Solid oxide fuel cell and method for producing same
The fuel cell design with convex portions on the electrolyte layer and matching concavities on the intermediate and cathode layers addresses the issue of increased reaction resistance, enhancing power generation efficiency.
Patent Information
- Application Number
- JP2020170421
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-08
- Publication Date
- 2024-12-05
- Estimated Expiration
- 2040-10-08
AI Technical Summary
The provision of a reaction prevention film in solid oxide fuel cells increases reaction resistance during power generation.
The solid oxide fuel cell design includes an electrolyte layer with convex portions arranged in a two-dimensional direction, an intermediate layer with matching convexities, and a cathode with corresponding concavities, enhancing the contact area between the intermediate and cathode layers to reduce reaction resistance.
This configuration reduces reaction resistance by increasing the contact interface area, leading to improved power generation performance.
Smart Images

Figure 0007594878000002 
Figure 0007594878000003 
Figure 0007594878000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a solid oxide fuel cell and a method for producing the same. [Background technology]
[0002] A solid oxide fuel cell has a structure in which a solid oxide electrolyte is sandwiched between an anode and a cathode. The cathode used in such a solid oxide fuel cell may react with the solid oxide electrolyte. Therefore, in order to suppress the reaction between the solid oxide electrolyte and the cathode, a technology has been disclosed in which a reaction prevention film such as GDC is provided between the cathode and the solid oxide electrolyte (for example, see Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2017-504946 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, providing a reaction-preventing film may increase reaction resistance during power generation.
[0005] The present invention has been made in consideration of the above-mentioned problems, and has an object to provide a solid oxide fuel cell capable of reducing reaction resistance, and a method for manufacturing the same. [Means for solving the problem]
[0006] The solid oxide fuel cell of the present invention comprises an electrolyte layer containing a solid oxide having oxide ion conductivity, an intermediate layer having oxide ion conductivity provided on the electrolyte layer, and a cathode provided on the intermediate layer, wherein the electrolyte layer has a plurality of protrusions arranged in a two-dimensional direction in a planar view on the surface facing the intermediate layer, and the cathode-side surface of the intermediate layer is formed to follow the shape of the surface of the electrolyte layer facing the intermediate layer.
[0007] In the solid oxide fuel cell, the plurality of protrusions may be formed in a particulate form.
[0008] In the above solid oxide fuel cell, the electrolyte layer includes a plurality of crystal particles, and the convex portion is formed so as to protrude toward the intermediate layer from the crystal particles on the surface of the electrolyte layer facing the intermediate layer, and the crystal particles on the surface of the electrolyte layer facing the intermediate layer may be larger than the convex portion.
[0009] In the solid oxide fuel cell, the size of crystal grains on the surface of the electrolyte layer facing the intermediate layer may be 1 μm or more and 5 μm or less.
[0010] In the solid oxide fuel cell, the number of protrusions in crystal grains on the surface of the electrolyte layer facing the intermediate layer may be 3 to 15 in a plan view of the electrolyte layer.
[0011] In the solid oxide fuel cell, there may be no crystal grain boundary between at least any of the protrusions and the crystal grains on the surface of the electrolyte layer facing the intermediate layer.
[0012] In the solid oxide fuel cell, the size of the protrusions may be in the range of 0.05 to 0.8 times the size of crystal grains on the surface of the electrolyte layer facing the intermediate layer.
[0013] In the solid oxide fuel cell, the height of the protrusions may be in the range of 0.025 to 0.4 times the size of crystal grains on the surface of the electrolyte layer facing the intermediate layer.
[0014] In the solid oxide fuel cell, the size of the protrusions may be not less than 0.2 μm and not more than 1.5 μm.
[0015] The method for producing a solid oxide fuel cell according to the present invention is characterized by the steps of: preparing an electrolyte layer green sheet by applying a slurry containing an oxide ion conductive material powder; applying a slurry containing an oxide ion conductive material powder having a D50% particle size smaller than the D50% particle size of the oxide ion conductive material powder in the electrolyte layer green sheet and resin particles onto the electrolyte layer green sheet, followed by firing; forming an intermediate layer having oxide ion conductivity but no cathode activity on the electrolyte layer obtained by firing, and forming a cathode on the intermediate layer. Effect of the Invention
[0016] According to the present invention, it is possible to provide a solid oxide fuel cell capable of reducing reaction resistance and a method for manufacturing the same. [Brief description of the drawings]
[0017] [Figure 1] 2 is a schematic cross-sectional view illustrating a stack structure of a fuel cell. FIG. [Diagram 2] FIG. 2 is an enlarged cross-sectional view illustrating details of the support, the mixed layer, and the anode. [Diagram 3] (a) is an enlarged cross-sectional view from the electrolyte layer to the cathode, and (b) is a plan view of the electrolyte layer. [Figure 4] 1 is a plan view of an electrolyte layer. [Diagram 5] 13(a) and (b) are diagrams for explaining the size of the protrusions. [Figure 6] FIG. 2 is a diagram illustrating a flow of a method for manufacturing a fuel cell. [Figure 7]4A to 4C are diagrams illustrating an electrolyte layer green sheet and a concave-convex layer green sheet in a lamination step. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] Hereinafter, an embodiment will be described with reference to the drawings.
[0019] Fig. 1 is a schematic cross-sectional view illustrating a stacked structure of a solid oxide fuel cell 100. As illustrated in Fig. 1, the fuel cell 100 has a structure in which a mixed layer 20, an anode 30, an electrolyte layer 40, an intermediate layer 50, and a cathode 60 are stacked in this order on a support 10, for example. A plurality of fuel cells 100 may be stacked to form a fuel cell stack.
[0020] The electrolyte layer 40 is a dense layer mainly composed of a solid oxide having oxide ion conductivity and having gas impermeability. The electrolyte layer 40 is preferably mainly composed of scandia-yttria stabilized zirconium oxide (ScYSZ), YSZ (yttria stabilized zirconium oxide), GDC (Gd-doped ceria) in which Gd (gadolinium) is doped into CeO2, or the like. When ScYSZ is used, the oxide ion conductivity is highest when the concentration of Y2O3+Sc2O3 is between 6 mol% and 15 mol%, and it is desirable to use a material with this composition. In addition, the thickness of the electrolyte layer 40 is preferably 20 μm or less, and more desirably 10 μm or less. The thinner the electrolyte, the better, but in order to manufacture it so that gas does not leak from both sides, a thickness of 1 μm or more is desirable.
[0021] The cathode 60 is an electrode having electrode activity as a cathode, and has electronic conductivity and oxide ion conductivity. For example, the cathode 60 is mainly composed of a ceramic material having electronic conductivity and oxide ion conductivity. As the ceramic material, for example, a LaCoO3-based material, a LaMnO3-based material, a LaFeO3-based material, etc. can be used. For example, as the LaCoO3-based material, LSC (lanthanum strontium cobaltite) etc. can be used. LSC is LaCoO3 doped with Sr (strontium).
[0022] The intermediate layer 50 is mainly composed of a component that prevents a reaction between the electrolyte layer 40 and the cathode 60. The constituent material of the intermediate layer 50 is different from the constituent material of the electrolyte layer 40. The intermediate layer 50 has oxide ion conductivity, but does not have electrode activity as a cathode. For example, the intermediate layer 50 has a structure in which an additive is added to ceria (CeO2). The additive is not particularly limited. For example, the intermediate layer 50 may be made of GDC (e.g., Ce 0.8 Gd 0.2 O 2-x As an example, when the electrolyte layer 40 contains ScYSZ and the cathode 60 contains LSC, the intermediate layer 50 prevents the following reaction: Sr+ZrO2 → SrZrO3 La+ZrO3→La2Zr2O7
[0023] Fig. 2 is an enlarged cross-sectional view illustrating the details of the support 10, the mixed layer 20, and the anode 30. As illustrated in Fig. 2, the support 10 is a member that has gas permeability and is capable of supporting the mixed layer 20, the anode 30, the electrolyte layer 40, the intermediate layer 50, and the cathode 60. The support 10 is a metal porous body mainly composed of a metal, such as a porous body of an Fe-Cr alloy.
[0024] The anode 30 is an electrode having electrode activity as an anode, and has an electrode skeleton made of a ceramic material. The electrode skeleton does not contain metal components. In this configuration, the decrease in the porosity of the anode due to the coarsening of the metal components during firing in a high-temperature reducing atmosphere is suppressed. In addition, alloying with the metal components of the support 10 is suppressed, and the decrease in catalytic function is suppressed.
[0025] The electrode skeleton of the anode 30 has electronic conductivity and oxide ion conductivity. The anode 30 contains an electronically conductive ceramic 31. As the electronically conductive ceramic 31, for example, a perovskite oxide having a composition formula of ABO3, in which the A site is at least one selected from the group consisting of Ca, Sr, Ba, and La, and the B site is at least one selected from Ti and Cr, can be used. The molar ratio of the A site to the B site may be B≧A. Specifically, as the electronically conductive ceramic 31, a LaCrO3-based material, a SrTiO3-based material, or the like can be used.
[0026] The electrode skeleton of the anode 30 contains oxide ion conductive ceramics 32. The oxide ion conductive ceramics 32 are ScYSZ or the like. For example, it is preferable to use ScYSZ having a composition range of 5 mol% to 16 mol% of scandia (Sc2O3) and 1 mol% to 3 mol% of yttria (Y2O3). It is more preferable to use ScYSZ in which the total amount of scandia and yttria added is 6 mol% to 15 mol%. This is because the oxide ion conductivity is highest in this composition range. The oxide ion conductive ceramics 32 are, for example, materials having an oxide ion transport number of 99% or more. GDC or the like may be used as the oxide ion conductive ceramics 32. In the example of FIG. 2, the same solid oxide as the solid oxide contained in the electrolyte layer 40 is used as the oxide ion conductive ceramics 32.
[0027] As shown in FIG. 2, in the anode 30, for example, an electron conductive ceramic 31 and an oxide ion conductive ceramic 32 form an electrode skeleton. This electrode skeleton forms a plurality of voids. An anode catalyst is supported on the surface of the electrode skeleton in the void portion. Therefore, in the electrode skeleton that is formed spatially continuously, a plurality of anode catalysts are arranged in a spatially dispersed manner. It is preferable to use a composite catalyst as the anode catalyst. For example, it is preferable that an oxide ion conductive ceramic 33 and a catalytic metal 34 are supported as the composite catalyst on the surface of the electrode skeleton. For example, Y-doped BaCe 1-x Zr x O3(BCZY, x=0~1), Y-doped SrCe 1-x Zr x O3 (SCZY, x=0-1), Sr-doped LaScO3 (LSS), GDC, etc. can be used. Ni, etc. can be used as the catalytic metal 34. The oxide ion conductive ceramics 33 may have the same composition as the oxide ion conductive ceramics 32, or may have a different composition. The metal functioning as the catalytic metal 34 may be in the form of a compound when power is not being generated. For example, Ni may be in the form of NiO (nickel oxide). These compounds are reduced by a reducing fuel gas supplied to the anode 30 during power generation, and take the form of a metal functioning as an anode catalyst.
[0028] The mixed layer 20 contains a metal material 21 and a ceramic material 22. In the mixed layer 20, the metal material 21 and the ceramic material 22 are randomly mixed. Therefore, a structure in which a layer of the metal material 21 and a layer of the ceramic material 22 are laminated is not formed. The mixed layer 20 is also porous, and a plurality of voids are formed. The metal material 21 is not particularly limited as long as it is a metal. In the example of FIG. 2, the same metal material as the support 10 is used as the metal material 21. For example, ScYSZ, GDC, SrTiO3-based material, LaCrO3-based material, etc. can be used as the ceramic material 22. Since the SrTiO3-based material and the LaCrO3-based material have high electronic conductivity, the ohmic resistance in the mixed layer 20 can be reduced.
[0029] The fuel cell 100 generates power by the following actions. An oxidant gas containing oxygen, such as air, is supplied to the cathode 60. In the cathode 60, due to the effect of the electrode activity of the cathode 60, the oxygen that has reached the cathode 60 reacts with electrons supplied from an external electric circuit to become oxide ions. The oxide ions move to the anode 30 side by conducting through the intermediate layer 50 and the electrolyte layer 40. Meanwhile, a fuel gas containing hydrogen, such as hydrogen gas or reformed gas, is supplied to the support 10. The fuel gas reaches the anode 30 through the support 10 and the mixed layer 20. Due to the effect of the electrode activity of the anode 30, the hydrogen that has reached the anode 30 releases electrons at the anode 30 and reacts with oxide ions that have been conducted through the electrolyte layer 40 from the cathode 60 side to become water (H2O). The released electrons are taken out by the external electric circuit. The electrons taken out are supplied to the cathode 60 after performing electrical work. Power is generated by the above actions.
[0030] In a fuel cell 100 provided with an intermediate layer 50, the location that contributes most to the cathode reaction is the interface where the intermediate layer 50 and the cathode 60 come into contact. The area of this contact interface is inversely proportional to the reaction resistance. Therefore, the larger the contact area per unit area, the lower the reaction resistance per unit area. For these reasons, the challenge in developing the fuel cell 100 is to increase the contact area between the intermediate layer 50 and the cathode 60.
[0031] Therefore, the fuel cell 100 according to this embodiment has a structure that improves the contact area between the intermediate layer 50 and the cathode 60. FIG. 3(a) is an enlarged cross-sectional view from the electrolyte layer 40 to the cathode 60. FIG. 3(b) is a diagram illustrating the electrolyte layer 40 in a plan view. As illustrated in FIG. 3(a), the electrolyte layer 40 is formed such that a plurality of protrusions 41 are arranged at a predetermined interval on the surface on the intermediate layer 50 side. The protrusions 41 protrude toward the intermediate layer 50 side. As illustrated in FIG. 3(b), the protrusions 41 are arranged not only in one direction but also in two-dimensional directions within the plane of the electrolyte layer 40. The two-dimensional directions do not necessarily need to be orthogonal within the plane of the electrolyte layer 40, as long as they intersect. In a plan view of the electrolyte layer 40, the protrusions 41 are in the form of particles and are arranged randomly within the plane of the electrolyte layer 40.
[0032] Since the electrolyte layer 40 has a plurality of convex portions 41 on the intermediate layer 50 side, the intermediate layer 50 also has concaves and convexes along the concaves and convexes formed by the plurality of convex portions 41. That is, in the intermediate layer 50, as illustrated in FIG. 3(a), convex portions 51 are formed on the cathode 60 side so as to follow the shape of the convex portions 41. That is, in a plan view of the electrolyte layer 40, the positions of the convex portions 41 and the convex portions 51 approximately coincide with each other. Therefore, the intermediate layer 50 also has concaves and convexes formed so as to be aligned in two-dimensional directions in the plane. Note that the intermediate layer 50 has concaves formed on the surface on the electrolyte layer 40 side so as to follow the shape of the convex portions 41.
[0033] Since the intermediate layer 50 has a plurality of protrusions 51 on the cathode 60 side, the surface of the cathode 60 on the intermediate layer 50 side also has protrusions and recesses along the protrusions and recesses formed by the plurality of protrusions 51. Therefore, the area of the contact interface between the intermediate layer 50 and the cathode 60 is increased. In addition, since the directions in which the protrusions and recesses of the intermediate layer 50 and the cathode 60 are aligned are two-dimensional in the plane, the area of the contact interface between the intermediate layer 50 and the cathode 60 is further increased. In this configuration, the number of reaction sites per unit area is increased, and the reaction resistance of the cathode 60 can be reduced.
[0034] Since the intermediate layer 50 has projections and recesses on both sides thereof so that the positions of the projections 41 and 51 are substantially aligned in a plan view of the electrolyte layer 40, the intermediate layer 50 is prevented from becoming thicker in parts, and the distance between the electrolyte layer 40 and the cathode 60 is shortened. Therefore, the reaction resistance of the cathode 60 can be reduced.
[0035] If the protrusions 41 are too large, the contact area between the intermediate layer 50 and the cathode 60 may become small. Therefore, it is preferable to set an upper limit on the size of the protrusions 41. The size of the protrusions 41 is, for example, preferably 1.5 μm or less, more preferably 1 μm or less, and even more preferably 0.5 μm or less. When the surface of the intermediate layer 50 is observed with a SEM (scanning electron microscope), protrusions 41 that are nearly spherical are observed, as shown in FIG. 3(b). The size of the protrusions 41 is approximately the same as the irregularity interval b shown in FIG. 5(b).
[0036] The average size of each protrusion 41 is preferably 1.5 μm or less, more preferably 1 μm or less, and even more preferably 0.5 μm or less. Three or more SEM photographs of the cross section are taken at a magnification of 10,000 times, and the unevenness interval b on the surface of each photograph is measured and the average value is taken as the average size.
[0037] On the other hand, if the protrusions 41 are too small, the cathode material will not easily enter the recesses, and as a result, the contact between the cathode 60 and the intermediate layer 50 may be point contact. Therefore, the contact area between the cathode 60 and the intermediate layer 50 may become smaller, which may cause problems such as increased reaction resistance. Therefore, it is preferable to set a lower limit for the size of the protrusions 41. The size of the protrusions 41 is, for example, preferably 0.2 μm or more, more preferably 0.5 μm or more, and even more preferably 0.8 μm or more.
[0038] Moreover, the average size of each of the protrusions 41 is preferably 0.2 μm or more, more preferably 0.5 μm or more, and even more preferably 0.8 μm or more.
[0039] As illustrated in FIG. 3(a), the electrolyte layer 40 includes a plurality of crystal grains 42. Each protrusion 41 is formed so as to protrude from the crystal grain 42 on the surface on the intermediate layer 50 side toward the intermediate layer 50 side. If the crystal grain 42 on the surface on the intermediate layer 50 side is large, the number of crystal grain boundaries is reduced, and the resistance (grain boundary resistance) when oxide ions pass through the cross section of the electrolyte layer 40 is reduced, resulting in good power generation performance. Therefore, it is preferable that the crystal grain 42 on the surface on the intermediate layer 50 side is larger than the protrusion 41. For example, the grain size of the crystal grain 42 on the surface on the intermediate layer 50 side of the electrolyte layer 40 is the maximum diameter in a direction parallel to the surface, and is preferably 1 μm or more, more preferably 2 μm or more, and even more preferably 3 μm or more.
[0040] The average grain size of each crystal grain 42 on the surface of the electrolyte layer 40 on the intermediate layer 50 side is preferably 1 μm or more, more preferably 2 μm or more, and even more preferably 3 μm or more. The average grain size of each crystal grain 42 may be determined by polishing the cell cross section, processing the cell cross section so that the grain boundaries between the electrolyte layer 40 and the protrusions 41 are visible by any one of chemical aging, CP processing, laser processing, and FIB processing, taking a cross-sectional image by an observation method such as SEM, STEM (scanning transmission electron microscope), and TEM (transmission electron microscope), taking three or more photographs at a magnification of 10,000 times, measuring the grain sizes of the particles in contact with the intermediate layer 50 in the electrolyte layer 40 in the photographs, the grain boundaries of which can all be observed, and averaging the measured values.
[0041] On the other hand, if the crystal grains 42 on the surface of the electrolyte layer 40 facing the intermediate layer 50 are too large, for example, when the thickness of the electrolyte layer 40 is reduced to 10 μm or less, cracks are likely to occur in the electrolyte layer 40, which may cause problems such as leakage of anode gas and cathode gas. Therefore, it is preferable to set an upper limit on the size of the crystal grains 42 on the surface of the intermediate layer 50. For example, the grain size of the crystal grains 42 on the surface of the intermediate layer 50 is preferably 5 μm or less, more preferably 4.5 μm or less, and even more preferably 4 μm or less.
[0042] The average grain size of the crystal grains 42 on the intermediate layer 50 side surface of the electrolyte layer 40 is preferably 5 μm or less, more preferably 4.5 μm or less, and even more preferably 4 μm or less.
[0043] For example, as illustrated in FIG. 4, in a plan view of the electrolyte layer 40, the number of protrusions 41 in the crystal grains 42 on the surface on the intermediate layer 50 side is about 3 to 15. The average value of the number of protrusions 41 in each crystal grain 42 on the surface of the electrolyte layer 40 on the intermediate layer 50 side is about 3 to 15. The surface of the electrolyte layer 40 is observed by SEM, and the acceleration voltage is increased to 25 kV so that depth information can also be obtained, so that the protrusions 41 and the crystal grains 42 can be observed simultaneously. The number of protrusions 41 can be measured by counting the number of protrusions 41 having a size of 0.2 μm or more and 1.5 μm or less on one crystal grain 42, as illustrated in FIG. 4. For example, the number of protrusions 41 on 20 or more crystal grains 42 can be counted and the average value can be used as the average value. For example, the number of protrusions 41 can be confirmed by cutting out the surface of a portion on the outer periphery of the cell where the cathode 60 is not printed and performing surface observation with an SEM. Furthermore, when the intermediate layer 50 is formed on the surface, the acceleration voltage can be further increased, for example to 40 kV, so that depth information can be obtained.
[0044] In the electrolyte layer 40, it is preferable that the crystal grains 42 on the intermediate layer 50 side surface and the protrusions 41 are integrated without any crystal grain boundaries. The absence of crystal grain boundaries between the protrusions 41 reduces grain boundary resistance when oxide ions pass through the electrolyte layer 40, resulting in higher power generation performance. For example, it is preferable that no crystal grain boundaries exist between 50% or more of the protrusions 41 on the intermediate layer 50 side surface and the crystal grains 42 on the intermediate layer 50 side surface of the electrolyte layer 40, more preferably no crystal grain boundaries exist for 70% or more, and even more preferably no crystal grain boundaries exist for 90% or more.
[0045] The unevenness interval b of the convex portion 41 is about 0.05 to 0.8 times the grain size of the crystal grain 42 on which the convex portion 41 is provided. The unevenness interval b is the average value of the distance from the bottom point of the unevenness formed by each convex portion 41 to the adjacent bottom point in the direction in which the electrolyte layer 40 extends, as exemplified in FIG. 5(b). The vertical distance a of the convex portion 41 is about half the unevenness interval b, and is in the range of 0.025 to 0.4 times the grain size of the crystal grain on which the convex portion 41 is provided. As exemplified in FIG. 5(a), the vertical distance a is the vertical distance from the apex of the convex portion 41 between the bottom point of the unevenness formed by each convex portion 41 to the line drawn between the bottom point and the adjacent bottom point of the unevenness formed by each convex portion 41. Such measurements are performed at 20 or more points, and the average value is taken as the average value of the vertical distance a.
[0046] The following describes a method for manufacturing the fuel cell 100. Fig. 6 is a diagram illustrating an example of the flow of the method for manufacturing the fuel cell 100.
[0047] (Support material preparation process) (S1) The support material is made into a slurry by mixing metal powder (for example, particle size 10 μm to 100 μm), plasticizer (for example, adjusted to 1 wt% to 6 wt% to adjust the adhesion of the sheet), solvent (toluene, 2-propanol (IPA), 1-butanol, terpineol, butyl acetate, ethanol, etc., 20 wt% to 30 wt% depending on the viscosity), dissipation material (organic matter), and binder (PVB, acrylic resin, ethyl cellulose, etc.). The support material is used as a material for forming the support 10. The volume ratio of the organic components (dissipation material, binder solids, plasticizer) to the metal powder is, for example, in the range of 1:1 to 20:1, and the amount of the organic components is adjusted depending on the porosity.
[0048] (Preparation process of materials for mixed layer) (S1) As the material for the mixed layer, ceramic material powder (for example, particle size 100 nm to 10 μm) which is the raw material of the ceramic material 22, metal material powder with a small particle size (for example, particle size 1 μm to 10 μm) which is the raw material of the metal material 21, solvent (toluene, 2-propanol (IPA), 1-butanol, terpineol, butyl acetate, ethanol, etc., 20 wt% to 30 wt% depending on the viscosity), plasticizer (for example, adjusted to 1 wt% to 6 wt% to adjust the adhesion of the sheet), vanishing material (organic matter), and binder (PVB, acrylic resin, ethyl cellulose, etc.) are mixed to form a slurry. The volume ratio of the organic component (vanishing material, binder solid content, plasticizer) to the ceramic material powder and metal material powder is, for example, in the range of 1:1 to 5:1, and the amount of the organic component is adjusted depending on the porosity. The pore size of the voids is controlled by adjusting the particle size of the vanishing material. The ceramic material powder may contain an electron conductive material powder and an oxide ion conductive material powder. In this case, the volume ratio of the electron conductive material powder to the oxide ion conductive material powder is preferably in the range of, for example, 1:9 to 9:1. Also, even if an electrolyte material such as ScYSZ or GDC is used instead of the electron conductive material, there is no peeling at the interface, and a cell can be fabricated. However, from the viewpoint of reducing the ohmic resistance, it is preferable to mix the electron conductive material with a metal powder.
[0049] (Anode material preparation process) (S1) As the anode material, a ceramic material powder constituting the electrode skeleton, a solvent (toluene, 2-propanol (IPA), 1-butanol, terpineol, butyl acetate, ethanol, etc., 20 wt% to 30 wt% depending on the viscosity), a plasticizer (for example, adjusted to 1 wt% to 6 wt% to adjust the adhesion of the sheet), a dissipating material (organic material), and a binder (PVB, acrylic resin, ethyl cellulose, etc.) are mixed to form a slurry. As the ceramic material powder constituting the electrode skeleton, an electron conductive material powder (for example, particle size 100 nm to 10 μm) which is the raw material of the electron conductive ceramic 31, an oxide ion conductive material powder (for example, particle size 100 nm to 10 μm) which is the raw material of the oxide ion conductive ceramic 32, etc. may be used. The volume ratio of the organic components (dissipating material, binder solids, plasticizer) to the electron conductive material powder is, for example, in the range of 1:1 to 5:1, and the amount of the organic components is adjusted depending on the porosity. The pore size of the voids is controlled by adjusting the particle size of the dissipating material. The volume ratio of the electron conductive material powder to the oxide ion conductive material powder is set to a range of 3:7 to 7:3, for example.
[0050] (Electrolyte layer material preparation process) (S1) As the material for the electrolyte layer, oxide ion conductive material powder (e.g., ScYSZ, YSZ, GDC, etc., with a particle size of D50%=10 nm to 1000 nm), solvent (toluene, 2-propanol (IPA), 1-butanol, terpineol, butyl acetate, ethanol, etc., 20 wt% to 30 wt% depending on the viscosity), plasticizer (e.g., adjusted to 1 wt% to 6 wt% to adjust the adhesion of the sheet), and binder (PVB, acrylic resin, ethyl cellulose, etc.) are mixed to form a slurry. The volume ratio of the organic components (binder solids, plasticizer) to the oxide ion conductive material powder is, for example, in the range of 6:4 to 3:4.
[0051] (Process for preparing material for uneven layer) (S1) The same material as the electrolyte layer material is used, and the viscosity, additives, solid content concentration, etc. are appropriately adjusted so that the dispersibility of the material is poor when preparing the slurry. Furthermore, resin particles are added to create an aggregation of materials such as ScYSZ, YSZ, and GDC. Examples of the resin particles include acrylic resin, polystyrene particles, nylon fine particles, and phenolic resin. The size of the resin particles is preferably larger than the particle size of the oxide ion conductive material powder. For example, the particle size of the resin particles is 1.5 times or more than the oxide ion conductive material powder. In addition, in order to increase the aggregation effect, the particle size of the resin particles is more preferably 3 times or more than the oxide ion conductive material powder. It is even more preferable that the particle size of the resin particles is 5 times or more than the oxide ion conductive material powder. Note that the particle size of the oxide ion conductive material powder in the uneven layer material is preferably smaller than the particle size of the oxide ion conductive material powder in the electrolyte layer material. This is because it is easier to form unevenness on the surface of the electrolyte layer 40. For example, the D50% particle size of the oxide ion conductive material powder in the material for the uneven layer is preferably 1 / 3 or less, more preferably 1 / 5 or less, and even more preferably 1 / 10 or less, of the D50% particle size of the oxide ion conductive material powder in the material for the electrolyte layer.
[0052] (Firing process) (S2) First, a support material is applied onto a PET (polyethylene terephthalate) film to prepare a support green sheet. A mixed layer material is applied onto another PET film to prepare a mixed layer green sheet. An anode material is applied onto another PET film to prepare an anode green sheet. An electrolyte layer material is applied onto another PET film to prepare an electrolyte layer green sheet. An uneven layer green sheet is applied onto another PET film to prepare an uneven layer green sheet. The uneven layer green sheet is used as a green sheet to be attached to the surface layer of the electrolyte layer green sheet, so it is a thin sheet, for example, 1 μm or less. For example, multiple support green sheets, one mixed layer green sheet, one anode green sheet, one electrolyte layer green sheet, and one uneven layer green sheet are laminated in this order, cut to a predetermined size, and then heated to a temperature of 100°C or lower to 300°C. -20 The mixture is fired in a reducing atmosphere of 1 atm or less at a temperature range of about 1100° C. to 1300° C. Thereby, a half cell including the support 10, the mixed layer 20, the electrode skeleton of the anode 30, the electrolyte layer 40, and the concave-convex layer can be obtained.
[0053] (Anode impregnation process) (S3) Next, the raw materials of the oxide ion conductive ceramics 33 and the catalytic metal 34 are impregnated into the electrode skeleton of the anode 30. For example, nitrates or chlorides of Zr, Y, Sc, Ce, Gd, and Ni are dissolved in water or alcohols (ethanol, 2-propanol, methanol, etc.) so that Gd-doped ceria or Sc, Y-doped zirconia and Ni are produced when fired at a predetermined temperature in a reducing atmosphere, and the half cell is impregnated, dried, and the heat treatment is repeated as many times as necessary.
[0054] (Intermediate layer formation process) (S4) The intermediate layer 50 is formed by depositing the oxide ion conductive ceramics contained in the intermediate layer 50 on the electrolyte layer 40 by, for example, PVD. 0.8 Gd 0.2 O 2-x The intermediate layer 50 is formed by depositing the above to a thickness of 1 μm.
[0055] (Cathode formation process) (S5) Next, a cathode material is applied onto the intermediate layer 50 by screen printing or the like, and dried. The cathode material is then sintered by heat treatment in an air atmosphere at a temperature of 1000° C. or less to form the cathode 60. To prevent oxidation of the metal, the heat treatment temperature is preferably 900° C. or less, and more preferably 800° C. or less.
[0056] According to the manufacturing method of this embodiment, as illustrated in FIG. 7, the green sheet 80 for the uneven layer is laminated on the electrolyte layer green sheet 70. The particle size of the oxide ion conductive material powder 81 contained in the green sheet 80 for the uneven layer is smaller than the particle size of the oxide ion conductive material powder 71 contained in the electrolyte layer green sheet 70. The green sheet 80 for the uneven layer contains resin particles 82. The resin particles 82 function as spacers, and the oxide ion conductive material powder 81 aggregates. The resin particles 82 are removed in the firing process. The aggregated oxide ion conductive material powder 81 becomes the protrusions 41 after firing. As a result, protrusions and recesses arranged in a two-dimensional direction are formed in the surface of the electrolyte layer 40 on the intermediate layer 50 side after firing. As a result, the intermediate layer 50 also follows the shape of the surface of the electrolyte layer 40 on the intermediate layer 50 side. Therefore, the protrusions 51 are formed on the surface of the intermediate layer 50 side on the cathode 60 side of the intermediate layer 50 so as to approximately coincide with the position of the protrusions 41. In the printing method, it is difficult to form unevenness only in one direction in the plane, but in the manufacturing method according to the present embodiment, unevenness can be formed in two directions in the plane. Incidentally, unevenness is also formed on the surface of the intermediate layer 50 facing the electrolyte layer 40, along the surface of the electrolyte layer 40 facing the cathode 60. Furthermore, unevenness is also formed on the surface of the cathode 60 facing the intermediate layer 50, so as to follow the shape of the surface of the intermediate layer 50 facing the cathode 60. EXAMPLES
[0057] A fuel cell 100 was produced according to the manufacturing method according to the above embodiment.
[0058] Example 1 SUS (stainless steel) powder was used as the support material. ScYSZ was used as the ceramic material for the electrolyte layer material. Acrylic resin, polystyrene particles, nylon fine particles, phenolic resin, etc. were added as resin particles for the uneven layer material. LaCrO3-based material was used as the electron conductive ceramic for the anode material, and ScYSZ was used as the oxide ion conductive ceramic. GDC was used as the ceramic material for the intermediate layer material. LSC was used as the ceramic material for the cathode material. LaCrO3-based material was used as the ceramic material for the mixed layer material. SUS was used as the metal material for the mixed layer material. The mixed layer green sheet, anode green sheet, electrolyte layer green sheet, and uneven layer green sheet were laminated on the support green sheet, cut to a specified size, and then heated in a 3000-kV furnace under an oxygen partial pressure of 10 -16 The anode was impregnated with GDC and Ni in a reducing atmosphere at or below 850°C. The anode was then fired in an air atmosphere at a temperature of 850°C or lower. 0.8 Gd 0.2 O 2-xThe intermediate layer was formed, and the cathode material was applied on the intermediate layer by screen printing or the like, and dried. Then, the cathode material was sintered by heat treatment in an air atmosphere at a temperature of 1000°C or less to form a cathode. In Example 1, the vertical distance a was 100 nm, and the unevenness interval b was 500 nm. It was also confirmed that there was no grain boundary between the crystal grains on the intermediate layer 50 side surface of the electrolyte layer 40 and 90% or more of the protrusions 51 on the intermediate layer 50 side surface. The surface of the fired half cell was observed with an SEM, and the number of protrusions 41 present on 20 crystal grains 42 was counted, and the average value was 11. Then, a PVD process was performed, and a cathode was printed to form a full cell. After the power generation evaluation, the cross section of the cell was observed. The grain size of the crystal grains 42 in the cross section was measured, and the average value was 3 μm. The presence of grain boundaries between the convex portions 51 on the surface on the intermediate layer 50 side and the crystal grains on the surface of the electrolyte layer 40 on the intermediate layer 50 side was also confirmed by cross-sectional observation. Furthermore, the average value of the vertical distance a and the average value of the unevenness interval b could be measured from the same cross-sectional photograph. The average values of the vertical distance a and the unevenness interval b were 100 nm and 500 nm, respectively.
[0059] Example 2 In Example 2, NiO / YSZ was used as the support material. Other manufacturing conditions were the same as in Example 1. In Example 2, the vertical distance a was 100 nm, and the unevenness interval b was 500 nm. It was also confirmed that there was no grain boundary between the crystal grains on the intermediate layer 50 side surface of the electrolyte layer 40 and 90% or more of the protrusions 51 on the intermediate layer 50 side surface of the electrolyte layer 40. When the number of protrusions 41 present on the crystal grains 42 was counted in the same manner as in Example 1, the average number was 11. After the power generation evaluation was performed in the same manner as in Example 1, the cross section was observed, and the average grain size of the crystal grains 42 was 3 μm. Furthermore, the average value of the vertical distance a and the average value of the unevenness interval b were 100 nm and 500 nm, respectively.
[0060] Example 3 In Example 3, the manufacturing conditions of the uneven sheet were changed to increase the proportion of the resin material and reduce the number of protrusions 41 present on the surface of the crystal particles 42. The other manufacturing conditions were the same as in Example 1. In Example 3, the vertical distance a was 100 nm and the unevenness interval b was 800 nm. It was also confirmed that there was no grain boundary between the crystal particles on the intermediate layer 50 side surface of the electrolyte layer 40 and 90% or more of the protrusions 51 on the intermediate layer 50 side surface of the electrolyte layer 40. When the number of protrusions 41 present on the crystal particles 42 was counted in the same manner as in Example 1, the average number was 7. After the power generation was evaluated in the same manner as in Example 1, the cross section was observed and the average particle size of the crystal particles 42 was 3 μm. Furthermore, the average value of the vertical distance a and the average value of the unevenness interval b were 100 nm and 800 nm, respectively.
[0061] (Comparative Example) In the comparative example, the green sheet for the uneven layer was not provided. The other conditions were the same as those in Example 1. In the comparative example, since the green sheet for the uneven layer was not provided, unevenness did not appear on the cathode side surface of the electrolyte layer, and unevenness did not appear on the intermediate layer and the cathode.
[0062] (Power generation evaluation) Impedance measurements were performed on the fuel cells of Examples 1 to 3 and the Comparative Example to separate the resistance values and measure the ohmic resistance of the entire fuel cell and the reaction resistance of the cathode. The results are shown in Table 1. As shown in Table 1, in the Comparative Example, the ohmic resistance was 0.25 Ω cm 2 The reason why the ohmic resistance was low in the comparative example is believed to be because no protrusions were formed on the intermediate layer side surface of the electrolyte layer. In Examples 1 and 3, the ohmic resistance was 0.25 Ω cm 2 In Example 2, the ohmic resistance was 0.30 Ω cm 2Thus, the ohmic resistance was also low in Example 1 and Example 2. This is believed to be because the convex portion on the intermediate layer side surface of the electrolyte layer did not form a crystal grain boundary with the crystal grains on the intermediate layer side surface of the electrolyte layer. The reason why the ohmic resistances of Example 1 and Example 3 were lower than that of Example 2 is believed to be because a metal support having high electronic conductivity was used. [Table 1]
[0063] In Example 1, the reaction resistance at the cathode is 0.27 Ω cm 2 In Example 2, the reaction resistance at the cathode was 0.27 Ω cm 2 In Example 3, the reaction resistance at the cathode was 0.31 Ω cm 2 Thus, in Examples 1 to 3, the reaction resistance in the cathode was low. This is believed to be because by forming two-dimensional irregularities in a plan view on the intermediate layer side surface of the electrolyte layer, irregularities were also formed on the cathode side surface of the intermediate layer, increasing the contact area between the intermediate layer and the cathode. In contrast, in the comparative example, the reaction resistance in the cathode was 0.56 Ω cm 2 This is believed to be because the contact area between the intermediate layer and the cathode was not large enough due to the absence of projections and recesses in the intermediate layer.
[0064] Although the embodiments of the present invention have been described in detail above, the present invention is not limited to such specific embodiments, and various modifications and variations are possible within the scope of the gist of the present invention described in the claims. [Explanation of symbols]
[0065] 10 Support 20 mixed layer 21 Metal materials 22 Ceramic Materials 30 Anode 31 Electronically Conductive Ceramics 32 Oxide-ion conductive ceramics 33 Oxide-ion conductive ceramics 34 Catalytic Metals 40 Electrolyte layer 41 Convex 50 Middle Class 51 Convex 60 Cathode 70 Electrolyte layer green sheet 71 Oxide-ion conductive material powder 80 Green sheet for uneven layer 81 Oxide-ion conductive material powder 82 Resin particles 100 fuel cell
Claims
1. an electrolyte layer including a solid oxide having oxide ion conductivity and including a plurality of crystal particles; an intermediate layer provided on the electrolyte layer and having oxide ion conductivity; a cathode provided on the intermediate layer; the electrolyte layer has a surface on the intermediate layer side, the surface having a plurality of protrusions arranged in a two-dimensional direction in a plan view; the protrusions are formed so as to protrude toward the intermediate layer from crystal grains on a surface of the electrolyte layer facing the intermediate layer, the crystal grains on the surface of the electrolyte layer facing the intermediate layer are larger than the protrusions, 1. A solid oxide fuel cell comprising: a surface of said intermediate layer facing said cathode, said surface being formed so as to conform to the shape of a surface of said electrolyte layer facing said intermediate layer.
2. 2. The solid oxide fuel cell according to claim 1, wherein the plurality of protrusions are formed in a particle shape.
3. 2. The solid oxide fuel cell according to claim 1, wherein the size of crystal grains on the surface of the electrolyte layer facing the intermediate layer is 1 [mu]m or more and 5 [mu]m or less.
4. 4. The solid oxide fuel cell according to claim 3, wherein the number of the protrusions in the crystal grains on the surface of the electrolyte layer facing the intermediate layer is 3 to 15 in a plan view of the electrolyte layer.
5. 2. The solid oxide fuel cell according to claim 1, wherein no crystal grain boundary exists between at least any of the protrusions and crystal grains on the surface of the electrolyte layer facing the intermediate layer.
6. 2. The solid oxide fuel cell according to claim 1, wherein the size of the protrusions is in the range of 0.05 to 0.8 times the size of the crystal grains on the surface of the electrolyte layer facing the intermediate layer.
7. 2. The solid oxide fuel cell according to claim 1, wherein the height of the protrusions is in the range of 0.025 to 0.4 times the size of crystal grains on the surface of the electrolyte layer facing the intermediate layer.
8. 2. The solid oxide fuel cell according to claim 1, wherein the size of the protrusions is 0.2 [mu]m or more and 1.5 [mu]m or less.
9. A slurry containing an oxide ion conductive material powder is applied to prepare an electrolyte layer green sheet; a step of applying a slurry containing an oxide ion conductive material powder having a D50% particle size smaller than the D50% particle size of the oxide ion conductive material powder of the electrolyte layer green sheet and resin particles onto the electrolyte layer green sheet, and firing the slurry; forming an intermediate layer having oxide ion conductivity and no cathode activity on the electrolyte layer obtained by firing; A method for producing a solid oxide fuel cell, comprising forming a cathode on the intermediate layer.
Citation Information
Patent Citations
Electrochemical element, electrochemical module, electrochemical device, energy system, solid oxide fuel cell, and method of manufacturing electrochemical element
JP2017174516A
Method of producing sofc cathode diffusion barrier layer and sofc
JP2017504946A
Electrochemical element, electrochemical module, electrochemical device, energy system, solid oxide fuel cell, and manufacturing method of electrochemical element
JP2018174117A
Electrochemical cell
JP2020155338A