Semiconductor Device
The semiconductor device with a corundum structure and oriented electrodes in the c-axis or m-axis directions addresses the challenges of growing high-quality gallium oxide films, achieving superior electrical properties and reduced defects for power applications.
Patent Information
- Application Number
- JP2020003249
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-01-10
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2040-01-10
AI Technical Summary
Conventional methods for growing high-quality gallium oxide films with a corundum structure face challenges such as dislocations, cracks, and poor electrical properties due to mismatched lattice constants and thermal expansion coefficients, limiting their application in semiconductor devices.
A semiconductor device is designed with a corundum structure semiconductor layer, where electrodes are oriented in the c-axis or m-axis directions, utilizing a mist CVD method for epitaxial growth, enhancing electrical properties by controlling crystal growth and thermal expansion.
The semiconductor device exhibits excellent electrical properties and improved crystal quality, suitable for power devices and modules, with enhanced anisotropy and reduced defects.
Smart Images

Figure 0007595254000001 
Figure 0007595254000002 
Figure 0007595254000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a semiconductor device that is useful for a power device or the like. [Background technology]
[0002] Conventionally, there is a problem of cracks and lattice defects occurring when growing crystals on a foreign substrate. To address this problem, methods such as matching the lattice constant and thermal expansion coefficient of the substrate and film have been considered. In addition, when mismatching occurs, film formation techniques such as ELO have also been considered.
[0003] Patent Document 1 describes a method of forming a buffer layer on a heterogeneous substrate and growing a zinc oxide-based semiconductor layer on the buffer layer. Patent Document 2 describes forming a nanodot mask on a heterogeneous substrate and then forming a single crystal semiconductor material layer. Non-Patent Document 1 describes a method of growing GaN crystals on sapphire via GaN nanocolumns. Non-Patent Document 2 describes a method of growing GaN crystals on Si(111) using a periodic SiN intermediate layer to reduce defects such as pits.
[0004] However, with each of these techniques, the deposition rate was slow, and cracks, dislocations, warping, and the like occurred in the substrate, and dislocations, cracks, and the like occurred in the epitaxial film, making it difficult to obtain a high-quality epitaxial film. Also, these techniques caused problems when increasing the diameter of the substrate and the thickness of the epitaxial film.
[0005] In addition, semiconductor devices using gallium oxide (Ga2O3), which has a large band gap, are attracting attention as next-generation switching elements that can achieve high voltage resistance, low loss, and high heat resistance, and are expected to be applied to power semiconductor devices such as inverters. Furthermore, due to its wide band gap, it is expected to be used as a light-emitting device such as an LED or a sensor. The band gap of gallium oxide can be controlled by mixing indium and aluminum, either individually or in combination, and it constitutes an extremely attractive material family as an InAlGaO-based semiconductor. Here, InAlGaO-based semiconductors refer to In X Al Y Ga Z O3 (0≦X≦2, 0≦Y≦2, 0≦Z≦2, X+Y+Z=1.5~2.5), and can be viewed as being in the same material family that contains gallium oxide.
[0006] However, since the most stable phase of gallium oxide is the β-gallium structure, it is difficult to form a crystalline film having a corundum structure unless a special film formation method is used, and many problems still remain in terms of crystal quality, etc. In response to this, several studies are currently being conducted on the formation of a crystalline semiconductor film having a corundum structure. Patent Document 3 describes a method for producing an oxide crystal thin film by mist CVD using gallium or indium bromide or iodide. Patent Documents 4 to 6 describe a multilayer structure in which a semiconductor layer having a corundum crystal structure and an insulating film having a corundum crystal structure are laminated on a base substrate having a corundum crystal structure.
[0007] Recently, as described in Patent Documents 7 to 9, ELO growth of a gallium oxide film having a corundum structure has been considered. According to the methods described in Patent Documents 7 to 9, it is possible to obtain a gallium oxide film having a good corundum structure. However, even with the ELO film formation method using the thermal expansion coefficient difference described in Patent Document 7, when the crystal film is actually examined, it tends to grow as facets, and there are problems such as dislocations and cracks caused by this facet growth. In addition, as described in Patent Document 10, it has been considered that the main surface is an m-plane to improve electrical properties, but it is still not satisfactory for application to a semiconductor device having excellent electrical properties. Patent Documents 3 to 10 are all publications related to patents or patent applications filed by the present applicant. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] JP 2010-232623 A [Patent Document 2] Special Publication No. 2010-516599 [Patent Document 3] Patent No. 5397794 [Patent Document 4] Patent No. 5343224 [Patent Document 5] Patent No. 5397795 [Patent Document 6] JP 2014-72533 A [Patent Document 7] JP 2016-98166 A [Patent Document 8] JP 2016-100592 A [Patent Document 9] JP 2016-100593 A [Patent Document 10] JP 2018-082144 A [Non-patent literature]
[0009] [Non-Patent Document 1] Kazuhide Kusakabe., et al., “Overgrowth of GaN layer on GaN nano-columns by RF-molecular beam epitaxy”, Journal of Crystal Growth 237-239 (2002) 988-992 [Non-Patent Document 2] KY Zang., et al., “Defect reduction by periodic SiNx interlayers in gallium nitride grown on Si (111)”, Journal of Applied Physics 101, 093502 (2007) Summary of the Invention [Problem to be solved by the invention]
[0010] An object of the present invention is to provide a semiconductor device having excellent semiconductor characteristics, particularly excellent electrical characteristics. [Means for solving the problem]
[0011] As a result of intensive research to achieve the above-mentioned object, the inventors have found that the electrical characteristics are anisotropic not in relation to the main surface of gallium oxide having a corundum structure, but in relation to each crystal axis and the direction of current flow. They have succeeded in creating a semiconductor device having at least a semiconductor layer having a corundum structure, a first electrode arranged on a first surface side of the semiconductor layer, and a second electrode arranged on a second surface side opposite to the first surface side, wherein the second electrode extends in at least a first direction further than the first electrode, and the first direction is the c-axis direction or m-axis direction of the semiconductor layer, and have found that such a semiconductor device has excellent semiconductor characteristics, particularly electrical characteristics, and can solve the above-mentioned conventional problems in one fell swoop. After obtaining the above findings, the inventors conducted further studies and completed the present invention.
[0012] That is, the present invention relates to the following inventions. [1] A semiconductor device having at least a semiconductor layer having a corundum structure, a first electrode arranged on a first surface side of the semiconductor layer, and a second electrode arranged on a second surface side opposite to the first surface side, wherein the second electrode extends further in at least a first direction than the first electrode, and the first direction is the c-axis direction or m-axis direction of the semiconductor layer. [2] The semiconductor device according to [1], wherein the semiconductor layer contains a metal oxide containing at least one metal selected from the group consisting of gallium, indium, rhodium and iridium. [3] The semiconductor device according to [1], wherein the semiconductor layer is mainly composed of a metal oxide containing at least gallium. [4] The carrier concentration of the semiconductor layer is 1×10 19 / cm 3 The semiconductor device according to any one of the above [1] to [3], [5] The semiconductor device according to any one of [1] to [4], wherein the first surface is a c-plane. [6] The semiconductor device according to any one of [1] to [5] above, which is a power device. [7] The semiconductor device according to [6] above, which is a power module, an inverter or a converter. [8] The semiconductor device according to [6] above, which is a power card. [9] The semiconductor device according to [8], further comprising a cooler and an insulating member, the cooler being provided on both sides of the semiconductor layer, with at least the insulating member interposed therebetween.
[10] The semiconductor device according to [9], wherein a heat dissipation layer is provided on each side of the semiconductor layer, and the cooler is provided on the outside of the heat dissipation layer via at least the insulating member.
[11] A semiconductor system including a semiconductor device, the semiconductor device being the semiconductor device according to any one of [1] to
[10] above. Effect of the Invention
[0013] The semiconductor device of the present invention has excellent semiconductor characteristics, particularly excellent electrical characteristics. [Brief description of the drawings]
[0014] [Figure 1] FIG. 1 is a schematic diagram showing the configuration of a film forming apparatus preferably used in the present invention. [Diagram 2] FIG. 2 is a schematic diagram of a film forming apparatus (mist CVD) of another embodiment different from that of FIG. 1, which is preferably used in the present invention. [Diagram 3] FIG. 1 is a diagram illustrating a preferred example of a power supply system. [Figure 4] FIG. 1 is a diagram illustrating a preferred example of a system device. [Diagram 5] FIG. 1 is a diagram illustrating a preferred example of a power supply circuit diagram of a power supply device. [Figure 6] FIG. 1 is a diagram showing a schematic longitudinal cross-sectional view of a preferred example of a Schottky barrier diode (SBD) using a rectangular semiconductor layer. [Figure 7] FIG. 1 is a diagram showing a schematic longitudinal cross-sectional view of a preferred example of a metal oxide semiconductor field effect transistor (MOSFET) using a rectangular semiconductor layer. [Figure 8] 8 is a schematic diagram for explaining a part of a manufacturing process of the metal oxide semiconductor field effect transistor (MOSFET) of FIG. 7. [Figure 9] FIG. 1 is a diagram showing a schematic longitudinal cross-sectional view of a preferred example of an insulated gate bipolar transistor (IGBT) using a rectangular semiconductor layer. [Figure 10] FIG. 1 is a diagram showing a schematic longitudinal cross-sectional view of a preferred example of a junction barrier Schottky diode (JBS) using a rectangular semiconductor layer. [Figure 11]FIG. 1 is a diagram showing a schematic longitudinal cross-sectional view of a preferred example of a junction barrier Schottky diode (JBS) using a rectangular semiconductor layer. [Figure 12] FIG. 2 is a diagram showing a schematic diagram of a preferred example of a power card. [Figure 13] FIG. 1 is a diagram showing the results of Test Example 1. [Figure 14] FIG. 1 shows the results of Test Example 2. [Figure 15] FIG. 13 is a graph showing the results of Test Example 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The semiconductor device of the present invention is a semiconductor device having at least a semiconductor layer having a corundum structure, a first electrode arranged on a first surface side of the semiconductor layer, and a second electrode arranged on a second surface side opposite the first surface side, characterized in that the second electrode extends further in at least a first direction than the first electrode, and the first direction is the c-axis direction or m-axis direction of the semiconductor layer.
[0016] In an embodiment of the present invention, the semiconductor layer contains a metal oxide containing at least one metal selected from gallium, indium, rhodium, and iridium. In an embodiment of the present invention, the semiconductor layer is mainly composed of a metal oxide containing at least gallium, which can provide better semiconductor properties such as high breakdown voltage. The term "main component" means that the metal oxide is contained in an atomic ratio of 50% or more of the total components in the semiconductor layer, preferably 70% or more, more preferably 90% or more, and may be 100% in some embodiments. It is also preferable that the metal oxide contains at least gallium and further contains indium, rhodium, or iridium, and it is also preferable that the metal oxide contains at least gallium and further contains indium or / and aluminum. It is more preferable that the metal oxide contains at least gallium, since it can provide better properties as a power device, such as switching properties. In the present invention, it is also preferable that the first surface is a c-plane, since it can provide better electrical properties.
[0017] The semiconductor layer is a crystalline oxide semiconductor layer, and preferably contains a crystalline oxide semiconductor. The crystalline oxide semiconductor contains the metal oxide, and as described above, it is preferable that it contains at least gallium, and more preferably contains gallium oxide and its mixed crystal as a main component. The crystal structure of the crystalline oxide semiconductor is not particularly limited, but in the present invention, the crystalline oxide semiconductor preferably contains a metal oxide having a corundum structure as a main component. The metal oxide is not particularly limited, but it is preferable that it contains at least one or more metals in the fourth to sixth periods of the periodic table, more preferably contains at least gallium, indium, rhodium or iridium, and most preferably contains gallium. In the present invention, the metal oxide also preferably contains gallium and indium and / or aluminum. Examples of the metal oxide containing gallium include α-Ga2O3 or its mixed crystal. A semiconductor layer containing such a preferable metal oxide as a main component can have better crystallinity and heat dissipation, and can also have better semiconductor properties. For example, when the metal oxide is α-Ga2O3, it is sufficient that the atomic ratio of gallium contained in the semiconductor layer is 50% or more relative to the total metal components in the semiconductor layer, and α-Ga2O3 is contained in the semiconductor layer. In the present invention, the atomic ratio of gallium in the metal elements of the semiconductor layer is preferably 70% or more, more preferably 80% or more, relative to the total metal components in the semiconductor layer. The semiconductor layer may be single crystal or polycrystalline. The semiconductor layer is usually in the form of a film, but is not particularly limited as long as it does not impede the object of the present invention, and may be in the form of a plate or a sheet.
[0018] The semiconductor layer may contain a dopant. The dopant is not particularly limited as long as it does not impede the object of the present invention. It may be an n-type dopant or a p-type dopant. Examples of the n-dopant include tin, germanium, silicon, titanium, zirconium, vanadium, and niobium. The carrier concentration may be appropriately set, and specifically, for example, about 1×10 16 / cm 3 ~1×10 22 / cm 3 Alternatively, the carrier concentration may be, for example, about 1×10 17 / cm 3 In addition, as an example of the embodiment, the carrier concentration of the semiconductor layer may be set to about 1×10 20 / cm 3 Although the above-mentioned high concentration may be used, in the embodiment of the present invention, a lower carrier concentration in the semiconductor layer can make the anisotropy more effective and improve the semiconductor characteristics. For example, the carrier concentration is set to 1×10 19 / cm 3 It is preferable to set it to 5×10 or less. 18 / cm 3 It is more preferable to set it to 1×10 or less. 18 / cm 3 Most preferably, the following:
[0019] The semiconductor layer can be obtained by, for example, the following suitable film formation method: For example, a crystal substrate having a second side shorter than a first side is used, and the second electrode extends in at least a first direction beyond the first electrode, and the first direction is the c-axis direction or m-axis direction of the semiconductor layer, so that the semiconductor layer is formed by epitaxial crystal growth by a mist CVD method or a mist epitaxy method, thereby fabricating a semiconductor device.
[0020] <Crystal substrate> The crystal substrate is not particularly limited as long as it does not impede the object of the present invention, and may be a known substrate. It may be an insulating substrate, a conductive substrate, or a semiconductor substrate. It may be a single crystal substrate or a polycrystalline substrate. The crystal substrate may be, for example, a substrate containing a crystalline material having a corundum structure as a main component. The "main component" refers to a substrate containing the crystalline material in a composition ratio of 50% or more, preferably 70% or more, and more preferably 90% or more. The crystal substrate having the corundum structure may be, for example, a sapphire substrate or an α-type gallium oxide substrate.
[0021] In the present invention, the crystal substrate is preferably a sapphire substrate. Examples of the sapphire substrate include a c-plane sapphire substrate, an m-plane sapphire substrate, an a-plane sapphire substrate, and an r-plane sapphire substrate. The sapphire substrate may have an off-angle. The off-angle is not particularly limited, and is, for example, 0.01° or more, preferably 0.2° or more, and more preferably 0.2° to 12°. The sapphire substrate preferably has a crystal growth surface that is a c-plane, and is also preferably a c-plane sapphire substrate having an off-angle of 0.2° or more. The thickness of the crystal substrate is not particularly limited, but is usually from 10 μm to 20 mm, and more preferably from 10 to 1000 μm.
[0022] In the present invention, an ELO mask may be used to control the direction of crystal growth, etc., in the semiconductor layer so that the second side is shorter than the first side, the linear thermal expansion coefficient in the first crystal axis direction is smaller than the linear thermal expansion coefficient in the second crystal axis direction, the first side direction is parallel or approximately parallel to the first crystal axis direction, and the second side direction is likely to be parallel or approximately parallel to the second crystal axis direction. Suitable shapes for the crystal substrate include, for example, polygonal shapes such as triangles, quadrilaterals (eg, rectangles or trapezoids), pentagons or hexagons, U-shapes, inverted U-shapes, L-shapes and C-shapes.
[0023] In the present invention, other layers such as a buffer layer and a stress relaxation layer may be provided on the crystal substrate. The buffer layer may be a layer made of a metal oxide having the same crystal structure as the crystal substrate or the semiconductor layer. The stress relaxation layer may be an ELO mask layer.
[0024] The epitaxial crystal growth means is not particularly limited and may be any known means as long as it does not impede the object of the present invention. Examples of the epitaxial crystal growth means include CVD, MOCVD, MOVPE, mist CVD, mist epitaxy, MBE, HVPE, pulse growth, and ALD. In the present invention, the epitaxial crystal growth means is preferably mist CVD or mist epitaxy.
[0025] In the mist CVD method or mist epitaxy method, a raw material solution containing a metal is atomized (atomization process), the droplets are suspended, the resulting atomized droplets are transported to the vicinity of the crystal substrate by a carrier gas (transportation process), and then the atomized droplets are thermally reacted (film formation process).
[0026] (Raw material solution) The raw material solution contains a metal as a film-forming raw material, and is not particularly limited as long as it can be atomized, and may contain an inorganic material or an organic material. The metal may be a single metal or a metal compound, and is not particularly limited as long as it does not impede the object of the present invention. Examples of the metal include gallium (Ga), iridium (Ir), indium (In), rhodium (Rh), aluminum (Al), gold (Au), silver (Ag), platinum (Pt), copper (Cu), iron (Fe), manganese (Mn), nickel (Ni), palladium (Pd), cobalt (Co), ruthenium (Ru), chromium (Cr), molybdenum (Mo), tungsten (Tb), and the like. Examples of suitable metals include one or more metals selected from the group consisting of W, tantalum (Ta), zinc (Zn), lead (Pb), rhenium (Re), titanium (Ti), tin (Sn), magnesium (Mg), calcium (Ca) and zirconium (Zr). In the present invention, the metal preferably includes at least one or more metals from the fourth to sixth periods of the periodic table, and more preferably includes at least gallium, indium, rhodium or iridium. In the present invention, the metal preferably includes gallium and indium and / or aluminum. By using such a preferred metal, the semiconductor layer can be formed, which can be more suitably used in semiconductor devices and the like.
[0027] In the present invention, the raw material solution can be suitably used in which the metal is dissolved or dispersed in an organic solvent or water in the form of a complex or salt. Examples of the complex include acetylacetonate complexes, carbonyl complexes, ammine complexes, and hydride complexes. Examples of the salt include organic metal salts (e.g., metal acetates, metal oxalates, and metal citrates), metal sulfides, metal nitrates, metal phosphates, and metal halides (e.g., metal chlorides, metal bromides, and metal iodides).
[0028] The solvent of the raw material solution is not particularly limited as long as it does not impair the object of the present invention, and may be an inorganic solvent such as water, an organic solvent such as alcohol, or a mixed solvent of an inorganic solvent and an organic solvent. In the present invention, it is preferable that the solvent contains water.
[0029] The raw material solution may be mixed with additives such as hydrohalogenated acid and oxidizing agents. Examples of the hydrohalogenated acid include hydrobromic acid, hydrochloric acid, and hydroiodic acid. Examples of the oxidizing agent include peroxides such as hydrogen peroxide (H2O2), sodium peroxide (Na2O2), barium peroxide (BaO2), and benzoyl peroxide (C6H5CO)2O2, hypochlorous acid (HClO), perchloric acid, nitric acid, ozone water, and organic peroxides such as peracetic acid and nitrobenzene.
[0030] The raw material solution may contain a dopant. The dopant is not particularly limited as long as it does not impede the object of the present invention. Examples of the dopant include n-type dopants such as tin, germanium, silicon, titanium, zirconium, vanadium, or niobium, or p-type dopants. The concentration of the dopant is usually about 1×10 16 / cm 3 ~1×10 22 / cm 3 Alternatively, the concentration of the dopant may be, for example, about 1×10 17 / cm 3 In accordance with the present invention, the dopant may be present in a concentration as low as about 1×10 20 / cm 3 It may be contained in a concentration higher than the above.
[0031] (Atomization process) In the atomization step, a raw solution containing a metal is prepared, the raw solution is atomized, the droplets are suspended, and the atomized droplets are generated. The blending ratio of the metal is not particularly limited, but is preferably 0.0001 mol / L to 20 mol / L with respect to the whole raw solution. The atomization means is not particularly limited as long as it can atomize the raw solution, and may be a known atomization means, but in the present invention, it is preferable that it is an atomization means using ultrasonic vibration. The mist used in the present invention is one that floats in the air, and is more preferably a mist that has an initial velocity of zero and can be transported as a gas floating in space, rather than being sprayed like a spray, for example. The droplet size of the mist is not particularly limited, and may be droplets of about several mm, but is preferably 50 μm or less, more preferably 1 to 10 μm.
[0032] (Transportation process) In the transport step, the atomized droplets are transported to the substrate by the carrier gas. The type of carrier gas is not particularly limited as long as it does not impede the object of the present invention, and suitable examples include oxygen, ozone, inert gas (e.g., nitrogen, argon, etc.), and reducing gas (hydrogen gas, forming gas, etc.). The type of carrier gas may be one type, but may be two or more types, and a dilution gas (e.g., 10-fold dilution gas, etc.) with a changed carrier gas concentration may be further used as a second carrier gas. The number of supply points of the carrier gas may be not only one but also two or more. The flow rate of the carrier gas is not particularly limited, but is preferably 1 LPM or less, and more preferably 0.1 to 1 LPM.
[0033] (Film forming process) In the film-forming step, the atomized droplets are reacted to form a film on the crystal substrate. The reaction is not particularly limited as long as a film is formed from the atomized droplets, but in the present invention, a thermal reaction is preferred. The thermal reaction may be performed as long as the atomized droplets react with heat, and the reaction conditions are not particularly limited as long as the object of the present invention is not hindered. In this step, the thermal reaction is usually performed at a temperature equal to or higher than the evaporation temperature of the solvent in the raw material solution, but is preferably at a temperature not too high, more preferably 650°C or lower. In addition, the thermal reaction may be performed under any atmosphere, such as a vacuum, a non-oxygen atmosphere, a reducing gas atmosphere, or an oxygen atmosphere, as long as the object of the present invention is not hindered, and may be performed under any condition, such as atmospheric pressure, pressurized, or reduced pressure. In the present invention, the thermal reaction is preferably performed under atmospheric pressure, because the calculation of the evaporation temperature is easier and the equipment can be simplified. The film thickness can be set by adjusting the film-forming time.
[0034] Hereinafter, a film forming apparatus 19 suitable for use in the present invention will be described with reference to the drawings. The film forming apparatus 19 in Fig. 1 includes a carrier gas source 22a for supplying a carrier gas, a flow rate control valve 23a for controlling the flow rate of the carrier gas sent from the carrier gas source 22a, a carrier gas (dilution) source 22b for supplying a carrier gas (dilution), a flow rate control valve 23b for controlling the flow rate of the carrier gas (dilution) sent from the carrier gas (dilution) source 22b, a mist generating source 24 in which a raw material solution 24a is stored, a container 25 in which water 25a is stored, an ultrasonic vibrator 26 attached to the bottom surface of the container 25, a film forming chamber 30, a quartz supply pipe 27 connecting the mist generating source 24 to the film forming chamber 30, and a hot plate (heater) 28 installed in the film forming chamber 30. A substrate 20 is placed on the hot plate 28.
[0035] Then, as shown in FIG. 1, the raw solution 24a is accommodated in the mist generating source 24. Next, the substrate 20 is placed on the hot plate 28, and the hot plate 28 is operated to raise the temperature in the film forming chamber 30. Next, the flow rate control valve 23 (23a, 23b) is opened to supply the carrier gas from the carrier gas source 22 (22a, 22b) into the film forming chamber 30, and the atmosphere in the film forming chamber 30 is sufficiently replaced with the carrier gas, and then the flow rate of the carrier gas and the flow rate of the carrier gas (dilution) are adjusted. Next, the ultrasonic vibrator 26 is vibrated, and the vibration is propagated to the raw solution 24a through the water 25a, thereby atomizing the raw solution 24a to generate the mist droplets 24b. The atomized droplets 24b are introduced into the film formation chamber 30 by the carrier gas and transported to the substrate 20. The atomized droplets 24b then undergo a thermal reaction in the film formation chamber 30 under atmospheric pressure, forming a film (semiconductor layer) on the substrate 20.
[0036] It is also preferable to use a mist CVD apparatus (film forming apparatus) 19 shown in Fig. 2. The mist CVD apparatus 19 in Fig. 2 includes a susceptor 21 on which a substrate 20 is placed, a carrier gas supplying means 22a for supplying a carrier gas, a flow rate control valve 23a for controlling the flow rate of the carrier gas sent from the carrier gas supplying means 22a, a carrier gas (dilution) supplying means 22b for supplying a carrier gas (dilution), a flow rate control valve 23b for controlling the flow rate of the carrier gas sent from the carrier gas (dilution) supplying means 22b, a mist generating source 24 in which a raw material solution 24a is stored, a container 25 in which water 25a is stored, an ultrasonic vibrator 26 attached to the bottom surface of the container 25, a supply pipe 27 made of a quartz tube with an inner diameter of 40 mm, a heater 28 installed in the periphery of the supply pipe 27, and an exhaust port 29 for discharging mist, droplets, and exhaust gas after the thermal reaction. The susceptor 21 is made of quartz, and the surface on which the substrate 20 is placed is inclined from the horizontal plane. By making both the supply pipe 27, which serves as the film formation chamber, and the susceptor 21 from quartz, impurities originating from the apparatus are prevented from being mixed into the film formed on the substrate 20. This mist CVD apparatus 19 can be used in the same manner as the film formation apparatus 19 described above.
[0037] By using the suitable film formation apparatus, the semiconductor layer can be more easily formed on the crystal growth surface of the crystal substrate. The semiconductor layer is usually formed by epitaxial crystal growth.
[0038] The semiconductor layer is useful for semiconductor devices, particularly power devices. Examples of semiconductor devices formed using the crystalline oxide semiconductor include transistors such as MIS and HEMT, TFTs, Schottky barrier diodes using semiconductor-metal junctions, JBS, PN or PIN diodes combined with other P layers, and light-emitting and receiving devices. In the present invention, the crystalline oxide semiconductor can be peeled off from the crystalline substrate as desired and used in a semiconductor device. The semiconductor layer can also be disposed on a substrate having a higher thermal conductivity than the crystalline substrate.
[0039] The semiconductor device is preferably a vertical device. Suitable examples of the semiconductor device include a Schottky barrier diode (SBD), a junction barrier Schottky diode (JBS), a metal semiconductor field effect transistor (MESFET), a high electron mobility transistor (HEMT), a metal oxide semiconductor field effect transistor (MOSFET), a static induction transistor (SIT), a junction field effect transistor (JFET), an insulated gate bipolar transistor (IGBT), and a light emitting diode (LED).
[0040] Hereinafter, preferred examples of the semiconductor device including a rectangular n-type semiconductor layer (an n+ type semiconductor layer, an n- type semiconductor layer, or the like) with the main surface as the c-axis and the longitudinal direction as the m-axis will be described with reference to the drawings, but the present invention is not limited to these examples.
[0041] Fig. 6 shows an example of a Schottky barrier diode (SBD) according to the present invention. The SBD in Fig. 6 includes an n-type semiconductor layer 101a, an n+ type semiconductor layer 101b, a Schottky electrode 105a, and an ohmic electrode 105b.
[0042] The materials for the Schottky electrode and the ohmic electrode may be known electrode materials, and examples of the electrode materials include metals such as Al, Mo, Co, Zr, Sn, Nb, Fe, Cr, Ta, Ti, Au, Pt, V, Mn, Ni, Cu, Hf, W, Ir, Zn, In, Pd, Nd, and Ag, or alloys thereof; metal oxide conductive films such as tin oxide, zinc oxide, rhenium oxide, indium oxide, indium tin oxide (ITO), and indium zinc oxide (IZO); organic conductive compounds such as polyaniline, polythiophene, and polypyrrole, or mixtures and laminates thereof.
[0043] The Schottky electrode and the ohmic electrode can be formed by known means such as vacuum deposition or sputtering. More specifically, when forming a Schottky electrode using two types of metals, a first metal and a second metal, the Schottky electrode can be formed by stacking a layer made of the first metal and a layer made of the second metal, and patterning the layer made of the first metal and the layer made of the second metal using a photolithography technique.
[0044] 6, a depletion layer (not shown) spreads into n-type semiconductor layer 101a, resulting in a high-voltage SBD. When a forward bias is applied, electrons flow from ohmic electrode 105b to Schottky electrode 105a. Thus, an SBD using the above semiconductor structure is excellent for high-voltage and large-current applications, has a fast switching speed, and is excellent in voltage resistance and reliability.
[0045] (MOSFET) An example of the case where the semiconductor device of the present invention is a MOSFET is shown in Fig. 7. The MOSFET in Fig. 7 is a trench type MOSFET, and includes an n- type semiconductor layer 131a, n+ type semiconductor layers 131b and 131c, a gate insulating film 134, a gate electrode 135a, a source electrode 135b, and a drain electrode 135c.
[0046] An n+ type semiconductor layer 131b having a thickness of, for example, 100 nm to 100 μm is formed on the drain electrode 135c, and an n- type semiconductor layer 131a having a thickness of, for example, 100 nm to 100 μm is formed on the n+ type semiconductor layer 131b. Furthermore, an n+ type semiconductor layer 131c is formed on the n- type semiconductor layer 131a, and a source electrode 135b is formed on the n+ type semiconductor layer 131c.
[0047] In addition, a plurality of trenches are formed in the n-type semiconductor layer 131a and the n+ type semiconductor layer 131c, each having a depth that penetrates the n+ semiconductor layer 131c and reaches partway through the n- type semiconductor layer 131a. A gate electrode 135a is embedded in the trench via a gate insulating film 134 having a thickness of, for example, 10 nm to 1 μm.
[0048] 7, when a voltage is applied between the source electrode 135b and the drain electrode 135c and a positive voltage is applied to the gate electrode 135a with respect to the source electrode 135b, a channel layer is formed on the side surface of the n-type semiconductor layer 131a, electrons are injected into the n-type semiconductor layer 131a, and the MOSFET is turned on. When the voltage of the gate electrode is set to 0V, no channel layer is formed and the n-type semiconductor layer 131a is filled with a depletion layer, turning the MOSFET off.
[0049] Fig. 8 shows a part of the manufacturing process of the MOSFET of Fig. 7. For example, using a semiconductor structure as shown in Fig. 8(a), an etching mask is provided in a predetermined region of the n-type semiconductor layer 131a and the n+type semiconductor layer 131c, and anisotropic etching is performed by reactive ion etching or the like using the etching mask as a mask to form a trench groove having a depth reaching from the surface of the n+type semiconductor layer 131c to the middle of the n-type semiconductor layer 131a as shown in Fig. 8(b). Next, as shown in Fig. 8(c), a gate insulating film 134 having a thickness of, for example, 50 nm to 1 μm is formed on the side and bottom of the trench groove by a known means such as thermal oxidation, vacuum deposition, sputtering, or CVD, and then a gate electrode material 135a such as polysilicon is formed in the trench groove to a thickness equal to or less than the thickness of the n-type semiconductor layer by CVD, vacuum deposition, sputtering, or the like.
[0050] Then, by using known means such as vacuum deposition, sputtering, CVD, etc., the source electrode 135b is formed on the n+ type semiconductor layer 131c, and the drain electrode 135c is formed on the n+ type semiconductor layer 131b, respectively, to manufacture a power MOSFET. The electrode materials of the source electrode and the drain electrode may be known electrode materials, and examples of the electrode materials include metals such as Al, Mo, Co, Zr, Sn, Nb, Fe, Cr, Ta, Ti, Au, Pt, V, Mn, Ni, Cu, Hf, W, Ir, Zn, In, Pd, Nd, Ag, etc., or alloys thereof, metal oxide conductive films such as tin oxide, zinc oxide, indium oxide, indium tin oxide (ITO), indium zinc oxide (IZO), etc., organic conductive compounds such as polyaniline, polythiophene, or polypyrrole, or mixtures thereof.
[0051] The MOSFET obtained in this way has a higher breakdown voltage than the conventional trench MOSFET. Although Fig. 7 shows an example of a trench vertical MOSFET, the present invention is not limited to this and can be applied to various MOSFET configurations. For example, the depth of the trench groove in Fig. 7 may be deepened to a depth reaching the bottom surface of the n-type semiconductor layer 131a to reduce the series resistance.
[0052] (IGBT) FIG. 9 shows a preferred example of an insulated gate bipolar transistor (IGBT) including an n-type semiconductor layer 151, an n-type semiconductor layer 151a, an n+ type semiconductor layer 151b, a p-type semiconductor layer 152, a gate insulating film 154, a gate electrode 155a, an emitter electrode 155b, and a collector electrode 155c.
[0053] FIG. 10 shows a junction barrier Schottky diode (JBS) according to a preferred embodiment of the present invention. The semiconductor device of FIG. 10 includes a semiconductor region (semiconductor layer) 3, a barrier electrode 2 provided on the semiconductor region and capable of forming a Schottky barrier between the semiconductor region and the barrier electrode 2, and a barrier height adjustment layer provided between the barrier electrode 2 and the semiconductor region 3 and capable of forming a Schottky barrier with a barrier height greater than the barrier height of the Schottky barrier of the barrier electrode 2 between the semiconductor region 3. The barrier height adjustment layer 1 is embedded in the semiconductor region 3. In the present invention, it is preferable that the barrier height adjustment layers are provided at regular intervals, and it is more preferable that the barrier height adjustment regions are provided between both ends of the barrier electrode and the semiconductor region. With this preferred embodiment, the JBS is configured to have better thermal stability and adhesion, a greater reduction in leakage current, and better semiconductor characteristics such as breakdown voltage. The semiconductor device of FIG. 10 includes an ohmic electrode 4 on the semiconductor region 3.
[0054] The means for forming each layer of the semiconductor device in Fig. 10 is not particularly limited as long as it does not impede the object of the present invention, and may be any known means, such as a means for forming a film by a vacuum deposition method, a CVD method, a sputtering method, various coating techniques, etc., followed by patterning by a photolithography method, or a means for directly patterning by a printing technique, etc.
[0055] FIG. 11 shows a junction barrier Schottky diode (JBS) which is one of the preferred embodiments of the present invention. The semiconductor device in FIG. 11 differs from the semiconductor device in FIG. 10 in that a guard ring 5 is provided on the outer periphery of the barrier electrode. This configuration makes it possible to obtain a semiconductor device with better semiconductor characteristics such as breakdown voltage. In the present invention, the breakdown voltage can be improved more effectively by embedding a part of the guard ring 5 in the surface of the semiconductor region (semiconductor layer) 3. Furthermore, by using a metal with a high barrier height for the guard ring, the guard ring can be provided industrially advantageously together with the formation of the barrier electrode, and can be formed without significantly affecting the semiconductor region or deteriorating the on-resistance.
[0056] The guard ring is usually made of a material with a high barrier height. Examples of the material used for the guard ring include conductive materials with a barrier height of 1 eV or more, and may be the same as the electrode material. In the present invention, the material used for the guard ring is preferably the metal, since it has a high degree of freedom in designing the pressure-resistant structure, can provide many guard rings, and can flexibly improve the pressure resistance. The shape of the guard ring is not particularly limited, and examples include a square shape, a circular shape, a U-shape, an L-shape, and a strip shape. The number of guard rings is not particularly limited, but is preferably 3 or more, more preferably 6 or more.
[0057] In addition to the above, the semiconductor device of the present invention can be suitably used as a power module, inverter, or converter by using a known method, and can also be suitably used in a semiconductor system using a power supply device. The power supply device can be manufactured from the semiconductor device or as the semiconductor device by connecting to a wiring pattern or the like in a normal manner. FIG. 3 shows a power supply system 170 using a plurality of the power supply devices 171 and 172 and a control circuit 173. The power supply system can be used in a system device 180 by combining an electronic circuit 181 and a power supply system 182 as shown in FIG. 4. An example of a power supply circuit diagram of a power supply device is shown in FIG. 5. FIG. 5 shows a power supply circuit of a power supply device consisting of a power circuit and a control circuit, in which a DC voltage is switched at a high frequency by an inverter 192 (composed of MOSFETs A to D) and converted to AC, then insulated and transformed by a transformer 193, rectified by a rectifier MOSFET 194 (A to B'), smoothed by a DCL 195 (smoothing coils L1, L2) and a capacitor, and a DC voltage is output. At this time, a voltage comparator 197 compares the output voltage with a reference voltage, and a PWM control circuit 196 controls an inverter 192 and a rectifying MOSFET 194 so as to obtain a desired output voltage.
[0058] In the present invention, the semiconductor device is preferably a power card, and includes a cooler and an insulating member. More preferably, the cooler is provided on both sides of the semiconductor layer via at least the insulating member, and most preferably, a heat dissipation layer is provided on both sides of the semiconductor layer, and the cooler is provided on the outside of the heat dissipation layer via at least the insulating member. FIG. 12 shows a power card according to a preferred embodiment of the present invention. The power card in FIG. 12 is a double-sided cooling type power card 201, and includes a refrigerant tube 202, a spacer 203, an insulating plate (insulating spacer) 208, a sealing resin part 209, a semiconductor chip 301a, a metal heat transfer plate (protruding terminal part) 302b, a heat sink and electrode 303, a metal heat transfer plate (protruding terminal part) 303b, a solder layer 304, a control electrode terminal 305, and a bonding wire 308. The thickness direction cross section of the refrigerant tube 202 has many flow paths 222 partitioned by many partition walls 221 extending in the flow path direction at a predetermined interval from each other. Such a suitable power card can realize higher heat dissipation and can satisfy higher reliability.
[0059] The semiconductor chip 301a is joined to the inner main surface of the metal heat transfer plate 302b with a solder layer 104, and the metal heat transfer plate (protruding terminal portion) 302b is joined to the remaining main surface of the semiconductor chip 301a with a solder layer 304, so that the anode electrode surface and the cathode electrode surface of the flywheel diode are connected in so-called anti-parallel to the collector electrode surface and the emitter electrode surface of the IGBT. Examples of materials for the metal heat transfer plates (protruding terminal portions) 302b and 303b include Mo and W. The metal heat transfer plates (protruding terminal portions) 302 and 303b have a thickness difference that absorbs the thickness difference of the semiconductor chips 101a and 101b, and as a result, the outer surface of the metal heat transfer plate 102 is flat.
[0060] Resin sealing portion 209 is made of, for example, epoxy resin, and is molded to cover the side surfaces of metal heat transfer plates 302b and 303b, and semiconductor chip 301a is molded with resin sealing portion 209. However, the outer main surfaces, i.e., the contact heat receiving surfaces, of metal heat transfer plates 302b and 303b are completely exposed. Metal heat transfer plates (protruding terminal portions) 302b and 303b protrude from resin sealing portion 209 to the right in Fig. 12, and control electrode terminal 305, which is a so-called lead frame terminal, connects, for example, the gate (control) electrode surface of semiconductor chip 301a on which an IGBT is formed to control electrode terminal 305.
[0061] The insulating plate 208, which is an insulating spacer, is made of, for example, an aluminum nitride film, but may be another insulating film. The insulating plate 208 completely covers and adheres to the metal heat transfer plates 302b and 303b, but the insulating plate 208 and the metal heat transfer plates 302b and 303b may simply be in contact with each other, or may be coated with a good heat transfer material such as silicon grease, or may be joined by various methods. Also, an insulating layer may be formed by ceramic spraying, or the insulating plate 208 may be joined to the metal heat transfer plate, or may be joined or formed on the refrigerant tube.
[0062] The refrigerant tubes 202 are made by cutting a plate material formed by pultrusion or extrusion of an aluminum alloy to a required length. The thickness direction cross section of the refrigerant tubes 202 has many flow paths 222 partitioned by many partition walls 221 extending in the flow path direction at a predetermined interval from each other. The spacer 203 may be, for example, a soft metal plate such as a solder alloy, or may be a film formed by coating or the like on the contact surface of the metal heat transfer plates 302b and 303b. The surface of this soft spacer 3 easily deforms and fits the minute unevenness and warping of the insulating plate 208 and the minute unevenness and warping of the refrigerant tubes 202 to reduce thermal resistance. Note that a known good thermal conductive grease or the like may be applied to the surface of the spacer 203, or the spacer 203 may be omitted.
[0063] (Test Examples 1 to 3) Using the mist CVD method, m-plane αGa2O3 semiconductor films and c-plane αGa2O3 semiconductor films were formed, and the relationship between electrical resistivity and carrier concentration × mobility (conductivity) was analyzed using a terahertz spectrometer (a general-purpose terahertz spectrometer manufactured by Nippo Precision Co., Ltd., "TeraProspector (registered trademark, trademark registration number 5550188)" (2019)). The anisotropy of the c-axis and a-axis was evaluated. The results are shown in Figure 13 (Test Example 1) and Figure 14 (Test Example 2). As is clear from Figures 13 and 14, anisotropy in which the resistivity is lower in the c-axis direction was confirmed, and further, anisotropy in which the resistivity is slightly lower in the m-axis direction was confirmed. In addition, when the carrier concentration of each sample in Test Example 1 was examined using a Hall effect measurement device, the results shown in Figure 15 (Test Example 3) were obtained, and it was found that the lower the carrier concentration, the greater the anisotropy. [Industrial Applicability]
[0064] The semiconductor device of the present invention can be used in a wide variety of fields, including semiconductors (eg, compound semiconductor electronic devices), electronic components, electrical equipment components, optical and electrophotographic related devices, and industrial materials, but is particularly useful as power devices. [Explanation of symbols]
[0065] 1. Barrier height adjustment layer 2 Barrier Electrode 3. Semiconductor region (semiconductor layer) 4 Ohmic electrodes 5 Guard Ring 19 Mist device (film forming device) 20 Substrate 21 Susceptor 22a Carrier gas supply means 22b Carrier gas (dilution) supply means 23a Flow control valve 23b Flow control valve 24 Mist Source 24a Raw material solution 25 Container 25a water 26 Ultrasonic transducer 27 Supply pipe 28 Heater 29 Exhaust port 30 Deposition chamber 101a n-type semiconductor layer 101b n+ type semiconductor layer 105a Schottky electrode 105b Ohmic electrode 131a n-type semiconductor layer 131b First n+ type semiconductor layer 131c second n+ type semiconductor layer 134 Gate insulating film 135a Gate electrode 135b Source electrode 135c Drain electrode 141a n-type semiconductor layer 141b First n+ type semiconductor layer 141c second n+ type semiconductor layer 145a Gate electrode 145b Source electrode 145c Drain electrode 151 n-type semiconductor layer 151a n-type semiconductor layer 151b n+ type semiconductor layer 152 p-type semiconductor layer 154 Gate insulating film 155a Gate electrode 155b Emitter electrode 155c Collector electrode 170 Power System 171 Power supply 172 Power supply 173 Control circuit 180 System Unit 181 Electronic circuit 182 Power System 192 Inverter 193 Trans 194 Rectifier MOSFET 195 DCL 196 PWM control circuit 197 Voltage Comparator 201 Double-sided cooled power card 202 Refrigerant tube 203 Spacer 208 Insulating plate (insulating spacer) 209 Sealing resin part 221 Bulkhead 222 Channel 301a Semiconductor chip 302b Metal heat transfer plate (protruding terminal part) 303 Heat sink and electrodes 303b Metal heat transfer plate (protruding terminal part) 304 solder layer 305 Control electrode terminal 308 Bonding Wire
Claims
1. A semiconductor device having at least a semiconductor layer having a corundum structure, a first electrode arranged on a first surface side of the semiconductor layer, and a second electrode arranged on a second surface side opposite to the first surface side, wherein the second electrode extends further in at least a first direction than the first electrode, the first direction is a c-axis direction of the semiconductor layer, and the carrier concentration of the semiconductor layer is 1 x 1019 / cm3 or less.
2. 2. The semiconductor device according to claim 1, wherein the semiconductor layer contains a metal oxide containing at least one metal selected from the group consisting of gallium, indium, rhodium and iridium.
3. 2. The semiconductor device according to claim 1, wherein the semiconductor layer is mainly composed of a metal oxide containing at least gallium.
4. 4. The semiconductor device according to claim 1, which is a power device.
5. 5. The semiconductor device according to claim 4, which is a power module, an inverter or a converter.
6. 5. The semiconductor device according to claim 4, which is a power card.
7. 7. The semiconductor device according to claim 6, further comprising a cooler and an insulating member, said cooler being provided on both sides of said semiconductor layer with at least said insulating member interposed therebetween.
8. 8. The semiconductor device according to claim 7, further comprising a heat dissipation layer provided on each side of said semiconductor layer, and said coolers being provided on the outer sides of said heat dissipation layers with at least said insulating member interposed therebetween.
9. A semiconductor system comprising a semiconductor device, the semiconductor device being the semiconductor device according to any one of claims 1 to 8.
Citation Information
Patent Citations
Fitting structure of pipe body
JP1978043224A
Crystal vibrator
JP1978097794A
Electrode forming method of piezoelectric vibrator