Raw material for composite material, its manufacturing method, and composite material
By forming a coating layer on particles within a resin dispersion medium through mechanical treatment, the method addresses the challenges of particle agglomeration and complex synthesis, resulting in composite materials with superior tensile strength and mechanical properties.
Patent Information
- Application Number
- JP2020147460
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-09-02
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2040-09-02
AI Technical Summary
Existing methods for producing particle-dispersed composite materials face challenges in achieving improved tensile strength due to particle agglomeration during drying and the complexity of synthesizing special graft polymers, which complicates the manufacturing process and reduces the effectiveness of the composite material's mechanical properties.
A method involving a dispersion medium containing resin and particles, where a coating layer is formed on the particle surface through mechanical treatment, eliminating the need for drying and special polymer synthesis, and enhancing adhesion and dispersibility by applying a shear force to the mixture.
This approach allows for the production of composite materials with improved tensile strength by ensuring high affinity between the resin and particles, resulting in enhanced mechanical properties without the need for additional surface modification steps.
Smart Images

Figure 0007595335000004 
Figure 0007595335000005 
Figure 0007595335000006
Abstract
Description
[Technical field]
[0001] The present invention relates to a raw material for a composite material, a method for producing the same, and a composite material. [Background technology]
[0002] Particle-dispersed composite materials, in which particles as reinforcing materials are dispersed in a resin as a base material, have been attracting attention in recent years because they may be able to simultaneously exhibit the excellent properties of both materials. Since this type of composite material is made up of a combination of resin and particles, it is important to improve the affinity between the resin and the particles and to uniformly disperse the particles in the resin. Previously, efforts have been made to improve the mechanical properties of composite materials, such as the tensile strength, by improving the affinity between the resin and the particles to improve the adhesion between them, or by improving the dispersibility of the particles in the resin by modifying the resin or particles.
[0003] Surface modification of particles by chemical reaction is widely used as a method for improving the adhesion between resin and particles in composite materials. For example, Patent Document 1 discloses a technology relating to a resin composition obtained by modifying the surface of a spherical substrate with a silane coupling agent, drying the modified surface, and dispersing the modified surface in a resin, and a resin molded product obtained by molding the modified surface. Patent Document 2 discloses a technology relating to a nanocomposite obtained by synthesizing a graft polymer having a graft chain with a specific functional group and dispersing nanoparticles in the graft polymer in order to uniformly disperse particles in a resin. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] WO2018 / 043246 publication [Patent Document 2] JP 2006-307199 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, the technique of Patent Document 1 requires drying the particles after modification with the silane coupling agent, which may lead to particle aggregation due to drying. The aggregated particles may lead to a decrease in the strength of the composite material. In addition, the technique of Patent Document 2 requires the advance synthesis of a special graft polymer to improve particle dispersion, which may complicate the manufacturing process of the raw material for the composite material. In addition, these techniques also require a separate process for uniformly dispersing the particles in the resin. Therefore, the conventional techniques make it difficult to relatively easily manufacture the raw material for the composite material that can obtain a composite material with improved tensile strength. As a result, it is also difficult to obtain a composite material with improved tensile strength using the raw material for the composite material.
[0006] The present invention has been made in consideration of such problems, and aims to provide a method for producing raw materials for composite materials that can relatively easily produce raw materials for composite materials from which composite materials with improved tensile strength can be obtained, raw materials for composite materials from which composite materials with improved tensile strength can be obtained, and composite materials with improved tensile strength. [Means for solving the problem]
[0007] One aspect of the present invention is A particle-reinforced composite material in which particles are dispersed as reinforcing material in a resin matrix. (However, this does not include the case where the particles as the reinforcing material are oriented in the resin as the base material.) A raw material for a composite material used in The base material of the composite material the above At least one of a resin and a resin component that is a component for constituting the resin that is the base material of the composite material (however, excluding a chain aliphatic epoxy resin having a hydrophilic group, a resin having a fluorene skeleton, and rubber latex). and a solvent A dispersion medium comprising A plurality of particles (including cellulose) dispersed in the dispersion medium. , a granular adsorbent filler in which a thermoplastic resin is adsorbed on a filler, and a nanoparticle in which one or more oligomers derived from two or more polymerizable units are covalently bonded via a coupling agent. ) and a coating layer covering the surface of the particle, The coating layer is derived from at least one of the resin and the resin component contained in the dispersion medium. , adsorbed on the surface of the particle Formed from resin-derived components And, The coating layer is formed by applying a shear force to a mixture containing the dispersion medium and the particles. , as a raw material for composite materials.
[0008] Another aspect of the present invention is A particle-reinforced composite material in which particles are dispersed as reinforcing material in a resin matrix. (However, this does not include the case where the particles as the reinforcing material are oriented in the resin as the base material.) A method for producing a raw material for a composite material used in above The composite material above The base material the above Resin and above The composite material above The base material above At least one of the resin components that are components for constituting the resin (however, excluding linear aliphatic epoxy resins having a hydrophilic group, resins having a fluorene skeleton, and rubber latex). and a solvent A dispersion medium containing a plurality of particles (including cellulose) mixed in the dispersion medium. , a granular adsorbent filler in which a thermoplastic resin is adsorbed on a filler, and a nanoparticle in which one or more oligomers derived from two or more polymerizable units are covalently bonded via a coupling agent. (excluding ). The prepared mixture is subjected to a mechanical treatment in which a shear force is applied to disperse a plurality of the particles in the dispersion medium, and a surface of the particles is coated with a polymer derived from at least one of the resin and the resin component contained in the dispersion medium. , adsorbed on the surface of the particle a mechanical treatment step of coating the surface with a coating layer formed from a resin-derived component; The present invention relates to a method for producing a raw material for a composite material, comprising the steps of:
[0009] Yet another aspect of the present invention is a composite material formed using the above-mentioned composite material raw material. Effect of the Invention
[0010] The method for producing the raw material for composite material has the above steps. Therefore, according to the method for producing the raw material for composite material, dispersion of particles in a dispersion medium containing at least one of a resin and a resin component, and surface coating of the particle surface with a resin-derived component derived from at least one of the resin and the resin component contained in the dispersion medium can be performed in one step. In addition, the method for producing the raw material for composite material does not necessarily require pretreatment of the particles with a surface modifier, and does not require synthesis of a special resin in advance. Therefore, the method for producing the raw material for composite material can produce the raw material for composite material relatively easily compared to conventional production methods.
[0011] The composite material raw material has the above-mentioned configuration. The composite material raw material can be obtained by the manufacturing method of the composite material raw material. The composite material molded using the composite material raw material can exhibit a high tensile strength compared to a reference composite material molded using a reference raw material to which particles are first mixed in a resin-free dispersion medium that does not contain resin and resin components, and then mechanically treated and then resin or resin components are added. This is thought to be due to the fact that in the composite material raw material, the resin or resin component and the coating layer are of the same resin system, so that the affinity is high, the adhesion between the particles and the coating layer is improved, and the particles have high dispersibility.
[0012] Therefore, according to the present invention, it is possible to provide a manufacturing method for a composite material raw material that can relatively easily produce a composite material raw material from which a composite material with improved tensile strength can be obtained, the composite material raw material from which a composite material with improved tensile strength can be obtained, and a composite material with improved tensile strength. [Brief description of the drawings]
[0013] [Figure 1] FIG. 1 is an explanatory diagram that illustrates a composite material raw material of the present embodiment. [Diagram 2]FIG. 2 is an explanatory diagram that shows a schematic diagram of the manufacturing method of the composite material raw material of this embodiment, where (a) is an explanatory diagram that shows a schematic diagram of the mixture prepared in the preparation step, and (b) is an explanatory diagram that shows a schematic diagram of the composite material raw material obtained through the mechanical treatment step. [Diagram 3] FIG. 3 is an explanatory diagram for explaining the mechanical treatment in the mechanical treatment step of the method for producing a raw material for a composite material of this embodiment. [Figure 4] FIG. 4 is an explanatory diagram showing details of a nozzle member provided in a dispersion nozzle section of a wet jet mill used in an experimental example, where (a) is a cross-sectional view of the nozzle member, (b) is an arrow view taken along line IVb-IVb in (a), (c) is an arrow view taken along line IVc-IVc in (a), (d) is an arrow view taken along line IVd-IVd in (a), and (e) is an arrow view taken along line IVe-IVe in (c). [Diagram 5] FIG. 5 is a scanning electron microscope photograph of a fracture surface after a tensile test on a composite material molded using the composite material raw material of Sample 1-1 obtained in an experimental example. [Figure 6] FIG. 6 is a scanning electron microscope photograph of a fracture surface after a tensile test on a composite material molded using the composite material raw material of Sample 1R obtained in an experimental example. [Figure 7] FIG. 7 shows an infrared spectrum of the epoxy base resin obtained by an infrared spectrophotometer in an experimental example. [Figure 8] FIG. 8 shows infrared spectra obtained with an infrared spectrophotometer in the experimental examples of the aluminum oxide powder itself, the aluminum oxide powders recovered from the composite material raw materials of Sample 1-1 and Sample 1-2, and the aluminum oxide powder recovered from the reference raw material of Sample 1R. [Figure 9] FIG. 9 shows infrared spectra obtained by an infrared spectrophotometer in the experimental example of the silicon dioxide powder itself, the silicon dioxide powder recovered from the composite material raw material of sample 2, and the silicon dioxide powder recovered from the reference raw material of sample 2R. [Figure 10] FIG. 10 is an enlarged view of the infrared spectrum shown in FIG. [Figure 11]FIG. 11 shows infrared spectra obtained with an infrared spectrophotometer in an experimental example of the magnesium oxide powder itself, the magnesium oxide powder recovered from the composite material raw material of sample 3, and the magnesium oxide powder recovered from the reference raw material of sample 3R. [Figure 12] FIG. 12 is a graph showing the relationship between the particle size (nm) and the accumulation (volume %) or frequency (volume %) before and after the mechanical treatment in the preparation of the composite material raw material of Sample 1-1. [Figure 13] FIG. 13 is a graph showing the relationship between the particle size (nm) and the accumulation (volume %) or frequency (volume %) before and after the mechanical treatment in the preparation of the composite material raw material of Sample 1-2. [Figure 14] FIG. 14 is a graph showing the relationship between the particle size (nm) and the accumulation (volume %) or frequency (volume %) before and after the mechanical treatment in the preparation of the composite material raw material of Sample 2. [Figure 15] FIG. 15 is a graph showing the relationship between the particle size (nm) and the accumulation (volume %) or frequency (volume %) before and after the mechanical treatment in the preparation of the composite material raw material of Sample 3. [Figure 16] FIG. 16 is a graph showing the relationship between the particle size (nm) and the accumulation (volume %) or frequency (volume %) before and after the mechanical treatment in the preparation of the composite material raw material of Sample 1R. [Figure 17] FIG. 17 is a graph showing the relationship between the particle size (nm) and the accumulation (volume %) or frequency (volume %) before and after the mechanical treatment in the preparation of the composite material raw material of sample 2R. [Figure 18] FIG. 18 is a graph showing the relationship between the particle size (nm) and the accumulation (volume %) or frequency (volume %) before and after the mechanical treatment in the preparation of the composite material raw material of sample 3R. [Figure 19] FIG. 19 is a diagram showing the relationship between particle size (nm) and accumulation (volume %) in the composite material raw materials of Samples 1-1C to 1-3C. [Figure 20] FIG. 20 is a diagram showing the relationship between particle size (nm) and frequency (volume %) in the composite material raw materials of Samples 1-1C to 1-3C. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The raw material for a composite material, the method for producing the raw material for a composite material, and the composite material of the present embodiment will be described in detail with reference to FIGS. 1 to 3. FIG.
[0015] (Raw material for composite materials) As illustrated in FIG. 1, the composite material raw material 1 of this embodiment includes a dispersion medium 10, a plurality of particles 11, and a coating layer 12.
[0016] The dispersion medium 10 contains at least one of a resin 101 and a resin component 102. The resin 101 contained in the dispersion medium 10 is a base material (matrix) of the composite material. Examples of the resin 101 include curable resins such as thermosetting resins and ultraviolet curable resins, and thermoplastic resins. These can be used alone or in combination of two or more. The resin component 102 contained in the dispersion medium 10 is a component for constituting the resin 101 that is a base material of the composite material, and specifically includes monomers, oligomers, prepolymers, and the like. These can be used alone or in combination of two or more. In addition, among the above-mentioned resins 101, the curable resin may be composed of a base agent and a curing agent (including a curing accelerator). The base agent and curing agent for constituting the curable resin are included in the concept of the resin component.
[0017] minutes The dispersion medium 10 contains, in addition to the resin 101 and the resin component 102, a solvent 103 (which may also be called a diluent) such as an aqueous solvent or an organic solvent. nothing. More specifically, when the resin 101 or the resin component 102 used is liquid, the dispersion medium 10 is , tree The dispersion medium 10 can be composed of the resin 101 or the resin component 102 and the solvent 103. When the resin 101 or the resin component 102 used is solid, the dispersion medium 10 can be composed of the resin 101 or the resin component 102 and the solvent 103. That is, in this case, the solid resin 101 or the resin component 102 is dissolved in the solvent 103. From the viewpoint of improving the dispersibility of the particles 11, the dispersion medium 10 preferably contains the solvent 103. do. Solvent 103 may be used alone or in combination of two or more kinds. The type of solvent 103 may be appropriately selected depending on the type of resin 101 and resin component 102 used. The aqueous solvent as solvent 103 may contain ions for adjusting pH or ionic strength.
[0018] Examples of the resin 101 include thermosetting resins such as epoxy resin, phenol resin, melamine resin, urea resin, unsaturated polyester resin, alkyd resin, oxazine resin, bismaleimide resin, and triazine resin, and thermoplastic resins such as polyamide, polyester, polycarbonate, acrylic polymer, methacrylic polymer, polyimide, liquid crystal polymer, polyolefin, polystyrene, and polyphenylene ether.
[0019] Examples of the resin component 102 include a base material of an epoxy resin, a hardener of an epoxy resin, a phenolic compound, melamine, urea, styrene, a fatty acid, benzoxazine, epsilon caprolactam, etc. The above-mentioned resin 101 and resin component 102 can be used alone or in combination of two or more kinds.
[0020] A plurality of particles 11 are dispersed in a dispersion medium 10. Examples of the shape of the particles 11 include spherical shapes such as perfect spheres, elliptical spheres, oval spheres, and chunky spheres, and shapes in which the length in the long axis direction differs from the length in the short axis direction, such as plate-like, scaly, rod-like, needle-like, and fibrous shapes. These shapes can be used alone or in combination of two or more kinds.
[0021] The particles 11 can be made of any material as long as it can improve at least the tensile strength of the mechanical properties of the composite material. Examples of the particles 11 include ceramic particles, metal particles, carbon particles, and organic particles. These can be used alone or in combination of two or more kinds. This configuration makes it easy to improve the tensile strength of the composite material.
[0022] Examples of ceramics constituting the ceramic particles include aluminum oxide (alumina), zinc oxide, magnesium oxide, silicon oxide, titanium oxide, beryllium oxide, boron nitride, aluminum nitride, silicon nitride, silicon carbide, aluminum hydroxide, magnesium hydroxide, zirconium oxide (zirconia), yttrium oxide (yttria), etc. These can be used alone or in combination of two or more.
[0023] Examples of metals constituting the metal particles include gold, silver, copper, platinum group metals, and alloys thereof, etc. These can be used alone or in combination of two or more kinds.
[0024] Examples of carbon constituting the carbon particles include carbon black, diamond, graphite, carbon nanotubes, carbon nanofibers, fullerenes, pulverized carbon fibers (milled fibers), etc. These can be used alone or in combination of two or more.
[0025] Examples of the organic matter constituting the organic particles include cellulose, chitosan, chitin, etc. These can be used alone or in combination of two or more kinds.
[0026] The coating layer 12 covers the surface of each particle 11. The coating layer 12 may cover the entire surface of the particle 11, or may cover a part of the surface of the particle 11. Here, the coating layer 12 is formed from a resin-derived component derived from at least one of the resin 101 and the resin component 102 contained in the dispersion medium 10. In other words, the coating layer 12 is formed from a part of the resin 101 and the resin component 102 contained in the dispersion medium 10. Specifically, the resin-derived component may be the same as at least one of the resin 101 and the resin component 102 contained in the dispersion medium 10, or may have a molecular structure that is partially different from that of at least one of the resin 101 and the resin component 102 contained in the dispersion medium 10 due to a chemical reaction with the particle surface, etc.
[0027] The resin-derived component may be configured to be adsorbed onto the surface of the particle 11. This configuration increases the adhesion between the particle 11 and the coating layer 12, ensuring an improvement in the tensile strength of the composite material. The adsorption may be either chemical adsorption or physical adsorption. Chemical adsorption is advantageous for improving the adhesion of the coating layer 12 by covalent bonding between the surface of the particle 11 and the resin-derived component.
[0028] The adsorption of the resin-derived component to the particle 11 surface can be confirmed by the following example. A plurality of particles 11 whose surfaces are covered with the coating layer 12 are collected from the composite material raw material 1 by centrifugation, filtration, or the like. Next, the collected plurality of particles 11 are thoroughly washed with a solvent in which the resin 101 and the resin component 102 dissolve in order to remove unnecessary components such as unadsorbed components, and are vacuum-dried to obtain a powder. Next, an infrared spectrum is obtained for the dried powder by a diffuse reflectance method using an infrared spectrophotometer. Next, the presence or absence of peaks derived from the resin and the resin component in the obtained infrared spectrum is observed. If a peak derived from the resin and the resin component is observed, it can be determined that at least a part of the resin 101 and the resin component 102 contained in the dispersion medium 10 is adsorbed to the surface of the particle 11. On the other hand, if a peak derived from the resin and the resin component is not observed, it can be determined that at least a part of the resin 101 and the resin component 102 contained in the dispersion medium 10 is not adsorbed to the surface of the particle 11.
[0029] In the present disclosure, the reference raw material is a raw material for a composite material prepared by using a dispersion medium that does not contain the resin 101 or resin component 102 contained in the coating layer 12 of the particle 11 instead of the dispersion medium 10 used in the raw material for a composite material 1. The coating ratio, which is defined as the ratio of the coating amount of the coating layer 12 covering the surface of the particle 11 in the raw material for a composite material 1 to the coating amount of the coating layer covering the surface of the particle in the reference raw material, can be 1.3 times or more. Note that the coating amount of the coating layer 12 can be said to be the adsorption amount of the resin-derived component on the surface of the particle 11 when the resin-derived component is adsorbed on the surface of the particle 11. In addition, the above-mentioned coating ratio can be, for example, 20.0 times or less from the viewpoint that if the coating ratio is too large, the apparent particle diameter becomes large and the maximum filling amount of the particle decreases.
[0030] The reference raw material is prepared as follows. Specifically, the type of particle 11 in the raw material 1 for composite material and the type of resin 101 or resin component 102 that is the source of the resin-derived component that forms the coating layer 12 that covers the surface of the particle 11 are identified. For the identification, a measurement method such as powder X-ray diffraction measurement, energy dispersive X-ray spectrometry, Fourier transform infrared spectrometry, Raman spectrometry, etc. can be used. A resin-free mixture containing a resin-free dispersion medium that does not contain the resin 101 and the resin component 102 and a plurality of particles 11 is prepared. After subjecting the prepared resin-free mixture to a mechanical treatment using a wet jet mill, the same resin 101 or resin component 102 as that specified above is mixed so that the volume ratio of the plurality of particles 11 is the same as that of the raw material 1 for composite material. The conditions for the mechanical treatment using the wet jet mill are: diameter of the small hole of the dispersion nozzle part of the wet jet mill: 0.17 mm, pressure: 200 MPa, and number of mechanical treatments: 5 times. The resin-containing mixture obtained in this manner is used as the reference raw material.
[0031] The amount of the coating layer 12 can be measured as follows. A plurality of particles 11 whose surfaces are covered with the coating layer 12 are collected from the raw material 1 for composite material by centrifugation, filtration, or the like. Next, the collected particles 11 are thoroughly washed with a solvent in which the resin 101 and the resin component 102 dissolve in order to remove unnecessary components such as unadsorbed components, and are vacuum-dried to obtain a powder. Next, the mass reduction rate of the dried powder is measured from 150°C to 600°C at a heating rate of 10°C / min using a thermogravimetric differential thermal analyzer. The mass reduction rate (mass%) can be calculated by the formula 100×(mass at 150°C-mass at 600°C) / (initial mass<mass at room temperature). The mass reduction rate obtained above is taken as the amount of the coating layer 12 on each particle 11. That is, the amount of the coating layer 12 is the mass% of the coating layer 12 relative to the particles 11 coated with the coating layer 12, as measured by thermogravimetric differential thermal analysis. The reference raw material can also be measured in the same manner.
[0032] Specifically, for example, when the particle 11 is made of aluminum oxide, the coating amount of the coating layer 12 can be preferably 0.25% by mass or more, more preferably 0.50% by mass or more, even more preferably 0.75% by mass or more, even more preferably 1.00% by mass or more, even more preferably 1.25% by mass or more, and most preferably 1.50% by mass or more. Also, for example, when the particle 11 is made of silicon dioxide, the coating amount of the coating layer 12 can be preferably 1.20% by mass or more, more preferably 1.30% by mass or more, and even more preferably 1.40% by mass or more. Also, for example, when the particle 11 is made of magnesium oxide, the coating amount of the coating layer 12 can be preferably 2.20% by mass or more, more preferably 2.40% by mass or more, even more preferably 2.60% by mass or more, even more preferably 2.80% by mass or more, and even more preferably 3.00% by mass or more. In addition, when the particles 11 are made of aluminum oxide, when the particles 11 are made of silicon dioxide, and when the particles 11 are made of magnesium oxide, the amount of coating layer 12 can be 10.00 mass % or less. If the amount of coating layer 12 is too large, the apparent particle size becomes large, and the maximum packing amount of the particles 11 decreases.
[0033] At least one of the resin 101 and the resin component 102 can have a reactive functional group in its molecular structure that reacts with the surface of the particle 11. The functional group may be one type or two or more types in the molecular structure. According to this configuration, a covalent bond can be formed between the surface of the particle 11 and the resin-derived component via the functional group contained in the resin-derived component. Therefore, according to this configuration, the adhesion between the particle 11 and the coating layer 12 is increased, which is advantageous for improving the tensile strength of the composite material.
[0034] At least one of the resin and the resin component may have, in its molecular structure, a functional group such as a hydroxyl group, an aldehyde group, a carboxyl group, a carbonyl group, an amino group, a nitro group, a sulfo group, a ketone group, an acetyl group, an azo group, a vinyl group, an epoxy group, a styryl group, a methacryl group, an acrylic group, an isocyanate group, a mercapto group, a silyl group, etc. One or more types of these functional groups may be contained in the molecular structure.
[0035] The median diameter D50 of the particles 11 whose surfaces are covered with the coating layer 12 is 3.0 nm or more and 1.0 × 10 5 The median diameter D50 of the particles 11 whose surfaces are covered with the coating layer 12 can be set to 1.0×10 nm or less. The median diameter D50 of the particles 11 whose surfaces are covered with the coating layer 12 is measured by a laser diffraction type particle size distribution measuring device. Specifically, the median diameter D50 of the particles 11 whose surfaces are covered with the coating layer 12 is the particle diameter at which the volume-based cumulative frequency distribution measured by the laser diffraction type particle size distribution measuring device indicates 50%. By setting the median diameter D50 of the particles 11 whose surfaces are covered with the coating layer 12 to 3.0 nm or more, the particles 11 are not too small, and the characteristics of the particles 11 can be easily reflected in the composite material. The median diameter D50 of the particles 11 whose surfaces are covered with the coating layer 12 can be set to 1.0×10 5 By setting the particle size to 0.1 nm or less, the surface area of the particles 11 is large, so that during the production of the composite material raw material 1 described below, the coating layer 12 is easily formed and mechanical treatment using a shear force is easily performed.
[0036] The median diameter D50 of the particles 11 whose surfaces are covered with the coating layer 12 is preferably 1.0×10 1 nm or more, more preferably 2.0×10 1 nm or more, more preferably 3.0×10 1 The median diameter D50 of the particles 11 whose surfaces are covered with the coating layer 12 is preferably 5.0×10 nm or more from the viewpoint of ensuring the above-mentioned effects. 4 nm or less, more preferably 3.0×10 4 nm or less, more preferably 1.0×10 4nm or less.
[0037] The volume ratio of the particles 11 to the total volume of the particles 11 and at least one of the resin 101 and the resin component 102 in the dispersion medium 10 can be 1.0 volume % or more and 90.0 volume % or less. In other words, the volume ratio of the particles 11 to at least one of the resin 101 and the resin component 102 in the dispersion medium 10 can be in the range of 1.0:99.0 to 90.0:10.0.
[0038] When the volume ratio of the particles 11 is 1.0 volume % or more, it is advantageous to improve the tensile strength of the composite material. When the volume ratio of the particles 11 is 90.0 volume % or less, it is possible to suppress an increase in viscosity during the production of the composite material raw material 1, and to suppress the occurrence of voids in the composite material that cause a decrease in tensile strength. The volume ratio of the particles 11 can be preferably 3.0 volume % or more, more preferably 5.0 volume % or more. The volume ratio of the particles 11 can be preferably 85.0 volume % or less, more preferably 80.0 volume % or less.
[0039] The total volume of at least one of the resin 101 and the resin component 102 and the plurality of particles 11 in the dispersion medium 10 means the total volume of the resin 101 and the plurality of particles 11 in the dispersion medium 10 when the dispersion medium 10 does not contain the resin component 102 but contains the resin 101, the total volume of the resin component 102 and the plurality of particles 11 in the dispersion medium 10 when the dispersion medium 10 does not contain the resin 101 but contains the resin component 102, and the total volume of both the resin 101 and the resin component 102 and the plurality of particles 11 in the dispersion medium 10 when the dispersion medium 10 contains both the resin 101 and the resin component 102. In other words, the total volume mentioned above does not include the volume of the above-mentioned solvent (diluent).
[0040] The content of the particles 11 contained in the composite material raw material 1 can be 0.5 volume % or more and 50.0 volume % or less. When the content of the particles 11 is 0.5 volume % or more, the amount of the dispersion medium 10 used can be reduced, making it easier to apply the composite material raw material 1 to various industrial fields. When the content of the particles 11 is 50.0 volume % or less, an increase in viscosity can be suppressed during the production of the composite material raw material 1, making it easier to apply a mechanical treatment to apply a shear force, which will be described later.
[0041] (Method of manufacturing raw materials for composite materials) The method for producing a raw material for a composite material according to the present embodiment includes a preparation step and a mechanical treatment step.
[0042] The preparation step is a step of preparing a mixture 2 containing a dispersion medium 10 containing at least one of a resin 101 and a resin component 102, and a plurality of particles 11 mixed in the dispersion medium 10, as illustrated in FIG. 2(a).
[0043] Conventionally, when manufacturing raw materials for composite materials, first, in a dispersion process, a plurality of dried particles are added to a solvent such as an organic solvent that does not contain resin or resin components, and the plurality of particles in the solvent are dispersed, and then the resin and resin components are mixed through a drying process. This is because, if the resin or resin components are added first in the dispersion process, the solvent that dissolves them is limited, and impurities such as resin and resin components should not be added to the device that disperses the particles. In contrast, in the above preparation process, a dispersion medium 10 containing at least one of the resin 101 and the resin component 102 and a plurality of particles 11 are intentionally mixed first to prepare a mixture 2 containing them. This is because, even if the particles 11 are mixed first in a resin-free dispersion medium that does not contain the resin 101 and the resin component 102, and the resin 101 or the resin component 102 is added after mechanical treatment, the adhesion between the particles 11 and the resin 101 or the resin component 102 is not improved, and a composite material with improved tensile strength cannot be obtained. In other words, in the manufacturing method for raw materials for composite materials of this embodiment, in order to obtain a composite material with improved tensile strength, resin 101 or resin component 102 is mixed with particles 11 at a stage prior to performing a mechanical process to disperse multiple particles 11 in a dispersion medium 10.
[0044] The mixing of the plurality of particles 11 and the dispersion medium 10 can be carried out using an existing mixing device such as a kneader or a stirrer. In addition, for example, when the resin 101 is a curable resin and is liquid, the plurality of particles 11 can be mixed with the liquid curable resin. In addition, as described above, the curable resin may be composed of a base agent and a curing agent. In this case, the base agent may be mixed with the plurality of particles 11, or the curing agent may be mixed with the plurality of particles 11. In addition, the base agent and the curing agent may be mixed with the plurality of particles 11. In addition, when the base agent and the plurality of particles 11 are mixed to prepare the mixture 2, the curing agent can be further mixed after the mechanical treatment. In addition, when the curing agent and the plurality of particles 11 are mixed to prepare the mixture 2, the base agent can be further mixed after the mechanical treatment. In addition, the liquid curable resin, the base agent, and the curing agent may be diluted with a solvent.
[0045] Furthermore, for example, when the resin 101 is a thermoplastic resin, the resin 101 can be dissolved in a solvent and then mixed with a plurality of particles 11.
[0046] In the mixture 2, the volume ratio of the plurality of particles 11 to the total volume of the plurality of particles 11 and at least one of the resin 101 and the resin component 102 in the dispersion medium 10 can be 1.0 volume % or more and 90.0 volume % or less.
[0047] When the volume ratio of the particles 11 is 1.0 volume % or more, it is advantageous to improve the tensile strength of the composite material. When the volume ratio of the particles 11 is 90.0 volume % or less, it is possible to suppress an increase in viscosity during the production of the composite material raw material 1, and to suppress the occurrence of voids in the composite material that cause a decrease in tensile strength. The volume ratio of the particles 11 can be preferably 3.0 volume % or more, more preferably 5.0 volume % or more. The volume ratio of the particles 11 can be preferably 85.0 volume % or less, more preferably 80.0 volume % or less.
[0048] The content of the particles 11 in the mixture 2 can be 0.5% by volume or more and 50.0% by volume or less. When the content of the particles 11 is 0.5% by volume or more, the amount of the dispersion medium 10 used can be reduced, making the mixture more applicable to various industrial fields. When the content of the particles 11 in the mixture 2 is 50.0% by volume or less, an increase in viscosity can be suppressed during the production of the composite material raw material 1, making it easier to carry out the mechanical treatment described below in which a shear force is applied.
[0049] The mechanical treatment step is a step of dispersing a plurality of particles 11 in the dispersion medium 10 by applying a shear force to the prepared mixture, and coating the surfaces of the particles 11 with a coating layer 12 formed from a resin-derived component derived from at least one of the resin 101 and the resin component 102 contained in the dispersion medium 10. In this mechanical treatment step, dispersion of the particles 11 in the dispersion medium 10 containing at least one of the resin 101 and the resin component 102, and surface coating of the surfaces of the particles 11 with the resin-derived component derived from at least one of the resin 101 and the resin component 102 contained in the dispersion medium 10 are simultaneously performed.
[0050] The mechanical treatment may be any method that can apply a shear force to the mixture 2. For example, a wet jet mill, a rotary disk mill, a high-pressure homogenizer, or the like, which is a mechanical device that can apply a shear flow in consideration of the movement of the fluid, can be suitably used for the mechanical treatment. In addition, for example, a planetary homogenizer, a high-speed mixer, a three-roll mill, or the like can also be used.
[0051] In the mechanical treatment step, the mixture 2 is pressurized to 30 MPa or more and 250 MPa or less, and the shear force generated when the mixture 2 passes through the small holes can be utilized. This configuration can ensure the dispersion of the particles 11 in the dispersion medium 10 and the formation of the coating layer 12 on the surface of the particles 11.
[0052] The pressure applied to the mixture 2 is preferably 50 MPa or more, more preferably 100 MPa or more, and even more preferably 150 MPa or more. The pressure applied to the mixture 2 is preferably 230 MPa or less, and more preferably 200 MPa or less. The diameter of the small hole is preferably 0.01 mm or more, more preferably 0.05 mm or more, and even more preferably 0.10 mm or more.
[0053] The temperature of the mixture 2 in the mechanical treatment step may be any temperature at which the mixture 2 does not vaporize or solidify. The temperature of the mixture 2 may increase due to the shear force generated when passing through the small holes. In this case, the mixture 2 can be appropriately cooled to prevent it from vaporizing.
[0054] FIG. 3 shows an example of mechanical processing using a wet jet mill. The wet jet mill 5 shown in FIG. 3 has a mill body 51 equipped with a plunger 510, a supply section 52 connected to the mill body 51, and a dispersion nozzle section 53 connected to an end of the mill body 51 downstream of the supply section 52. The mill body 51 and the supply section 52 of the wet jet mill 5 are filled with a mixture 2 containing a liquid dispersion medium 10 containing at least one of a resin 101 and a resin component 102 and a plurality of particles 11. In addition, the dispersion nozzle section 53 is formed with a small hole 530 that sharply narrows the flow path through which the mixture 2 flows. A high pressure is applied to the mixture 2 in the mill body 51 by the plunger 510. The mixture 2 to which the high pressure is applied is guided to the dispersion nozzle section 53 and passes through the small hole 530. When passing through the small holes 530, a shear force acts on the mixture 2, dispersing the particles 11 in the dispersion medium 10 and simultaneously coating the surfaces of the particles 11 with a resin-derived component derived from at least one of the resin 101 and the resin component 102 contained in the dispersion medium 10. The composite material raw material 1 produced by passing through the small holes 530 is collected in a container (not shown) or the like. The diameter of the small holes 530 can be, for example, 0.01 mm or more and 0.50 mm or less.
[0055] The mechanical treatment can be performed once or multiple times. When the mechanical treatment is performed multiple times, specifically, after the prepared mixture 2 is subjected to a mechanical treatment in which a shear force is applied, the mixture 2 that has been subjected to the mechanical treatment is further subjected to the mechanical treatment once or multiple times. When the mechanical treatment is performed multiple times, the dispersion of the particles 11 in the dispersion medium 10 and the surface coverage of the surfaces of the particles 11 with the resin-derived component can be made more sufficient.
[0056] According to the method for producing the composite material raw material of this embodiment, the composite material raw material 1 of this embodiment can be obtained.
[0057] From the viewpoint of ensuring an improvement in the tensile strength of the composite material, the composite material raw material 1 obtained by the composite material raw material manufacturing method of this embodiment has a coating ratio, which is defined as the ratio of the coating amount of the coating layer covering the surface of the particles in the composite material raw material to the coating amount of the coating layer covering the surface of the particles in the reference raw material, of preferably 1.3 times or more, more preferably 1.5 times or more, and even more preferably 1.7 times or more. Moreover, the above-mentioned coating ratio is preferably 20.0 times or less, more preferably 17.5 times or less, and even more preferably 15.0 times or less.
[0058] Furthermore, from the viewpoint of ensuring an improvement in the tensile strength of the composite material, the tensile strength of the composite material molded using the composite material raw material 1 obtained by the manufacturing method for the composite material raw material of the present embodiment is preferably 1.1 times or more, more preferably 1.2 times or more, and even more preferably 1.3 times or more, of the tensile strength of the reference composite material molded using the reference raw material.
[0059] The method for measuring the coating amount of the coating layer and the reference raw materials are as described above in (Raw materials for composite materials).
[0060] (composite material) The composite material of this embodiment is formed using the composite material raw material 1 of this embodiment. The composite material raw material 1 of this embodiment may be obtained by the manufacturing method for the composite material raw material of this embodiment, or may be manufactured by another manufacturing method.
[0061] The molding method of the composite material is not particularly limited. For example, when the composite material raw material 1 does not contain a solvent, it can be molded into a desired shape by a known molding method such as injection molding, extrusion molding, press molding, vacuum press molding, etc. Also, for example, when the composite material raw material 1 contains a solvent 103, the solvent 103 can be removed and then molded into a desired shape by the above molding method. Also, for example, when the composite material raw material 1 contains a resin component 102, the remaining resin component required to constitute the resin 101 can be mixed into the composite material raw material 1, and then this can be molded into a desired shape by the above molding method. Also, for example, the particles 11 whose surfaces are covered with the coating layer 12 can be collected from the composite material raw material 1, and the particles 11 and the resin 101 can be mixed and molded into a desired shape by the above molding method.
[0062] The tensile modulus and tensile strength of the composite material can be measured as follows. A dumbbell-shaped No. 7 composite material test piece as specified in JIS K6251 is prepared from the composite material raw material 1 from which the solvent has been removed. The tensile modulus and tensile strength of the prepared composite material test piece can be measured by performing a tensile test at room temperature and a tensile speed of 1 mm / min using a universal testing machine.
[0063] The above-mentioned composite material can be used, for example, as a structural material for automobiles, aircraft, and the like.
[0064] The contents of the respective descriptions of the raw material for a composite material, the method for producing a raw material for a composite material, and the composite material of the present embodiment described above can be appropriately referred to and applied to each other as necessary.
[0065] <Experimental Example> (Sample 1-1) 35.3 g (10.0 cm) of aluminum oxide ceramic powder (Kanto Chemical Co., Ltd., "NanoTek", single particle diameter 52 nm) 3 ) and a thermosetting resin, epoxy resin base (hereinafter referred to as epoxy base) (manufactured by Mitsubishi Chemical Corporation, "JER827") 29.0 g (25.0 cm 3) and 12.4 g (15.4 cm3) of methyl ethyl ketone, a solvent used as a diluent. 3 ) and ethanol 354.8 g (449.9 cm 3 ) was mixed and stirred in a planetary mixer to prepare a liquid mixture (suspension). The particle size of the aluminum oxide powder was determined by observing the powder with a scanning electron microscope and arithmetic mean value of particle sizes of 100 random particles. The same measurement method was used for each sample described later.
[0066] The volume ratio of the aluminum oxide powder to the total volume of the epoxy base material and the aluminum oxide powder in the mixture is 28.6% by volume. The content of the aluminum oxide powder in the mixture is 2.0% by volume. The median diameter D50 of the aluminum oxide powder in the mixture, measured using a laser diffraction particle size distribution measuring device (HORIBA, Ltd., "LA-950V2"), is 8.3 x 10 3 The results of the particle size distribution measurements and their discussion will be described in more detail later. The same applies to the other samples described later.
[0067] Next, the prepared mixture was subjected to mechanical treatment using a wet jet mill (Advanced Nano Technology, "LSU2540-P20D-AP"). The conditions for mechanical treatment using the wet jet mill were: diameter of the small hole in the dispersion nozzle of the wet jet mill: 0.17 mm, pressure: 200 MPa, number of mechanical treatments: 5 times. This is the raw material for the composite material of sample 1-1.
[0068] In this experimental example, the dispersion nozzle part described above specifically has a nozzle member 53A having a shape shown in FIG. 4. More specifically, the nozzle member 53A has a first flow path component 531 and a second flow path component 532 laminated on the first flow path component 531. A small hole 530 is formed in the center of the first flow path component 531 so as to be aligned with the pressurizing direction of the mixture 2 by the plunger 510 described above. A narrow groove 534 having a width equal to the diameter of the small hole 530, a groove depth equal to the diameter of the small hole 530, and a length equal to the length of the small hole 530 is formed on the surface of the second flow path component 532 on the first flow path component 531 side. The small hole 530 is connected to the center of the long direction of the narrow groove 534. In addition, a pair of large holes 535 is formed in the second flow path component 532 so as to be aligned with the pressurizing direction. The diameter of the pair of large holes 535 is larger than the diameter of the small hole 530. One end of each large hole 535 is connected to both ends of the elongated groove 534. The other end of each large hole 535 is open to the surface of the second flow path forming member 532 opposite to the surface on the first flow path forming member 531 side. In the nozzle member 53A, the small hole 530, the elongated groove 534, and the pair of large holes 535 form an intra-nozzle flow path. The mixture 2 flows in through the small hole 530. In this experimental example, the diameter φ of the small hole 530 1 is 0.17mm, the length of the small hole 530 L 1 (length of cylinder) is 1.1 mm, width w of the elongated groove 534 is 0.17 mm, depth d of the elongated groove 534 is 0.17 mm, length L of the elongated groove 534 in the planar direction 2 1.1mm, large hole diameter φ535 2 is 0.7 mm, the length of the large hole 535 L 3 The length of the cylinder was 2.5 mm. The nozzle member 53A was made of sintered diamond. The diameter of the flow path through which the mixture 2 flows before the nozzle member 53A was 3.2 mm.
[0069] The prepared composite material raw material of Sample 1-1 was centrifuged at 3500 rpm for 60 minutes, and the precipitated aluminum oxide powder was collected. The collected aluminum oxide powder was then washed three times with methyl ethyl ketone and then vacuum dried for 8 hours. The mass reduction rate of the dried aluminum oxide powder was measured from 150°C to 600°C at a heating rate of 10°C / min using a thermogravimetric differential thermal analyzer (manufactured by Rigaku Corporation, "TG-8120"). Since a mass reduction was observed in the aluminum oxide powder after the above washing, it was confirmed that the surface of the aluminum oxide particles constituting the aluminum oxide powder was covered with a coating layer formed from a resin-derived component derived from the epoxy base agent. In addition, since the resin-derived component was not removed by the above washing, it can be said that the resin-derived component is adsorbed on the surface of the aluminum oxide particles. More details will be described later using the measurement results using an infrared spectrophotometer. According to the measurement results of the mass reduction rate, the coating amount (adsorption amount of resin-derived component) of the coating layer covering the surface of the aluminum oxide particles was 1.97 mass%.
[0070] As a result of the above, a composite material raw material of sample 1-1 was obtained, which had a dispersion medium containing an epoxy base resin and a solvent, a plurality of aluminum oxide particles dispersed in the dispersion medium, and a coating layer formed from a resin-derived component derived from the epoxy base resin that covered the surfaces of the aluminum oxide particles.
[0071] The median diameter D50 of the aluminum oxide powder covered with the coating layer of the composite material sample 1-1, measured using the above-mentioned laser diffraction particle size distribution analyzer (HORIBA, Ltd., "LA-950V2"), was 7.0 × 10 1 The results of the particle size distribution measurements and their discussion will be described in more detail later. The same applies to the other samples described later.
[0072] Next, the solvents in the composite material raw material of Sample 1-1, ethanol and methyl ethyl ketone, were removed using an evaporator. 1.4 g (1.2 cm3) of epoxy resin hardener (sometimes called epoxy hardener) (manufactured by Mitsubishi Chemical Corporation, "ST11") was added to 5.0 g of the composite material raw material from which the solvent had been removed. 3 ) was added and stirred with a planetary mixer. The resulting mixture was poured into a silicone mold capable of forming dumbbell test pieces (dumbbell No. 7 as specified in JIS K6251) for tensile testing, and heated at 80°C for 3 hours to harden the epoxy resin, producing a composite material. The aluminum oxide powder mixture ratio in the produced composite material was 20.0% by volume.
[0073] Next, a tensile test was performed on the prepared composite material using a universal testing machine (Shimadzu Corporation, "EZ-SX") at room temperature and a tensile speed of 1 mm / min to measure the tensile modulus and tensile strength. The tensile modulus of the obtained composite material was 3.07 GPa and the tensile strength was 92.5 MPa.
[0074] Next, the microstructure of the fracture surface of the composite material of Sample 1-1 after the tensile test was observed with a scanning electron microscope (manufactured by JEOL Ltd., "JSM-IT300HR"). The results are shown in FIG. 4. As shown in FIG. 4, it can be seen that aluminum oxide particles are embedded inside the epoxy resin in the composite material of Sample 1-1. From this result, it was confirmed that the adhesion between the resin and the particles is improved by forming a composite material using the composite material raw material of the present disclosure.
[0075] (Sample 1-2) Methyl ethyl ketone 12.4g (15.4cm 3 ) and ethanol 354.8 g (449.9 cm 3 ) to 374.3 g (463.6 cm 3 ), the composite material raw material and composite material of Sample 1-2 were prepared in the same manner as Sample 1-1.
[0076] The volume ratio of the aluminum oxide powder to the total volume of the epoxy base material and the aluminum oxide powder in the mixture is 28.6 volume %. The content of the aluminum oxide powder in the mixture is 2.0 volume %. The median diameter D50 of the aluminum oxide powder in the mixture is 1.3 x 10 4 nm. The amount of coating (adsorption amount) of the coating layer that covers the surface of the aluminum oxide particles was 0.79 mass%. The median diameter D50 of the aluminum oxide powder whose surface was covered with the coating layer in the composite material raw material of Sample 1-2 was 7.4 × 10 1 The composite material had a tensile modulus of 3.03 GPa and a tensile strength of 85.1 MPa.
[0077] (Sample 2) The aluminum oxide powder was replaced with silicon dioxide powder, a ceramic powder (manufactured by Sakai Chemical Industry Co., Ltd., "Sciqas GRADE 0.25 μm," single particle diameter 2.6 × 10 2 nm) 66.3g (25.0cm 3 ) changed to epoxy base 72.5g (62.5cm 3 ), methyl ethyl ketone 31.0g (38.4cm 3 ), ethanol 295.0g (374.1cm 3 ), the composite material raw material and composite material of Sample 2 were prepared in the same manner as Sample 1-1. The composite material raw material of Sample 2 has a dispersion medium containing an epoxy base agent and a solvent, a plurality of silicon dioxide particles dispersed in the dispersion medium, and a coating layer formed from a resin-derived component derived from the epoxy base agent that covers the surfaces of the silicon dioxide particles.
[0078] The volume ratio of the silicon dioxide powder to the total volume of the epoxy base material and the silicon dioxide powder in the mixture is 28.6 volume%. The content of the silicon dioxide powder in the mixture is 5.0 volume%. The median diameter D50 of the silicon dioxide powder in the mixture is 2.7 x 10 2nm. The amount of the coating layer covering the surface of the silicon dioxide particles was 1.53 mass%. The median diameter D50 of the silicon dioxide powder whose surface was covered with the coating layer in the composite material raw material of sample 2 was 1.9 × 10 2 The composite material had a tensile modulus of 2.67 GPa and a tensile strength of 104.6 MPa.
[0079] (Sample 3) Silicon dioxide powder was replaced with magnesium oxide powder, a ceramic powder (manufactured by Tateho Corporation, "PUREMAG (registered trademark) FNMG", single particle diameter 3.9 × 10 2 nm) 90.0g (25.0cm 3 ), the composite material raw material and composite material of Sample 3 were prepared in the same manner as Sample 2. The composite material raw material of Sample 3 has a dispersion medium containing an epoxy base agent and a solvent, a plurality of magnesium oxide particles dispersed in the dispersion medium, and a coating layer formed from a resin-derived component derived from the epoxy base agent that covers the surfaces of the magnesium oxide particles.
[0080] The volume ratio of the magnesium oxide powder to the total volume of the epoxy base material and the magnesium oxide powder in the mixture is 28.6% by volume. The content of the magnesium oxide powder in the mixture is 5.0% by volume. The median diameter D50 of the magnesium oxide powder in the mixture is 9.5×10 2 nm. The amount of coating (adsorption amount) of the coating layer that coats the surface of the magnesium oxide particles was 3.02 mass%. The median diameter D50 of the magnesium oxide powder whose surface was covered with the coating layer in the composite material raw material of Sample 2 was 1.9 × 10 2 The composite material had a tensile modulus of 2.82 GPa and a tensile strength of 91.1 MPa.
[0081] (Sample 1R) A reference material for sample 1R and a reference composite material using this were prepared in the same manner as sample 1-1, except that a liquid mixture of aluminum oxide powder, methyl ethyl ketone, and ethanol was subjected to mechanical treatment and then an epoxy base resin was added.
[0082] The volume ratio of the aluminum oxide powder to the total volume of the epoxy base material and the aluminum oxide powder in the reference raw material is 28.6 volume %. The content of the aluminum oxide powder contained in the reference raw material is 2.0 volume %. The median diameter D50 of the aluminum oxide powder contained in the reference raw material is 1.0 x 10 4 nm. The amount of the coating layer covering the surface of the aluminum oxide particles was 0.17 mass %. The median diameter D50 of the aluminum oxide powder whose surface was covered with the coating layer in the reference composite material of sample 1R was 7.3 × 10 1 The average particle size of the composite material was 2.43 GPa and the tensile strength was 68.5 MPa.
[0083] Next, the microstructure of the fracture surface of the reference composite material of sample 1R after the tensile test was observed using the above-mentioned scanning electron microscope. The results are shown in Figure 6. As shown in Figure 6, in the reference composite material of sample 1R, the aluminum oxide particles peeled off from the epoxy resin, and voids of the same shape as the aluminum oxide particles were observed. This is because the resin-derived components that form the coating layer that covers the particle surfaces were not sufficiently adsorbed onto the particle surfaces, resulting in poor adhesion at the interface between the two.
[0084] (Sample 2R) A reference material for Sample 2R and a reference composite material using this were prepared in the same manner as Sample 2, except that a liquid mixture of silicon dioxide powder, methyl ethyl ketone, and ethanol was subjected to mechanical treatment and then an epoxy base resin was added.
[0085] The volume ratio of silicon dioxide powder to the total volume of the epoxy base material and silicon dioxide powder in the reference raw material is 28.6 volume%. The content of silicon dioxide powder contained in the reference raw material is 5.0 volume%. The median diameter D50 of the silicon dioxide powder contained in the reference raw material is 3.2 x 10 2 nm. The amount of the coating layer covering the surface of the silicon dioxide particles was 0.85 mass%. The median diameter D50 of the silicon dioxide powder whose surface was covered with the coating layer in the reference composite material of sample 2R was 2.1 × 10 2 The thickness of the composite material was 1.0 nm. The mixing ratio of silicon dioxide powder in the prepared reference composite material was 20.0 volume %. The tensile modulus of the prepared reference composite material was 2.28 GPa, and the tensile strength was 90.7 MPa.
[0086] (Sample 3R) A reference material for Sample 3R and a reference composite material using this were prepared in the same manner as Sample 3, except that a liquid mixture of magnesium oxide powder, methyl ethyl ketone, and ethanol was subjected to mechanical treatment and then an epoxy base resin was added.
[0087] The volume ratio of the magnesium oxide powder to the total volume of the epoxy base material and the magnesium oxide powder in the reference raw material is 28.6 volume %. The content of the magnesium oxide powder contained in the reference raw material is 5.0 volume %. The median diameter D50 of the magnesium oxide powder contained in the reference raw material is 6.4 × 10 3 nm. The amount of the coating layer covering the surface of the magnesium oxide particles was 1.58 mass%. The median diameter D50 of the magnesium oxide powder whose surface was covered with the coating layer in the reference composite material of sample 3R was 1.9 × 10 2 The average particle size of the composite material was 1.0 nm. The mixing ratio of magnesium oxide powder in the prepared reference composite material was 20.0 volume %. The tensile modulus of the prepared reference composite material was 2.57 GPa and the tensile strength was 58.1 MPa.
[0088] (Sample 1-1C) Aluminum oxide powder 92.9g (26.3Rm 3 ) and 395g of ethanol (500cm 3 ) and 0.5 g (0.5 cm 3 ) was mixed and stirred in a planetary mixer to prepare a liquid mixture (suspension). Next, 16.5 g of 3-glycidoxypropyltriethoxysilane, a silane coupling agent, was added to this mixture, and the mixture was stirred for 2 hours. Next, a wet jet mill was used to mechanically treat the mixture to which the silane coupling agent had been added. At this time, the conditions for the mechanical treatment using the wet jet mill were a small hole diameter of 0.17 mm, pressure of 200 MPa, and number of mechanical treatments: 10 times. This was used as the raw material for the composite material of sample 1-1C.
[0089] The composite material raw material of the prepared sample 1-1C was centrifuged and the supernatant was removed. The precipitated aluminum oxide was dried at 120°C for 2 hours. The median diameter D50 of the dried magnesium oxide powder was 7.4×10 1 nm. 2.74g of dried aluminum oxide powder, 2.26g of epoxy base material, and 1.35g of epoxy hardener were mixed and stirred in a planetary mixer. The resulting liquid mixture was poured into a silicone mold capable of forming dumbbell test pieces for tensile testing, and heated at 80°C for 3 hours to harden the epoxy resin, producing a composite material. The mixture ratio of aluminum oxide powder in the produced composite material was 20.0% by volume. The tensile modulus of the obtained composite material was 2.66 GPa, and the tensile strength was 67.9 MPa.
[0090] (Sample 1-2C) After mechanical treatment and before mixing with the epoxy base, the median diameter D50 of the magnesium oxide powder contained in the composite material raw material of sample 1-1C was 7.2 × 10 1nm. The composite material raw material of sample 1-1C was centrifuged and the supernatant liquid was removed. 7.46 g of precipitated aluminum oxide was mixed with 14.81 g of methyl ethyl ketone and 4.81 g of epoxy base material, and stirred in a planetary mixer. The resulting liquid mixture was dried under reduced pressure to remove the methyl ethyl ketone. Next, 2.89 g of epoxy hardener was added to it, and stirred in a planetary mixer. The resulting liquid mixture was poured into a silicone mold capable of forming a dumbbell test piece to be used in a tensile test, and heated at 80°C for 3 hours to harden the epoxy resin, thereby producing a composite material of sample 1-2C. The mixture ratio of aluminum oxide powder in the produced composite material was 20.0 volume %. The tensile modulus of the obtained composite material was 2.98 GPa, and the tensile strength was 78.2 MPa.
[0091] (Sample 1-3C) The composite material raw material and composite material of Sample 1-3C were prepared in the same manner as Sample 1-2C, except that no mechanical treatment using a wet jet mill was performed. The median diameter D50 of the magnesium oxide powder contained in the composite material raw material of Sample 1-3C before mixing with the epoxy base agent was 6.1 × 10 3 The thickness of the composite material was 2.41 GPa and the tensile strength was 70.6 MPa.
[0092] The details of each sample and the results obtained for each sample are summarized in Tables 1 and 2. In addition, FIG. 7 shows the infrared spectrum of the epoxy base resin. FIG. 8 shows the infrared spectrum of the aluminum oxide powder itself, the aluminum oxide powders recovered from the composite material raw materials of Samples 1-1 and 1-2, and the aluminum oxide powder recovered from the reference raw material of Sample 1R. FIG. 9 shows the infrared spectrum of the silicon dioxide powder itself, the silicon dioxide powder recovered from the composite material raw material of Sample 2, and the silicon dioxide powder recovered from the reference raw material of Sample 2R. FIG. 10 shows an enlarged view of the infrared spectrum shown in FIG. 9. FIG. 11 shows the infrared spectrum of the magnesium oxide powder itself, the magnesium oxide powder recovered from the composite material raw material of Sample 3, and the magnesium oxide powder recovered from the reference raw material of Sample 3R. The infrared spectrophotometer used to measure the infrared spectrum was "Spectrum Two" manufactured by PerkinElmer Japan. The powders used for the infrared spectroscopy measurements were prepared by washing the powders recovered from the raw materials for each composite material and the reference raw material three times with methyl ethyl ketone and then drying them in a vacuum for eight hours.
[0093] 12 to 18 show the relationship between particle size (nm) and cumulative (volume %) or frequency (volume %) before and after mechanical treatment in the preparation of the composite material raw materials of Samples 1-1 to 3 and Samples 1R to 3R. FIG. 19 and FIG. 20 show the relationship between particle size (nm) and frequency (volume %) in the composite material raw materials of Samples 1-1C to 1-3C. Table 3 shows the particle size distribution data in numerical form. In Table 3, the particle size D10 is the particle size when the volume-based cumulative frequency distribution measured by a laser diffraction particle size distribution analyzer is 10%, and the particle size D90 is the particle size when the volume-based cumulative frequency distribution measured by a laser diffraction particle size distribution analyzer is 90%.
[0094] [Table 1]
[0095] [Table 2]
[0096] [Table 3]
[0097] The following can be seen from Tables 1 and 2 and Figures 7 to 11. Compared to Sample 1R, Sample 1-1 had a coating amount and tensile strength that were increased by 1060% and 35%, respectively. From these results, it can be seen that by performing a mechanical treatment in which a shear force is applied to a specified mixture, a part of the resin component in the dispersion medium (epoxy base in this experimental example) is adsorbed onto the surface of the particles (ceramic particles in this experimental example), and the tensile strength of the composite material is improved. Furthermore, Sample 1-2 had a coating amount and tensile strength that were increased by 365% and 24%, respectively, compared to Sample 1R. From these results, it was confirmed that the tensile strength of the composite material can be improved even if the type of solvent contained in the mixture to which the mechanical treatment is performed is changed. Furthermore, as shown in Figures 7 and 8, Sample 1-1 had a coating amount and tensile strength that were increased by 365% and 24%, respectively, in the coating layer. -1 There are three in the range of 1511, 1250, and 1185 cm -1 A peak of the resin-derived component was observed in each of the samples. In sample 1-2, a peak of the resin-derived component was observed, although the peak intensity was weaker than in sample 1-1. From these results, it became clear that in samples 1-1 and 1-2, the resin-derived component that forms the coating layer that covers the surface of the particles is adsorbed onto the particle surface. On the other hand, in sample 1R, no peak of the resin-derived component was observed, indicating that the resin-derived component that forms the coating layer that covers the surface of the particles is not adsorbed onto the particle surface.
[0098] The coating amount and tensile strength of sample 2 were increased by 80% and 15%, respectively, compared to sample 2R. The coating amount and tensile strength of sample 3 were increased by 91% and 57%, respectively, compared to sample 3R. From these results, it was confirmed that the tensile strength of the composite material can be improved even if the type of particles contained in the mixture to be mechanically treated is changed. In addition, as shown in Figures 7, 9, and 10, peaks of resin-derived components were observed in sample 2 and sample 2R, but no difference between the two could be observed. In addition, as shown in Figures 7 and 11, peaks of resin-derived components were observed in sample 3 and sample 3R, but the peak strength of sample 3 was higher than that of sample 3R.
[0099] Furthermore, according to Tables 1 and 3, in Samples 1-1 to 3, the median diameter D50 of the multiple particles is smaller after the mechanical treatment than before the mechanical treatment, which shows that the multiple particles are well dispersed.
[0100] In contrast, sample 1-1C was modified by the conventional method of surface modification of particles using a silane coupling agent, but the tensile strength decreased. This is due to the aggregation of particles during drying after the silane coupling reaction. In sample 1-2C, the aggregation of particles could be suppressed by not performing a drying operation after the silane coupling reaction, but the increase in tensile strength was only 14% compared to sample 1R. In sample 1-3C, the median diameter D50 was large and the tensile strength hardly increased at all because no mechanical treatment was performed to apply a shear force to the mixture.
[0101] The following can also be seen from Table 3, Fig. 19 and Fig. 20. It can be seen that particles are aggregated in the raw materials used for Samples 1-1C to 1-3C. It can also be seen that, although many particles are dispersed in Sample 1-1C, aggregated particles are present in 92% or more of the region. This is thought to be due to the influence of drying. It can also be seen that Sample 1-2C is in the same state as Sample 1-1C before drying, and the particles are dispersed without aggregation. It can also be seen that many aggregated particles are present in Sample 1-3C, since no mechanical treatment using a wet jet mill was performed.
[0102] The present invention is not limited to the above-described embodiments and experimental examples, and various modifications are possible without departing from the spirit and scope of the present invention. Furthermore, the configurations shown in the embodiments and experimental examples can be combined in any manner. [Industrial Applicability]
[0103] The above-mentioned composite material raw materials and composite materials are useful as structural members for automobiles, aircraft, sporting goods, etc., and heat dissipating members for electronic devices, etc. [Explanation of symbols]
[0104] 1 Raw materials for composite materials 10 Dispersion medium 101 Resin 102 Resin components 11 particles 12 Covering layer 2 mixture
Claims
1. A particle-dispersion-reinforced composite material in which particles are dispersed as a reinforcing material in a resin as a matrix (however, this does not include a composite material in which the particles as the reinforcing material are oriented in the resin as the matrix). A raw material for a composite material used in a dispersion medium containing at least one of the resin serving as the base material of the composite material and a resin component serving as a component for constituting the resin serving as the base material of the composite material (excluding a chain aliphatic epoxy resin having a hydrophilic group, a resin having a fluorene skeleton, and a rubber latex) and a solvent; A plurality of particles dispersed in the dispersion medium (excluding, however, cellulose, an adsorbent filler in which a thermoplastic resin is adsorbed on a filler, and nanoparticles in which one or more oligomers derived from two or more polymerizable units are covalently bonded via a coupling agent), a coating layer covering the surface of the particle, the coating layer is formed from a resin-derived component that is derived from at least one of the resin and the resin component contained in the dispersion medium and that is adsorbed on the surface of the particle, The coating layer is formed by applying a shear force to a mixture containing the dispersion medium and the particles.
2. 2. The raw material for composite materials according to claim 1, wherein a coating ratio, defined as the ratio of the coating amount of the coating layer covering the surface of the particle in the raw material for composite materials to the coating amount of the coating layer covering the surface of the particle in the reference raw material, is 1.3 times or more. However, the above reference material is a resin-containing mixture prepared as follows. A resin-free mixture containing the resin and a resin-free dispersion medium that does not contain the resin component and a plurality of the particles is prepared, and the prepared resin-free mixture is subjected to mechanical treatment using a wet jet mill, and then the resin or the resin component is mixed so that the volume ratio of the plurality of particles is the same as that of the raw material for the composite material to obtain a resin-containing mixture. The conditions for the mechanical treatment using the wet jet mill are: diameter of the small hole of the dispersion nozzle part in the wet jet mill: 0.17 mm, pressure: 200 MPa, and number of times of the mechanical treatment: 5 times.
3. The median diameter D50 of the particles whose surfaces are covered with the coating layer, as measured by a laser diffraction particle size distribution analyzer, is 3.0 nm or more and 1.0 × 10 5 3. The composite material raw material according to claim 1, wherein the particle size is 0.1 nm or less.
4. 4. The composite material raw material according to claim 1, wherein the particles are at least one type selected from the group consisting of ceramic particles, metal particles, carbon particles, and organic particles.
5. 5. The raw material for a composite material according to claim 4, wherein the ceramic constituting the ceramic particles is at least one selected from the group consisting of aluminum oxide, zinc oxide, magnesium oxide, silicon oxide, titanium oxide, beryllium oxide, boron nitride, aluminum nitride, silicon nitride, silicon carbide, aluminum hydroxide, magnesium hydroxide, zirconium oxide, and yttrium oxide.
6. 5. The composite material raw material according to claim 4, wherein the metal constituting the metal particles is gold, silver, copper, a platinum group metal, or an alloy thereof.
7. 5. The composite material raw material according to claim 4, wherein the carbon constituting the carbon particles is at least one selected from the group consisting of carbon black, diamond, graphite, carbon nanotubes, carbon nanofibers, fullerenes, and pulverized carbon fibers.
8. 5. The composite material raw material according to claim 4, wherein the organic matter constituting the organic particles is at least one selected from the group consisting of chitosan and chitin.
9. 9. The composite material raw material according to claim 1, wherein at least one of the resin and the resin component has a reactive functional group in its molecular structure that reacts with the surface of the particles.
10. 9. The raw material for a composite material according to claim 1, wherein at least one of the resin and the resin component has at least one functional group selected from the group consisting of a hydroxyl group, an aldehyde group, a carboxyl group, a carbonyl group, an amino group, a nitro group, a sulfo group, a ketone group, an acetyl group, an azo group, a vinyl group, an epoxy group, a styryl group, a methacryl group, an acrylic group, an isocyanate group, a mercapto group, and a silyl group in its molecular structure.
11. A raw material for composite materials according to any one of claims 1 to 10, wherein the volume ratio of the plurality of particles to the total volume of at least one of the resin and the resin component in the dispersion medium and the plurality of particles is 1.0 volume % or more and 90.0 volume % or less.
12. The composite material raw material according to claim 1 , wherein the content of the plurality of particles contained in the composite material raw material is 0.5 volume % or more and 50.0 volume % or less.
13. A particle-dispersion-reinforced composite material in which particles are dispersed as a reinforcing material in a resin as a matrix (however, this does not include a composite material in which the particles as the reinforcing material are oriented in the resin as the matrix). A method for producing a raw material for a composite material used in a preparation step of preparing a mixture including a dispersion medium containing at least one of the resin serving as the base material of the composite material and a resin component serving as a component for constituting the resin serving as the base material of the composite material (excluding a chain aliphatic epoxy resin having a hydrophilic group, a resin having a fluorene skeleton, and a rubber latex) and a solvent, and a plurality of particles (excluding cellulose, an adsorbent filler in which a thermoplastic resin is adsorbed on a filler, and nanoparticles in which one or more oligomers derived from two or more polymerizable units are covalently bonded via a coupling agent) mixed in the dispersion medium; a mechanical treatment step of dispersing a plurality of the particles in the dispersion medium by applying a shear force to the prepared mixture, and coating the surfaces of the particles with a coating layer formed from a resin-derived component adsorbed on the surfaces of the particles, the resin being derived from at least one of the resin and the resin component contained in the dispersion medium; The method for producing a raw material for a composite material comprising the steps of:
14. 14. The method for producing a raw material for a composite material according to claim 13, wherein in the mechanical treatment step, the mixture is pressurized to a pressure of 30 MPa or more and 250 MPa or less, and a shear force generated when the mixture passes through small holes is utilized.
15. The method for producing a raw material for a composite material according to claim 13 or 14, wherein the tensile strength of a composite material molded using the raw material for a composite material obtained by the method for producing a raw material for a composite material is 1.1 times or more the tensile strength of a reference composite material molded using a reference raw material. However, the above reference material is a resin-containing mixture prepared as follows. A resin-free mixture containing the resin and a resin-free dispersion medium that does not contain the resin component and a plurality of the particles is prepared, and the prepared resin-free mixture is subjected to mechanical treatment using a wet jet mill, and then the resin or the resin component is mixed so that the volume ratio of the plurality of particles is the same as that of the raw material for the composite material to obtain a resin-containing mixture. The conditions for the mechanical treatment using the wet jet mill are: diameter of the small hole of the dispersion nozzle part in the wet jet mill: 0.17 mm, pressure: 200 MPa, and number of times of the mechanical treatment: 5 times.
16. A composite material formed using the composite material raw material according to any one of claims 1 to 12.
Citation Information
Patent Citations
NANO composite
JP2006307199A
Fluorene-based resin composition
JP2009235359A
Thermosetting resin composition
JP2011068778A
Rubber wet master batch and method of producing the same, rubber composition, and pneumatic tire
JP2012207088A
Modified thermally conductive filler, thermally conductive material, and thermally conductive member
JP2015108058A