive with excellent peeling properties, but in reality, the hardness is so high that the abrasive is not crushed during abrasion, and therefore the abrasive power of the spherical abrasive is weak, and it was found that the abrasive power is not as strong as expected.
[0005] Patent Document 1 (JP Patent Publication No. 09-142840) describes "cerium oxide ultrafine particles consisting of cerium oxide single crystals having a particle size of 10 to 80 nm, and a method for producing said cerium oxide ultrafine particles, which comprises stirring and mixing an aqueous solution of cerous nitrate and a base in a ratio such that the pH is 5 to 10, followed by rapidly heating to 90 to 100°C and maturing at that temperature," and explains that "the present invention provides cerium oxide ultrafine particles which not only have an average particle size of 10 to 80 nm, but are also uniform in particle size and have the shape of each particle which is as uniform as possible, and a method for producing the same."
[0006] However, Patent Document 1 states that the present invention is "a method for removing a hard coating film made of a powder selected from alumina, white alundum, silica, zirconia, silicon nitride, silicon carbide, GC, B4C, etc., or a mixture thereof, having a Vickers hardness (HV) of 3 to 20 (GPa), a particle size of 30 μm to 300 μm, and a specific gravity of 0.1 or more, and having a hollow or solid shape." Agent Liquid peeling agent containing these powders or a solution in which the powders are dispersed, and calcium hydroxide, sodium hydroxide, magnesium hydroxide, or potassium hydroxide at a concentration of 10 to 40% by weight. Agent , and the polishing Agent Or the polishing Agent Liquid peeling agent dispersed in Agent There is no description at all about a "method of peeling off a hard coating film by spraying the above-mentioned on the surface of the hard coating film to peel off said film surface."
[0007] Furthermore, Patent Document 2 (JP Patent Publication No. 11-279537) describes that "a cerium raw material is heated and vaporized by a DC arc plasma method, and the cerium vapor is oxidized and cooled to obtain cerium oxide ultrafine particles having a pH of 4.2 to 5.3 for a 5 wt % aqueous dispersion and an average particle size of 5 to 70 nm, which are dispersed in water as a dispersion medium to obtain an aqueous dispersion of cerium oxide ultrafine particles," and explains that "there is provided an aqueous dispersion of cerium oxide ultrafine particles that does not aggregate when made into an aqueous dispersion and can be easily redispersed, and a method for producing the same."
[0008] However, Patent Document 2 states that the present invention is "a method for removing a hard coating film made of a powder selected from alumina, white alundum, silica, zirconia, silicon nitride, silicon carbide, GC, B4C, etc., or a mixture thereof, having a Vickers hardness (HV) of 3 to 20 (GPa), a particle size of 30 μm to 300 μm, and a specific gravity of 0.1 or more, and having a hollow or solid shape." AgentLiquid peeling agent containing these powders or a solution in which the powders are dispersed, and calcium hydroxide, sodium hydroxide, magnesium hydroxide, or potassium hydroxide at a concentration of 10 to 40% by weight. Agent , and the polishing Agent Or the polishing Agent Liquid peeling agent dispersed in Agent There is no description at all about a "method of peeling off a hard coating film by spraying the above-mentioned on the surface of the hard coating film to peel off said film surface."
[0009] Furthermore, Patent Document 3 (JP 2013-119131 A) describes "silica-based composite particles having an amorphous oxide layer C on the surface of amorphous silica particle A, the amorphous oxide layer C being different from the amorphous silica layer and containing one or more specific elements selected from aluminum, and further having a crystalline oxide layer B thereon containing one or more specific elements selected from zirconium, titanium, iron, and the like," and explains that "by reducing the amount of cerium used or using a substitute for cerium, the production costs are low and the decrease in polishing rate is significantly greater than that of conventional silica sols, and thus abrasive fine particles that can be used as a substitute for cerium oxide particles, a production method thereof, and a polishing slurry containing the abrasive fine particles are provided."
[0010] However, Patent Document 3 states that the present invention is "a method for removing a hard coating film, which is made of a powder selected from alumina, silica, zirconia, silicon nitride, silicon carbide, B4C, etc., or a mixture thereof, has a Vickers hardness (HV) of 3 to 20 (GPa), a particle size of 30 μm to 300 μm, and a specific gravity of 0.1 or more, and is made of a hollow or solid shape. Agent Liquid peeling agent containing these powders or a solution in which the powders are dispersed, and calcium hydroxide, sodium hydroxide, magnesium hydroxide, or potassium hydroxide at a concentration of 10 to 40% by weight. Agent , and the polishing Agent Or the polishing Agent Liquid peeling agent dispersed in AgentThere is no description at all about a "method of peeling off a hard coating film by spraying the above-mentioned on the surface of the hard coating film to peel off said film surface."
[0011] Furthermore, Patent Document 4 (JP 2014-58683 A) describes a method for producing a paint for forming a transparent coating, which comprises forming a silica coating layer to a thickness of 1 to 10 nm on composite oxide core microparticles composed of silica and inorganic oxides other than silica and having an average particle size of 19 to 70 nm, removing inorganic oxides other than silica to produce silica-based hollow particles having an average particle size (Dn) in the range of 20 to 80 nm and a refractive index in the range of 1.10 to 1.40, adjusting the particle size variation coefficient of the silica-based hollow microparticles to a range of 1 to 50% by combining methods (1) to (6), and then mixing the obtained silica-based hollow microparticles with a matrix-forming component and a polar solvent, and explaining that a paint for forming a transparent coating is provided that has excellent anti-reflection performance, strength, scratch resistance, etc.
[0012] However, Patent Document 4 states that the present invention is "a method for removing a hard coating film, which is made of a powder selected from alumina, silica, zirconia, silicon nitride, silicon carbide, B4C, etc., or a mixture thereof, has a Vickers hardness (HV) of 3 to 20 (GPa), a particle size of 30 μm to 300 μm, and a specific gravity of 0.1 or more, and is made of a hollow or solid shape. Agent Liquid peeling agent containing these powders or a solution in which the powders are dispersed, and calcium hydroxide, sodium hydroxide, magnesium hydroxide, or potassium hydroxide at a concentration of 10 to 40% by weight. Agent , and the polishing Agent Or the polishing Agent Liquid peeling agent dispersed in Agent There is no description at all about a "method of peeling off a hard coating film by spraying the above-mentioned on the surface of the hard coating film to peel off said film surface."
[0013] Furthermore, Patent Document 5 (JP 2014-1449879) describes that "in the process of supplying raw material shirasu 14 to a fluidized bed heating furnace 12 and heating and foaming to obtain shirasu balloons 4, which are then cooled in a fluidized bed cooler 2, the raw material solution delivered from a film-forming raw material solution tank 10 and a raw material supply pump 11 is intermittently sprayed from a spray nozzle 3 provided inside the fluidized bed cooler 2 onto the shirasu balloons 4 while the spray nozzle 3 is moved by an air compressor 8 and a nozzle moving device 9, thereby forming a coating of a functional metal oxide or composite metal oxide on the surface," and explains that "there is provided a method that makes it possible to directly produce inexpensive, high-performance functional fine hollow glass spheres from volcanic glass deposits."
[0014] However, Patent Document 5 states that the present invention is "a method for removing a hard coating film, which is made of a powder selected from alumina, silica, zirconia, silicon nitride, silicon carbide, B4C, etc., or a mixture thereof, has a Vickers hardness (HV) of 3 to 20 (GPa), a particle size of 30 μm to 300 μm, and a specific gravity of 0.1 or more, and is made of a hollow or solid shape. Agent Liquid peeling agent containing these powders or a solution in which the powders are dispersed, and calcium hydroxide, sodium hydroxide, magnesium hydroxide, or potassium hydroxide at a concentration of 10 to 40% by weight. Agent , and the polishing Agent Or the polishing Agent Liquid peeling agent dispersed in Agent There is no description at all about a "method of peeling off a hard coating film by spraying the above-mentioned on the surface of the hard coating film to peel off said film surface."
[0015] Furthermore, Patent Document 6 (JP 2017-20018 A) states that "the abrasive grains as tertiary particles 4 are formed when fine primary particles 1 are bonded together without a binder to form secondary particles 2, which are further bonded together by a binder 3. In this abrasive grain, the bonding force between the primary particles 1 is weaker than the bonding force between the secondary particles 2 and the binder 3. Therefore, the abrasive grains do not fall off from the polishing tool 7 as secondary particles 2 during polishing, and the flat wear state of the abrasive grains can be maintained." It also explains that "We provide abrasive grains, a polishing tool, and a method for manufacturing abrasive grains that are capable of improving processing efficiency." The [Claims] state that the abrasive grain is characterized in that the secondary particles are formed by bonding fine primary particles without the use of a binder, and the secondary particles are further bonded by a binder to form tertiary particles, the bonding strength between the primary particles being weaker than the bonding strength between the secondary particles and the binder, the average particle size of the tertiary particles is 100 μm or more, the interior of the abrasive grain is hollow, and the primary particles are either zirconium oxide, cerium oxide, or silica.
[0016] However, Patent Document 6 states that the present invention is "a method for peeling off a hard coating film, which is made of a powder selected from alumina, silica, zirconia, silicon nitride, silicon carbide, B4C, etc., or a mixture thereof, has a Vickers hardness (HV) of 3 to 20 (GPa), a particle size of 30 μm to 300 μm, and a specific gravity of 0.1 or more, and is made of a hollow or solid shape. Agent Liquid peeling agent containing these powders or a solution in which the powders are dispersed, and calcium hydroxide, sodium hydroxide, magnesium hydroxide, or potassium hydroxide at a concentration of 10 to 40% by weight. Agent , and the polishing Agent Or the polishing Agent Liquid peeling agent dispersed in Agent There is no description at all about a "method of peeling off a hard coating film by spraying the above-mentioned on the surface of the hard coating film to peel off said film surface."
[0017] In addition, Patent Document 7 (JP Patent Publication 2019-127405 A) describes a ceria-based hollow composite microparticle dispersion liquid containing ceria-based hollow composite microparticles having an average particle diameter of 20 to 400 nm and having the characteristics of [1] to [3]. [1] The ceria-based hollow composite microparticles have a hollow structure having voids inside a cerium-containing silica layer as an outer shell, and child particles mainly composed of crystalline ceria are dispersed inside the cerium-containing silica layer. [2] The ceria-based hollow composite microparticles are detected as having only a ceria crystalline phase by X-ray diffraction. [3] The ceria-based hollow composite microparticles are measured by X-ray diffraction and have an average crystallite diameter of the crystalline ceria of 8 to 25 nm. It is described that "the present invention provides a silica-based composite particle dispersion liquid that can polish silica films, Si wafers, and difficult-to-process materials at high speed and achieve high surface accuracy at the same time."
[0018] However, Patent Document 7 states that the present invention is "a method for removing a hard coating film, which is made of a powder selected from alumina, silica, zirconia, silicon nitride, silicon carbide, B4C, etc., or a mixture thereof, has a Vickers hardness (HV) of 3 to 20 (GPa), a particle size of 30 μm to 300 μm, and a specific gravity of 0.1 or more, and is made of a hollow or solid shape. Agent Liquid peeling agent containing these powders or a solution in which the powders are dispersed, and calcium hydroxide, sodium hydroxide, magnesium hydroxide, or potassium hydroxide at a concentration of 10 to 40% by weight. Agent , and the polishing Agent Or the polishing Agent Liquid peeling agent dispersed in Agent There is no description at all about a "method of peeling off a hard coating film by spraying the above-mentioned on the surface of the hard coating film to peel off said film surface." Problem to be solved by the invention
[0019] Conventional methods of removing hard coatings using diamond grindstones or diamond brushes have the problem of easily damaging the PVC itself and requiring expensive tools for removal. The present invention uses inorganic materials with appropriately controlled Viscosity Hardness (HV), particle size, and specific gravity to easily remove hard coatings, completely removing the hard coating layer without scratching the base material itself, and polishing the hard coating layer. Agent The polishing power can be improved by peeling off the hard coating film Agent and liquid peeling Agent It is also an object of the present invention to provide a peeling method. Means for solving the problem
[0020] No. The present invention relates to a method for peeling hard coating films, comprising a type of inorganic powder or a mixture thereof, with a Vickers hardness (HV) of 3 to 20 (GPa), a particle size of 30 μm to 300 μm, and a specific gravity of 0.1 or more. Agent This provides:
[0021] In this invention, a polishing powder with a Vickers hardness (HV) of 3 to 20 (GPa), a particle size of 30 μm to 300 μm, and a specific gravity of 0.1 or more is used. Agent The particles are broken into small pieces by the pressure during crushing, and the fine, sharp crushed particles improve the peelability of the hard coating film and significantly improve the peeling efficiency. The crushed particles are very fine, so the PV of the coating floor is C It does not leave any noticeable scratches on the surface. Even if the hardness of the hard coating film is relatively low, the PV of the coating floor is CIt does not scratch the surface. With a Vickers hardness (HV) of less than 3, only small scratches are made in the coating layer, and the coating layer is not completely peeled off. With a Vickers hardness of more than 20, the abrasive is difficult to pulverize, and the coating layer is only deeply scratched and not peeled off. With a particle size of less than 30 μm, the particles are too fine and even if crushed, they do not peel off, but are more like polishing. With a particle size of more than 300 μm, the crushed abrasive is large and it takes time to improve the peelability, so 300 μm or less is preferable. With a specific gravity of less than 0.1, it is easy to scatter and is difficult to interpose between the coating layer and the polisher during polishing, making it difficult to obtain abrasive properties and resulting in poor peelability.
[0022] No. The invention in question is record removal away Agent But due to its hollow shape Hard Peeling of porous coating film Agent This provides:
[0023] In this invention, since the inside of the particles is hollow, they are easily crushed even with a relatively weak pressure during crushing, so they are suitable for peeling off hard coating films with low hardness, and are not crushed during polishing. Agent The shape of the surface is sharp, which can improve the peeling action.
[0024] No. The invention in question is record removal away Agent But from a solid shape Hard Peeling of porous coating film Agent This provides:
[0025] In this invention, since the inside of the particle is solid, it is easily crushed by the relatively high pressure during crushing, and is more suitable for peeling off a hard coating film having a higher hardness than a hollow shape, and is crushed during polishing. Agent The shape of the surface is sharp, which can improve the peeling action.
[0026] No.The fourth invention is a method for removing a hard coating film, which is made of a type of inorganic powder or a mixture thereof, and has a Vickers hardness (HV) of 3 to 20 (GPa), a particle size of 30 μm to 300 μm, and a specific gravity of 0.1 or more, or a solution in which the powder is dispersed, and contains calcium hydroxide, sodium hydroxide, magnesium hydroxide, or potassium hydroxide at a weight percent concentration of 10 to 40%. Agent This provides:
[0027] In this invention, a polishing powder with a Vickers hardness (HV) of 3 to 20 (GPa), a particle size of 30 μm to 300 μm, and a specific gravity of 0.1 or more is used. Agent The crushing pressure breaks the particles into small pieces, and the crushed fine particles have a sharp shape, which improves the peeling efficiency when peeling off hard coating films, and the crushed particles are very fine, so the PV of the coating bed is reduced. C It does not leave any noticeable scratches on the surface. Even if the hardness of the hard coating film is relatively low, the PV of the coating floor is C Peeling without damaging the surface Agent can be provided.
[0028] No. The fifth invention relates to an abrasive comprising one or a mixture of inorganic powders, having a Vickers hardness (HV) of 3 to 20 (GPa), a particle size of 30 μm to 300 μm, and a specific gravity of 0.1 or more. Agent Or the polishing Agent Dispersed peeling Agent Spray onto the hard coating film surface. The hard coating having the abrasive or the release agent dispersed therein. Membrane surface Pressure Add force At the same time, While polishing The above By crushing the release agent The hard coating Peel off the film surface R The present invention provides a method for removing a hard coating film.
[0029] In this invention, since abrasives using soft powders are easier to crush during polishing, the crushed sharp abrasives can improve the polishing power. The particles have a Vickers hardness (HV) of 3-20 (GPa), a particle size of 30μm-300μm, and a specific gravity of 0.1 or more, so the particles are broken down into small pieces by the pressure during crushing, and the crushed fine sharp crushed particles peel off the hard coating, improving the peeling efficiency and further improving the polishing power due to the crushed fine abrasives. In addition, since the crushed crushed particles are very fine, the PV of the coating bed is improved. C It does not leave any noticeable scratches on the surface. Even if the hardness of the hard coating film is relatively low, the PV of the coating floor is C It is possible to provide a method for peeling off a hard coating film without damaging the surface.
[0030] [Patent Document 1] Japanese Patent Application Publication No. 09-142840 [Patent Document 2] Japanese Patent Application Publication No. 11-279537 [Patent Document 3] JP 2013-119131 A [Patent Document 4] JP 2014-58683 A [Patent Document 5] Patent Publication 2014-1449879 [Patent Document 6] JP 2017-20018 A [Patent Document 7] JP 2019-127405 A Examples of the present invention
[0031] An embodiment of the present invention will be described below. There are two types of methods for removing hard coating agents: (1) a method using a diamond brush and (2) a method using a diamond grindstone. The diamond brush method (1) is a method of attaching 5 to 8 diamond brushes to a floor cleaning polisher to scrape off the hard coating agent. This method can remove the hard coating layer without scraping the PVC tile, but it has problems such as the time required for removal and the high cost due to the expensive tools, making it difficult to use it in various places. On the other hand, the diamond grindstone method (2) has a high abrasive power, but it is not a recommended method for removal because it scrapes off the PVC itself and the polishing scratches are noticeable. Furthermore, chemical peeling is difficult for non-tangible coating agents (glass-based coating agents). Therefore, once the application is performed, it is not easy to remove compared to conventional wax application, and it is difficult to use it in a general purpose manner from the perspective of risk management.
[0032] The general physical properties of the main components of industrial abrasives, such as Vickers hardness (HV) and specific gravity, are shown in Table 1 below. [Table 1]
[0033] Conventionally, polishing was used to remove hard coating agents. Agent As a polishing material, green carbonite (SiC) and boron carbide (B4C), which have relatively high Vickers hardness, are used. Agent Previously, the peeling was performed using abrasives with high Vickers hardness. AgentWhen using an abrasive such as silica (SiO2), which has a low Vickers hardness, the peelability is reduced and the PVC floor itself is scratched. On the other hand, when an abrasive such as silica (SiO2) with a low Vickers hardness is used, the crushed particles penetrate the coating surface when crushed into small particles, scraping off the coating layer and becoming even finer particles, which is contrary to expectations and significantly improves peelability. The reason for this is that the abrasive is crushed during the peeling process, becoming sharper, and the abrasive power required for peeling is improved. Photo 1 is a photo of a solid abrasive before the peeling process, Photo 2 is a photo of a solid abrasive after the peeling process, Photo 3 is a photo of a hollow abrasive before the peeling process, and Photo 4 is a photo of a hollow abrasive after the peeling process. After the peeling process, the stripping agent becomes finer and sharper. In addition, as the abrasive scrapes off the coating surface during peeling, it is crushed even finer, making it less likely to scratch the PVC floor itself. During the peeling process, compressive and shear loads are applied to the abrasive between the polisher and the coating surface, which increases the abrasive strength. Agent It can be assumed that this is because the abrasive is crushed into small pieces, and the sharp shapes of the crushed pieces improve the abrasive power. It is also believed that the fine crushed abrasive further improves the abrasive power. As a result, it has become relatively easy to remove hard coating agents, which was previously difficult to do. Table 2 shows the results of a peeling test using a high-hardness abrasive such as green carbonite (GC) and a low-hardness abrasive such as SiO2. It is clear that the use of a low-hardness abrasive such as SiO2 provides superior peeling properties. 。
[0034] The results of peeling tests using high-hardness abrasives such as green carbonite (SiC) and wear tests using low-hardness abrasives such as silicon dioxide (SiO2) were used to show the peelability results. [Table 2] Test method: Plastic was replaced with coated PVC according to the abrasive wear test method JIS K7205-1995. The coating used was one that did not peel off in the cross-cut test JIS K5600-5-6, and the hardness of the coating was 6H (scratch hardness (pencil method) JIS K5600-5-4). The amount of coating that peeled off was calculated from the weight of the coating before the test and the weight after the test, and the amount that peeled off was calculated from the weight of the original coating itself. In addition, the particle size of the abrasives used was 80 μm on average. As a test result, the value obtained by dividing the amount of peeling by the original coating weight is recorded as the peeling rate. There is no standard for the peeling method using abrasives as a criterion for judging peelability. In this test, it was judged that those with a peeling rate of less than 50% had poor peelability even if time was required, and it was difficult to use them as a peeling agent in reality, so those with a peeling rate of less than 50% were rated as × for peelability, and those with a peeling rate of 50% or more were rated as ○ for peelability.
[0035] As shown in the results in Table 2, green carbonite and boron carbonite had deep scratches in the coating, but the coating itself was not thinned, and they tended to have poor peelability. Even over time, deeper scratches appeared, and the PVC itself was scratched, indicating poor peelability. On the other hand, silica, zirconia, silicon nitrogen, and white alundum had fine scratches in the coating layer, causing it to be thinned. Due to their low Vickers hardness, they were crushed while scratching the coating layer when rubbed against it, and it was found that the fine particles were thinning the coating layer.
[0036] [Table 2] shows the results for a particle size of 80 μm, so the differences in peelability for each particle size are shown in [Table 3]. [Table 3] Test method: Plastic was replaced with coated PVC according to the abrasive wear test method JIS K7205-1995. The coating used was one that did not peel off in the cross-cut test JIS K5600-5-6, and the hardness of the coating was 6H (scratch hardness (pencil method) JIS K5600-5-4). The amount of coating that peeled off was calculated by the weight of the coating before the test and the weight after the test, and the amount that peeled off was calculated from the weight of the original coating itself. The peeling rate is the value obtained by dividing the amount of peeling by the original coating weight as the test result. There is no standard for the peeling method using abrasives as a criterion for judging peelability. In this test, it was judged that those with a peeling rate of less than 50% had poor peelability even if time was required, and it was difficult to use them as a peeling agent in reality, so those with a peeling rate of less than 50% were rated as × for peelability, and those with a peeling rate of 50% or more were rated as ○ for peelability.
[0037] From the results in Table 3, it was found that even when using abrasives with the same ingredients, the smaller or larger the particle size, the poorer the peelability tends to be. Small particle sizes of less than 30 μm become even finer when crushed under pressure, causing small scratches on the surface of the high-humidity coating, and it takes a long time to peel off. In addition, large particle sizes of more than 300 μm increase the hardness of the larger particle size to a certain extent, making it difficult to crush under the pressure of the hard coating layer. Therefore, it was found that the larger the particle size, the longer it takes to peel off, and the efficiency of peeling tends to be poor.
[0038] We also investigated hollow abrasives as shown below. For example, when comparing hollow Shirasu balloons with solid silica, both of which have the same main component SiO2 and an average particle size of 80μm, the Vickers hardness of the hollow abrasives is lower, as shown in Table 4 below. [Table 4]
[0039] Although the hollow shape has a lower abrasive power than the solid shape, it is believed that it can be used as a stripping agent. As described in
[0006] , this is also thought to be because the powder is crushed during polishing, and the crushed particles bite into the coating layer and scrape it off. However, due to the low Vickers hardness, the polishing ability was inferior to that of the solid shape. The results are shown in Table 5 below. [Table 5] Test method: Plastic was replaced with coated PVC according to the abrasive wear test method JIS K7205-1995. The coating used was one that did not peel off in the cross-cut test JIS K5600-5-6, and the hardness of the coating was 6H (scratch hardness (pencil method) JIS K5600-5-4). The particle size of the abrasives used was 80μm on average. The amount of coating that peeled off was calculated based on the weight of the coating before the test and the weight after the test, and the amount that peeled off was calculated from the weight of the original coating itself. The peeling rate is calculated by dividing the amount of peeling by the original coating weight as the test result. There is no standard for the peeling method using abrasives as a criterion for judging peelability. In this test, it was judged that those with a peeling rate of less than 50% had poor peelability even if time was required, and it was difficult to use them as a peeling agent in reality, so those with a peeling rate of less than 50% were rated as × for peelability, and those with a peeling rate of 50% or more were rated as ○ for peelability.
[0040] Regarding the components of the abrasive, the specific gravity basically depends on the main component of the abrasive, but even if the main component is the same as above, the specific gravity differs between solid and hollow shapes. For example, a Shirasu balloon with a particle size of 80 μm and a specific gravity of less than 0.1 is inferior to one with a specific gravity of 0.1 or more. This is because the specific gravity is too small and it is prone to scattering, and it is difficult to interpose between the polisher and the coating layer during the peeling process, resulting in poor peeling properties. The results are shown in [Table 6]. [Table 6] Test method: Plastic was replaced with coated PVC according to the abrasive wear test method JIS K7205-1995. The coating used was one that did not peel off in the cross-cut test JIS K5600-5-6, and the hardness of the coating was 6H (scratch hardness (pencil method) JIS K5600-5-4). The particle size of the abrasives used was 80μm on average. The amount of coating that peeled off was calculated based on the weight of the coating before the test and the weight after the test, and the amount that peeled off was calculated from the weight of the original coating itself. The peeling rate is calculated by dividing the amount of peeling by the original coating weight as the test result. There is no standard for the peeling method using abrasives as a criterion for judging peelability. In this test, it was judged that those with a peeling rate of less than 50% had poor peelability even if time was required, and it was difficult to use them as a peeling agent in reality, so those with a peeling rate of less than 50% were rated as × for peelability, and those with a peeling rate of 50% or more were rated as ○ for peelability.
[0041] By mixing these powders or dispersed solutions with calcium hydroxide, sodium hydroxide, magnesium hydroxide, or potassium hydroxide at a concentration of 10 to 40% by weight, it is possible to further improve the peelability. The results of comparing silica and silica mixed with calcium hydroxide at a concentration of 10 to 40% by weight are shown in Table 6 below. Although peeling is possible with silica alone, the peelability is improved by mixing calcium hydroxide. This is presumed to be because the alkaline component calcium hydroxide penetrates into the scratches caused by the crushed abrasive, softening the coating layer and further improving the abrasiveness. In addition, when the concentration of calcium hydroxide, sodium hydroxide, magnesium hydroxide, or potassium hydroxide exceeds 40%, the peelability becomes worse. This is thought to be because the proportion of abrasive decreases, making it difficult for scratches to occur in the coating layer. The formulations are shown in Table 6 below, and the results in Table 7.
[0042] [Table 6]
[0043] [Table 7] Test method: Plastics were replaced with coated PVC according to the abrasive wear test method JIS K7205-1995. The coatings used were those that did not peel off in the cross-cut test JIS K5600-5-6, and had a hardness of 6H (scratch hardness (pencil method) JIS K5600-5-4). The average particle size of the abrasives used was 80μm. In this test, the alkalinity of the powdered calcium hydroxide, sodium hydroxide, magnesium hydroxide, and potassium hydroxide mixed with the abrasives is important, so 1cc of water was dropped onto the coated PVC test piece, and the abrasive mixed with calcium hydroxide, sodium hydroxide, magnesium hydroxide, and potassium hydroxide was dropped to perform the test. The average particle size of the abrasives used was 80μm. The amount of coating that peeled off was calculated from the weight of the coated specimen before the test and the weight after the test, and the amount that peeled off was calculated from the weight of the original coating itself. The test results are reported as the peeling rate, calculated by dividing the amount of peeling by the original coating weight. No standard is set for the peeling method using an abrasive as a criterion for judging peelability. In this test, it was determined that those with a peeling rate of less than 50% had poor peelability even if time was required, and were practically difficult to use as a peeling agent, so those with a peeling rate of less than 50% were rated as × for peelability, and those with a peeling rate of 50% or more were rated as ○ for peelability. Effects of the Invention
[0044] In this invention, abrasives using a Vickers hardness (HV) of 3 to 20 (GPa), a particle size of 30 μm to 300 μm, and a specific gravity of 0.1 or more are used. Agent The crushing pressure breaks the particles into small pieces, and the crushed particles have a sharp shape, so they bite into the coating surface, scraping off the coating layer and becoming even finer particles. The crushed particles are so fine that the PV of the coating bed is reduced. CIt does not leave any noticeable scratches on the surface. Even if the hardness of the hard coating film is relatively low, the PV of the coating floor is C Will not damage the surface.
[0045] In this invention, the particles having a hollow interior are easily crushed even under a relatively weak pressure during crushing, and are therefore suitable for peeling off hard coating films having low hardness. Agent The shape becomes sharp, and the polishing power can be improved.
[0046] In this invention, the particles having a solid interior are easily crushed under a relatively high pressure during crushing, and are more suitable for peeling off a hard coating film having a higher hardness than the particles having a hollow interior. The particles are crushed during polishing, and are polished. Agent The shape becomes sharp, and the polishing power can be improved.
[0047] In this invention, a polishing powder having a Vickers hardness (HV) of 3 to 20 (GPa), a particle size of 30 μm to 300 μm, and a specific gravity of 0.1 or more is used. Agent The particles are broken down into small pieces by the pressure during crushing, and when they are crushed into small pieces, they bite into the coating surface, scraping off the coating layer and becoming even finer particles. This improves the peeling efficiency, and at the same time, the crushed particles are very fine, so the PV of the coating bed is improved. C It does not leave any noticeable scratches on the surface. Even if the hardness of the hard coating film is relatively low, the PV of the coating floor is C It is possible to provide a release agent that does not damage the surface. [Brief description of the drawings]
[0048] [Figure 1] A photograph of a solid abrasive before peeling (2.0x magnification). [Diagram 2] A photograph of a solid abrasive after peeling (2.0x magnification). [Diagram 3] A photograph of the hollow shaped abrasive before peeling (2.0x magnification). [Figure 4] A photograph of the hollow shaped abrasive after peeling (2.0x magnification).
Claims
1. The powder or powder dispersion solution is made of one type of inorganic powder or a mixture of these, and has a Vickers hardness (HV) of 3 to 20 (GPa), a particle size of 30 μm to 300 μm, and a specific gravity of 0.1 or more, and contains calcium hydroxide, sodium hydroxide, magnesium hydroxide, or potassium hydroxide at a weight percent concentration of 10 to 40%. Stripping agent.
2. A polishing agent consisting of one type of inorganic powder or a mixture thereof, having a Vickers hardness (HV) of 3 to 20 (GPa), a particle size of 30 μm to 300 μm, and a specific gravity of 0.1 or more, or a release agent in which the polishing agent is dispersed, is sprayed onto a hard coating film surface, and pressure is applied to the hard coating film surface onto which the polishing agent or release agent has been sprayed, while the release agent is crushed while being polished, thereby peeling off the hard coating film surface. A method for removing hard coating films.
Citation Information
Patent Citations
Abrasive grain for magnetic polishing and its manufacturing method
JP2002080826A
Film stripping method and regenerating method for hard carbon coating film, and regenerated base material
JP2003200350A
Slip resistant floor coating remover composition
JP2004518000A
Floor coating removal brush and floor coating removal method
JP2017221240A
Polishing composition, polishing method, and method for producing polishing composition
JP2018090682A