Coil-type electronic components

The coil type electronic component uses first and second soft magnetic metal particles with varying saturation magnetization to enhance inductance and DC superimposition characteristics, addressing the low direct current superimposition issue in laminated coils.

JP7594967B2Active Publication Date: 2024-12-05TDK CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021067203
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-04-12
Publication Date
2024-12-05
Estimated Expiration
2041-04-12

AI Technical Summary

Technical Problem

Laminated coils using Fe-Ni particles as a magnetic material have high inductance but low direct current superimposition characteristics.

Method used

The coil type electronic component incorporates first and second soft magnetic metal particles, where the first particles have higher saturation magnetization than the second, with specific arrangements and ratios to enhance inductance and DC superimposition characteristics.

Benefits of technology

The configuration results in a coil with sufficiently high inductance and DC superimposition characteristics, improved plating elongation suppression, and reduced short circuits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007594967000022
    Figure 0007594967000022
  • Figure 0007594967000023
    Figure 0007594967000023
  • Figure 0007594967000024
    Figure 0007594967000024
Patent Text Reader

Abstract

To provide a coil type electronic component with sufficiently high inductance (L) and DC superimposition characteristics (Idc).SOLUTION: A laminated coil 1 includes a magnetic element 4 and a coil conductor 5. An interlayer first magnetic element 40a positioned between layers of coil conductors adjacent to each other in the axial center N direction of the coil conductor 5 contains first soft magnetic metal particles. A second magnetic element 42 located outside along the axis N contains second soft magnetic metal particles. The first soft magnetic metal particles have higher saturation magnetization (Ms) than that of the second soft magnetic metal particles.SELECTED DRAWING: Figure 1A
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a coil-type electronic component. [Background technology]

[0002] Patent Document 1 describes an invention related to a soft magnetic alloy powder, which is characterized by containing Fe-Ni based particles in which the contents of Fe, Ni, Co and Si are each controlled within a specific range.

[0003] However, while multilayer coils that use Fe-Ni particles as the magnetic material have high inductance, they suffer from the problem of low DC bias characteristics. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2008-135674 A Summary of the Invention [Problem to be solved by the invention]

[0005] An object of the present invention is to provide a coil-type electronic component having sufficiently high inductance (L) and DC superposition characteristics (Idc). [Means for solving the problem]

[0006] The coil-type electronic component according to the present invention comprises: An electronic component including an element having a magnetic body and a coil conductor, the magnetic body located between adjacent layers of the coil conductor in an axial direction of the coil conductor includes first soft magnetic metal particles, the magnetic element located on the outer side along the axis includes second soft magnetic metal particles, The first soft magnetic metal particles have a higher saturation magnetization than the second soft magnetic metal particles.

[0007] The coil-type electronic component according to the present invention has the above-mentioned configuration and therefore has sufficiently high inductance and DC bias characteristics.

[0008] The first soft magnetic metal particles are preferably Fe-Si alloys. This allows the saturation magnetization of the first soft magnetic metal particles to be higher. As a result, the saturation magnetization of the first soft magnetic metal particles is easier to be made higher than that of the second soft magnetic metal particles, and therefore the inductance and DC bias characteristics can be sufficiently increased.

[0009] The second soft magnetic metal particles are preferably an Fe-Ni alloy, which makes it easier to make the saturation magnetization of the first soft magnetic metal particles higher than that of the second soft magnetic metal particles, thereby making it possible to sufficiently increase the inductance and DC bias characteristics.

[0010] It is preferable that the inner diameter second magnetic element present in at least a portion of the axial center inner diameter region of the element including the axial center of the coil conductor contains the second soft magnetic metal particles.

[0011] In a cross section perpendicular to the axis of the coil conductor, the ratio of the area of ​​the inner diameter second magnetic body to the area of ​​the axial center inner diameter region is preferably 30% or more, thereby making it possible to improve the balance of inductance and DC bias characteristics.

[0012] The first soft magnetic metal particles preferably have an average particle size of 1 to 6 μm. When the first soft magnetic metal particles have an average particle size of 1 to 6 μm, the inductance can be increased compared to when the first soft magnetic metal particles have an average particle size of less than 1 μm. When the first soft magnetic metal particles have an average particle size of 1 to 6 μm, the inductance can be increased, plating elongation can be suppressed, and the number of short circuits can be reduced compared to when the first soft magnetic metal particles have an average particle size of more than 6 μm.

[0013] The second soft magnetic metal particles preferably have an average particle size of 1 to 15 μm. When the second soft magnetic metal particles have an average particle size of 1 to 15 μm, the inductance can be increased compared to when the second soft magnetic metal particles have an average particle size of less than 1 μm. When the second soft magnetic metal particles have an average particle size of 1 to 15 μm, the DC bias characteristics can be improved, plating elongation can be suppressed, and the number of short circuits can be reduced compared to when the second soft magnetic metal particles have an average particle size of more than 15 μm.

[0014] The second magnetic element, which is present in at least a portion of the axially central outer diameter region of the element located radially outward of the coil conductor, preferably contains the second soft magnetic metal particles, thereby making it possible to further increase inductance.

[0015] In a cross section perpendicular to the axis of the coil conductor, the ratio of the area of ​​the outer diameter of the second magnetic body to the area of ​​the axial center outer diameter region may be 15% or more, thereby making it possible to further improve the DC bias characteristic. [Brief description of the drawings]

[0016] [Figure 1] FIG. 1 is a perspective view of a laminated coil according to one embodiment of the present invention. [Figure 1A] FIG. 1A is a schematic cross-sectional view taken along line IA-IA in FIG. [Figure 1A1] FIG. 1A1 is a schematic cross-sectional view taken along line IAI-IAI in FIG. [Figure 1B] FIG. 1B is a schematic cross-sectional view of a laminated coil according to another embodiment of the present invention. [Figure 1C] FIG. 1C is a schematic cross-sectional view of a laminated coil according to another embodiment of the present invention. [Figure 1D] FIG. 1D is a schematic cross-sectional view of a laminated coil according to another embodiment of the present invention. [Figure 1E] FIG. 1E is a schematic cross-sectional view of a laminated coil according to another embodiment of the present invention. [Figure 2a]FIG. 2a is an explanatory diagram of a method for manufacturing the laminated coil shown in FIG. 1A. [Figure 2b] FIG. 2b is an explanatory diagram of a method for manufacturing the laminated coil shown in FIG. 1A. [Figure 2c] FIG. 2c is an explanatory diagram of a method for manufacturing the laminated coil shown in FIG. 1A. [Figure 2d] FIG. 2d is an explanatory diagram of a method for manufacturing the laminated coil shown in FIG. 1A. [Figure 2e] FIG. 2e is an explanatory diagram of a method for manufacturing the laminated coil shown in FIG. 1A. [Figure 2f] FIG. 2f is an explanatory diagram of a method for manufacturing the laminated coil shown in FIG. 1A. [Figure 2g] FIG. 2g is an explanatory diagram of a method for manufacturing the laminated coil shown in FIG. 1A. [Figure 2h] FIG. 2h is an explanatory diagram of a method for manufacturing the laminated coil shown in FIG. 1A. [Diagram 3] FIG. 3 is a schematic cross-sectional view of a laminated coil according to another embodiment of the present invention. [Figure 4] FIG. 4 is a perspective view of a laminated coil according to another embodiment of the present invention. [Figure 4A] FIG. 4A is a schematic cross-sectional view taken along line IVA-IVA in FIG. [Figure 5A] FIG. 5A is a schematic cross-sectional view of a laminated coil according to a comparative example of the present invention. [Figure 5B] FIG. 5B is a schematic cross-sectional view of a laminated coil according to a comparative example of the present invention. [Figure 5C] FIG. 5C is a schematic cross-sectional view of a laminated coil according to a comparative example of the present invention. [Figure 6] FIG. 6 is a graph in which the X-axis represents the inner diameter second magnetic body ratio (%) and the Y-axis represents (ΔL / L)+(ΔIdc / Idc) (%). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] First embodiment In the following, a laminated coil 1 shown in FIG. 1 will be described as one embodiment of the coil-type electronic component according to this embodiment.

[0018] As shown in Fig. 1, a laminated coil 1 according to this embodiment has an element 2 and a terminal electrode 3. The element 2 has a configuration in which a coil conductor 5 is embedded three-dimensionally and spirally inside a magnetic base body 4. Terminal electrodes 3 are formed on both ends of the element 2, and the terminal electrodes 3 are connected to the coil conductor 5 via lead electrodes 5a1, 5a2. Note that in Fig. 1 and Figs. 1A to 1E, 1A1, 3, 4, 4A, and 5A to 5C described below, the X-axis, Y-axis, and Z-axis are perpendicular to one another.

[0019] In this embodiment, the term "inner side" refers to the side closer to the center of the laminated coil 1 (the axis N of the coil conductor 5), and the term "outer side" refers to the side away from the center of the laminated coil 1.

[0020] The material of the terminal electrode 3 is not particularly limited as long as it is an electrical conductor. For example, Ag, Cu, Au, Al, Ag alloy, Cu alloy, etc. are used. In particular, Ag is preferably used because it is inexpensive and has low resistance. The terminal electrode 3 may contain glass frit. The terminal electrode 3 may have a two-layer structure formed on the element 2, including a metal layer made of the above metal or the above metal and glass frit, and a resin layer made of a conductive resin formed on the metal layer. There is no particular limit to the type of metal contained in the conductive resin. For example, Ag can be used. The terminal electrode 3 may have a surface plated. For example, Cu plating, Ni plating, Sn plating, Cu-Ni-Sn plating, and / or Ni-Sn plating may be appropriately applied.

[0021] The coil conductor 5 and the lead electrodes 5a1 and 5a2 may be made of any material that is an electrical conductor. For example, Ag, Cu, Au, Al, Ag alloy, Cu alloy, etc. are used. In particular, Ag is preferably used because it is inexpensive and has low resistance. The coil conductor 5 may contain glass frit.

[0022] The number of turns of the coil conductor 5 around the axis N is not particularly limited and is, for example, 1.5 to 15.5. The thickness (Te) of the coil conductor 5 is also not particularly limited and is, for example, 5 to 60 μm.

[0023] Fig. 1A is a schematic cross-sectional view taken along line IA-IA in Fig. 1, and is a cross-sectional view parallel to the YZ axes. That is, Fig. 1A is a cross-sectional view in which lead electrodes 5a1 and 5a2 and terminal electrode 3 are visible.

[0024] As shown in FIG. 1A, element 2 can be divided along winding axis N of coil conductor 5 (parallel to the Z-axis) into axial end region 2a1, axial central region 2b, and axial end region 2a2 from the bottom.

[0025] In other words, the element 2 can be divided into an axial center region 2b in which the coil conductor 5 is embedded, and axial end regions 2a1, 2a2 located above and below the axial center region 2b in the axial direction (Z-axis direction) and in which the coil conductor 5 is not embedded. The axial direction of the coil conductor 5 is parallel to the lamination direction of the coil conductors 5.

[0026] Specifically, with respect to a virtual line perpendicular to the axial direction (Z-axis direction) and along the outer sides of the extraction electrodes 5a1, 5a2, the outer sides along the axis N are defined as axial end regions 2a1, 2a2, and the inner side is defined as axial central region 2b. In this embodiment, the axial central region 2b is a range that includes the extraction electrodes 5a1, 5a2.

[0027] In addition, the element 2 can be divided in a radial direction (Y-axis direction) perpendicular to the axial direction into an inner diameter region 4b of the coil conductor 5, a coil region 4a in which the coil conductor 5 is wound, and an outer diameter region 4c located radially outside the coil conductor 5.

[0028] In this embodiment, as described above, the element 2 is divided into axial end regions 2a1, 2a2 and axial central region 2b in the Z-axis direction, and into inner diameter region 4b, coil region 4a, and outer diameter region 4c in the radial direction.

[0029] In this embodiment, the region located in the shaft center region 2b and also located in the inner diameter region 4b is referred to as a shaft center inner diameter region 24bb. The region located in the shaft center region 2b and also located in the coil region 4a is referred to as a shaft center coil region 24ba. The region located in the shaft center region 2b and also located in the outer diameter region 4c is referred to as a shaft center outer diameter region 24bc.

[0030] In this embodiment, the region of the element 2 located in the middle between the coil conductors 5 adjacent in the axial direction in the axial center coil region 24ba is defined as the interlayer region 24ba1. The thickness (Ti) of the interlayer region 24ba1 in the Z-axis direction is not particularly limited and is, for example, 5 to 100 μm.

[0031] The magnetic element body 4 according to this embodiment is configured with a first magnetic element body 40 including first soft magnetic metal particles and a second magnetic element body 42 including second soft magnetic metal particles in a predetermined arrangement.

[0032] In this embodiment, the first magnetic body 40 is composed of an inter-layer first magnetic body 40a located in the axial center coil region 24ba, an inner diameter first magnetic body 40b located in the axial center inner diameter region 24bb, and an outer diameter first magnetic body 40c located in the axial center outer diameter region 24bc.

[0033] In addition, the second magnetic body 42 is composed of axial end second magnetic bodies 42a1, 42a2 located in the axial end regions 2a1, 2a2, an inner diameter second magnetic body 42b located in the axial center inner diameter region 24bb, and an outer diameter second magnetic body 42c located in the axial center outer diameter region 24bc.

[0034] Specifically, as shown in FIG. 1A, the interlayer region 24ba1 of the coil conductor 5 is composed of first interlayer magnetic bodies 40a including first soft magnetic metal particles.

[0035] The inner diameter first magnetic element 40b is formed continuously from the inter-layer first magnetic element 40a. The shape of the inner diameter first magnetic element 40b is not particularly limited, but is preferably substantially rectangular along the axial center region 2b. In this embodiment, the term "substantially rectangular" means that the outline of the rectangle may have some unevenness or inclination.

[0036] 1A, the outer first magnetic body 40c is formed continuously from the inter-layer first magnetic body 40a. The shape of the outer first magnetic body 40c is not particularly limited, but is preferably substantially rectangular along the axial center region 2b.

[0037] In this embodiment, the shaft end regions 2a1, 2a2 located on the outer side along the coil conductor 5 are constituted by shaft end second magnetic bodies 42a1, 42a2.

[0038] The second magnetic element 42 may constitute a region other than the axial end regions 2a1, 2a2. For example, as shown in FIG. 1A, an inner diameter second magnetic element 42b may be provided that is continuous with the axial end second magnetic elements 42a1, 42a2 and constitutes a part of the axial center inner diameter region 24bb of the coil conductor 5. In other words, the inner diameter second magnetic element 42b may constitute the inside of the inner diameter first magnetic element 40b in the axial center inner diameter region 24bb. It is preferable that the inner diameter second magnetic element 42b is substantially rectangular along the axial center region 2b.

[0039] Although the above description has been given along the YZ cross-sectional view shown in FIG. 1A, the structure is the same in any cross-section including the axis N of the coil conductor 5, for example, in a ZX cross-section.

[0040] FIG. 1A1 is a cross-sectional view taken along line IAI-IAI in FIG. 1. That is, FIG. 1A1 is a cross-sectional view perpendicular to the axial center N of the coil conductor 5 in the axial center region 2b. In the cross-section perpendicular to the axial center N of the coil conductor 5 in the axial center region 2b, the boundary between the axial center coil region 24ba and the axial center inner diameter region 24bb is indicated by a dashed line as the inner diameter boundary line R. In addition, the boundary between the axial center coil region 24ba and the axial center outer diameter region 24bc is indicated by a dashed line as the outer diameter boundary line S. Since the coil conductor 5 is layered to draw a spiral, as shown in FIG. 1A1, in the cross-section perpendicular to the axial direction, the coil conductor 5 is not arranged in part of the axial center coil region 24ba, and there is a portion where the interlayer second magnetic body 42a is arranged. That is, the portion where the interlayer second magnetic body 42a is arranged is the interlayer region 24ba1.

[0041] In this embodiment, in a cross section perpendicular to the axis N of the coil conductor 5 in the axial center region 2b, the ratio of the area of ​​the inner diameter second magnetic body 42b to the area of ​​the axial center inner diameter region 24bb (hereinafter referred to as the "inner diameter second magnetic body ratio") is preferably 30% or more, and more preferably 30 to 75%. In this embodiment, in a cross section perpendicular to the axis N of the coil conductor 5 in the axial center region 2b, the axial center inner diameter region 24bb is the region inside the inner diameter boundary line R.

[0042] In addition, in a cross section perpendicular to the axis N of the coil conductor 5 in the axial center region 2b, the ratio of the area of ​​the outer diameter second magnetic body 42c to the area of ​​the axial center outer diameter region 24bc (hereinafter referred to as the "outer diameter second magnetic body ratio") is preferably 15% or more, and more preferably 15 to 50%. In this embodiment, in a cross section perpendicular to the axis N of the coil conductor 5 in the axial center region 2b, the axial center outer diameter region 24bc is the region outside the outer diameter boundary line S.

[0043] In this embodiment, the first soft magnetic metal particles have a higher saturation magnetization (Ms) than the second soft magnetic metal particles. When the saturation magnetization of the first soft magnetic metal particles is "first Ms" and the saturation magnetization of the second soft magnetic metal particles is "second Ms", (first Ms / second Ms) is preferably 1.07 to 1.80, and more preferably 1.16 to 1.50. In the following, the "first soft magnetic metal particles" and the "second soft magnetic metal particles" may be collectively referred to as "soft magnetic metal particles".

[0044] The material of the first soft magnetic metal particles according to the present embodiment is not particularly limited, and may be, for example, an Fe-Si alloy, an Fe-Si-Cr alloy, pure Fe, an Fe-Ni alloy, or an Fe-Si-Al alloy, preferably an Fe-Si alloy, which can increase the saturation magnetization of the first soft magnetic metal particles.

[0045] When the total content of Fe and Si in the first soft magnetic metal particles is taken as 100 mass %, the Fe content in the first soft magnetic metal particles is preferably 92.0 to 97.0 mass %, and more preferably 92.5 to 96.5 mass %.

[0046] When the total content of Fe and Si in the first soft magnetic metal particles is taken as 100 mass%, the Cr content in the first soft magnetic metal particles is preferably 5 mass% or less, and more preferably less than 2 mass%, which leads to a better balance between inductance and DC bias characteristics, a higher evaluation of plating elongation suppression, and a smaller number of short circuits.

[0047] When the total content of Fe and Si in the first soft magnetic metal particles is taken as 100 mass %, the content of P in the first soft magnetic metal particles is preferably 10 to 700 ppm, and more preferably 40 to 650 ppm, which provides a better balance between inductance and DC bias characteristics, a higher evaluation of plating elongation suppression, and a smaller number of short circuits.

[0048] When the total content of Fe and Si in the first soft magnetic metal particles is taken as 100 mass%, the content of elements other than Fe, Si, Cr and P in the first soft magnetic metal particles is preferably less than 3 mass%. Elements other than Fe, Si, Cr and P in the first soft magnetic metal particles include Ni, O, Co, Al, etc.

[0049] The material of the second soft magnetic metal particles according to this embodiment is not particularly limited, and may be, for example, an Fe-Ni alloy, an Fe-Si-Cr alloy, or an Fe-Si-Al alloy, and is preferably an Fe-Ni alloy. This makes it easier to make the saturation magnetization of the first soft magnetic metal particles higher than that of the second soft magnetic metal particles, and therefore makes it possible to sufficiently increase the inductance and the DC bias characteristics.

[0050] When the total content of Fe, Ni, Si, Co, Cr and P in the second soft magnetic metal particles is 100 mass%, the Fe content in the second soft magnetic metal particles is preferably 33.0 to 68.0 mass%, and more preferably 37.0 to 55.0 mass%.

[0051] When the total content of Fe, Ni, Si, Co, Cr and P in the second soft magnetic metal particles is taken as 100 mass%, the Ni content in the second soft magnetic metal particles is preferably 14.0 to 56.0 mass%, and more preferably 15.0 to 55.0 mass%, which provides a better balance between inductance and DC bias characteristics, a higher evaluation of plating elongation suppression, and a smaller number of short circuits.

[0052] When the total content of Fe, Ni, Si, Co, Cr and P in the second soft magnetic metal particles is taken as 100 mass%, the content of Si in the second soft magnetic metal particles is preferably 2.0 to 6.0 mass%, which provides a better balance between inductance and DC bias characteristics, a higher evaluation of plating elongation suppression, and a smaller number of short circuits.

[0053] When the total content of Fe, Ni, Si, Co, Cr and P in the second soft magnetic metal particles is taken as 100 mass%, the Co content in the second soft magnetic metal particles is preferably 2.0 to 40.0 mass%, which provides a better balance between inductance and DC bias characteristics, a higher evaluation of plating elongation suppression, and a smaller number of short circuits.

[0054] When the total content of Fe, Ni, Si, Co, Cr and P in the second soft magnetic metal particles is taken as 100 mass %, the Cr content in the second soft magnetic metal particles is preferably 1.8 mass % or less, which provides a better balance between inductance and DC bias characteristics.

[0055] When the total content of Fe, Ni, Si, Co, Cr and P in the second soft magnetic metal particles is taken as 100 mass %, the content of P in the second soft magnetic metal particles is preferably 10 to 6000 ppm, and more preferably 100 to 5000 ppm, which provides a better balance between inductance and DC bias characteristics, a higher evaluation of plating elongation suppression, and a smaller number of short circuits.

[0056] When the total content of Fe, Ni, Si, Co, Cr and P in the second soft magnetic metal particles is taken as 100 mass%, the content of elements other than Fe, Ni, Si, Co, Cr and P in the second soft magnetic metal particles is preferably less than 3 mass%. Note that elements other than Fe, Ni, Si, Co, Cr and P in the second soft magnetic metal particles include, for example, Al or O.

[0057] The first soft magnetic metal particles according to this embodiment preferably have an average particle size of 1 to 6 μm. When the first soft magnetic metal particles have an average particle size of 1 to 6 μm, the inductance can be increased compared to when the first soft magnetic metal particles have an average particle size of less than 1 μm. When the first soft magnetic metal particles have an average particle size of 1 to 6 μm, the inductance can be increased, plating elongation can be suppressed, and the number of short circuits can be reduced compared to when the first soft magnetic metal particles have an average particle size of more than 6 μm.

[0058] The second soft magnetic metal particles according to this embodiment preferably have an average particle size of 1 to 15 μm. When the average particle size of the second soft magnetic metal particles is 1 to 15 μm, the inductance can be increased compared to when the average particle size of the second soft magnetic metal particles is less than 1 μm. When the average particle size of the second soft magnetic metal particles is 1 to 15 μm, the DC bias characteristics can be improved, plating elongation can be suppressed, and the number of short circuits can be reduced compared to when the average particle size of the second soft magnetic metal particles exceeds 15 μm.

[0059] The average particle size of the first soft magnetic metal particles is preferably equal to or smaller than the average particle size of the second soft magnetic metal particles. When the average particle size of the first soft magnetic metal particles is the "first average particle size" and the average particle size of the second soft magnetic metal particles is the "second average particle size", (first average particle size / second average particle size) is preferably 0.2 to 1.0, and more preferably 0.2 to 0.5.

[0060] The method for measuring the average particle size of the soft magnetic metal particles is not particularly limited, but in this embodiment, the area of ​​the soft magnetic metal particles is calculated by performing image analysis on the cross section of the resin-embedded laminated coil 1 (electronic component) using an SEM, STEM, etc., and the value (area diameter) calculated as the diameter of a circle equivalent to that area (circle equivalent diameter) is taken as the particle size of the soft magnetic metal particle, and the average value of the particle sizes of multiple soft magnetic metal particles is taken as the average particle size.

[0061] The shape of the soft magnetic metal particles is not particularly limited.

[0062] The magnetic base body 4 according to this embodiment has a configuration in which multiple soft magnetic metal particles are connected to each other by sintering. Specifically, elements contained in the soft magnetic metal particles that are in contact with each other react with other elements (e.g., O) by sintering, and the multiple soft magnetic metal particles are connected to each other through bonds resulting from the reaction. In the magnetic base body 4 according to this embodiment, the soft magnetic metal particles derived from the soft magnetic metal powder, which is the raw material powder of the soft magnetic metal particles, are connected to each other by heat treatment, but the soft magnetic metal particles hardly undergo grain growth.

[0063] Furthermore, the content of the first soft magnetic metal particles in the first magnetic body 40 is preferably 90% by mass or more, and more preferably 95% by mass or more. As long as the content of the first soft magnetic metal particles in the first magnetic body 40 is the above amount or more, the first magnetic body 40 does not have to be composed entirely of first soft magnetic metal particles. For example, the first magnetic body 40 may contain a small number of metal particles having a saturation magnetization equal to or less than that of the second soft magnetic metal particles.

[0064] The content of the second soft magnetic metal particles in the second magnetic body 42 is preferably 90% by mass or more, and more preferably 95% by mass or more. If the content of the second soft magnetic metal particles in the second magnetic body 42 is the above amount or more, the second magnetic body 42 does not have to be composed entirely of second soft magnetic metal particles, and may, for example, contain a small number of metal particles with saturation magnetization equal to or greater than that of the first soft magnetic metal particles.

[0065] The soft magnetic metal particles may be covered with a coating film. Specifically, the coating film may be an oxide film, and the oxide film may include a layer made of an oxide containing Si. By covering the soft magnetic metal particles with a coating film, the insulation between the soft magnetic metal particles is improved, thereby improving the Q value. In addition, by including a layer made of a compound containing Si in the oxide film, it is also possible to prevent the formation of oxides of Fe.

[0066] The method for determining the regions of the first magnetic body 40 and the second magnetic body 42 of the element 2 according to this embodiment is not particularly limited, and may be determined by performing component analysis by obtaining element mapping by EDS, for example.

[0067] In addition, because the first magnetic body 40 and the second magnetic body 42 have different compositions, the regions of the first magnetic body 40 and the second magnetic body 42 can be identified by contrast by performing image analysis of a cross section of element 2 using SEM, STEM, etc. Furthermore, if the average grain size of the first soft magnetic metal particles and the average grain size of the second soft magnetic metal particles are different, it is easy to identify the regions of the first magnetic body 40 and the second magnetic body 42 by contrast by performing image analysis of a cross section of element 2 using SEM, STEM, etc.

[0068] In this embodiment, the raw material of the first soft magnetic metal particles is sometimes referred to as the "first soft magnetic metal powder", the raw material of the second soft magnetic metal particles is sometimes referred to as the "second soft magnetic metal powder", and the raw material of the soft magnetic metal particles is sometimes referred to as the "soft magnetic metal powder". In other words, the raw material of the first soft magnetic metal particles and the raw material of the second soft magnetic metal particles are sometimes collectively referred to as the "soft magnetic metal powder".

[0069] An example of a method for producing the first soft magnetic metal powder and the second soft magnetic metal powder according to this embodiment will be described below.

[0070] In this embodiment, as the raw material of the first soft magnetic metal powder, a simple substance or an alloy of a constituent element can be used, and for example, simple substance Fe, simple substance Si, simple substance Cr, etc. can be used.

[0071] As the raw material for the second soft magnetic metal powder, an alloy or a simple substance of the constituent elements can be used, for example, an Fe-Ni alloy, simple Fe, simple Ni, simple Si, simple Co, simple Cr, etc.

[0072] In this embodiment, the soft magnetic metal powder can be obtained using a method similar to the known method for producing soft magnetic metal powder. Specifically, the soft magnetic metal powder can be produced using a gas atomization method, a water atomization method, a rotating disk method, etc. Among these, the water atomization method is preferably used from the viewpoint that it is easy to obtain a soft magnetic metal powder having the desired magnetic properties.

[0073] In the water atomization method, raw materials in the form of ingots, chunks, or shots are prepared, and these raw materials are mixed to obtain a desired composition and placed in a crucible disposed in a water atomization apparatus.

[0074] Next, in an inert atmosphere, the crucible is heated to 1600°C or higher by high-frequency induction using a work coil provided outside the crucible, and the ingots, chunks, or shots in the crucible are melted and mixed to obtain a molten metal.

[0075] The molten raw material (molten metal) is supplied as a continuous linear fluid through a nozzle installed at the bottom of the crucible, and high-pressure (approximately 50 MPa) water is sprayed onto the supplied molten metal to turn the molten metal into droplets, which are then rapidly cooled, dehydrated, dried, and classified to obtain soft magnetic metal powder with the desired average particle size.

[0076] In this embodiment, for example, each raw material is melted, P is added to the melt, and the melt is pulverized by a water atomization method, thereby manufacturing the soft magnetic metal powder according to this embodiment. In addition, when P is contained as an impurity in the raw material, for example, in the Fe raw material, the total content of P as an impurity and the amount of P to be added may be adjusted to manufacture a soft magnetic metal powder containing a desired amount of P. Alternatively, a plurality of Fe raw materials with different P contents may be used, and the melt in which the P content has been adjusted may be pulverized by a water atomization method.

[0077] In this embodiment, the first soft magnetic metal powder, which is the raw material powder of the first soft magnetic metal particles, and the second soft magnetic metal powder, which is the raw material powder of the second soft magnetic metal particles, are each prepared by the above-mentioned method.

[0078] Next, a method for manufacturing the laminate coil 1 shown in Fig. 1, Fig. 1A, and Fig. 1A1 will be described. First, the obtained first soft magnetic metal powder is slurried together with additives such as a solvent and a binder to prepare a first paste. Similarly, the obtained second soft magnetic metal powder is slurried together with additives such as a solvent and a binder to prepare a second paste.

[0079] Then, the second paste is used to form second shaft-end green sheets which, after firing, will become the shaft-end second magnetic bodies 42a1 that constitute the shaft-end region 2a1.

[0080] Next, a conductor 50a1, a first green sheet 400a made of the first paste, and a second green sheet 420a made of the second paste are printed on the shaft end second green sheet to form a print body 100a shown in FIG. 2a.

[0081] Conductor 50a1 and conductor 50a2, described later, are conductors such as silver (Ag) that become lead electrodes 5a1, 5a2 of coil conductor 5 after firing. First green sheet 400a and first green sheets 400b-400h, described later, become first magnetic body 40 after firing. Second green sheet 420a and second green sheets 420b-420h, described later, become second magnetic body 42 after firing. Therefore, at the stage of the process shown in FIG. 2a, second green sheet 420a is formed so as to have a desired inner diameter second magnetic body ratio after firing.

[0082] Next, the conductor 50b, the first green sheet 400b made of the first paste, and the second green sheet 420b made of the second paste are printed on the printed body 100a shown in Fig. 2a to form the printed body 100b shown in Fig. 2b. That is, in the printed body shown in Fig. 2b, the conductor 50b is printed so as to be connected to the conductor 50a1, and the second green sheet 420b is printed so as to overlap the second green sheet 420a shown in Fig. 2a.

[0083] The conductor 50b and conductors 50c to 50g, which will be described later, are made of conductors such as silver (Ag) that become the coil conductor 5 after firing.

[0084] Next, the conductor 50c, the first green sheet 400c made of the first paste, and the second green sheet 420c made of the second paste are printed on the printed body 100b shown in Fig. 2b so as to form the printed body 100c shown in Fig. 2c. That is, the conductor 50c is printed so that a part of it (the conductor 50c1) can be connected to a part of the conductor 50b (50b1), and the second green sheet 420c is printed so as to overlap the second green sheet 420b shown in Fig. 2b.

[0085] Next, conductor 50d, a first green sheet 400d made of the first paste, and a second green sheet 420d made of the second paste are printed on printed body 100c shown in Fig. 2c to form printed body 100d shown in Fig. 2d. That is, conductor 50d is printed so that a part of it (conductor 50d1) can be connected to a part of conductor 50c (50c2), and second green sheet 420d is printed so as to overlap second green sheet 420c shown in Fig. 2c.

[0086] Next, the conductor 50e, the first green sheet 400e made of the first paste, and the second green sheet 420e made of the second paste are printed on the printed body 100d shown in Fig. 2d so as to form the printed body 100e shown in Fig. 2e. That is, the conductor 50e is printed so as to be connected to the conductor 50d, and the second green sheet 420e is printed so as to overlap the second green sheet 420d shown in Fig. 2d.

[0087] Next, conductor 50f, a first green sheet 400f made of the first paste, and a second green sheet 420f made of the second paste are printed on printed body 100e shown in Fig. 2e so as to form printed body 100f shown in Fig. 2f. That is, conductor 50f is printed so that a part of it (conductor 50f1) can be connected to a part of conductor 50e (50e1), and second green sheet 420f is printed so as to overlap second green sheet 420e shown in Fig. 2e.

[0088] Thereafter, after repeating the printing shown in Figures 2d to 2f, conductor 50g, a first green sheet 400g made of the first paste, and a second green sheet 420g made of the second paste are printed on printed body 100f shown in Figure 2f to form printed body 100g shown in Figure 2g. That is, conductor 50g is printed so that a part of it (conductor 50g1) can be connected to a part of conductor 50f (50f2), and second green sheet 420g is printed so as to overlap second green sheet 420f shown in Figure 2f.

[0089] Next, the conductor 50a2, the first green sheet 400h made of the first paste, and the second green sheet 420h made of the second paste are printed on the printed body 100g shown in Fig. 2g so as to form the printed body 100h shown in Fig. 2h. That is, the conductor 50a2 is printed so as to be connected to the conductor 50g, and the second green sheet 420h is printed so as to overlap the second green sheet 420g shown in Fig. 2g.

[0090] In addition, in Figs. 2a to 2h, the printing order when printing the conductor, the first green sheet, and the second green sheet on the same plane is not particularly limited.

[0091] Furthermore, a second paste is used on the printed body 100h shown in FIG. 2h to form a second shaft-end green sheet which will become the shaft-end second magnetic body 42a2 that constitutes the shaft-end region 2a2 after firing.

[0092] In the laminate thus obtained, first, the conductor 50a1 of the printed body 100a shown in FIG. 2a and the conductor 50b of the printed body 100b shown in FIG. 2b are in contact with each other widely and are electrically connected.

[0093] Furthermore, conductor 50b1 of conductor 50b of printed body 100b shown in Figure 2b and conductor 50c1 of conductor 50c of printed body 100c shown in Figure 2c are both in the range between imaginary lines J and K, and are in contact with each other, so are conductive.

[0094] Furthermore, conductor 50c2 of conductor 50c of printed body 100c shown in Figure 2c and conductor 50d1 of conductor 50d of printed body 100d shown in Figure 2d are both in the range between imaginary lines L and M, and are in contact and therefore conductive.

[0095] Furthermore, the conductors 50d of the printed body 100d shown in FIG. 2d and the conductors 50e of the printed body 100e shown in FIG. 2e are in wide contact with each other and are electrically connected.

[0096] Furthermore, 50e1 of conductor 50e of printed body 100e shown in FIG. 2e and 50f1 of conductor 50f of printed body 100f shown in FIG. 2f are both within the range between imaginary lines J and K, and therefore are conductive.

[0097] Furthermore, conductor 50f2 of conductor 50f of printed body 100f shown in Figure 2f and conductor 50g1 of conductor 50g of printed body 100g shown in Figure 2g are both in the range between imaginary lines L and M, and are in contact and therefore conductive.

[0098] Furthermore, the conductor 50g of the printed body 100g shown in FIG. 2g and the conductor 50a2 of the printed body 100h shown in FIG. 2h are in wide contact with each other and are electrically connected.

[0099] Here, the presence of the printed body 100d shown in Fig. 2d makes it possible to prevent contact between 50c1 of the printed body 100c shown in Fig. 2c and 50e1 of the printed body 100e shown in Fig. 2e, thereby preventing a short circuit and obtaining a green laminate in which the coil conductor 5 is formed three-dimensionally and spirally.

[0100] Although the lead electrode 5a1 in Fig. 2a and the lead electrode 5a2 in Fig. 2h are drawn with the same thickness (Te) as the coil conductor 5 other than the lead electrodes 5a1, 5a2, the thickness of the lead electrodes 5a1, 5a2 may be thinner than the thickness (Te) of the coil conductor 5 other than the lead electrodes 5a1, 5a2. By making the thickness of the lead electrodes 5a1, 5a2 thinner than the thickness of the coil conductor 5 other than the lead electrodes 5a1, 5a2, the number of coil turns per unit volume can be increased, and the inductance can be increased.

[0101] For example, after the printing shown in Fig. 2a is repeated 1-2 times, the printing shown in Fig. 2b may be repeated 3-8 times, the printings shown in Fig. 2c-2f may be repeated about 10 times each, and further the printing shown in Fig. 2g may be repeated 3-8 times, followed by the printing shown in Fig. 2h 1-2 times. In this way, the thickness of the lead electrodes 5a1, 5a2 can be made thinner than the thickness of the coil conductor 5 other than the lead electrodes 5a1, 5a2.

[0102] Although the method for producing a laminate by printing has been described above, a laminate having the above structure can also be obtained by a sheet method.

[0103] The obtained laminate is subjected to heat treatment (binder removal step and sintering step) to remove the binder, and a sintered body (element) is obtained in which the soft magnetic metal particles contained in the soft magnetic metal powder are connected and fixed (integrated) to each other. The holding temperature in the binder removal step (binder removal temperature) is not particularly limited as long as it is a temperature at which the binder can be decomposed and removed as a gas. For example, it may be 300°C or higher and 450°C or lower. Furthermore, the holding time in the binder removal step (binder removal time) is also not particularly limited. For example, it may be 0.5 hours or higher and 2.0 hours or lower.

[0104] The holding temperature (sintering temperature) in the sintering step is not particularly limited as long as it is a temperature at which the soft magnetic metal particles constituting the soft magnetic metal powder are connected to each other. It may be 550°C or higher and 850°C or lower. In addition, the holding time (sintering time) in the sintering step is also not particularly limited. It may be 0.5 hours or higher and 3.0 hours or lower.

[0105] In this embodiment, it is preferable to adjust the atmosphere during binder removal and firing.

[0106] After firing, an annealing treatment (heat treatment) may be performed. There are no particular limitations on the conditions for the annealing treatment. For example, the annealing treatment may be performed at 500 to 800° C. for 0.5 to 2.0 hours. There are also no particular limitations on the atmosphere after annealing.

[0107] Next, the terminal electrodes 3 are formed on the element. There are no particular limitations on the method for forming the terminal electrodes 3, and they are usually prepared by forming a slurry of a metal (such as Ag) that will become the terminal electrodes 3 together with additives such as a solvent and a binder.

[0108] The laminated coil 1 according to this embodiment is obtained by the above method.

[0109] In the laminated coil 1 according to this embodiment, the interlayer magnetic element 40a located in the interlayer region 24ba1 of the coil conductor 5 contains first soft magnetic metal particles, and the axial end magnetic elements 42a1, 42a2 located on the outside along the axial center N of the coil conductor 5 contain second soft magnetic metal particles, the first soft magnetic metal particles having higher saturation magnetization than the second soft magnetic metal particles. With this configuration, the laminated coil 1 (coil-type electronic component) according to this embodiment has sufficiently high inductance and DC superposition characteristics.

[0110] Second embodiment The second embodiment will be described below, but unless otherwise specified, it is the same as the first embodiment.

[0111] 3, the laminated coil 1 according to this embodiment has a configuration in which the coil conductor 5 is embedded three-dimensionally in a double helix shape. Although the coil conductor 5 has a double helix shape, the coil conductor 5 has a continuous structure extending from one extraction electrode 5a1 to the other extraction electrode 5a2.

[0112] Specifically, in the cross section shown in Figure 3, the first layer extraction electrode 5a1, second layer outer coil conductors 501, 502, second layer inner coil conductors 503, 504, third layer inner coil conductors 505, 506, seventh layer inner coil conductors 521, 522, seventh layer outer coil conductors 523, 524, eighth layer outer coil conductors 525, 526, eighth layer inner coil conductors 527, 528, and ninth layer extraction electrode 5a2 are connected in this order in a spiral structure.

[0113] By forming the coil conductor 5 in a double helix shape, the coil becomes denser, and the inductance can be increased.

[0114] In addition, although the coil conductor 5 in FIG. 3 has a double spiral shape with two turns per layer, the coil conductor 5 may have three or more turns per layer.

[0115] The method for manufacturing the laminated coil 1 according to the present embodiment is not particularly limited. For example, the laminated coil 1 according to the present embodiment can be obtained by changing the arrangement of the conductor, the first green sheet, and the second green sheet in the above Figures 2a to 2h so that the coil conductor 5 is three-dimensional and double-spiral, thereby obtaining a green laminate.

[0116] Third embodiment The third embodiment will be described below, but unless otherwise specified, it is the same as the first embodiment.

[0117] As shown in Fig. 4, in the laminated coil 1 according to this embodiment, the axial direction of the coil conductor 5 is parallel to the Y-axis direction. Fig. 4A is a schematic cross-sectional view taken along line IVA-IVA in Fig. 4. In this embodiment, as shown in Fig. 4A, the laminated coil 1 is divided into an axial end region 2a and an axial central region 2b along the Y-axis direction. Also, the laminated coil 1 is divided into a coil region 4a, an inner diameter region 4b, and an outer diameter region 4c along the Z-axis direction.

[0118] In the third embodiment, the outer side is the axial end regions 2a1, 2a2, and the inner side is the axial central region 2b, with respect to a virtual line along the outside of the outermost coil conductor 5. That is, in the third embodiment, the axial central region 2b is a range that does not include the extraction electrodes 5a1, 5a2.

[0119] (Fourth embodiment) The fourth embodiment will be described below, but unless otherwise specified, it is the same as the first embodiment.

[0120] The magnetic body according to this embodiment is made of soft magnetic metal particles and resin.

[0121] In the elements obtained by the methods described in the first to third embodiments, gap spaces exist in the magnetic body except for the soft magnetic metal particles. In this embodiment, the gap spaces are filled with resin, for example, by impregnating the element with resin.

[0122] By filling the gaps with resin, the strength (especially the flexural strength) of the laminated coil is increased. In addition, the insulation between the soft magnetic metal particles is further improved, which makes it easier to improve the inductance and Q value. Furthermore, the reliability and heat resistance are improved. Furthermore, the laminated coil is less likely to short out.

[0123] There are no particular limitations on the method of impregnating the resin. For example, a method using vacuum impregnation can be used. Vacuum impregnation is performed by immersing the elements of the laminated coil in resin and controlling the air pressure. The resin penetrates into the magnetic body by lowering the air pressure. That is, since there are gap spaces in the magnetic body, the resin can penetrate into the magnetic body through the gap spaces by the principle of capillary action, especially into the interlayer regions where it is most difficult for resin to penetrate. After the magnetic body is impregnated with the resin, the resin is hardened by heating. The heating conditions vary depending on the type of resin.

[0124] The type of resin is not particularly limited. For example, when phenolic resin or epoxy resin is used, the resin penetrates sufficiently into the gap spaces inside the magnetic body (particularly the interlayer regions) and is likely to fill the gap spaces sufficiently even after curing. Furthermore, it is not easily decomposed even when heated, so it has high heat resistance. In particular, when phenolic resin or epoxy resin is used, the resin easily penetrates sufficiently into the gap spaces inside the magnetic body (particularly the interlayer regions) compared to when silicone resin is used. It is preferable that the resin is phenolic resin, since it is inexpensive and easy to handle.

[0125] The resin content in the magnetic body of the final laminate coil is preferably 0.5% by mass or more and 3.0% by mass or less. The resin content can be controlled by changing the resin solution concentration during impregnation, the immersion time, the number of immersions, etc.

[0126] In this embodiment, electrolytic plating can be performed on the terminal electrodes after filling with resin. Since the resin fills the gaps, even if the magnetic body is immersed in a plating solution, the plating solution does not easily penetrate into the magnetic body. Therefore, even after plating, short circuits do not occur in the laminated coil, and inductance is maintained high.

[0127] Although the embodiment of the present invention has been described above, the present invention is not limited to the above embodiment, and may be modified in various aspects within the scope of the present invention.

[0128] For example, as shown in Fig. 1B, the first magnetic body 40 does not have to include the inner diameter first magnetic body 40b shown in Fig. 1A. In other words, the inner diameter second magnetic body 42b may constitute the entire axial center inner diameter region 24bb.

[0129] For example, as shown in FIG. 1C, an outer second magnetic body 42c may be provided along the axial center region 2b on the outside of an outer first magnetic body 40c.

[0130] For example, as shown in Fig. 1D, the first magnetic body 40 does not have to include the inner first magnetic body 40b and the outer first magnetic body 40c shown in Fig. 1A. In other words, the entire axial center inner diameter region 24bb may be made up of the inner second magnetic body 42b, and the entire axial center outer diameter region 24bc may be made up of the outer second magnetic body 42c.

[0131] For example, as shown in Fig. 1E, the entire shaft center inner diameter region 24bb may be made up of the inner diameter first magnetic body 40b, and the entire shaft center outer diameter region 24bc may be made up of the outer diameter first magnetic body 40c. In other words, the second magnetic body 42 does not have to include the inner diameter second magnetic body 42b and the outer diameter second magnetic body 42c shown in Fig. 1A.

[0132] The method of changing the arrangement of the first magnetic base body 40 and the second magnetic base body 42 as shown in Figures 1B to 1E is not particularly limited, but one example is a method of changing the arrangement of the first green sheet and the second green sheet in the printed bodies 100a to 100h shown in Figures 2a to 2h above so as to achieve the desired arrangement of the first magnetic base body 40 and the second magnetic base body 42.

[0133] In the above, the inner diameter second magnetic body ratio and the outer diameter second magnetic body ratio were calculated based on a cross section perpendicular to the axial direction of the coil conductor 5, but it is also possible to obtain multiple cross sections parallel to the axial direction of the coil conductor 5 and calculate the inner diameter second magnetic body ratio and the outer diameter second magnetic body ratio from these.

[0134] In this embodiment, a laminated coil is illustrated as an example of a coil-type electronic component, but other known coil-type electronic components include transformers, choke coils, coils, etc. The coil-type electronic component according to this embodiment is suitable for use as an inductor, impedance, etc. in the power supply circuits of various electronic devices such as portable devices. EXAMPLES

[0135] The present invention will be described in more detail below using examples, but the present invention is not limited to these examples.

[0136] (Samples in Tables 1 to 3) Each raw material was prepared so as to obtain each soft magnetic metal powder having the composition shown in Table 1 or Table 2. In Table 1, [mass %] and [ppm] refer to the content of each component when the total content of Fe and Si is taken as 100 mass %. In Table 2, [mass %] and [ppm] refer to the content of each component when the total content of Fe, Ni, Si, Co, Cr and P is taken as 100 mass %.

[0137] The composition of each of the obtained soft magnetic metal powders was analyzed by ICP analysis, and it was confirmed that each of the obtained soft magnetic metal powders had the composition shown in Table 1 or Table 2. Therefore, in the examples and comparative examples described later, it was presumed that the composition of the raw materials charged was the same as the composition of each of the obtained soft magnetic metal powders.

[0138] The saturation magnetization of each of the obtained soft magnetic metal powders was measured in an external magnetic field of 795.8 kA / m (10 kOe) using a vibrating sample magnetometer (VSM-3S-15 manufactured by Toei Industry Co., Ltd.). The results are shown in Tables 1 and 2.

[0139] A first paste was prepared using the obtained first soft magnetic metal powder, and a second paste was prepared using the obtained second soft magnetic metal powder.

[0140] As shown in FIG. 1E, the arrangement of the first and second green sheets was changed in the printed bodies 100a-100h shown in FIG. 2a-2h so that the second magnetic body 42 constitutes the shaft end regions 2a1, 2a2, and the first magnetic body 40 constitutes the interlayer region 24ba1, the shaft center inner diameter region 24bb, and the shaft center outer diameter region 24bc, to obtain a green laminate having a thickness of 0.8 mm. The conductor was an Ag conductor, and the number of turns was 7.5Ts. The obtained green laminate was then cut into a shape of 1.6 mm×0.8 mm to obtain a green laminated coil.

[0141] Next, the obtained green laminated coil was subjected to a binder removal process in an inert atmosphere (N2 gas atmosphere) at 400°C. After that, it was fired in a reducing atmosphere (mixed gas atmosphere of N2 gas and H2 gas (hydrogen concentration 1.0%) at 750°C for 1 hour to obtain a fired body.

[0142] A terminal electrode paste was applied to both end faces of the obtained sintered body, dried, and baked at 700° C. for 1 hour in an atmosphere with an oxygen partial pressure of 1%, forming terminal electrodes 3 and obtaining a sintered laminated coil product.

[0143] Each of the resulting laminated coil baked products was impregnated with resin. Specifically, the laminated coil baked products were vacuum-impregnated with a raw material mixture of phenol resin, and then heated to harden the resin at 150°C for 2 hours, filling the laminated coil baked products with resin. Note that the solvent contained in the raw material mixture evaporated when the resin was hardened. After that, electrolytic plating was performed to form Ni plating layers and Sn plating layers on the terminal electrodes, and the laminated coil 1 was obtained.

[0144] The internal dimensions of the obtained laminated coil were a thickness (Te) of the coil conductor 5 of 40 μm and a thickness (T1) of the interlayer region 24ba1 of 15 μm.

[0145] The obtained laminate coil was subjected to component analysis, and measurements of average grain size, saturation magnetization, inductance, and DC bias characteristics were performed as described below.

[0146] <Component analysis> For the laminated coil of Example 1, elemental mapping photographs of the axial end regions 2a1, 2a2, the axial center inner diameter region 24bb, the interlayer region 24ba1, and the axial center outer diameter region 24bc were obtained, and component analysis was performed. As a result, it was confirmed that the first soft magnetic metal particles having the same composition as the first soft magnetic metal powder were formed in the area where the first soft magnetic metal powder was used, and the second soft magnetic metal particles having the same composition as the second soft magnetic metal powder were formed in the area where the second soft magnetic metal powder was used. Therefore, in the examples and comparative examples described later, it was estimated that the first soft magnetic metal particles having the same composition as the first soft magnetic metal powder were formed in the area where the first soft magnetic metal powder was used, and the second soft magnetic metal particles having the same composition as the second soft magnetic metal powder were formed in the area where the second soft magnetic metal powder was used.

[0147] <Average particle size> The cross section of the laminate coil of Example 1 was image-analyzed by SEM to determine the circle-equivalent diameters of the first soft magnetic metal particles and the second soft magnetic metal particles, and the circle-equivalent diameters were used as particle sizes. The particle sizes of 400 particles of each of the first soft magnetic metal particles and the second soft magnetic metal particles were determined, and the average particle size of the first soft magnetic metal particles and the average particle size of the second soft magnetic metal particles were determined. The average particle size of the first soft magnetic metal particles is shown in Table 1, and the average particle size of the second soft magnetic metal particles is shown in Table 2.

[0148] <Saturation magnetization (Ms)> The first magnetic element and the second magnetic element of the laminate coil of Example 1 were cut out by micromachining using laser processing, and the saturation magnetization of the first soft magnetic metal particles and the second soft magnetic metal particles was measured in an external magnetic field of 795.8 kA / m (10 kOe) using a vibration sample magnetometer (VSM-3S-15 manufactured by Toei Industry Co., Ltd.). As a result, it was confirmed that the saturation magnetization of the first soft magnetic metal particles was the same as that of the first soft magnetic metal powder, and the saturation magnetization of the second soft magnetic metal particles was the same as that of the second soft magnetic metal powder. Therefore, in the examples and comparative examples described later, it was estimated that the saturation magnetization of the first soft magnetic metal particles was the same as that of the first soft magnetic metal powder, and the saturation magnetization of the second soft magnetic metal particles was the same as that of the second soft magnetic metal powder.

[0149] <Inductance (L) measurement> The inductance (L) of the obtained laminated coils was measured using an LCR meter (HEWLETT PACKARD: 4285A) at f=2MHz and I=0.1A. The average value of L was calculated for 30 laminated coils of each type. The results are shown in Table 3. ΔL / L was calculated as the rate of change of L for the "subject for comparison of ΔL / L and ΔIdc / Idc" shown in Table 3 relative to the average value. For example, since the "subject for comparison of ΔL / L and ΔIdc / Idc" in Example 1 is "Comparative Example 1," ΔL / L was calculated using the following formula (1). ΔL / L of Example 1=100×{(L of Example 1−L of Comparative Example 1) / L of Comparative Example 1} (1)

[0150] <DC superimposition characteristic Idc> The inductance of the obtained laminated coil was measured when a direct current was applied. The inductance was measured while changing the applied direct current from 0 to 3 A, and the results were graphed with the direct current on the horizontal axis and the inductance on the vertical axis. The current value at which the inductance decreased by 30% from when the direct current was 0 A was determined as Idc. The average value of Idc for 30 laminated coils was determined. The results are shown in Table 3. In addition, ΔIdc / Idc was determined as the rate of change relative to the average value of Idc for comparison. For example, since the "comparison of ΔL / L and ΔIdc / Idc" for Example 1 is "Comparative Example 1," ΔIdc / Idc was determined by the following formula (2). ΔIdc / Idc of Example 1=100×{(Idc of Example 1−Idc of Comparative Example 1) / Idc of Comparative Example 1} (2)

[0151] <Verdict> When ΔL / L was -30% or more and ΔIdc / Idc was 50% or more, it was judged as passing and was recorded as "OK" in Table 3. When ΔL / L or ΔIdc / Idc was outside the above range, it was recorded as "NG" in Table 3.

[0152] [Table 1]

[0153] [Table 2]

[0154] [Table 3]

[0155] From Tables 1 to 3, it can be seen that when the interlayer region is composed of a first magnetic body, the shaft end region is composed of a second magnetic body, and the saturation magnetization of the first soft magnetic metal particles is higher than the saturation magnetization of the second soft magnetic metal particles (Example 1, Example 1a, Example 2, Example 3, Example 3a, Example 3b, Example 3c, Example 3d), the result is OK, confirming that the inductance and DC superposition characteristics are sufficiently high.

[0156] In Comparative Examples 1, 2, 3, 3b, and 3d, the first soft magnetic metal particles and the second soft magnetic metal particles had the same composition and had the structure shown in FIG. 5A.

[0157] In addition, in Comparative Example 1a, the first soft magnetic metal particles had a lower saturation magnetization than the second soft magnetic metal particles, and therefore the structure shown in FIG. 5B was obtained.

[0158] (Samples in Tables 4 to 6) For each sample in Tables 4 to 6, the composition of each soft magnetic metal powder was changed to the composition shown in Table 4 or Table 5, and the inner diameter second magnetic body ratio and the outer diameter second magnetic body ratio were changed as shown in Table 6. Except for this, laminated coils were obtained in the same manner as for each sample in Tables 1 to 3, and the average particle size of the soft magnetic metal particles was measured, and L and Idc were measured to obtain (ΔL / L) and (ΔIdc / Idc). The average particle size of the first soft magnetic metal particles is shown in Table 4, and the average particle size of the second soft magnetic metal particles is shown in Table 5. The results of L, Idc, (ΔL / L) and (ΔIdc / Idc) are shown in Table 6.

[0159] In addition, for each sample in Tables 4 to 6, "(ΔL / L)+(ΔIdc / Idc)" was calculated as a measure of the balance between "inductance L" and "DC bias characteristic Idc." The results are shown in Table 6.

[0160] [Table 4]

[0161] [Table 5]

[0162] [Table 6]

[0163] FIG. 6 is a graph in which the X-axis represents the inner diameter portion second magnetic body ratio (%) and the Y-axis represents (ΔL / L)+(ΔIdc / Idc) (%) for Example 5a and Examples 4 to 7.

[0164] From Table 6 and FIG. 6, it was confirmed that when the ratio of the second magnetic body to the inner diameter is 30% or more, (ΔL / L)+(ΔIdc / Idc) is high and the balance between the inductance and the DC bias characteristics is better.

[0165] From Table 6, it was confirmed that when the proportion of the second magnetic body in the outer diameter is 15% or more, a better balance between the inductance and the DC bias characteristics is achieved.

[0166] In addition, in Comparative Example 4, the first soft magnetic metal particles had a lower saturation magnetization than the second soft magnetic metal particles, and therefore the structure shown in FIG. 5C was obtained.

[0167] (Samples in Tables 7 to 9) In each sample in Tables 7 to 9, the composition of each soft magnetic metal powder was changed to the composition shown in Table 7 or Table 8. In addition, the arrangement of the conductor, the first green sheet, and the second green sheet was changed in FIG. 2a to FIG. 2h so that the coil conductor 5 was three-dimensional and double-spiral as shown in FIG. 3 to obtain a green laminate. Furthermore, the ratio of the second magnetic element body to the inner diameter and the ratio of the second magnetic element body to the outer diameter were changed as shown in Table 9. A laminate coil was obtained in the same manner as each sample in Tables 1 to 3 except for the above, and the average particle size of the soft magnetic metal particles was measured, and L and Idc were measured to obtain "ΔL / L" and "ΔIdc / Idc". The average particle size of the first soft magnetic metal particles is shown in Table 7, and the average particle size of the second soft magnetic metal particles is shown in Table 8. The results of L, Idc, (ΔL / L) and (ΔIdc / Idc) are shown in Table 9.

[0168] [Table 7]

[0169] [Table 8]

[0170] [Table 9]

[0171] From Table 9, it can be seen that even when the coil conductor 5 is three-dimensional and double-spiral, when the interlayer region is made up of the first magnetic base body, the axial end region is made up of the second magnetic base body, and the saturation magnetization of the first soft magnetic metal particles is higher than that of the second soft magnetic metal particles (Examples 11 to 15), the result is OK, and it can be confirmed that the inductance and DC superposition characteristics are sufficiently high.

[0172] (Samples in Tables 10 to 21) For each sample in Tables 10 to 21, a laminated coil was obtained in the same manner as in Example 4, except that the composition and average particle size of each soft magnetic metal powder were changed to be those shown in Tables 10, 11, 13, 14, 16, 17, 19, and 20. That is, each sample in Tables 10 to 21 was produced to have the structure shown in FIG. 1A.

[0173] For the obtained laminated coil, the average particle size of the soft magnetic metal particles was measured, L and Idc were measured, and (ΔL / L) and (ΔIdc / Idc) were obtained in the same manner as described above. The average particle size of the first soft magnetic metal particles is shown in Tables 10, 13, 16, and 19, and the average particle size of the second soft magnetic metal particles is shown in Tables 11, 14, 17, and 20. The results of L, Idc, (ΔL / L), and (ΔIdc / Idc) are shown in Tables 12, 15, 18, and 21.

[0174] In addition, for each sample in Tables 10 to 21, "restraint of plating elongation" and "short circuit rate" were measured by the following methods.

[0175] <Suppression of plating elongation> The suppression of plating elongation was evaluated by observing the appearance of the laminate coil. A was given when no plating elongation was observed, B when plating elongation was observed but 50 μm or less, C when plating elongation was more than 50 μm and less than 400 μm, and D when plating elongation was 400 μm or more. The results are shown in Tables 12, 15, 18, and 21.

[0176] <Number of shorts> Thirty laminated coils were fabricated, and the number of short-circuited laminated coils was measured using an LCR meter. A value of 0 / 30 was considered to be good. The results are shown in Tables 12, 15, 18, and 21.

[0177] [Table 10]

[0178] [Table 11]

[0179] [Table 12]

[0180] [Table 13]

[0181] [Table 14]

[0182] [Table 15]

[0183] [Table 16]

[0184] [Table 17]

[0185] [Table 18]

[0186] [Table 19]

[0187] [Table 20]

[0188] [Table 21]

[0189] From Tables 10 to 12, it was confirmed that when the average particle size of the first soft magnetic metal particles was 1 to 6 μm (Example 4, Example 16 to Example 18), the balance of inductance and DC bias characteristics was better, the evaluation of plating elongation suppression was higher, and the number of short circuits was fewer.

[0190] From Tables 10 to 12, it was confirmed that when the average particle size of the second soft magnetic metal particles was 1 to 15 μm (Example 4, Example 20 to Example 23), the balance between the inductance and the DC bias characteristics was better and the number of short circuits was smaller.

[0191] From Tables 13 to 15, it was confirmed that when the P content of the first soft magnetic metal particles was 10 to 40 ppm (Examples 26 to 28), the evaluation of inhibition of plating elongation was higher and the number of short circuits was smaller.

[0192] From Tables 13 to 15, it was confirmed that when the P content of the second soft magnetic metal particles was 100 to 6000 ppm (Examples 30 to 33), the evaluation of inhibition of plating elongation was higher and the number of short circuits was smaller.

[0193] From Tables 16 to 18, it was confirmed that when the Ni content of the second soft magnetic metal particles was greater than 14.0 mass% and less than 56.0 mass% (Examples 35 to 38), the inductance was large and the balance between inductance and DC bias characteristics was better.

[0194] From Tables 19 to 21, it was confirmed that when the Si content of the first soft magnetic metal particles was 3.5 to 7.5 mass% (Examples 41 to 43), the balance between inductance and DC bias characteristics was better, the evaluation of plating elongation suppression was higher, and the number of short circuits was reduced.

[0195] From Tables 19 to 21, it was confirmed that when the Si content of the second soft magnetic metal particles was 2.0 to 6.0 mass% (Examples 46 and 47), the balance between inductance and DC bias characteristics was better, the evaluation of plating elongation suppression was higher, and the number of short circuits was reduced. [Explanation of symbols]

[0196] 1... Multilayer coil 2... Element 2a1,2a2…Shaft end area 2b… ​​Axis center area 24ba…Axis center coil area 24ba1… Interlayer area 24bb… Shaft center inner diameter area 24bc... Shaft center outer diameter area 3…Terminal electrode 4…Magnetic element 4a… Coil area 4b… Inner diameter area 4c…Outer diameter area 40... first magnetic element 40a... Interlayer first magnetic element 40b... Inner diameter first magnetic element 40c... Outer diameter first magnetic element 400a~400h... 1st Green Sheet 42…Second magnetic element 42a1,42a2... Second magnetic element at shaft end 42a... Interlayer second magnetic element 42b… Inner diameter second magnetic element 42c... Second outer diameter magnetic element 420a~420h... 2nd Green Sheet 5... Coil conductor 501, 502... 2nd layer outer coil conductor 503,504… 2nd layer inner coil conductor 505,506… 3rd layer inner coil conductor 521,522...7th layer inner coil conductor 523,524…7th layer outer coil conductor 525,526… 8th layer outer coil conductor 527,528… 8th layer inner coil conductor 50b, 50b1, 50c, 50c1, 50c2, 50d, 50d1, 50e, 50e1, 50f, 50f1, 50f2, 50g, 50g1... Conductor 5a1,5a2… Extraction electrode 50a1, 50a2... conductor 100a~100h… Printed

Claims

1. An electronic component including an element having a magnetic body and a coil conductor, the magnetic body located between adjacent coil conductor layers in an axial direction of the coil conductor includes first soft magnetic metal particles, the magnetic body located on the outer side along the axis includes second soft magnetic metal particles, an inner diameter second magnetic element that is present in at least a portion of an axial center inner diameter region of the element including the axial center of the coil conductor includes the second soft magnetic metal particles; the first soft magnetic metal particles have a higher saturation magnetization than the second soft magnetic metal particles, 1st Ms / 2nd Ms is 1.07 to 1.80, The first Ms is the saturation magnetization of the first soft magnetic metal particle, The second Ms is the saturation magnetization of the second soft magnetic metal particles.

2. 2. The coil-type electronic component according to claim 1, wherein the first soft magnetic metal particles are made of an Fe--Si alloy.

3. 3. The coil-type electronic component according to claim 1, wherein the second soft magnetic metal particles are made of an Fe--Ni alloy.

4. 2. The coil-type electronic component according to claim 1, wherein in a cross section perpendicular to the axis of the coil conductor, the ratio of the area of ​​the inner diameter second magnetic body to the area of ​​the axial center inner diameter region is 30% or more.

5. 5. The coil-type electronic component according to claim 1, wherein the first soft magnetic metal particles have an average particle size of 1 to 6 μm.

6. 6. The coil-type electronic component according to claim 1, wherein the second soft magnetic metal particles have an average particle size of 1 to 15 μm.

7. A coil-type electronic component described in any one of claims 1 to 6, wherein an outer diameter second magnetic body present in at least a portion of the axial central outer diameter region of the element located radially outside the coil conductor contains the second soft magnetic metal particles.

8. 8. The coil-type electronic component according to claim 7, wherein in a cross section perpendicular to the axis of the coil conductor, the ratio of the area of ​​the outer diameter second magnetic body to the area of ​​the axial center outer diameter region is 15% or more.

Citation Information

Patent Citations

  • Soft magnetic alloy powder, compact, and inductance element

    JP2008135674A

  • Laminated electronic component

    JP2016009859A

  • Magnetic material and electronic component

    JP2018011043A

  • Magnetic coupling type coil component and manufacturing method thereof

    JP2020013936A

  • Coil component

    JP2021174937A