Method for forming oxide semiconductor film and method for manufacturing thin film transistor
By adjusting the distance between the target and substrate during sputtering with a mixed gas of argon and oxygen, the method forms oxide semiconductor films with different crystallinity without affecting film density, enhancing the reliability of thin film transistors.
Patent Information
- Application Number
- JP2020210353
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-18
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2040-12-18
AI Technical Summary
Existing methods for controlling the crystallinity of oxide semiconductor films by adjusting oxygen gas partial pressure during sputtering result in significant reductions in film density, making it difficult to form films with different crystallinity without affecting density.
A film formation method that controls the crystallinity of oxide semiconductor films by varying the distance between the target and the substrate during sputtering, using a mixed gas of argon and oxygen, and maintaining consistent oxygen partial pressure, allowing for the formation of both amorphous and crystalline films without altering film density.
This method enables the production of oxide semiconductor films with varying crystallinity while maintaining film density, reducing oxygen vacancies, and improving the reliability of thin film transistors by minimizing defects at the interface.
Smart Images

Figure 0007595246000001 
Figure 0007595246000002 
Figure 0007595246000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a film formation method for forming an oxide semiconductor film by sputtering a target using plasma, and a method for manufacturing a thin film transistor using the film formation method. [Background technology]
[0002] In recent years, there has been active development of thin-film transistors that use oxide semiconductors such as In-Ga-Zn-O (IGZO) for the channel layer. In the manufacturing process of thin-film transistors with such semiconductor layers, if there are many defects such as oxygen vacancies in the semiconductor layer, the electrical conductivity of the semiconductor layer may change, which may deteriorate the electrical characteristics of the thin-film transistor. Therefore, various attempts have been made to reduce defects such as oxygen vacancies in the semiconductor layer.
[0003] For example, Patent Document 1 describes an oxide semiconductor layer having a multilayer structure in which a first semiconductor layer made of an amorphous oxide semiconductor film and a second semiconductor layer made of a crystalline oxide semiconductor film are laminated. Patent Document 1 describes that by laminating a crystalline second semiconductor layer on an amorphous first semiconductor layer, oxygen defects at the interface with an insulating layer formed thereon can be reduced, and the gate threshold voltage of a thin film transistor can be increased. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] International Publication No. WO2019 / 181095 Summary of the Invention [Problem to be solved by the invention]
[0005] Incidentally, the above-mentioned Patent Document 1 describes that the crystallinity of an oxide semiconductor film is controlled by changing the partial pressure of oxygen gas in a sputtering gas. Specifically, it describes that an amorphous oxide semiconductor film is formed by lowering the partial pressure of oxygen gas, and a crystalline oxide semiconductor film is formed by increasing the partial pressure of oxygen gas. However, such a method of controlling the crystallinity of an oxide semiconductor film by changing the partial pressure of oxygen gas has a problem in that the film density of an amorphous oxide semiconductor film formed at a low partial pressure of oxygen gas is significantly reduced compared to a crystalline oxide semiconductor film formed at a high partial pressure of oxygen gas.
[0006] The present invention has been made in view of the above problems, and an object of the present invention is to provide a film formation method by which oxide semiconductor films having different crystallinity can be formed without significantly changing the film density. [Means for solving the problem]
[0007] As a result of intensive research by the present inventors to solve the above problems, it has been found that in a film formation method in which an oxide semiconductor film is formed by sputtering a target using plasma, there is a correlation between the distance between the target and a substrate and the crystallinity of the oxide semiconductor film. As a result of further intensive research, the present inventors have found that a crystalline oxide semiconductor film can be formed by performing sputtering with a short distance between the target and the substrate, and that an amorphous oxide semiconductor film can be formed by performing sputtering with a long distance between the target and the substrate.
[0008] That is, the film formation method of the present invention is a method for forming an oxide semiconductor film on a substrate by sputtering a target using plasma, and is characterized in that the crystallinity of the oxide semiconductor film is controlled by changing the distance between the substrate and the target.
[0009] In this deposition method, the crystallinity of the oxide semiconductor film can be controlled by changing the distance between the substrate and the target, so that it is not necessary to change the partial pressure of oxygen gas during sputtering when depositing a plurality of oxide semiconductor films with different crystallinity, which makes it possible to form oxide semiconductor films with different crystallinity without significantly changing the film density. Note that "forming an oxide semiconductor film on a substrate" means not only forming an oxide semiconductor film directly on the surface of a substrate, but also forming an oxide semiconductor film with a film of another component interposed between the oxide semiconductor film and the substrate.
[0010] It is preferable that the film formation method includes a first film formation step of forming the oxide semiconductor film as an amorphous film by performing sputtering with a predetermined first distance between the substrate and the target, and a second film formation step of forming a crystalline oxide semiconductor film by performing sputtering with a predetermined second distance between the substrate and the target that is shorter than the first distance. In this manner, by performing sputtering while changing the distance between the substrate and the target, an amorphous oxide semiconductor film and a crystalline oxide semiconductor film can be formed separately.
[0011] In the film forming method, it is preferable that sputtering is performed using a mixed gas of argon gas and oxygen gas as a sputtering gas. In this case, by containing oxygen gas in the sputtering gas, oxygen vacancies in the oxide semiconductor film can be further reduced and the film density can be improved.
[0012] In the film formation method, it is preferable that the oxygen partial pressure in the sputtering gas is the same in the first film formation step and the second film formation step. In this way, since there is no need to change the oxygen partial pressure in the sputtering gas between the first and second film formation processes, the first and second film formation processes can be transitioned with the plasma maintained in a stable state. This shortens the tact time and reduces the manufacturing cost. In addition, since the oxygen partial pressure is the same in each film formation process, the film density does not change significantly.
[0013] In the film formation method, it is preferable that the partial pressure of the oxygen gas in the sputtering gas is 2.5% or more. In this manner, oxygen vacancies in the oxide semiconductor layer can be further reduced, and the crystallinity of the oxide semiconductor film formed in the second film formation step can be further improved.
[0014] In a specific embodiment of the film formation method, the crystallinity of the oxide semiconductor film is controlled by changing the distance between the substrate and the target while maintaining the plasma.
[0015] A specific example of the oxide semiconductor film is In-Ga-Zn-O (IGZO).
[0016] In the first and second film forming steps, sputtering is preferably performed by applying a target bias voltage to the target that is a negative voltage of −1.0 kV or more. In this way, the absolute value of the target bias voltage is small, at 1.0 kV or less, so that the generation of sputtered particles from which oxygen has been desorbed can be suppressed. As a result, a film that maintains the same oxide state as the target material is formed on the substrate, and a high-quality oxide semiconductor layer with higher film density can be formed.
[0017] In the film forming method, it is preferable that sputtering is performed using a sputtering apparatus capable of independently controlling a target bias voltage applied to the target and a high frequency power supplied to the antenna. By using such a sputtering device, the bias voltage applied to the target can be set independently of the plasma generation, so the bias voltage can be set to a low voltage that attracts ions in the plasma to the target and sputters them. This makes it possible to set the negative bias voltage applied to the target during sputtering to a small value of -1 kV or more.
[0018] Further, a method for manufacturing a thin film transistor of the present invention is a method for manufacturing a thin film transistor in which a gate electrode, a gate insulating layer, an oxide semiconductor layer, a source electrode and a drain electrode are stacked on a substrate, and is characterized in that the oxide semiconductor layer is formed by the above-mentioned film formation method. Such a manufacturing method can provide the same effects as the above-described film forming method of the present invention. Effect of the Invention
[0019] According to the present invention configured as above, it is possible to provide a film formation method capable of forming oxide semiconductor films having different crystallinity without a large change in film density. [Brief description of the drawings]
[0020] [Figure 1] FIG. 2 is a diagram illustrating a configuration of a thin film transistor according to the present embodiment. [Diagram 2] 3A to 3C are diagrams illustrating a manufacturing process of the thin film transistor according to the embodiment. [Diagram 3] FIG. 2 is a diagram illustrating a configuration of a sputtering apparatus used in a semiconductor layer formation process of the thin film transistor according to the embodiment. [Figure 4] FIG. 11 is a diagram illustrating a configuration of a thin film transistor according to another embodiment. [Diagram 5] 13 is a graph showing the relationship between the deposition distance and the crystallinity of an oxide semiconductor film in an experimental example. [Figure 6] 13 is a graph showing the relationship between the deposition distance and the crystallinity and film density of an oxide semiconductor film in an experimental example. [Figure 7]13 is a graph showing the relationship between the partial pressure of oxygen gas and the crystallinity of an oxide semiconductor film in a comparative example. [Figure 8] 13 is a graph showing the relationship between the partial pressure of oxygen gas and the crystallinity and film density of an oxide semiconductor film in a comparative example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] A thin film transistor and a method for manufacturing the same according to one embodiment of the present invention will be described below.
[0022] <1. Thin-film transistor> The thin film transistor 1 of this embodiment is a so-called bottom gate type. Specifically, as shown in Fig. 1, the thin film transistor 1 has a substrate 2, a gate electrode 3, a gate insulating layer 4, an oxide semiconductor layer 5 as a channel layer, a source electrode 6, a drain electrode 7, and a protective layer 8, which are arranged (formed) in this order from the substrate 2 side. Each part will be described in detail below.
[0023] The substrate 2 is made of a material that can transmit light, and may be made of, for example, a resin material such as polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polyethersulfone (PES), acrylic, or polyimide, or glass.
[0024] A gate electrode 3 is provided on the surface of the substrate 2. The gate electrode 3 is made of a material having high conductivity, and may be made of one or more metals selected from, for example, Si, Al, Mo, Cr, Ta, Ti, Pt, Au, Ag, etc. Alternatively, the gate electrode 3 may be made of a conductive film of a metal oxide such as Al-Nd, Ag alloy, tin oxide, zinc oxide, indium oxide, indium tin oxide (ITO), indium zinc oxide (IZO), In-Ga-Zn-O (IGZO), etc. The gate electrode 3 may be made of a single layer structure of these conductive films or a laminated structure of two or more layers.
[0025] A gate insulating layer 4 is disposed on the gate electrode 3. The gate insulating layer 4 is made of a material having high insulating properties, such as SiO2, SiN x , SiON, Al2O3, Y2O3, Ta2O5, Hf2, etc. The gate insulating layer 4 may be a single-layer structure or a laminate structure of two or more layers of these conductive films.
[0026] An oxide semiconductor layer 5 is disposed on the gate insulating layer 4. The oxide semiconductor layer 5 of this embodiment has a multi-layer structure in which a first semiconductor layer 5a and a second semiconductor layer 5b are disposed in this order from the substrate 2 side. Both the first semiconductor layer 5a and the second semiconductor layer 5b are made of an oxide semiconductor layer mainly composed of an oxide containing In, and are preferably made of, for example, In-Ga-Zn-O, In-Al-Mg-O, In-Al-Zn-O, or In-Hf-Zn-O. The first semiconductor layer 5a is a layer made of an amorphous oxide semiconductor film, and the second semiconductor layer 5b is a layer made of a crystalline oxide semiconductor film.
[0027] When the first semiconductor layer 5a is an oxide semiconductor film made of In-Ga-Zn-O (IGZO), the fact that the first semiconductor layer 5a is an amorphous oxide semiconductor film can be confirmed by the absence of a steep peak near 2θ=31° in measurement by XRD (X-ray diffraction) using a θ-2θ method with a Cu light source (Cu-Kα radiation).
[0028] The higher the crystallinity of the second semiconductor layer 5b, the more oxygen defects at the interface can be reduced, and the lower the gate threshold voltage V th (Drain current I d = 1nA at gate voltage V g) can be increased. Therefore, it is preferable that the crystallinity of the second semiconductor layer 5b is high. When the second semiconductor layer 5b is an oxide semiconductor film made of In-Ga-Zn-O (IGZO), the degree of crystallinity of the second semiconductor layer 5b can be evaluated by the full width at half maximum of the peak that can be confirmed near 2θ=31° in the measurement by XRD (X-ray diffraction) described above. Specifically, it can be evaluated that the smaller the full width at half maximum of the peak, the higher the crystallinity of the second semiconductor layer 5b.
[0029] A source electrode 6 and a drain electrode 7 are disposed on the oxide semiconductor layer 5. The source electrode 6 and the drain electrode 7 are formed apart from each other so as to partially cover the surface of the semiconductor layer 5. The source electrode 6 and the drain electrode 7 are each made of a material having high conductivity so as to function as an electrode. For example, they may be made of the same material as the gate electrode 2, or may be made of a different material. The source electrode 6 and the drain electrode 7 may be made of a single layer structure of a metal or a conductive oxide, or may be made of a laminate structure of two or more layers.
[0030] A protective layer (passivation layer) 8 for protecting the oxide semiconductor 5, the source electrode 6, and the drain electrode 7 is disposed on the oxide semiconductor 5, the source electrode 6, and the drain electrode 7. The protective layer 8 is made of an insulating material, and may be, for example, a fluorine-containing silicon nitride film (SiN:F), a fluorine-containing silicon oxide film (SiO:F), a silicon nitride film (SiN x ), silicon oxide film (SiO x ) etc.
[0031] 2. Thin-film transistor manufacturing method Next, a method for manufacturing the thin film transistor 1 having the above-described structure will be described with reference to FIG. The method for manufacturing the thin film transistor 1 of this embodiment includes a gate electrode forming step, a gate insulating layer forming step, a semiconductor layer forming step, a source / drain electrode forming step, and a protective layer forming step. Each step will be described below.
[0032] (1) Gate electrode formation process 2(a), a substrate 2 made of a resin material such as PET is prepared, and a gate electrode 3 is formed on the surface of the substrate 2. The method for forming the gate electrode 3 is not particularly limited, and the gate electrode 3 may be formed by a known method such as a vacuum deposition method or a DC sputtering method.
[0033] (2) Gate insulation layer formation process 2(b), a gate insulating layer 4 is formed so as to cover the surfaces of the substrate 2 and the gate electrode 3. There are no particular limitations on the method for forming the gate insulating layer 4, and it may be formed by a known method.
[0034] (3) Semiconductor layer formation process 2(c), an oxide semiconductor layer 5 serving as a channel layer is formed on the gate insulating layer 4. This semiconductor layer formation process includes a first film formation process for forming a first semiconductor layer 5a and a second film formation process for forming a second semiconductor layer 5b.
[0035] (3-1) Sputtering equipment In this semiconductor layer forming process, a sputtering apparatus 100 is used that sputters a target T using an inductively coupled plasma P as shown in Fig. 3. The sputtering apparatus 100 includes a vacuum vessel 20, a substrate holder 30 that holds a substrate 2 in the vacuum vessel 20, a target holder 40 that holds a target T facing the substrate 2 in the vacuum vessel 20, a plurality of antennas 50 that are arranged along the surface of the substrate 2 held by the substrate holder 30 and generate a plasma P, a high-frequency power supply 60 (frequency 13.56 MHz) that applies a high-frequency to the plurality of antennas 50 to generate an inductively coupled plasma P in the vacuum vessel 20, and a target bias power supply 11 that applies a target bias voltage to the target T. By using such a sputtering apparatus 100, the high-frequency voltage supplied to the antenna 50 to generate the plasma P and the target bias voltage applied to the target T can be controlled independently. Therefore, independent of the generation of plasma P, the bias voltage can be set to a low voltage that attracts ions in the plasma P to the target T and causes sputtering, and the negative bias voltage applied to the target T during sputtering can be set to a negative voltage of -1 kV or more (i.e., an absolute value of 1 kV or less). Furthermore, independent of the generation of plasma P, the value of the bias voltage applied to the target T can be arbitrarily changed during sputtering. Sputtering is performed by placing the target T (e.g., IGZO) on the target holding part 40 of the sputtering device 100 and placing the substrate 2 on the substrate holding part 30. Note that in this sputtering device 100, the height position in the vertical direction of the substrate holding part 30 or the target holding part 40 is variable, and this allows the distance between the target T and the substrate to be changed during plasma processing.
[0036] (3-2) First film formation process Using the above-described sputtering apparatus 100, first, an amorphous first semiconductor layer 5a is formed on the gate insulating layer 4. Specifically, the vacuum chamber 20 of the sputtering apparatus 100 is set to, for example, 3×10 -6After evacuating to Torr or less, the pressure in the vacuum vessel 20 is adjusted to, for example, 0.5 Pa to 3.1 Pa while introducing a sputtering gas at a flow rate of 50 sccm to 200 sccm. Then, high-frequency power is supplied from the high-frequency power source 60 to the multiple antennas 50 to generate and maintain an inductively coupled plasma P. A DC voltage pulse is applied from the target bias power source 11 to the target T to perform sputtering of the target T. From the viewpoint of reducing oxygen deficiency in the first semiconductor layer 5a, the voltage applied to the target T is preferably a negative voltage of -1 kV or more, more preferably a negative voltage of -600 V or more. As a result, the first semiconductor layer 5a is formed on the gate insulating layer 4 as shown in FIG. 2(c). The pressure in the vacuum vessel 20, the flow rate of the sputtering gas, the high-frequency power density, etc. may be changed as appropriate.
[0037] (3-3) Second film formation process After the first film formation process, a crystalline second semiconductor layer 5b is formed on the first semiconductor layer 5a by performing sputtering using the sputtering apparatus 100. Conditions in the second film formation process, such as the pressure in the vacuum chamber, the flow rate of the sputtering gas, the high-frequency power density, and the negative voltage value applied to the target T, may be the same as those in the first film formation process or may be changed as appropriate.
[0038] (3-4) Distance between substrate and target Here, in the semiconductor layer forming process of this embodiment, the crystallinity of the oxide semiconductor film is controlled by changing the distance (hereinafter, the film forming distance) between the substrate and the target T in the sputtering device 100, and the first semiconductor layer 5a, which is amorphous, and the second semiconductor layer 5b, which is crystalline, are separately formed. Specifically, in this semiconductor layer forming process, the film forming distance is made different between the first film forming process and the second film forming process, and the film forming distance in the second film forming process (referred to as the second film forming distance) is made shorter than the film forming distance in the first film forming process (referred to as the first film forming distance). More specifically, in the first film forming process, plasma P is generated in the vacuum container 20, and sputtering is performed at the first film forming distance to form the first semiconductor layer 5a with a predetermined thickness on the gate insulating layer. Then, while maintaining the plasma P generated in the vacuum container 20, the distance between the substrate and the target T is narrowed, and sputtering is performed at the second film forming distance to form the second semiconductor layer 5b on the first semiconductor layer 5a. The film formation distance means the distance between the surface of the substrate holder 30 of the sputtering apparatus 100 on which the substrate 2 is placed and the surface of the target T facing the surface of the substrate holder 30 .
[0039] (3-5) Oxygen partial pressure in sputtering gas In the first and second film formation steps, the sputtering gas supplied may be argon gas alone or a mixed gas of argon gas and oxygen gas. From the viewpoint of reducing oxygen vacancies in the semiconductor layer 5 and improving the film density, the sputtering gas supplied is preferably a mixed gas of argon gas and oxygen gas. In this case, from the viewpoint of forming a second semiconductor layer 5b with higher crystallinity in the second film formation step, the partial pressure of oxygen gas in the mixed gas is preferably 2.5% or more, and more preferably 5% or more. In addition, the partial pressure of oxygen gas in the mixed gas may be different or the same between the first and second film formation steps.
[0040] (4) Source and drain electrode formation process 2(e), a source electrode 6 and a drain electrode 7 are formed on the oxide semiconductor layer 5. The source electrode 6 and the drain electrode 7 can be formed by a known method using, for example, RF magnetron sputtering. The source electrode 6 and the drain electrode 7 are formed to be spaced apart from each other on the surface of the semiconductor layer 5 and to expose a part of the surface of the semiconductor layer 5.
[0041] (5) Protective layer formation process Thereafter, as shown in FIG. 2(f), a protective film 8 is formed by, for example, a plasma CVD method so as to cover the upper surfaces of the formed oxide semiconductor layer 5, the source electrode 6, and the drain electrode .
[0042] In this manner, the thin film transistor 1 of the present embodiment can be obtained.
[0043] <3. Effects of this embodiment> In the method for manufacturing the thin film transistor 1 of the present embodiment configured as described above, since the crystallinity can be controlled by changing the film formation distance without changing the oxygen gas partial pressure during sputtering in the semiconductor layer formation step, both the amorphous oxide semiconductor film and the crystalline oxide semiconductor film can be formed with excellent film density. This can reduce the defect density at the interface between the gate insulating layer 4 or the protective layer 8 and the oxide semiconductor layer 5, and therefore a high-reliability, excellent thin film transistor can be manufactured.
[0044] <4. Other Modified Embodiments> The present invention is not limited to the above-described embodiment.
[0045] For example, the thin film transistor 1 in the above embodiment is a bottom-gate type in which the gate electrode 3, the gate insulating layer 4, and the oxide semiconductor layer 5 are stacked in this order from the substrate 2 side, but is not limited to this. In other embodiments, the thin film transistor 1 may be a top-gate type in which the oxide semiconductor layer 5, the gate insulating layer 4, and the gate electrode 3 are stacked in this order from the substrate 2 side, as shown in FIG.
[0046] In the thin film transistor 1 of the embodiment, the oxide semiconductor layer 5 has a two-layer structure in which the amorphous first semiconductor layer 5a and the crystalline second semiconductor layer 5b are laminated, but this is not limited thereto. In other embodiments, the oxide semiconductor layer 5 may have a structure of, for example, three or more layers.
[0047] In the manufacturing method of the above embodiment, the amorphous first semiconductor layer 5a is formed first, and then the crystalline second semiconductor layer 5b is formed, but this is not limited thereto. In other embodiments, the amorphous first semiconductor layer 5a may be formed after the crystalline second semiconductor layer 5b is formed.
[0048] In the manufacturing method of the above embodiment, the first film formation process is started by changing the film formation distance while maintaining the plasma P generated in the vacuum vessel 20, but this is not limited to the above. In other embodiments, the generation of the plasma P may be stopped between the first film formation process and the second film formation process.
[0049] Furthermore, the present invention is not limited to the above-described embodiment, and it goes without saying that various modifications are possible without departing from the spirit of the present invention. EXAMPLES
[0050] The present invention will be described in more detail below with reference to examples. The present invention is not limited to the following examples, and can be practiced with appropriate modifications within the scope of the above and below-mentioned aims, and all such modifications are included in the technical scope of the present invention.
[0051] 1. Relationship between deposition distance and crystallinity and film density of oxide semiconductor film As an experimental example showing the effect of the present invention, the sputtering apparatus 100 of the present embodiment described above was used to evaluate the relationship between the film formation distance during sputtering and the crystallinity and film density of the oxide semiconductor film formed.
[0052] (Sample Preparation) Specifically, the vacuum chamber 20 of the sputtering apparatus 100 is set to 4.0×10 -4 After evacuation to below 10 Pa, a mixed gas of argon and oxygen (oxygen partial pressure: 5%) was supplied as a sputtering gas at a flow rate of 5 sccm, and the pressure inside the vacuum chamber 20 was adjusted to 0.9 Pa. Then, high-frequency power was supplied from a high-frequency power supply 60 to a plurality of antennas 50 to generate and maintain an inductively coupled plasma. IGZO (1114) was used as the target T, and a direct-current voltage pulse (-400 V, 75 kHz, Duty 95.7%) was applied to the target T to perform sputtering, thereby forming an oxide semiconductor film (IGZO film) on a glass substrate (SiO2). Here, three oxide semiconductor films with different film formation conditions were formed by changing the film formation distance (124 mm, 153 mm, 183 mm).
[0053] (Evaluation of crystallinity) X-ray diffraction (XRD) was performed on the three samples prepared using a Bruker AXS X-ray diffractometer (model: D8 DISCOVER) using a Cu light source (Cu-Kα radiation). The results are shown in Figure 5. The diffraction peaks in the spectrum shown in Figure 5 are due to In in the IGZO film. As can be seen from this, in the sample with a deposition distance of 183 mm, no diffraction peak appeared near 2θ=31°, but a diffraction peak appeared near 2θ=33°, indicating that an amorphous IGZO film (a-IGZO) was mainly formed. On the other hand, in the samples with a relatively short deposition distance (153 mm, 124 mm), no diffraction peak appeared near 2θ=33°, but a steep diffraction peak appeared near 2θ=31°, indicating that a crystalline IGZO film (c-IGZO) was mainly formed. From this result, it was confirmed that the crystallinity of the oxide semiconductor film can be controlled by changing the distance between the substrate and the target during sputtering. In the sample with the longest deposition distance, the sputtered particles ejected from the target collide with each other more times before reaching the substrate than in the other samples, which is thought to result in a decrease in crystallinity and mainly an amorphous IGZO film being deposited. Conversely, in the sample with a relatively short deposition distance, the sputtered particles ejected from the target collide with each other less times before reaching the substrate, which is thought to result in mainly a crystalline IGZO film being deposited.
[0054] (Evaluation of film density) Next, the film density of each sample was measured. The film density was measured by X-ray reflectivity (XRR method, measuring device: Bruker D8 DISCOVER). The results are shown in Figure 6. Figure 6 shows the film density for each film formation distance and the full width at half maximum of the diffraction peak (diffraction peak derived from In in the IGZO film) appearing in the spectrum obtained by the above-mentioned X-ray diffraction. As can be seen from Figure 6, by changing the film formation distance, it was confirmed that the crystallinity of the IGZO film can be controlled without significantly decreasing the film density, and that it is possible to produce crystalline IGZO films and amorphous IGZO films separately.
[0055] 2. Relationship between oxygen partial pressure and crystallinity and film density of oxide semiconductor film Next, as a comparative example, the relationship between the oxygen partial pressure in the sputtering gas and the crystallinity and film density of the oxide semiconductor film formed was evaluated using the sputtering apparatus 100 of the above-described embodiment.
[0056] (Sample Preparation) Specifically, the vacuum chamber 20 of the sputtering apparatus 100 is set to 4.0×10 -4After evacuation to below 1 Pa, a mixed gas of argon and oxygen was supplied as a sputtering gas at a flow rate of 5 sccm, and the pressure inside the vacuum chamber 20 was adjusted to 0.9 Pa. Then, high-frequency power was supplied from a high-frequency power source 60 to a plurality of antennas 50 to generate an inductively coupled plasma, which was then maintained. IGZO (1114) was used as the target T, and a direct-current voltage pulse (-400 V, 75 kHz, Duty 95.7%) was applied to the target T to perform sputtering, thereby forming an oxide semiconductor film (IGZO film) on a glass substrate (SiO2). The sputtering was performed with the film formation distance fixed at 124 mm. Here, three oxide semiconductor films with different film formation conditions were formed by changing the oxygen partial pressure in the sputtering gas (0.5%, 2.5%, 5%).
[0057] (Evaluation of crystallinity) Then, X-ray diffraction (XRD) was performed on the three samples prepared using the X-ray diffraction apparatus described above. The results are shown in Figure 7. As can be seen from this, in the sample with an oxygen partial pressure of 0.5%, no diffraction peak appears near 2θ=31°, but a diffraction peak appears near 2θ=33°, indicating that an amorphous IGZO film (a-IGZO) is mainly formed. On the other hand, in the sample with a relatively high oxygen partial pressure (5%), a steep diffraction peak appears near 2θ=31°, indicating that a crystalline IGZO film (c-IGZO) is mainly formed. In the sample with an oxygen partial pressure of 2.5%, diffraction peaks appear near 2θ=33° and 2θ=31°, indicating that both an amorphous IGZO film (a-IGZO) and a crystalline IGZO film (c-IGZO) are formed. From this result, it was confirmed that the crystallinity of the oxide semiconductor film can be controlled by changing the oxygen partial pressure in the sputtering gas.
[0058] (Evaluation of film density) Next, the film density of each sample was measured by the X-ray reflectivity method described above. The results are shown in Figure 8. Figure 8 shows the film density for each oxygen partial pressure and the full width at half maximum of the diffraction peak appearing in the spectrum obtained by the X-ray diffraction described above. As can be seen from Figure 8, by changing the oxygen partial pressure during film formation, it is possible to control the crystallinity of the oxide semiconductor film and to form either a crystalline IGZO film or an amorphous IGZO film, but it was confirmed that the film density is significantly reduced when forming an amorphous IGZO film. [Explanation of symbols]
[0059] 2. Circuit Board 5. Oxide semiconductor layer 100 Sputtering equipment 20...vacuum container 50 Antenna T ···Target P...Plasma
Claims
1. 1. A method for forming an oxide semiconductor film on a substrate by sputtering a target using plasma, comprising the steps of: the crystallinity of the oxide semiconductor film is controlled by changing the distance between the substrate and the target, thereby forming the oxide semiconductor film either amorphous or crystalline.
2. a first film formation step of performing sputtering with a first distance between the substrate and the target to form the amorphous oxide semiconductor film; and a second film formation step of performing sputtering at a second distance between the substrate and the target that is shorter than the first distance to form the oxide semiconductor film that is crystalline.
3. 3. The method according to claim 1, wherein the sputtering is carried out using a mixed gas of argon gas and oxygen gas as a sputtering gas.
4. 4. The film forming method according to claim 3, which cites claim 2, wherein the oxygen partial pressure in the sputtering gas is the same in the first film forming step and the second film forming step.
5. 5. The film forming method according to claim 4, wherein the partial pressure of the oxygen gas in the sputtering gas is 2.5% or more.
6. 6. The method according to claim 1, wherein the crystallinity of the oxide semiconductor film is controlled by changing a distance between the substrate and the target while maintaining the plasma.
7. 7. The method according to claim 1, wherein the oxide semiconductor film is made of In--Ga--Zn--O.
8. The film forming method according to any one of claims 1 to 7, wherein sputtering is performed by applying a target bias voltage to the target at a negative voltage of -1.0 kV or more.
9. 9. The film forming method according to claim 1, wherein sputtering is performed using a sputtering device capable of independently controlling a target bias voltage applied to the target and a high frequency power supplied to an antenna for generating plasma.
10. A method for manufacturing a thin film transistor in which a gate electrode, a gate insulating layer, an oxide semiconductor layer, a source electrode, and a drain electrode are stacked on a substrate, the method comprising the steps of: A method for manufacturing a thin film transistor, comprising forming the oxide semiconductor layer by the film formation method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Method for manufacturing group iii nitride semiconductor light-emitting device, group iii nitride semiconductor light-emitting device, and lamp
JP2008198705A
Semiconductor device and method for manufacturing the same
JP2013021308A
Zno-based piezoelectric film and piezoelectric element
JP2018170488A
Thin film transistor and method of manufacturing the same
JP2020092222A
Film formation method, method for manufacturing thin-film transistor, and thin-film transistor