Resin composition

The resin composition with an active ester curing agent addresses the issue of low dielectric properties and flow marks in semiconductor chip packages, ensuring long-term adhesion and improved storage modulus.

JP7595402B2Active Publication Date: 2024-12-06AJINOMOTO CO INC
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2018238724
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2018-12-20
Publication Date
2024-12-06
Estimated Expiration
2038-12-20

AI Technical Summary

Technical Problem

Conventional insulating materials for semiconductor chip packages have low dielectric properties and are prone to flow marks, which are exacerbated by demands for smaller sizes and thinner films.

Method used

A resin composition comprising an epoxy resin, a curing agent, and an inorganic filler, where the curing agent is an active ester resin with a softening point of 100°C or less, a difunctional active ester resin, or an active ester resin with a molecular weight of 1,000 or less, to reduce dielectric properties and suppress flow marks.

Benefits of technology

The resin composition achieves reduced dielectric properties and suppresses flow marks, providing long-term adhesion to semiconductor chips and excellent storage modulus, suitable for semiconductor chip packages and circuit boards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007595402000001
    Figure 0007595402000001
  • Figure 0007595402000002
    Figure 0007595402000002
  • Figure 0007595402000003
    Figure 0007595402000003
Patent Text Reader

Abstract

To provide a resin composition that reduction of dielectric characteristics of a hardened material and generation control of a flow mark are possible.SOLUTION: A resin composition contains (A) epoxy resin, (B) curing agent and (C) inorganic filler. The (B) component contains (B-1) an active ester resin that the softening point is not more than 100°C, (B-2) an active ester resin with two functional groups, or (B-3) an active ester resin that the molecular weight is not more than 1000.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition containing an epoxy resin and a curing agent; a cured product of the resin composition; a resin sheet containing the resin composition; a circuit board containing the cured product; a semiconductor chip package containing the cured product; and a semiconductor device including the semiconductor chip package. [Background technology]

[0002] In recent years, the demand for small, highly functional electronic devices such as smartphones and tablet devices has been increasing, and accordingly, insulating materials for semiconductor chip packages used in these small electronic devices are required to have higher functionality. Such insulating layers are known to be formed by curing a resin composition (see, for example, Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2017-008312 A Summary of the Invention [Problem to be solved by the invention]

[0004] Insulating materials for semiconductor chip packages are required to have low dielectric properties to meet the ever-increasing demand for smaller and thinner packages. However, among conventional insulating materials, materials with low dielectric properties are prone to generating flow marks.

[0005] An object of the present invention is to provide a resin composition which is capable of reducing the dielectric properties of the cured product and suppressing the occurrence of flow marks. [Means for solving the problem]

[0006] In order to achieve the objects of the present invention, the present inventors conducted extensive research and found that the above objects can be achieved by using, as the (B) curing agent, (B-1) an active ester resin having a softening point of 100° C. or less, (B-2) a difunctional active ester resin, or (B-3) an active ester resin having a molecular weight of 1,000 or less, and thus completed the present invention.

[0007] That is, the present invention includes the following. [1] A resin composition comprising (A) an epoxy resin, (B) a curing agent, and (C) an inorganic filler, wherein the component (B) comprises (B-1) an active ester resin having a softening point of 100°C or lower. [2] The resin composition according to the above [1], wherein the content of the component (B-1) is 1% by mass to 50% by mass, relative to 100% by mass of the non-volatile components in the resin composition. [3] A resin composition comprising (A) an epoxy resin, (B) a curing agent, and (C) an inorganic filler, wherein the component (B) comprises (B-2) a difunctional active ester resin. [4] The component (B-2) is represented by the formula (1):

[0008] [ka]

[0009] [In the formula, rings X, Y and Z each independently represent an aromatic ring which may further have a substituent.] The resin composition according to the above [3], wherein the compound is represented by the formula: [5] The resin composition according to any one of the above [1] to [4], wherein the component (B) further contains one or more curing agents selected from a phenol-based curing agent, a naphthol-based curing agent, an amine-based curing agent, and an acid anhydride-based curing agent. [6] The resin composition according to any one of the above [1] to [5], wherein the component (A) is a liquid epoxy resin. [7] The resin composition according to any one of the above [1] to [6], wherein the average particle size of the component (C) is 1 μm to 40 μm. [8] The resin composition according to any one of the above [1] to [7], wherein the content of the component (C) is 80 mass% or more, based on 100 mass% of the non-volatile components in the resin composition. [9] The resin composition according to any one of the above [1] to [8], which is liquid at 25°C.

[10] The resin composition according to any one of the above [1] to [9] for forming an insulating layer of a semiconductor chip package.

[11] The resin composition according to any one of the above [1] to [9] for forming an insulating layer of a circuit board.

[12] The resin composition according to any one of the above [1] to [9] for encapsulating a semiconductor chip in a semiconductor chip package.

[13] A cured product of the resin composition according to any one of [1] to

[12] above.

[14] A resin sheet comprising: a support; and a resin composition layer provided on the support, the resin composition layer comprising the resin composition according to any one of [1] to

[12] above.

[15] A circuit board comprising an insulating layer formed from a cured product of the resin composition according to any one of the above [1] to

[12] .

[16] A semiconductor chip package comprising the circuit board according to

[15] above and a semiconductor chip mounted on the circuit board.

[17] A semiconductor chip package comprising: a semiconductor chip; and a cured product of the resin composition according to any one of [1] to

[12] above that encapsulates the semiconductor chip.

[18] A semiconductor device comprising the semiconductor chip package according to

[16] or

[17] above.

[19] A resin composition comprising (A) an epoxy resin, (B) a curing agent, and (C) an inorganic filler, wherein the (B) component contains (B-3) an active ester resin having a molecular weight of 1,000 or less. Effect of the Invention

[0010] According to the present invention, it is possible to provide a resin composition capable of reducing the dielectric properties of a cured product and suppressing the occurrence of flow marks; a cured product of the resin composition; a resin sheet including the resin composition; a circuit board including the cured product; a semiconductor chip package including the cured product; and a semiconductor device including the semiconductor chip package. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The present invention will be described in detail below with reference to preferred embodiments. However, the present invention is not limited to the following embodiments and examples, and can be modified and implemented as desired without departing from the scope of the claims of the present invention and their equivalents.

[0012] <Resin composition> The resin composition of the present invention includes (A) an epoxy resin, (B) a curing agent, and (C) an inorganic filler. In a first embodiment, the component (B) includes (B-1) an active ester resin having a softening point of 100° C. or less. In a second embodiment, the component (B) includes (B-2) a difunctional active ester resin. In a third embodiment, the component (B) includes (B-3) an active ester resin having a molecular weight of 1,000 or less.

[0013] By using such a resin composition, it is possible to achieve both reduction in the dielectric properties of the cured product and suppression of the occurrence of flow marks. Furthermore, in one embodiment, the resin composition can provide a cured product having excellent adhesion to semiconductor chips and excellent storage modulus that can be maintained for a long period of time.

[0014] The resin composition of the present invention may further contain optional components in addition to (A) epoxy resin, (B) curing agent, and (C) inorganic filler. Examples of the optional components include (D) curing accelerator, (E) organic solvent, and (F) other additives. Each component contained in the resin composition will be described in detail below.

[0015] <(A) Epoxy resin> The resin composition of the present invention contains (A) an epoxy resin.

[0016] Examples of the epoxy resin (A) include bixylenol type epoxy resin, bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol S type epoxy resin, bisphenol AF type epoxy resin, dicyclopentadiene type epoxy resin, trisphenol type epoxy resin, naphthol novolac type epoxy resin, phenol novolac type epoxy resin, tert-butyl-catechol type epoxy resin, naphthalene type epoxy resin, naphthol type epoxy resin, anthracene type epoxy resin, glycidylamine type epoxy resin, glycidyl ester type epoxy resin, cresol novolac type epoxy resin, biphenyl type epoxy resin, linear aliphatic epoxy resin, epoxy resin having a butadiene structure, alicyclic epoxy resin, heterocyclic epoxy resin, spiro ring-containing epoxy resin, cyclohexane type epoxy resin, cyclohexane dimethanol type epoxy resin, naphthylene ether type epoxy resin, trimethylol type epoxy resin, tetraphenylethane type epoxy resin, etc. The epoxy resin may be used alone or in combination of two or more types.

[0017] The resin composition preferably contains, as the epoxy resin (A), an epoxy resin having two or more epoxy groups in one molecule. From the viewpoint of significantly obtaining the desired effects of the present invention, the proportion of the epoxy resin having two or more epoxy groups in one molecule is preferably 50% by mass or more, more preferably 60% by mass or more, and particularly preferably 70% by mass or more, based on 100% by mass of the non-volatile components of the epoxy resin (A).

[0018] Epoxy resins include epoxy resins that are liquid at a temperature of 20°C (hereinafter sometimes referred to as "liquid epoxy resins") and epoxy resins that are solid at a temperature of 20°C (hereinafter sometimes referred to as "solid epoxy resins"). In one embodiment, the resin composition of the present invention contains a liquid epoxy resin as the epoxy resin. In one embodiment, the resin composition of the present invention contains a solid epoxy resin as the epoxy resin. The liquid epoxy resin and the solid epoxy resin may be used in combination. It is preferable that the resin composition of the present invention contains only a liquid epoxy resin as the epoxy resin.

[0019] The liquid epoxy resin is preferably a liquid epoxy resin having two or more epoxy groups in one molecule.

[0020] As the liquid epoxy resin, bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol AF type epoxy resin, naphthalene type epoxy resin, glycidyl ester type epoxy resin, glycidyl amine type epoxy resin, phenol novolac type epoxy resin, alicyclic epoxy resin having an ester skeleton, cyclohexane type epoxy resin, cyclohexane dimethanol type epoxy resin, and epoxy resin having a butadiene structure are preferred.

[0021] Specific examples of liquid epoxy resins include "HP4032", "HP4032D", and "HP4032SS" (naphthalene type epoxy resins) manufactured by DIC Corporation; "828US", "828EL", "jER828EL", "825", and "Epikote 828EL" (bisphenol A type epoxy resins) manufactured by Mitsubishi Chemical Corporation; "jER807" and "1750" (bisphenol F type epoxy resins) manufactured by Mitsubishi Chemical Corporation; "jER152" (phenol novolac type epoxy resin) manufactured by Mitsubishi Chemical Corporation; "630" and "630LSD" (glycidylamine type epoxy resins) manufactured by Mitsubishi Chemical Corporation; and "EP-3950S", "EP-3950L", and "EP-3950L" manufactured by ADEKA Corporation. 980S" (glycidylamine type epoxy resin); "ZX1059" (a mixture of bisphenol A type epoxy resin and bisphenol F type epoxy resin) manufactured by Nippon Steel & Sumitomo Metal Chemical Co., Ltd.; "EX-721" (glycidyl ester type epoxy resin) manufactured by Nagase ChemteX Corporation; "Celloxide 2021P (CEL2021P)" (alicyclic epoxy resin having an ester skeleton) manufactured by Daicel Corporation; "PB-3600" manufactured by Daicel Corporation, "JP-100" and "JP-200" (epoxy resin having a butadiene structure) manufactured by Nippon Soda Co., Ltd.; "ZX1658" and "ZX1658GS" (liquid 1,4-glycidylcyclohexane type epoxy resin) manufactured by Nippon Steel & Sumitomo Metal Chemical Co., Ltd. may be used alone or in combination of two or more types.

[0022] As the solid epoxy resin, a solid epoxy resin having three or more epoxy groups in one molecule is preferable, and an aromatic solid epoxy resin having three or more epoxy groups in one molecule is more preferable.

[0023] As the solid epoxy resin, bixylenol type epoxy resin, naphthalene type epoxy resin, naphthalene type tetrafunctional epoxy resin, cresol novolac type epoxy resin, dicyclopentadiene type epoxy resin, trisphenol type epoxy resin, naphthol type epoxy resin, biphenyl type epoxy resin, naphthylene ether type epoxy resin, anthracene type epoxy resin, bisphenol A type epoxy resin, bisphenol AF type epoxy resin, and tetraphenylethane type epoxy resin are preferred.

[0024] Specific examples of solid epoxy resins include "HP4032H" (naphthalene type epoxy resin) manufactured by DIC Corporation; "HP-4700" and "HP-4710" (naphthalene type tetrafunctional epoxy resins) manufactured by DIC Corporation; "N-690" (cresol novolac type epoxy resin) manufactured by DIC Corporation; "N-695" (cresol novolac type epoxy resin) manufactured by DIC Corporation; "HP-7200" (dicyclopentadiene type epoxy resin) manufactured by DIC Corporation; "HP-7200HH" and " HP-7200H, EXA-7311, EXA-7311-G3, EXA-7311-G4, EXA-7311-G4S, HP6000 (naphthylene ether type epoxy resin); EPPN-502H (trisphenol type epoxy resin) manufactured by Nippon Kayaku Co., Ltd.; NC7000L (naphthol novolac type epoxy resin) manufactured by Nippon Kayaku Co., Ltd.; NC3000H, NC3000, NC3000L, NC3100 (biphenyl type epoxy resin) manufactured by Nippon Kayaku Co., Ltd. "Ethanol type epoxy resins" manufactured by Nippon Steel & Sumitomo Metal Chemical Co., Ltd.; "ESN475V" (naphthol type epoxy resins) manufactured by Nippon Steel & Sumitomo Metal Chemical Co., Ltd.; "ESN485" (naphthol novolac type epoxy resins) manufactured by Nippon Steel & Sumitomo Metal Chemical Co., Ltd.; "YX4000H", "YX4000", "YL6121" (biphenyl type epoxy resins) manufactured by Mitsubishi Chemical Corporation; "YX4000HK" (bixylenol type epoxy resins) manufactured by Mitsubishi Chemical Corporation; "YX8800" (anthracene type epoxy resins) manufactured by Mitsubishi Chemical Corporation; " Examples of epoxy resins include "YX7700" (xylene structure-containing novolac type epoxy resin); "PG-100" and "CG-500" manufactured by Osaka Gas Chemicals; "YL7760" (bisphenol AF type epoxy resin) manufactured by Mitsubishi Chemical; "YL7800" (fluorene type epoxy resin) manufactured by Mitsubishi Chemical; "jER1010" (solid bisphenol A type epoxy resin) manufactured by Mitsubishi Chemical; and "jER1031S" (tetraphenylethane type epoxy resin) manufactured by Mitsubishi Chemical. These may be used alone or in combination of two or more.

[0025] When a liquid epoxy resin and a solid epoxy resin are used in combination as the (A) epoxy resin, the mass ratio of the liquid epoxy resin to the solid epoxy resin (liquid epoxy resin / solid epoxy resin) is, in mass ratio, preferably at least 1, more preferably at least 10, and particularly preferably at least 50. When the mass ratio of the liquid epoxy resin to the solid epoxy resin is within this range, the desired effects of the present invention can be significantly obtained.

[0026] The epoxy equivalent of the (A) epoxy resin is preferably 50 g / eq. to 5000 g / eq., more preferably 50 g / eq. to 3000 g / eq., even more preferably 80 g / eq. to 2000 g / eq., and even more preferably 110 g / eq. to 1000 g / eq. When it is in this range, the crosslink density of the cured product of the resin sheet is sufficient, and an insulating layer with small surface roughness can be obtained. The epoxy equivalent is the mass of a resin containing one equivalent of an epoxy group. This epoxy equivalent can be measured according to JIS K7236.

[0027] From the viewpoint of significantly obtaining the desired effects of the present invention, the weight average molecular weight (Mw) of the epoxy resin (A) is preferably 100 to 5000, more preferably 100 to 3000, and further preferably 100 to 1500. The weight average molecular weight of the resin can be measured as a polystyrene-equivalent value by gel permeation chromatography (GPC).

[0028] When the "non-volatile components" in the resin composition are taken as 100% by mass, the content of the (A) epoxy resin is not particularly limited, but from the viewpoint of significantly obtaining the desired effects of the present invention, it is preferably 1% by mass or more, more preferably 2% by mass or more, even more preferably 3% by mass or more, and particularly preferably 4% by mass or more. From the viewpoint of significantly obtaining the desired effects of the present invention, the upper limit is preferably 50% by mass or less, more preferably 30% by mass or less, even more preferably 20% by mass or less, and particularly preferably 10% by mass or less.

[0029] When the "resin component" in the resin composition is taken as 100% by mass, the content of the (A) epoxy resin is not particularly limited, but from the viewpoint of significantly obtaining the desired effects of the present invention, it is preferably 20% by mass or more, more preferably 30% by mass or more, even more preferably 40% by mass or more, and particularly preferably 45% by mass or more. From the viewpoint of significantly obtaining the desired effects of the present invention, the upper limit is preferably 90% by mass or less, more preferably 70% by mass or less, even more preferably 60% by mass or less, and particularly preferably 50% by mass or less.

[0030] In this specification, the term "resin component" refers to all non-volatile components remaining in the resin composition excluding the inorganic filler (C). Therefore, the term "resin component" may also include low molecular weight compounds.

[0031] <(B) Hardener> The resin composition of the present invention contains a curing agent (B). The curing agent (B) has the function of curing the epoxy resin (A).

[0032] When the "non-volatile components" in the resin composition are taken as 100% by mass, the content of the (B) curing agent is not particularly limited, but from the viewpoint of significantly obtaining the desired effects of the present invention, it is preferably 1% by mass or more, more preferably 3% by mass or more, even more preferably 4% by mass or more, and particularly preferably 5% by mass or more. From the viewpoint of significantly obtaining the desired effects of the present invention, the upper limit is preferably 50% by mass or less, more preferably 30% by mass or less, even more preferably 20% by mass or less, and particularly preferably 10% by mass or less.

[0033] When the "resin component" in the resin composition is taken as 100% by mass, the content of the (B) curing agent is not particularly limited, but from the viewpoint of significantly obtaining the desired effects of the present invention, it is preferably 20% by mass or more, more preferably 30% by mass or more, even more preferably 40% by mass or more, and particularly preferably 50% by mass or more. From the viewpoint of significantly obtaining the desired effects of the present invention, the upper limit is preferably 90% by mass or less, more preferably 70% by mass or less, even more preferably 60% by mass or less, and particularly preferably 55% by mass or less.

[0034] In a first embodiment, the (B) curing agent includes (B-1) an active ester resin having a softening point of 100° C. or less. In a second embodiment, the (B) component includes (B-2) a difunctional active ester resin. In a third embodiment, the (B) component includes (B-3) an active ester resin having a molecular weight of 1,000 or less.

[0035] An active ester resin is an ester compound capable of undergoing an addition reaction with the epoxy group of an epoxy resin. An active ester resin has the characteristic of not generating hydroxyl groups in an addition reaction with the epoxy group of an epoxy resin. Therefore, by using an active ester resin as a curing agent, the polar group concentration in the obtained cured product can be reduced, thereby realizing low dielectric properties.

[0036] <(B-1) Active ester resin with a softening point of 100°C or less> The active ester resin of the component (B-1) is not particularly limited as long as it has a softening point of 100° C. or less. The softening point can be measured, for example, by the ring and ball method based on JIS K2351. By using the component (B-1), the uniformity of the composition of the resin composition can be improved, and the occurrence of flow marks can be suppressed. The component (B-1) is preferably a bifunctional active ester resin having a softening point of 100° C. or less (see the explanation below for "bifunctional active ester resin"), and more preferably a bifunctional active ester resin represented by the formula (1):

[0037] [ka]

[0038] [In the formula, rings X, Y and Z each independently represent an aromatic ring which may further have a substituent.] Among the bifunctional active ester resins represented by the formula (2):

[0039] [ka]

[0040] [In the formula, rings A, B, C, D and E each independently represent a benzene ring which may further have a substituent.] Among the bifunctional active ester resins represented by the above formula, the softening point is 100° C. or less.

[0041] In this specification, the term "aromatic ring" refers to a ring that conforms to the Huckel rule in which the number of electrons contained in the π electron system on the ring is 4n+2 (n is a natural number), and examples of such rings include aromatic hydrocarbon rings and aromatic heterocycles.

[0042] In the present specification, the term "aromatic hydrocarbon ring" refers to an aromatic ring having carbon atoms as ring-constituting atoms. The "aromatic hydrocarbon ring" is preferably an aromatic hydrocarbon ring having 6 to 14 carbon atoms, more preferably an aromatic hydrocarbon ring having 6 to 10 carbon atoms. Examples of the "aromatic hydrocarbon ring" include a benzene ring, a naphthalene ring, and an anthracene ring.

[0043] In the present specification, the term "aromatic heterocycle" refers to an aromatic ring containing, as ring-constituting atoms other than carbon atoms, heteroatoms such as nitrogen atoms, sulfur atoms, oxygen atoms, etc. (preferably 1 to 4) The "aromatic heterocycle" preferably includes a 5- to 14-membered aromatic heterocycle, more preferably a 5- to 10-membered aromatic heterocycle. Examples of the "aromatic heterocycle" include 5- or 6-membered monocyclic aromatic heterocycles such as a thiophene ring, a furan ring, a pyrrole ring, an imidazole ring, a pyrazole ring, a thiazole ring, an isothiazole ring, an oxazole ring, an isoxazole ring, a pyridine ring, a pyrazine ring, a pyrimidine ring, a pyridazine ring, a 1,2,4-oxadiazole ring, a 1,3,4-oxadiazole ring, a 1,2,4-thiadiazole ring, a 1,3,4-thiadiazole ring, a triazole ring, a tetrazole ring, and a triazine ring; and 8- to 14-membered fused aromatic heterocycles such as a benzothiophene ring, a benzofuran ring, a benzimidazole ring, a benzoxazole ring, a benzisoxazole ring, a benzothiazole ring, a benzisothiazole ring, and a benzotriazole ring.

[0044] The further substituent in each of the "optionally further substituted aromatic ring" in formula (1) and the "optionally further substituted benzene ring" in formula (2) is not particularly limited, and examples thereof include a halogen atom, an alkyl group, an alkenyl group, an alkoxy group, an alkylcarbonyl group, an aryl group, an aryloxy group, an arylcarbonyl group, an aralkyl group, an aromatic heterocyclic group, and a non-aromatic heterocyclic group.

[0045] In the present specification, examples of the "halogen atom" include a fluorine atom, a chlorine atom, a bromine atom, an iodine atom and the like.

[0046] In the present specification, the term "alkyl group" refers to a linear, branched, or cyclic monovalent aliphatic saturated hydrocarbon group. The number of carbon atoms in the "alkyl group" is preferably 1 to 6, more preferably 1 to 4, and even more preferably 1 to 3. Examples of the "alkyl group" include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, a pentyl group, an isopentyl group, a neopentyl group, a 1-ethylpropyl group, a hexyl group, an isohexyl group, a 1,1-dimethylbutyl group, a 2,2-dimethylbutyl group, a 3,3-dimethylbutyl group, a 2-ethylbutyl group, a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, and a cyclohexyl group.

[0047] In the present specification, the term "alkenyl group" refers to a linear, branched or cyclic monovalent unsaturated aliphatic hydrocarbon group having at least one carbon-carbon double bond. The number of carbon atoms in the "alkenyl group" is preferably 2 to 6, more preferably 2 to 4, and even more preferably 2 or 3. Examples of the "alkenyl group" include ethenyl group, 1-propenyl group, 2-propenyl group, 2-methyl-1-propenyl group, 1-butenyl group, 2-butenyl group, 3-butenyl group, 3-methyl-2-butenyl group, 1-pentenyl group, 2-pentenyl group, 3-pentenyl group, 4-pentenyl group, 4-methyl-3-pentenyl group, 1-hexenyl group, 3-hexenyl group, 5-hexenyl group, cyclobutenyl group, cyclopentenyl group, and cyclohexenyl group.

[0048] In the present specification, the term "alkoxy group" refers to a monovalent group (alkyl-O-) formed by bonding an alkyl group to an oxygen atom. The number of carbon atoms in the "alkoxy group" is preferably 1 to 6, more preferably 1 to 4, and further preferably 1 to 3. Examples of the "alkoxy group" include a methoxy group, an ethoxy group, a propoxy group, an isopropoxy group, a butoxy group, an isobutoxy group, a sec-butoxy group, a tert-butoxy group, a pentyloxy group, and a hexyloxy group.

[0049] In the present specification, the term "alkylcarbonyl group" refers to a monovalent group (alkyl-CO-) formed by bonding an alkyl group to a carbonyl. The number of carbon atoms in the "alkylcarbonyl group" is preferably 2 to 7, more preferably 2 to 5, and further preferably 2 to 4. Examples of the "alkylcarbonyl group" include an acetyl group, a propanoyl group, a butanoyl group, a 2-methylpropanoyl group, a pentanoyl group, a 3-methylbutanoyl group, a 2-methylbutanoyl group, a 2,2-dimethylpropanoyl group, a hexanoyl group, and a heptanoyl group.

[0050] In the present specification, the term "aryl group" refers to a monovalent aromatic hydrocarbon group. The number of carbon atoms in the "aryl group" is preferably 6 to 14, and more preferably 6 to 10. Examples of the "aryl group" include a phenyl group, a 1-naphthyl group, a 2-naphthyl group, a 1-anthryl group, a 2-anthryl group, and a 9-anthryl group.

[0051] In the present specification, the term "aryloxy group" refers to a monovalent group (aryl-O-) formed by bonding an aryl group to an oxygen atom. The number of carbon atoms in the "aryloxy group" is preferably 6 to 14, and more preferably 6 to 10. Examples of the "aryloxy group" include a phenoxy group and a naphthoxy group.

[0052] In the present specification, the term "arylcarbonyl group" refers to a monovalent group (aryl-CO-) formed by bonding an aryl group to a carbonyl. The number of carbon atoms in the "arylcarbonyl group" is preferably 7 to 15, and more preferably 7 to 11. Examples of the "arylcarbonyl group" include a benzoyl group, a 1-naphthoyl group, and a 2-naphthoyl group.

[0053] In the present specification, the term "aralkyl group" refers to an alkyl group substituted with one or more aryl groups. The number of carbon atoms in the "aralkyl group" is preferably 7 to 15, and more preferably 7 to 11. Examples of the "aralkyl group" include a benzyl group, a phenethyl group, and a 2-naphthylmethyl group.

[0054] In the present specification, the term "aromatic heterocyclic group" refers to an aromatic ring group containing, as ring-constituting atoms other than carbon atoms, heteroatoms such as nitrogen atoms, sulfur atoms, oxygen atoms, etc. (preferably 1 to 4) The "aromatic heterocyclic group" preferably includes a 5- to 14-membered aromatic heterocyclic group, more preferably a 5- to 10-membered aromatic heterocyclic group. Examples of the "aromatic heterocyclic group" include 5- or 6-membered monocyclic aromatic heterocyclic groups such as thienyl, furyl, pyrrolyl, imidazolyl, pyrazolyl, thiazolyl, isothiazolyl, oxazolyl, isoxazolyl, pyridyl, pyrazinyl, pyrimidinyl, pyridazinyl, 1,2,4-oxadiazolyl, 1,3,4-oxadiazolyl, 1,2,4-thiadiazolyl, 1,3,4-thiadiazolyl, triazolyl, tetrazolyl, and triazinyl groups; and 8- to 14-membered condensed aromatic heterocyclic groups such as benzothiophenyl, benzofuranyl, benzimidazolyl, benzoxazolyl, benzoisoxazolyl, benzothiazolyl, benzoisothiazolyl, and benzotriazolyl groups.

[0055] In the present specification, the term "non-aromatic heterocyclic group" refers to a non-aromatic ring group containing, as ring-constituting atoms other than carbon atoms, heteroatoms such as nitrogen atoms, sulfur atoms, oxygen atoms, etc. (preferably 1 to 4) as atoms. The "non-aromatic heterocyclic group" preferably includes a 3- to 14-membered non-aromatic heterocyclic group, more preferably a 4- to 10-membered non-aromatic heterocyclic group. Examples of the "non-aromatic heterocyclic group" include an aziridinyl group, an oxiranyl group, a thiiranyl group, an azetidinyl group, an oxetanyl group, a thietanyl group, a tetrahydrothienyl group, a tetrahydrofuranyl group, a pyrrolinyl group, a pyrrolidinyl group, an imidazolinyl group, an imidazolidinyl group, an oxazolinyl group, an oxazolidinyl group, a pyrazolinyl group, a pyrazolidinyl group, a thiazolinyl group, a thiazolidinyl group, a tetrahydroisothiazolyl ... Examples of the heterocyclic groups include 3- to 8-membered monocyclic non-aromatic heterocyclic groups, such as a dihydrooxazolyl group, a tetrahydroisoxazolyl group, a piperidinyl group, and a piperazinyl group; and 9- to 14-membered fused non-aromatic heterocyclic groups, such as a dihydrobenzofuranyl group, a dihydrobenzimidazolyl group, a dihydrobenzoxazolyl group, a dihydrobenzothiazolyl group, a dihydrobenzisothiazolyl group, a dihydronaphtho[2,3-b]thienyl group, and a tetrahydroisoquinolyl group.

[0056] In formula (1), rings X, Y and Z are preferably each independently an aromatic hydrocarbon ring which may further have a substituent, more preferably a benzene ring or naphthalene ring which may further have a substituent, and further preferably an unsubstituted benzene ring or naphthalene ring.

[0057] In formula (2), rings A, B, C, D and E are preferably unsubstituted benzene rings.

[0058] The softening point of the component (B-1) is preferably 90° C. or lower, more preferably 85° C. or lower, and even more preferably 80° C. or lower.

[0059] The molecular weight of the (B-1) component is preferably 1,000 or less, more preferably 700 or less, even more preferably 600 or less, even more preferably 500 or less, and particularly preferably 450 or less. The lower limit is not particularly limited, but may be 200, for example.

[0060] Specific examples of the component (B-1) include those represented by formula (3):

[0061] [ka]

[0062] and the like.

[0063] The component (B-1) may be a commercially available product or may be synthesized by a known method. The component (B-1) may be used alone or in combination of two or more types.

[0064] <(B-2) Bifunctional active ester resin> The active ester resin of the component (B-2) is not particularly limited as long as it is bifunctional. A bifunctional active ester resin means a compound having two ester structures capable of addition reaction with the epoxy group of an epoxy resin. By using the component (B-2), the uniformity of the composition of the resin composition can be improved, so that the occurrence of flow marks can be suppressed. The component (B-2) is preferably a compound represented by the formula (1):

[0065] [ka]

[0066] [In the formula, rings X, Y and Z each independently represent an aromatic ring which may further have a substituent.] More preferably, the bifunctional active ester resin is represented by the formula (2):

[0067] [ka]

[0068] [In the formula, rings A, B, C, D and E each independently represent a benzene ring which may further have a substituent.] It is a bifunctional active ester resin represented by the formula:

[0069] The softening point of the component (B-2) is preferably 100° C. or lower, more preferably 90° C. or lower, even more preferably 85° C. or lower, and particularly preferably 80° C. or lower.

[0070] The molecular weight of the (B-2) component is preferably 1,000 or less, more preferably 700 or less, even more preferably 600 or less, even more preferably 500 or less, and particularly preferably 450 or less. The lower limit is not particularly limited, but may be 200, for example.

[0071] Specific examples of the component (B-2) include those represented by formula (3):

[0072] [ka]

[0073] and the like.

[0074] The component (B-2) may be a commercially available product or may be synthesized by a known method. The component (B-2) may be used alone or in combination of two or more types.

[0075] <(B-3) Active ester resin with molecular weight of 1,000 or less> The active ester resin of the component (B-3) is not particularly limited as long as it has a molecular weight of 1,000 or less. By using the component (B-3), the compositional uniformity of the resin composition can be improved, and the occurrence of flow marks can be suppressed. The component (B-3) is preferably a bifunctional active ester resin having a molecular weight of 1,000 or less (see above for the explanation of "bifunctional active ester resin"), and more preferably a bifunctional active ester resin having a molecular weight of 1,000 or less ... most preferably a bifunctional active ester resin having a molecular weight of 1,000 or less.

[0076] [ka]

[0077] [In the formula, rings X, Y and Z each independently represent an aromatic ring which may further have a substituent.] Among the bifunctional active ester resins represented by the formula (2):

[0078] [ka]

[0079] [In the formula, rings A, B, C, D and E each independently represent a benzene ring which may further have a substituent.] The bifunctional active ester resin has a molecular weight of 1,000 or less.

[0080] The softening point of the component (B-3) is preferably 100° C. or lower, more preferably 90° C. or lower, even more preferably 85° C. or lower, and particularly preferably 80° C. or lower.

[0081] The molecular weight of the (B-3) component is preferably 700 or less, more preferably 600 or less, even more preferably 500 or less, and particularly preferably 450 or less. The lower limit is not particularly limited, but may be 200, for example.

[0082] Specific examples of the component (B-3) include those represented by formula (3):

[0083] [ka]

[0084] and the like.

[0085] The (B-3) component may be a commercially available product or may be synthesized by a known method. The (B-3) component may be used alone or in combination of two or more types.

[0086] When the "non-volatile components" in the resin composition are taken as 100% by mass, the content of the (B-1), (B-2) or (B-3) component is not particularly limited, but from the viewpoint of significantly obtaining the desired effects of the present invention, it is preferably 1% by mass or more, more preferably 1.5% by mass or more, even more preferably 2% by mass or more, still more preferably 2.5% by mass or more, and particularly preferably 3% by mass or more. From the viewpoint of significantly obtaining the desired effects of the present invention, the upper limit is preferably 50% by mass or less, more preferably 20% by mass or less, even more preferably 10% by mass or less, and particularly preferably 5% by mass or less.

[0087] When the "resin component" in the resin composition is taken as 100% by mass, the (B-1), (B-2) or (B-3) component is not particularly limited, but from the viewpoint of significantly obtaining the desired effects of the present invention, it is preferably 10% by mass or more, more preferably 15% by mass or more, even more preferably 20% by mass or more, and particularly preferably 25% by mass or more. From the viewpoint of significantly obtaining the desired effects of the present invention, the upper limit is preferably 60% by mass or less, more preferably 50% by mass or less, even more preferably 45% by mass or less, and particularly preferably 40% by mass or less.

[0088] The mass ratio of the (B-1), (B-2) or (B-3) component to the (B) curing agent is not particularly limited, but from the viewpoint of significantly obtaining the desired effect of the present invention, when the (B) curing agent in the resin composition is taken as 100 mass%, it is preferably 5 mass% or more, more preferably 15 mass% or more, even more preferably 25 mass% or more, and particularly preferably 35 mass% or more. The upper limit is preferably 100 mass% or less, more preferably 90 mass% or less, even more preferably 80 mass% or less, and particularly preferably 75 mass% or less.

[0089] <Optional curing agent other than components (B-1) to (B-3)> The (B) curing agent may further contain any other curing agent in addition to the (B-1), (B-2) or (B-3) component. The optional curing agent other than the (B-1), (B-2) or (B-3) component is not particularly limited as long as it has the function of curing the epoxy resin, and examples thereof include phenol-based curing agents, naphthol-based curing agents, acid anhydride-based curing agents, active ester-based curing agents other than the (B-1), (B-2) or (B-3) components, benzoxazine-based curing agents, cyanate ester-based curing agents, carbodiimide-based curing agents and amine-based curing agents. Among them, phenol-based curing agents, naphthol-based curing agents, amine-based curing agents and acid anhydride-based curing agents are preferred, and acid anhydride-based curing agents are more preferred. Such curing agents may be used alone or in combination of two or more.

[0090] As the phenol-based curing agent and naphthol-based curing agent, from the viewpoint of heat resistance and water resistance, a phenol-based curing agent having a novolac structure or a naphthol-based curing agent having a novolac structure is preferred. Also, from the viewpoint of adhesion to the adherend, a nitrogen-containing phenol-based curing agent or a nitrogen-containing naphthol-based curing agent is preferred, and a triazine skeleton-containing phenol-based curing agent or a triazine skeleton-containing naphthol-based curing agent is more preferred. Among them, from the viewpoint of highly satisfying heat resistance, water resistance, and adhesion, a triazine skeleton-containing phenol novolac resin is preferred. Specific examples of phenol-based curing agents and naphthol-based curing agents include, for example, "MEH-7700", "MEH-7810", and "MEH-7851" manufactured by Meiwa Kasei Co., Ltd., "NHN", "CBN", and "GPH" manufactured by Nippon Kayaku Co., Ltd., "SN-170", "SN-180", "SN-190", "SN-475", "SN-485", "SN-495", "SN-375", and "SN-395" manufactured by Nippon Steel & Sumikin Chemical Co., Ltd., and "LA-7052", "LA-7054", "LA-3018", "LA-3018-50P", "LA-1356", "TD2090", and "TD-2090-60M" manufactured by DIC Corporation.

[0091] Examples of the acid anhydride curing agent include a curing agent having one or more acid anhydride groups in one molecule. Specific examples of the acid anhydride curing agent include phthalic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, methylnadic anhydride, hydrogenated methylnadic anhydride, trialkyltetrahydrophthalic anhydride, dodecenyl succinic anhydride, 5-(2,5-dioxotetrahydro-3-furanyl)-3-methyl-3-cyclohexene-1,2-dicarboxylic anhydride, trimellitic anhydride, pyromellitic anhydride, and benzophenonetetracarboxylic dianhydride. Examples of acid anhydrides include anhydrides, biphenyltetracarboxylic dianhydride, naphthalenetetracarboxylic dianhydride, oxydiphthalic dianhydride, 3,3'-4,4'-diphenylsulfonetetracarboxylic dianhydride, 1,3,3a,4,5,9b-hexahydro-5-(tetrahydro-2,5-dioxo-3-furanyl)-naphtho[1,2-C]furan-1,3-dione, ethylene glycol bis(anhydrotrimellitate), and polymeric acid anhydrides such as styrene-maleic acid resin, which is a copolymer of styrene and maleic acid. Commercially available acid anhydride curing agents include "HNA-100", "MH-700", "MTA-15", "DDSA", "HF-08", and "OSA" manufactured by New Japan Chemical Co., Ltd., "YH306" and "YH307" manufactured by Mitsubishi Chemical Corporation, "H-TMAn" manufactured by Mitsubishi Gas Chemical Company, Inc., and "HN-2200", "HN-2000", "HN-5500", and "MHAC-P" manufactured by Hitachi Chemical Co., Ltd.

[0092] The active ester curing agent other than the (B-1), (B-2) or (B-3) component is not particularly limited, but generally, compounds having three or more highly reactive ester groups in one molecule, such as phenol esters, thiophenol esters, N-hydroxyamine esters, and esters of heterocyclic hydroxy compounds, are preferably used. The active ester curing agent is preferably one obtained by a condensation reaction between a carboxylic acid compound and / or a thiocarboxylic acid compound and a hydroxy compound and / or a thiol compound. In particular, from the viewpoint of improving heat resistance, an active ester curing agent obtained from a carboxylic acid compound and a hydroxy compound is preferred, and an active ester curing agent obtained from a carboxylic acid compound and a phenol compound and / or a naphthol compound is more preferred. Examples of the carboxylic acid compound include compounds having three or more carboxy groups. Examples of phenol compounds or naphthol compounds include hydroquinone, resorcin, bisphenol A, bisphenol F, bisphenol S, phenolphthaline, methylated bisphenol A, methylated bisphenol F, methylated bisphenol S, phenol, o-cresol, m-cresol, p-cresol, catechol, α-naphthol, β-naphthol, 1,5-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, dihydroxybenzophenone, trihydroxybenzophenone, tetrahydroxybenzophenone, phloroglucin, benzenetriol, dicyclopentadiene-type diphenol compounds, phenol novolac, etc. Here, the term "dicyclopentadiene-type diphenol compounds" refers to diphenol compounds obtained by condensing one molecule of dicyclopentadiene with two molecules of phenol.

[0093] Specifically, active ester compounds containing a dicyclopentadiene-type diphenol structure, active ester compounds containing a naphthalene structure, active ester compounds containing an acetylated product of phenol novolac, and active ester compounds containing a benzoylated product of phenol novolac are preferred, and among these, active ester compounds containing a naphthalene structure and active ester compounds containing a dicyclopentadiene-type diphenol structure are more preferred. The "dicyclopentadiene-type diphenol structure" refers to a divalent structural unit consisting of phenylene-dicyclopentalene-phenylene.

[0094] Commercially available active ester curing agents other than the component (B-1), the component (B-2) or the component (B-3) include active ester compounds containing a dicyclopentadiene-type diphenol structure, such as "EXB9451", "EXB9460", "EXB9460S", "HPC-8000", "HPC-8000H", "HPC-8000-65T", "HPC-8000H-65TM", "EXB-8000L", and "EXB-8000L-65TM" (manufactured by DIC Corporation); and active ester compounds containing a naphthalene structure, such as "EXB9416-70BK" and "EXB-8150-65T" (manufactured by DIC Corporation). Examples of active ester compounds that contain an acetylated phenol novolac include "DC808" (manufactured by Mitsubishi Chemical Corporation); active ester compounds that contain a benzoylated phenol novolac include "YLH1026" (manufactured by Mitsubishi Chemical Corporation); active ester curing agents that are acetylated phenol novolac include "DC808" (manufactured by Mitsubishi Chemical Corporation); and active ester curing agents that are benzoylated phenol novolac include "YLH1026" (manufactured by Mitsubishi Chemical Corporation), "YLH1030" (manufactured by Mitsubishi Chemical Corporation), and "YLH1048" (manufactured by Mitsubishi Chemical Corporation).

[0095] Specific examples of benzoxazine-based curing agents include "JBZ-OP100D" and "ODA-BOZ" manufactured by JFE Chemical Corporation; "HFB2006M" manufactured by Showa Polymer Co., Ltd.; and "Pd" and "Fa" manufactured by Shikoku Chemical Industry Co., Ltd.

[0096] Examples of the cyanate ester curing agent include bifunctional cyanate resins such as bisphenol A dicyanate, polyphenol cyanate (oligo(3-methylene-1,5-phenylene cyanate)), 4,4'-methylenebis(2,6-dimethylphenyl cyanate), 4,4'-ethylidene diphenyl dicyanate, hexafluorobisphenol A dicyanate, 2,2-bis(4-cyanate)phenylpropane, 1,1-bis(4-cyanate phenylmethane), bis(4-cyanate-3,5-dimethylphenyl)methane, 1,3-bis(4-cyanate phenyl-1-(methylethylidene))benzene, bis(4-cyanate phenyl)thioether, and bis(4-cyanate phenyl)ether; polyfunctional cyanate resins derived from phenol novolac and cresol novolac; and prepolymers in which these cyanate resins are partially converted to triazine. Specific examples of cyanate ester-based curing agents include "PT30" and "PT60" (both of which are phenol novolac-type multifunctional cyanate ester resins), "BA230" and "BA230S75" (prepolymers in which part or all of bisphenol A dicyanate has been converted to triazine to form a trimer), all of which are manufactured by Lonza Japan.

[0097] Specific examples of carbodiimide-based curing agents include "V-03" and "V-07" manufactured by Nisshinbo Chemical Inc.

[0098] The amine-based curing agent may be a curing agent having one or more amino groups in one molecule, such as aliphatic amines, polyether amines, alicyclic amines, aromatic amines, etc., and among them, aromatic amines are preferred from the viewpoint of achieving the desired effects of the present invention. The amine-based curing agent is preferably a primary amine or a secondary amine, and more preferably a primary amine. Specific examples of amine-based curing agents include 4,4'-methylenebis(2,6-dimethylaniline), diphenyldiaminosulfone, 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylsulfone, 3,3'-diaminodiphenylsulfone, m-phenylenediamine, m-xylylenediamine, diethyltoluenediamine, 4,4'-diaminodiphenylether, 3,3'-dimethyl-4,4'-diaminobiphenyl, 2,2'-dimethyl-4,4'-diaminobiphenyl, 3,3'-dihydroxybenzidine, 2,2-bis(3-amino-4-hydroxyphenyl)propanediamine, and the like. bis(4-aminophenyl)propane, 3,3-dimethyl-5,5-diethyl-4,4-diphenylmethanediamine, 2,2-bis(4-aminophenyl)propane, 2,2-bis(4-(4-aminophenoxy)phenyl)propane, 1,3-bis(3-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, 4,4'-bis(4-aminophenoxy)biphenyl, bis(4-(4-aminophenoxy)phenyl)sulfone, bis(4-(3-aminophenoxy)phenyl)sulfone, etc. The amine-based curing agent may be a commercially available product, for example, "KAYABOND C-200S", "KAYABOND C-100", "KAYAHARD AA", "KAYAHARD AB", "KAYAHARD AS" manufactured by Nippon Kayaku Co., Ltd., and "Epicure W" manufactured by Mitsubishi Chemical Corporation.

[0099] When the resin composition contains any curing agent other than the (B-1), (B-2) or (B-3) component, the content of the any curing agent other than the (B-1), (B-2) or (B-3) component is not particularly limited, but is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, even more preferably 1% by mass or more, and particularly preferably 1.5% by mass or more, when the "non-volatile components" in the resin composition are 100% by mass. The upper limit is preferably 50% by mass or less, more preferably 20% by mass or less, even more preferably 10% by mass or less, and particularly preferably 5% by mass or less.

[0100] When the resin composition contains any curing agent other than the (B-1), (B-2) or (B-3) component, the content of the any curing agent other than the (B-1), (B-2) or (B-3) component is not particularly limited, but is preferably 1% by mass or more, more preferably 5% by mass or more, even more preferably 10% by mass or more, and particularly preferably 15% by mass or more, when the "resin component" in the resin composition is 100% by mass. The upper limit is preferably 60% by mass or less, more preferably 50% by mass or less, even more preferably 40% by mass or less, and particularly preferably 30% by mass or less.

[0101] The ratio of the amount of the epoxy resin (A) to the curing agent (B) is preferably 1:0.2 to 1:2, more preferably 1:0.3 to 1:1.5, and even more preferably 1:0.4 to 1:1.2, in terms of the ratio of [total number of epoxy groups in the epoxy resin] to [total number of reactive groups in the curing agent]. Here, the reactive groups in the curing agent are active hydroxyl groups, active ester groups, etc., and vary depending on the type of curing agent. The total number of epoxy groups in the epoxy resin is the total value of the non-volatile component mass of each epoxy resin divided by the epoxy equivalent weight, and the total number of reactive groups in the curing agent is the total value of the non-volatile component mass of each curing agent divided by the reactive group equivalent weight, for all curing agents. By setting the ratio of the amount of the epoxy resin to the curing agent in this range, the heat resistance of the obtained cured product is further improved.

[0102] <(C) Inorganic filler> The resin composition of the present invention contains (C) an inorganic filler.

[0103] The material of the (C) inorganic filler is not particularly limited, but examples thereof include silica, alumina, glass, cordierite, silicon oxide, barium sulfate, barium carbonate, talc, clay, mica powder, zinc oxide, hydrotalcite, boehmite, aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, magnesium oxide, boron nitride, aluminum nitride, manganese nitride, aluminum borate, strontium carbonate, strontium titanate, calcium titanate, magnesium titanate, bismuth titanate, titanium oxide, zirconium oxide, barium titanate, barium zirconate titanate, barium zirconate, calcium zirconate, zirconium phosphate, and zirconium tungstate phosphate, and silica and alumina are particularly preferred. Examples of silica include amorphous silica, fused silica, crystalline silica, synthetic silica, and hollow silica. As the silica, spherical silica is preferred. The (C) inorganic filler may be used alone or in combination of two or more.

[0104] (C) Commercially available inorganic fillers include, for example, "UFP-30" manufactured by Denka Chemical Industry Co., Ltd.; "SP60-05" and "SP507-05" manufactured by Nippon Steel & Sumikin Materials Co., Ltd.; "YC100C", "YA050C", "YA050C-MJE", "YA010C", "FE9 series", "FEB series", and "FED series" manufactured by Admatechs Co., Ltd.; "UFP-30" manufactured by Denka Company, Limited; "Silfill NSS-3N", "Silfill NSS-4N", and "Silfill NSS-5N" manufactured by Tokuyama Corporation; and "SC2500SQ", "SO-C4", "SO-C2", and "SO-C1" manufactured by Admatechs Co., Ltd.

[0105] (C) The average particle size of the inorganic filler is not particularly limited, but from the viewpoint of suppressing the occurrence of flow marks, it is preferably 40 μm or less, more preferably 30 μm or less, even more preferably 25 μm or less, even more preferably 20 μm or less, and particularly preferably 15 μm or less. The lower limit of the average particle size of the inorganic filler is not particularly limited, but is preferably 0.1 μm or more, more preferably 1 μm or more, even more preferably 3 μm or more, even more preferably 5 μm or more, even more preferably 7 μm or more, and particularly preferably 8 μm or more. The average particle size of the inorganic filler can be measured by a laser diffraction / scattering method based on the Mie scattering theory. Specifically, the particle size distribution of the inorganic filler is created on a volume basis using a laser diffraction / scattering type particle size distribution measuring device, and the median diameter is used as the average particle size. The measurement sample can be prepared by weighing 100 mg of the inorganic filler and 10 g of methyl ethyl ketone into a vial and dispersing it by ultrasonic waves for 10 minutes. The measurement sample was measured using a laser diffraction type particle size distribution measuring device with blue and red light source wavelengths, and the particle size distribution of the inorganic filler on a volume basis was measured using a flow cell method, and the average particle size was calculated as the median diameter from the particle size distribution obtained. An example of a laser diffraction type particle size distribution measuring device is the "LA-960" manufactured by Horiba, Ltd.

[0106] From the viewpoint of improving moisture resistance and dispersibility, the (C) inorganic filler is preferably treated with one or more surface treatment agents such as aminosilane coupling agents, epoxysilane coupling agents, mercaptosilane coupling agents, alkoxysilane compounds, organosilazane compounds, titanate coupling agents, etc. Commercially available surface treatment agents include, for example, Shin-Etsu Chemical Co., Ltd.'s "KBM403" (3-glycidoxypropyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM803" (3-mercaptopropyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBE903" (3-aminopropyltriethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM573" (N-phenyl-3-aminopropyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "SZ-31" (hexamethyldisilazane), Shin-Etsu Chemical Co., Ltd.'s "KBE903" (3-aminopropyltriethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM573" (N-phenyl-3-aminopropyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBE903" (3-aminopropyltriethoxy ... Examples of the silane coupling agent include "KBM103" (phenyltrimethoxysilane) manufactured by Etsu Chemical Co., Ltd., "KBM-4803" (long-chain epoxy type silane coupling agent) manufactured by Shin-Etsu Chemical Co., Ltd., "KBM-7103" (3,3,3-trifluoropropyltrimethoxysilane) manufactured by Shin-Etsu Chemical Co., Ltd., "KBM503" (3-methacryloxypropyltrimethoxysilane) manufactured by Shin-Etsu Chemical Co., Ltd., and "KBM5783" (N-phenyl-3-aminooctyltrimethoxysilane) manufactured by Shin-Etsu Chemical Co., Ltd.

[0107] The degree of surface treatment with the surface treatment agent is preferably within a predetermined range from the viewpoint of improving the dispersibility of the inorganic filler. Specifically, 100% by mass of the inorganic filler is preferably surface-treated with 0.2% to 5% by mass of the surface treatment agent, more preferably 0.2% to 3% by mass, and even more preferably 0.3% to 2% by mass.

[0108] The degree of surface treatment with the surface treatment agent can be evaluated by the amount of carbon per unit surface area of ​​the inorganic filler. From the viewpoint of improving the dispersibility of the inorganic filler, the amount of carbon per unit surface area of ​​the inorganic filler is set to 0.02 mg / m 2 More than 0.1 mg / m is preferable. 2 More preferably, 0.2 mg / m or more 2On the other hand, from the viewpoint of preventing an increase in the melt viscosity of the resin varnish or the melt viscosity in the form of a sheet, it is more preferable that the content be 1 mg / m 2 Less than 0.8 mg / m is preferred. 2 Less than 0.5 mg / m is more preferable. 2 The following is even more preferred:

[0109] (C) The amount of carbon per unit surface area of ​​the inorganic filler can be measured after the surface-treated inorganic filler is washed with a solvent (e.g., methyl ethyl ketone (MEK)). Specifically, a sufficient amount of MEK as a solvent is added to the inorganic filler that has been surface-treated with a surface treatment agent, and ultrasonic cleaning is performed at 25°C for 5 minutes. After removing the supernatant and drying the solid content, the amount of carbon per unit surface area of ​​the inorganic filler can be measured using a carbon analyzer. As the carbon analyzer, the "EMIA-320V" manufactured by Horiba, Ltd., or the like can be used.

[0110] From the viewpoint of further improving the effects of the present invention, the specific surface area of ​​the (C) inorganic filler is preferably 0.01 m 2 / g or more, more preferably 0.1m 2 / g or more, particularly preferably 0.2m 2 / g or more. There is no particular upper limit, but it is preferably 50m 2 / g or less, more preferably 20m 2 / g or less, 10m 2 / g or less or 5m 2 The specific surface area of ​​the inorganic filler is obtained by adsorbing nitrogen gas onto the surface of a sample using a specific surface area measuring device (Macsorb HM-1210 manufactured by Mountech Co., Ltd.) according to the BET method, and calculating the specific surface area using the BET multipoint method.

[0111] The content of the (C) inorganic filler is not particularly limited, but is preferably 20% by mass or more, more preferably 50% by mass or more, even more preferably 70% by mass or more, and particularly preferably 80% by mass or more, when the "non-volatile components" in the resin composition are 100% by mass. The upper limit is not particularly limited, but may be, for example, 98% by mass or less, 95% by mass or less, 92% by mass or less, 90% by mass or less, etc.

[0112] <(D) Curing accelerator> The resin composition of the present invention may contain (D) a curing accelerator as an optional component.

[0113] (D) Examples of the curing accelerator include phosphorus-based curing accelerators, amine-based curing accelerators, imidazole-based curing accelerators, guanidine-based curing accelerators, and metal-based curing accelerators. Among them, phosphorus-based curing accelerators, amine-based curing accelerators, imidazole-based curing accelerators, and metal-based curing accelerators are preferred, amine-based curing accelerators, imidazole-based curing accelerators, and metal-based curing accelerators are more preferred, and imidazole-based curing accelerators are particularly preferred. The curing accelerator may be used alone or in combination of two or more types.

[0114] Examples of phosphorus-based curing accelerators include triphenylphosphine, phosphonium borate compounds, tetraphenylphosphonium tetraphenylborate, n-butylphosphonium tetraphenylborate, tetrabutylphosphonium decanoate, (4-methylphenyl)triphenylphosphonium thiocyanate, tetraphenylphosphonium thiocyanate, and butyltriphenylphosphonium thiocyanate.

[0115] Examples of the amine curing accelerator include trialkylamines such as triethylamine and tributylamine, 4-dimethylaminopyridine (DMAP), benzyldimethylamine, 2,4,6-tris(dimethylaminomethyl)phenol, and 1,8-diazabicyclo(5,4,0)-undecene, with 4-dimethylaminopyridine being preferred.

[0116] Examples of the imidazole-based curing accelerator include 2-methylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, and 1-benzyl-2-methylimidazole. Phenylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazolium trimellitate, 1-cyanoethyl-2-phenylimidazolium trimellitate, 2,4-diamino-6-[2'-methylimidazolyl -(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-undecylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, 2-phenylimidazole isocyanuric acid adduct imidazole compounds such as 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 2,3-dihydro-1H-pyrrolo[1,2-a]benzimidazole, 1-dodecyl-2-methyl-3-benzylimidazolium chloride, 2-methylimidazoline, and 2-phenylimidazoline, as well as adducts of imidazole compounds and epoxy resins.

[0117] As the imidazole-based curing accelerator, a commercially available product may be used, for example, "P200-H50" manufactured by Mitsubishi Chemical Corporation.

[0118] Examples of the guanidine curing accelerator include dicyandiamide, 1-methylguanidine, 1-ethylguanidine, 1-cyclohexylguanidine, 1-phenylguanidine, 1-(o-tolyl)guanidine, dimethylguanidine, diphenylguanidine, trimethylguanidine, tetramethylguanidine, pentamethylguanidine, 1,5,7-triazabicyclo[4.4.0]dec-5-ene, 7-methyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene, 1-methylbiguanide, 1-ethylbiguanide, 1-n-butylbiguanide, 1-n-octadecylbiguanide, 1,1-dimethylbiguanide, 1,1-diethylbiguanide, 1-cyclohexylbiguanide, 1-allylbiguanide, 1-phenylbiguanide, and 1-(o-tolyl)biguanide.

[0119] Examples of metal-based curing accelerators include organometallic complexes or organometallic salts of metals such as cobalt, copper, zinc, iron, nickel, manganese, and tin. Specific examples of organometallic complexes include organocobalt complexes such as cobalt(II) acetylacetonate and cobalt(III) acetylacetonate, organocopper complexes such as copper(II) acetylacetonate, organozinc complexes such as zinc(II) acetylacetonate, organoiron complexes such as iron(III) acetylacetonate, organonickel complexes such as nickel(II) acetylacetonate, and organomanganese complexes such as manganese(II) acetylacetonate. Examples of organometallic salts include zinc octylate, tin octylate, zinc naphthenate, cobalt naphthenate, tin stearate, and zinc stearate.

[0120] When the resin composition contains the (D) curing accelerator, the content of the (D) curing accelerator is not particularly limited, but is preferably 0.001% by mass or more, more preferably 0.01% by mass or more, even more preferably 0.05% by mass or more, and particularly preferably 0.1% by mass or more, when the "non-volatile components" in the resin composition are 100% by mass. The upper limit is preferably 2% by mass or less, more preferably 1% by mass or less, even more preferably 0.5% by mass or less, and particularly preferably 0.2% by mass or less.

[0121] When the resin composition contains the (D) curing accelerator, the content of the (D) curing accelerator is not particularly limited, but is preferably 0.001% by mass or more, more preferably 0.01% by mass or more, even more preferably 0.1% by mass or more, and particularly preferably 0.5% by mass or more, when the "resin component" in the resin composition is 100% by mass. The upper limit is preferably 5% by mass or less, more preferably 2% by mass or less, even more preferably 1% by mass or less, and particularly preferably 0.6% by mass or less.

[0122] <(E) Organic solvent> The resin composition of the present invention may further contain (E) an organic solvent as an optional volatile component.

[0123] Examples of organic solvents include ketone-based solvents such as acetone, methyl ethyl ketone, and cyclohexanone; ester-based solvents such as ethyl acetate, butyl acetate, cellosolve acetate, propylene glycol monomethyl ether acetate, carbitol acetate, ethyl diglycol acetate, and γ-butyrolactone; carbitol solvents such as cellosolve and butyl carbitol; aromatic hydrocarbon-based solvents such as benzene, toluene, xylene, ethylbenzene, and trimethylbenzene; amide-based solvents such as dimethylformamide, dimethylacetamide (DMAc), and N-methylpyrrolidone; alcohol-based solvents such as methanol, ethanol, and 2-methoxypropanol; and hydrocarbon-based solvents such as cyclohexane and methylcyclohexane. The organic solvents may be used alone or in combination of two or more at any ratio.

[0124] <(F) Other additives> The resin composition may further contain other additives as optional components in addition to the above-mentioned components. Examples of such additives include organic fillers, thickeners, defoamers, leveling agents, adhesion promoters, polymerization initiators, and flame retardants. These additives may be used alone or in combination of two or more. The content of each additive can be appropriately set by a person skilled in the art.

[0125] <Method of producing resin composition> In one embodiment, the resin composition of the present invention can be produced, for example, by a method including a step of adding and mixing (A) an epoxy resin, (B) a curing agent, (C) an inorganic filler, if necessary (D) a curing accelerator, if necessary (E) an organic solvent, and if necessary (F) other additives in any order and / or all at the same time to a reaction vessel to obtain a resin composition.

[0126] In the above steps, the temperature during the process of adding each component can be appropriately set, and heating and / or cooling may be performed temporarily or throughout the process of adding each component. Stirring or shaking may be performed during the process of adding each component. In addition, it is preferable to further include a step of stirring the resin composition using a stirring device such as a mixer to uniformly disperse the resin composition after the above steps.

[0127] <Characteristics of resin composition> The resin composition of the present invention comprises (A) an epoxy resin, (B) a curing agent, and (C) an inorganic filler, and the (B) component comprises (B-1) an active ester resin having a softening point of 100° C. or less, (B-2) a difunctional active ester resin, or (B-3) an active ester resin having a molecular weight of 1,000 or less, so that a cured product can be obtained in which the dielectric properties are reduced and the occurrence of flow marks is suppressed. In one embodiment, the resin composition of the present invention can provide a cured product having adhesion to semiconductor chips that can be maintained for a long period of time and an excellent storage modulus.

[0128] Regarding the low dielectric properties, which is one of the characteristics of the cured product of the resin composition of the present invention, in one embodiment, for example, the dielectric loss tangent (tan δ) of the cured product obtained by thermally curing the resin composition, measured by the Fabry-Perot method (measurement frequency 79 GHz), is preferably 0.01 or less, more preferably 0.005 or less, even more preferably 0.004 or less, and particularly preferably 0.003 or less. The lower limit of the dielectric loss tangent is not particularly limited, but may be 0.001 or more, 0.0001 or more, 0.00001 or more, etc.

[0129] Regarding adhesion to semiconductor chips that can be maintained over a long period of time, which is one of the characteristics of the cured product of the resin composition of the present invention in one embodiment, even when a resin composition layer formed from the resin composition is compression molded on a silicon wafer and thermally cured, and then subjected to a high temperature and high humidity environmental test (HAST) for 100 hours under conditions of 130°C and 85% RH, no peeling occurs at the interface between the cured product of the resin composition layer and the underlying silicon wafer.

[0130] Regarding the excellent storage modulus, which is one of the characteristics of the cured product of the resin composition of the present invention in one embodiment, for example, the storage modulus at 25°C of the layered cured product obtained by thermally curing the resin composition, measured under conditions of a frequency of 1 Hz and a heating rate of 5°C / min, is preferably 40 GPa or less, more preferably 30 GPa or less, and even more preferably 25 GPa or less. The lower limit of the storage modulus is not particularly limited, but may be 10 GPa or more, 1 GPa or more, 0.1 GPa or more, etc.

[0131] In one embodiment, the resin composition of the present invention is compression molded to form a resin composition layer, and even after heating for 60 minutes at 150° C., no flow marks are generated on the surface of the resin composition layer. In one embodiment, the resin composition of the present invention has a flowable liquid property at 25° C.

[0132] <Applications of resin composition> The cured product of the resin composition of the present invention is useful for semiconductor encapsulation and insulating layers due to the above-mentioned advantages, and therefore the resin composition can be used as a resin composition for semiconductor encapsulation or insulating layers.

[0133] For example, the resin composition of the present invention can be suitably used as a resin composition for forming an insulating layer of a semiconductor chip package (a resin composition for an insulating layer of a semiconductor chip package) and a resin composition for forming an insulating layer of a circuit board (including a printed wiring board) (a resin composition for an insulating layer of a circuit board).

[0134] Furthermore, for example, the resin composition of the present invention can be suitably used as a resin composition for encapsulating a semiconductor chip in a semiconductor chip package (a resin composition for encapsulating a semiconductor chip).

[0135] Examples of semiconductor chip packages to which a sealing layer or insulating layer formed from a cured product of the resin composition of the present invention can be applied include FC-CSP, MIS-BGA package, ETS-BGA package, Fan-out type WLP (Wafer Level Package), Fan-in type WLP, Fan-out type PLP (Panel Level Package), and Fan-in type PLP.

[0136] The resin composition of the present invention may also be used as an underfill material, for example, as a material for MUF (molding under filling) that is used after a semiconductor chip is connected to a substrate.

[0137] Furthermore, the resin composition of the present invention can be used in a wide range of applications in which resin compositions are used, such as sheet-like laminate materials such as resin sheets and prepregs, liquid materials such as resin inks for solder resists and the like, die bonding materials, hole filling resins, and component embedding resins.

[0138] <Resin sheet> The resin sheet of the present invention has a support and a resin composition layer provided on the support. The resin composition layer is a layer containing the resin composition of the present invention and is usually formed of a resin composition.

[0139] From the viewpoint of thinning, the thickness of the resin composition layer is preferably 600 μm or less, more preferably 500 μm or less. The lower limit of the thickness of the resin composition layer is preferably 1 μm or more, 5 μm or more, more preferably 10 μm or more, even more preferably 50 μm or more, and particularly preferably 100 μm or more.

[0140] The thickness of the cured product obtained by curing the resin composition layer is preferably 1 μm or more, 5 μm or more, more preferably 10 μm or more, further preferably 50 μm or more, and particularly preferably 100 μm or more.

[0141] Examples of the support include films made of plastic materials, metal foils, and release papers, with films made of plastic materials and metal foils being preferred.

[0142] When a film made of a plastic material is used as the support, examples of the plastic material include polyesters such as polyethylene terephthalate (hereinafter sometimes abbreviated as "PET") and polyethylene naphthalate (hereinafter sometimes abbreviated as "PEN"); polycarbonate (hereinafter sometimes abbreviated as "PC"); acrylic polymers such as polymethyl methacrylate (hereinafter sometimes abbreviated as "PMMA"); cyclic polyolefins; triacetyl cellulose (hereinafter sometimes abbreviated as "TAC"); polyether sulfide (hereinafter sometimes abbreviated as "PES"); polyether ketone; polyimide; and the like. Among these, polyethylene terephthalate and polyethylene naphthalate are preferred, and inexpensive polyethylene terephthalate is particularly preferred.

[0143] When a metal foil is used as the support, examples of the metal foil include copper foil and aluminum foil. Among them, copper foil is preferable. As the copper foil, a foil made of a single metal of copper may be used, or a foil made of an alloy of copper and another metal (e.g., tin, chromium, silver, magnesium, nickel, zirconium, silicon, titanium, etc.) may be used.

[0144] The surface of the support to be bonded to the resin composition layer may be subjected to a matte treatment, a corona treatment, an antistatic treatment or the like.

[0145] In addition, the support may be a support with a release layer having a release layer on the surface to be bonded to the resin composition layer. Examples of the release agent used in the release layer of the support with a release layer include one or more release agents selected from the group consisting of alkyd resins, polyolefin resins, urethane resins, and silicone resins. Examples of commercially available release agents include alkyd resin-based release agents such as "SK-1", "AL-5", and "AL-7" manufactured by Lintec Corporation. Examples of the support with a release layer include "Lumirror T60" manufactured by Toray Industries, Inc.; "Purex" manufactured by Teijin Limited; and "Unipeel" manufactured by Unitika Limited.

[0146] The thickness of the support is preferably in the range of 5 μm to 75 μm, more preferably in the range of 10 μm to 60 μm. When a support with a release layer is used, the total thickness of the support with a release layer is preferably in the above range.

[0147] The resin sheet can be produced, for example, by applying the resin composition onto a support using a coating device such as a die coater. If necessary, the resin composition may be dissolved in an organic solvent to prepare a resin varnish, and the resin sheet may be produced by applying the resin varnish. By using a solvent, the viscosity can be adjusted to improve the coatability. When the resin varnish is used, the resin varnish is usually dried after application to form a resin composition layer.

[0148] Drying may be performed by a known method such as heating or hot air blowing. Drying conditions are such that the content of the organic solvent in the resin composition layer is usually 10% by mass or less, preferably 5% by mass or less. Although it varies depending on the boiling point of the organic solvent in the resin varnish, for example, when a resin varnish containing 30% by mass to 60% by mass of the organic solvent is used, the resin composition layer can be formed by drying at 50°C to 150°C for 3 minutes to 10 minutes.

[0149] The resin sheet may include any layer other than the support and the resin composition layer as necessary. For example, in the resin sheet, a protective film similar to that of the support may be provided on the surface of the resin composition layer not bonded to the support (i.e., the surface opposite to the support). The thickness of the protective film is, for example, 1 μm to 40 μm. The protective film can prevent the adhesion of dirt and the like to the surface of the resin composition layer and scratches. When the resin sheet has a protective film, the resin sheet can be used by peeling off the protective film. In addition, the resin sheet can be stored by being wound into a roll.

[0150] The resin sheet can be suitably used to form an insulating layer in the manufacture of a semiconductor chip package (resin sheet for insulating a semiconductor chip package). For example, the resin sheet can be used to form an insulating layer of a circuit board (resin sheet for insulating a circuit board). Examples of packages using such boards include FC-CSP, MIS-BGA packages, and ETS-BGA packages.

[0151] The resin sheet can also be suitably used to seal a semiconductor chip (semiconductor chip sealing resin sheet). Applicable semiconductor chip packages include, for example, fan-out type WLP, fan-in type WLP, fan-out type PLP, fan-in type PLP, etc.

[0152] The resin sheet may also be used as a material for the MUF that is used after the semiconductor chip is connected to the substrate.

[0153] Furthermore, the resin sheet can be used in a wide range of other applications requiring high insulation reliability, for example, the resin sheet can be suitably used to form an insulating layer of a circuit board such as a printed wiring board.

[0154] <Circuit board> The circuit board of the present invention includes an insulating layer formed from a cured product of the resin composition of the present invention. The circuit board can be produced, for example, by a production method including the following steps (1) and (2). (1) A step of forming a resin composition layer on a substrate. (2) A step of thermally curing the resin composition layer to form an insulating layer.

[0155] In step (1), a substrate is prepared. Examples of the substrate include glass epoxy substrates, metal substrates (such as stainless steel and cold-rolled steel sheet (SPCC)), polyester substrates, polyimide substrates, BT resin substrates, and thermosetting polyphenylene ether substrates. The substrate may have a metal layer such as copper foil on the surface as a part of the substrate. For example, a substrate having a peelable first metal layer and a peelable second metal layer on both surfaces may be used. When such a substrate is used, a conductor layer as a wiring layer that can function as a circuit wiring is usually formed on the surface of the second metal layer opposite to the first metal layer. Examples of substrates having such a metal layer include "Micro Thin", an ultra-thin copper foil with a carrier copper foil manufactured by Mitsui Mining & Smelting Co., Ltd.

[0156] A conductor layer may be formed on one or both surfaces of the substrate. In the following description, a member including a substrate and a conductor layer formed on the substrate surface may be referred to as a "substrate with wiring layer" as appropriate. Examples of the conductor material included in the conductor layer include materials including one or more metals selected from the group consisting of gold, platinum, palladium, silver, copper, aluminum, cobalt, chromium, zinc, nickel, titanium, tungsten, iron, tin, and indium. The conductor material may be a single metal or an alloy. Examples of the alloy include alloys of two or more metals selected from the above group (e.g., nickel-chromium alloy, copper-nickel alloy, and copper-titanium alloy). Among them, from the viewpoints of versatility, cost, and ease of patterning in the formation of the conductor layer, chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver, or copper as single metals; and alloys of nickel-chromium alloy, copper-nickel alloy, and copper-titanium alloy as alloys; are preferred. Among these, the single metals chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver and copper; and nickel-chromium alloys; are more preferable, and the single metal copper is particularly preferable.

[0157] The conductor layer may be patterned, for example, to function as a wiring layer. In this case, the line (circuit width) / space (width between circuits) ratio of the conductor layer is not particularly limited, but is preferably 20 / 20 μm or less (i.e., pitch is 40 μm or less), more preferably 10 / 10 μm or less, even more preferably 5 / 5 μm or less, even more preferably 1 / 1 μm or less, and particularly preferably 0.5 / 0.5 μm or more. The pitch does not need to be the same throughout the conductor layer. The minimum pitch of the conductor layer may be, for example, 40 μm or less, 36 μm or less, or 30 μm or less.

[0158] The thickness of the conductor layer depends on the design of the circuit board, but is preferably 3 μm to 35 μm, more preferably 5 μm to 30 μm, further preferably 10 μm to 20 μm, and particularly preferably 15 μm to 20 μm.

[0159] The conductor layer can be formed, for example, by a method including a step of laminating a dry film (photosensitive resist film) on a substrate, a step of forming a pattern by exposing and developing the dry film under predetermined conditions using a photomask to obtain a patterned dry film, a step of forming a conductor layer by a plating method such as electrolytic plating using the developed patterned dry film as a plating mask, and a step of peeling off the patterned dry film. As the dry film, a photosensitive dry film made of a photoresist composition can be used, and for example, a dry film formed of a resin such as a novolac resin or an acrylic resin can be used. The lamination conditions of the substrate and the dry film can be the same as the lamination conditions of the substrate and the resin sheet described later. The peeling off of the dry film can be carried out using, for example, an alkaline peeling solution such as a sodium hydroxide solution.

[0160] After preparing the substrate, a resin composition layer is formed on the substrate. When a conductor layer is formed on the surface of the substrate, the resin composition layer is preferably formed so that the conductor layer is embedded in the resin composition layer.

[0161] The resin composition layer is formed, for example, by laminating a resin sheet and a substrate. This lamination can be performed, for example, by bonding the resin sheet to the substrate from the support side under heat and pressure, thereby laminating the resin composition layer to the substrate. Examples of the member for heat-pressing the resin sheet to the substrate (hereinafter, sometimes referred to as a "heat-pressing member") include a heated metal plate (such as a SUS plate) or a metal roll (such as a SUS roll). It is preferable to press the heat-pressing member through an elastic material such as heat-resistant rubber so that the resin sheet can sufficiently follow the surface irregularities of the substrate, rather than directly pressing the resin sheet.

[0162] The lamination of the substrate and the resin sheet may be carried out, for example, by a vacuum lamination method. In the vacuum lamination method, the thermocompression temperature is preferably in the range of 60°C to 160°C, more preferably in the range of 80°C to 140°C. The thermocompression pressure is preferably in the range of 0.098MPa to 1.77MPa, more preferably in the range of 0.29MPa to 1.47MPa. The thermocompression time is preferably in the range of 20 seconds to 400 seconds, more preferably in the range of 30 seconds to 300 seconds. The lamination is preferably carried out under reduced pressure conditions of a pressure of 13hPa or less.

[0163] After lamination, the laminated resin sheets may be smoothed under normal pressure (atmospheric pressure), for example, by pressing the support side with a thermocompression member. The pressing conditions for the smoothing treatment may be the same as the thermocompression conditions for the lamination. The lamination and smoothing treatment may be performed successively using a vacuum laminator.

[0164] The resin composition layer can be formed, for example, by compression molding. The molding conditions may be the same as those of the method for forming the resin composition layer in the step of forming the sealing layer of the semiconductor chip package described later.

[0165] After forming the resin composition layer on the substrate, the resin composition layer is thermally cured to form an insulating layer. The thermal curing conditions for the resin composition layer vary depending on the type of resin composition, but the curing temperature is usually in the range of 120°C to 240°C (preferably in the range of 150°C to 220°C, more preferably in the range of 170°C to 200°C), and the curing time is in the range of 5 minutes to 120 minutes (preferably in the range of 10 minutes to 100 minutes, more preferably in the range of 15 minutes to 90 minutes).

[0166] Before the resin composition layer is thermally cured, the resin composition layer may be subjected to a preheating treatment at a temperature lower than the curing temperature. For example, prior to thermally curing the resin composition layer, the resin composition layer may be preheated at a temperature of usually 50° C. or more and less than 120° C. (preferably 60° C. or more and 110° C. or less, more preferably 70° C. or more and 100° C. or less) for usually 5 minutes or more (preferably 5 minutes to 150 minutes, more preferably 15 minutes to 120 minutes).

[0167] In the manner described above, a circuit board having an insulating layer can be manufactured. The method for manufacturing a circuit board may further include any optional step. For example, when a circuit board is manufactured using a resin sheet, the manufacturing method of the circuit board may include a step of peeling off the support of the resin sheet. The support may be peeled off before or after the resin composition layer is thermally cured.

[0168] The method for manufacturing a circuit board may include, for example, a step of polishing the surface of the insulating layer after forming the insulating layer. The polishing method is not particularly limited. For example, the surface of the insulating layer can be polished using a surface grinder.

[0169] The method for manufacturing a circuit board may include, for example, a step (3) of connecting the conductor layers to each other, that is, a step of drilling holes in the insulating layer. This allows holes such as via holes and through holes to be formed in the insulating layer. Examples of methods for forming via holes include laser irradiation, etching, and mechanical drilling. The dimensions and shape of the via holes may be appropriately determined depending on the design of the circuit board. In addition, in the step (3), the insulating layer may be polished or ground to perform the interlayer connection.

[0170] After the via holes are formed, it is preferable to carry out a step of removing smears in the via holes. This step is sometimes called a desmear step. For example, when the conductive layer is formed on the insulating layer by a plating step, the via holes may be subjected to a wet desmear process. When the conductive layer is formed on the insulating layer by a sputtering step, a dry desmear process such as a plasma treatment process may be carried out. Furthermore, the insulating layer may be roughened by the desmear process.

[0171] Furthermore, before forming the conductor layer on the insulating layer, the insulating layer may be subjected to a roughening treatment. This roughening treatment usually roughens the surface of the insulating layer including the inside of the via hole. The roughening treatment may be either a dry or wet roughening treatment. An example of the dry roughening treatment is a plasma treatment. An example of the wet roughening treatment is a method in which a swelling treatment using a swelling liquid, a roughening treatment using an oxidizing agent, and a neutralization treatment using a neutralizing liquid are performed in this order.

[0172] After the via holes are formed, a conductor layer may be formed on the insulating layer. By forming a conductor layer at the position where the via holes are formed, the newly formed conductor layer and the conductor layer on the surface of the substrate are electrically connected to each other, and interlayer connection is performed. Examples of the method for forming the conductor layer include plating, sputtering, and vapor deposition, among which plating is preferred. In a preferred embodiment, the surface of the insulating layer is plated by an appropriate method such as a semi-additive method or a full-additive method to form a conductor layer having a desired wiring pattern. In addition, when the support in the resin sheet is a metal foil, a conductor layer having a desired wiring pattern can be formed by a subtractive method. The material of the conductor layer to be formed may be a single metal or an alloy. In addition, this conductor layer may have a single layer structure, or may have a multi-layer structure including two or more layers of different types of materials.

[0173] Here, an example of an embodiment in which a conductor layer is formed on an insulating layer will be described in detail. A plating seed layer is formed on the surface of the insulating layer by electroless plating. Then, a mask pattern is formed on the formed plating seed layer, exposing a part of the plating seed layer corresponding to a desired wiring pattern. After forming an electrolytic plating layer on the exposed plating seed layer by electrolytic plating, the mask pattern is removed. Thereafter, unnecessary plating seed layer is removed by a process such as etching, and a conductor layer having a desired wiring pattern can be formed. Note that, when forming the conductor layer, the dry film used to form the mask pattern is the same as the above-mentioned dry film.

[0174] The method for producing a circuit board may include a step (4) of removing the substrate. By removing the substrate, a circuit board having an insulating layer and a conductor layer embedded in the insulating layer is obtained. This step (4) can be performed, for example, when a substrate having a peelable metal layer is used.

[0175] <Semiconductor chip package> The semiconductor chip package according to the first embodiment of the present invention includes the above-mentioned circuit board and a semiconductor chip mounted on the circuit board. The semiconductor chip package can be manufactured by bonding the semiconductor chip to the circuit board.

[0176] The bonding conditions between the circuit board and the semiconductor chip may be any conditions that allow conductive connection between the terminal electrodes of the semiconductor chip and the circuit wiring of the circuit board. For example, the conditions used in flip-chip mounting of the semiconductor chip may be used. Also, for example, the semiconductor chip and the circuit board may be bonded via an insulating adhesive.

[0177] An example of a bonding method is a method in which a semiconductor chip is pressure-bonded to a circuit board. Pressure-bonding conditions are a pressure-bonding temperature usually in the range of 120°C to 240°C (preferably in the range of 130°C to 200°C, more preferably in the range of 140°C to 180°C), and a pressure-bonding time usually in the range of 1 second to 60 seconds (preferably in the range of 5 seconds to 30 seconds).

[0178] Another example of the bonding method is a method of bonding a semiconductor chip to a circuit board by reflow. The reflow conditions may be in the range of 120°C to 300°C.

[0179] After the semiconductor chip is bonded to the circuit board, the semiconductor chip may be filled with a molded underfill material. As the molded underfill material, the above-mentioned resin composition or the above-mentioned resin sheet may be used.

[0180] The semiconductor chip package according to the second embodiment of the present invention includes a semiconductor chip and a cured product of the resin composition that encapsulates the semiconductor chip. In such a semiconductor chip package, the cured product of the resin composition usually functions as an encapsulation layer. An example of the semiconductor chip package according to the second embodiment is a fan-out type WLP.

[0181] The method for manufacturing such a semiconductor chip package includes: (A) a step of laminating a temporary fixing film on a substrate; (B) a step of temporarily fixing a semiconductor chip on a temporary fixing film; (C) forming an encapsulation layer on the semiconductor chip; (D) peeling the substrate and the temporary fixing film from the semiconductor chip; (E) a step of forming a rewiring formation layer as an insulating layer on the surface of the semiconductor chip from which the base material and the temporary fixing film have been peeled off; (F) forming a rewiring layer as a conductor layer on the rewiring formation layer; and (G) forming a solder resist layer on the rewiring layer; The method for manufacturing the semiconductor chip package further comprises: (H) A process of dicing and separating multiple semiconductor chip packages into individual semiconductor chip packages. may also include

[0182] (Process (A)) Step (A) is a step of laminating a temporary fixing film on a substrate. The lamination conditions for the substrate and the temporary fixing film can be the same as the lamination conditions for the substrate and the resin sheet in the method for producing a circuit board.

[0183] Examples of the substrate include silicon wafers; glass wafers; glass substrates; metal substrates such as copper, titanium, stainless steel, and cold-rolled steel (SPCC); substrates such as FR-4 substrates in which glass fibers are impregnated with epoxy resin or the like and then heat-cured; and substrates made of bismaleimide triazine resins such as BT resin.

[0184] The temporary fixing film may be made of any material that can be peeled off from the semiconductor chip and can temporarily fix the semiconductor chip. Commercially available products include "Riva Alpha" manufactured by Nitto Denko Corporation.

[0185] (Process (B)) Step (B) is a step of temporarily fixing the semiconductor chip on the temporary fixing film. The temporary fixing of the semiconductor chip can be performed using, for example, a device such as a flip chip bonder or a die bonder. The layout and number of the semiconductor chips can be appropriately set depending on the shape and size of the temporary fixing film, the number of semiconductor chip packages to be produced, etc. For example, the semiconductor chips may be temporarily fixed by arranging them in a matrix shape of multiple rows and multiple columns.

[0186] (Process (C)) Step (C) is a step of forming an encapsulating layer on the semiconductor chip. The encapsulating layer is formed by a cured product of the above-mentioned resin composition. The encapsulating layer is usually formed by a method including a step of forming a resin composition layer on the semiconductor chip and a step of thermally curing the resin composition layer to form the encapsulating layer.

[0187] Taking advantage of the excellent compression moldability of the resin composition, the resin composition layer is preferably formed by a compression molding method. In the compression molding method, the semiconductor chip and the resin composition are usually placed in a mold, and pressure and, if necessary, heat are applied to the resin composition in the mold to form a resin composition layer covering the semiconductor chip.

[0188] A specific operation of the compression molding method can be, for example, as follows. An upper mold and a lower mold are prepared as molds for compression molding. A resin composition is applied to the semiconductor chip temporarily fixed on the temporary fixing film as described above. The semiconductor chip to which the resin composition is applied is attached to the lower mold together with the substrate and the temporary fixing film. Then, the upper mold and the lower mold are clamped, and heat and pressure are applied to the resin composition to perform compression molding.

[0189] In addition, the specific operation of the compression molding method may be, for example, as follows. An upper mold and a lower mold are prepared as molds for compression molding. A resin composition is placed on the lower mold. Also, a semiconductor chip is attached to the upper mold together with a substrate and a temporary fixing film. Thereafter, the upper mold and the lower mold are clamped so that the resin composition placed on the lower mold contacts the semiconductor chip attached to the upper mold, and heat and pressure are applied to perform compression molding.

[0190] The molding conditions vary depending on the composition of the resin composition, and appropriate conditions can be adopted so that good sealing is achieved. For example, the temperature of the mold during molding is preferably a temperature at which the resin composition can exhibit excellent compression moldability, and is preferably 80°C or higher, more preferably 100°C or higher, particularly preferably 120°C or higher, and preferably 200°C or lower, more preferably 170°C or lower, and particularly preferably 150°C or lower. The pressure applied during molding is preferably 1 MPa or higher, more preferably 3 MPa or higher, particularly preferably 5 MPa or higher, preferably 50 MPa or lower, more preferably 30 MPa or lower, and particularly preferably 20 MPa or lower. The cure time is preferably 1 minute or more, more preferably 2 minutes or more, particularly preferably 5 minutes or more, and preferably 60 minutes or less, more preferably 30 minutes or less, and particularly preferably 20 minutes or less. Usually, the mold is removed after the formation of the resin composition layer. The mold may be removed before or after the resin composition layer is thermally cured.

[0191] The resin composition layer may be formed by laminating a resin sheet and a semiconductor chip. For example, the resin composition layer of the resin sheet and the semiconductor chip are heated and pressed to form a resin composition layer on the semiconductor chip. The lamination of the resin sheet and the semiconductor chip is usually performed in the same manner as the lamination of the resin sheet and the substrate in the manufacturing method of the circuit board, using a semiconductor chip instead of the substrate.

[0192] After forming a resin composition layer on the semiconductor chip, the resin composition layer is thermally cured to obtain an encapsulation layer that covers the semiconductor chip. This encapsulates the semiconductor chip with a cured product of the resin composition. The thermal curing conditions of the resin composition layer may be the same as the thermal curing conditions of the resin composition layer in the manufacturing method of the circuit board. Furthermore, before thermally curing the resin composition layer, a preheating treatment may be performed on the resin composition layer at a temperature lower than the curing temperature. The treatment conditions of this preheating treatment may be the same as the preheating treatment in the manufacturing method of the circuit board.

[0193] (Process (D)) Step (D) is a step of peeling off the substrate and the temporary fixing film from the semiconductor chip. It is desirable to adopt an appropriate peeling method according to the material of the temporary fixing film. For example, the peeling method may be a method of heating, foaming or expanding the temporary fixing film to peel it off. In addition, for example, the peeling method may be a method of irradiating the temporary fixing film with ultraviolet light through the substrate to reduce the adhesive strength of the temporary fixing film to peel it off.

[0194] In the method of peeling off the temporary fixing film by heating, foaming or expanding it, the heating conditions are usually 100° C. to 250° C. for 1 second to 90 seconds or 5 minutes to 15 minutes. In the method of peeling off the temporary fixing film by reducing the adhesive strength of the temporary fixing film by irradiating it with ultraviolet light, the irradiation amount of ultraviolet light is usually 10 mJ / cm 2 ~1000mJ / cm 2 It is.

[0195] (Process (E)) Step (E) is a step of forming a rewiring formation layer as an insulating layer on the surface of the semiconductor chip from which the base material and the temporary fixing film have been peeled off.

[0196] The material of the rewiring formation layer can be any material having insulating properties. Among them, photosensitive resins and thermosetting resins are preferred from the viewpoint of ease of manufacturing the semiconductor chip package. The resin composition of the present invention may be used as the thermosetting resin.

[0197] After forming the rewiring formation layer, via holes may be formed in the rewiring formation layer to provide interlayer connection between the semiconductor chip and the rewiring layer.

[0198] In the method of forming a via hole when the material of the rewiring formation layer is a photosensitive resin, the surface of the rewiring formation layer is usually irradiated with active energy rays through a mask pattern to photocure the rewiring formation layer in the irradiated portion. Examples of active energy rays include ultraviolet rays, visible rays, electron beams, X-rays, etc., and ultraviolet rays are particularly preferred. The irradiation amount and irradiation time of the ultraviolet rays can be appropriately set according to the photosensitive resin. Examples of the exposure method include a contact exposure method in which a mask pattern is attached to the rewiring formation layer and exposed, and a non-contact exposure method in which a mask pattern is not attached to the rewiring formation layer and exposed using parallel rays.

[0199] After the rewiring formation layer is photocured, the rewiring formation layer is developed to remove the unexposed portion to form a via hole. The development may be performed by either wet development or dry development. Examples of the development method include a dip method, a paddle method, a spray method, a brushing method, and a scraping method, and the paddle method is preferable from the viewpoint of resolution.

[0200] When the material of the rewiring formation layer is a thermosetting resin, the method of forming the via hole may be, for example, laser irradiation, etching, mechanical drilling, etc. Among them, laser irradiation is preferable. The laser irradiation can be performed using an appropriate laser processing machine using a light source such as a carbon dioxide laser, a UV-YAG laser, or an excimer laser.

[0201] The shape of the via hole is not particularly limited, but is generally circular (approximately circular). The top diameter of the via hole is preferably 50 μm or less, more preferably 30 μm or less, and even more preferably 20 μm or less, and is preferably 3 μm or more, preferably 10 μm or more, and more preferably 15 μm or more. Here, the top diameter of the via hole refers to the diameter of the opening of the via hole on the surface of the rewiring formation layer.

[0202] (Process (F)) Step (F) is a step of forming a rewiring layer as a conductor layer on the rewiring formation layer. The method of forming the rewiring layer on the rewiring formation layer can be the same as the method of forming a conductor layer on an insulating layer in the manufacturing method of a circuit board. Steps (E) and (F) may be repeated to alternately stack (build up) the rewiring layers and the rewiring formation layers.

[0203] (Process (G)) Step (G) is a step of forming a solder resist layer on the rewiring layer. Any material having insulating properties can be used as the material of the solder resist layer. Among them, photosensitive resins and thermosetting resins are preferred from the viewpoint of ease of manufacturing the semiconductor chip package. The resin composition of the present invention may be used as the thermosetting resin.

[0204] In step (G), bumping processing may be performed to form bumps, if necessary. The bumping processing can be performed by a method such as solder balls or solder plating. In addition, the formation of via holes in the bumping processing can be performed in the same manner as in step (E).

[0205] (Process (H)) The method for manufacturing a semiconductor chip package may include a step (H) in addition to the steps (A) to (G). The step (H) is a step of dicing a plurality of semiconductor chip packages into individual semiconductor chip packages to separate them. The method for dicing the semiconductor chip packages into individual semiconductor chip packages is not particularly limited.

[0206] <Semiconductor device> The semiconductor device includes a semiconductor chip package. Examples of the semiconductor device include various semiconductor devices used in electrical products (e.g., computers, mobile phones, smartphones, tablet devices, wearable devices, digital cameras, medical devices, televisions, etc.) and vehicles (e.g., motorcycles, automobiles, trains, ships, aircraft, etc.). EXAMPLES

[0207] The present invention will be specifically described below with reference to examples. The present invention is not limited to these examples. In the following, "parts" and "%" representing amounts mean "parts by mass" and "% by mass", respectively, unless otherwise specified.

[0208] <Synthesis Example 1: Synthesis of active ester resin> 288 parts by mass of 1-naphthol and 1400 parts by mass of toluene were charged into a reaction vessel, and dissolved while the inside of the vessel was purged with nitrogen under reduced pressure. Then, 203 parts by mass of isophthalic acid chloride was charged and dissolved. While purging the inside of the vessel with nitrogen, 400 g of 20% aqueous sodium hydroxide solution was dropped over 3 hours. At that time, the temperature inside the system was controlled to 60°C or less. Then, the mixture was stirred for 1 hour to react. After the reaction was completed, the reaction product was separated and the aqueous layer was removed. This operation was repeated until the pH of the aqueous layer became 7, and toluene and the like were distilled off under heating and reduced pressure conditions to obtain an active ester resin (compound of the above formula (3); molecular weight 418.4). The functional group equivalent of the active ester resin was 209 g / equivalent, and the softening point was 78°C.

[0209] <Example 1> Glycidylamine type epoxy resin (ADEKA "EP-3980S", epoxy equivalent 115g / eq.) 2 parts, alicyclic epoxy resin (DAICEL "CELLOXIDE 2021P", epoxy equivalent 136g / eq.) 7 parts, active ester resin (softening point 78°C) obtained in Synthesis Example 1 5 parts, acid anhydride hardener (Shin Nippon Rika "MH-700") 5 parts, silica A (average particle size 9um, specific surface area 5.0m 2A resin composition was obtained by uniformly dispersing 140 parts of a polyurethane foam (surface-treated with KBM573 (manufactured by Shin-Etsu Chemical Co., Ltd.)) and 0.1 parts of a curing accelerator (1B2PZ, 1-benzyl-2-phenylimidazole, manufactured by Shikoku Kasei Co., Ltd.) using a mixer.

[0210] <Example 2> Instead of using 140 parts of silica A, alumina A (average particle size 10 μm, specific surface area 0.3 m 2 The same procedure as in Example 1 was carried out except that 170 parts of 1,2-dichloro-2,3-tetrafluoroethylene (1 / g, surface-treated with KBM5783 (manufactured by Shin-Etsu Chemical Co., Ltd.) was used, to obtain a resin composition.

[0211] <Example 3> Instead of using 140 parts of silica A, silica B (average particle size 9 μm, specific surface area 5.0 m 2 The same procedure as in Example 1 was carried out except that 140 parts of 1,2-dichlorophenyl ether (1 / g, surface-treated with KBM503 (manufactured by Shin-Etsu Chemical Co., Ltd.) was used, to obtain a resin composition.

[0212] <Example 4> A resin composition was obtained by carrying out the same operations as in Example 1, except that the amount of the active ester resin (softening point 78° C.) obtained in Synthesis Example 1 was changed from 5 parts to 3 parts, and the amount of the acid anhydride curing agent ("MH-700" manufactured by New Japan Chemical Co., Ltd.) was changed from 5 parts to 7 parts.

[0213] <Example 5> A resin composition was obtained by carrying out the same operations as in Example 1, except that the amount of the active ester resin (softening point 78° C.) obtained in Synthesis Example 1 was changed from 5 parts to 7 parts, and the amount of the acid anhydride curing agent ("MH-700" manufactured by New Japan Chemical Co., Ltd.) was changed from 5 parts to 3 parts.

[0214] <Comparative Example 1> A resin composition was obtained by the same procedure as in Example 1, except that the active ester resin (softening point 78° C.) obtained in Synthesis Example 1 was not used, and the amount of the acid anhydride curing agent ("MH-700" manufactured by New Japan Chemical Co., Ltd.) used was changed from 5 parts to 10 parts.

[0215] <Comparative Example 2> A resin composition was obtained by carrying out the same operation as in Example 1, except that 5 parts of a commercially available active ester resin ("HPC-8000" manufactured by DIC Corporation, softening point 152°C) was used instead of 5 parts of the active ester resin (softening point 78°C) obtained in Synthesis Example 1.

[0216] <Test Example 1: Evaluation of adhesion to silicon wafer after high temperature and high humidity environmental test (HAST)> The resin compositions prepared in the examples and comparative examples were compression molded on a 12-inch silicon wafer using a compression molding device (mold temperature: 130°C, pressure: 6MPa, cure time: 10 minutes) to form a resin composition layer with a thickness of 300 μm. After that, the resin composition layer was heat-cured by heating at 180°C for 90 minutes to prepare a sample. The prepared sample was subjected to a high temperature and high humidity environmental test for 100 hours under conditions of 130°C and 85% RH using a highly accelerated life tester (Kusumoto Chemical Industries, Ltd. "PM422"). After the test, the sample was checked for peeling at the interface between the cured product and the underlying silicon wafer. The case where there was no peeling at the interface between the cured product and the underlying silicon wafer was evaluated as "○", and the case where there was peeling at the interface between the cured product and the underlying silicon wafer was evaluated as "×".

[0217] <Test Example 2: Measurement of dielectric tangent> The resin compositions prepared in the Examples and Comparative Examples were compression molded on a release-treated 12-inch silicon wafer using a compression molding device (mold temperature: 130°C, pressure: 6 MPa, cure time: 10 minutes) to form a resin composition layer with a thickness of 300 μm. Thereafter, the resin composition was peeled off from the release-treated silicon wafer and heated at 180°C for 90 minutes to thermally cure the resin composition to prepare a sample. The dielectric loss tangent was measured at 79 GHz by the Fabry-Perot method. Measurements were performed on three test pieces, and the average value was calculated.

[0218] <Test Example 3: Measurement of storage modulus> The resin compositions prepared in the examples and comparative examples were compression molded on a release-treated 12-inch silicon wafer using a compression molding device (mold temperature: 130°C, pressure: 6 MPa, cure time: 10 minutes) to form a resin composition layer with a thickness of 300 μm. Thereafter, the resin composition was peeled off from the release-treated silicon wafer and heated at 180°C for 90 minutes to thermally cure the resin composition to prepare a cured product sample. The cured product was cut into a test piece with a width of 7 mm and a length of 40 mm, and dynamic mechanical analysis was performed in a tensile mode using a dynamic mechanical analyzer DMS-6100 (manufactured by Seiko Instruments Inc.). After mounting the test piece on the device, it was measured under the measurement conditions of a frequency of 1 Hz and a temperature rise rate of 5°C / min. The value of the storage modulus (E') GPa at 25°C in the measurement was read.

[0219] <Test Example 4: Evaluation of flow marks> The resin compositions prepared in the Examples and Comparative Examples were compression molded on a 12-inch silicon wafer using a compression molding device (mold temperature: 130°C, pressure: 6 MPa, cure time: 10 minutes) to form a resin composition layer with a thickness of 300 μm. After heating at 150°C for 60 minutes, the surface of the resin composition layer was visually confirmed for flow marks. Those with flow marks were marked with "X" and those without flow marks were marked with "O".

[0220] <Test Example 5: Evaluation of properties of resin composition> The properties of the resin compositions prepared in the examples and comparative examples were evaluated. When the resin composition was in a liquid state with flowability at 25°C, it was evaluated as "liquid", and when it was in a clay-like state with no flowability, it was evaluated as "clay-like".

[0221] The non-volatile components and the amounts used of the resin compositions of the Examples and Comparative Examples, as well as the measurement results and evaluation results of the Test Examples, are shown in Table 1 below.

[0222] [Table 1]

[0223] As the above results show, when the components (B-1) to (B-3) are used as the curing agent (B), it is possible to obtain a cured product with reduced dielectric properties and suppressed occurrence of flow marks.

Claims

1. A resin composition comprising (A) an epoxy resin, (B) a curing agent, and (C) an inorganic filler, wherein the component (B) is represented by formula (B-1) (1): 【Chemistry 1】 [In the formula, rings X, Y, and Z each independently represent an aromatic ring which may have a substituent selected from a halogen atom, an alkyl group, an alkenyl group, an alkoxy group, an alkylcarbonyl group, an aryl group, an aryloxy group, an arylcarbonyl group, an aralkyl group, an aromatic heterocyclic group, and a non-aromatic heterocyclic group.] and further comprising an acid anhydride curing agent, wherein the component (A) contains a liquid epoxy resin, and the content of the component (C) is 50% by mass or more when the total amount of non-volatile components in the resin composition is 100% by mass.

2. The component (B) is represented by formula (B-1) (2): 【Chemistry 2】 [In the formula, rings A, B, C, D, and E each independently represent a benzene ring which may have a substituent selected from a halogen atom, an alkyl group, an alkenyl group, an alkoxy group, an alkylcarbonyl group, an aryl group, an aryloxy group, an arylcarbonyl group, an aralkyl group, an aromatic heterocyclic group, and a non-aromatic heterocyclic group.] 2. The resin composition according to claim 1, further comprising an acid anhydride curing agent, and further comprising a difunctional active ester resin represented by the following formula (1):

3. The resin composition according to claim 1 or 2, wherein the content of the component (B-1) is 1% by mass to 20% by mass, when the total amount of non-volatile components in the resin composition is 100% by mass.

4. The resin composition according to any one of claims 1 to 3, wherein the component (C) comprises silica.

5. The resin composition according to any one of claims 1 to 4, wherein the average particle size of the component (C) is 1 µm to 40 µm.

6. The resin composition according to any one of claims 1 to 5, wherein the content of the component (C) is 70 mass% or more when the non-volatile components in the resin composition are 100 mass%.

7. The resin composition according to any one of claims 1 to 6, wherein the content of the component (C) is 80 mass% or more when the non-volatile components in the resin composition are 100 mass%.

8. The resin composition according to any one of claims 1 to 7, which is liquid at 25°C.

9. The resin composition according to any one of claims 1 to 8, for forming an insulating layer of a semiconductor chip package.

10. The resin composition according to any one of claims 1 to 8, for forming an insulating layer of a circuit board.

11. The resin composition according to any one of claims 1 to 8, for encapsulating a semiconductor chip in a semiconductor chip package.

12. A cured product of the resin composition according to any one of claims 1 to 11.

13. A resin sheet comprising a support and a resin composition layer comprising the resin composition according to any one of claims 1 to 11 provided on the support.

14. A circuit board comprising an insulating layer formed from a cured product of the resin composition according to any one of claims 1 to 11.

15. A semiconductor chip package comprising the circuit board according to claim 14 and a semiconductor chip mounted on the circuit board.

16. A semiconductor chip package comprising: a semiconductor chip; and a cured product of the resin composition according to any one of claims 1 to 11 that encapsulates the semiconductor chip.

17. A semiconductor device comprising the semiconductor chip package according to claim 15 or 16.

Citation Information

Patent Citations

  • Epoxy resin composition for low-dielectric material

    JP2002012650A

  • Epoxy resin composition for electronic material and electronic material having low permittivity

    JP2003082063A

  • Epoxy resin composition, cured product of the same, and buildup film insulating material

    JP2010077343A

  • Epoxy resin composition, cured product of the same, and resin composition for electronic part board

    JP2010077345A

  • Resin composition for mold underfill

    JP2017008312A