Laminated core and rotating electrical machine

The laminated core design with adhesive and welded portions effectively enhances fixing strength without compromising magnetic properties, demonstrated by improved breaking stress and reduced iron loss.

JP7595407B2Active Publication Date: 2024-12-06NIPPON STEEL CORPORATION
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2019132041
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2019-07-17
Publication Date
2024-12-06
Estimated Expiration
2039-07-17

AI Technical Summary

Technical Problem

Conventional laminated cores face challenges in improving lamination fixing strength without deteriorating magnetic properties.

Method used

A laminated core design incorporating adhesive sections between electromagnetic steel plates and welded portions, with specific dimensions and configurations, including ring-shaped core back portions, teeth protrusions, and strategic adhesive and weld placement, enhances fixing strength while maintaining magnetic properties.

Benefits of technology

The proposed design improves lamination fixing strength and maintains magnetic properties, as evidenced by increased breaking stress and reduced iron loss in the laminated core.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007595407000002
    Figure 0007595407000002
  • Figure 0007595407000003
    Figure 0007595407000003
  • Figure 0007595407000004
    Figure 0007595407000004
Patent Text Reader

Abstract

To improve the laminated fixing strength without deteriorating the magnetic characteristics of a laminated core.SOLUTION: A laminated core 21 include a plurality of electromagnetic steel sheets 40 laminated to each other and coated on both sides with an insulating coating, an adhesive portion 41 provided between the electromagnetic steel sheets 40 adjacent to each other in the stacking direction and bonding the electromagnetic steel sheets 40 to each other, and a welded portion 42 that welds the electromagnetic steel sheets 40 to each other.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laminated core and a rotating electric machine. [Background technology]

[0002] Conventionally, there is known a laminated core as described in the following Patent Document 1. In this laminated core, adjacent electromagnetic steel sheets in the lamination direction are bonded together. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2011-023523 A Summary of the Invention [Problem to be solved by the invention]

[0004] The conventional laminated core has room for improvement in terms of increasing the lamination fixing strength without deteriorating the magnetic properties.

[0005] The present invention has been made in consideration of the above-mentioned circumstances, and has an object to improve the lamination fixing strength without deteriorating the magnetic properties of the laminated core. [Means for solving the problem]

[0006] In order to solve the above problems, the present invention proposes the following means. [1] A magnetic coil assembly comprising: a plurality of electromagnetic steel sheets stacked on top of each other and coated on both sides with an insulating coating; adhesive portions provided between adjacent electromagnetic steel sheets in a stacking direction and bonding the electromagnetic steel sheets together; and welded portions at which the electromagnetic steel sheets are welded together; the electromagnetic steel sheets each having an annular core back portion and a plurality of teeth portions protruding radially from the core back portion and arranged at intervals in the circumferential direction of the core back portion; the adhesive portions provided on the teeth portions by an adhesive, the welded portions provided on the core back portion by welding, and the welded portions provided by welding along the outer circumferential edge of the core back portion. The teeth are joined only by the adhesive portion. Laminated core. [2] The adhesive is applied to the teeth portion, and the core back portion is welded to the core back portion. Welding The laminated core according to [1], having only [3] The laminated core according to [1] or [2], wherein the adhesive joints are dots having an average diameter of 3 to 7 mm. [4] The laminated core according to any one of [1] to [3], wherein the adhesive area ratio of the adhesive joint to the electromagnetic steel sheets is 1 to 40%. [5] The laminated core according to any one of [1] to [4], wherein the aluminum content of the electromagnetic steel sheets is 0.001 to 2.0 mass %. [6] A rotating electric machine comprising the laminated core according to any one of [1] to [5]. Effect of the Invention

[0007] According to the present invention, the lamination fixing strength can be improved without deteriorating the magnetic properties of the laminated core. [Brief description of the drawings]

[0008] [Figure 1] 1 is a plan view of a rotating electrical machine including a laminated core according to an embodiment of the present invention; [Diagram 2] FIG. 2 is a side view of the laminated core shown in FIG. [Diagram 3] 2 is a partial plan view of a first surface of an electromagnetic steel sheet in a laminated core according to an embodiment of the present invention. FIG. [Figure 4] 5 is a partial plan view of a first surface of an electromagnetic steel sheet in a laminated core according to another embodiment of the present invention. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, a laminated core according to an embodiment of the present invention and a rotating electric machine including this laminated core will be described with reference to the drawings. In this embodiment, the rotating electric machine will be described by taking an electric motor, specifically an AC electric motor, more specifically a synchronous electric motor, and even more specifically a permanent magnet field type electric motor, as an example. This type of electric motor is preferably used in, for example, electric vehicles.

[0010] 1, the rotating electric machine 10 includes a stator 20, a rotor 30, a case 50, and a rotating shaft 60. The stator 20 and the rotor 30 are housed in the case 50. The stator 20 is fixed to the case 50. In this embodiment, an inner rotor type rotating electric machine 10 is used in which the rotor 30 is located inside the stator 20. However, an outer rotor type rotating electric machine 10 in which the rotor 30 is located outside the stator 20 may also be used. Also, in this embodiment, the rotating electric machine 10 is a three-phase AC motor with 12 poles and 18 slots. However, the number of poles, the number of slots, the number of phases, etc. can be changed as appropriate. The rotating electric machine 10 can rotate at a rotation speed of 1000 rpm by applying an excitation current with an effective value of 10 A and a frequency of 100 Hz to each phase, for example.

[0011] The stator 20 includes a stator core 21 and a winding (not shown). The stator core 21 includes an annular core back portion 22 and a plurality of teeth portions 23. The core back portion 22 is an area surrounded by an outer peripheral edge 22a of the core back portion and an inner peripheral edge 22b (indicated by a broken line in FIG. 3) of the core back portion. Hereinafter, the direction of the central axis O of the stator core 21 (or the core back portion 22) is referred to as the axial direction, the radial direction (direction perpendicular to the central axis O) of the stator core 21 (or the core back portion 22) is referred to as the radial direction, and the circumferential direction (direction going around the central axis O) of the stator core 21 (or the core back portion 22) is referred to as the circumferential direction.

[0012] The core back portion 22 is formed in an annular shape when viewed in a plan view of the stator 20 in the axial direction. The multiple teeth portions 23 protrude radially inward from the core back portion 22 (toward the central axis O of the core back portion 22 along the radial direction). The multiple teeth portions 23 are arranged at equal intervals in the circumferential direction. In this embodiment, 18 teeth portions 23 are provided at central angle intervals of 20 degrees around the central axis O. The multiple teeth portions 23 are formed to have the same shape and size as one another. Eighteen approximately trapezoidal slots 24 are formed radially between the multiple teeth portions 23. The winding is wound around the teeth portion 23. The winding may be a concentrated winding or a distributed winding.

[0013] The rotor 30 is disposed radially inside the stator 20 (the stator core 21). The rotor 30 includes a rotor core 31 and a plurality of permanent magnets 32. The rotor core 31 is formed in an annular (circular) shape and is disposed coaxially with the stator 20. The rotating shaft 60 is disposed within the rotor core 31. The rotating shaft 60 is fixed to the rotor core 31. The permanent magnets 32 are fixed to the rotor core 31. In this embodiment, a pair of the permanent magnets 32 forms one magnetic pole. The pairs of the permanent magnets 32 are arranged at equal intervals in the circumferential direction. In this embodiment, 12 pairs of the permanent magnets 32 (total of 24 magnets) are provided at central angle intervals of 30 degrees around the central axis O.

[0014] In this embodiment, an embedded magnet motor is used as the permanent magnet field type motor. A rotor core 31 is formed with a plurality of through holes 33 that pass through the rotor core 31 in the axial direction. The plurality of through holes 33 are provided corresponding to a plurality of permanent magnets 32. Each permanent magnet 32 ​​is fixed to the rotor core 31 while being disposed in the corresponding through hole 33. Each permanent magnet 32 ​​can be fixed to the rotor core 31 by, for example, bonding the outer surface of the permanent magnet 32 ​​to the inner surface of the through hole 33 with an adhesive. Note that a surface magnet motor may be used as the permanent magnet field type motor instead of the embedded magnet motor.

[0015] Both the stator core 21 and the rotor core 31 are laminated cores. As shown in Fig. 2, the stator 20 is formed by laminating a plurality of electromagnetic steel sheets 40. Welded portions 42 are formed on the outer circumferential surface of the stator 20. The welded portions 42 join the electromagnetic steel sheets 40 adjacent to each other in the lamination direction. The lamination thickness of each of the stator core 21 and the rotor core 31 is, for example, 50.0 mm. The outer diameter of the stator core 21 is, for example, 250.0 mm. The inner diameter of the stator core 21 is, for example, 165.0 mm. The outer diameter of the rotor core 31 is, for example, 163.0 mm. The inner diameter of the rotor core 31 is, for example, 30.0 mm. However, these values ​​are merely examples, and the lamination thickness, outer diameter, and inner diameter of the stator core 21 and the lamination thickness, outer diameter, and inner diameter of the rotor core 31 are not limited to these values. Here, the inner diameter of the stator core 21 is based on the tip end of the teeth portion 23 of the stator core 21. The inner diameter of the stator core 21 is the diameter of an imaginary circle inscribed in the tips of all the teeth portions 23.

[0016] Each of the electromagnetic steel sheets 40 forming the stator core 21 and the rotor core 31 is formed, for example, by punching an electromagnetic steel sheet as a base material. The electrical steel sheet 40 contains the elements carbon (C), silicon (Si), manganese (Mn), aluminum (Al), phosphorus (P), sulfur (S), nitrogen (N), and tin (Sn), with the remainder being iron (Fe) and impurities. The impurities refer to components contained in raw materials or components mixed in during the manufacturing process, but not intentionally contained in the steel sheet.

[0017] The carbon content (also referred to as C content) of the electrical steel sheet 40 is preferably more than 0 and 0.01 mass % or less with respect to the mass of the electrical steel sheet 40 . The silicon content (also referred to as the Si content) of the electromagnetic steel sheet 40 is preferably 2.0 to 4.0 mass % relative to the mass of the electromagnetic steel sheet 40 . The manganese content (also referred to as Mn content) of the electrical steel sheet 40 is preferably 0.1 to 4.0 mass % relative to the mass of the electrical steel sheet 40 . The aluminum content (also referred to as the Al content) of the electromagnetic steel sheets 40 will be described later. The phosphorus content (also referred to as the P content) of the electrical steel sheet 40 is preferably more than 0 and 0.2 mass % or less with respect to the mass of the electrical steel sheet 40 . The sulfur content (also referred to as S content) of the electrical steel sheet 40 is preferably more than 0 and 0.006 mass % or less with respect to the mass of the electrical steel sheet 40 . The nitrogen content (also referred to as N content) of the magnetic steel sheet 40 is preferably more than 0 and 0.005 mass % or less with respect to the mass of the magnetic steel sheet 40 . The tin content (also referred to as Sn content) of the electrical steel sheet 40 is preferably more than 0 and 0.10 mass % or less with respect to the mass of the electrical steel sheet 40 .

[0018] The Al content of the electromagnetic steel sheet 40 is preferably 0.001 to 2.0 mass%, more preferably 0.01 to 2.0 mass%, and even more preferably 0.03 to 2.0 mass%, relative to the mass of the electromagnetic steel sheet 40. When the Al content of the electromagnetic steel sheet 40 is equal to or greater than the above lower limit, deoxidation of the molten pool when welding the electromagnetic steel sheet 40 is promoted, and the occurrence of welding blowholes is easily suppressed. This makes it possible to widen the weld bead width, making it easier to suppress the occurrence of welding defects. When the Al content of the electromagnetic steel sheet 40 is equal to or less than the above upper limit, the mechanical strength of the electromagnetic steel sheet 40 is easily improved.

[0019] The contents of elements contained in the electrical steel sheet 40 can be measured by a general analytical method. For example, they can be measured using ICP-AES (Inductively Coupled Plasma-Atomic Emission Spectrometry). The C content and S content can be measured using a combustion-infrared absorption method. The N content can be measured using an inert gas fusion-thermal conductivity method.

[0020] In order to improve the workability of the electromagnetic steel sheet and the iron loss of the laminated core, both sides of the electromagnetic steel sheet 40 are covered with an insulating coating. Examples of the material that constitutes the insulating coating include (1) an inorganic compound, (2) an organic resin, and (3) a mixture of an inorganic compound and an organic resin. Examples of the inorganic compound include (1) a complex of dichromate and boric acid, and (2) a complex of phosphate and silica. Examples of the organic resin include epoxy resin, acrylic resin, acrylic styrene resin, polyester resin, silicone resin, and fluororesin. The organic resin may be the same as or different from the organic resin contained in the adhesive described below.

[0021] In order to ensure the insulating performance between the stacked magnetic steel sheets 40, the thickness of the insulating coating (the thickness per one side of the magnetic steel sheets 40) is preferably 0.1 μm or more. On the other hand, as the insulating coating becomes thicker, the insulating effect becomes saturated. Also, as the insulating coating becomes thicker, the space factor decreases, and the performance as a laminated core decreases. Therefore, it is preferable that the insulating coating is thin as long as the insulating performance can be ensured. The thickness of the insulating coating (thickness per one side of the magnetic steel sheet 40) is preferably 0.1 μm or more and 5 μm or less, and more preferably 0.1 μm or more and 2 μm or less. The thickness of the insulating coating can be measured, for example, by observing a cross section obtained by cutting the magnetic steel sheet 40 in the thickness direction with a microscope or the like.

[0022] As the magnetic steel sheet 40 becomes thinner, the effect of improving iron loss gradually saturates. Furthermore, as the magnetic steel sheet 40 becomes thinner, the manufacturing cost of the magnetic steel sheet 40 increases. Therefore, taking into consideration the effect of improving iron loss and the manufacturing cost, it is preferable that the thickness of the magnetic steel sheet 40 be 0.10 mm or more. On the other hand, if the electromagnetic steel sheet 40 is too thick, it becomes difficult to perform the press punching operation on the electromagnetic steel sheet 40. Therefore, in consideration of the press punching operation on the electromagnetic steel sheet 40, it is preferable that the thickness of the electromagnetic steel sheet 40 be 0.65 mm or less. Furthermore, the iron loss increases as the thickness of the electromagnetic steel sheet 40 increases. Therefore, taking into consideration the iron loss characteristics of the electromagnetic steel sheet 40, the thickness of the electromagnetic steel sheet 40 is preferably 0.35 mm or less, more preferably 0.25 mm or less, and even more preferably 0.20 mm or less. In consideration of the above, the thickness of each of the electromagnetic steel sheets 40 is, for example, preferably 0.10 mm to 0.65 mm, more preferably 0.10 mm to 0.35 mm, further preferably 0.10 mm to 0.25 mm, and particularly preferably 0.10 mm to 0.20 mm. The thickness of the electromagnetic steel sheets 40 includes the thickness of the insulating coating. The thickness of the electromagnetic steel sheet 40 can be measured, for example, with a micrometer.

[0023] The electromagnetic steel sheets 40 of this embodiment are not provided with any grooves for injecting adhesive to form the adhesive portions 41. This reduces the complexity involved in punching the electromagnetic steel sheets 40 and laminating and adhering the electromagnetic steel sheets 40 when manufacturing a laminated core. From the viewpoint of reducing iron loss by applying a large tension between the electromagnetic steel sheets 40, the arithmetic mean roughness (Ra) of the electromagnetic steel sheets 40 is preferably 0.5 μm or less, and more preferably 0.3 μm or less. The lower limit of Ra of the electromagnetic steel sheets 40 is not particularly limited, but is preferably 0.1 μm, for example. The Ra of the electromagnetic steel sheet 40 can be measured in accordance with the method described in JIS B0601:2013.

[0024] 2, the plurality of electromagnetic steel sheets 40 that form the stator core 21 are stacked in the thickness direction. The thickness direction is the thickness direction of the electromagnetic steel sheets 40, and corresponds to the stacking direction of the electromagnetic steel sheets 40.

[0025] As shown in Fig. 3, a plurality of electromagnetic steel sheets 40 forming the stator core 21 are fixed together by adhesive parts 41 and welded parts 42 provided on a front surface (first surface) 40a of the electromagnetic steel sheets 40. Fig. 3 shows approximately half of a plan view of the stator 20.

[0026] The adhesive portion 41 is a series of adhesive that is provided between the adjacent magnetic steel sheets 40 in the stacking direction and hardens without being separated. As the adhesive, for example, a thermosetting adhesive by polymerization bonding or the like is used. As the adhesive composition, (1) an acrylic resin, (2) an epoxy resin, (3) a composition containing an acrylic resin and an epoxy resin, and the like can be used.

[0027] The tensile modulus of the adhesive is preferably 2500 MPa to 5000 MPa, and more preferably 3000 MPa to 4000 MPa. When the tensile modulus of the adhesive is equal to or greater than the lower limit, it is easy to prevent the rigidity of the laminated core from decreasing. When the tensile modulus of the adhesive is equal to or less than the upper limit, it is easy to prevent the stress strain applied to the electromagnetic steel sheets 40 from increasing, and it is easy to prevent the magnetic property of the laminated core from deteriorating.

[0028] The tensile modulus of the cured adhesive, i.e., the adhesive joint 41, is measured by a resonance method. Specifically, the tensile modulus is measured in accordance with JIS R1602:1995. The tensile modulus of elasticity of the cured adhesive can be adjusted by the type, physical properties, molecular weight, amount added, etc. of the resin contained in the adhesive. For example, when the molecular weight of the resin contained in the adhesive is reduced, the tensile modulus of elasticity tends to increase.

[0029] As an adhesion method, for example, a method in which an adhesive is applied to the electromagnetic steel sheet 40 and then the magnetic steel sheet 40 is adhered by either or both of heating and compression bonding can be adopted. The heating means may be any means, such as heating in a high-temperature bath or electric furnace, or direct application of electricity.

[0030] In order to obtain a stable and sufficient adhesive strength, the thickness of the adhesive portion 41 is preferably 1 μm or more. On the other hand, when the thickness of the adhesive portion 41 exceeds 100 μm, the adhesive strength is saturated. Also, as the adhesive portion 41 becomes thicker, the space factor decreases, and the magnetic properties such as iron loss of the laminated core deteriorate. Therefore, the thickness of the adhesive portion 41 is preferably 1 μm or more and 100 μm or less, and more preferably 1 μm or more and 10 μm or less. The thickness of the adhesive portion 41 can be measured in the same manner as the thickness of the insulating coating. The thickness of the adhesive portion 41 can be adjusted by changing the type and amount of adhesive applied to the electromagnetic steel sheet 40 .

[0031] 3, the adhesive portion 41 is formed in the form of a plurality of circular dots. More specifically, the adhesive portion 41 is formed in the form of dots having an average diameter of 5 mm on each of the teeth 23. The average diameter shown here is an example. The average diameter of the dot-like adhesive portions 41 is preferably 3 to 7 mm. When the average diameter is equal to or greater than the above lower limit, the magnetic steel sheets 40 can be easily bonded together sufficiently. When the average diameter is equal to or less than the above upper limit, the iron loss of the laminated core can be easily suppressed. The average diameter is obtained by using a ruler to measure the diameter of the adhesive mark at the bonded portion 41 after peeling the electromagnetic steel sheets 40 apart. If the shape of the adhesive mark in plan view is not a perfect circle, the diameter is the diameter of the circumscribing circle (perfect circle) of the adhesive mark in plan view. The formation pattern of the adhesive portions 41 in FIG. 3 is one example, and the number, shape, and arrangement of the adhesive portions 41 provided between the electromagnetic steel sheets 40 can be appropriately changed as necessary.

[0032] Generally, when an adhesive is cured, curing shrinkage occurs. This curing shrinkage applies compressive stress and tensile stress to the electromagnetic steel sheet 40. When these stresses are applied to the electromagnetic steel sheet 40, distortion occurs. In particular, in the case of a thermosetting adhesive, the applied stress becomes large due to the difference in the thermal expansion coefficient between the electromagnetic steel sheet 40 and the adhesive part. Distortion of the electromagnetic steel sheet 40 increases the iron loss of the rotating electric machine 10. The influence of distortion of the electromagnetic steel sheets 40 constituting the stator core 21 on iron loss is greater than the influence of distortion of the steel sheets constituting the rotor core 31 on iron loss. In this embodiment, since the adhesive portion 41 is provided partially, the stress applied to the magnetic steel sheet 40 due to hardening shrinkage is reduced compared to when the adhesive portion 41 is provided over the entire surface.

[0033] The adhesive area ratio of the adhesive portion 41 to the electromagnetic steel sheet 40 is preferably 1 to 40%, more preferably 1 to 30%, and even more preferably 1 to 20%. When the adhesive area ratio is equal to or greater than the lower limit, the mechanical strength of the laminated core is ensured. When the adhesive area ratio is equal to or less than the upper limit, the iron loss suppression effect is more excellent. The adhesive area ratio of the electromagnetic steel sheet 40 by the adhesive portion 41 is the ratio of the area of ​​the region (adhesive region) on the first surface where the adhesive portion 41 is provided to the area of ​​the first surface of the electromagnetic steel sheet 40. The region where the adhesive portion 41 is provided is a region (adhesive region) on the first surface of the electromagnetic steel sheet 40 where a continuous, hardened adhesive is provided without being separated. The area of ​​the region where the adhesive portion 41 is provided can be found, for example, by photographing the first surface of the electromagnetic steel sheet 40 after peeling and performing image analysis on the photographed result. The area of ​​the first surface of the electromagnetic steel sheet 40 includes the area of ​​a welded portion 42, which will be described later.

[0034] As shown in Fig. 3, welded portions 42 are provided along the outer peripheral edge 22a of the core back portion 22 of the electromagnetic steel sheet 40. That is, the electromagnetic steel sheets 40 are joined together by a combination of adhesive portions 41 and welded portions 42. By using the adhesive portions 41 and welded portions 42 together, the laminated fixing strength of the stator 20 can be improved compared to a case where the same area is fixed only by adhesion. In addition, by using the adhesive portions 41 and welded portions 42 together, the electromagnetic steel sheets 40 can be laminated together with high accuracy. This can further improve the magnetic properties of the laminated core.

[0035] The welded portion 42 is formed of a weld metal. Here, the weld metal means a metal in which the magnetic steel sheet 40 and the welding wire are melted and mixed together. The welded portion 42 is formed, for example, by arc welding the electromagnetic steel sheets 40 together using a welding wire. As the welding wire, solid wires of various component systems can be used.

[0036] In this embodiment, the welded portion 42 is formed on the first surface 40a of the electromagnetic steel sheet 40 outside the outer circumferential edge 22a of the core back portion 22. 3, welded portions 42 are provided intermittently along the outer peripheral edge 22a on the outside of the outer peripheral edge 22a of the core back portion 22. Part of the welded portions 42 is embedded into the inner side of the outer peripheral edge 22a of the core back portion 22. 3, the welded portions 42 are formed in six locations along the circumferential direction. The welded portions 42 are formed at positions corresponding to the teeth portions 23. The welded portions 42 are formed at every third location on the teeth portions 23. In other words, six welded portions 42 are provided at central angle intervals of 60 degrees around the central axis O. The circumferential width (bead width) of welded portion 42 is, for example, preferably 1 to 10 mm, more preferably 2 to 8 mm, and even more preferably 3 to 6 mm. When the bead width of welded portion 42 is equal to or greater than the above lower limit, the lamination fixing strength of stator 20 can be further improved. When the bead width of welded portion 42 is equal to or less than the above upper limit, the magnetic properties of stator 20 are easily maintained. The bead width of welded portion 42 in FIG. 3 is 4 mm. The bead width of welded portion 42 can be measured, for example, with a ruler. When the welded portion 42 is provided as shown in FIG. 3, the ratio of the size (bead width) of the welded portion 42 to the length of the outer peripheral edge 22a of the core back portion 22 of the first surface 40a of the electromagnetic steel sheet 40 (100%) is, for example, 3%. The length of the outer circumferential edge 22a is determined from the outer diameter of the stator core 21, for example.

[0037] As shown in FIG. 4, the welded portion 42 is provided at 18 positions at 20 degree intervals around the central axis O along the outer peripheral edge 22a of the core back portion 22 on the outside of the outer peripheral edge 22a. FIG. 4 shows approximately half of a plan view of the stator 20A. A part of the welded portion 42 is embedded inside the outer peripheral edge 22a of the core back portion 22. In the example shown in FIG. 4, the welded portion 42 is shifted from the tooth portion 23 in the circumferential direction. The welded portion 42 is provided at a position corresponding to the slot 24 on the outer peripheral edge 22a of the core back portion 22. That is, the welded portion 42 is not provided on the portion of the outer peripheral edge 22a of the core back portion 22 located radially outside the tooth portion 23. By providing the welded portions 42 at 18 locations along the outer peripheral edge 22a of the core-back portion 22, the lamination fixing strength of the stator 20A can be further improved compared to the stator 20. When the welded portion 42 is provided as shown in FIG. 4, the ratio of the size (bead width) of the welded portion 42 to the length of the outer peripheral edge 22a of the core back portion 22 of the first surface 40a of the electromagnetic steel sheet 40 (100%) is, for example, 9%.

[0038] The formation patterns of the welded portions 42 in FIG. 3 and FIG. 4 are just examples, and the number, shape, and arrangement of the welded portions 42 provided between the magnetic steel sheets 40 can be appropriately changed as necessary.

[0039] As a welding method, for example, a method can be used in which the electromagnetic steel sheets 40 are fixed with an adhesive, a welding wire is placed on the outer peripheral edge 22a of the core back portion 22 along the stacking direction of the electromagnetic steel sheets 40, and welding is performed by arc welding. The welding method may be, for example, a method in which an adhesive is applied to the electromagnetic steel sheet 40, a welding wire is placed on the outer peripheral edge 22a of the core back portion 22 of the electromagnetic steel sheet 40, and the sheets are bonded by either or both of heating and crimping, and then welded by arc welding. Another welding method is laser welding.

[0040] In this embodiment, the multiple electromagnetic steel sheets 40 that form the rotor core 31 are fixed to each other by crimping C (dowels). However, the multiple electromagnetic steel sheets that form the rotor core may be bonded to each other by either or both of adhesive joints and welded joints. Incidentally, the laminated cores such as the stator core 21 and the rotor core 31 may be formed by so-called rotational lamination.

[0041] As described above, in the stator core 21 (laminated core) according to this embodiment, the teeth portion 23 is provided with a plurality of adhesive portions 41, and the core back portion 22 has welded portions 42 intermittently provided along the outer circumferential edge 22a. This configuration can further improve the lamination fixing strength of stator 20. In addition, by using adhesive parts 41 and welded parts 42 in combination, magnetic steel sheets 40 can be laminated with high precision. This can suppress deterioration of the magnetic properties of the laminated core.

[0042] The technical scope of the present invention is not limited to the above-described embodiment, and various modifications can be made without departing from the spirit of the present invention.

[0043] The shape of the stator core is not limited to the shape shown in the above embodiment. Specifically, the outer diameter and inner diameter of the stator core, the lamination thickness, the number of slots, the circumferential and radial dimensional ratio of the teeth portion 23, and the radial dimensional ratio of the teeth portion 23 and the core back portion 22 can be designed as desired according to the characteristics of the rotating electric machine.

[0044] In the rotor in the above embodiment, a pair of permanent magnets 32 form one magnetic pole, but the present invention is not limited to this. For example, one permanent magnet 32 ​​may form one magnetic pole, or three or more permanent magnets 32 may form one magnetic pole.

[0045] In the above embodiment, a permanent magnet field type electric motor has been used as an example of a rotating electric motor, but the structure of the rotating electric motor is not limited to this, as exemplified below, and various known structures not exemplified below can also be adopted. In the above embodiment, a permanent magnet field motor is used as an example of a synchronous motor, but the present invention is not limited to this. For example, the rotating electric machine may be a reluctance motor or an electromagnetic field motor (wound field motor). In the above embodiment, a synchronous motor is used as an example of an AC motor, but the present invention is not limited to this. For example, the rotating electric machine may be an induction motor. In the above embodiment, an AC motor is used as an example of the electric motor, but the present invention is not limited to this. For example, the rotating electric machine may be a DC motor. In the above embodiment, an electric motor is used as an example of a rotating electric machine, but the present invention is not limited to this. For example, the rotating electric machine may be a generator.

[0046] In the above embodiment, the laminated core according to the present invention is applied to a stator core, but it can also be applied to a rotor core.

[0047] In addition, within the scope of the invention, the components in the above-described embodiments may be replaced with well-known components, and the above-described modified examples may be combined as appropriate. EXAMPLES

[0048] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples.

[0049] [Example 1] As shown in Fig. 3, adhesive was applied in dots to the teeth portions on the first surfaces of the electromagnetic steel sheets, and multiple electromagnetic steel sheets were stacked and pressed together to obtain a laminate. Welding wire was placed at six locations on the outer periphery of the core back portion along the stacking direction of the obtained laminate, and welds were formed by arc welding to obtain a laminated core. The bonding area ratio to the area of ​​the first surface of the electromagnetic steel sheet was set to 1%. The ratio of the size of the weld (bead width) to the outer periphery length of the core-back portion of the first surface of the electromagnetic steel sheet (100%) was set to 3%. The laminated core was obtained using an electromagnetic steel sheet having the following chemical composition and a thickness of 0.20 mm. <Chemical composition of electrical steel sheet> Carbon content: 0.002 mass% based on the mass of the electrical steel sheet. ·Si content: 3.2 mass% based on the mass of the electrical steel sheet. Mn content: 0.5 mass% based on the mass of the electrical steel sheet. · Al content: 0.5 mass% based on the mass of the electrical steel sheet. P content: 0.01 mass% based on the mass of the electrical steel sheet. S content: 0.0015 mass% based on the mass of the electrical steel sheet. N content: 0.002 mass% based on the mass of the electrical steel sheet. Sn content: 0.03 mass% based on the mass of the electrical steel sheet.

[0050] [Example 2] A laminated core was obtained in the same manner as in Example 1, except that the bonding area ratio to the area of ​​the first surface of the electromagnetic steel sheet was 20%.

[0051] [Example 3] A laminated core was fabricated in the same manner as in Example 2, except that the electromagnetic steel sheets used had a Si content of 3.5 mass % and an Al content of 0.001 mass % relative to the mass of the electromagnetic steel sheets.

[0052] [Example 4] A laminated core was fabricated in the same manner as in Example 2, except that the electromagnetic steel sheets used had a Si content of 1.7 mass % and an Al content of 2.0 mass % relative to the mass of the electromagnetic steel sheets.

[0053] [Comparative Example 1] A laminated core was fabricated in the same manner as in Example 2, except that the adhesive area ratio to the area of ​​the first surface of the electromagnetic steel sheets was 0%, ie, no adhesive portion was provided.

[0054] [Comparative Example 2] A laminated core was constructed in the same manner as in Example 2, except that the ratio of the size of the weld (bead width) to the outer circumferential length of the core back portion on the first surface of the electromagnetic steel sheet was 0%, i.e., no weld was provided.

[0055] <Rigidity evaluation> A rectangular steel plate (width 25 mm × length 100 mm) was cut out from the electromagnetic steel plate used in each example, and two steel plates were overlapped to form an overlapping portion with an overlap length of 12.5 mm. An adhesive was applied to the overlapping portion so as to achieve the adhesive area ratio and welded portion size ratio of the laminated core obtained in each example, a welding wire was placed, and arc welding was performed while crimping to obtain a test piece. For each test piece, a tensile shear adhesive strength test was performed in accordance with JIS K6850:1999 to measure the breaking stress (MPa). The tensile test environment was room temperature (25°C). The test speed was 3 mm / min. The number of test pieces was 3. The average breaking stress of the three test pieces was calculated, and the rigidity was evaluated based on the following evaluation criteria. The results are shown in Table 1. Evaluation Criteria A: The average breaking stress is 10 MPa or more. B: The average breaking stress is 5 MPa or more and less than 10 MPa. C: The average breaking stress is less than 5 MPa.

[0056] <Evaluation of magnetic properties> Next, a verification test was carried out to verify the above-mentioned effects. Note that this verification test was carried out by evaluation using an actual motor. The motor used for the actual machine evaluation had the shape shown in FIG. 1, and the lamination thickness of each of the stator core 21 and rotor core 31 was 50.0 mm. The outer diameter of the stator core 21 was 250.0 mm. The inner diameter of the stator core 21 was 165.0 mm. The outer diameter of the rotor core 31 was 163.0 mm. The inner diameter of the rotor core 31 was 30.0 mm. The winding of the stator core 21 was concentrated winding with 10 turns in the slots 24. An excitation current of 10 A effective value and 100 Hz frequency was applied to each phase to rotate the motor at a rotation speed of 1000 rpm, and the iron loss was calculated by subtracting the output from the input power and the copper loss due to the winding of the stator core.

[0057] The iron loss of the laminated core of each example was determined by the above test. For comparison, the iron loss of a laminated core in which multiple electromagnetic steel sheets are all crimped was also determined. The iron loss of each example of the laminated core was divided by the iron loss of the laminated core for comparison (iron loss ratio). When the iron loss of each example of the laminated core is equal to the iron loss of the laminated core for comparison, the iron loss ratio is 100%. The smaller the iron loss ratio, the smaller the iron loss of the laminated core for each example, and the better the magnetic properties as a laminated core. The iron loss ratio of each example of the laminated core was calculated, and the magnetic properties of each example of the laminated core were evaluated based on the following evaluation criteria. The results are shown in Table 1. Evaluation Criteria A: Iron loss ratio is less than 100%. C: Iron loss ratio is 100% or more.

[0058] [Table 1]

[0059] As shown in Table 1, in Examples 1 to 4 in which the present invention was applied, the average breaking stress was 10 MPa or more and the iron loss ratio was less than 100%, and the laminate fixing strength was improved without deteriorating the magnetic properties. On the other hand, in Comparative Example 1, which does not have a bonded portion, the iron loss ratio was 100% or more. In Comparative Example 2, which had no welded portion, the average breaking stress was less than 5 MPa.

[0060] From the above results, it is clear that the laminated core of the present invention can improve the laminated fixing strength while suppressing iron loss, and can improve the laminated fixing strength without degrading the magnetic properties of the laminated core. [Explanation of symbols]

[0061] 20 Stator 21 Stator core (laminated core) 22 Core back section 22a Outer periphery of the core back part 22b Inner edge of core back part 23 Teeth 24 Slots 40 Electrical steel sheet 40a Surface of electromagnetic steel sheet (first side) 41 Adhesive part 42 Welding

Claims

1. A plurality of electromagnetic steel sheets stacked on top of each other and coated on both sides with insulating films; Adhesive portions provided between the electromagnetic steel sheets adjacent to each other in a stacking direction and adhering the electromagnetic steel sheets to each other; and a welded portion at which the electromagnetic steel sheets are welded to each other, the electromagnetic steel sheet includes an annular core back portion and a plurality of teeth portions protruding radially from the core back portion and arranged at intervals in a circumferential direction of the core back portion, The adhesive portion is provided on the teeth portion, The welded portion is provided on the core back portion by welding, The welded portion is provided along an outer circumferential edge of the core back portion, The teeth portion are joined only by the adhesive portion.

2. The adhesive portion is formed on the teeth portion by an adhesive; The laminated core according to claim 1 , wherein the core back portion has only the welded portion formed by welding.

3. 3. The laminated core according to claim 1, wherein the adhesive joints are dot-shaped with an average diameter of 3 to 7 mm.

4. The laminated core according to any one of claims 1 to 3, wherein the adhesive area ratio of the electromagnetic steel sheets at the adhesive joint is 1 to 40%.

5. The laminated core according to any one of claims 1 to 4, wherein the aluminum content of the electromagnetic steel sheets is 0.001 to 2.0 mass%.

6. A rotating electric machine comprising the laminated core according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • Motor

    JP2002078251A

  • Electromagnetic steel sheet laminated core which has good thermal conductivity, and method of manufacturing the same

    JP2011023523A

  • Laminated core, stator, method of manufacturing laminated core, method of manufacturing stator

    JP2015136228A

  • Laminated electrical steel plate for motor core and production method therefor

    JP2017011863A

  • Method of manufacturing laminated core

    JP2019071745A