Method for producing anion-modified colloidal silica
By ion-exchanging and anion-modifying colloidal silica using an ion exchange resin and silane coupling agents, the method achieves high-speed polishing of silicon nitride films while minimizing the polishing rate of silicon oxide films, addressing the selectivity challenge in CMP processes.
Patent Information
- Application Number
- JP2020098159
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-06-05
- Publication Date
- 2024-12-05
- Estimated Expiration
- 2040-06-05
AI Technical Summary
Existing CMP methods struggle to polish silicon nitride films at high speed while simultaneously suppressing the polishing rate of silicon oxide films, as conventional anion-modified colloidal silica solutions prioritize high polishing rates for silicon nitride at the expense of silicon oxide.
A method involving ion-exchanging raw material colloidal silica using an ion exchange resin and anion-modifying the ion-exchanged silica to produce anion-modified colloidal silica, which includes steps of mixing, reacting with a silane coupling agent, and oxidizing to introduce sulfonic acid groups, thereby controlling polishing rates for both film types.
The method enables high-speed polishing of silicon nitride films while reducing the polishing rate of silicon oxide films, enhancing the selectivity and efficiency of chemical mechanical polishing processes.
Smart Images

Figure 0007594864000001 
Figure 0007594864000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing anion-modified colloidal silica. [Background technology]
[0002] In recent years, new microfabrication technologies have been developed to accompany the high integration and high performance of LSI (Large Scale Integration). Chemical mechanical polishing (CMP) is one of these technologies, and is frequently used in the LSI manufacturing process, especially in the multi-layer wiring formation process, for planarizing interlayer insulating films, forming metal plugs, and forming buried wiring (damascene wiring).
[0003] The CMP has been applied to each process in semiconductor manufacturing, and one aspect of the invention is the application to a gate formation process in transistor fabrication. When fabricating a transistor, materials such as metal, silicon, silicon oxide, polycrystalline silicon, and silicon nitride film may be polished, and there is a demand for polishing each material at high speed in order to improve productivity. In order to meet such a demand, for example, Patent Document 1 discloses a technology for providing a polishing composition capable of polishing a polishing target having poor chemical reactivity such as silicon nitride at high speed, in which colloidal silica (sulfonic acid group (anion) modified colloidal silica) having an organic acid fixed thereto is contained as an abrasive grain in the composition, and the pH is set to 6 or less. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2012-040671 A Summary of the Invention [Problem to be solved by the invention]
[0005] It is true that the anion-modified colloidal silica described in Patent Document 1 can be used to polish a silicon nitride film at a high polishing rate.
[0006] The present inventors have found that in CMP in semiconductor manufacturing, while a silicon nitride film is polished at a high polishing rate, it is sometimes preferable in terms of manufacturing to keep the polishing rate as low as possible for a silicon oxide film.
[0007] Therefore, an object of the present invention is to provide a method for producing anion-modified colloidal silica that can polish a silicon nitride film at high speed while suppressing the polishing rate of a silicon oxide film. [Means for solving the problem]
[0008] The present inventors have conducted extensive research to solve the above problems, and as a result, have found that the above problems can be solved by subjecting raw colloidal silica to ion exchange using an ion exchange resin, and then anion-modifying the ion-exchanged raw colloidal silica to anion-modified colloidal silica, thereby completing the present invention.
[0009] That is, according to one embodiment of the present invention, there is provided a method for producing anion-modified colloidal silica, comprising: an ion exchange step of performing ion exchange on raw colloidal silica using an ion exchange resin; and a modification step of anion-modifying the ion-exchanged raw colloidal silica to obtain anion-modified colloidal silica. Effect of the Invention
[0010] According to the present invention, there is provided a method for producing anion-modified colloidal silica that can polish a silicon nitride film at high speed while suppressing the polishing rate of a silicon oxide film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] An embodiment according to one aspect of the present invention will be described below, but the present invention is not limited to the following embodiment.
[0012] In this specification, the range "X to Y" means "X or more and Y or less." Furthermore, unless otherwise specified, the operations and measurements of physical properties are performed under conditions of room temperature (20 to 25°C) and relative humidity of 40 to 50% RH.
[0013] One embodiment of the present invention is a method for producing anion-modified colloidal silica, comprising an ion exchange step of ion-exchanging raw colloidal silica with an ion exchange resin, and a modification step of anion-modifying the ion-exchanged raw colloidal silica to obtain anion-modified colloidal silica. By carrying out the ion exchange step and the modification step in combination, the method for producing anion-modified colloidal silica of this embodiment can obtain anion-modified colloidal silica that can polish a silicon nitride film at a high speed and suppress the polishing speed of a silicon oxide film.
[0014] In this specification, "modified colloidal silica" means that anionic groups (for example, sulfonic acid groups) are bonded to the surface of colloidal silica particles.
[0015] Hereinafter, a production method according to one embodiment of the present invention will be described in detail.
[0016] <Ion exchange process> The manufacturing method of this embodiment includes an ion exchange step of ion-exchanging raw colloidal silica with an ion exchange resin.
[0017] The ion exchange step may be carried out once, or may be carried out two or more times as necessary.
[0018] [Raw material colloidal silica] The raw colloidal silica is a raw material before being anion-modified (modified) using the modification process described below, and contains silica particles. The raw colloidal silica may be produced by a sodium silicate method or a sol-gel method. The raw colloidal silica may be synthesized or may be a commercially available product. The raw colloidal silica may be unmodified or modified. Modified raw colloidal silica includes, for example, modified colloidal silica treated with aluminic acid.
[0019] In the production method of this embodiment, aggregation of silica particles can be suppressed regardless of the purity of the raw material colloidal silica.
[0020] In one embodiment, the raw colloidal silica is colloidal silica obtained by a sodium silicate method. The sodium silicate method is a method in which activated silicic acid obtained by ion-exchanging an aqueous solution of an alkali silicate such as water glass is used as a raw material and the particles are grown.
[0021] The lower limit of the average primary particle size of raw colloidal silica is preferably 1 nm or more, more preferably 5 nm or more, and even more preferably 7 nm or more.The upper limit of the average primary particle size of raw colloidal silica is preferably 100 nm or less, more preferably 50 nm or less, and even more preferably 20 nm or less.Within such a range, the polishing composition containing the produced anion-modified colloidal silica can polish silicon nitride film at high speed and suppress the polishing speed of silicon oxide film.The average primary particle size of colloidal silica is calculated based on the specific surface area of colloidal silica measured by BET method, for example.
[0022] The lower limit of the average secondary particle size of raw colloidal silica is preferably 2nm or more, more preferably 10nm or more, and even more preferably 15nm or more.The upper limit of the average secondary particle size of raw colloidal silica is preferably 200nm or less, more preferably 150nm or less, and even more preferably 100nm or less.Within such a range, the polishing composition containing the produced anion-modified colloidal silica can polish silicon nitride film at high speed and suppress the polishing speed of silicon oxide film.The average secondary particle size of colloidal silica can be measured by, for example, dynamic light scattering method represented by laser diffraction scattering method.
[0023] The average degree of association (average secondary particle size / average primary particle size) of the raw colloidal silica is not particularly limited, and is, for example, 1.0 to 5.0, preferably 2.5 to 5.0, and more preferably 4.0 to 5.0. If it is within such a range, in a polishing composition containing the produced anion-modified colloidal silica, a silicon nitride film can be polished at high speed, and the polishing rate of a silicon oxide film can be suppressed.
[0024] The concentration of silica particles (solid content) in the raw colloidal silica is not particularly limited as long as it is a concentration suitable for ion exchange. The concentration of silica particles (solid content) in the raw colloidal silica is, for example, 1% by mass or more and 40% by mass or less, preferably 5% by mass or more and 30% by mass or less, and more preferably 10% by mass or more and 20% by mass or less.
[0025] [Ion exchange resin] The ion exchange resin is not particularly limited, but examples thereof include strongly acidic cation exchange resins, weakly acidic cation exchange resins, strongly basic anion exchange resins type I, strongly basic anion exchange resins type II, weakly basic anion exchange resins, etc. The ion exchange resin is preferably a strongly acidic cation exchange resin or a weakly acidic cation exchange resin.
[0026] The exchange group of the strongly acidic cation exchange resin may be a sulfonic acid group.
[0027] Examples of the exchange group possessed by the weakly acidic cation exchange resin include a carboxy group and a phenolic hydroxyl group.
[0028] The exchange group of the strongly basic anion exchange resin type I includes a trimethylammonium group.
[0029] The exchange group of the strongly basic anion exchange resin type II includes a dimethylethanolammonium group.
[0030] The exchange group of the weakly basic anion exchange resin may be a tertiary amino group.
[0031] As the ion exchange resin, commercially available products may be used, and examples of such commercially available products include SGC650 (manufactured by Purolite Co., Ltd.), Diaion (trademark) series (manufactured by Mitsubishi Chemical Corporation), Amberlite (trademark), and Amberjet (trademark) (manufactured by Organo Corporation).
[0032] [Ion exchange] The method for ion-exchanging the raw colloidal silica with an ion exchange resin is not particularly limited, and a conventionally known method can be used. For example, a method of mixing the raw colloidal silica with an ion exchange resin, a method of passing the raw colloidal silica through a column packed with an ion exchange resin, etc. can be mentioned.
[0033] When mixing the raw colloidal silica with the ion exchange resin, the amount of the ion exchange resin used can be appropriately adjusted according to the raw colloidal silica used. The amount of the ion exchange resin used is, for example, 10 parts by mass or more and 50 parts by mass or less, preferably 20 parts by mass or more and 30 parts by mass or less, relative to 15 parts by mass of the raw colloidal silica (solid content).
[0034] The temperature for mixing (stirring) the raw colloidal silica and the ion exchange resin is, for example, from 10° C. to 50° C., and preferably from 20° C. to 30° C. The time for mixing (stirring) the raw colloidal silica and the ion exchange resin is, for example, from 1 hour to 30 hours, and preferably from 10 hours to 20 hours.
[0035] After the ion exchange is completed, the ion exchange resin is separated and removed to obtain the ion-exchanged raw colloidal silica to be used in the modification step. The method for separating and removing the ion exchange resin is not particularly limited, and for example, the ion exchange resin is allowed to settle naturally and the supernatant liquid is collected to obtain the ion-exchanged raw colloidal silica.
[0036] When the raw colloidal silica is passed through a column packed with an ion exchange resin, the speed at which the raw colloidal silica passes through the column (space velocity) is, for example, from 1 to 30 per hour, and preferably from 5 to 15. In this case, the temperature of the raw colloidal silica is, for example, from 0°C to 50°C, and preferably from 10°C to 30°C.
[0037] The raw colloidal silica after passing the liquid can be used as the ion-exchanged raw colloidal silica in the modification step.
[0038] <Denaturation process> The manufacturing method of the present embodiment includes a modification step of anion-modifying ion-exchanged raw colloidal silica to obtain anion-modified colloidal silica. By using ion-exchanged raw colloidal silica, it is possible to suppress the generation of impurities and the aggregation of silica.
[0039] In the modification step, the specific form of the anion modification treatment is not particularly limited, and any treatment capable of anion-modifying colloidal silica among conventionally known modification treatments for colloidal silica can be appropriately used.
[0040] In the following, as a preferred embodiment, an example of a method for obtaining anion-modified modified colloidal silica by modifying raw colloidal silica with sulfonic acid group is described.In this method, the modification step includes a first reaction step of adding a silane coupling agent having a functional group that can be chemically converted into sulfonic acid group to the above-mentioned ion-exchanged raw colloidal silica, heating a mixture containing the ion-exchanged raw colloidal silica and the silane coupling agent to obtain a reactant, and a second reaction step of treating the reactant to convert the functional group into a sulfonic acid group.
[0041] (First reaction step) In the first reaction step, a silane coupling agent having a functional group that can be chemically converted to a sulfonic acid group is added to the ion-exchanged raw colloidal silica, and a mixture containing the ion-exchanged raw colloidal silica and the silane coupling agent is heated. This results in a reaction product (a silane coupling agent having a functional group that can be chemically converted to a sulfonic acid group bonded to the surface of silica particles). In this way, the silane coupling agent having a functional group different from the sulfonic acid group is reacted with the ion-exchanged raw colloidal silica, and then the functional group is converted to a sulfonic acid group (the second reaction step described below) because it is generally difficult to stably obtain a silane coupling agent in the form of a sulfonic acid group substituted.
[0042] Examples of silane coupling agents having functional groups that can be chemically converted to sulfonic acid groups include 1) silane coupling agents having sulfonic acid ester groups that can be converted to sulfonic acid groups by hydrolysis, and 2) silane coupling agents having mercapto and / or sulfide groups that can be converted to sulfonic acid groups by oxidation. Note that, since the sulfonic acid modification of the colloidal silica surface is carried out in a solution, it is preferable to use the latter coupling agents having mercapto and / or sulfide groups in order to increase the efficiency of modification.
[0043] Examples of silane coupling agents having a mercapto group include 3-mercaptopropyltrimethoxysilane, 2-mercaptopropyltriethoxysilane, 2-mercaptoethyltrimethoxysilane, 2-mercaptoethyltriethoxysilane, etc. Examples of coupling agents having a sulfide group include bis(3-triethoxysilylpropyl)disulfide, etc.
[0044] Alternatively, the silane coupling agent may be hydrolyzed in advance with an acid, and then subjected to a condensation reaction with the ion-exchanged raw material colloidal silica.
[0045] Since the silane coupling agent is difficult to dissolve in water, it is preferable to add the silane coupling agent in the form of a solution. In addition, as the solvent of the solution, it is preferable to use an organic solvent (hydrophilic solvent) for the purpose of dissolving the silane coupling agent. Examples of such organic solvents (hydrophilic solvents) include organic solvents such as methanol, ethanol, and isopropanol. As the organic solvent, methanol or ethanol is preferable from the viewpoint of low vapor pressure, and ethanol is more preferable from the viewpoint of easy handling.
[0046] The amount of the silane coupling agent used in the first reaction step is not particularly limited, but is preferably 0.5% by mass or more and 10% by mass or less, more preferably 1% by mass or more and 5% by mass or less, based on 100% by mass of silica particles (solid content) contained in the ion-exchanged raw colloidal silica. If the amount of the silane coupling agent added is 0.5% by mass or more, the surface of the silica particles can be sufficiently anionized, and when used as an abrasive (abrasive grains in a polishing composition), excellent performance can be exhibited. On the other hand, if the amount of the silane coupling agent added is 10% by mass or less, gelation of the resulting reaction product (anion-modified colloidal silica) over time can be prevented. In addition, the amount of the organic solvent (hydrophilic solvent) used to dissolve the silane coupling agent is preferably 300% by volume or more and 3000% by volume or less, more preferably 400% by volume or more and 2000% by volume or less, based on 100% by volume of the silane coupling agent.
[0047] The temperature when the silane coupling agent is added is not limited, but is preferably in the range from room temperature (about 20°C) to the boiling point of the reaction solvent. The reaction time is also not limited, but is preferably from 10 minutes to 30 hours, more preferably from 30 minutes to 20 hours. However, from the viewpoint of completing the hydrolysis of the coupling agent, it is preferable that the first reaction step is carried out under a temperature condition of 50°C or higher for 15 hours or more. The pH at the time of addition is not particularly limited.
[0048] (Second reaction step) In the second reaction step, the reaction product obtained in the first reaction step (a silane coupling agent having a functional group that can be chemically converted to a sulfonic acid group bonded to the surface of the silica particles) is treated, thereby converting the "functional group that can be chemically converted to a sulfonic acid group" possessed by the silane coupling agent into a sulfonic acid group.
[0049] The specific form of the "treatment" carried out to convert the "functional group that can be chemically converted into a sulfonic acid group" of the silane coupling agent to a sulfonic acid group is not particularly limited, and can be appropriately selected according to the structure of the silane coupling agent used. For example, when a silane coupling agent having a sulfonate ester group that can be converted into a sulfonic acid group by hydrolysis is used in the first reaction step, the functional group (sulfonate ester group) of the silane coupling agent can be hydrolyzed by carrying out a hydrolysis treatment on the reaction product. As a result, the sulfonate ester group is converted into a sulfonic acid group.
[0050] In addition, when a silane coupling agent having a mercapto group and / or a sulfide group that can be converted to a sulfonic acid group by oxidation (2) is used in the first reaction step, the functional group (mercapto group and / or sulfide group) of the silane coupling agent can be oxidized by subjecting the reaction product to an oxidation treatment, whereby the mercapto group or sulfide group is converted to a sulfonic acid group.
[0051] To subject the reactant to oxidation treatment, for example, the reactant may be reacted with an oxidizing agent. Examples of the oxidizing agent include nitric acid, hydrogen peroxide, oxygen, ozone, organic peracids (percarboxylic acids), bromine, hypochlorite, potassium permanganate, and chromic acid. Among these oxidizing agents, hydrogen peroxide and organic peracids (peracetic acid, perbenzoic acids) are preferred because they are relatively easy to handle and have a good oxidation yield. In addition, considering the by-products of the reaction, it is most preferred to use hydrogen peroxide. From the viewpoint of ensuring the amount required for the reaction and reducing the amount of residual oxidizing agent, the amount of oxidizing agent added is preferably 3 to 5 times the amount of the silane coupling agent by mole. By setting the amount of oxidizing agent added to a value within such a range, it is possible to minimize the residual oxidizing agent concentration in the obtained anion-modified colloidal silica. There is no particular restriction on the specific value of the residual oxidizing agent concentration in the obtained anion-modified colloidal silica, but it is preferably 1000 mass ppm or less, more preferably 700 mass ppm or less, and particularly preferably 500 mass ppm or less. Here, if the residual oxidizing agent concentration in the obtained anion-modified colloidal silica exceeds 1000 mass ppm, when the anion-modified colloidal silica itself or the polishing composition to which the anion-modified colloidal silica is added as an abrasive (abrasive grain) is stored or transported in a sealed container, the oxidizing agent such as hydrogen peroxide may decompose to generate gas such as oxygen, and the internal pressure of the container may increase. On the other hand, as described above, the residual oxidizing agent concentration in the obtained anion-modified colloidal silica is reduced, which is preferable because it reduces the risk of such an increase in internal pressure. In addition, when used as a polishing composition, it has the advantage that the occurrence of problems such as wafer dishing, which may occur when a large amount of oxidizing agent is contained, can be suppressed. In addition, the colloidal silica and the silane coupling agent have a stable structure in the oxidation reaction except for the functional group that is oxidized (converted) to a sulfonic acid group, so there are no by-products.
[0052] When the anion-modified colloidal silica obtained according to the above method contains a solvent other than water, a solvent removal step for removing the solvent may be included after the modification step, if necessary. For example, the dispersion medium mainly consisting of the reaction solvent may be replaced with water, or the solvent may be removed using an evaporator. This water replacement may be performed after the addition of the silane coupling agent and before the addition of the oxidizing agent. The method for replacing the solvent other than water with water is not particularly limited, and for example, a method of dropping a certain amount of water while heating the anion-modified colloidal silica may be mentioned. In addition, a method of separating the anion-modified colloidal silica from the solvent other than water by precipitation / separation, centrifugation, etc., and then redispersing it in water may be mentioned.
[0053] <Polishing composition> The anion-modified colloidal silica obtained by the above-mentioned production method can be used as an abrasive (abrasive grains) contained in a polishing composition. Thus, one embodiment of the present invention is a polishing composition containing abrasive grains and a dispersion medium, and the abrasive grains contain the anion-modified colloidal silica obtained by the above-mentioned production method.
[0054] The lower limit of the content of the abrasive grains in the polishing composition of this embodiment is preferably 0.01 mass% or more, more preferably 0.05 mass% or more, even more preferably 0.1 mass% or more, and even more preferably 1.0 mass% or more. The upper limit of the content of the abrasive grains is preferably 20 mass% or less, more preferably 10 mass% or less, and even more preferably 5 mass% or less.
[0055] The dispersion medium preferably contains water. Furthermore, from the viewpoint of preventing the influence of impurities on other components of the polishing composition, it is preferable to use water with as high purity as possible. Specifically, it is preferable to use deionized water (ion-exchanged water), pure water, ultrapure water, distilled water, etc. Furthermore, the dispersion medium may further contain an organic solvent, etc., for the purpose of controlling the dispersibility of other components of the polishing composition.
[0056] The polishing composition of the present embodiment may further contain, as necessary, known additives such as a pH adjuster, a chelating agent, a thickener, an oxidizing agent, a dispersant, a surface protective agent, a wetting agent, a surfactant, an antirust agent, an antiseptic agent, an antifungal agent, etc. The content of the additives may be appropriately set depending on the purpose of their addition.
[0057] As the pH adjuster, known acids, bases other than basic inorganic compounds, or salts thereof can be used. Specific examples of acids that can be used as a pH adjuster include inorganic acids such as hydrochloric acid, sulfuric acid, hydrofluoric acid, boric acid, carbonic acid, hypophosphorous acid, phosphorous acid, and phosphoric acid, and organic acids such as formic acid, acetic acid, propionic acid, butyric acid, valeric acid, 2-methylbutyric acid, n-hexanoic acid, 3,3-dimethylbutyric acid, 2-ethylbutyric acid, 4-methylpentanoic acid, n-heptanoic acid, 2-methylhexanoic acid, n-octanoic acid, 2-ethylhexanoic acid, benzoic acid, glycolic acid, salicylic acid, glyceric acid, oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, maleic acid, phthalic acid, malic acid, tartaric acid, citric acid, lactic acid, diglycolic acid, 2-furancarboxylic acid, 2,5-furandicarboxylic acid, 3-furancarboxylic acid, 2-tetrahydrofurancarboxylic acid, methoxyacetic acid, methoxyphenylacetic acid, and phenoxyacetic acid.
[0058] Examples of bases other than basic inorganic compounds that can be used as pH adjusters include aliphatic amines such as ethanolamine and 2-amino-2-ethyl-1,3-propanediol, aromatic amines, basic organic compounds such as quaternary ammonium hydroxide, and ammonia.
[0059] The above pH adjusters may be used alone or in combination of two or more kinds.
[0060] The amount of the pH adjuster to be added is not particularly limited, and may be adjusted so that the pH of the polishing composition falls within a desired range. The amount of the saturation can be adjusted appropriately.
[0061] The upper limit of the pH of the polishing composition of this embodiment is preferably 5.0 or less, more preferably 4.0 or less, and even more preferably 3.0 or less. The lower limit of the pH of the polishing composition is not particularly limited, but is preferably 1.5 or more.
[0062] The method for producing the polishing composition of this embodiment is not particularly limited, and can be obtained by, for example, stirring and mixing abrasive grains and, if necessary, additives in a dispersion medium.The temperature when mixing each component is not particularly limited, but is preferably 10°C or more and 40°C or less, and may be heated to increase dissolution speed.In addition, the mixing time is also not particularly limited.
[0063] <Polishing method> One aspect of the present invention is a polishing method comprising polishing an object to be polished with the polishing composition described above.
[0064] The object to be polished includes silicon nitride and silicon oxide. Examples of films including silicon oxide include a TEOS (Tetraethyl Orthosilicate) type silicon oxide film (hereinafter, simply referred to as a "TEOS film") produced using tetraethyl orthosilicate as a precursor, a HDP (High Density Plasma) film, a USG (Undoped Silicate Glass) film, a PSG (Phosphorus Silicate Glass) film, a BPSG (Boron-Phospho Silicate Glass) film, and a RTO (Rapid Thermal Oxidation) film.
[0065] In addition to silicon nitride and silicon oxide, the polishing target may include other materials, such as silicon carbonitride, polysilicon, titanium nitride, tungsten, and the like.
[0066] As a polishing device, a general polishing device can be used which is equipped with a holder for holding a substrate or the like having an object to be polished, a motor whose rotation speed can be changed, and a polishing platen onto which a polishing pad (polishing cloth) can be attached.
[0067] The polishing pad may be made of any material, including general nonwoven fabric, polyurethane, and porous fluororesin, without any particular limitations. The polishing pad is preferably provided with grooves for accumulating the polishing composition.
[0068] There is no particular restriction on the polishing conditions, for example, the rotation speed of the polishing platen is preferably 10 rpm or more and 500 rpm or less, the rotation speed of the carrier is preferably 10 rpm or more and 500 rpm or less, and the pressure (polishing pressure) applied to the substrate having the object to be polished is preferably 0.1 psi or more and 10 psi or less. There is no particular restriction on the method of supplying the polishing composition to the polishing pad, for example, a method of continuously supplying the composition by a pump or the like is adopted. There is no restriction on the amount of supply, but it is preferable that the surface of the polishing pad is always covered with the polishing composition of the present invention. EXAMPLES
[0069] The present invention will be described in more detail using the following examples and comparative examples. However, the technical scope of the present invention is not limited to the following examples. Unless otherwise specified, "%" and "parts" mean "% by mass" and "parts by mass", respectively. In the following examples, unless otherwise specified, the operations were performed under the conditions of room temperature (20 to 25°C) / relative humidity 40 to 50% RH.
[0070] Example 1 1 kg of aluminate-modified colloidal silica (silica particle concentration: 15 mass%, average primary particle size: 12 nm, average secondary particle size: 54 nm, average degree of association: 4.5) produced by the sodium silicate method was mixed with 200 mL of ion exchange resin (strong acid cation exchange resin SGC650; manufactured by Purolite Co., Ltd.) and stirred for 18 hours to carry out ion exchange. After completion of the ion exchange, the ion exchange resin was allowed to settle naturally, and the supernatant liquid (ion-exchanged colloidal silica) was collected.
[0071] 5 mL of 3-mercaptopropyltrimethoxysilane mixed with 20 mL of ethanol was added to 900 mL of ion-exchanged colloidal silica, and the mixture was heated at 70° C. for 18 hours. Then, 80 mL of 31% by mass hydrogen peroxide solution was added, and the mixture was heated at 65° C. for 18 hours. After heating, the ethanol was removed using an evaporator to prepare anion-modified colloidal silica.
[0072] Example 2 Anion-modified colloidal silica was prepared in the same manner as in Example 1, except that the amount of 3-mercaptopropyltrimethoxysilane added was 4 mL.
[0073] Example 3 An anion-modified colloidal silica was prepared in the same manner as in Example 1, except that the ethanol was not removed using an evaporator.
[0074] Example 4 Anion-modified colloidal silica was prepared in the same manner as in Example 1, except that the amount of 3-mercaptopropyltrimethoxysilane added was 3 mL.
[0075] Example 5 Anion-modified colloidal silica was prepared in the same manner as in Example 1, except that the amount of 3-mercaptopropyltrimethoxysilane added was 2 mL.
[0076] Example 6 Anion-modified colloidal silica was prepared in the same manner as in Example 1, except that the amount of 3-mercaptopropyltrimethoxysilane added was 1 mL.
[0077] Example 7 1 kg of aluminate-modified colloidal silica produced by the sodium silicate method (silica particle concentration: 15 mass%, average primary particle diameter: 12 nm, average secondary particle diameter: 54 nm, average degree of association: 4.5) was subjected to ion exchange with 200 mL of ion exchange resin for 18 hours.
[0078] 20 mL of methanol and 5 mL of 3-mercaptopropyltrimethoxysilane were added to 900 mL of the ion-exchanged colloidal silica, and the mixture was heated at 60° C. for 18 hours. Then, 80 mL of a 31% by mass hydrogen peroxide solution was added, and the mixture was heated at 65° C. for 18 hours. After heating, the methanol was removed using an evaporator to prepare an anion-modified colloidal silica.
[0079] Comparative Example 1 A comparative colloidal silica was prepared by subjecting 1 kg of aluminate-modified colloidal silica (silica particle concentration: 15 mass%, average primary particle diameter: 12 nm, average secondary particle diameter: 54 nm, average degree of association: 4.5) produced by the sodium silicate method to ion exchange with 200 mL of ion exchange resin for 18 hours.
[0080] Comparative Example 2 1 kg of aluminate-modified colloidal silica produced by the sodium silicate method (silica particle concentration: 15 mass%, average primary particle diameter: 12 nm, average secondary particle diameter: 54 nm, average degree of association: 4.5) was subjected to ion exchange with 200 mL of ion exchange resin for 18 hours.
[0081] To 900 mL of the ion-exchanged colloidal silica, 4 mL of 3-mercaptopropyltrimethoxysilane mixed with 20 mL of ethanol was added, and the mixture was heated at 70° C. for 18 hours to prepare a comparative colloidal silica.
[0082] Comparative Example 3 1 kg of aluminate-modified colloidal silica produced by the sodium silicate method (silica particle concentration: 15 mass%, average primary particle diameter: 12 nm, average secondary particle diameter: 54 nm, average degree of association: 4.5) was subjected to ion exchange with 200 mL of ion exchange resin for 18 hours.
[0083] To 920 mL of the ion-exchanged colloidal silica, 80 mL of a 31 mass % hydrogen peroxide solution was added, and the mixture was heated at 65° C. for 18 hours. Ethanol was removed using an evaporator to prepare a comparative colloidal silica.
[0084] Comparative Example 4 4 mL of 3-mercaptopropyltrimethoxysilane mixed with 20 mL of ethanol was added to 900 mL of aluminate-modified colloidal silica (silica particle concentration: 15% by mass, average primary particle size: 12 nm, average secondary particle size: 54 nm, average degree of association: 4.5) produced by the sodium silicate method, and the mixture was heated at 70°C for 18 hours. Then, 80 mL of a 31% by mass hydrogen peroxide solution was added, and the mixture was heated at 65°C for 18 hours. The ethanol was removed using an evaporator to prepare colloidal silica for the comparative example. Comparative Example 5 1 kg of colloidal silica produced by the sol-gel method (silica particle concentration: 20 mass%, average primary particle size: 35 nm, average secondary particle size: 69 nm, average degree of association: 2.0) was mixed with 200 mL of ion exchange resin (strong acid cation exchange resin SGC650; manufactured by Purolite Co., Ltd.) and stirred for 18 hours to carry out ion exchange. After completion of the ion exchange, the ion exchange resin was allowed to settle naturally, and the supernatant liquid (ion-exchanged colloidal silica) was collected.
[0085] 5 mL of 3-mercaptopropyltrimethoxysilane mixed with 20 mL of ethanol was added to 900 mL of ion-exchanged colloidal silica, and the mixture was heated at 70° C. for 18 hours. Then, 80 mL of 31% by mass hydrogen peroxide solution was added, and the mixture was heated at 65° C. for 18 hours. After heating, the ethanol was removed using an evaporator to prepare a colloidal silica of the comparative example.
[0086] [evaluation] <Evaluation of average secondary particle size> The average secondary particle size of the anion-modified colloidal silica prepared in Example 2 and the colloidal silica prepared in Comparative Example 4 was measured by a light scattering method using laser light. The measuring device used was a dynamic light scattering particle size distribution analyzer UPA-UT151 manufactured by Nikkiso Co., Ltd.
[0087] The average secondary particle diameter of the anion-modified colloidal silica prepared in Example 2 was 54 nm, and the average secondary particle diameter of the colloidal silica prepared in Comparative Example 4 was 80 nm.
[0088] Therefore, it is understood that the aggregation of silica particles can be suppressed by carrying out ion exchange.
[0089] <Evaluation of polishing speed> (Preparation of Polishing Composition) The anion-modified colloidal silica of Examples 1 to 7, the colloidal silica of Comparative Examples 1 to 5, or the colloidal silica of Comparative Example 6 (aluminate-modified colloidal silica produced by a sodium silicate method (silica particle concentration: 15 mass%, average primary particle size: 54 nm, average degree of association: 4.5)) obtained above was mixed with ion-exchanged water to give a silica particle concentration of 4 mass%, to obtain a mixed liquid. Then, maleic acid was added to the mixed liquid so that the pH was 2.0, to prepare polishing compositions 1 to 13.
[0090] The pH of the polishing composition (liquid temperature: 25° C.) was confirmed with a pH meter (manufactured by Horiba, Ltd., model number: LAQUA).
[0091] (Zeta potential measurement) The polishing compositions 1 to 13 prepared above were fed to an ELS-Z2 manufactured by Otsuka Electronics Co., Ltd., and measured by a laser Doppler method (electrophoretic light scattering measurement method) using a flow cell at a measurement temperature of 25°C. The obtained data was analyzed by the Smoluchowski formula to calculate the zeta potential of the colloidal silica contained in the polishing composition. The results are shown in Table 1.
[0092] (Evaluation of polishing speed) The object to be polished is 200mm wafer (SiN (silicon nitride) film), 200mm wafer (TEOS (silicon oxide film)), Each wafer was polished using the polishing composition obtained above under the following polishing conditions, and the polishing rate was measured. Also, the selectivity was calculated.
[0093] [Polishing conditions] Polishing machine: CMP single-sided polishing machine for 200mm wafers Polishing pad: Polyurethane pad (IC1010: manufactured by Rohm and Haas) Pressure: 4.0 psi (approx. 27.6 kPa) Platen rotation speed: 90 rpm Head (carrier) rotation speed: 87 rpm Flow rate of polishing composition: 200ml / min Polishing time: 1 minute.
[0094] [Polishing speed] The polishing speed (polishing rate) was calculated by the following formula.
[0095]
number
[0096] The film thickness was measured using an optical interference type film thickness measuring device (KLA-Tencor Corporation, type The results were calculated using the ASET (number: ASET) and the difference was divided by the polishing time. As shown in Table 1.
[0097] [Table 1]
[0098] As shown in Table 1, it can be seen that by using the anion-modified colloidal silica of the Examples, it is possible to polish a silicon nitride film at a higher speed and suppress the polishing rate of a silicon oxide film, compared to the colloidal silica of the Comparative Examples.
Claims
1. an ion exchange step of ion-exchanging the raw colloidal silica obtained by the sodium silicate method with an ion exchange resin; a first reaction step of adding a silane coupling agent having a functional group that can be chemically converted into a sulfonic acid group in a state of solution to the ion-exchanged raw colloidal silica (wherein the solvent of the solution contains an organic solvent), and heating a mixture containing the ion-exchanged raw colloidal silica and the silane coupling agent to obtain a reaction product; a second reaction step in which the reaction product is treated to convert the functional group into a sulfonic acid group; a solvent removal step of removing the solvent after the second reaction step; A method for producing an anion-modified colloidal silica, comprising:
2. The method according to claim 1 , wherein the solvent of the solution is an organic solvent.
Citation Information
Patent Citations
Production of high-purity aqueous silica sol
JP1993097422A
Device and method for grinding semiconductor wafer
JP1997314466A
Method for producing high purity aqueous silica sol
JP2006213541A
Polishing composition and polishing method using the same
JP2012040671A
Polishing composition and manufacturing method thereof, polishing method, and method for manufacturing semiconductor substrate
JP2019169589A