Internal resistance reducing agent for positive electrode active material layer, and positive electrode material for secondary battery using the same

By adding an ionic crystalline compound with specific parameters to the positive electrode active material layer, the internal resistance is reduced, addressing the insufficient charge/discharge rate issue in sulfur-based secondary batteries and improving their performance.

JP7594884B2Active Publication Date: 2024-12-05NISSAN MOTOR CO LTD +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020185781
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-11-06
Publication Date
2024-12-05
Estimated Expiration
2040-11-06

AI Technical Summary

Technical Problem

Secondary batteries using sulfur-based positive electrode active materials face insufficient charge/discharge rate characteristics, limiting their ability to support rapid charging and discharging.

Method used

Incorporating an ionic crystalline compound with specific parameters into the positive electrode active material layer, defined by a formula where 0.032≦X≦0.072, to reduce internal resistance and enhance charge/discharge rate characteristics.

Benefits of technology

The addition of the ionic crystalline compound improves the charge/discharge rate characteristics of secondary batteries containing sulfur-based positive electrode materials, reducing internal resistance and enhancing the battery's performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007594884000007
    Figure 0007594884000007
  • Figure 0007594884000008
    Figure 0007594884000008
  • Figure 0007594884000009
    Figure 0007594884000009
Patent Text Reader

Abstract

To provide means capable of improving charge / discharge rate characteristics in a secondary battery using a positive electrode active material containing sulfur.SOLUTION: An ionic crystalline compound has a basic structure consisting of an atom A that becomes a cation atom and an atom B that becomes an anion atom when dissociated into ions in a positive electrode active material layer of a positive electrode for a secondary battery containing a positive electrode active material containing sulfur, and a compound in which a parameter X represented by the following formula 1 satisfies 0.032≤X≤0.072 is added to reduce the internal resistance of the positive electrode active material layer. In the formula, Eatom represents the energy [eV] per atom of the ionic crystalline compound, Zcat represents the atomic number of the atom A, and La represents the length [Å] of the crystal lattice a of the ionic crystalline compound.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an internal resistance reducing agent for a positive electrode active material layer, and a positive electrode material for a secondary battery using the same. [Background technology]

[0002] In recent years, there has been a strong desire to reduce carbon dioxide emissions in order to combat global warming. In the automobile industry, there are high hopes for a reduction in carbon dioxide emissions through the introduction of electric vehicles (EVs) and hybrid electric vehicles (HEVs), and there has been active development of non-aqueous electrolyte secondary batteries, such as motor drive secondary batteries, which hold the key to putting these into practical use.

[0003] Secondary batteries for driving motors are required to have extremely high output characteristics and high energy compared to consumer lithium secondary batteries used in mobile phones, notebook computers, etc. Therefore, lithium secondary batteries, which have the highest theoretical energy of all practical batteries, have attracted attention and are currently being rapidly developed.

[0004] Currently, lithium secondary batteries in widespread use use flammable organic electrolytes as electrolytes, and these liquid-based lithium secondary batteries require stricter safety measures against leakage, short circuits, overcharging, etc. than other batteries.

[0005] In recent years, research and development of all-solid-state lithium secondary batteries using oxide-based or sulfide-based solid electrolytes has been actively conducted. A solid electrolyte is a material mainly composed of an ion conductor capable of ion conduction in a solid state. Therefore, in principle, all-solid-state lithium secondary batteries do not have various problems caused by flammable organic electrolytes, as in conventional liquid-based lithium secondary batteries. In addition, the use of high-potential, large-capacity positive electrode materials and large-capacity negative electrode materials generally leads to a significant improvement in the output density and energy density of the battery. For example, elemental sulfur (S8), a candidate for the positive electrode active material, has an extremely large theoretical capacity of about 1670 mAh / g, and has the advantages of being low cost and abundant in resources.

[0006] However, due to the low electronic conductivity of sulfur, the high capacity characteristic of sulfur-containing positive electrode active materials has not yet been fully utilized.

[0007] For the purpose of fully utilizing the high capacity characteristics of a positive electrode active material such as elemental sulfur, for example, Patent Document 1 discloses a technique for preparing a positive electrode material by adding an ion-conductive material and activated carbon coated with a conductive material having a conductivity equal to or higher than a predetermined value to sulfur and / or its discharge product. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2015-176849 A Summary of the Invention [Problem to be solved by the invention]

[0009] According to the study by the present inventors, it was found that when a secondary battery is manufactured using the technology described in Patent Document 1, there is a problem that sufficient capacity cannot be obtained during charging and discharging at a high charging and discharging rate (i.e., the so-called charge and discharge rate characteristics are insufficient). A secondary battery with such insufficient charge and discharge rate characteristics cannot utilize sufficient capacity in response to rapid charging and discharging.

[0010] Therefore, an object of the present invention is to provide a means for improving the charge / discharge rate characteristics of a secondary battery using a positive electrode active material containing sulfur. [Means for solving the problem]

[0011] The present inventors have conducted extensive research to solve the above problems, and as a result, have found that the above problems can be solved by adding an ionic crystalline compound, in which a parameter defined by a predetermined mathematical formula is within a predetermined range, to a positive electrode active material layer together with a positive electrode active material containing sulfur, and have thus completed the present invention.

[0012] One aspect of the present invention is a cathode active material layer of a secondary battery cathode containing a sulfur-containing cathode active material, the cathode active material layer being added thereto to reduce the internal resistance of the cathode active material layer, The present invention comprises an ionic crystalline compound as an active ingredient, the ionic crystalline compound having a basic structure consisting of an atom A which becomes a cationic atom when the ionic crystalline compound dissociates into ions, and an atom B which becomes an anionic atom, The ionic crystalline compound has a parameter X, which is expressed by the following formula 1, that satisfies 0.032≦X≦0.072.

[0013]

number

[0014] In the formula, E atom represents the energy per atom of the ionic crystalline compound [eV], and Z cat represents the atomic number of the atom A, and L a represents the length [Å] of the crystal lattice a of the ionic crystalline compound. Effect of the Invention

[0015] According to the present invention, in a secondary battery using a positive electrode active material containing sulfur, the charge and discharge rate characteristics can be improved. [Brief description of the drawings]

[0016] [Figure 1] FIG. 1 is a perspective view showing the appearance of a flat laminated type all-solid-state lithium ion secondary battery, which is one embodiment of the lithium ion secondary battery according to the present invention. [Diagram 2]FIG. 2 is a cross-sectional view taken along line 2-2 shown in FIG. [Diagram 3] FIG. 3 is an energy diagram of the rate-limiting reactions in both the charge and discharge processes of a lithium ion secondary battery using a sulfur-containing positive electrode active material. [Figure 4A] FIG. 4A is a graph plotting the relationship between the parameter element ((Eatom+12.79) / 11.77) normalized to the energy per atom (Eatom) of the ionic crystalline compounds described in the examples and comparative examples in Table 3 and the Gibbs free energy (ΔG) of the above reaction. [Figure 4B] FIG. 4B is a graph plotting the relationship between the parameter element ((Zcat-94) / 93) normalized by the atomic number (Zcat) of atom A constituting the ionic crystalline compounds described in the examples and comparative examples in Table 3 and the Gibbs free energy (ΔG) of the above reaction. [Figure 4C] FIG. 4C is a graph plotting the relationship between the parameter element ((La-70.68) / 68.54) normalized for the length (La) of the crystal lattice a of the ionic crystalline compounds described in the examples and comparative examples in Table 3 and the Gibbs free energy (ΔG) of the above reaction. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] Hereinafter, the above-mentioned embodiment of the present invention will be described with reference to the drawings, but the technical scope of the present invention should be determined based on the description of the claims, and is not limited to only the following embodiment. The dimensional ratios in the drawings are exaggerated for convenience of explanation and may differ from the actual ratios. Hereinafter, the present invention will be described by taking as an example a stacked type (internal parallel connection type) all-solid-state lithium secondary battery, which is one form of secondary battery. As described above, the solid electrolyte constituting the all-solid-state lithium secondary battery is a material mainly composed of an ion conductor capable of ion conduction in a solid. For this reason, the all-solid-state lithium secondary battery has the advantage that, in principle, various problems caused by a flammable organic electrolyte do not occur as in the conventional liquid-based lithium secondary battery. In addition, in general, there is also the advantage that the output density and energy density of the battery can be significantly improved by using a high-potential, large-capacity positive electrode material and a large-capacity negative electrode material.

[0018] One aspect of the present invention is a cathode active material layer of a secondary battery cathode containing a sulfur-containing cathode active material, the cathode active material layer being added thereto to reduce the internal resistance of the cathode active material layer, The present invention comprises an ionic crystalline compound as an active ingredient, the ionic crystalline compound having a basic structure consisting of an atom A which becomes a cationic atom when the ionic crystalline compound dissociates into ions, and an atom B which becomes an anionic atom, The parameter X of the ionic crystalline compound, which is expressed by the above mathematical formula 1, satisfies 0.032≦X≦0.072 in the internal resistance reducing agent for the positive electrode active material layer.

[0019] The internal resistance reducing agent for the positive electrode active material layer according to the present embodiment (containing a specific ionic crystalline compound as an active ingredient) is added to the positive electrode active material layer of a secondary battery positive electrode containing a sulfur-containing positive electrode active material, and an interaction occurs between the additive and the surface of sulfur, and the Gibbs free energy (ΔG) in the reaction (and the reverse reaction) in which the elemental sulfur (S) contained in the positive electrode active material layer bonds with Li to produce Li2S8 can be reduced. As a result, the internal resistance of the positive electrode active material layer can be reduced. As a result, it is possible to improve the charge and discharge rate characteristics in a secondary battery using a sulfur-containing positive electrode active material. The estimated mechanism by which the specific ionic crystalline compound, which is the active ingredient of the internal resistance reducing agent according to the present embodiment, reduces the internal resistance of the positive electrode active material layer of a secondary battery using a sulfur-containing positive electrode active material will be described later.

[0020] FIG. 1 is a perspective view showing the appearance of a flat-laminated all-solid-state lithium-ion secondary battery, which is one embodiment of the lithium-ion secondary battery according to the present invention. FIG. 2 is a cross-sectional view taken along line 2-2 shown in FIG. 1. The laminated type allows the battery to be compact and have a high capacity. In this specification, the flat-laminated non-bipolar lithium-ion secondary battery shown in FIG. 1 and FIG. 2 (hereinafter, also simply referred to as a "laminated battery") will be described in detail as an example. However, in terms of the internal electrical connection form (electrode structure) of the lithium-ion secondary battery according to this embodiment, it can be applied to both non-bipolar (internal parallel connection type) batteries and bipolar (internal series connection type) batteries.

[0021] 1, the stacked battery 10a has a flat rectangular shape, with a negative electrode current collector 25 and a positive electrode current collector 27 for extracting electric power extending from both sides. The power generating element 21 is wrapped in a battery exterior material (laminate film 29) of the stacked battery 10a, and the periphery is heat-sealed, with the power generating element 21 being sealed with the negative electrode current collector 25 and the positive electrode current collector 27 extending to the outside.

[0022] The lithium ion secondary battery according to the present embodiment is not limited to a laminated flat shape. A wound lithium ion secondary battery may be cylindrical, or may be a rectangular flat shape obtained by deforming such a cylindrical shape, and is not particularly limited. The cylindrical shape may be a laminate film or a conventional cylindrical can (metal can) as an exterior material, and is not particularly limited. Preferably, the power generating element is housed inside a laminate film containing aluminum. This form can achieve weight reduction.

[0023] There is also no particular limitation on the removal of the current collectors (25, 27) shown in Fig. 1. The negative current collector 25 and the positive current collector 27 may be pulled out from the same side, or the negative current collector 25 and the positive current collector 27 may each be divided into a plurality of pieces and removed from each side, and are not limited to what is shown in Fig. 1. In addition, in a wound type lithium ion battery, the terminals may be formed using, for example, a cylindrical can (metal can) instead of a tab.

[0024] 2, the stacked battery 10a of this embodiment has a structure in which a flat, generally rectangular power generating element 21, where charge and discharge reactions actually proceed, is sealed inside a laminate film 29, which is a battery exterior material. Here, the power generating element 21 has a structure in which a positive electrode, a solid electrolyte layer 17, and a negative electrode are laminated. The positive electrode has a structure in which positive electrode active material layers 15 containing a positive electrode active material are disposed on both sides of a positive electrode collector 11". The negative electrode has a structure in which negative electrode active material layers 13 containing a negative electrode active material are disposed on both sides of a negative electrode collector 11'. Specifically, the positive electrode, solid electrolyte layer, and negative electrode are stacked in this order such that one positive electrode active material layer 15 and an adjacent negative electrode active material layer 13 face each other with a solid electrolyte layer 17 interposed therebetween. As a result, the adjacent positive electrode, solid electrolyte layer, and negative electrode constitute one unit cell layer 19. Therefore, it can be said that the stacked battery 10a shown in FIG. 1 has a structure in which a plurality of unit cell layers 19 are stacked and electrically connected in parallel.

[0025] As shown in FIG. 2, the outermost positive electrode current collectors located on both outermost layers of the power generating element 21 each have a positive electrode active material layer 15 disposed on only one side, but active material layers may be provided on both sides. In other words, instead of using a current collector exclusively for the outermost layer with an active material layer provided on only one side, a current collector having active material layers on both sides may be used as it is as the outermost layer current collector. In some cases, the negative electrode active material layer 13 and the positive electrode active material layer 15 may be used as the negative electrode and positive electrode, respectively, without using the current collectors (11', 11")

[0026] Negative current collector 11′ and positive current collector 11″ are respectively attached with negative current collector plate (tab) 25 and positive current collector plate (tab) 27 that are electrically connected to the respective electrodes (positive and negative electrodes), and have a structure in which they are sandwiched between ends of laminate film 29, which is a battery exterior material, and are led out of laminate film 29. Positive current collector 27 and negative current collector 25 may be attached to positive current collector 11″ and negative current collector 11′ of each electrode by ultrasonic welding, resistance welding, or the like, respectively, via positive electrode leads and negative electrode leads (not shown) as necessary.

[0027] The main components of the lithium ion secondary battery according to this embodiment will be described below.

[0028] [Current collector] The current collector has a function of mediating the movement of electrons from the electrode active material layer. There are no particular limitations on the material constituting the current collector. For example, metals and conductive resins can be used as the material constituting the current collector.

[0029] Specifically, the metal may be aluminum, nickel, iron, stainless steel, titanium, copper, etc. In addition to these, a clad material of nickel and aluminum, a clad material of copper and aluminum, etc. may be used. Also, a foil in which a metal surface is coated with aluminum may be used. Among them, aluminum, stainless steel, copper, and nickel are preferable from the viewpoint of electronic conductivity, battery operating potential, adhesion of the negative electrode active material by sputtering to the current collector, etc.

[0030] The latter conductive resin may be a resin obtained by adding a conductive filler to a non-conductive polymeric material as required.

[0031] Examples of non-conductive polymeric materials include polyethylene (PE; high density polyethylene (HDPE), low density polyethylene (LDPE), etc.), polypropylene (PP), polyethylene terephthalate (PET), polyethernitrile (PEN), polyimide (PI), polyamideimide (PAI), polyamide (PA), polytetrafluoroethylene (PTFE), styrene-butadiene rubber (SBR), polyacrylonitrile (PAN), polymethyl acrylate (PMA), polymethyl methacrylate (PMMA), polyvinyl chloride (PVC), polyvinylidene fluoride (PVdF), polystyrene (PS), etc. Such non-conductive polymeric materials can have excellent electric potential resistance or solvent resistance.

[0032] A conductive filler may be added to the conductive polymer material or non-conductive polymer material as necessary. In particular, when the resin serving as the base material of the current collector is made of only a non-conductive polymer, a conductive filler is necessarily required to impart conductivity to the resin.

[0033] The conductive filler can be used without any particular limitation as long as it is a material having electrical conductivity. For example, metals and conductive carbons can be mentioned as materials having excellent electrical conductivity, potential resistance, or lithium ion blocking properties. The metal is not particularly limited, but preferably contains at least one metal selected from the group consisting of Ni, Ti, Al, Cu, Pt, Fe, Cr, Sn, Zn, In, and Sb, or an alloy or metal oxide containing these metals. The conductive carbon is also not particularly limited. Preferably, it contains at least one selected from the group consisting of acetylene black, Vulcan (registered trademark), Black Pearl (registered trademark), carbon nanofiber, Ketjen Black (registered trademark), carbon nanotube, carbon nanohorn, carbon nanoballoon, and fullerene.

[0034] The amount of conductive filler added is not particularly limited as long as it is an amount that can impart sufficient conductivity to the current collector, and is generally 5 to 80 mass % relative to the total mass of the current collector (100 mass %).

[0035] The current collector may have a single layer structure made of a single material, or may have a laminate structure in which layers made of these materials are appropriately combined. From the viewpoint of reducing the weight of the current collector, it is preferable to include at least a conductive resin layer made of a resin having conductivity. In addition, from the viewpoint of blocking the movement of lithium ions between the single cell layers, a metal layer may be provided on a part of the current collector. Furthermore, if the negative electrode active material layer and the positive electrode active material layer described later are conductive by themselves and can perform a current collecting function, it is not necessary to use a current collector as a member separate from these electrode active material layers. In such a form, the negative electrode active material layer described later constitutes the negative electrode as it is, and the positive electrode active material layer described later constitutes the positive electrode as it is.

[0036] [Negative electrode (negative electrode active material layer)] In the secondary battery according to this embodiment, the negative electrode active material layer 13 contains a negative electrode active material. The type of the negative electrode active material is not particularly limited, but may include a carbon material, a metal oxide, and a metal active material. Examples of the carbon material include natural graphite, artificial graphite, mesocarbon microbeads (MCMB), highly oriented graphite (HOPG), hard carbon, and soft carbon. Examples of the metal oxide include Nb2O5, Li4Ti5O 12 and the like. Furthermore, silicon-based negative electrode active materials and tin-based negative electrode active materials may be used. Here, silicon and tin belong to the 14th group of elements, and are known to be negative electrode active materials that can greatly improve the capacity of non-aqueous electrolyte secondary batteries. These simple substances can absorb and release a large number of charge carriers (lithium ions, etc.) per unit volume (mass), and therefore become high-capacity negative electrode active materials. Here, it is preferable to use Si simple substance as the silicon-based negative electrode active material. Similarly, SiO 2 disproportionated into two phases, a Si phase and a silicon oxide phase, is also used. xIt is also preferable to use silicon oxides such as (0.3≦x≦1.6). In this case, the range of x is more preferably 0.5≦x≦1.5, and even more preferably 0.7≦x≦1.2. Furthermore, an alloy containing silicon (silicon-containing alloy-based negative electrode active material) may be used. On the other hand, examples of negative electrode active materials containing tin element (tin-based negative electrode active materials) include simple Sn, tin alloys (Cu-Sn alloys, Co-Sn alloys), amorphous tin oxides, tin silicon oxides, and the like. Among these, examples of amorphous tin oxides include SnB 0.4 P 0.6 O 3.1 Examples of the tin silicon oxide include SnSiO3. Metals containing lithium may be used as the negative electrode active material. Such negative electrode active materials are not particularly limited as long as they are active materials containing lithium, and examples thereof include metallic lithium and lithium-containing alloys. Examples of the lithium-containing alloys include alloys of Li and at least one of In, Al, Si, and Sn. In some cases, two or more negative electrode active materials may be used in combination. Of course, negative electrode active materials other than the above may be used. The negative electrode active material preferably contains metallic lithium, a silicon-based negative electrode active material, or a tin-based negative electrode active material, and particularly preferably contains metallic lithium.

[0037] The shape of the negative electrode active material may be, for example, particulate (spherical, fibrous), thin film, etc. When the negative electrode active material is particulate, its average particle diameter (D 50 ) is, for example, preferably in the range of 1 nm to 100 μm, more preferably in the range of 10 nm to 50 μm, further preferably in the range of 100 nm to 20 μm, and particularly preferably in the range of 1 to 20 μm. In this specification, the average particle diameter (D 50 The value of can be measured by a laser diffraction scattering method.

[0038] The content of the negative electrode active material in the negative electrode active material layer is not particularly limited, but is, for example, preferably in the range of 40 to 99 mass %, and more preferably in the range of 50 to 90 mass %.

[0039] The negative electrode active material layer preferably further includes a solid electrolyte. By including the solid electrolyte in the negative electrode active material layer, the ionic conductivity of the negative electrode active material layer can be improved. Examples of the solid electrolyte include sulfide solid electrolytes and oxide solid electrolytes, and the sulfide solid electrolyte is preferable.

[0040] Examples of sulfide solid electrolytes include LiI-Li2S-SiS2, LiI-Li2S-P2O5, LiI-Li3PO4-P2S5, Li2S-P2S5, LiI-Li3PS4, and LiI-LiBr-Li3PS 4、 Li3PS 4、 Li2S-P2S5, Li2S-P2S5-LiI, Li2S-P2S5-Li2O, Li2S-P2S5-Li2O-LiI, Li2S-SiS2, Li2S-SiS2-LiI, Li2 S-SiS2-LiBr, Li2S-SiS2-LiCl, Li2S-SiS2-B2S3-LiI, Li2S-SiS2-P2S5-LiI, Li2S-B2S3, Li2S-P2S5-Z m S n (where m and n are positive numbers, and Z is Ge, Zn, or Ga), Li2S-GeS2, Li2S-SiS2-Li3PO4, Li2S-SiS2-Li x MO y (wherein x and y are positive numbers, and M is any one of P, Si, Ge, B, Al, Ga, and In). The description "Li2S-P2S5" means a sulfide solid electrolyte obtained by using a raw material composition containing Li2S and P2S5, and the same applies to other descriptions.

[0041] The sulfide solid electrolyte may have, for example, a Li3PS4 skeleton, a Li4P2S7 skeleton, or a Li4P2S6 skeleton. Examples of sulfide solid electrolytes having a Li3PS4 skeleton include LiI-Li3PS4 and LiI-LiBr-Li3PS 4、Examples include Li3PS4. Also, examples of sulfide solid electrolytes having a Li4P2S7 skeleton include Li-P-S-based solid electrolytes called LPS (e.g., Li7P3S 11 ). Also, as the sulfide solid electrolyte, for example, Li (4-x) Ge (1-x) P x S4 (where x satisfies 0 < x < 1), such as LGPS, may be used. Among them, the sulfide solid electrolyte contained in the active material layer is preferably a sulfide solid electrolyte containing P element, and the sulfide solid electrolyte is more preferably a material mainly composed of Li2S-P2S5. Furthermore, the sulfide solid electrolyte may contain halogen (F, Cl, Br, I). In a preferred embodiment, the sulfide solid electrolyte contains Li6PS5X (where X is Cl, Br, or I, preferably Cl).

[0042] Also, when the sulfide solid electrolyte is of the Li2S-P2S5 type, the ratio of Li2S and P2S5 is preferably in the range of Li2S:P2S5 = 50:50 to 100:0 in molar ratio, and more preferably Li2S:P2S5 = 70:30 to 80:20.

[0043] Also, the sulfide solid electrolyte may be a sulfide glass, a crystallized sulfide glass, or a crystalline material obtained by a solid-phase method. The sulfide glass can be obtained, for example, by performing mechanical milling (such as a ball mill) on the raw material composition. Also, the crystallized sulfide glass can be obtained, for example, by performing heat treatment on the sulfide glass at a temperature above the crystallization temperature. Also, the ionic conductivity (e.g., Li ion conductivity) of the sulfide solid electrolyte at room temperature (25°C) is preferably, for example, 1×10 -5 S / cm or more, and more preferably 1×10 -4 S / cm or more. The value of the ionic conductivity of the solid electrolyte can be measured by the AC impedance method.

[0044] Examples of oxide solid electrolytes include compounds having a NASICON structure. An example of a compound having a NASICON structure is represented by the general formula Li 1+x Al x Ge 2-x Compounds represented by the formula (PO4)3 (0≦x≦2) (LAGP), general formula Li 1+x Al x Ti 2-x (PO4)3 (0≦x≦2) (LATP) and the like. Another example of an oxide solid electrolyte is LiLaTiO (for example, Li 0.34 La 0.51 TiO3), LiPON (e.g., Li 2.9 PO 3.3 N 0.46 ), LiLaZrO (e.g., Li7La3Zr2O 12 ) etc.

[0045] The shape of the solid electrolyte may be, for example, a particulate shape such as a spherical shape or an oval spherical shape, or a thin film shape. When the solid electrolyte is particulate, its average particle diameter (D 50 ) is not particularly limited, but is preferably 40 μm or less, more preferably 20 μm or less, and even more preferably 10 μm or less. 50 ) is preferably 0.01 μm or more, and more preferably 0.1 μm or more.

[0046] The content of the solid electrolyte in the negative electrode active material layer is, for example, preferably in the range of 1 to 60 mass %, and more preferably in the range of 10 to 50 mass %.

[0047] The negative electrode active material layer may further contain at least one of a conductive assistant and a binder, in addition to the above-mentioned negative electrode active material and solid electrolyte.

[0048] Examples of the conductive assistant include metals such as aluminum, stainless steel (SUS), silver, gold, copper, and titanium, alloys or metal oxides containing these metals; carbon fibers (specifically, vapor-grown carbon fibers (VGCF), polyacrylonitrile-based carbon fibers, pitch-based carbon fibers, rayon-based carbon fibers, activated carbon fibers, etc.), carbon nanotubes (CNTs), and carbon black (specifically, acetylene black, Ketjen Black (registered trademark), furnace black, channel black, thermal lamp black, etc.), but are not limited thereto. In addition, a particulate ceramic material or a resin material coated with the above-mentioned metal material by plating or the like can also be used as a conductive assistant. Among these conductive assistants, from the viewpoint of electrical stability, it is preferable to include at least one selected from the group consisting of aluminum, stainless steel, silver, gold, copper, titanium, and carbon, more preferably to include at least one selected from the group consisting of aluminum, stainless steel, silver, gold, and carbon, and even more preferably to include at least one carbon. These conductive assistants may be used alone or in combination of two or more.

[0049] The conductive assistant is preferably in the form of particles or fibers. When the conductive assistant is in the form of particles, the shape of the particles is not particularly limited, and may be any shape such as powder, sphere, rod, needle, plate, column, irregular shape, scale, spindle shape, etc.

[0050] When the conductive assistant is particulate, the average particle diameter (primary particle diameter) is not particularly limited, but is preferably 0.01 to 10 μm from the viewpoint of the electrical properties of the battery. In this specification, the "particle diameter of the conductive assistant" means the maximum distance L between any two points on the contour line of the conductive assistant. The value of the "average particle diameter of the conductive assistant" is calculated as the average value of particle diameters of particles observed in several to several tens of fields of view using an observation means such as a scanning electron microscope (SEM) or a transmission electron microscope (TEM).

[0051] When the negative electrode active material layer contains a conductive assistant, the content of the conductive assistant in the negative electrode active material layer is not particularly limited, but is preferably 0 to 10 mass%, more preferably 2 to 8 mass%, and further preferably 4 to 7 mass% relative to the total mass of the negative electrode active material layer. If the content is within such a range, a stronger electron conduction path can be formed in the negative electrode active material layer, which can effectively contribute to improving the battery characteristics.

[0052] On the other hand, the binder is not particularly limited, but examples thereof include the following materials:

[0053] Thermoplastic polymers such as polybutylene terephthalate, polyethylene terephthalate, polyvinylidene fluoride (PVDF) (including compounds in which hydrogen atoms are replaced by other halogen elements), polyethylene, polypropylene, polymethylpentene, polybutene, polyether nitrile, polytetrafluoroethylene, polyacrylonitrile, polyimide, polyamide, ethylene-vinyl acetate copolymer, polyvinyl chloride, styrene-butadiene rubber (SBR), ethylene-propylene-diene copolymer, styrene-butadiene-styrene block copolymer and its hydrogenated derivatives, styrene-isoprene-styrene block copolymer and its hydrogenated derivatives, tetrafluoroethylene-hexafluoropropylene copolymer (FEP), tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (PFA), ethylene-tetrafluoroethylene copolymer (ETFE), polychlorotrifluoroethylene (PCTFE), ethylene Examples of such fluororesins include ethylene-chlorotrifluoroethylene copolymer (ECTFE) and polyvinyl fluoride (PVF), vinylidene fluoride-hexafluoropropylene-based fluororubber (VDF-HFP-based fluororubber), vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene-based fluororubber (VDF-HFP-TFE-based fluororubber), vinylidene fluoride-pentafluoropropylene-based fluororubber (VDF-PFP-based fluororubber), vinylidene fluoride-pentafluoropropylene-tetrafluoroethylene-based fluororubber (VDF-PFP-TFE-based fluororubber), vinylidene fluoride-perfluoromethylvinyl ether-tetrafluoroethylene-based fluororubber (VDF-PFMVE-TFE-based fluororubber), and vinylidene fluoride-chlorotrifluoroethylene-based fluororubber (VDF-CTFE-based fluororubber), as well as epoxy resins. Among these, polyimide, styrene-butadiene rubber, carboxymethyl cellulose, polypropylene, polytetrafluoroethylene, polyacrylonitrile, and polyamide are more preferable.

[0054] The thickness of the negative electrode active material layer differs depending on the intended configuration of the secondary battery, but is preferably within the range of, for example, 0.1 to 1000 μm.

[0055] [Solid electrolyte layer] In the secondary battery according to this embodiment, the solid electrolyte layer is interposed between the above-mentioned positive electrode active material layer and negative electrode active material layer, and is a layer that essentially contains a solid electrolyte.

[0056] There is no particular restriction on the specific form of the solid electrolyte contained in the solid electrolyte layer, and the solid electrolytes exemplified in the section on the negative electrode active material layer and their preferred forms can be similarly adopted. In some cases, a solid electrolyte other than the above-mentioned solid electrolyte may be used in combination. However, the content ratio of the sulfide solid electrolyte in the total amount of the solid electrolyte (100 mass%) is preferably 50 mass% or more, more preferably 70 mass% or more, even more preferably 80 mass% or more, even more preferably 90 mass% or more, particularly preferably 95 mass% or more, and most preferably 100 mass%.

[0057] The solid electrolyte layer may further contain a binder in addition to the above-mentioned solid electrolyte. The examples and preferred forms described in the section on the negative electrode active material layer may also be adopted for the binder that may be contained in the solid electrolyte layer.

[0058] The thickness of the solid electrolyte layer varies depending on the configuration of the intended lithium ion secondary battery, but from the viewpoint of improving the volumetric energy density of the battery, it is preferably 600 μm or less, more preferably 500 μm or less, and even more preferably 400 μm or less. On the other hand, there is no particular restriction on the lower limit of the thickness of the solid electrolyte layer, but it is preferably 10 μm or more, more preferably 50 μm or more, and even more preferably 100 μm or more.

[0059] [Cathode active material layer] In the secondary battery according to this embodiment, the positive electrode active material layer includes a positive electrode active material containing sulfur. The type of the positive electrode active material containing sulfur is not particularly limited, but may include, in addition to elemental sulfur (S), particles or thin films of organic sulfur compounds or inorganic sulfur compounds, and may be any material capable of releasing lithium ions during charging and absorbing lithium ions during discharging by utilizing the oxidation-reduction reaction of sulfur. Examples of the organic sulfur compound include disulfide compounds, sulfur-modified polyacrylonitrile, sulfur-modified polyisoprene, rubeanic acid (dithiooxamide), polycarbonate sulfide, and the like, which are typified by compounds described in the pamphlet of International Publication No. 2010 / 044437. Among these, disulfide compounds, sulfur-modified polyacrylonitrile, and rubeanic acid are preferred, and sulfur-modified polyacrylonitrile is particularly preferred. As the disulfide compound, a compound having a dithiobiurea derivative, a thiourea group, a thioisocyanate, or a thioamide group is more preferred. Here, the sulfur-modified polyacrylonitrile is a modified polyacrylonitrile containing sulfur atoms, which is obtained by mixing sulfur powder with polyacrylonitrile and heating the mixture under an inert gas or under reduced pressure. Its estimated structure is, for example, as shown in Chem. Mater. 2011, 23, 5024-5028, in which polyacrylonitrile is ring-closed to form a polycyclic ring, and at least a part of S is bonded to C. The compound described in this document has a peak at 1330 cm in the Raman spectrum. -1 and 1560cm -1 There is a strong peak signal near 307 cm -1 , 379cm -1 , 472cm -1 , 929cm -1There is a peak around 1000 nm. On the other hand, inorganic sulfur compounds are preferred because of their excellent stability, and specific examples thereof include sulfur element (S), TiS2, TiS3, TiS4, NiS, NiS2, CuS, FeS2, Li2S, MoS2, and MoS3. Among them, S, S-carbon composite, TiS2, TiS3, TiS4, FeS2, and MoS2 are preferred, sulfur element (S), TiS2, and FeS2 are more preferred, and sulfur element (S) is particularly preferred from the viewpoint of high capacity. As the sulfur element (S), α-sulfur, β-sulfur, or γ-sulfur having an S8 structure can be used. These sulfur elements absorb lithium ions during discharge and exist in the positive electrode active material layer in the form of lithium (poly)sulfides.

[0060] Here, when elemental sulfur (S) is used as the positive electrode active material, the elemental sulfur (S) as the positive electrode active material is preferably contained in the positive electrode active material in the form of a composite material obtained by compounding with a conductive material. This composite material is in a state where a mixture of elemental sulfur and a conductive material is compounded by heat treatment or mechanical mixing. More specifically, it is in a state where sulfur is distributed on the surface or in the pores of the conductive material, a state where sulfur and the conductive material are uniformly dispersed at the nano level and aggregated to form particles, a state where the conductive material is distributed on the surface or inside of fine sulfur particles, or a state where a plurality of these states are combined.

[0061] As the conductive material constituting the composite material, a carbon material is preferably used. The carbon material is not particularly limited, but examples thereof include activated carbon (for example, MSC-30 manufactured by Kansai Thermochemical Co., Ltd.), carbon black, acetylene black, Ketjen Black (registered trademark), carbon fiber, graphene, etc. In addition, it is also possible to use these in combination. For example, when activated carbon and Ketjen Black (registered trademark) are used in combination, there is an advantage that the plateau region in charge and discharge is expanded, and the maintenance rate of the charge and discharge capacity is high even if the charge and discharge cycles are repeated. Among them, it is preferable that the carbon material has pores, and more preferably, it is activated carbon. In addition, when the conductive material has pores, it is particularly preferable that the positive electrode active material and the internal resistance reducing agent are arranged inside the pores.

[0062] The positive electrode active material layer may further contain a positive electrode active material that does not contain sulfur in addition to the positive electrode active material that contains sulfur. Examples of the positive electrode active material that does not contain sulfur include layered rock salt type active materials such as LiCoO2, LiMnO2, LiNiO2, LiVO2, and Li(Ni-Mn-Co)O2, LiMn2O4, LiNi 0.5 Mn 1.5 Examples of oxide active materials other than those mentioned above include spinel-type active materials such as LiFePO4 and LiMnPO4, olivine-type active materials such as Li2FeSiO4 and Li2MnSiO4, and Si-containing active materials such as Li4Ti5O 12 Examples include:

[0063] In some cases, two or more kinds of positive electrode active materials may be used in combination. Of course, other positive electrode active materials than those mentioned above may be used. However, the content ratio of the positive electrode active material containing sulfur in the total amount of the positive electrode active material (100% by mass) is preferably 50% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, even more preferably 90% by mass or more, particularly preferably 95% by mass or more, and most preferably 100% by mass.

[0064] The shape of the positive electrode active material may be, for example, particulate (spherical, fibrous), thin film, etc. When the positive electrode active material is particulate, its average particle diameter (D 50 ) is, for example, preferably in the range of 1 nm to 100 μm, more preferably in the range of 10 nm to 50 μm, further preferably in the range of 100 nm to 20 μm, and particularly preferably in the range of 1 to 20 μm. In this specification, the average particle diameter (D 50 The value of can be measured by a laser diffraction scattering method.

[0065] The content of the positive electrode active material in the positive electrode active material layer is not particularly limited, but is preferably within a range of 35 to 99 mass %, and more preferably within a range of 40 to 90 mass %. When the positive electrode active material is in the form of the composite material, the content is calculated based on the mass of only the positive electrode active material (sulfur element) excluding the conductive material.

[0066] The positive electrode active material layer may further include a conductive assistant and / or a binder, and the specific and preferred forms thereof may be the same as those described in the section on the negative electrode active material layer above. Similarly, the positive electrode active material layer preferably further includes a solid electrolyte, and more preferably includes a sulfide solid electrolyte. The specific and preferred forms of the solid electrolyte, such as the sulfide solid electrolyte, may be the same as those described in the section on the negative electrode active material layer above.

[0067] Therefore, according to a preferred embodiment of the present invention, a secondary battery positive electrode material is provided, which includes a positive electrode active material containing sulfur, a conductive material, a sulfide solid electrolyte, and the internal resistance reducing agent according to this embodiment. According to another preferred embodiment of the present invention, a secondary battery positive electrode material is also provided, which includes a positive electrode active material containing sulfur, a conductive material having pores, a sulfide solid electrolyte, and the internal resistance reducing agent according to this embodiment, and the positive electrode active material and the internal resistance reducing agent are disposed inside the pores. According to the secondary battery positive electrode material according to these embodiments, it is possible to make a large amount of the internal resistance reducing agent present in the reaction field where the electrode reaction of sulfur progresses, and also to sufficiently secure the electron conduction path to sulfur, which has the advantage that the effect of the present invention can be further exerted.

[0068] In the internal resistance reducing agent for the positive electrode active material layer according to the present embodiment, the active ingredient is an ionic crystalline compound having a basic structure consisting of atoms A and B. Here, the atom A constituting the basic structure of the ionic crystalline compound, which is the active ingredient of the internal resistance reducing agent, is an atom that becomes a cationic atom when the ionic crystalline compound dissociates into ions. On the other hand, the atom B constituting the basic structure is an atom that becomes an anionic atom when the ionic crystalline compound dissociates into ions. The ionic crystalline compound "has a basic structure consisting of atoms A and B" means that the ionic crystalline compound contains, as the main component of the compound, a crystal structure formed by regularly arranging atoms A and B, respectively. Therefore, as long as this definition and the definition of the mathematical formula 1 described later are satisfied, the ionic crystalline compound may be one in which at least a part of atom A or atom B is replaced by another atom. There is no particular limitation on the specific type of atom that can replace atom A and / or atom B, and it can be replaced by any atom that satisfies the valence of the ionic crystalline compound. Furthermore, with regard to the above-mentioned "main component", the content of other atoms substituting atom A and / or atom B is preferably 5 atomic % or less, more preferably 3 atomic % or less, even more preferably 1 atomic % or less, and most preferably 0 atomic %, based on 100 mol % of all atoms constituting the ionic crystalline compound.

[0069] The ionic crystalline compound that is the active ingredient of the internal resistance reducing agent is also characterized in that the parameter X of the compound, which is expressed by the following mathematical formula 1, satisfies 0.032≦X≦0.072.

[0070]

number

[0071] In Formula 1, E atom represents the energy per atom of the ionic crystalline compound [eV], and Z cat represents the atomic number of the atom A, and L a represents the length [Å] of the crystal lattice a of the ionic crystalline compound. The process of deriving the relational expression (0.032≦X≦0.072) using the parameter X will be described below.

[0072] In order to identify the rate-determining step in the charge / discharge reaction in a lithium-ion secondary battery using a sulfur-containing positive electrode active material, the present inventors analyzed the elementary reactions that constitute the above-mentioned charge / discharge reaction using the density functional theory, which is an electronic state calculation method based on the density functional theory (DFT). Here, the density functional theory (DFT) (density functional theory) is a type of first-principles calculation that predicts physical properties and chemical reactions from the Schrödinger equation (Dirac equation) without using experimental data or empirical parameters, and is a method of calculating the formation energy Eg and the energy level of the molecular orbital (the orbit in which the electrons that constitute the molecule can exist) for the molecular structure to be calculated.

[0073] Here, since elemental sulfur (S8) does not contain lithium, when viewed as a positive electrode active material, it can be said that a lithium ion secondary battery containing this positive electrode active material is in the most charged state. On the other hand, as the discharge of this lithium secondary battery progresses, elemental sulfur (S8), which is the positive electrode active material, gradually combines with lithium to form various reduction products, and finally becomes Li2S. In other words, it can be said that a lithium ion secondary battery containing only Li2S as a positive electrode active material is in the most discharged state.

[0074] Here, the reduction products (intermediates) that have different molar ratios of sulfur atoms and lithium atoms between elemental sulfur (S8) and Li2S can be assumed to be (S8) → Li2S8 → Li2S7 → Li2S6 → Li2S5 → Li2S4 → Li2S3 → Li2S2 → (Li2S). Therefore, the inventors performed structural optimization (calculation to change the positions of atoms constituting the molecule and obtain the structure with the lowest formation energy) based on DFT for elemental sulfur (S8) and Li2S and each of these assumed reduction products (intermediates), and calculated the formation energy for a stable atomic configuration. Then, for all cases assumed as combinations of reactants and products, the formation energy of the product (E products ) to the energy of formation of the reactants (E reactants The Gibbs free energy (ΔG) for each reaction was calculated by subtracting the above factor from the equation. The detailed calculation conditions are as follows: Simulation program: Vienna ab-initio simulation package (VASP) Correlation functional: B3LYP Cutoff energy: 400 [eV] Pseudopotential: PAW GGA Electronic relaxation algorithm: preconditioned residuum-minimization Ion relaxation algorithm: RMM-DIIS.

[0075] Here, in the charging reaction, ΔG in each reaction is a positive value, and the product is energetically more unstable than the reactants. For this reason, in the charging reaction, it was determined that the reaction with the smallest ΔG among the reactions assumed when the reactants are fixed is actually proceeding. The results of actual calculations assuming the charging reaction of a lithium secondary battery containing Li2S as the positive electrode active material, which is the most discharged state, are shown in Table 1 below (values ​​are rounded to two decimal places).

[0076] [Table 1]

[0077] As shown in Table 1, for Li2S, for example, the reaction (2Li2S → Li2S2 + 2Li) is assumed to release lithium and generate Li2S2. The energy of reaction (E reactants ) and the energy of formation of the reactants (E products ) are 14.41 [eV] and 15.44 [eV], respectively, and the Gibbs free energy calculated as the difference between these (ΔG = E products -E reactants ) is calculated to be 1.02 [eV].

[0078] In addition to the above, Li2S is also expected to react with Li2S2, Li2S3, Li2S4, Li2S5, Li2S6, and Li2S7 to produce Li2S3, Li2S4, Li2S5, Li2S6, Li2S7, and Li2S8, respectively. The ΔG of each of these reactions is shown in Table 1 above, but all of them are larger than the ΔG of the reaction that produces Li2S2. Therefore, it was concluded that the reaction that produces Li2S2, which has the smallest ΔG, actually proceeds with Li2S. Furthermore, this analysis was continued in the same way, and it was concluded that the reaction that actually proceeds with the smallest ΔG (shown in bold in Table 1) among the reactions that are expected for each reactant. As a result, it was thought that in the charging reaction, Li2S produces Li2S2, and then Li2S3, Li2S4, Li2S5, Li2S6, Li2S7, Li2S8, and S8 in that order. Here, the reaction with the largest ΔG among the eight reactions from Li2S to S8 is the reaction of producing S8 from Li2S in the final stage (Li2S8→S8+2Li). Based on this, it was thought that this reaction of producing S8 is the reaction with the slowest reaction rate (rate-determining reaction) in the charging process.

[0079] On the other hand, for the discharge reaction, we assumed that the discharge reaction of a lithium secondary battery containing S8 as the positive electrode active material, which is in the most charged state, would proceed, and the results of the calculations are shown in Table 2 below. Note that in the discharge reaction, ΔG in each reaction is a negative value, and the product is more energetically stable than the reactant. For this reason, in the discharge reaction, we determined that the reaction with the largest absolute value of ΔG is actually proceeding among the reactions assumed when the reactants are fixed.

[0080] [Table 2]

[0081] As shown in Table 2, only the reaction that produces Li2S8 (S8+2Li→Li2S8) is assumed for S8. After that, Li2S8 produces Li2S4 (Li2S8+2Li→2Li2S4), Li2S4 produces Li2S2 (Li2S4+2Li→2Li2S2), and Li2S2 produces Li2S (Li2S2+2Li→2Li2S) so that the absolute value of ΔG is maximized (shown in bold in Table 2). Here, as mentioned above, in the discharge reaction, the product is more energetically stable than the reactant. However, in order for the reaction to actually proceed, it is necessary to exceed the excitation energy of the reactant of each reaction. Therefore, the excitation energy of the reactants (S8, Li2S8, Li2S4, Li2S2) was calculated for each of the four reactions from S8 to Li2S mentioned above. Specifically, the energy level (E LUMO ) and the Fermi level (the energy level at which the probability of an electron existing is 50%; E fermi ) corresponds to the excitation energy, and the excitation energy E° is expressed as E°=E LUMO -E fermiThe calculation was performed according to the formula. As a result, the excitation energy E° of each of the above four reactions was calculated as the value shown in Table 2 above. Here, the reaction with the largest excitation energy E° among the four reactions from S8 to Li2S is the reaction of producing Li2S8 from S8 in the first stage (S8+2Li→Li2S8). From this, it was considered that the reaction of producing Li2S8 from S8 is the reaction with the slowest reaction rate (rate-determining reaction) in the discharge process.

[0082] From the above-mentioned DFT-based calculations, it was determined that the rate-limiting reaction in the charging process of a lithium-ion secondary battery using a positive electrode active material containing sulfur is the reaction of forming S8 from Li2S (Li2S8 → S8 + 2Li). Similarly, it was determined that the rate-limiting reaction in the discharging process of a lithium-ion secondary battery using a positive electrode active material containing sulfur is the reaction of forming Li2S8 from S8 (S8 + 2Li → Li2S8). Here, the energy phase diagram of the above two rate-limiting reactions is shown in Figure 3. As shown in Figure 3, the reaction of forming Li2S8 from S8 (S8 + 2Li → Li2S8), which is the rate-limiting reaction in the discharging reaction, is an exothermic reaction with a negative ΔG value. However, although this reaction is an exothermic reaction, the band gap energy (activation energy) E b Unless energy exceeding this is given, the reaction will not proceed. In contrast, the rate-determining reaction in the charging reaction, the production reaction of S8 from Li2S (Li2S8 → S8 + 2Li), is an endothermic reaction with a positive ΔG. This reaction is determined by the Gibbs free energy (ΔG) and the band gap energy (activation energy) E b The energy barrier (E a ) energy is required for the reaction to proceed.

[0083] Based on these findings, the present inventors have searched for additives that can reduce ΔG, which is one of the indicators of the energy barrier in the reaction of producing S8 from Li2S (Li2S8 → S8 + 2Li) among the two rate-determining reactions mentioned above. Specifically, the present inventors have conducted research on various ionic crystalline compounds. In the process, for 26 types of physical parameters possessed by various ionic crystalline compounds, physical parameters that have a large effect on the reduction of the Gibbs free energy (ΔG) of the above reaction (i.e., have a large correlation coefficient with the reduction of the Gibbs free energy (ΔG) of the above reaction) were examined by statistical analysis. In this case, the values ​​of the 26 types of physical parameters were adopted from the values ​​listed on the Materials Project website (https: / / materialsproject.org / ). Meanwhile, the values ​​of the Gibbs free energy (ΔG) of the above reaction when Li2S8 comes into contact with each ionic crystalline compound were calculated using the same simulation program as above. Detailed calculation conditions are as follows: Simulation program: Vienna ab-initio simulation package (VASP) Correlation functional: B3LYP Cutoff energy: 500 [eV] Pseudopotential: PAW GGA Electronic relaxation algorithm: preconditioned residuum-minimization Ion relaxation algorithm: RMM-DIIS.

[0084] Various software can be used for statistical analysis, but here we used JUSE-StatWorks (Japan Science and Technology Training Institute, Inc.). As a result, we identified the following three types of physical property parameters that have a high correlation coefficient with the reduction in the Gibbs free energy (ΔG) of the above reaction: (1) Energy per atom of ionic crystalline compounds (E atom ) [eV]; (2) The atomic number of the atom A (Z cat )[-]; (3) The length of the crystal lattice a of an ionic compound (L a ) [Å].

[0085] The three types of physical parameters thus identified have different units and digits. For this reason, the above formula 1 is the result of multiplying the three types of physical parameters after standardizing them. atom The value of "Final Energy / Atom" listed on the "Calculation Summary" page for the compound in question on the Materials Project website is used. cat The value of is used as given in the periodic table. a The value of a is taken from the "Lattice Parameters" for the compound in question on the Materials Project website.

[0086] The relationship between the parameter X obtained by substituting the physical property parameters of 11 kinds of ionic compounds into the mathematical formula 1 derived in this way and the Gibbs free energy (ΔG) of the reaction calculated above was examined. The results are shown in Table 3 below.

[0087] [Table 3]

[0088] As shown in Table 3, among various ionic crystalline compounds, if the parameter X satisfies 0.032≦X≦0.072, the Gibbs free energy (ΔG) of the above reaction when the compound comes into contact with Li2S8 is positive and smaller than that when graphite is added as an additive. A positive and smaller ΔG is preferable because it means that the reaction barrier is smaller without destabilizing the above reaction.

[0089] For the above reasons, the parameter X is set to a range of 0.032 to 0.072 (0.032≦X≦0.072) so that ΔG is positive and smaller compared to when graphite is used as an additive among the ionic crystalline compounds as additives. From the viewpoint of excellent ΔG reduction effect, the parameter X preferably satisfies 0.037≦X≦0.072, more preferably satisfies 0.042≦X≦0.072, and further preferably satisfies 0.061≦X≦0.072. Here, FIG. 4A shows the energy (E atom ) is normalized as the parameter element ((E atom 4B is a graph plotting the relationship between the atomic number (Z + 12.79) / 11.77) of the atom A constituting the ionic crystalline compounds described in the examples and comparative examples in Table 3 and the Gibbs free energy (ΔG) of the above reaction. cat ) is normalized as a parameter element ((Z cat 4C is a graph plotting the relationship between the Gibbs free energy (ΔG) of the above reaction and the crystal lattice a length (L a ) is normalized as the parameter element ((L a 4A to 4C, the relationship between the Gibbs free energy (ΔG) of the above reaction and the normalized parameter X (−70.68) / 68.54) is plotted. As can be seen from the graphs shown in FIG. 4A to FIG. 4C, the correlation with ΔG is not so large for each of these three types of normalized parameter elements, and it cannot be concluded that the larger these normalized parameter elements (or parameters before normalization) are, the greater the effect of reducing ΔG is. In contrast, according to the present invention, it has been found that by controlling the parameter X represented by the above-mentioned formula 1 to a value within a predetermined range, it can be suitably used as an internal resistance reducer for the positive electrode active material layer through the effect of reducing the Gibbs free energy (ΔG) of the above reaction.

[0090] There is no particular restriction on the specific ionic crystalline compound that satisfies the above-mentioned specification regarding the parameter X, and any compound that has a parameter X calculated by the above-mentioned calculation process within the above-mentioned range can be used without any particular restriction. From the viewpoint of excellent effects of the present invention, preferred examples of the atoms A and B constituting the ionic crystalline compound that can be used as an active ingredient of the internal resistance reducing agent according to this embodiment include, but are not limited to, O, N, P, C, and S as the atom B that becomes an anion upon dissociation. On the other hand, the atom A that becomes a cation upon dissociation includes, but is not limited to, Ta, Pb, Cs, In, and Zn. Specific examples of ionic crystalline compounds having a basic structure consisting of these atoms A and B include TaC, PbS, Cs3P7, In5S4, or ZnS. Among them, from the viewpoint of a higher effect of reducing ΔG, preferably PbS, Cs3P7, In5S4 or ZnS is used, more preferably Cs3P7, In5S4 or ZnS is used, further preferably In5S4 or ZnS is used, and most preferably ZnS is used. When these preferred compounds are used as additives, the value of the Gibbs free energy (ΔG) of the reaction (rate-determining reaction in the charging process) generating S8 from Li2S8 becomes particularly small, and the internal resistance of the positive electrode active material layer is reduced, making it possible to significantly improve the charge and discharge rate characteristics of the secondary battery.

[0091] As described above, the internal resistance reducing agent for the positive electrode active material layer according to the present embodiment can be added to the positive electrode active material layer of a secondary battery positive electrode containing a sulfur-containing positive electrode active material to reduce the internal resistance of the positive electrode active material layer. As a result, the charge / discharge rate characteristics can be improved in a secondary battery using a sulfur-containing positive electrode active material. Here, the estimated mechanism by which the internal resistance reducing agent according to the present embodiment reduces the internal resistance in the positive electrode active material layer of a secondary battery using a sulfur-containing positive electrode active material is speculated as follows.

[0092] That is, as a result of the above-mentioned statistical analysis, the above three types of physical parameters have been identified as physical parameters with a large correlation coefficient with the reduction in the Gibbs free energy (ΔG) of the reaction that produces S8 from Li2S8 (the rate-determining reaction in the charging process). Considering the influence that these three types of physical parameters may have on the reduction in ΔG, first, the energy per atom of the ionic crystalline compound (E atom ) means that the larger this value is, the higher the stability of the crystal of the basic structure of the ionic crystalline compound. atom It is believed that adding an ionic crystalline compound with a large atomic number a of the ionic crystalline compound promotes the reaction of S8 to Li2S8 even when there is interaction with other atoms. The larger the atomic number of atom A, the greater the number of electrons and the longer the interatomic distance in the crystal. For this reason, it is believed that adding an ionic crystalline compound with atom A with a large atomic number promotes the compound to interact more strongly with the sulfur atom, making it easier to break the SS bond and promoting the reaction of S8 to Li2S8. Finally, the length a of the crystal lattice of the ionic crystalline compound (L a ), the larger this value, the smaller the electrostatic repulsion with sulfur. Therefore, the length of the crystal lattice a of the ionic crystalline compound (L a It is believed that when an ionic crystalline compound with a large valence ratio is added, the compound interacts more strongly with the sulfur atom, making it easier to break the S-S bond and promoting the reaction of S8 to Li2S8.

[0093] In the positive electrode material for secondary batteries according to this embodiment, the content of the internal resistance reducing agent is not particularly limited, but is preferably 5% by mass or less, more preferably 2% by mass or less, and even more preferably 1% by mass or less, relative to 100% by mass of the positive electrode material. By adopting such a configuration, the content of the positive electrode active material contained in the positive electrode material is prevented from becoming too small more than necessary, which can effectively contribute to improving the energy density of the battery. In addition, the blending balance of each component in the positive electrode active material layer is appropriate, and the paths of electronic conduction and ion conduction can be sufficiently secured. There is no particular limit on the lower limit of the content of the internal resistance reducing agent, but from the viewpoint of expressing the function as an internal resistance reducing agent, it is preferably 0.1% by mass or more, more preferably 0.3% by mass or more, and particularly preferably 0.5% by mass or more. In addition, when the positive electrode material for secondary batteries according to this embodiment contains a conductive material together with a sulfide solid electrolyte, the mass ratio of the internal resistance reducing agent to the conductive material is not particularly limited. However, from the viewpoint of sufficiently securing an electron conduction path to sulfur, the ratio of the mass of the conductive material to the mass of the internal resistance reducing agent (conductive material / internal resistance reducing agent) is preferably 8 or more, more preferably 10 or more, even more preferably 13 or more, and particularly preferably 17 or more. There is no particular restriction on the upper limit of this value, but an example is 200 or less, preferably 150 or less, more preferably 100 or less, and particularly preferably 50 or less.

[0094] [Positive and negative current collectors] The material constituting the current collector plates (25, 27) is not particularly limited, and any known highly conductive material conventionally used as a current collector plate for a secondary battery may be used. As the material constituting the current collector plates, for example, metal materials such as aluminum, copper, titanium, nickel, stainless steel (SUS), and alloys thereof are preferable. From the viewpoints of light weight, corrosion resistance, and high conductivity, aluminum and copper are more preferable, and aluminum is particularly preferable. The positive electrode current collector plate 27 and the negative electrode current collector plate 25 may be made of the same material or different materials.

[0095] [Positive and negative leads] Although not shown in the figures, the current collectors (11', 11") and the current collecting plates (25, 27) may be electrically connected via positive and negative electrode leads. As the constituent materials of the positive and negative electrode leads, materials used in known lithium ion secondary batteries may be similarly used. Note that the parts removed from the exterior are preferably covered with a heat-resistant insulating heat-shrink tube or the like to prevent them from coming into contact with peripheral devices or wiring, causing electric leakage and affecting products (e.g., automobile parts, particularly electronic devices, etc.).

[0096] [Battery exterior materials] As the battery exterior material, a known metal can case can be used, and a bag-shaped case using a laminate film 29 containing aluminum, which can cover the power generating element as shown in Figs. 1 and 2, can be used. The laminate film can be, for example, a three-layer laminate film formed by laminating PP, aluminum, and nylon in this order, but is not limited thereto. A laminate film is preferable from the viewpoint of being excellent in high output and cooling performance and being suitable for use in batteries for large equipment such as EVs and HEVs. In addition, a laminate film containing aluminum is more preferable as the exterior body because it can easily adjust the group pressure applied to the power generating element from the outside.

[0097] The stacked battery according to the present embodiment has a configuration in which a plurality of unit cell layers are connected in parallel, and thus has high capacity and excellent cycle durability, and is therefore suitable for use as a driving power source for EVs and HEVs.

[0098] While one embodiment of a lithium ion secondary battery has been described above, the present invention is not limited to the configuration described in the above embodiment, and may be modified as appropriate based on the claims.

[0099] For example, the type of battery to which the lithium ion secondary battery according to the present invention can be applied includes a bipolar battery including a bipolar electrode having a positive electrode active material layer electrically bonded to one surface of a current collector and a negative electrode active material layer electrically bonded to the opposite surface of the current collector.

[0100] In addition, the secondary battery according to the present embodiment does not have to be an all-solid-state type. That is, the solid electrolyte layer may further contain a conventionally known liquid electrolyte (electrolytic solution). There is no particular limit to the amount of liquid electrolyte (electrolytic solution) that can be contained in the solid electrolyte layer, but it is preferable that the amount is such that the shape of the solid electrolyte layer formed by the solid electrolyte is maintained and leakage of the liquid electrolyte (electrolytic solution) does not occur.

[0101] The liquid electrolyte (electrolytic solution) that can be used has a form in which a lithium salt is dissolved in an organic solvent. Examples of the organic solvent that can be used include dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), ethyl methyl carbonate (EMC), methyl propionate (MP), methyl acetate (MA), methyl formate (MF), 4-methyldioxolane (4MeDOL), dioxolane (DOL), 2-methyltetrahydrofuran (2MeTHF), tetrahydrofuran (THF), dimethoxyethane (DME), propylene carbonate (PC), butylene carbonate (BC), dimethyl sulfoxide (DMSO), and γ-butyrolactone (GBL). Among these, from the viewpoint of further improving the rapid charging characteristics and output characteristics, the organic solvent is preferably a chain carbonate, more preferably at least one selected from the group consisting of diethyl carbonate (DEC), ethyl methyl carbonate (EMC) and dimethyl carbonate (DMC), and more preferably selected from ethyl methyl carbonate (EMC) and dimethyl carbonate (DMC).

[0102] Examples of the lithium salt include Li(FSO2)2N (lithium bis(fluorosulfonyl)imide; LiFSI), Li(C2F5SO2)2N, LiPF6, LiBF4, LiClO4, LiAsF6, and LiCF3SO3. Among these, the lithium salt is preferably Li(FSO2)2N (LiFSI) from the viewpoints of battery output and charge / discharge cycle characteristics.

[0103] The liquid electrolyte (electrolytic solution) may further contain additives other than the above-mentioned components. Specific examples of such compounds include ethylene carbonate, vinylene carbonate, methylvinylene carbonate, dimethylvinylene carbonate, phenylvinylene carbonate, diphenylvinylene carbonate, ethylvinylene carbonate, diethylvinylene carbonate, vinylethylene carbonate, 1,2-divinylethylene carbonate, 1-methyl-1-vinylethylene carbonate, 1-methyl-2-vinylethylene carbonate, 1-ethyl-1-vinylethylene carbonate, 1-ethyl-2-vinylethylene carbonate, and 1-ethyl-2-vinylethylene carbonate. Examples of the additives include ethylene carbonate, vinyl vinylene carbonate, allyl ethylene carbonate, vinyloxymethyl ethylene carbonate, allyloxymethyl ethylene carbonate, acryloxymethyl ethylene carbonate, methacryloxymethyl ethylene carbonate, ethynyl ethylene carbonate, propargyl ethylene carbonate, ethynyloxymethyl ethylene carbonate, propargyl oxyethylene carbonate, methylene ethylene carbonate, and 1,1-dimethyl-2-methylene ethylene carbonate. These additives may be used alone or in combination of two or more. The amount of additive used in the electrolyte solution may be appropriately adjusted.

[0104] [Battery pack] A battery pack is a device that consists of multiple batteries connected together. More specifically, it is a device that uses at least two batteries and is configured in series or parallel or both. By connecting them in series or parallel, it is possible to freely adjust the capacity and voltage.

[0105] A small, removable assembled battery can be formed by connecting a plurality of batteries in series or in parallel. Then, a large capacity, high output assembled battery (battery module, battery pack, etc.) suitable for a vehicle driving power source or an auxiliary power source that requires a high volumetric energy density and a high volumetric output density can be formed by further connecting a plurality of such small, removable assembled batteries in series or in parallel. How many batteries are connected to form an assembled battery, and how many stages of small assembled batteries are stacked to form a large capacity assembled battery can be determined according to the battery capacity and output of the vehicle (electric vehicle) in which the battery is to be installed.

[0106] [vehicle] The battery or a battery pack formed by combining a plurality of batteries can be mounted on a vehicle. In the present invention, a battery with excellent long-term reliability and long life can be configured, and thus, by mounting such a battery, a plug-in hybrid electric vehicle with a long EV driving distance or an electric vehicle with a long driving distance per charge can be configured. For example, if the battery or a battery pack formed by combining a plurality of batteries is used in a hybrid vehicle, a fuel cell vehicle, or an electric vehicle (all of which include four-wheeled vehicles (commercial vehicles such as passenger cars, trucks, and buses, and light vehicles, etc.), as well as two-wheeled vehicles (motorcycles) and three-wheeled vehicles), the vehicle will have a long life and high reliability. However, the application is not limited to automobiles, and the battery pack can be applied to, for example, various power sources for other vehicles, such as moving bodies such as trains, and can also be used as a mounted power source for an uninterruptible power supply device or the like. [Explanation of symbols]

[0107] 10a Stacked battery, 11' negative electrode current collector, 11” positive electrode current collector, 13 negative electrode active material layer, 15 positive electrode active material layer, 17 solid electrolyte layer, 19 cell layer, 21 Power generation elements, 25 negative current collector plate, 27 Positive current collector, 29 Laminating film.

Claims

1. The sulfur-containing cathode active material is added to a cathode active material layer of a secondary battery cathode containing an elemental sulfur, and is used to reduce the internal resistance of the cathode active material layer, The present invention comprises an ionic crystalline compound as an active ingredient, the ionic crystalline compound having a basic structure consisting of an atom A which becomes a cationic atom when the ionic crystalline compound dissociates into ions, and an atom B which becomes an anionic atom, An internal resistance reducing agent for a positive electrode active material layer, in which a parameter X represented by the following mathematical formula 1 for the ionic crystalline compound satisfies 0.032≦X≦0.072: [0010] In the formula, E atom represents the energy [eV] per atom of the ionic crystalline compound, Z cat represents the atomic number of the atom A, and L a represents the length [Å] of the crystal lattice a of the ionic crystalline compound.

2. The internal resistance reducing agent according to claim 1, wherein X satisfies 0.042≦X≦0.

072.

3. The internal resistance reducing agent according to claim 1 or 2, wherein the atom B is O, N, P, C or S.

4. The internal resistance reducing agent according to any one of claims 1 to 3, wherein the atom A is Ta, Pb, Cs, In or Zn.

5. The ionic crystalline compound is TaC, PbS, Cs 3 P 7 , In 5 S 4 The internal resistance reducing agent according to claim 1 , further comprising ZnS.

6. The ionic crystalline compound is Cs 3 P 7 , In 5 S 4 The internal resistance reducing agent according to claim 5 , further comprising ZnS.

7. A positive electrode material for a secondary battery, comprising: a positive electrode active material containing elemental sulfur; a conductive material; a sulfide solid electrolyte; and the internal resistance reducing agent according to any one of claims 1 to 6.

8. 8. The positive electrode material for a secondary battery according to claim 7, wherein the conductive material has pores, and the positive electrode active material and the internal resistance reducing agent are disposed inside the pores.

9. 9. The positive electrode material for a secondary battery according to claim 7, wherein the content of the internal resistance reducing agent is 2 mass% or less with respect to 100 mass% of the positive electrode material.

Citation Information

Patent Citations

  • Nonaqueous electrolyte battery

    JP2005251469A

  • Lithium-ion battery

    JP2012146399A

  • Positive electrode for lithium ion secondary battery, lithium ion secondary battery, and method for producing positive electrode for lithium ion secondary battery

    JP2012150948A

  • Positive electrode mixture and all-solid-state lithium sulfur battery

    JP2015176849A

  • Positive electrode active material for lithium-sulfur batteries containing metal sulfide nanoparticles and method for manufacturing the same

    JP2019517729A